Squeeze container

A squeeze container with dual oxygen barrier layers containing ethylene-vinyl alcohol copolymer and polyethylene, along with a compatibilizer, addresses odor transfer and squeezeability issues by enhancing adhesion and reducing rigidity, ensuring effective odor suppression and ease of use.

JP7580903B2Active Publication Date: 2024-11-12MEBIUS PACKAGING CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2018204688
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2018-10-31
Publication Date
2024-11-12
Estimated Expiration
2038-10-31

AI Technical Summary

Technical Problem

Squeeze containers made with a multilayer structure face issues with odor transfer from a regrind layer and reduced squeezeability due to the use of multiple oxygen barrier layers made of EVOH alone.

Method used

A squeeze container design with an outer oxygen barrier layer A, a regrind layer, and an inner oxygen barrier layer B, where both barrier layers contain ethylene-vinyl alcohol copolymer, polyethylene, and a compatibilizer, enhancing adhesion and reducing rigidity while blocking odor transfer.

Benefits of technology

The design effectively suppresses odor transfer from the regrind layer to the contents and maintains high squeezing properties by using a dual oxygen barrier layer structure with polyethylene and a compatibilizer, improving both odor barrier and squeezeability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580903000002
    Figure 0007580903000002
  • Figure 0007580903000003
    Figure 0007580903000003
  • Figure 0007580903000001
    Figure 0007580903000001
Patent Text Reader

Abstract

To provide a squeeze container which can suppress shift of odor derived from a regrind layer to a content, and which has a high squeezing property.SOLUTION: A squeeze container includes an oxygen barrier layer A, a regrind layer, and an oxygen barrier layer B in this order from the outside. The oxygen barrier layer A and the oxygen barrier layer B include ethylene-vinyl alcohol copolymer, polyethylene and compatibilizer, respectively.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a squeeze container. [Background technology]

[0002] Generally, metal cans, glass bottles, various plastic containers, and the like are used as packaging containers. Among these, plastic containers are widely used for various purposes because they are easy to mold and can be manufactured inexpensively. For example, plastic containers are used as squeeze containers that hold contents such as ketchup and mayonnaise and squeeze the body to expel the contents. These packaging containers are required to suppress deterioration of the contents and deterioration of flavor due to oxygen remaining in the container or oxygen that permeates the container wall. In particular, oxygen does not permeate through the container wall in metal cans and glass bottles, but oxygen may permeate through the container wall in plastic containers.

[0003] In order to suppress the oxygen permeation, plastic containers have been made to have a multilayer structure. For example, as layers constituting a plastic container, in addition to outer and inner layers containing an olefin-based resin, an oxygen barrier layer containing an oxygen barrier resin such as an ethylene-vinyl alcohol copolymer (hereinafter also referred to as EVOH) has been provided (e.g., Patent Document 1). These layers are generally bonded to each other via an adhesive layer containing an adhesive resin. Meanwhile, Patent Document 2 discloses a multilayer packaging material that enhances the adhesive strength when inner and outer layers mainly made of polyolefin and an intermediate layer mainly made of EVOH are laminated together to form the multilayer structure, without providing any adhesive layer between the layers.

[0004] When oxygen permeation is suppressed by an oxygen barrier layer containing EVOH as a primary component, the oxygen barrier properties of the oxygen barrier layer are reduced by the humidity when a container contains a high-moisture content. To prevent this, the oxygen barrier layer is typically placed on the side with lower humidity, i.e., as far outside the container as possible. To simplify the layer structure of the container, the oxygen barrier layer is typically provided as a single layer. However, since a large amount of scrap, such as flash, is generated during the production of containers by direct blow molding, it is typically crushed, mixed with virgin material, and recycled as part of the container (regrind layer) from the perspectives of cost reduction and environmental conservation. As mentioned above, the oxygen barrier layer is positioned as far outside the container as possible, and the regrind layer is typically positioned inside the oxygen barrier layer.

