Substrate liquid processing method and recording medium

A substrate liquid processing method using a pretreatment liquid with a reducing agent and pH adjuster addresses the challenge of filling recesses with plating metal, achieving seamless and complete deposition by controlling the electroless plating process to prevent seed layer corrosion and voids.

JP7581498B2Active Publication Date: 2024-11-12TOKYO ELECTRON LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023517431
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-04-26
Filing Date
2022-04-13
Publication Date
2024-11-12
Estimated Expiration
2042-04-13

AI Technical Summary

Technical Problem

The challenge of properly filling minute recesses in substrates with plating metal using electroless plating methods, particularly due to issues with voids or seams formation and seed layer corrosion, is exacerbated by the need for thinner seed layers in finer wiring.

Method used

A substrate liquid processing method involving the application of a pretreatment liquid containing a reducing agent, pH adjuster, and additives to modify the seed layer, followed by electroless plating solution, to control the deposition of plating metal in a bottom-up manner, minimizing seed layer corrosion and ensuring complete filling of recesses.

Benefits of technology

The method effectively embeds plating metal into recesses without voids or seams, while preventing seed layer thinning, by promoting controlled electroless plating reactions and ensuring uniform deposition.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581498000001
    Figure 0007581498000001
  • Figure 0007581498000002
    Figure 0007581498000002
  • Figure 0007581498000003
    Figure 0007581498000003
Patent Text Reader

Abstract

This substrate liquid processing method includes: a step for preparing a substrate which has a concave portion and in which a seed layer is formed on the surface of the concave portion; a step for bringing a first pretreatment liquid into contact with the seed layer, the first pretreatment liquid containing a reducing agent, a pH adjuster, and an additive for promoting or suppressing an electroless plating reaction; and a step for supplying a first electroless plating liquid to the concave portion and precipitating a plating metal in the concave portion, after bringing the first pretreatment liquid into contact with the seed layer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a substrate liquid processing method and a recording medium. [Background technology]

[0002] Electroless plating technology is sometimes used to form fine wiring on semiconductor substrates (wafers).

[0003] For example, in the wiring formation method disclosed in Patent Document 1, a connection hole is formed in an insulating film, a diffusion prevention layer is deposited on the inner surface of the connection hole, a Cu seed layer is deposited on the diffusion prevention layer, and a Cu plating layer is embedded in the connection hole by electroless plating. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2001-102448 A Summary of the Invention

[0005] As wiring becomes increasingly finer, it is becoming more difficult to properly fill minute recesses (such as vias and trenches) in a substrate with plating metal.

[0006] In order to prevent the occurrence of voids and seams in the plating metal filling the recesses of the substrate, it is effective to gradually deposit the plating metal from the bottom of the recesses, but it is not easy to control the deposition of the plating metal in the fine recesses in such a bottom-up manner.

[0007] In addition, when a plating metal is deposited on a seed layer, the seed layer needs to be thinned as the wiring becomes finer. As the seed layer becomes thinner, the corrosion of the seed layer by the electroless plating solution tends to have a large effect on the electroless plating process. In particular, immediately after the start of the electroless plating process, while no or almost no plating metal is deposited, the corrosion of the seed layer by the electroless plating solution progresses, and the seed layer may unintentionally become thinner.

[0008] The present disclosure provides an advantageous technique for properly filling recesses in a substrate with plating metal by electroless plating.

[0009] One aspect of the present disclosure relates to a substrate liquid processing method including the steps of: preparing a substrate having a recess, the substrate having a seed layer formed on a surface of the recess; contacting the seed layer with a first pretreatment liquid containing a reducing agent, a pH adjuster, and an additive that promotes or suppresses an electroless plating reaction; and supplying a first electroless plating liquid to the recess after contacting the seed layer with the first pretreatment liquid, thereby depositing a plating metal in the recess.

[0010] According to the present disclosure, it is advantageous to appropriately fill recesses in a substrate with plating metal by electroless plating processing. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a schematic diagram showing a plating processing apparatus as an example of a substrate liquid processing apparatus according to an embodiment of the present disclosure. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing the configuration of the plating processing section. [Diagram 3] FIG. 3 is an enlarged cross-sectional view of an example of a substrate (particularly a recess) for illustrating an example of a plating method. [Figure 4] FIG. 4 is an enlarged cross-sectional view of an example of a substrate (particularly a recess) for illustrating an example of a plating method. [Diagram 5] FIG. 5 is an enlarged cross-sectional view of an example of a substrate (particularly a recess) for illustrating an example of a plating method. [Figure 6] FIG. 6 is an enlarged cross-sectional view of an example of a substrate (particularly a recess) for illustrating an example of a plating method. [Figure 7] FIG. 7 is a diagram showing an example of the relationship between the time (horizontal axis) in the electroless plating process and the thickness (vertical axis) of the metal film (including the seed layer and plating metal) on the surface of the recessed portion of the substrate. [Figure 8] FIG. 8 is an enlarged cross-sectional view of an example of a substrate (particularly a recess) for illustrating a plating method according to a first modified example. [Figure 9] FIG. 9 is an enlarged cross-sectional view of an example of a substrate (particularly a recess) for illustrating a plating method according to a first modified example. [Figure 10] FIG. 10 is an enlarged cross-sectional view of an example of a substrate (particularly a recess) for illustrating a plating method according to a first modified example. [Figure 11] FIG. 11 is an enlarged cross-sectional view of an example of a substrate (particularly a recess) for illustrating a plating method according to a first modified example. [Figure 12] FIG. 12 is an enlarged cross-sectional view of an example of a substrate (particularly a recess) for illustrating a plating method according to a first modified example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, an embodiment of the present disclosure will be described with reference to the drawings.

[0013] FIG. 1 is a schematic diagram showing a plating processing apparatus as an example of a substrate liquid processing apparatus according to an embodiment of the present disclosure.

[0014] The plating processing apparatus 1 is an apparatus that supplies a plating liquid (processing liquid) to a substrate W to perform plating processing (liquid processing) on ​​the substrate W. The plating processing apparatus 1 shown in FIG. 1 includes a plating processing unit 2 and a control unit 3 that controls the plating processing unit 2.

[0015] The plating unit 2 performs various types of treatment on the substrate W. The various types of treatment performed by the plating unit 2 will be described later.

[0016] The control unit 3 is, for example, a computer, and has an operation execution unit and a memory unit. The operation execution unit includes, for example, a CPU (Central Processing Unit), and controls the operation of the plating processing unit 2 by reading and executing programs stored in the memory unit. The memory unit is composed of a storage device such as a RAM (Random Access Memory), a ROM (Read Only Memory), or a hard disk. The memory unit stores programs that control various processes executed in the plating processing unit 2.

[0017] The program may be recorded on a computer-readable recording medium 31, or may be installed in the storage unit from the recording medium 31. Examples of the computer-readable recording medium 31 include a hard disk (HD), a flexible disk (FD), a compact disk (CD), a magnet optical disk (MO), and a memory card. The various programs recorded on the recording medium 31 include, for example, a program in which a computer controls the plating processing apparatus 1 and causes the plating processing apparatus 1 to execute a plating processing method (substrate liquid processing method).

[0018] The plating process unit 2 has a loading / unloading station 21 and a process station 22 provided adjacent to the loading / unloading station 21 .

[0019] The loading / unloading station 21 includes a placement section 211 and a transport section 212 provided adjacent to the placement section 211. A plurality of transport containers (hereinafter referred to as "carriers C") that accommodate a plurality of substrates W in a horizontal state are placed on the placement section 211. The transport section 212 includes a transport mechanism 213 and a delivery section 214. The transport mechanism 213 includes a holding mechanism that holds the substrates W, and is configured to be capable of moving in the horizontal and vertical directions and rotating about a vertical axis.

