Highly dielectric resin composition, carrier-attached resin film, prepreg, laminate, printed wiring board and semiconductor device each using the same
The high dielectric resin composition with epoxy resin and inorganic filler addresses the challenge of balancing dielectric constant and loss tangent, enhancing signal quality and enabling miniaturization in communication and semiconductor devices.
Patent Information
- Application Number
- JP2020095443
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-06-01
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-06-01
AI Technical Summary
Conventional high dielectric resin compositions struggle to achieve a balance between high dielectric constant and low dielectric loss tangent, particularly at higher frequencies, which is essential for reducing transmission loss and enabling miniaturization in communication and semiconductor devices.
A high dielectric resin composition comprising an epoxy resin and an inorganic filler with a dielectric constant of 6 or more, optimized to achieve a dielectric constant of 4 to 10 and a dielectric loss tangent of 0.003 to 0.015, enhancing adhesion to copper foil and supporting higher frequencies and smaller sizes.
The composition provides an excellent balance between high dielectric constant and low dielectric loss tangent, improving signal quality and enabling higher frequency and miniaturization in printed wiring boards and semiconductor devices.
Smart Images

Figure 0007581662000010 
Figure 0007581662000011 
Figure 0007581662000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a highly dielectric resin composition, and a resin film with a carrier, a prepreg, a laminate, a printed wiring board and a semiconductor device each using the same. [Background technology]
[0002] As communication information becomes larger and more diverse, communication speeds are increasing for printed circuit boards for communication base stations, server boards, router boards, etc. To accommodate the increased communication speeds, it is necessary to increase the frequency of signals.
[0003] Reducing transmission loss is important to ensure signal quality. Transmission loss is mainly classified as dielectric loss caused by resin and conductor loss caused by conductor. The former, dielectric loss, tends to decrease as the dielectric tangent of the resin becomes smaller. The latter, conductor loss, is caused by the fact that as the frequency increases, the cross-sectional area through which current flows decreases due to the skin effect (the phenomenon in which signals flow through a thickness of 1 to 2 μm from the surface of the conductor), and resistance increases.
[0004] On the other hand, it is known that a high dielectric constant has the advantage that the antenna shape can be made smaller. For example, Patent Document 1 discloses a resin composition containing an epoxy resin, a dielectric powder such as barium titanate, a nonionic surfactant, and a curing agent in order to obtain a high dielectric constant resin layer by suppressing the formation of agglomerates of the dielectric powder. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2017-14406 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, in recent years, the technical level required for various properties of high dielectric resin compositions has become increasingly higher. The present inventors focused on the development of a new material that realizes a high dielectric constant and a low dielectric tangent. As a result of intensive investigation, it was found that the conventional technology described in the above Patent Document 1 has room for improvement in terms of responding to high frequencies and miniaturization. [Means for solving the problem]
[0007] As a result of further investigation, the present inventors have found that in a high dielectric resin composition containing an epoxy resin (A) and an inorganic filler (B) having a dielectric constant (1 MHz) of 6 or more, by controlling the dielectric constant and dielectric dissipation factor as indicators, it is possible to achieve an excellent balance between a high dielectric constant and a low dielectric dissipation factor and to improve adhesion to copper foil, thereby realizing a higher level of high frequency and miniaturization than ever before.
[0008] According to the present invention, there is provided a high dielectric resin composition comprising an epoxy resin (A) and an inorganic filler (B) having a dielectric constant (1 MHz) of 6 or more, The present invention provides a highly dielectric resin composition, the cured product of which has a dielectric constant (Dk: εr) of 4 to 10 at 10 GHz, and a dielectric loss tangent (Df: tan δ) of 0.003 to 0.015 at 10 GHz.
[0009] According to the present invention, there is also provided a cured product of the above-mentioned highly dielectric resin composition.
[0010] According to the present invention, there is also provided a prepreg comprising the above-mentioned highly dielectric resin composition and a fibrous base material.
[0011] The present invention also provides a laminate comprising the prepreg and a metal layer disposed on at least one surface of the prepreg.
[0012] According to the present invention, there is also provided a resin film with a carrier, comprising a carrier base material and a resin film formed on the carrier base material and made of the above-mentioned high dielectric resin composition.
[0013] According to the present invention, there is also provided a printed wiring board comprising an insulating layer made of a cured product of the above-mentioned highly dielectric resin composition.
[0014] Further, according to the present invention, The printed wiring board; and a semiconductor element mounted on a circuit layer of the printed wiring board or embedded in the printed wiring board. Effect of the Invention
[0015] According to the present invention, there are provided a highly dielectric resin composition capable of realizing high frequency and miniaturization, and a resin film with a carrier, a prepreg, a laminate, a printed wiring board and a semiconductor device each using the same. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a diagram illustrating an example of a configuration of a substrate-attached resin sheet according to an embodiment of the present invention. [Diagram 2] 1A to 1C are cross-sectional views showing an example of a manufacturing process for the semiconductor device according to the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In all drawings, the same components are given the same reference numerals and the description will be omitted as appropriate. In addition, the drawings are schematic diagrams and do not correspond to the actual dimensional ratio. In addition, in this specification, the expression "a to b" in the explanation of a numerical range means from a to b, unless otherwise specified. For example, "1 to 5% by mass" means "1% by mass to 5% by mass."
[0018] In the present embodiment, the "cured product" of the high dielectric resin composition refers to a resin plate obtained by stacking a plurality of resin sheets and curing them in a vacuum press at a temperature of 225°C, a pressure of 0.5 MPa, and a curing time of 2 hours, for example, 100 mm square and 0.5 mm thick.
[0019] In this embodiment, the content of each component contained in the highly dielectric resin composition is the content (mass %) relative to 100 mass % of the solid content of the highly dielectric resin composition, unless otherwise specified.
[0020] <Highly dielectric resin composition> The high dielectric resin composition of the present embodiment contains an epoxy resin (A) and an inorganic filler (B) having a dielectric constant (1 MHz) of at least 6. The cured product of the high dielectric resin composition has a dielectric constant (Dk: εr) of 4 to 10 at 10 GHz, and a dielectric loss tangent (Df: tan δ) of 0.003 to 0.015 at 10 GHz. This provides an excellent balance between high dielectric constant and low dielectric tangent, while also improving adhesion to copper foil, enabling the realization of higher frequencies and smaller size than ever before.
[0021] [Dielectric constant / dielectric tangent] The dielectric constant (Dk: εr) at 10 GHz of the cured product of the high dielectric resin composition of this embodiment is 4-10, preferably 5-9, more preferably 6-8, and further preferably 6-7. By setting the dielectric constant to be equal to or greater than the lower limit, miniaturization becomes possible, whereas by setting the dielectric constant to be equal to or less than the upper limit, a good balance between high frequency and miniaturization can be maintained.
[0022] The dielectric loss tangent (Df: tan δ) at 10 GHz of the cured product of the high dielectric resin composition of this embodiment is 0.003 to 0.015, preferably 0.003 to 0.010, more preferably 0.003 to 0.009, and further preferably 0.003 to 0.008. By setting the dielectric loss tangent to the lower limit or more, it is possible to improve the adhesion reliability between the conductor line serving as the antenna and the dielectric layer, and to stably maintain antenna performance while maintaining a good balance between high frequency and miniaturization. On the other hand, by setting the dielectric loss tangent to the upper limit or less, it is possible to suppress energy loss and accommodate higher frequencies. That is, from the viewpoint of reducing transmission loss, the lower the dielectric loss tangent, the better, but the lower the dielectric, the lower the adhesion to the conductor serving as the antenna tends to be. Therefore, from the viewpoint of achieving both high frequency and miniaturization, it is preferable to set the dielectric loss tangent to the lower limit or more while retaining a certain degree of polarity.
[0023] The dielectric constant and dielectric loss tangent can be controlled by known methods such as appropriately selecting the type and amount of each component contained in the high dielectric resin composition, the preparation method of the high dielectric resin composition, etc. For example, the higher the content of the inorganic filler (B) having a large dielectric constant, the more the relative dielectric constant (εr) of the cured product of the high dielectric resin composition can be improved.
[0024] [Peel Strength] The peel strength of the cured film made of the high dielectric resin composition of this embodiment against copper foil is preferably 0.5 kN / m or more, and more preferably 0.6 kN / m or more. This provides high adhesion to the copper foil.
[0025] In this embodiment, the peel strength is measured, for example, as follows. First, a resin layer made of the high dielectric resin composition is formed on a substrate, and a copper foil having a surface roughness Rz of 2 μm or less is placed on the resin layer, and vacuum pressed at a temperature of 225° C. to form a laminate of the cured film of the resin layer and the copper foil. The stress when peeling the cured film from the copper foil using the obtained laminate is taken as the peel strength. The peel strength can be measured in accordance with "JIS C 6481". If necessary, the copper foil may be copper plated to increase the thickness, for example to about 20 μm, before measurement.
