Biaxially oriented polyester film
A biaxially oriented polyester film with controlled expansion coefficients and surface properties addresses dimensional instability and smoothness issues, enhancing stability and reducing data loss in high-density magnetic recording media.
Patent Information
- Application Number
- JP2020159795
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-30
- Filing Date
- 2020-09-24
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-09-24
AI Technical Summary
Existing biaxially oriented polyester films do not adequately address dimensional stability and surface smoothness across various temperature and humidity ranges, leading to issues with high-density magnetic recording media, such as data loss and missing pulses due to environmental changes.
A biaxially oriented polyester film with specific expansion coefficients, surface roughness, and structural properties, including a humidity expansion coefficient of 4.5-6.5 ppm/%RH, temperature expansion coefficient of -3.0-7.0 ppm/°C, and surface protrusions controlled to 60 nm or more, ensuring dimensional stability and smoothness.
The film exhibits excellent slitting properties and dimensional stability, reducing missing pulses and data loss in high-density magnetic recording media by maintaining stability across temperature and humidity changes.
Smart Images

Figure 0007581733000009 
Figure 0007581733000001 
Figure 0007581733000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a biaxially oriented polyester film having excellent dimensional stability and surface properties, and to a biaxially oriented polyester film that can be suitably used as a base film for coating-type magnetic recording media such as data storage. [Background technology]
[0002] Biaxially oriented polyester films are used in various applications due to their excellent thermal properties, dimensional stability, mechanical properties, and ease of control of surface morphology, and are particularly well known for their usefulness as supports for magnetic recording media, etc. Magnetic recording media are always required to achieve high density recording.
[0003] Generally, there are three methods for achieving high density recording: increasing the number of tracks, shortening the recording wavelength, and increasing the tape length.
[0004] Increasing the number of tracks narrows the width of each track, so even slight dimensional changes can cause data loss, making it important to control the dimensional stability across the width of the tape. Such dimensional changes can be divided into irreversible changes such as thermal contraction and reversible changes such as expansion and contraction due to temperature and humidity. It is preferable that there are no irreversible changes, but they can be removed by annealing or other processes during processing. In contrast, reversible changes cannot be easily removed, so if the temperature and humidity change during storage, the film will expand or contract, causing the recorded data to shift from its original position and become unreadable.
[0005] Furthermore, in order to achieve sufficient electromagnetic conversion characteristics while shortening the recording wavelength, surface smoothness is required, and it is effective to further improve the smoothness of the magnetic layer surface by making the magnetic layer thinner or by using fine particle magnetic material.
[0006] In recent magnetic recording medium supports made of ferromagnetic hexagonal ferrite powder, the magnetic layer, non-magnetic layer, backcoat layer, and even the support itself have become thinner, and as a result, the roughness of not only the smooth surface but also the running surface has been restricted. When the magnetic recording medium is stored in a rolled state during the manufacturing process, the protrusions formed on the running surface are transferred to the magnetic surface, forming depressions on the smooth magnetic layer surface, and as the support becomes thinner, large particles contained in the support are pushed up onto the smooth surface, generating gentle convex waves on the magnetic layer surface, which reduces the smoothness of the magnetic layer surface and causes an error signal (missing pulse). If the particles contained in the support are made smaller in diameter to increase the smoothness of the magnetic layer surface and the smoothness is improved to create an ultra-high-definition surface, the running property, winding property, and even surface durability become insufficient. Therefore, the demand for improvement in properties such as compatibility between slitting property and surface smoothness can be said to be a constant issue for high-density recording.
[0007] In order to solve the above problems, polyester films with excellent dimensional stability in temperature and humidity ranges that can respond to all environmental changes (e.g., Patent Documents 1 and 2) have been studied. However, the reality is that a support surface that can ensure the smoothness of the magnetic layer surface using a thin magnetic layer or fine magnetic material such as ferromagnetic hexagonal ferrite powder has not been obtained. In addition, there are polyester films that are excellent in humidity expansion and that achieve both runnability and smoothness by controlling the number of protrusions of a specific height (e.g., Patent Documents 3 and 4), and polyester films that achieve both dimensional stability against heat and film rigidity (e.g., Patent Document 5). [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2005-163020 A [Patent Document 2] JP 2015-25047 A [Patent Document 3] JP 2016-79410 A [Patent Document 4] JP 2018-150463 A [Patent Document 5] JP 2000-141475 A Summary of the Invention [Problem to be solved by the invention]
[0009] However, none of these methods take into consideration thermal expansion at all, and no film has been developed that exhibits excellent dimensional change over the entire range of temperatures and humidities, from room temperature to high temperature and humidity.
[0010] An object of the present invention is to stably provide a biaxially oriented polyester film which has excellent dimensional stability in all temperature and humidity ranges, including low temperature and low humidity, low temperature and high humidity, high temperature and low humidity, and which also has excellent surface smoothness and slitting properties. [Means for solving the problem]
[0011] The present invention, which has been made to solve the above problems, is characterized by the following configurations.
[0012] (1) The humidity expansion coefficient in the width direction is 4.5 to 6.5 ppm / % RH, the temperature expansion coefficient in the width direction is -3.0 to 7.0 ppm / °C, and the number of protrusions having a height of 60 nm or more on at least one outermost layer surface is 0 to 200 / mm 2 A biaxially oriented polyester film.
[0013] (2) The biaxially oriented polyester film according to (1) above, having a heat shrinkage rate in the width direction of 1.0% or less.
[0014] (3) The biaxially oriented polyester film according to (1) or (2), having a Young's modulus in the transverse direction of 7.0 to 12.0 GPa.
[0015] (4) The biaxially oriented polyester film according to any one of (1) to (3) above, which has a minute melting peak temperature (T-meta) of 210 to 240°C.
[0016] (5) The biaxially oriented polyester film according to any one of (1) to (4) above, wherein at least one surface roughness (Sa1) is 3.0 to 7.0 nm.
[0017] (6) The biaxially oriented polyester film according to (5) above, wherein the surface roughness (Sa2) of the outermost layer surface opposite to the surface constituting Sa1 is 0.5 to 5.0 nm.
[0018] (7) The biaxially oriented polyester film according to any one of (1) to (6) above, which is used as a base film for a coating-type digital recording medium. Effect of the Invention
[0019] The biaxially oriented polyester film of the present invention is a biaxially oriented polyester film that has excellent slitting properties and dimensional stability in all temperature and humidity ranges, including low temperature and low humidity, low temperature and high humidity, high temperature and low humidity, and high temperature and high humidity.When made into a magnetic recording medium, it is possible to obtain a biaxially oriented polyester film that serves as a high-density magnetic recording medium having a smooth magnetic layer, little dimensional change due to environmental changes in temperature and humidity and due to storage, and in which the generation of missing pulses is suppressed. [Brief description of the drawings]
[0020] [Figure 1] FIG. 2 is a schematic diagram of a film dimension measuring device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] The polyester used in the present invention may be, for example, a polymer having an acid component such as an aromatic dicarboxylic acid, an alicyclic dicarboxylic acid, or an aliphatic dicarboxylic acid, or a diol component as a constituent unit (polymerization unit). The polyester film in the present invention refers to a film whose main component is polyester.
[0022] Examples of the aromatic dicarboxylic acid component include terephthalic acid, isophthalic acid, phthalic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, and 4,4'-diphenylsulfonedicarboxylic acid. Of these, terephthalic acid, phthalic acid, and 2,6-naphthalenedicarboxylic acid are preferably used. Examples of the alicyclic dicarboxylic acid component include cyclohexanedicarboxylic acid. Examples of the aliphatic dicarboxylic acid component include adipic acid, suberic acid, sebacic acid, and dodecanedioic acid. Only one of these acid components may be used, or two or more of them may be used in combination.
[0023] As the diol component, for example, ethylene glycol, 1,2-propanediol, 1,3-propanediol, neopentyl glycol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,2-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,4-cyclohexanedimethanol, diethylene glycol, triethylene glycol, polyalkylene glycol, 2,2'-bis(4'-β-hydroxyethoxyphenyl)propane, etc. can be used, among which, ethylene glycol, 1,4-butanediol, 1,4-cyclohexanedimethanol, diethylene glycol, etc. can be preferably used, and particularly preferably, ethylene glycol, etc. can be used. Only one of these diol components may be used, or two or more of them may be used in combination.
