Method for increasing oxide / nitride selectivity and achieving low uniformity in oxide trench dishing in shallow trench isolation (STI) chemical mechanical planarization (CMP) - Patent Application 20070123633

JP7580909B2Active Publication Date: 2024-11-12VERSUM MATERIALS US LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2019175002
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-09-20
Filing Date
2019-09-26
Publication Date
2024-11-12
Estimated Expiration
2039-09-26

AI Technical Summary

Technical Problem

Existing shallow trench isolation (STI) polishing compositions fail to address the issue of non-uniform trench dishing and high oxide trench loss, leading to transistor isolation failures and reduced device manufacturing yield.

Method used

A chemical mechanical polishing (CMP) composition comprising ceria-coated inorganic oxide particles, chemical additives with carboxylic acid groups and hydroxyl functional groups, and a pH adjuster, which reduces SiN film removal rate and oxide trench dishing, ensuring uniform trench dishing and high selectivity across various pH conditions.

Benefits of technology

The CMP composition achieves high oxide film removal rates with low SiN film removal rates, significantly reducing oxide trench dishing and improving the planarity of patterned wafers, thereby enhancing transistor performance and yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000037_0000
    Figure 00000037_0000
  • Figure 00000038_0000
    Figure 00000038_0000
  • Figure 00000039_0000
    Figure 00000039_0000
Patent Text Reader

Abstract

To provide a chemical mechanical planarization (CMP) composition for shallow trench isolation (STI).SOLUTION: A CMP composition includes ceria-coated inorganic metal oxide particles such as ceria-coated silica particles or ceria-coated inorganic metal oxide particles as other core particles as an abrasive, a suitable chemical additive having at least one organic carboxylic acid group, at least one carboxylic acid group, or at least one carboxylic acid ester group, and two or more hydroxyl functional groups in the same molecule, a water-soluble solvent, and a biocide and a pH adjuster optionally. The pH of the composition is 2 to 12, preferably 3 to 10, more preferably 4 to 9.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application is a non-provisional application of U.S. Provisional Application No. 62 / 736,963 with a filing date of September 26, 2018, and the entire disclosure of the provisional application is incorporated herein by reference.

[0002] The present invention relates to STI CMP chemical mechanical polishing compositions and chemical mechanical planarization (CMP) for shallow trench isolation (STI) processes.

[0003] In the fabrication of microelectronic devices, polishing, particularly chemical-mechanical polishing of surfaces for the restoration of selected materials and / or planarization of structures, is an important step.

[0004] For example, a SiN layer is deposited under a SiO2 layer and functions as a polish stop layer. The role of such a polish stop layer is particularly important in shallow trench isolation (STI) structures. Selectivity is typically expressed as the ratio of the nitride polish rate to the oxide polish rate. An example is the enhanced polish selectivity of silicon dioxide (SiO2) over silicon nitride (SiN).

[0005] In the global planarization of patterned STI structures, reducing oxide trench dishing is a key factor to be considered. By reducing the loss of trench oxide, current leakage between adjacent transistors is avoided. Non-uniform trench oxide loss across the die (within the die) affects transistor performance and device manufacturing yield. High trench oxide loss (large oxide trench dishing) causes transistor isolation failure and leads to device failure. Therefore, it is important to reduce trench oxide loss by reducing oxide trench dishing in STI CMP polishing compositions.

[0006] U.S. Patent No. 5,876,490 discloses an abrasive composition containing abrasive particles and exhibiting a normal stress effect. The slurry further contains non-abrasive particles, which reduce the polishing speed in recesses, while the abrasive particles ensure a high polishing speed in convex areas. This improves planarization. More specifically, the slurry contains cerium oxide particles and a polymer electrolyte and can be used for shallow trench isolation (STI) polishing applications.

[0007] U.S. Patent No. 6,964,923 teaches an abrasive composition for shallow trench isolation (STI) polishing comprising cerium oxide particles and a polyelectrolyte. The polyelectrolyte used comprises a salt of polyacrylic acid, similar to U.S. Patent No. 5,876,490. Ceria, alumina, silica, and zirconia are used as abrasives. The molecular weights of the described polyelectrolytes range from 300 to 20,000, but the total is <100,000.

[0008] U.S. Patent No. 6,616,514 discloses a chemical mechanical polishing slurry used to remove a first substance from the surface of an article in preference to silicon nitride by chemical mechanical polishing. The chemical mechanical polishing slurry according to the invention comprises an abrasive, an aqueous medium, and a proton-non-dissociating organic polyol, wherein the organic polyol comprises a compound having at least three hydroxyl groups that do not dissociate in the aqueous medium, or a polymer formed from at least one monomer having at least three hydroxyl groups that do not dissociate in the aqueous medium.

[0009] U.S. Patent No. 5,738,800 discloses a composition for polishing a composite comprising silica and silicon nitride, the composition comprising an aqueous medium, abrasive particles, a surfactant, and a compound that forms a complex with silica and silicon nitride, wherein the complexing agent has two or more identical or different functional groups that are proton-dissociable.

[0010] International Publication No. 2007 / 086665 discloses a CMP slurry in which a compound having a weight-average molecular weight of 30 to 500 and containing a hydroxyl group (OH), a carboxyl group (COOH), or both is added to a CMP slurry containing abrasive particles and water and having a first viscosity, thereby controlling the CMP slurry to have a second viscosity that is 5 to 30% lower than the first viscosity. The publication also discloses a method for polishing semiconductor wafers using the CMP slurry. According to the disclosed invention, it is possible to reduce the viscosity of the CMP slurry and improve the global planarization of the wafer during polishing, while also reducing the aggregate particle size of the abrasive particles in the CMP slurry. Therefore, the CMP slurry can be advantageously used in the manufacturing process of semiconductor devices that require fine patterns, and its use in semiconductor processes can improve the reliability and productivity of semiconductor devices. [Overview of the project] [Problems that the invention aims to solve]

[0011] However, these conventionally disclosed shallow trench isolation (STI) polishing compositions did not address the importance of reducing dishing of oxide trenches in the polished pattern wafer with high oxide / nitride selectivity, and of making the dishing of oxide trenches more uniform.