[0026] The peel strength of the highly dielectric resin composition of the present embodiment can be controlled by the number of polar functional groups of the resin composition, etc.
[0027] [Complex dynamic viscosity] The minimum value of complex dynamic viscosity η1 of the high dielectric resin composition in a dynamic viscoelasticity test at a measurement range of 50 to 200°C, a heating rate of 3°C / min, and a frequency of 62.83 rad / sec is preferably 50 to 2000 Pa s, and more preferably 100 to 1500 Pa s. This improves the dispersibility of the inorganic filler (B) described below, and makes it possible to stably obtain a good balance between a high dielectric constant and a low dielectric loss tangent.
[0028] The complex dynamic viscosity of the high dielectric resin composition of the present embodiment can be controlled by adjusting the content of the inorganic filler, changing the particle size of the inorganic filler, or the like.
[0029] [Glass transition temperature] In this embodiment, the glass transition temperature of the cured product of the high dielectric resin composition is preferably 100° C. or higher, more preferably 120° C. or higher, and even more preferably 140° C. or higher. This makes it possible to more effectively improve the heat resistance of the cured product of the high dielectric resin composition. On the other hand, the upper limit of the glass transition temperature is not particularly limited, but can be, for example, 250° C.
[0030] The glass transition temperature of the cured product of the highly dielectric resin composition can be measured, for example, as follows. The cured product of the highly dielectric resin composition is further post-cured at 175°C for 4 hours, and then measured using a thermomechanical analyzer (Seiko Denshi Kogyo Co., Ltd., TMA100) under conditions of a measurement temperature range of 0°C to 320°C and a heating rate of 5°C / min. The glass transition temperature is calculated from the measurement results.
[0031] The glass transition temperature of the highly dielectric resin composition of the present embodiment can be controlled by appropriately adjusting the types and blending ratios of the components constituting the highly dielectric resin composition.
[0032] Each component contained in the resin composition of the present embodiment will be described in detail below.
[0033] As the epoxy resin (A), any monomer, oligomer or polymer having two or more epoxy groups in one molecule can be used, and the molecular weight and molecular structure thereof are not particularly limited. In the present embodiment, examples of the epoxy resin (A) include biphenyl-type epoxy resins; bisphenol-type epoxy resins such as bisphenol A-type epoxy resins, bisphenol F-type epoxy resins, and tetramethylbisphenol F-type epoxy resins; stilbene-type epoxy resins; novolac-type epoxy resins such as phenol novolac-type epoxy resins and cresol novolac-type epoxy resins; multifunctional epoxy resins such as triphenolmethane-type epoxy resins and alkyl-modified triphenolmethane-type epoxy resins; aralkyl-type epoxy resins such as phenol aralkyl-type epoxy resins having a phenylene skeleton and phenol aralkyl-type epoxy resins having a biphenylene skeleton; naphthol-type epoxy resins such as dihydroxynaphthalene-type epoxy resins and epoxy resins obtained by glycidyl etherifying a dimer of dihydroxynaphthalene; triazine nucleus-containing epoxy resins such as triglycidyl isocyanurate and monoallyl diglycidyl isocyanurate; and bridged cyclic hydrocarbon compound-modified phenol-type epoxy resins such as dicyclopentadiene-modified phenol-type epoxy resins. These may be used alone or in combination of two or more. Among these, from the viewpoint of improving the balance between moisture resistance reliability and moldability, the epoxy resin (A) preferably contains one or more types selected from the group consisting of bisphenol type epoxy resins, novolac type epoxy resins, biphenyl type epoxy resins, phenol aralkyl type epoxy resins, and triphenol methane type epoxy resins, and more preferably contains at least one type selected from the group consisting of biphenyl type epoxy resins and phenol aralkyl type epoxy resins.
[0034] It is more preferable to use, as the epoxy resin (A), one containing at least one selected from the group consisting of epoxy resins represented by the following formula (1), epoxy resins represented by the following formula (2), and epoxy resins represented by the following formula (3).
[0035] [ka] (In formula (1), Ar 1 represents a phenylene group or a naphthylene group, Ar 1 When Ar is a naphthylene group, the glycidyl ether group may be bonded to either the α-position or the β-position. 2 R represents any one of a phenylene group, a biphenylene group, and a naphthylene group. a and R b each independently represents a hydrocarbon group having 1 to 10 carbon atoms; g is an integer of 0 to 5, and h is an integer of 0 to 8. 3 represents the degree of polymerization, the average value of which is 1 to 3.)
[0036] [ka] (In formula (2), there are multiple R c Each of n independently represents a hydrogen atom or a hydrocarbon group having 1 to 4 carbon atoms. 5 represents the degree of polymerization, the average value of which is 0 to 4.)
[0037] [ka] (In formula (3), there are multiple R d and R e Each of n independently represents a hydrogen atom or a hydrocarbon group having 1 to 4 carbon atoms. 6 represents the degree of polymerization, the average value of which is 0 to 4.)
[0038] In this embodiment, the content of the epoxy resin (A) in the high dielectric resin composition is preferably 3% by mass or more, more preferably 7% by mass or more, and even more preferably 10% by mass or more, when the entire high dielectric resin composition is taken as 100% by mass. By making the content of the epoxy resin (A) equal to or more than the above lower limit, sufficient fluidity can be achieved during molding, and filling properties and moldability can be improved. On the other hand, the content of the epoxy resin (A) in the high dielectric resin composition is preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less, when the entire high dielectric resin composition is taken as 100% by mass. By making the content of the epoxy resin (A) equal to or less than the above upper limit, it is possible to improve the moisture resistance reliability and reflow resistance of the cured product of the high dielectric resin composition.
[0039] [Inorganic filler (B)] In this embodiment, the inorganic filler (B) has a dielectric constant (1 MHz) of at least 6. This makes it possible to realize a resin composition with a high dielectric constant even if it has a low dielectric tangent. The inorganic filler (B) is not particularly limited as long as it has a dielectric constant (1 MHz) of 6 or more, and any known filler can be used. Specifically, the inorganic filler (B) may be, for example, one or more selected from the group consisting of titanium oxide, magnesium oxide, alumina, tantalum pentoxide, and niobium pentoxide. Among them, it is preferable that the inorganic filler (B) does not contain a perovskite structure, for example, it is preferable that the inorganic filler (B) does not contain barium titanate, and it is more preferable that the inorganic filler (B) contains titanium oxide in order to further reduce the dielectric tangent.
[0040] The inorganic filler (B) may be surface-treated with inorganic and organic substances. Surface treatment methods can be broadly classified into (1) modification by coating, (2) topochemical modification, (3) modification by mechanochemical reaction, (4) modification by encapsulation, and (5) combined use with radiation exposure. In detail, (1) is fatty acid treatment, surfactant treatment, etc., (2) is a method of organifying surface functional groups with organic substances or coupling agents, (3) is a method of utilizing the activity of newly generated solid surfaces by mechanical treatment such as grinding, and (4) is a method of encapsulating inorganic substances by wrapping them in polymers. Among these, it is preferable to make the surface functional groups organic by using the organic substance or coupling agent described in (2) above.
[0041] The content of the inorganic filler (B) is preferably 30% by mass or more, more preferably 35% by mass or more, and even more preferably 40% by mass or more, based on the total amount of the high dielectric resin composition. By making the content of the inorganic filler (B) equal to or more than the above lower limit, the dielectric properties of the high dielectric resin composition can be further improved. On the other hand, the content of the inorganic filler (B) is preferably 80 mass% or less, more preferably 70 mass% or less, and even more preferably 55 mass% or less, based on the total amount of the high dielectric resin composition. By making the content of the inorganic filler (B) equal to or less than the above upper limit, it is possible to more effectively improve the flowability and filling property during molding of the high dielectric resin composition.
[0042] The average particle diameter D50 of the inorganic filler (B) is preferably 0.01 μm or more and 10 μm or less, more preferably 0.05 μm or more and 8 μm or less. By making the average particle diameter D50 equal to or more than the lower limit, the flowability of the high dielectric resin composition can be improved, and the moldability can be more effectively improved. In addition, by making the average particle diameter D50 equal to or less than the upper limit, the occurrence of gate clogging can be reliably suppressed. The average particle size D90 of the inorganic filler (B) is preferably 0.05 μm or more and 20 μm or less, and more preferably 0.2 μm or more and 15 μm or less.
[0043] The particle size of the inorganic filler (B) and the inorganic filler (b) described below can be determined by measuring the particle size distribution of the particles on a volume basis using a commercially available laser particle size distribution meter (e.g., SALD-7000, manufactured by Shimadzu Corporation), and the cumulative 50% and cumulative 90% of the frequency of the median diameters are defined as D50 and D90, respectively.
