Modified polyolefin resin composition

The modified polyolefin resin composition addresses viscosity issues by stabilizing the acid-modified polyolefin resin with an alcohol, ensuring long-term adhesion and stability, particularly in the presence of hydroxyl-containing substances.

JP7581185B2Active Publication Date: 2024-11-12NIPPON PAPER IND CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021514924
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-17
Filing Date
2020-04-10
Publication Date
2024-11-12
Estimated Expiration
2040-04-10

AI Technical Summary

Technical Problem

Acid-modified polyolefin resins experience viscosity increase when stored for long periods, especially when substances containing hydroxyl groups are present, leading to difficulties in application and adhesion to substrates.

Method used

A modified polyolefin resin composition is developed by grafting an α,β-unsaturated carboxylic acid derivative onto polyolefin, followed by modification with an alcohol to stabilize the structure and inhibit crosslinking, maintaining adhesion and stability.

Benefits of technology

The composition ensures good adhesion to non-polar resin substrates and maintains stability over time, preventing thickening and ensuring effective dispersion and hue stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581185000001
    Figure 0007581185000001
  • Figure 0007581185000002
    Figure 0007581185000002
  • Figure 0007581185000003
    Figure 0007581185000003
Patent Text Reader

Abstract

The present invention provides a modified polyolefin resin composition that includes a modified polyolefin resin (X) in which an acid-modified polyolefin resin (A) is modified by a modifying component including an alcohol (B) and satisfies (I)-(III), and the use thereof. (I) Resin (A) is a resin in which a polyolefin (a) is modified by an α,β-unsaturated carboxylic acid and a derivative thereof (b) having a structure (b1) derived from at least one carboxyl group. (II) The residual percentage of structure (b1) in resin (X) is from more than 0% to 50%. (III) The content of alcohol in the composition is 1.0-5.0 mol per 1.0 mol of structure (b1) in resin (A).
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a modified polyolefin resin composition, and more particularly to a modified polyolefin resin composition, its uses, and its production method. [Background technology]

[0002] Polyolefin substrates are inexpensive, lightweight, easy to process, and have many other advantages, and are widely used as substrates for various products such as automobiles and food packaging. A problem with polyolefin substrates is that they have low surface free energy, resulting in low adhesion to paints and inks. When modified polyolefin resins are used as active ingredients in paints, acid-modified polyolefin resins are widely used to improve the coatability of polyolefin substrates. By acid modification treatment, which modifies polyolefins with acid components, acid component groups can be grafted to polyolefin chains. As a result, acid-modified polyolefin resins exhibit good affinity with paints and can ensure adhesion between the substrate and the paint. Acid modification treatment with maleic anhydride is usually performed by extrusion modification using an extruder, or solution modification in a solution, both of which can be performed easily and inexpensively. For this reason, acid-modified polyolefin resins are widely used (e.g., Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2004-114610 A Summary of the Invention [Problem to be solved by the invention]

[0004] One of the problems with acid-modified polyolefin resins is that when a dispersion (or solution) of the acid-modified polyolefin resin is left standing for a long time, the solution thickens. In particular, when a substance containing a hydroxyl group or a substance containing a hydroxyl group equivalent structure is mixed into a dispersion containing an acid-modified polyolefin resin, the dispersion thickens significantly. This is thought to be because the acid component group in the acid-modified polyolefin resin reacts with the hydroxyl group to form a crosslinked structure. When the dispersion thickens, it becomes difficult to mix the dispersion into a paint or to apply it to a substrate, making it unsuitable for practical use. Up to now, attempts have been made to suppress the thickening of the dispersion, but all of them have problems such as not being able to guarantee adhesion to the substrate and not being able to suppress the thickening during storage at high temperatures for long periods of time.

[0005] An object of the present invention is to provide a modified polyolefin resin composition containing an acid-modified polyolefin resin, which has good storage stability at high temperatures and for long periods while ensuring good adhesion (bonding) to a substrate. [Means for solving the problem]

[0006] The present invention provides [1] to

[15] . [1] A modified polyolefin resin composition comprising a modified polyolefin resin (X) in which an acid-modified polyolefin resin (A) is modified with a modifying component containing an alcohol (B), and which satisfies the following (I) to (III): (I) The acid-modified polyolefin resin (A) is a resin in which a polyolefin (a) is modified with an α,β-unsaturated carboxylic acid or its derivative (b) having a structure (b1) derived from at least one carboxyl group. (II) The residual rate of the structure (b1) in the modified polyolefin resin (X) is more than 0% and not more than 50%. (III) The content of alcohol in the composition is 1.0 to 5.0 mol per 1.0 mol of the structure (b1) contained in the acid-modified polyolefin resin (A). [2] The modified polyolefin resin composition according to [1], wherein the structure (b1) is a group represented by the formula (1): -(C=O)-O-(C=O)-. [3] The modified polyolefin resin composition according to [1] or [2], wherein the α,β-unsaturated carboxylic acid and its derivative (b) is an α,β-unsaturated polycarboxylic acid cyclic anhydride. [4] The modified polyolefin resin composition according to any one of [1] to [3], wherein the modified polyolefin resin (X) is a modified chlorinated polyolefin resin (X1). [5] The modified polyolefin resin composition according to any one of [1] to [4], wherein the acid-modified polyolefin resin (A) is an acid-modified chlorinated polyolefin resin (A1). [6] The modified polyolefin resin composition according to any one of [1] to [5], further comprising a substance (D) having a hydroxyl group or a hydroxyl group equivalent structure. [7] The modified polyolefin resin composition according to any one of [1] to [6], wherein the alcohol (B) contains at least an alcohol having 2 to 4 carbon atoms. [8] The modified polyolefin resin composition according to any one of [1] to [7], wherein the alcohol (B) contains at least a primary alcohol. [9] The modified polyolefin resin composition according to any one of [1] to [8], further comprising an organic solvent (C).

[10] The modified polyolefin resin composition according to any one of [1] to [9], wherein the content of the α,β-unsaturated carboxylic acid and its derivative (b) in the acid-modified polyolefin resin (A) is 0.5 to 20% by weight.

[11] The modified polyolefin resin composition according to any one of [1] to

[10] , wherein the acid-modified polyolefin resin (A) has a weight average molecular weight of 5,000 to 300,000.

[12] A primer comprising the modified polyolefin resin composition according to any one of [1] to

[11] .

[13] A coating material comprising the modified polyolefin resin composition according to any one of [1] to

[11] .

[14] An ink comprising the modified polyolefin resin composition according to any one of [1] to

[11] .

[15] Modifying a polyolefin (a) with an α,β-unsaturated carboxylic acid having a structure (b1) derived from at least one carboxyl group and a derivative thereof (b) to obtain an acid-modified polyolefin resin (A); and modifying an acid-modified polyolefin resin (A) with a modifying component containing an alcohol (B) in an amount of 1.0 to 5.0 mol per 1.0 mol of the structure (b1) of the acid-modified polyolefin resin (A) to obtain a modified polyolefin resin (X); The method for producing the modified polyolefin resin composition according to any one of [1] to

[11] , comprising at least Effect of the Invention

[0007] The modified polyolefin resin composition of the present invention has good high-temperature and long-term storage stability while ensuring good adhesion to non-polar resin substrates such as polyolefin resins. In addition, the modified polyolefin resin composition of the present invention is inhibited from thickening even after long-term storage at high temperatures in the presence of a substance containing a hydroxyl group or a hydroxyl group equivalent structure, and can exhibit good adhesion, pigment dispersibility, and color stability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The modified polyolefin resin composition contains a modified polyolefin resin (X). The modified polyolefin resin (X) is a resin obtained by modifying an acid-modified polyolefin resin (A) with an alcohol (B).

[0009] [Acid-modified polyolefin resin (A)] The acid-modified polyolefin resin (A) (hereinafter sometimes referred to as "resin (A)") is an acid-modified polyolefin resin in which a polyolefin (a) is graft-modified with an α,β-unsaturated carboxylic acid and its derivative (b) (hereinafter sometimes referred to as "acid component (b)") (condition (I)), and has a structure derived from the polyolefin (a) and a structure derived from the acid component (b). The resin (A) may be one type of acid-modified polyolefin resin or a combination of two or more types. In this specification, the acid-modified polyolefin resin may be an acid-modified chlorinated polyolefin resin or an acid-modified non-chlorinated polyolefin resin.

