CURABLE ORGANOPOLYSILOXANE COMPOSITION AND DEVICE

The curable organopolysiloxane composition addresses thermal conductivity and reliability issues in semiconductor devices by forming a continuous path-like structure during curing, ensuring effective heat dissipation and preventing contamination.

JP7580897B2Active Publication Date: 2024-11-12SHIN ETSU CHEMICAL CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2023517215
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-04-28
Filing Date
2022-03-31
Publication Date
2024-11-12
Estimated Expiration
2042-03-31

AI Technical Summary

Technical Problem

Conventional thermally conductive materials face issues such as insufficient thermal conductivity, contamination, leakage, and the formation of cracks and voids when used in heat-generating electronic components, leading to inadequate heat dissipation and reliability concerns.

Method used

A curable organopolysiloxane composition is developed, incorporating organopolysiloxane with varying viscosities, low melting point gallium and/or its alloy, and a specific alkoxy polysiloxane, which upon curing forms a continuous path-like structure with thermally conductive fillers, ensuring uniform dispersion and effective heat conduction without gaps.

Benefits of technology

The composition provides superior heat dissipation performance by minimizing thermal resistance, preventing contamination, and maintaining structural integrity, enhancing the reliability of semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580897000009
    Figure 0007580897000009
  • Figure 0007580897000001
    Figure 0007580897000001
  • Figure 0007580897000002
    Figure 0007580897000002
Patent Text Reader

Abstract

The present invention provides a curable organopolysiloxane composition which is in a grease state before curing and exhibits excellent workability and excellent heat dissipation effect, while forming a cured product that has been free from the occurrence of cracks or voids during the curing. A curable organopolysiloxane composition which contains the components described below. (A) Organopolysiloxanes that have different viscosities, which are (A-1) 0.01 to 10 Pa·s and (A-2) 11 to 1,000 Pa·s, while containing two or more alkenyl groups in each molecule, the alkenyl groups being bonded to a silicon atom (B) An organohydrogen polysiloxane that has two or more hydrogen atoms in each molecule, the hydrogen atoms being bonded to a silicon atom (C) Gallium and / or a gallium alloy, which has a melting point of -20°C to 70°C (D) A thermally conductive filler which has an average particle diameter of 0.1 μm to 100 μm (E) A platinum group metal catalyst (G-1) An organopolysiloxane represented by general formula (1) (In the formula (1), R1 represents an alkyl group; R2 represents an alkyl group; a represents an integer of 5 to 100; and b represents an integer of 1 to 3.)
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a curable organopolysiloxane composition, a method for producing the same, a cured product thereof, use of the cured product as a thermally conductive layer, a semiconductor device having the thermally conductive layer, and a method for producing the semiconductor device. [Background technology]

[0002] Heat-generating electronic components mounted on a printed wiring board, for example, IC packages such as CPUs, may lose performance or be damaged due to temperature rise caused by heat generation during use, so in the past, a thermally conductive sheet with good thermal conductivity was placed between the IC package and a heat dissipation member having heat dissipation fins, or thermally conductive grease was applied to efficiently conduct heat generated from the IC package to the heat dissipation member and dissipate the heat. However, as the performance of electronic components and the like improves, the amount of heat generated by them tends to increase, and there is a demand for the development of materials and components with even better thermal conductivity than conventional ones.

[0003] Conventional thermally conductive sheets have the advantage of being easily mounted and attached. In addition, thermally conductive grease is not affected by the unevenness of the surfaces of the CPU, heat dissipation components, etc., and can adhere to the unevenness without creating a gap between the two, and has the advantage of having low interfacial thermal resistance. However, both thermally conductive sheets and thermally conductive grease are obtained by blending a thermally conductive filler to impart thermal conductivity, but in the case of thermally conductive sheets, in order to avoid impairing the workability and processability in the manufacturing process, and in the case of thermally conductive grease, in order to avoid problems with the workability when applying it to heat-generating electronic components using a syringe, etc., it is necessary to suppress the upper limit of the apparent viscosity to a certain limit, so that the upper limit of the blending amount of thermally conductive filler is limited in both cases, and there is a disadvantage that sufficient thermal conductivity effect cannot be obtained.

[0004] Therefore, a method of blending a low melting point metal in a thermally conductive paste (Patent Document 1: JP Patent Publication No. 7-207160, Patent Document 2: JP Patent Publication No. 8-53664), a granular material that fixes and stabilizes liquid metal in a three-phase composite (Patent Document 3: JP Patent Publication No. 2002-121292), etc. have been proposed. However, these thermally conductive materials using low melting point metals have problems such as contaminating parts other than the coated part and leaking oily substances when used for a long period of time. To solve these problems, a method of dispersing gallium and / or a gallium alloy in a curable silicone (Patent Document 4: Japanese Patent No. 4551074) has been proposed, but when the thickness of the composition is large, the thermal conductivity is low and this is not fully satisfactory. In addition, methods for increasing the thermal conductivity have been proposed (Reference 5: Patent No. 4913874 and Reference 6: Patent No. 5640945), but cracks and voids tend to occur during hardening, and sufficient performance cannot be achieved. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 7-207160 [Patent Document 2] Japanese Patent Application Publication No. 8-53664 [Patent Document 3] JP 2002-121292 A [Patent Document 4] Patent No. 4551074 [Patent Document 5] Patent No. 4913874 [Patent Document 6] Patent No. 5640945 Summary of the Invention [Problem to be solved by the invention]

[0006] It is therefore an object of the present invention to obtain a curable organopolysiloxane composition which contains a necessary and sufficient amount of a material having excellent thermal conductivity, said material being uniformly dispersed in the form of fine particles in a matrix made of a resin component, and which gives a cured product which does not generate cracks or voids upon curing, and also to provide a method for producing said curable organopolysiloxane composition. Another object of the present invention is to provide a thermally conductive layer comprising a cured product crosslinked by heat treatment, in which the curable organopolysiloxane composition is disposed between a heat-generating electronic component and a heat-dissipating member in the same manner as conventional thermally conductive greases, without forming gaps due to conforming to the irregularities on the surface of the component or member.A further object of the present invention is to provide a semiconductor device having excellent heat dissipation performance, in which a heat-generating electronic component and a heat-dissipating member are joined via the thermally conductive layer, and a method for producing the same. [Means for solving the problem]

[0007] As a result of intensive research by the inventors to solve the above-mentioned problems, it has been found that by using an organopolysiloxane having two types of alkenyl groups with different viscosities and blending low-melting point gallium and / or its alloy, a specific alkoxypolysiloxane, a specific organohydrogenpolysiloxane bonded to silicon atoms, and a thermally conductive filler, a composition in which the gallium and / or its alloy are uniformly dispersed in a fine particle state can be easily obtained, and in the process of heat-treating the composition to form a cured product, the occurrence of cracks and voids is reduced, and the liquid gallium and / or its alloy aggregate to form large liquid particles, and at the same time, the liquid particles are further linked to the thermally conductive filler to form a kind of continuous pathway, and that the pathway-like structure is fixed and maintained in the crosslinked network formed by curing the resin component.

