Composite particles and method for producing the same

By forming composite particles with micronized cellulose and core particles through an O/W Pickering emulsion, the method addresses low solid content issues, achieving stable and efficient handling and dispersion, thus enhancing the viability of micronized cellulose applications.

JP7581650B2Active Publication Date: 2024-11-13TOPPAN HOLDINGS INC
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020075374
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-04-21
Publication Date
2024-11-13
Estimated Expiration
2040-04-21

AI Technical Summary

Technical Problem

The practical application of micronized cellulose is hindered by low solid content concentration in dispersions, leading to high transportation costs, solvent handling issues, and stability problems, which affect business viability and functionality as an additive.

Method used

The production of composite particles by bonding finely divided cellulose with anionic functional groups to core particles through an O/W Pickering emulsion, using polymerizable monomers to stabilize and solidify the interface, resulting in a high-density, stable, and easily handled dry powder form.

Benefits of technology

The method provides stable, high-density composite particles with improved handling and dispersion stability, reducing transportation costs and enhancing addition efficiency to resins while maintaining functional properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581650000004
    Figure 0007581650000004
  • Figure 0007581650000005
    Figure 0007581650000005
  • Figure 0007581650000006
    Figure 0007581650000006
Patent Text Reader

Abstract

To provide a composite particle in which fine cellulose is stably adhered onto a core particle of various kinds, and a manufacturing method of a composite particle.SOLUTION: A composite particle 5 includes at least one kind of core particle 3. Fine cellulose 1 having an anionic functional group is bonded onto a surface of the core particle 3. In the fine cellulose 1, volume based particle size distribution has two or more particle size peaks. The particle size peaks are within a range of a volume based particle diameter of 0.01 to 20 μm.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composite particle comprising finely divided cellulose and a core particle, and a method for producing the composite particle. [Background technology]

[0002] In recent years, active efforts have been made to refine the cellulose fibers in wood so that at least one side of the structure is on the order of nanometers and to utilize them as new functional materials.

[0003] For example, as shown in Patent Document 1, it is disclosed that micronized cellulose, i.e., cellulose nanofibers (hereinafter also referred to as CNF), can be obtained by repeatedly mechanically treating wood cellulose with a blender or grinder. It has been reported that the CNF obtained by this method has a minor axis diameter of 10 to 50 nm and a major axis diameter ranging from 1 μm to 10 mm. This CNF is one-fifth the weight of steel and more than five times the strength, and can be stretched up to 250 m. 2 / g, it is expected to be used as a filler for reinforcing resins and as an adsorbent.

[0004] In addition, attempts to produce CNF by chemically treating cellulose fibers in wood in advance to facilitate finer processing, and then finer processing by low-energy mechanical processing such as a household mixer are actively being made. The above-mentioned chemical treatment method is not particularly limited, but a method in which ionic functional groups are introduced into cellulose fibers to facilitate finer processing is preferred. By introducing ionic functional groups into cellulose fibers, the solvent is easily infiltrated between the cellulose microfibril structures due to the osmotic effect, and the energy required for finer processing of cellulose raw materials can be significantly reduced. The above-mentioned method of introducing ionic functional groups is not particularly limited, but for example, Non-Patent Document 1 discloses a method of selectively phosphorylating the surface of cellulose fine fibers using a phosphoric acid esterification treatment. In addition, Patent Document 2 discloses a method of carboxymethylating cellulose by reacting it with monochloroacetic acid or sodium monochloroacetate in a high-concentration alkaline aqueous solution. In addition, carboxy groups may be introduced by directly reacting cellulose with a carboxylic anhydride compound such as maleic acid or phthalic acid gasified in an autoclave.

[0005] A method has also been reported in which the surface of cellulose fine fibers is selectively oxidized using a relatively stable N-oxyl compound, 2,2,6,6-tetramethylpiperidinyl-1-oxy radical (TEMPO), as a catalyst (see, for example, Patent Document 3). The oxidation reaction using TEMPO as a catalyst (TEMPO oxidation reaction) allows for environmentally friendly chemical modification that proceeds in an aqueous system at room temperature and normal pressure, and when applied to cellulose in wood, the reaction does not proceed inside the crystals, and only the alcoholic primary carbons of the cellulose molecular chains on the crystal surface can be selectively converted to carboxy groups.

[0006] The osmotic pressure effect caused by the ionization of carboxy groups selectively introduced to the crystal surface by TEMPO oxidation makes it possible to obtain cellulose single nanofibers (hereinafter also referred to as CSNF) in which each cellulose microfibril unit is dispersed in a solvent. CSNF exhibits high dispersion stability derived from the carboxy groups on the surface. It has been reported that wood-derived CSNF obtained from wood by the TEMPO oxidation reaction has a high aspect ratio structure with a short axis diameter of about 3 nm and a long axis diameter ranging from several tens of nm to several μm, and that its aqueous dispersion and molded body have high transparency. Patent Document 4 also reports that a laminated film obtained by applying and drying a CSNF dispersion has gas barrier properties.

[0007] As an example of a coating composition using microfibrillated cellulose (including CSNF, CNF, CNC, and cellulose nanofibers), for example, Patent Document 5 discloses a method of forming a laminate by coating an anchor layer with an aqueous coating liquid containing TEMPO-oxidized cellulose nanofibers, and reports that a laminate having good coatability and barrier properties can be obtained. Alternatively, Patent Document 6 discloses a coating liquid containing TEMPO-oxidized cellulose nanofibers in which carbon fine particles are dispersed and stabilized by the effect of the entanglement of the high aspect ratio fibers of cellulose nanofibers, their thickening properties, and the electric charge derived from the carboxyl group.

[0008] On the other hand, the problem of commercializing CNF is that the solid content concentration of the obtained CNF dispersion is low, about 0.1 to 5%. For example, when attempting to transport a finely divided cellulose dispersion, it is equivalent to transporting a large amount of solvent, which leads to a rise in transportation costs and significantly impairs business viability. In addition, when used as an additive for strengthening resins, there are problems such as a decrease in addition efficiency due to the low solid content, and difficulty in compounding when the solvent water is not compatible with the resin. In addition, when handling in a water-containing state, there is a risk of spoilage, so measures such as refrigerated storage and preservative treatment are required, which may increase costs.

[0009] However, if the solvent in the microfibrillated cellulose dispersion is simply removed by heat drying, the microfibrillated cellulose will aggregate and keratinize, or form a membrane, making it difficult to stably express its functions as an additive. Furthermore, because the solid concentration of CNF is low, the process of removing the solvent by drying itself requires a large amount of energy, which is also a factor that impairs the business viability.

[0010] Since handling CNF in the form of a dispersion liquid itself is a cause for loss of business viability, there is a strong need to provide a new method for easily handling CNF.

[0011] CNFs with a high aspect ratio have been developed in recent years, and their application to various applications is being considered. Meanwhile, cellulose nanocrystals (hereinafter also referred to as CNCs) have been developed as fine cellulose with a low aspect ratio and nano-sized size, which is made by removing the amorphous parts of cellulose and extracting only the highly crystalline parts. CNCs are mainly produced by hydrolyzing cellulose to break down the amorphous parts, followed by purification. For hydrolysis, for example, a method can be used in which the cellulose raw material is suspended in an aqueous solution of sulfuric acid, hydrochloric acid, hydrobromic acid, etc. Due to the simplicity of the process, it has a high cost advantage compared to CNFs.

[0012] CNCs have the appearance of needle-shaped particles with diameters ranging from several nm to several tens of nm and lengths of several hundred nm. Due to the low aspect ratio, the fibers are hardly entangled with each other, and during the manufacturing process, anions are introduced into some hydroxyl groups by sulfate ions, causing electrostatic repulsion between the fibers. As a result, compared to CNF, they are less likely to thicken in water, and their dispersion stability is high, making it possible to fill them at high concentrations. Furthermore, as mentioned above, only the crystalline parts are extracted, so one of their characteristics is that they have improved heat resistance compared to CNF. In addition, taking advantage of the high strength and high Young's modulus derived from their high crystallinity, they are used as reinforcement materials in the civil engineering and construction fields, automotive and aviation industries, and as flow control agents for paints and drilling mud, and it is expected that their applications will be expanded to a wider range of fields in the future.

[0013] Thus, various studies are being conducted on the development of high-performance components that impart new functionality to finely divided cellulose, a carbon-neutral material.

[0014] Meanwhile, various microparticles and microcapsules have been put to practical use as functional materials in various fields. Usually, microparticles are micro-sized particles formed from various polymers, and are used as fillers, spacers, abrasives, etc. In addition, attempts have been made to impart and express further functionality by forming a microcapsule structure in which the surface of a microparticle is covered with a wall membrane using a microparticle as a core substance. Specifically, by incorporating functional materials such as magnetic materials, medicines, pesticides, fragrances, adhesives, enzymes, pigments, dyes, etc. into the core substance and then microencapsulating it, it becomes possible to protect the functional materials and control their release behavior. It is also possible to impart functional materials to the wall membrane itself that covers the core substance. However, microparticles on the order of microns generally tend to aggregate easily due to their high specific surface area, making dispersion stability an issue. Depending on the application, biodegradability and biocompatibility are also required.

