Semiconductor device manufacturing method
The method of oxygen ion implantation and heat treatment in silicon carbide semiconductor devices stabilizes Schottky barrier height, addressing variations and enhancing device performance by ensuring consistent rectification characteristics and material flexibility.
Patent Information
- Application Number
- JP2023086651
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-05-14
AI Technical Summary
Variations in Schottky barrier height in silicon carbide-based semiconductor devices lead to inconsistent rectification characteristics and potential device failure due to localized low Schottky barriers and reduced breakdown voltage.
A manufacturing method involving oxygen ion implantation into a silicon carbide layer, followed by heat treatments, to create an oxygen region where one oxygen atom bonds to four silicon atoms, stabilizing the Schottky barrier height at approximately 0.8 eV, thereby suppressing variations.
The method stabilizes Schottky barrier height, ensuring consistent rectification characteristics and allowing for the selection of anode electrode materials, reducing the risk of device failure and enhancing device performance.
Smart Images

Figure 0007581421000001 
Figure 0007581421000002 
Figure 0007581421000003
Abstract
Description
[Technical field]
[0001] An embodiment of the present invention relates to a semiconductor device, a method for manufacturing a semiconductor device, an inverter circuit, a drive device, a vehicle, and an elevator. [Background technology]
[0002] Silicon carbide (SiC) is expected to be a material for next-generation semiconductor devices. Compared to silicon (Si), silicon carbide has excellent physical properties, such as a band gap about three times larger, a breakdown electric field strength about ten times larger, and a thermal conductivity about three times larger. By utilizing these properties, it is possible to realize semiconductor devices that are low-loss and capable of operating at high temperatures.
[0003] In a Schottky barrier diode (SBD) using silicon carbide, if the Schottky barrier height between a silicon carbide layer and an electrode varies, the rectification characteristics of the SBD varies. Therefore, it is desired to realize a semiconductor device in which the variation in the Schottky barrier height is suppressed. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-126604 A Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a method for manufacturing a semiconductor device in which the variation in Schottky barrier height is suppressed. [Means for solving the problem]
[0006] A method for manufacturing a semiconductor device according to an embodiment includes ion-implanting oxygen into a silicon carbide layer having an n-type first silicon carbide region, forming a conductive film on the silicon carbide layer, and performing a first heat treatment. After the ion implantation and before the conductive film is formed, a second heat treatment is further performed at a temperature higher than that of the first heat treatment. . [Brief description of the drawings]
[0007] [Figure 1] 1 is a schematic cross-sectional view of a semiconductor device according to a first embodiment. [Diagram 2] FIG. 4 is an explanatory diagram of an oxygen region in the first embodiment. [Diagram 3] FIG. 4 is a graph showing the oxygen concentration distribution in the semiconductor device according to the first embodiment. [Figure 4] FIG. 2 is a process flow diagram illustrating a method for manufacturing the semiconductor device according to the first embodiment. [Diagram 5] 2A to 2C are schematic cross-sectional views showing a method for manufacturing the semiconductor device according to the first embodiment. [Figure 6] 2A to 2C are schematic cross-sectional views showing a method for manufacturing the semiconductor device according to the first embodiment. [Figure 7] 2A to 2C are schematic cross-sectional views showing a method for manufacturing the semiconductor device according to the first embodiment. [Figure 8] 2A to 2C are schematic cross-sectional views showing a method for manufacturing the semiconductor device according to the first embodiment. [Figure 9] 2A to 2C are schematic cross-sectional views showing a method for manufacturing the semiconductor device according to the first embodiment. [Figure 10] 5A to 5C are explanatory diagrams illustrating the operation and effects of the semiconductor device according to the first embodiment. [Figure 11] 5A to 5C are explanatory diagrams illustrating the operation and effects of the semiconductor device according to the first embodiment. [Figure 12] 5A to 5C are explanatory diagrams illustrating the operation and effect of the method for manufacturing the semiconductor device according to the first embodiment. [Figure 13] FIG. 5 is a schematic cross-sectional view of a semiconductor device according to a second embodiment. [Figure 14] FIG. 11 is a schematic cross-sectional view of a semiconductor device according to a third embodiment. [Figure 15] FIG. 11 is an equivalent circuit diagram of a semiconductor device according to a third embodiment. [Figure 16] FIG. 13 is a schematic cross-sectional view of a semiconductor device according to a first modified example of the third embodiment. [Figure 17] FIG. 13 is a schematic cross-sectional view of a semiconductor device according to a second modified example of the third embodiment. [Figure 18] FIG. 13 is a schematic cross-sectional view of a semiconductor device according to a fourth embodiment. [Figure 19] FIG. 13 is a schematic top view of a semiconductor device according to a fourth embodiment. [Figure 20] FIG. 13 is a schematic cross-sectional view of a semiconductor device according to a fourth embodiment. [Figure 21] 13A to 13C are top views of the fourth embodiment and a modification example. [Figure 22] FIG. 13 is a schematic cross-sectional view of a semiconductor device according to a fifth embodiment. [Diagram 23] FIG. 13 is a schematic cross-sectional view of a semiconductor device according to a modified example of the fifth embodiment. [Figure 24] FIG. 13 is a schematic top view of a semiconductor device according to a modified example of the fifth embodiment. [Diagram 25] 13 is a schematic cross-sectional view of a semiconductor device according to a modification of the fifth embodiment; [Figure 26] FIG. 13 is a schematic cross-sectional view of a semiconductor device according to a sixth embodiment. [Figure 27] FIG. 13 is a schematic cross-sectional view of a semiconductor device according to a seventh embodiment. [Figure 28] FIG. 13 is a schematic cross-sectional view of a semiconductor device according to an eighth embodiment. [Figure 29] FIG. 13 is a schematic top view of a semiconductor device according to an eighth embodiment. [Diagram 30] FIG. 13 is a schematic cross-sectional view of a semiconductor device according to a ninth embodiment. [Diagram 31] FIG. 23 is a schematic diagram of a drive device according to a tenth embodiment. [Diagram 32] FIG. 23 is a schematic diagram of a vehicle according to an eleventh embodiment. [Diagram 33] FIG. 23 is a schematic diagram of a vehicle according to a twelfth embodiment. [Diagram 34] FIG. 23 is a schematic diagram of an elevator according to a thirteenth embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In the following description, the same reference numerals will be used to designate the same or similar components, and the description of components that have already been described will be omitted as appropriate.
[0009] In the following description, n + , n, n - And, p + , p, p -When the notation "n" is used, it indicates the relative level of impurity concentration in each conductivity type. + has a relatively higher n-type impurity concentration than n, - indicates that the n-type impurity concentration is relatively lower than that of n. + has a relatively higher p-type impurity concentration than p, - indicates that the p-type impurity concentration is relatively lower than that of p. + type, n - The types are simply n-type and p-type. + type, p - The type may be simply referred to as p-type. The impurity concentration of each region is represented by, for example, the impurity concentration value at the center of each region, unless otherwise specified.
[0010] The impurity concentration can be measured, for example, by SIMS (Secondary Ion Mass Spectrometry). The relative level of the impurity concentration can also be determined from the level of the carrier concentration obtained, for example, by SCM (Scanning Capacitance Microscopy). Distances such as the width and depth of the impurity region can be obtained, for example, by SIMS. Distances such as the width and depth of the impurity region can also be obtained, for example, from an SCM image.
[0011] The depth of the trench, the thickness of the insulating layer, etc. can be measured on images of, for example, SIMS or a TEM (Transmission Electron Microscope).
[0012] The bonding state of oxygen atoms in the silicon carbide layer can be identified by X-ray photoelectron spectroscopy (XPS method), and whether or not oxygen atoms in the silicon carbide layer are located at carbon sites in the crystal structure of silicon carbide can be determined by, for example, Raman spectroscopy.
[0013] (First embodiment) The semiconductor device of the first embodiment includes a first electrode, a second electrode, and a silicon carbide layer located between the first electrode and the second electrode, the silicon carbide layer including: an n-type first silicon carbide region; and a second silicon carbide region located between the first silicon carbide region and the first electrode, in contact with the first electrode, and including one oxygen atom bonded to four silicon atoms.
[0014] 1 is a schematic cross-sectional view of a semiconductor device according to a first embodiment. The semiconductor device according to the first embodiment is a Schottky Barrier Diode (SBD). The semiconductor device according to the first embodiment is an SBD 100. The SBD 100 uses electrons as carriers.
[0015] The SBD 100 includes a silicon carbide layer 10, an anode electrode 12 (first electrode), and a cathode electrode 14 (second electrode).
[0016] The anode electrode 12 is an example of a first electrode, and the cathode electrode 14 is an example of a second electrode.
[0017] The silicon carbide layer 10 includes a cathode region 16, a drift region 18 (first silicon carbide region), and an oxygen region 20 (second silicon carbide region).
