Resin composition

The resin composition addresses viscosity and thixotropy issues in adhesives and sealants by combining specific polymers and compounds, ensuring effective thixotropy without viscosity increase, enhancing coating properties and workability.

JP7581616B2Active Publication Date: 2024-11-13THREE BOND CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021554293
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-10-30
Filing Date
2020-10-12
Publication Date
2024-11-13
Estimated Expiration
2040-10-12

AI Technical Summary

Technical Problem

Conventional methods for increasing thixotropy in adhesives and sealants lead to increased viscosity, making dispensing difficult and causing issues like clogging, while methods using poorly compatible compounds result in resin bleed-out and poor curing.

Method used

A resin composition comprising specific combinations of polymers with alkenyl groups, polyorganosiloxanes with hydroxyl groups, silica powder treated with alkylsilane, and compounds containing boron, phosphorus, sulfur, or nitrogen, which adjust thixotropy without significantly increasing viscosity, ensuring excellent coating properties and workability.

Benefits of technology

The resin composition effectively maintains thixotropy without viscosity increase, preventing resin flow after application, allowing for proper coating and improved workability across various application methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581616000001
    Figure 0007581616000001
  • Figure 0007581616000002
    Figure 0007581616000002
  • Figure 0007581616000003
    Figure 0007581616000003
Patent Text Reader

Abstract

The present invention relates to a curable resin composition, etc., having excellent applyability and workability. Specifically, the present invention relates to a resin composition, etc., that includes (A) a polymer having two or more alkenyl groups, (B) one or more base polymers selected from the group consisting of polyorganosiloxanes having a hydroxyl group bonded to a silicon atom, (C) silica powder surface treated by an alkyl silane, and (D) a compound including one or more elements selected from the group consisting of boron, phosphorus, sulfur, and nitrogen.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition having excellent coatability and workability. [Background technology]

[0002] In order to improve the workability when applying adhesives, sealants, coating agents, etc., the viscosity and thixotropy are generally adjusted. In particular, it is essential to increase the thixotropy to enable application to vertical surfaces and to adjust the flowability to prevent the resin from flowing into an area greater than necessary, which causes problems, when using adhesives and sealants. Various methods are generally used to increase the thixotropy, such as adding a filler to the adhesive or sealant, or adding a compound that is poorly compatible with the base binder resin to the adhesive or sealant to cause chemical repulsion with the base resin and thereby express thixotropy (Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2015-010131 A Summary of the Invention

[0004] However, in the conventional method of adding a filler, the viscosity increases with the increase in the filler content, and when the filler content exceeds a certain amount, there are problems such as difficulty in discharging with a dispenser, and the filler can cause clogging in screen printing, significantly reducing workability. Also, in the method of improving thixotropy by adding a compound that is poorly compatible with the base binder resin, there are problems such as the resin bleeding out over time after application, leading to poor curing.

[0005] As a result of intensive research to achieve the above object, the present inventors have found a method for obtaining a resin composition with excellent coatability and workability by suppressing an increase in viscosity and effectively imparting thixotropy, and have arrived at the present invention. Note that thixotropy is also called thixotropic property, and the better the thixotropy, the lower the viscosity becomes under a high shear rate condition such as when applying a paint, but the higher the viscosity becomes under a low shear rate condition such as after application, and the paint after application does not flow (drip) downward, and appropriate application can be completed.

[0006] The present invention may be any one of the following [1] to

[13] . Appropriate combinations of the specific elements described in [1] to

[13] are also within the scope of the present invention. [1] (A) one or more base polymers selected from the group consisting of a polymer having two or more alkenyl groups, and (B) a polyorganosiloxane having a hydroxyl group bonded to a silicon atom; (C) Silica powder surface-treated with alkylsilane, and (D) a compound containing one or more elements selected from the group consisting of boron, phosphorus, sulfur, and nitrogen; A resin composition comprising: [2] The resin composition according to [1] above, wherein the component (D) is an acid or an acid ester compound. [3] The resin composition according to [1] above, wherein the component (D) is selected from the group consisting of boric acid, borate esters, phosphoric acid, phosphate esters, sulfuric acid, and nitric acid. [4] The resin composition according to any one of the above [1] to [3], wherein the silica powder of the component (C) is a fumed silica powder. [5] The resin composition according to any one of the above [1] to [4], wherein the component (C) is silica powder that has been surface-treated with octylsilane. [6] The resin composition according to any one of the above [1] to [5], wherein the component (A) is a vinyl polymer (A-1) having two or more alkenyl groups or a polyorganosiloxane (A-2) having two or more alkenyl groups. [7] The resin composition according to any one of the above [1] to [6], wherein a mass ratio of the component (C) to the component (D) is 9:1 to 1:9. [8] A curable resin composition comprising the resin composition according to any one of the above [1] to [7], a crosslinking agent, and a curing catalyst. [9] A cured product obtained by curing the curable resin composition described in [8] above.

[10] An adhesive comprising the curable resin composition according to [8] above.

[11] A sealant comprising the curable resin composition according to [8] above.

[12] (A) one or more base polymers selected from the group consisting of a polymer having two or more alkenyl groups, and (B) a polyorganosiloxane having a hydroxyl group bonded to a silicon atom; (C) Silica powder surface-treated with alkylsilane, and (D) one or more compounds selected from the group consisting of acids containing one or more elements selected from the group consisting of boron, phosphorus, sulfur, and nitrogen, and derivatives thereof; A method for producing a resin composition comprising mixing the above components.

[13] (A) one or more base polymers selected from the group consisting of a polymer having two or more alkenyl groups, and (B) a polyorganosiloxane having a hydroxyl group bonded to a silicon atom; (C) Silica powder surface-treated with alkylsilane, and (D) one or more compounds selected from the group consisting of acids containing one or more elements selected from the group consisting of boron, phosphorus, sulfur, and nitrogen, and derivatives thereof; to produce a resin composition; mixing the resin composition with a crosslinker and a curing catalyst; and a step of curing the resin composition to produce a cured product under a curing temperature of 30 to 300°C when component (A) is the base polymer, or in the presence of water vapor under a curing temperature of 10 to 50°C when component (B) is the base polymer; A method for producing a cured product comprising the steps of:

[0007] The resin composition of the present invention is extremely useful for improving coatability and workability because it allows adjustment of thixotropy without increasing viscosity, does not bleed out over time, and has excellent shape retention after application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The details of the present invention will be described below. Note that the preferred and more preferred embodiments exemplified below can be used in appropriate combination with each other regardless of the expressions such as "preferable" and "more preferred". Furthermore, the description of the numerical range is an example, and ranges obtained by appropriately combining the upper and lower limits of each range and the numerical values ​​of the examples can also be preferably used regardless of the expressions such as "preferable" and "more preferred". Furthermore, the terms "contain" or "include" may be read as "essentially consisting of" or "consisting only of" as appropriate.

