Manufacturing method of magnetoplumbite-type hexagonal ferrite magnetic powder and magnetoplumbite-type hexagonal ferrite magnetic powder
By adding metal chloride during the production of magnetoplumbite-type hexagonal ferrite magnetic powder and controlling its composition and crystallite diameter, the material achieves effective radio wave absorption in the 28 GHz band, addressing the lack of suitable materials for 5G communication.
Patent Information
- Application Number
- JP2020127712
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-28
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-07-28
AI Technical Summary
Existing materials do not have sufficient radio wave absorption ability in the 28 GHz band, which is essential for emerging applications like 5G communication in portable devices.
A method for producing magnetoplumbite-type hexagonal ferrite magnetic powder by adding metal chloride during firing, controlling the composition and crystallite diameter, and incorporating it into a resin to form a radio wave absorber.
The resulting magnetoplumbite-type hexagonal ferrite magnetic powder exhibits excellent radio wave absorption ability in the 28 GHz band, achieving transmission attenuation of 10 dB or more.
Smart Images

Figure 0007580961000003 
Figure 0007580961000004 
Figure 0007580961000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing magnetoplumbite-type hexagonal ferrite magnetic powder and to a magnetoplumbite-type hexagonal ferrite magnetic powder obtained thereby. [Background technology]
[0002] In recent years, with the advancement of information and communication technology, radio waves in the GHz band have come to be used for various purposes. Examples of applications using such high-frequency technology include mobile phones, wireless LAN, satellite broadcasting, intelligent road transport systems, non-stop automatic toll collection systems (ETC), and automated highway systems (AHS). As the use of radio waves in the high-frequency range becomes more diverse, there are concerns about failures, malfunctions, and malfunctions due to interference between electronic components, and EMC measures become important. One effective method is to use radio wave absorbers to absorb unnecessary radio waves and prevent them from being reflected or entering.
[0003] Patent Document 1 describes AFe (12-x) (B1 0.5 B2 0.5 ) x O 19 The document discloses a radio wave absorber using magnetoplumbite-type hexagonal ferrite represented by the formula (1) having an absorption peak at 15 GHz, etc. The document also describes that radio wave absorption characteristics can be obtained independent of the thickness of the radio wave absorber. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2006-137653 A Summary of the Invention [Problem to be solved by the invention]
[0005] As mentioned above, frequency bands are allocated according to various applications, and radio wave absorbers corresponding to each frequency band are being developed. In particular, in the fifth generation mobile communication system (5G), communication is now performed through high frequency bands of several tens of gigahertz, and these have begun to be used in mobile devices such as smartphones. For new bands to be used, it is essential to utilize radio waves in frequency bands that have not been used before, including the 28 GHz band, and the development of corresponding radio wave absorbers is also being considered at the same time. However, materials manufactured using the same manufacturing method as existing materials do not provide the desired characteristics, and no materials with sufficient radio wave absorption capacity at frequencies in the 28 GHz band have been obtained so far.
[0006] Therefore, in order to solve the above-mentioned problems, the present invention aims to provide a method for producing magnetoplumbite-type hexagonal ferrite magnetic powder suitable for use as a material for a radio wave absorber having excellent radio wave absorption capacity in the 28 GHz band, and to provide the magnetoplumbite-type hexagonal ferrite magnetic powder obtained by the method. [Means for solving the problem]
[0007] The present inventors have conducted extensive research to solve the above problems. The resonance frequency of a radio wave absorber is a value specific to the composition, and magnetoplumbite-type hexagonal ferrite magnetic powder also exhibits different resonance frequencies depending on the substitution elements and the substitution ratios. (12-x) (B1 0.5 B2 0.5 ) x O 19 It was confirmed that the magnetoplumbite-type hexagonal ferrite magnetic powder represented by the formula (1) has a resonant frequency in the 28 GHz band when metal chloride is added during sintering. It was also confirmed that the magnetoplumbite-type hexagonal ferrite magnetic powder thus manufactured can have a large crystallite diameter, and therefore can achieve excellent radio wave absorption performance in the 28 GHz band even with the same composition. That is, the gist of the present invention is as follows.
