Sheet for absorbent article and absorbent article including same

The laminated nonwoven fabric sheet with an uneven surface and nanofiber layer addresses the issue of leak-proofing in absorbent articles, ensuring effective liquid containment during movement by repelling liquids with low surface tension.

JP7581111B2Active Publication Date: 2024-11-12KAO CORP
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2021059734
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-31
Publication Date
2024-11-12
Estimated Expiration
2041-03-31

AI Technical Summary

Technical Problem

Existing nonwoven fabrics used in absorbent articles do not provide sufficient leak-proof properties when the wearer moves, leading to potential liquid leakage.

Method used

A sheet for absorbent articles is designed with a laminated structure of nonwoven fabric layers, featuring an uneven surface with convex portions and concave portions, and includes a nanofiber layer to enhance water repellency, specifically against liquids with a surface tension of 60 mN/m or lower.

Benefits of technology

The sheet exhibits high leakproof properties, effectively preventing liquid seepage even when the wearer moves, by combining an uneven structure with a nanofiber layer to repel liquids with low surface tension.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581111000002
    Figure 0007581111000002
  • Figure 0007581111000003
    Figure 0007581111000003
  • Figure 0007581111000004
    Figure 0007581111000004
Patent Text Reader

Abstract

To provide a high leakproof sheet for absorbent articles regardless of being constituted of a nonwoven fabric.SOLUTION: A sheet 10 for absorbent articles is formed by laminating a plurality of nonwoven fabric layers. The absorbent article sheet 10 includes at least one surface 21 having an uneven structure. The absorbent article sheet 10 has water repellency with respect to liquid with surface tension of 60 mN / m. The width W of a projection part 11 in the uneven structure is preferably 0.5 mm or more and 8 mm or less. The nonwoven fabric layer preferably includes a nanofiber layer 14 using a fiber with a fiber diameter of 1 μm or less as a constituent fiber. It is preferable that the nanofiber layer 14 has an uneven structure.SELECTED DRAWING: Figure 7
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a sheet for absorbent articles. The present invention also relates to an absorbent article provided with the sheet for absorbent articles. [Background technology]

[0002] There is a known technology for using a nonwoven fabric having an uneven surface as a component of an absorbent article. For example, Patent Document 1 describes a laminated material composed of a first substantially non-stretchable layer and a second layer. The second layer and the first layer are attached by a plurality of spaced adhesive regions. As a result, the laminated material has a plurality of adhesive regions and non-adhesive regions, and a bulky pillow portion is formed in the laminated material. This laminated material is used as a back sheet of an absorbent article.

[0003] Patent Document 2 describes a method of forming a honeycomb pattern (hexagonal concave pattern) by embossing a spunbond-meltblown-meltblown-spunbond nonwoven fabric, with the center of the pattern raised. This nonwoven fabric is used as a leg cuff for an absorbent article. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 6-255006 [Patent Document 2] JP 2004-129810 A Summary of the Invention [Problem to be solved by the invention]

[0005] As described above, the nonwoven fabrics described in Patent Documents 1 and 2 are used as components of absorbent articles that require leakproofing. However, the nonwoven fabrics described in these documents do not have sufficient leakproofing properties in situations where liquid leakage is likely to occur, such as when a wearer moves while wearing the absorbent article. SUMMARY OF THE PRESENT EMBODIMENTS Accordingly, an object of the present invention is to provide a sheet for absorbent articles which can overcome the above-mentioned drawbacks of the prior art. [Means for solving the problem]

[0006] The present invention relates to a sheet for absorbent articles comprising a plurality of nonwoven fabric layers laminated together, At least one surface of the sheet has a concave-convex structure, The present invention provides a sheet for absorbent articles that has water repellency against liquids with a surface tension of 60 mN / m. Effect of the Invention

[0007] The sheet for absorbent articles of the present invention is highly leak-proof despite being made of a nonwoven fabric, and therefore liquid is less likely to seep through the sheet for absorbent articles even if a wearer moves around while wearing an absorbent article equipped with the sheet for absorbent articles. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is an explanatory diagram showing the width, pitch and height of protrusions in an absorbent article sheet of the present invention. [Diagram 2] FIG. 2 is a perspective view showing one embodiment of the sheet for absorbent articles of the present invention. [Diagram 3] FIG. 3 is a perspective view showing another embodiment of the sheet for absorbent articles of the present invention. [Figure 4] 4(a) to (c) are schematic diagrams showing the cross-sectional structure in the thickness direction of the absorbent article sheet of the present invention. [Diagram 5] FIG. 5 is a schematic diagram showing a cross-sectional structure in the thickness direction of the sheet for absorbent articles of the present invention. [Figure 6] 6(a) and (b) are schematic diagrams showing the cross-sectional structure in the thickness direction of the sheet for absorbent articles of the present invention. [Figure 7] 7(a) and (b) are schematic diagrams showing the cross-sectional structure in the thickness direction of the sheet for absorbent articles of the present invention. [Figure 8] FIG. 8 is a schematic diagram showing the cross-sectional structure in the thickness direction of the sheet for absorbent articles of the present invention. [Figure 9] 9(a) and (b) are schematic diagrams showing the cross-sectional structure in the thickness direction of the sheet for absorbent articles of the present invention. [Figure 10] FIG. 10 is a schematic diagram showing a cross-sectional structure in the thickness direction of the sheet for absorbent articles of the present invention. [Figure 11] FIG. 11 is a schematic diagram showing an example of a suitable apparatus used for producing the absorbent article sheet of the present invention. [Figure 12] FIG. 12 is a schematic diagram showing an example of another preferred apparatus used for producing the absorbent article sheet of the present invention. [Figure 13] Figures 13(a) to (d) are schematic diagrams showing an example of another suitable apparatus used for producing the absorbent article sheet of the present invention, and schematic diagrams showing the sheet production process using the apparatus. [Figure 14] Figures 14(a) to (e) are schematic diagrams showing an example of another suitable apparatus used for producing the absorbent article sheet of the present invention, and schematic diagrams showing the sheet production process using the apparatus. [Figure 15] FIG. 15 is a schematic diagram showing an example of another suitable apparatus used for producing the absorbent article sheet of the present invention. [Figure 16] FIG. 16 is a schematic diagram showing an example of another preferred apparatus used for producing the absorbent article sheet of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present invention will now be described based on its preferred embodiments. The sheet for absorbent articles of the present invention (hereinafter, also simply referred to as "sheet") is a fiber sheet composed of a nonwoven fabric. The sheet of the present invention is used as a constituent member of an absorbent article. The sheet of the present invention is a fiber sheet and does not have a film of a liquid-impermeable layer. The absorbent article using the sheet of the present invention generally has a vertically elongated shape with a longitudinal direction corresponding to the direction extending from the wearer's abdominal side through the crotch region to the dorsal side and a width direction perpendicular to the longitudinal direction. The absorbent article has a crotch portion disposed in the crotch region of the wearer, and abdominal and dorsal portions extending in front and behind the crotch portion. The crotch portion has an excretory portion-facing portion that is disposed facing the excretory portion of the wearer when the absorbent article is worn, and the excretory portion-facing portion is usually located in the longitudinal center of the absorbent article or in the vicinity thereof.

[0010] An absorbent article generally comprises a top sheet located on the wearer's skin-facing side, a back sheet located on the non-skin-facing side, and an absorbent interposed between the two sheets. The top sheet may be a liquid-permeable sheet, such as a nonwoven fabric or a perforated film. The top sheet may have an uneven surface on its skin-facing side. For example, a plurality of convex portions may be formed in a scattered pattern on the skin-facing side of the top sheet. Alternatively, ridges and grooves extending in one direction may be formed alternately on the skin-facing side of the top sheet. For such a purpose, the top sheet may be formed using two or more sheets of nonwoven fabric. On the other hand, the back sheet may be, for example, a liquid-impermeable nonwoven fabric.

[0011] The absorbent body has an absorbent core. The absorbent core is composed of, for example, a stack of hydrophilic fibers such as cellulose including pulp, a mixed stack of the hydrophilic fibers and an absorbent polymer, a stack of absorbent polymer, a laminated structure in which an absorbent polymer is supported between two absorbent sheets, or the like. At least the skin-facing surface of the absorbent core may be covered with a liquid-permeable core wrap sheet, or the entire surface including the skin-facing surface and the non-skin-facing surface may be covered with the core wrap sheet. As the core wrap sheet, for example, a tissue paper made of hydrophilic fibers or a liquid-permeable nonwoven fabric can be used. As described later, the sheet of the present invention is preferably used as a back sheet.

[0012] In addition to the above-mentioned top sheet, back sheet and absorbent body, leakage-preventing cuffs extending along the longitudinal direction may be arranged on both longitudinal sides of the skin-facing side depending on the specific use of the absorbent article. The leakage-preventing cuffs generally have a base end and a free end. The leakage-preventing cuffs have a base end on the skin-facing side of the absorbent article and stand up from the skin-facing side. The leakage-preventing cuffs are made of a liquid-resistant or water-repellent material and are breathable. The sheet of the present invention is suitably used as leakage-preventing cuffs. An elastic member made of rubber thread or the like may be arranged in a stretched state at or near the free end of the leakage-preventing cuff. When the absorbent article is worn, this elastic member contracts, causing the leakage-preventing cuffs to stand up toward the wearer's body, effectively preventing liquid excreted on the top sheet from leaking outward in the width direction of the absorbent article along the top sheet.

[0013] The absorbent article may further have an adhesive layer on the non-skin facing surface. The adhesive layer is used to fix the absorbent article to an undergarment or another absorbent article when the absorbent article is worn.

[0014] Examples of absorbent articles having the above-mentioned configuration include flat-type disposable diapers, pants-type disposable diapers, sanitary napkins, incontinence pads, etc., but are not limited to these.

[0015] The sheet of the present invention is suitable for use as a component of an absorbent article that requires high leak-proofing due to its high leak-proofing properties. For example, the sheet of the present invention can be used as a back sheet or as a leak-proof cuff.

[0016] The sheet of the present invention has a structure in which a plurality of nonwoven fabric layers are laminated. Furthermore, it is preferable that at least one surface of the sheet of the present invention has an uneven structure. One of the features of the sheet of the present invention is its high water repellency. In detail, the sheet of the present invention is preferably water repellent to a liquid having a surface tension of 60 mN / m (hereinafter also referred to as "low surface tension liquid"), more preferably water repellent to a liquid having a surface tension of 50 mN / m, and even more preferably water repellent to a liquid having a surface tension of 40 mN / m. By having such water repellency, the sheet of the present invention exhibits high leakproofness. In order for the sheet of the present invention to exhibit such water repellency, as described above, it is preferable that at least one surface of the sheet has an uneven structure. In addition, in order for the sheet of the present invention to exhibit such water repellency, it is advantageous for the sheet to have a nanofiber layer described later. In order to further increase the water repellency, a water repellent agent may be added to the sheet of the present invention. Details of the water repellent agent will be described later. It should be noted that surface tension depends on temperature, and the above surface tension values ​​are those at 25°C.

[0017] Whether or not the sheet of the present invention has water repellency to a low surface tension liquid is judged by the following method. As a low surface tension liquid, a "mixture for wetting tension test" available from Kanto Chemical Co., Ltd. is prepared. A sheet of the present invention having an area capable of covering the entire area of ​​a filter paper having a diameter of 7 cm is placed on the sheet of the present invention. A dry pulp sheet (basis weight 44 g / m) cut to the same size as the sheet is placed on the sheet of the present invention. 2) is placed on the sheet. 1 g of low surface tension liquid is dropped on the center of the dry pulp sheet, and a 6 cm diameter acrylic resin plate is placed on the dropping position. A weight is placed on the plate so that a pressure of 2 kPa is applied to the sheet of the present invention. After applying this pressure for 1 hour, the filter paper is removed and the area of ​​the low surface tension liquid attached to the filter paper is measured. For example, the area can be measured by photographing the filter paper or scanning it with a scanner, and binarizing the image obtained by this with image analysis software. If the area measured in this way is divided by the area of ​​the filter paper and multiplied by 100 to obtain an area ratio (%) of less than 5%, the sheet is judged to have water repellency. The area ratio is measured for 10 different sheets, and the arithmetic average value of the area ratio is taken as the area ratio value.

[0018] In the sheet of the present invention, it is preferable that the width of the convex portions in the concavo-convex structure formed on at least one surface is set to a specific range. The inventors have found that such a sheet has excellent ability to prevent liquid penetration. The width of the convex portion of the concave-convex structure is defined according to the shape of the concave-convex structure. For example, as shown in Fig. 2 described later, when the convex portions are arranged in a scattered manner, the width of the convex portion means the linear distance between the most depressed portion located between the convex portions as the starting point and the end point (linear distance when the sheet is viewed in a plane) when the start point passes through the top of the convex portion and the end point is the depressed portion located opposite to the start point in a plan view of the sheet. On the other hand, for example, as shown in Figure 3 described below, when the convex portion is formed in the form of a stripe extending continuously along one direction, the width of the convex portion means the straight-line distance between the start point and the end point (the straight-line distance when the sheet is viewed in a plane) when the start point is the most recessed point in the thickness direction located between the convex portions in a direction perpendicular to the direction in which the convex portions extend, and the end point is a recessed point that passes through the top of the convex portion and is located opposite the start point when viewed in a plane of the sheet.