[0015] Patent Document 7 describes composite particles in which fine cellulose is bonded to polymer particles. The composite particles described in Patent Document 7 provide a new mode of handling polymer particles and fine cellulose. In addition, by bonding fine cellulose to polymer particles having various functions, new functionality can be imparted to the fine cellulose. It is desired to more stably adsorb fine cellulose to various types of core particles. [Prior art documents] [Patent documents]

[0016] [Patent Document 1] JP 2010-216021 A [Patent Document 2] International Publication No. 2014 / 088072 [Patent Document 3] JP 2008-001728 A [Patent Document 4] International Publication No. 2013 / 042654 [Patent Document 5] Patent No. 5928339 [Patent Document 6] Patent No. 6020454 [Patent Document 7] International Publication No. 2019 / 135384 [Non-patent literature]

[0017] [Non-Patent Document 1] Noguchi Y, Homma I, Matsubara Y. Complete nanofibrillation of cellulose prepared by phosphorylation. Cellulose. 2017;24:1295.10.1007 / s10570-017-1191-3 Summary of the Invention [Problem to be solved by the invention]

[0018] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide composite particles in which micronized cellulose is stably adsorbed onto various types of core particles, and a method for producing the composite particles. [Means for solving the problem]

[0019] In order to solve the above problems, the present invention proposes the following means. Composite particles according to one embodiment of the present invention teeth, The present invention comprises at least one type of core particle, and microfibrillated cellulose having an anionic functional group is bonded to the surface of the core particle. The microfibrillated cellulose has two or more particle size peaks in a volumetric particle size distribution, and the particle size peaks are in the volumetric particle size range of 0.01 μm or more and 20 μm or less. The core particle has at least one polymerizable functional group. Polymerizable Obtained by polymerizing monomers The polymerizable monomer is a (meth)acrylic monomer or a vinyl monomer. .

[0020] A method for producing composite particles according to one aspect of the present invention includes a first step of defibrating a cellulose raw material in a solvent to obtain a dispersion of finely divided cellulose having two or more particle size peaks in a volume-based particle size distribution in the volume-based particle size range of 0.01 μm to 20 μm, a second step of dispersing core particle precursors as droplets in a medium containing the dispersion, coating the surfaces of the core particle precursors with the finely divided cellulose, and stabilizing the core particle precursors as an emulsion, and a third step of solidifying the droplets to obtain composite particles in which core particles are coated with the finely divided cellulose. The second step includes adding a polymerizable monomer containing a polymerization initiator to the dispersion to form an emulsion. The polymerizable monomer is a (meth)acrylic monomer or a vinyl monomer. do. Effect of the Invention

[0021] According to one embodiment of the composite particle and the method for producing the composite particle of the present invention, it is possible to provide composite particles that are stably adsorbed to various types of core particles. [Brief description of the drawings]

[0022] [Figure 1] FIG. 1 is a schematic diagram of a composite particle according to one embodiment of the present invention. [Diagram 2] This is an SEM image (magnification: 200 times) of the appearance of the composite particle. [Diagram 3] This is an SEM image (magnification: 30,000 times) of the appearance of the composite particle. [Figure 4] 1 is a SEM image (magnification: 30,000 times) of the appearance of a composite particle when the present invention is not used. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. However, in each of the drawings described below, the same reference numerals are used to designate corresponding parts, and the description of overlapping parts will be omitted as appropriate. In addition, this embodiment is an example of a configuration for embodying the technical idea of ​​the present invention, and the material, shape, structure, arrangement, dimensions, etc. of each part are not specified as described below. The technical idea of ​​the present invention can be modified in various ways within the technical scope defined by the claims described in the claims.

[0024] <Composite particle 5> First, a composite particle 5 of fine cellulose / core particle according to one embodiment of the present invention will be described. One aspect of the core particle is a resin, which contains at least one type of polymer. Fig. 1 is a schematic diagram of an O / W Pickering emulsion using fine cellulose 1, and a composite particle 5 obtained by solidifying a liquid core particle precursor 2 (hereinafter also simply referred to as "droplet 2") inside the emulsion.

[0025] The composite particle 5 is a composite particle that contains at least one type of core particle 3, has a microfibrillated cellulose layer 10 composed of microfibrillated cellulose 1 on the surface of the core particle 3, and is in a state in which the core particle 3 and the microfibrillated cellulose 1 are bonded to each other.

[0026] The method for producing the composite particles 5 is not particularly limited, and known methods can be used. For example, a polymerization granulation method (emulsion polymerization method, suspension polymerization method, seed polymerization method, radiation polymerization method, etc.) in which particles are formed during polymerization using a monomer having a polymerizable functional group (also called a polymerizable monomer) as a core particle precursor, and a dispersion granulation method (spray drying method, in-liquid curing method, solvent evaporation method, phase separation method, solvent dispersion cooling method, etc.) in which particles are formed from a polymer solution in fine droplets can be used. The details of the production method will be described later.

[0027] For example, an O / W type Pickering emulsion is stabilized by adsorbing microfine cellulose 1 to the interface of droplets 2 of core particles 3 dispersed in a hydrophilic solvent, and by solidifying the droplets 2 inside the emulsion while maintaining the stabilized state, composite particles 5 can be produced using the emulsion as a template. In addition, solidifying the core particle precursor includes (1) polymerizing the polymerizable monomer droplets, (2) solidifying the polymer droplets, and (3) solidifying the polymerizable monomer droplets and the polymer droplets.

[0028] In this case, the mechanism by which the fine cellulose 1 is adsorbed to the interface of the droplets 2 and the O / W type Pickering emulsion is stabilized is believed to be due to the decrease in interfacial energy caused by adsorption. The fine cellulose 1, which is a solid particle that has been finely divided into nano- to micron-sized particles, is adsorbed to the droplet interface by physical forces and forms a cellulose barrier against the aqueous phase. Once adsorbed and an interface is formed, the emulsion structure is stabilized because a larger energy is required for desorption. Furthermore, fine cellulose is amphiphilic, and it is believed that the hydrophobic side of the fine cellulose 1 is adsorbed to the hydrophobic droplets 2, and the hydrophilic side of the fine cellulose is directed toward the dispersion solvent side, which is hydrophilic, thereby improving the stabilization of the droplet interface. However, the adsorption force at this interface depends on the affinity of the solid particles to the oil phase and the aqueous phase, that is, the affinity of the liquid core particle precursor of the fine cellulose to the dispersion solvent of the fine cellulose.

[0029] The bonding mechanism between the finely divided cellulose 1 and the core particle 3 in the composite particle 5 is not clear, but it is presumed that since the composite particle 5 is produced using an O / W type emulsion stabilized by the finely divided cellulose 1 as a template, the solidification of the droplets 2 inside the emulsion progresses while the finely divided cellulose 1 is in contact with the droplets 2, so that the finely divided cellulose 1 is physically fixed to the solidified droplets 2, and finally the core particle 3 and the finely divided cellulose 1 are bonded to each other. Here, the O / W type emulsion is also called oil-in-water type, in which water is the continuous phase and oil is dispersed as oil droplets (oil particles).

[0030] In addition, since the composite particles 5 are prepared using the O / W type emulsion stabilized by the fine cellulose 1 as a template, the shape of the composite particles 5 is characterized by being spherical due to the O / W type emulsion. In detail, the fine cellulose layer 10 made of the fine cellulose 1 is formed with a relatively uniform thickness on the surface of the spherical core particles 3. The average thickness of the fine cellulose layer 10 can be calculated by cutting the composite particles 5 fixed with an embedding resin with a microtome, observing the same with a scanning electron microscope, measuring the thickness of the fine cellulose layer 10 in the cross-sectional image of the composite particles 5 in the image at 100 random points on the image, and taking the average value. In addition, the composite particles 5 are characterized by being uniformly covered with the fine cellulose layer 10 with a relatively uniform thickness, and specifically, the coefficient of variation of the thickness value of the above-mentioned fine cellulose layer 10 is preferably 0.5 or less, more preferably 0.4 or less.

[0031] The fine cellulose 1 in this embodiment is not particularly limited, but has anionic functional groups on the crystal surface, and the content of the anionic functional groups is preferably 0.1 mmol or more and 5.0 mmol or less per 1 g of cellulose.

[0032] The microfibrillated cellulose 1 has at least a volumetric particle size distribution in the volumetric particle size range of 0.01 μm to 20 μm, and has two or more particle size peaks. The two or more particle size peaks are in the volumetric particle size range of 0.01 μm to 20 μm. Here, the volumetric particle size distribution is a distribution obtained by measuring the size distribution of microfibrillated cellulose in an aqueous dispersion on a volumetric basis. The volumetric particle size is a particle size obtained by measuring the size of microfibrillated cellulose in an aqueous dispersion on a volumetric basis. The particle size peak is a peak in the volumetric particle size distribution.

[0033] When there are two particle size peaks in the volumetric particle size distribution of the fine cellulose 1, the fine cellulose 1 having the smaller particle size peak is referred to as "fine cellulose 1A", and the fine cellulose 1 having the larger particle size peak is referred to as "fine cellulose 1B". The fine cellulose 1A preferably has one or more particle size peaks in the volumetric particle size range of 0.01 μm or more and 1 μm or less. The fine cellulose 1B preferably has one or more particle size peaks in the volumetric particle size range of 1 μm or more and 20 μm or less.