[0020] The processing station 22 includes a plating processor 5. In this embodiment, the processing station 22 has two or more plating processors 5, but may have only one. The plating processors 5 are arranged on both sides of a transport path 221 extending in a predetermined direction (on both sides in a direction perpendicular to the moving direction of the transport mechanism 222). The transport path 221 is provided with a transport mechanism 222. The transport mechanism 222 includes a holding mechanism for holding the substrate W, and is configured to be capable of moving in the horizontal and vertical directions and rotating about a vertical axis.

[0021] In the plating processing unit 2, the transport mechanism 213 of the loading / unloading station 21 transports the substrate W between the carrier C and the delivery section 214. Specifically, the transport mechanism 213 takes out the substrate W from the carrier C placed on the placement section 211, and places the taken-out substrate W on the delivery section 214. The transport mechanism 213 also takes out the substrate W placed on the delivery section 214 by the transport mechanism 222 of the processing station 22, and stores it in the carrier C of the placement section 211.

[0022] In the plating processing unit 2, the transport mechanism 222 of the processing station 22 transports the substrate W between the delivery section 214 and the plating processing section 5, and between the plating processing section 5 and the delivery section 214. Specifically, the transport mechanism 222 removes the substrate W placed in the delivery section 214, and carries the removed substrate W into the plating processing section 5. The transport mechanism 222 also removes the substrate W from the plating processing section 5, and places the removed substrate W in the delivery section 214.

[0023] FIG. 2 is a schematic cross-sectional view showing the configuration of the plating unit 5. As shown in FIG.

[0024] The plating processing section 5 is configured to perform a liquid processing including an electroless plating process. The plating processing section 5 includes a chamber 51, a substrate holding section 52 arranged in the chamber 51 and holding the substrate W horizontally, and a plating liquid supply section 53 (processing liquid supply section) that supplies a plating liquid L1 (processing liquid) to the upper surface (processing surface) of the substrate W held by the substrate holding section 52. In this embodiment, the substrate holding section 52 has a chuck member 521 that vacuum-sucks the lower surface (rear surface) of the substrate W. The chuck member 521 is a so-called vacuum chuck type in the example shown in FIG. 2, but is not limited to the vacuum chuck type. The substrate holding section 52 may be a so-called mechanical chuck type, and may grip the outer edge of the substrate W by a chuck mechanism or the like.

[0025] A rotary motor 523 (rotation drive unit) is connected to the substrate holding unit 52 via a rotary shaft 522. When the rotary motor 523 is driven, the substrate holding unit 52 rotates together with the substrate W. The rotary motor 523 is supported by a base 524 fixed to the chamber 51.

[0026] A cooling plate 525 is provided on the rotary motor 523. A cooling groove 525a through which a cooling liquid (for example, cooling water) flows is provided on the upper surface of the cooling plate 525. The cooling groove 525a is formed so as to surround the rotary shaft 522 when viewed from above. The cooling liquid from a cooling liquid supply source flows into the cooling groove 525a, flows through the cooling groove 525a, and flows out from the cooling groove 525a. While flowing through the cooling groove 525a, the cooling liquid exchanges heat with the rotary motor 523 to cool the rotary motor 523 and suppress a rise in temperature of the rotary motor 523.

[0027] The plating solution supply unit 53 has a plating solution nozzle 531 (treatment solution nozzle) that supplies a plating solution L1 (first electroless plating solution) to the substrate W held by the substrate holding unit 52, and a plating solution supply source 532 that supplies the plating solution L1 to the plating solution nozzle 531. The plating solution supply source 532 is configured to supply the plating solution L1, the temperature of which is adjusted to a predetermined temperature, to the plating solution nozzle 531. The temperature of the plating solution L1 when discharged from the plating solution nozzle 531 is, for example, 55° C. or more and 75° C. or less, and more preferably 60° C. or more and 70° C. or less. The plating solution nozzle 531 is held by a nozzle arm 57 and configured to be movable.

[0028] The plating solution L1 is a plating solution for autocatalytic (reducing) electroless plating. The plating solution L1 contains metal ions such as cobalt (Co) ions, nickel (Ni) ions, tungsten (W) ions, copper (Cu) ions, palladium (Pd) ions, and gold (Au) ions, and a reducing agent such as hypophosphorous acid and dimethylamine borane. The plating solution L1 may contain additives. Examples of plating films (plating metals) that can be formed from the plating solution L1 include metals such as Co, Ni, Cu, Pd, and Au, and alloys such as CoWB, CoB, CoWP, CoWBP, NiWB, NiB, NiWP, and NiWBP.

[0029] The plating processing unit 5 further includes a cleaning liquid supply unit 54 that supplies a cleaning liquid L2 to the upper surface of the substrate W held by the substrate holding unit 52, a rinsing liquid supply unit 55 that supplies a rinsing liquid L3 to the upper surface of the substrate W, and a pre-treatment liquid supply unit 56 that supplies a pre-treatment liquid L4 to the upper surface of the substrate W.

[0030] The cleaning liquid supply unit 54 has a cleaning liquid nozzle 541 that ejects the cleaning liquid L2 onto the substrate W held by the substrate holding unit 52, and a cleaning liquid supply source 542 that supplies the cleaning liquid L2 to the cleaning liquid nozzle 541. As the cleaning liquid L2, for example, organic acids such as formic acid, malic acid, succinic acid, citric acid, malonic acid, etc., and hydrofluoric acid (DHF) (aqueous solution of hydrogen fluoride) diluted to a concentration that does not corrode the plating surface of the substrate W, etc., can be used. The cleaning liquid nozzle 541 is held by a nozzle arm 57 and is movable together with the plating liquid nozzle 531.

[0031] The rinsing liquid supply unit 55 has a rinsing liquid nozzle 551 that discharges the rinsing liquid L3 onto the substrate W held by the substrate holding unit 52, and a rinsing liquid supply source 552 that supplies the rinsing liquid L3 to the rinsing liquid nozzle 551. The rinsing liquid nozzle 551 is held by a nozzle arm 57 and is movable together with the plating liquid nozzle 531 and the cleaning liquid nozzle 541. For example, pure water can be used as the rinsing liquid L3.

[0032] The pre-treatment liquid supply unit 56 has a pre-treatment liquid nozzle 561 that ejects a pre-treatment liquid L4 (first pre-treatment liquid) onto the substrate W held by the substrate holding unit 52, and a pre-treatment liquid supply source 562 that supplies the pre-treatment liquid L4 to the pre-treatment liquid nozzle 561. The pre-treatment liquid nozzle 561 is held by a nozzle arm 57 and is movable together with the plating liquid nozzle 531, the cleaning liquid nozzle 541, and the rinsing liquid nozzle 551. The pre-treatment liquid supply source 562 is configured to supply the pre-treatment liquid L4, the temperature of which has been adjusted, to the pre-treatment liquid nozzle 561.

[0033] Although there are no limitations on the composition of the liquid that can be used as the pretreatment liquid L4, the pretreatment liquid L4 of this embodiment contains a reducing agent, a pH adjuster, and an additive that promotes or suppresses the electroless plating reaction (i.e., an accelerator or suppressor).

[0034] The reducing agent contained in the pretreatment liquid L4 reduces the surface oxide film of the substrate W, modifying the surface of the substrate W so as to increase the activity of the plating reaction of the substrate W. This allows the electroless plating reaction to occur actively immediately after the plating solution L1 is applied to the substrate W. This makes it possible to shorten the time (incubation time) from the application of the plating solution L1 to the actual deposition of the plating metal, and even to make it as close to zero (0). This makes it possible to effectively prevent "thinning of the seed layer 11 due to corrosion of the seed layer 11 by the electroless plating solution," which may occur immediately after the application of the plating solution L1 to the substrate W.

[0035] In this embodiment, the reducing agent contained in the pretreatment liquid L4 is the same as the reducing agent contained in the plating liquid L1, but may be different from the reducing agent contained in the plating liquid L1. The concentration of the reducing agent in the pretreatment liquid L4 is higher than the concentration of the reducing agent in the plating liquid L1. This allows the surface of the substrate W to be effectively modified in the pretreatment. If the plating liquid L1 contains a high concentration of a reducing agent, the plating reaction may become unstable, but the pretreatment liquid L4 can contain a high concentration of a reducing agent without impairing the stability of the plating reaction.