[0008] The inventors then discovered that by arranging the cured product obtained as described above in a layer so as to be sandwiched between a heat-generating electronic component and a heat dissipation member, it can be used as a thermally conductive layer with low thermal resistance, and that heat generated during operation of the heat-generating electronic component can be rapidly conducted to the heat dissipation member via the thermally conductive layer containing gallium and / or its alloy fixed and held in the structure described above, thereby obtaining a semiconductor product with excellent heat dissipation characteristics. Based on these discoveries, the inventors have completed the present invention. That is, the present invention provides the following curable organopolysiloxane composition and a semiconductor device using the curable organopolysiloxane composition.

[0009] <1> (A) 100 parts by mass of an organopolysiloxane consisting of the following (A-1) and (A-2), in which the ratio of (A-1) to the total of (A-1) and (A-2) is 10 to 90% by mass: (A-1) An organopolysiloxane having two or more silicon-bonded alkenyl groups per molecule, with a viscosity of 0.01 to 10 Pa s at 25°C. (A-2) An organopolysiloxane having two or more alkenyl groups bonded to silicon atoms per molecule, with a viscosity of 11 to 1,000 Pa s at 25°C. (B) an organohydrogenpolysiloxane having two or more hydrogen atoms bonded to silicon atoms per molecule: an amount such that the number of hydrogen atoms bonded to silicon atoms in the component is 0.1 to 5.0 per alkenyl group in the component (A); (C) one or more selected from the group consisting of gallium and gallium alloys, each having a melting point of −20 to 70° C.: 300 to 20,000 parts by mass; (D) a thermally conductive filler having an average particle size of 0.1 to 100 μm: 10 to 1,000 parts by mass, (E) Platinum group metal catalyst: 0.1 to 500 ppm by mass of platinum group metal relative to the mass of component (A) and, (G-1) Organopolysiloxane represented by the following general formula (1): 10 to 500 parts by mass [ka] (In formula (1), R 1 are the same or different alkyl groups, R 2 is an alkyl group, a is an integer of 5 to 100, and b is an integer of 1 to 3. 1. A curable organopolysiloxane composition comprising: <2> Furthermore, (G-2) the following general formula (2): R 3 c R 4 d Si(OR 5 ) 4-c-d (2) (In formula (2), R 3 are independently alkyl groups having 6 to 16 carbon atoms, R 4 are independently unsubstituted or substituted monovalent hydrocarbon groups having 1 to 8 carbon atoms, R 5 are independently an alkyl group having 1 to 6 carbon atoms, c is an integer of 1 to 3, d is an integer of 0 to 2, and the sum of c and d is an integer of 1 to 3. The alkoxysilane compound represented by the formula (1) is contained in an amount of 0.1 to 100 parts by mass per 100 parts by mass of the component (A). <1> 2. The curable organopolysiloxane composition according to claim 1 . <3> Further, (G-3) trifluoropropyltrimethoxysilane is contained in an amount of 0.1 to 100 parts by mass per 100 parts by mass of the component (A), <1> or <2> 2. The curable organopolysiloxane composition according to claim 1 . <4> Component (B) has five or more hydrogen atoms bonded to silicon atoms at non-terminal locations in each molecule and is represented by the following formula (3): 0.1<α / β (3) (In formula (3), α represents the number of hydrogen atoms bonded to silicon atoms not at the molecular chain terminals, and β represents the total number of silicon atoms in component (B).) It is an organohydrogenpolysiloxane that satisfies the above. <1> ~ <3> 10. The curable organopolysiloxane composition according to claim 9, <5> The component (C) is dispersed in the composition in the form of particles having a size of 1 to 200 μm. <1> ~ <4> 10. The curable organopolysiloxane composition according to claim 9, <6> <1> ~ <5> 1. A thermally conductive silicone grease composition comprising the curable organopolysiloxane composition according to any one of claims 1 to 9. <7> <1> ~ <5> 13. A cured product of the curable organopolysiloxane composition according to any one of claims 1 to 12. <8> <7> 2. Use of the cured product according to claim 1 as a thermally conductive layer disposed between a heat-generating electronic component and a heat dissipation member. <9> A heat-generating electronic component and a heat dissipation member, <7> 13. A semiconductor device having a thermally conductive layer made of the cured product according to claim 12, wherein the heat-generating electronic component and the heat dissipation member are joined via the thermally conductive layer. <10> <9> A method for manufacturing a semiconductor device according to the present invention, (a) On the surface of a heat-generating electronic component, <1> ~ <5> applying the curable organopolysiloxane composition according to any one of the above items to the surface to form a coating layer made of the composition; (b) pressing and fixing a heat dissipation member to the coating layer; and (c) A step of heating the structure obtained after step (b) at 80 to 180° C. to harden the coating layer to form a thermally conductive layer. A method for manufacturing a semiconductor device having the above structure. Effect of the Invention

[0010] The curable organopolysiloxane composition of the present invention is in a grease-like state before curing, and therefore exhibits good workability when applied to heat-generating electronic components such as CPUs. Furthermore, when the heat dissipation component is pressed against the composition, the composition conforms to the irregularities on the surfaces of both components, allowing the two to be tightly attached to each other without any gaps being generated between them, and therefore no interfacial thermal resistance is generated.

[0011] In addition, cracks and voids are rarely generated during the heat treatment process when the resin component is cured by the addition reaction, and the gallium and / or its alloy contained in the composition of the present invention aggregate to form liquid particles with a large particle size, and the liquid particles are connected to each other and further to the thermally conductive filler to form a kind of path, and the path-like structure is fixed and held in the three-dimensional crosslinked network formed by the curing of the resin component, so that the heat generated from the heat-generating electronic component can be quickly conducted to the heat dissipation member, and therefore a higher heat dissipation effect can be reliably exhibited than that of conventional thermally conductive sheets or thermally conductive greases. And, since the gallium and / or its alloy contained in the thermally conductive layer made of the cured product of the composition of the present invention incorporated in the semiconductor device and forming the path is fixed and held in the three-dimensional crosslinked network of the cured resin, it does not contaminate other components, which was a problem in the case of conventional thermally conductive greases, and does not leak oily substances over time. Therefore, the reliability of the semiconductor device can be further improved. [Brief description of the drawings]

[0012] [Figure 1] 1 is a schematic vertical cross-sectional view showing an example of a semiconductor device to which a composition of the present invention is applied. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] [Curable organopolysiloxane composition] <(A) Organopolysiloxane> Component (A) of the composition of the present invention is an organopolysiloxane having two or more alkenyl groups bonded to silicon atoms in each molecule, and is the main component (base polymer) in the addition reaction curing system of the present invention. Component (A) is composed of the following components (A-1) and (A-2):

[0014] (A-1) An organopolysiloxane having two or more silicon-bonded alkenyl groups per molecule, with a viscosity of 0.01 to 10 Pa s at 25°C. (A-2) An organopolysiloxane having two or more alkenyl groups bonded to silicon atoms per molecule, with a viscosity of 11 to 1,000 Pa s at 25°C.

