Silicon nitride sintered body, wear-resistant member, and method for manufacturing silicon nitride sintered body
The silicon nitride sintered body with optimized Raman spectroscopy peaks and controlled manufacturing enhances wear resistance and durability by reducing aggressiveness towards mating members, addressing the limitations of existing technologies.
Patent Information
- Application Number
- JP2023511258
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-03-30
- Filing Date
- 2022-03-28
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2042-03-28
AI Technical Summary
Existing silicon nitride sintered bodies, despite improving heat dissipation and bearing ball durability, fail to sufficiently reduce the aggressiveness towards mating members (outer and inner rings), leading to decreased durability of the bearing due to uneven wear.
A silicon nitride sintered body with specific Raman spectroscopy peak patterns and composition, including silicon nitride crystal grains and a grain boundary phase, optimized through controlled manufacturing processes to enhance wear resistance and reduce aggressiveness.
The optimized silicon nitride sintered body improves the durability of wear-resistant members by suppressing aggression towards mating members, extending the life of bearings and reducing electrolytic corrosion, while maintaining high strength and thermal conductivity.
Smart Images

Figure 0007581487000009 
Figure 0007581487000010 
Figure 0007581487000011
Abstract
Description
[Technical field]
[0001] The embodiments generally relate to a silicon nitride sintered body, a wear-resistant member, and a method for manufacturing the silicon nitride sintered body. [Background technology]
[0002] Silicon nitride sintered bodies are used as wear-resistant members such as bearing balls and rollers, taking advantage of their wear resistance. For example, Japanese Patent No. 5002155 (Patent Document 1) discloses a silicon nitride sintered body to which yttrium oxide, aluminum oxide, silicon carbide, etc. are added as sintering aids. The silicon nitride powder disclosed in Patent Document 1 is synthesized by a metal nitriding method. This method can provide a silicon nitride sintered body with high strength even if it contains a large amount of impurities such as Fe. Wear-resistant members using such silicon nitride sintered bodies exhibit excellent durability. For example, a bearing has a structure in which bearing balls are arranged between an outer ring and an inner ring. The lifespan of a bearing is affected by the lifespan of the bearing balls, the outer ring, and the inner ring. In Patent Document 1, the durability of the bearing balls made of sintered silicon nitride is improved. Meanwhile, bearing steel (SUJ2) is used for the outer ring and the inner ring. Even if the durability of the bearing balls is improved, the outer ring and the inner ring wear out, and the durability of the bearing decreases. In Japanese Patent Laid-Open Publication No. 2003-65337 (Patent Document 2), bearing balls made of sintered silicon nitride, which has high thermal conductivity, are used. By increasing the thermal conductivity of the sintered silicon nitride, heat dissipation is improved. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 5002155 [Patent Document 2] JP 2003-65337 A Summary of the Invention [Problem to be solved by the invention]
[0004] By improving the heat dissipation of the bearing balls, it was possible to suppress the thermal expansion of the outer and inner rings. However, no further effect was obtained. When the cause of this was investigated, it was found that the aggressiveness of the bearing balls towards the mating components (the outer and inner rings) had not been sufficiently reduced, which reduced durability. The present invention has been made to address such problems, and aims to provide a silicon nitride sintered body capable of improving the durability of a wear-resistant member. [Means for solving the problem]
[0005] The silicon nitride sintered body according to the embodiment includes silicon nitride crystal grains and a grain boundary phase, and when a 20 μm×20 μm region in a central cross section of the silicon nitride sintered body is subjected to Raman spectroscopy, two or more peaks are detected at 780 cm -1 ~810cm -1 and 1340cm -1 ~1370cm -1 , with four to six peaks at 170 cm -1 ~190cm -1 , 607cm -1 ~627cm -1 , 720cm -1 ~740cm -1 , and 924 cm -1 ~944cm -1 The detection range is [Brief description of the drawings]
[0006] [Figure 1] FIG. 2 is a diagram showing a part of a cross-sectional structure of a silicon nitride sintered body according to an embodiment. [Diagram 2] FIG. 2 is a diagram illustrating a schematic example of an analysis result by Raman spectroscopy of the silicon nitride sintered body according to the embodiment. [Diagram 3] 3A and 3B are diagrams illustrating an example of a bearing ball according to the embodiment. [Figure 4] FIG. 2 is a diagram showing an example of a bearing according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] The silicon nitride sintered body according to the embodiment includes silicon nitride crystal grains and a grain boundary phase, and when a 20 μm×20 μm region in a central cross section of the silicon nitride sintered body is subjected to Raman spectroscopy, two or more peaks are detected at 780 cm -1 ~810cm -1 and 1340cm -1 ~1370cm -1 , with four to six peaks at 170 cm -1 ~190cm -1 , 607cm -1 ~627cm -1 , 720cm -1 ~740cm -1 , and 924 cm -1 ~944cm -1 The detection range is FIG. 1 is a diagram showing a part of the cross-sectional structure of a silicon nitride sintered body according to an embodiment. In Fig. 1, 10 is a silicon nitride sintered body, 11 is silicon nitride crystal grains, and 12 is a grain boundary phase. As shown in Fig. 1, the silicon nitride sintered body 10 according to the embodiment includes silicon nitride crystal grains 11 and a grain boundary phase 12. The grain boundary phase is formed by a reaction between sintering aid powders or a reaction between the sintering aid powder and impurities in the silicon nitride powder. The grain boundary phase fills the gaps between the silicon nitride crystal grains. This can improve the strength of the sintered body. The invention according to the embodiment is characterized in that, when a central cross section of a silicon nitride sintered body is analyzed by Raman spectroscopy, a peak is detected in a predetermined wave number range.
[0008] Raman spectroscopy is a method for evaluating materials using Raman scattered light. Raman scattered light is a phenomenon in which light with different wave numbers corresponding to vibrational energy is scattered from excitation light. The difference in wavelength corresponds to the energy of the molecular vibration of the material. Raman scattered light with different wavelengths can be obtained between materials with different molecular structures. By examining the Raman scattered light, the vibrational mode of the atoms in the sample can be identified and data on the bonding state can be obtained. For example, even if the composition is the same, the obtained Raman scattered light will be different if the orientation or crystallinity is different.