[0010] (Polyolefin (a)) The polyolefin (a) may be a polymer of an olefin. The polymerization catalyst used for the polymerization of the olefin is not particularly limited, but is preferably a Ziegler-Natta catalyst or a metallocene catalyst. By using a metallocene catalyst, it is possible to obtain a polyolefin (a) having characteristics such as a narrow molecular weight distribution, excellent random copolymerization, a narrow composition distribution, and a wide range of comonomers that can be copolymerized. The metallocene catalyst may be a known one. For example, a catalyst obtained by combining the following components (1) and (2), and further, if necessary, component (3) may be mentioned. Among them, the metallocene catalyst is preferably a catalyst obtained by combining the following components (1) and (2), and further, if necessary, component (3). Component (1): A metallocene complex which is a transition metal compound of Groups 4 to 6 of the periodic table having at least one conjugated five-membered ring ligand. Component (2): Ion-exchangeable layered silicate. Component (3): Organoaluminum compound.

[0011] Examples of polyolefin (a) include polypropylene resins and propylene-based copolymers (random copolymers, block copolymers) obtained by copolymerizing propylene with α-olefins (e.g., ethylene, butene, 3-methyl-1-butene, 3-methyl-1-heptene). Preferred are propylene-based copolymers (especially random copolymers) obtained using a metallocene catalyst, more preferably polypropylene resins, ethylene-propylene copolymers, propylene-butene copolymers, or ethylene-propylene-butene copolymers (especially random copolymers) obtained using a metallocene catalyst, and even more preferably ethylene-propylene copolymers (especially random copolymers).

[0012] The propylene unit content of the polyolefin (a) is preferably 60% by weight or more, more preferably 70% by weight or more, and even more preferably 80% by weight or more. The propylene unit content of the polyolefin (a) may be the proportion of the raw material used or may be a value calculated by NMR analysis. Both values ​​usually coincide with each other.

[0013] The structure of the polyolefin (a) may be any of isotactic, atactic, and syndiotactic structures that can be taken by ordinary polymer compounds, and polyolefins having an isotactic structure are preferred. Polyolefins obtained using a metallocene catalyst usually have an isotactic structure.

[0014] The polyolefin (a) may be one kind of polyolefin (a) alone, or may be a combination of a plurality of polyolefins (a).

[0015] (Acid component (b)) The acid-modified polyolefin resin (A) is obtained by graft-modifying the polyolefin (a) with the acid component (b). The acid-modified polyolefin resin (A) contains a structure derived from the acid component (b), so that the modified polyolefin resin composition can exhibit better adhesion, solution stability, pigment dispersibility, and color stability. As described above, the acid component (b) is an α,β-unsaturated carboxylic acid or a derivative thereof.

[0016] The α,β-unsaturated carboxylic acid and its derivatives have a structure (b1) (hereinafter also referred to as "structure (b1)") derived from at least one carboxyl group. Examples of the structure (b1) include substituents such as amino groups, sulfonic acid groups, and carboxyl groups, and structures derived from these substituents. The structure (b1) is preferably a structure derived from two or more carboxyl groups, more preferably a divalent group in which two or more carboxyl groups are condensed, and even more preferably a group represented by formula (1): -(C=O)-O-(C=O)-.

[0017] Examples of the α,β-unsaturated carboxylic acid and its derivative having the structure (b1) include maleic anhydride, citraconic anhydride, itaconic anhydride, aconitic anhydride, maleic acid, citraconic acid, itaconic acid, aconitic acid, (meth)acrylonitrile, (meth)acrylamide, N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, N,N-dimethylaminopropyl (meth)acrylamide, methylene bis (meth)acrylamide, ethylene bis (meth)acrylamide, dimethylaminoethyl (meth)acrylate, an adduct of glycidyl (meth)acrylate and amines, and polymerizable unsaturated monomers having a sulfonic acid group. Among them, maleic anhydride, aconitic anhydride, and itaconic anhydride are preferred, and maleic anhydride is more preferred.

[0018] The acid component (b) may be a compound selected from a single type of α,β-unsaturated carboxylic acid and its derivatives, or a combination of two or more types. Examples of the combination of two or more types include a combination of one or more of the above α,β-unsaturated carboxylic acids and one or more of their derivatives, a combination of two or more of the above α,β-unsaturated carboxylic acids, and a combination of two or more of the above derivatives of the α,β-unsaturated carboxylic acids. Any of these combinations may be used.

[0019] (Acid component (b) content) The content of the acid component (b) (ratio of the content of the acid component (b) to the content of the resin (A) (wt%); graft weight) is preferably 0.5 wt% or more, more preferably 1.0 wt% or more, and even more preferably 2.0 wt% or more. The upper limit is preferably 20.0 wt% or less, more preferably 15.0 wt% or less. Therefore, the content of the acid component (b) is preferably 0.5 to 20 wt%, more preferably 1.0 to 20.0 wt%, and even more preferably 2.0 to 15.0 wt%. This can improve the adhesion to the substrate. The content of the acid component (b) can be measured by alkali titration based on a method in accordance with JIS K 0070:1992.

[0020] (Method for producing resin (A)) The method for producing the resin (A) is not particularly limited as long as it is a method that at least includes modifying the polyolefin (a) with the acid component (b). For example, there is a method in which the polyolefin (a) is graft-modified with the acid component (b), and preferably, the method in which the polyolefin (a) is radical-reacted with the acid component (b) in the presence of a radical generator.

[0021] (Radical generator) The radical generator may be appropriately selected from known radical generators, and organic peroxide compounds are preferred.As organic peroxide compounds, for example, di-t-butyl peroxide, dicumyl peroxide, t-butyl cumyl peroxide, benzoyl peroxide, dilauryl peroxide, cumene hydroperoxide, t-butyl hydroperoxide, 1,4-bis[(t-butylperoxy)isopropyl]benzene, 1,1-bis(t-butylperoxy)-3,5,5-trimethylcyclohexane, 1,1-bis(t-butylperoxy)-cyclohexane, cyclohexanone peroxide, t-butyl peroxybenzoate, t-butyl peroxyisobutyrate, t-butyl peroxy-3,5,5-trimethylhexanoate, t-butyl peroxy-2-ethylhexanoate, t-butyl peroxyisopropyl carbonate, cumyl peroxyoctoate can be mentioned. Of these, di-t-butyl peroxide, dicumyl peroxide, and dilauryl peroxide are preferred.

[0022] The radical generator may be a single type of radical generator or a combination of multiple types of radical generators.

[0023] The amount of the radical generator used is preferably 0.1% by weight or more, more preferably 1% by weight or more, based on the total weight of the polyolefin (a). This allows sufficient graft efficiency to be maintained. The upper limit is usually 100% by weight or less, preferably 50% by weight or less. This allows the weight average molecular weight of the polyolefin (a) to be prevented from decreasing. Therefore, the amount is preferably 0.1 to 100% by weight, more preferably 1 to 50% by weight.

[0024] (Weight average molecular weight of resin (A)) The weight average molecular weight of the resin (A) is preferably 5,000 or more, more preferably 7,000 or more, even more preferably 10,000 or more, and even more preferably 30,000 or more or 50,000 or more. The upper limit is preferably 300,000 or less, more preferably 250,000 or less, even more preferably 200,000 or less, even more preferably 150,000 or less or 120,000 or less. Therefore, the weight average molecular weight of the resin (A) is preferably 5,000 to 300,000, more preferably 7,000 to 250,000, even more preferably 10,000 to 200,000, even more preferably 30,000 to 150,000, and particularly preferably 50,000 to 150,000. This can improve the solution properties when the modified polyolefin resin composition is dispersed in an organic solvent, and can improve the adhesion to the substrate.