[0015] The viscosity of (A-1) is preferably in the range of 0.1 to 5 Pa s, and more preferably 0.1 to 1 Pa s. If the viscosity of (A-1) is less than 0.01 Pa s, the cured product will be brittle and prone to cracking, whereas if it is more than 10 Pa s, the cured product will be soft and prone to voids.

[0016] The viscosity of (A-2) is preferably in the range of 15 to 500 Pa s, and more preferably in the range of 20 to 100 Pa s. If the viscosity of (A-2) is less than 11 Pa s, stirring shear is not applied to the material during production, making it difficult for the composition to become grease-like, while if it is more than 1000 Pa s, the viscosity of the composition becomes too high, making it difficult to handle.

[0017] In the present invention, the viscosity is a value measured at 25° C. using a spiral viscometer PC-ITL (manufactured by Malcom Co., Ltd.).

[0018] The proportion of (A-1) in the total of (A-1) and (A-2) is from 10 to 90% by mass, preferably from 20 to 80% by mass, and more preferably from 30 to 70% by mass. If the proportion of (A-1) is less than 10 mass %, the cured product will be soft and voids will be more likely to appear during curing. If it is more than 90 mass %, the materials will not be subjected to stirring shear during production, making it difficult for the composition to become grease-like.

[0019] There are no limitations on the molecular structure of the organopolysiloxanes (A-1) and (A-2), and examples thereof include linear, branched, and partially branched linear structures, with linear structures being particularly preferred.

[0020] The number of alkenyl groups bonded to silicon atoms in each of (A-1) and (A-2) may be 2 or more, preferably 2 to 10, and more preferably 2 to 5, per molecule. Examples of the alkenyl group bonded to a silicon atom include a vinyl group, an allyl group, a 1-butenyl group, and a 1-hexenyl group. Among these, a vinyl group is preferred because of its high versatility. This alkenyl group may be bonded to either a silicon atom at the end of the molecular chain or a silicon atom in the middle of the molecular chain, but it is preferred that the alkenyl group is bonded only to a silicon atom at the end of the molecular chain in order to improve the flexibility of the resulting cured product.

[0021] Examples of groups bonded to silicon atoms other than alkenyl groups include unsubstituted or substituted monovalent hydrocarbon groups, such as alkyl groups such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, and dodecyl groups; cycloalkyl groups such as cyclopentyl and cyclohexyl groups; aryl groups such as phenyl, tolyl, xylyl, and naphthyl groups; aralkyl groups such as benzyl, 2-phenylethyl, and 2-phenylpropyl groups; and halogenated alkyl groups such as chloromethyl, 3,3,3-trifluoropropyl, and 3-chloropropyl groups. From the viewpoints of synthesis and economy, it is preferable that 90% or more of these groups are methyl groups.

[0022] Specific examples of suitable organopolysiloxanes include polydimethylsiloxanes terminally blocked with dimethylvinylsiloxy groups, polydimethylsiloxanes terminally blocked with methyldivinylsiloxy groups, and dimethylsiloxane-methylphenylsiloxane copolymers terminally blocked with dimethylvinylsiloxy groups.

[0023] <(B) Organohydrogenpolysiloxane> The component (B) of the composition of the present invention is an organohydrogenpolysiloxane having two or more hydrogen atoms bonded to silicon atoms (hereinafter referred to as "Si-H groups") in one molecule, and acts as a crosslinking agent for the above-mentioned component (A). That is, the Si-H groups in the component (B) undergo a hydrosilylation reaction with the alkenyl groups in the component (A) under the action of the platinum catalyst in the component (E) described below, to give a crosslinked cured product having a three-dimensional network structure with crosslinked bonds.

[0024] The number of Si-H groups in component (B) is at least 2 in one molecule, preferably at least 5 from the viewpoint of suppressing voids during curing, and more preferably at least 10. Furthermore, component (B) is more preferably an organohydrogenpolysiloxane that has at least 5 hydrogen atoms bonded to silicon atoms at non-terminal locations in one molecule and satisfies the following formula (3): 0.1<α / β (3) (In formula (3), α represents the number of hydrogen atoms bonded to silicon atoms not at the molecular chain terminals, and β represents the total number of silicon atoms in component (B).) If the above α / β range is as small as 0.1 or less, voids are likely to occur during curing, so it is also necessary that 0.1<α / β is satisfied. In this case, α / β is preferably 0.11 or more, particularly 0.12 or more, and although there is no upper limit, it is preferably 0.95 or less, particularly 0.90 or less.

[0025] The molecular structure of component (B) is not particularly limited as long as it satisfies the above requirements, and may be any of the conventionally known structures, such as linear, cyclic, branched, three-dimensional network (resinous), etc. The number of silicon atoms (or degree of polymerization) in one molecule is usually 3 to 1,000, preferably 5 to 400, more preferably 10 to 300, even more preferably 10 to 100, and particularly preferably 10 to 60.

[0026] The kinetic viscosity of the organohydrogenpolysiloxane of component (B) is usually 1 to 10,000 mm 2 / s, preferably 3 to 5,000 mm 2 / s, more preferably 5 to 3,000 mm 2 The kinematic viscosity is preferably 1 / s and is liquid at room temperature (25° C.). Note that this kinematic viscosity is a value measured at 25° C. using an Ostwald viscometer.

[0027] As an organohydrogenpolysiloxane satisfying the above requirements, for example, one represented by the following average composition formula (4) is preferred. R 6e H f SiO (4-e-f) / 2 (4) (In formula (4), R 6 represents an unsubstituted or substituted monovalent hydrocarbon group having no aliphatic unsaturated bonds, e is a number from 0.7 to 2.2, f is a number from 0.001 to 0.5, and e+f is a number that satisfies the range of 0.8 to 2.5.

[0028] In the above formula (4), R 6 is usually an unsubstituted or substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, preferably 1 to 6 carbon atoms, and having no aliphatic unsaturated bonds. Specific examples thereof include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, cyclohexyl, octyl, nonyl, and decyl groups; aryl groups such as phenyl, tolyl, xylyl, and naphthyl groups; aralkyl groups such as benzyl, phenylethyl, and phenylpropyl groups; and 3,3,3-trifluoropropyl groups in which some or all of the hydrogen atoms of these groups are substituted with halogen atoms such as fluorine and chlorine, among which preferred are alkyl groups, aryl groups, and 3,3,3-trifluoropropyl groups, and more preferred are methyl, phenyl, and 3,3,3-trifluoropropyl groups.

[0029] In the above formula (4), e, f, and e+f are as defined above, but e is preferably a number from 0.9 to 2.1, f is preferably a number from 0.002 to 0.2, particularly preferably a number from 0.005 to 0.1, and e+f is preferably a number satisfying the range of 1.0 to 2.3, particularly preferably 1.5 to 2.2.

[0030] The molecular structure of the organohydrogenpolysiloxane represented by the above formula (4) is not particularly limited and may be any of linear, cyclic, branched, three-dimensional network (resinous), etc. Among them, those in which the number of silicon atoms in one molecule and the kinetic viscosity satisfy the above-mentioned ranges are particularly preferred, and linear ones are particularly preferred.