[0019] Regardless of the shape of the unevenness structure, it is preferable that the width of the convex portion is 0.5 mm or more in terms of ease of forming the unevenness structure, and from this viewpoint, it is more preferable that the width of the convex portion is 1 mm or more, and even more preferable that it is 1.5 mm or more. On the other hand, the width of the protrusions is preferably 8 mm or less, since the protrusions are less likely to be crushed and the concave-convex structure can be stably maintained. From the viewpoint of making this advantage more prominent, the width of the protrusions is more preferably 6 mm or less, and even more preferably 4 mm or less. Considering all of the above, the width of the convex portion is preferably 0.5 mm or more and 8 mm or less, more preferably 1 mm or more and 6 mm or less, and even more preferably 1.5 mm or more and 4 mm or less.

[0020] The width W of the protrusion is measured by the following method. As shown in FIG. 1, the sheet is cut along its thickness direction so that the convex portions 11 and the concave portions 12 are arranged alternately, and the cut sheet is placed on a smooth table so that the convex portions 11 face upward. A flat plate is placed on the sheet, and a pressure of 49 Pa is applied. The shortest straight line distance (length of a line segment parallel to the table) from the most recessed point of the concave portion 12, passing through the top of the convex portion, to the most recessed point of the adjacent concave portion 12 is measured using a microscope. When the concave portion 12 is an embossed portion (fused portion), the distance is the distance from the edge of the embossed portion closest to the convex portion 11 to the edge of the opposing embossed portion (the edge of the embossed portion closest to the convex portion). Five different cross sections are measured, and the distance is measured at three positions per cross section. The arithmetic average of a total of 15 measured values ​​is calculated, and this value is the width W of the convex portion 11. The calculation is performed in millimeter order, and the value is rounded off to the nearest tenth place.

[0021] In the sheet of the present invention, the uneven structure is observed when no pressure is applied to the sheet. In addition, it is preferable from the viewpoint of improving leakproofness that the uneven structure is observed even when a pressure of 49 Pa is applied to the sheet of the present invention.

[0022] The sheet of the present invention can sufficiently prevent liquid permeation as long as it has an uneven structure on at least one surface, and therefore the other surface may be a flat surface or may have an uneven structure.

[0023] The sheet of the present invention may have, for example, a configuration in which convex portions are arranged in a scattered manner on one surface of the sheet, and concave portions are located between adjacent convex portions. Specifically, the sheet of the present invention may have, on one surface, convex portions and concave portions alternately arranged along one direction, and convex portions and concave portions alternately arranged along a direction perpendicular to the one direction. An example of a sheet of this configuration is shown in FIG. 2. In the sheet 10 shown in the figure, the convex portions are indicated by the reference numeral 11, and the concave portions are indicated by the reference numeral 12.

[0024] 2, the shape of the protrusions 11 in plan view may be, for example, a circle or an ellipse; a polygon such as a triangle, a rectangle, or a hexagon; or a combination thereof. The shapes of the protrusions 11 in plan view may all be the same or different. On the other hand, in the sheet 10 in the form shown in FIG. 2, the shape of the recesses 12 in plan view may be, for example, a circle or an ellipse; a polygon such as a triangle, a rectangle, or a hexagon; a cross shape; or a combination thereof.

[0025] Another embodiment of the sheet of the present invention is a form in which, on one surface of the sheet, protrusions extending continuously in stripes along one direction in the plane and recesses extending continuously in stripes along the one direction are alternately arranged in a direction perpendicular to the one direction. An example of a sheet of this form is shown in Figure 3. In the sheet 10 shown in the figure, the protrusions are indicated by reference numeral 11 and the recesses are indicated by reference numeral 12.

[0026] 2 and 3, the pitch of the protrusions is preferably 1 mm or more in terms of ease of forming a concave-convex structure. From the viewpoint of making this advantage more prominent, the pitch of the protrusions is more preferably 1.5 mm or more, and even more preferably 2 mm or more. On the other hand, it is preferable that the pitch of the convex portions is 10 mm or less, because this allows a sufficient number of concaves and convexes to be provided per unit area, and the convex portions are less likely to be crushed, so that the concave-convex structure can be stably maintained. From the viewpoint of making this advantage more prominent, it is more preferable that the pitch of the convex portions is 9 mm or less, and even more preferable that it is 8 mm or less. Considering all of the above, the pitch of the convex portions is preferably 1 mm or more and 10 mm or less, more preferably 1.5 mm or more and 9 mm or less, and even more preferably 2 mm or more and 8 mm or less.

[0027] In either case of the embodiment of the sheet of the present invention shown in Fig. 2 or Fig. 3, the pitch of the protrusions means the distance between the apexes of adjacent protrusions. When the pitch is not constant, the arithmetic average value is taken as the pitch of the protrusions.

[0028] The pitch P of the protrusions is measured by the following method. As shown in FIG. 1, the sheet is cut along its thickness direction so that the convex portions 11 and the concave portions 12 are arranged alternately, and the cut sheet is placed on a smooth table so that the convex portions 11 face upward. A flat plate is placed on the sheet, and a pressure of 49 Pa is applied. The shortest linear distance (the length of a line segment parallel to the table) from the highest point of the convex portion 11 to the highest point of the adjacent convex portion 11 across the concave portion 12 is measured using a microscope. Five different cross sections are measured, and the distance is measured at three positions per cross section. The arithmetic average of the 15 measured values ​​in total is calculated, and this value is the pitch P of the convex portions 11. The calculation is performed in millimeters and rounded off to the nearest tenth place.

[0029] Regardless of whether the sheet of the present invention is the embodiment shown in Fig. 2 or Fig. 3, the protrusions in the sheet may be solid or hollow. The protrusions being solid means that the protrusions are filled with fibers. The protrusions being hollow means that there is space inside the protrusions. When the inside of the protrusions is hollow, the space inside the protrusions prevents liquid from passing through, which is advantageous in that the leakproofness of the sheet of the present invention is improved, whereas when the inside of the protrusions is solid, the sheet of the present invention is advantageous in that a cushioning feeling is imparted and the protrusions are unlikely to be crushed.

[0030] Regardless of whether the protrusions in the sheet of the present invention are solid or hollow, the height of the protrusions in the sheet is preferably 0.5 mm or more, more preferably 0.7 mm or more, and even more preferably 0.9 mm or more, from the viewpoint of imparting high leak-proofing properties to the sheet. The height of the protrusions is preferably 5 mm or less, more preferably 4 mm or less, and even more preferably 3 mm or less. By making the protrusions lower than this value, it is possible to effectively prevent the protrusions from being excessively crushed by the pressure of the wearer when the absorbent article is worn. Considering all of the above, the height of the convex portion is preferably 0.5 mm or more and 5 mm or less, more preferably 0.7 mm or more and 4 mm or less, and even more preferably 0.9 mm or more and 3 mm or less.

[0031] The height H of the protrusion is measured by the following method. As shown in FIG. 1, the sheet is cut along its thickness direction so that the convex portions 11 and the concave portions 12 are arranged alternately, and the cut sheet is placed on a smooth table so that the convex portions 11 face upward. A flat plate is placed on the sheet, and with a pressure of 49 Pa applied, an imaginary line is drawn parallel to the plate and the table, passing through the top of the concave portions 12. The distance between the imaginary line and the bottom surface of the plate is measured using a microscope. Five different cross sections are measured, and the distance is measured at three positions per cross section. The arithmetic average of the 15 measured values ​​in total is calculated, and this value is the height H of the convex portions 11. The calculation is performed in millimeters and rounded off to the nearest tenth.

[0032] As described above, the sheet of the present invention has a structure in which a plurality of nonwoven fabric layers are laminated, and the plurality of nonwoven fabric layers preferably includes at least a nanofiber layer. The nanofiber layer is a layer formed by depositing nanofibers. In this specification, the nanofiber generally refers to a fiber having a thickness of 0.01 μm or more and 3 μm or less when expressed as a circle equivalent diameter.

[0033] The nanofiber layer can be, for example, a meltblown layer. Also, the nanofiber layer can be, for example, an electrospun layer. The meltblown layer is a layer of nonwoven fabric produced by the meltblown method, and more specifically, is a layer of nonwoven fabric produced by forming fibers by stretching a molten liquid of a raw material resin having fiber-forming ability with hot air, and then depositing the fibers on a collector. The electrospinning layer is a layer of nonwoven fabric produced by the electrospinning method. More specifically, the electrospinning layer is a layer of nonwoven fabric produced by charging a solution or melt of a resin having fiber-forming ability and discharging it into an electric field, stretching the discharged liquid by the electric field to form fibers, and depositing the fibers on a collector. Nanofibers having the above-mentioned thickness can be easily produced by either the meltblowing method or the electrospinning method.

[0034] The nanofiber layer preferably contains fibers with a fiber diameter of 1 μm or less. In particular, the present inventors have found that a sheet made of a nonwoven fabric having a nanofiber layer with an uneven surface structure has an even better ability to block liquid permeation. The present inventors believe that this is because the nanofiber layer made of fine fibers and the uneven surface structure act synergistically to block liquid permeation. However, the present invention is not bound by this theory.

[0035] From the viewpoint of further improving the leakproofness, the fiber diameter of the constituent fibers of the nanofiber layer is preferably 1 μm or less, more preferably 0.9 μm or less, as described above. There is no particular limit to the lower limit of the fiber diameter, and the smaller the fiber diameter, the higher the leakproofness of the sheet of the present invention, but sufficient leakproofness is achieved when the fibers are as thin as about 0.4 μm. Considering the above, the fiber diameter of the fibers constituting the nanofiber layer is preferably 0.4 μm or more and 1 μm or less, and more preferably 0.4 μm or more and 0.9 μm or less. To produce a nanofiber layer consisting of fibers with a fiber diameter of 1 μm or less, for example, by a meltblown method, it is sufficient to appropriately adjust conditions during production, such as the temperature and discharge amount of the resin, the temperature, volume and speed of the hot air, the temperature of the spinning die, and the nozzle diameter, and the setting of these conditions is within the scope of common technical knowledge of a person skilled in the art.

[0036] The fiber diameter of the constituent fibers of the nanofiber layer is measured by the following method. Five small samples are randomly taken from the nanofiber layer. Next, a scanning electron microscope is used to take a photograph at 1000 to 10000 times magnification so that 20 to 60 fibers of the nanofiber layer are visible in the field of view. The fiber diameters of 100 or more fibers are measured so that all fibers in the field of view are counted once, and the average value is calculated in micrometer order and rounded off to the nearest tenth. The value obtained in this manner is the fiber diameter of the fibers constituting the nanofiber layer.

[0037] When the sheet of the present invention has a nanofiber layer, the nanofiber layer has a basis weight of 1 g / m2 in order to further enhance the leakproofness of the sheet.2 It is preferable that the content is 1.5 g / m or more. 2 More preferably, it is 2 g / m or more. 2 The larger the basis weight of the nanofiber layer, the higher the leakproofness. However, from the viewpoint of the feel of the sheet and economic efficiency, it is preferable that the basis weight is 10 g / m or more. 2 Preferably, it is 9 g / m or less. 2 More preferably, it is 8 g / m or less. 2 It is even more preferable that: In summary, the nanofiber layer has a basis weight of 1 g / m 2 More than 10g / m 2 It is preferable that the content is 1.5 g / m or less. 2 More than 9g / m 2 More preferably, it is 2 g / m or less. 2 More than 8g / m 2 It is even more preferable that:

[0038] The basis weight of the nanofiber layer is measured by the following method. A 10 cm x 10 cm test piece is cut out from the sheet of the present invention using a razor. If it is not possible to cut out a test piece of this size, cut out a test piece with as large an area as possible. Carefully remove the nanofiber layer from the test piece using hands or tweezers. Measure the mass of the nanofiber and divide it by the area of ​​the test piece to obtain the basis weight of the nanofiber layer.

[0039] In relation to the above-mentioned basis weight, from the viewpoint of further enhancing the leakproofness of the sheet of the present invention, the nanofiber layer preferably has a thickness of 3 μm or more and 150 μm or less, more preferably 10 μm or more and 120 μm or less, and even more preferably 15 μm or more and 100 μm or less.

[0040] The thickness of the nanofiber layer is measured by the following method. The sheet of the present invention is cut in its thickness direction with a razor or the like so that convex and concave portions are arranged alternately, and a photograph is taken with a scanning electron microscope at a magnification of 150 to 1000 times so that the nanofiber layer is in the center of the field of view and the layers adjacent to the nanofiber layer above and below it. A boundary line is drawn between the nanofiber layer and adjacent layers based on the difference in fiber diameter. The shortest straight-line distance between two boundaries sandwiching the nanofiber layer is measured. This operation is performed on 10 different cross sections, and the arithmetic mean of the measured values, 1 point per cross section, for a total of 10 points, is calculated. The mean value is calculated in the order of micrometers and rounded off to the first decimal place.