[0034] The fine cellulose 1A is needle-like or short fiber-like, and CNC or short fiber CNF having a number average minor axis diameter of 1 nm to 50 nm and a number average major axis diameter of 50 nm to 1 μm can be used. The fine cellulose 1B is preferably fibrous having a number average minor axis diameter of 1 nm to 50 nm and a number average major axis diameter of 1 μm to 20 μm. It is technically difficult to produce fine cellulose having a number average minor axis diameter of less than 1 nm. In addition, if the number average minor axis diameter is greater than 50 nm, the rigidity of the fine cellulose 1 becomes excessive, the adsorption force to the droplets 2 decreases, and the stability of the emulsion decreases. The volume-based particle size distribution and volume-based particle size of the fine cellulose 1 can be measured by any existing method, and for example, a particle size distribution meter using a dynamic light scattering method or the like can be used. The shape of the finely divided cellulose 1 can be determined by any existing method, for example, by adding water to the finely divided cellulose 1 to prepare a dilute dispersion, dropping the resulting solution onto mica, drying the solution, and observing the result with a scanning probe microscope.

[0035] Since the fine cellulose 1 has two or more particle size peaks in the volumetric particle size range of 0.01 μm or more and 20 μm or less, the amount of the fine cellulose 1 adsorbed to the droplets 2 increases, and as a result, the fine cellulose 1 is densely bonded to the composite particles 5. The mechanism by which the amount of the fine cellulose 1 adsorbed to the droplets 2 increases is not clear, but the fine cellulose 1B, which has a large particle size peak, entangles with the composite particles 5 to cover them and form a layer, and the fine cellulose 1A, which has a small particle size peak, is adsorbed into the gaps between the entanglements, and as a result, the amount of the fine cellulose 1 adsorbed to the composite particles 5 increases.

[0036] When a thermoplastic resin or the like is used for the core particle 3, the adsorption of the fine cellulose 1 to the droplet 2 may be weakened. In this case, when only the fine cellulose 1B is adsorbed to the droplet 2, a part of the fine cellulose 1B may peel off from the composite particle 5. On the other hand, when the fine cellulose 1A is adsorbed to the droplet 2 in addition to the fine cellulose 1B, the fine cellulose 1A is directly bonded to the interface of the droplet 2 and forms a physical bond with the fine cellulose layer made of the fine cellulose 1B, thereby preventing a part of the fine cellulose 1 from peeling off.

[0037] The amount of adsorption of the finely divided cellulose 1 can be measured by any method, but for example, it can be determined by measuring the zeta potential of the composite particles 5 in water and deriving it from the electric potential of the finely divided cellulose 1 adsorbed to the composite particles, or by dissolving the finely divided cellulose 1 coated on the surface of the composite particles and calculating it using the phenol-sulfuric acid method.

[0038] <Method of manufacturing composite particles> Next, a method for producing the composite particles according to this embodiment will be described. The method for producing the composite particles according to this embodiment includes a step (first step) of defibrating a cellulose raw material in a solvent to obtain a dispersion of fine cellulose 1 having two or more particle size peaks in the volumetric particle size range of 0.01 μm to 20 μm, a step (second step) of dispersing core particle precursors as droplets 2 in a medium containing the dispersion, coating the surfaces of the core particle precursors with the fine cellulose 1, and stabilizing them as an emulsion, and a step (third step) of solidifying the droplets 2 to obtain composite particles 5 in which core particles 3 are coated with the fine cellulose 1.

[0039] The second step is a method for producing composite particles using any one of the following steps: adding a polymerizable monomer containing a polymerization initiator to the fine cellulose dispersion to emulsify it; dissolving a core particle precursor in a solvent that has low compatibility with the fine cellulose dispersion and adding it to the fine cellulose dispersion to emulsify it; or adding a core particle precursor that is solid at room temperature to the fine cellulose dispersion, heating it to above its melting point to melt it and emulsify it.

[0040] In the first step, the fine cellulose 1 has two or more particle size peaks in the volumetric particle size range of 0.01 μm to 20 μm. The fine cellulose 1 having two or more particle size peaks can be prepared by using a mechanical treatment, a chemical treatment, or both of them in the process of preparing the fine cellulose 1.

[0041] The composite particles 5 obtained by the above manufacturing method are obtained as a dispersion. The composite particles 5 are obtained as a dry solid by further removing the solvent. The method of removing the solvent is not particularly limited, and for example, the excess water can be removed by centrifugation or filtration, and the dry solid can be obtained by further heat drying in an oven. In this case, the dry solid obtained does not become a film or aggregate, but is obtained as a finely textured powder. Although the reason for this is not clear, it is known that when the solvent is usually removed from a finely refined cellulose dispersion, the finely refined cellulose particles are strongly aggregated and formed into a film. On the other hand, in the case of a dispersion containing the composite particles 5, since the finely refined cellulose 1 is a spherical composite particle fixed to the surface, the finely refined cellulose 1 does not aggregate even when the solvent is removed, and only points between the composite particles are in contact, so that the dry solid is considered to be obtained as a finely textured powder. In addition, since there is no aggregation between the composite particles 5, the composite particles 5 obtained as a dry powder can be easily redispersed in a solvent again, and even after redispersion, the composite particles 5 show dispersion stability derived from the finely refined cellulose 1 bonded to the surface of the composite particles 5. Furthermore, the fine cellulose 1 on the surface of the obtained composite particles 5 is accumulated at a high density and is bonded in such a way that it is difficult to peel off.

[0042] The dry powder of the composite particles 5 is a dry solid that contains almost no solvent and can be redispersed in a solvent. Specifically, the solid content can be 80% or more, 90% or more, or 95% or more. Since the solvent can be almost completely removed, favorable effects can be obtained from the viewpoints of reducing transportation costs, preventing spoilage, improving the additive rate, and improving the efficiency of kneading with resin. When the solid content is increased to 80% or more by drying, the fine cellulose 1 is prone to hygroscopicity, so that the solid content may be reduced over time by adsorbing moisture in the air. However, considering the technical concept of the present invention, which is characterized in that the composite particles 5 can be easily obtained as a dry powder and can be redispersed, any dry solid that includes a process for increasing the solid content of the dry powder containing the composite particles 5 to 80% or more is defined as being within the technical scope of the present invention.

[0043] Each step will be described in detail below.

[0044] (1st step) The first step is a step of obtaining a microfibrillated cellulose dispersion by fibrillating the cellulose raw material in a solvent. First, various cellulose raw materials are dispersed in a solvent to obtain a suspension. The concentration of the cellulose raw material in the suspension is preferably 0.1% or more and less than 10%. If it is less than 0.1%, it is not preferable because the amount of solvent is excessive and productivity is impaired. If it is 10% or more, it is not preferable because the suspension rapidly thickens as the cellulose raw material is fibrillated, making it difficult to perform a uniform fibrillation process. The solvent used to prepare the suspension preferably contains 50% or more of water. If the proportion of water in the suspension is 50% or less, the dispersion of the microfibrillated cellulose 1 is inhibited in the step of obtaining a microfibrillated cellulose dispersion by fibrillating the cellulose raw material in a solvent, which will be described later. In addition, a hydrophilic solvent is preferable as the solvent contained other than water. There is no particular restriction on the hydrophilic solvent, but alcohols such as methanol, ethanol, and isopropanol, and cyclic ethers such as tetrahydrofuran are preferable. If necessary, the pH of the suspension may be adjusted to increase the dispersibility of the cellulose and the resulting microfibrillated cellulose 1. Examples of the aqueous alkali solution used for adjusting the pH include an aqueous sodium hydroxide solution, an aqueous lithium hydroxide solution, an aqueous potassium hydroxide solution, an aqueous ammonia solution, an aqueous tetramethylammonium hydroxide solution, an aqueous tetraethylammonium hydroxide solution, an aqueous tetrabutylammonium hydroxide solution, an aqueous benzyltrimethylammonium hydroxide solution, and other organic alkali solutions. In terms of cost, an aqueous sodium hydroxide solution is preferred.

[0045] The suspension is then subjected to a physical defibration treatment to pulverize the cellulose raw material. The method of physical defibration treatment is not particularly limited, but includes mechanical treatments such as a high-pressure homogenizer, an ultra-high-pressure homogenizer, a ball mill, a roll mill, a cutter mill, a planetary mill, a jet mill, an attritor, a grinder, a juicer mixer, a homomixer, an ultrasonic homogenizer, a nanogenizer, and underwater counter-collision. By performing such physical defibration treatment, the cellulose in the suspension is pulverized, and a dispersion of cellulose 1 in which at least one side of the structure is pulverized to the nanometer order can be obtained. In addition, the volume-based particle size distribution, number average minor axis diameter, and number average major axis diameter of the obtained pulverized cellulose 1 can be adjusted by the time and number of times of the physical defibration treatment at this time.

[0046] The microfibrillated cellulose 1 includes microfibrillated cellulose 1A and microfibrillated cellulose 1B having a volumetric particle size distribution different from that of the microfibrillated cellulose 1A. The microfibrillated cellulose 1A and the microfibrillated cellulose 1B may be produced from different cellulose raw materials or by different treatments. The microfibrillated cellulose 1A and the microfibrillated cellulose 1B may be produced from the same cellulose raw material or by the same treatment, but subjected to different types of defibration treatments.