[0031] Specific examples of organohydrogenpolysiloxanes represented by the above formula (4) include dimethylsiloxane-methylhydrogensiloxane copolymers capped at both molecular chain ends with dimethylhydrogensiloxy groups, methylhydrogensiloxane-dimethylsiloxane-diphenylsiloxane copolymers capped at both molecular chain ends with dimethylhydrogensiloxy groups, dimethylsiloxane-methylhydrogensiloxane copolymers capped at one molecular chain end with a dimethylhydrogensiloxy group and one trimethylsiloxy group, methylhydrogensiloxane-dimethylsiloxane-diphenylsiloxane copolymers capped at one molecular chain end with a dimethylhydrogensiloxy group and one trimethylsiloxy group, and (CH3)2HSiO 1 / 2 Units and (CH3)3SiO 1 / 2 Units and (CH3)HSiO 2 / 2 Units and SiO 4 / 2 A copolymer consisting of (CH3)2HSiO units. 1 / 2 Units and (CH3)3SiO 1 / 2 Units and (CH3)HSiO 2 / 2 Units and (CH3)2SiO 2 / 2 Units and SiO 4 / 2 A copolymer consisting of (CH3)2HSiO units. 1 / 2 Units and (CH3)HSiO 2 / 2 Units and (CH3)2SiO 2 / 2 Units and SiO 4 / 2 A copolymer consisting of (CH3)2HSiO units. 1 / 2 Units and SiO 4 / 2 Units and (CH3)HSiO 2 / 2 Units and (CH3)2SiO 2 / 2 Units and (C6H5)3SiO 1 / 2 A copolymer consisting of (CH3)2HSiO units. 1 / 2 Units and (CH3)3SiO 1 / 2 Units and (C6H5)2SiO 2 / 2 Units and (CH3)HSiO 2 / 2 Units and (CH3)2SiO 2 / 2 Units and SiO 4 / 2 and copolymers consisting of a unit.

[0032] The amount of component (B) blended is such that there are 0.1 to 5.0 silicon-bonded hydrogen atoms in component (B) per silicon-bonded alkenyl group in component (A), preferably 0.3 to 3.0, and more preferably 0.5 to 2.0. If there are fewer than 0.1 silicon-bonded hydrogen atoms, the crosslink density will be too low and voids will be more likely to occur during curing, while if there are more than 5.0, the resulting thermally conductive silicone composition will be too hard and will have poor reliability. The organohydrogenpolysiloxane of the component (B) may use either a single compound, or a combination of two or more different compounds.

[0033] <(C) Gallium and / or its alloy> The component (C) of the composition of the present invention is gallium and / or an alloy thereof having a melting point of −20 to 70° C. The component (C) is blended in order to impart good thermal conductivity to a cured product obtained from the composition of the present invention, and the inclusion of this component is a characteristic of the present invention.

[0034] As described above, the melting point of this component (C) must be in the range of -20 to 70°C. Although a material below -20°C can be physically used in the present invention, it is difficult to obtain a material with a melting point of less than -20°C, which is economically undesirable. Conversely, if the melting point exceeds 70°C, the material does not melt quickly in the composition preparation process, resulting in poor workability. Therefore, as described above, the melting point of the component (C) is appropriately in the range of -20 to 70°C. In particular, a material within the range of -19 to 50°C is preferred because it is easy to prepare the composition of the present invention.

[0035] The melting point of metallic gallium is 29.8°C. Representative examples of gallium alloys include gallium-indium alloys such as Ga-In (mass ratio = 75.4:24.6, melting point = 15.7°C), gallium-tin alloys, gallium-tin-zinc alloys such as Ga-Sn-Zn (mass ratio = 82:12:6, melting point = 17°C), gallium-indium-tin alloys such as Ga-In-Sn (mass ratio = 68.5:21.5:10, melting point = -19°C, mass ratio = 62:25:13, melting point = 5.0°C, mass ratio = 21.5:16.0:62.5, melting point = 10.7°C), and gallium-indium-bismuth-tin alloys such as Ga-In-Bi-Sn (mass ratio = 9.4:47.3:24.7:18.6, melting point = 48.0°C).

[0036] The component (C) may use either a single compound, or a combination of two or more different compounds. The shape of the liquid or solid fine particles of gallium and / or its alloy present in the composition of the present invention in an uncured state is approximately spherical, and may include particles of an indefinite shape. The average particle size is usually 1 to 200 μm, particularly 5 to 150 μm, and more preferably 10 to 100 μm. If the average particle size is too small, the viscosity of the composition becomes too high, resulting in poor extensibility and problems with coating workability. Conversely, if the average particle size is too large, the composition becomes non-uniform, making it difficult to apply a thin film to heat-generating electronic components, etc. As described above, the shape, average particle size, and dispersion state in the composition can be maintained until the coating process on heat-generating electronic components, etc., because the composition is quickly stored at low temperatures after preparation. The average particle size was calculated by sandwiching the composition before curing between two slide glasses and observing it with a VR-3000 manufactured by Keyence Corporation. That is, 30 particles were randomly selected from the image captured by this measuring device, the particle size of each was measured, and the average value was calculated.

[0037] The amount of the (C) component is 300 to 20,000 parts by mass, particularly preferably 2,000 to 15,000 parts by mass, and even more preferably 3,000 to 12,000 parts by mass, per 100 parts by mass of the (A) component. If the amount is less than 300 parts by mass, the thermal conductivity is low, and if the composition is thick, sufficient heat dissipation performance cannot be obtained. If the amount is more than 20,000 parts by mass, it is difficult to obtain a uniform composition, and the viscosity of the composition is too high, so that it may not be possible to obtain a composition in the form of a grease with extensibility.

[0038] <(D) Thermally conductive filler> The composition of the present invention needs to contain, together with the component (C), a thermally conductive filler (D) (excluding component (C)) that is conventionally blended in a thermally conductive sheet or thermally conductive grease.

[0039] The component (D) is not particularly limited as long as it has good thermal conductivity, and any conventionally known component can be used, such as aluminum powder, zinc oxide powder, alumina powder, boron nitride powder, aluminum nitride powder, silicon nitride powder, copper powder, diamond powder, nickel powder, zinc powder, stainless steel powder, carbon powder, etc. The component (D) can be used alone or in combination of two or more. In particular, from the viewpoints of availability and economy, zinc oxide powder and alumina powder are particularly preferred.

[0040] The average particle size of component (D) is 0.1 to 100 μm, preferably within the range of 1 to 20 μm. If the average particle size is too small, the viscosity of the resulting composition will be too high, resulting in poor extensibility. Conversely, if the average particle size is too large, it will be difficult to obtain a uniform composition. The average particle size is the volume average diameter [MV] measured by volume using a Microtrac MT3300EX (manufactured by Nikkiso Co., Ltd.).

[0041] If the amount of component (D) is less than 10 parts by mass per 100 parts by mass of component (A), the gallium and / or its alloy will not disperse uniformly in (A) or in a mixture of component (A) and component (G) described below. If the amount of component (D) is more than 1,000 parts by mass, the viscosity of the composition will increase and it will be difficult to obtain a grease-like composition having extensibility. Therefore, the amount should be in the range of 10 to 1,000 parts by mass, and preferably 50 to 500 parts by mass.