[0012] From the above, it is clear that in this technical field, there is a need for STI chemical mechanical polishing (CMP) compositions, methods, and systems that, in addition to high silicon dioxide removal rates and high selectivity of silicon dioxide over silicon nitride, can reduce dishing of oxide trenches of various sizes and provide more uniform oxide trench dishing for polishing patterned wafers in the STI chemical mechanical polishing (CMP) process. [Means for solving the problem]

[0013] The present invention relates to a composition for shallow trench isolation (STI) chemical mechanical polishing in a wide pH range including acidic, neutral, and alkaline pH conditions. By introducing chemical additives such as a SiN film removal rate reducer and an oxide trench dishing reducer, the invention not only enhances oxide / nitride selectivity but also reduces dishing of oxide trenches on the polished pattern wafer for oxide trenches of various sizes, and makes the dishing of the oxide trenches more uniform.

[0014] The shallow trench isolation (STI) chemical mechanical polishing composition of this disclosure has a unique combination of ceria-coated inorganic oxide particles as an abrasive and appropriate chemical additives as an oxide trench dishing reducer and a nitride removal rate reducer.

[0015] In one way, Ceria-coated inorganic metal oxide particles; A chemical additive having at least one carboxylic acid group (R-COOH), at least one carboxylic acid salt group, or at least one carboxylic acid ester group and at least two hydroxyl functional groups (OH) within the same molecule; Water-soluble solvents; and at will Bioside; and pH adjuster; Includes, The pH is 2 to 12, preferably 3 to 10, more preferably 4 to 9, and most preferably 4.5 to 7.5. STI CMP polishing composition It will be provided.

[0016] Ceria-coated inorganic oxide particles include, but are not limited to, ceria-coated colloidal silica, ceria-coated high-purity colloidal silica, ceria-coated alumina, ceria-coated titania, ceria-coated zirconia, or other ceria-coated inorganic metal oxide particles.

[0017] Water-soluble solvents include, but are not limited to, deionized (DI) water, distilled water, and alcoholic organic solvents.

[0018] The chemical additives function as a SiN film removal rate reducer and an oxide trench dishing reducer.

[0019] These chemical additives may have the general molecular structures shown below.

Chemical Formula 1

[0020] In the above general molecular structures (a) or (b), n is selected from 1 to 5000, preferably 2 to 12, and more preferably 3 to 6.

[0021] R1, R2, R3, and R4 can be the same or different atoms or functional groups. They can be independently selected from the group consisting of hydrogen, alkyl, alkoxy, organic groups with one or more hydroxyl groups, substituted organic sulfonic acids, substituted organic sulfonate salts, substituted organic carboxylic acids, substituted organic carboxylate salts, organic carboxylic acid esters, organic amine groups, and combinations thereof, and at least two or more, preferably three or more, can be hydrogen atoms.

[0022] Furthermore, either R1, R4, or both R1 and R4 can be metal ions or ammonium ions. The metal ions include, but are not limited to, sodium ions and potassium ions.

[0023] When all of R1, R2, R3, and R4 are hydrogen atoms, the chemical additive has one (structure (a)) or two (structure (b)) organic carboxylic acid groups and two (structure (b)) or more (structure (a)) hydroxyl functional groups.

[0024] An example of the molecular structure of such a chemical additive is shown below.

Chemical Formula 2

Chemical Formula 3

[0025] When R1 is a metal ion or an ammonium ion in Structure (a), the chemical additive has a general molecular structure as shown below.

Chemical Formula 4

[0026] When both R1 and R4 are metal ions or ammonium ions in Structure (b), the chemical additive has the general molecular structure shown below.

Chemical Formula 5

[0027] In Structure (i), when R1 is a metal ion and all of R2, R3, and R4 are hydrogen atoms, an example of the molecular structure of such a chemical additive is as shown below.

Chemical Formula 6

[0028] In Structure (a), when R1 is an organic alkyl group, the chemical additive has an organic acid ester functional group and a plurality of hydroxyl functional groups within the same molecule. The general molecular structure is as shown below.

Chemical Formula 7

[0029] In Structure (v), when R2, R3, and R4 are hydrogen atoms, an example of the molecular structure of such a chemical additive is as shown below.

Chemical Formula 8

[0030] In another aspect, in a shallow trench isolation (STI) process, a method for chemically mechanical polishing (CMP) a substrate having at least one surface containing silicon dioxide using the above-described chemical mechanical polishing (CMP) composition is provided.

[0031] In another aspect, in a shallow trench isolation (STI) process, a system for chemically mechanical polishing (CMP) a substrate having at least one surface containing silicon dioxide using the above-described chemical mechanical polishing (CMP) composition is provided.

[0032] The oxide film to be polished may be a chemical vapor deposition (CVD), plasma CVD (PECVD), high-density deposition CVD (HDP), or spin-on oxide film.

[0033] The substrate may further have a silicon nitride surface. The removal selectivity for SiO2:SiN is greater than 25, preferably greater than 30, and more preferably greater than 35. [Brief explanation of the drawing]

[0034] [Figure 1] Figure 1 shows the effect of gluconic acid on film RR (Å / min) and TEOS:SiN selectivity.

[0035] [Figure 2] Figure 2 shows the effect of gluconic acid on the oxide trench dishing rate.

[0036] [Figure 3] Figure 3 shows the effect of gluconic acid on the oxide trench loss rate (A / Sec).

[0037] [Figure 4] Figure 4 shows the effect of gluconic acid on oxide trench dishing vs. OP time (sec).

[0038] [Figure 5] Figure 5 shows the effect of gluconic acid on oxide trench dishing vs. OP time (sec).

[0039] [Figure 6] Figure 6 shows the effect of gluconic acid on oxide trench dishing vs. OP time (sec).