[0008] (1) A method for producing magnetoplumbite-type hexagonal ferrite magnetic powder, comprising the steps of: a raw material mixing step of mixing raw material powders containing iron, barium, metal element B1, metal element B2, and metal chloride to obtain a raw material mixture; A firing step of firing the raw material mixture to obtain a fired product; A pulverization step of pulverizing the sintered product to obtain the magnetoplumbite-type hexagonal ferrite magnetic powder, The magnetoplumbite-type hexagonal ferrite magnetic powder has the composition formula BaFe (12-x) (B1 0.5 B2 0.5 ) x O 19 wherein the metal element B1 is one or two selected from the group consisting of Ti and Zr, the metal element B2 is one or more selected from the group consisting of Co, Mn, Cu, Mg, Zn and Ni, and a composition ratio x in the composition formula is 0.1 to 2.6.
[0009] (2) The method for producing the magnetoplumbite-type hexagonal ferrite magnetic powder according to (1) above, wherein the composition ratio x is 1.0 to 1.4.
[0010] (3) The method for producing magnetoplumbite-type hexagonal ferrite magnetic powder according to (1) or (2), wherein in the firing step, the mass of Cl per unit volume in the gas retention space is 5.0 g / L or more.
[0011] (4) A method for producing a radio wave absorber, comprising kneading the magnetoplumbite-type hexagonal ferrite magnetic powder obtained by the method for producing a radio wave absorber according to any one of (1) to (3) above with a resin, and then molding the mixture.
[0012] (5) Formula: BaFe (12-x) (B1 0.5 B2 0.5 ) x O 19 It is expressed as The metal element B1 is one or two selected from the group consisting of Ti and Zr, The metal element B2 is one or more selected from the group consisting of Co, Mn, Cu, Mg, Zn, and Ni, The composition ratio x in the composition formula is 0.1 to 2.6, The crystallite size is 100 nm or more. Magnetoplumbite type hexagonal ferrite magnetic powder.
[0013] (6) The magnetoplumbite-type hexagonal ferrite magnetic powder according to (4) above, wherein the composition ratio x is 1.0 to 1.4.
[0014] (7) The magnetoplumbite-type hexagonal ferrite magnetic powder according to (5) or (6), wherein the crystallite size is 120 nm or more.
[0015] (8) A radio wave absorber comprising the magnetoplumbite hexagonal ferrite magnetic powder according to any one of (5) to (7) above and a resin. Effect of the Invention
[0016] According to the present invention, it is possible to provide magnetoplumbite-type hexagonal ferrite magnetic powder suitable for use as a material for a radio wave absorber having excellent radio wave absorbing ability in the 28 GHz band, and a method for producing the same. [Brief description of the drawings]
[0017] [Figure 1] FIG. 2 is a diagram illustrating a manufacturing flow according to an embodiment of the present invention. [Figure 2A] FIG. 2 is a diagram showing the state of the gas retention space when the lid of the firing container is not placed in the firing process according to one embodiment of the present invention. [Figure 2B] FIG. 2 is a diagram showing the state of the gas retention space when the lid of the firing container is closed in the firing process according to one embodiment of the present invention. [Diagram 3]1 is a profile showing the transmission attenuation S21 in the frequency range of 27 GHz to 30 GHz in Examples 1 to 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The crystallite diameter in this specification is the crystallite diameter Dx that can be determined by X-ray diffraction measurement, and X-ray diffraction measurement was also adopted in the examples described below. Note that the crystallite diameter Dx indicates the size of a single crystal in the structure of the magnetoplumbite-type hexagonal ferrite magnetic powder, and is different from the particle diameter that indicates the size of the particle. In addition, the composition ratio of the obtained magnetoplumbite-type hexagonal ferrite magnetic powder was determined by ICP (inductively coupled plasma) atomic emission spectrometry.
[0019] A method for producing magnetoplumbite-type hexagonal ferrite magnetic powder according to the present invention will be described with reference to Fig. 1. This method includes at least a raw material mixing step of mixing raw material powders each containing iron, barium, metal element B1, metal element B2, and metal chloride to obtain a raw material mixture, and a firing step of firing the raw material mixture in a firing furnace to obtain a fired product. Each component and step will be described in detail below.
[0020] (Raw material mixing process) First, the raw material mixing process is carried out with the composition formula BaFe (12-x) (B1 0.5 B2 0.5 ) x O 19 As the raw material of the magnetoplumbite-type hexagonal ferrite magnetic powder represented by the formula (1), raw material powders containing iron, barium, metal element B1, metal element B2, and metal chlorides are mixed to obtain a raw material mixture. The raw material powders are not particularly limited, but powders such as BaCO3, Fe2O3, TiO2, ZrO2, MnO2, CuO, NiO, MgO, Co3O4, and ZnO can be used, and powders such as BaCl2 or BaCl2·2H2O can be used as metal chlorides. The method of mixing the raw material powders is not particularly limited, and mixing can be performed using a known mixing device such as a Henschel mixer.
