Thin film carbon material and its manufacturing method

The use of argon gas cluster ion-assisted irradiation and an optional intermediate layer in DLC film production addresses the issue of residual stress, resulting in a durable, low-friction, and long-lasting carbon film for wear-resistant applications.

JP7581680B2Active Publication Date: 2024-11-13NOMURA PLATING CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020120427
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-07-14
Publication Date
2024-11-13
Estimated Expiration
2040-07-14

AI Technical Summary

Technical Problem

Existing DLC thin films suffer from high residual stress due to high-energy ion bombardment, leading to micro-chipping, peeling, and reduced lifespan despite their high hardness and density, which affects their wear resistance and peeling resistance.

Method used

A thin film carbon material produced by argon gas cluster ion-assisted irradiation with controlled energy and argon-to-carbon atom ratio, forming a dense diamond-like carbon film with low residual stress, and optionally incorporating an intermediate layer of silicon, chromium, tungsten, or their carbides to enhance bonding strength.

Benefits of technology

The resulting film exhibits low residual stress, high wear resistance, and improved peeling resistance, with a smooth surface and extended lifespan, suitable for sliding and wear-resistant applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581680000002
    Figure 0007581680000002
  • Figure 0007581680000003
    Figure 0007581680000003
  • Figure 0007581680000004
    Figure 0007581680000004
Patent Text Reader

Abstract

To provide a thin film carbon material excellent in abrasion resistance and peeling resistance in order to further extend the life of a DLC film, and a method for producing the same.SOLUTION: When forming a thin film carbon material consisting only of carbon excluding impurities which has a film thickness of 50 nm to 1 μm with a density and hardness determined by using an indentation type hardness meter in a density and hardness range surrounded by 4 points: A (density 2.90 g / cm3, hardness 45 GPa), B (density 2.90 g / cm3, hardness 35 GPa), C (density 3.20 g / cm3, hardness 55 GPa) and D (density 3.20 g / cm3, hardness 45 GPa) and which has a vapor-deposited surface formed by argon gas cluster ion-assisted irradiation, the ratio of the number of carbon atoms to the number of argon atoms is set to 1: 500 to 30,000, and argon is accelerated to 7 to 20 eV per atom.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thin film carbon material that is used for wear-resistant components such as sliding members of machine parts and tools and has excellent peeling resistance, and a manufacturing method thereof. The thin film carbon material can also be used for biomaterials that are expected to have properties similar to those of diamond. [Background technology]

[0002] Carbon-based thin films used in sliding and wear-resistant components are made of diamond or a material generally known as DLC (Diamond-like-carbon). Diamond thin films, the hardest material, have strong crystals and rough surfaces that are difficult to mirror finish, so their use as sliding components is limited.

[0003] Meanwhile, DLC is classified into four types according to ISO20523: ta-C, aC, ta-C:H, and aC:H. Of the four types, ta-C:H and aC:H are carbon materials that generally contain a large amount of hydrogen (10-40 at%) in their composition, and have a low hardness of 30 GPa or less, resulting in a short lifespan for the components. In addition, ta-C and aC are basically carbon materials that do not contain hydrogen, and their CC bonds are the SP bonds of diamond. 3 Hybrid orbital bonding and SP in graphite 2 Classified according to the ratio of hybrid orbital bonds, ta-C is known to be a material with high hardness and density, with diamond bonds predominating. However, while some ta-C exhibit high hardness of over 70 GPa, the method of producing ta-C involves bombarding the substrate with carbon ions at high energy in order to make diamond bonds predominate over graphite bonds, which results in large residual stress in the carbon film. This results in low adhesion strength and brittleness, which leads to a short lifespan.

[0004] There are two methods for producing DLC ​​films, which are carbon materials: CVD (chemical vapor deposition) and PVD (physical vapor deposition). Both methods use stable graphite SP 2Carbon in the raw material, which is the carbon source, such as a carbon target having hybrid orbital bonds or methane gas, is ionized, or carbon and carbon ions are ionized together with argon in the atmospheric gas, and bombarded with high energy to form diamond SPs with carbon bonds. 3 By forming a carbon film with an increased amount of hybrid orbital bonds, a high-hardness DLC can be produced. By performing this high-energy ion bombardment simultaneously with film formation, it is possible to increase the hardness and density at the same time.