[0005] In recent years, with the diversification of contents packed in plastic containers, there has been an ever-increasing demand for suppressing odors originating from the containers. The regrind layer is thought to be a cause of odor because it contains materials that have been subjected to heat history. Patent Document 3 describes the provision of an odor barrier layer to prevent migration of odorous components originating from an oxygen-absorbing layer that may be contained in a plastic container to the inside and outside. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Laid-Open No. 2001-253426 [Patent Document 2] Japanese Unexamined Patent Publication No. 49-35482 [Patent Document 3] Japanese Patent Application Laid-Open No. 2005-1371 Summary of the Invention [Problem to be solved by the invention]

[0007] In order to adequately block odorous components originating from the regrind layer, the inventors attempted to place oxygen barrier layers made of EVOH alone on both sides of the regrind layer. However, when multiple oxygen barrier layers made of EVOH alone were placed, the rigidity increased when used as a squeeze container, and the squeezability decreased.

[0008] An object of the present invention is to provide a squeeze container that can suppress the transfer of odors from the regrind layer to the contents and has high squeezability. [Means for solving the problem]

[0009] The squeeze container according to the present invention is a squeeze container including, from the outside, an oxygen barrier layer A, a regrind layer, and an oxygen barrier layer B in this order, The oxygen barrier layer A and the oxygen barrier layer B each contain an ethylene-vinyl alcohol copolymer, polyethylene, and a compatibilizer. [Effects of the Invention]

[0010] According to the present invention, it is possible to provide a squeeze container that can suppress the transfer of odors from the regrind layer to the contents and has high squeezability. [Brief explanation of the drawings]

[0011] [Figure 1] 1 is a front view showing an example of a squeeze container according to the present invention. FIG. [Figure 2] 1 is a cross-sectional view showing an example of a layer structure of a squeeze container according to the present invention. DETAILED DESCRIPTION OF THE INVENTION

[0012] The squeeze container according to the present invention comprises, in this order from the outside, an oxygen barrier layer A, a regrind layer, and an oxygen barrier layer B. The oxygen barrier layer A and the oxygen barrier layer B each comprise an ethylene-vinyl alcohol copolymer, polyethylene, and a compatibilizer. That is, the oxygen barrier layer A comprises an ethylene-vinyl alcohol copolymer, polyethylene, and a compatibilizer, and the oxygen barrier layer B comprises an ethylene-vinyl alcohol copolymer, polyethylene, and a compatibilizer.

[0013] In the squeeze container of the present invention, not only is an oxygen barrier layer A provided outside the regrind layer to suppress oxygen permeation, but an oxygen barrier layer B is also provided separately inside the regrind layer, thereby suppressing the migration of odorous components contained in the regrind layer to the contents. Furthermore, while an oxygen barrier layer made of EVOH alone has high rigidity, the squeeze container of the present invention uses oxygen barrier layers A and B containing polyethylene and a compatibilizer in addition to EVOH, resulting in low rigidity and high squeezability (extrusion ability). Furthermore, because the oxygen barrier layers A and B have adhesive properties, there is no need to provide a separate adhesive layer, simplifying the manufacturing process. The present invention will be described in detail below.

[0014] An example of a squeeze container according to the present invention is shown in Figure 1. The squeeze container shown in Figure 1 comprises a mouth 1 that can be opened and closed with a cap, a body 2 that is the center of the squeeze container, and a bottom 3. By pressing the body 2, the contents are forced out from the mouth 1. Note that the shape of the body 2 of the squeeze container according to the present invention may be any shape in cross section, and it may not have a bottom 3. For example, the squeeze container may be in the form of a tube in which the end portion of the body 2 is sealed by welding or folding.

[0015] The layer structure of the squeeze container according to the present invention is not particularly limited, as long as it includes, from the outside in order, an oxygen barrier layer A, a regrind layer, and an oxygen barrier layer B. For example, the squeeze container may include an outer layer and an inner layer in addition to the oxygen barrier layer A, the regrind layer, and the oxygen barrier layer B, and may further include other layers. Examples of such other layers include a virgin layer made of a virgin material, as described below. It is preferable that the squeeze container does not include an oxygen-absorbing layer having oxygen-absorbing properties. Furthermore, because the oxygen barrier layer A and the oxygen barrier layer B have adhesive properties, it is preferable that the squeeze container does not include a general adhesive layer other than the oxygen barrier layer A and the oxygen barrier layer B. Here, a general adhesive layer refers to a layer made of an adhesive resin that does not contain a material having oxygen barrier properties, such as a layer made of a modified polyolefin resin. The squeeze container has at least two oxygen barrier layers, but may have three or more layers.