[0018] The silicon carbide layer 10 is, for example, a single crystal of 4H-SiC. The silicon carbide layer 10 has a first surface P1 and a second surface P2. The second surface P2 faces the first surface P1. The first surface P1 is a front surface of the silicon carbide layer 10, and the second surface P2 is a back surface of the silicon carbide layer 10.
[0019] The silicon carbide layer 10 is located between an anode electrode 12 and a cathode electrode 14 .
[0020] In this specification, the term "depth" refers to the distance in a direction from the first plane P1 toward the second plane P2, with the first plane P1 being used as a reference.
[0021] Hereinafter, a case will be described as an example in which the first surface P1 of the silicon carbide layer 10 is inclined at an angle of 0 to 10 degrees with respect to the silicon surface, and the second surface P2 is inclined at an angle of 0 to 10 degrees with respect to the carbon surface. The first surface P1 of the silicon carbide layer 10 has an off angle of 0 to 10 degrees with respect to the silicon surface.
[0022] The cathode region 16 is + The cathode region 16 is made of n-type SiC. The cathode region 16 contains, for example, nitrogen (N) as an n-type impurity. The n-type impurity concentration of the cathode region 16 is, for example, 1×10 18 cm -3 More than 1×10 21 cm -3 The following is the result.
[0023] The drift region 18 is - The drift region 18 is located between the cathode region 16 and the anode electrode 12. The drift region 18 is located between the cathode region 16 and the first plane P1.
[0024] The drift region 18 contains, for example, nitrogen (N) as an n-type impurity. The n-type impurity concentration of the drift region 18 is, for example, 1×10 15 cm -3 More than 2×10 16 cm -3 The n-type impurity concentration of the drift region 18 is lower than the n-type impurity concentration of the cathode region 16.
[0025] The drift region 18 is, for example, an epitaxially grown layer of SiC formed by epitaxial growth on the cathode region 16. The drift region 18 has a thickness of, for example, 5 μm or more and 100 μm or less.
[0026] The oxygen region 20 is - The oxygen region 20 is located between the drift region 18 and the anode electrode 12. The oxygen region 20 is located between the drift region 18 and the first plane P1. The oxygen region 20 contacts the anode electrode 12.
[0027] The oxygen region 20 contains oxygen as an impurity. The maximum concentration of oxygen in the oxygen region 20 is, for example, 1×10 17 cm -3 More than 1×10 21 cm -3 The following is the result.
[0028] Oxygen region 20 includes one oxygen atom bonded to four silicon atoms.
[0029] The oxygen region 20 contains, for example, nitrogen (N) as an n-type impurity. The n-type impurity concentration of the oxygen region 20 is, for example, 1×10 15 cm -3 More than 2×10 16 cm -3 The following is the result.
[0030] 2A and 2B are explanatory diagrams of the oxygen region of the first embodiment, Fig. 2(a) is a diagram showing the crystal structure of silicon carbide, and Fig. 2(b) is a diagram showing the structure present in the oxygen region 20.
[0031] As shown in Fig. 2(b), oxygen region 20 has one oxygen atom bonded to four silicon atoms. In other words, oxygen region 20 has one oxygen atom located at a carbon site in the silicon carbide crystal structure shown in Fig. 2(a). In other words, oxygen region 20 has a structure in which one oxygen atom replaces a carbon atom in the silicon carbide crystal structure.
[0032] Fig. 3 is a diagram showing the oxygen concentration distribution in the semiconductor device of the first embodiment. Fig. 3 shows the oxygen concentration distribution in the depth direction of the anode electrode 12 and the silicon carbide layer 10. Fig. 3 shows the oxygen concentration distribution in the depth direction of the anode electrode 12, the oxygen region 20, and the drift region 18.
[0033] The concentration distribution of oxygen in the anode electrode 12 and the oxygen region 20 has a first peak. The distance between the interface between the anode electrode 12 and the oxygen region 20 and the first peak is 1 nm or less. In the oxygen region 20, oxygen piles up at the interface between the anode electrode 12 and the oxygen region 20.
[0034] The oxygen concentration of the first peak is, for example, 1×10 17 cm -3 More than 1×10 21 cm -3 The following is the result.
[0035] The oxygen concentration distribution in the anode electrode 12 and the oxygen region 20 has a second peak between the first peak and the drift region 18. The oxygen concentration of the second peak is, for example, lower than the oxygen concentration of the first peak.
[0036] The anode electrode 12 is located on the first face P1 side of the silicon carbide layer 10. The anode electrode 12 is electrically connected to the oxygen region 20 and the drift region .
[0037] The anode electrode 12 is in contact with the silicon carbide layer 10. The anode electrode 12 is in contact with the oxygen region 20.
[0038] There is a Schottky contact between the anode electrode 12 and the oxygen region 20. The Schottky barrier height between the anode electrode 12 and the oxygen region 20 is, for example, 0.7 eV or more and 1.0 eV or less. The Schottky barrier height between the anode electrode 12 and the oxygen region 20 is, for example, about 0.8 eV.
[0039] The anode electrode 12 is a conductor, and may be, for example, a metal, an intermetallic compound, a metal nitride, a metal silicide, or a semiconductor.
[0040] The anode electrode 12 may have, for example, a laminated structure. The anode electrode 12 has, for example, a laminated structure of two different metals. The anode electrode 12 has, for example, a laminated structure of a metal silicide and a metal.
[0041] The anode electrode 12 has, for example, a laminated structure of titanium and aluminum. The anode electrode 12 includes, for example, nickel silicide. The anode electrode 12 has, for example, a laminated structure of nickel silicide and aluminum.
[0042] The cathode electrode 14 is located on the second face P2 side of the silicon carbide layer 10. The cathode electrode 14 is in contact with the cathode region 16. The cathode electrode 14 is electrically connected to the cathode region 16.
[0043] The cathode electrode 14 is a conductor, and may be, for example, a metal, an intermetallic compound, a metal nitride, a metal silicide, or a semiconductor.
[0044] The cathode electrode 14 is, for example, nickel. The nickel may react with the silicon carbide layer 10 to form nickel silicide. The nickel silicide is, for example, NiSi or Ni2Si.
[0045] Next, an example of a method for manufacturing the semiconductor device of the first embodiment will be described.
[0046] The method for manufacturing a semiconductor device according to the first embodiment includes ion implanting oxygen into a silicon carbide layer having an n-type first silicon carbide region, forming a conductive film on the silicon carbide layer, and performing a first heat treatment. After the ion implantation, and before forming the conductive film, a second heat treatment is further performed at a temperature higher than that of the first heat treatment.
[0047] Fig. 4 is a process flow diagram illustrating the method for manufacturing the semiconductor device of the first embodiment. Fig. 5, Fig. 6, Fig. 7, Fig. 8, and Fig. 9 are schematic cross-sectional views showing the method for manufacturing the semiconductor device of the first embodiment. Fig. 5, Fig. 6, Fig. 7, Fig. 8, and Fig. 9 show cross sections corresponding to Fig. 1.
[0048] Hereinafter, an example will be described in which the anode electrode 12 has a laminated structure of titanium and aluminum, and the cathode electrode 14 is made of nickel.
[0049] As shown in FIG. 4, the method for manufacturing a semiconductor device includes silicon carbide layer preparation (step S100), oxide film formation (step S102), oxygen ion implantation (step S104), diffusion annealing (step S106), oxide film removal (step S108), titanium film / aluminum film formation (step S110), pile-up annealing (step S112), and backside nickel film formation (step S114).
[0050] In step S100, a silicon carbide layer 10 is prepared (FIG. 5). The silicon carbide layer 10 is + The cathode region 16 and the n - The drift region 18 is, for example, + The silicon carbide layer 10 is formed by epitaxial growth on the cathode region 16 of the silicon carbide layer 10. The silicon carbide layer 10 has a first surface P1 and a second surface P2.
[0051] In step S102, an oxide film 22 is formed on the silicon carbide layer 10 (FIG. 6). The oxide film 22 is formed by a chemical vapor deposition method (CVD method) or a thermal oxidation method.
[0052] In step S102, oxygen ions are implanted into the silicon carbide layer 10 (FIG. 7). The oxygen ions that have passed through the oxide film 22 are introduced into the silicon carbide layer 10. The oxygen ion implantation breaks carbon bonds in the silicon carbide layer 10, and carbon vacancies in the silicon carbide layer 10 increase.
[0053] By the ion implantation of oxygen, an oxygen region 20 containing oxygen is formed.
[0054] In step S102, diffusion annealing is performed. The diffusion annealing is an example of a second heat treatment. The diffusion annealing causes oxygen to diffuse in the silicon carbide layer 10. Furthermore, the diffusion annealing causes oxygen atoms to enter carbon vacancies, generating a structure in which one oxygen atom replaces a carbon atom in the silicon carbide crystal structure.