[0036] The additives contained in the pretreatment liquid L4 (particularly an accelerator that promotes the electroless plating reaction or an inhibitor that suppresses the electroless plating reaction) adhere to the exposed surface of the seed layer 11. Depending on the adhesion state (e.g., the adhesion amount, adhesion density, etc.) of the additives to the seed layer 11, the progress of the electroless plating reaction when the plating liquid L1 is subsequently applied onto the substrate W can be controlled.

[0037] The specific composition of the additives contained in the pretreatment liquid L4 is not limited, and the pretreatment liquid L4 contains an additive selected according to the plating metal to be deposited. For example, when depositing copper plating by electroless plating, typically, an organic sulfur compound, an organic nitrogen compound, or a polymer compound can be used as the additive contained in the pretreatment liquid L4.

[0038] The pH adjuster contained in the pretreatment solution L4 can enhance the effect of modifying the seed layer 11 by the reducing agent, and also controls the adhesion state of the additive to the seed layer 11. That is, by adjusting the pretreatment solution L4 to a high pH (i.e., alkaline) by the pH adjuster, the effect of reducing the seed layer 11 by the reducing agent can be enhanced, and the incubation time of the electroless plating reaction can be further shortened.

[0039] The pH adjuster also adjusts the zeta potential of the additive, thereby controlling the adhesion of the additive to the seed layer 11. That is, the adhesion state of the additive to the seed layer 11 varies depending on the pH of the pretreatment liquid L4. Therefore, the pH of the pretreatment liquid L4 is adjusted to a desired pH by the pH adjuster contained in the pretreatment liquid L4, and the pH is stabilized, whereby the adhesion state of the additive to the seed layer 11 can be controlled.

[0040] The specific composition of the pH adjuster contained in the pretreatment liquid L4 is not limited. The optimum pH of the pretreatment liquid L4 for obtaining a desired adhesion state of the additive to the seed layer 11 varies depending on the type of additive. Therefore, the pH adjuster adjusts the pretreatment liquid L4 to alkaline, neutral, or acidic depending on the additive actually used. To adjust the pH of the pretreatment liquid L4 to alkaline, for example, a strong alkaline quaternary ammonium compound or the like can be used as the pH adjuster. On the other hand, to adjust the pH of the pretreatment liquid L4 to acidic, for example, an aqueous solution of an inorganic acid or the like can be used as the pH adjuster. For example, when an organic sulfur compound is used as the additive, the pH adjuster adjusts the pretreatment liquid L4 to acidic (for example, pH 3 or less (as an example, "pH=2")), so that the plating metal can be precipitated in each recess 10 in a bottom-up manner.

[0041] In addition, if the pretreatment liquid L4 is acidic, the seed layer 11 may be corroded by the pretreatment liquid L4. Therefore, by using an alkaline pretreatment liquid L4, it is possible to effectively avoid or reduce the corrosion of the seed layer 11. In addition, the alkaline pretreatment liquid L4 reduces the surface oxide film of the seed layer 11, and thus, in combination with the reducing action of the reducing agent contained in the pretreatment liquid L4, the surface of the seed layer 11 can be modified more effectively. Thus, from the viewpoint of suppressing corrosion of the seed layer 11 or promoting modification, it is preferable that the pretreatment liquid L4 has alkaline properties (for example, a pH of "11" or higher).

[0042] A nozzle moving mechanism (not shown) is connected to the nozzle arm 57 that holds the above-mentioned plating solution nozzle 531, cleaning solution nozzle 541, rinsing solution nozzle 551, and pre-treatment solution nozzle 561. The nozzle moving mechanism moves the nozzle arm 57 in the horizontal and vertical directions. More specifically, the nozzle moving mechanism allows the nozzle arm 57 to move between a discharge position where the processing liquid (plating solution L1, cleaning solution L2, rinsing solution L3, or pre-treatment liquid L4) is discharged onto the substrate W and a retreat position retreated from the discharge position. The discharge position is not particularly limited as long as the processing liquid can be supplied to any position on the upper surface of the substrate W, and is set to a position where the processing liquid can be supplied to the center of the substrate W, for example. The discharge position of the nozzle arm 57 may be different between the case where the plating solution L1 is supplied onto the substrate W, the case where the cleaning solution L2 is supplied, the case where the rinsing solution L3 is supplied, and the case where the pre-treatment liquid L4 is supplied. The retreat position is a position in the chamber 51 that does not overlap with the substrate W when viewed from above and is away from the discharge position. When the nozzle arm 57 is positioned at the retracted position, interference between the moving lid body 6 and the nozzle arm 57 is avoided.

[0043] A cup 571 is provided around the substrate holder 52. The cup 571 is formed in a ring shape when viewed from above, and receives the processing liquid splashed from the substrate W when the substrate W rotates, and guides it to the drain duct 581. An atmosphere blocking cover 572 is provided on the outer periphery of the cup 571, and prevents the atmosphere around the substrate W from diffusing into the chamber 51. The atmosphere blocking cover 572 is formed in a cylindrical shape extending in the vertical direction, and has an open upper end. A lid body 6 can be inserted into the atmosphere blocking cover 572 from above.

[0044] A drain duct 581 is provided below the cup 571. The drain duct 581 is formed in a ring shape when viewed from above, and receives and discharges the processing liquid received by the cup 571 and descending, or the processing liquid that descends directly from around the substrate W. An inner cover 582 is provided on the inner periphery of the drain duct 581. The inner cover 582 is disposed above the cooling plate 525, and prevents the processing liquid and the atmosphere around the substrate W from diffusing. A guide member 583 that guides the processing liquid to the drain duct 581 is provided above the exhaust pipe 81. The guide member 583 prevents the processing liquid descending above the exhaust pipe 81 from entering the exhaust pipe 81, and is configured to be received by the drain duct 581.

[0045] The substrate W held by the substrate holding part 52 is covered by the lid body 6. The lid body 6 has a ceiling part 61 and a side wall part 62 extending downward from the ceiling part 61. When the lid body 6 is positioned at the first spacing position and the second spacing position, the ceiling part 61 is disposed above the substrate W held by the substrate holding part 52 and faces the substrate W at a relatively small interval.

[0046] The ceiling portion 61 includes a first ceiling plate 611 and a second ceiling plate 612 provided on the first ceiling plate 611. A heater 63 (heating portion) is interposed between the first ceiling plate 611 and the second ceiling plate 612. The first ceiling plate 611 and the second ceiling plate 612 are configured to seal the heater 63 and prevent the heater 63 from coming into contact with a processing liquid such as the plating liquid L1. More specifically, a seal ring 613 is provided between the first ceiling plate 611 and the second ceiling plate 612 on the outer periphery side of the heater 63, and the heater 63 is sealed by the seal ring 613. The first ceiling plate 611 and the second ceiling plate 612 are preferably resistant to corrosion against a processing liquid such as the plating liquid L1, and may be formed of, for example, an aluminum alloy. In order to further increase the corrosion resistance, the first ceiling plate 611, the second ceiling plate 612, and the side wall portion 62 may be coated with Teflon (registered trademark).

[0047] A lid moving mechanism 7 is connected to the lid 6 via a lid arm 71. The lid moving mechanism 7 moves the lid 6 horizontally and vertically. More specifically, the lid moving mechanism 7 has a rotation motor 72 that moves the lid 6 horizontally, and a cylinder 73 (distance adjustment unit) that moves the lid 6 vertically. The rotation motor 72 is attached to a support plate 74 that is provided so as to be movable vertically relative to the cylinder 73. An actuator (not shown) including a motor and a ball screw may be used instead of the cylinder 73.