[0047] The mixing ratio of the fine cellulose 1A and the fine cellulose 1B per dry weight is preferably in the range of 1 / 99 to 99 / 1 (fine cellulose 1A / fine cellulose 1B), and more preferably in the range of 10 / 90 to 80 / 20 (fine cellulose 1A / fine cellulose 1B). If the ratio of the fine cellulose 1A is too high, the stability of the droplets 2 during emulsion is reduced, and the amount of the fine cellulose 1 adsorbed to the composite particles 5 is reduced. On the other hand, if the ratio of the fine cellulose 1A is too low, the filling effect due to the adsorption of the finer fine cellulose 1A is reduced.

[0048] As described above, a dispersion (fine cellulose dispersion) of cellulose 1 which has been finely divided to such an extent that at least one side of the structure is on the order of nanometers is obtained. The obtained dispersion can be used as it is or after dilution, concentration, etc., as a stabilizer for O / W emulsions, which will be described later.

[0049] In addition, the fine cellulose dispersion may contain other components other than cellulose and the components used for pH adjustment, as necessary, within a range that does not impair the effects of the present invention. The other components are not particularly limited and can be appropriately selected from known additives depending on the application of the composite particles 5. Specifically, organic metal compounds such as alkoxysilanes or hydrolysates thereof, inorganic layered compounds, inorganic acicular minerals, defoamers, inorganic particles, organic particles, lubricants, antioxidants, antistatic agents, ultraviolet absorbers, stabilizers, magnetic powders, alignment promoters, plasticizers, crosslinkers, magnetic materials, pharmaceuticals, pesticides, fragrances, adhesives, enzymes, pigments, dyes, deodorants, metals, metal oxides, inorganic oxides, etc. may be mentioned.

[0050] The type and crystal structure of cellulose that can be used as the raw material for the fine cellulose 1 are not particularly limited. Specifically, as the raw material consisting of cellulose type I crystals, for example, in addition to wood-based natural cellulose, non-wood-based natural cellulose such as cotton linter, bamboo, hemp, bagasse, kenaf, bacterial cellulose, sea squirt cellulose, and valonia cellulose can be used. Furthermore, regenerated cellulose represented by rayon fiber and cupra fiber consisting of cellulose type II crystals can also be used. In view of ease of material procurement, it is preferable to use wood-based natural cellulose as the raw material. The wood-based natural cellulose is not particularly limited, and can be one that is generally used in the production of cellulose nanofibers, such as softwood pulp, hardwood pulp, and waste paper pulp. Softwood pulp is preferable in view of ease of purification and fineness.

[0051] Furthermore, it is preferable that the fine cellulose raw material is chemically modified. More specifically, it is preferable that anionic functional groups are introduced to the crystal surfaces of the fine cellulose raw material. This is because the introduction of anionic functional groups to the cellulose crystal surfaces makes it easier for the solvent to penetrate between the cellulose crystals due to the osmotic pressure effect, and the fine cellulose raw material is more likely to proceed.

[0052] The type and method of the anionic functional group to be introduced onto the crystal surface of the cellulose are not particularly limited, but a carboxy group, a phosphate group, a sulfate group, or a derivative thereof is preferred.

[0053] The method of introducing carboxyl groups to the fiber surface of cellulose is not particularly limited. Specifically, for example, carboxymethylation may be performed by reacting cellulose with monochloroacetic acid or sodium monochloroacetate in a high-concentration aqueous alkali solution. Alternatively, carboxyl groups may be introduced by directly reacting cellulose with a carboxylic anhydride compound such as maleic acid or phthalic acid gasified in an autoclave. Furthermore, a method using a co-oxidant in the presence of an N-oxyl compound such as TEMPO, which has high selectivity for the oxidation of alcoholic primary carbon, while maintaining the structure as much as possible under relatively mild aqueous conditions, may be used. Oxidation using an N-oxyl compound is more preferable for selectivity of the carboxyl group introduction site and reduction of environmental load.

[0054] Here, examples of the N-oxyl compound include TEMPO (2,2,6,6-tetramethylpiperidinyl-1-oxy radical), 2,2,6,6-tetramethyl-4-hydroxypiperidine-1-oxyl, 4-methoxy-2,2,6,6-tetramethylpiperidine-N-oxyl, 4-ethoxy-2,2,6,6-tetramethylpiperidine-N-oxyl, and 4-acetamido-2,2,6,6-tetramethylpiperidine-N-oxyl. Among these, TEMPO, which has high reactivity, is preferred. The amount of the N-oxyl compound used may be the amount used as a catalyst, and is not particularly limited. Usually, it is about 0.01 to 5.0% by mass based on the solid content of the wood-based natural cellulose to be oxidized.

[0055] An example of an oxidation method using an N-oxyl compound is a method in which wood-based natural cellulose is dispersed in water and oxidized in the presence of an N-oxyl compound. In this case, it is preferable to use a co-oxidizing agent together with the N-oxyl compound. In this case, the N-oxyl compound is sequentially oxidized by the co-oxidizing agent in the reaction system to generate an oxoammonium salt, and the cellulose is oxidized by the oxoammonium salt. This oxidation treatment allows the oxidation reaction to proceed smoothly even under mild conditions, improving the efficiency of introducing a carboxyl group. When the oxidation treatment is performed under mild conditions, the crystal structure of cellulose is easily maintained.

[0056] As the co-oxidizing agent, any oxidizing agent can be used as long as it can promote the oxidation reaction, such as halogen, hypohalous acid, halo-ous acid, perhalogen acid, or their salts, halogen oxide, nitrogen oxide, peroxide, etc. Sodium hypochlorite is preferred in view of availability and reactivity. The amount of the co-oxidizing agent used is not particularly limited, and may be an amount that can promote the oxidation reaction. Usually, it is about 1 to 200 mass% based on the solid content of the wood-based natural cellulose to be oxidized.

[0057] In addition, at least one compound selected from the group consisting of bromides and iodides may be used in combination with the N-oxyl compound and the co-oxidizing agent. This allows the oxidation reaction to proceed smoothly, and improves the efficiency of introducing a carboxyl group. As such a compound, sodium bromide or lithium bromide is preferred, and sodium bromide is more preferred in terms of cost and stability. The amount of the compound used is not particularly limited, and may be an amount that can promote the oxidation reaction. Usually, it is about 1 to 50% by mass based on the solid content of the wood-based natural cellulose to be oxidized.

[0058] The reaction temperature of the oxidation reaction is preferably 4 to 80° C., more preferably 10 to 70° C. If it is less than 4° C., the reactivity of the reagent decreases and the reaction time becomes longer. If it is more than 80° C., side reactions are promoted, the sample becomes low molecular weight, and the highly crystalline rigid fine cellulose fiber structure collapses, making it impossible to use it as a stabilizer for O / W type emulsions.

[0059] The reaction time for the oxidation treatment can be appropriately set in consideration of the reaction temperature, the desired amount of carboxy groups, etc., and is not particularly limited, but is usually about 10 minutes to 5 hours.

[0060] The pH of the reaction system during the oxidation reaction is not particularly limited, but is preferably 9 to 11. When the pH is 9 or more, the reaction can proceed efficiently. When the pH exceeds 11, a side reaction may proceed, which may accelerate the decomposition of the sample. In addition, in the oxidation treatment, as the oxidation proceeds, carboxyl groups are generated, which lowers the pH in the system, so it is preferable to keep the pH of the reaction system at 9 to 11 during the oxidation treatment. As a method for keeping the pH of the reaction system at 9 to 11, a method of adding an alkaline aqueous solution in response to the decrease in pH can be mentioned.

[0061] Examples of the aqueous alkali solution include organic alkali solutions such as an aqueous sodium hydroxide solution, an aqueous lithium hydroxide solution, an aqueous potassium hydroxide solution, an aqueous ammonia solution, an aqueous tetramethylammonium hydroxide solution, an aqueous tetraethylammonium hydroxide solution, an aqueous tetrabutylammonium hydroxide solution, and an aqueous benzyltrimethylammonium hydroxide solution. In terms of cost, an aqueous sodium hydroxide solution is preferred.

[0062] The oxidation reaction by the N-oxyl compound can be stopped by adding an alcohol to the reaction system. In this case, it is preferable to keep the pH of the reaction system within the above range. As the alcohol to be added, low molecular weight alcohols such as methanol, ethanol, and propanol are preferable in order to quickly terminate the reaction, and ethanol is particularly preferable in view of the safety of by-products generated by the reaction.

[0063] The reaction solution after the oxidation treatment may be directly subjected to the microparticulation step, but it is preferable to recover the oxidized cellulose contained in the reaction solution and wash it with a washing solution in order to remove catalysts such as N-oxyl compounds, impurities, etc. The recovery of the oxidized cellulose can be carried out by a known method such as filtration using a glass filter or a nylon mesh with a pore size of 20 μm. Pure water is preferable as the washing solution used to wash the oxidized cellulose.

[0064] When the obtained TEMPO-oxidized cellulose is subjected to defibration treatment, cellulose single nanofibers (CSNF) with a uniform fiber width of 3 nm are obtained. When CSNF is used as the raw material for the micronized cellulose 1 of the composite particle 5, the particle size of the obtained O / W type emulsion tends to be uniform due to its uniform structure.