[0041] The fibers constituting the nanofiber layer are preferably made of a thermoplastic resin having fiber forming ability. The fibers constituting the nanofiber layer are preferably made of polyolefins such as polypropylene, polyethylene, ethylene-α-olefin copolymers, polyesters such as polyethylene terephthalate, etc. From the viewpoint of easily producing a nanofiber layer with a small fiber diameter, it is preferable to use polypropylene.

[0042] The sheet of the present invention preferably includes another nonwoven fabric layer in addition to the nanofiber layer. The other nonwoven fabric layer is used for the purpose of, for example, imparting a good feel to the sheet of the present invention, imparting an uneven structure to the surface of the sheet of the present invention, or supporting the nanofiber layer. Examples of the other nonwoven fabric layer include layers manufactured by various nonwoven fabric manufacturing methods, such as a spunbond layer, an air-through layer, an airlaid layer, a spunlace layer, and a needle punch layer. In addition, it is also preferable that the other nonwoven fabric layer has elasticity in order to improve the ability to follow the wearer's movements when wearing an absorbent article including the sheet of the present invention.

[0043] When the sheet of the present invention has a nanofiber layer, it is preferable that the nanofiber layer is a meltblown layer, and that the meltblown layer has a spunbond layer disposed on at least one side thereof. As described above, the meltblown layer is composed of fine fibers, and therefore tends to have low strength. Therefore, by disposing a spunbond layer adjacent to the meltblown layer on at least one side of the meltblown layer, the strength of the meltblown layer is maintained. From this viewpoint, it is more preferable that the meltblown layer has a spunbond layer disposed adjacent to the meltblown layer on both sides thereof.

[0044] In the following description, a laminated structure of a nanofiber layer such as a meltblown layer or an electrospun layer and a pair of spunbond layers arranged adjacent to the nanofiber layer on both sides of the nanofiber layer is also referred to as an "SNS layer."

[0045] When the sheet of the present invention has an SNS layer, the spunbond layers in the SNS layer may have the same or different basis weights and / or thicknesses, and the resin types of the constituent fibers of the spunbond layers in the SNS layer may be the same or different. Each spunbond layer in the SNS layer has a basis weight of 3 g / m 2 More than 50g / m 2 Preferably, it is 4 g / m or less. 2 More than 40g / m 2 More preferably, it is 5 g / m or less. 2 More than 30g / m 2 It is even more preferable that: Each spunbond layer in the SNS layer preferably has a thickness of 50 μm to 500 μm, more preferably 60 μm to 400 μm, and even more preferably 70 μm to 300 μm. The thickness of the spunbond layer is measured in the same manner as the method for measuring the thickness of the nanofiber layer described above. It is preferred that the resin of the constituent fibers of each of the spunbond layers in the SNS layer is independently composed of, for example, polyolefin such as polypropylene, polyethylene, ethylene-α-olefin copolymer, or polyester such as polyethylene terephthalate.

[0046] When the sheet of the present invention has an SNS layer, the SNS layer may (a) constitute the uneven structure of the sheet of the present invention, (b) be present in a portion other than the uneven structure, or (c) be present in both the uneven structure and in a portion other than the uneven structure. In the case of (a), there is an advantage that the SNS layer itself is less likely to be pulled even if the sheet itself is pulled, and therefore, even if the wearer moves while wearing an absorbent article including the sheet of the present invention, the leakproofness of the SNS layer is likely to be maintained. In the case of (b), there is an advantage that the sheet can be easily produced without destroying the fiber structure of the SNS layer. In the case of (c), even if the fiber structure of the SNS layer that constitutes the uneven structure is destroyed during the manufacturing process of the sheet, the SNS layer present in areas other than the uneven structure can ensure leak resistance.

[0047] Fig. 4(a) shows a schematic cross-sectional structure in the thickness direction of the sheet of the present invention. The sheet 10 shown in the figure has a first surface 21 and a second surface 22 located on the opposite side. The first surface 21 side of the sheet 10 has an uneven structure. On the other hand, the second surface 22 is a flat surface. A single spunbond layer 13 is positioned on the first surface 21 side of the sheet 10. The spunbond layer 13 forms protrusions 11 and recesses 12. The inside of the protrusions 11 is hollow. Located on the second surface 22 side of the sheet 10 is an SNS layer 15 made up of a spunbond layer 13, a nanofiber layer 14 and another spunbond layer 13. Each surface of the SNS layer 15 is flat. The spunbond layer 13 located on the first surface 21 side is bonded at its recesses 12 to the spunbond layer 13 in the SNS layer 15 located on the second surface 22 side. This bonding forms bonded portions 16. The shape of the bonded portions 16 in a plan view can take various shapes depending on the shape of the protrusions 11 in a plan view. When the protrusions 11 have the shape shown in FIG. 2, for example, the bonded portions 16 can be arranged in a scattered dot pattern, and can be, for example, circular, elliptical, polygonal, or cross-shaped. When the protrusions 11 have the shape shown in FIG. 3, for example, the bonded portions 16 can be linear, curved, or dashed. The joint 16 is formed by various joining means such as fusion or adhesion. The sheet 10 of the embodiment shown in FIG. 4(a) has protrusions 11 and a nanofiber layer 14, and therefore exhibits high leakproofness.

[0048] 4(b), a spunbond layer 13, a nanofiber layer 14, and an SNS layer 15 composed of the spunbond layer 13 are located on the first surface 21 side. The SNS layer 15 constitutes protrusions 11 and recesses 12. The interiors of the protrusions 11 are hollow. A single spunbond layer 13 is located on the second surface 22 of the sheet 10. The spunbond layer 13 has flat surfaces on both sides. The SNS layer 15 is bonded at the recess 12 to the spunbond layer 13 located on the second surface 22 side. A bonded portion 16 is formed by this bonding. The rest of the configuration is the same as that of the embodiment shown in FIG. The sheet 10 of the embodiment shown in FIG. 4(b) has protrusions 11 and the meltblown layer 14 is located at the protrusions 11, and therefore exhibits higher leak prevention properties than the embodiment shown in FIG. 4(a).

[0049] 4(c) has a first SNS layer 15a, which is composed of a spunbond layer 13, a nanofiber layer 14 and another spunbond layer 13, positioned on the first surface 21 side of the sheet 10. The first SNS layer 15a forms protrusions 11 and recesses 12. The interiors of the protrusions 11 are hollow. A second SNS layer 15b is located on the second surface 22 side of the sheet 10. The second SNS layer 15b also comprises a spunbond layer 13, a nanofiber layer 14, and another spunbond layer 13. Each surface of the second SNS layer 15b is flat. The rest of the configuration is similar to that of the embodiment shown in FIG. According to the embodiment of the sheet 10 shown in FIG. 4(c), in addition to the nanofiber layer 14 being located on the protrusions 11, the nanofiber layer 14 is also located on the second surface 22 side, so that the leakproofness is further improved compared to the embodiment shown in FIG. 4(b).

[0050] The sheet of the present invention preferably has an air-through layer. The air-through layer is used for the purpose of imparting a good touch to the sheet of the present invention. When the sheet of the present invention is produced by the method shown in Fig. 11 described later, the air-through layer is used for the purpose of imparting an uneven shape to the surface of the sheet of the present invention.

[0051] When the sheet of the present invention includes an air-through layer, the air-through layer can be disposed adjacent to the nanofiber layer. For example, an air-through layer can be disposed adjacent to one side of the nanofiber layer. Alternatively, an air-through layer can be disposed adjacent to each side of the nanofiber layer.

[0052] When an air-through layer is disposed on each side of the nanofiber layer, the air-through layers may be the same or different in basis weight and / or thickness, and the type of resin of the constituent fibers of the air-through layers may be the same or different. Each air-through layer has a basis weight of 6 g / m 2 More than 70g / m 2 Preferably, it is 8 g / m or less. 2 More than 60g / m 2 More preferably, it is 10 g / m or less. 2 More than 50g / m 2 It is even more preferable that: Each air-through layer preferably has a thickness of 0.3 mm to 5 mm, more preferably 0.4 mm to 4 mm, and even more preferably 0.5 mm to 3 mm. The thickness of the air-through layer is measured in the same manner as the method for measuring the thickness of the nanofiber layer described above. The resin of the constituent fibers of each air-through layer is preferably composed of polyolefins such as polypropylene, polyethylene, ethylene-α-olefin copolymers, and polyesters such as polyethylene terephthalate. The resins of the constituent fibers of each air-through layer may be the same or different. Each air-through layer may be composed of core-sheath type composite fibers or side-by-side type composite fibers containing these resins.

[0053] Fig. 5 shows a schematic cross-sectional structure in the thickness direction of a sheet of the present invention. The sheet 10 shown in the figure has a first surface 21 and a second surface 22 located on the opposite side. The first surface 21 side of the sheet 10 has an uneven structure. On the other hand, the second surface 22 is a flat surface. The sheet 10 shown in Fig. 5 has a structure in which air-through layers 17a, 17b are arranged on each side of the nanofiber layer 14. The nanofiber layer 14 and the pair of air-through layers 17a, 17b each protrude toward the first surface 21 to form a protrusion 11. The inside of the protrusion 11 is solid. The inside of the protrusion 11 is filled mainly with the constituent fibers of the air-through layer 17b located on the second surface 22 side. Of the pair of air through layers 17a, 17b, the air through layer 17b located on the second surface 22 side has a flat outer surface (ie, exposed surface). The nanofiber layer 14 and the pair of air-through layers 17a, 17b are consolidated and integrally bonded in the recesses 12 of the sheet 10. The rest of the configuration is the same as that of the embodiment shown in FIG. The sheet 10 of the embodiment shown in FIG. 5 has protrusions 11 and the nanofiber layer 14 is located on the protrusions 11, and therefore exhibits high leakproofness.

[0054] When the sheet of the present invention has an SNS layer, it is also preferable that an air-through layer is disposed on the outer surface of at least one of a pair of spunbond layers in the SNS layer (i.e., the surface opposite to the surface facing the nanofiber layer). In other words, the sheet of the present invention preferably has an SNS layer and an air-through layer disposed adjacent to the outer surface of at least one spunbond layer in the SNS layer. In the following description, the laminated structure of the SNS layer and the air-through layer disposed adjacent to the outer surface of at least one spunbond layer in the SNS layer is also referred to as an "[SNS+AT] layer."

[0055] When the sheet of the present invention has an [SNS+AT] layer, the air-through layer in the [SNS+AT] layer may (a) constitute the uneven structure of the sheet of the present invention, or (b) be present in a portion other than the uneven structure. In the case of (a), when the uneven surface is the skin-facing surface, the uneven structure has the advantage of reducing the contact area with the absorbent and suppressing adhesion of body fluids to the SNS layer. On the other hand, when the uneven surface is the non-skin-facing surface, the advantage is that the appearance of the sheet can be designed. In this case, the suitable basis weight of the air-through layer is as described above. In the case of (b), when the air-through layer is located on the skin-facing side, there is an advantage that the contact area between the absorbent and the SNS layer can be reduced. When the air-through layer is located on the non-skin-facing side, there is an advantage that the feel against the skin can be improved. The suitable basis weight of the air-through layer in this case is as described above.

[0056] Fig. 6(a) shows a schematic cross-sectional structure in the thickness direction of a sheet of the present invention having an [SNS+AT] layer. The sheet 10 shown in the figure has a first surface 21 and a second surface 22 located on the opposite side. The first surface 21 side of the sheet 10 has an uneven structure. On the other hand, the second surface is flat. 6(a), the air through layer 17 is located on the first surface 21 side. The air through layer 17 constitutes the protrusions 11 and the recesses 12. The inside of the protrusions 11 is solid. The SNS layer 15 is located on the second surface 22 side of the sheet 10. The SNS layer 15 has each flat surface. The air-through layer 17 is consolidated and integrally bonded at the recess 12 to the SNS layer 15 located on the second surface 22 side. A bonded portion 16 is formed by this bonding. The rest of the configuration is the same as that of the embodiment shown in FIG. The sheet 10 shown in FIG. 6(a) has protrusions 11 and a nanofiber layer 14, and therefore exhibits high leak-proofing properties.

[0057] In the sheet 10 shown in Fig. 6(b), the inside of the protrusions 11 formed by the air-through layer 17 is hollow. The rest of the configuration is the same as in the embodiment shown in Fig. 6(a). In the sheet 10 shown in FIG. 6(b), the insides of the protrusions 11 are hollow, and therefore the sheet 10 has a higher liquid permeability barrier than the sheet shown in FIG. 6(a).

[0058] Fig. 7(a) shows a schematic cross-sectional structure in the thickness direction of a sheet having an [SNS+AT] layer according to another embodiment of the present invention. The sheet 10 shown in the figure has a first surface 21 and a second surface 22 located on the opposite side. The first surface 21 side of the sheet 10 has an uneven structure. On the other hand, the second surface is flat. 7(a), the SNS layer 15 is located on the first surface 21 side. The SNS layer 15 constitutes the protrusions 11 and the recesses 12. The air-through layer 17 is located on the second surface 22 side of the sheet 10. The outer surface (i.e., the exposed surface) of the air-through layer 17 is flat. The surface of the air-through layer 17 facing the SNS layer 15 has an uneven structure. This uneven structure has a complementary shape to the uneven structure formed by the SNS layer 15. Therefore, the inside of the protrusions 11 is solid, and is filled with the constituent fibers of the air-through layer 17. The SNS layer 15 is consolidated and integrally joined at the recess 12 to the air-through layer 17 located on the second surface 22 side. The rest of the configuration is the same as that of the embodiment shown in FIG. The sheet 10 shown in FIG. 7(a) has protrusions 11 and a nanofiber layer 14, and therefore exhibits high leak-proofing properties.