[0048] The swivel motor 72 of the lid body moving mechanism 7 moves the lid body 6 between an upper position disposed above the substrate W held by the substrate holder 52 and a retracted position retracted from the upper position. The upper position is a position facing the substrate W held by the substrate holder 52 at a relatively large distance and overlapping the substrate W when viewed from above. The retracted position is a position in the chamber 51 that does not overlap the substrate W when viewed from above. When the lid body 6 is positioned at the retracted position, the moving nozzle arm 57 is prevented from interfering with the lid body 6. The rotation axis of the swivel motor 72 extends in the vertical direction, and the lid body 6 is capable of swivel movement in the horizontal direction between the upper position and the retracted position.

[0049] The cylinder 73 of the lid moving mechanism 7 moves the lid 6 in the vertical direction to adjust the distance between the upper surface of the substrate W and the first ceiling plate 611 of the ceiling portion 61. More specifically, the cylinder 73 can position the lid 6 at the first distance position, the second distance position, and the above-mentioned upper position (the position indicated by the two-dot chain line in FIG. 2).

[0050] By disposing the cover 6 at the first interval position, the interval between the substrate W and the first ceiling plate 611 becomes the smallest first interval, and the first ceiling plate 611 is closest to the substrate W. In this case, by setting the first interval to a interval such that the first ceiling plate 611 does not come into contact with the liquid on the substrate W, it is possible to effectively prevent the liquid from being contaminated or bubbles from being generated in the liquid.

[0051] When the cover 6 is disposed at the second distance position, the distance between the substrate W and the first ceiling board 611 becomes the second distance larger than the first distance. As a result, the cover 6 is positioned higher than the first distance position.

[0052] By disposing the lid body 6 in the upper position, the distance between the substrate W and the first ceiling board 611 becomes larger than the second distance, and the lid body 6 is positioned above the second distance position. This makes it possible to prevent the lid body 6 from interfering with surrounding structures such as the cup 571 and the atmosphere blocking cover 572 when the lid body 6 is pivoted in the horizontal direction.

[0053] When the cover 6 is positioned at the first spacing position and the second spacing position, the heater 63 is driven to heat the liquid on the substrate W. In other words, the cylinder 73 is capable of adjusting the distance between the substrate W and the first ceiling plate 611 to a first distance or a second distance when heating the liquid on the substrate W.

[0054] The side wall 62 of the cover 6 extends downward from the peripheral portion of the first ceiling plate 611 of the ceiling portion 61, and is disposed on the outer periphery side of the substrate W when heating the liquid on the substrate W (when the cover 6 is positioned at the first spacing position and the second spacing position). When the cover 6 is positioned at the first spacing position, the lower end of the side wall 62 is positioned at a position lower than the substrate W. In this case, the vertical distance between the lower end of the side wall 62 and the lower surface of the substrate W can be, for example, 10 to 30 mm. Even when the cover 6 is positioned at the second spacing position, the lower end of the side wall 62 is positioned at a position lower than the substrate W. In this case, the vertical distance between the lower end of the side wall 62 and the lower surface of the substrate W can be, for example, 4 to 5 mm.

[0055] The heater 63 heats the processing liquid (eg, plating liquid L1) on the substrate W when the cover 6 is positioned at the first spaced position and the second spaced position.

[0056] An inert gas (e.g., nitrogen (N2) gas) is supplied to the inside of the lid 6 by an inert gas supply unit 66. The inert gas supply unit 66 has a gas nozzle 661 that discharges an inert gas to the inside of the lid 6, and an inert gas supply source 662 that supplies the inert gas to the gas nozzle 661. The gas nozzle 661 is provided on the ceiling portion 61 of the lid 6, and discharges the inert gas toward the substrate W with the lid 6 covering the substrate W.

[0057] The ceiling 61 and the side wall 62 of the lid 6 are covered by the lid cover 64. The lid cover 64 is placed on the second ceiling plate 612 of the lid 6 via the support 65. That is, a plurality of support parts 65 protruding upward from the upper surface of the second ceiling plate 612 are provided on the second ceiling plate 612, and the lid cover 64 is placed on the support parts 65. The lid cover 64 is movable in the horizontal direction and the vertical direction together with the lid 6. In addition, the lid cover 64 preferably has higher heat insulation than the ceiling 61 and the side wall 62 in order to suppress the heat in the lid 6 from escaping to the surroundings. For example, the lid cover 64 is preferably formed of a resin material, and it is even more preferable that the resin material has heat resistance.

[0058] A fan filter unit 59 (gas supply unit) is provided at the top of the chamber 51 to supply clean air (gas) around the lid 6. The fan filter unit 59 supplies air into the chamber 51 (particularly, into the atmosphere blocking cover 572), and the supplied air flows toward the exhaust pipe 81. A downflow in which air flows downward is formed around the lid 6, and gas vaporized from the processing liquid, such as the plating liquid L1, flows toward the exhaust pipe 81 by the downflow. In this way, the gas vaporized from the processing liquid is prevented from rising and diffusing into the chamber 51.

[0059] The gas supplied from the fan filter unit 59 is exhausted by the exhaust mechanism 8. The exhaust mechanism 8 has two exhaust pipes 81 provided below the cup 571 and an exhaust duct 82 provided below the drain duct 581. The two exhaust pipes 81 penetrate the bottom of the drain duct 581 and are each connected to the exhaust duct 82. The exhaust duct 82 is formed in a substantially semicircular ring shape when viewed from above. In this embodiment, one exhaust duct 82 is provided below the drain duct 581, and two exhaust pipes 81 are connected to this exhaust duct 82.

[0060] Next, an example of a plating method performed by the plating apparatus 1 will be described.

[0061] 3 to 6 are enlarged cross-sectional views of an example of a substrate W (particularly a recess 10) for explaining an example of a plating method. For ease of understanding, the plating solution L1 and the pretreatment solution L4 are omitted from FIGS.

[0062] The plating method performed by the plating processing device 1 is implemented by appropriately controlling the plating processing section 5 by the control section 3. During the processing described below, clean air is supplied from the fan filter unit 59 into the chamber 51 and flows toward the exhaust pipe 81. In addition, a cooling liquid is passed through the cooling grooves 525a of the cooling plate 525 provided on the rotary motor 523 to cool the rotary motor 523.

[0063] [Substrate holding process] First, the substrate W is prepared. That is, the substrate W to be processed is carried into the plating processing section 5 and held by the substrate holding section 52.

[0064] The upper surface (i.e., the processing surface) of the substrate W used in this embodiment has a large number of recesses 10 (see FIG. 3). A plating metal (see reference numeral "13" in FIGS. 5 and 6) that functions as wiring is filled in the recesses 10 by an electroless plating process described later.

[0065] 3, the substrate W has a substrate main body W0 and a seed layer 11 laminated on the substrate main body W0, and the upper surface of the substrate W is formed by the seed layer 11. In this embodiment, the seed layer 11 is provided over the entire upper surface of the substrate W, and the entire surface of each recess 10 is formed by the seed layer 11. The seed layer 11 acts as a catalyst for the electroless plating reaction and promotes the deposition of the plating metal.

[0066] Although the specific composition of the seed layer 11 is not limited, the seed layer 11 can be made of a metal selected according to the plating metal to be deposited in the electroless plating process. For example, when copper (Cu) is to be deposited as the plating metal, the seed layer 11 can be made of a cobalt-based material.

[0067] [Substrate cleaning process] Next, a cleaning process is performed on the upper surface of the substrate W held by the substrate holder 52. Specifically, the rotation motor 523 is driven to rotate the substrate W. Meanwhile, the nozzle arm 57, which was positioned at the retracted position, moves to the discharge position. Then, the cleaning liquid L2 is supplied from the cleaning liquid nozzle 541 to the rotating substrate W, thereby cleaning the surface of the substrate W. The cleaning liquid L2 washes away deposits and the like from the substrate W, and is discharged into the drain duct 581.