[0024] The polyester may be copolymerized with monofunctional compounds such as lauryl alcohol and phenyl isocyanate, or with trifunctional compounds such as trimellitic acid, pyromellitic acid, glycerol, pentaerythritol, and 2,4-dioxybenzoic acid, without excessive branching or crosslinking, so long as the polymer is substantially linear. In addition to the acid component and diol component, aromatic hydroxycarboxylic acids such as p-hydroxybenzoic acid, m-hydroxybenzoic acid, and 2,6-hydroxynaphthoic acid, as well as p-aminophenol and p-aminobenzoic acid, may be further copolymerized in small amounts that do not impair the effects of the present invention.
[0025] The copolymerization ratio of the polymer can be investigated by the NMR method (nuclear magnetic resonance method) or the microscopic FT-IR method (Fourier transform microscopic infrared spectroscopy method).
[0026] The polyester can be preferably used with a glass transition temperature of less than 150° C. in order to be able to perform biaxial stretching and to realize the effects of the present invention, such as dimensional stability. The polyester used in the present invention is preferably polyethylene terephthalate or polyethylene naphthalate (polyethylene-2,6-naphthalate), and may also be a copolymer or modified product thereof, or a polymer alloy with other thermoplastic resins. The polymer alloy here means a polymer multicomponent system, and may be a block copolymer by copolymerization, or a polymer blend by mixing or the like. In particular, the polyester used in the present invention is more preferably mainly composed of polyethylene terephthalate, since a process for increasing the crystallite size and the degree of crystal orientation can be easily applied. Here, the main component means 80% by mass or more in the film composition.
[0027] When the polyethylene terephthalate used in the present invention is used as a polymer alloy, the other thermoplastic resin is preferably a polymer compatible with polyester, more preferably a polyetherimide resin, etc. As the polyetherimide resin, for example, the following can be used.
[0028] [ka]
[0029] (In the above formula, R1 is a divalent aromatic or aliphatic residue having 6 to 30 carbon atoms, and R2 is a divalent organic group selected from the group consisting of a divalent aromatic residue having 6 to 30 carbon atoms, an alkylene group having 2 to 20 carbon atoms, a cycloalkylene group having 2 to 20 carbon atoms, and a polydiorganosiloxane group chain-terminated with an alkylene group having 2 to 8 carbon atoms.) Examples of R1 and R2 above include aromatic residues represented by the following formulae:
[0030] [ka]
[0031] (n is an integer of 2 or more, preferably an integer of 20 to 50.) In the present invention, from the viewpoints of affinity with polyester, cost, melt moldability, and the like, a polymer having a repeating unit represented by the following formula, which is a condensation product of 2,2-bis[4-(2,3-dicarboxyphenoxy)phenyl]propane dianhydride and m-phenylenediamine or p-phenylenediamine, is preferred.
[0032] [ka]
[0033] or
[0034] [ka]
[0035] The polyetherimides are available from SABIC Innovative Plastics under the "Ultem" trade name and are known by such trademark names as the "Ultem® 1000," "Ultem® 1010," "Ultem® 1040," "Ultem® 5000," "Ultem® 6000," and "Ultem® XH6050" series, as well as "Extem® XH" and "Extem® UH."
[0036] In the present invention, for example, the method of mixing polyester and polyimide includes a method of pre-melting and kneading (pelletizing) a mixture of polyester and polyimide before melt extrusion to form a master chip, and a method of mixing and melt kneading during melt extrusion. Among them, a method of pre-melting and forming a master chip using a high shear mixer such as a twin-screw extruder that applies shear stress is preferably exemplified. In that case, the mixed master chip raw material may be put into a normal single-screw extruder to be melt-formed into a film, or may be directly sheeted without forming a master chip in a state where high shear is applied. When mixing with a twin-screw extruder, it is preferable to use a twin-screw extruder equipped with a three-screw twin-screw or two-screw twin-screw type screw from the viewpoint of reducing poorly dispersed materials. In addition, when mixing polyester and polyimide, since there is a difference in melt viscosity, it is preferable to prepare a master chip in which the polyimide resin is mixed at a high concentration, and in particular, it is preferable to set the mixing weight ratio of polyester / polyimide to 10 / 90 to 70 / 30, and more preferably to be in the range of 30 / 70 to 60 / 40.
[0037] In the present invention, the content of the polyimide resin in the polyester film is preferably 0.1% by weight to 20% by weight or less, more preferably 3% by weight to 15% by weight or less, and even more preferably 5% by weight to 10% by weight or less, based on the entire film. If the content exceeds the upper limit, the humidity expansion coefficient in the width direction of the present invention may not be obtained.
[0038] The humidity expansion coefficient in the width direction of the biaxially oriented polyester film of the present invention is 4.5 to 6.5 ppm / % RH, preferably 5.0 to 6.0 ppm / % RH. If the humidity expansion coefficient is greater than 6.5 ppm / % RH, the film expands in the width direction in response to humidity changes in the environment in which magnetic data is recorded and reproduced, which makes reproduction failure more likely to occur. If the humidity expansion coefficient is less than 4.5 ppm / % RH, it may be difficult to control the temperature expansion coefficient of the film within the range of the present application. The humidity expansion coefficient in the width direction can be controlled by the width direction stretching ratio described later. If the stretching ratio is increased, the humidity expansion coefficient decreases. However, if the stretching ratio in the width direction is increased, the temperature expansion coefficient may become too small together with the humidity expansion coefficient, so it is important to adjust the stretching ratio and the heat setting temperature.
[0039] The temperature expansion coefficient in the width direction of the biaxially oriented polyester film of the present invention is -3.0 to 7.0 ppm / °C, preferably -2.0 to 5.0 ppm / °C. If the temperature expansion coefficient is below -3.0 ppm / °C, the film will shrink significantly in the width direction in response to temperature changes in the environment in which magnetic data is recorded and reproduced. On the other hand, the magnetic head expands in response to temperature changes (usually 7 ppm / °C), which makes it easy for reproduction defects to occur due to excessive dimensional changes between the two. If the temperature expansion coefficient exceeds 7.0 ppm / °C, the humidity expansion coefficient cannot be controlled within the range of the present application, and the film will expand in the width direction in response to changes in temperature and humidity in the environment in which magnetic data is recorded and reproduced, making it easy for reproduction defects to occur. The temperature expansion coefficient in the width direction can be controlled by the width direction stretching ratio described later. The temperature expansion coefficient decreases when the stretching ratio is increased. In order to keep the temperature and humidity expansion coefficient in the width direction within the range of the present invention, it is important to adjust the width direction stretching ratio and heat setting temperature. Furthermore, it is preferable that the film contains 2 to 20% by weight or less, preferably 3 to 15% by weight or less, and more preferably 5 to 10% by weight or less of polyetherimide, since this makes it easier to obtain the temperature and humidity expansion coefficient in the width direction of the present invention.
[0040] The number of protrusions having a height of 60 nm or more on the surface of at least one outermost layer of the biaxially oriented polyester film of the present invention is 0 to 200 / mm 2 , preferably 0 to 150 pieces / mm 2 , and more preferably 0 to 100 pieces / mm 2 The number of protrusions with a height of 60 nm or more is 200 / mm 2 If it exceeds this value, the surface smoothness will deteriorate and missing pulses may occur.
[0041] The number of protrusions having a height of 60 nm in the present invention is the number of protrusions at a height of 60 nm from a reference surface determined by scanning white light interference microscope measurement. 2 If it exceeds this value, for example, when the magnetic recording tape is wound up, the irregularities on the surface of the backcoat layer are transferred to the surface of the magnetic layer, increasing the number of transfer marks and the frequency of occurrence of missing pulses.
[0042] The heat shrinkage ratio in the width direction of the biaxially oriented polyester film of the present invention is preferably 1.0% or less. If the heat shrinkage ratio in the width direction exceeds 1.0%, the film may shrink in the width direction during the processing step of the magnetic recording medium, causing wrinkles on the surface of the magnetic recording medium and reducing the smoothness of the magnetic layer surface.
[0043] The biaxially oriented polyester film of the present invention preferably has a Young's modulus in the width direction of 7.0 to 12.0 GPa, and more preferably 7.0 to 11.0 GPa from the viewpoint of controlling the humidity expansion coefficient in the width direction. When the Young's modulus in the width direction is within the above range, the dimensional stability against environmental changes during recording and reproduction of the magnetic recording medium tends to be good when used for the magnetic recording medium. The Young's modulus in the width direction can be controlled by the temperature and ratio of TD stretching 1 and 2 described later. In particular, the total TD ratio has an effect, and the higher the total TD ratio, the higher the TD Young's modulus.