[0044] The highly dielectric resin composition of the present embodiment may further contain the following components.
[0045] [Cyanate resin (C)] The cyanate resin (C) makes it easier to impart a low thermal expansion coefficient and heat resistance to the resin composition. The cyanate resin (C) is preferably an aromatic cyanate resin, and specific examples thereof include novolac-type cyanate resins such as phenol novolac type and cresol novolac type; aralkyl-type cyanate resins such as phenyl aralkyl type, biphenyl aralkyl type and naphthalene aralkyl type; and bisphenol-type cyanate resins such as bisphenol A type cyanate resin, bisphenol E type cyanate resin and tetramethyl bisphenol F type cyanate resin. Among these, bisphenol-type cyanate and / or novolac-type cyanate resins are preferred, and it is more preferred to use both in combination. The reason for this is that bisphenol-type cyanate ester resins have fewer crosslinking points, so that when triazine rings are formed, unreacted cyanate groups are less likely to remain, making it easier to maintain good dielectric properties. In addition, novolac-type cyanate resins form triazine rings after the curing reaction, which can improve rigidity and heat resistance, making it easier to respond to miniaturization and high frequency.
[0046] As the novolac type cyanate resin, for example, one represented by the following general formula (I) can be used.
[0047] [ka]
[0048] The average repeating unit n of the novolac cyanate resin (C) represented by the general formula (I) is any integer. The average repeating unit n is not particularly limited, but is preferably 1 or more, more preferably 2 or more. When the average repeating unit n is equal to or more than the above lower limit, the heat resistance of the novolac cyanate resin (C) is improved, and the elimination and volatilization of low molecular weight compounds during heating can be suppressed. In addition, the average repeating unit n is not particularly limited, but is preferably 10 or less, more preferably 7 or less. When n is equal to or less than the above upper limit, the melt viscosity can be suppressed from increasing, and the moldability of the prepreg can be improved.
[0049] The cyanate resin (C) may be modified, and may contain, for example, a butadiene-modified cyanate modified with butadiene. Specifically, the butadiene-modified cyanate may be one obtained by mixing a cyanate ester compound with polybutadiene and then subjecting it to thermal polymerization, and / or one obtained by mixing a polymer of a cyanate ester compound with polybutadiene and then subjecting it to thermal polymerization. This allows the heat resistance to be well maintained while achieving both dielectric properties and miniaturization.
[0050] The weight average molecular weight (Mw) of the cyanate resin (C) is not particularly limited, but is preferably Mw500 or more, more preferably Mw600 or more. When Mw is equal to or more than the above lower limit, the occurrence of tackiness can be suppressed when a prepreg is produced, and the prepregs can be prevented from adhering to each other when they come into contact with each other, or from transferring. Furthermore, Mw is not particularly limited, but is preferably Mw4,500 or less, more preferably Mw3,000 or less. When Mw is equal to or less than the above upper limit, the cyclization reaction of the cyanate resin (C) can be prevented from becoming too fast, and the occurrence of defects in the insulating layer and the decrease in the peel strength between the insulating layer and the metal layer can be prevented.
[0051] The Mw of the cyanate resin (C) can be measured, for example, by GPC (gel permeation chromatography, standard substance: polystyrene equivalent).
[0052] The cyanate resin (C) may be used alone or in combination of two or more types having different Mw, or in combination of one or more types and their prepolymers.
[0053] In this embodiment, the content of the cyanate resin (C) in the high dielectric resin composition is preferably 7 mass% or more, more preferably 10 mass% or more, and even more preferably 12 mass% or more, when the entire high dielectric resin composition is 100 mass%. On the other hand, the content of the cyanate resin (C) in the high dielectric resin composition is preferably 30 mass% or less, more preferably 27 mass% or less, and even more preferably 25 mass% or less, when the entire high dielectric resin composition is 100 mass%.
[0054] [Cumarone resin (D)] The coumarone resin (D) in this embodiment refers to a (co)polymer containing a coumarone residue in its skeleton structure and having an average degree of polymerization of 4 to 8, and may be a coumarone (1-benzofuran) polymer, as well as a copolymer with indene (C9H8), styrene (C8H8), α-methylstyrene, methylindene, and vinyltoluene. Among these, a coumarone-indene copolymer and a coumarone-indene-styrene copolymer are preferred.
[0055] The indene-cumarone resin contains a structural unit A derived from an indene monomer and a structural unit B derived from a cumarone monomer. The indene-cumarone resin may have a structural unit derived from another monomer. The indene-cumarone resin may have, for example, a structural unit C derived from a styrene monomer. The indene-cumarone resin may have a repeating structure of these structural units.
[0056] The structural unit A derived from the indene monomer is, for example, one represented by the following general formula (M1).
[0057] [ka]
[0058] (In general formula (M1), R 1 From R 7 are each independently a hydrogen atom or an organic group having 1 to 3 carbon atoms.
[0059] The structural unit B derived from the coumarone monomer is, for example, one represented by the following general formula (M2).
[0060] [ka]
[0061] (In general formula (M2), R C is hydrogen or an organic group having 1 to 3 carbon atoms. C may be the same as or different from each other.)
[0062] The structural unit C derived from the styrene-based monomer is, for example, one represented by the following general formula (M3). [ka]
[0063] (In general formula (M3), R S is hydrogen or an organic group having 1 to 3 carbon atoms. S may be the same as or different from each other.)
[0064] In the above general formulas (M1) to (M3), R1 to R7, RC and RS may contain atoms other than hydrogen and carbon in the structure of the organic group, for example. Specific examples of atoms other than hydrogen and carbon include oxygen atoms, nitrogen atoms, sulfur atoms, phosphorus atoms, silicon atoms, fluorine atoms, chlorine atoms, etc. The atoms other than hydrogen and carbon may include one or more of the above specific examples.
[0065] In the above general formulas (M1) to (M3), R1 to R7, RC and RS are each independently, for example, hydrogen or an organic group having 1 to 3 carbon atoms, preferably hydrogen or an organic group having 1 carbon atom, and more preferably hydrogen.
[0066] In the above general formulas (M1) to (M3), specific examples of the organic groups constituting R1 to R7, RC and RS include alkyl groups such as a methyl group, an ethyl group, and an n-propyl group; alkenyl groups such as an allyl group and a vinyl group; alkynyl groups such as an ethynyl group; alkylidene groups such as a methylidene group and an ethylidene group; cycloalkyl groups such as a cyclopropyl group; and heterocyclic groups such as an epoxy group and an oxetanyl group.
[0067] The indene-cumarone resin may contain a copolymer of indene, cumarone and styrene, which can improve the low dielectric properties.
[0068] In addition, the indene-cumarone resin can have a reactive group in the molecule that reacts with the epoxy group of the epoxy resin, thereby improving the low dielectric properties. Examples of the reactive group include an OH group and a COOH group. The indene-cumarone resin may have an aromatic structure having a phenolic hydroxyl group inside or at a terminal thereof.
[0069] The upper limit of the weight average molecular weight Mw of the indene-cumarone resin is, for example, preferably 4000 or less, more preferably 2000 or less, even more preferably 1500 or less, and even more preferably 1200 or less. This improves the compatibility of the indene-cumarone resin with the epoxy resin, and allows the indene-cumarone resin to be appropriately dispersed. On the other hand, the lower limit of the weight average molecular weight Mw of the indene-cumarone resin is, for example, preferably 400 or more, more preferably 500 or more, even more preferably 550 or more, and even more preferably 600 or more. This allows the indene-cumarone resin to be appropriately dispersed in the resin composition.
[0070] The lower limit of the content of the indene-cumarone resin is, for example, 1% by mass or more, preferably 3% by mass or more, and more preferably 5% by mass or more, when the entire high dielectric resin composition of this embodiment is taken as 100% by mass. This can improve low dielectric properties and low water absorption properties. On the other hand, the upper limit of the content of the indene-cumarone resin is, for example, 15% by mass or less, preferably 12% by mass or less, and more preferably 10% by mass or less, when the entire high dielectric resin composition of this embodiment is taken as 100% by mass. This can achieve a balance with other physical properties.
[0071] The melting point of the chroman resin (D) is preferably from 40° C. to 120° C., and the melting point can be controlled by the molecular weight and the degree of polymerization.
[0072] The content of the coumarone resin (D) is preferably from 1 to 25% by mass, more preferably from 5 to 20% by mass, and even more preferably from 8 to 15% by mass, when the entire highly dielectric resin composition is taken as 100% by mass.