[0009] <Resin composition> One aspect of the present invention is a composition comprising: (A) one or more base polymers selected from the group consisting of a polymer having two or more alkenyl groups; and (B) a polyorganosiloxane having a hydroxyl group bonded to a silicon atom; (C) Silica powder surface-treated with alkylsilane, and (D) one or more compounds selected from the group consisting of acids containing one or more elements selected from the group consisting of boron, phosphorus, sulfur, and nitrogen, and derivatives thereof; The resin composition includes:

[0010] [Component (A)] The component (A) used in the present invention is a base polymer, which is a main component that exerts the properties of the resin composition, and is also called a base binder when it has binder properties. The component (A) is a polymer having two or more alkenyl groups, and may have two or more alkenyl groups attached or bonded to the terminals of the polymer molecules constituting the main chain or to the molecular chain. The main chain of the polymer constituting the component (A) is not particularly limited, and various main chains can be used. From the viewpoint of versatility, it is preferable that the main chain of the polymer is a vinyl copolymer or a polyorganosiloxane. In such a case, the component (A) can be a vinyl copolymer (A-1) having two or more alkenyl groups, and a polyorganosiloxane (A-2) having two or more alkenyl groups, respectively. The number average molecular weight of the polymer constituting the main chain is, for example, in the range of 500 to 1,000,000, preferably 1000 to 100,000. Unless otherwise specified, the number average molecular weight in this specification is calculated by a standard polystyrene conversion method using size exclusion chromatography (SEC). The viscosity of the component (A-1) at 25°C is, for example, preferably 0.03 Pa·s to 1500 Pa·s, more preferably 0.05 Pa·s to 1000 Pa·s, and particularly preferably 0.3 Pa·s to 800 Pa·s. Unless otherwise specified, the viscosity testing method in this specification complies with JIS Z 8803. The alkenyl group content of component (A) can be, for example, 0.01 mmol / g to 5 mmol / g, and is preferably in the range of 0.05 mmol / g to 1 mmol / g.

[0011] The alkenyl groups constituting the component (A) are each independently represented by the general formula (I): R 2 R 3 C=C(R 1 In formula (I), R 1 , R 2 , and R 3may each independently be hydrogen or an organic group having 1 to 20 carbon atoms. The organic group having 1 to 20 carbon atoms is not particularly limited, but is preferably an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms, and specifically, examples thereof include the following group: -(CH2) n -CH3, -CH(CH3)-(CH2) n -CH3, -CH(CH2CH3)-(CH2) n -CH3, -CH(CH2CH3)2, -C(CH3)2-(CH2) n -CH3, -C(CH3)(CH2CH3)-(CH2) n -CH3, -C6H5, -C6H4(CH3), -C6H3(CH3)2, -(CH2) n -C6H5, -(CH2) n -C6H4(CH3), -(CH2) n Examples include -C6H3(CH3)2 (n is an integer of 0 or more, 1 or more, 3 or more, or 5 or more, and the total number of carbon atoms in each group is 20 or less, 18 or less, 15 or less, or 10 or less). In these groups, R 1 is hydrogen or a methyl group, 2 and R 3 Hydrogen is more preferred as the hydrogen atom. The number of alkenyl groups constituting the component (A) is two or more, and it is preferable that one alkenyl group is present at each end of the polymer molecule.

[0012] The vinyl monomer that is a structural unit of the copolymer that constitutes the main chain of the component (A-1) is not particularly limited, and various monomers can be used. For example, the monomers include (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, cyclohexyl (meth)acrylate, n-heptyl (meth)acrylate, n-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, cyclohexyl (meth)acrylate, n-heptyl (meth)acrylate, n-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, cyclohexyl (meth)acrylate, n-heptyl (meth)acrylate, n-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, cyclohexyl (meth)acrylate, n-heptyl (meth)acrylate, tert-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-butyl (meth)acrylate, tert-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, tert-butyl ... Octyl, (meth)acrylate-2-ethylhexyl, (meth)acrylate-nonyl, (meth)acrylate-decyl, (meth)acrylate-dodecyl, (meth)acrylate-phenyl, (meth)acrylate-toluyl, (meth)acrylate-benzyl, (meth)acrylate-2-methoxyethyl, (meth)acrylate-3-methoxybutyl, (meth)acrylate-2-hydroxyethyl, (meth)acrylate-2-aminoethyl, γ-(methacryloyloxypropyl)trimethoxysilane, (meth) (Meth)acrylic acid monomers such as ethylene oxide adducts of acrylic acid, trifluoromethylmethyl (meth)acrylate, 2-trifluoromethylethyl (meth)acrylate, 2-perfluoroethylethyl (meth)acrylate, 2-perfluoroethylmethyl (meth)acrylate, 2-perfluorohexylethyl (meth)acrylate, 2-perfluorodecylethyl (meth)acrylate, and 2-perfluorohexadecylethyl (meth)acrylate; styrene monomers such as styrene, vinyltoluene, α-methylstyrene, chlorostyrene, styrenesulfonic acid and its salts; fluorine-containing vinyl monomers such as perfluoroethylene, perfluoropropylene, and vinylidene fluoride; silicon-containing vinyl monomers such as vinyltrimethoxysilane and vinyltriethoxysilane; maleic anhydride, maleic acid, and monoalkyl and dialkyl esters of maleic acid; fumaric acid, and monoalkyl and dialkyl esters of fumaric acid;Examples of the monomers include maleimide monomers such as maleimide, methylmaleimide, octylmaleimide, dodecylmaleimide, stearylmaleimide, phenylmaleimide, and cyclohexylmaleimide; nitrile group-containing vinyl monomers such as acrylonitrile and methacrylonitrile; amide group-containing vinyl monomers such as acrylamide and methacrylamide; vinyl esters such as vinyl acetate, vinyl propionate, vinyl pivalate, vinyl benzoate, and vinyl cinnamate; alkenes such as ethylene and propylene; conjugated dienes such as butadiene and isoprene; vinyl chloride, vinylidene chloride, allyl chloride, and allyl alcohol. These may be used alone or may be copolymerized in combination. Among these, styrene monomers and (meth)acrylic acid monomers are preferred from the viewpoint of the physical properties of the product. More preferred are acrylic acid ester monomers and methacrylic acid ester monomers, particularly preferred are acrylic acid ester monomers, and most preferred is butyl acrylate. In the present invention, the above monomer may be copolymerized with other monomers, or may be block copolymerized. In that case, the above monomer is preferably contained in an amount of, for example, 40% or more, preferably 50% or more, more preferably 60% or more, and even more preferably 70% or more by mass ratio. In the above expression, for example, (meth)acrylic acid represents acrylic acid and / or methacrylic acid.

[0013] The number average molecular weight of the vinyl polymer of the present invention (the polymer constituting the main chain of the component (A-1)) is in the range of 500 or more and less than 1,000,000, and more preferably 1000 or more and less than 100,000. If the molecular weight is 500 or more, the amount of hydrosilyl bonds present in the cured product is appropriate, so that the inherent properties of the vinyl polymer are easily expressed, and if it is less than 1,000,000, handling difficulties such as difficulty in dispense application are avoided.

[0014] The vinyl polymer can be obtained by various polymerization methods, and the method is not particularly limited, but from the viewpoints of versatility of monomers and ease of control, radical polymerization is preferred. Among radical polymerization methods, controlled radical polymerization is preferred, living radical polymerization is more preferred, and atom transfer radical polymerization is particularly preferred.

[0015] The alkenyl group contained in the component (A-1) of the present invention is preferably one that undergoes a hydrosilyl reaction with a crosslinking agent described below, and is represented by the general formula (II): H2C=C(R 4 )- is preferred. In the above formula (II), R 4 is hydrogen or an organic group having 1 to 20 carbon atoms. The organic group having 1 to 20 carbon atoms is not particularly limited, but is preferably an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, or an aralkyl group having 7 to 20 carbon atoms, and specific examples thereof include the following groups: -(CH2) n -CH3, -CH(CH3)-(CH2) n -CH3, -CH(CH2CH3)-(CH2) n -CH3, -CH(CH2CH3)2, -C(CH3)2-(CH2) n -CH3, -C(CH3)(CH2CH3)-(CH2) n -CH3, -C6H5, -C6H4(CH3), -C6H3(CH3)2, -(CH2) n -C6H5, -(CH2) n -C6H4(CH3), -(CH2) n -C6H3(CH3)2 (n is an integer of 0 or more, 1 or more, 3 or more, or 5 or more, and the total number of carbon atoms in each group is 20 or less, 18 or less, 15 or less, or 10 or less). Among these, R 4 is preferably a hydrogen atom or a methyl group.