[0009] The measurement area for the Raman spectroscopy was set to a unit area of 20 μm × 20 μm in the central cross section. With this size, both silicon nitride crystal grains and grain boundary phases can be included in the measurement area. The central cross section is a cross section that passes through the center of the silicon nitride sintered body. In other words, a 20 μm × 20 μm area including the center of the silicon nitride sintered body is set as the measurement area. If the sintered body is a sphere, the center of gravity is the center. If the sintered body is a rectangular parallelepiped, the intersection of the diagonals is the center. In addition, the silicon nitride sintered body can be surface-ground to produce a wear-resistant component. Since the surface is removed by grinding, the central cross section of the sintered body was set as the measurement area. The measurement equipment used for the Raman spectroscopy was a Renishaw inVia Reflex microscope (resolution: 0.3 cm). -1) or a device with equivalent or higher performance is used. The excitation laser used was a LD excitation green laser (wavelength 532 nm, output 100 mW). The irradiation laser beam diameter was set to 0.7 μm. The exposure time was set to 1 second per measurement point, and the stage movement step was set to 0.4 μm. Multivariate curve resolution (MCR) using the image analysis software WiRe4Empty Modelling was used for data analysis. Here, in the obtained Raman spectrum, the peaks detected by this analysis software were used as peaks, and the peak positions, their intensities, and half-widths were also determined using the analysis software. The peak intensity obtained by the analysis software at this time is the value obtained by the difference between the absolute value of the peak and the baseline value. The baseline value can also be obtained by the analysis software. In addition, the total number of measurement points was 2601. By performing an averaging process on the spectra of these total measurement points, a spectrum with an improved SN ratio (ratio of the noise magnitude to the spectrum magnitude) was obtained. In addition, by performing measurements while moving the stage, a Raman spectrum with little measurement point dependency was obtained. The temperature during the measurement was 25 degrees Celsius (25°C). The measurement was performed at a location away from the surface. The appearance of the obtained sintered body was gray.
[0010] For the silicon nitride sintered body according to the embodiment, two or more peaks are present at 780 cm -1 ~810cm -1 and 1340cm -1 ~1370cm -1 For example, the detection range is 780 cm. -1 ~810cm -1 At least one peak was detected in the range of 1340 cm -1 ~1370cm -1 One or more peaks are detected in the range of 780 cm -1 ~810cm -1 No peak was detected in the range of 1340 cm -1 ~1370cm -1 Two or more peaks may be detected in the range of 1340 cm or 1340 cm. -1 ~1370cm -1No peak was detected in the range of 780 cm -1 ~810cm -1 Two or more peaks may be detected in the range. Also, 170cm -1 ~190cm -1 , 607cm -1 ~627cm -1 , 720cm -1 ~740cm -1 , and 924 cm -1 ~944cm -1 In other words, the number of peaks detected in the range is more than 3 and does not exceed 6. The number of peaks is more preferably 4 or 5. For example, at 170 cm -1 ~190cm -1 Range: 607cm -1 ~627cm -1 Range: 720cm -1 ~740cm -1 range, and 924 cm -1 ~944cm -1 In each of the ranges, one or two peaks may be detected. In some of these ranges, no peaks may be detected, and in other ranges, two or more peaks may be detected. However, it is more preferable that one or two peaks are detected in each of the wave number ranges of the ranges. The number of peaks in the above range is too large, suggesting that there are a large amount of molecules with different bond strengths in the sintered body. In other words, the number of peaks is too large, suggesting, for example, that there may be a large amount of impurities, that there may be too many types of components added as auxiliary agents, or that there may be variation in the bond strength of the molecules present in the sintered body. If there are many types of components added as auxiliary agents, it may be difficult to control the amount added or the dispersibility of the auxiliary agent in the mixing process or subsequent processes. If there is unevenness in the bond strength between molecules, there may also be unevenness in the aggressiveness to the mating member. Therefore, 170 cm -1 ~190cm -1 , 607cm -1 ~627cm -1 , 720cm-1 ~740cm -1 , and 924 cm -1 ~944cm -1 It is preferable that 4 to 6 peaks are detected in the range. In this application, the expression "x to y" means "x or more and y or less," and "x" and "y" are included in the range. In the silicon nitride sintered body according to the embodiment, a peak may be detected in a range other than the above. The peak that can be observed in the range other than the above is not particularly limited, but may be, for example, 805 cm -1 ~815cm -1 , 715cm -1 ~725cm -1 , 270cm -1 ~280cm -1 , 410cm -1 ~420cm -1 There may be a peak in the range of 270 cm -1 ~280cm -1 The peak detected in the range of 410 cm is due to tungsten oxide. -1 ~420cm -1 The peaks detected in the range are due to iron oxide. In addition, 515cm -1 ~525cm -1 The peak intensity detected in the range of 400 cm -1 ~1200cm -1 It is preferable that the peak is not the strongest peak among the peaks detected between 400 cm and 400 cm. -1 ~1200cm -1 The intensity of at least one peak detected between 515 cm -1 ~525cm -1 The intensity of the peak detected in the range of 515 cm -1 ~525cm -1 The smaller the peak intensity in the range, the better. -1 ~525cm -1 It is more preferable that there is no peak in the range of 515 cm -1 ~525cm -1The peak in the range may be due to free Si. The presence of free Si may reduce the durability of the wear-resistant member made of the silicon nitride sintered body.
[0011] The type of chemical bond can be identified from the position of the peak detected by Raman spectroscopy. The full width at half maximum of the peak indicates the degree of crystallinity. Hereinafter, "full width at half maximum" will be simply referred to as "half width". The smaller the half width of the peak, the higher the crystallinity. The peak intensity is also affected by the orientation and concentration. The peak shift value is affected by the stress and amount of strain. Even for materials with the same composition, the number, intensity, and half width of the peaks will vary depending on the bonding state, crystallinity, orientation, amount of strain, etc. As described above, the detection position of the Raman spectroscopic peak varies depending on the bonding state, crystallinity, orientation, amount of strain, etc. The silicon nitride sintered body having the above-mentioned Raman spectroscopic peak can improve the wear resistance. In addition, when the silicon nitride sintered body is used as a wear-resistant member, the attacking property to the counter member can be suppressed.