[0059] In the sheet 10 shown in Fig. 7(b), the constituent fibers of the air-through layer 17 are present inside the protrusions 11. However, the constituent fibers of the air-through layer 17 do not completely fill the inside of the protrusions 11, and spaces exist inside the protrusions 11, making the insides of the protrusions hollow. The rest of the configuration is the same as in the embodiment shown in Fig. 7(a). In the sheet 10 shown in FIG. 7(b), the insides of the protrusions 11 are hollow, and therefore the sheet 10 has a higher liquid permeability barrier than the sheet shown in FIG. 7(a).

[0060] Fig. 8 shows a schematic cross-sectional structure in the thickness direction of a sheet having an [SNS+AT] layer according to another embodiment of the present invention. The sheet 10 shown in the figure has a first surface 21 and a second surface 22 located on the opposite side. The first surface 21 of the sheet 10 has an uneven structure. On the other hand, the second surface 22 is a flat surface. The sheet 10 shown in Fig. 8 has a structure in which air-through layers 17a, 17b are disposed on each side of an SNS layer 15. The SNS layer 15 and the pair of air-through layers 17a, 17b each protrude toward the first surface 21 to form a protrusion 11. The inside of the protrusion 11 is solid. The inside of the protrusion 11 is filled mainly with the constituent fibers of the air-through layer 17b located on the second surface 22 side. Of the pair of air through layers 17a, 17b, the air through layer 17b located on the second surface 22 side has a flat outer surface (ie, exposed surface). The SNS layer 15 and the pair of air-through layers 17a, 17b are consolidated and integrally bonded in the recesses 12 of the sheet 10. The rest of the configuration is the same as that of the embodiment shown in FIG. The sheet 10 of the embodiment shown in FIG. 8 has protrusions 11 and the nanofiber layer 14 is located on the protrusions 11, and therefore exhibits high leakproofness.

[0061] 9(a) shows a schematic cross-sectional structure in the thickness direction of a sheet having an [SNS+AT] layer according to another embodiment of the present invention. The sheet 10 shown in the figure has a first surface 21 and a second surface 22 located on the opposite side. The first surface 21 side of the sheet 10 has an uneven structure. On the other hand, the second surface is flat. 9(a), a first SNS layer 15a consisting of a spunbond layer 13, a nanofiber layer 14 and another spunbond layer 13 is positioned on the first surface 21 side of the sheet 10. The first SNS layer 15a forms protrusions 11 and recesses 12. A second SNS layer 15b is located on the second surface 22 side of the sheet 10. The second SNS layer 15b also comprises a spunbond layer 13, a nanofiber layer 14, and another spunbond layer 13. Each surface of the second SNS layer 15b is flat. An air-through layer 17 is disposed between the first SNS layer 15a and the second SNS layer 15b. The air-through layer 17 is located within the protrusions 11 so as to fill the entire space of the protrusions 11 defined by the first SNS layer 15a and the second SNS layer 15b. Therefore, the inside of the protrusions 11 is solid and is filled with the constituent fibers of the air-through layer 17. According to the embodiment of the sheet 10 shown in FIG. 9(a), in addition to the nanofiber layer 14 being located on the protrusions 11, the nanofiber layer 14 is also located on the second surface 22 side, thereby further improving the leakproofness.

[0062] In the sheet 10 shown in Fig. 9(b), the constituent fibers of the air-through layer 17 are present inside the protrusions 11 defined by the first SNS layer 15a and the second SNS layer 15b. However, the constituent fibers of the air-through layer 17 do not completely fill the inside of the protrusions 11, and spaces exist inside the protrusions 11, making the insides of the protrusions hollow. The rest of the configuration is the same as in the embodiment shown in Fig. 9(a). In the sheet 10 shown in FIG. 9(b), the insides of the protrusions 11 are hollow, and therefore the sheet 10 has a higher liquid permeability barrier than the sheet shown in FIG. 9(a).

[0063] Fig. 10 shows yet another embodiment of a sheet 10 of the present invention. The sheet 10 shown in this figure has a first surface 21 and a second surface 22 located on the opposite side. The first surface 21 side of the sheet 10 has an uneven structure. On the other hand, the second surface 22 is a flat surface. The sheet 10 has a first nonwoven fabric layer 23 having an uneven structure located on the first surface 21 side. The second nonwoven fabric layer 24 is located on the second surface 22 side. The two nonwoven fabric layers 23, 24 are joined at a joining portion 16.

[0064] The first nonwoven fabric layer 23 of the sheet 10 constitutes the protrusions 11 and the recesses 12. The inside of the protrusions 11 is hollow. The first nonwoven fabric layer 23 is made of a nanofiber layer or a nonwoven fabric layer containing a nanofiber layer. When the first nonwoven fabric layer 23 is made of a nanofiber layer, the nanofiber layer is preferably a meltblown layer or an electrospun layer. On the other hand, when the first nonwoven fabric layer 23 is made of a nonwoven fabric layer containing a nanofiber layer, the first nonwoven fabric layer 23 is preferably a laminated nonwoven fabric in which a spunbonded nonwoven fabric or an air-through nonwoven fabric is laminated on one or both sides of the nanofiber layer. The nanofiber layer is preferably a meltblown layer or an electrospun layer.

[0065] The second nonwoven fabric layer 24 located on the second surface 22 side of the sheet 10 shown in FIG. 10 has flat surfaces. The second nonwoven fabric layer 24 is preferably a nonwoven fabric containing elastic filaments, and a particularly preferred nonwoven fabric is a nonwoven fabric containing elastic filaments and non-elastic fibers. In the second nonwoven fabric layer 24, the elastic filaments 25 are preferably bonded in a substantially unstretched state to nonwoven fabrics 26, 26 containing inelastic fibers. Also, the second nonwoven fabric layer 24 preferably has a configuration in which a plurality of elastic filaments 25 are bonded to two nonwoven fabrics 26, 26. The elastic filaments 25 are preferably arranged to extend in one direction X without crossing each other, thereby enabling the elastic filaments 25 to be stretched in the one direction X. As long as the elastic filaments 25 do not cross each other, they may extend linearly or in a meandering manner. Moreover, the elastic filaments 25 are preferably arranged at intervals in a direction perpendicular to the X direction (ie, a direction perpendicular to the paper surface).

[0066] It is preferable that each of the nonwoven fabrics 26, 26 constituting the second nonwoven fabric layer 24 is extensible. The nonwoven fabrics 26, 26 typically contain substantially inelastic fibers and are substantially inelastic. The "elasticity" of the elastic filaments 25 and the non-elasticity of the nonwoven fabric 26 refer to the property of being stretchable and returning to a length of 110% or less of the original length when the force is released from a state stretched 50% of the original length (150% of the original length, i.e., 1.5 times the length). The nonwoven fabrics 26, 26 are preferably stretchable in the same direction as the X direction in which the elastic filaments 25 extend. In this specification, "stretchable" includes (i) the case where the constituent fibers of the nonwoven fabrics 26, 26 themselves stretch, and (ii) the case where the constituent fibers themselves do not stretch, but the nonwoven fabric as a whole stretches as a result of fibers that were bonded at intersections separating from each other, the three-dimensional structure formed by multiple fibers due to bonding between fibers, etc., changing structurally, constituent fibers breaking, or slack fibers being stretched. Each of the nonwoven fabrics 26, 26 may be already extensible in the state of a raw roll before being joined to the elastic filament 25. Alternatively, the nonwoven fabrics 26, 26 may not be extensible in the state of a raw roll before being joined to the elastic filament 25, but may be processed so as to become extensible after being joined to the elastic filament 25. Specific methods for making the nonwoven fabric 26 extensible include heat treatment, stretching between rolls, intermeshing stretching with teeth or gears, and tensile stretching with a tenter. In view of a suitable manufacturing method for the sheet 10 described later, it is preferable that the nonwoven fabric 26 is not extensible in the state of its raw roll in order to improve the transportability of the nonwoven fabric 26 when the elastic filament 25 is fused to the nonwoven fabric 26.

[0067] The plurality of elastic filaments 25 constituting the second nonwoven fabric layer 24 are preferably each substantially continuous over the entire length of the second nonwoven fabric layer 24. Each elastic filament 25 typically contains an elastic resin.

[0068] The elastic filament 25 may be a synthetic or natural rubber in the form of a thread. Alternatively, it may be obtained by dry spinning (melt spinning) or wet spinning. The elastic filament 25 is preferably obtained by direct melt spinning without first winding it. Also, the elastic filament 25 is preferably obtained by drawing an undrawn thread. In addition, the elastic filaments 25 are preferably formed by stretching the elastic resin in a molten or softened state, which makes it easier to bond the elastic filaments 25 to the nonwoven fabric 26 in a non-stretched state. Specific examples of the stretching operation include (a) melt-spinning the resin that is the raw material of the elastic filaments 25 to obtain an unstretched yarn, and then reheating the elastic filaments of the unstretched yarn to stretch them at a temperature equal to or higher than the softening temperature (glass transition temperature Tg of the hard segment), and (b) directly stretching the molten fibers obtained by melt-spinning the resin that is the raw material of the elastic filaments 25. In a suitable method for producing the sheet 10 described later, the elastic filaments 25 are obtained by directly stretching the molten fibers obtained by melt-spinning.

[0069] Each elastic filament 25 is preferably bonded to the nonwoven fabrics 26, 26 along its entire length. "Bonded throughout its entire length" does not require that all fibers (constituent fibers of nonwoven fabric 26) in contact with elastic filament 25 are bonded to said elastic filament 25, but means that elastic filament 25 and constituent fibers of nonwoven fabric 26 are bonded in such a manner that there are no intentionally formed unbonded portions in elastic filament 25. The elastic filament 25 and the nonwoven fabrics 26, 26 may be joined by, for example, welding or bonding with an adhesive. It is also preferable to weld the elastic filament 25 to the nonwoven fabric 26 before solidification of the elastic filament 25 obtained by melt spinning. In this case, an adhesive can be applied as an auxiliary joining means before joining the nonwoven fabric 26 and the elastic filament 25. Alternatively, after joining each nonwoven fabric 26 and the elastic filament 25, a heat treatment (steam jet, heat embossing) or mechanical entanglement (needle punch, spun lace) can be performed as an auxiliary joining means. The bonding between the nonwoven fabric 26 and the elastic filaments 25 is preferably achieved simply by the elastic filaments 25 in a molten or softened state solidifying when in contact with the nonwoven fabric 26, i.e., without using any adhesive, in order to improve the flexibility of the second nonwoven fabric layer 24.

[0070] The stretchability of the second nonwoven fabric layer 24 is manifested by the elasticity of the elastic filaments 25. When the second nonwoven fabric layer 24 is stretched in the same direction as the extension direction of the elastic filaments 25, the elastic filaments 25 and the nonwoven fabrics 26, 26 are elongated. When the stretching of the second nonwoven fabric layer 24 is released, the elastic filaments 25 contract, and as the contraction occurs, the nonwoven fabric 26 returns to its state before being stretched.

[0071] As the second nonwoven fabric layer 24, it is preferable to use a non-stretchable composite material produced by bonding elastic filaments 25 in a non-stretched state to non-stretchable nonwoven fabrics 26, 26, and then passing this composite material as a raw sheet between a pair of interlocking uneven surfaces having alternating ridges and grooves, specifically, between a pair of rolls having tooth grooves, to thereby develop stretchability. The details of this manufacturing method will be described later.

[0072] In the sheet of the present invention, it is preferable that a part or the whole of the nanofiber layer is located on one side of the half of the thickness direction. This further enhances the leakproofness of the sheet of the present invention. In particular, when the sheet of the present invention is incorporated into an absorbent article as a constituent member of the absorbent article, it is preferable that a part or the whole of the nanofiber layer is located closer to the absorbent body than the half of the thickness direction of the sheet, and in particular that the whole of the nanofiber layer is located, in order to further enhance the leakproofness. From this viewpoint, for example, in the embodiments shown in Figures 4(b), 4(c), 5, 7(a), 7(b), 8, 9(a), 9(b), and 10, it is preferable to arrange the sheet 10 so that the first surface 21 faces the absorbent body, and in the embodiments shown in Figures 4(a), 6(a), and 6(b), it is preferable to arrange the sheet 10 so that the second surface 22 faces the absorbent body. The above-mentioned "half of the thickness direction" refers to half of the thickness measured in a state where a pressure of 49 Pa is applied to the sheet of the present invention.