[0044] The biaxially oriented polyester film of the present invention preferably has a Young's modulus in the longitudinal direction of 3.5 to 8.0 GPa. When the Young's modulus in the longitudinal direction is within the above range, the storage stability of the magnetic recording medium due to the tension during storage is improved when the film is used for the magnetic recording medium. The Young's modulus in the longitudinal direction is more preferably in the range of 3.8 to 7.0 GPa, and even more preferably in the range of 4.0 to 6.0 GPa. The Young's modulus in the longitudinal direction can be controlled by the MD stretching ratio. The higher the MD ratio, the higher the MD Young's modulus.
[0045] The micromelting peak temperature (T-meta) of the biaxially oriented polyester film of the present invention is preferably 210 to 240°C, more preferably 220 to 235°C. If the micromelting peak temperature is less than 210°C, the structure of the biaxially oriented polyester film may not be sufficiently fixed, making it difficult to control the temperature expansion coefficient within the range of the present application. If the micromelting peak temperature exceeds 240°C, the TD orientation relaxation is too promoted, so that the humidity expansion coefficient becomes too large, and the dimensional stability decreases. Furthermore, the smoothness of the surface decreases, making it difficult to control the surface roughness and protrusion height of the present invention.
[0046] The surface roughness (Sa1) of at least one of the outermost layers of the biaxially oriented polyester film of the present invention is preferably 3.0 to 7.0 nm, more preferably 3.0 to 5.0 nm. In order to achieve the object of the present invention, it is preferable that the surface functions as a surface responsible for running properties and slitting properties. If the surface roughness (Sa1) is less than 3.0 nm, running properties and slitting properties tend to be poor, and if the surface roughness (Sa1) is more than 7.0 nm, when the film is used as a magnetic recording medium, missing pulses tend to occur frequently due to a decrease in smoothness of the magnetic layer surface.
[0047] In addition, the surface roughness (Sa2) of the outermost surface opposite to the surface constituting the above-mentioned Sa1 is preferably smaller than the above-mentioned surface roughness (Sa1), and in order to satisfy the missing pulse of the present invention, it is preferable to coat a magnetic layer on this surface side. The surface roughness (Sa2) is preferably 0.5 to 5.0 nm, more preferably 0.5 to 3.0 nm. If the surface roughness (Sa2) is outside the above range, when a magnetic layer is provided on the surface to form a magnetic recording medium, it may be difficult to achieve both running properties, slit properties, and missing pulses.
[0048] In order to control the surface roughness (Sa1) and (Sa2) of the present invention, it is preferable to have a laminated structure of two or more layers having at least one layer (B layer) containing inactive particles having an average primary particle size of 0.01 to 0.3 μm in the range of 0.01 to 0.5 mass %. In this case, the B layer functions as a layer responsible for runnability and is provided as one of the outermost layers of the film, and the other outermost layer is provided with a layer (A layer) responsible for smoothness. When the A layer contains inactive particles, it is preferable to use particles having an average primary particle size of 0.01 to 0.1 μm, since this makes it easier to control the surface roughness (Sa2) of the present invention. The content of the inactive particles can be added in the range of 0.01 to 0.2 mass %. The biaxially oriented polyester film of the present invention is preferable because it is easier to control the smoothness of the surfaces of both outermost layers by having a laminated structure of at least two layers, and excellent surface smoothness can be achieved at the same time as runnability and slitability.
[0049] In the biaxially oriented polyester film of the present invention, a preferred embodiment is that the outermost layer having the above-mentioned number of protrusions having a height of 60 nm or more and a surface roughness (Sa1) of 3.0 to 7.0 nm is layer B.
[0050] The number of protrusions having a height of 60 nm or more in the present invention can be controlled by the average primary particle size, amount added, lamination thickness, and heat setting temperature of the particles contained in layer B. In particular, it is important that the average primary particle size of the particles contained in layer B is 0.3 μm or less, preferably that two or more types of particles having different average primary particle sizes of 0.01 to 0.2 μm are used in combination.
[0051] The particles preferably contained in the B layer of the biaxially oriented polyester film of the present invention are not particularly limited, and both inorganic particles and organic particles can be used.Specific types include inorganic particles such as clay, mica, titanium oxide, calcium carbonate, wet silica, dry silica, colloidal silica, calcium phosphate, barium sulfate, alumina silicate, kaolin, talc, montmorillonite, alumina, and zirconia, organic particles containing acrylic acids, styrene resins, silicone, imide, and the like as components, and core-shell type organic particles.However, in order to control the height and number of protrusions of 60 nm or more in the present invention, organic particles that are monodispersed spherical particles and colloidal silica are particularly preferred.Furthermore, it is preferable to add alumina particles to the B layer in order to improve running property and slit property, as this can be efficiently improved.
[0052] The content of the particles added to layer B of the biaxially oriented polyester film of the present invention is preferably, for example, 0.005 to 0.8% by mass, and more preferably 0.01 to 0.5% by mass.
[0053] The lamination thickness (t) of layer B of the biaxially oriented polyester film of the present invention is preferably 1 μm or less, more preferably 0.6 μm or less. If the lamination thickness is 1 μm or more, it may be difficult to control the number of protrusions having a height of 60 nm or more within the range of the present invention.
[0054] When producing the biaxially oriented polyester film of the present invention, it is important to carry out stepwise high-temperature heat setting by dividing the heat setting temperature into two or more stages within the range of 190 to 235 ° C. The higher the heat setting temperature, the higher the projection height and surface roughness tend to be, but by adopting stepwise high-temperature heat setting, it is possible to suppress the increase in projection height and surface roughness due to high-temperature heat setting. Furthermore, if the heat setting temperature is set high, orientation relaxation is likely to occur, and the humidity expansion coefficient in the width direction of the present application may become uncontrollable, but by adopting stepwise high-temperature heat setting, the orientation relaxation in the width direction in particular becomes gentle, making it possible to control the temperature-humidity expansion coefficient of the present application within a preferred range.
[0055] The thickness of the biaxially oriented polyester film of the present invention is preferably in the range of 3.5 to 4.6 μm. If the thickness is less than 3.5 μm, the rigidity and dimensional stability are deteriorated, and the stiffness of the tape is insufficient, and the electromagnetic conversion characteristics tend to deteriorate when the film is used as a magnetic recording medium. In addition, it becomes difficult to suppress the particles contained in the B layer from pushing up against the smooth surface (A side). In addition, if the thickness is more than 4.6 μm, the length of one roll of the tape becomes short, making it difficult to respond to miniaturization and high capacity of the magnetic tape. As a method for adjusting the thickness, it is possible to adjust the film thickness after biaxial stretching by adjusting the discharge amount of the screw during melt extrusion of the polymer during film formation of the biaxially oriented polyester film and controlling the thickness of the unstretched film from the die.
[0056] When the biaxially oriented polyester film of the present invention is used as a base film for magnetic recording media, it is preferable to provide a backcoat layer (hereinafter referred to as BC layer) on the surface (B side) of the B layer side described above in order to obtain a high-density magnetic recording medium. In magnetic recording media using ferromagnetic hexagonal ferrite powder in the magnetic layer, the thickness of not only the base film but also the magnetic layer, the nonmagnetic lower layer, and the BC layer itself tends to be thin. In particular, when the thickness of the BC layer is thinned to 0.4 μm or less, the BC layer surface is easily affected by protrusions caused by the support, and the smoothness of the BC layer surface decreases. By defining the number of protrusions of a specific height on the B layer surface within the range of the present invention, even a thinner BC layer can exhibit electromagnetic conversion characteristics with excellent missing pulse occurrence frequency without impairing the smoothness of its surface.
[0057] The biaxially oriented polyester film of the present invention as described above can be produced, for example, as follows.
[0058] First, polyester pellets are melted using an extruder, extruded from a die, cooled and solidified, and molded into a sheet. At this time, it is preferable to filter the polymer through a sintered stainless steel metal filter in order to remove unmelted material in the polymer.
[0059] As long as the characteristic aspects of the present invention are not impaired, various additives, such as compatibilizers, plasticizers, weather resistance agents, antioxidants, heat stabilizers, lubricants, antistatic agents, brightening agents, colorants, conductive agents, crystal nucleating agents, ultraviolet absorbers, flame retardants, flame retardant assistants, pigments, dyes, and the like, may be added.