[0016] The squeeze container may have, for example, a five-layer structure of outer layer / oxygen barrier layer A / regrind layer / oxygen barrier layer B / inner layer, a six-layer structure of outer layer / oxygen barrier layer A / virgin layer / regrind layer / oxygen barrier layer B / inner layer, or a seven-layer structure of outer layer / oxygen barrier layer A / virgin layer / regrind layer / virgin layer / oxygen barrier layer B / inner layer. As an example, Fig. 2 shows a cross-sectional view of a squeeze container having a seven-layer structure of outer layer 4 / oxygen barrier layer A5 / virgin layer 6 / regrind layer 7 / virgin layer 6 / oxygen barrier layer B8 / inner layer 9.

[0017] The thickness of the thinnest part of the squeeze container's body is preferably 180 to 1500 μm, more preferably 200 to 1200 μm, and even more preferably 300 to 1100 μm. A thickness of 180 μm or more prevents the container from deforming or breaking when squeezed, allowing the contents to be stably stored. Furthermore, if the thickness exceeds 1500 μm, squeezing becomes difficult. Here, the body of the squeeze container refers to the content-accommodating portion excluding the mouth, and refers to the portion 5 mm above the bottom surface.

[0018] A squeeze container is filled with ultrapure water at 85°C, sealed, sterilized by inversion for 10 minutes, cooled to room temperature, and stored for one week. The TOC (Total Organic Carbon) content of the ultrapure water is preferably less than 0.7 ppm by mass, more preferably 0.5 ppm by mass or less, and even more preferably 0.4 ppm by mass or less. The TOC content is an index of the amount of odorous components, such as aldehydes and ketones, contained in the regrind layer that migrate into the contents. The lower the TOC content, the less odorous components migrate into the contents. A TOC content of less than 0.7 ppm by mass sufficiently suppresses the migration of odorous components into the contents. The TOC content can be measured using a total organic carbon meter (trade name: TOC-V CPH, manufactured by Shimadzu Corporation).

[0019] Regarding the rigidity of the squeeze container, the compressive strength in the vertical direction (direction from the mouth to the bottom of the squeeze container) of the squeeze container is preferably 70 N or less, more preferably 40 to 70 N. A compressive strength of 70 N or less allows the contents of the squeeze container to be easily pushed out, improving squeezability. Furthermore, a compressive strength of 40 N or more improves the container's self-supporting ability. The compressive strength is a value measured by the following method. The squeeze container is filled with water in an amount equal to the amount of the contents, and after conditioning at 23°C for 24 hours, the squeeze container is compressed in the vertical direction using a compression tester to measure the compressive strength. Compression is performed at 20 mm / min without a V-notch. A Tensilon universal testing machine (trade name: RTG-1310, manufactured by A&D Co., Ltd.) can be used as the compression tester.

[0020] (Oxygen barrier layer A and oxygen barrier layer B) The oxygen barrier layer A and the oxygen barrier layer B each contain EVOH, polyethylene, and a compatibilizer. Because the oxygen barrier layer A and the oxygen barrier layer B contain EVOH, which has gas barrier properties, they function to block the permeation of oxygen and odorous components contained in the regrind layer. Furthermore, because the EVOH and the polyethylene are compatibilized by the compatibilizer and are uniformly distributed, the oxygen barrier layer A and the oxygen barrier layer B exhibit excellent adhesion to the outer layer, inner layer, and regrind layer due to the polyethylene. The composition and thickness (mass ratio) of the oxygen barrier layer A and the oxygen barrier layer B may be the same or different.

[0021] The EVOH is preferably a saponified copolymer obtained by saponifying an ethylene-vinyl acetate copolymer having an ethylene content of 20 to 60 mol% to a degree of saponification of 96 mol% or more, particularly 99 mol% or more. From the viewpoint of gas barrier properties, the ethylene content is preferably 20 to 38 mol%. The EVOH (saponified ethylene-vinyl acetate copolymer) may have an intrinsic viscosity of 0.01 dL / g or more, particularly 0.05 dL / g or more, measured at 30°C in a mixed solvent of phenol / water in a mass ratio of 85 / 15.

[0022] The polyethylene is preferably low-density polyethylene (hereinafter also referred to as LDPE). LDPE has a density of 0.910 g / cm 3 More than 0.930g / cm 3 The polyethylene is preferably polyethylene having a melt flow rate (MFR) of 0.1 g / 10 min or more at 190°C under a load of 2.16 kg, from the viewpoint of suppressing phase separation with EVOH during molding and preventing delamination. Furthermore, from the viewpoint of moldability, the MFR is preferably 30 g / 10 min or less. The MFR is more preferably 0.3 to 10 g / 10 min.