[0040] [Figure 7] Figure 7 shows the effect of changing the weight percentage of gluconic acid (GA) on film RR (A / min) and TEOS:SiN selectivity.

[0041] [Figure 8] Figure 8 shows the effect of changing the weight percentage of gluconic acid (GA) on the oxide trench dishing rate.

[0042] [Figure 9] Figure 9 shows the effect of changing the weight percentage of gluconic acid (GA) on the oxide trench loss rate (A / Sec).

[0043] [Figure 10] Figure 10 shows the effect of varying the weight percentage of gluconic acid on oxide trench dishing vs. OP time (sec).

[0044] [Figure 11] Figure 11 shows the effect of varying the weight percentage of gluconic acid on oxide trench dishing vs. OP time (sec).

[0045] [Figure 12] Figure 12 shows the effect of varying the weight percentage of gluconic acid on oxide trench dishing vs. OP time (sec).

[0046] [Figure 13] Figure 13 shows the effects of pH and 0.01 wt% gluconic acid (GA) on film RR (A / min) and TEOS:SiN selectivity.

[0047] [Figure 14] Figure 14 shows the effect of pH on oxide trench dishing rate when 0.01 wt% gluconic acid (GA) is used.

[0048] [Figure 15] Figure 15 shows the effect of pH on oxide trench loss rate when 0.01 wt% gluconic acid (GA) is used.

[0049] [Figure 16] Figure 16 shows the effect of pH on oxide trench dishing vs. OP time (sec) when 0.01 wt% gluconic acid (GA) is used.

[0050] [Figure 17] Figure 17 shows the effect of pH on oxide trench dishing vs. OP time (sec) when 0.01 wt% gluconic acid (GA) is used.

[0051] [Figure 18] Figure 18 shows the effect of pH on oxide trench dishing vs. OP time (sec) when 0.01 wt% gluconic acid (GA) is used. [Modes for carrying out the invention]

[0052] In the global planarization of patterned STI structures, key factors to consider include reducing the SiN removal rate, minimizing oxide trench dishing, and achieving more uniform oxide trench dishing across oxide trenches of various sizes. Reducing trench oxide loss prevents current leakage between adjacent transistors. Non-uniform trench oxide loss throughout the die (within the die) affects transistor performance and device manufacturing yield. High trench oxide loss (large oxide trench dishing) leads to transistor isolation failure and ultimately device failure. Therefore, in STI CMP polishing compositions, it is crucial to reduce trench oxide loss by minimizing oxide trench dishing.

[0053] The present invention relates to a CMP composition used in chemical mechanical polishing (CMP) of shallow trench isolation (STI).

[0054] More specifically, the CMP composition of this disclosure used in chemical mechanical polishing (CMP) of shallow trench isolation (STI) has a unique combination of ceria-coated inorganic oxide particles as inorganic metal oxide abrasive particles and appropriate chemical additives as oxide trench dishing reducers and nitride removal rate reducers.

[0055] Suitable chemical additives include, but are not limited to, organic carboxylic acid molecules, organic carboxylic acid salts, or organic carboxylic acid ester molecules having multiple hydroxyl functional groups within the same molecule.

[0056] Chemical additives contain, within the same molecule, at least one of an organic carboxylic acid group, an organic carboxylic acid base, or a carboxylic acid ester group, and two or more hydroxyl functional groups.

[0057] The chemical additives offer advantages such as achieving a high oxide film removal rate, a low SiN film removal rate, and high and tunable oxide:SiN selectivity, and more importantly, significantly reducing dishing of oxide trenches and improving polishing window stability when polishing patterned wafers.

[0058] In one embodiment, an STI CMP polishing composition, Ceria-coated inorganic metal oxide particles; Chemical additives used as agents to reduce the rate of SiN film removal and oxide trench dishing during the polishing of patterned wafers; Water-soluble solvent; and at will Bioside; and pH adjuster; Includes, The pH is 2 to 12, preferably 3 to 10, more preferably 4 to 9, and most preferably 4.5 to 7.5. An STI CMP polishing composition is provided.

[0059] Ceria-coated inorganic metal oxide particles include, but are not limited to, ceria-coated colloidal silica, ceria-coated high-purity colloidal silica, ceria-coated alumina, ceria-coated titania, ceria-coated zirconia, or other ceria-coated inorganic metal oxide particles.

[0060] The particle size of the ceria-coated inorganic metal oxide particles in the invention disclosed herein (measured by Dynamic Light Scattering DLS technology) is in the range of 10 nm to 1000 nm, the preferred average particle size is in the range of 20 nm to 500 nm, and the more preferred average particle size is in the range of 50 nm to 250 nm.

[0061] The concentration of these ceria-coated inorganic metal oxide particles ranges from 0.01% by weight to 20% by weight, with a preferred concentration ranging from 0.05% by weight to 10% by weight, and a more preferred concentration ranging from 0.1% by weight to 5% by weight.

[0062] A preferred ceria-coated inorganic metal oxide particle is a ceria-coated colloidal silica particle.

[0063] Preferred chemical additives as SiN film removal rate reducers and oxide trench dishing reducers have at least one carboxylic acid group (R-COOH), at least one carboxylic acid salt group or at least one carboxylic acid ester group and at least two hydroxyl functional groups (OH) within the same molecule.

[0064] These chemical additives may have the general molecular structures shown below. [C9]

[0065] In the general molecular structure (a) or (b), n is selected from 1 to 5000, preferably 2 to 12, and more preferably 3 to 6.

[0066] R1, R2, R3, and R4 may be the same or different atoms or functional groups. They may be independently selected from the group consisting of hydrogen, alkyl, alkoxy, organic groups having one or more hydroxyl groups, substituted organic sulfonic acids, substituted organic sulfonates, substituted organic carboxylic acids, substituted organic carboxylate salts, organic carboxylic acid esters, organic amine groups, and combinations thereof, and at least two, preferably three or more, may be hydrogen atoms.