[0060] The sheet is then simultaneously biaxially stretched in the longitudinal and transverse directions, and then stretched again in the transverse direction and heat-treated. Simultaneous biaxial stretching is preferred because it makes it easier to control the number and height of the protrusions having a height of 60 nm or more according to the present invention.
[0061] As the stretching method, a method of simultaneous biaxial stretching followed by further stretching in the width direction is preferred. In the sequential biaxial stretching method, the stretching stress is likely to concentrate on the particle part when stretching in the longitudinal direction and then in the width direction, so the protrusion height is likely to be high. Furthermore, voids are likely to be formed, which may cause breakage during stepwise high-temperature heat setting. In addition, if the orientation in the width direction becomes too high, it may be difficult to control the temperature-humidity expansion coefficient within the range of the present invention.
[0062] The method for producing the film of the present invention will be described below using, as a representative example, an example in which polyethylene terephthalate (PET) is used as the polyester. The present invention is not limited to PET films, and other polymers may be used. For example, when a polyester film is formed using polyethylene-2,6-naphthalenedicarboxylate, which has a high glass transition temperature or melting point, extrusion and stretching may be performed at a temperature higher than the temperatures shown below.
[0063] First, PET pellets are produced. PET is produced by one of the following processes: (1) a process in which terephthalic acid and ethylene glycol are used as raw materials, and low molecular weight PET or oligomers are obtained by a direct esterification reaction, and then a polymer is obtained by a polycondensation reaction using antimony trioxide or a titanium compound as a catalyst, or (2) a process in which dimethyl terephthalate and ethylene glycol are used as raw materials, and low molecular weight PET is obtained by a transesterification reaction, and then a polymer is obtained by a polycondensation reaction using antimony trioxide or a titanium compound as a catalyst.
[0064] In order to incorporate particles into the PET constituting the film, it is preferable to disperse the particles in ethylene glycol in the form of a slurry at a predetermined ratio, and add this ethylene glycol during polymerization. When adding particles, for example, the particles in the water slurry or alcohol slurry obtained during particle synthesis are added without drying once, which improves the dispersibility of the particles. Here, in order to control the number of protrusions with a height of 60 nm or more within the range of the present invention, it is important to make the particle slurry concentration 5 mass % or less. When the particles to be added are inorganic particles, it is also very effective to add glass beads with an average particle size of 0.5 to 0.05 mm to the particle-containing slurry adjusted to a specific concentration and stir at 1,000 to 5,000 rpm for 1 to 5 hours.
[0065] Next, it is particularly important to directly mix the water slurry of the particles with PET pellets and knead it into PET using a vented twin-screw kneading extruder so that the particle content is 0.1 to 0.5% by mass to prepare a particle master pellet. As a method for adjusting the particle content, a method is preferred in which the particle master pellet of a specific concentration prepared by the above method is diluted with PET that does not substantially contain particles during film formation to adjust the particle content. In this case, it is particularly important to make the blending ratio of the PET pellets that does not substantially contain particles 50% by mass or less, preferably 35% by mass or less, in order to improve the particle dispersibility and to make it easier to control the number of protrusions with a height of 60 nm or more according to the present invention. It is also particularly important because it leads to a reduction in film breakage due to high-temperature heat fixation. Furthermore, when two or more types of particle master pellets are used, it is preferable to blend them in advance to a predetermined desired content, and then use a two-stage kneaded particle master that has been melt-kneaded again to improve the particle dispersibility, since film breakage during stepwise high-temperature stretching is reduced.
[0066] Next, the obtained PET pellets are dried under reduced pressure at 180°C for 3 hours or more, and then fed to an extruder heated to 270-320°C under nitrogen gas flow or reduced pressure so as not to reduce the intrinsic viscosity, extruded from a slit-shaped die, and cooled on a casting roll to obtain an unstretched film. At this time, it is preferable to use various filters, such as high-precision filters made of materials such as sintered metal, porous ceramic, sand, and wire mesh, to remove foreign matter and degraded polymers. In addition, it is extremely preferable to provide a gear pump to improve the quantitative supply and obtain the desired lamination thickness in forming the above-mentioned characteristic aspects. To laminate the film, it is preferable to melt-laminate multiple different polymers using two or more extruders and a manifold or merging block.
[0067] Next, a method of simultaneously biaxially stretching the unstretched film thus obtained and then stretching it again in the width direction will be described.
[0068] In the present invention, MD refers to the longitudinal direction (machine direction) of the biaxially oriented polyester film, and TD refers to the width direction (transverse direction) of the biaxially oriented polyester film.
[0069] First, the unstretched film is simultaneously biaxially stretched in the MD and TD directions. The stretching temperature varies depending on the type of polymer used, but can be determined based on the glass transition temperature (Tg) of the unstretched film. It is preferably in the range of Tg+20 to Tg+50°C, more preferably Tg+20°C to Tg+30°C. If the stretching temperature is lower than the above range, film breakage occurs frequently, productivity decreases, and it may be difficult to stably stretch the film when stretching again in the width direction after simultaneous biaxial stretching. The MD stretching ratio during simultaneous biaxial stretching is 3 to 6 times, preferably 3.1 to 5.0 times. The TD stretching ratio is 3.3 to 6 times, preferably 3.5 to 5 times.
[0070] Next, the film is stretched again in the TD direction (TD stretching 2). The stretching temperature in TD stretching 2 is 180 to 220°C, preferably 190 to 210°C. The stretching ratio in TD stretching 2 is preferably 1.3 to 2 times, more preferably 1.4 to 1.7 times. If the stretching ratio or stretching temperature in TD stretching 2 is outside the range of the present invention, the temperature-humidity expansion coefficient may not be controlled within the range of the present application. In addition, simultaneous biaxial stretching in the MD direction within the range of 1.05 to 1.3 times at this time has the effect of suppressing the surface protrusions of the B side from being too connected in the TD direction when the film is stretched again in the TD direction. The area ratio is 12 to 30 times, preferably 14 to 25 times. If the area ratio is outside the range of the present application, it may be difficult to achieve both the temperature-humidity expansion coefficient and the area ratio. If the area ratio exceeds 30 times, the temperature-humidity expansion coefficient may not be controlled within the range of the present invention, or the number of protrusions having a height of 60 nm or more may become too large. If the area magnification is less than 12 times, it tends to be difficult to obtain the temperature-humidity expansion coefficient of the present invention.
[0071] Next, the biaxially stretched film is heat set while being relaxed in the width direction. As heat setting conditions, the heat setting temperature is preferably 190 to 235°C, more preferably 200 to 230°C. The heat setting temperature is preferably divided into two or more stages and stepwise high temperature heat setting is performed from the viewpoints of achieving both the temperature and humidity expansion coefficient of the present invention, controlling the number of protrusions having a height of 60 nm or more, surface roughness, and film breakage. As conditions for stepwise high temperature heat setting, the first stage heat setting temperature (HS1) is preferably (stretching temperature of TD stretching 2+3°C) to (stretching temperature of TD stretching 2+20°C). The second stage heat setting temperature (HS2) is preferably in the range of (HS1+5°C) to (HS1+15°C). The third stage heat setting temperature (HS3) is preferably in the range of (HS2) to (HS2+10°C), more preferably (HS2+2°C) to (HS2+10°C). To obtain the thermal and hygroscopic expansion coefficient and minute melting peak temperature (T-meta) of the present invention, it is preferable to set the second stage heat setting temperature to 215° C. or higher, preferably 220 to 235° C., since this makes it easier to control.
[0072] The heat setting time is preferably in the range of 0.5 to 10 seconds, and the relaxation rate in the width direction is preferably 0.8 to 2.0%. Then, the film is guided to a cooling zone adjusted to 130 to 180° C. and slowly cooled, after which the film edges are cut and taken up on a roll to obtain the biaxially oriented polyester film of the present invention.
[0073] There is a difference between the stretching temperature of TD stretching 2 and the first stage heat setting temperature, and if the heat setting temperature is higher than the above range, the film is likely to relax, making it difficult to obtain the humidity expansion coefficient of the present invention, and the dimensional stability is likely to decrease. Furthermore, the surface smoothness may decrease, making it difficult to obtain the surface roughness of the present invention. On the other hand, if the heat setting temperature is too low, the TD heat shrinkage rate may not be controlled within the range of the present application, or the crystallinity may be low, and the flatness of the base film may decrease in the manufacturing process of the magnetic recording medium, and the frequency of occurrence of missing pulses may increase.
[0074] Next, the magnetic recording medium is manufactured, for example, as follows.