[0005] In Non-Patent Document 1, the film density and film hardness of various types of DLC films produced by various film formation methods currently used for DLC film formation (arc ion plating method, sputtering method, CVD method), and the C-C bond (SP 2 Hybrid orbital bonds and SP 3 The relationship between the density and hardness of the DLC film and the ratio of hybrid orbital bonds was evaluated. As a result, even though the DLC films were produced using different deposition methods and conditions, the relationship between the film density and hardness of the DLC film, as shown in Figure 1 in particular, shows a linear relationship over a wide range from low hardness to high hardness (15 GPa to 80 GPa).

[0006] Patent Document 1 discloses a method for manufacturing a molding member, in which a metal or ceramic intermediate layer is formed on a substrate surface under gas cluster ion beam assisted irradiation, and then a carbon film is formed under gas cluster ion beam assisted irradiation. The carbon film obtained by this method has excellent hardness, flatness, heat resistance, etc., and can be used as a protective film for precision molding dies, etc., and it is also disclosed that the carbon film has excellent adhesion to the substrate at low to high temperatures. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2005-169816 A [Non-patent literature]

[0008] [Non-Patent Document 1] Kanagawa Prefectural Industrial Technology Center Research Report (December 2011, Issue 17, Pages 9-12) Title: "Relationship between film density, film hardness, and Raman spectrum of DLC films produced using different film formation methods and conditions" Summary of the Invention [Problem to be solved by the invention]

[0009] The present invention relates to a thin carbon film material used for wear-resistant members such as sliding members and tools, and is a long-life DLC (Diamond-like-carbon) thin film material that is excellent in wear resistance and peeling resistance. The long life of a wear-resistant member is achieved not only by the property of low friction wear with a mating material due to high hardness, but also by a combination of properties such as resistance to minor chipping and peeling. In particular, DLC thin film materials require the conversion of the C-C bonds of the carbon components in a carbon target or a hydrocarbon gas to diamond-type bonds, so that a diamond-like carbon film is produced by ionizing carbon, accelerating it with a voltage, and impacting the substrate with high energy. Although the high-energy impact can achieve high hardness and high density of the thin carbon film material, there is a problem in that a strong compressive residual stress remains in the thin film, making it easy to cause minor chipping and film peeling.

[0010] In industrial applications of thin films, including DLC ​​films, used in machine parts and tools, high hardness properties, including wear resistance, are important. Indentation hardness testers are used to measure the hardness of thin films, including DLC ​​films. Hardness measured with an indentation hardness tester is determined from the relationship between the applied load and the indentation depth (surface area of ​​the indentation). Unlike conventional Vickers hardness (which measures plastic deformation), the hardness is the sum of plastic deformation and elastic deformation, and measures the deformation resistance.

[0011] If residual stress exists in the film, the yield strength will change, so it is natural to think that the hardness will change due to the residual stress. As mentioned above, residual stress is caused by the impact of ions accelerated with high energy. In general ceramic thin films such as titanium nitride, metal ions such as titanium are accelerated at 50 to 100 V in a vacuum and impact the substrate, but in the case of DLC films, they are impacted with the substrate at high speeds of 100 V to several kV, which simultaneously densifies the film and converts it into diamond. It is believed that the strong residual stress caused by this high-speed impact increases the deformation resistance during hardness measurement, indicating high hardness.

[0012] On the other hand, in terms of density, graphite has a density of 2.2 g / cm 3 In comparison, diamond weighs about 3.5g / cm 3 As a guideline for turning carbon materials into diamond, not only hardness but also how close the film density is to diamond is extremely important, and film density is considered to be a more important factor than film hardness, which is easily affected by residual stress that can cause micro-cracks and peeling of the film. However, at present, not only is the film denser, but high-energy ion bombardment is required to promote the transformation into diamond, and the lifespan of DLC films cannot be further extended.