[0065] The method of introducing phosphate groups onto the fiber surface of cellulose is not particularly limited. For example, it is preferable to disperse wood-based natural cellulose in water, mix it with a phosphoric acid or a phosphoric acid compound of its derivatives, and a urea compound containing urea or a derivative thereof, and heat it while treating it. Examples of phosphoric acid compounds include, but are not limited to, phosphoric acid or a salt thereof, dehydrated condensed phosphoric acid or a salt thereof, and phosphoric anhydride. Examples of urea compounds include urea and its derivatives, and include urea, biuret, 1-methylurea, 1-ethylurea, 1-phenylurea, and 1-benzylurea. The treatment temperature is preferably 50°C or higher and 300°C or lower, and more preferably 130°C or higher and 200°C or lower, as a temperature at which phosphoric acid groups can be efficiently introduced. The treatment time can be appropriately set in consideration of the reaction temperature, the desired amount of phosphoric acid groups, and the like, and is not particularly limited, but is usually in the range of 1 second to 1000 seconds. The treatment may be repeated multiple times.

[0066] After the treatment, in order to remove impurities, it is preferable to recover the cellulose contained in the reaction solution and wash it with a washing solution. The recovery of the cellulose can be carried out by a known method such as filtration using a glass filter or a nylon mesh with a pore size of 20 μm. Pure water is preferable as a washing solution used for washing the cellulose. Next, a water suspension of cellulose is prepared, and the pH is adjusted to about 12 using an aqueous sodium hydroxide solution, and the suspension is repeatedly filtered and dehydrated to obtain cellulose with a phosphate group introduced therein.

[0067] The obtained cellulose is subjected to a defibration treatment in a dispersion medium to obtain a dispersion of nanofibered cellulose.

[0068] The method for introducing sulfate groups onto the fiber surface of cellulose is not particularly limited. For example, a method is common in which wood-based natural cellulose is dispersed in water and treated with sulfuric acid while heating. The sulfuric acid concentration used may be adjusted to 4 mol / L to 18 mol / L. The treatment temperature is preferably 4 to 80°C, more preferably 10 to 50°C. The treatment time can be appropriately set in consideration of the reaction temperature, the desired amount of sulfate groups, etc., and is not particularly limited, but is usually in the range of 30 minutes to 3 hours.

[0069] After the treatment, in order to remove impurities, it is preferable to recover the cellulose contained in the reaction solution and wash it with a washing solution. The recovery of the cellulose can be carried out by a known method such as filtration using a glass filter or a nylon mesh with a pore size of 20 μm. Pure water is preferable as a washing solution used for washing the cellulose. Next, a water suspension of cellulose is prepared, and the pH is adjusted to about 12 using an aqueous sodium hydroxide solution, and the suspension is repeatedly filtered and dehydrated to obtain cellulose with sulfate groups introduced therein.

[0070] When the obtained cellulose is subjected to a defibration process, the amorphous parts are removed and short fibers are obtained as cellulose nanocrystals (CNC).

[0071] As described above, the CSNF and fine cellulose used in this embodiment can be obtained by a process of chemically treating the cellulose raw material and a process of mechanically finely pulverizing and dispersing. The amount of anionic functional groups in the fine cellulose obtained by the above method is preferably 0.1 mmol / g or more and 5.0 mmol / g or less per dry weight of the fine cellulose. Here, if the amount of carboxyl groups is less than 0.1 mmol / g, the solvent does not penetrate between the cellulose microfibrils due to the osmotic pressure effect, so it is difficult to finely pulverize the cellulose and disperse it uniformly. If the amount of carboxyl groups exceeds 5.0 mmol / g, the cellulose microfibrils are depolymerized due to side reactions accompanying the chemical treatment, so that a highly crystalline rigid fine cellulose fiber structure cannot be obtained, and the cellulose cannot be used as a stabilizer for O / W type emulsions.

[0072] (2nd process) The second step is a step of coating the surfaces of the liquid core particle precursors 2 with the fine cellulose 1 in a dispersion of the fine cellulose, thereby stabilizing the core particle precursors as an emulsion.

[0073] Specifically, this is a process in which a liquid core particle precursor is added to the micronized cellulose dispersion obtained in the first step, the liquid core particle precursor is dispersed in the micronized cellulose dispersion as droplets 2, and the surface of the liquid core particle precursor is coated with micronized cellulose 1 to produce an O / W type emulsion stabilized by the micronized cellulose 1.

[0074] The method for producing the O / W emulsion is not particularly limited, and may be a general emulsification treatment, such as various homogenizer treatments or mechanical stirring treatments, and specific examples of such mechanical treatments include high-pressure homogenizers, ultra-high-pressure homogenizers, universal homogenizers, ball mills, roll mills, cutter mills, planetary mills, jet mills, attritors, grinders, juicer mixers, homomixers, ultrasonic homogenizers, nanogenizers, underwater counter-impingement, paint shakers, etc. A combination of multiple mechanical treatments may also be used.

[0075] For example, when an ultrasonic homogenizer is used, the core particle precursor is added to the fine cellulose dispersion obtained in the first step to prepare a mixed solvent, and the tip of the ultrasonic homogenizer is inserted into the mixed solvent to perform ultrasonic treatment. The treatment conditions for the ultrasonic homogenizer are not particularly limited, but for example, a frequency of 20 kHz or more is generally used, and an output of 10 W / cm 2 The above is typical. There is no particular restriction on the treatment time, but it is usually about 10 seconds to 1 hour.

[0076] The ultrasonic treatment described above disperses the liquid core particle precursor in the fine cellulose dispersion, and emulsification proceeds. Furthermore, fine cellulose 1 is selectively adsorbed to the liquid / liquid interface between droplet 2 and the fine cellulose dispersion, and droplet 2 is coated with fine cellulose 1 to form a stable structure as an O / W type emulsion. An emulsion stabilized by the adsorption of a solid substance to the liquid / liquid interface in this way is academically called a "Pickering emulsion." As mentioned above, the mechanism by which Pickering emulsion is formed by fine cellulose fibers is unclear, but cellulose exhibits amphiphilicity due to its molecular structure having hydrophilic sites derived from hydroxyl groups and hydrophobic sites derived from hydrocarbon groups, and it is considered that cellulose is adsorbed to the liquid / liquid interface between the hydrophobic monomer and the hydrophilic solvent due to its amphiphilicity.

[0077] The fine cellulose 1 contains at least fine cellulose 1A and fine cellulose 1B. The fine cellulose 1 may be in a state in which fine cellulose 1A and fine cellulose 1B are mixed before emulsification, or fine cellulose 1A and a core particle precursor may be emulsified in advance, and then fine cellulose 1B may be added and further emulsified, or the order of mixing fine cellulose 1A and fine cellulose 1B may be reversed.

[0078] The O / W emulsion structure can be confirmed by observation with an optical microscope. The particle size of the O / W emulsion is not particularly limited, but is usually about 0.1 μm to 1000 μm.

[0079] In the O / W emulsion structure, the thickness of the fine cellulose layer formed on the surface of the droplet 2 is not particularly limited, but is usually about 3 nm to 1000 nm. The thickness of the fine cellulose layer can be measured, for example, using a cryo-TEM.

[0080] The type of liquid core particle precursor that can be used in the second step is not particularly limited as long as it is incompatible with water and is (1) a monomer having a polymerizable functional group that can form a solid polymer by a polymerization reaction, or (2) a thermoplastic polymer that melts into a liquid state when heated and undergoes a phase transition to become a solid at room temperature, or (3) a non-curable polymer that dissolves or disperses in a solvent into a liquid state and becomes a solid at room temperature when the solvent is removed.

[0081] In (1), the polymerizable monomer has at least one polymerizable functional group. A polymerizable monomer having one polymerizable functional group is also called a monofunctional monomer. A polymerizable monomer having two or more polymerizable functional groups is also called a polyfunctional monomer. The type of polymerizable monomer is not particularly limited, and examples thereof include (meth)acrylic monomers and vinyl monomers. It is also possible to use polymerizable monomers having an epoxy group or a cyclic ether structure such as an oxetane structure (e.g., ε-caprolactone, etc.). The term "(meth)acrylate" includes both "acrylate" and "methacrylate".

[0082] Examples of monofunctional (meth)acrylic monomers include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, glycidyl (meth)acrylate, acryloylmorpholine, N-vinylpyrrolidone, tetrahydrofurfuryl acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and isobornyl (meth)acrylate. acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, benzyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, ethyl carbitol (meth)acrylate, phosphate (meth)acrylate, ethylene oxide modified phosphate (meth)acrylate, phenoxy (meth)acrylate, ethylene oxide modified phenoxy (meth)acrylate, propylene oxide modified fluorine Phenoxy (meth)acrylate, nonylphenol (meth)acrylate, ethylene oxide modified nonylphenol (meth)acrylate, propylene oxide modified nonylphenol (meth)acrylate, methoxydiethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, methoxypropylene glycol (meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxypropyl phthalate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxypropyl phthalate, diethyl hydrogen phthalate, 2-(meth)acryloyloxypropyl hydrogen phthalate, 2-(meth)acryloyloxypropyl hexahydrohydrogen phthalate, 2-(meth)acryloyloxypropyl tetrahydrohydrogen phthalate, dimethylaminoethyl (meth)acrylate, trifluoroethyl (meth)acrylate, tetrafluoropropyl (meth)acrylate, hexafluoropropyl (meth)acrylate, octafluoropropyl (meth)acrylate, octafluoropropyl (meth)acrylate,Examples of the mono(meth)acrylate include adamantane derivative mono(meth)acrylates such as adamantyl acrylate having a monovalent mono(meth)acrylate derived from 2-adamantane and adamantanediol.