[0075] The magnetic recording medium support (biaxially oriented polyester film) obtained as described above is slit into a width of, for example, 0.1 to 3 m, and while conveying at a speed of 20 to 300 m / min and a tension of 50 to 300 N / m, a non-magnetic paint is applied to one side with a thickness of 0.5 to 1.5 μm by an extrusion coater, dried, and then a magnetic paint is applied to a thickness of 0.1 to 0.3 μm. Thereafter, the support coated with the magnetic paint and the non-magnetic paint is magnetically oriented and dried at a temperature of 80 to 130° C. Next, a back coat is applied to the opposite side with a thickness of 0.3 to 0.8 μm, calendered, and then wound up. The calendering is performed using a small test calendering device (metal roll, 7 stages) at a temperature of 70 to 120° C. and a linear pressure of 0.5 to 5 kN / cm. Then, the aging treatment is performed at 60 to 80° C. for 24 to 72 hours, slit into a width of 12.65 mm, and pancakes are produced. Next, a specific length of the pancake is assembled into a cassette to form a cassette tape type magnetic recording medium.
[0076] Here, the composition of the magnetic paint may be, for example, as follows:
[0077] Hereinafter, when simply "parts" is mentioned, it means "parts by mass".
[0078] [Magnetic layer forming coating liquid] Barium ferrite magnetic powder 100 parts [Plate diameter: 20.5 nm, plate thickness: 7.6 nm, plate ratio: 2.7, Hc: 191 kA / m (≒ 2400 Oe), saturation magnetization: 44 Am 2 / kg, BET specific surface area: 60m 2 / g〕 Polyurethane resin 12 parts Mass average molecular weight 10,000 Sulfonic acid functional group 0.5meq / g α-alumina HIT60 (Sumitomo Chemical Co., Ltd.) 8 parts Carbon black #55 (Asahi Carbon Co., Ltd.) particle size 0.015 μm 0.5 parts Stearic acid 0.5 parts Butyl stearate 2 parts Methyl ethyl ketone 180 parts Cyclohexanone 100 parts [Coating liquid for forming non-magnetic layer] Non-magnetic powder α-iron oxide 100 parts Average major axis length: 0.09 μm, specific surface area by BET method: 50 m 2 / g Average acicular ratio: 7 DBP oil absorption: 27~38ml / 100g Surface treatment layer: Al2O3 8% by mass Carbon black 25 parts Conductex SC-U (manufactured by Columbian Carbon) Vinyl chloride copolymer MR104 (manufactured by Zeon Corporation) 13 parts Polyurethane resin UR8200 (manufactured by Toyobo Co., Ltd.) 5 parts Phenylphosphonic acid 3.5 parts Butyl stearate 1.0 part The magnetic recording medium can be suitably used, for example, for data recording purposes, specifically for backing up computer data (for example, linear tape-type recording media (LTO7, LTO8, next-generation LTO tape (LTO9)) and for recording digital images such as video.
[0079] An example of a coating-type digital recording medium in which the biaxially oriented polyester film of the present invention can be suitably used is a coating-type magnetic recording medium in which a magnetic layer is formed by uniformly dispersing a ferromagnetic powder such as barium ferrite in a binder such as polyurethane resin to create a magnetic coating liquid, and then coating the coating liquid.
[0080] (Methods for measuring physical properties and evaluating effects) The methods for measuring the characteristic values and evaluating the effects of the present invention are as follows.
[0081] (1) Humidity expansion coefficient in the transverse direction (ppm / %RH) The following device was placed in a thermo-hygrostat and the deformation amount was measured in the width direction of the film under the following conditions, and the average value of three measurement results was taken as the humidity expansion coefficient in the width direction in the present invention.
[0082] Measuring device: Tape elongation tester 1TTM1 manufactured by Okura Industry Co., Ltd. Temperature and humidity chamber: KATO Corporation TP Instrumentation Version 1.04 Sample size: Width 10mm x Length 200mm (sample length) Load: 10g Number of measurements: 3 Temperature: 30℃ Humidity conditions: <1> Hold at 40% RH for 6 hours <2> Maintain 80% RH for 6 hours (humidity increase rate: 0.7% RH / min) <3> Dehumidify to 40%RH (humidification rate: 1.4%RH / min) and hold for 6 hours <4> Humidification to 80%RH (humidification rate: 0.7%RH / min) Measurement (L 40 ):Humidity conditions <3> Measure the sample length after keeping it at 40% RH for 6 hours (L 40 ) Measurement (L 80 ):Humidity conditions <4> The sample length was measured when the humidity was increased from 40% RH to 80% RH (humidity increase rate: 0.7% RH / min). 80 ).
[0083] ΔL(mm): Dimensional change ΔL(L 80 -L 40 ) The humidity expansion coefficient (ppm / %RH) was calculated using the following formula: Humidity expansion coefficient (ppm / %RH) = 10 6 ×{(ΔL / (sample length before measurement × humidity difference)} Sample length before measurement = 200 (mm) Humidity difference=40(%) (2) Thermal expansion coefficient in the transverse direction (ppm / ℃) Measurements were carried out in a nitrogen atmosphere in the width direction of the film under the conditions below, and the average value of three measurement results was taken as the thermal expansion coefficient in the present invention.
[0084] Measurement equipment: Thermo-mechanical tester manufactured by Shinku Riko Co., Ltd. TM-9400 (balance and heating furnace) TMS-9000 (Multi Thermal Analysis Station) Sample size: Width 4mm x Length 15mm (sample length) Load: 5g Number of times: 3 Temperature: 25℃→50℃→20℃→50℃ (heating rate: 1℃ / min) Measurement (L0): Sample length at 30°C when reheated (L0) Measurement (L1): Sample length at 40°C when reheated (L1) ΔL(mm): Dimensional change ΔL(L1-L0) The thermal expansion coefficient was calculated from the following formula:
[0085] Thermal expansion coefficient (ppm / ℃) = 10 6 ×{(ΔL / (sample length before measurement × temperature difference)} Sample length before measurement = 15 (mm) Temperature difference=10(℃) (3) Number of protrusions with a height of 60 nm or more (pieces / mm 2 ) Using a scanning white light interference microscope, measurements were taken in 100 different fields of view. The sample was set so that the Y-axis direction of the stage was the longitudinal direction of the sample film (the longitudinal direction is the direction in which the film runs during the film manufacturing process).
[0086] Measurements are performed under the following measurement conditions. The images obtained are analyzed using the attached analysis software, and the height threshold is set to 60 nm to count the number of protrusions with a height of 60 nm or more in each field of view. The total number is calculated by dividing the total by 1 mm. 2 The converted value per unit area was taken as the number of protrusions with a height of 60 nm or more. [Measurement conditions] Equipment: Hitachi High-Tech Science VS1540 Scanning White Light Interferometry Microscope Objective lens: 50x Wavelength filter: 530white Measurement mode: Wave [Conversion processing conditions] and Interpolation: Full Interpolation Filter: Median 3×3 Surface correction: 4th order (4) Heat shrinkage rate Measurements were made in accordance with JIS C2318 (1997). The longitudinal direction of the sample size was set to the width direction of the film, and measurements were made under the following conditions to determine the thermal shrinkage rate in the width direction.
[0087] Sample size: width 10mm, mark spacing 200mm Measurement conditions: Temperature 100℃, treatment time 30 minutes Load: No load Heat shrinkage rate (%) = [(L0-L) / L0] x 100 L0: Gauge distance before heat treatment L: Gauge distance after heat treatment (5) Young’s modulus The Young's modulus of the film was measured in accordance with ASTM-D882 (1997). An Instron-type tensile tester was used under the following conditions. The average value of five measurements was taken as the Young's modulus in the present invention.
[0088] Measurement equipment: Instron ultra-precision material testing machine MODEL5848 Sample size: When measuring Young's modulus in the film width direction Film length direction 2mm x film width direction 12.6mm (Grip interval is 8mm across the film) When measuring Young's modulus in the longitudinal direction of a film Film width direction 2mm x film length direction 12.6mm (Grip interval is 8 mm in the longitudinal direction of the film) Pulling speed: 1mm / min Measurement environment: temperature 23℃, humidity 65%RH Number of measurements: 5.
[0089] (6) Minor melting peak temperature (T-meta) According to JIS-K7121 (1987), a differential scanning calorimeter was used, a Seiko Instruments DSC (RDC220) and a data analyzer, a Disk Station (SSC / 5200) was used, and 5 mg of the sample was placed on an aluminum tray and heated from 25°C to 300°C at a heating rate of 20°C / min. The peak temperature of the endothermic peak of melting observed at this time was taken as the melting point (Tm), and the temperature of the minute endothermic peak that appeared slightly lower than Tm was taken as T-meta. The heat calculated from the peak area of Tm was taken as the heat of fusion ΔHm.