[0067] Furthermore, R1, R4, or both R1 and R4 may be metal ions or ammonium ions. The metal ions are not limited to, but include sodium ions and potassium ions.

[0068] If R1, R2, R3, and R4 are all hydrogen, the chemical additive has one (structure (a)) or two (structure (b)) organic carboxylic acid groups and two (structure (b)) or more (structure (a)) hydroxyl functional groups.

[0069] An example of the molecular structure of such a chemical additive is shown below. [C10] [C11]

[0070] When R1 in structure (a) is a metal ion or an ammonium ion, the chemical additive has the following general molecular structure. [C12]

[0071] In structure (b), if both R1 and R4 are metal ions or ammonium ions, the chemical additive has the following general molecular structure. [C13]

[0072] In structure (i), if R1 is a metal ion and R2, R3, and R4 are all hydrogen atoms, the molecular structure of an example of such a chemical additive is shown below. [C14]

[0073] In structure (a), if R1 is an organic alkyl group, the chemical additive has an organic acid ester functional group and multiple hydroxyl functional groups within the same molecule. The general molecular structure is shown below. [C15]

[0074] When R2, R3, and R4 are hydrogen atoms in structure (v), the molecular structure of an example of such a chemical additive is shown below. [C16]

[0075] The STI CMP composition contains chemical additives in amounts of 0.0001% to 2.0% by weight, 0.0002% to 1.0% by weight, 0.0003% to 0.75% by weight, 0.0004% to 0.5% by weight, 0.0005% to 0.5% by weight, 0.0006% to 0.25% by weight, or 0.0007% to 0.1% by weight, as SiN film removal rate reducers and oxide trench dishing reducers.

[0076] The water-soluble solvent is not particularly limited, but includes deionized (Di) water, distilled water, and alcoholic organic solvents.

[0077] The preferred water-soluble solvent is DI water.

[0078] The STI CMP composition may contain 0.0001% to 0.05% by weight, preferably 0.0005% to 0.025% by weight, and more preferably 0.001% to 0.01% by weight of bioside.

[0079] Biosides include, but are not limited to, Kathon®, Kathon® CG / ICP II, and Bioban, manufactured by DuPont / Dow Chemical. These contain the active ingredients 5-chloro-2-methyl-4-isothiazolin-3-one and 2-methyl-4-isothiazolin-3-one.

[0080] The STI CMP composition may contain a pH adjuster.

[0081] To achieve the optimal pH value of the STI polishing composition, an acidic or basic pH adjuster may be used.

[0082] pH adjusters include, but are not limited to, nitric acid, hydrochloric acid, sulfuric acid, phosphoric acid, other inorganic or organic acids, and mixtures thereof.

[0083] The pH adjuster may include a base pH adjuster such as sodium hydride, potassium hydroxide, ammonium hydroxide, tetraalkylammonium hydroxide, organic quaternary ammonium hydroxide compounds, organic amines, and other chemical reagents that can be used to adjust the pH toward a more alkaline direction.

[0084] The STI CMP composition contains a pH adjuster in an amount of 0% to 1% by weight, preferably 0.01% to 0.5% by weight, and more preferably 0.1% to 0.25% by weight.

[0085] The chemical additives used as SiN film removal rate reducers and oxide trenching dishing reducers are organic carboxylic acid molecules, organic carboxylic acid salts, or organic carboxylic acid ester molecules that have multiple hydroxyl functional groups within the same molecule.

[0086] In another embodiment, a method is provided for chemically mechanically polishing (CMP) a substrate having at least one silicon dioxide-containing surface using the above-described chemical mechanical polishing (CMP) composition in a shallow trench isolation (STI) process.

[0087] In another embodiment, a system is provided for chemically mechanically polishing (CMP) a substrate having at least one silicon dioxide-containing surface using the above-described chemical mechanical polishing (CMP) composition in a shallow trench isolation (STI) process.

[0088] The oxide film to be polished may be a chemical vapor deposition (CVD), plasma CVD (PECVD), high-density deposition CVD (HDP), or spin-on oxide film.

[0089] The substrate may further have a silicon nitride surface. The removal selectivity for SiO2:SiN is greater than 25, preferably greater than 30, and more preferably greater than 35.

[0090] In another embodiment, a method is provided for chemically mechanically polishing (CMP) a substrate having at least one silicon dioxide-containing surface using the above-described chemical mechanical polishing (CMP) composition in a shallow trench isolation (STI) process. The oxide film to be polished may be a CVD oxide, a PECVD oxide, a high-density oxide, or a spin-on oxide film.

[0091] The present invention will be further explained below with reference to examples, but the present invention is not limited thereto.

[0092] CMP method In the following examples of this disclosure, the CMP experiment was performed using the following procedure and experimental conditions.

[0093] term Ceria-coated silica: Used as an abrasive with a particle size of approximately 100 nanometers (nm); such ceria-coated silica particles may have particle sizes ranging from approximately 20 nanometers (nm) to 500 nanometers (nm).

[0094] Ceria-coated silica particles (of various sizes) are provided by JGC Ltd. of Japan and are obtained by the methods described in Japanese Patent Publication No. 2013-119131, Japanese Patent Publication No. 2013-133255, and International Publication No. 2016 / 159167; and Japanese Patent Applications No. 2015-169967 and 2015-183942.

[0095] Chemical additives such as maltitol, D-fructose, dulcitol, D-sorbitol, gluconic acid, mucoic acid, tartaric acid, and other chemical raw materials were supplied by Sigma-Aldrich Company in St. Louis, Missouri.

[0096] TEOS: Tetraethyl orthosilicate

[0097] Polishing pads: Polishing pads provided by Dow, including IC1010 and other pads, were used during CMP.