[0055] The diffusion annealing is performed in an atmosphere containing, for example, argon (Ar) or nitrogen (N). The diffusion annealing is performed in an atmosphere of an inert gas such as argon (Ar) gas.
[0056] The temperature of the diffusion annealing is, for example, higher than the temperature of the pile-up annealing that is performed later, and is, for example, 800° C. or higher and 1000° C. or lower.
[0057] In step S108, the oxide film 22 is removed (FIG. 8). The oxide film 22 is removed by, for example, wet etching.
[0058] In step S110, a laminated film 24 of a titanium film and an aluminum film is formed on the silicon carbide layer 10 (FIG. 9). The laminated film 24 is formed by, for example, a sputtering method. The laminated film 24 is an example of a conductive film. The laminated film 24 will eventually become the anode electrode 12.
[0059] In step S112, pile-up annealing is performed. The pile-up annealing is an example of a first heat treatment. By the pile-up annealing, oxygen in the oxygen region 20 piles up at the interface between the anode electrode 12 and the oxygen region 20.
[0060] The pile-up annealing is performed, for example, in an atmosphere containing argon (Ar) or nitrogen (N). The pile-up annealing is performed, for example, in an atmosphere of an inert gas such as argon (Ar) gas.
[0061] The pile-up annealing temperature is, for example, lower than the diffusion annealing temperature, and is, for example, 300° C. or higher and 700° C. or lower.
[0062] In step S114, a nickel film is formed on the second face P2 of the silicon carbide layer 10. The nickel film is formed on the back face of the silicon carbide layer 10. The nickel film is formed by using, for example, a sputtering method. The nickel film will eventually become the cathode electrode 14.
[0063] By the above manufacturing method, the SBD 100 shown in FIG. 1 is manufactured.
[0064] Next, the operation and effects of the semiconductor device and the method for manufacturing the semiconductor device according to the first embodiment will be described.
[0065] In a Schottky barrier diode (SBD) using silicon carbide, the Schottky barrier height between the silicon carbide layer and the electrode may vary. Variation in the Schottky barrier height between the silicon carbide layer and the electrode causes variation in the rectification characteristics of the SBD.
[0066] For example, if a low Schottky barrier occurs locally, the on-state voltage (V F ) variations. Furthermore, if a part with a locally low Schottky barrier occurs, for example, an excessive forward current (on-state current) may flow through the part with a low Schottky barrier, which may destroy the SBD 100. Furthermore, if a part with a locally low Schottky barrier occurs, there is a risk that the breakdown voltage under reverse bias may be locally reduced. Therefore, it is desirable to realize an SBD in which the variations in the Schottky barrier height are suppressed.
[0067] The variation in the Schottky barrier height is caused by, for example, the variation in the reaction between the silicon carbide layer and the electrode, the variation in the carbon vacancy density in the silicon carbide layer, the variation in the n-type impurity concentration, and the like.
[0068] The SBD 100 includes an oxygen region 20 in the silicon carbide layer 10, which is in contact with the anode electrode 12. The oxygen region 20 includes one oxygen atom bonded to four silicon atoms. By including the oxygen region 20, the SBD 100 can suppress variations in the Schottky barrier height. This will be described in detail below.
[0069] As a result of first-principles calculations by the inventors, it was revealed that when carbon vacancies and oxygen atoms coexist in the crystal structure of silicon carbide, the structure in which one oxygen atom fills the carbon vacancy and bonds to four silicon atoms is energetically stable, as shown in Figure 2(b). In other words, it was revealed that the structure in which one oxygen atom is located at the carbon site of the silicon carbide crystal structure is energetically stable.
[0070] Fig. 10 is an explanatory diagram of the operation and effect of the semiconductor device of the first embodiment. Fig. 10 is a band diagram in the case where one oxygen atom is located at a carbon site of the crystal structure of silicon carbide. As shown in Fig. 10, a localized state is formed at the lower end of the conduction band in the band gap (Eg in Fig. 10).
[0071] 11 is an explanatory diagram of the operation and effect of the semiconductor device of the first embodiment, and is an explanatory diagram of a localized state formed in the band gap.
[0072] 11, the localized state is formed at a position about 0.8 eV from the bottom of the conduction band. The energy difference between the localized state and the bottom of the conduction band is, for example, not less than 0.7 eV and not more than 1.0 eV.
[0073] When a localized state exists in the oxygen region 20, electrons move between the localized state and the anode electrode 12 in contact with the oxygen region 20. This electron movement fixes the Schottky barrier height between the anode electrode 12 and the oxygen region 20 to about 0.8 eV. The Schottky barrier height between the anode electrode 12 and the oxygen region 20 is fixed to about 0.8 eV by the occurrence of so-called Fermi level pinning.
[0074] By fixing the Schottky barrier height at about 0.8 eV, the variation in the Schottky barrier height of the SBD 100 is suppressed.
[0075] In addition, a localized state is formed in the band gap, and Fermi level pinning occurs, so that the Schottky barrier height is fixed at approximately 0.8 eV, regardless of the material of the anode electrode 12. Therefore, it becomes possible to arbitrarily select the material of the anode electrode 12.
[0076] From the viewpoint of forming a sufficient amount of localized states in the oxygen region 20 and stably fixing the Schottky barrier height, the maximum oxygen concentration in the oxygen region 20 is 1×10 17 cm -3 It is preferable that the concentration is 1×10 or more. 18 cm -3 More preferably, it is 1×10 19 cm -3 More preferably, it is equal to or greater than this.
[0077] The oxygen concentration distribution in the anode electrode 12 and the oxygen region 20 has a first peak. The oxygen concentration of the first peak is 1×10 17 cm -3 It is preferable that the concentration is 1×10 or more. 18 cm -3 More preferably, it is 1×10 19 cm -3 More preferably, it is equal to or greater than this.
[0078] From the viewpoint of facilitating the transfer of electrons between the localized state and the anode electrode 12, it is preferable that the distance between the interface between the anode electrode 12 and the oxygen region 20 and the first peak is 1 nm or less.
[0079] From the viewpoint of forming a sufficient amount of localized states in the oxygen region 20 and stably fixing the Schottky barrier height, it is preferable that the ratio of one oxygen atom bonded to four silicon atoms among the oxygen atoms contained in the oxygen region 20 is higher than the ratio of oxygen atoms having other bond states. The other bond states are, for example, a state in which an oxygen atom exists between the lattices of the crystal structure of silicon carbide. Also, for example, a case in which two oxygen atoms exist in pairs at the carbon site of the crystal structure of silicon carbide. For example, the ratio of one oxygen atom bonded to four silicon atoms among the oxygen atoms contained in the oxygen region 20 is higher than the ratio of oxygen atoms existing between the lattices of the crystal structure of silicon carbide. Also, for example, the ratio of one oxygen atom bonded to four silicon atoms among the oxygen atoms contained in the oxygen region 20 is higher than the ratio of oxygen atoms existing in pairs at the carbon site of the crystal structure of silicon carbide.
[0080] In the method for manufacturing SBD 100 of the first embodiment, oxygen is introduced into silicon carbide layer 10 by ion implantation. The energy of the ion implantation breaks carbon bonds in silicon carbide layer 10, forming a large number of carbon vacancies. By filling the large number of carbon vacancies with oxygen atoms, it is possible to form a large number of localized states in oxygen region 20. Furthermore, oxygen is introduced into silicon carbide layer 10 in the form of atoms (ions) rather than molecules, making it easy to fill the carbon vacancies with a single oxygen atom.
[0081] Fig. 12 is an explanatory diagram of the action and effect of the manufacturing method of the semiconductor device of the first embodiment. Fig. 12 is a diagram showing the oxygen concentration distribution in the manufacturing method of the semiconductor device of the first embodiment. Fig. 12 shows the oxygen concentration distribution in the depth direction of the anode electrode 12 and the silicon carbide layer 10. Fig. 12 shows the oxygen concentration distribution in the depth direction of the anode electrode 12, the oxygen region 20, and the drift region 18.
[0082] In Fig. 12, the dashed curve indicates the oxygen concentration distribution immediately after oxygen ion implantation, and the solid curve indicates the oxygen concentration distribution after pile-up annealing.
[0083] Immediately after the ion implantation, a peak of the oxygen concentration distribution is formed at a depth determined by the acceleration energy of the ion implantation. Thereafter, before the formation of the anode electrode 12, diffusion annealing is performed, whereby oxygen is diffused toward the front and back sides of the silicon carbide layer 10.
[0084] Then, by performing pile-up annealing after the formation of the anode electrode 12, oxygen piles up at the interface between the anode electrode 12 and the oxygen region 20. This is because the structure in which the carbon vacancy is filled with one oxygen atom becomes more energetically stable as it approaches the anode electrode 12. As it approaches the anode electrode 12, the movement of localized electrons between the anode electrode 12 and the structure in which the carbon vacancy is filled with one oxygen atom becomes easier, so that the structure in which the carbon vacancy is filled with one oxygen atom becomes more energetically stable.