[0073] [Inorganic filler (b)] The high dielectric resin composition of the present embodiment may contain an inorganic filler other than the above-mentioned inorganic filler (B), that is, an inorganic filler (b) having a dielectric constant (1 MHz) of less than 6. Examples of the inorganic filler (b) having a dielectric constant (1 MHz) of less than 6 include silicates such as talc, calcined clay, uncalcined clay, mica, and glass; oxides such as titanium oxide, alumina, boehmite, silica, and fused silica; carbonates such as calcium carbonate, magnesium carbonate, and hydrotalcite; hydroxides such as aluminum hydroxide, magnesium hydroxide, and calcium hydroxide; sulfates or sulfites such as barium sulfate, calcium sulfate, and calcium sulfite; borates such as zinc borate, barium metaborate, aluminum borate, calcium borate, and sodium borate; and nitrides such as aluminum nitride, boron nitride, silicon nitride, and carbon nitride. The inorganic filler (b) may be surface-treated with an inorganic or organic substance in the same manner as the above-mentioned inorganic filler (B). Among these, talc, alumina, glass, silica, mica, aluminum hydroxide, and magnesium hydroxide are preferable, and silica is more preferable. The dielectric constant of the inorganic filler (b) is not particularly limited, and may be, for example, 1-5 or 2-4.
[0074] The average particle diameter D50 of the inorganic filler (b) is not particularly limited, but is preferably 0.01 to 10 μm, more preferably 0.05 to 5 μm, and even more preferably 0.2 to 3 μm. By making the average particle diameter D50 of the inorganic filler (b) equal to or greater than the lower limit, the increase in viscosity can be suppressed and good workability can be maintained. On the other hand, by making the average particle diameter D50 of the inorganic filler (b) equal to or less than the upper limit, the dispersibility of the inorganic filler (b) can be improved.
[0075] [Hardening agent] The high dielectric resin composition may contain, for example, a curing agent. The curing agent is not particularly limited as long as it reacts with the epoxy resin (A) to cure, and examples of the curing agent include linear aliphatic diamines having 2 to 20 carbon atoms, such as ethylenediamine, trimethylenediamine, tetramethylenediamine, and hexamethylenediamine, metaphenylenediamine, paraphenylenediamine, paraxylenediamine, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylpropane, 4,4'-diaminodiphenylether, 4,4'-diaminodiphenylsulfone, 4,4'-diaminodicyclohexane, bis(4-aminophenyl)phenylmethane, 1,5-diaminonaphthalene, metaxylenediamine, paraxylenediamine, 1,1-bis(4-aminophenyl)cyclohexane, and dicyanodiamide; resol-type phenolic resins, such as aniline-modified resol resins and dimethyl ether resol resins; phenol novolac resins, cresol novolac resins, and tert-butylphenol. Examples of the phenolic resins include novolac-type phenolic resins such as novolac resins and nonylphenol novolac resins; polyfunctional phenolic resins such as trisphenolmethane-type phenolic resins; phenolic aralkyl resins such as phenylene skeleton-containing phenolic aralkyl resins and biphenylene skeleton-containing phenolic aralkyl resins; phenolic resins having a condensed polycyclic structure such as a naphthalene skeleton or an anthracene skeleton; polyoxystyrenes such as polyparaoxystyrene; alicyclic acid anhydrides such as hexahydrophthalic anhydride (HHPA) and methyltetrahydrophthalic anhydride (MTHPA), and aromatic acid anhydrides such as trimellitic anhydride (TMA), pyromellitic anhydride (PMDA), and benzophenonetetracarboxylic acid (BTDA); polymercaptan compounds such as polysulfides, thioesters, and thioethers; isocyanate compounds such as isocyanate prepolymers and blocked isocyanates; and organic acids such as carboxylic acid-containing polyester resins. These may be used alone or in combination of two or more.
[0076] The content of the curing agent in the high dielectric resin composition is not particularly limited, but for example, when the entire high dielectric resin composition is taken as 100 mass%, it is preferably 0.1 mass% or more and 20 mass% or less, more preferably 0.5 mass% or more and 10 mass% or less, and even more preferably 1 mass% or more and 5 mass% or less.
[0077] [Coupling agent] The high dielectric resin composition may contain, for example, a coupling agent, such as various known coupling agents including silane-based compounds such as epoxysilane, mercaptosilane, aminosilane, alkylsilane, ureidosilane, and vinylsilane, titanium-based compounds, aluminum chelates, and aluminum / zirconium-based compounds. Examples of these include vinyltrichlorosilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltris(β-methoxyethoxy)silane, γ-methacryloxypropyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, γ-glycidoxypropylmethyldimethoxysilane, γ-methacryloxypropylmethyldiethoxysilane, γ-methacryloxypropyltriethoxy Silane, vinyltriacetoxysilane, γ-mercaptopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-anilinopropyltrimethoxysilane, γ-anilinopropylmethyldimethoxysilane, γ-[bis(β-hydroxyethyl)]aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane, N-phenyl N-(vinylbenzylaminoethyl)-γ-aminopropyltrimethoxysilane, γ-(β-aminoethyl)aminopropyldimethoxymethylsilane, N-(trimethoxysilylpropyl)ethylenediamine, N-(dimethoxymethylsilylisopropyl)ethylenediamine, methyltrimethoxysilane, dimethyldimethoxysilane, methyltriethoxysilane, N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltrimethoxysilane, γ-chloropropyltrimethoxysilane, hexamethyldisilane, vinyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, Silane coupling agents such as tripropylmethyldimethoxysilane, 3-isocyanatopropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, and hydrolyzates of 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine; isopropyl triisostearoyl titanate, isopropyl tris(dioctylpyrophosphate) titanate, isopropyl tri(N-aminoethyl-aminoethyl) titanate, tetraoctylbis(ditridecylphosphite) titanate, tetra(2,Examples of titanate-based coupling agents include 2-diallyloxymethyl-1-butyl)bis(ditridecyl)phosphite titanate, bis(dioctyl pyrophosphate)oxyacetate titanate, bis(dioctyl pyrophosphate)ethylene titanate, isopropyl trioctanoyl titanate, isopropyl dimethacryl isostearoyl titanate, isopropyl tridodecylbenzenesulfonyl titanate, isopropyl isostearoyl diacryl titanate, isopropyl tri(dioctyl phosphate) titanate, isopropyl tricumyl phenyl titanate, and tetraisopropyl bis(dioctyl phosphite) titanate. These may be used alone or in combination of two or more.
[0078] The content of the coupling agent in the high dielectric resin composition is not particularly limited, but for example, when the entire high dielectric resin composition is taken as 100 mass%, it is preferably 0.01 mass% or more and 3 mass% or less, and more preferably 0.1 mass% or more and 2 mass% or less. By making the content of the coupling agent equal to or more than the above lower limit, the dispersibility of the inorganic filler (B) in the high dielectric resin composition can be improved. In addition, by making the content of the coupling agent equal to or less than the above upper limit, the flowability of the high dielectric resin composition can be improved, and the moldability can be improved.
[0079] [Other ingredients] In addition to the above components, the high dielectric resin composition may contain various additives such as a phosphorus atom-containing compound such as an organic phosphine, a tetra-substituted phosphonium compound, a phosphobetaine compound, an adduct of a phosphine compound and a quinone compound, or an adduct of a phosphonium compound and a silane compound, or an amidine compound such as 1,8-diazabicyclo(5.4.0)undecene-7, imidazole, or the like, a tertiary amine such as benzyldimethylamine, an amidinium salt which is a quaternary onium salt of the above compound, or an ammonium salt, or the like, a hardening accelerator such as a compound in which a hydroxyl group is bonded to each of two or more adjacent carbon atoms constituting an aromatic ring; a colorant such as carbon black; a release agent such as natural wax, synthetic wax, higher fatty acid or its metal salt, paraffin, or polyethylene oxide; a stress reducing agent such as a polybutadiene compound, an acrylonitrile butadiene copolymer compound, silicone oil, or silicone rubber; an ion trapping agent such as hydrotalcite; a flame retardant such as aluminum hydroxide; and an antioxidant.
[0080] <Varnish> The highly dielectric resin composition of the present embodiment can be dissolved in a solvent to form a varnish. Examples of the solvent include organic solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, toluene, ethyl acetate, cyclohexane, heptane, cyclohexane, cyclohexanone, tetrahydrofuran, dimethylformamide, dimethylacetamide, dimethylsulfoxide, ethylene glycol, cellosolve-based solvents, carbitol-based solvents, anisole, and N-methylpyrrolidone. These may be used alone or in combination of two or more kinds.
[0081] When the high dielectric resin composition of the present embodiment is in the form of a varnish, the solid content of the resin composition may be, for example, 30% by mass or more and 80% by mass or less, more preferably 40% by mass or more and 70% by mass or less, which can provide excellent workability and film-forming properties.