[0021] In addition, a step of granulating the obtained raw material mixture to obtain a molded body may be provided. The granulation method is not particularly limited, and the molded body can be molded into pellets by any method. If the molded body contains moisture, a drying step may be further provided thereafter.
[0022] (Firing process) Next, the obtained raw material mixture is fired at a temperature of 1150 to 1400 ° C. in an arbitrary firing furnace. At this time, it is preferable to fire the raw material mixture with Cl content in an amount such that the Cl concentration in the atmosphere in contact with the raw material mixture is 0.5 g / L or more, and more preferably, it is fired with an amount of 5.0 g / L to 10.0 g / L. Here, refer to FIG. 2A. For example, when using a box-type firing furnace 20, the raw material can be filled into a firing container 10. Also, refer to FIG. 2B, by putting a lid 12 on the firing container 10, the gas retention space during firing can be the firing container space 15 of the firing container 10. Also, when the raw material is directly charged into the firing furnace, the furnace space becomes the gas retention space. The firing atmosphere is preferably an oxidizing atmosphere, and the oxidizing atmosphere is preferably an atmosphere such as air, oxygen, a mixed gas of oxygen and nitrogen, or a mixed gas of oxygen and rare gas.
[0023] (Crushing process) Next, the obtained sintered product is pulverized in a pulverization step to obtain magnetoplumbite-type hexagonal ferrite magnetic powder. In the pulverization step, coarse pulverization and fine pulverization may be performed. Here, coarse pulverization refers to disintegrating the sintered product, and any pulverization method such as impact pulverization using a hammer mill can be used. In addition, fine pulverization refers to further reducing the sintered product after coarse pulverization to a finer state, and any method such as wet pulverization using an attritor can be used. The slurry after wet pulverization is subjected to solid-liquid separation and drying by any method to obtain magnetoplumbite-type hexagonal ferrite magnetic powder.
[0024] Furthermore, the magnetoplumbite-type hexagonal ferrite magnetic powder obtained in the pulverization step may be optionally subjected to an annealing treatment, and can be heat-treated at a temperature of 900° C. to 1000° C. in the air by any heat treatment method.
[0025] Here, the technical significance of adding a metal chloride and then firing in this embodiment will be described in detail with reference to FIGS. 2A and 2B.
[0026] <Addition of metal chlorides> In the manufacturing method according to the present embodiment, a metal chloride is added to the raw material powder in the mixing step. Although the theoretical background of adding a metal chloride has not been elucidated, and the present invention is not bound by theory, the inventors believe that the effect of the present invention is due to the following reasons. That is, when BaCl2 is added as a metal chloride to the raw material and then fired, BaCl2 vaporizes from the raw material mixture in the firing step, and the Cl concentration in the atmosphere in contact with the raw material mixture increases. In addition, since vaporization and liquefaction are equilibrium reactions, if the Cl concentration in the atmosphere increases, it becomes difficult for solid BaCl2 to vaporize (volatilize) further, and it is considered that the amount of BaCl2 remaining in the raw material mixture without volatilization increases. And, it is considered that this BaCl2 effectively functions as a solution (flux) in the raw material mixture, so that the crystals of the magnetoplumbite-type hexagonal ferrite magnetic powder grow and the crystallite diameter Dx increases. In addition, the content of the metal chloride (e.g., BaCl2·2H2O) powder in the raw powder of the magnetoplumbite type hexagonal ferrite magnetic powder is preferably 0.1 mass% or more (in terms of BaCl2 in the case of BaCl2·2H2O powder) from the viewpoint of crystal growth of the magnetoplumbite type hexagonal ferrite magnetic powder. On the other hand, if the content of the metal chloride powder in the raw powder of the magnetoplumbite type hexagonal ferrite magnetic powder is too high, it is not preferable because Cl remains in the magnetoplumbite type hexagonal ferrite magnetic powder. Therefore, the content of the metal chloride in the raw powder is preferably 20 mass% or less, and more preferably 0.5 to 10 mass%. In addition, as the metal chloride, any chloride of Ba, Sr, or Pb can be used from the viewpoint of an element that can enter the divalent metal site of the magnetoplumbite type hexagonal ferrite magnetic powder.