[0042] <(E) Platinum group metal catalyst> The platinum group metal catalyst of component (E) of the composition of the present invention is a component that is blended in order to promote the addition reaction between the alkenyl groups in component (A) and the SiH in component (B) above, thereby providing a crosslinked cured product in a three-dimensional network state from the composition of the present invention.

[0043] Any of the known compounds used in normal hydrosilylation reactions can be used as this component (E), including, for example, platinum metal (platinum black), chloroplatinic acid, platinum-olefin complexes, platinum-alcohol complexes, platinum coordination compounds, etc. The amount of component (E) to be added is not particularly limited as long as it is an effective amount required for curing the composition of the present invention, but it is usually preferable that the amount is, for example, about 0.1 to 500 ppm in terms of platinum atoms relative to the mass of component (A).

[0044] <(G-1) Surface treatment agent> The composition of the present invention contains a polysiloxane represented by the following general formula (1) as a surface treatment agent (G-1) for the purposes of hydrophobizing the gallium and / or alloy thereof, component (C), during preparation of the composition, improving the wettability of component (C) with the organopolysiloxane, component (A), and dispersing component (C) as fine particles uniformly in the matrix made of component (A).

[0045] Furthermore, this component (G-1) also has the effect of improving the wettability of the surface of the thermally conductive filler (D) mentioned above, thereby improving its uniform dispersibility.

[0046] The component (G-1) is represented by the following general formula (1): [ka] (In formula (1), R 1 are the same or different alkyl groups, R 2 is an alkyl group, a is an integer of 5 to 100, and b is an integer of 1 to 3. It is a polysiloxane in which one end of the molecular chain is blocked with a hydrolyzable group, and has a kinetic viscosity of 10 to 10,000 mm at 25°C. 2 The kinematic viscosity is measured at 25°C using an Ostwald viscometer.

[0047] R in the above general formula (1) 1 Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a tert-butyl group, a pentyl group, a neopentyl group, a hexyl group, a cyclohexyl group, an octyl group, a nonyl group, a decyl group, etc. Among these, a methyl group and an ethyl group are particularly preferred.

[0048] R in the above general formula (1) 2 Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a tert-butyl group, a pentyl group, a neopentyl group, a hexyl group, a cyclohexyl group, an octyl group, a nonyl group, a decyl group, etc. Among these, a methyl group and an ethyl group are particularly preferred.

[0049] If the amount of the (G-1) component is 10 parts by mass or more per 100 parts by mass of the (A) component, the (C) and (D) components are sufficiently dispersed to form a uniform grease composition, which is preferable, but if it is more than 500 parts by mass, the amount of the (A) component is relatively small, which causes a problem that the obtained composition is difficult to harden. If the grease does not harden, it may shift after being applied to a device such as a CPU, resulting in a significant decrease in performance. Therefore, the amount of the (G-1) component is in the range of 10 to 500 parts by mass, and preferably 50 to 300 parts by mass.

[0050] <Other ingredients> In addition to the essential components described above, the curable organopolysiloxane composition of the present invention may contain the following components, if necessary. <(F) Addition reaction regulator> The addition reaction inhibitor, component (F) of the composition of the present invention, is an optional component that inhibits the hydrosilylation reaction caused by the action of the platinum-based catalyst at room temperature, thereby ensuring the pot life (shelf life, pot life) of the composition of the present invention and preventing interference with the coating operation of heat-generating electronic components, etc.

[0051] As this component (F), any of the known addition reaction inhibitors used in ordinary addition reaction curing silicone compositions can be used, including, for example, acetylene compounds such as 1-ethynyl-1-cyclohexanol and 3-butyn-1-ol, various nitrogen compounds, organic phosphorus compounds, oxime compounds, organic chloro compounds, and the like.

[0052] The amount of the (F) component to be blended varies depending on the amount of the (E) component used, and cannot be generally stated, but is not particularly limited as long as it is an effective amount that can suppress the progress of the hydrosilylation reaction. For example, it is usually about 0.001 to 5 parts by mass per 100 parts by mass of the (A) component. If the amount of the (F) component to be blended is too small, it is not possible to ensure sufficient pot life, and if it is too large, the curability of the composition of the present invention decreases. Note that the (F) component can be used after diluting it with an organic solvent such as toluene, xylene, or isopropyl alcohol, as necessary, in order to improve its dispersibility in the composition.

[0053] The composition of the present invention may further contain the following alkoxysilane as component (G-2). (G-2) The following general formula (2): R 3 c R 4 d Si(OR 5 ) 4-c-d (2) (In formula (2), R 3are independently alkyl groups having 6 to 16 carbon atoms, R 4 are independently unsubstituted or substituted monovalent hydrocarbon groups having 1 to 8 carbon atoms, R 5 are independently an alkyl group having 1 to 6 carbon atoms, c is an integer of 1 to 3, d is an integer of 0 to 2, and the sum of c and d is an integer of 1 to 3.

[0054] R in the above general formula (2) 3 Examples of the alkyl group include hexyl, octyl, nonyl, decyl, dodecyl, tetradecyl, etc. If the number of carbon atoms is less than 6, the improvement in the wettability of the components (C) and (D) is insufficient, and if it exceeds 16, the organosilane of the component (G-2) solidifies at room temperature, making it inconvenient to handle and reducing the low-temperature properties of the resulting composition.

[0055] In addition, R in the above general formula (2) 4 Examples of the alkyl group include alkyl groups such as methyl, ethyl, propyl, hexyl, and octyl; cycloalkyl groups such as cyclopentyl and cyclohexyl; alkenyl groups such as vinyl and allyl; aryl groups such as phenyl and tolyl; aralkyl groups such as 2-phenylethyl and 2-methyl-2-phenylethyl; and halogenated hydrocarbon groups such as 3,3,3-trifluoropropyl, 2-(nanofluorobutyl)ethyl, 2-(heptadecafluorooctyl)ethyl, and p-chlorophenyl. Of these, methyl and ethyl groups are particularly preferred.

[0056] In addition, R in the above general formula (2) 5 Examples of the alkyl group include methyl, ethyl, propyl, butyl, pentyl, hexyl, etc. Of these, methyl and ethyl are particularly preferred.

[0057] Specific examples of suitable components (G-2) include the following: C6H 13 Si(OCH3)3 C 10 H 21 Si(OCH3)3 C 12 H 25 Si(OCH3)3 C 12 H 25 Si(OC2H5)3 C 10 H 21 (CH3)Si(OCH3)2 C 10 H 21 (C6H5)Si(OCH3)2 C 10 H 21 (CH3)Si(OC2H5)2 C 10 H 21 (CH=CH2)Si(OCH3)2

[0058] The (G-2) component can be used alone or in combination of two or more. The amount of the (G-2) component to be blended is preferably in the range of 0.1 to 100 parts by mass, since the viscosity of the composition is likely to be in the desired range if it is 0.1 part by mass or more relative to 100 parts by mass of the (A) component, and more than 100 parts by mass is uneconomical without increasing the wetter effect. More preferably, it is in the range of 1 to 50 parts by mass.

