Manufacturing method of injection molding material and injection molding material

By adding a water-soluble polymer to cellulose and mixing with starch in air, the method addresses the issue of weakened fiber bonds in dry defibration, enhancing the mechanical strength of cellulose-based molded products.

JP7581752B2Active Publication Date: 2024-11-13DAIHO INDUSTRIAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020168313
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-05
Publication Date
2024-11-13
Estimated Expiration
2040-10-05

AI Technical Summary

Technical Problem

Existing methods for producing cellulose-based molded products using a dry defibration process result in silicone surfactants remaining on the fibers, which weaken the bond between fibers and reduce the mechanical strength of the molded products.

Method used

A method involving the addition of a water-soluble polymer to the cellulose raw material, followed by defibration and mixing with starch in air, to maintain fiber length and improve mechanical strength.

Benefits of technology

The method effectively maintains cellulose fiber length during defibration, resulting in molded products with enhanced mechanical strength and improved properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581752000001
    Figure 0007581752000001
Patent Text Reader

Abstract

To provide a method for manufacturing a molding material that can maintain long fiber lengths of cellulose even after a dry defibrating step, and can ensure high strength of a molded product of the resulting cellulose.SOLUTION: A method for manufacturing an injection molding material includes: an imparting step of imparting a water-soluble polymer to a cellulose raw material; a defibrating step of defibrating the cellulose raw material having the water-soluble polymer imparted thereto to form a defibrated material; and a mixing step of mixing the defibrated material with starch in a gas atmosphere.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an injection molding material and an injection molding material. [Background technology]

[0002] A method that uses little or no water, called a dry method, is expected to be developed as a method for manufacturing products containing cellulose fibers, such as paper, paper plates, and paper boards. Since a large amount of water is generally used to mold paper products, development is being carried out with the aim of reducing the amount of water used.

[0003] For example, Patent Document 1 discloses a method for obtaining defibrated cellulose fibers by mechanically defibrating a cellulose raw material together with a silicone-based surfactant, and also discloses a method for producing a resin composition using the defibrated cellulose fibers. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2019-001938 A Summary of the Invention [Problem to be solved by the invention]

[0005] Patent Document 1 describes that the addition of a silicone surfactant suppresses the breakage of cellulose fibers caused by mechanical defibration. However, when this method is used, the silicone surfactant remains in the cellulose fibers after defibration. The silicone surfactant may weaken the bond between fibers, and even if the fiber length of the cellulose fibers after defibration is maintained long, the mechanical strength of the molded product made using the same may not necessarily be high.

[0006] There is a demand for a molding material that can maintain the cellulose fiber length long even after the cellulose raw material has been subjected to a dry fiberization process, and that can provide molded products using the resulting cellulose with good mechanical strength. [Means for solving the problem]

[0007] One aspect of the method for producing an injection molding material according to the present invention is to An application step of applying a water-soluble polymer to a cellulose raw material; a defibration step of defibrating the cellulose raw material to which the water-soluble polymer has been applied to produce a defibrated material; a mixing step of mixing the defibrated material and starch in air; Includes.

[0008] One aspect of the injection molding material according to the present invention is Fiberized cellulose; A water-soluble polymer; Starch and Including, Density: 0.001g / cm 3 More than 1.3g / cm 3 The following is the result. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a diagram illustrating a manufacturing apparatus according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Several embodiments of the present invention will be described below. The embodiments described below are merely examples of the present invention. The present invention is not limited to the following embodiments, and includes various modified forms that are implemented within the scope of the present invention. Note that not all of the configurations described below are necessarily essential configurations of the present invention.

[0011] 1. Manufacturing method of injection molding material The manufacturing method of the injection molding material according to this embodiment includes an application step of applying a water-soluble polymer to a cellulose raw material, a defibration step of defibrating the cellulose raw material to which the water-soluble polymer has been applied to produce a defibrated material, and a mixing step of mixing the defibrated material with starch in air.

[0012] 1.1. Application process The method for producing an injection molding material according to this embodiment includes a step of adding a water-soluble polymer to a cellulose raw material. The step is carried out before the fiberization step, and this step can suppress the cellulose from being broken down into short fibers during the fiberization step.

[0013] 1.1.1. Cellulose raw materials The cellulose raw material is not particularly limited as long as it contains cellulose. For example, pulp (sheets and bales of broadleaf trees, coniferous trees, kenaf, bagasse, kapok, etc.), paper (copy paper, printing paper, cardboard, etc.), waste paper, tissue paper, kitchen paper, cleaner, filter, liquid absorbent, sound absorber, cushioning material, mat, cardboard, etc. may be used as the cellulose raw material. In addition, multiple types of the exemplified cellulose raw materials may be used.

[0014] The cellulose in the cellulose raw material may be entangled or bound. The cellulose raw material may be a molded product produced from the injection molding material of the present embodiment. The cellulose raw material is more preferably naturally derived or biomass derived. The cellulose raw material may be one that has been subjected to a treatment such as bleaching.