[0016] The viscosity of component (A-1) at 25°C is preferably 0.03 Pa·s or more and less than 1500 Pa·s, more preferably 0.05 Pa·s or more and less than 1000 Pa·s, and particularly preferably 0.3 Pa·s or more and less than 800 Pa·s. The alkenyl group content of the (A-1) component is preferably 0.01 mmol / g or more and 5 mmol / g or less, more preferably 0.05 mmol / g or more and 1 mmol / g or less, and by being within the above range, a resin composition having excellent reactivity and flexibility can be obtained.

[0017] A particularly preferred component (A-1) is a (meth)acrylic copolymer having vinyl groups (H2C=CH-) at both ends, and examples of commercially available products of such component (A-1) include XMAP SA100A and XMAP OR100A manufactured by Kaneka Corporation.

[0018] The polyorganosiloxane having an alkenyl group of the component (A-2) is not particularly limited, and various types can be used. The molecular structure of the polyorganosiloxane having an alkenyl group is substantially linear, but may have a branched structure in part. For example, polydimethylsiloxane capped with vinyl groups at both molecular chain ends; dimethylsiloxane-diphenylsiloxane copolymer capped with vinyl groups at both molecular chain ends; dimethylsiloxane-methylvinylsiloxane-diphenylsiloxane copolymer capped with vinyl groups at both molecular chain ends; polydimethylsiloxane capped with vinyl groups at one molecular chain end and trimethoxy groups at the other molecular chain end; polydimethylsiloxane capped with vinyl groups at one molecular chain end and trimethylsiloxy groups at the other molecular chain end; dimethylsiloxane-methylvinylsiloxane-diphenylsiloxane copolymer capped with trimethylsiloxy groups at both molecular chain ends. Among these, polydimethylsiloxanes capped with vinyl groups at both molecular chain terminals are preferred because of their versatility and excellent curability. These may be used alone or in combination of two or more. However, component (A-2) cannot be a polyorganosiloxane (component (B)) having a hydroxyl group bonded to a silicon atom.

[0019] The alkenyl group contained in the component (A-2) of the present invention is preferably one that undergoes a hydrosilyl reaction with the crosslinking agent described below, and may be any of the alkenyl groups exemplified in the above (A) and (A-1), and is preferably a vinyl group (HC=CH-) that bonds to Si in the polyorganosiloxane main chain.

[0020] The viscosity of component (A-2) at 25°C is preferably 0.03 Pa·s or more and less than 1500 Pa·s, more preferably 0.05 Pa·s or more and less than 1000 Pa·s, and particularly preferably 0.3 Pa·s or more and less than 800 Pa·s. The number average molecular weight of the polyorganosiloxane in component (A-2) of the present invention is in the range of 500 or more and less than 1,000,000, and more preferably 1000 or more and less than 100,000. If the molecular weight is 500 or more, the amount of hydrosilyl bonds present in the cured product is appropriate, so that the inherent properties of the vinyl polymer are easily expressed, and if it is less than 1,000,000, handling difficulties such as difficulty in dispense application are avoided.

[0021] The alkenyl group content of the (A-2) component is preferably 0.01 mmol / g or more and 5 mmol / g or less, more preferably 0.05 mmol / g or more and 1 mmol / g or less, and by being within the above range, a resin composition having excellent reactivity and flexibility can be obtained.

[0022] In the component (A), the method for introducing an alkenyl group into the main chain polymer can be any known method. Taking the method for introducing an alkenyl group into a vinyl polymer as an example, the following method can be mentioned. (1) A method in which, when synthesizing a vinyl polymer by radical polymerization, preferably living radical polymerization, a compound having both a low polymerizable alkenyl group and a relatively high polymerizable alkenyl group in one molecule is reacted as a second monomer. (2) A method in which, when synthesizing a vinyl polymer by living radical polymerization, a compound having at least two alkenyl groups having low polymerizability, such as 1,5-hexadiene, 1,7-octadiene, 1,9-decadiene, etc., is reacted at the end of the polymerization reaction or after the completion of the reaction of a specified monomer. (3) A method in which a vinyl polymer having at least one highly reactive carbon-halogen bond is reacted with various organometallic compounds having an alkenyl group, such as organotins such as allyltributyltin and allyltrioctyltin, to substitute the halogen. (4) A method in which a vinyl polymer having at least one highly reactive carbon-halogen bond is reacted with a stabilized carbanion having an alkenyl group to substitute for a halogen. (5) A method in which a vinyl polymer having at least one highly reactive carbon-halogen bond is allowed to react with a metal such as zinc or an organometallic compound to prepare an enolate anion, and then the enolate anion is reacted with an electrophilic compound having an alkenyl group, such as an alkenyl-group-containing compound having a leaving group such as a halogen or an acetyl group, a carbonyl compound having an alkenyl group, an isocyanate compound having an alkenyl group, or an acid halide having an alkenyl group. (6) A method in which a vinyl polymer having at least one highly reactive carbon-halogen bond is reacted with an oxyanion or a carboxylate anion having an alkenyl group to substitute for a halogen. (7) A method of reacting a hydroxyl group of a vinyl polymer having at least one hydroxyl group with an alkenyl group-containing halide, an alkenyl group-containing isocyanate compound, an alkenyl group-containing carboxylic acid or an alkenyl group-containing acid halide, or a method of reacting the above-mentioned hydroxyl group with a diisocyanate and further reacting it with a compound containing a hydroxyl group and an alkenyl group. Among these, methods (2), (6) and (7) are preferred because they are easier to control.

[0023] [(B) Component] The component (B) used in the present invention is a polyorganosiloxane having a hydroxyl group bonded to a silicon atom. However, the component (B) is different from the component (A). Among them, the polyorganosiloxane represented by the following general formula (III), in which both terminal groups are hydroxyl groups, i.e., blocked with hydroxyl groups, is preferred as the component (B). TIFF0007581616000001.tif4275 (in formula (III), R 5 and R 6 R may be the same or different, and may be a substituted or unsubstituted monovalent hydrocarbon group, preferably a hydrocarbon group having 12 or less carbon atoms, more preferably an alkyl group having 1 to 10, 1 to 8, or 2 to 6 carbon atoms, and more preferably an alkyl group such as methyl, ethyl, or propyl; a cycloalkyl group such as cyclohexyl; an alkenyl group such as vinyl or allyl; or an aryl group such as phenyl or tolyl. 5 and R 6 may be a substituted hydrocarbon group in which the hydrogen atoms of the group are partially substituted with halogen atoms or the like. In formula (III), n is, for example, an integer of 5 or more, preferably 10 to 100, and more preferably 15 to 50.

[0024] The viscosity of component (B) at 25°C is preferably 10 mm 2 / s or more 1000mm 2 / s, and more preferably less than 20 mm 2 / s or more 500mm 2 / s, most preferably less than 30 mm 2 / s~100mm 2 / s. 10mm 2 / s or more 1000mm 2 If the viscosity is less than 1 / s, the resin composition can be prevented from undergoing a change in viscosity over time. The number average molecular weight of the component (B) is, for example, within the range of 500 to 1,000,000, and preferably 1,000 to 100,000.