[0083] Examples of bifunctional (meth)acrylic monomers include di(meth)acrylates such as ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, hexanediol di(meth)acrylate, nonanediol di(meth)acrylate, ethoxylated hexanediol di(meth)acrylate, propoxylated hexanediol di(meth)acrylate, diethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, ethoxylated neopentyl glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, and hydroxypivalic acid neopentyl glycol di(meth)acrylate.

[0084] Examples of the trifunctional or higher (meth)acrylic monomer include tri(meth)acrylates such as trimethylolpropane tri(meth)acrylate, ethoxylated trimethylolpropane tri(meth)acrylate, propoxylated trimethylolpropane tri(meth)acrylate, tris(2-hydroxyethylisocyanurate tri(meth)acrylate, and glycerin tri(meth)acrylate; trifunctional (meth)acrylate compounds such as pentaerythritol tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, and ditrimethylolpropane tri(meth)acrylate. Examples of the (meth)acrylate include polyfunctional (meth)acrylate compounds having three or more functional groups, such as pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, ditrimethylolpropane penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and ditrimethylolpropane hexa(meth)acrylate, as well as polyfunctional (meth)acrylate compounds in which a portion of these (meth)acrylates is substituted with an alkyl group or ε-caprolactone.

[0085] As the monofunctional vinyl monomer, for example, a vinyl ether type, a vinyl ester type, an aromatic vinyl type, particularly styrene and a styrene type monomer, etc., which are liquids that are incompatible with water at room temperature, are preferable. Examples of the (meth)acrylate among the monofunctional vinyl monomers include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, alkyl (meth)acrylate, tridecyl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl (meth)acrylate, benzyl (meth)acrylate, isobornyl (meth)acrylate, glycidyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, allyl (meth)acrylate, diethylaminoethyl (meth)acrylate, trifluoroethyl (meth)acrylate, heptafluorodecyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, and tricyclodecanyl (meth)acrylate. Examples of monofunctional aromatic vinyl monomers include styrene, α-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, ethylstyrene, isopropenyltoluene, isobutyltoluene, tert-butylstyrene, vinylnaphthalene, vinylbiphenyl, and 1,1-diphenylethylene.

[0086] The polyfunctional vinyl monomer may be a polyfunctional monomer having an unsaturated bond such as divinylbenzene, etc. A liquid that is incompatible with water at room temperature is preferred. Specific examples of polyfunctional vinyl monomers include: (1) divinyls such as divinylbenzene, 1,2,4-trivinylbenzene, and 1,3,5-trivinylbenzene; (2) dimethacrylates such as ethylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, polyethylene glycol dimethacrylate, 1,3-propylene glycol dimethacrylate, 1,4-butylene glycol dimethacrylate, 1,6-hexamethylene glycol dimethacrylate, neopentyl glycol dimethacrylate, dipropylene glycol dimethacrylate, polypropylene glycol dimethacrylate, and 2,2-bis(4-methacryloxydiethoxyphenyl)propane; (3) trimethacrylates such as trimethylolpropane trimethacrylate and triethylolethane trimethacrylate; (4) ethylene glycol diacrylate, diethylene glycol dimethacrylate, and diethylene glycol dimethacrylate; diacrylates such as aryl diacrylate, triethylene glycol diacrylate, polyethylene glycol diacrylate, 1,3-dipropylene glycol diacrylate, 1,4-dibutylene glycol diacrylate, 1,6-hexylene glycol diacrylate, neopentyl glycol diacrylate, dipropylene glycol diacrylate, polypropylene glycol diacrylate, 2,2-bis(4-acryloxypropoxyphenyl)propane, 2,2-bis(4-acryloxydiethoxyphenyl)propane, (5) triacrylates such as trimethylolpropane triacrylate, triethylolethane triacrylate, (6) tetraacrylates such as tetramethylolmethane tetraacrylate, and (7) others, for example, tetramethylene bis(ethyl fumarate), hexamethylene bis(acrylamide), triallyl cyanurate, and triallyl isocyanurate. For example, specific examples of functional styrene monomers include divinylbenzene, trivinylbenzene, divinyltoluene, divinylnaphthalene, divinylxylene, divinylbiphenyl, bis(vinylphenyl)methane, bis(vinylphenyl)ethane, bis(vinylphenyl)propane, and bis(vinylphenyl)butane.

[0087] In addition to these, polyether resins, polyester resins, polyurethane resins, epoxy resins, alkyd resins, spiroacetal resins, polybutadiene resins, polythiolpolyene resins, and the like having at least one polymerizable functional group can also be used, and the material is not particularly limited.

[0088] The above polymerizable monomers may be used alone or in combination of two or more kinds.

[0089] (2) The thermoplastic polymer preferably has a melting point of 40°C or more and 85°C or less. If the melting point is lower than 40°C, it is difficult to maintain the shape as a solid at room temperature, and the use environment is extremely limited, which is not preferable. On the other hand, if the melting point exceeds 85°C, it is difficult to maintain the molten state in the microfibrillated cellulose dispersion in the manufacturing process, which is not preferable. More preferably, the melting point is 45°C or more and 75°C or less. In addition, it is preferable that the melt flow index at or above the melting point is 10 or more. If it is less than 10, it is not preferable because a large amount of emulsification energy is required in the above-mentioned emulsification treatment.

[0090] (3) The non-curable polymer dissolves in a solvent other than water and assumes a liquid state. Here, the solvent for dissolving the non-curable polymer preferably has a water solubility of 20 g or more and 2000 g or less per 1 L of water at 20°C. Examples of the solvent for dissolving the non-curable polymer include ethyl acetate, acetylacetone, cyclohexanone, and benzyl alcohol. If it is less than 20 g, the affinity between the droplets containing the solvent and the CNF is low, and the emulsion stabilization effect of the CNF decreases. On the other hand, if it is more than 2000 g, the diffusion speed of the solvent in the CNF dispersion is so fast that the droplets cannot be maintained, and the droplet covering effect of the CNF is impaired.

[0091] The materials for the thermoplastic polymer (2) and the non-curable polymer (3) above are not limited as long as the function of this embodiment is not impaired. Examples of the materials that can be used include the monofunctional monomers described above, polymers made from polymerizable monomers having a cyclic ether structure such as an epoxy group or an oxetane structure as a starting material, cellulose-based resins (e.g., cellulose acetate, cellulose propionate, cellulose butyrate, etc.) produced by chemically modifying natural polysaccharides such as cellulose, polyether resins, polyester resins, polyurethane resins, epoxy resins, alkyd resins, spiroacetal resins, polybutadiene resins, polythiolpolyene resins, etc.

[0092] The weight ratio of the microfibrillated cellulose fiber dispersion and the liquid core particle precursor that can be used in the second step is not particularly limited, but it is preferable that the liquid core particle precursor is 1 part by mass or more and 50 parts by mass or less per 100 parts by mass of the microfibrillated cellulose fiber dispersion. If the liquid core particle precursor is 1 part by mass or less, the yield of the composite particles 5 decreases, which is not preferable, and if it exceeds 50 parts by mass, it becomes difficult to uniformly coat the droplets 2 with the microfibrillated cellulose 1, which is also not preferable.

[0093] In addition, when a polymerizable monomer is used as a liquid core particle precursor, a polymerization initiator may be included in advance. Typical polymerization initiators include radical initiators such as organic peroxides and azo polymerization initiators.

[0094] Examples of the organic peroxide include peroxyketals, hydroperoxides, dialkyl peroxides, diacyl peroxides, peroxycarbonates, and peroxyesters.

[0095] Examples of the azo polymerization initiator include ADVN and AIBN. For example, 2,2-azobis(isobutyronitrile) (AIBN), 2,2-azobis(2-methylbutyronitrile) (AMBN), 2,2-azobis(2,4-dimethylvaleronitrile) (ADVN), 1,1-azobis(1-cyclohexanecarbonitrile) (ACHN), dimethyl-2,2-azobisisobutyrate (MAIB), 4,4-azobis(4-cyanovaleric acid) (ACVA), 1,1-azobis(1-acetoxy-1-phenylethane), 2,2-azobis(2-methylbutyramide), 2,2-azobis(4- Methoxy-2,4-dimethylvaleronitrile), 2,2-azobis(2-methylamidinopropane) dihydrochloride, 2,2-azobis[2-(2-imidazolin-2-yl)propane], 2,2-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], 2,2-azobis(2,4,4-trimethylpentane), 2-cyano-2-propylazoformamide, 2,2-azobis(N-butyl-2-methylpropionamide), 2,2-azobis(N-cyclohexyl-2-methylpropionamide), and the like.

[0096] If a polymerizable monomer that already contains a polymerization initiator is used in the second step, the polymerization initiator will be contained in the polymerizable monomer droplets 2 inside the emulsion particles when the O / W type emulsion is formed, and this makes it easier for the polymerization reaction to proceed when the monomer inside the emulsion is polymerized in the third step described below.