[0098] parameters General Å or ​​A: Angstrom (unit of length)

[0099] BP: back pressure, psi

[0100] CMP: Chemical mechanical planarization = chemical mechanical polishing

[0101] CS: Conveying speed

[0102] DF: Downforce: Pressure applied during CMP, psi

[0103] min: minutes

[0104] ml: milliliter

[0105] mV: millivolts

[0106] psi: pounds per square inch

[0107] PS: Platen rotation speed of grinding tool, rpm (revolutions per minute)

[0108] SF: Composition flow, ml / min

[0109] Wt.%: Weight percentage (of the listed ingredients)

[0110] TEOS:SiN selectivity:(TEOS removal rate) / (SiN removal rate)

[0111] HDP: High-density plasma deposition TEOS

[0112] TEOS or HDP removal rate: The TEOS or HDP removal rate measured at a specified downward pressure. In the above example, the downward pressure of the CMP tool was 2.0, 3.0, or 4.0 psi.

[0113] SiN removal rate: The SiN removal rate measured at a predetermined downward pressure. In the example above, the downward pressure of the CMP tool was 3.0 psi.

[0114] measurement Film measurements were performed using a ResMap CDE 168 instrument manufactured by Creative Design Engineering, Inc. (Cupertino, California 95014, 20565 Alves Drive). The ResMap instrument is a 4-point probe sheet resistance instrument. A 49-point diameter scan was performed, excluding the 5mm edge of the film.

[0115] CMP equipment The CMP equipment used was a 200mm Mirra or 300mm Reflexion from Applied Materials, Inc. (Santa Clara, California 95054, 3050 Bowers Avenue). IC1010 pads provided by Dow Corporation (Delaware, 19713) were used on platen 1 for blanket and patterned wafer experiments.

[0116] IC1010 pads or other pads failed after conditioning them for 18 minutes at a downforce of 7 pounds. To certify tool settings and pad break-in, two tungsten monitors and two TEOS monitors were polished in baseline conditions with Versum STI2305 composition supplied by Versum Materials.

[0117] wafer Polishing experiments were performed using PECVD, LECVD, or HD TEOS wafers. These blanket wafers were purchased from Silicon Valley Microelectronics, Inc. (2985 Kiffer Road, Santa Clara, California 95051).

[0118] Polishing experiment In the blanket wafer experiment, oxide blanket wafers and SiN blanket wafers were polished under baseline conditions. The baseline conditions of the equipment were: table speed: 87 rpm, head speed: 93 rpm, film thickness: 2.0 psi, internal tube pressure: 2.0 psi, holding ring pressure: 2.9 psi, and composition flow rate: 200 ml / min.

[0119] The composition was used in the polishing of pattern wafers (MIT860) manufactured by SWK Associates, Inc. (Santa Clara, California 95054, 2920 Scott Boulevard). These wafers were measured using a Veeco VX300 profiler / AFM instrument. Three different pitch sizes were employed for oxide dishing measurements. The wafers were measured at the center, middle, and edge die positions.

[0120] TEOS:SiN selectivity: (TEOS removal rate) / (SiN removal rate) obtained from an adjustable STI CMP polishing composition.

[0121] Examples In the following examples, an STI polishing composition containing 0.2% by weight of ceria-coated silica, 0.0001% to 0.05% by weight of bioside, and deionized water was prepared as a reference example.

[0122] The polishing compositions according to the examples were prepared using the above reference example (0.2% by weight of ceria-coated silica, a bioside in the range of 0.0001% to 0.05% by weight, and deionized water) and a chemical additive of the present disclosure in the range of 0.0025% to 0.015% by weight.

[0123] Example 1 Table 1 shows the polishing compositions used in Example 1. A reference sample was prepared using 0.2% by weight of ceria-coated silica and a very low concentration of bioside. 0.01% by weight of gluconic acid was used as a chemical additive. Both samples had similar pH levels (approximately 5.35).

[0124] The removal rate (RR, Å / min) was tested for different films. The effect of gluconic acid, a chemical additive, on film removal rate and selectivity was confirmed.

[0125] The test results are shown in Table 1 and Figure 1 below, respectively. [Table 1]

[0126] As shown in Table 1 and Figure 1, the addition of gluconic acid to the polishing composition resulted in high TEOS and HDP removal rates, while effectively reducing the SiN removal rate. This yielded a significantly higher TEOS:SiN film selectivity compared to the reference example where gluconic acid was not used as a chemical additive.

[0127] In other words, the polishing composition resulted in a decrease in the SiN film removal rate and a high oxide / silicon nitride selectivity.

[0128] The effect of gluconic acid, a chemical additive in the polishing composition, on oxide trench dishing rate was tested. The results are shown in Table 2 and Figure 2. [Table 2]

[0129] As shown in Table 2 and Figure 2, the addition of a chemical additive, namely gluconic acid, to the polishing composition reduced the oxide trench dishing rate by at least 72% for all oxide trench features of different sizes compared to the reference example without gluconic acid.

[0130] The effect of adding a chemical additive, specifically gluconic acid, to the polishing composition was confirmed in terms of oxide trench loss rate (A / sec) by comparing it with the polishing results of a reference example in which gluconic acid was not used as an additive.

[0131] The test results are shown in Table 3 and Figure 3, respectively. [Table 3]

[0132] As shown in Table 3 and Figure 3, the addition of a chemical additive, namely gluconic acid, to the polishing composition significantly reduced the oxide trench loss rate by at least 81% for all oxide trench features of different sizes compared to the reference example without gluconic acid.

[0133] The effect of adding a chemical additive, specifically gluconic acid, to the polishing composition was confirmed in oxide trench dishing with respect to over-polishing time, by comparing it with the polishing results of a reference example in which gluconic acid was not used as an additive.

[0134] Regarding the effect of oxide trench dishing on over-polishing time, the test results of the effect of gluconic acid, a chemical additive in the polishing composition, are shown in Table 4, and in Figures 4, 5, and 6, respectively. [Table 4]

[0135] As shown in Table 4, Figures 4, 5, and 6, the addition of a chemical additive, gluconic acid, to the polishing composition significantly reduced oxide trench dishing for all oxide trench features of different sizes and improved the over-polishing stability window for different over-polishing times compared to the reference example without gluconic acid.