[0025] Commercially available products of component (B) include X-21-5841 and KF-9701 manufactured by Shin-Etsu Chemical Co., Ltd., BY16-873 manufactured by Dow Corning Toray Co., Ltd., and XC96-723 manufactured by Momentive Corporation. The base polymer of the above component (A) and / or component (B) may contain either component (A) or component (B), or both.

[0026] [(C) component] The component (C) used in the present invention is a silica powder surface-treated with an alkylsilane. The component (C) of the present invention can exhibit remarkable thixotropy when used in combination with the component (D) described below. The alkylsilane may be represented by the general formula (IV): Si(R 7 From the viewpoint of excellent dispersibility in the component (A) and the component (B) and of exerting high thixotropy with the component (D), an alkylsilane compound represented by the general formula (IV) represented by R 7 R in the above general formula (IV) may be the same or different, and is preferably an alkyl group having 3 to 15 carbon atoms, more preferably an alkyl group having 5 to 10 carbon atoms, and most preferably an alkyl group having 8 to 10 carbon atoms. 7 Specific examples of the alkyl group include propyl group, isopropyl group, butyl group, isobutyl group, pentyl group, isopentyl group, hexyl group, isohexyl group, heptyl group, isoheptyl group, octyl group, isooctyl group, nonyl group, isononyl group, decyl group and isodecyl group, with octyl group being preferred.

[0027] The silica powder of component (C) is preferably fumed silica powder. Fumed silica powder is made of silicon dioxide obtained by flame hydrolysis, and forms spherical particles, with multiple particles agglomerating and fusing together like beads to form bulky aggregates.

[0028] The average particle size of the primary particles of the alkylsilane-treated silica powder (C) is preferably 1 nm or more and less than 300 nm, more preferably 3 nm or more and less than 100 nm, and most preferably 5 nm or more and less than 50 nm. The average particle size of the primary particles in the present invention is measured and calculated by a general method such as a centrifugal sedimentation light transmission method, a laser diffraction method, or a method of measurement using a transmission electron microscope, but unless otherwise specified, the average particle size of the primary particles in this specification is a value obtained by measuring the major axis and minor axis of a two-dimensional projection image of each primary particle using a transmission electron microscope in accordance with JIS H 7804:2005 and averaging the measured values.

[0029] The BET specific surface area of ​​the silica powder surface-treated with alkylsilane (component C) is 300 m 2 / g, and more preferably less than 250m 2 The lower limit of the BET specific surface area is, for example, 100 m / g from the viewpoint of the packing ratio of the component (A) and the component (B). 2 / g or more, preferably 150m 2 / g or more.

[0030] From the viewpoint of preventing the sedimentation of component (C) in the resin composition over time, the apparent density of the surface-treated silica powder of component (C) is preferably 1 g / L or more and less than 100 g / L, more preferably 10 g / L or more and less than 80 g / L. Note that the apparent density referred to in this specification is a value measured by measuring the apparent density after sufficient tapping in accordance with DIN ISO 787-11.

[0031] The content of the (C) component is preferably 0.01 to 100 parts by mass, more preferably 0.1 to 50 parts by mass, and most preferably 0.5 to 30 parts by mass, per 100 parts by mass of the base polymer of the (A) component and / or the (B) component. By including the (C) component in an amount of 0.01 to 100 parts by mass, it is possible to control the viscosity characteristics while maintaining the properties of the base polymer.

[0032] Commercially available products of component (C) include AEROSIL R805 (manufactured by Evonik) and CAB-O-SIL TS-530 (manufactured by CABOT).

[0033] [(D) component] The component (D) that can be used in the present invention is a compound containing one or more elements selected from the group consisting of boron, phosphorus, sulfur, and nitrogen. The component (D) is a main component that suppresses the increase in viscosity caused by the component (C) and increases the effect of imparting thixotropy. The component (D) may be an acid containing the above-mentioned element, as well as a derivative of the acid, such as an ester of the acid (acid ester compound) or a salt of the acid. Examples of the component (D) include boric acid, boric acid esters, phosphoric acid, phosphoric acid esters, sulfuric acid, sulfuric acid esters, nitric acid, and nitric acid esters. Among these, boric acid, boric acid esters, phosphoric acid, and phosphoric acid esters are preferred from the viewpoint of curability and storage stability, and boric acid esters and phosphoric acid esters are preferred from the viewpoint of the effect of imparting thixotropy, with boric acid esters being particularly preferred.

[0034] Any borate ester can be used, but in the present invention, a compound having one borate ester in the molecule and represented by the following general formula (V) is more preferred. B-(OR 8 )3(V) In formula (V), R 8 is hydrogen or a functional group selected from an alkyl group having 1 to 6 carbon atoms, which may have a substituent, an aryl group, a carbonyl group, and an acetyl group, and all three may be the same or different. Examples of the compound include borate trialkyl ester compounds such as trimethyl borate, triethyl borate, and tributyl borate, and tributyl borate is preferred from the viewpoint of storage stability of the resin composition.

[0035] Examples of phosphate esters include, but are not limited to, ethyl acid phosphate, butyl acid phosphate, butoxyethyl acid phosphate, oleyl acid phosphate, 2-ethylhexyl acid phosphate, 2-hydroxyethyl methacrylate acid phosphate, dibutyl phosphate, and the like.

[0036] The content of the (D) component is preferably 0.05 to 20 parts by mass, more preferably 0.1 to 12 parts by mass, and most preferably 0.2 to 7 parts by mass, per 100 parts by mass of the base polymer of the (A) component and / or the (B) component. By including the (D) component in an amount of 0.05 to 20 parts by mass, the thixotropy can be maintained without affecting the properties of the resin composition.

[0037] In order to suppress an increase in viscosity and improve only the thixotropy, the mass ratio of the (C) component to the (D) component in the resin composition is, for example, (C) component:(D) component=15:1 to 1:15, preferably 9:1 to 1:9, more preferably 8:2 to 2:8, and most preferably 7:3 to 3:7.

[0038] [Optional ingredients] In addition to the above components (A) to (D), the resin composition of the present invention may contain optional components different from the above components (A) to (D), such as a filler, an antioxidant, a light stabilizer, a storage stabilizer, an antifoaming agent, a coupling agent, a leveling agent, a dispersant, a pH adjuster, a solvent, an adhesion imparting agent, a plasticizer, a pigment, a flame retardant, and a surfactant, within the scope of the object of the present invention. By adding these, a resin composition excellent in coatability, film-forming property, storage stability, etc. can be obtained. In the present invention, a filler may be added to an extent that does not impair storage stability, for the purpose of improving the elastic modulus, resin strength, fluidity, etc. of the cured product. Specific examples include organic powder, inorganic powder, metallic powder, etc. Examples of inorganic powder fillers include glass, alumina, mica, ceramics, silicone rubber powder, calcium carbonate, aluminum nitride, carbon powder, kaolin clay, dried clay mineral, dried diatomaceous earth, etc. The blending amount of the inorganic powder is preferably about 0.1 to 100 parts by mass per 100 parts by mass of the base polymer of the (A) component and / or the (B) component. If it is 100 parts by mass or less, sufficient fluidity as a resin composition is obtained, and good workability is obtained.

[0039] Examples of organic powder fillers include polyethylene, polypropylene, nylon, cross-linked acrylic, cross-linked polystyrene, polyester, polyvinyl alcohol, polyvinyl butyral, and polycarbonate. The amount of organic powder is preferably about 0.1 to 100 parts by mass per 100 parts by mass of the base polymer of the component (A) and / or the component (B). If the amount is more than 0.1 parts by mass, the effect is not reduced, and even if the amount is 100 parts by mass or less, sufficient fluidity as a resin composition is obtained, and good workability is obtained.