[0013] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a thin film carbon material having excellent abrasion resistance and peeling resistance, and a method for producing the same, in order to enable a further extension of the life of the DLC film. [Means for solving the problem]

[0014] The invention of claim 1 has a deposition surface formed by argon gas cluster ion assisted irradiation, and has a density and a hardness measured by a penetration hardness tester of A (density 2.90 g / cm 3 , hardness 45 GPa), B (density 2.90 g / cm 3 , hardness 35 GPa), C (density 3.20 g / cm 3 , hardness 55GPa), D(density 3.20g / cm 3 The density and hardness of the film thickness of 50 nm to 1 μm is the range surrounded by four points (hardness 45 GPa).Carbon with hydrogen content of 1 at% or less This is a thin film carbon material consisting of

[0015] The invention of claim 2 is a thin film carbon material characterized in that an intermediate layer film made of one or more of silicon, chromium, tungsten, titanium, and carbides thereof is formed on a surface of a substrate, and the carbon film of claim 1 is formed on the surface of the intermediate layer film.

[0016] The invention of claim 3 is a method for producing a thin film carbon material of claim 1 or 2, characterized in that when forming a carbon film by argon gas cluster ion assisted irradiation, the ratio of the number of carbon atoms to the number of argon atoms is 1:500-30000, and the argon is accelerated to 7-20 eV per atom. Effect of the Invention

[0017] The thin film carbon material of claim 1 has a high film density but low hardness, so the residual stress in the film is low and the film is not easily broken, and therefore has excellent peeling resistance. In addition, since it has an extremely flat surface, the sliding resistance is low, and together with the wear resistance due to the high density, it has the effect of extending the life of the material as a sliding member or wear-resistant member.

[0018] According to the invention of claim 2, the intermediate layer can increase the bonding strength of the carbon film, which has the effect of further improving peel resistance. In addition, if the intermediate layer is also formed under gas cluster ion beam assisted irradiation, it is possible to make the surface of the intermediate layer even flatter than the surface of the substrate, which further flattens the surface of the carbon film, thereby further reducing the sliding resistance, improving peel resistance and wear resistance, and providing a thin film carbon material with a longer life.

[0019] According to the invention of claim 3, by keeping the ion energy low during film formation, it is possible to produce a thin film carbon material with a long life, since the residual stress in the film can be kept low while the film density is high. [Brief description of the drawings]

[0020] [Figure 1] FIG. 1 is a diagram showing the relationship between hardness and density of a thin film carbon material of the present invention and a conventional thin film carbon material. [Diagram 2] FIG. 1 is a schematic diagram showing the overall configuration of a sliding scratch test device for evaluating durability. [Diagram 3] FIG. 1 is a diagram showing the appearance of parts used in a sliding scratch test device for durability evaluation. [Figure 4] FIG. 13 is a diagram showing surface observation images as results of a scratch test. [Diagram 5] FIG. 1 is a diagram showing a cross-sectional curve obtained by a contact needle type surface roughness meter as a result of a scratch test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] As shown in the ranges A, B, C, and D in Fig. 1, the thin-film carbon material of the present invention is a thin-film carbon material having a density closest to that of diamond, but a hardness of 35 GPa to 55 GPa, which is 20% or more lower than the maximum level of 70 GPa. This is produced under conditions where the ratio of the number of carbon atoms to the number of argon atoms is 1:500 to 30,000 and argon is accelerated to 7 to 20 eV per atom under argon gas cluster ion beam assisted irradiation, and compared to the film density and film hardness of DLC films produced by other film formation methods (arc ion plating method, sputtering method, CVD method), the hardness is low considering its high density.

[0022] Hardness is a key consideration for materials that require wear resistance, such as machine parts and tools. In general, an indentation hardness tester (nanoindentation method) is used to measure the hardness of thin films with a thickness of around 1 μm. Diamond, known as the hardest material, has an indentation hardness of 90 to 100 GPa. Meanwhile, other carbon materials that are the same as diamond include graphite and amorphous carbon (glassy carbon), which have a hardness of 10 GPa or less. Diamond-like carbon (DLC) is a material that has a C-C bond (SP 3 Hybrid orbital bonds) and CC bonds such as graphite (SP2 It is a carbon material that has both C-C bonds (hybrid orbital bonds) and shows a film hardness of 10 to 80 GPa, roughly depending on the ratio of the amount of C-C bonds between the two. In general, it is often thought that the wear resistance and hardness of parts correspond one-to-one, but in the case of DLC thin films in particular, hardness is a physical number that measures the resistance to deformation, and it is unreasonable to think that it coincides with wear resistance.