[0012] 780cm -1 ~810cm -1 Peaks detected in the range of 1340 cm -1 ~1370cm -1 The peak detected in the range is due to carbon or carbide. In other words, it is preferable that the silicon nitride sintered body contains carbon or carbide. When carbon or carbide is mixed into the raw material of the silicon nitride sintered body, the peak detected in the range of 780 cm -1 ~810cm -1 or 1340cm -1 ~1370cm -1 A peak is detected in the range. 170cm -1 ~190cm -1 Peaks detected in the range of 607 cm -1 ~627cm -1 Peaks detected in the range of 720 cm -1 ~740cm -1 and peaks detected in the range of 924 cm -1 ~944cm -1The peaks detected in the range are due to silicon nitride crystal grains.
[0013] Also, 170cm -1 ~190cm -1 The peak intensity of the strongest peak detected in the range of 780 cm was defined as I1. -1 ~810cm -1 When the peak intensity of the strongest peak detected in this range is I2, the peak intensity ratio I1 / I2 is preferably within the range of 1.2 or more and 2.0 or less. 170cm -1 ~190cm -1 In the range of 170 cm, the largest peak due to silicon nitride crystal particles is detected. -1 ~190cm -1 In the range of 780 cm, the main peak of silicon nitride crystal grains is detected. -1 ~810cm -1 The strongest peaks detected in the range are due to carbon or carbides. The peak intensity ratio I1 / I2 being in the range of 1.2 or more and 2.0 or less indicates that a certain amount of peak intensity of carbon or carbide is present relative to the main peak of silicon nitride crystal grains. The peak intensity is mainly affected by the orientation and concentration. Carbon or carbide is a component that improves the strength of silicon nitride sintered bodies. Carbon or carbide also has an effect as a lubricant. When the peak intensity ratio I1 / I2 is in the range of 1.2 or more and 2.0 or less, aggressiveness to the mating member can be further suppressed.
[0014] Also, 607cm -1 ~627cm -1 The peak intensity of the strongest peak at 720 cm is defined as I3. -1 ~740cm -1 The peak intensity of the strongest peak at 924 cm is designated as I4. -1 ~944cm -1 The peak intensity of the strongest peak at 1340 cm was defined as I5. -1 ~1370cm -1The peak intensity of the strongest peak at 780 cm is defined as I6. In this case, the peak intensity ratio I1 / I3 is preferably 2 or more and 20 or less. The peak intensity ratio I1 / I4 is preferably 2 or more and 20 or less. The peak intensity ratio I1 / I5 is preferably 2 or more and 20 or less. The peak intensity ratio I1 / I6 is preferably 2 or more and 20 or less. This is because -1 ~810cm -1 This shows that, apart from the strongest peak detected in the range, there are relatively small peaks. This allows the effect of carbon or carbides to be obtained.
[0015] Also, 170cm -1 ~190cm -1 , 607cm -1 ~627cm -1 , 720cm -1 ~740cm -1 , and 1340 cm -1 ~1370cm -1 At least one peak is detected in at least one of the four ranges, and the half-width of the detected peak is 70 cm -1 It is preferable that the distance does not exceed 45 cm. -1 More preferably, the half width of the peak is not more than 3 cm. -1 More than 40cm -1 The following is true: It is more preferable that the half-width of the peak in each peak range is as described below. -1 ~810cm -1 The half-width of the peak at -1 ~25cm -1 It is within the range of 607cm. -1 ~627cm -1 The half-width of the peak at -1 ~25cm -1 It is within the range of 720cm. -1 ~740cm -1 The half-width of the peak at -1 ~25cm -1 It is within the range of 924cm. -1 ~944cm -1The half-width of the peak at is 10 cm -1 ~40cm -1 is within the range.
[0016] FIG. 2 is a diagram illustrating a schematic example of an analysis result by Raman spectroscopy of the silicon nitride sintered body according to the embodiment. In the Raman spectrum RS shown in Figure 2, the horizontal axis is the Raman shift (cm -1 ), and the vertical axis represents the scattering intensity. When the silicon nitride sintered body according to the embodiment is analyzed by Raman spectroscopy, a plurality of peaks including peaks P1 to P6 are detected, as shown in FIG. 2. Peak P1 is at 170 cm -1 ~190cm -1 The peak P2 is in the range of 607 cm -1 ~627cm -1 The peak P3 is in the range of 720 cm -1 ~740cm -1 Peak P4 is in the range of 780 cm -1 ~810cm -1 Peak P5 is in the range of 924 cm -1 ~944cm -1 Peak P6 is in the range of 1340 cm -1 ~1370cm -1 It exists in the range of 515cm. -1 ~525cm -1 There is no peak in the range. Also, 170cm -1 ~190cm -1 The peak intensity of the peak P1 is I1, and the peak intensity of the peak P2 is I2 at 780 cm -1 ~810cm -1 When the peak intensity of the peak P4 is I2, the peak intensity ratio I1 / I2 is 1.2 or more and 2.0 or less. -1 ~190cm -1 Peak P1, 607cm -1 ~627cm -1 Peak P2, 720cm -1 ~740cm -1 Peaks P3 and 1340 cm -1 ~1370cm -1 The half-width of each of the peaks P4 is 45 cm-1 The following is true: 170cm -1 ~190cm -1 , 607cm -1 ~627cm -1 , 720cm -1 ~740cm -1 , and 1340 cm -1 ~1370cm -1 In the range, the half-width is 45 cm -1 No peaks above this level are detected.