[0059] In addition, the composition of the present invention may further contain trifluoropropyltrimethoxysilane as component (G-3) in some cases. The amount of trifluoropropyltrimethoxysilane to be added is preferably in the range of 0.1 to 100 parts by mass, since the viscosity of the composition is likely to be in the desired range if it is 0.1 parts by mass or more relative to 100 parts by mass of component (A), and if it is more than 100 parts by mass, it is uneconomical because the wetter effect is not increased. More preferably, it is 1 to 50 parts by mass. The components (G-1), (G-2) and (G-3) may be used alone or in combination.

[0060] <Optional ingredients other than those listed above> The composition of the present invention may also contain an organopolysiloxane represented by the following average compositional formula (5) within the scope of the invention.

[0061] Average composition formula (5): R 7 g SiO (4-g) / 2 (5) (In formula (5), R 7 are independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 18 carbon atoms and no aliphatic unsaturated bonds, and g is a number from 1.8 to 2.2. The kinetic viscosity at 25°C is 10 to 100,000 mm 2 and / s, and one type may be used alone, or two or more types may be used in combination.

[0062] Above R 7 R is independently an unsubstituted or substituted monovalent hydrocarbon group having 1 to 18 carbon atoms. 7 Examples of the alkyl group include alkyl groups such as methyl, ethyl, propyl, hexyl, octyl, decyl, dodecyl, tetradecyl, hexadecyl, and octadecyl; cyclohexyl groups such as cyclopentyl and cyclohexyl; alkenyl groups such as vinyl and allyl; aryl groups such as phenyl and tolyl; aralkyl groups such as 2-phenylethyl and 2-methyl-2-phenylethyl; and halogenated hydrocarbon groups such as 3,3,3-trifluoropropyl, 2-(perfluorobutyl)ethyl, 2-(perfluorooctyl)ethyl, and p-chlorophenyl.

[0063] The composition of the present invention may further contain, for example, heat resistance improvers such as iron oxide and cerium oxide; viscosity adjusters such as silica; colorants, and the like.

[0064] <Viscosity of Composition> As described below, the composition of the present invention is applied to the surface of a heat-generating electronic component, and after a heat dissipation member is pressed onto it, it is cured by heat treatment to form a thermally conductive layer. In this case, in order to improve workability, the composition of the present invention needs to be in a grease-like form.

[0065] For example, the composition of the present invention is stored in a syringe, and is applied from the syringe to the surface of a heat-generating electronic component such as a CPU to form a coating layer, to which a heat dissipation member is pressed. Therefore, the viscosity of the composition of the present invention is usually preferably 10 to 1,000 Pa·s, particularly 30 to 400 Pa·s. If the viscosity is too low, dripping may occur during application, which may cause problems in operation. Conversely, if the viscosity is too high, it may be difficult to extrude the composition from the syringe, which may result in poor efficiency in application. The viscosity is a value measured at 25°C using a spiral viscometer PC-ITL (manufactured by Malcom Co., Ltd.).

[0066] [Preparation of the composition of the present invention] The curable organopolysiloxane composition of the present invention comprises: (i) a step of kneading the (A), (C), (D) and (G-1), and, when contained, the (G-2) and (G-3) components at a temperature within a range of 20 to 120°C and at a temperature equal to or higher than the melting point of the (C) component to obtain a uniform mixture (i); (ii) stopping the kneading of the mixture (i) and cooling the temperature of the mixture (i) to a temperature lower than the melting point of the (C) component to obtain a mixture (ii); and (iii) adding the (B) component, the (E) component, the (F) component if contained, and optionally other components to the mixture (ii), and kneading them at a temperature below the melting point of the (C) component to obtain a homogeneous mixture (iii); However, the present invention is not limited to the above-described manufacturing method.

[0067] In the above-mentioned production method, a stirring / kneading machine such as a conditioning mixer or a planetary mixer equipped with a heating means and, if necessary, a cooling means is used.

[0068] In the step (i), the liquid of gallium and / or its alloy, component (C), and the thermally conductive filler, component (D), are uniformly dispersed in a mixed liquid of component (A), (G-1), and any one or more of components (G-2) and (G-3).

[0069] The temperature-lowering or cooling operation in the step (ii) is preferably carried out quickly. In the step (ii), the component (C) in the form of liquid fine particles or solid fine particles uniformly dispersed in the matrix of the mixed liquid of the component (A), the component (G-1), and any one or a combination of two or more of the components (G-2) and (G-3) maintains its average particle size and the above-mentioned dispersion state.

[0070] It is also preferable to complete the step (iii) in as short a time as possible. At the end of the step (iii), there is substantially no change in the dispersion state of the fine particles of the component (C). After the end of the step (iii), the produced composition is preferably placed in a container and promptly stored in a freezer or freezer room at a temperature of about -30 to -10°C, preferably -25 to -15°C. In addition, it is also preferable to use a vehicle equipped with a freezer for transportation. By storing and transporting the composition at such low temperatures, the composition and dispersion state of the composition of the present invention can be stably maintained, for example, even during long-term storage.

[0071] [Application to semiconductor devices] The composition of the present invention can be cured by maintaining it at a temperature of 80 to 180° C. for about 30 to 240 minutes. The cured product of the composition of the present invention can be used as a thermally conductive cured product for forming a thermally conductive layer by being interposed between a heat-generating electronic component and a heat-dissipating member. In this case, the composition of the present invention can be used to obtain a semiconductor device having excellent heat dissipation characteristics, i.e., a semiconductor device having a heat-generating electronic component, a heat dissipation member, and a thermally conductive layer made of a cured product of the composition of the present invention, in which the heat-generating electronic component and the heat dissipation member are bonded via the thermally conductive layer.

[0072] The semiconductor device includes: (a) applying the composition of the present invention to a surface of a heat-generating electronic component to form a coating layer made of the composition on the surface; (b) pressing and fixing a heat dissipation member to the coating layer; and (c) A step of heating the structure obtained after step (b) at 80 to 180° C. to harden the coating layer to form a thermally conductive layer. The composition can be obtained by a manufacturing method having the following steps. The semiconductor device and the method for producing the same will be described with reference to Fig. 1. Note that the device shown in Fig. 1 merely shows one example of the application of the composition of the present invention to a semiconductor device, and is not intended to limit the semiconductor device of the present invention to that shown in Fig. 1.

[0073] First, the composition of the present invention in a frozen state is left at room temperature to thaw naturally into a grease-like state, and then the liquid composition of the present invention is placed in an application tool such as a syringe.

[0074] The composition of the present invention is applied (dispensed) from a syringe or the like onto the surface of a heat-generating electronic component, such as a CPU 2 which is a heat-generating electronic component mounted on a substrate 3 as shown in Fig. 1, to form a curable composition layer (coating layer) 1. At the same time, an adhesive 5 is also applied to fix a heat dissipation member 4, and the heat dissipation member 4 is pressed against the CPU 2 via the coating layer 1 to be fixed thereto.