[0040] Examples of the metallic powder filler include gold, platinum, silver, copper, indium, palladium, nickel, alumina, tin, iron, aluminum, stainless steel, etc. The amount of the metallic powder to be blended is preferably about 0.1 to 100 parts by mass, more preferably 1 to 50 parts by mass, per 100 parts by mass of the base polymer of component (A) and / or component (B).

[0041] Examples of the antioxidant include quinone compounds such as β-naphthoquinone, 2-methoxy-1,4-naphthoquinone, methylhydroquinone, hydroquinone, hydroquinone monomethyl ether, mono-tert-butylhydroquinone, 2,5-di-tert-butylhydroquinone, p-benzoquinone, 2,5-diphenyl-p-benzoquinone, and 2,5-di-tert-butyl-p-benzoquinone; phenothiazine, 2,2-methylene-bis(4-methyl-6-tert-butylphenol), catechol, tert-butylcatechol, and 2-butyl-4 -Hydroxyanisole, 2,6-di-tert-butyl-p-cresol, 2-tert-butyl-6-(3-tert-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenyl acrylate, 2-[1-(2-hydroxy-3,5-di-tert-pentylphenyl)ethyl]-4,6-di-tert-pentylphenyl acrylate, 4,4'-butylidenebis(6-tert-butyl-3-methylphenol), 4,4'-thiobis(6-tert-butyl-3-methylphenol), 3,9-bis[2-[3-(3-tert-butyl ethyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl]-2,4,8,10-tetraoxaspiro[5,5]undecane, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], thiodiethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, N,N'-hexane-1,6-diylbis[3-(3,5-di -tert-butyl-4-hydroxyphenyl)propionamide], benzenepropanoic acid, 3,5-bis(1,1-dimethylethyl)-4-hydroxy, C7-C9 side chain alkyl ester, 2,4-dimethyl-6-(1-methylpentadecyl)phenol, diethyl [[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]phosphonate, 3,3',3'',5,5',5''-hexa-tert-butyl-a,a',a''-(mesitylene-2,4,6-tolyl)tri-p-cresol, calcium diethyl bis[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]phosphonate, 4,6-bis(octylthiomethyl)-o-cresol, ethylene bis(oxyethylene)bis[3-(5-tert-butyl-4-hydroxy-m-tolyl)propionate], hexamethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzoyl) 1,3,5-tris[(4-tert-butyl-3-hydroxy-2,6-xylyl)methyl]-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, reaction products of N-phenylbenzenamine with 2,4,6-trimethylpentene, 2,6-di-tert-butyl-4-(4,6-bis(octylthio)-1,3,5-triazin-2-ylamino)pheno phenols such as phenol, picric acid, and citric acid; tris(2,4-di-tert-butylphenyl)phosphite, tris[2-[[2,4,8,10-tetra-tert-butyldibenzo[d,f][1,3,2]dioxaphosphen-6-yl]oxy]ethyl]amine, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, bis[2,4-bis(1,1-dimethylethyl)-6-methylphenyl]ethyl ether Examples of such compounds include phosphorus compounds such as steric phosphorous acid, tetrakis(2,4-di-tert-butylphenyl)[1,1-bisphenyl]-4,4'-diylbisphosphonite, and 6-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetra-tert-butyldibenz[d,f][1,3,2]dioxaphosphene; amine compounds such as phenothiazine; lactone compounds; and vitamin E compounds. Among these, phenol compounds are preferred.

[0042] Examples of the light stabilizer include bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate, 4-benzoyloxy-2,2,6,6-tetramethylpiperidine, 1-[2-[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyloxy]ethyl]-4-[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyloxy]-2,2,6,6-tetramethylpiperidine, 1,2,2,6,6-pentamethyl-4-piperidine, Lysinyl methacrylate, bis(1,2,2,6,6-pentamethyl-4-piperidinyl) [[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl] butyl malonate, decanedioic acid bis(2,2,6,6-tetramethyl-1(octyloxy)-4-piperidinyl) ester, reaction products of 1,1-dimethylethyl hydroperoxide with octane, N,N',N'',N'''-tetrakis-(4,6-bis-(butyl-(N-methyl-2,2,6,6-tetramethylpiperidin-4-yl)amino)-triazine- 2-yl)-4,7-diazadecane-1,10-diamine, polycondensation product of dibutylamine·1,3,5-triazine·N,N′-bis(2,2,6,6-tetramethyl-4-piperidyl-1,6-hexamethylenediamine and N-(2,2,6,6-tetramethyl-4-piperidyl)butylamine, poly[[6-(1,1,3,3-tetramethylbutyl)amino-1,3,5-triazine-2,4-diyl][(2,2,6,6-tetramethyl-4-piperidyl)imino]hexamethylene[(2,2,6,6-tetramethyl-4-piperidyl)imino] 〕, polymer of dimethyl succinate and 4-hydroxy-2,2,6,6-tetramethyl-1-piperidineethanol, 2,2,4,4-tetramethyl-20-(β-lauryloxycarbonyl)ethyl-7-oxa-3,20-diazadispiro〔5,1,11,2〕heneicosan-21-one, β-alanine, N,-(2,2,6,6-tetramethyl-4-piperidinyl)-dodecyl ester / tetradecyl ester, N-acetyl-3-dodecyl-1-(2,2,6,6-tetramethyl-4-piperidinyl)pyrrolidine-2,5-dione, 2,2,4,4-Tetramethyl-7-oxa-3,20-diazadispiro[5,1,11,2]heneicosan-21-one, 2,2,4,4-tetramethyl-21-oxa-3,20-diazadicyclo-[5,1,11,2]heneicosane-20-propanoic acid dodecyl ester / tetradecyl ester, propanediol acid, [(4-methoxyphenyl)-methylene]-bis(1,2,2,6,6-pentamethyl-4-piperidinyl) ester, 2, Hindered amines such as higher fatty acid esters of 2,6,6-tetramethyl-4-piperidinol, 1,3-benzenedicarboxamide, and N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl); benzophenone compounds such as octabenzone; 2-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol, 2-(2-hydroxy-5-methylphenyl)benzotriazole, 2-[2-hydroxyphenyl]benzotriazole, benzotriazole-based compounds such as 2-(3,4,5,6-tetrahydrophthalimido-methyl)-5-methylphenyl]benzotriazole, 2-(3-tert-butyl-2-hydroxy-5-methylphenyl)-5-chlorobenzotriazole, 2-(2-hydroxy-3,5-di-tert-pentylphenyl)benzotriazole, reaction products of methyl 3-(3-(2H-benzotriazol-2-yl)-5-tert-butyl-4-hydroxyphenyl)propionate with polyethylene glycol, and 2-(2H-benzotriazol-2-yl)-6-dodecyl-4-methylphenol; benzoate-based compounds such as 2,4-di-tert-butylphenyl-3,5-di-tert-butyl-4-hydroxybenzoate; and triazine-based compounds such as 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[(hexyl)oxy]phenol. Particularly preferred are hindered amine compounds. The amount of the optional components contained in the resin composition of the present invention is, for example, 0.05 to 100 parts by mass, preferably 0.1 to 50 parts by mass, and more preferably 0.2 to 20 parts by mass, relative to 100 parts by mass of the base polymer of the (A) component and / or the (B) component.