[0025] The weight average molecular weight can be determined from a standard polystyrene calibration curve by gel permeation chromatography (GPC). The measurement conditions for GPC are shown below. Equipment: HLC-8320GPC (Tosoh Corporation) Column: TSK-gel G-6000 H×L, G-5000 H×L, G-4000 H×L, G-3000 H×L, G-2000 H×L (Tosoh Corporation) Eluent:THF Flow rate: 1mL / min Temperature: Pump oven, column oven 40℃ Injection volume: 100μL Standard material: Polystyrene EasiCal PS-1 (Agilent Technology)

[0026] [Denaturing ingredients including alcohol (B)] (Alcohol (B)) Alcohol (B) is one of the modifying components when obtaining modified polyolefin resin (X) from acid-modified polyolefin resin (A). It is presumed that when alcohol (B) acts on acid-modified polyolefin resin (A), it can convert structure (b1) in resin (A) into a more stable structure (e.g., when structure (b1) is a group represented by formula (1), it can be converted into an ester).

[0027] The alcohol preferably has 2 to 4 carbon atoms and / or is a primary alcohol. This improves the reactivity of the acid component (b) grafted to the resin (A) with the alcohol (B), suppressing the increase in molecular weight over time, and as a result, the thickening suppression effect can be fully exerted. It is presumed that the effect of improving the reactivity of the acid component (b) with the alcohol (B) is due to the fact that the bulkiness of the alcohol molecule becomes smaller, making it easier to approach the acid component (b) grafted to the resin. Examples of the alcohol include ethanol, 1-propanol, and 1-butanol. The alcohol (B) may be a single alcohol or a combination of two or more alcohols.

[0028] The alcohol (B) can improve the storage stability of the modified polyolefin resin composition (preferably in the form of a dispersion containing an organic solvent). The mechanism is presumed to be as follows. When the resin (A) is dispersed in an organic solvent to obtain a dispersion, and the alcohol (B) is added to the obtained dispersion, the acid component (b) reacts with the alcohol (B) to form an ester structure. Therefore, it is presumed that the interaction between the acid components (b) in the dispersion can be inhibited, and the association of the resin components can be suppressed. In addition, when the dispersion further contains a substance (D) containing a hydroxyl group, it is presumed that the reaction between the acid component (b) and the hydroxyl group can be inhibited, and the formation of a crosslinked structure can be suppressed.

[0029] (Alcohol (B) content) The content of the alcohol (B) in the modified polyolefin resin composition (amount relative to 1 mol of the structure (b1)) is preferably 1.0 mol or more, more preferably 1.2 mol or more, and even more preferably 1.3 mol or more. The upper limit is preferably 5.0 mol or less, more preferably 4.9 mol or less, even more preferably 4.5 mol or less or 4.0 mol or less. Therefore, the content of the alcohol (B) is preferably 1.0 to 5.0 mol (condition (III)), more preferably 1.2 to 4.9 mol, even more preferably 1.2 to 4.5 mol, and even more preferably 1.3 to 4.0 mol. This can increase the storage stability of the dispersion, and the modified polyolefin resin can be well dispersed in the dispersion. The content of the alcohol (B) corresponds to the amount of alcohol added when modifying the resin (A). Therefore, the amount of unreacted alcohol that may be contained in the modified polyolefin resin composition is also included in the above content.

[0030] (Denaturing ingredients other than alcohol) Examples of the modifying component other than the alcohol (B) include α,β-unsaturated carboxylic acids (e.g., acrylic acid, methacrylic acid, maleic acid, citraconic acid, fumaric acid, mesaconic acid, itaconic acid, aconitic acid), (meth)acrylic acid esters, (meth)acrylonitrile, monomers containing a vinyl group (e.g., styrene, vinyl acetate), polystyrene, or macromonomers having a polymerizable (meth)acryloyl group at the end of poly(meth)acrylate. The modifying component other than the alcohol (B) may include an acid component (b).

[0031] (Method of modification using a modifying component containing alcohol (B)) The method of modifying the resin (A) with the modifying component containing the alcohol (B) may be, for example, a method in which the resin (A) and the modifying component containing the alcohol (B) are simultaneously or sequentially dispersed or dissolved in a solvent (e.g., an organic solvent (C)) and reacted. The conditions for modification are not particularly limited.

[0032] [Remaining rate of structure (b1)] The residual ratio of structure (b1) in modified polyolefin resin (X) is the ratio of the amount of structure (b1) in modified polyolefin resin (X) to the amount of structure (b1) in acid-modified polyolefin resin (A). It is a value indicating the degree to which structure (b1) remains after modification with a modifying component containing alcohol (B) before modification.

[0033] The residual rate of the structure (b1) in the modified polyolefin resin (X) is usually 50% or less (condition (II)), preferably 45% or less, more preferably 40% or less, and even more preferably 30% or less. The lower limit of the residual rate is usually more than 0%, preferably 2% or more, more preferably 5% or more, and even more preferably 10% or more. When the residual rate is within the above-mentioned range, the polarity of the modified polyolefin resin remains in an optimal range, and the modified polyolefin resin components appropriately interact with each other, the solvent molecules in the system, and other molecules, improving the solution stability.

[0034] The residual rate is the ratio (%) of the amount of structure (b1) in the modified polyolefin resin (X) to the amount of structure (b1) in the acid-modified polyolefin resin (A), and can be calculated by the following formula (1). Formula (1): Residual rate of structure (b1) (%) = Ac / Aa × 100 Aa: 1780 cm in the infrared absorption spectrum of acid-modified polyolefin resin (A) -1 The peak area around 1450 cm is characteristic of polyolefins. -1 Divided by the area of ​​the peak nearby Ac: 1780cm in the infrared absorption spectrum of modified polyolefin resin (X) -1 The peak area around 1450 cm is characteristic of polyolefins. -1 Divided by the area of ​​the peak nearby

[0035] [Chlorination] The modified polyolefin resin (X) may be a modified chlorinated polyolefin resin (X1) or a modified non-chlorinated polyolefin resin (X2). By using the modified chlorinated polyolefin resin (X1), adhesion to non-polar resin substrates and compatibility with other components are improved, and good pigment dispersibility and color stability are obtained.

[0036] (Chlorination Method) The modified chlorinated polyolefin resin (X1) may be obtained by chlorination at any stage of production. Examples of the stage at which chlorination is carried out include (Example 1) chlorination of polyolefin (a) (before graft polymerization of acid component (b)), (Example 2) chlorination of resin (A) (after graft polymerization of acid component (b)), and (Example 3) after modification with alcohol (B). Examples 1 and 2 are preferred, and Example 2 is more preferred. That is, it is preferred that resin (A) is an acid-modified chlorinated polyolefin resin (A1).

[0037] Chlorination may be any method that introduces chlorine atoms into the target material, and may be, for example, a method in which the target material is dissolved in a solvent such as water, carbon tetrachloride, or a chlorine-based solvent (e.g., chloroform) and then chlorine gas is blown into the solution. When blowing in chlorine gas, ultraviolet light may be irradiated or a radical reaction initiator may be present, if necessary. Examples of radical reaction initiators include organic peroxide compounds (e.g., the organic peroxide compounds exemplified in the above description of the radical generator) and azonitriles (e.g., azobisisobutyronitrile). The pressure and temperature when blowing in chlorine gas are not particularly limited, but the pressure may be either normal pressure or under pressure. The temperature is usually 50 to 140°C. The chlorine-based solvent in the system is usually distilled off by reducing pressure or the like after the chlorination is completed, or replaced with an organic solvent.

[0038] (Chlorine content (chlorination degree)) The chlorine content of the modified chlorinated polyolefin resin (X1) is not particularly limited. For example, the chlorine content of the acid-modified chlorinated polyolefin resin (A1) is preferably 10% by weight or more, more preferably 15% by weight or more. The upper limit is preferably 40% by weight or less, more preferably 30% by weight or less. Therefore, the chlorine content of the acid-modified chlorinated polyolefin resin (A1) is preferably 10 to 40% by weight, more preferably 15 to 30% by weight. This allows the polarity of the modified polyolefin resin composition to be adjusted within a certain range. As a result, when used together with other resin components for coating applications, the compatibility with the other resin components can be improved. In addition, the modified polyolefin resin composition can exhibit sufficient adhesion to non-polar substrates such as polyolefin resins. The chlorine content can be measured based on JIS-K7229:1995. The chlorine contents of the resins (X1) and (A1) are usually the same value.