[0082] The varnish-like resin composition can be prepared by dissolving, mixing, and stirring the above-mentioned components in a solvent using various mixers such as those used in an ultrasonic dispersion system, a high-pressure collision dispersion system, a high-speed rotation dispersion system, a bead mill system, a high-speed shear dispersion system, and a rotation-revolution dispersion system.
[0083] <Resin film> Next, the resin film of this embodiment will be described. The resin film of this embodiment can be obtained by forming the above-mentioned resin composition in a varnish form into a film. For example, the resin film of this embodiment can be obtained by removing the solvent from a coating film obtained by applying the resin composition in a varnish form. In such a resin film, the solvent content can be 5 mass % or less with respect to the entire resin film. In this embodiment, the step of removing the solvent may be carried out under conditions of, for example, 100°C to 150°C and 1 minute to 5 minutes. This makes it possible to sufficiently remove the solvent while suppressing the progress of curing of the resin film containing a thermosetting resin.
[0084] The resin film of the present embodiment may be composed of a resin film alone, or may be composed so as to include a fiber base material therein.
[0085] <Prepreg> The prepreg of the present embodiment is configured to contain a fibrous base material in the high dielectric resin composition of the present embodiment. The prepreg is obtained by impregnating a fibrous base material with the resin composition. For example, prepreg can be used as a sheet-like material obtained by impregnating a fiber substrate with a resin composition and then semi-curing the same. A sheet-like material having such a structure has excellent properties such as dielectric properties and mechanical and electrical connection reliability under high temperature and humidity, and is suitable for producing an insulating layer for a printed wiring board.
[0086] In this embodiment, the method of impregnating the resin composition into the fiber substrate is not particularly limited, but examples thereof include a method of dissolving the resin composition in a solvent to prepare a resin varnish and immersing the fiber substrate in the resin varnish, a method of applying the resin varnish to the fiber substrate using various coaters, a method of spraying the resin varnish onto the fiber substrate using a sprayer, and a method of laminating both sides of the fiber substrate with the resin film consisting of the resin composition.
[0087] Examples of the fiber substrate include glass fiber substrates such as woven glass cloth and nonwoven glass cloth, inorganic fiber substrates such as woven or nonwoven cloth containing inorganic compounds other than glass as components, and organic fiber substrates composed of organic fibers such as aromatic polyamideimide resin, polyamide resin, aromatic polyester resin, polyester resin, polyimide resin, and fluororesin, etc. Among these substrates, the use of a glass fiber substrate typified by glass woven cloth in terms of strength can improve the mechanical strength and heat resistance of the printed wiring board.
[0088] The thickness of the fiber base material is not particularly limited, but is preferably 5 μm to 150 μm, more preferably 10 μm to 100 μm, and even more preferably 12 μm to 90 μm. By using a fiber base material having such a thickness, the handleability during the production of the prepreg can be further improved. When the thickness of the fiber substrate is equal to or less than the upper limit, the impregnation of the resin composition in the fiber substrate is improved, and the occurrence of strand voids and deterioration of insulation reliability can be suppressed. In addition, the formation of through holes by carbon dioxide, UV, excimer, or other lasers can be facilitated. In addition, when the thickness of the fiber substrate is equal to or more than the lower limit, the strength of the fiber substrate and prepreg can be improved. As a result, the handling property can be improved, the preparation of prepreg can be facilitated, and warping of the resin substrate can be suppressed.
[0089] As the above-mentioned glass fiber substrate, for example, a glass fiber substrate formed of one or more types of glass selected from E glass, S glass, D glass, T glass, NE glass, UT glass, L glass, HP glass and quartz glass is suitably used.
[0090] In this embodiment, the prepreg can be used to form, for example, an insulating layer in a build-up layer or an insulating layer in a core layer of a printed wiring board. When the prepreg is used to form an insulating layer in a core layer of a printed wiring board, for example, two or more prepregs can be stacked and the resulting laminate can be heat-cured to form an insulating layer for the core layer.
[0091] <Metal-clad laminate> The laminate of the present embodiment is a metal-clad laminate in which a metal layer is disposed on at least one surface of the cured product of the prepreg.
[0092] A method for producing a metal-clad laminate using a prepreg is, for example, as follows. A metal foil is placed on both the upper and lower sides or one side of the outer side of a prepreg or a laminate of two or more prepregs, and these are bonded under high vacuum conditions using a laminator or Becquerel device, or a metal foil is placed on both the upper and lower sides or one side of the outer side of the prepreg as is. When two or more prepregs are laminated, a metal foil is placed on both the upper and lower sides or one side of the outermost side of the laminated prepregs. Next, a metal-clad laminate can be obtained by hot-press molding the laminate of the prepreg and the metal foil. Here, it is preferable to continue pressing until the end of cooling during hot-press molding.
[0093] Examples of the metals constituting the metal foil include copper, copper-based alloys, aluminum, aluminum-based alloys, silver, silver-based alloys, gold, gold-based alloys, zinc, zinc-based alloys, nickel, nickel-based alloys, tin, tin-based alloys, iron, iron-based alloys, Fe-Ni-based alloys such as Kovar (trade name), 42 alloy, Invar, and Super Invar, W, and Mo. Among these, the metal constituting the metal foil 105 is preferably copper or a copper alloy, because it has excellent conductivity, is easy to form a circuit by etching, and is inexpensive. That is, the metal foil 105 is preferably a copper foil. As the metal foil, a metal foil with a carrier or the like can also be used. The thickness of the metal foil is preferably 0.5 μm or more and 20 μm or less, and more preferably 1.5 μm or more and 18 μm or less.
[0094] <Resin film with carrier> Next, the resin film with a carrier of this embodiment will be described. FIG. 1 is a diagram showing an example of the configuration of a resin film 10 with a carrier.
[0095] An example of the resin film 10 with a carrier includes a carrier substrate 30 and a resin film 20) made of a resin composition provided on the carrier substrate 30.
[0096] The resin film 10 with a carrier may be in the form of a roll that can be wound up as shown in FIG. 1(a), or in the form of a rectangular sheet.
[0097] As the carrier substrate 30, for example, a polymer film or a metal foil can be used. The polymer film is not particularly limited, but examples thereof include polyolefins such as polyethylene and polypropylene, polyesters such as polyethylene terephthalate and polybutylene terephthalate, polycarbonate, release paper such as silicone sheets, and thermoplastic resin sheets having heat resistance such as fluorine-based resins and polyimide resins. The metal foil is not particularly limited, but examples thereof include copper and / or copper-based alloys, aluminum and / or aluminum-based alloys, iron and / or iron-based alloys, silver and / or silver-based alloys, gold and gold-based alloys, zinc and zinc-based alloys, nickel and nickel-based alloys, and tin and tin-based alloys. Among these, a sheet made of polyethylene terephthalate is most preferable because it is inexpensive and the peel strength can be easily adjusted. This makes it easy to peel off the resin film 10 with the carrier with an appropriate strength.
[0098] The surface of the carrier-attached resin film 10 may be exposed or may be covered with a protective film (cover film 50). As the protective film, a film having a known protective function may be used, for example, a PET film may be used. As shown in FIG. 1(b), the resin film 20 may be formed between the carrier substrate 30 and the cover film 50. This improves the handleability of the resin film 20.
[0099] The resin film 20 of the carrier-attached resin film 10 of this embodiment may be a single layer or a multilayer, and may be composed of one or more types of films. When the resin sheet is a multilayer, it may be composed of the same type or different types.
[0100] The lower limit of the thickness of the resin film 20 is, for example, 5 μm or more, and preferably 10 μm or more. This can improve the insulation reliability. On the other hand, the upper limit of the thickness of the resin film 20 is, for example, 50 μm or less, and preferably 40 μm or less. This can realize a thin-layered printed wiring board. Furthermore, by setting the thickness of the resin film 20 within the above range, it is possible to fill the unevenness of the inner layer circuit when manufacturing the printed wiring board, and to ensure a suitable insulating resin layer thickness of the build-up layer.
[0101] The thickness of the carrier base 30 is not particularly limited, but may be, for example, 10 to 100 μm, or 10 to 70 μm, which is preferable because it improves the handleability when producing the carrier-attached resin film 10.
[0102] <Printed wiring board> The printed wiring board of this embodiment includes an insulating layer made of the cured product of the above-mentioned resin film (cured product of the resin composition). In this embodiment, the cured resin film can be used, for example, as a build-up layer of a normal printed wiring board, a build-up layer in a printed wiring board having no core layer, a build-up layer of a coreless substrate used in PLP, a build-up layer of an MIS substrate, etc. The insulating layer constituting such a build-up layer can also be suitably used as a build-up layer constituting a large-area printed wiring board used to collectively produce a plurality of semiconductor packages.