[0068] [Substrate rinsing process] Next, a rinsing process is performed on the upper surface of the substrate W held by the substrate holder 52. Specifically, a rinsing liquid L3 is supplied from a rinsing liquid nozzle 551 to the rotating substrate W. The rinsing liquid L3 washes away the cleaning liquid L2 remaining on the substrate W, and is discharged into the drain duct 581.

[0069] [Pretreatment process] Next, the pretreatment liquid L4 is applied to the upper surface of the substrate W held by the substrate holding part 52, and the pretreatment liquid L4 is brought into contact with the seed layer 11. Specifically, in a room temperature environment (for example, in an environment of about 1 to 30° C.), the pretreatment liquid L4 is supplied from the pretreatment liquid nozzle 561 to the rotating substrate W. After a predetermined amount of the pretreatment liquid L4 is discharged from the pretreatment liquid nozzle 561, the feeding of the plating liquid L1 from the plating liquid supply source 532 to the plating liquid nozzle 531 is stopped, and the supply of the plating liquid L1 to the substrate W is stopped.

[0070] The pretreatment liquid L4 applied to the substrate W from the pretreatment liquid nozzle 561 spreads over the entire upper surface of the substrate W, forming a liquid pool layer (i.e., a puddle) on the upper surface of the substrate W. As a result, the entire upper surface of the substrate W is covered with the pretreatment liquid L4, and each recess 10 is filled with the pretreatment liquid L4. In this embodiment, the state in which the substrate W is covered with the pretreatment liquid L4 (i.e., the state in which the pretreatment liquid L4 is in contact with the seed layer 11 in the recess 10) is maintained for a predetermined time or more (e.g., about 30 seconds or more) in a room temperature environment.

[0071] As a result, the surface of the seed layer 11 is reduced and modified by the reducing agent contained in the pretreatment liquid L4, and the additive 12 contained in the pretreatment liquid L4 adheres to the surface of the seed layer 11.

[0072] The additive 12 exemplified in FIG. 4 is an inhibitor that inhibits an electroless plating reaction. When an inhibitor that inhibits an electroless plating reaction is used as the additive 12, the inhibitor adheres to the portion of the seed layer 11 that constitutes the upper side surface of the recess 10 at a higher density than the portion of the seed layer 11 that constitutes the bottom surface and lower side surface of the recess 10. When an accelerator that promotes an electroless plating reaction is used as the additive 12, the accelerator adheres to the portion of the seed layer 11 that constitutes the bottom surface and lower side surface of the recess 10 at a higher density than the portion of the seed layer 11 that constitutes the upper side surface of the recess 10. According to these embodiments, the deposition rate of the plating metal in the lower region of the recess 10 becomes faster than the deposition rate of the plating metal in the upper region of the recess 10, and the deposition of the plating metal in the recess 10 can be controlled in a bottom-up manner.

[0073] 4 showing the pretreatment step, the pretreatment liquid L4 is omitted, but in reality, the entire seed layer 11 shown in Fig. 4 is covered with the pretreatment liquid L4, and the pretreatment liquid L4 is filled into each recess 10. In addition, although the additive 12 is clearly shown in Fig. 4, the additive 12 is actually attached to the seed layer 11 at a molecular level, and it is difficult to confirm the additive 12 by direct visual inspection.

[0074] The rotation speed of the substrate W when the pretreatment liquid L4 is supplied to the substrate W is lower than the rotation speed during the above-mentioned rinsing process, and is adjusted to, for example, 50 to 150 rpm. This can promote the spreading of the pretreatment liquid L4 on the substrate W and promote the uniformity of the film thickness of the puddle of the pretreatment liquid L4. A part of the pretreatment liquid L4 applied to the substrate W flows out from the upper surface of the substrate W and is discharged from the drain duct 581. Note that the rotation of the substrate W may be stopped when the pretreatment liquid L4 is supplied to the substrate W. In this case, a large amount of the pretreatment liquid L4 can be held on the substrate W, and the film thickness of the puddle of the pretreatment liquid L4 can be increased.

[0075] Furthermore, the pretreatment liquid L4 on the substrate W may be heated by the heater 63. That is, although the pretreatment step is performed in a room temperature environment in the above example, the pretreatment step may be performed in a high temperature environment in which the substrate W and / or the pretreatment liquid L4 are actively heated. In this case, the pretreatment of the substrate W may be promoted. The heating treatment of the pretreatment liquid L4 may be performed by a process similar to that of the plating liquid L1 described later, and therefore a detailed description of the heating treatment of the pretreatment liquid L4 will be omitted.

[0076] As described above, in this process, the pretreatment liquid L4 is applied to the substrate W prior to the application of the plating liquid L1, thereby facilitating the electroless plating process using the plating liquid L1 described below, and enabling the plating metal 13 to be properly filled into the recesses 10 of the substrate W.

[0077] [Electroless plating process] After the pretreatment liquid L4 is brought into contact with the seed layer 11, a plating liquid L1 is supplied to the upper surface of the substrate W (including the recess 10), and a plating metal 13 is precipitated on the upper surface of the substrate W (including the recess 10) (see Figures 5 and 6).

[0078] Specifically, plating liquid L1 is supplied from plating liquid nozzle 531 to the rotating substrate W. The plating liquid L1 spreads over the entire upper surface of the substrate W, and forms a liquid puddle on the upper surface of the substrate W. As a result, the entire upper surface of the substrate W is covered with plating liquid L1, and each recess 10 is filled with plating liquid L1.

[0079] Although the plating solution L1 is omitted in Figures 5 and 6 which show the electroless plating process, in reality, the entire seed layer 11 shown in Figures 5 and 6 is covered with the plating solution L1, and the recess 10 shown in Figures 5 and 6 is filled with the plating solution L1.

[0080] As a result, the seed layer 11 is used as a catalyst in the plating solution L1 on the substrate W, and the plating metal 13 is gradually deposited on the seed layer 11 by an electroless plating reaction, and finally the plating metal 13 is filled into the entire recesses 10. Since the plating solution L1 is applied onto the seed layer 11 whose properties have been modified by the pretreatment solution L4 as described above, the plating metal 13 is filled into each recess 10 in a desired state, and it is possible to effectively suppress the occurrence of voids and seams in the plating metal 13 (see FIG. 6).

[0081] That is, since the surface of the seed layer 11 is modified by the reducing agent contained in the pretreatment liquid L4, the plating metal 13 can be deposited on the seed layer 11 immediately after the plating liquid L1 is applied to the seed layer 11. Therefore, it is possible to suppress the thinning of the seed layer 11 caused by the corrosion of the seed layer 11 by the plating liquid L1. In addition, the additive 12 is attached to the surface of the seed layer 11 so as to promote the deposition of the plating metal 13 in a bottom-up manner. Therefore, the plating metal 13 gradually deposits from the bottom upward in the recess 10 (see FIG. 5), suppressing the occurrence of voids and seams.

[0082] The electroless plating process of this embodiment, which is carried out using the above-mentioned plating processing unit 5 (see FIG. 2), includes the following plating solution piling step and plating solution heating step. <Plating solution application process> The plating liquid L1 is supplied and piled on the substrate W pretreated with the pretreatment liquid L4. In this case, the rotation speed of the substrate W may be reduced from the rotation speed during the rinsing process, for example, to 50 to 150 rpm. This can promote the spreading of the plating liquid L1 on the substrate W while promoting the uniformity of the thickness of the puddle of the plating liquid L1. A part of the plating liquid L1 applied to the substrate W flows out from the upper surface of the substrate W and is discharged from the drain duct 581. Note that the rotation of the substrate W may be stopped when the plating liquid L1 is supplied to the substrate W. In this case, a large amount of the plating liquid L1 can be held on the substrate W, and the thickness of the puddle of the plating liquid L1 can be increased.

[0083] Thereafter, the nozzle arm 57, which was positioned at the ejection position, is moved to the retracted position.