[0085] In the SBD 100 of the first embodiment, the variation in Schottky barrier height is suppressed by providing the oxygen region 20. Therefore, the SBD 100 with stable rectification characteristics can be realized.
[0086] In the SBD 100 of the first embodiment, the Schottky barrier height is fixed at approximately 0.8 eV by providing the oxygen region 20. This allows the material of the anode electrode 12 to be selected arbitrarily. This increases the degree of freedom in the structural design and manufacturing process of the SBD 100.
[0087] As described above, according to the first embodiment, a semiconductor device in which the variation in Schottky barrier height is suppressed can be realized.
[0088] Second embodiment The semiconductor device of the second embodiment differs from the semiconductor device of the first embodiment in that the silicon carbide layer further includes a pair of p-type third silicon carbide regions in contact with the first electrode, sandwiching the second silicon carbide region therebetween. Hereinafter, some of the description that overlaps with the first embodiment will be omitted.
[0089] 13 is a schematic cross-sectional view of a semiconductor device according to a second embodiment. The semiconductor device according to the second embodiment is a JBS (Junction Barrier Schottky) diode. The semiconductor device according to the second embodiment is a JBS diode 200. The JBS diode 200 uses electrons as carriers.
[0090] The JBS diode 200 includes a silicon carbide layer 10, an anode electrode 12 (first electrode), and a cathode electrode 14 (second electrode).
[0091] The anode electrode 12 is an example of a first electrode, and the cathode electrode 14 is an example of a second electrode.
[0092] The silicon carbide layer 10 includes a cathode region 16, a drift region 18 (first silicon carbide region), an oxygen region 20 (second silicon carbide region), and a number of p-type regions 26 (third silicon carbide regions).
[0093] The multiple p-type regions 26 are located between the drift region 18 and the anode electrode 12. The p-type regions 26 are located between the drift region 18 and the first plane P1. The p-type regions 26 contact the anode electrode 12.
[0094] A pair of p-type regions 26 sandwich the oxygen region 20. The depth of the p-type region 26 is, for example, deeper than the depth of the oxygen region 20. The pair of p-type regions 26 sandwich the drift region 18 therebetween.
[0095] The p-type region 26 includes a p-type impurity. The p-type region 26 includes, for example, aluminum (Al) or boron (B) as a p-type impurity. The p-type impurity concentration of the p-type region 26 is, for example, 1×10 18 cm -3 More than 1×10 21 cm -3 The following is the result.
[0096] In the JBS diode 200, when reverse bias is applied, a depletion layer is connected to the drift region 18 between the p-type regions 26. Therefore, leakage current when reverse bias is applied is suppressed.
[0097] As described above, according to the second embodiment, a semiconductor device in which the variation in Schottky barrier height is suppressed can be realized, as in the first embodiment, and a semiconductor device in which the leakage current during reverse bias is suppressed can be realized.
[0098] (Third embodiment) The semiconductor device of the third embodiment includes a first electrode, a second electrode, and a silicon carbide layer between the first electrode and the second electrode, the silicon carbide layer including an n-type first silicon carbide region, a second silicon carbide region between the first silicon carbide region and the first electrode, contacting the first electrode, and containing one oxygen atom bonded to four silicon atoms, a p-type third silicon carbide region between the first silicon carbide region and the first electrode, and a fourth n-type silicon carbide region between the third silicon carbide region and the first electrode, contacting the first electrode, and having a higher n-type impurity concentration than the first silicon carbide region, a gate electrode located on the first electrode side of the silicon carbide layer, and a gate insulating layer located between the gate electrode and the third silicon carbide region. Hereinafter, some of the contents that overlap with the first embodiment will be omitted.
[0099] 14 is a schematic cross-sectional view of a semiconductor device according to the third embodiment. The semiconductor device according to the third embodiment is a planar gate vertical MOSFET 300. The MOSFET 300 is an n-channel transistor that uses electrons as carriers.
[0100] The MOSFET 300 includes an SBD as a built-in diode. The SBD as the built-in diode has the same structure as the SBD 100 of the first embodiment.
[0101] The MOSFET 300 includes a silicon carbide layer 10, a source electrode 42 (first electrode), a drain electrode 44 (second electrode), a gate insulating layer 46, a gate electrode 50, and an interlayer insulating layer 52. The source electrode 42 has a first portion 42X and a second portion 42Y.
[0102] The source electrode 42 is an example of a first electrode, and the drain electrode 44 is an example of a second electrode.
[0103] The silicon carbide layer 10 includes a drain region 54, a drift region 56 (first silicon carbide region), an oxygen region 57 (second silicon carbide region), a p-well region 58 (third silicon carbide region), a source region 60 (fourth silicon carbide region), and a p-well contact region 62.
[0104] The silicon carbide layer 10 is, for example, a single crystal of 4H-SiC. The silicon carbide layer 10 has a first surface P1 and a second surface P2. The second surface P2 faces the first surface P1. The first surface P1 is a front surface of the silicon carbide layer 10, and the second surface P2 is a back surface of the silicon carbide layer 10.
[0105] Silicon carbide layer 10 is located between source electrode 42 and drain electrode 44 .
[0106] In this specification, the term "depth" refers to the distance in a direction from the first plane P1 toward the second plane P2, with the first plane P1 being used as a reference.
[0107] The drain region 54 is + The drain region 54 is made of SiC of the n-type. The drain region 54 contains, for example, nitrogen (N) as an n-type impurity. The n-type impurity concentration of the drain region 54 is, for example, 1×10 18 cm -3 More than 1×10 21 cm -3 The following is the result.
[0108] The drift region 56 is - The drift region 56 is a type of SiC. The drift region 56 is located between the drain region 54 and the source electrode 42. The drift region 56 is located between the drain region 54 and the first plane P1. A portion of the drift region 56 contacts the first plane P1.
[0109] The drift region 56 contains, for example, nitrogen (N) as an n-type impurity. The n-type impurity concentration of the drift region 56 is, for example, 1×10 15 cm -3More than 2×10 16 cm -3 The n-type impurity concentration of the drift region 56 is lower than the n-type impurity concentration of the drain region 54.
[0110] The drift region 56 is, for example, an epitaxially grown layer of SiC formed by epitaxial growth on the drain region 54. The drift region 56 has a thickness of, for example, 5 μm or more and 100 μm or less.
[0111] The oxygen region 57 is - The oxide region 57 is located between the drift region 18 and the source electrode 42. The oxygen region 57 is located between the drift region 18 and the first plane P1. The oxygen region 57 contacts the source electrode 42.
[0112] The oxygen region 57 contains oxygen as an impurity. The maximum concentration of oxygen in the oxygen region 57 is, for example, 1×10 17 cm -3 More than 1×10 21 cm -3 The following is the result.
[0113] Oxygen region 57 contains one oxygen atom bonded to four silicon atoms.
[0114] The oxygen region 57 contains, for example, nitrogen (N) as an n-type impurity. The n-type impurity concentration of the oxygen region 57 is, for example, 1×10 15 cm -3 More than 2×10 16 cm -3 The following is the result.
[0115] The oxygen region 57 is sandwiched between a pair of p-well regions 58 .
[0116] The p-well region 58 is made of p-type SiC. The p-well region 58 is located between the drift region 56 and the source electrode 42. The p-well region 58 is located between the drift region 56 and the first plane P1. A portion of the p-well region 58 contacts the first plane P1.
[0117] The p-well region 58 contains, for example, aluminum (Al) as a p-type impurity. The p-type impurity concentration of the p-well region 58 is, for example, 1×10 16 cm -3 More than 1×10 20 cm -3 The following is the result.
[0118] The depth of the p-well region 58 is, for example, not less than 0.4 μm and not more than 0.8 μm. The p-well region 58 functions as a channel region of the MOSFET 300.
[0119] The source region 60 is + The source region 60 is located between the p-well region 58 and the source electrode 42. The source region 60 is located between the p-well region 58 and the first face P1. A portion of the source region 60 contacts the first face P1.
[0120] The source region 60 contains phosphorus (P) or nitrogen (N) as an n-type impurity. The n-type impurity concentration of the source region 60 is, for example, 1×10 18 cm -3 More than 1×10 22 cm -3 The n-type impurity concentration of the source region 60 is higher than the n-type impurity concentration of the drift region 56.
[0121] The depth of the source region 60 is shallower than the depth of the p-well region 58. The depth of the source region 60 is, for example, not less than 0.1 μm and not more than 0.4 μm.
[0122] The p-well contact region 62 is + The p-well contact region 62 is located between the p-well region 58 and the source electrode 42. The p-well contact region 62 is located between the p-well region 58 and the first face P1. The p-well contact region 62 is adjacent to the source region 60.