[0103] In the present embodiment, the resin film made of the resin composition for forming the insulating film may be impregnated with glass fibers. In a semiconductor package using such a resin film as a build-up layer, the linear expansion coefficient of the cured resin film can be reduced, so that package warpage can be sufficiently suppressed.
[0104] <Semiconductor packages> 2A to 2C are cross-sectional views showing an example of a manufacturing process for the semiconductor package 200 of this embodiment. The semiconductor device (semiconductor package 200) of this embodiment can include a printed wiring board and a semiconductor element 240 mounted on a circuit layer of the printed wiring board or embedded in the printed wiring board.
[0105] An outline of the manufacturing process for the semiconductor package 200 of this embodiment will be described below. First, as shown in FIG. 2(a), a core layer 100 including an insulating layer 102, a via hole 104, and a metal layer 108 is prepared. A via hole 104 is formed in the insulating layer 102. A metal layer (via) is embedded in the via hole 104. The metal layer may be covered with an electroless metal plating film 106. The metal layer 108 (a circuit layer having a predetermined circuit pattern) formed on the surface of the insulating layer 102 is electrically connected to the via formed in the via hole 104. In FIG. 2(a), the metal layer 108 is formed on one surface of the core layer 100, but it may be formed on both surfaces.
[0106] Next, a resin film 20 made of the above resin composition is formed on one surface of the core layer 100 so as to embed the metal layer 108. For example, the cover film 50 may be peeled off from the resin film 10 with the carrier, and the resin film 20 (insulating film) may be placed on the circuit formation surface of the core layer 100. A carrier base material 30 is provided on the surface of this resin film 20. The carrier base material 30 may be separated from the resin film 20 at this point, or may be used as a mask. The resin film 20 may be a single insulating layer, or may be made up of multiple layers including an insulating layer and a primer layer.
[0107] Next, an opening (not shown) is formed in the resin film 20 via the carrier substrate 30. The opening can be formed so as to expose the metal layer 108. The method for forming the opening is not particularly limited, and may be, for example, a laser processing method, an exposure and development method, or a blasting method.
[0108] In this embodiment, after forming such openings, the resin film 20 may be thermally cured, and then the carrier base 30 is peeled off.
[0109] In addition, a desmear process can be performed as necessary, which can remove smears generated inside the openings and roughen the surface of the resin film 20.
[0110] The method of the desmear treatment is not particularly limited, but can be performed, for example, as follows. First, the core layer 100 on which the resin film 20 is laminated can be immersed in a swelling liquid containing an organic solvent, and then immersed in an alkaline permanganate aqueous solution to neutralize and roughen the surface. As the organic solvent, diethylene glycol monobutyl ether, ethylene glycol, or the like can be used. As such a swelling liquid, for example, "Swelling Dip Securigant P" manufactured by Atotech Japan can be used. As the permanganate, for example, potassium permanganate, sodium permanganate, or the like can be used. The liquid temperature of the swelling liquid or the permanganate aqueous solution may be, for example, 50°C or higher and 100°C or lower. The immersion time in the swelling liquid or the permanganate aqueous solution may be, for example, 1 minute or more and 30 minutes or less.
[0111] In the desmearing step, only the above-mentioned wet desmearing can be performed, but plasma irradiation may be performed in addition to the desmearing.
[0112] Next, an electroless metal plating film 202 is formed on the resin film 20 or on a primer layer (not shown) formed on the resin film 20. An example of an electroless plating method will be described. For example, catalytic nuclei are provided on the surface of the underlayer. The catalytic nuclei are not particularly limited, but for example, precious metal ions or palladium colloids can be used. Then, the electroless metal plating film 202 is formed by electroless plating using the catalytic nuclei as nuclei. For example, a plating solution containing copper sulfate, formalin, a complexing agent, sodium hydroxide, etc. can be used for the electroless plating. After the electroless plating, a heat treatment at 100 to 250° C. can be performed to stabilize the plating film.
[0113] Subsequently, as shown in FIG. 2(b), a resist 204 having a predetermined opening pattern (openings 206) may be formed on the electroless metal plating film 202. This opening pattern corresponds to, for example, a circuit pattern. The resist 204 is not particularly limited and may be any known material, but may be liquid or dry film. In the case of forming fine wiring, the resist 204 may be a photosensitive dry film or the like. An example using a photosensitive dry film will be described. For example, a photosensitive dry film is laminated on the electroless metal plating film 202, the non-circuit forming area is exposed to light to harden, and the unexposed area is dissolved and removed with a developer. The hardened photosensitive dry film is left behind to form the resist 204.
[0114] 2(c), an electrolytic metal plating layer 208 is formed by electroplating at least inside the opening pattern of the resist 204 and on the electroless metal plating film 202. The electroplating method is not particularly limited, but a known method used in ordinary printed wiring boards can be used, for example, a method of passing an electric current through a plating solution such as copper sulfate while immersed in the plating solution can be used. The electrolytic metal plating layer 208 may have a single layer or a multilayer structure. The material of the electrolytic metal plating layer 208 is not particularly limited, but for example, one or more of copper, copper alloy, 42 alloy, nickel, iron, chromium, tungsten, gold, and solder can be used.
[0115] Next, as shown in FIG. 2(d), the resist 204 is removed using an alkaline remover, sulfuric acid, or a commercially available resist remover.
[0116] 2(e), the electroless metal plating film 202 is removed from the area (opening 210) other than the area where the electrolytic metal plating layer 208 is formed. That is, the electroless metal plating film 202 of the lower layer is selectively removed using the electrolytic metal plating layer 208 as a mask. For example, the electroless metal plating film 202 can be removed by using soft etching (flash etching) or the like. Here, the soft etching process can be performed by etching using an etching solution containing sulfuric acid and hydrogen peroxide. This allows the metal layer 220 having a predetermined pattern to be formed. In this way, the metal layer 220 composed of the electroless metal plating film 202 and the electrolytic metal plating layer 208 can be formed on the insulating layer made of the cured product of the resin film of this embodiment by the semi-additive process (SAP).
[0117] Furthermore, a multi-layer structure can be created by stacking build-up layers as necessary on a printed wiring board composed of the core layer 100 and the above-mentioned build-up layers, and repeating the process of forming interlayer connections and circuits using a semi-additive process. In this manner, the printed wiring board of the present embodiment is obtained.
[0118] 2(f), a build-up layer is laminated on the obtained printed wiring board as necessary, and the process of forming interlayer connections and circuits by a semi-additive process is repeated. Then, a solder resist layer 230 is laminated on both sides or one side of the printed wiring board as necessary.
[0119] The method for forming the solder resist layer 230 is not particularly limited, but may be, for example, a method in which a dry film type solder resist is laminated, exposed to light, and developed, or a method in which a liquid resist is printed and then exposed to light and developed.
[0120] Next, a reflow process is performed to fix the semiconductor element 240 onto the connection terminals, which are part of the wiring pattern, via the solder bumps 250. Thereafter, the semiconductor element 240, the solder bumps 250, etc. are covered with a sealing material layer 260 for sealing. As a result of the above, a semiconductor package 200 shown in FIG.