[0084] <Plating solution heating process> Thereafter, the plating solution L1 piled on the substrate W is heated. This plating solution heating process includes a step of covering the substrate W with the lid 6, a step of supplying an inert gas, a first heating process of heating the plating solution L1 with a first gap between the substrate W and the first ceiling board 611, and a second heating process of heating the plating solution L1 with the second gap. In the plating solution heating process, the substrate W may be rotated at the same or a different rotation speed as in the plating solution piling process, or the rotation may be stopped.

[0085] In the plating solution heating process of this example, first, the substrate W is covered with the lid body 6. That is, the rotation motor 72 of the lid body moving mechanism 7 is driven, and the lid body 6 positioned at the retracted position is rotated in the horizontal direction and positioned at the upper position. Next, the cylinder 73 of the lid body moving mechanism 7 is driven, and the lid body 6 positioned at the upper position is lowered and positioned at the first interval position. As a result, the interval between the substrate W and the first ceiling plate 611 of the lid body 6 becomes the first interval, the side wall portion 62 of the lid body 6 is disposed on the outer periphery side of the substrate W, and the lower end of the side wall portion 62 of the lid body 6 is positioned at a position lower than the lower surface of the substrate W. As a result, the substrate W is covered with the lid body 6.

[0086] With the substrate W covered by the lid 6, the gas nozzles 661 provided on the ceiling 61 of the lid 6 discharge an inert gas to the inside of the lid 6, creating a low-oxygen atmosphere around the substrate W. The inert gas is discharged for a predetermined time, and then the discharge of the inert gas is stopped.

[0087] Then, the heater 63 is driven to heat the plating solution L1 piled on the substrate W. That is, the heat generated by the heater 63 is transferred to the plating solution L1 on the substrate W, and the temperature of the plating solution L1 increases. The plating solution L1 is heated so that the temperature of the plating solution L1 increases to a predetermined temperature. When the temperature of the plating solution L1 increases to a temperature at which the plating metal 13 precipitates, the plating metal 13 precipitates on the upper surface of the substrate W.

[0088] Thereafter, the cylinder 73 of the lid moving mechanism 7 is driven, the lid 6 rises from the first spacing position to be positioned at the second spacing position, and the spacing between the substrate W and the first ceiling plate 611 of the lid 6 becomes the second spacing. In this case, the side wall 62 of the lid 6 is disposed on the outer periphery of the substrate W, and the lower end of the side wall 62 is positioned at a position lower than the lower surface of the substrate W. Therefore, the substrate W is still covered by the lid 6.

[0089] Then, the heater 63 is driven to heat the plating solution L1 piled on the substrate W. At this time, the temperature of the plating solution L1 does not substantially increase, and the temperature of the plating solution L1 is maintained, so that the plating solution L1 is kept warm. In this manner, the second spaced position is set at a position where the plating solution L1 is kept warm by the heat generated by the heater 63, and the plating solution L1 is prevented from excessively increasing in temperature, thereby preventing deterioration of the plating solution L1.

[0090] The plating solution L1 is heated in this manner so as to obtain a plating metal 13 of a desired thickness.

[0091] Thereafter, the lid body moving mechanism 7 is driven to position the lid body 6 at the retracted position. That is, the cylinder 73 of the lid body moving mechanism 7 is driven to raise the lid body 6 positioned at the second interval position to be positioned at the upper position. Thereafter, the swivel motor 72 of the lid body moving mechanism 7 is driven to swivel the lid body 6 positioned at the upper position in the horizontal direction to be positioned at the retracted position.

[0092] In this manner, the plating solution heating process for the substrate W is completed.

[0093] [Substrate rinsing process] After the plating metal 13 is embedded in the recesses of the substrate W, a rinse process is performed on the substrate W held by the substrate holder 52. Specifically, a rinse liquid L3 is supplied from a rinse liquid nozzle 551 to the rotating substrate W. The rinse liquid L3 washes away the plating liquid L1 remaining on the substrate W, and is discharged to the drain duct 581.

[0094] In this substrate rinsing process, the rotation speed of the substrate W is increased compared to the rotation speed during plating. For example, the substrate W is rotated at the same rotation speed as in the substrate rinsing process before plating. Then, the rinsing liquid nozzle 551, which has been positioned at the retreated position, moves to the discharge position. Next, the rinsing liquid nozzle 551 supplies the rinsing liquid L3 to the rotating substrate W, cleaning the surface of the substrate W. This washes away the plating liquid L1 remaining on the substrate W.

[0095] [Substrate drying process] Next, the rinsed substrate W is dried. In this case, for example, the rotation speed of the substrate W is increased to be higher than the rotation speed in the substrate rinsing process, and the substrate W is rotated at a high speed. As a result, the rinsing liquid L3 remaining on the substrate W is shaken off and removed, and the substrate W on which the plating film is formed is obtained. In this case, an inert gas such as nitrogen gas may be sprayed onto the substrate W to promote drying of the substrate W.

[0096] [Substrate removal process] Thereafter, the substrate W is removed from the substrate holder 52 and carried out of the plating processing section 5.

[0097] In this manner, a series of steps of the plating process for the substrate W using the plating process apparatus 1 is completed.

[0098] [First observation] FIG. 7 is a diagram showing an example of the relationship between the time (horizontal axis) in the electroless plating process and the thickness (vertical axis) of the metal film (including the seed layer 11 and plating metal 13) on the surface of the recess 10 of the substrate W.

[0099] The present inventors actually used the above-mentioned plating processing unit 5 to deposit a plating metal 13 (specifically, copper) on a substrate W having a seed layer 11, and measured the thickness of the metal film including the seed layer 11 and the plating metal 13 over time. Specifically, FIG. 7 shows a case where the plating metal 13 is deposited on the substrate W based on the above-mentioned plating method including the pretreatment using the pretreatment liquid L4, and a case where the plating metal 13 is deposited on the substrate W based on the above-mentioned plating method not including the pretreatment. In FIG. 7, the results obtained by the above-mentioned plating method including the pretreatment using the pretreatment liquid L4 are plotted with circles, and the results obtained by the above-mentioned plating method not including the pretreatment are plotted with triangles. In FIG. 7, the origin of the horizontal axis (see symbol "t0") indicates the start time of application of the plating liquid L1 to the substrate W, and the metal film thickness at t0 is the film thickness of the seed layer 11.

[0100] When no pretreatment was performed (see the plot of triangles in FIG. 7), the thickness of the metal film (specifically, the seed layer 11) was reduced (see "t0" to "t1" in FIG. 7) immediately after starting application of the plating solution L1 to the substrate W. This is due to corrosion of the seed layer 11 by the plating solution L1.

[0101] On the other hand, when the pretreatment was performed (see the plots indicated by circles in FIG. 7), the thickness of the metal film increased immediately after application of the plating solution L1 to the substrate W (see "t0" to "t1" in FIG. 7). This is because the plating metal 13 was deposited on the seed layer 11 immediately after application of the plating solution L1 was started.

[0102] It can also be seen from the results shown in FIG. 7 that the incubation time for deposition of the plating metal 13 can be shortened by performing pretreatment using the pretreatment liquid L4.

[0103] The present inventors confirmed by a micrograph the plating state at the bottom of the recess 10 of the substrate W immediately after starting application of the plating solution L1 (specifically, 5 seconds after starting application of the plating solution L1).The micrograph confirmed that when the pretreatment was performed, extremely small lumps of the plating metal 13 (i.e., plating metal nuclei) appeared at a higher density than when the pretreatment was not performed.

[0104] [Second observation] The present inventors actually used the above-mentioned plating processing unit 5 to deposit a plating metal 13 (specifically, copper) on a substrate W provided with a seed layer 11 while changing the components contained in the pretreatment liquid L4, and confirmed the deposition state of the plating metal 13 by microscopic photographs. Specifically, pretreatment was performed using each of pretreatment liquid L4 containing a reducing agent and a pH adjuster but not containing the above-mentioned additives, pretreatment liquid L4 containing an additive (accelerator) and a pH adjuster but not containing a reducing agent, and pretreatment liquid L4 containing all of a reducing agent, an additive (accelerator), and a pH adjuster.