[0123] The p-well contact region 62 contains, for example, aluminum as a p-type impurity. The p-type impurity concentration of the p-well contact region 62 is, for example, 1×1018 cm -3 More than 1×10 22 cm -3 The p-type impurity concentration of the p-well contact region 62 is higher than the p-type impurity concentration of the p-well region 58.
[0124] The depth of the p-well contact region 62 is shallower than the depth of the p-well region 58. The depth of the p-well contact region 62 is, for example, not less than 0.1 μm and not more than 0.4 μm.
[0125] The gate insulating layer 46 is located between the silicon carbide layer 10 and the gate electrode 50. The gate insulating layer 46 is located between the p-well region 58 and the gate electrode 50.
[0126] The gate insulating layer 46 is, for example, an oxide or an oxynitride. The gate insulating layer 46 is, for example, a silicon oxide. The thickness of the gate insulating layer 46 is, for example, 30 nm or more.
[0127] The gate insulating layer 46 is in contact with the p-well region 58. The p-well region 58 in the vicinity of the gate insulating layer 46 becomes the channel region of the MOSFET 300.
[0128] The gate electrode 50 is located on the first face P1 side of the silicon carbide layer 10. The gate electrode 50 is provided on the gate insulating layer 46. The gate electrode 50 sandwiches the gate insulating layer 46 between the drift region 56, the source region 60, and the p-well region 58.
[0129] The gate electrode 50 is a conductor. The gate electrode 50 is, for example, polycrystalline silicon containing n-type impurities or p-type impurities. The gate electrode 50 may be, for example, a metal such as titanium nitride, tungsten nitride, tungsten, aluminum, copper, ruthenium, cobalt, nickel, cobalt silicide, or nickel silicide. The gate electrode 50 may have a stacked structure of any one of the above metals and polycrystalline silicon containing n-type impurities or p-type impurities.
[0130] The interlayer insulating layer 52 is formed on the gate electrode 50. The interlayer insulating layer 52 electrically separates the gate electrode 50 from the source electrode 42. The interlayer insulating layer 52 is, for example, silicon oxide.
[0131] The source electrode 42 is located on the first face P1 side of the silicon carbide layer 10. The source electrode 42 is electrically connected to the oxygen region 57, the source region 60, and the p-well contact region 62. The source electrode 42 contacts the oxygen region 57, the source region 60, and the p-well contact region 62. The source electrode 42 also functions as a p-well electrode that applies a potential to the p-well region 58.
[0132] An ohmic contact is formed between the source electrode 42 and the source region 60. An ohmic contact is formed between the source electrode 42 and the p-well contact region 62.
[0133] There is a Schottky contact between the source electrode 42 and the oxygen region 57. The Schottky barrier height between the source electrode 42 and the oxygen region 57 is, for example, not less than 0.7 eV and not more than 1.0 eV. The Schottky barrier height between the source electrode 42 and the oxygen region 57 is, for example, about 0.8 eV.
[0134] The source electrode 42 is a conductor, for example, a metal, an intermetallic compound, a metal nitride, a metal silicide, or a semiconductor.
[0135] The source electrode 42 may have, for example, a laminated structure. The source electrode 42 has, for example, a laminated structure of two different metals. The source electrode 42 has, for example, a laminated structure of a metal silicide and a metal.
[0136] The source electrode 42 has, for example, a laminated structure of titanium and aluminum. The source electrode 42 includes, for example, nickel silicide. The source electrode 42 has, for example, a laminated structure of nickel silicide and aluminum.
[0137] The source electrode 42 has a first portion 42X and a second portion 42Y. The first portion 42X contacts the oxygen region 57. The second portion 42Y contacts the source region 60. The first portion 42X and the second portion 42Y are, for example, made of the same material. The first portion 42X and the second portion 42Y have, for example, the same chemical composition.
[0138] The drain electrode 44 is located on the second face P2 side of the silicon carbide layer 10. The drain electrode 44 is in contact with the drain region 54. The drain electrode 44 is electrically connected to the drain region 54.
[0139] The drain electrode 44 is a conductor, for example, a metal, an intermetallic compound, a metal nitride, a metal silicide, or a semiconductor.
[0140] The drain electrode 44 is, for example, nickel. Nickel may react with the silicon carbide layer 10 to form nickel silicide. The nickel silicide is, for example, NiSi or Ni2Si.
[0141] The operation and effects of the semiconductor device of the third embodiment will be described below.
[0142] 15 is an equivalent circuit diagram of the semiconductor device of the third embodiment. A pn diode and an SBD are connected as built-in diodes in parallel to a transistor having a gate electrode 50 between a source electrode 42 and a drain electrode 44. The source electrode 42 is the anode of the pn junction diode, and the drain electrode 44 is the cathode of the pn junction diode. In addition, the source electrode 42 is the anode of the SBD, and the drain electrode 44 is the cathode of the SBD.
[0143] The source electrode 42, the oxygen region 57, the drift region 56, the drain region 54, and the drain electrode 44 constitute an SBD.
[0144] For example, consider a case where MOSFET 300 is used as a switching element connected to an inductive load. When MOSFET 300 is off, a load current caused by the inductive load may apply a voltage that makes source electrode 42 positive with respect to drain electrode 44. In this case, a forward current flows through the built-in diode. This state is also called a reverse conduction state.
[0145] The forward voltage (Vf) at which forward current begins to flow through the SBD is lower than the forward voltage (Vf) of a pn junction diode. Therefore, initially, forward current flows through the SBD.
[0146] The forward voltage (Vf) of the SBD is, for example, 0.8 V. The forward voltage (Vf) of the pn junction diode is, for example, 2.5 V.
[0147] The SBD operates in a unipolar manner, so that even if a forward current flows, stacking faults will not grow in the silicon carbide layer 10 due to carrier recombination energy, and therefore no fluctuation in on-resistance occurs due to the growth of stacking faults.
[0148] Moreover, the SBD of the MOSFET 300 includes an oxygen region 57. Therefore, similar to the SBD 100 of the first embodiment, the variation in Schottky barrier height is suppressed, and an SBD with stable rectification characteristics is realized.
[0149] In the MOSFET 300, in order to reduce the on-resistance, it is preferable that the second portion 42Y of the source electrode 42 and the source region 60 have an ohmic contact and low contact resistance. On the other hand, in order to realize the rectification action of the SBD, the first portion 42X of the source electrode 42 and the oxygen region 57 need to have a Schottky contact.
[0150] In the MOSFET 300, by providing the oxygen region 57, a Schottky contact is formed between the first portion 42X and the oxygen region 57, regardless of the material of the first portion 42X. Therefore, an optimal material for the source electrode 42 can be selected so that an ohmic contact and low contact resistance are formed between the second portion 42Y and the source region 60.
[0151] That is, the first portion 42X and the second portion 42Y can be made of the same material. Therefore, it is not necessary to adopt a complicated device structure in which different materials are used for the first portion 42X and the second portion 42Y. In addition, since the first portion 42X and the second portion 42Y can be made of the same material, the manufacturing process is simplified. Therefore, a MOSFET with an SBD having a simple device structure and a simple manufacturing process can be realized.
[0152] (First Modification) The semiconductor device according to the first modification of the third embodiment differs from the semiconductor device according to the third embodiment in that the silicon carbide layer includes a current spreading region.
[0153] 16 is a schematic cross-sectional view of a semiconductor device according to a first modification of the third embodiment. The semiconductor device according to the first modification of the third embodiment is a planar gate vertical MOSFET 310.
[0154] The silicon carbide layer 10 of the MOSFET 310 includes a current spreading region 63 .
[0155] The current spreading region 63 is made of n-type SiC. The current spreading region 63 is located between the drift region 56 and the p-well region 58.
[0156] The current spreading region 63 contains, for example, nitrogen (N) as an n-type impurity. The n-type impurity concentration of the current spreading region 63 is, for example, 2×10 15 cm -3 5×10 or more 16 cm -3 The n-type impurity concentration of the current spreading region 63 is higher than the n-type impurity concentration of the drift region 56.
[0157] The MOSFET 310 includes the current spreading region 63, which reduces the on-resistance compared to the MOSFET 300. In other words, the on-current of the MOSFET 310 is increased compared to the MOSFET 300. Furthermore, the forward current of the SBD built into the MOSFET 310 is also increased compared to the MOSFET 300.
[0158] (Second Modification) The semiconductor device according to the second modification of the third embodiment differs from the semiconductor device according to the third embodiment in that the semiconductor device according to the second modification includes a silicide layer whose side surface is in contact with the fourth silicon carbide region.
[0159] 17 is a schematic cross-sectional view of a semiconductor device according to a second modification of the third embodiment. The semiconductor device according to the second modification of the third embodiment is a planar gate vertical MOSFET 320.