[0015] Cellulose is a plant-derived, abundant natural material, which can more appropriately address environmental issues and save buried resources, and is also preferred from the viewpoints of stable supply of injection molding materials and molded articles produced using the same, cost reduction, etc. Furthermore, cellulose has particularly high theoretical strength among various fibers, and is advantageous from the viewpoint of further improving the strength of molded articles. Furthermore, cellulose has good biodegradability.

[0016] 1.1.2.Water-soluble polymer The water-soluble polymer is added to the cellulose raw material, and as a result, the fiber length of the cellulose in the cellulose raw material is prevented from being shortened when the cellulose is defibrated in the defibration process. The water-soluble polymer is not limited as long as it is a polymer having water solubility. Since the water-soluble polymer can break the hydrogen bonds between cellulose, the fiber can be defibrated with less damage even in dry defibration.

[0017] Examples of water-soluble polymers include synthetic polymers such as polyvinyl alcohol (PVA), polyvinylpyrrolidone (PVP), polyacrylic acid, ethylene-acrylic acid copolymer, polyethylene glycol (PEG), and polypropylene glycol (PPG); modified celluloses such as carboxymethyl cellulose (CMC), methyl cellulose (MC), and hydroxyethyl cellulose (HEC); and natural or naturally derived polymers and polysaccharides such as guar gum, carrageenan, sodium alginate, cationized guar gum, xanthan gum, sodium chondroitin sulfate, sodium hyaluronate, glue, and casein.

[0018] Among these, the fact that it can suppress the shortening of cellulose fibers due to defibration and that it is easily available are the advantages. In some respects, it is preferred to select from polyvinyl alcohol (PVA), polyacrylic acid, ethylene-acrylic acid copolymers, polyethylene glycol, polypropylene glycol, polysaccharides, modified celluloses, glue, and casein. Two or more types of water-soluble polymers may be mixed and used.

[0019] Furthermore, when polyvinyl alcohol (PVA) is used as the water-soluble polymer, the degree of polymerization of the PVA is preferably from 300 to 2000, more preferably from 400 to 1500, and even more preferably from 500 to 1200. By using PVA with such a degree of polymerization, the effect of suppressing the shortening of cellulose fibers can be further enhanced, water solubility can be improved, and the viscosity of the aqueous solution can be kept low.

[0020] Furthermore, when polyvinyl alcohol (PVA) is used as the water-soluble polymer, the saponification degree of the PVA is preferably 75% or more and 99% or less, more preferably 80% or more and 95% or less. By using PVA with such a saponification degree, the water solubility can be easily adjusted to an appropriate range for use in the application step.

[0021] 1.1.3. Method of application process The method for applying the water-soluble polymer to the cellulose raw material is not particularly limited, but examples include a method in which an aqueous solution of the water-soluble polymer is prepared and the cellulose raw material is immersed in the solution, a method in which the aqueous solution is sprayed or applied to the cellulose raw material, and a method in which the water-soluble polymer is sprinkled in powder form on the cellulose raw material, with water being added as necessary.

[0022] The amount of the water-soluble polymer added to the cellulose raw material is preferably 0.01% by mass or more, more preferably 0.02% by mass or more, preferably 0.05% by mass or more, and preferably 0.1% by mass or more, relative to the cellulose raw material. The upper limit of the amount added is not particularly limited, but is preferably 100.0% by mass or less, and preferably 80.0% by mass or less.

[0023] When the amount of the water-soluble polymer applied to the cellulose raw material is equal to or greater than the lower limit, the cellulose can be prevented from being broken during defibration. When the amount is equal to or less than the upper limit, adhesion of the water-soluble polymer to the defibrator can be easily prevented.

[0024] When an aqueous solution is used to apply the water-soluble polymer to the cellulose raw material in the application step, the concentration of the aqueous solution is not particularly limited and can be appropriately set taking into consideration the amount of the water-soluble polymer to be applied to the cellulose raw material, the viscosity of the aqueous solution, the ease of handling of the aqueous solution, etc.

[0025] When moisture is added to the cellulose raw material in the adding step, the moisture may or may not be dried before the defibration step. When the defibration step is performed in a moisture-free state, it is preferable to dry the moisture added in the adding step.

[0026] 1.2. Defibration process The manufacturing method of the injection molding material of this embodiment includes a defibration step. The defibration step can be performed by dry defibration of the cellulose raw material. A defibrated material containing cellulose that has been fibrousized by the defibration step is obtained. Defibration can be performed, for example, by a defibration unit of a manufacturing device described later. The defibration step may be performed together with a small amount of water as necessary.

[0027] In the defibration process, defibration is not performed using a large amount of liquid water, but is performed in a gas such as air or nitrogen. That is, the defibration process may be performed in a completely dry state without water, or in a state where a small amount of liquid water or water vapor is present.

[0028] Water or steam may be intentionally added in the defibration process. In that case, it is preferable to add water or steam to an extent that does not require too much energy or time to remove the water by heating or the like in the subsequent process.