[0105] A plating metal 13 was deposited on the substrate W under the same conditions according to the plating method described above, except for the components contained in the pretreatment liquid L4.

[0106] As a result, when pretreatment was performed using pretreatment solution L4 containing a reducing agent and a pH adjuster but not the above-mentioned additives, the plating metal 13 was precipitated immediately after the start of application of plating solution L1, and it was confirmed that pretreatment solution L4 accelerated the electroless plating reaction. However, the plating metal 13 was deposited and grew almost uniformly over the entire surface of seed layer 11, and even in recesses 10, the plating metal 13 was deposited and grew (conformal growth) according to the surface shape of recesses 10. Thus, it could not be said that the deposition of plating metal 13 in recesses 10 was sufficiently controlled in a bottom-up manner.

[0107] Furthermore, when pretreatment was performed using pretreatment solution L4 containing the above-mentioned additives and pH adjuster but not a reducing agent, the plating metal 13 was deposited immediately after the start of application of plating solution L1, and the promotion of the electroless plating reaction by pretreatment solution L4 was confirmed. However, the plating metal 13 was deposited and grew almost uniformly over the entire surface of seed layer 11, and conformal growth of the plating metal 13 was also confirmed in recesses 10. This is because, although the precipitation of the plating metal 13 was promoted by the additives contained in pretreatment solution L4, the precipitation of the plating metal 13 in recesses 10 could not be sufficiently controlled in a bottom-up manner.

[0108] On the other hand, when pretreatment was performed using pretreatment liquid L4 containing all of the reducing agent, additive, and pH adjuster, it was confirmed that plating metal 13 precipitated immediately after the start of application of plating solution L1, and plating metal 13 was deposited in a bottom-up manner in recess 10.

[0109] [Third Observation] The present inventors actually confirmed the deposition state of the plating metal 13 by microscopic photographs for each of the cases where pretreatment was not performed and where pretreatment was performed (but where the pH of the pretreatment liquid L4 was changed) using the above-mentioned plating processing unit 5. In particular, for the case where pretreatment was performed, the cases were one in which the pretreatment liquid L4 contained a pH adjuster that adjusted the pretreatment liquid L4 to alkaline, and one in which the pretreatment liquid L4 contained a pH adjuster that adjusted the pretreatment liquid L4 to acidic.

[0110] The pretreatment liquid L4 contains an accelerator for accelerating the electroless plating reaction as an additive, and the accelerator is one that is likely to adhere to the seed layer 11 (particularly the recesses 10) in a desired state (i.e., a state that promotes bottom-up deposition of the plating metal 13) when the pretreatment liquid L4 is acidic.

[0111] A plating metal 13 was deposited on the substrate W under the same conditions according to the plating method described above, except for the pretreatment and the pH of the pretreatment solution L4.

[0112] As a result, it was confirmed that when pretreatment was performed (when the pretreatment liquid L4 was acidic and when the pretreatment liquid L4 was alkaline), the plating metal 13 was efficiently deposited on the seed layer 11 of the substrate W compared to when pretreatment was not performed.

[0113] When the alkaline pretreatment liquid L4 was used, the plating metal 13 was deposited and grew almost uniformly over the entire surface of the seed layer 11, and it was confirmed that the precipitation of the plating metal 13 in the recesses 10 could not be sufficiently controlled in a bottom-up manner.

[0114] On the other hand, when the acidic pretreatment liquid L4 was used, the plating metal 13 was deposited and grew over the entire surface of the seed layer 11, and it was confirmed that the precipitation of the plating metal 13 in the recess 10 was controlled in a bottom-up manner.

[0115] As described above, by using the pretreatment solution L4 containing a reducing agent, an additive, and a pH adjuster, it is possible to activate the electroless plating reaction on the substrate W, shorten the incubation period for deposition of the plating metal 13, and promote bottom-up deposition of the plating metal 13 in the recesses 10. As a result, the electroless plating process can properly fill the recesses 10 of the substrate W with the plating metal 13 while preventing the occurrence of voids and seams.

[0116] [First Modification] In this modification, elements that are the same as or correspond to those in the above-described embodiment are given the same reference numerals, and detailed descriptions thereof will be omitted.

[0117] 8 to 12 are enlarged cross-sectional views of an example of a substrate W (particularly a recess 10) for illustrating a plating method according to a first modified example. To facilitate understanding, the plating solution and the pretreatment solution are omitted from FIGS.

[0118] In the plating method according to this modification, prior to the application of the pretreatment liquid L4 (first pretreatment liquid) and the plating liquid L1 (first electroless plating liquid), a preceding pretreatment step (second pretreatment liquid) and a step of applying a preceding electroless plating liquid (second electroless plating liquid) to the substrate W are performed. As a result, the process of depositing the plating metal 13 on the substrate W is divided into multiple stages (two stages).

[0119] As in the above-described embodiment, the substrate W to be processed is transported into the plating processing section 5 and held by the substrate holding section 52 (substrate holding process), cleaned with the cleaning liquid L2 (substrate cleaning processing process), and rinsed with the rinsing liquid L3 (substrate rinsing processing process).

[0120] [Pre-treatment process] Thereafter, the preceding pre-treatment liquid (second pre-treatment liquid) is applied to the upper surface of the substrate W held by the substrate holding part 52, and the preceding pre-treatment liquid is brought into contact with the seed layer 11. This preceding pre-treatment step can basically be performed under the same conditions as the "pre-treatment step" in the above-mentioned embodiment.

[0121] The preceding pretreatment liquid contains a reducing agent and a pH adjuster. The preceding pretreatment liquid is adjusted to a desired pH (e.g., alkaline) by the pH adjuster. The reducing agent contained in the preceding pretreatment liquid reduces the oxide film on the surface of the substrate W, and modifies the surface of the substrate W so as to increase the activity of the plating reaction of the substrate W. In this modification, the concentration of the reducing agent differs between the preceding pretreatment liquid and the pretreatment liquid L4, and the preceding pretreatment liquid contains a reducing agent at a higher concentration than the pretreatment liquid L4.

[0122] The preceding pretreatment solution of this modification does not contain an additive that promotes or inhibits the electroless plating reaction, but may contain such an additive. In this case, the electroless plating reaction caused by the preceding electroless plating solution can be controlled by the additive contained in the preceding pretreatment solution.

[0123] 8, the preceding pretreatment liquid supplied from the preceding pretreatment liquid supply source 566 to the preceding pretreatment liquid nozzle 565 is discharged from the preceding pretreatment liquid nozzle 565 towards the substrate W. The preceding pretreatment liquid nozzle 565 is supported by a nozzle arm 57 (see FIG. 2) and is provided movable together with the nozzle arm 57. The preceding pretreatment liquid nozzle 565 and the above-mentioned pretreatment liquid nozzle 561 (see FIG. 2) may be configured as a common nozzle. Furthermore, the preceding pretreatment liquid supply source 566 and the pretreatment liquid supply source 562 (see FIG. 2) may be configured as a common supply source.

[0124] [Pre-electroless plating process] After the preliminary pretreatment solution is brought into contact with the seed layer 11, a preliminary electroless plating solution is supplied to the upper surface of the substrate W (including the recess 10), and a plating metal 13 is precipitated on the upper surface of the substrate W (including the recess 10) (see Figures 9 and 10).

[0125] The preceding electroless plating solution is applied onto the seed layer 11 modified by the preceding pretreatment solution. Therefore, deposition of the plating metal 13 on the seed layer 11 starts immediately after the preceding electroless plating solution is applied to the seed layer 11. Therefore, it is possible to increase the overall thickness of the metal film including the seed layer 11 and the plating metal 13 while suppressing corrosion of the seed layer 11 by the preceding electroless plating solution (see FIG. 10).