[0023] Compatibilizers are used to make EVOH and polyethylene compatible, reduce the size of the phase-separated structure between them, and increase the cohesive strength between EVOH and polyethylene. Examples of compatibilizers include carboxylic acids or their anhydrides, such as maleic acid, itaconic acid, and fumaric acid; maleic acid-polyethylene copolymers; maleic anhydride-polyethylene copolymers; graft-modified olefin resins graft-modified with amides or esters; ethylene-(meth)acrylic acid copolymers; ethylene-vinyl acetate copolymers; saponified ethylene-vinyl acetate copolymers with a saponification degree of 20 to 100%; ethylene-vinyl alcohol copolymers with an ethylene content of 85% or more; hydrotalcite compounds; and ionomers (ionically cross-linked olefin copolymers). These may be used alone or in combination. Among these, resins that do not contain acids or acid anhydrides that chemically react with EVOH are preferred as compatibilizers, with ionomers being particularly preferred.

[0024] The oxygen barrier layer A and the oxygen barrier layer B each preferably contain EVOH and polyethylene in a mass ratio of 95:5 to 50:50, more preferably 90:10 to 55:45, even more preferably 85:15 to 60:40, and particularly preferably 80:20 to 65:35. Furthermore, the oxygen barrier layer A and the oxygen barrier layer B each preferably contain 1 to 49 parts by mass of a compatibilizer per 100 parts by mass of the total amount of EVOH and polyethylene, more preferably 2 to 40 parts by mass, even more preferably 3 to 30 parts by mass, and particularly preferably 4 to 20 parts by mass. By containing EVOH, polyethylene, and a compatibilizer within the above mass ratio ranges, respectively, the rigidity of the squeeze container can be reduced while maintaining gas barrier properties.

[0025] The EVOH, polyethylene, and compatibilizer can be mixed by melt-kneading in a kneading section provided in an extruder or an injector, for example.

[0026] The ratio of the total mass of the oxygen barrier layer A and the oxygen barrier layer B to the mass of the squeeze container is preferably 1 to 30% by mass, more preferably 3 to 20% by mass, and even more preferably 5 to 10% by mass. When this ratio is 1% by mass or more, it is possible to sufficiently block the permeation of oxygen and odorous components contained in the regrind layer. Furthermore, when this ratio is 30% by mass or less, it is possible to improve squeezability.

[0027] The mass ratio of the oxygen barrier layer B to the mass of the squeeze container is preferably 0.5 to 15 mass%, more preferably 1.5 to 10 mass%, and even more preferably 2.5 to 5 mass%. When the ratio is 0.5 mass% or more, permeation of odorous components contained in the regrind layer can be sufficiently blocked. Furthermore, when the ratio is 15 mass% or less, squeezability can be improved. The preferred range of the mass ratio of the oxygen barrier layer A to the mass of the squeeze container is the same as that of the oxygen barrier layer B.

[0028] (Regrind layer) The regrind layer, also known as the repro layer, is a layer containing scrap resin, which is made by crushing parts other than the container, such as resin and flash, that are discarded at the start of molding. In other words, scrap resin is a mixture of materials that make up the various layers of the container, and the regrind layer is a layer containing this mixture. Reusing this scrap resin reduces the amount of virgin resin used, which is environmentally friendly and reduces manufacturing costs. However, because the scrap resin has a thermal history, it contains odorous components, such as carbonyl-containing compounds such as aldehydes and ketones, which are decomposition products of the resin. In the squeeze container of the present invention, the oxygen barrier layer B prevents these odorous components from migrating to the contents.

[0029] The regrind layer can contain the virgin material in addition to the scrap resin. Examples of the virgin material include LDPE. However, the content of the scrap resin in the regrind layer is preferably 1 to 100% by mass. In other words, the regrind layer can be made of the scrap resin.

[0030] The mass ratio of the regrind layer to the mass of the squeeze container is not particularly limited, but can be, for example, 30 to 80 mass %, preferably 35 to 70 mass %, and more preferably 40 to 60 mass %.

[0031] The fact that the layer contained in the squeeze container is a regrind layer can be confirmed, for example, by optical microscopic observation of a section prepared with a microtome, material analysis using a Fourier transform infrared spectrophotometer, or a combination of these. Specifically, optical microscopic observation reveals a sea-island structure in which materials with different refractive indices are dispersed, and material analysis using a Fourier transform infrared spectrophotometer reveals a spectrum based on the stretching vibration of OH groups that is characteristic of EVOH in addition to polyethylene.