[0027] <Gas retention space> As described above, in the present invention, the firing atmosphere in the firing step is a characteristic part of the present invention. In the firing step, the gas retention space refers to a space in which the raw material mixture exists during firing and does not substantially exchange gas directly with the outside. When gas that affects the reaction is generated during firing, the size of this gas retention space will change the gas concentration of the atmosphere to which the raw material mixture is substantially exposed. That is, even with the same amount of gas generated, if the gas retention space is large, the gas concentration will be small, and conversely, if the gas retention space is small, the gas concentration will be large. Therefore, in the present embodiment described in FIG. 2A, when the firing container 10 is filled with the molded body 30 obtained by granulating the raw material mixture without the lid 12 and fired in the box-type firing furnace 20, the space 25 in the box-type firing furnace becomes the gas retention space, and when the firing is performed with the lid 12 closed as shown in FIG. 2B, the space 15 in the firing container 10 becomes the gas retention space. In addition, by limiting the gas retention space, the amount of Cl in the gas retention space can be increased without changing the content of metal chloride in the molded body 30. For this reason, reducing the gas retention space is an especially effective measure when a high metal chloride content in the raw material powder is undesirable. The gas retention space may be a space that is not open to the atmosphere and allows heat treatment in a chloride atmosphere during firing, so the shape of the furnace used in the firing step, the heat treatment method, and the method of filling the raw material mixture are not particularly limited. For example, when a large firing furnace is used and the raw material mixture is directly filled into the furnace, the space inside the furnace can be called the gas retention space.
[0028] The magnetoplumbite-type hexagonal ferrite magnetic powder obtained in this manner has excellent radio wave absorbing properties and is suitable as a material for radio wave absorbers for the millimeter wave band of 28 GHz.
[0029] (Making of radio wave absorbers) Moreover, the obtained magnetoplumbite hexagonal ferrite magnetic powder can be kneaded with a resin to produce a radio wave absorber. This radio wave absorber can be formed into various shapes depending on the application, but when producing a sheet-shaped radio wave absorber (radio wave absorber sheet), the radio wave absorber material (kneaded product) obtained by kneading the magnetoplumbite hexagonal ferrite magnetic powder with a resin may be rolled to a desired thickness (preferably 0.1 to 4.0 mm, more preferably 0.2 to 2.5 mm) using a rolling roll or the like.
[0030] Next, the magnetoplumbite-type hexagonal ferrite magnetic powder obtained by the above-mentioned production method will be described.
[0031] The magnetoplumbite-type hexagonal ferrite magnetic powder according to the present invention has the composition formula BaFe (12-x) (B1 0.5 B2 0.5 ) x O 19 In the composition formula, the metal element B1 is one or two selected from the group consisting of Ti and Zr, the metal element B2 is one or more selected from the group consisting of Co, Mn, Cu, Mg, Zn and Ni, the composition ratio x is 0.1 to 2.6, and the crystallite size is 100 nm or more.
[0032] <Particle size and crystallite size> As mentioned above, the crystallite diameter of the magnetoplumbite hexagonal ferrite magnetic powder according to the present invention can be determined by X-ray diffraction measurement. Here, the crystallite diameter Dx is 100 nm or more, and preferably 120 nm to 150 nm. The particle diameter of the magnetoplumbite hexagonal ferrite magnetic powder can be measured by a laser diffraction type particle size distribution measuring device, and the volume-based cumulative 50% particle diameter (D50) is preferably 5.5 μm or less. Since it is possible to thin the radio wave absorber sheet using the magnetoplumbite hexagonal ferrite magnetic powder, the volume-based cumulative 50% particle diameter (D50) is more preferably in the range of 1.0 μm to 5.2 μm, and most preferably in the range of 1.0 μm to 5.0 μm.