[0121] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can be adopted. Furthermore, the present invention is not limited to the above-described embodiments, and modifications and improvements within the scope of the present invention are included in the present invention. For example, the resin composition of the present embodiment can also be used as an encapsulant for encapsulating a semiconductor chip. Below, examples of reference forms are given. 1. A high dielectric resin composition comprising an epoxy resin (A) and an inorganic filler (B) having a dielectric constant (1 MHz) of 6 or more, A highly dielectric resin composition, the cured product of which has a dielectric constant (Dk: εr) of 4 to 10 at 10 GHz, and a dielectric loss tangent (Df: tan δ) of 0.003 to 0.015 at 10 GHz. 2. The high dielectric resin composition according to 1., which contains a cyanate resin (C). 3. The highly dielectric resin composition according to 1 or 2, wherein the inorganic filler (B) does not include one having a perovskite structure. 4. The highly dielectric resin composition according to any one of 1 to 3, wherein a cured film made of the highly dielectric resin composition has a peel strength against copper foil of 0.5 kN / m or more. 5. The highly dielectric resin composition according to any one of 1. to 4., wherein the complex dynamic viscosity η1 of the highly dielectric resin composition is in the range of 50 to 200°C, at a heating rate of 3°C / min and at a frequency of 62.83 rad / sec, and has a minimum value of 50 to 2000 Pa s, as measured in a dynamic viscoelasticity test. 6. The highly dielectric resin composition according to any one of 1. to 5., wherein the inorganic filler (B) comprises one or more materials selected from the group consisting of titanium oxide, magnesium oxide, alumina, tantalum pentoxide, and niobium pentoxide. 7. The highly dielectric resin composition according to any one of 1. to 6., wherein the inorganic filler (B) is surface-treated with an inorganic substance and an organic substance. 8. The highly dielectric resin composition according to any one of 1 to 7, wherein the epoxy resin (A) comprises one or more types selected from the group consisting of bisphenol type epoxy resins, novolac type epoxy resins, biphenyl type epoxy resins, phenol aralkyl type epoxy resins, and triphenolmethane type epoxy resins. 9. The high dielectric resin composition according to 2., wherein the cyanate resin (C) contains a butadiene-modified cyanate. 10. The highly dielectric resin composition according to any one of 1. to 9., further comprising a coumarone resin (D). 11. The highly dielectric resin composition according to any one of 1 to 10, wherein the content of the inorganic filler (B) is 30% by mass or less and 80% by mass or less based on the total amount of the highly dielectric resin composition. 12. A cured product of the high dielectric resin composition described in any one of 1. to 11. 13. A prepreg comprising a fiber base material in the highly dielectric resin composition described in any one of 1. to 11. 14. A laminate comprising the prepreg according to 13, and a metal layer disposed on at least one surface of the prepreg. 15. A carrier substrate; A resin film formed on the carrier substrate and made of the high dielectric resin composition according to any one of 1. to 11.; A resin film with a carrier. 16. A printed wiring board having an insulating layer composed of a cured product of the high dielectric resin composition described in any one of 1. to 11. 17. The printed wiring board according to 16., a semiconductor element mounted on a circuit layer of the printed wiring board or embedded in the printed wiring board. EXAMPLES
[0122] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the descriptions of these examples.
[0123] <Examples and Comparative Examples> (Preparation of High Dielectric Resin Composition) Each component was dissolved or dispersed at the solid content shown in Table 1, and the non-volatile content was adjusted to 70 mass% with methyl ethyl ketone. The mixture was then stirred using a high-speed stirrer to prepare a varnish-like high dielectric resin composition (resin varnish P). The numerical values showing the blending ratio of each component in Table 1 indicate the blending ratio (mass %) of each component relative to the total solid content of the highly dielectric resin composition. Next, each of the evaluations described below was carried out, and the results are shown in Table 1.
[0124] Details of the raw materials for each component in Table 1 are as follows: (1) Epoxy resin (A) Epoxy resin 1: Biphenyl type epoxy resin (Mitsubishi Chemical Corporation, YX-4000K) Epoxy resin 2: Phenol aralkyl type epoxy resin having a biphenylene skeleton (manufactured by Nippon Kayaku Co., Ltd., NC-3000) Epoxy resin 3: Phenol aralkyl type epoxy resin having a biphenylene skeleton (manufactured by Nippon Kayaku Co., Ltd., NC-3500) (2) Inorganic filler (B) with a dielectric constant (1 MHz) of 6 or more High dielectric inorganic filler 1: Titanium oxide (manufactured by Ishihara Sangyo Kaisha, Ltd., Typek PF-728, D50: 0.21 μm, particle size D90: 1.0 μm, relative dielectric constant (1 MHz): 90, specific surface area: 20 m 2 / g, shape: spherical, content of particles with a particle size of 0.5 μm or less: 80% by mass Highly dielectric inorganic filler 2: Alumina (Micron Corporation, AX3-20R, D50: 3 μm, particle size D90: 10 μm, specific surface area: 0.6 m 2 / g, relative dielectric constant (1MHz): 8.9, shape: spherical, content of particles with a particle size of 0.5 μm or less: 14% by mass High dielectric inorganic filler 3: Barium titanate (manufactured by Nippon Chemical Industry Co., Ltd., B-Palceram BTUP-2, D50: 2 μm, particle size D90: 2.8 μm, relative dielectric constant (1 MHz): 1500, specific surface area: 0.8 m 2 / g, Shape: crushed, Content of particles with a particle size of 0.5 μm or less: 13% by mass (3) Inorganic filler with a dielectric constant (1 MHz) of less than 6 (b) Silica particle 1: Silica (manufactured by Admatechs Co., Ltd., SC-C6, D50: 2.0 μm, particle size D90: 8 μm, relative dielectric constant (1 MHz): 4, specific surface area: 2.0 m 2 / g, shape: spherical, content of particles with a particle size of 0.5 μm or less: 19% by mass Silica particle 2: Silica (manufactured by Admatechs Co., Ltd., SC-2500-SQ, D50: 0.55 μm, particle size D90: 1.0 μm, relative dielectric constant (1 MHz): 4, specific surface area: 6.4 m 2 / g, shape: spherical, particle content of 0.5 μm or less: 54% by mass (4) Cyanate resin (C) Cyanate resin 1: Novolac type cyanate resin, manufactured by Lonza, product name PT-30 Cyanate resin 2: Bisphenol A type cyanate resin, manufactured by Lonza, product name BA-230S, 75% solids by weight, 25% methyl ethyl ketone by weight (5) Coumarone resin (D) Coumarone resin 1: Indene-coumaron-styrene copolymer containing phenol groups at the ends (Nitto Chemical Industry Co., Ltd., V-120S, weight average molecular weight: 950, hydroxyl value: 30 mg KOH / g) (6) Coupling Agent Coupling agent 1: N-phenyl-γ-aminopropyltrimethoxysilane (manufactured by Dow Corning Toray Co., Ltd., CF4083) (7)Other Catalyst: Shikoku Kasei Co., Ltd., "2PZ-PW"
[0125] In each of the Examples and Comparative Examples, the obtained resin varnish P (resin composition) was used to prepare a resin film with a carrier, a prepreg, a printed wiring board, and a semiconductor package as follows.
[0126] (Resin film with carrier: Preparation of resin sheet) The obtained resin varnish P was applied to one side of a 38 μm-thick PET film using a comma coater so that the total thickness of the resin layer after drying would be 30 μm, and this was dried for 3 minutes in a drying device at 160°C to obtain a resin sheet (resin film with carrier) in which a resin film was laminated on the PET film.
[0127] (Prepreg) The obtained resin varnish was impregnated into a glass woven fabric (cloth type #1078, E glass, basis weight 47.5 g / m2) using a coating device, and then dried for 4 minutes in a hot air dryer at 150°C to obtain a prepreg with a thickness of 80 μm.
[0128] (Laminated plate) Ultra-thin copper foil (Mitsui Mining & Smelting, Microthin FL, 1.5 μm) was laminated on both sides of the prepreg, and the laminate was heated and pressurized at a pressure of 3 MPa and a temperature of 225° C. for 2 hours to obtain a laminate with metal foil. The thickness of the core layer (the portion made of the resin substrate) of the obtained laminate with metal foil was 0.080 mm.
[0129] (Printed circuit board manufacturing) After the ultra-thin copper foil layer on the surface of the resin substrate with metal foil obtained in the previous section was roughened to a thickness of about 1 μm, a through hole of φ80 μm for interlayer connection was formed by a carbon dioxide laser. Next, it was immersed in a swelling liquid (Swelling Dip Securigant P, manufactured by Atotech Japan) at 60°C for 10 minutes, and further immersed in an aqueous potassium permanganate solution (Concentrate Compact CP, manufactured by Atotech Japan) at 80°C for 20 minutes, neutralized, and desmeared in the through hole. Next, electroless copper plating was performed to a thickness of 0.5 μm, a resist layer for electrolytic copper plating was formed to a thickness of 18 μm, pattern copper plating was performed, and post-curing was performed by heating at a temperature of 150°C for 30 minutes. Next, the plating resist was peeled off and the entire surface was flash etched to obtain an inner layer core circuit board with a pattern of L / S=15 / 15 μm and 60% remaining copper. Next, the prepregs obtained in the examples were placed on both sides of the inner layer core circuit board, and an ultra-thin copper foil (Mitsui Mining & Smelting Co., Ltd., Microthin FL, 1.5 μm) was layered on top of them, and the resulting laminate was heated and pressurized at a pressure of 3 MPa and a temperature of 225°C for 2 hours to obtain a multilayer laminate with metal foil. Next, blind vias were formed in the multilayer laminate using a carbon dioxide laser. The inside of the via was immersed in a swelling liquid (Swelling Dip Securigant P, manufactured by Atotech Japan) at 60°C for 10 minutes, and then immersed in an aqueous potassium permanganate solution (Concentrate Compact CP, manufactured by Atotech Japan: sodium permanganate concentration 60g / l, NaOH concentration 45g / l) at 80°C for 20 minutes, and then neutralized and desmeared inside the via. After the process of degreasing, catalyst application, and activation, an electroless copper plating film of about 0.5 μm was formed, a resist was formed, and a pattern of electroplated copper of 20 μm was formed using the electroless copper plating film as a power supply layer, and circuit processing was performed. Next, annealing was performed for 60 minutes at 200 ° C in a hot air drying device, and the power supply layer was removed by flash etching. Next, a solder resist layer was formed, and an opening was formed so that the semiconductor element mounting pad and the like were exposed. Finally, a plating layer consisting of an electroless nickel plating layer of 3 μm and an electroless gold plating layer of 0.1 μm was formed on the circuit layer exposed from the solder resist layer, and the obtained board was cut into a size of 50 mm × 50 mm to obtain a printed wiring board.