[0039] [Organic solvent (C)] The organic solvent (C) is one of the optional components that the modified polyolefin resin composition may contain in addition to the modified polyolefin resin (X) described above. By containing the organic solvent (C) (hereinafter sometimes referred to as "solvent (C)"), the modified polyolefin resin composition can more efficiently exert the effects of the present invention in various applications as a dispersion.

[0040] Examples of the solvent (C) include aromatic solvents such as toluene and xylene, ester solvents such as ethyl acetate and butyl acetate, ketone solvents such as methyl ethyl ketone, methyl butyl ketone and ethylcyclohexane, and aliphatic or alicyclic hydrocarbon solvents such as cyclohexane, methylcyclohexane, nonane and decane. The solvent (C) may be one of the above organic solvents alone or a combination of two or more of them (e.g., a mixed solvent).

[0041] The content of the solvent (C) (amount relative to the resin (A)) is not particularly limited, but is preferably 10% by weight to 90% by weight, and more preferably 20% by weight to 80% by weight.

[0042] [Substances containing hydroxyl groups or hydroxyl equivalent structures (D)] The substance (D) containing a hydroxyl group or a hydroxyl group equivalent structure (hereinafter sometimes referred to as "substance (D)") is one of the optional components that the modified polyolefin resin composition may contain in addition to the modified polyolefin resin (X) described above. By containing the substance (D), effects such as further improvement of adhesion to the substrate and prevention of deterioration of the resin component can be exhibited.

[0043] Examples of the substance containing a hydroxyl group (hereinafter, sometimes referred to as "substance (D-1)") include resins other than polyolefin (a), such as acrylic resins, polyol resins, and polyurethane resins, and acrylic resins are preferred. The acrylic resin is preferably an acrylic resin having one hydroxyl group at one end or an acrylic resin having a diol at one end, and more preferably an acrylic resin having a diol at one end. The molecular weight of the acrylic resin is preferably 1,000 to 200,000, more preferably 3,000 to 100,000. The hydroxyl value of the acrylic resin is preferably 1 to 200, more preferably 10 to 100. In addition, examples of the effects of including substance (D-1) include the following effects: improved adhesion to substrates; and, when a topcoat agent is further applied, improved adhesion due to interaction with the topcoat agent.

[0044] Examples of substances containing a hydroxyl group equivalent structure (hereinafter, sometimes referred to as "substance (D-2)") include compounds containing an epoxy ring, such as epoxy-based stabilizers. Examples of epoxy-based stabilizers include epoxy compounds having an epoxy equivalent of about 100 to 500 and containing one or more epoxy groups in one molecule. More specifically, the following compounds can be mentioned:

[0045] Epoxidized soybean oil and linseed oil obtained by epoxidizing vegetable oils having natural unsaturated groups with a peracid such as peracetic acid; epoxidized fatty acid esters obtained by epoxidizing unsaturated fatty acids such as oleic acid, tall oil fatty acid, and soybean oil fatty acid; epoxidized alicyclic compounds such as epoxidized tetrahydrophthalate; condensation of bisphenol A or polyhydric alcohol with epichlorohydrin, such as bisphenol A glycidyl ether, ethylene glycol glycidyl ether, propylene glycol glycidyl ether, glycerol polyglycidyl ether, and sorbitol polyglycidyl ether; and monoepoxy compounds such as butyl glycidyl ether, 2-ethylhexyl glycidyl ether, decyl glycidyl ether, stearyl glycidyl ether, allyl glycidyl ether, phenyl glycidyl ether, sec-butylphenyl glycidyl ether, tert-butylphenyl glycidyl ether, and phenol polyethylene oxide glycidyl ether. Further, a stabilizer that does not contain an epoxy ring may be used, and examples thereof include metal soaps such as calcium stearate and lead stearate, which are used as stabilizers for polyvinyl chloride resins; organometallic compounds such as dibutyltin dilaurate and dibutyl maleate; and hydrotalcite compounds.

[0046] By including the substance (D-2), it is possible to capture hydrogen chloride that is generated when the polyolefin resin component is chlorinated, thereby preventing deterioration of the resin component.

[0047] The content of the substance (D) (amount relative to the resin (A)) is preferably 1% by weight or more, more preferably 10% by weight or more, and even more preferably 30% by weight or more. The upper limit is preferably 300% by weight or less, more preferably 200% by weight or less, and even more preferably 100% by weight or less. Therefore, the content of the substance (D) is preferably 1 to 300% by weight, more preferably 10 to 200% by weight, and even more preferably 30 to 100% by weight. This can enhance the interaction with the substrate and topcoat, and ensure sufficient adhesion. In addition, when the modified polyolefin resin composition contains a solvent (C), the substance (D) can be well dispersed in the resin solution.

[0048] The substance (D) may be one selected from the above substances (D-1) and (D-2) alone or a combination of two or more thereof, but it is preferable that the substance (D) contains at least one each of substances (D-1) and (D-2).

[0049] [Resin (X) content] The content (solid content) of the modified polyolefin resin (X) in the modified polyolefin resin composition may be appropriately set according to the application of the modified polyolefin resin composition, and is preferably 10% by weight or more, more preferably 20% by weight or more. This further improves the adhesion to various substrates. The upper limit may be 100% by weight, and is preferably 90% by weight or less, more preferably 80% by weight or less.

[0050] [Optional ingredients] The modified polyolefin resin composition contains at least the modified polyolefin resin (X) described above, and may further contain an organic solvent (C) and a substance (D) as described above. In addition, it may contain optional components as necessary. Examples of optional components include stabilizers, resins other than the modified polyolefin resin (X) (e.g., polyolefin (a), chlorinated polyolefin resins, resins other than polyolefin (a) and substance (D) (e.g., alkyd resins, polyacrylic polyols, polyester resins, polyester polyols, polyether resins, polyether polyols, polyurethane resins)), unreacted modified components (e.g., acid component (b), alcohol (B), modified components other than alcohol (B)), pigments, and additives (e.g., ultraviolet absorbers, antioxidants, pigment sedimentation inhibitors).

[0051] [Dispersion] The form of the modified polyolefin resin composition is not particularly limited. For example, it may be a dispersion, a solution, or a solid, but is preferably a dispersion. The dispersion as the modified polyolefin resin composition can be obtained by heating and stirring each component constituting the composition.

[0052] [Uses of modified polyolefin resin composition] The modified polyolefin resin composition has excellent adhesion and maintains good solution properties even after long-term storage, and can therefore be suitably used, for example, as a binder (e.g., paint binder, ink binder), primer, paint, ink, adhesive, etc. The binder, primer, paint, and ink containing the modified polyolefin resin composition may contain components other than the modified polyolefin resin composition (e.g., so-called additives such as antioxidants, light stabilizers, ultraviolet absorbers, pigments, dyes, and inorganic fillers) as necessary.

[0053] [Method of producing modified polyolefin resin composition] The modified polyolefin resin composition described above is A polyolefin (a) is modified with an α,β-unsaturated carboxylic acid having a structure (b1) derived from at least one carboxyl group and a derivative thereof (b) to obtain an acid-modified polyolefin resin (A); and The acid-modified polyolefin resin (A) is modified with a modifying component containing an alcohol (B) in an amount of 1.0 to 5.0 mol per 1.0 mol of the structure (b1) of the acid-modified polyolefin resin (A) to obtain a modified polyolefin resin (X). The respective raw materials and the conditions for modification and the like are as described above.

[0054] The above-mentioned production method may include adding an organic solvent (C), a substance (D), and other components to the composition as needed. The timing of adding these components is not particularly limited, and they may be added during modification with the acid component (b), during modification with the alcohol (B), or to the modified polyolefin resin (X). The organic solvent (C) is preferably added to the acid-modified polyolefin resin (A) during modification with the alcohol (B), and more preferably, the acid-modified polyolefin resin (A) is added to the organic solvent (C) to dissolve or disperse it, and then the alcohol (B) is added. The substance (D-1) is preferably added to the acid-modified polyolefin resin (A) during modification with the alcohol (B), and more preferably, it is added simultaneously with the addition of the alcohol (B) or subsequent to the addition of the alcohol (B). The substance (D-2) is preferably added during the production process of the modified polyolefin resin (X), and more preferably, it is added after the acid modification or after the chlorination that is performed as needed. EXAMPLES

[0055] The present invention will be described in detail below with reference to examples. The following examples are provided to better explain the present invention, but are not intended to limit the present invention. The measurement and evaluation methods for the physical properties of the production examples, examples, and comparative examples are shown below (unless otherwise specified, the above-mentioned methods were followed). In addition, "parts" are by weight unless otherwise specified.