[0023] On the other hand, the density of carbon materials is 1.5 g / cm for amorphous carbon. 3 , and 2.2 g / cm for graphite with a two-dimensionally dense C-C bond structure. 3 whereas diamond, which has a three-dimensionally dense C-C bond structure, has a density of 3.5 g / cm 3 The density of DLC (Diamond-like-carbon) thin films is 2.0 to 3.2 g / cm depending on the C-C bond ratio. 3 The value ranges from 0.01 to 0.05. Producing high-quality thin-film DLC by CVD (chemical vapor deposition) or PVD (physical vapor deposition) means producing a carbon material with high density and hardness, that is, DLC in which the graphite C-C bonds, which are stable at room temperature and normal pressure, are excited into the high-energy diamond C-C bonds.

[0024] In the conventional DLC film fabrication method, in order to excite the C-C bonds in the carbon source such as carbon target or methane gas into diamond-type, carbon is ionized or an inert gas such as argon in the atmosphere is ionized, electrically accelerated, and bombarded with high energy on the substrate. DLC with different densities and hardness can be fabricated depending on the magnitude and amount of this ion energy. However, the ions in the conventional CVD and PVD methods are single atoms, and in order to form a film by the collision of a single atom with the substrate surface, a huge number of ion bombardments are required, and the carbon atoms that arrive must bond with nearby carbon atoms to form diamond-type C-C bonds. Furthermore, in order to aggregate the diamond-type C-C bonds over a wider surface and fabricate dense diamond-type DLC, even greater energy is required. From this, it is considered that the ion bombardment energy in the conventional DLC film fabrication method is 50 to 1000 keV, which is much higher than the C-C bond energy of diamond, 7.2 eV. Although the high-energy bombardment can achieve high hardness and high density of the DLC film, at the same time, strong compressive residual stress remains in the thin film. Since indentation hardness measurement is a measurement based on deformation resistance, strong compressive stress strongly affects the hardness, resulting in a high measured value. It is important to suppress the generation of compressive stress in the film as much as possible and promote excitation of the diamond-type C-C bonds.

[0025] Figure 1 shows the results of measuring the film density and film hardness of DLC films for 18 types of samples produced by 11 surface treatment manufacturers using their respective manufacturing methods. Film density was measured using an X-ray total reflection method (X-ray reflectometer), and film hardness was measured using a nanoindenter. The square marks indicate the measurement results for samples produced by various manufacturing methods, namely, CVD method, △ mark indicates the Arc method (arc ion plating method), and ○ mark indicates the SP method (sputtering method). From low to high film density samples, it is known that there is a fairly linear relationship between hardness and density, as shown by the straight line approximated by the least squares method. However, since these samples were produced by excessive ion bombardment, it is thought that strong residual stress was formed in the film, resulting in a high hardness compared to the film density. Furthermore, the strong compressive residual stress makes the film prone to destruction and peeling, and when such DLC thin films are applied to machine parts and tools, the lifespan is actually shortened, and the hardness and lifespan do not correspond.

[0026] In order to suppress the residual stress of the DLC film and form a dense, high-density thin film, it is necessary to deposit a carbonaceous material consisting only of carbon under argon gas cluster ion beam assisted irradiation, and to control the acceleration energy of the argon cluster to a low level that can stably form diamond-type C-C bonds, specifically 7 to 20 eV per argon atom. In order to form an even denser film, it is preferable to set the ratio of the number of atoms of the carbon material to be deposited to the number of argon atoms to be assisted irradiated to 1:500 to 30,000. By forming a film under these conditions, the density and hardness measured by a penetration hardness tester will be greater than A (density 2.90 g / cm 3 , hardness 45 GPa), B (density 2.90 g / cm 3 , hardness 35 GPa), C (density 3.20 g / cm 3 , hardness 55GPa), D(density 3.20g / cm 3 A DLC thin film having a hardness of 45 GPa or less can be produced. The argon cluster size under these conditions is preferably 100 to 5000, and more preferably 500 to 2000.

[0027] The DLC film thickness of the present invention is preferably 50 nm to 1 μm. If the film thickness is thicker than 1 μm, the film is likely to peel off when used in mechanical parts and other applications where strong stress is applied to the film. The DLC film of the present invention has small residual stress, a density close to that of diamond, and a small coefficient of friction because of excellent surface flatness due to gas cluster ion beam assisted irradiation. For this reason, even a thin film thickness of 100 nm or less exhibits excellent wear resistance and a long life.