[0043] <Curable resin composition> The above-mentioned resin composition of the present invention may be present as a curable resin composition by appropriately adding curable components such as a crosslinking agent, a catalyst, and a coupling agent. The curable resin composition can be cured under any conditions to obtain a cured product of the curable resin composition. The curable resin composition of the present invention can be used as a one-liquid type curable resin composition obtained by mixing all the components, as well as a two-liquid type curable resin composition kit in which some components are prepared and stored separately and mixed when used.

[0044] When a resin composition containing component (A) as a base polymer is used, a compound having one or more hydrosilyl groups in one molecule can be used as a crosslinking agent. The hydrosilyl group refers to a group having a SiH bond. The crosslinking agent is not particularly limited as long as it can be cured by a hydrosilylation reaction with component (A), and examples thereof include polysiloxanes, preferably organohydrogenpolysiloxanes, and silicones containing hydrosilyl groups in the molecule, which are made of linear, branched, cyclic or network molecules. In addition, from the viewpoint of resin strength and curability, compounds having two or more hydrosilyl groups in one molecule are preferred.

[0045] The viscosity of the crosslinking agent at 25°C is preferably 1 mPa·s or more and less than 10 Pa·s, more preferably 5 mPa·s or more and less than 5 Pa·s, and particularly preferably 7 mPa·s or more and less than 1 Pa·s, from the viewpoint of compatibility with the (A) component. The SiH value of the crosslinking agent is preferably 10 or more and less than 1000 g / mol, more preferably 50 or more and less than 700 g / mol, and most preferably 100 or more and less than 500 g / mol, from the viewpoint of curability of the resin composition. Here, the SiH value means the concentration (g / mol) of SiH groups in one molecule.

[0046] The substituents other than hydrogen atoms bonded to silicon atoms of the crosslinking agent are preferably alkyl groups having 1 to 20 carbon atoms and phenyl groups, but may be other groups.

[0047] Commercially available crosslinking agents include, but are not limited to, CR-300, CR-500 (manufactured by Kaneka Corporation), HMS-013, HMS-151, HMS-301 (manufactured by Azmax Corporation), and SH1107 Fluid (manufactured by Dow Corning Toray Co., Ltd.).

[0048] The amount of the crosslinking agent added is preferably 0.5 to 1.5 equivalents per hydrosilyl group in the crosslinking agent and per alkenyl group contained in the (A) component. More preferably, it is 0.8 to 1.2 equivalents. If it is more than 0.5 equivalents, the crosslinking density will not be too low, and if it is less than 1.5 equivalents, the problem of foaming due to dehydrogenation reaction will not occur, and the heat resistance will not be affected. In addition, from the viewpoint of curability, the mixing ratio of the (A) component and the (C) component is preferably in the range of 0.2 to 5, more preferably 0.4 to 2.5, in terms of the molar ratio of the hydrosilyl group of the (C) component to 1 mole of the alkenyl group of the (A) component. If the molar ratio is less than 5, sufficient curability can be obtained, and if it is 0.2 or more, a uniform and strong cured product without cracks or voids can be obtained after curing.

[0049] When component (A) is used, it is preferable to use an addition reaction type curing catalyst as the catalyst. The addition reaction type curing catalyst preferably contains a hydrosilylation catalyst. There is no particular limitation on the hydrosilylation catalyst as long as it can catalyze the hydrosilylation reaction, and any catalyst can be used, for example, radical initiators such as organic peroxides and azo compounds, and transition metal catalysts. Among these, transition metal catalysts are preferred because of their high reactivity.

[0050] Specific examples of transition metal catalysts include platinum alone, platinum solid supported on a support such as alumina, silica, or carbon black; chloroplatinic acid; complexes of chloroplatinic acid with alcohols, aldehydes, ketones, etc.; platinum-olefin complexes; Pt n (ViMe2SiOSiMe2Vi) n , Pt〔(MeViSiO)4〕 mplatinum-vinylsiloxane complexes such as Pt(PPh3)4 and Pt(PBu3)4; platinum-phosphine complexes such as Pt[P(OPh)3]4 and Pt[P(OBu)3]4; and platinum-phosphite complexes such as Pt(acac)2. In the above formulas, Me represents a methyl group, Bu represents a butyl group, Vi represents a vinyl group, Ph represents a phenyl group, acac represents acetylacetonate, and n and m represent integers. Other examples include the platinum-hydrocarbon complexes described in U.S. Pat. Nos. 3,159,601 and 3,159,662 to Ashby et al., and the platinum alcoholate catalysts described in U.S. Pat. No. 3,220,972 to Lamoreaux et al. From the viewpoint of curing properties, preferred catalysts include chloroplatinic acid, platinum alone, solid platinum supported on a support such as alumina, silica, or carbon black; complexes of chloroplatinic acid with alcohols, aldehydes, ketones, etc.; platinum-olefin complexes such as Pt(CH2=CH2)2Cl2; platinum divinyltetramethyldisiloxane complex; Pt n (ViMe2SiOSiMe2Vi) x , Pt[(MeViSiO)4] y and platinum-phosphite complexes such as Pt(PPh3)4 and Pt(PBu3)4. Among these, from the viewpoint of excellent activity, chloroplatinic acid, platinum-olefin complexes, and platinum-vinylsiloxane complexes are preferred.

[0051] Further, examples of catalysts other than platinum compounds include RhCl(PPh3)3, RhCl3, Rh / Al2O3, RuCl3, IrCl3, FeCl3, AlCl3, PdCl2·xH2O, NiCl2, TiCl4, etc. These catalysts may be used alone or in combination of two or more kinds.

[0052] The amount of catalyst is not particularly limited. When component (A) is used, the amount of catalyst is preferably 1×10 -8 mol or more 1×10 -1 It is preferable to use it in the range of less than 1×10 -6 mol or more 1×10 -2In addition, when a hydrosilylation catalyst is used as the catalyst, it is preferable to use it in an amount of less than 1×10 mol because the hydrosilylation catalyst is generally expensive and corrosive, and may generate a large amount of hydrogen gas, causing foaming of the cured product. -1 The absolute amount of the catalyst present in the curable resin composition is, for example, 0.01 to 1 part by mass, preferably 0.020 to 0.5 parts by mass, and more preferably 0.03 to 0.1 parts by mass, relative to 100 parts by mass of the component (A). The catalyst may be in the form of either a solid or liquid, but it is suitable to use, for example, in the form of an alcohol solution, preferably in the form of a solution in methanol, ethanol, propanol, or the like, and more preferably in the form of an isopropanol solution.

[0053] When a curable resin composition is obtained using a resin composition containing the (B) component as a base polymer, it is preferable to further contain a compound having a polyfunctional hydrolyzable silyl group. Furthermore, in order to cause a condensation reaction between the compound and the (B) component, it is appropriate to use an organic tin complex, an amine compound, or an organic complex of a Group 4 element of titanium or zirconium as a condensation reaction catalyst. Depending on the type of hydrolyzable group, there are condensation reaction catalysts of the dealcoholization type, the oxime removal type, the acetate removal type, the ketone removal type, and the like.

[0054] The compound having a polyfunctional hydrolyzable silyl group is not limited as long as it has 2 to 3 hydrolyzable silyl groups in one molecule, and is preferably a silane coupling agent. Examples of hydrolyzable silyl groups include acyloxysilyl groups such as acetoxysilyl, octanoyloxysilyl, and benzoyloxysilyl; ketoximesilyl groups such as dimethylketoximesilyl, methylethylketoximesilyl, and diethylketoximesilyl; alkoxysilyl groups such as methoxysilyl, ethoxysilyl, and propoxy; alkenyloxysilyl groups such as isopropenyloxysilyl and 1-ethyl-2-methylvinyloxysilyl; aminosilyl groups such as dimethylaminosilyl, diethylaminosilyl, butylaminosilyl, and cyclohexylaminosilyl; aminoxysilyl groups such as dimethylaminooxysilyl and diethylaminooxysilyl; and amidosilyl groups such as N-methylacetamidosilyl, N-ethylacetamidosilyl, and N-methylbenzamidosilyl. In consideration of the human body and the environment, methoxysilyl, ethoxysilyl, and propoxysilyl groups are preferred.