[0160] The MOSFET 320 includes a silicide layer 65 .
[0161] The p-well contact region 62 is deeper than the source region 60 .
[0162] The silicide layer 65 is provided between the source electrode 42 and the p-well contact region 62. The side surface of the silicide layer 65 contacts the source region 60.
[0163] The silicide layer 65 is in contact with the source electrode 42. The silicide layer 65 can also be considered as a part of the source electrode 42. The silicide layer 65 is, for example, nickel silicide.
[0164] The MOSFET 320 includes the silicide layer 65, which reduces the electrical resistance between the source electrode 42 and the source region 60. Therefore, the on-resistance of the MOSFET 320 is reduced compared to the MOSFET 300. In other words, the on-current of the MOSFET 320 is increased compared to the MOSFET 300.
[0165] As described above, according to the third embodiment and its modifications, a semiconductor device in which the variation in Schottky barrier height is suppressed can be realized. In addition, a semiconductor device having a simple device structure and a simple manufacturing process can be realized.
[0166] (Fourth embodiment) The semiconductor device of the fourth embodiment differs from the semiconductor device of the third embodiment in that the third silicon carbide region is in contact with the second silicon carbide region. Hereinafter, some of the contents that overlap with the third embodiment will not be described.
[0167] Fig. 18 is a schematic cross-sectional view of the semiconductor device of the fourth embodiment. Fig. 19 is a schematic top view of the semiconductor device of the fourth embodiment. Fig. 20 is a schematic cross-sectional view of the semiconductor device of the fourth embodiment. Fig. 18 is an AA' cross section of Fig. 19. Fig. 20 is a BB' cross section of Fig. 19.
[0168] The semiconductor device of the fourth embodiment is a planar gate vertical MOSFET 400. The MOSFET 400 is an n-channel transistor that uses electrons as carriers.
[0169] The MOSFET 400 includes an SBD as a built-in diode. The SBD as the built-in diode has the same structure as the SBD 100 of the first embodiment. The built-in diode is a Merged PiN Schottky (MPS) diode.
[0170] The MOSFET 400 includes a silicon carbide layer 10, a source electrode 42 (first electrode), a drain electrode 44 (second electrode), a gate insulating layer 46, a gate electrode 50, and an interlayer insulating layer 52. The source electrode 42 has a first portion 42X and a second portion 42Y.
[0171] The source electrode 42 is an example of a first electrode, and the drain electrode 44 is an example of a second electrode.
[0172] The silicon carbide layer 10 includes a drain region 54, a drift region 56 (first silicon carbide region), an oxygen region 57 (second silicon carbide region), a p-well region 58 (third silicon carbide region), a source region 60 (fourth silicon carbide region), and a p-well contact region 62.
[0173] The oxygen region 57 is - The oxide region 57 is located between the drift region 18 and the source electrode 42. The oxygen region 57 is located between the drift region 18 and the first plane P1. The oxygen region 57 contacts the source electrode 42.
[0174] The oxygen region 57 is surrounded by the p-well contact region 62. The oxygen region 57 contacts the p-well contact region 62.
[0175] The p-well contact region 62 is + The p-well contact region 62 is located between the p-well region 58 and the source electrode 42. The p-well contact region 62 is located between the p-well region 58 and the first face P1. The p-well contact region 62 is adjacent to the source region 60.
[0176] A p-well contact region 62 surrounds the oxygen region 57 .
[0177] Fig. 21 is a top view of the fourth embodiment and the modification thereof Fig. 21 shows the layout pattern of the oxygen region 57 and the p-well contact region 62 of the fourth embodiment and the modification thereof.
[0178] FIG. 21(a) is a top view of the fourth embodiment, FIG. 21(b) is a top view of the first modified example, FIG. 21(c) is a top view of the second modified example, FIG. 21(d) is a top view of the third modified example, and FIG. 21(e) is a top view of the fourth modified example.
[0179] The layout pattern of the oxygen regions 57 and the p-well contact regions 62 may be a lattice pattern as shown in Fig. 21(b), a stripe pattern as shown in Fig. 21(c) or Fig. 21(d), or a hexagonal pattern as shown in Fig. 21(e).
[0180] As described above, according to the fourth embodiment, a semiconductor device in which the variation in Schottky barrier height is suppressed can be realized. In addition, a semiconductor device having a simple device structure and a simple manufacturing process can be realized.
[0181] Fifth embodiment The semiconductor device of the fifth embodiment differs from the semiconductor device of the fourth embodiment in that the interface between the second silicon carbide region and the first electrode is closer to the second surface than to the first surface. Hereinafter, some of the contents that overlap with the fourth embodiment will not be described.
[0182] Fig. 22 is a schematic cross-sectional view of a semiconductor device according to a fifth embodiment, which corresponds to Fig. 18 of the fourth embodiment.
[0183] The semiconductor device of the fifth embodiment is a planar gate vertical MOSFET 500. The MOSFET 500 is an n-channel transistor that uses electrons as carriers.
[0184] The MOSFET 500 includes an SBD as a built-in diode. The SBD as the built-in diode has the same structure as the SBD 100 of the first embodiment. The built-in diode is an MPS diode.
[0185] The MOSFET 500 includes a silicon carbide layer 10, a source electrode 42 (first electrode), a drain electrode 44 (second electrode), a gate insulating layer 46, a gate electrode 50, and an interlayer insulating layer 52. The source electrode 42 has a first portion 42X and a second portion 42Y.
[0186] The source electrode 42 is an example of a first electrode, and the drain electrode 44 is an example of a second electrode.
[0187] The silicon carbide layer 10 includes a drain region 54, a drift region 56 (first silicon carbide region), an oxygen region 57 (second silicon carbide region), a p-well region 58 (third silicon carbide region), a source region 60 (fourth silicon carbide region), and a p-well contact region 62.
[0188] The oxygen region 57 is - The oxide region 57 is located between the drift region 18 and the source electrode 42. The oxygen region 57 is located between the drift region 18 and the first plane P1. The oxygen region 57 contacts the source electrode 42.
[0189] The oxygen region 57 is surrounded by the p-well contact region 62. The oxygen region 57 contacts the p-well contact region 62.
[0190] The interface between the oxygen region 57 and the source electrode 42 is located closer to the second face P2 than to the first face P1. For example, a part of the source electrode 42 is embedded in a groove provided in the silicon carbide layer 10.
[0191] (Modification) The semiconductor device of the modification of the fifth embodiment differs from the semiconductor device of the fifth embodiment in that the pattern of the fourth silicon carbide region is different.
[0192] Fig. 23 is a schematic cross-sectional view of a semiconductor device according to a modification of the fifth embodiment. Fig. 24 is a schematic top view of a semiconductor device according to a modification of the fifth embodiment. Fig. 25 is a schematic cross-sectional view of a semiconductor device according to a modification of the fifth embodiment. Fig. 23 is a cross-section taken along CC' in Fig. 24. Fig. 25 is a cross-section taken along DD' in Fig. 24.
[0193] The semiconductor device according to the modification of the fifth embodiment is a planar gate vertical MOSFET 510.
[0194] A portion of the source electrode 42 is embedded in a groove provided in the silicon carbide layer 10. The source region 60 contacts a side surface of the portion of the source electrode 42 embedded in the groove.
[0195] As shown in FIG. 24, on the first face P1 of the silicon carbide layer 10, the source region 60 is sandwiched between p-well contact regions 62.
[0196] Oxygen region 57 is surrounded by p-well contact region 62 and p-well region 58 .
[0197] The MOSFET 510 reduces the electrical resistance between the source electrode 42 and the source region 60 compared to the MOSFET 500. Therefore, the on-resistance of the MOSFET 510 is reduced compared to the MOSFET 500. In other words, the on-current of the MOSFET 510 is increased compared to the MOSFET 500.
[0198] As described above, according to the fifth embodiment and its modifications, a semiconductor device in which the variation in Schottky barrier height is suppressed can be realized. In addition, a semiconductor device having a simple device structure and a simple manufacturing process can be realized.
[0199] Sixth embodiment The semiconductor device of the sixth embodiment differs from the semiconductor device of the third embodiment in that the sixth embodiment includes a gate trench and a source trench. In the following, some of the contents that overlap with the third embodiment will not be described.
[0200] 26 is a schematic cross-sectional view of a semiconductor device according to the sixth embodiment. The semiconductor device according to the sixth embodiment is a trench-gate vertical MOSFET 600. In the MOSFET 600, a part of the source electrode is provided in the source trench. The MOSFET 600 is a so-called double trench structure MOSFET. It is an n-channel transistor that uses electrons as carriers.
[0201] The MOSFET 600 includes an SBD as a built-in diode. The SBD as the built-in diode has the same structure as the SBD 100 of the first embodiment.