[0032] (outer layer, inner layer) The outer layer and the inner layer may contain an olefin-based resin. Examples of olefin-based resins include polyethylenes such as low-density polyethylene (LDPE), medium-density polyethylene (MDPE), high-density polyethylene (HDPE), linear low-density polyethylene (LLDPE), and linear very-low-density polyethylene (LVLDPE), as well as polypropylene, ethylene-propylene copolymers, polybutene-1, ethylene-butene-1 copolymers, propylene-butene-1 copolymers, ethylene-propylene-butene-1 copolymers, ethylene-vinyl acetate copolymers, and ionically crosslinked olefin copolymers (ionomers). These may be used alone or in combination of two or more. Among these, polyethylene is preferred from the viewpoint of better adhesion to the oxygen barrier layer A and the oxygen barrier layer B, and low-density polyethylene (LDPE) is more preferred.

[0033] The materials constituting the outer layer and the inner layer may be the same or different, and the outer layer and the inner layer may contain lubricants, modifiers, pigments, ultraviolet absorbers, etc., as necessary.

[0034] The ratio of the mass of the outer layer to the mass of the squeeze container is not particularly limited, but may be, for example, 5 to 30% by mass, and preferably 10 to 20% by mass. The ratio of the mass of the inner layer to the mass of the squeeze container is not particularly limited, but may be, for example, 10 to 40% by mass, and preferably 15 to 30% by mass.

[0035] (virgin layer) The squeeze container according to the present invention may contain a virgin layer as needed. Examples of the virgin material contained in the virgin layer include the virgin material that can be contained in the regrind layer. When the squeeze container has a virgin layer, the mass ratio of the virgin layer to the mass of the squeeze container is not particularly limited, but may be, for example, 0.1 to 5 mass%.

[0036] (Method for manufacturing squeeze containers) The method for producing a squeeze container according to the present invention is not particularly limited, but may include, for example, the steps of producing a tubular parison including, from the outside in, an oxygen barrier layer A, a regrind layer, and an oxygen barrier layer B, in that order; and sandwiching the parison between molds to pinch off and fuse the parison, and then blowing gas into the interior of the parison to form it. Specifically, the materials for the layers constituting the tubular container are first co-extruded using a multi-layer die to produce a tubular parison. The melt-extruded parison is then fed into a mold, where it is sandwiched between the molds from both sides to pinch off and fuse the parison. Compressed gas, such as air, is then blown into the interior of the parison to expand it and mold it into the shape of the container. The parison is then cooled, and the mold is opened to remove the molded product.

[0037] (Application) The squeeze container according to the present invention can be used as a container for storing and preserving viscous foods such as wasabi, ginger, mustard, ketchup, mayonnaise, jam, and chocolate, as well as toothpaste and cosmetics. Use of the squeeze container according to the present invention can prevent the odor of the container itself from transferring to the contents. Furthermore, the squeeze container according to the present invention has high squeezability, allowing the contents to be easily squeezed out. [Example]

[0038] The present invention will be described in more detail below with reference to examples, but is not limited to these examples. The flavor, dissolution, and rigidity of the bottles obtained in Example 1 and Comparative Example 1 were evaluated by the following methods.

[0039] [Flavor Evaluation] The bottles obtained in Example 1 and Comparative Example 1 were filled with 400 g of ultrapure water at 85°C, and the openings were sealed with a sealant. After sterilization by inversion for 10 minutes, the bottles were cooled to room temperature under running water and stored for one week. The flavor of the ultrapure water (hereinafter also referred to as test solution) in the bottles after storage was evaluated using the following three-point discrimination and preference test.

[0040] (3-point discrimination and preference method) A discrimination test was conducted by a panel of 10 members using the test liquid of Example 1 and the test liquid of Comparative Example 1 by a three-point discrimination method. Specifically, a combination of three test liquids, two of Example 1's test liquids and one of Comparative Example 1's test liquid, or a combination of three test liquids, two of Comparative Example 1's test liquids and one of Example 1's test liquid, was presented to the panel, and each panelist was asked to identify only one different test liquid. The number of correct answers out of the total number of responses (20) is shown in Table 1. In addition, as a preference test, the panelists who answered the discrimination test correctly were asked which of the discriminated test liquids they preferred as their flavor. The results are shown in Table 1.