[0055] Specific examples of the condensation reaction catalyst include organotin complexes such as dibutyltin bistriethoxysilicate, dibutyltin dioctoate, dibutyltin acetate, dibutyltin dilaurate, butyltin-2-ethylhexoate, stannous caprylate, tin naphthenate, tin oleate, and tin butyrate, and titanium catalysts such as tetraisopropyl titanate, tetra-n-butyl titanate, butyl titanate dimer, tetraoctyl titanate, titanium acetylacetonate, titanium octylene glycolate, titanium tetraacetylacetonate, titanium ethylacetoacetate, polyhydroxytitanium stearate, titanium lactate, and titanium triethanolamine. Zirconium catalysts include tetra-normal propoxy zirconium, tetra-normal butoxy zirconium, zirconium tetraacetylacetonate, zirconium monobutoxy acetylacetonate bis(ethylacetoacetate), zirconium dibutoxy bis(ethylacetoacetate), zirconium tetraacetylacetonate, and zirconium tributoxy stearate. However, the catalyst is not particularly limited to these. In addition, a compound having an amine in the structure of a crosslinking agent can also be used as a catalyst. Specific examples of the amine compound include 3-(2-aminoethyl)aminopropyl trimethoxysilane, N-2-(aminoethyl)-3-aminopropyl methyl dimethoxysilane, N-2-(aminoethyl)-3-aminopropyl trimethoxysilane, N-2-(aminoethyl)-3-aminopropyl methyl diethoxysilane, N-2-(aminoethyl)-3-aminopropyl triethoxysilane, 3-aminopropyl trimethoxysilane, and 3-aminopropyl triethoxysilane.

[0056] The amounts of the compound having a hydrolyzable silyl group and the condensation reaction catalyst added are 0.1 to 25 parts by mass, preferably 1 to 20 parts by mass, of the compound having a hydrolyzable silyl group, and 0.001 to 1 part by mass, preferably 0.01 to 0.5 part by mass, of the condensation reaction catalyst, relative to 100 parts by mass of component (B).

[0057] <Application> The resin composition of the present invention is used as a part of the material of a curable resin composition for use in a sealant, adhesive, etc. The curable resin composition of the present invention can be used as a sealant, adhesive, coating agent, etc. The cured product obtained by curing the curable resin composition of the present invention can be used as a seal layer or seal part formed by curing the above-mentioned sealant, an adhesive layer or adhesive part formed by curing the above-mentioned adhesive, or a coating layer or coating part formed by curing the above-mentioned coating agent. <Application method> The resin composition and curable resin composition of the present invention can be applied to an adherend by a known application method for a sealant or adhesive. For example, dispensing using an automatic coater, spraying, inkjet, screen printing, gravure printing, dipping, spin coating, and other methods can be used. From the viewpoint of coatability, the resin composition and curable resin composition of the present invention are preferably liquid at 25°C.

[0058] <Curing method and cured product> The curable resin composition of the present invention can be cured by a known method using heat, moisture, etc. to obtain a cured product. Specifically, the method for producing the cured product includes a step of producing a resin composition by mixing the above components (A) to (D) and, if necessary, the above optional components; An example of a method for producing a cured product includes a step of mixing a crosslinking agent and a curing catalyst with the resin composition, and a step of curing the resin composition to produce a cured product under a curing temperature of 30 to 300°C when component (A) is the base polymer, or in the presence of water vapor under a curing temperature of 10 to 50°C when component (B) is the base polymer.

[0059] When the curable resin composition using the component (A) of the present invention is heat cured, the curing temperature is not particularly limited, but is preferably 30 to 300° C., more preferably 50 to 200° C., and even more preferably 60 to 150° C. The curing time is not particularly limited, but when the temperature is 60 to 150° C., it is preferably 20 minutes or more and less than 5 hours, and even more preferably 40 minutes or more and less than 3 hours. When the curable resin composition using the component (B) of the present invention is moisture-cured with water vapor, the curing temperature is not particularly limited, but is preferably 10° C. to 50° C., and more preferably 15° C. to 30° C. The relative humidity is preferably 40% RH or more, and the curing time is preferably 1 hour or more and less than 2 weeks.

[0060] <Method of producing resin composition> The resin composition of the present invention is produced by mixing the various components. The order of mixing the various components is not particularly limited, and the (C) component may be dispersed in the (A) component and / or the (B) component using a mixer, and then the (D) component may be added, or the (D) component may be added to the (A) component and / or the (B) component, and after stirring in a mixer, the (C) component may be added and dispersed. The resin composition of the present invention can be further mixed with a curable component such as a crosslinking agent or a catalyst to produce a curable resin composition. Specifically, the curable resin composition is produced by the following procedure. When component (A) is used: After components (A) to (D) (component (B) is optional) are added, the mixture is stirred with a mixer, and curable components such as a crosslinking agent and a catalyst are added and stirred. When component (B) is used: Components (A) to (D) are added (component (A) is optional), and then curable components such as a crosslinking agent and a catalyst are added and stirred under reduced pressure. EXAMPLES

[0061] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples.

[0062] [Examples 1 to 7, Comparative Examples 1 to 7] The following ingredients were prepared to prepare the desired resin composition:

[0063] (A-1) Component: XMAP OR100A (Kaneka): Acrylic copolymer with one vinyl group at each end as an alkenyl group, viscosity (25°C) 700 Pa s Component (A-2): XF40-A1987 (Shin-Etsu Chemical Co., Ltd.): polyorganosiloxane having one vinyl group at each end as an alkenyl group, viscosity (25°C) 13 Pa s, alkenyl group (vinyl group) content 0.13 mmol / g (B) Component: KF-9701 (Shin-Etsu Chemical Co., Ltd.): dimethylsilicone oil with silanol ends at both ends, viscosity (25°C) 60 mm 2 / s (C) Ingredient: AEROSIL, R805 (manufactured by Evonik): fumed silica powder surface-treated with octylsilane, average primary particle size of 12 nm, BET specific surface area of ​​150 m 2 / g, apparent specific gravity 60g / l (C'1) Component: AEROSIL R972 (manufactured by Nippon Aerosil Co., Ltd.): fumed silica powder surface-treated with dimethylsilyl, average primary particle diameter of 16 nm, BET specific surface area of ​​110 m 2 / g, apparent specific gravity 50g / l (C'2) Component: AEROSIL 200 (manufactured by Nippon Aerosil Co., Ltd.): untreated fumed silica powder, average primary particle size of 12 nm, BET specific surface area of ​​200 m 2 / g, apparent specific gravity 50g / l (C'3) Component: AEROXIDE, T805 (manufactured by Nippon Aerosil Co., Ltd.) Titanium powder surface-treated with octylsilane, average primary particle size 21 nm, BET specific surface area 45 m 2 / g, apparent specific gravity 200g / l (D-1) Component: Tributyl borate (reagent) (D-2) Component: Phosphoric acid (reagent) (D-3) Component: Sulfuric acid (reagent) (D-4) Ingredient: Nitric acid (reagent) Component (D'-1): methacrylic acid (manufactured by Mitsubishi Rayon Co., Ltd.) (D'-2) Component: Acetic acid (reagent)