[0033] The BET specific surface area of this magnetoplumbite hexagonal ferrite magnetic powder is 2.0m 2 / g or less, and 0.5m 2 / g~2.0m 2 / g. The product (BET × D50) of the BET specific surface area and the cumulative 50% particle diameter on a volume basis (D50) is preferably 5.0 μm m 2 / g or less, and 4.5 μm m 2 / g or less, and more preferably 1.0 μm m 2 / g~4.5μm m 2 / g. It is most preferable that this product (BET × D50) is 5.0 μm m 2 / g or less, the transmission attenuation of the radio wave absorber sheet using the magnetoplumbite-type hexagonal ferrite magnetic powder can be increased (radio wave absorption ability can be increased) while maintaining the coercive force Hc of the magnetoplumbite-type hexagonal ferrite magnetic powder at a high level. In addition, the peak particle size (the most frequent particle size) in the particle size distribution of the magnetoplumbite-type hexagonal ferrite magnetic powder is preferably 10.0 μm or less, more preferably 8.0 μm or less, and most preferably 1.0 μm to 7.0 μm.
[0034] (Production and evaluation of radio wave absorbers) Moreover, a radio wave absorber can be manufactured by kneading the magnetoplumbite hexagonal ferrite magnetic powder of the above-mentioned embodiment with a resin. This radio wave absorber can be formed into various shapes depending on the application, but when manufacturing a sheet-shaped radio wave absorber (radio wave absorber sheet), the radio wave absorber material (kneaded product) obtained by kneading the magnetoplumbite hexagonal ferrite magnetic powder with a resin may be rolled to a desired thickness (preferably 0.1 to 4.0 mm, more preferably 0.2 to 2.5 mm) using a rolling roll or the like. Moreover, the content of the magnetoplumbite hexagonal ferrite magnetic powder in the radio wave absorber material (kneaded product) is preferably 70 to 95 mass % in order to obtain a radio wave absorber with excellent radio wave absorbing ability in the 28 GHz band. Moreover, the content of the resin in the radio wave absorber material (kneaded product) is preferably 5 to 30 mass % in order to sufficiently disperse the magnetoplumbite hexagonal ferrite magnetic powder in the radio wave absorber material (kneaded product). The total content of magnetoplumbite-type hexagonal ferrite magnetic powder and resin in the electromagnetic wave absorber material (kneaded material) is preferably 99% by mass or more. In order to have excellent electromagnetic wave absorbing ability as an electromagnetic wave absorber, the transmission attenuation at the relevant frequency is preferably 10 dB or more, and more preferably 12 dB or more. EXAMPLES
[0035] Hereinafter, examples of the magnetoplumbite-type hexagonal ferrite magnetic powder and the method for producing the same according to the present invention will be described in detail.
[0036] [Example 1] First, 1484g of BaCO3 with a purity of 99% by mass, 6491g of Fe2O3 with a purity of 99% by mass, 358g of TiO2 with a purity of 99.9% by mass, 180g of Co3O4 with a purity of 99.9% by mass, 182g of ZnO with a purity of 99.9% by mass, and 222g of BaCl2·2H2O with a purity of 99% by mass were weighed as raw material powders. Next, all the weighed raw material powders were mixed in a Henschel mixer, and then further mixed by a dry method using a vibration mill. The mass of Cl in this raw material powder was 64g. The raw material mixture thus obtained was granulated into pellets to obtain a compact, which had a width of 310 mm, depth of 310 mm, height of 100 mm, and internal base area of 300 mm x 300 mm = 900 cm. 2 And the internal volume: 300mm x 300mm x 100mm = 9000cm 3 A sintering container was prepared, and 9000 g of the obtained molded body was filled in the sintering container. The prepared sintering container was covered and placed in a box-shaped sintering furnace with a width of 500 mm, a depth of 530 mm, a height of 720 mm, and an internal volume of 191 L in room temperature air, and sintered at 1279 ° C for 4 hours to obtain a sintered product. Here, the mass of Cl converted as the amount of Cl in the chloride in the molded body filled in the sintering container was 64 g, and the amount of Cl in the gas retention space was the mass (g) of Cl in the molded body relative to the internal volume (L) of the sintering container, which was 7.17 g / L. Then, after pulverizing this sintered product with a hammer mill, the obtained coarse powder was wet-pulverized for 10 minutes with an attritor using water as a solvent. The obtained slurry was subjected to solid-liquid separation, and the obtained cake was dried and crushed to obtain magnetoplumbite-type hexagonal ferrite magnetic powder (hereinafter simply referred to as "magnetic powder"). It should be noted that it was confirmed by a powder X-ray diffraction apparatus as described later that the obtained magnetic powder was magnetoplumbite-type hexagonal ferrite.