[0041] [Evaluation of dissolution] The TOC (Total Organic Carbon) amounts of the test solutions of Example 1 and Comparative Example 1 in the flavor evaluation were measured using a total organic carbon meter (product name: TOC-V CPH, manufactured by Shimadzu Corporation). The measurement was performed three times, and the average value was calculated. The results are shown in Table 1.

[0042] [Rigidity evaluation] The bottles obtained in Example 1 and Comparative Example 1 were filled with 400 g of water and conditioned at 23°C for 24 hours. Using a compression tester (Tensilon Universal Tester, product name: RTG-1310, manufactured by A&D Co., Ltd.), the bottles were compressed in the vertical direction (from the mouth of the bottle to the bottom) (20 mm / min, no V-notch) to measure the compressive strength. Measurements were made on 24 bottles, and the average results are shown in Table 1.

[0043] [Example 1] LDPE (product name: LB420M, manufactured by Japan Polyethylene Co., Ltd.) was prepared as the material for the inner layer, outer layer, and virgin layer. A mixture containing 70 parts by mass of EVOH (product name: DC3203RB, manufactured by Nippon Synthetic Co., Ltd.), 20 parts by mass of LDPE (product name: LB420M, manufactured by Japan Polyethylene Co., Ltd.), and 10 parts by mass of an ionomer resin (product name: Himilan 1601, manufactured by Mitsui-DuPont Polychemicals) was prepared as the material for the oxygen barrier layers A and B. A mixture of 60 parts by mass of LDPE (product name: LB420M, manufactured by Japan Polyethylene Co., Ltd.) and 40 parts by mass of a mixture of recycled layer materials (scrap resin) was prepared as the material for the regrind layer. The materials for the inner layer, outer layer, virgin layer, oxygen barrier layers A and B, and regrind layer were fed into three extruders, respectively, and a multilayer parison consisting of six layers: outer layer / oxygen barrier layer A / virgin layer / regrind layer / oxygen barrier layer B / inner layer was extruded. Next, the multilayer parison was molded by direct blow molding to obtain a bottle, a squeeze container with a volume of 420 ml and a mass of 18 g.

[0044] The bottle had a body with a thickness of 300 μm at its thinnest point, and the mass fraction of each layer was: outer layer (15.0 mass%) / oxygen barrier layer A (3.3 mass%) / virgin layer (1.0 mass%) / regrind layer (52.4 mass%) / oxygen barrier layer B (3.3 mass%) / inner layer (25.0 mass%).

[0045] The bottles were subjected to the flavor evaluation, dissolution evaluation, and rigidity evaluation, and the results are shown in Table 1.

[0046] [Comparative Example 1] LDPE (trade name: LB420M, manufactured by Japan Polyethylene Co., Ltd.) was prepared as the material for the inner and outer layers. EVOH (trade name: DC3203RB, manufactured by Nippon Synthetic Co., Ltd.) was prepared as the material for the oxygen barrier layer. Modified polyolefin resin (trade name: Modic L522, manufactured by Mitsubishi Chemical Corporation) was prepared as the material for the adhesive layer. A mixture of 60 parts by mass of LDPE (trade name: LB420M, manufactured by Japan Polyethylene Co., Ltd.) and 40 parts by mass of a mixture of recycled materials (scrap resin) for each layer was prepared as the material for the regrind layer. The materials for the inner and outer layers, oxygen barrier layer, adhesive layer, and regrind layer were each fed into four extruders, and a multilayer parison consisting of six layers (outer layer / adhesive layer / oxygen barrier layer / adhesive layer / regrind layer / inner layer) was extruded. The multilayer parison was then directly blow molded to obtain a bottle, a squeeze container with a capacity of 420 ml and a mass of 18 g.

[0047] The bottle had a body with a thickness of 300 μm at its thinnest point, and the mass fractions of the individual layers were: outer layer (15.0% by mass), adhesive layer (1.0% by mass), oxygen barrier layer (2.4% by mass), adhesive layer (1.0% by mass), regrind layer (65.6% by mass), and inner layer (15.0% by mass).

[0048] The bottles were subjected to the flavor evaluation, dissolution evaluation, and rigidity evaluation, and the results are shown in Table 1.