[0073] Regardless of which embodiment of the sheet of the present invention is shown in Fig. 4 to Fig. 10, when the sheet of the present invention is used as a component of an absorbent article, it is preferable to arrange the surface of the sheet having the uneven structure so as to face the absorbent body. For example, the sheet of the present invention can be arranged on the non-skin facing surface of the absorbent body and arranged so that the surface of the sheet having the uneven structure faces the absorbent body, and used as a back sheet. The sheet of the present invention can also be used as a leakproof cuff, with the surface of the sheet having the uneven structure facing the inner surface (i.e., the surface facing the absorbent body). By arranging the sheet of the present invention in this way, it is possible to further improve the leakproofness of the sheet.

[0074] When the surface of the sheet of the present invention having the concave-convex structure is arranged to face the absorbent body, the sheet preferably has a nonwoven fabric layer flatter than the skin-facing surface on the non-skin-facing side of the nanofiber layer. This makes it easier to maintain the concave-convex structure. Therefore, even if the wearer moves while wearing the absorbent article including the sheet of the present invention, the contact area between the sheet of the present invention and the absorbent body can be stably reduced. The nonwoven fabric layer flatter than the skin-facing surface is preferably a layer other than the nanofiber layer, but may be a nanofiber layer or a layer including a nanofiber layer. From this viewpoint, for example, in the embodiments shown in Figures 4(b), 4(c), 5, 7(a), 7(b), 8, 9(a), 9(b), and 10, the sheet 10 is preferably arranged so that the first surface 21 faces the absorbent body.

[0075] When the surface of the sheet of the present invention having the uneven structure is disposed so as to face an absorbent body, the sheet also preferably has an air-through layer on the non-skin facing side of the nanofiber layer, which enhances the cushioning effect of the air-through layer and improves the feel of the absorbent article against the skin. For example, in the embodiments shown in Figures 5, 7(a), 7(b), 8, 9(a), 9(b) and 10, it is preferable to use the first surface 21 as the skin-facing surface and the second surface 22 as the non-skin-facing surface.

[0076] When the surface of the sheet of the present invention having the uneven structure is disposed so as to face an absorbent body, the sheet also preferably has an air-through layer on the skin-facing side of the nanofiber layer, which enhances the cushioning effect of the air-through layer and improves the feel of the absorbent article against the skin. For example, in the embodiment shown in FIG. 5, it is preferable to use the first surface 21 as the skin-facing surface and the second surface 22 as the non-skin-facing surface.

[0077] Regardless of which embodiment of the sheet of the present invention is shown in Figures 4 to 10, the sheet of the present invention may or may not have elasticity. If the sheet of the present invention has elasticity, there is an advantage that the sheet can better conform to the wearer's movements when wearing an absorbent article including the sheet of the present invention. In this specification, elasticity refers to the property of being stretchable in a predetermined direction and shrinking when the stretch is released.

[0078] Next, a preferred method for producing the sheet of the present invention will be described. An example of a preferred apparatus used for producing the sheet of the present invention is shown in schematic form in Fig. 11. The apparatus 40 shown in the figure is preferably used for producing the sheet 10 shown in Figs. 7(a), 7(b) and 8, for example.

[0079] The apparatus 30 shown in Fig. 11 includes a carding machine 31. In the carding machine 31, a carded web 32 is produced. The carded web 32 preferably contains heat-shrinkable fibers that can shrink when heat is applied. It is preferable to use latent crimp fibers as the heat-shrinkable fibers, from the viewpoint of obtaining a sheet having clear protrusions.

[0080] The carded web 32 fed from the carding machine 31 is overlapped with the SNS web 33 during the transport process. The SNS web 33 is a laminated web with a three-layer structure in which a spunbond layer is disposed on each side of a meltblown layer. In the SNS web 33, the three layers may be bonded and integrated by various bonding means such as heat embossing or adhesives. Alternatively, the three layers may be laminated without being bonded. Note that instead of the SNS web 33, a meltblown web or a two-layer laminated web in which a spunbond layer is disposed on one side of a meltblown layer may be used.

[0081] The card web 32 and the SNS web 33 are introduced into a thermal embossing roll device 34 equipped with an embossing roll 34a and an anvil roll 34b, and are thermally embossed. The two webs 32, 33 are partially joined and integrated by the thermal embossing process, thereby obtaining a precursor 35 of the desired sheet.

[0082] The obtained sheet precursor 35 is introduced into a heat treatment device 36 arranged on the transport path thereof and subjected to a heat treatment. The heat treatment is performed at a temperature equal to or higher than the heat shrinkage initiation temperature of the heat-shrinkable fiber contained in the card web 32. The heat treatment causes the heat-shrinkable fibers in the carded web 32 to shrink, and the dimension of the carded web 32 in its planar direction is shortened. On the other hand, since the SNS web 33 does not contain any heat-shrinkable fibers, the SNS web 33 does not shrink due to heat. Even if the dimension of the carded web 32 in the planar direction is shortened, the dimension of the SNS web 33 in the planar direction does not change, so the fibers constituting the SNS web 33 have nowhere to go and move in the thickness direction. As a result, the SNS web 33 bulges. The SNS web 33 bulges between the joints between the carded web 32 and the SNS web 33. This causes a large number of protrusions in the SNS web 33. The joints become recesses located between the protrusions. In this manner, the desired sheet 10 is obtained. The heat treatment in the heat treatment device 36 may be performed by blowing hot air using an air-through method, or may be performed by irradiating microwaves, blowing steam, irradiating infrared rays, or contacting with a heat roll. During the heat treatment, it is preferable to fix the sheet precursor 35 with a pin tenter from the viewpoint of forming clear protrusions 11.

[0083] When the heat treatment conditions in the heat treatment device 36 are appropriately controlled to increase the degree of shrinkage of the carded web 32, a sheet 10 in which the insides of the protrusions 11 are filled with fibers is obtained, as shown in Fig. 7(a). On the other hand, when the degree of shrinkage of the carded web 42 is small, a sheet 10 in which the insides of the protrusions 11 have spaces is obtained, as shown in Fig. 7(b).

[0084] An example of an apparatus suitable for use in producing the sheet of the present invention is shown in schematic form in Fig. 12. The apparatus 40 shown in the figure is suitable for use in producing the sheet 10 shown in Figs. 4(a), 4(b), 4(c), 6(b) and 7(b), for example.

[0085] 12, the sheet 10 is manufactured by using the device 40, which includes a step of overlapping a second fiber sheet 42 on one side of a first fiber sheet 41 having an uneven surface formed thereon, and a step of joining the first fiber sheet 41 and the second fiber sheet 42. Before the joining step, a step of forming the first fiber sheet 41 into an uneven surface is performed. The first fiber sheet 41 is a raw sheet of the nonwoven fabric layer located on the first surface 21 side of the sheet 10, and in the sheet 10 shown in FIG. 4(a), for example, it is a raw sheet of the spunbond layer 13 having a concavo-convex structure. The second fiber sheet 42 is a raw sheet of a nonwoven fabric layer located on the second surface 22 side of the sheet 10, and is, for example, a raw sheet of the SNS layer 15 in the sheet 10 shown in FIG.

[0086] The production of the sheet 10 using the device 40 shown in Fig. 12 will be described in detail. First, the uneven shaping of the first fiber sheet 41 will be described. The uneven shaping of the first fiber sheet 41 is preferably performed by a shaping device 45 including a first roll 43 having an uneven peripheral surface, and a second roll 44 having an uneven peripheral surface that meshes with the uneven surface of the first roll 43. It is preferable that each of the first roll 43 and the second roll 44 has a structure in which convex streaks 46A and concave streaks 46B extending along the rotation axis of the roll are alternately arranged along the rotation direction of the roll. The first roll 43 and the second roll 44 are configured to rotate in opposite directions with the peripheral surfaces of the two rolls meshing with each other.

[0087] With both rolls 43, 44 in mesh, the first fiber sheet 41 is supplied to the meshing portion of the rolls 43, 44 to impart projections and recesses to the first fiber sheet 41. At the meshing portion of the rolls 43, 44, multiple locations of the first fiber sheet 41 are pressed into the recesses of the first roll 43 by the protruding portions of the second roll 44, and the pressed portions become the projections 11 of the target sheet 10.

[0088] When forming the unevenness, it is preferable to suck air from the outside of the peripheral surface of the first roll 43 toward the inside of the roll 43 to bring the first fiber sheet 41 into close contact with the peripheral surface, in order to reliably form the unevenness on the first fiber sheet 41. For this purpose, it is preferable to provide suction holes (not shown) in the grooves provided in the first roll 43, and to suck air from the outside of the roll 43 toward the inside through the suction holes.

[0089] It is preferable that the first fiber sheet 41 having the irregular shape is conveyed while being held on the peripheral surface of the first roll 43, and moves from the meshing portion. Meanwhile, the second fiber sheet 42 is unwound from its original roll and overlapped with the unevenly shaped first fiber sheet 41. Simultaneously with or after overlapping of the two sheets 41, 42, the two sheets 41, 42 are introduced into a joining device 47. The joining device 47 may be, for example, a heat roll as shown in the figure. Alternatively, the joining device 47 may be an ultrasonic sealing device (not shown) equipped with an ultrasonic horn. In the joining device 47, the first fiber sheet 41 and the second fiber sheet 42 are partially joined together to form the joint portion 16 described above.

[0090] In manufacturing the sheet 10 using the device 40 shown in FIG. 12, it is preferable to set the supply speed V1 of the first fiber sheet 41 faster than the supply speed V2 of the second fiber sheet 42. This makes the first fiber sheet 41 less susceptible to damage when the first fiber sheet 41 is shaped to have projections and recesses. This is particularly effective when the first fiber sheet 41 contains a meltblown layer. This is because the meltblown layer has a relatively low strength and is easily damaged by the shaping of projections and recesses. The supply speed V1 of the first fiber sheet 41 should be faster than the supply speed V2 of the second fiber sheet 42 to an extent that the shaping of projections and recesses is possible, and the speed can be appropriately set according to the degree of the projection and recess structure.

[0091] Figures 13(a) to (d) show another example of an apparatus suitable for use in producing the sheet of the present invention. The apparatus 50 shown in the figure is suitable for use in producing the sheet 10 shown in Figures 4(a), 4(b) and 4(c), for example.

[0092] 13(a), a plurality of partition walls 52 are arranged in parallel at regular intervals on the main surface of a flat substrate 51. This apparatus 50 is used as a member for forming projections and recesses on a sheet.

[0093] As shown in Fig. 13(b), a first fiber sheet 53 is placed on the partition wall 52 of the apparatus 50 shown in Fig. 13(a). The first fiber sheet 53 may be, for example, a spunbond layer or an SNS layer.

[0094] 13(c), the first fiber sheet 53 is pressed into the spaces between the partition walls 52 using a pressing member 54 to impart projections and recesses to the first fiber sheet 53. There are no particular limitations on the type of material for the pressing member 54 as long as it is capable of pressing the first fiber sheet 53 into the spaces between the partition walls 52. Therefore, the pressing member 54 may be, for example, a filament-like body. Of course, the pressing member 54 may also be a rigid body such as a rod-like body.

[0095] After the first fiber sheet 53 has been formed with projections and recesses, the second fiber sheet 55 is placed on the first fiber sheet 53 as shown in Fig. 13(d). Since the first fiber sheet 53 has been formed with projections and recesses as described above, the tops of the projections on the first fiber sheet 53 come into contact with the second fiber sheet 55. The second fiber sheet 55 can be, for example, a spunbond layer or an SNS layer. With the second fiber sheet 55 placed on the first fiber sheet 53, heat is applied to both sheets 53, 55 to bond the two sheets 53, 55 at the contacting portions of the two sheets 53, 55. Methods of applying heat include pressing a heater against the second fiber sheet 55, blowing hot air, and irradiating infrared rays.

[0096] Another example of an apparatus suitable for use in producing the sheet of the present invention is shown in Figures 14(a) to (e). The apparatus 60 shown in the figure is suitable for use in producing the sheet 10 shown in Figures 4(a), 4(b), 4(c) and 6(b), for example.

[0097] In the device 60 shown in Fig. 14(a), a plurality of columnar members 62 are arranged at regular intervals in the vertical and horizontal directions on the main surface of a flat substrate 61. This device 60 is used as a member for forming irregularities in a sheet. The columnar members 62 may be either cylindrical or rectangular. As shown in Fig. 14(b), in the apparatus 60, a shaping restricting member 63 is disposed between adjacent columnar members 62. The shaping restricting member 63 is disposed for the purpose of adjusting the degree of uneven shaping applied to the first fiber sheet 64 in the step shown in Fig. 14(d) described later. Under the condition shown in Fig. 14(b), a first fiber sheet 64 is placed on the columnar member 62 of the apparatus 60 as shown in Fig. 14(c). The first fiber sheet 64 may be, for example, a spunbond layer or an SNS layer. Alternatively, the first fiber sheet 64 may be a carded web.

[0098] 14(d), the first fiber sheet 64 is pressed into the spaces between the columnar members 62 using a pressing member 65 to form a primary uneven shape on the first fiber sheet 64. The pressing member 65 may be a rigid body such as a rod-shaped body. The pressing of the first fiber sheet 64 by the pressing member 65 is adjusted to a certain degree by the shape forming restricting member 63.