[0202] The MOSFET 600 includes a silicon carbide layer 10, a source electrode 42 (first electrode), a drain electrode 44 (second electrode), a gate insulating layer 46, a gate electrode 50, and an interlayer insulating layer 52. The source electrode 42 has a first portion 42X and a second portion 42Y.
[0203] The source electrode 42 is an example of a first electrode, and the drain electrode 44 is an example of a second electrode.
[0204] The silicon carbide layer 10 includes a drain region 54, a drift region 56 (first silicon carbide region), an oxygen region 57 (second silicon carbide region), a p-well region 58 (third silicon carbide region), a source region 60 (fourth silicon carbide region), a p-well contact region 62, an electric field relaxation region 64, a gate trench 70, and a source trench 80.
[0205] The gate trench 70 is provided on the first face P1 side of the silicon carbide layer 10. The depth of the gate trench 70 is deeper than the depth of the p-well region 58.
[0206] The gate insulating layer 46 is disposed in the gate trench 70. The gate electrode 50 is disposed in the gate trench 70. The gate electrode 50 is disposed on the gate insulating layer 46.
[0207] The source trench 80 is provided on the first face P1 side of the silicon carbide layer 10. The depth of the source trench 80 is deeper than the depth of the p-well region 58.
[0208] A portion of the source electrode 42 is provided in the source trench 80. The oxygen region 57 and the source electrode 42 are in contact with each other on a side surface of the source trench 80. The p-well contact region 62 and the source electrode 42 are in contact with each other on a side surface of the source trench 80.
[0209] The electric field relaxation region 64 is p+ The electric field relaxation region 64 is provided between the drift region 56 and the source trench 80. The electric field relaxation region 64 is provided at the bottom of the source trench 80. The electric field relaxation region 64 has a function of reducing the electric field strength applied to the gate insulating layer 46 in the gate trench 70.
[0210] The electric field buffer region 64 contains, for example, aluminum as a p-type impurity. The p-type impurity concentration of the electric field buffer region 64 is, for example, 1×10 18 cm -3 More than 1×10 22 cm -3 The p-type impurity concentration of the electric field buffer region 64 is higher than the p-type impurity concentration of the p-well region 58.
[0211] According to the MOSFET 600 of the sixth embodiment, the double trench structure enables miniaturization, and the on-resistance per unit area can be reduced.
[0212] As described above, according to the sixth embodiment, a semiconductor device in which the variation in Schottky barrier height is suppressed can be realized. In addition, a semiconductor device having a simple device structure and a simple manufacturing process can be realized. In addition, a semiconductor device in which the on-resistance per unit area can be reduced can be realized.
[0213] Seventh embodiment The semiconductor device of the seventh embodiment differs from the semiconductor device of the sixth embodiment in that an oxygen region is provided at the bottom of a source trench. Hereinafter, some of the contents that overlap with the sixth embodiment will not be described.
[0214] 27 is a schematic cross-sectional view of a semiconductor device according to the seventh embodiment. The semiconductor device according to the seventh embodiment is a trench-gate vertical MOSFET 700. In addition, a part of the source electrode of the MOSFET 700 is provided in the source trench. The MOSFET 700 is a so-called double trench structure MOSFET. It is an n-channel transistor that uses electrons as carriers.
[0215] The MOSFET 700 includes an SBD as a built-in diode. The SBD as the built-in diode has the same structure as the SBD 100 of the first embodiment.
[0216] The MOSFET 700 includes a silicon carbide layer 10, a source electrode 42 (first electrode), a drain electrode 44 (second electrode), a gate insulating layer 46, a gate electrode 50, and an interlayer insulating layer 52. The source electrode 42 has a first portion 42X and a second portion 42Y.
[0217] The source electrode 42 is an example of a first electrode, and the drain electrode 44 is an example of a second electrode.
[0218] The silicon carbide layer 10 includes a drain region 54, a drift region 56 (first silicon carbide region), an oxygen region 57 (second silicon carbide region), a p-well region 58 (third silicon carbide region), a source region 60 (fourth silicon carbide region), a p-well contact region 62, an electric field relaxation region 64, a gate trench 70, and a source trench 80.
[0219] A portion of the source electrode 42 is provided in the source trench 80. The oxygen region 57 and the source electrode 42 are in contact with each other at the bottom of the source trench 80. The p-well contact region 62 and the source electrode 42 are in contact with each other at the side of the source trench 80.
[0220] The electric field relaxation region 64 is p + The electric field relaxation region 64 is provided between the drift region 56 and the gate trench 70.
[0221] According to the MOSFET 700 of the seventh embodiment, the double trench structure enables miniaturization, and the on-resistance per unit area can be reduced.
[0222] As described above, according to the seventh embodiment, a semiconductor device in which the variation in Schottky barrier height is suppressed can be realized. In addition, a semiconductor device having a simple device structure and a simple manufacturing process can be realized. In addition, a semiconductor device in which the on-resistance per unit area can be reduced can be realized.
[0223] Eighth embodiment The semiconductor device of the eighth embodiment is different from the semiconductor device of the sixth embodiment in that two source trenches are provided and the oxygen region and the first electrode are in contact with each other on the first surface. Hereinafter, some of the contents that overlap with the sixth embodiment will be omitted.
[0224] Fig. 28 is a schematic cross-sectional view of the semiconductor device of the eighth embodiment. Fig. 29 is a schematic top view of the semiconductor device of the eighth embodiment. Fig. 28 is an EE' cross section of Fig. 29.
[0225] The semiconductor device of the eighth embodiment is a trench-gate vertical MOSFET 800. In the MOSFET 800, a part of the source electrode is provided in the source trench. The MOSFET 800 is a so-called double-trench structure MOSFET. It is an n-channel transistor that uses electrons as carriers.
[0226] The MOSFET 800 includes an SBD as a built-in diode. The SBD as the built-in diode has the same structure as the SBD 100 of the first embodiment. The built-in diode is an MPS diode.
[0227] The MOSFET 800 includes a silicon carbide layer 10, a source electrode 42 (first electrode), a drain electrode 44 (second electrode), a gate insulating layer 46, a gate electrode 50, and an interlayer insulating layer 52. The source electrode 42 has a first portion 42X and a second portion 42Y.
[0228] The source electrode 42 is an example of a first electrode, and the drain electrode 44 is an example of a second electrode.
[0229] The silicon carbide layer 10 includes a drain region 54, a drift region 56 (first silicon carbide region), an oxygen region 57 (second silicon carbide region), a p-well region 58 (third silicon carbide region), a source region 60 (fourth silicon carbide region), a p-well contact region 62, a gate trench 70, a first source trench 80a, and a second source trench 80b.
[0230] A portion of the source electrode 42 is provided in the first source trench 80a and the second source trench 80b. The oxygen region 57 and the source electrode 42 are in contact with each other at a first surface P1.
[0231] The oxygen region 57 is sandwiched between the first source trench 80a and the second source trench 80b. The oxygen region 57 is sandwiched between the p-well contact regions 62. The oxygen region 57 contacts the p-well contact regions 62. The p-well contact regions 62 also function as electric field relief regions.
[0232] As described above, according to the eighth embodiment, a semiconductor device in which the variation in Schottky barrier height is suppressed can be realized. In addition, a semiconductor device having a simple device structure and a simple manufacturing process can be realized. In addition, a semiconductor device in which the on-resistance per unit area can be reduced can be realized.
[0233] Ninth embodiment The semiconductor device of the ninth embodiment differs from the semiconductor device of the eighth embodiment in that another trench is provided between the two source trenches. Hereinafter, some of the contents that overlap with the eighth embodiment will not be described.
[0234] Fig. 30 is a schematic cross-sectional view of a semiconductor device according to a ninth embodiment, which corresponds to Fig. 28 of the eighth embodiment.
[0235] The semiconductor device of the ninth embodiment is a trench-gate vertical MOSFET 900. In the MOSFET 900, a part of the source electrode is provided in the source trench. The MOSFET 900 is a so-called double-trench structure MOSFET. It is an n-channel transistor that uses electrons as carriers.
[0236] The MOSFET 900 includes an SBD as a built-in diode. The SBD as the built-in diode has the same structure as the SBD 100 of the first embodiment. The built-in diode is an MPS diode.
[0237] The MOSFET 900 includes a silicon carbide layer 10, a source electrode 42 (first electrode), a drain electrode 44 (second electrode), a gate insulating layer 46, a gate electrode 50, and an interlayer insulating layer 52. The source electrode 42 has a first portion 42X and a second portion 42Y.
[0238] The source electrode 42 is an example of a first electrode, and the drain electrode 44 is an example of a second electrode.
[0239] The silicon carbide layer 10 includes a drain region 54, a drift region 56 (first silicon carbide region), an oxygen region 57 (second silicon carbide region), a p-well region 58 (third silicon carbide region), a source region 60 (fourth silicon carbide region), a p-well contact region 62, a p-region 66, a gate trench 70, a first source trench 80a, a second source trench 80b, and an intermediate trench 82.