[0028] It is known that the deposition surface formed by argon gas cluster ion assisted irradiation can have good flatness with a surface roughness (Ra) of 0.1 μm or less. For example, according to Patent Document 1 (paragraphs 0077 to 0079), the surface roughness (Ra) can be 10 nm or less, and more preferably, the surface roughness (Ra) can be 5 nm or less.

[0029] It is desirable that the DLC film of the present invention does not contain hydrogen. Hydrogen easily bonds with carbon to form C-H bonds. This C-H bond is contrary to the purpose of increasing the C-C bonds of diamond by cluster ion beam assisted irradiation. For this reason, it is preferable to form the DLC film under high vacuum and using raw materials that do not contain hydrogen. However, hydrogen is generated by decomposition of water molecules adhering to the walls of the vacuum furnace. Even if the amount of hydrogen generated is small, carbon easily bonds with hydrogen and is easily incorporated into the DLC. C-H bonds in DLC can also cause a decrease in DLC density. The amount of hydrogen contained in DLC is preferably 1 at% or less, more preferably 0.5 at% or less.

[0030] In the present invention, in order to increase the bonding strength between the DLC thin film and the substrate, an intermediate layer made of one or more of silicon, chromium, tungsten, titanium, and their carbides can be provided. These metals react with carbon to easily form carbides. It is also preferable for carbon to diffuse into the interface between the DLC thin film and the intermediate layer to form a very thin diffusion layer in order to increase the bonding strength between the two. The thickness of the intermediate layer is not particularly limited, but is preferably equal to or less than the thickness of the DLC thin film.

[0031] The present invention will be described in more detail below by showing examples based on the test results of the present invention. Of course, the present invention is not limited to the following examples, and various more specific embodiments can be taken as a matter of course. EXAMPLES

[0032] A carbonaceous material was deposited under argon gas cluster ion beam-assisted irradiation to produce a DLC thin film with a thickness of 200 nm on the surface of a Si substrate. As shown in Table 1, the film formation conditions were set to variables of the acceleration energy per argon atom and the ratio of the number of carbon atoms to the number of argon atoms, and samples 1 to 4 of the present invention and samples 1 to 3 for comparison were produced. In addition, the hardness of each sample was measured using a nanoindenter, and the film density was measured using an X-ray total reflection method.

[0033] [Table 1]

[0034] All of the samples 1 to 4 of the present invention showed hardness and density within the range of the present invention. In the comparative sample 1, although the number of carbon atoms was large relative to the number of argon atoms, the acceleration voltage was excessively larger than the C-C bond energy of diamond, 7.2 eV, so a large stress remained in the film and a high-hardness coating was formed, but the density decreased because the film grew while destroying the C-C bonds of diamond. In the comparative sample 2, an acceleration voltage slightly higher than the C-C bond energy of diamond, 7.2 eV, was applied, but since the number of argon atoms was small relative to the number of carbon atoms supplied for coating formation, the energy to form the C-C bonds of diamond was insufficient, resulting in a graphite C-C bond state, and the coating could not be densified and was formed as a porous coating. In the comparative sample 3, the number of carbon atoms was small relative to the number of argon atoms, so no coating was formed. EXAMPLES

[0035] A 600 nm thick DLC thin film was formed on the surface of a titanium substrate under argon gas cluster ion beam assisted irradiation under the conditions of invention 2, and designated invention sample 5. In addition, a 300 nm thick DLC was prepared by arc ion plating at an acceleration voltage of 100 eV, and a 700 nm thick DLC was prepared by CVD at an acceleration voltage of 1 keV, and designated comparative samples 4 and 5, respectively. Comparative sample 4 had a hardness of 72 GPa and a density of 3.1 g / cm. 3 Comparative sample 5 has a hardness of 20 GPa and a density of 2.1 g / cm 3 Each sample was subjected to a scratch test using a stainless steel scaler at a force of 3.9 N. Figure 2 shows the scratch test device, and Figure 3 shows the scratch test method.