[0056] [Weight average molecular weight (Mw) and number average molecular weight (Mn)] The resins produced in the Production Examples were measured by GPC under the following conditions. Equipment: HLC-8320GPC (Tosoh Corporation) Column: TSK-gel G-6000 H×L, G-5000 H×L, G-4000 H×L, G-3000 H×L, G-2000 H×L (Tosoh Corporation) Eluent:THF Flow rate: 1mL / min Temperature: Pump oven, column oven 40℃ Injection volume: 100μL Standard material: Polystyrene EasiCal PS-1 (Agilent Technology)

[0057] [Acid component (b1) content (%)] The measurement was carried out using an alkali titration method in accordance with JIS K 0070:1992.

[0058] [Chlorine content (wt%)] The measurements were carried out according to JIS-K7229:1995.

[0059] [Evaluation of the stability of the dispersion immediately after preparation] The dispersions with a resin component solid content of 50% prepared in the examples and comparative examples were visually evaluated for solution properties immediately after preparation and classified into the following categories A to D. If they fall into the categories A to C, it can be determined that there is no problem in practical use. A: No thickening or separation of the solution was observed, and the solution was transparent in color. B: The solution does not thicken or separate, but is slightly cloudy. C: No separation of the solution is observed, but the solution is clearly cloudy. D: The solution separates into two layers, becomes significantly more viscous, or aggregates are visually observed.

[0060] [Residual ratio of structure represented by the formula: -(C=O)-O-(C=O)-] The infrared absorption spectrum of the acid-modified polyolefin obtained in each production example was measured, and the infrared absorption spectrum was -1 The peak present around 1450 cm is considered to be a peak specific to the structure. -1The value obtained by dividing the area by the peak area specific to the polyolefin present in the vicinity was designated as Aa. Next, the infrared absorption spectrum of the dispersion obtained in each example (1 hour after adding the alcohol (B)) was measured, and the value Ac was obtained by the same procedure as for Aa. The values ​​Aa and Ac were substituted into the following formula (1) to obtain the residual ratio of the structure. Formula (1): Survival rate=Ac / Aa×100(%)

[0061] [Evaluation of storage stability of dispersion] The dispersions judged as A to C in the evaluation test of the stability of the dispersion immediately after preparation were subjected to this test. The dispersions with a solid content of 50% of the resin component prepared in the examples and comparative examples were stored at 40°C for one month, and then the solution properties were similarly visually observed. If the dispersions were rated as A to C, they could be judged to have no practical problems. A: No thickening or separation of the solution was observed, and the appearance was the same as immediately after preparation. B: No thickening or separation of the solution was observed, but the solution was slightly more thick than immediately after preparation. C: No separation of the solution is observed, but the viscosity has clearly increased compared to immediately after preparation. D: The solution separates into two layers, becomes significantly more viscous, or aggregates are visually observed. The dispersions that were determined to have no practical problems in this test were subjected to an adhesion test.

[0062] [Preparation of test specimens] The surface of an ultra-high rigidity polypropylene plate was degreased with isopropyl alcohol, spray-painted with a dispersion of resin components so that the dry coating thickness was 10 to 15 μm, and preheated for 5 minutes at the melting point of the resin components + 15°C. Next, 1K base (1K coating for base coat) containing resin components was spray-painted, and after leaving it to stand for 10 minutes, 2K clear (2K coating for base coat) was painted. After that, a baking process was performed for 30 minutes at the melting point of the resin components + 15°C to prepare a test specimen. The following adhesion test was performed using this test specimen.

[0063] [Adhesion test] Linear indentations were made vertically and horizontally at 1 mm intervals on the coating film of the test piece, reaching the base material, to create 100 sections (grids), which were then adhered with cellophane adhesive tape and peeled off in a 180° direction. The operation of adhering the cellophane adhesive tape and peeling it off was performed 10 times for each of the 100 sections, and the adhesion (bonding) was evaluated according to the following criteria. If 50 or fewer sections of the coating film peeled off (i.e., evaluations A to C), it can be determined that there is no problem in practical use. A: There is no peeling of the coating. B: The number of peeled sections of the coating is 1 to 10. C: The number of peeled sections of the coating is more than 10 and not more than 50. D: More than 50 patches of peeled coating.

[0064] [Pigment dispersion and preparation of pigmented paints]: 40 parts of the dispersion liquid with a solid content of 50% of the resin component prepared in the examples and comparative examples, 20 parts of pigment, 10 parts of xylene, 10 parts of butyl acetate, and glass beads of the same volume as the resin component were charged into a batch SG mill and dispersed for 4 hours (60 mm impeller, 2000 rpm). 20 parts of acrylic resin were further blended and stirred with a disperser to prepare pigmented paints (blue, yellow, red, white). The details of the resin components and pigments used are shown in Table 3. The details of the pigments and acrylic resins are as follows. Blue pigment: fastogen (registered trademark) Blue 5480 (manufactured by Dainippon Ink Co., Ltd.) Yellow pigment: HOSTAPERM YELLOW H3g (Clariant) Red pigment: Irgazin (registered trademark) DPP Red BO (manufactured by Ciba Specialty Co., Ltd.) White pigment: Titanium oxide R-820 (manufactured by Ishihara Sangyo Kaisha) Acrylic resin: Dianale (registered trademark) BR-116 (manufactured by Mitsubishi Rayon Co., Ltd.)

[0065] The prepared pigmented paints (blue, yellow, red, and white) were evaluated for pigment dispersibility and hue stability by the following methods.

[0066] [Pigment dispersion in pigmented paints]: The resulting paint was stored at room temperature for 3 days, and then the state of pigment separation was visually observed. In addition, the pigment dispersibility was evaluated using a grain gauge according to the following evaluation criteria in accordance with the JISK-5600-2-5 Dispersion Test. If the pigment component is dispersed at less than 10 μm (i.e., if it is rated A to C), it can be determined that there is no problem in practical use. A: The pigments are evenly dispersed in the paint, and the color remains the same as immediately after preparation. B: The pigment is evenly dispersed in the paint, but shadows (haze) can be seen in the paint when it is shaken. C: Pigment components are dispersed with a particle gauge of less than 10 μm. D: The pigment component has a grain gauge of 10 μm or more.

[0067] [Color stability of pigmented paints]: After storing the pigment-containing paint at room temperature for 3 days, it was applied to a tin plate with an 8-mil doctor blade and dried at 60°C for 3 minutes. The dried product was measured with a digital colorimeter (manufactured by Suga Test Instruments Co., Ltd.). ΔE was calculated from this value and the initial value before storage. If the ΔE value is 10 or less (i.e., A to C evaluation), it can be judged that there is no problem in practical use. A: The ΔE value is 0.5 or less. B: The ΔE value is higher than 0.5 and is equal to or less than 2. C: ΔE value is greater than 2 and less than 10. D: ΔE value is higher than 10.

[0068] (Production Example 1: Production of Acid-Modified Chlorinated Polyolefin Resin (A-1)) 100 parts of a propylene-based random copolymer (propylene constituent unit content: 96 wt%, ethylene constituent unit content: 4 wt%) as polyolefin (a) produced using a metallocene catalyst as a polymerization catalyst, 10 parts of maleic anhydride as an α,β-unsaturated carboxylic acid cyclic anhydride, and 2 parts of di-t-butyl peroxide as a radical generator were uniformly mixed and fed to a twin-screw extruder (L / D=60, diameter=15 mm, 1st to 14th barrels).

[0069] The reaction was carried out under the conditions of a residence time of 10 minutes, a rotation speed of 200 rpm, and barrel temperatures of 100°C (1st and 2nd barrels), 200°C (3rd to 8th barrels), 90°C (9th and 10th barrels), and 110°C (11th to 14th barrels). Thereafter, a reduced pressure treatment was carried out to remove unreacted maleic anhydride, and an acid-modified polyolefin (ethylene-propylene) resin modified with maleic anhydride was obtained.