[0017] The silicon nitride sintered body preferably contains 80% by mass or more of silicon nitride, 2% by mass or more and 4% by mass or less of rare earth elements calculated as oxides, and 2% by mass or more and 6% by mass or less of Al components calculated as oxides. The silicon nitride sintered body preferably contains 1% by mass or more and 7% by mass or less of a carbide compound. The carbide compound includes, for example, silicon carbide. More preferably, the silicon nitride sintered body contains 2% by mass or more and 7% by mass or less of silicon carbide. The silicon nitride sintered body preferably contains at least one selected from the group consisting of Ti, Zr, Hf, W, Mo, Ta, Nb and Cr in an amount of 3 mass% or less calculated as an oxide. When one or more components selected from the group consisting of Ti, Zr, Hf, W, Mo, Ta, Nb and Cr are contained, the total amount is more preferably 0.5 mass% or more and 3 mass% or less calculated as an oxide. Even more preferably, the total amount is 0.8 mass% or more and 2.5 mass% or less. The rare earth element has an effect of improving sinterability. The rare earth element is preferably yttrium (Y) or a lanthanoid element. When a rare earth element is added as a sintering aid, it is preferable to add a rare earth oxide. Even when two or more rare earth oxides are added, the total content of the rare earth elements is preferably within a range of 2% by mass to 4% by mass in terms of rare earth oxide. When an Al (aluminum) component is added as a sintering aid, the Al component may be one or two selected from aluminum oxide and aluminum nitride. Aluminum oxide (Al2O3) or aluminum nitride (AlN) has the effect of promoting the sintering of rare earth oxides. Aluminum nitride (AlN) has the effect of preventing silicon nitride crystal particles from decomposing. Even when both aluminum oxide and aluminum nitride are used as the Al component, the total content of the Al components is preferably within the range of 2 mass% to 10 mass% in terms of oxide. The rare earth oxide and the Al component react with each other to form a grain boundary phase. Silicon carbide (SiC) can be made to exist as particles in the grain boundary phase, which strengthens the grain boundary phase. Silicon carbide also has lubricity, and therefore has the effect of improving wear resistance. Silicon carbide can also be made to exist in the silicon nitride sintered body by mixing silicon carbide with the raw material of the silicon nitride sintered body.
[0018] The component selected from the group consisting of Ti, Zr, Hf, W, Mo, Ta, Nb, and Cr is present in the silicon nitride sintered body as one or more selected from oxides, nitrides, and carbides. These components have the effect of promoting sintering and strengthening the grain boundary phase. If the content of these components exceeds 3 mass%, the effect of silicon carbide may be reduced. The lower limit of the content of the component selected from the group consisting of Ti, Zr, Hf, W, Mo, Ta, Nb, and Cr is not particularly limited, but the total value is preferably 0.5 mass% or more.
[0019] In the silicon nitride sintered body, the area ratio of silicon nitride crystal grains with a major axis of 2 μm or more is preferably 40% or more. The area ratio of silicon nitride crystal grains with an aspect ratio of 1.5 or less is preferably 50% or more. In other words, it is preferable that there are many silicon nitride crystal grains with a major axis of 2 μm or more and an aspect ratio of 1.5 or less. By controlling the size of the silicon nitride crystal grains, the orientation, amount of distortion, etc. can be homogenized. To measure the long axis and aspect ratio of silicon nitride crystal particles, a scanning electron microscope (SEM) photograph of any cross section is used. The long axis is the maximum diameter of each silicon nitride crystal particle seen in a unit area of 20 μm x 20 μm on the SEM photograph. The short axis is the length of a line segment extended vertically from the center of the long axis. The aspect ratio = long axis / short axis. The area ratio of silicon nitride crystal particles with a long axis of 2 μm or more seen in a 20 μm x 20 μm area is calculated. Similarly, the area ratio of silicon nitride crystal particles with an aspect ratio of 1.5 or less seen in a 20 μm x 20 μm area is calculated. The major axis and aspect ratio are measured using the portion of the SEM photograph in which the silicon nitride crystal grains are visible. When the silicon nitride crystal grains overlap, only the portion visible in the SEM photograph is used for measurement. When the individual silicon nitride crystal grains cannot be distinguished, the grain boundary phase may be removed by etching.
[0020] The silicon nitride sintered body described above has a porosity of 1% or less, a three-point bending strength of 800 MPa or more, and a fracture toughness of 5.7 MPa m 1 / 2 It can do more than that. Porosity can be measured by the Archimedes method. By keeping the porosity at 1% or less, it is possible to prevent pores from becoming the starting point of fracture. Three-point bending strength can be measured in accordance with JIS-R-1601 (2008). Fracture toughness can be measured using the Niihara formula based on the IF method of JIS-R-1607 (2015). Bearing balls made of sintered silicon nitride are graded in JIS-R-1669 (2014). Three-point bending strength of 800 MPa or more and fracture toughness of 5.7 MPa m 1 / 2 The above silicon nitride sintered bodies correspond to grade 1 or grade 2. JIS-R-1601(2008) corresponds to ISO 14704:2000(MOD). JIS-R-1607(2015) corresponds to ISO 15732:2003(MOD). JIS-R-1669(2014) corresponds to ISO 26602:2009(MOD).
[0021] The silicon nitride sintered body having the above-mentioned Raman spectroscopic peak can improve the wear resistance. Therefore, the durability of the wear-resistant member using the silicon nitride sintered body according to the embodiment can be improved. In particular, the aggressiveness to the counter member can be suppressed, so that the durability of the counter member can also be improved. Examples of such wear-resistant members include bearing members, roll members, compressor members, pump members, engine members, and friction stir welding device members. A bearing is a combination of bearing components consisting of rolling elements and raceways. The rolling elements are spherical or roller-shaped components. The rolling elements are called bearing balls. The spherical shape is a ball, and the roller shape is a cylinder. Components that use spherical rolling elements are called ball bearings. Components that use roller-shaped rolling elements are called roller bearings. Roller bearings also include needle bearings, tapered roller bearings, and spherical roller bearings. The raceways include outer and inner rings. Examples of roll members include rolling rollers and rollers for feeding parts of electronic devices. Examples of compressor or pump members include vanes. Here, compressors are devices that increase pressure, and pumps are devices that decrease pressure, so they are distinguished from each other. Examples of engine members include cam rollers, cylinders, pistons, check balls, etc. Examples of friction stir welding device members include tool members for friction stir welding devices.