[0240] The intermediate trench is provided between the first source trench 80a and the second source trench 80b.
[0241] A portion of the source electrode 42 is provided in the first source trench 80a, the second source trench 80b, and the intermediate trench 82. The oxygen region 57 and the source electrode 42 are in contact with each other at a first surface P1.
[0242] The oxygen region 57 is sandwiched between the first source trench 80 a and the intermediate trench 82 . Oxygen region 57 is sandwiched between intermediate trench 82 and second source trench 80b. Oxygen region 57 is sandwiched between p-well contact region 62 and p-region 66. Oxygen region 57 borders p-well contact region 62 and p-region 66.
[0243] As described above, according to the ninth embodiment, a semiconductor device in which the variation in Schottky barrier height is suppressed can be realized. In addition, a semiconductor device having a simple device structure and a simple manufacturing process can be realized. In addition, a semiconductor device in which the on-resistance per unit area can be reduced can be realized.
[0244] (Tenth embodiment) The inverter circuit and the drive device of the tenth embodiment are an inverter circuit and a drive device including the semiconductor device of the third embodiment.
[0245] 31 is a schematic diagram of a driving device according to a tenth embodiment. The driving device 1000 includes a motor 140 and an inverter circuit 150.
[0246] The inverter circuit 150 is composed of three semiconductor modules 150a, 150b, and 150c, each of which uses the MOSFET 300 of the third embodiment as a switching element. By connecting the three semiconductor modules 150a, 150b, and 150c in parallel, a three-phase inverter circuit 150 having three AC voltage output terminals U, V, and W is realized. The motor 140 is driven by the AC voltage output from the inverter circuit 150.
[0247] According to the tenth embodiment, the MOSFET 300 with improved characteristics is provided, and thus the characteristics of the inverter circuit 150 and the driving device 1000 are improved.
[0248] (Eleventh embodiment) The vehicle of the eleventh embodiment is a vehicle equipped with the semiconductor device of the third embodiment.
[0249] 32 is a schematic diagram of a vehicle according to an eleventh embodiment. A vehicle 1100 according to the eleventh embodiment is a railcar. The vehicle 800 includes a motor 140 and an inverter circuit 150.
[0250] The inverter circuit 150 is composed of three semiconductor modules using the MOSFET 300 of the third embodiment as a switching element. By connecting the three semiconductor modules in parallel, a three-phase inverter circuit 150 having three AC voltage output terminals U, V, and W is realized. The AC voltage output from the inverter circuit 150 drives the motor 140. The wheels 90 of the vehicle 1100 are rotated by the motor 140.
[0251] According to the eleventh embodiment, the vehicle 1100 is provided with the MOSFET 300 having improved characteristics, thereby improving the characteristics of the vehicle 1100.
[0252] (Twelfth embodiment) The vehicle of the twelfth embodiment is a vehicle equipped with the semiconductor device of the third embodiment.
[0253] 33 is a schematic diagram of a vehicle according to a twelfth embodiment. A vehicle 1200 according to the twelfth embodiment is an automobile. The vehicle 1200 includes a motor 140 and an inverter circuit 150.
[0254] The inverter circuit 150 is composed of three semiconductor modules using the MOSFET 300 of the third embodiment as a switching element. By connecting the three semiconductor modules in parallel, a three-phase inverter circuit 150 having three AC voltage output terminals U, V, and W is realized.
[0255] The motor 140 is driven by the AC voltage output from the inverter circuit 150. The motor 140 causes the wheels 90 of the vehicle 900 to rotate.
[0256] According to the twelfth embodiment, the vehicle 1200 is provided with the MOSFET 300 having improved characteristics, thereby improving the characteristics of the vehicle 1200.
[0257] Thirteenth embodiment The elevator of the thirteenth embodiment is an elevator including the semiconductor device of the third embodiment.
[0258] 34 is a schematic diagram of an elevator according to the thirteenth embodiment. The elevator 1300 according to the thirteenth embodiment includes a car 610, a counterweight 612, a wire rope 614, a hoist 616, a motor 140, and an inverter circuit 150.
[0259] The inverter circuit 150 is composed of three semiconductor modules using the MOSFET 300 of the third embodiment as a switching element. By connecting the three semiconductor modules in parallel, a three-phase inverter circuit 150 having three AC voltage output terminals U, V, and W is realized.
[0260] The motor 140 is driven by the AC voltage output from the inverter circuit 150. The motor 140 rotates the hoist 616, causing the car 610 to rise and fall.
[0261] According to the thirteenth embodiment, the elevator 1300 is provided with the MOSFET 300 having improved characteristics, thereby improving the characteristics of the elevator 1300.
[0262] While the above first to ninth embodiments have been described taking as an example the case of 4H—SiC as the crystal structure of silicon carbide, the present invention can also be applied to silicon carbide having a 3C—SiC or 6H—SiC crystal structure.
[0263] The present invention can also be applied to an MPS (Merged PiN Schottky) diode. For example, in the second embodiment shown in FIG. 13, if the p-type region 26 (third silicon carbide region) and the anode electrode 12 are brought into ohmic contact, an MPS is obtained. At this time, the drift region 18 and the anode electrode 12 form a Schottky contact having a stable barrier due to the oxygen region 20 (second silicon carbide region).
[0264] In the first to ninth embodiments, the n-type impurity is nitrogen or phosphorus. However, it is also possible to use arsenic (As) or antimony (Sb) as the n-type impurity.
[0265] Furthermore, in the first to ninth embodiments, the p-type impurity is aluminum or boron, but it is also possible to use gallium (Ga) or indium (In) as the p-type impurity.
[0266] In addition, in the tenth to thirteenth embodiments, the semiconductor device of the present invention is described as being applied to vehicles and elevators, but the semiconductor device of the present invention can also be applied to, for example, a power conditioner of a solar power generation system.
[0267] In addition, in the tenth to thirteenth embodiments, the case where the semiconductor device of the third embodiment is applied has been described as an example, but it is also possible to apply, for example, the semiconductor device of the fourth to ninth embodiments.
[0268] Although some embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. For example, components of one embodiment may be replaced or changed with components of another embodiment. These embodiments and their modifications are included in the scope and spirit of the invention, and are included in the scope of the invention and its equivalents described in the claims. [Explanation of symbols]
[0269] 10 Silicon carbide layer 12 Anode electrode (first electrode) 14 Cathode electrode (second electrode) 18 Drift region (first silicon carbide region) 20 Oxygen region (second silicon carbide region) 22 Oxide film 24 Laminated film (conductive film) 26 p-type region (third silicon carbide region) 42 source electrode (first electrode) 42X First Part 42Y Second Part 44 Drain electrode (second electrode) 46 Gate Insulation Layer 50 Gate electrode 56 Drift region (first silicon carbide region) 57 Oxygen region (second silicon carbide region) 58 p-well region (third silicon carbide region) 60 source region (fourth silicon carbide region) 100 SBD (semiconductor device) 150 Inverter circuit 200 JBS Diode (Semiconductor Device) 300 MOSFET (semiconductor device) 400 MOSFET (semiconductor device) 500 MOSFET (semiconductor device) 600 MOSFET (semiconductor device) 700 MOSFET (semiconductor device) 800 MOSFET (semiconductor device) 900 MOSFET (semiconductor device) 1000 Drive Unit 1100 vehicles 1200 vehicles 1300 Elevator
Claims
1. performing ion implantation of oxygen into a silicon carbide layer having an n-type first silicon carbide region; forming a conductive film on the silicon carbide layer; A first heat treatment is performed; a second heat treatment having a temperature higher than that of the first heat treatment is further performed after the ion implantation and before the conductive film is formed.
2. forming an oxide film on the silicon carbide layer prior to the ion implantation; 2. The method for manufacturing a semiconductor device according to claim 1, further comprising the steps of: removing the oxide film after the ion implantation and before forming the conductive film.
3. 3. The method for manufacturing a semiconductor device according to claim 1, wherein the temperature of the first heat treatment is 300.degree. C. or more and 700.degree. C. or less.
4. A method for manufacturing a semiconductor device described in any one of claims 1 to 3, wherein the temperature of the second heat treatment is 800°C or higher and 1000°C or lower.
Citation Information
Patent Citations
Semiconductor device and manufacturing method of the same
JP2015185617A
Method for forming semiconductor device, and semiconductor device
JP2015216371A
Semiconductor device, semiconductor device manufacturing method, inverter circuit, driving device, vehicle and lift
JP2016181672A
Semiconductor device, method of manufacturing the same, inverter circuit, drive device, vehicle, and elevator
JP2017126604A
Manufacturing method of semiconductor device
JP2018085382A