[0136] Therefore, by comparing the polishing results with those of a reference example in which gluconic acid was not used as a chemical additive, it was found that the CMP composition containing the chemical additive ensures high TEOS and HDP film removal rates while reducing the SiN removal rate, increasing TEOS:SiN film selectivity, significantly reducing oxide trench dishing, and improving the shape of the polished pattern wafer.

[0137] Example 2 In Example 2, polishing compositions were prepared as shown in Table 5. Different weight percentages of gluconic acid, a chemical additive, were used. The pH of all compositions was approximately 5.35.

[0138] The results for various film polishing and removal speeds and TEOS:SiN selectivity are shown in Table 5 and Figure 7. [Table 5]

[0139] As shown in Table 5 and Figure 7, the SiN removal rate was consistently reduced for all compositions containing different concentrations of gluconic acid. For all compositions except the one containing 0.1% by weight gluconic acid, a high TEOS and HDP film removal rate was maintained, while a significantly higher TEOS:SiN film selectivity was obtained compared to the reference example without gluconic acid as a chemical additive. The composition containing 0.1% by weight gluconic acid showed a reduced removal rate for all tested films and an extremely low oxide:SiN selectivity.

[0140] The oxide trench dishing rate using the composition was also tested. The test results are shown in Table 6 and Figure 8. [Table 6]

[0141] As shown in Table 6 and Figure 8, the addition of 0.005 wt% gluconic acid reduced the oxide trench dishing rate by more than 32% for 100 μm and 200 μm trenches. The addition of 0.01 wt% or more gluconic acid significantly reduced the oxide trench dishing rate by at least more than 70% for all oxide trench features of different sizes.

[0142] Regarding the oxide trench loss rate (A / sec), the effects of adding a chemical additive, namely gluconic acid, at different concentrations in the polishing composition were confirmed by comparing the polishing results with those of a reference example where gluconic acid was not used as an additive.

[0143] The test results are shown in Table 7 and Figure 9, respectively. [Table 7]

[0144] As shown in Table 7 and Figure 9, the addition of 0.005 wt% gluconic acid reduced the oxide trench loss rate to at least over 16% for 1000 μm and to 38% for 100 μm and 200 μm. The addition of 0.01 wt% or more of gluconic acid was extremely effective in reducing the oxide trench loss rate to at least over 81% for all oxide trench features of different sizes.

[0145] Regarding oxide trench dishing with respect to over-polishing time, the effects of adding chemical additives, namely gluconic acid, used at different concentrations in the polishing composition were confirmed by comparing the polishing results with those of a reference example where gluconic acid was not used as an additive.

[0146] The test results are shown in Table 8 and in Figures 10, 11, and 12, respectively. [Table 8]

[0147] As shown in Table 8, Figures 10, 11, and 12, the addition of 0.0025% by weight of gluconic acid to the composition reduced oxide trench dishing and improved the over-polishing stability window. The effect became more pronounced as the gluconic acid concentration increased within the confirmed concentration range.

[0148] By comparing the polishing results with a reference example in which gluconic acid was not used as a chemical additive, it was found that even with CMP compositions containing different concentrations of chemical additives, high TEOS and HDP film removal rates were maintained while reducing the SiN removal rate, increasing TEOS:SiN film selectivity, significantly reducing oxide trench dishing, and improving the shape of the polished pattern wafer.

[0149] Example 3 In Example 3, gluconic acid was added as a chemical additive at a concentration of 0.01% by weight, and the pH conditions were varied for testing. The tested compositions and pH conditions are shown in Table 9.

[0150] Table 9 and Figure 13 show the film removal speed and TEOS:SiN selectivity. [Table 9]

[0151] As shown in Table 9 and Figure 13, compared to polishing compositions that did not use gluconic acid as a chemical additive, the SiN film removal rate was significantly reduced to at least 82% and the TEOS:SiN selectivity was increased to at least 300% at all pH conditions tested.

[0152] The effect of pH conditions on the dishing rate of oxide trench features of various sizes was investigated for compositions using 0.01% by weight of gluconic acid as a chemical additive. The results are shown in Table 10 and Figure 14. [Table 10]

[0153] As shown in Table 10 and Figure 14, when 0.01% by weight of gluconic acid was used as a chemical additive in the polishing composition, the oxide trench dishing rate was significantly reduced at all tested pH conditions compared to the polishing composition without gluconic acid as a chemical additive.

[0154] The STI CMP polishing composition according to the present invention can be used in a wide pH range, including acidic, neutral, or alkaline conditions.

[0155] The effect of pH conditions on oxide trench loss rates of various sizes was investigated for compositions using 0.01% by weight of gluconic acid as a chemical additive. The results are shown in Table 11 and Figure 15. [Table 11]

[0156] As shown in Table 11 and Figure 15, when 0.01% by weight of gluconic acid was used as a chemical additive in the polishing composition, the oxide trench loss rate was significantly reduced at all tested pH conditions compared to the polishing composition without gluconic acid as a chemical additive.

[0157] Regarding oxide trench dishing with respect to over-polishing time, the effect of the chemical additive gluconic acid, used at 0.01% and at different pH levels in the polishing composition, was confirmed by comparing it with the polishing results of a reference example in which gluconic acid was not used as an additive. The test results are shown in Table 12, Figure 16, Figure 17, and Figure 18, respectively. [Table 12]

[0158] As shown in Table 12, Figures 16, 17, and 18, when gluconic acid was used as a chemical additive at a concentration of 0.01% by weight, oxide trench dishing was significantly reduced and the over-polishing stability window was significantly improved for all oxide trench features of different sizes at all pH conditions tested, compared to the reference example without the use of gluconic acid as a chemical additive.

[0159] Example 4 In Example 4, gluconic acid, mucoic acid, or tartaric acid; ceria-coated silica composite particles were used in different compositions. A reference example of an abrasive composition without chemical additives is also shown. All compositions used bioside in an amount ranging from 0.0001% to 0.05% by weight, and deionized water. All compositions tested had the same pH of 5.3.