[0022] Fig. 3 is a diagram showing an example (bearing ball) of the wear resistant member according to the embodiment, and Fig. 4 is a diagram showing another example (bearing) of the wear resistant member according to the embodiment. 3 and 4, 1 is a bearing ball, 2 is a bearing, 3 is an inner ring, and 4 is an outer ring. The bearing 2 has a structure in which a bearing ball 1 is arranged between the inner ring 3 and the outer ring 4. Four or more bearing balls 1 are arranged in the bearing 2. The inner ring 3 and the outer ring 4 are mating members of the bearing ball 1. The bearing ball 1 is made of the silicon nitride sintered body according to the embodiment. If necessary, polishing may be performed so that the surface roughness Ra is 0.1 μm or less. For bearing balls, the surface roughness Ra according to the grade is specified in ASTM F2094 by the American Society for Testing and Materials. Therefore, polishing may be performed to the surface roughness according to the grade. Note that ASTM is a standard issued by ASTM International. The former name of ASTM International is American Society for Testing and Materials (ASTM). Even when applied to wear-resistant members other than bearing balls, surface polishing may be performed if necessary. In other words, the wear-resistant member according to the embodiment preferably has a polished surface with a surface roughness Ra of 0.1 μm or less, and further preferably Ra of 0.02 μm or less. When the silicon nitride sintered body according to the embodiment is applied to a bearing ball 1, aggressiveness towards the outer ring 4 and the inner ring 3 is reduced, and therefore the durability of the bearing 2 can be improved. A plurality of bearing balls 1 are used in the bearing 2. By reducing the aggressiveness of each bearing ball 1 towards the outer ring 4 and the inner ring 3, the durability of the bearing 2 can be improved. In the case of the bearing ball using the silicon nitride sintered body according to the embodiment, the crushing load can be set to 150 MPa or more and 200 MPa or less. The crushing load was measured by placing two bearing balls one on top of the other in the height direction and applying a load from above. The load at which one of the bearing balls breaks was taken as the crushing load. In addition, the bearing ball using the silicon nitride sintered body according to the embodiment can achieve a rolling fatigue life of 400 hours or more. The rolling fatigue life is defined as the time until the surface of a bearing ball peels off when a load is applied to three bearing balls arranged on a raceway and the bearing balls are rotated while the bearing balls have a diameter of 9.525 mm (3 / 8 inch). The raceway is set on the upper surface of a bearing steel SUJ2 plate and has a diameter of 40 mm. A load is applied to the three bearing balls so that a maximum contact stress of 5.9 GPa acts on them. The rotation speed is set to 1200 rpm. If the diameter of the bearing ball is not 9.525 mm, the diameter of the bearing steel is adjusted to match the diameter of the ball. That is, the diameter of the bearing steel is adjusted so that the ratio of the diameter of the bearing ball to the diameter of the bearing steel is 9.525:40. The above-mentioned bearing ball can suppress the aggressiveness to the mating member while maintaining durability. Therefore, the bearing 2 also has the effect of suppressing the temperature rise during rotation and suppressing the increase of sliding noise. In recent years, inverter-driven motors have become popular. Inverter drive is a method in which the rotation speed of the motor is variable. Generally, the rotation speed of the motor is within the range of 0 to 15,000 rpm. 0 rpm is a state in which the motor is stopped. The bearing rotates according to the rotation speed of the motor. By reducing the aggressiveness, durability is good even when the rotation speed changes. Thus, the silicon nitride sintered body according to the embodiment is suitable for a wear-resistant member using a mating member.
[0023] When the silicon nitride sintered body according to the embodiment is used in a flat wear-resistant member, the rolling life is 1×10 7 The rolling life was measured by placing three SUJ2 rolling steel balls on a raceway set on the upper surface of the wear-resistant member and rotating the rolling steel balls while applying a load. Kei It is defined as the number of revolutions of the wear-resistant member until the surface of the bare wear-resistant member peels off. The diameter of the raceway is set to 40 mm. The diameter of each rolling steel ball is 9.525 mm. The load applied to the rolling steel ball is 39.2 MPa. The rotation speed is set to 1200 rpm. The shape of the wear-resistant member according to the embodiment is not limited to a sphere, and various shapes can be applied. Examples of shapes of the wear-resistant member other than a sphere include a cylindrical shape. Furthermore, the bearing ball 1 according to the embodiment can reduce aggressiveness towards the mating member, thereby suppressing the occurrence of electrolytic corrosion. Electrolytic corrosion is a phenomenon in which a partial discharge occurs between the bearing ball and the inner ring and between the bearing ball and the outer ring, causing the surfaces of the inner ring and the outer ring to be eroded. In bearings, sintered silicon nitride is used for the bearing balls, and metals such as bearing steel SUJ2 are used for the inner ring and the outer ring. When electrolytic corrosion occurs, the inner ring and the outer ring, which are metals, are eroded. As the erosion progresses, the function of the bearing deteriorates. When the function deteriorates, an increase in sliding noise occurs, for example. In general, bearings are filled with grease between the bearing balls and the inner ring and between the bearing balls and the outer ring. The grease has lubricity and insulation properties. There are various types of grease, such as lithium soap grease. When a partial discharge phenomenon occurs between the bearing balls and the inner ring and between the bearing balls and the outer ring, the grease deteriorates. When the grease deteriorates, the lubricity and insulation properties decrease. This makes it easier for electrolytic corrosion to occur. When the grease deteriorates, the grease discolors. For example, in the case of lithium soap grease, the color changes from transparent to black. In the bearing ball according to the embodiment, the aggressiveness to the mating member is reduced, so that the deterioration of the grease can be suppressed. From this point of view, the bearing can have a long life. Grease deterioration can be caused by physical factors, chemical factors, or the intrusion of foreign matter. The main physical factor is change over time. This is deterioration that occurs as a result of continued use. Other physical factors include mechanical shear and centrifugal force. The main chemical factor is electrical corrosion. Other chemical factors include oxidation due to heat. The main cause of foreign matter intrusion is contact between the bearing balls and the inner or outer ring. When the bearing balls come into contact with the inner or outer ring, wear powder is generated. These effects cause the grease to harden, resulting in poor lubrication and reduced insulation properties. The bearing ball according to the embodiment can suppress aggressiveness to the mating member, and therefore can suppress the generation of electrolytic corrosion or wear powder, which in turn can suppress the deterioration of the grease and extend the life of the bearing.