[0126] In this step, it is not necessarily required to deposit the plating metal 13 in the recesses 10 in a bottom-up manner. Therefore, as shown in Fig. 10, the deposition and growth of the plating metal 13 precipitated from the preceding electroless plating solution in the recesses 10 is conformal growth following the surface shape of the recesses 10. However, in this step, too, the plating metal 13 precipitated from the preceding electroless plating solution may be deposited in the recesses 10 in a bottom-up manner. In this case, by adding an additive that promotes or suppresses the electroless plating reaction to the preceding pretreatment solution, it is possible to control the precipitation of the plating metal 13 in the recesses 10 in a bottom-up manner.

[0127] This step can be carried out basically under the same conditions as the "electroless plating step" of the above embodiment. In this modification, the preceding electroless plating solution has the same composition as the plating solution L1 of the above embodiment, and the plating metal 13 having the same composition as the plating metal 13 deposited from the plating solution L1 is deposited from the preceding electroless plating solution.

[0128] 9, the preceding electroless plating solution supplied from a preceding plating solution supply source 568 to a preceding plating solution nozzle 567 is discharged from the preceding plating solution nozzle 567 toward the substrate W. The preceding plating solution nozzle 567 is supported by a nozzle arm 57 (see FIG. 2) and is provided so as to be movable together with the nozzle arm 57. The preceding plating solution nozzle 567 and the above-mentioned plating solution nozzle 531 (see FIG. 2) may be configured as a common nozzle. Furthermore, the preceding plating solution supply source 568 and the plating solution supply source 532 (FIG. 2) may be configured as a common supply source.

[0129] Thereafter, similarly to the pretreatment process of the above-described embodiment, the pretreatment liquid L4 is applied to the substrate W to perform pretreatment of the substrate W. In this modification, the pretreatment liquid L4 comes into contact with the layer of plating metal 13 deposited from the preceding electroless plating solution. As a result, the exposed surface of the layer of plating metal 13 is modified by the reducing agent, and the additive 12 adheres to the layer of plating metal 13 (see FIG. 11).

[0130] Thereafter, similarly to the electroless plating process of the above-described embodiment, plating solution L1 is applied to the substrate W, and electroless plating is performed on the substrate W. In this modification, plating solution L1 comes into contact with a layer of plating metal 13 precipitated from the preceding electroless plating solution, and the layer of plating metal 13 is used as a catalyst to gradually precipitate the plating metal 13 by an electroless plating reaction. As a result, the entire recess 10 is filled with plating metal 13, and the upper surface of the substrate W is covered with plating metal 13 (see FIG. 12).

[0131] Thus, in this modification, the layer of plating metal 13 precipitated from the preceding electroless plating solution essentially functions as a seed layer, and plating metal 13 precipitated from pretreatment solution L4 is deposited on the layer of plating metal 13. Therefore, the electroless plating process in this modification can be carried out under conditions suitable for precipitating plating metal 13 on the layer of plating metal 13.

[0132] Thereafter, similarly to the above-described embodiment, a substrate rinsing process, a substrate drying process, and a substrate removal process are performed.

[0133] As described above, according to this modification, before the pretreatment liquid L4 is brought into contact with the seed layer 11, the preliminary electroless plating liquid is supplied to the recesses 10 of the substrate W, and the plating metal 13 is deposited in the recesses 10.

[0134] As a result, the process of depositing the plating metal 13 on the substrate W is divided into a preliminary electroless plating process and an electroless plating process. Therefore, it is possible to carry out the preliminary electroless plating process so as to meet the conditions required for the initial stage of the electroless plating reaction, while carrying out the electroless plating process so as to meet the conditions required for the middle and subsequent stages of the electroless plating reaction. As a result, the electroless plating reaction can be carried out under desirable conditions throughout the entire process from the initial stage to the final stage, and the plating metal 13 can be appropriately filled into the recesses 10 of the substrate W.

[0135] Therefore, the preliminary electroless plating process can be performed under conditions optimized for avoiding "thinning of the seed layer 11 due to corrosion of the seed layer 11 by the plating solution", which is a concern in the early stage of the electroless plating reaction. On the other hand, in the subsequent electroless plating process, the conditions can be appropriately determined without considering the avoidance of "thinning of the seed layer 11 due to corrosion of the seed layer 11 by the plating solution".

[0136] Furthermore, even if the seed layer 11 is thin and discontinuous, by depositing the plating metal 13 on the bottom and sidewall surfaces of the recess 10 in the prior electroless plating process, the portions of the surface defining the recess 10 where the seed layer 11 is not present are also covered with the plating metal 13. As a result, the plating metal 13 can be appropriately filled into the recess 10 in the subsequent electroless plating process.

[0137] Prior to supplying the preceding electroless plating solution to the recess 10 of the substrate W, a preceding pretreatment solution containing a reducing agent and a pH adjuster is supplied to the recess 10. The concentration of the reducing agent differs between the pretreatment solution L4 and the preceding pretreatment solution.

[0138] This allows the plating metal 13 to be precipitated from the preceding electroless plating solution on the substrate W in a short period of time, and makes it possible to suppress corrosion of the seed layer 11 by the preceding electroless plating solution.

[0139] It should be noted that the embodiments and modifications disclosed in this specification are merely illustrative in all respects and are not to be construed as limiting. The above-mentioned embodiments and modifications can be omitted, substituted, and modified in various forms without departing from the scope and spirit of the appended claims. For example, the above-mentioned embodiments and modifications may be combined in part or in whole, and an embodiment other than the above-mentioned may be combined in part or in whole with the above-mentioned embodiment or modification.

[0140] Furthermore, the technical category in which the above-mentioned technical idea is embodied is not limited. For example, the above-mentioned substrate liquid processing apparatus may be applied to other apparatuses. Furthermore, the above-mentioned technical idea may be embodied by a computer program for causing a computer to execute one or more procedures (steps) included in the above-mentioned substrate liquid processing method. Furthermore, the above-mentioned technical idea may be embodied by a computer-readable non-transitory recording medium on which such a computer program is recorded.

Claims

1. providing a substrate having a recess, the substrate having a seed layer formed on a surface of the recess; a step of contacting the seed layer with a first pretreatment solution containing a reducing agent, a pH adjuster, and an additive that promotes or suppresses an electroless plating reaction; supplying a first electroless plating solution to the recesses after contacting the seed layer with the first pretreatment solution, thereby depositing a plating metal in the recesses; supplying a second electroless plating solution to the recess prior to contacting the first pretreatment solution with the seed layer to deposit a plating metal in the recess.

2. 2. The substrate liquid processing method according to claim 1, wherein a concentration of the reducing agent in the first pretreatment solution is higher than a concentration of the reducing agent in the first electroless plating solution.

3. supplying a second pretreatment liquid containing a reducing agent and a pH adjuster to the recess prior to supplying the second electroless plating solution to the recess; 3. The substrate processing method according to claim 1, wherein a concentration of a reducing agent in the first pretreatment liquid is different from that in the second pretreatment liquid.

4. On the computer, providing a substrate having a recess, the substrate having a seed layer formed on a surface of the recess; a step of contacting the seed layer with a first pretreatment solution containing a reducing agent, a pH adjuster, and an additive that promotes or suppresses an electroless plating reaction; supplying a first electroless plating solution to the recesses after contacting the seed layer with the first pretreatment solution, thereby depositing a plating metal in the recesses; supplying a second electroless plating solution to the recesses prior to contacting the first pretreatment solution with the seed layer to deposit a plating metal in the recesses; A computer-readable recording medium having a program recorded thereon for executing the above.

Citation Information

Patent Citations

  • Pretreating liquid for chemical plating

    JP1981123363A

  • Pretreating solution for electroless plating

    JP1994049649A

  • Formation method for wiring

    JP2001102448A

  • Electroless copper plating solution and electroless copper plating method using the same

    JP2003193249A

  • Pretreatment agent and pretreatment method for semiconductor wafer

    JP2008001963A