[0070] 100 parts of the acid-modified polyolefin resin was placed in a glass-lined reaction vessel. Chloroform was added and the mixture was stirred at 2 kgf / cm 2 After the resin was fully dissolved at a temperature of 110°C under a pressure of 1.0 kgf / cm, 2 parts of azobisisobutyronitrile was added as a radical generator, and the pressure in the vessel was increased to 2 kgf / cm. 2 Chlorination was carried out by blowing in chlorine gas while controlling the temperature.

[0071] After the reaction was completed, 6 parts of an epoxy compound (Epocizer W-100EL, manufactured by Dainippon Ink and Chemicals, Inc.) was added as a substance (D) (stabilizer) containing a hydroxyl group or a hydroxyl group equivalent structure, and the mixture was fed to a vented extruder equipped with a desolvation suction section on the screw shaft, where the solvent was removed and solidified to obtain an acid-modified chlorinated polyolefin resin (A-1). The resulting acid-modified chlorinated polyolefin resin (A-1) had a weight average molecular weight of 50,000, a maleic anhydride content of 5% by weight, and a chlorine content of 20% by weight.

[0072] (Production Example 2: Production of Acid-Modified Chlorinated Polyolefin Resin (A-2)) 100 parts of a propylene-based random copolymer (propylene constituent unit content: 96 wt%, ethylene constituent unit content: 4 wt%) as polyolefin (a) produced using a metallocene catalyst as a polymerization catalyst, 15 parts of maleic anhydride as an α,β-unsaturated carboxylic acid cyclic anhydride, and 2 parts of di-t-butyl peroxide as a radical generator were uniformly mixed and fed to a twin-screw extruder (L / D=60, diameter=15 mm, 1st to 14th barrels).

[0073] The reaction was carried out under the conditions of a residence time of 10 minutes, a rotation speed of 200 rpm, and barrel temperatures of 100°C (1st and 2nd barrels), 200°C (3rd to 8th barrels), 90°C (9th and 10th barrels), and 110°C (11th to 14th barrels). Thereafter, a reduced pressure treatment was carried out to remove unreacted maleic anhydride, and an acid-modified polyolefin (ethylene-propylene) resin modified with maleic anhydride was obtained.

[0074] 100 parts of the acid-modified polyolefin resin was placed in a glass-lined reaction vessel. Chloroform was added and the mixture was stirred at 2 kgf / cm 2 After the resin was fully dissolved at a temperature of 110°C under a pressure of 1.0 kgf / cm, 2 parts of azobisisobutyronitrile was added as a radical generator, and the pressure in the vessel was increased to 2 kgf / cm. 2 Chlorination was carried out by blowing in chlorine gas while controlling the temperature.

[0075] After the reaction was completed, 6 parts of an epoxy compound (Epocizer W-100EL, manufactured by Dainippon Ink and Chemicals, Inc.) was added as a substance (D) (stabilizer) containing a hydroxyl group or a hydroxyl group equivalent structure, and the mixture was fed to a vented extruder equipped with a desolvation suction section on the screw shaft, where the solvent was removed and solidified to obtain an acid-modified chlorinated polyolefin resin (A-2). The resulting acid-modified chlorinated polyolefin resin (A-2) had a weight average molecular weight of 10,000, a maleic anhydride content of 10% by weight, and a chlorine content of 10% by weight.

[0076] (Production Example 3: Production of Acid-Modified Chlorinated Polyolefin Resin (A-3)) 100 parts of a propylene-based random copolymer (propylene constituent unit content: 96% by weight, ethylene constituent unit content: 4% by weight) as polyolefin (a) produced using a metallocene catalyst as a polymerization catalyst, 3 parts of maleic anhydride as an α,β-unsaturated carboxylic acid cyclic anhydride, and 2 parts of di-t-butyl peroxide as a radical generator were uniformly mixed and fed to a twin-screw extruder (L / D=60, diameter=15 mm, 1st to 14th barrels).

[0077] The reaction was carried out under the conditions of a residence time of 10 minutes, a rotation speed of 200 rpm, and barrel temperatures of 100°C (1st and 2nd barrels), 200°C (3rd to 8th barrels), 90°C (9th and 10th barrels), and 110°C (11th to 14th barrels). Thereafter, a reduced pressure treatment was carried out to remove unreacted maleic anhydride, and an acid-modified polyolefin (ethylene-propylene) resin modified with maleic anhydride was obtained.

[0078] 100 parts of the acid-modified polyolefin resin was placed in a glass-lined reaction vessel. Chloroform was added and the mixture was stirred at 2 kgf / cm 2 After the resin was fully dissolved at a temperature of 110°C under a pressure of 1.0 kgf / cm, 2 parts of azobisisobutyronitrile was added as a radical generator, and the pressure in the vessel was increased to 2 kgf / cm. 2 Chlorination was carried out by blowing in chlorine gas while controlling the temperature.

[0079] After the reaction was completed, 6 parts of an epoxy compound (Epocizer W-100EL, manufactured by Dainippon Ink and Chemicals, Inc.) was added as a substance (D) (stabilizer) containing a hydroxyl group or a hydroxyl group equivalent structure, and the mixture was fed to a vented extruder equipped with a desolvation suction section on the screw shaft, where the solvent was removed and solidified to obtain an acid-modified chlorinated polyolefin resin (A-3). The resulting acid-modified chlorinated polyolefin resin (A-3) had a weight average molecular weight of 200,000, a maleic anhydride content of 1% by weight, and a chlorine content of 30% by weight.

[0080] (Production Example 4: Production of Acid-Modified Polyolefin Resin (A-4)) 100 parts of a propylene-based random copolymer (propylene constituent unit content: 96 wt%, ethylene constituent unit content: 4 wt%) as polyolefin (a) produced using a metallocene catalyst as a polymerization catalyst, 10 parts of maleic anhydride as an α,β-unsaturated carboxylic acid cyclic anhydride, and 2 parts of di-t-butyl peroxide as a radical generator were uniformly mixed and fed to a twin-screw extruder (L / D=60, diameter=15 mm, 1st to 14th barrels).

[0081] The reaction was carried out under the conditions of a residence time of 10 minutes, a rotation speed of 200 rpm, and barrel temperatures of 100°C (1st and 2nd barrels), 200°C (3rd to 8th barrels), 90°C (9th and 10th barrels), and 110°C (11th to 14th barrels). Thereafter, a reduced pressure treatment was carried out to remove unreacted maleic anhydride, and an acid-modified polyolefin (ethylene-propylene) resin modified with maleic anhydride was obtained.

[0082] After the reaction was completed, 6 parts of an epoxy compound (Epocizer W-100EL, manufactured by Dainippon Ink and Chemicals, Inc.) was added as a substance (D) (stabilizer) containing a hydroxyl group or a hydroxyl group equivalent structure, and the mixture was fed to a vented extruder equipped with a desolvation suction section on the screw shaft, where the solvent was removed and solidified to obtain an acid-modified polyolefin resin (A-4). The resulting acid-modified polyolefin resin (A-4) had a weight average molecular weight of 50,000 and a maleic anhydride content of 5% by weight.

[0083] (Production Example 5: Production of chlorinated polyolefin resin (A-5)) 100 parts of a propylene-based random copolymer (propylene constituent unit content: 96% by weight, ethylene constituent unit content: 4% by weight) as polyolefin (a) produced using a metallocene catalyst as a polymerization catalyst, and 2 parts of di-t-butyl peroxide as a radical generator were uniformly mixed and fed to a twin-screw extruder (L / D=60, diameter=15 mm, barrels 1 to 14).

[0084] The reaction was carried out under conditions of a residence time of 10 minutes, a rotation speed of 200 rpm, and barrel temperatures of 100°C (1st and 2nd barrels), 200°C (3rd to 8th barrels), 90°C (9th and 10th barrels), and 110°C (11th to 14th barrels), to obtain a polyolefin (ethylene-propylene) resin.