[0024] Next, a method for producing the silicon nitride sintered body according to the embodiment will be described. As long as the silicon nitride sintered body according to the embodiment has the above-mentioned configuration, the method for producing the silicon nitride sintered body is not particularly limited. The following examples are given as methods for obtaining the silicon nitride sintered body with a high yield. First, silicon nitride powder and sintering aid powder are prepared. The silicon nitride powder preferably has an alpha content of 80 mass% or more, an oxygen content of 1.5 mass% or less, and an average particle size of 1.2 μm or less. The silicon nitride powder may also have an impurity Fe content of 5 wtppm or more and 3500 wtppm or less, an impurity Ca content of 5 wtppm or more and 3000 wtppm or less, and an impurity Mg content of 1 wtppm or more and 1000 wtppm or less. Such silicon nitride powder may be powder synthesized by a direct nitriding method. The average particle size of the sintering aid powder is preferably 2 μm or less. The amount of the rare earth oxide powder is set within a range of 2 mass% to 4 mass% in terms of oxide. The amount of the Al component powder is set within a range of 2 mass% to 10 mass% in terms of mass. The amount of silicon carbide is set within a range of 2 mass% to 7 mass% in terms of mass. It is preferable to use silicon carbide powder. In addition, when at least one selected from the group consisting of Ti, Zr, Hf, W, Mo, Ta, Nb, and Cr is added as the sintering aid powder, the amount is set within a range of 0.5 mass% to 3 mass% in terms of oxide. The amount of each component of the sintering aid added is a value when the total of the silicon nitride powder and the sintering aid powder is 100 mass%.
[0025] Next, a raw material powder mixing step is performed in which silicon nitride powder and sintering aid powder are mixed. In the raw material powder mixing step, a bead mill or a ball mill is used. Also, the mixing step is performed using raw material powder slurry mixed with a binder and a solvent. Next, a molding process is performed to create a molded body using the raw material powder (including the raw material powder slurry). The molding method can be a die pressing method, a cold isostatic pressing (CIP) method, a sheet molding method, or the like. The sheet molding method can be a doctor blade method, a roll molding method, or the like. These molding methods can also be combined. If necessary, the raw material powder (including the raw material powder slurry) can be mixed with a solvent such as toluene, ethanol, or butanol. If necessary, the raw material powder (including the raw material powder slurry) is mixed with an organic binder. Examples of the organic binder include butyl methacrylate, polyvinyl butyral, and polymethyl methacrylate. When the raw material mixture (the total amount of the silicon nitride powder and the sintering aid powder) is 100 parts by mass, the amount of the organic binder added is preferably 3 parts by mass or more and 17 parts by mass or less. If the amount of the organic binder added is less than 3 parts by mass, the amount of the binder is too small and it is difficult to maintain the shape of the molded body. Furthermore, if the amount exceeds 17 parts by mass, the pores in the green body after the degreasing step (green body after the degreasing treatment) will become large, making it impossible to obtain a dense sintered body.
[0026] Next, the green body is subjected to a degreasing process. In the degreasing process, the green body is heated in a non-oxidizing atmosphere at a temperature of 500°C to 800°C for 1 hour to 4 hours, thereby degreasing most of the organic binder that was added beforehand. Examples of non-oxidizing atmospheres include a nitrogen gas atmosphere and an argon gas atmosphere. If necessary, the green body is treated in an oxidizing atmosphere such as air to control the amount of organic matter remaining in the degreased body. Next, the degreased body (the degreased molded body) is placed in a sintering container and sintered in a non-oxidizing atmosphere in a sintering furnace. In the sintering process, the heating rate in the temperature range of 1400°C to 1480°C in the non-oxidizing atmosphere is set to 100°C / hour or more, and the maximum sintering temperature is maintained at 1700°C to 1800°C for 5 hours or more. Examples of the non-oxidizing atmosphere in the sintering process include a nitrogen gas atmosphere and an argon gas atmosphere.
[0027] It is effective to increase the heating rate to 100°C / hour or more in the temperature range of 1400°C to 1480°C. This temperature range is the temperature at which the sintering aid starts to melt and the liquid phase starts to form. It is also the temperature at which the silicon nitride starts to shrink due to the formation of the liquid phase. By increasing the heating rate in this temperature range, it is possible to suppress the volatilization and decomposition of the liquid phase and to construct silicon nitride crystal particles with optimal crystal bonding state and crystal orientation. As a result, it is possible to obtain a silicon nitride sintered body having the desired Raman spectroscopy peak. There is no particular limit to the upper limit of the heating rate, but it is preferably 500°C / hour or less. If the heating rate is too fast, the burden on the furnace may be large.
[0028] Moreover, the rate of temperature rise from 1480°C to the maximum sintering temperature is preferably set to less than 100°C / hour. The temperature range from 1480°C to the maximum sintering temperature is the region where the sintered body begins to densify. By slowing down the rate of temperature rise in this temperature range, the degree of grain growth of silicon nitride crystal grains can be made uniform. Grain growth affects the bonding state and orientation of the crystals. The rate of temperature rise from room temperature to 1400°C is arbitrary.
[0029] In addition, the temperature of the sintering process is preferably in the range of 1700°C to 1800°C. The maximum sintering temperature is set in the range of 1700°C to 1800°C. If the degreased body is sintered at a low temperature of less than 1700°C, the grain growth of silicon nitride crystal particles is insufficient, making it difficult to obtain a dense sintered body. On the other hand, if the degreased body is sintered at a sintering temperature higher than 1800°C, silicon nitride may decompose into Si and N2 if the atmospheric pressure in the furnace is low. For this reason, it is preferable to control the sintering temperature within the above range. In addition, the sintering time is preferably in the range of 3 hours to 12 hours. After the sintering step, it is preferable to carry out a hot isostatic pressing (HIP) process. In the HIP process, the sintered body is subjected to the HIP process. The process of sintering the degreased body is called the first sintering process, and the process of HIPing the sintered body is called the second sintering process. In the HIP treatment, the temperature is preferably in the range of 1600°C to 1800°C, and the pressure is preferably in the range of 80MPa to 200MPa. The HIP treatment can reduce the number of pores in the sintered body, which allows a dense sintered body to be obtained. If the pressure is less than 80MPa, the effect of applying pressure is insufficient. Also, if the pressure is higher than 200MPa, the load on the manufacturing equipment may be increased. The silicon nitride sintered body thus obtained may be polished as required. When multiple pieces are to be obtained, the silicon nitride sintered body may be cut.
[0030] (Example) (Examples 1 to 3, Comparative Examples 1 to 2) The combinations shown in Table 1 were prepared as raw material powders. The silicon nitride powders used in the examples and comparative examples had an alpha conversion rate of 80 mass% or more, an average particle size of 1.2 μm or less, and an impurity oxygen content of 2 mass% or less. In addition, silicon nitride powders synthesized by a direct nitriding method were used. Therefore, the impurity Fe content in the silicon nitride powder was 100 wtppm to 2500 wtppm, the impurity Ca content was 10 wtppm to 1500 wtppm, and the impurity Mg content was 3 wtppm to 1000 wtppm. In addition, sintering aid powders with an average particle size of 2 μm or less were used.