[0075] In this case, the thickness of the coating layer 1 sandwiched between the CPU 2 and the heat dissipation member 4 is preferably adjusted to be usually 5 to 100 μm, and particularly preferably 10 to 70 μm. If the thickness is too thin, peeling is likely to occur, resulting in poor reliability, whereas if it is too thick, the thermal resistance increases, making it difficult to obtain a sufficient heat dissipation effect.

[0076] Next, the coating layer 1 made of the composition of the present invention is cured in a heating device of the apparatus configured as described above to form a thermally conductive layer 1. The temperature required for this curing is 80 to 180° C., and particularly preferably 100 to 150° C. If the temperature is less than 80° C., curing will be insufficient, and conversely, if the temperature is higher than 180° C., electronic components and substrates may deteriorate.

[0077] In the process of raising the temperature to the curing temperature conditions, the liquid or solid fine particles of gallium and / or its alloy, component (C), in the composition of the present invention aggregate with each other to form liquid particles with a large particle size, and at the same time, they also connect with the above-mentioned component (D) to form a kind of continuous pathway.

[0078] Furthermore, the liquid particles of component (C) are fused to the surfaces of the CPU 2 and heat dissipation member 4 in contact with them. Therefore, the CPU 2 and heat dissipation member 4 are substantially integrally continuous and highly thermally conductive via a kind of pathway in which the liquid particles of component (C) and the thermally conductive filler of component (D) are linked together. Furthermore, the pathway structure is fixed and maintained in the three-dimensional crosslinked network of the cured product formed by the addition reaction of components (A) and (B).

[0079] In addition, when the semiconductor device obtained as described above is operated and used, the surface temperature of heat-generating electronic components such as a CPU usually reaches a high temperature of about 60 to 120°C. In response to this heat generation, the thermally conductive layer made of the cured product of the composition of the present invention exhibits high thermal conductivity as described above, and exhibits a significantly excellent action and effect of being superior in heat dissipation characteristics compared to conventional thermally conductive sheets and thermally conductive greases. Furthermore, even when the semiconductor device is continuously operated and used for a long period of time, the gallium and / or its alloy of component (C) contained in the thermally conductive layer and forming the pathways is fixed and held in the three-dimensional crosslinked network of the cured product, and therefore does not leak out of the thermally conductive layer.

[0080] Furthermore, this thermally conductive layer has tackiness, and therefore maintains stable flexibility even if the heat dissipation component is misaligned or even after long-term use, and will not peel off from the heat-generating electronic component or heat dissipation component.

[0081] The same effect can be obtained by preparing a sheet-like cured product of the composition of the present invention in advance to a desired thickness and then interposing this between a heat-generating electronic component and a heat-dissipating member in the same manner as a conventional thermally conductive sheet. In addition, a sheet of the cured product of the composition of the present invention can also be used as appropriate as a part of other devices, etc., which require thermal conductivity and heat resistance. EXAMPLES

[0082] The present invention will be described in more detail below with reference to examples, but the present invention is not limited thereto. Components (A) to (G) used in the following examples and comparative examples are shown below. The viscosity was measured using a spiral viscometer PC-ITL (manufactured by Malcom Co., Ltd.), and the kinetic viscosity was measured using an Ostwald viscometer.

[0083] (A) Component: A dimethylpolysiloxane capped at both ends with dimethylvinylsilyl groups, having a viscosity at 25°C as follows: (A-1-1) Viscosity: 0.1Pa·s (A-1-2) Viscosity: 1.0Pa (A-2-1) Viscosity: 30Pa s (A-2-2) Viscosity: 100Pa·s

[0084] (B) Ingredients: (B-1) Organohydrogenpolysiloxane represented by the following structural formula (α / β=0.35, kinematic viscosity at 25°C: 113 mm 2 / s) [ka] (In the formula, the order of the siloxane units in parentheses is not specified.) (B-2) Organohydrogenpolysiloxane represented by the following structural formula (α / β=0.29, kinematic viscosity at 25°C: 27 mm 2 / s) [ka] (In the formula, the order of the siloxane units in parentheses is not specified.)

[0085] (C) Ingredients: (C-1) Metallic gallium [melting point = 29.8°C] (C-2) Ga-In alloy [mass ratio = 75.4:24.6, melting point = 15.7°C] (C-3) Ga-In-Sn alloy [mass ratio = 68.5:21.5:10, melting point = -19°C] (C-4) Ga-In-Sn alloy [mass ratio = 62:25:13, melting point = 5.0°C] (C-5) Metallic indium [melting point = 156.2℃] <for comparison>

[0086] (D) Ingredients: (D-1): Alumina powder [average particle size: 8.2 μm] (D-2): Zinc oxide powder [average particle size: 1.0 μm]

[0087] (E) Ingredients: (E-1): A solution of platinum-divinyltetramethyldisiloxane complex in dimethylpolysiloxane (both ends blocked with dimethylvinylsilyl groups, viscosity: 0.6 Pa s) [platinum atom content: 1% by mass]

[0088] (F) Ingredients: (F-1) 1-Ethynyl-1-cyclohexanol

[0089] (G) Ingredients: (G-1) Kinematic viscosity 32mm represented by the following structural formula 2 / s Dimethylpolysiloxane capped at one end with trimethoxysilyl group [ka] (G-2)Structural formula:C 10 H 21 Organosilane represented by Si(OCH3)3 (G-3) Trifluoropropyltrimethoxysilane In the procedure for preparing the composition, "Component (G)" refers collectively to (G-1), (G-2), and (G-3) used in each example described in Table 1 or Table 2.

[0090] [Examples 1 to 6, Comparative Examples 1 to 5] <Preparation of Composition> Each component was collected in the composition ratio shown in Tables 1 and 2, and compositions were prepared as follows. Components (A), (C), (D) and (G) were placed in a 250 mL conditioning mixer (Thinky Corporation, product name: Awatori Rentaro) and heated to 70° C., maintained at that temperature and kneaded for 5 minutes. Then, kneading was stopped and the mixture was cooled to 15° C. Next, components (B), (E), and (F) were added to a mixture of components (A), (C), (D), and (G), and the mixture was kneaded at 25°C until homogeneous to prepare each composition.

[0091] <Viscosity measurement> The absolute viscosity of the composition was measured at 25° C. using a model PC-1TL (10 rpm) manufactured by Malcom Co., Ltd.

[0092] <(C) Measurement of particle size of components> Each composition obtained above was sandwiched between two glass slides, and 30 particles were randomly selected from the images taken with a VR-3000 manufactured by Keyence Corporation, the particle size of each was measured, and the average value was calculated.

[0093] <Preparation of cured product> Each of the compositions obtained above was applied to the entire surface of an aluminum plate having a diameter of 1.26 mm and a thickness of 1 mm (hereinafter referred to as a "standard aluminum plate"), and another standard aluminum plate was placed on top of it, and the plate was subjected to a pressure of about 175.5 kPa (1.80 kgf / cm 2 ) to obtain a three-layer structure. The three-layer structure was then heated to 150°C in an electric furnace and held at that temperature for one hour to harden each composition, and then left to cool to room temperature to prepare a sample for measuring thermal resistance. The thickness of each of the obtained samples was measured, and the thickness of each of the cured compositions was calculated by subtracting the known thickness of the standard aluminum plate. Note that a micrometer (Mitutoyo Corporation, model: M820-25VA) was used to measure the thickness of each of the above samples. The thickness of each of the cured compositions is shown in Tables 1 and 2.