[0085] The polyolefin resin was placed in a glass-lined reaction vessel. Chloroform was added and the pressure was adjusted to 2 kgf / cm. 2 After the resin was fully dissolved at a temperature of 110°C under a pressure of 1.0 kgf / cm, 2 parts of azobisisobutyronitrile was added as a radical generator, and the pressure in the vessel was increased to 2 kgf / cm. 2Chlorination was carried out by blowing in chlorine gas while controlling the temperature.

[0086] After the reaction was completed, 6 parts of an epoxy compound (Epocizer W-100EL, manufactured by Dainippon Ink and Chemicals, Inc.) was added as a substance (D) (stabilizer) containing a hydroxyl group or a hydroxyl group equivalent structure, and the mixture was fed to a vented extruder equipped with a desolvation suction section on the screw shaft, where the solvent was removed and solidified to obtain a chlorinated polyolefin resin (A-5) as a chlorinated polypropylene resin. The resulting chlorinated polyolefin resin (A-5) had a weight average molecular weight of 50,000 and a chlorine content of 20% by weight.

[0087] (Production Example 6: Production of polyolefin resin (A-6)) 100 parts of a propylene-based random copolymer (propylene constituent unit content: 96% by weight, ethylene constituent unit content: 4% by weight) as polyolefin (a) produced using a metallocene catalyst as a polymerization catalyst, and 2 parts of di-t-butyl peroxide as a radical generator were uniformly mixed and fed to a twin-screw extruder (L / D=60, diameter=15 mm, barrels 1 to 14).

[0088] The reaction was carried out under conditions of a residence time of 10 minutes, a rotation speed of 200 rpm, and barrel temperatures of 100°C (1st and 2nd barrels), 200°C (3rd to 8th barrels), 90°C (9th and 10th barrels), and 110°C (11th to 14th barrels), to obtain a polyolefin (ethylene-propylene) resin.

[0089] After the reaction was completed, 6 parts of an epoxy compound (Epocizer W-100EL, manufactured by Dainippon Ink and Chemicals, Inc.) was added as a substance (D) (stabilizer) containing a hydroxyl group or a hydroxyl group equivalent structure, and the mixture was fed to a vented extruder equipped with a desolvation suction section on the screw shaft, where the solvent was removed and solidified to obtain polyolefin resin (A-6). The resulting polyolefin resin (A-6) had a weight average molecular weight of 50,000.

[0090] [Table 1]

[0091] (Example 1: Preparation of dispersion of resin component (X-1)) 40 parts of the acid-modified chlorinated polyolefin resin (A-1) obtained in Production Example 1 was dissolved in 48 parts of toluene as an organic solvent (C), 2 parts of 1-butanol was added as an alcohol (B), and 10 parts of an acrylic resin (Actflow (registered trademark) UT-1001, manufactured by Soken Chemical & Engineering, molecular weight 3500, hydroxyl value 57±2) as a substance containing a hydroxyl group or a hydroxyl group equivalent structure (D) was added, and the mixture was heated and stirred to obtain a dispersion of resin component (X-1) with a solid content of 50% by weight.

[0092] (Example 2: Preparation of dispersion of resin component (X-2)) 40 parts of the acid-modified chlorinated polyolefin resin (A-2) obtained in Production Example 2 was dissolved in 38 parts of butyl acetate as an organic solvent (C), 12 parts of 1-propanol as an alcohol (B) was added, and 10 parts of an acrylic resin (Actflow (registered trademark) UT-1001, manufactured by Soken Chemical & Engineering, molecular weight 3500, hydroxyl value 57±2) as a substance (D) was added, and the mixture was heated and stirred to obtain a dispersion of resin component (X-2) with a solid content of 50% by weight.

[0093] (Example 3: Preparation of dispersion of resin component (X-3)) 40 parts of the acid-modified chlorinated polyolefin resin (A-3) obtained in Production Example 3 was dissolved in 49.6 parts of xylene as an organic solvent (C), 0.4 parts of ethanol as an alcohol (B) was added, and 10 parts of an acrylic resin (Actflow (registered trademark) UT-1001, manufactured by Soken Chemical & Engineering, molecular weight 3500, hydroxyl value 57±2) as a substance (D) was added, and the mixture was heated and stirred to obtain a dispersion of resin component (X-3) with a solid content of 50% by weight.

[0094] (Example 4: Preparation of dispersion of resin component (X-4)) 40 parts of the acid-modified polyolefin resin (A-4) obtained in Production Example 4 was dissolved in 48 parts of toluene as an organic solvent (C), 2 parts of 1-butanol as an alcohol (B) was added, and 10 parts of an acrylic resin (Actflow (registered trademark) UT-1001, manufactured by Soken Chemical & Engineering, molecular weight 3500, hydroxyl value 57±2) as a substance (D) was added, and the mixture was heated and stirred to obtain a dispersion of resin component (X-4) with a solid content of 50% by weight.

[0095] (Comparative Example 1: Preparation of Dispersion of Resin Component (X-5)) 40 parts of the acid-modified chlorinated polyolefin resin (A-5) obtained in Production Example 5 was dissolved in 48 parts of toluene as an organic solvent (C), 2 parts of 1-butanol as an alcohol (B) was added, and 10 parts of an acrylic resin (Actflow (registered trademark) UT-1001, manufactured by Soken Chemical & Engineering, molecular weight 3500, hydroxyl value 57±2) as a substance containing a hydroxyl group or a hydroxyl group equivalent structure (D) was added, and the mixture was heated and stirred to obtain a dispersion of a resin component (X-5) having a solid content of 50% by weight.

[0096] (Comparative Example 2: Preparation of Dispersion of Resin Component (X-6)) 40 parts of the acid-modified chlorinated polyolefin resin (A-1) obtained in Production Example 1 was dispersed in 48 parts of water as a solvent (C'), and then 2 parts of 1-butanol as the alcohol (B) was added, and 10 parts of an acrylic resin (Actflow (registered trademark) UT-1001, manufactured by Soken Chemical & Engineering, molecular weight 3500, hydroxyl value 57±2) was added as a substance (D) containing a hydroxyl group or a hydroxyl group equivalent structure, and the mixture was heated and stirred to obtain a dispersion of resin component (X-6) with a solid content of 50% by weight.

[0097] (Comparative Example 3: Preparation of Dispersion of Resin Component (X-7)) 40 parts of the acid-modified chlorinated polyolefin resin (A-1) obtained in Production Example 1 was dissolved in 50 parts of toluene as an organic solvent (C), and 10 parts of an acrylic resin (Actflow (registered trademark) UT-1001, manufactured by Soken Chemical & Engineering, molecular weight 3500, hydroxyl value 57±2) as a substance (D) containing a hydroxyl group or a hydroxyl group equivalent structure was added and stirred while heating to obtain a dispersion of a resin component (X-7) having a solid content of 50% by weight.

[0098] (Comparative Example 4: Preparation of Dispersion of Resin Component (X-8)) 40 parts of the acid-modified chlorinated polyolefin resin (A-1) obtained in Production Example 1 was dissolved in 48 parts of toluene as an organic solvent (C), 2 parts of 2-butanol was added as an alcohol (B), and 10 parts of an acrylic resin (Actflow (registered trademark) UT-1001, manufactured by Soken Chemical & Engineering, molecular weight 3500, hydroxyl value 57±2) was added as a substance containing a hydroxyl group or a hydroxyl group equivalent structure (D), and the mixture was heated and stirred to obtain a dispersion of a resin component (X-8) having a solid content of 50% by weight.

[0099] (Comparative Example 5: Preparation of Dispersion of Resin Component (X-9)) 40 parts of the acid-modified chlorinated polyolefin resin (A-1) obtained in Production Example 1 was dissolved in 48 parts of toluene as an organic solvent (C), 2 parts of 1-pentanol was added as an alcohol (B), and 10 parts of an acrylic resin (Actflow (registered trademark) UT-1001, manufactured by Soken Chemical & Engineering, molecular weight 3500, hydroxyl value 57±2) was added as a substance containing a hydroxyl group or a hydroxyl group equivalent structure (D), and the mixture was heated and stirred to obtain a dispersion of a resin component (X-9) having a solid content of 50% by weight.