[0097] The weight ratio of the polymerizable monomer and the polymerization initiator that can be used in the second step is not particularly limited, but it is usually preferable that the amount of the polymerization initiator is 0.1 part by mass or more per 100 parts by mass of the polymerizable monomer. If the amount of the polymerizable monomer is less than 0.1 part by mass, the polymerization reaction does not proceed sufficiently, and the yield of the composite particles 5 decreases, which is not preferable.

[0098] The polymerizable monomer may contain functional components other than the polymerization initiator in advance. Specific examples include magnetic materials, pharmaceuticals, agricultural chemicals, fragrances, adhesives, enzymes, pigments, dyes, deodorants, metals, metal oxides, inorganic oxides, and the like. When the polymerizable monomer contains functional components other than the polymerization initiator in advance, the above-mentioned functional components can be contained inside the particles when formed into composite particles 5, making it possible to express functions according to the application.

[0099] (3rd step) The third step is a step of solidifying the liquid core particle precursor (droplets) 2 to obtain composite particles 5 in which core particles 3 are coated with pulverized cellulose 1.

[0100] When a polymerizable monomer is used, the polymerization method is not particularly limited and can be appropriately selected depending on the type of polymerizable monomer and the type of polymerization initiator used. For example, a suspension polymerization method can be used.

[0101] The specific suspension polymerization method is not particularly limited, and can be carried out using a known method. For example, the suspension polymerization can be carried out by heating while stirring the O / W type emulsion in which the monomer droplets 2 containing the polymerization initiator are coated with the fine cellulose 1 and stabilized, which is prepared in the second step. The stirring method is not particularly limited, and a known method can be used, and specifically, a disperser or a stirrer can be used. Also, only the heat treatment can be performed without stirring. The temperature conditions during heating can be appropriately set depending on the type of polymerizable monomer and the type of polymerization initiator, but it is preferably 20 degrees or more and 150 degrees or less. If it is less than 20 degrees, the polymerization reaction rate decreases, which is not preferable, and if it exceeds 150 degrees, the fine cellulose 1 may be denatured, which is not preferable. The time for the polymerization reaction can be appropriately set depending on the type of polymerizable monomer and the type of polymerization initiator, but is usually about 1 hour to 24 hours. The polymerization reaction may be performed by irradiation with ultraviolet light, which is a type of electromagnetic wave. In addition to electromagnetic waves, particle beams such as electron beams may be used.

[0102] When a thermoplastic polymer is used, the polymer melted by heating is solidified by undergoing a phase transition. A cooling method can be used as a method for the phase transition. At this time, the crystallinity of the thermoplastic polymer can be controlled by controlling the cooling rate. The cooling method can be a method of diffusing the polymer in water or ice water, a method of contacting the polymer with a refrigerant such as liquid nitrogen, or a method of allowing the polymer to cool naturally.

[0103] When a non-curable polymer is used, the polymer is solidified by removing the solvent. The method for removing the solvent is not particularly limited, and may be a method of heating, a method of reducing pressure, a method of dissolving only the solvent, a method of irradiating with electromagnetic waves, or a combination of these methods.

[0104] Through the above-mentioned steps, a spherical composite particle 5 in which the core particle 3 is covered with the micronized cellulose 1 can be produced.

[0105] In addition, immediately after solidification, the dispersion of the composite particles 5 contains a large amount of water and free micronized cellulose 1 that does not contribute to the formation of the coating layer of the composite particles 5. Therefore, it is necessary to recover and purify the prepared composite particles 5, and the recovery and purification method is preferably washing by centrifugation or washing by filtration. As a method for washing by centrifugation, a known method can be used. Specifically, the composite particles 5 are precipitated by centrifugation, the supernatant is removed, and the composite particles 5 can be recovered by repeating the operation of redispersing the composite particles 5 in a water-methanol mixed solvent, and finally removing the residual solvent from the precipitate obtained by centrifugation. A known method can also be used for filtration and washing. For example, a PTFE membrane filter with a pore size of 0.1 μm is used to repeatedly perform suction filtration with water and methanol, and finally, the composite particles 5 can be recovered by further removing the residual solvent from the paste remaining on the membrane filter.

[0106] The method for removing the residual solvent is not particularly limited, and can be performed by air drying or heat drying in an oven. The dried solid material containing the composite particles 5 thus obtained is obtained as a finely textured powder without being in the form of a film or aggregate as described above.

[0107] (Effects of the Invention) According to the composite particle 5 of this embodiment, it is possible to provide powdery fine particles in which the micronized cellulose is stably bonded to the core particle 3 at a high density and firmly.

[0108] According to the method for producing the composite particle 5 according to the present embodiment, it is possible to provide a novel method for producing the composite particle 5, which has a low environmental impact and can be provided in a simple manner. The dry solid containing the composite of the micronized cellulose 1 can be provided in a form that can be redispersed in a solvent.

[0109] According to the composite particle 5 of this embodiment, since it is possible to remove almost all of the solvent, it is expected to have the following effects: reduced transportation costs, reduced risk of spoilage, improved efficiency of addition as an additive, and improved efficiency of kneading into hydrophobic resins.

[0110] Although one embodiment of the present invention has been described in detail above with reference to the drawings, the specific configuration is not limited to this embodiment, and design modifications and the like that do not depart from the gist of the present invention are also included. Also, the components shown in the above embodiment and modified examples can be appropriately combined to form a configuration. EXAMPLES

[0111] The present invention will be described in detail below with reference to examples, but the technical scope of the present invention is not limited to these examples. In each of the following examples, "%" indicates % by weight unless otherwise specified.

[0112] <Example 1> (Step 1: Step of obtaining cellulose nanofiber dispersion) (TEMPO oxidation of wood cellulose) 70g of softwood kraft pulp was suspended in 3500g of distilled water, and a solution of 0.7g of TEMPO and 7g of sodium bromide dissolved in 350g of distilled water was added, and the mixture was cooled to 20℃. 450g of 2mol / L sodium hypochlorite aqueous solution with a density of 1.15g / mL was added dropwise to start the oxidation reaction. The temperature in the system was always kept at 20℃, and the pH was maintained at 10 by adding 0.5N sodium hydroxide aqueous solution to prevent a decrease in pH during the reaction. When the total amount of sodium hydroxide added relative to the weight of cellulose reached 3.50mmol / g, about 100mL of ethanol was added to stop the reaction. After that, filtration and washing with distilled water were repeated using a glass filter to obtain oxidized pulp. The obtained oxidized pulp was added to a hydrogen chloride aqueous solution adjusted to pH 2, dehydrated, washed with water, and then added to a hydrogen chloride aqueous solution adjusted to pH 3. After that, dehydration and washing were repeated to obtain a purified oxidized pulp.

[0113] (Measurement of carboxyl group content of oxidized pulp) The oxidized pulp and reoxidized pulp obtained by the above TEMPO oxidation were weighed out in solid weight of 0.1 g, dispersed in water at 1% concentration, and adjusted to pH 2.5 by adding hydrochloric acid. The amount of carboxyl groups (mmol / g) was then determined by conductometric titration using 0.5 M sodium hydroxide solution. The result was 1.6 mmol / g.

[0114] (Oxidized pulp defibration treatment) The oxidized pulp obtained by the above method was dispersed in distilled water and refined in a juicer mixer for 120 minutes to obtain CNF dispersion NC-1 with a CNF concentration of 0.5% (see Table 1). Similarly, oxidized pulp prepared was used and refined in a juicer mixer for 30 minutes to obtain CNF dispersion NC-2 with a CNF concentration of 0.5% (see Table 1). CNF dispersions NC-1 and NC-2 were treated with a centrifugal defoamer for defoaming as necessary. The obtained CNF dispersions NC-1 and NC-2 showed high transparency. In addition, CNF dispersions NC-1 and NC-2 showed thixotropy. The obtained CNF dispersions NC-1 and NC-2 were mixed.

[0115] (Second step: Preparation of O / W type emulsion) Next, cellulose acetate propionate (hereinafter also referred to as CAP), a non-curable polymer, was used as a core particle precursor, and CAP was dissolved in ethyl acetate to a concentration of 20%, to prepare a CAP / ethyl acetate solution as a core particle precursor. A CNF / ethyl acetate solution and a CAP / ethyl acetate solution were added to a CNF concentration of 0.5% in which a saturated amount of ethyl acetate had been dissolved in advance, so that the solid weight ratio of the resin (CAP) to the CNF in each solution was 10:1, and the two liquids separated into two layers with high transparency.

[0116] Next, the shaft of an ultrasonic homogenizer was inserted from the liquid surface of the upper layer of the mixed liquid in the state of being separated into two layers, and ultrasonic homogenization was performed for 3 minutes under the conditions of a frequency of 24 kHz and an output of 400 W. The appearance of the mixed liquid after ultrasonic homogenization was a cloudy emulsion. When a drop of the mixed liquid was dropped onto a slide glass, sealed with a cover glass, and observed under an optical microscope, it was confirmed that countless emulsion droplets of about 1 to several μm were generated and the dispersion was stabilized as an O / W type emulsion.