[0099] After the first fiber sheet 64 has been formed into the primary unevenness, the pushing member 65 is retracted and the shape restricting member 63 is removed. Next, as shown in Fig. 14(e), hot air is blown onto the first fiber sheet 64 to form the secondary unevenness. Hot air may be blown only once, or may be blown two or more times. When blowing hot air two or more times, it is preferable to set the hot air temperature the same for the first and second or subsequent blows and to set the hot air speed slower than the first blow, since this allows for clear unevenness to be formed.

[0100] Once the first fiber sheet 64 has been shaped to have projections and recesses in this manner, a second fiber sheet (not shown) is placed on the first fiber sheet 64 in the same manner as in the procedure shown in Fig. 13(d) described above. The second fiber sheet can be, for example, a spunbond layer or an SNS layer. Thereafter, the first fiber sheet and the second fiber sheet are bonded together in the same manner as in the procedure shown in Fig. 13(d) described above to obtain the desired sheet. Note that a hot melt adhesive can also be used to bond the first fiber sheet and the second fiber sheet.

[0101] Another example of a suitable apparatus used for producing the sheet of the present invention is shown in Figures 15 and 16. The apparatus 70 shown in Figure 16 is suitable for use in producing the sheet 10 shown in Figure 10, for example. 16, a method for producing a sheet 10 using the present production apparatus 70 includes a joining step of partially joining a first fiber sheet 23A, which is an original roll of the first nonwoven fabric layer 23, and a second fiber sheet 24A, which is an original roll of the second nonwoven fabric layer 24, to obtain the sheet 10. Specifically, the present production method preferably includes a step of overlapping the second fiber sheet 24A, which has elasticity, on one side of the first fiber sheet 23A while the second fiber sheet 24A is in a stretched state, and a step of partially joining both sheets 23A, 24A.

[0102] In addition, the manufacturing method of the sheet 10 using the manufacturing apparatus 70 preferably includes a precursor manufacturing process of manufacturing a composite material 24B, which is a precursor of the second fiber sheet 24A, as a raw cloth for the second nonwoven fabric layer 24, as shown in FIG. 15, and an elasticity developing process of applying a stretching process to the composite material 24B to obtain an elastic second fiber sheet 24A, which is a raw cloth for the second nonwoven fabric layer 24, as shown in FIG. 16.

[0103] In the precursor manufacturing process, as shown in Fig. 15, it is preferable to bond a plurality of elastic filaments 25 to nonwoven fabrics 26, 26 so as to extend in one direction and in a substantially unstretched state to obtain a composite material 24B, which is a precursor of the second fiber sheet 24A. More specifically, it is preferable to melt and attach the elastic filaments 25 to two nonwoven fabrics 26, 26 so that the elastic filaments 25 are arranged in one direction without crossing each other before solidification while drawing a large number of molten elastic filaments 25 spun from a spinning nozzle 86 at a predetermined speed. In this way, a composite material 24B, which is a precursor of the second fiber sheet 24A, is manufactured in which a plurality of elastic filaments 25 are bonded to the nonwoven fabrics 26, 26 over their entire length in a substantially unstretched state.

[0104] In the stretchability developing treatment step in this embodiment, a groove-drawing device 75 is used to perform a drawing process on the composite material 24B serving as a precursor of the second fiber sheet 24A. This stretching process is a process for stretching the composite material 24B along the direction in which the elastic filaments 25 extend, thereby imparting extensibility to both nonwoven fabrics 26, 26. The imparting of extensibility here also includes a case in which the extensibility of the nonwoven fabric 26, which already has some extensibility, is greatly improved.

[0105] It is preferable that the tooth groove extension device 75 has teeth, which are axially extending convex portions, and grooves formed between the teeth and extending in the axial direction, which are alternately arranged in the circumferential direction, and is provided with a pair of tooth groove rolls 76, 77 that mesh with each other. In the elasticity developing treatment step using the tooth groove stretching device 75, the composite material 24B obtained in the precursor manufacturing step is supplied between a pair of tooth groove rolls 76, 77, and the composite material 24B is stretched to obtain a second fiber sheet 24A in which the nonwoven fabrics 26, 26 contained in the composite material 24B are stretchable. In order to effectively perform the stretching, it is preferable to arrange a first nip roll 88 on the upstream side of the tooth groove stretching device 75 and a second nip roll 89 on the downstream side of the tooth groove stretching device 75, and to perform the elasticity developing treatment step under a state in which tension is applied to the composite material 24B. As the tooth profile of the tooth-groove rolls 76, 77, a general involute tooth profile or cycloid tooth profile is used, and in particular, those having a narrow tooth width are preferable.

[0106] In this manner, the composite material 24B is partially stretched by the pair of grooved rolls 76, 77, etc., to obtain the second fiber sheet 24A. The obtained second fiber sheet 24A exhibits elasticity along the extension direction of the elastic filaments 25. Note that Figures 15 and 16 show a case in which composite material 24B is wound into a roll to form roll-shaped material 24R, and then composite material 24B unwound from roll-shaped material 24R is subjected to a stretching process. However, the manufactured composite material 24B may also be introduced into a tooth groove stretching device using tooth groove rolls 76, 77 without being wound into a roll. As shown in FIG. 16, the first fiber sheet 23A can be used by unwinding it from a roll 23R of the first fiber sheet 23A. The above describes a method of stretching the composite material 24B using the toothed rolls 76, 77 to impart elasticity to the composite material 24B. However, instead of this method, it is also possible to produce the second fiber sheet 24A by using an elastic nonwoven fabric as the second fiber sheet without using the toothed rolls and bonding the nonwoven fabric in a stretched state.

[0107] In the joining step in this embodiment, it is preferable to subject the laminated sheet 10A, in which the second fiber sheet 24A and the first fiber sheet 23A are stacked in an extended state, to a joining process for partially joining the first fiber sheet 23A and the second fiber sheet 24A. For the joining process, any device capable of partially joining the first fiber sheet 23A and the second fiber sheet 24A can be used, such as a heat sealer, an ultrasonic sealer, or a high-frequency sealer. 16 shows a state in which the first fiber sheet 23A and the second fiber sheet 24A are partially joined together using an ultrasonic sealing device 71A. The ultrasonic sealing device 71A includes an ultrasonic horn 72 and an anvil roll 71 disposed opposite the horn 72. The laminated sheet 10A is transported along the circumferential surface of the anvil roll 71. During the transport process, the laminated sheet 10A is irradiated with ultrasonic waves by the ultrasonic horn 72, thereby partially joining the second fiber sheet 24A and the first fiber sheet 23A together.

[0108] In the manufacture of the sheet of the present invention using the above-mentioned devices 30, 40, 50, 60, 70 shown in Figs. 11 to 16, a water repellent agent can be added to the sheet 10 after manufacture. Alternatively, a water repellent agent can be added to the raw roll before manufacture. The addition of a water repellent agent further enhances the leakproofness of the sheet of the present invention. A water repellent agent may be added to the resin used when spinning the spunbond nonwoven fabric, meltblown nonwoven fabric, or electrospun nonwoven fabric. The water repellent agent added to the resin bleeds out, imparting water repellency to the fiber surface. Examples of the water repellent include nonionic water repellents, anionic water repellents, cationic water repellents, amphoteric water repellents, silicone water repellents, fluorine compound water repellents, and oils and fats. As long as the effects of the present invention are achieved, the water repellent is not limited to these water repellents, but from the viewpoint of water repellency, it is preferable to use fluorine compound water repellents and oils and fats. As the oils and fats, triglycerides are preferable, and palmitic acid triglyceride, stearic acid triglyceride, palm extremely hardened oil, and high erucic rapeseed hardened oil are more preferable.

[0109] Although the present invention has been described based on the preferred embodiment, the present invention is not limited to the above embodiment. For example, in the embodiment shown in Figures 4 to 10, the first surface 21 of the sheet 10 has an uneven structure and the second surface 22 is a flat surface, but instead, both the first surface 21 and the second surface 22 may have an uneven structure.

[0110] In relation to the above-mentioned embodiment, the present invention further discloses the following sheet for absorbent articles. <1> A sheet for absorbent articles comprising a plurality of nonwoven fabric layers laminated together, At least one surface of the sheet has a concave-convex structure, A sheet for absorbent articles that is water-repellent to liquids with a surface tension of 60 mN / m.

[0111] <2> The surface tension of the surface layer is preferably 50 mN / m, and more preferably 40 mN / m. <1> The sheet for absorbent articles according to claim 1. <3> Within one surface of the sheet, protrusions and recesses are alternately arranged along one direction, and protrusions and recesses are alternately arranged along a direction perpendicular to the one direction. <1> or <2> The sheet for absorbent articles according to claim 1. <4> The sheet has convex portions extending continuously in stripes along one direction on one surface thereof and concave portions extending continuously in stripes along the one direction, the concave portions being alternately arranged along a direction perpendicular to the one direction. <1> or <2> The sheet for absorbent articles according to claim 1. <5> The width of the convex portion in the concave-convex structure is 0.5 mm or more and 8 mm or less. <1> Or <4> 13. The sheet for absorbent articles according to claim 12. <6> The width of the convex portion in the concave-convex structure is preferably 1 mm or more, and more preferably 1.5 mm or more. The width of the convex portion in the concave-convex structure is preferably 6 mm or less, and more preferably 4 mm or less. <5> The sheet for absorbent articles according to claim 1.

[0112] <7> The pitch of the convex portions in the concave-convex structure is preferably 1 mm or more, more preferably 1.5 mm or more, and even more preferably 2 mm or more. The pitch of the projections in the uneven structure is preferably 10 mm or less, more preferably 9 mm or less, and even more preferably 8 mm or less. <1> Or <6> 13. The sheet for absorbent articles according to claim 12. <8> The height of the convex portions in the concave-convex structure is preferably 0.5 mm or more, more preferably 0.7 mm or more, and even more preferably 0.9 mm or more. The height of the convex portions in the concave-convex structure is preferably 5 mm or less, more preferably 4 mm or less, and even more preferably 3 mm or less. <1> Or <7> 13. The sheet for absorbent articles according to claim 12. <9> The inside of the protrusion in the concave-convex structure is solid. <1> Or <8> 13. The sheet for absorbent articles according to claim 12. <10> The inside of the protrusions in the concave-convex structure is hollow. <1> Or <8> 13. The sheet for absorbent articles according to claim 12. <11> The nanofiber layer is included. <1> Or <10> 13. The sheet for absorbent articles according to claim 12.

[0113] <12> The nanofiber layer has an uneven structure. <11> The sheet for absorbent articles according to claim 1. <13> A part or the whole of the nanofiber layer is located on one side of the halfway point in the thickness direction. <11> or <12> The sheet for absorbent articles according to claim 1. <14> The entire nanofiber layer is located on one side of the halfway point in the thickness direction. <13> The sheet for absorbent articles according to claim 1. <15> The nanofiber layer includes fibers having a fiber diameter of 1 μm or less. <11> Or <14> 13. The sheet for absorbent articles according to claim 12. <16> The fiber diameter of the constituent fibers of the nanofiber layer is preferably 1 μm or less, and more preferably 0.9 μm or less. The fiber diameter of the fibers constituting the nanofiber layer is preferably 0.4 μm or more. <11> Or <15> 13. The sheet for absorbent articles according to claim 12.

[0114] <17> The thickness of the nanofiber layer is preferably 3 μm or more and 150 μm or less, more preferably 10 μm or more and 120 μm or less, and even more preferably 15 μm or more and 100 μm or less. <11> Or <16> 13. The sheet for absorbent articles according to claim 12. <18> In addition to the nanofiber layer, another nonwoven fabric layer is provided, The other nonwoven fabric layer has elasticity. <11> Or <17> 13. The sheet for absorbent articles according to claim 12. <19> The nanofiber layer is a meltblown layer, The meltblown layer is disposed between a pair of spunbond layers. <11> Or <18> 13. The sheet for absorbent articles according to claim 12. <20> The meltblown layer is disposed between a pair of the spunbond layers to form an SNS layer, which constitutes the uneven structure. <19> The sheet for absorbent articles according to claim 1. <21> The air-through layer is provided. <1> Or <20> 13. The sheet for absorbent articles according to claim 12.

[0115] <22> The SNS layer is formed by disposing a nanofiber layer between a pair of spunbond layers, An air-through layer is disposed on an outer surface of at least one of the pair of spunbond layers in the SNS layer. <21> The sheet for absorbent articles according to claim 1. <23> The air-through layer constitutes the uneven structure. <21> or <22> The sheet for absorbent articles according to claim 1. <24> The air-through layer is present in a portion other than the concave-convex structure. <21> or <22> The sheet for absorbent articles according to claim 1. <25> The air-through layer is disposed on each side of the nanofiber layer, Each of the nanofiber layer and the air-through layer protrudes toward one surface side of the sheet to form a convex portion, The inside of the protrusion is solid. <21> Or <24> 13. The sheet for absorbent articles according to claim 12. <26> The air-through layer includes crimped fibers. <21> Or <25> 13. The sheet for absorbent articles according to claim 12.