[0100] (Comparative Example 6: Production of Dispersion of Resin Component (X-10)) 40 parts of the acid-modified chlorinated polyolefin resin (A-1) obtained in Production Example 1 was dissolved in 48 parts of toluene as an organic solvent (C), 2 parts of methanol was added as an alcohol (B), and 10 parts of an acrylic resin (Actflow (registered trademark) UT-1001, manufactured by Soken Chemical & Engineering, molecular weight 3500, hydroxyl value 57±2) was added as a substance containing a hydroxyl group or a hydroxyl group equivalent structure (D), and the mixture was heated and stirred to obtain a dispersion of a resin component (X-10) having a solid content of 50% by weight.

[0101] (Comparative Example 7: Production of Dispersion of Resin Component (X-11)) 40 parts of the polyolefin resin (A-6) obtained in Production Example 6 was dissolved in 48 parts of toluene as an organic solvent (C), 2 parts of 1-butanol was added as an alcohol (B), and 10 parts of an acrylic resin (Actflow (registered trademark) UT-1001, manufactured by Soken Chemical & Engineering, molecular weight 3500, hydroxyl value 57±2) was added as a substance containing a hydroxyl group or a hydroxyl group equivalent structure (D), and the mixture was heated and stirred to obtain a dispersion of a resin component (X-11) having a solid content of 50% by weight.

[0102] (Comparative Example 8: Preparation of Dispersion of Resin Component (X-12)) 40 parts of the acid-modified chlorinated polyolefin resin (A-1) obtained in Production Example 1 was dissolved in 49.8 parts of toluene as an organic solvent (C), 0.2 parts of 1-butanol was added as an alcohol (B), and 10 parts of an acrylic resin (Actflow (registered trademark) UT-1001, manufactured by Soken Chemical & Engineering, molecular weight 3500, hydroxyl value 57±2) was added as a substance containing a hydroxyl group or a hydroxyl group equivalent structure (D), and the mixture was heated and stirred to obtain a dispersion of a resin component (X-12) having a solid content of 50% by weight.

[0103] (Comparative Example 9: Preparation of Dispersion of Resin Component (X-13)) 40 parts of the acid-modified chlorinated polyolefin resin (A-1) obtained in Production Example 1 was dissolved in 43.8 parts of toluene as an organic solvent (C), and 6.2 parts of 1-butanol was added as an alcohol (B). 10 parts of an acrylic resin (Actflow (registered trademark) UT-1001, manufactured by Soken Chemical & Engineering Co., Ltd., molecular weight 3500, hydroxyl value 57±2) was added as a substance containing a hydroxyl group or a hydroxyl group equivalent structure (D). The mixture was heated and stirred to obtain a dispersion of a resin component (X-13) having a solid content of 50% by weight.

[0104] [Table 2]

[0105] The stability of the dispersions of each Example and Comparative Example was evaluated, and test pieces were prepared and adhesion tests were performed. In addition, the dispersions, pigments, and compatibilizers were mixed to prepare paints, and the pigment dispersibility and color stability were evaluated. The evaluation results are shown in Table 3.

[0106] [Table 3]

[0107] From the above test results, it can be seen that the resin composition obtained in the examples, in which an acid-modified polyolefin resin was dispersed in an organic solvent and an alcohol in the corresponding range was added, had good solution properties immediately after preparation, did not show significant thickening even after one month, and also had good adhesion to the substrate, pigment dispersibility, and hue stability, compared to the comparative example composition.

Claims

1. A modified polyolefin resin composition comprising a modified polyolefin resin (X) in which an acid-modified polyolefin resin (A) is modified with a modifying component containing an alcohol (B), an organic solvent (C), and at least one member selected from the group consisting of an acrylic resin containing a hydroxyl group, a polyol resin containing a hydroxyl group, and a polyurethane resin containing a hydroxyl group, and satisfying the following (I) to (V): (I) The acid-modified polyolefin resin (A) is a resin in which a polyolefin (a) is modified with an α,β-unsaturated carboxylic acid derivative (b) having a structure (b1), wherein the structure (b1) is a group represented by the formula (1): -(C═O)-O-(C═O)-. (II) The residual rate of the structure (b1) in the modified polyolefin resin (X) is more than 0% and 50% or less. (III) The total content of the group derived from the alcohol (B) and the alcohol (B) in the composition is 1.0 to 5.0 mol per 1.0 mol of the structure (b1) in the acid-modified polyolefin resin (A). (VI) The alcohol (B) is an alcohol having 2 to 4 carbon atoms. (V) The organic solvent (C) is one or more solvents selected from the group consisting of aromatic solvents, ester solvents, aliphatic hydrocarbon solvents, and alicyclic hydrocarbon solvents.

2. The modified polyolefin resin composition according to claim 1, wherein the residual rate of the structure (b1) in the modified polyolefin resin (X) is 2% or more.

3. 3. The modified polyolefin resin composition according to claim 1, wherein the derivative (b) of the α,β-unsaturated carboxylic acid is an α,β-unsaturated carboxylic acid cyclic anhydride.

4. The modified polyolefin resin composition according to any one of claims 1 to 3, wherein the modified polyolefin resin (X) is a modified chlorinated polyolefin resin (X1).

5. The modified polyolefin resin composition according to any one of claims 1 to 4, wherein the acid-modified polyolefin resin (A) is an acid-modified chlorinated polyolefin resin (A1).

6. A modified polyolefin resin composition described in any one of claims 1 to 5, further comprising a compound containing an epoxy ring.

7. The modified polyolefin resin composition according to any one of claims 1 to 6, wherein the total content of the group derived from the alcohol (B) and the alcohol (B) in the composition is 1.2 mol or more per 1.0 mol of the structure (b1) of the acid-modified polyolefin resin (A).

8. The modified polyolefin resin composition according to any one of claims 1 to 7, wherein the alcohol (B) contains at least a primary alcohol.

9. The modified polyolefin resin composition according to any one of claims 1 to 8, wherein the organic solvent (C) comprises one or more selected from toluene, xylene, ethyl acetate, butyl acetate, nonane, decane, cyclohexane, methylcyclohexane, and ethylcyclohexane.

10. The modified polyolefin resin composition according to any one of claims 1 to 9, wherein the content of the α,β-unsaturated carboxylic acid derivative (b) in the acid-modified polyolefin resin (A) is 0.5 to 20% by weight.

11. The modified polyolefin resin composition according to any one of claims 1 to 10, wherein the acid-modified polyolefin resin (A) has a weight average molecular weight of 5,000 to 300,000.

12. A primer comprising the modified polyolefin resin composition according to any one of claims 1 to 11.

13. A coating material comprising the modified polyolefin resin composition according to any one of claims 1 to 11.

14. An ink comprising the modified polyolefin resin composition according to any one of claims 1 to 11.

15. A polyolefin (a) is modified with a derivative (b) of an α,β-unsaturated carboxylic acid having a structure (b1) derived from at least one carboxyl group to obtain an acid-modified polyolefin resin (A); modifying an acid-modified polyolefin resin (A) with a modifying component containing an alcohol (B) having 2 to 4 carbon atoms in an amount of 1.0 to 5.0 mol per 1.0 mol of the structure (b1) of the acid-modified polyolefin resin (A) to obtain a modified polyolefin resin (X); adding an organic solvent (C) which is one or more selected from the group consisting of aromatic solvents, ester solvents, aliphatic hydrocarbon solvents, and alicyclic hydrocarbon solvents, and one or more selected from the group consisting of acrylic resins containing a hydroxyl group, polyol resins containing a hydroxyl group, and polyurethane resins containing a hydroxyl group; The method for producing a modified polyolefin resin composition according to any one of claims 1 to 11, wherein the structure (b1) is a group represented by formula (1): -(C=O)-O-(C=O)-.

Citation Information

Patent Citations

  • Polyolefin composition

    JP1986111346A

  • Adhesion accelerator composition for polyolefin base material

    JP1991115476A

  • Dispersion of modified propylene polymer

    JP1992288336A

  • Modified polyolefin resin composition using same direction twin screw extruder and its manufacturing method

    JP2004114610A

  • Modified chlorinated carboxylated polyolefins and their use as adhesion promoters

    JP2008516053A