[0036] (Scratching and curettage evaluation test) In order to evaluate the susceptibility of the sample surface to scratches, a dental scaler was pressed against the surfaces of the present invention sample 5 and the comparative samples 4 and 5 with a load of F = 3.9N (about 400g weight) using a sliding scratch tester shown in Figure 2, and a repeated scratch test was performed 20,000 times. In Figure 2, 1 is a test device, 2 is a scaler, 3 is a jig for supporting the scaler, 4 is a hexagonal socket bolt for positioning and fixing the scaler 2 to the jig 3, 5 is a load application part, 6 is a screw for connecting the jig 3 and the load application part 5, and 7 is a test piece. The tip of the scaler 2 is pressed against the surface of the test piece 7 with a predetermined load F by the load application part 5. In this state, the test piece 7 moves relative to the scaler 2, and the sliding scratch test is performed.

[0037] Figure 3 is an explanatory diagram showing the vicinity of the tip of the scaler 2, as seen from the direction of load F in Figure 2. A load (3.9 N) is applied to the cutting edge at the tip, and the scaler is moved back and forth in the sliding and scratching direction shown in the figure to scratch the surface of the test piece 7. The scaler 2 used was a Gracy Scaler (G curette point type #G7) made by YDM Corporation, made of SUS440C (HV ≒ 640).

[0038] As a result of the scratch test, FIG. 4 shows a surface observation image, and FIG. 5 shows a cross-sectional curve obtained by a contact needle type surface roughness meter. In FIG. 4 and FIG. 5, (a) shows the test results of the present invention sample 5, (b) shows the test results of the comparative sample 4, and (c) shows the test results of the comparative sample 5. In the present invention sample 5 prepared under argon gas cluster ion beam assisted irradiation, shallow scratch marks can be observed after 20,000 repeated scratch tests, but there is no evidence of the coating being worn from the cross-sectional curve. The scratch marks are thought to be due to the plastic deformation of the substrate, which is soft and has a hardness of HV140, and therefore the DLC of the present invention showed sufficient strength against film destruction. On the other hand, the DLC film of the comparative sample 4 prepared by the arc ion plating method was significantly destroyed after 20 to 50 scratch tests, so the test was stopped after 50 times. The destruction is also clear from the cross-sectional curve of the scratch marks, and it is thought that the film was destroyed due to the plastic deformation of the substrate due to the large residual stress in the film, and the titanium surface was exposed early. In addition, the comparative sample 5, which was produced by the plasma CVD method, was able to withstand 20,000 repeated scratch tests, but showed larger wear marks than the product of the present invention. The concave cross-sectional curve of the scratch marks indicates that the coating has been worn away, and the adhesion of tiny pieces of titanium wear to the cutting edge of the scaler definitely indicates that microscopic film destruction has occurred.

[0039] The high-density DLC containing a large amount of diamond C-C bonds produced by the present invention under argon gas cluster ion beam-assisted irradiation does not have a large residual compressive stress and is resistant to film peeling and destruction, and can be used for machine parts and tool components that require low friction, high wear resistance, and long life.

Claims

1. The deposition surface was formed by argon gas cluster ion assisted irradiation, and the density and hardness measured by a penetration hardness tester were A (density 2.90 g / cm 3 , hardness 45 GPa), B (density 2.90 g / cm 3 , hardness 35 GPa), C (density 3.20 g / cm 3 , hardness 55 GPa), D (density 3.20 g / cm 3 A thin film carbon material having a density and hardness in the range surrounded by four points (a thickness of 50 nm to 1 μm and a hydrogen content of 1 at % or less).

2. 10. A thin film carbon material comprising an intermediate layer film made of one or more of silicon, chromium, tungsten, titanium and carbides thereof formed on a surface of a substrate, and the carbon film of claim 1 formed on the surface of the intermediate layer film.

3. 3. The method for producing a thin film carbon material according to claim 1 or 2, characterized in that, when forming a carbon film by argon gas cluster ion assisted irradiation, the ratio of the number of carbon atoms to the number of argon atoms is set to 1:500 to 30,000, and the argon is accelerated to 7 to 20 eV per atom.

Citation Information

Patent Citations

  • Method for depositing carbonaceous hard film and system therefor

    JP2001192807A

  • DLC coated tool

    JP2005022073A

  • Molding member having heat-resistant carbon film, and method and apparatus for manufacturing the same

    JP2005169816A

  • Diamond-like carbon (DLC) film and DLC coated die