[0037] For the magnetic powder thus obtained, the BET specific surface area, particle size distribution, and crystallite diameter Dx were determined by X-ray diffraction (XRD) measurement.
[0038] The BET specific surface area of the magnetic powder was measured by the BET single point method using a specific surface area measuring device (Macsorb model-1210 manufactured by Mountec Co., Ltd.). As a result, the BET specific surface area of the magnetic powder was 0.87 m 2 / g.
[0039] The particle size distribution of the magnetic powder was measured by dry dispersion at a dispersion pressure of 1.7 bar using a laser diffraction particle size distribution analyzer (HELOS&RODOS, manufactured by JEOL Ltd.). The volume-based cumulative 50% particle size (D50) was calculated as the average particle size and found to be 4.99 μm. The product of the BET specific surface area and the volume-based cumulative 50% particle size (D50) was 4.35 μm m. 2 / g.
[0040] The X-ray diffraction measurement of the magnetic powder was carried out by powder X-ray diffraction method (XRD) using a powder X-ray diffractometer (Rigaku Corporation horizontal multipurpose X-ray diffractometer Ultima IV) with a CuKα radiation source, a tube voltage of 40 kV, a tube current of 40 mA, and a measurement range of 2θ = 10° to 75°. As a result of this X-ray diffraction measurement, it was confirmed that the obtained magnetic powder was magnetoplumbite-type hexagonal ferrite.
[0041] The composition of the magnetic powder obtained can be measured by any method, but in the present invention, the composition was analyzed by an inductively coupled plasma emission spectrometer (ICP-720ES manufactured by Agilent Technologies). The obtained composition ratio is consistent with the amount estimated from the ratio of the charged amounts, and the composition formula is BaFe (12-x) (Ti 0.5 Co 0.25 Zinc 0.25 )xO 19 The composition was expressed by (x=1.20). The same results were obtained in Examples 2 to 4 described below.
[0042] Here, the crystallite diameter Dx of the magnetic powder was calculated by Scherrer's formula (Dx=Kλ / βcosθ). In this formula, Dx is the size of the crystallite diameter (angstroms), λ is the wavelength of the measured X-ray (angstroms), β is the spread of the diffraction line due to the size of the crystallite (rad) (expressed using half-width), θ is the Bragg angle of the diffraction angle (rad), and K is the Scherrer constant (K=0.94). Note that the calculation used peak data of the (114) plane at a diffraction angle 2θ=34.0°-34.8°. As a result, the crystallite diameter Dx calculated from the (114) plane of the magnetic powder was 123.3 nm.
[0043] The magnetic properties of the magnetic powder were evaluated by measuring the BH curve at an applied magnetic field of 1193 kA / m (15 kOe) using a vibrating sample magnetometer (VSM) (VSM-7P manufactured by Toei Kogyo Co., Ltd.), and evaluating the coercive force Hc, saturation magnetization σs, and squareness ratio SQ. The results were: coercive force Hc was 31 kA / m (393 Oe), saturation magnetization σs was 63.9 Am 2 / kg, and the squareness ratio SQ was 0.186.
[0044] (Evaluation of radio wave absorption characteristics) The magnetic powder thus obtained was kneaded with nitrile rubber (NBR, N215SL manufactured by JRS) as a polymer base material so that the content was 80 mass %, to produce a radio wave absorber material (kneaded material). Further, this radio wave absorber material was rolled to a thickness of 2 mm with a rolling roll to obtain a radio wave absorber sheet.
[0045] The radio wave absorption characteristics of the obtained radio wave absorber sheet were measured using a free space measurement device (manufactured by Keycom Corporation) and a vector network analyzer (ME7838A manufactured by Anritsu Corporation). As a result, when the strength of the electromagnetic wave transmitted by the S21 parameter according to the free space method was measured as the electromagnetic absorption characteristics, the transmission attenuation was 13.1 dB at a frequency of 28 GHz, and the transmission attenuation was 12.4 dB at a frequency of 30 GHz.
[0046] [Example 2] A magnetic powder was produced under the same conditions as in Example 1, except that the magnetic powder obtained in Example 1 was further annealed at a temperature of 950° C. for 1 hour, and evaluated under the same conditions as in Example 1. The evaluation results are shown in Table 2.