[0116] <27> A first surface and a second surface located opposite the first surface, The first surface has an uneven structure, The second surface is a flat surface, A single spunbond layer is located on the first surface side, The spunbond layer forms protrusions and recesses, The inside of the protrusion is hollow, An SNS layer including a spunbond layer, a nanofiber layer, and a spunbond layer is located on the second surface side, The SNS layer has flat surfaces on each side. <1> Or <26> 13. The sheet for absorbent articles according to claim 12. <28> A first surface and a second surface located opposite the first surface, An SNS layer including a spunbond layer, a nanofiber layer, and a spunbond layer is located on the first surface side, The SNS layer constitutes a protrusion 11 and a recess 12, The inside of the protrusion is hollow, A single spunbond layer is located on the second surface side, The spunbond layer has flat surfaces on each side. <1> Or <26> 13. The sheet for absorbent articles according to claim 12. <29> A first surface and a second surface located opposite the first surface, A first SNS layer is located on the first surface side and is composed of a spunbond layer, a nanofiber layer, and a spunbond layer, the first SNS layer defines a protrusion and a recess; The inside of the protrusion is hollow, A second SNS layer is located on the second surface side, the second SNS layer being composed of a spunbond layer, a nanofiber layer, and a spunbond layer, The second SNS layer has flat surfaces. <1> Or <26> 13. The sheet for absorbent articles according to claim 12. <30> A first surface and a second surface located opposite the first surface, The first surface has an uneven structure, The second surface is a flat surface, The structure has an air-through layer disposed on each side of the nanofiber layer, The nanofiber layer and the pair of air-through layers each have a convex portion protruding toward the first surface side, The inside of the protrusion is solid, the inside of the protrusion is filled mainly with constituent fibers of the air-through layer located on the second surface side, Of the pair of air-through layers, the air-through layer located on the second surface side has a flat outer surface, The nanofiber layer and the pair of air-through layers are consolidated and integrally bonded in the recesses of the sheet. <1> Or <26> 13. The sheet for absorbent articles according to claim 12. <31> A first surface and a second surface located opposite the first surface, The first surface has an uneven structure, The second surface is a flat surface, An air-through layer is located on the first surface side, The air-through layer has a convex portion and a concave portion, The inside of the protrusion is solid, An SNS layer is located on the second surface side, the SNS layer being formed by disposing a nanofiber layer between a pair of spunbond layers, The SNS layer has flat surfaces on each side, The air-through layer is consolidated and integrally joined to the SNS layer located on the second surface side at the recessed portion. <1> Or <26> 13. The sheet for absorbent articles according to claim 12.

[0117] <32> A first surface and a second surface located opposite the first surface, The first surface has an uneven structure, The second surface is a flat surface, An air-through layer is located on the first surface side, The air-through layer has a convex portion and a concave portion, The inside of the protrusion is hollow, An SNS layer is located on the second surface side, the SNS layer being formed by disposing a nanofiber layer between a pair of spunbond layers, The SNS layer has flat surfaces on each side, The air-through layer is consolidated and integrally joined to the SNS layer located on the second surface side at the recessed portion. <1> Or <26> 13. The sheet for absorbent articles according to claim 12. <33> A first surface and a second surface located opposite the first surface, The first surface has an uneven structure, The second surface is a flat surface, An SNS layer is located on the first surface side, the SNS layer being formed by disposing a nanofiber layer between a pair of spunbond layers, The SNS layer comprises a protrusion and a recess, An air-through layer is located on the second surface side, The air-through layer has a flat outer surface, The surface of the air-through layer facing the SNS layer has an uneven structure, the relief structure has a shape complementary to a relief structure formed by the SNS layer; The inside of the protrusion is solid, The inside of the protrusion is filled with the constituent fibers of the air-through layer, The SNS layer is consolidated and integrally joined to the air-through layer located on the second surface side at the recessed portion. <1> Or <26> 13. The sheet for absorbent articles according to claim 12. <34> A first surface and a second surface located opposite the first surface, The first surface has an uneven structure, The second surface is a flat surface, An SNS layer is located on the first surface side, the SNS layer being formed by disposing a nanofiber layer between a pair of spunbond layers, The SNS layer comprises a protrusion and a recess, An air-through layer is located on the second surface side, The air-through layer has a flat outer surface, The surface of the air-through layer facing the SNS layer has an uneven structure, The fibers constituting the air-through layer are present inside the protrusions, the constituent fibers of the air-through layer do not completely fill the inside of the protrusions, and spaces exist inside the protrusions, making the inside of the protrusions hollow; The SNS layer is consolidated and integrally joined to the air-through layer located on the second surface side at the recessed portion. <1> Or <26> 13. The sheet for absorbent articles according to claim 12. <35> A first surface and a second surface located opposite the first surface, The first surface has an uneven structure, The second surface is a flat surface, The SNS layer is formed by disposing a nanofiber layer between a pair of spunbond layers, and an air-through layer is disposed on each side of the SNS layer. each of the SNS layer and the pair of air-through layers protrudes toward the first surface side to form a convex portion; The inside of the protrusion is solid, the inside of the protrusion is filled mainly with constituent fibers of the air-through layer located on the second surface side, The air-through layer located on the second surface side has a flat outer surface, The SNS layer and the pair of air-through layers are consolidated and integrally joined at the recesses of the sheet. <1> Or <26> 13. The sheet for absorbent articles according to claim 12. <36> A first surface and a second surface located opposite the first surface, The first surface has an uneven structure, The second surface is a flat surface, A first SNS layer is located on the first surface side, the first SNS layer being formed by disposing a nanofiber layer between a pair of spunbond layers, the first SNS layer defines a protrusion and a recess; A second SNS layer is located on the second surface side, the second SNS layer being formed by disposing a nanofiber layer between a pair of spunbond layers, The second SNS layer has flat surfaces on each side, an air-through layer is disposed between the first SNS layer and the second SNS layer; the air-through layer is located within the protrusion so as to fill the entire space of the protrusion defined by the first SNS layer and the second SNS layer, The inside of the protrusion is solid, The inside of the protrusion is filled with the constituent fibers of the air-through layer. <1> Or <26> 13. The sheet for absorbent articles according to claim 12.

[0118] <37> A first surface and a second surface located opposite the first surface, The first surface has an uneven structure, The second surface is a flat surface, A first SNS layer is located on the first surface side, the first SNS layer being formed by disposing a nanofiber layer between a pair of spunbond layers, the first SNS layer defines a protrusion and a recess; A second SNS layer is located on the second surface side, the second SNS layer being formed by disposing a nanofiber layer between a pair of spunbond layers, The second SNS layer has flat surfaces on each side, an air-through layer is disposed between the first SNS layer and the second SNS layer; The air-through layer has constituent fibers present within a protrusion defined by the first SNS layer and the second SNS layer, The fibers constituting the air-through layer do not completely fill the inside of the protrusions, and spaces exist inside the protrusions, making the inside of the protrusions hollow. <1> Or <26> 13. The sheet for absorbent articles according to claim 12. <38> A first surface and a second surface located opposite the first surface, The first surface has an uneven structure, The second surface is a flat surface, A first nonwoven fabric layer having a concave-convex structure is located on the first surface side, A second nonwoven fabric layer 24 is located on the second surface side, The first nonwoven fabric layer defines a protrusion and a recess, The inside of the protrusion is hollow, the first nonwoven fabric layer is a nanofiber layer or a nonwoven fabric layer containing a nanofiber layer; The second nonwoven fabric layer has flat surfaces on each side, The second nonwoven fabric layer is a nonwoven fabric containing elastic filaments and inelastic fibers, The second nonwoven fabric layer has elastic filaments bonded to the nonwoven fabric containing the inelastic fibers in a substantially non-stretched state. <1> Or <26> 13. The sheet for absorbent articles according to claim 12. <39> The absorbent body and the <1> Or <38> An absorbent article comprising the sheet for absorbent articles according to any one of the above items, The sheet for absorbent articles is disposed so that the surface of the sheet for absorbent articles having the uneven structure faces the absorbent body. <40> The sheet for absorbent articles has a nanofiber layer, a nonwoven fabric layer that is flatter than the skin-facing surface and is located on the non-skin-facing surface side of the nanofiber layer; <39> The absorbent article according to claim 1. <41> The air-through layer is disposed on the skin-facing side of the nanofiber layer. <40> The absorbent article according to claim 1. <42> The sheet for absorbent articles is disposed on the non-skin facing side of the absorbent body. <39> Or <41> 13. An absorbent article according to any one of claims 1 to 12. EXAMPLES

[0119] The present invention will be described in more detail below with reference to examples. However, the scope of the present invention is not limited to such examples. Unless otherwise specified, "%" means "% by mass".

[0120] Example 1 In this example, the apparatus shown in FIG. 11 was used to manufacture a sheet for absorbent articles having the structure shown in FIG. 2 and FIG. 7(b). (1) Manufacturing of card web The core is made of low-density polyethylene (hereinafter also referred to as "LDPE") and the sheath is made of polyethylene (hereinafter also referred to as "PE"), and the eccentric core-sheath type composite fiber has a basis weight of 27 g / m 2 A carded web of the above was produced. The eccentric sheath-core type composite fiber had a fineness of 2.3 dtex and a fiber length of 51 mm. The eccentric sheath-core type composite fiber was a latent crimp fiber that exhibited crimping when heat was applied. (2) SNS web production Made of polypropylene (hereinafter also referred to as "PP") fibers with an average fiber diameter of 20 μm and a basis weight of 9 g / m 2 On top of the spunbond nonwoven fabric, a PP fiber with a basis weight of 5g / m 2 A meltblown nonwoven fabric of 9 g / m2 with an average fiber diameter of 20 μm was laminated on top of the nonwoven fabric. 2 The meltblown nonwoven fabric had a fiber diameter of 0.8 μm. (3) Linking the card web and the SNS web An SNS web, which was continuously transported in one direction, was superimposed on a card web, which was continuously transported in the same direction, and the two were bonded by ultrasonic embossing. The linear pressure of the ultrasonic embossing was set to 60 N / cm. This resulted in a sheet precursor. The shape of the bonded part was a cross shape. (4) Heat treatment of sheet precursor While both side edges of the sheet precursor being continuously conveyed in one direction were fixed by pin tenters, hot air was blown onto the sheet precursor by the air-through method. This caused the eccentric core-sheath type composite fibers constituting the carded web to develop crimps and shrink. As a result, many convex portions were formed on the SNS web. In this way, a sheet for absorbent articles having the structure shown in Figure 7(b) was obtained. This sheet for absorbent articles had elasticity. The temperature of the hot air was set to 105° C., and the speed of the hot air was set to 1.7 m / sec. The shrinkage rate of the sheet precursor was 80% in the conveying direction and 90% in the direction perpendicular to the conveying direction. (5) Adding water repellent An ethanol solution of Asahi Guard AG-E082, a fluorine-based water- and oil-repellent agent available from AGC Inc., was prepared (concentration 1%). The absorbent article sheet obtained in (4) was immersed in this ethanol solution, and then annealed and dried at 80°C for 2 hours to impart the water-repellent agent to the sheet.

[0121] Example 2 In Example 1, the fiber diameter of the constituent fibers of the meltblown nonwoven fabric in the SNS web was set to 2 μm. Except for this, a sheet for absorbent articles having the structure shown in Figures 2 and 7(b) was obtained in the same manner as in Example 1. This sheet for absorbent articles had stretchability.

[0122] Example 3 In this example, the apparatus shown in FIG. 11 was used to manufacture a sheet for absorbent articles having the structure shown in FIG. 2 and FIG. (1) Manufacturing of card web The same as in Example 1. (2) Manufacturing of meltblown composite webs A core-sheath composite fiber with a core made of polyethylene terephthalate and a sheath made of PE, with a basis weight of 9g / m 2 On top of the air-through nonwoven fabric, a PP fiber sheet with a basis weight of 5 g / m 2 The meltblown nonwoven fabrics were laminated to produce a meltblown composite web having a two-layer structure. The fiber diameter of the constituent fibers of the meltblown nonwoven fabric was 0.8 μm. The core-sheath type composite fiber constituting the air-through nonwoven fabric had a fineness of 2.4 dtex and a fiber length of 51 mm. (3) Joining the card web and the meltblown composite web A meltblown composite web, which was continuously transported in one direction, was superposed on a carded web, which was continuously transported in the same direction. The superposition was performed so that the meltblown nonwoven fabric in the meltblown composite web faced the carded web. The rest was the same as in Example 1. (4) Heat treatment of sheet precursor The same as in Example 1. (5) Adding water repellent The same procedure was followed as in Example 1. The sheet for absorbent articles thus obtained had stretchability.