[0160] Table 13 shows the removal rates for various films. [Table 13]

[0161] Compared to the PECVD SiN film removal rate using a polishing composition in a reference example without additives, the PECVD SiN film removal rate was significantly reduced when gluconic acid, mucoic acid, or tartaric acid was used in addition to ceria-coated silica as an abrasive at a concentration of 0.01% by weight.

[0162] These results demonstrate that organic acids having one or two carboxylic acid groups and two or more hydroxyl groups are extremely effective as SiN removal rate reducers.

[0163] The effect of using an STI oxide polishing composition containing ceria-coated silica composite particles as an abrasive to reduce the total number of defects in polished TEOS and SiN wafers was tested.

[0164] Table 14 shows the comparison results of the total number of defects. [Table 14]

[0165] As shown in Table 14, under the same pH conditions and with the same chemical additive of 0.01% by weight of gluconic acid, the polishing composition using ceria-coated silica composite particles as polishing particles showed a significant reduction in the total number of defects in both polished TEOS and SiN films.

[0166] The results shown in Table 14 demonstrate that polishing compositions using mucilaginous acid or tartaric acid resulted in a greater reduction in the total number of defects across all test wafers compared to polishing compositions using gluconic acid.

[0167] Example 5 In Example 5, polishing compositions using gluconic acid, mucoic acid, or tartaric acid as chemical additives were tested under the same pH conditions, compared to the polishing composition in the reference example that did not use any chemical additives.

[0168] Table 15 shows the compositions tested, pH conditions, HDP film removal rate, P200 trench loss rate, and P200 trench / blanket ratio. [Table 15]

[0169] As shown in Table 15, under the same pH conditions, compositions using the same concentration of chemical additives (0.01% by weight) showed similar HDP film removal rates compared to the reference example composition without chemical additives, but significantly lower trench loss rates and trench loss rate / blanket loss rate ratios.

[0170] Over-polishing time and trench dishing were tested. The results are shown in Table 16. [Table 16]

[0171] As shown in Table 16, under the same pH conditions, compositions using the same concentration of chemical additives (0.01% by weight) showed a more significant reduction in trench dishing when an over-polishing time of 60 seconds or 120 seconds was applied.

[0172] The results shown in Table 16 demonstrate that, under different over-polishing time conditions, mucoic acid or gluconic acid are more effective chemical additives than tartaric acid in reducing trench dishing in the polishing composition.

[0173] The embodiments of the present invention described above, including the examples, are illustrative of the many forms that can be created from the present invention. Numerous other configurations can be adopted with respect to the process, and it is believed that many other materials besides those specifically disclosed in the present invention can be selected for use in the process.

Claims

1. ceria-coated inorganic metal oxide particles; 0.0006% to 0.25% by weight of a chemical additive having at least one organic carboxylic acid group, at least one carboxylic acid salt group, or at least one carboxylic acid ester group and at least two hydroxyl functional groups in the same molecule; a water-soluble solvent; and arbitrarily Biocides; pH adjuster; Including, a pH of 4 to 9; and The chemical additive has the following general molecular structure: Chemical mechanical polishing composition. [Formula 1] wherein n is selected from 2 to 12; R1, R2, R3, and R4 are the same or different atoms or the same or different functional groups, and are independently selected from hydrogen; alkyl; alkoxy; organic groups having at least one hydroxyl group; substituted organic sulfonic acids; substituted organic sulfonate salts; substituted organic carboxylic acids; substituted organic carboxylate salts; organic carboxylic acid esters; organic amine groups; metal ions selected from the group consisting of sodium ions and potassium ions; ammonium ions; and combinations thereof; and at least two of R1, R2, R3, and R4 are hydrogen atoms.

2. the ceria-coated inorganic oxide particles are in the range of 0.1 wt % to 5 wt % and are selected from the group consisting of ceria-coated colloidal silica, ceria-coated high-purity colloidal silica, ceria-coated alumina, ceria-coated titania, ceria-coated zirconia particles, and combinations thereof; The chemical-mechanical polishing composition of claim 1.

3. the aqueous solvent is selected from the group consisting of deionized (DI) water, distilled water, and alcoholic organic solvents; The chemical-mechanical polishing composition of claim 1.

4. the chemical additive is in the range of 0.0007% to 0.1% by weight; The pH of the composition is 4.5 to 7.

5. The chemical-mechanical polishing composition of claim 1.

5. the chemical additive is selected from the group consisting of tartaric acid, cholic acid, shikimic acid, mucic acid having two acid groups, asiatic acid, 2,2-bis(hydroxymethyl)propionic acid, gluconic acid, sodium gluconate, potassium gluconate, ammonium gluconate, gluconic acid methyl ester, and combinations thereof; The chemical-mechanical polishing composition of claim 1.

6. the chemical additive is selected from the group consisting of gluconic acid, gluconic acid methyl ester, gluconic acid ethyl ester, and combinations thereof; The chemical-mechanical polishing composition of claim 1.

7. ceria-coated colloidal silica particles; a chemical additive selected from the group consisting of gluconic acid, gluconates, gluconic acid alkyl esters, and combinations thereof; and water Including, The chemical-mechanical polishing composition of claim 1.

8. 0.0005% to 0.025% by weight of a biocide containing the active ingredients 5-chloro-2-methyl-4-isothiazolin-3-one and 2-methyl-isothiazolin-3-one; 0.01% to 0.5% by weight of a pH adjuster selected from the group consisting of nitric acid, hydrochloric acid, sulfuric acid, phosphoric acid, other inorganic or organic acids, and mixtures thereof for acidic pH conditions, or 0.01% to 0.5% by weight of a pH adjuster selected from the group consisting of sodium hydroxide, potassium hydroxide, ammonium hydroxide, tetraalkylammonium hydroxide, organic quaternary ammonium hydroxides, organic amines, and combinations thereof for alkaline pH conditions; further comprising at least one of The chemical-mechanical polishing composition of claim 1.