[0047] [Example 3] Magnetic powder was produced under the same conditions as in Example 1, except that 2000 g of the green body obtained by granulating the raw material mixture described in Example 1 was packed into a sintering vessel and sintered without a lid. Therefore, the mass of Cl converted as the amount of Cl in chlorides in the green body packed into the sintering vessel is 14 g, and the amount of Cl in the gas retention space is the mass (g) of Cl in the green body relative to the internal volume (L) of the sintering furnace, which is 0.08 g / L. The evaluation results are shown in Table 2.
[0048] [Example 4] A magnetic powder was produced under the same conditions as in Example 3, except that the magnetic powder obtained in Example 3 was further annealed at a temperature of 950° C. for 1 hour, and evaluated under the same conditions as in Example 1. The evaluation results are shown in Table 2.
[0049] The production conditions and characteristics of the magnetic powder obtained in these examples and the characteristics of the radio wave absorber sheet are shown in Tables 1 and 2.
[0050] [Table 1]
[0051] [Table 2]
[0052] From the results of Table 2 and Figure 3, it can be seen that Examples 1 to 4 have excellent radio wave absorption properties of 10 dB or more in the transmission attenuation at both 28 GHz and 30 GHz. In addition, Examples 1 and 2, which were fired with a lid, have a larger transmission attenuation at 28 GHz to 30 GHz than Examples 3 and 4, which were not fired with a lid during the firing process. Considering this together with the tendency of the crystallite size, it can be considered that in Examples 1 and 2, firing with a lid increases the amount of Cl in the gas retention space, which increases the crystallite size and increases the attenuation. [Industrial Applicability]
[0053] According to the present invention, it is possible to provide magnetoplumbite-type hexagonal ferrite magnetic powder suitable for use as a material for a radio wave absorber having excellent radio wave absorbing ability in the 28 GHz band, and a method for producing the same. [Explanation of symbols]
[0054] 10. Baking container 12 Lid 15. Space inside the firing vessel 20 Box-type firing furnace 25 Box-type kiln interior space 30 Molded body
Claims
1. A method for producing magnetoplumbite-type hexagonal ferrite magnetic powder, comprising the steps of: a raw material mixing step of mixing raw material powders containing iron, barium, metal element B1, metal element B2, and metal chloride to obtain a raw material mixture; A firing step of firing the raw material mixture to obtain a fired product; A pulverization step of pulverizing the sintered product to obtain the magnetoplumbite-type hexagonal ferrite magnetic powder, The magnetoplumbite type hexagonal ferrite magnetic powder has the composition formula BaFe (12-x) (B1 0.5 B2 0.5 ) x O 19 wherein the metal element B1 is one or two selected from the group consisting of Ti and Zr, the metal element B2 is one or more selected from the group consisting of Co, Mn, Cu, Mg, Zn and Ni, and the composition ratio x in the composition formula is 0.1 to 2.6; A method for producing magnetoplumbite-type hexagonal ferrite magnetic powder, characterized in that in the firing step, a sintering container in which the raw material mixture is filled is covered before firing.
2. The method for producing magnetoplumbite-type hexagonal ferrite magnetic powder according to claim 1, wherein the composition ratio x is 1.0 to 1.
4.
3. 3. The method for producing magnetoplumbite-type hexagonal ferrite magnetic powder according to claim 1, wherein in the firing step, the mass of Cl per unit volume in the gas retention space is 5.0 g / L or more.
4. A method for producing a radio wave absorber, comprising kneading the magnetoplumbite-type hexagonal ferrite magnetic powder obtained by the method according to any one of claims 1 to 3 with a resin, and then molding the mixture.
5. Formula: BaFe (12-x) (B1 0.5 B2 0.5 ) x O 19 It is expressed as The metal element B1 is one or two selected from the group consisting of Ti and Zr, The metal element B2 is one or more selected from the group consisting of Co, Mn, Cu, Mg, Zn, and Ni, The composition ratio x in the composition formula is 1.0 to 1.4, The crystallite size is 120 nm or more. Magnetoplumbite type hexagonal ferrite magnetic powder.
6. A radio wave absorber comprising the magnetoplumbite hexagonal ferrite magnetic powder according to claim 5 and a resin.
Citation Information
Patent Citations
Hexagonal ferrite magnetic body for magnetic recording and its manufacture
JP1986136923A
High density and high output recording medium of magnetoplumbite with coexisting magnetic element
JP1990033723A
Production of ferrite material
JP1996026731A
Radio wave absorber
JP1999354972A
Magnetic recording medium
JP2003228811A