[0031] [Table 1]
[0032] Silicon nitride powder and sintering aid powder were mixed in a ball mill to prepare raw material powder. A binder and a solvent were added to the raw material powder to prepare raw material powder slurry. A molded body was produced using the raw material powder slurry. In the molding process, molding was performed using a die. Two types of molded bodies were produced, including a molded body for obtaining a bearing ball with a size of 3 / 8 inch (diameter 9.525 mm) and a molded body for measuring bending strength. Next, the molded body was subjected to a degreasing process at 500 to 800°C for 1 to 4 hours. Next, a sintering process was carried out in a non-oxidizing atmosphere at a pressure of 0.7 MPa. The temperature profile of the sintering process was set as shown in Table 2.
[0033] [Table 2]
[0034] The obtained sintered body was subjected to HIP treatment at 1600-1700°C for 3-5 hours under a pressure of 100-200 MPa. The sintered body after HIP treatment was polished so that the surface roughness Ra was 0.02 μm or less. By such a process, the silicon nitride sintered body according to the examples and comparative examples was produced. The silicon nitride sintered bodies according to the examples and comparative examples were analyzed by Raman spectroscopy. The central cross section of the silicon nitride sintered body was used for the Raman spectroscopy. The Raman spectroscopy was performed using a Renishaw inVia Reflex laser microscope (resolution: 0.3 cm). -1 ) was used. An LD-pumped green laser (wavelength 532 nm, output 100 mW) was used as the excitation laser, and the irradiation laser beam diameter was set to 0.7 μm, the exposure time to 1 second per measurement point, and the stage movement step to 0.4 μm. Multivariate curve resolution (MCR) using the image analysis software WiRe4Empty Modelling was used for data analysis. The results are shown in Table 3. In Table 3, a result marked "Yes" indicates that one peak was detected in that range.
[0035] [Table 3]
[0036] As can be seen from Table 3, the silicon nitride sintered body according to the embodiment has a thickness of 170 cm -1 ~190cm -1 , 607cm -1 ~627cm -1 , 720cm -1 ~740cm -1 , 780cm -1~810cm -1 , 924cm -1 ~944cm -1 , and 1340 cm -1 ~1370cm -1 In contrast, in Comparative Example 1, peaks were detected in the range of 1340 cm -1 ~1370cm -1 Peaks are detected within the range figure In the other ranges, one peak each was observed. From this point, it can be seen that even if the sintering aid is similar, the Raman spectroscopic peaks obtained differ depending on the manufacturing method. -1 ~627cm -1 , 780cm -1 ~810cm -1 , and 1340 cm -1 ~1370cm -1 No peaks were detected in the three ranges. In the silicon nitride sintered body according to the embodiment, the -1 ~525cm -1 No peak was detected in the range. Next, the half-width and peak intensity of the Raman spectroscopy peak were determined, and the results are shown in Tables 4 and 5. 170cm -1 ~190cm -1 The peak intensity of the strongest peak detected in the range of 780 cm was designated as I1. -1 ~810cm -1 The peak intensity of the strongest peak detected in the range of 607 cm was taken as I2. -1 ~627cm -1 The peak intensity of the strongest peak at 720 cm was designated as I3. -1 ~740cm -1 The peak intensity of the strongest peak at 924 cm was designated as I4. -1 ~944cm -1 The peak intensity of the strongest peak at 1340 cm was designated as I5. -1 ~1370cm -1 The peak intensity of the strongest peak was designated as I6.
[0037] [Table 4]
[0038] [Table 5]
[0039] As can be seen from Tables 4 and 5, the half-width and peak intensity ratio were within the preferred ranges in the Examples, whereas the half-width or peak intensity ratio was outside the range in the Comparative Examples. Next, the porosity, three-point bending strength, and fracture toughness of the silicon nitride sintered body were measured. The porosity was measured by the Archimedes method. The three-point bending strength was measured according to JIS-R-1601 (2008). The fracture toughness was measured by the Niihara formula based on the IF method of JIS-R-1607 (2015). The structure of the silicon nitride sintered body was also examined. An arbitrary cross section of the silicon nitride sintered body was observed using a SEM. The area ratio (%) of silicon nitride crystal grains with a major axis of 2 μm or more in an area of 20 μm x 20 μm was calculated. Similarly, the area ratio (%) of silicon nitride crystal grains with an aspect ratio of 1.5 or less in an area of 20 μm x 20 μm was calculated. The results are shown in Table 6. In Table 6, the area ratio of silicon nitride crystal grains with a major axis of 2 μm or more is shown as "area ratio A (%)." The area ratio of silicon nitride crystal grains with an aspect ratio of 1.5 or less is shown as "area ratio B (%)."
[0040] [Table 6]
[0041] Next, a durability test was conducted using the bearing balls according to the examples and comparative examples. In the durability test, a thrust type rolling fatigue tester was used to measure the rolling life under conditions of a maximum contact pressure of 5.9 MPa and a rotation speed of 1200 rpm. A plate material made of bearing steel SUJ2 was used as the mating member. The time until the surface of the bearing ball peeled off was measured. The measurement time was set to an upper limit of 400 hours. Bearing balls for which no surface peeling was confirmed even after 400 hours were indicated as "400 hours or more." The crushing load of the bearing balls according to the embodiment and the comparative example was also measured. The crushing load was measured by placing two bearing balls one on top of the other in the height direction and applying a load from above. The load at which one of the bearing balls broke was taken as the crushing load. The results are shown in Table 7.
[0042] [Table 7]
[0043] As can be seen from Table 7, the wear resistance as a bearing ball was equivalent between the examples and the comparative examples. Next, bearings were made using the bearing balls according to the embodiment and the comparative example. The inner and outer rings were made of bearing steel SUJ2. The bearings were assembled using 16 bearing balls. Transparent lithium soap grease was used as the grease. The rate of change in the sliding sound of the bearings and the presence or absence of discoloration of the grease were measured. A rotating shaft was attached to the bearing and rotated at 1200 rpm. To calculate the rate of change in the sliding sound, the sliding sound after 10 continuous hours and after 300 continuous hours were measured. The rate of change in the sliding sound from 10 continuous hours to 250 continuous hours in Comparative Example 1 was set to 1. The change in the sliding sound of each bearing was compared with this rate of change. If the change in the sliding sound is small, the rate of change will be a value smaller than 1. In addition, to check for discoloration of the grease, the bearings were dismantled after 300 hours and the color (brightness) of the grease was examined. The results are shown in Table 8.