[0064] The components other than those shown in Tables 1 and 2 below are as follows. All amounts added are based on 100 parts by mass of the base polymer of component (A) or component (B). When component (A) is used CR-500 (crosslinking agent) Hydrosilyl group-containing compound (Kaneka Corporation) 16 parts by mass (1.0 equivalent to component A) SiH value: 253 g / mol Pt-VTS-3.0IPA (transition metal catalyst) 0.03 parts by mass of platinum divinyltetramethyldisiloxane complex in isopropyl alcohol (manufactured by Umicore Precious Metals Japan, Inc.) (B) When component is used 3-(2-aminoethyl)aminopropyltrimethoxysilane (condensation reaction catalyst, Z-6020, manufactured by Dow Corning Toray Co., Ltd.) 9 parts by mass Dibutyltin bistriethoxysilicate (condensation reaction catalyst, Neostan U-303, manufactured by Nitto Kasei Co., Ltd.) 0.2 parts by mass

[0065] The (A) component or the (B) component was weighed into a stirring vessel, and the (C) component was weighed into a stirring vessel and stirred for 30 minutes. The (D) component was weighed and stirred for 10 minutes. In addition, a crosslinking agent and a catalyst were weighed and added to obtain each curable resin composition. The detailed preparation amounts are shown in Tables 1 and 2, and all values ​​are expressed in parts by mass.

[0066] [viscosity] The viscosity (Pa s) of the curable resin composition was measured using a cone-plate viscometer under the following measurement conditions. It was evaluated according to the following criteria, and the results are shown in Table 1. Shear rate: 1.0s -1 Measurement time: 3 min Temperature conditions: 25℃ Resin amount: 0.5mL By measuring the viscosity, it is possible to evaluate the thixotropy of the sample, such as whether the viscosity is low under a high shear rate condition when the sample is applied. [Sagging evaluation] Droopiness is a measurement of how much paint moves vertically after a certain period of time has elapsed since the paint was applied to the surface to be coated. Droopiness measurement can be used to evaluate the thixotropy of the sample, whether or not the sample has high viscosity at low shear rate after application. Specifically, a marked line was drawn 10 mm from the short side of a SUS304 test piece (thickness 1.0 x short side 25 x long side 100 mm), and a bead of each resin with a diameter of 2.5 mm was applied on the marked line using a dispenser. The test piece was set up vertically, and the distance the resin moved from the marked line was measured over time (10 minutes, 30 minutes, and 60 minutes). The test was performed at 25°C. <Evaluation criteria> ◎ (Excellent): Distance traveled after 60 minutes is less than 3 mm ○ (Good): Distance traveled after 60 minutes is less than 5 mm △ (Acceptable): Distance traveled after 30 minutes is less than 5 mm × (Not acceptable): Distance traveled after 10 minutes is 5 mm or more When measuring the sagging property, the applicability and workability were also evaluated in terms of ease of application and the ease of work associated therewith.

[0067] Table 1 TIFF0007581616000002.tif60150

[0068] Table 2 TIFF0007581616000003.tif75150

[0069] As shown in Table 1, it can be seen that Examples 1 to 7, particularly Examples 1 to 5, and particularly Examples 3 and 5, have sufficiently low viscosity and are easy to apply. In addition, when actually measuring sagging, application was easy and the work could be performed well. Furthermore, regardless of the viscosity values ​​of Examples 1 to 7, the sagging was good. On the other hand, the resin compositions using the (C') component and the (D') component shown in Table 2 did not show satisfactory results in terms of sagging. Also, even a high-viscosity composition not containing the (D) component, such as Comparative Example 7, showed poor sagging results. [Industrial Applicability]

[0070] The resin composition of the present invention can effectively impart thixotropy regardless of viscosity, and therefore has good workability and can be applied to various coating methods, making it extremely useful.

Claims

1. (A) one or more base polymers selected from the group consisting of a vinyl polymer (A-1) having two or more alkenyl groups or a polyorganosiloxane (A-2) having two or more alkenyl groups, and (B) a polyorganosiloxane having two or more hydroxyl groups bonded to silicon atoms; (C) a silica powder surface-treated with an alkylsilane having an alkyl group having 3 to 15 carbon atoms, and (D) one or more compounds selected from the group consisting of boric acid, boric acid esters, phosphoric acid, phosphoric acid esters, sulfuric acid, and nitric acid; A resin composition comprising:

2. The resin composition according to claim 1 , wherein both terminal groups of the component (B) are hydroxyl groups.

3. 3. The resin composition according to claim 1, wherein the component (C) is a silica powder that has been surface-treated with an alkylsilane having an alkyl group having 5 to 10 carbon atoms.

4. The resin composition according to any one of claims 1 to 3, wherein the silica powder of the component (C) is a fumed silica powder.

5. The resin composition according to any one of claims 1 to 4, wherein the component (C) is a silica powder whose surface has been treated with octylsilane.

6. The resin composition according to any one of claims 1 to 5, wherein the component (D) is a boric acid ester.

7. The resin composition according to any one of claims 1 to 6, wherein the mass ratio of the component (C) to the component (D) is 9:1 to 1:

9.

8. A curable resin composition comprising the resin composition according to any one of claims 1 to 7, a crosslinking agent, and a curing catalyst.

9. A cured product obtained by curing the curable resin composition according to claim 8.

10. An adhesive comprising the curable resin composition according to claim 8.

11. A sealant comprising the curable resin composition according to claim 8.

12. (A) one or more base polymers selected from the group consisting of a vinyl polymer (A-1) having two or more alkenyl groups or a polyorganosiloxane (A-2) having two or more alkenyl groups, and (B) a polyorganosiloxane having two or more hydroxyl groups bonded to silicon atoms; (C) a silica powder surface-treated with an alkylsilane having an alkyl group having 3 to 15 carbon atoms, and (D) one or more compounds selected from the group consisting of one or more acids selected from the group consisting of boric acid, boric acid esters, phosphoric acid, phosphoric acid esters, sulfuric acid, and nitric acid, and derivatives thereof; A method for producing a resin composition comprising mixing the above components.

13. (A) one or more base polymers selected from the group consisting of a vinyl polymer (A-1) having two or more alkenyl groups or a polyorganosiloxane (A-2) having two or more alkenyl groups, and (B) a polyorganosiloxane having two or more hydroxyl groups bonded to silicon atoms; (C) a silica powder surface-treated with an alkylsilane having an alkyl group having 3 to 15 carbon atoms, and (D) one or more compounds selected from the group consisting of one or more acids selected from the group consisting of boric acid, boric acid esters, phosphoric acid, phosphoric acid esters, sulfuric acid, and nitric acid, and derivatives thereof; to produce a resin composition; mixing the resin composition with a crosslinker and a curing catalyst; and a step of curing the resin composition to produce a cured product under conditions of a curing temperature of 30 to 300° C. when component (A) is the base polymer, or in the presence of water vapor under conditions of a curing temperature of 10 to 50° C. when component (B) is the base polymer; A method for producing a cured product comprising the steps of:

Citation Information

Patent Citations

  • Alpha-cyanoacrylate adhesive composition

    JP1987020577A

  • Silicone adhesive composition having excellent heat resistance and production method

    JP2006028311A

  • Method of forming antifouling layer

    JP2008284408A

  • Coating composition and article with coating film

    JP2013023683A

  • Curable resin composition and cured product obtained by curing the same

    JP2015010131A