[0049] [Table 1]

[0050] As shown in Table 1, in the flavor evaluation (three-point discrimination / preference method), Example 1 was significantly distinguished from Comparative Example 1, and it was confirmed that Example 1 was preferred over Comparative Example 1. Furthermore, many of the panelists who answered correctly in the discrimination test commented that Example 1 had a weaker taste and smell of plastic, etc., than Comparative Example 1. Furthermore, in the elution evaluation, it was confirmed that Example 1 had a lower TOC amount than Comparative Example 1. From these evaluations, it is inferred that in Example 1, the migration of odorous components such as aldehydes and ketones contained in the regrind layer to the contents was partially blocked by the oxygen barrier layer B present between the regrind layer and the inner layer.

[0051] Furthermore, in the rigidity evaluation, it was confirmed that Example 1 had lower compressive strength and rigidity, i.e., higher squeezability, than Comparative Example 1. In Comparative Example 1, EVOH alone was used as the material for the oxygen barrier layer, whereas in Example 1, a mixture containing LDPE and a compatibilizer in addition to EVOH was used as the material for oxygen barrier layers A and B, and it is presumed that this caused the rigidity of the entire bottle in Example 1 to decrease. The present invention includes the following embodiments. [1] A squeeze container including, from the outside, an oxygen barrier layer A, a regrind layer, and an oxygen barrier layer B in this order, The squeeze container, wherein the oxygen barrier layer A and the oxygen barrier layer B each contain an ethylene-vinyl alcohol copolymer, polyethylene, and a compatibilizer. [2] The squeeze container according to [1], wherein the oxygen barrier layer A and the oxygen barrier layer B each contain an ethylene-vinyl alcohol copolymer and polyethylene in a mass ratio of 95:5 to 50:50, and further contain 1 to 49 parts by mass of a compatibilizer per 100 parts by mass of the total amount of the ethylene-vinyl alcohol copolymer and the polyethylene. [3] The squeeze container according to [1] or [2], wherein the ratio of the total mass of the oxygen barrier layer A and the oxygen barrier layer B to the mass of the squeeze container is 1 to 30 mass %. [4] The squeeze container according to any one of [1] to [3], wherein the mass ratio of the oxygen barrier layer B to the mass of the squeeze container is 0.5 to 15 mass %. [5] The squeeze container according to any one of [1] to [4], wherein the thickness of the thinnest part of the body of the squeeze container is 180 to 1500 μm. [6] The squeeze container according to any one of [1] to [5], wherein the squeeze container comprises an outer layer, the oxygen barrier layer A, the regrind layer, the oxygen barrier layer B, and an inner layer in this order. [Explanation of symbols]

[0052] 1 Mouth 2. Torso 3 bottom 4 Outer layer 5 Oxygen barrier layer A 6 Virgin Layer 7 Regrind layer 8 Oxygen barrier layer B 9 Inner layer

Claims

1. A squeeze container including, in order from the outside, an oxygen barrier layer A, a regrind layer, and an oxygen barrier layer B, The oxygen barrier layer A and the oxygen barrier layer B each contain an ethylene-vinyl alcohol copolymer, polyethylene, and a compatibilizer, The oxygen barrier layer A and the oxygen barrier layer B each contain an ethylene-vinyl alcohol copolymer and polyethylene in a mass ratio of 80:20 to 65:35, and further contain 4 parts by mass or more and less than 20 parts by mass of a compatibilizer per 100 parts by mass of the total amount of the ethylene-vinyl alcohol copolymer and the polyethylene.

2. The squeeze container according to claim 1, wherein a ratio of a total mass of the oxygen barrier layer A and the oxygen barrier layer B to a mass of the squeeze container is 1 to 30 mass%.

3. The squeeze container according to claim 1 or 2, wherein a ratio of a mass of the oxygen barrier layer B to a mass of the squeeze container is 0.5 to 15 mass%.

4. The squeeze container according to any one of claims 1 to 3, wherein the thickness of the thinnest part of the body of the squeeze container is 180 to 1500 µm.

5. The squeeze container according to claim 1 , comprising an outer layer, the oxygen barrier layer A, the regrind layer, the oxygen barrier layer B, and an inner layer in this order.

Citation Information

Patent Citations

  • JP1974035482A

  • Lightweight squeeze bottle

    JP2001253426A

  • Squeezing-out multi-layer container

    JP2003063543A

  • Multilayer structure

    JP2005001371A