[0123] Example 4 In this example, the apparatus shown in FIG. 13 was used to manufacture a sheet for absorbent articles having the structure shown in FIG. 3 and FIG. 4(b). (1) SNS web production Made of PP fibre with an average fibre diameter of 20μm and a basis weight of 9g / m 2 On top of the spunbond nonwoven fabric, a PP fiber with a basis weight of 5g / m 2 A meltblown nonwoven fabric of 9 g / m2 with an average fiber diameter of 20 μm was laminated on top of the nonwoven fabric. 2 The SNS web was manufactured by laminating the spunbond nonwoven fabric of the above three layers. The fiber diameter of the meltblown nonwoven fabric was 0.8 μm. The three layers were bonded by ultrasonic embossing. The linear pressure of the ultrasonic embossing was set to 60 N / cm. (2) SNS Web unevenness The apparatus 50 shown in FIG. 13(a) was used to impart projections and recesses to the SNS web in the procedure shown in FIG. 13(b) and FIG. 13(c). (3) Overlapping of spunbond webs The procedure shown in Fig. 13(d) was used to fabricate a 9g / m2 PP fiber sheet with an average fiber diameter of 20 μm. 2 The spunbond web was placed on the SNS web having the concave and convex shapes. Then, a heater heated to 155° C. was pressed against the spunbond nonwoven fabric to bond the spunbond web and the SNS web. (4) Adding water repellent The same procedure was followed as in Example 1. The sheet for absorbent articles thus obtained had no stretchability.

[0124] Example 5 In this example, the apparatus shown in FIG. 14 was used to manufacture a sheet for absorbent articles having the structure shown in FIG. 2 and FIG. 6(b). (1) Manufacturing of card web A carded web was produced using a core-sheath type composite fiber having a fineness of 1.8 dtex. The core of the core-sheath type composite fiber was made of polyethylene terephthalate (hereinafter also referred to as "PET") and the sheath was made of PE. The mass ratio of the core to the sheath was 5:5. (2) Primary uneven shaping of card web Using the device 60 shown in Figures 14(a) and 14(b), a card web was first unevenly shaped in the manner shown in Figures 14(c) and 14(d). The pressing depth of the pressing member 65 was set to 2 mm. (3) Secondary uneven shaping of card web Hot air was blown onto the carded web in the procedure shown in Figure 14(e) to form secondary unevenness. Hot air was blown twice. The first blowing was performed under conditions of a temperature of 160°C, a wind speed of 68 m / sec, and a blowing time of 5 seconds. The second blowing was performed under conditions of a temperature of 160°C, a wind speed of 6.0 m / sec, and a blowing time of 5 seconds. The carded web after the unevenness formation had a constituent fiber fineness of 1.8 dtex and a basis weight of 40 g / m 2 It was. (4) Overlay of SNS web Made of PP fibre with an average fibre diameter of 20μm and a basis weight of 9g / m 2 On top of the spunbond nonwoven fabric, a PP fiber with a basis weight of 5g / m 2 A meltblown nonwoven fabric of 9 g / m2 with an average fiber diameter of 20 μm was laminated on top of the nonwoven fabric. 2 The carded web was laminated with the spunbond nonwoven fabric to produce an SNS web having a three-layer structure. The fiber diameter of the constituent fibers of the meltblown nonwoven fabric was 0.8 μm. After the hot melt adhesive was applied to the carded web described above, the SNS web was placed on the applied surface, and the SNS web and the carded web were joined together. (5) Adding water repellent The same procedure was followed as in Example 1. The sheet for absorbent articles thus obtained had no stretchability.

[0125] Example 6 In Example 1, the joining pattern between the card web and the SNS web was changed, and the width and pitch of the convex portions were changed. Except for this, a sheet for absorbent articles having the structure shown in Figures 2 and 7(b) was obtained in the same manner as in Example 1. The sheet for absorbent articles obtained in this manner had stretchability.

[0126] Example 7 In Example 1, fibers that do not develop crimps when heat is applied were used as the fibers used in producing the carded web. Except for this, a sheet for absorbent articles having the structure shown in Fig. 2 and Fig. 7(b) was obtained in the same manner as in Example 1. The sheet for absorbent articles thus obtained had no stretchability.

[0127] Example 8 In Example 1, the joining pattern between the card web and the SNS web was changed, and the width and pitch of the convex portions were changed. Except for this, a sheet for absorbent articles having the structure shown in Figures 3 and 7(b) was obtained in the same manner as in Example 1. The sheet for absorbent articles obtained in this manner had stretchability.

[0128] Example 9 In this example, a sheet having the structure shown in FIG. 10 was manufactured according to the method shown in FIGS. (1) Preparation of the first fiber sheet The average fiber diameter is 15μm and the basis weight is 18g / m 2 A spunbond nonwoven fabric made of PP resin was prepared. (2) Manufacturing of the first fiber sheet A nanofiber layer made of PP resin was formed on one surface of the spunbond nonwoven fabric by electrospinning. The nanofiber layer had a basis weight of 3 g / m 2 The average fiber diameter was 500 nm. (3) Manufacturing of the second fiber sheet The average fiber diameter is 18μm and the basis weight is 18g / m 2A composite material 24B shown in FIG. 15 was produced by disposing a plurality of elastic filaments having a diameter of 100 μm between two sheets of spunbond nonwoven fabric made of PP resin. The total basis weight of the elastic filaments was 9 g / m2 relative to the area of ​​the composite material 24B. 2 This composite material 24B was passed between a pair of grooved rolls 76 and 77 shown in FIG. 16 to develop elasticity, thereby producing a second fiber sheet 24A. (4) Seat manufacturing According to the method shown in FIG. 16, the first fiber sheet 23A having the nanofiber layer and the second fiber sheet 24A were overlapped and joined together while the second fiber sheet 24A was in an elongated state, to produce a sheet.

[0129] Comparative Example 1 (1) SNS web production Made of PP fibre with an average fibre diameter of 20μm and a basis weight of 9g / m 2 On top of the spunbond nonwoven fabric, a PP fiber with a basis weight of 5g / m 2 A meltblown nonwoven fabric of 9 g / m2 with an average fiber diameter of 20 μm was laminated on top of the nonwoven fabric. 2 The SNS web was manufactured by laminating the spunbond nonwoven fabric of the above three layers. The fiber diameter of the meltblown nonwoven fabric was 0.8 μm. The three layers were bonded by ultrasonic embossing. The linear pressure of the ultrasonic embossing was set to 60 N / cm. (2) Adding water repellent The same procedure was followed as in Example 1. The sheet for absorbent articles thus obtained had no stretchability.

[0130] Comparative Example 2 The SNS web obtained in Comparative Example 1 was pressed with a concave-convex shaping press equipped with a pair of shaping plates that mesh with each other. The pressing pressure was 0.4 MPa. A sheet for absorbent articles was obtained in the same manner as in Comparative Example 1 except for this. The sheet for absorbent articles obtained in this manner had no stretchability.

[0131] 〔evaluation〕 For the absorbent article sheets obtained in the examples and comparative examples, the width W, height H, and pitch P of the convex portions were measured by the above-mentioned method. In addition, the water repellency against low surface tension liquid was evaluated by the above-mentioned method. The results are shown in Table 1. Furthermore, the degree of penetration of the low surface tension liquid into the meltblown layer was evaluated by the method described below. The results are shown in Table 1. Furthermore, the absorbent sheets obtained in the Examples and Comparative Examples were incorporated into sanitary napkins, and a dynamic seepage test was carried out according to the following procedure, and the leakproofness was evaluated according to the following criteria. The results are shown in Table 1.

[0132] [Dynamic Exudation Test] The back sheet of Kao Corporation's sanitary napkin "Lorier (registered trademark) F Happy Bare Skin Super Slim Daytime" (manufactured in 2019, 22.5 cm) was carefully removed using cold spray. In place of the removed back sheet, the absorbent article sheets obtained in the Examples and Comparative Examples were adhered to the absorbent body with hot melt. The absorbent article sheets were arranged so that the first surface having an uneven structure faced the absorbent body. A hot melt adhesive was applied to the non-skin side of the absorbent article sheet to secure the napkin to the shorts. The sanitary napkin thus obtained was placed horizontally with the topsheet facing vertically upward, and in this state, an elliptical injection port (long diameter 50 mm, short diameter 23 mm) was placed on the topsheet. 6.0 g of defibered horse blood with adjusted viscosity was injected through the elliptical injection port and allowed to stand for 1 minute. The defibered horse blood was manufactured by Japan Biotest Co., Ltd. and had a viscosity adjusted to 8 cp at a liquid temperature of 25°C. The viscosity was measured using a TVB-10M viscometer manufactured by Toki Sangyo Co., Ltd., using a rotor with the rotor name L / AdP (rotor code 19) at a rotation speed of 12 rpm. The sanitary napkin into which the fiber-free horse blood had been injected was attached to the movable female waist model shown in Fig. 9 of JP-A-9-187476, and shorts were then worn over it. After this model was made to walk at a speed of 100 steps / min for one hour, the shorts and sanitary napkin were removed and visually observed to see whether or not horse blood had seeped out of the shorts. When the absorbent sheets obtained in the Examples and Comparative Examples were incorporated into a napkin, the uneven surface of the sheet was made to face the absorbent body. However, in the case of the absorbent sheet obtained in Example 6, the uneven surface was made to face the outer surface of the napkin.

[0133] [Degree of penetration into meltblown layer] After the dynamic seepage test described above, the sanitary napkin was removed from the shorts. The non-skin side of the absorbent article sheet in the removed sanitary napkin was visually observed. When spots were confirmed in which horse blood had reached the surface of the non-skin side of the absorbent article sheet, the number of spots was visually counted. When horse blood had not reached the surface of the non-skin side of the absorbent article sheet, 10 sites were selected where the redness of the horse blood looked darker than the surroundings when the absorbent article sheet was visually observed from the non-skin side. Each site was cut in the thickness direction from the non-skin side with a razor or the like, and the cross section was observed under a microscope. When horse blood had seeped into the entire area in the thickness direction of the meltblown layer, the number of spots where the horse blood had seeped into the meltblown layer was counted.

[0134] [Table 1]

[0135] As is clear from the results shown in Table 1, the sheets for absorbent articles obtained in each Example have water repellency against low surface tension liquids. It is also evident that when the sheets for absorbent articles obtained in the respective Examples are used as the backsheet of a sanitary napkin, seepage of liquid is prevented. [Explanation of symbols]

[0136] 10. Sheets for absorbent articles 11 Convex 12 Recess 13 Spunbond layer 14 Meltblown layer 15 SNS layer 16 Joint 17 Air-through layer 21 Page 1 22 Page 2

Claims

1. A sheet for absorbent articles comprising a plurality of nonwoven fabric layers laminated together, The nonwoven fabric layers include an SNS layer in which a nanofiber layer is disposed between a pair of spunbond layers, and an air-through layer located on an outer surface of at least one of the pair of spunbond layers in the SNS layer, The fiber diameter of the constituent fibers of the nanofiber layer is 0.4 μm or more and 1 μm or less, The absorbent article sheet has a first surface on which the SNS layer is located and a second surface on which the air-through layer is located, The sheet for absorbent articles has an uneven structure on the first surface side, and the SNS layer constitutes a convex portion and a concave portion, The surface of the air-through layer facing the SNS layer has an uneven structure, and fibers constituting the air-through layer are present inside the protrusions, The outer surface of the air-through layer is flat, A sheet for absorbent articles, which has water repellency against liquids with a surface tension of 60 mN / m.

2. The sheet for absorbent articles according to claim 1 , wherein the width of the convex portions in the concave-convex structure is 0.5 mm or more and 8 mm or less.

3. A sheet for absorbent articles as described in claim 1 or 2, wherein the inside of the convex portion is filled with the constituent fibers of the air-through layer.

4. A sheet for absorbent articles as described in claim 1 or 2, wherein the inside of the convex portion is not completely filled with the constituent fibers of the air-through layer, and a space exists inside the convex portion.

5. A sheet for absorbent articles as described in any one of claims 1 to 4, wherein, on one surface of the sheet, convex portions and concave portions are alternately arranged along one direction, and convex portions and concave portions are alternately arranged along a direction perpendicular to the one direction.

6. The sheet for absorbent articles according to claim 1 , wherein the nanofiber layer is a meltblown layer.

7. A sheet for absorbent articles as described in any one of claims 1 to 4, wherein convex portions extending continuously in a stripe-like manner along one direction on one surface of the sheet and concave portions extending continuously in a stripe-like manner along the one direction are arranged alternately along a direction perpendicular to the one direction.

8. The sheet for absorbent articles according to claim 1 , wherein the air-through layer comprises crimped fibers.

9. A sheet for absorbent articles described in any one of claims 1 to 8, wherein the pitch of the convex portions in the uneven structure is 1 mm or more and 10 mm or less.

10. An absorbent article sheet described in any one of claims 1 to 9, wherein the nanofiber layer has a thickness of 3 μm or more and 150 μm or less.

11. An absorbent article comprising an absorbent body and the sheet for absorbent articles according to any one of claims 1 to 10, The sheet for absorbent articles is arranged so that the surface of the SNS layer having the uneven structure in the sheet for absorbent articles faces the absorbent body.

12. The absorbent article according to claim 11, wherein the sheet for absorbent articles is disposed on a non-skin facing side of the absorbent body.

Citation Information

Patent Citations

  • High-bulk laminated material provided with pillow part by stretching and its production

    JP1994255006A

  • Trunks type disposable pants

    JP2001224615A

  • Disposable diaper

    JP2002360629A

  • Nonwoven fabric for hygienic material

    JP2004129810A

  • Disposable pants-type diaper

    JP2005027838A