[0090] (7) Surface roughness (Sa1), (Sa2) For both sides of the film, measurements were taken in 100 different locations under the same conditions using the device described in (3) above, and after conversion processing, the surface roughness (Sa) of each field was calculated using the accompanying analysis software. The average value of the 100 fields for each side was calculated, and the larger value was designated Sa1 and the smaller value was designated Sa2.
[0091] (8) Lamination thickness (μm) Under the conditions below, cross-section observation was performed in 10 fields of view at different locations, and the average of the obtained thicknesses (μm) was calculated and defined as the thickness (μm) of layer A.
[0092] Measurement equipment: Transmission electron microscope (TEM) Hitachi H-7100FA Measurement conditions: Acceleration voltage 100 kV Measurement magnification: 10,000 times Sample preparation: Ultrathin sectioning Observation surface: TD-ZD cross section (TD: width direction, ZD: thickness direction) Number of measurements: 3 points per field, 10 fields of view were measured.
[0093] (9) Slittability When the film was slit into a width of 1 m, the slitting speed was changed and the sharpness of the film edge was visually evaluated according to the following method, where C was determined as poor slitting performance.
[0094] AA: The edges can be slit without distortion even at a speed of 70 m / min.
[0095] A: Distortion occurs at the ends when the speed is between 60 m / min or more and less than 70 m / min.
[0096] B: Distortion occurs at the ends when the speed is between 50 m / min or more and less than 60 m / min.
[0097] C: At a speed of less than 50 m / min, wrinkles appear on the film surface and the edges become distorted.
[0098] (10) Missing pulse occurrence frequency The film slit to a width of 1 m was conveyed with a tension of 200 N, and one surface of the support was coated with magnetic paint and non-magnetic paint as described below, and slit to a width of 12.65 mm to prepare a pancake. A length of 200 m was then inserted into a cassette to prepare a magnetic tape.
[0099] (Hereinafter, "parts" means "parts by mass.") Magnetic layer forming coating liquid Barium ferrite magnetic powder 100 parts (Plate diameter: 20.5nm, plate thickness: 7.6nm, Plate ratio: 2.7, Hc: 191kA / m (≒2400Oe) Saturation magnetization: 44Am 2 / kg, BET specific surface area: 60m 2 / g) Polyurethane resin 12 parts Mass average molecular weight 10,000 Sulfonic acid functional group 0.5meq / g α-alumina HIT60 (Sumitomo Chemical Co., Ltd.) 8 parts Carbon black #55 (Asahi Carbon Co., Ltd.) Particle size 0.015μm 0.5 parts Stearic acid 0.5 parts Butyl stearate 2 parts Methyl ethyl ketone 180 parts Cyclohexanone 100 parts Coating liquid for forming non-magnetic layer Non-magnetic powder α-iron oxide 85 parts Average major axis length: 0.09μm, specific surface area by BET method: 50m 2 / g Average acicular ratio: 7 DBP oil absorption: 27~38ml / 100g Surface treatment layer: Al2O3 8% by mass Carbon black 15 parts "Conductex" (registered trademark) SC-U (manufactured by Columbian Carbon Co., Ltd.) Polyurethane resin UR8200 (manufactured by Toyobo Co., Ltd.) 22 parts Phenylphosphonic acid 3 parts Cyclohexanone 140 parts Methyl ethyl ketone 170 parts Butyl stearate 1 part Stearic Acid 2 parts For each of the above coating liquids, each component was kneaded with a kneader. The coating liquid was pumped through a horizontal sand mill containing 0.5 mmφ zirconia beads in an amount that filled 65% of the volume of the dispersion section, and dispersed at 2,000 rpm for 120 minutes (time spent substantially in the dispersion section). 5.0 parts of polyisocyanate were added to the resulting dispersion for the nonmagnetic layer paint, and 2.5 parts were added to the magnetic layer paint, and 3 parts of methyl ethyl ketone were further added. The mixture was filtered using a filter with an average pore size of 1 μm to prepare coating liquids for forming the nonmagnetic layer and magnetic layer, respectively.
[0100] The obtained coating solution for forming a non-magnetic layer was applied to a PET film so that the thickness after drying was 0.8 μm, and then the coating solution for forming a magnetic layer was applied so that the thickness after drying was 0.07 μm. While the magnetic layer was still in a wet state, it was oriented and dried using a cobalt magnet with a magnetic force of 6,000 G (600 mT) and a solenoid with a magnetic force of 6,000 G (600 mT). Then, a backcoat layer (carbon black average particle size: 17 nm 100 parts, calcium carbonate average particle size: 40 nm 80 parts, α-alumina average particle size: 200 nm 5 parts dispersed in polyurethane resin and polyisocyanate) was applied so that the thickness after calendering was 0.35 μm. Next, calendering was performed with a calender at a temperature of 90 ° C. and a linear pressure of 300 kg / cm (294 kN / m), and then cured at 65 ° C. for 72 hours. Furthermore, the nonwoven fabric and razor blade were attached to a device having a slit product delivery and take-up device so that they were pressed against the magnetic surface, and the surface of the magnetic layer was cleaned with a tape cleaning device to obtain a magnetic tape.
[0101] The magnetic tape cartridge obtained above (total magnetic tape length 500 m) was set in an IBM LTO-7 drive, and the magnetic tape was run 1,500 times back and forth at a tension of 0.55 N and a running speed of 8 m / sec.
[0102] The magnetic tape cartridge after the above running was set in a reference drive (IBM LTO7 drive), and the magnetic tape was run to perform recording and playback. The playback signal during running was input to an external AD (Analog / Digital) conversion device, and a signal where the playback signal amplitude was 80% or more lower than the average (average of the measured values for all tracks) was defined as a missing pulse, and the frequency of occurrence was divided by the total length of the magnetic tape to obtain the missing pulse occurrence frequency (unit: times / m) per unit length of magnetic tape. Tapes with a missing pulse occurrence frequency of 2.5 times / m or less were considered to be reliable magnetic tapes, and tapes with a missing pulse occurrence frequency of more than 2.5 times / m were considered to be defective, and were judged according to the following criteria.
[0103] AA: Missing pulse occurrence frequency is less than 1.5 times / m A: Missing pulse occurrence frequency is 1.5 times / m or more and less than 2.0 times / m B: Missing pulse occurrence frequency is 2.0 times / m or more and less than 2.5 times / m C: Missing pulse occurrence frequency is 2.5 times / m or more.
[0104] (11) Stability of magnetic tape to environmental changes The magnetic tape prepared in (10) above was set in a film dimension measuring device (FIG. 1) installed in a thermo-hygrostat, and the width of the tape was measured under the following temperature and humidity conditions with a load of 50 g.
[0105] ·Temperature and humidity conditions <1> : 10℃ 10%RH <2> : 10℃ 80%RH <3> : 29℃ 80%RH <4> : 45℃ 24%RH <5> : 45℃ 10%RH Dimensional measurements are <1> → <2> → <3> → <4> → <5> After reaching each temperature and humidity, the tape width was measured after leaving it for 2 hours (each tape width was L <1> , L <2> , L <3> , L <4> , L <5> (Assuming that.)
[0106] The change in tape width between conditions was calculated, and then a correction was made taking into account the temperature expansion of the magnetic head (7 ppm / ℃) (subtract 7 ppm / ℃ x the temperature difference between each condition) to calculate the change in tape width between conditions according to the following formula.
[0107] Change (1) ΔL <3> -L <1> = |L <3> -L <1> -(7×19)| Change (2) ΔL <5> -L <2> = |L <5> -L <2> -(7×35)| The larger of the above changes (1) and (2) was divided by the tape width (12.65 mm) and converted to ppm to determine the tape width change (ppm) due to temperature and humidity environment changes, and was evaluated according to the following criteria.
[0108] A: Less than 500 ppm B: 500 ppm or more and less than 800 ppm C:800ppm or more EXAMPLES
[0109] The embodiments of the present invention will be described with reference to the following examples, in which polyethylene terephthalate is abbreviated as PET, polyethylene naphthalate as PEN, and polyetherimide as PEI.