9. 1. A method of chemical mechanical polishing (CMP) a semiconductor substrate having at least one surface comprising a silicon oxide film, comprising: providing the semiconductor substrate; Preparing the polishing pad; ceria-coated inorganic metal oxide particles; 0.0006% to 0.25% by weight of a chemical additive having at least one organic carboxylic acid group, at least one carboxylic acid salt group, or at least one carboxylic acid ester group and at least two hydroxyl functional groups in the same molecule; a water-soluble solvent; and arbitrarily Biocides; pH adjuster; Including, a pH of 4 to 9; and a chemical mechanical polishing (CMP) composition wherein the chemical additive has the following general molecular structure: To prepare [Case 2] wherein n is selected from 2 to 12; R1, R2, R3, and R4 are the same or different atoms or the same or different functional groups, and are independently selected from hydrogen; alkyl; alkoxy; organic groups having at least one hydroxyl group; substituted organic sulfonic acids; substituted organic sulfonate salts; substituted organic carboxylic acids; substituted organic carboxylate salts; organic carboxylic acid esters; organic amine groups; metal ions selected from the group consisting of sodium ions and potassium ions; ammonium ions; and combinations thereof; and at least two of R1, R2, R3, and R4 are hydrogen atoms. contacting the surface of the semiconductor substrate with the polishing pad and the chemical-mechanical polishing composition; and polishing said at least one surface comprising silicon dioxide; A method for providing the above.

10. the ceria-coated inorganic oxide particles are in the range of 0.1 wt % to 5 wt % and are selected from the group consisting of ceria-coated colloidal silica, ceria-coated high-purity colloidal silica, ceria-coated alumina, ceria-coated titania, ceria-coated zirconia particles, and combinations thereof; the aqueous solvent is selected from the group consisting of deionized (DI) water, distilled water, and alcoholic organic solvents; The silicon oxide film is selected from the group consisting of chemical vapor deposition (CVD), plasma-enhanced CVD (PECVD), high-density deposition CVD (HDP), or spin-on silicon oxide films; The method of claim 9.

11. the chemical additive is in the range of 0.0007% to 0.1% by weight, and the pH of the composition is 4.5 to 7.5; The method of claim 9.

12. the chemical additive is selected from the group consisting of tartaric acid, cholic acid, shikimic acid, mucic acid having two acid groups, asiatic acid, 2,2-bis(hydroxymethyl)propionic acid, gluconic acid, sodium gluconate, potassium gluconate, ammonium gluconate, gluconic acid methyl ester, and combinations thereof; The method of claim 9.

13. the composition comprising: ceria-coated colloidal silica particles; 0.0007% to 0.1% by weight of the chemical additive selected from the group consisting of gluconic acid, gluconates, gluconate alkyl esters, and combinations thereof; and water. The method of claim 9.

14. the semiconductor substrate further having a silicon nitride surface; Silicon oxide:silicon nitride removal selectivity is greater than 25; The method of claim 9.

15. 1. A system for chemical mechanical polishing (CMP) a semiconductor substrate having at least one surface comprising a silicon oxide film, comprising: a. the semiconductor substrate; b. a chemical mechanical polishing (CMP) composition 1) Ceria-coated inorganic metal oxide particles; 2) 0.0006% to 0.25% by weight of a chemical additive having at least one organic carboxylic acid group, at least one carboxylic acid salt group, or at least one carboxylic acid ester group and at least two hydroxyl functional groups in the same molecule; 3) a water-soluble solvent; and 4) Arbitrarily 5) Biocides; 6) pH adjusters; Including, pH is 4 to 9, and The chemical additive has the following general molecular structure: chemical mechanical polishing composition [C3] wherein n is selected from 2 to 12; R1, R2, R3, and R4 are the same or different atoms or the same or different functional groups, and are independently selected from hydrogen; alkyl; alkoxy; organic groups having at least one hydroxyl group; substituted organic sulfonic acids; substituted organic sulfonate salts; substituted organic carboxylic acids; substituted organic carboxylate salts; organic carboxylic acid esters; organic amine groups; metal ions selected from the group consisting of sodium ions and potassium ions; ammonium ions; and combinations thereof; and at least two of R1, R2, R3, and R4 are hydrogen atoms. c.Scouring pad; Equipped with the at least one surface comprising the silicon oxide film is contacted with the polishing pad and the chemical-mechanical polishing composition; system.

16. the ceria-coated inorganic oxide particles are in the range of 0.1 wt % to 5 wt % and are selected from the group consisting of ceria-coated colloidal silica, ceria-coated high-purity colloidal silica, ceria-coated alumina, ceria-coated titania, ceria-coated zirconia particles, and combinations thereof; the aqueous solvent is selected from the group consisting of deionized (DI) water, distilled water, and alcoholic organic solvents; The silicon oxide film is selected from the group consisting of chemical vapor deposition (CVD), plasma-enhanced CVD (PECVD), high-density deposition CVD (HDP), or spin-on silicon oxide films; 16. The system of claim 15.

17. the chemical additive is in the range of 0.0007% to 0.1% by weight, and the pH of the composition is 4.5 to 7.5; 16. The system of claim 15.

18. the chemical additive is selected from the group consisting of tartaric acid, cholic acid, shikimic acid, mucic acid having two acid groups, asiatic acid, 2,2-bis(hydroxymethyl)propionic acid, gluconic acid, sodium gluconate, potassium gluconate, ammonium gluconate, gluconic acid methyl ester, and combinations thereof; 16. The system of claim 15.

19. the composition comprising: ceria-coated colloidal silica particles; 0.0007% to 0.1% by weight of the chemical additive selected from the group consisting of gluconic acid, gluconates, gluconate alkyl esters, and combinations thereof; and water.

16. The system of claim 15.

20. the semiconductor substrate further having a silicon nitride surface; Silicon oxide:silicon nitride removal selectivity is greater than 25; 16. The system of claim 15.