[0130] (Semiconductor package manufacturing) The semiconductor package was obtained by mounting a semiconductor element (TEG chip, size 10 mm x 10 mm, thickness 0.1 mm) having solder bumps on the obtained printed wiring board by heat and pressure bonding using a flip chip bonder. Next, the solder bumps were melted and bonded in an IR reflow furnace, and then liquid sealing resin (manufactured by Sumitomo Bakelite Co., Ltd., CRP-4152S) was filled, and the liquid sealing resin was then cured to obtain a semiconductor package. The liquid sealing resin was cured at a temperature of 150°C for 120 minutes. The solder bumps of the semiconductor element were formed from a eutectic of Sn / Pb composition. Finally, the semiconductor package was obtained by cutting into individual pieces of 14 mm x 14 mm size using a router.
[0131] The resin film with carrier, printed wiring board, and semiconductor package obtained using the above-mentioned resin varnish P (resin composition) were evaluated based on the following evaluation items and in accordance with the judgment criteria shown in Table 2. The results are shown in Table 1.
[0132] (1) Dielectric constant and dielectric tangent Four sheets of the obtained resin film with a carrier, each having a thickness of 30 μm, were stacked together and hot-pressed with copper foil at 225°C and 1 kgf / mm 2The resin film was cured by heating and pressing for 2 hours under the pressing conditions of 1. Next, the copper foil of the obtained cured product was removed by etching to produce a cured product as a sample. The dielectric constant and dielectric loss tangent at 10 GHz of the resulting cured product were measured by a cavity resonator method.
[0133] (2) Complex dynamic viscosity The PET film (carrier substrate) was peeled off from the obtained resin film with carrier, and the resin film in the B stage was prepared as a measurement sample. Next, a dynamic viscoelasticity test was carried out on this measurement sample using a dynamic viscoelasticity measuring device (manufactured by Anton Paar, device name Physica MCR-301) under the following conditions to measure the complex dynamic viscosity. (conditions) Frequency: 62.83rad / sec Measurement temperature: 50~200℃ Heating rate: 3℃ / min Geometry: Parallel plate Plate diameter: 10mm Plate spacing: 0.1mm Load (normal force): 0N (constant) Strain: 0.3% Measurement atmosphere: Air
[0134] (3) Peel strength The peel strength was measured in accordance with JISC6481. The sample used was a laminate with metal foil, electroplated with 30 μm copper.
[0135] (4) Glass transition temperature The dynamic viscoelasticity measurement was performed in accordance with JISC-6481 (DMA method) using a dynamic viscoelasticity device. The sample used was a laminate with metal foil that had been etched to remove the copper.
[0136] (5) Thermal expansion coefficient The thermal expansion coefficient was measured by preparing a 4 mm x 20 mm test piece using a TMA (thermomechanical analysis) device (TA Instruments, Q400) and measuring the linear expansion coefficient (CTE) at 50 to 100°C in the second cycle under the conditions of a temperature range of 30 to 300°C, 10°C / min, and a load of 5g. The sample used was a laminate with metal foil that had been etched to remove the copper.
[0137] (6) Laser processability The periphery of the bottom of the via hole of the above printed wiring board was observed with a scanning electron microscope (SEM), and the maximum smear length from the wall surface of the bottom of the via hole was measured from the obtained image. The smear removal performance was evaluated according to the standard from the maximum smear length. The plating penetration length was also observed.
[0138] (7) Formability The formability was evaluated according to the criteria by visually inspecting the embeddability of the outer copper foil of the printed wiring board in the inner layer pattern and by observing the cross section after etching the entire surface of the outer copper foil.
[0139] (8) Moisture absorption and solder heat resistance All of the copper foil on the metal foil laminate was etched away from except for half of one side of a 50 mm x 50 mm square sample, and the sample was treated for a specified period of time at 121°C and 2 atmospheres in a pressure cooker tester (manufactured by Espec Corporation), and then floated in a solder bath at 260°C for 60 seconds. The sample was then visually inspected for any abnormal changes in appearance and evaluated according to the criteria.
[0140] (9) Insulation The through-hole insulation reliability was evaluated by continuously measuring the through-hole wall distance of 0.1 mm on the printed wiring board under the conditions of an applied voltage of 5.5 V, a temperature of 130°C and a humidity of 85%, and was determined according to the standard. The measurement was terminated when the insulation resistance value became less than 106Ω.
[0141] [Table 1]
[0142] [Table 2] [Explanation of symbols]
[0143] 10 Resin film with carrier 20 Resin Film 30 Carrier substrate 50 Cover Film 100 Core Layer 102 Insulating layer 104 Beer Hall 106 Electroless metal plating film 108 Metal layer 200 Semiconductor Packages 202 Electroless metal plating film 204 Resist 206 Opening 208 Electrolytic metal plating layer 210 Opening 220 metal layer 230 Solder resist layer 240 Semiconductor Devices 250 solder bumps 260 Encapsulant layer
Claims
1. A high dielectric resin composition comprising: an epoxy resin (A), an inorganic filler (B) having a dielectric constant (1 MHz) of 6 or more, an inorganic filler (b) having a dielectric constant (1 MHz) of less than 6, a cyanate resin (C), and a coumarone resin (D), the epoxy resin (A) comprises at least one selected from the group consisting of biphenyl-type epoxy resins and phenol aralkyl-type epoxy resins, The inorganic filler (B) contains one or more selected from the group consisting of titanium oxide, alumina, and barium titanate, The content of the inorganic filler (B) is 30% by mass or less and 80% by mass or less with respect to the total amount of the high dielectric resin composition, A cured product of the high dielectric resin composition has a dielectric constant (Dk: εr) of 4 to 10 at 10 GHz, and a dielectric loss tangent (Df: tan δ) of 0.003 to 0.015 at 10 GHz.
2. 2. The highly dielectric resin composition according to claim 1, wherein the inorganic filler (B) does not include one having a perovskite structure.
3. 3. The highly dielectric resin composition according to claim 1, wherein a cured film made of the highly dielectric resin composition has a peel strength against copper foil of 0.5 kN / m or more.
4. The highly dielectric resin composition according to any one of claims 1 to 3, wherein the minimum value of complex dynamic viscosity η1 in a dynamic viscoelasticity test of the highly dielectric resin composition is 50 to 200 ° C., at a temperature rise rate of 3 ° C. / min and at a frequency of 62.83 rad / sec.
5. The highly dielectric resin composition according to claim 1 , wherein the inorganic filler (B) is surface-treated with an inorganic substance and an organic substance.
6. The highly dielectric resin composition according to claim 1 , wherein the cyanate resin (C) comprises a butadiene-modified cyanate.
7. A high dielectric resin composition described in any one of claims 1 to 6, wherein the inorganic filler (b) having a dielectric constant (1 MHz) of less than 6 is one or more selected from talc, calcined clay, uncalcined clay, mica, glass, titanium oxide, alumina, boehmite, silica, fused silica, calcium carbonate, magnesium carbonate, hydrotalcite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide, barium sulfate, calcium sulfate, calcium sulfite, zinc borate, barium metaborate, aluminum borate, calcium borate, sodium borate, aluminum nitride, boron nitride, silicon nitride, and carbon nitride.
8. A cured product of the highly dielectric resin composition according to any one of claims 1 to 7.
9. A prepreg comprising a fiber base material in the highly dielectric resin composition according to any one of claims 1 to 7.
10. A laminate comprising the prepreg according to claim 9 and a metal layer disposed on at least one surface of the prepreg.
11. A carrier substrate; A resin film formed on the carrier substrate and made of the high dielectric resin composition according to claim 1 ; A resin film with a carrier.
12. A printed wiring board comprising an insulating layer made of a cured product of the highly dielectric resin composition according to claim 1 .
13. The printed wiring board according to claim 12; a semiconductor element mounted on a circuit layer of the printed wiring board or embedded in the printed wiring board.
Citation Information
Patent Citations
Printed-wiring board and electronic component
JP2006059999A
Resin composition
JP2017014406A
Resin composition
JP2017179014A
Curable resin composition, dry film, cured product, laminate structure and electronic component
JP2020055927A
Resin composition, prepreg, metal foil-clad laminated sheet, resin sheet, and printed wiring board