[0117] (Third step: A step of obtaining composite particles 5 coated with CNF by solidifying the core particle precursor) The O / W emulsion dispersion was poured into 10 times the amount of pure water, and ethyl acetate was dissolved from the CAP solution to solidify the CAP. The resulting dispersion was centrifuged at 75,000g for 5 minutes to obtain a precipitate. The supernatant was removed by decantation to collect the precipitate, which was then repeatedly washed with pure water using a PTFE membrane filter with a pore size of 0.01μm. The purified and collected material was redispersed at a concentration of 1%, and the particle size was evaluated using a particle size distribution analyzer (NANOTRAC UPA-EX150, Nikkiso Co., Ltd.), giving an average particle size of 0.4μm. The purified and collected material was then air-dried and further vacuum-dried at room temperature of 25°C for 24 hours to obtain a finely textured dry powder (composite particle 5).

[0118] (Shape observation using a scanning electron microscope) The results of observing the obtained dry powder with a scanning electron microscope are shown in Figures 2 and 3. As is clear from Figure 2, it was confirmed that countless spherical composite particles 5 were formed, which were derived from the shape of the emulsion droplets, by carrying out solidification using the O / W emulsion droplets as a template, and further, as shown in Figure 3, it was confirmed that the surface was uniformly covered with CNFs having a width of several nm. In addition, despite repeated washing by filtration and washing, the surface of the composite particles 5 was equally and uniformly covered with CNFs, indicating that in the composite particles 5 of the present invention, the monomers and CNFs inside the composite particles are in a bonded state.

[0119] <Examples 2, 3, and 4> (Step 1: Step of obtaining cellulose nanofiber dispersion) According to Non-Patent Document 1, chemically treated pulp obtained by phosphorylating softwood kraft pulp was subjected to defibration treatment to prepare CNF dispersion NC-3 (see Table 1).

[0120] In addition, softwood kraft pulp was treated with 8 mol / L sulfuric acid at 40°C for 1 hour to obtain chemically treated pulp, which was then defibrated to produce CNF dispersion NC-4 (see Table 1). When the dried powder of the obtained CNF dispersion NC-4 was observed with a scanning electron microscope, it was confirmed that the length was 100 to 400 nm, and that CNCs with shorter lengths in the major axis direction had been prepared compared to the CNFs in the CNF dispersions NC-1, NC-2, NC-3, and NC-5.

[0121] In the above-mentioned TEMPO oxidation treatment, the treatment was stopped when the total amount of sodium hydroxide added reached 1.0 mmol / g. The resulting TEMPO oxidized pulp was then subjected to a defibration treatment to produce CNF dispersion NC-5 (see Table 1).

[0122] Composite particle 5 was produced under the same conditions as in Example 1, except that the type and mixing ratio of the cellulose nanofiber dispersion were changed as shown in Table 2.

[0123] <Example 5> Composite particle 5 was produced under the same conditions as in Example 1, except that instead of dispersing CAP dissolved in ethyl acetate as a core particle precursor and solidifying it by dissolving the ethyl acetate in the CAP, a 20% MEK solution of polycaprolactone (PCL, molecular weight 10,000, melting point 61°C) was used, emulsified in a CNF dispersion heated to 75°C, and then solidified by pouring it into ice water (see Table 2).

[0124] <Example 6> Composite particle 5 was produced under the same conditions as in Example 1, except that instead of dispersing CAP dissolved in ethyl acetate as the core particle precursor and dissolving the ethyl acetate to solidify it, divinylbenzene (hereinafter, referred to as DVB) and an initiator ADVN were used to perform a polymerization reaction at 70°C for 8 hours to solidify it (see Table 2).

[0125] <Comparative Examples 1, 2, and 3> As shown in Table 3, the mixing ratio of the CNF dispersion was changed, and composite particles were produced under the same conditions as in Example 1. <Comparative Example 4>

[0126] As shown in Table 3, the mixing ratio of the CNF dispersion was changed, and composite particles were produced under the same conditions as in Example 5. <Comparative Example 5>

[0127] As shown in Table 3, the mixing ratio of the CNF dispersion was changed, and composite particles were produced under the same conditions as in Example 6.

[0128] The compositions and evaluation results of the following Examples and Comparative Examples are shown in Tables 2 and 3. In Tables 2 and 3, the average particle size was determined by observing the composite particles obtained with a scanning electron microscope and measuring the particle size of 100 particles randomly selected. The evaluation of "peeling" was performed by observing the composite particles at a magnification of 50,000 times, with those in which peeling of the CNF layer on the particle surface was not observed being marked "good" and those in which peeling was observed being marked "bad." Furthermore, the amount of CNF adsorption was determined by treating the composite particles obtained with concentrated sulfuric acid to dissolve the cellulose on the particle surface, adding a phenol aqueous solution, and calculating the cellulose concentration from the absorbance at 490 nm using the phenol-sulfuric acid method, and then dividing the cellulose concentration by the dry weight of the composite particles.

[0129] [Table 1]

[0130] [Table 2]

[0131] [Table 3]

[0132] As is clear from the evaluation results of Examples 1 to 6 in Table 2 and Comparative Examples 1 to 5 in Table 3, composite particles 5 (Examples 1 to 6) made from finified cellulose 1 having two or more particle size peaks in the volumetric particle size range of 0.01 μm to 20 μm tend to have smaller particle sizes and larger amounts of CNF adsorbed. This is believed to be because, in the adsorption of CNF to the core particle precursor, the adsorption stabilization by finified cellulose 1B with a large particle size peak and the filling effect of CNF coating by finified cellulose 1A with a small particle size peak act synergistically.

[0133] When a non-curable resin or a thermoplastic resin was used for the composite particle 5 (Examples 1 to 5), the CNF layer on the surface of the composite particle was hardly peeled off by using the fine cellulose 1A with a small particle size peak in combination. This is considered to be because the fine cellulose 1A with a small particle size peak tightly binds to the core particle precursor, and the fine cellulose 1B with a large particle size peak becomes entangled therewith, exerting an anchor effect.

[0134] On the other hand, the results of observing the dry powder obtained in Comparative Example 1 with a scanning electron microscope are shown in Fig. 4. As shown in Fig. 4, it was confirmed that the surface of the composite particle was uniformly covered with CNFs having a width of several nm, but it was observed that some of the CNFs had turned up and peeled off from the core particle. [Industrial Applicability]

[0135] The composite particles of the present invention can be used for various applications due to the new handling characteristics, the new functionality imparted thereto, and the stable adsorption of finely divided cellulose to the core particles. [Explanation of symbols]

[0136] 1. Micronized cellulose 2 Droplets (core particle precursors) 3 Core Particles 4 CNF dispersion 5 Composite particles

Claims

1. At least one type of core particle is included, A finely divided cellulose having an anionic functional group is bound to the surface of the core particle, The microfibrillated cellulose has a volume-based particle size distribution having two or more particle size peaks, The particle size peak is in a volumetric particle size range of 0.01 μm or more and 20 μm or less, the core particle is obtained by polymerizing a polymerizable monomer having at least one polymerizable functional group, and the polymerizable monomer is a (meth)acrylic monomer or a vinyl monomer; composite particles.

2. A method for producing a polymeric material comprising the steps of: A finely divided cellulose having an anionic functional group is bound to the surface of the core particle, The microfibrillated cellulose has a volume-based particle size distribution having two or more particle size peaks, The particle size peak is in a volumetric particle size range of 0.01 μm or more and 20 μm or less, The core particles are non-curable, dissolve in a solvent other than water, and are in a liquid state. composite particles.

3. The volumetric particle size has one or more particle size peaks in the range of 0.01 μm or more and 1 μm or less, The volumetric particle size has one or more particle size peaks in the range of 1 μm or more and 20 μm or less. The composite particle according to claim 1 or 2.

4. The number average minor axis diameter of the pulverized cellulose is 1 nm or more and 50 nm or less. The composite particle according to any one of claims 1 to 3.

5. The core particle comprises at least one polymer. The composite particle according to any one of claims 1 to 4.

6. A first step of defibrating a cellulose raw material in a solvent to obtain a dispersion of finely divided cellulose having a volume-based particle size distribution with two or more particle size peaks in the volume-based particle size range of 0.01 μm or more and 20 μm or less; a second step of dispersing core particle precursors as droplets in a medium containing the dispersion liquid, coating the surfaces of the core particle precursors with the micronized cellulose, and stabilizing the core particle precursors as an emulsion; a third step of solidifying the droplets to obtain composite particles in which core particles are coated with the micronized cellulose; Equipped with the second step includes adding a polymerizable monomer containing a polymerization initiator to the dispersion liquid to form an emulsion, the polymerizable monomer being a (meth)acrylic monomer or a vinyl monomer; A method for producing composite particles.

7. The core particle precursor has thermoplasticity. The method for producing composite particles according to claim 6 .

8. The core particle precursor has non-curable properties. The method for producing the composite particle according to claim 6 or 7.

9. The core particle precursor is a droplet formed by dissolving or dispersing in a solvent having a water solubility at 20° C. of 20 g or more and 2000 g or less per 1 L of water. The method for producing composite particles according to claim 8 .

Citation Information

Patent Citations

  • Formation of pattern

    JP1984028339A

  • luminaire

    JP1985020454A

  • Compact

    JP2005096845A

  • Fine cellulose fiber

    JP2008001728A

  • Method for producing cellulose nanofiber

    JP2010216021A