[0094] <Measurement of thermal resistance> Using each of the above samples, the thermal resistance (mm 2 The thermal resistance (K / W) was measured using a thermal resistance measuring device (NETZSCH model: LFA447). The measurement results are shown in Tables 1 and 2.

[0095] <Void test> 0.2 g of each composition was sandwiched between two 5 x 7 cm glass slides, a 1 kg weight was placed on top, and the test pieces were left at room temperature for 15 minutes. The weight was then removed, and the test pieces were left in an oven at 150°C for 1 hour before being removed. The cured products sandwiched between the glass slides were observed visually and with a microscope (Keyence Corporation: Model VR-3200). [evaluation] Cracks were visually observed: × - One or more circular voids (voids) with a diameter of 1.0 mm or more were observed under a microscope: × · No cracks or circular voids (voids) with a diameter of 1.0 mm or more are observed visually or under a microscope: ○

[0096] <Measurement of thermal conductivity> The thermal conductivity of each of the above samples was measured at 25° C. using a TPS-2500S manufactured by Kyoto Electronics Manufacturing Co., Ltd.

[0097] <(D) Measurement of particle size of components> The particle size of the thermally conductive filler is a cumulative average diameter on a volume basis measured by a particle size analyzer, Microtrac MT3300EX, manufactured by Nikkiso Co., Ltd.

[0098] <Application to semiconductor devices> 0.2 g of the composition obtained in each of the above Examples 1 to 6 was applied to the surface of a 2 cm x 2 cm CPU to form a coating layer. A heat dissipation member was placed on the coating layer and cured to obtain a semiconductor device in which the CPU and the heat dissipation member were bonded via a thermally conductive layer having a thickness of 10 to 70 μm. When each of these devices was incorporated into a host computer, personal computer, etc. and operated, the heat generation temperature of the CPU was about 100°C, but in each case, stable heat conduction and heat dissipation were possible for a long time, and performance deterioration and damage of the CPU due to overheat accumulation were prevented. Therefore, it was confirmed that the reliability of semiconductor devices was improved by adopting a cured product of the composition of the present invention.

[0099] [Table 1] *For the sake of convenience, the number of silicon-bonded hydrogen atoms in component (B) per silicon-bonded alkenyl group in component (A) is represented as H / Vi (the same applies below).

[0100] [Table 2] Note: It was not possible to obtain a uniform grease-like composition. [Explanation of symbols]

[0101] 1. Curable composition layer (coating layer) (thermal conductive layer) 2 CPU (Central Processing Unit) 3. Substrate 4 Heat dissipation materials 5. Glue

Claims

1. (A) 100 parts by mass of an organopolysiloxane consisting of the following (A-1) and (A-2), in which the ratio of (A-1) to the total of (A-1) and (A-2) is 10 to 90% by mass: (A-1) An organopolysiloxane having two or more silicon-bonded alkenyl groups per molecule, the viscosity of which at 25°C is 0.01 to 10 Pa·s. (A-2) An organopolysiloxane having two or more silicon-bonded alkenyl groups per molecule, and having a viscosity at 25°C of 11 to 1,000 Pa·s. (B) an organohydrogenpolysiloxane having two or more hydrogen atoms bonded to silicon atoms per molecule: an amount such that the number of hydrogen atoms bonded to silicon atoms in said component is 0.1 to 5.0 per alkenyl group in component (A); (C) one or more selected from the group consisting of gallium and gallium alloys having a melting point of −20 to 70° C.: 300 to 20,000 parts by mass, (D) a thermally conductive filler having an average particle size of 0.1 to 100 μm: 10 to 1,000 parts by mass, (E) Platinum group metal catalyst: 0.1 to 500 ppm by mass of platinum group metal relative to the mass of component (A). and, (G-1) Organopolysiloxane represented by the following general formula (1): 10 to 500 parts by mass 【Chemistry 1】 (In formula (1), R 1 are the same or different alkyl groups, R 2 is an alkyl group, a is an integer from 5 to 100, and b is an integer from 1 to 3.

1. A curable organopolysiloxane composition comprising:

2. Furthermore, (G-2) the following general formula (2): R 3 c R 4 d Si(OR 5 ) 4-c-d (2) (In formula (2), R 3 are independently alkyl groups having 6 to 16 carbon atoms; R 4 are independently unsubstituted or substituted monovalent hydrocarbon groups having 1 to 8 carbon atoms; R 5 are independently an alkyl group having 1 to 6 carbon atoms, c is an integer of 1 to 3, d is an integer of 0 to 2, and the sum of c and d is an integer of 1 to 3. The curable organopolysiloxane composition according to claim 1, comprising an alkoxysilane compound represented by the following formula (1) in an amount of 0.1 to 100 parts by mass per 100 parts by mass of component (A).

3. 3. The curable organopolysiloxane composition according to claim 1, further comprising (G-3) trifluoropropyltrimethoxysilane in an amount of 0.1 to 100 parts by mass per 100 parts by mass of component (A).

4. Component (B) has five or more hydrogen atoms bonded to silicon atoms at non-terminal locations in each molecule and is represented by the following formula (3): 0.1<α/β (3) (In formula (3), α represents the number of hydrogen atoms bonded to silicon atoms not at the molecular chain terminals, and β represents the total number of silicon atoms in component (B).) 4. The curable organopolysiloxane composition according to claim 1, which is an organohydrogenpolysiloxane that satisfies the above requirements.

5. 5. The curable organopolysiloxane composition according to claim 1, wherein component (C) is dispersed in the composition in the form of particles having a size of 1 to 200 μm.

6. 6. A thermally conductive silicone grease composition comprising the curable organopolysiloxane composition according to any one of claims 1 to 5.

7. A cured product of the curable organopolysiloxane composition according to any one of claims 1 to 5.

8. Use of the cured product according to claim 7 as a thermally conductive layer disposed between a heat-generating electronic component and a heat dissipating member.

9. A semiconductor device having a heat-generating electronic component, a heat dissipation member, and a thermally conductive layer made of the cured product described in claim 7, wherein the heat-generating electronic component and the heat dissipation member are bonded via the thermally conductive layer.

10. 10. The method of manufacturing a semiconductor device according to claim 9, (a) applying the curable organopolysiloxane composition according to any one of claims 1 to 5 to a surface of a heat-generating electronic component to form a coating layer made of the composition on the surface; (b) pressing and fixing a heat dissipation member to the coating layer; and (c) heating the structure obtained after step (b) at 80 to 180° C. to harden the coating layer into a thermally conductive layer. A method for manufacturing a semiconductor device having the above structure.

Citation Information

Patent Citations

  • JP1974013874A

  • Decentralized processing system

    JP1981040945A

  • Silicone composition and its production

    JP1995207160A

  • Thermally conductive material and its production, method for cooling electronic part, method for cooling circuit board, and method for mounting electronic part

    JP1996053664A

  • Method for producing heat conductive compound by using liquid metal-crosslinked particle cluster

    JP2002121292A