[0044] [Table 8] In Table 8, a value of 9 or more but less than 9.5 is defined as "light gray." A value of less than 9 and greater than 4 is defined as "dark gray." A value of less than 4 is defined as "black." The Munsell color system was used as the standard for these values of lightness. The Munsell color system corresponds to JIS Z8721 (1993). The more the grease deteriorates, the smaller the value becomes.
[0045] As can be seen from Table 8, in the embodiment, the rate of change in sliding sound and discoloration of the grease were improved. In the bearing according to the embodiment, the color of the grease was light gray. The grease, which was initially transparent, became colored, which is due to physical factors. In the comparative example, the coloring of the grease was further advanced compared to the embodiment. Although no significant difference was confirmed in the thrust test, differences were confirmed in the above tests regarding the change in sliding sound and the color of the grease. This is because the contact variation between the bearing ball and the mating member was reduced, and the aggressiveness of the bearing ball to the mating member was reduced.
[0046] Although some embodiments of the present invention have been illustrated above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, modifications, etc. can be made without departing from the gist of the invention. Modifications of these embodiments are included in the scope and gist of the invention, and are included in the scope of the invention and its equivalents described in the claims. In addition, the above-mentioned embodiments can be implemented in combination with each other. [Explanation of symbols]
[0047] 1...Bearing ball 2. Bearing 3. Inner circle 4…Outer ring 10...Silicon nitride sintered body 11...Silicon nitride crystal grains 12...Grain boundary RS…Raman spectrum P1~P6…Peak
Claims
1. A silicon nitride sintered body having silicon nitride crystal grains and a grain boundary phase, When a 20 μm × 20 μm region in the central cross section of the silicon nitride sintered body is subjected to Raman spectroscopy, two or more peaks are detected at 780 cm -1 ~810cm -1 and 1340 cm -1 ~1370cm -1 , and four to six peaks are detected in the range of 170 cm -1 ~190cm -1 , 607 cm -1 ~627cm -1 , 720cm -1 ~740cm -1 , and 924 cm -1 ~944cm -1 A silicon nitride sintered body, characterized in that the concentration of the sintered silicon nitride is detected in the range of
2. 2. The silicon nitride sintered body according to claim 1, characterized in that it contains 1 mass % or more of a carbide compound.
3. 170cm -1 ~190cm -1 The peak intensity of the strongest peak in the range of I 1 And 780 cm -1 ~810cm -1 The peak intensity of the strongest peak in the range of I 2 When Peak intensity ratio I 1 / I 2 3. The silicon nitride sintered body according to claim 1, wherein the ratio of the surface area of the silicon nitride to the surface area of the silicon nitride is 1.2 or more and 2.0 or less.
4. 170cm -1 ~190cm -1 , 607 cm -1 ~627cm -1 , 720cm -1 ~740cm -1 , and 1340 cm -1 ~1370cm -1 In the range, the full width at half maximum is 70 cm -1 4. The silicon nitride sintered body according to claim 1, wherein no peak exceeding the value is detected.
5. 5. The silicon nitride sintered body according to claim 2, wherein the carbide compound contained in the silicon nitride sintered body includes silicon carbide.
6. The silicon nitride sintered body is 80% by mass or more of silicon nitride; A rare earth element in an oxide equivalent amount of 2% by mass or more and 4% by mass or less; An Al component of 2 mass% or more and 10 mass% or less in terms of oxide; 2% by mass or more and 7% by mass or less of silicon carbide; 6. The silicon nitride sintered body according to claim 1, further comprising:
7. The silicon nitride sintered body according to any one of claims 1 to 6, characterized in that the silicon nitride sintered body contains at least one selected from the group consisting of Ti, Zr, Hf, W, Mo, Ta, Nb, and Cr in an amount of 3 mass% or less, calculated as an oxide.
8. The porosity is 1% or less, It has a three-point bending strength of 800 MPa or more, 5.7MPa·m 1/2 8. The silicon nitride sintered body according to claim 1, which has a fracture toughness value of at least 100%.
9. 9. A wear-resistant member comprising the silicon nitride sintered body according to claim 1.
10. 10. The wear-resistant member according to claim 9, wherein the wear-resistant member is a bearing ball.
11. 11. The wear-resistant member according to claim 10, wherein the crushing load of the bearing ball is 150 MPa or more and 200 MPa or less.
12. 12. The wear-resistant member according to claim 10, wherein, when the bearing balls have a diameter of 9.525 mm (3 / 8 inch), a raceway of 40 mm diameter is set on the upper surface of a bearing steel SUJ2 plate, three bearing balls are arranged on the raceway, and the three bearing balls are rotated at a rotational speed of 1200 rpm under a load applied thereto so that a maximum contact stress of 5.9 GPa acts on the three bearing balls, the rolling fatigue life defined as the time until the surface of any of the three bearing balls peels off is 400 hours or more.
13. A method for producing a silicon nitride sintered body according to any one of claims 1 to 8, comprising the steps of: A method for producing a silicon nitride sintered body, comprising a sintering step carried out in a non-oxidizing atmosphere, in which the heating rate in the temperature range of 1400°C or higher and 1480°C or lower is set to 100°C / hour or more, and a maximum sintering temperature of 1700°C or higher and 1800°C or lower is maintained for 5 hours or more.
14. 14. The method for producing a silicon nitride sintered body according to claim 13, wherein in the sintering step, the rate of temperature rise from 1480° C. to the maximum sintering temperature is set to less than 100° C. / hour.
15. 15. The method for producing a silicon nitride sintered body according to claim 13, further comprising the step of subjecting the sintered body obtained by said sintering step to a hot isostatic press treatment.
Citation Information
Patent Citations
JP1975002155A
Rolling bearing
JP2003065337A
Nitrided silicon sintered body and abrasion resistant member using the same
JP2017075073A
Silicon nitride-based sintered object and cutting tool
WO2014104112A1
Sintered body, board, circuit board, and method for manufacturing sintered body
WO2018194052A1