[0110] (1) Preparation of PET pellets: 194 parts by mass of dimethyl terephthalate and 124 parts by mass of ethylene glycol were charged into an ester exchange reactor, and the contents were heated to 140°C to dissolve. Then, 0.3 parts by mass of magnesium acetate tetrahydrate and 0.05 parts by mass of antimony trioxide were added while stirring the contents, and an ester exchange reaction was carried out while distilling off methanol at 140 to 230°C. Next, 0.5 parts by mass of a 5% by mass ethylene glycol solution of trimethyl phosphate (0.025 parts by mass as trimethyl phosphate) and 0.3 parts by mass of a 5% by mass ethylene glycol solution of sodium dihydrogen phosphate dihydrate (0.015 parts by mass as sodium dihydrogen phosphate dihydrate) were added.
[0111] When the ethylene glycol solution of trimethyl phosphate was added, the temperature of the reaction contents dropped. Therefore, the excess ethylene glycol was distilled off while stirring was continued until the temperature of the reaction contents returned to 230°C. After the temperature of the reaction contents in the transesterification reactor reached 230°C in this way, the reaction contents were transferred to the polymerization reactor.
[0112] After the transition, the reaction system was gradually heated from 230°C to 275°C, and the pressure was lowered to 0.1kPa. The time to reach the final temperature and the final pressure was both 60 minutes. After reaching the final temperature and the final pressure, the reaction was continued for 2 hours (3 hours from the start of polymerization), and the stirring torque of the polymerization apparatus showed a predetermined value (the specific value differs depending on the specifications of the polymerization apparatus, but the value shown by polyethylene terephthalate with an intrinsic viscosity of 0.62 in this polymerization apparatus was set as the predetermined value). The reaction system was then purged with nitrogen and returned to normal pressure to stop the polycondensation reaction, and the mixture was discharged into cold water in the form of strands, which were immediately cut to obtain PET pellets of polyethylene terephthalate with an intrinsic viscosity of 0.62 (raw material-1).
[0113] (2-a) Preparation of particle-containing PET pellets: 90 parts by mass of the above-mentioned PET pellets (raw material-1) and 10 parts by mass of a 10% by mass water slurry of cross-linked polystyrene particles with an average particle size of 0.45 μm (1 part by mass as cross-linked polystyrene particles) were fed into a co-rotating, vented twin-screw kneading extruder heated to 280°C, and the vent hole was kept at a reduced pressure of 1 kPa or less to remove moisture, thereby obtaining particle-containing pellets (raw material-2a) containing 1% by mass of cross-linked polystyrene particles and having an intrinsic viscosity of 0.62.
[0114] (2-b) Preparation of particle-containing PET pellets: 90 parts by mass of the above-mentioned PET pellets (raw material-1) and 10 parts by mass of a 5% by mass water slurry of cross-linked polystyrene particles with an average particle size of 0.30 μm (0.5 parts by mass as cross-linked polystyrene particles) were fed into a vented twin-screw kneading extruder of the same rotation type heated to 280°C, and the vent hole was kept at a reduced pressure of 1 kPa or less to remove moisture, thereby obtaining particle-containing pellets (raw material-2b) containing 0.5% by mass of cross-linked polystyrene particles and having an intrinsic viscosity of 0.62.
[0115] (2-c) Preparation of particle-containing PET pellets: 90 parts by mass of the above-mentioned PET pellets (raw material-1) and 10 parts by mass of a 5% by mass water slurry of cross-linked polystyrene particles with an average particle size of 0.15 μm (0.5 parts by mass as cross-linked polystyrene particles) were fed into a vented twin-screw kneading extruder of the same rotation type heated to 280°C, and the vent hole was kept at a reduced pressure of 1 kPa or less to remove moisture, thereby obtaining particle-containing pellets (raw material-2c) containing 0.5% by mass of cross-linked polystyrene particles and having an intrinsic viscosity of 0.62.
[0116] (2-d) Preparation of particle-containing PET pellets: 90 parts by mass of the above-mentioned PET pellets (raw material-1) and 10 parts by mass of a 5% by mass water slurry of cross-linked polystyrene particles with an average particle size of 0.17 μm (0.5 parts by mass as cross-linked polystyrene particles) were fed into a vented twin-screw kneading extruder of the same rotation type heated to 280°C, and the vent hole was kept at a reduced pressure of 1 kPa or less to remove moisture, thereby obtaining particle-containing pellets (raw material-2d) containing 0.5% by mass of cross-linked polystyrene particles and having an intrinsic viscosity of 0.62.
[0117] (2-e) Preparation of particle-containing PET pellets: 94 parts by mass of the above-mentioned PET pellets (raw material-1) and 5% by mass water slurry of colloidal silica particles with an average particle size of 0.060 μm to which glass beads with an average particle size of 0.05 mm were added were fed into a vented twin-screw kneading extruder of the same rotation type heated to 280°C, and the water slurry was stirred at 1,000 rpm for 2 hours, filtered to remove the glass beads, and 6 parts by mass (0.3 parts by mass as colloidal silica particles) were fed. The vent hole was kept at a reduced pressure of 1 kPa or less to remove moisture, and particle-containing pellets (raw material-2e) containing 0.3% by mass of colloidal silica particles and having an intrinsic viscosity of 0.62 were obtained.
[0118] (2-f) Preparation of particle-containing PET pellets: 90 parts by mass of the above-mentioned PET pellets (raw material-1) and 5% by mass water slurry of colloidal silica particles with an average particle size of 0.20 μm with glass beads with an average particle size of 0.05 mm were fed into a vented twin-screw kneading extruder of the same rotation type heated to 280°C, and 10 parts by mass (0.5 parts by mass as colloidal silica particles) of the water slurry, which was stirred at 3,000 rpm for 2 hours and then filtered to remove the glass beads, were fed into the extruder, and the vent hole was kept at a reduced pressure of 1 kPa or less to remove moisture, thereby obtaining particle-containing pellets (raw material-2f) containing 0.5% by mass of colloidal silica particles and having an intrinsic viscosity of 0.62.
[0119] (2-g) Preparation of particle-containing PET pellets: 90 parts by mass of the above-mentioned PET pellets (raw material-1) and 10 mass% water slurry of alumina particles with a primary average particle size of 0.02 μm to which zirconia beads with an average particle size of 0.5 mm were added were fed into a vented twin-screw kneading extruder of the same rotation type heated to 280°C, and the mixture was stirred at 3,000 rpm for 2 hours, and then 10 mass parts (1 mass part as alumina particles) of the water slurry from which the zirconia beads had been removed by filtration were fed. The vent hole was kept at a reduced pressure of 1 kPa or less to remove moisture, and particle-containing pellets (raw material-2g) containing 1 mass% alumina particles and having an intrinsic viscosity of 0.62 were obtained.
[0120] (3) Preparation of two-component composition (PET / PEI) pellets: The PET pellets (raw material-1) obtained by the above method and pellets of PEI “Ultem” (registered trademark) 1010 manufactured by SABIC Innovative Plastics were fed into a vented twin-screw extruder (manufactured by Japan Steel Works, Ltd., screw diameter 30 mm, screw length / screw diameter = 45.5) of the same rotation type equipped with three kneading paddle kneading sections heated to a temperature of 280 ° C., and the pellets were mixed at a shear rate of 100 sec -1 The mixture was melt-extruded with a residence time of 1 minute to obtain two-component composition pellets containing 50% by mass of PEI. The glass transition temperature of the two-component composition pellets thus produced was 150° C. (raw material-3).
[0121] Example 1 Two extruders E1 and E2 were used. The extruder E1 was heated to 280°C, and 29 parts by mass of PET pellets (raw material-1), 4 parts by mass of two-component composition pellets (raw material-3), and 67 parts by mass of pellets containing colloidal silica particles with an average particle size of 0.06 μm (raw material-2c) were fed to the extruder E1, which was heated to 280°C, after drying them under reduced pressure for 3 hours at 180°C. The extruder E2 was also heated to 280°C, and 28 parts by mass of PET pellets (raw material-1), 4 parts by mass of two-component composition pellets (raw material-3), 64 parts by mass of pellets containing colloidal silica particles with an average particle size of 0.20 μm (raw material-2e), and 4 parts by mass of pellets containing crosslinked polystyrene particles with an average particle size of 0.30 μm (raw material-2a) were blended as the B layer raw materials, and dried under reduced pressure for 3 hours at 180°C, after which they were fed. In order to laminate these into two layers, the lamination thickness ratio (layer A | layer B) = 8 | 1 was set in a T-die, and they were joined so that the layer B side was facing the casting drum surface.Then, while applying a static charge to the casting drum with a surface temperature of 25°C, the films were brought into close contact and cooled to solidify, producing a laminated unstretched film.
[0122] This laminated unstretched film was stretched 3.3 times in the longitudinal direction (MD direction) (MD stretching 1) and 3.5 times in the transverse direction (TD direction) (TD stretching 1) at 100 ° C. in a simultaneous biaxial stretching machine, and then stretched 1.1 times in the longitudinal direction (MD stretching 2) and 1.5 times in the transverse direction (TD stretching 2) simultaneously in a heating zone at a temperature of 200 ° C. Subsequently, while increasing the heat treatment temperature stepwise in the heat treatment zone in the tenter, the first stage was heat treated at a temperature of 212 ° C. for 2 seconds, the second stage was heat treated at a temperature of 222 ° C. for 5 seconds, and the third stage was heat treated at a temperature of 224 ° C. for 3 seconds, and a 1.7% relaxation treatment was performed in the transverse direction at a temperature of 150 ° C. Next, after uniformly cooling to 25 ° C., the film edges were removed and the film was wound on a core to obtain a biaxially stretched polyester film having a thickness of 4.5 μm. The resulting biaxially oriented polyester film had good film formation stability, and when its physical properties were evaluated, as shown in Table 4, it had excellent properties when used as a magnetic tape.
[0123] The following tables show the raw material compositions, film-forming conditions, physical properties of the biaxially oriented polyester films, characteristics of the magnetic tapes, etc., of the respective Examples and Comparative Examples.
[0124] (Examples 2 to 4) The B layer raw material and stretching conditions were changed to obtain a biaxially stretched polyester film with a thickness of 4.5 μm so as to obtain the particle formulation shown in the table. The film formation stability of the obtained biaxially oriented polyester film was good, and when the physical properties were evaluated, it had excellent characteristics when used as a magnetic tape, as shown in the table.
[0125] Example 5 Two extruders E1 and E2 were used, and the extruder E1 was heated to 280°C. As the A layer raw materials, 29 parts by mass of PET pellets (raw material-1), 4 parts by mass of two-component composition pellets (raw material-3), and 67 parts by mass of pellets containing colloidal silica particles with an average particle size of 0.06 μm (raw material-2c) were fed after drying under reduced pressure at 180°C for 3 hours. Similarly, the extruder E2 was heated to 280°C. As the B layer raw materials, 20 parts by mass of PET pellets (raw material-1), 12 parts by mass of two-component composition pellets (raw material-3), 64 parts by mass of pellets containing colloidal silica particles with an average particle size of 0.20 μm (raw material-2e), and 4 parts by mass of pellets containing crosslinked polystyrene particles with an average particle size of 0.30 μm (raw material-2a) were blended and dried under reduced pressure at 180°C for 3 hours before feeding. In order to laminate these into two layers, the lamination thickness ratio (layer A | layer B) = 8 | 1 was set in a T-die, and they were joined so that the layer B side was facing the casting drum surface.Then, while applying a static charge to the casting drum with a surface temperature of 25°C, the films were brought into close contact and cooled to solidify, producing a laminated unstretched film.
[0126] This laminated unstretched film was stretched 3.1 times in the longitudinal direction (MD direction) (MD stretching 1) and 3.5 times in the transverse direction (TD direction) (TD stretching 1) at 100 ° C. in a simultaneous biaxial stretching machine, and then stretched 1.1 times in the longitudinal direction (MD stretching 2) and 1.6 times in the transverse direction (TD stretching 2) simultaneously in a heating zone at a temperature of 200 ° C. Subsequently, while increasing the heat treatment temperature stepwise in the heat treatment zone in the tenter, the first stage was heat treated at a temperature of 212 ° C. for 2 seconds, the second stage was heat treated at a temperature of 222 ° C. for 5 seconds, and the third stage was heat treated at a temperature of 224 ° C. for 3 seconds, and a 1.7% relaxation treatment was performed in the transverse direction at a temperature of 150 ° C. Next, after uniformly cooling to 25 ° C., the film edges were removed and the film was wound around a core to obtain a biaxially stretched polyester film having a thickness of 4.5 μm. The resulting biaxially oriented polyester film had good film formation stability, and when its physical properties were evaluated, as shown in Table 4, it had excellent properties when used as a magnetic tape.
[0127] Comparative Example 1 As shown in the table, the stretching conditions were changed to obtain a biaxially stretched polyester film having a thickness of 4.5 μm.
[0128] Comparative Example 2 The raw materials with the particle formulation shown in the table were dried under reduced pressure at 180°C for 3 hours and then supplied. To laminate these in two layers, the lamination thickness ratio (A layer|B layer) was set to 4|1 in a T-die, and the layers were joined so that the B layer side was on the casting drum surface side. The layers were then brought into close contact with the casting drum at a surface temperature of 25°C while applying a static charge, and cooled and solidified to produce a laminated unstretched film.
[0129] This laminated unstretched film was stretched 3.5 times in the longitudinal direction in three stages at 90° C. using a roll-type stretching machine. The stretching was performed by utilizing the difference in peripheral speed between two sets of rolls, at 2.5 times in the first stage, 1.34 times in the second stage, and 1.05 times in the third stage.
[0130] The obtained uniaxially stretched film was guided to a preheating zone at 95°C in a tenter while holding both ends with clips, and then continuously stretched 3.5 times in the width direction (TD direction) perpendicular to the longitudinal direction in a heating zone at 90°C (TD stretching 1), and then further stretched 1.4 times in the width direction in a heating zone at 195°C (TD stretching 2). Subsequently, the film was subjected to a heat treatment at 190°C for 10 seconds in a heat treatment zone in the tenter, and further subjected to a relaxation treatment in the width direction by 0.5% at a temperature of 150°C. Next, after uniformly cooling to 25°C, the film edges were removed and the film was wound on a core to obtain a biaxially stretched polyester film having a thickness of 4.5 μm.
[0131] Comparative Example 3 The raw materials, stretching conditions, and heat setting temperature were changed so as to obtain the particle formulation shown in the table, and a biaxially stretched polyester film having a thickness of 4.4 μm was obtained.
[0132] Comparative Example 4 As shown in the table, a biaxially oriented polyester film having a thickness of 4.5 μm was obtained in the same manner as in Example 2, except that the heat setting temperature was changed.
[0133] Comparative Example 5 As shown in the table, a biaxially oriented polyester film having a thickness of 4.5 μm was obtained in the same manner as in Example 1, except that the heat setting temperature was changed.
[0134] Comparative Example 6 As shown in the table, a biaxially stretched polyester film having a thickness of 4.5 μm was obtained in the same manner as in Example 4, except that the stretching conditions and heat setting temperature were changed.
[0135] [Table 1]
[0136] [Table 2]
[0137] [Table 3]
[0138] [Table 4] [Explanation of symbols]
[0139] 1: Laser transmitter 2: Light receiving part 3: Load detector 4: Load 5~8: Freeroll 9: Magnetic tape 10: Laser light
Claims
1. The humidity expansion coefficient in the width direction is 4.5 to 6.5 ppm / % RH, the temperature expansion coefficient in the width direction is -3.0 to 7.0 ppm / °C, and the number of protrusions having a height of 60 nm or more on at least one outermost layer surface is 0 to 200 / mm 2 and a minor melting peak temperature (T-meta) of 212 to 240°C.
2. 2. The biaxially oriented polyester film according to claim 1, which has a heat shrinkage rate in the width direction of 1.0% or less.
3. 3. The biaxially oriented polyester film according to claim 1, wherein the Young's modulus in the transverse direction is 7.0 to 12.0 GPa.
4. The biaxially oriented polyester film according to any one of claims 1 to 3, wherein at least one surface roughness (Sa1) is 3.0 to 7.0 nm.
5. The biaxially oriented polyester film according to claim 4, wherein the surface roughness (Sa2) of the outermost layer surface opposite to the surface constituting Sa1 is 0.5 to 5.0 nm.
6. The biaxially oriented polyester film according to any one of claims 1 to 5, which is used as a base film for a coating-type digital recording medium.
Citation Information
Patent Citations
Biaxially oriented polyester film and its production
JP2000141475A
Biaxially oriented polyester film
JP2005163020A
Biaxially oriented polyester film and magnetic recording medium
JP2009221278A
Biaxially oriented polyester film
JP2012067239A
Biaxially oriented polyester film and coat-type magnetic recording tape using the same
JP2015025047A