[0029] Therefore, the injection molding material produced by the production method of this embodiment contains fiberized cellulose. The fiberized cellulose is one component of the molded product produced by using the injection molding material, and contributes to maintaining the shape of the molded product and maintains and improves the properties of the molded product, such as its strength.

[0030] In this specification, "fibrillated cellulose" refers to cellulose that has been made into a fibrous form by defibrating a cellulose-containing raw material such as pulp or paper. Fiberized cellulose can refer to a single fibrous cellulose strand or to an aggregate of multiple fibrous cellulose strands (e.g., in a cotton-like state). Through fiberization, the cellulose in the raw cellulose material is disentangled into fibers.

[0031] The average length of the fiberized cellulose is not particularly limited, but is preferably 0.1 mm or more and 50.0 mm or less, more preferably 0.2 mm or more and 5.0 mm or less, and even more preferably 0.3 mm or more and 3.0 mm or less. The length of the fiberized cellulose may have variation (distribution).

[0032] This makes it possible to improve the shape stability, strength, etc. of molded products produced using the injection molding material.

[0033] The average thickness of the fiberized cellulose is not particularly limited, but is preferably 0.005 mm or more and 0.5 mm or less, and more preferably 0.010 mm or more and 0.05 mm or less. The thickness of the fiberized cellulose may have variation (distribution).

[0034] This makes it possible to improve the stability of shape, strength, etc. of the molded product produced using the injection molding material. In addition, it is possible to further suppress the occurrence of irregularities on the surface of the molded product produced using the injection molding material.

[0035] The average aspect ratio of the fiberized cellulose, that is, the average length to the average thickness, is not particularly limited, but is preferably 10 or more and 1,000 or less, and more preferably 15 or more and 500 or less.

[0036] This makes it possible to improve the stability of shape, strength, etc. of the molded product produced using the injection molding material. In addition, it is possible to further suppress the occurrence of irregularities on the surface of the molded product produced using the injection molding material.

[0037] The average length, average thickness, and average aspect ratio of the fiberized cellulose can be measured, for example, by using a commercially available fiber tester.

[0038] The fiberized cellulose has hydroxyl groups, and hydrogen bonds are easily formed between the fiberized cellulose and starch described below, which can improve the bonding strength between the fiberized cellulose and starch, the overall strength of the molded product produced using the injection molding material, for example, the specific tensile strength of a sheet-like molded product, etc.

[0039] The content of fiberized cellulose in the injection molding material is not particularly limited, but is preferably 20.0% by mass or more and 99.0% by mass or less, more preferably 25.0% by mass or more and 98.0% by mass or less, and more preferably 28.0% by mass or more and 97.0% by mass or less. The content of the fiberized cellulose in the injection molding material can be adjusted by the amount of the cellulose mixed in the mixing step described below.

[0040] This makes it possible to improve the shape stability, strength, and other properties of a molded product produced using the injection molding material. In addition, it is possible to improve the moldability during production of the molded product, which is also advantageous in terms of improving the productivity of the molded product.

[0041] In this embodiment, the defibration process is carried out in a state in which cellulose fibers and water-soluble polymers coexist, so the fiberized cellulose obtained by the defibration process is less likely to have a short fiber length compared to the cellulose in the original cellulose raw material.

[0042] 1.3.Mixing process The manufacturing method of the injection molding material of this embodiment includes a mixing step, in which the defibrated material produced in the defibrating step and starch are mixed in air.

[0043] 1.3.1. Starch The injection molding material of the present embodiment contains starch. Starch is one component of a molded product produced using the injection molding material, and contributes to maintaining the shape of the molded product and maintains and improves the strength and other properties of the molded product. Starch is a component that functions as a binder that binds together fiberized cellulose in a molded product produced using the injection molding material.

[0044] Starch is a polymeric material formed by the polymerization of multiple α-glucose molecules through glycosidic bonds. Starch may be linear or branched.

[0045] Starch derived from various plants can be used. Examples of starch sources include cereals such as corn, wheat, and rice, beans such as broad beans, mung beans, and red beans, tubers such as potato, sweet potato, and tapioca, wild plants such as dogtooth violets, bracken, and kudzu, and palms such as sago palm.

[0046] In addition, processed starch or modified starch may be used as the starch. Examples of the processed starch include acetylated adipic acid crosslinked starch, acetylated starch, oxidized starch, sodium octenyl succinate starch, hydroxypropyl starch, hydroxypropylated phosphate crosslinked starch, phosphorylated starch, phosphate esterified phosphate crosslinked starch, urea phosphate esterified starch, sodium starch glycolate, and high amylose corn starch. Examples of the modified starch include alpha-starch, dextrin, lauryl polyglucose, cationic starch, thermoplastic starch, and carbamic acid starch.

[0047] The starch content in the total amount of the injection molding material is preferably 2.0% by mass or more and 70.0% by mass or less, more preferably 3.0% by mass or more and 65.0% by mass or less, and even more preferably 10.0% by mass or more and 30.0% by mass or less. The starch content can be measured by component analysis such as NMR method, and can be measured using a pretreatment method such as enzymatic decomposition as necessary. The starch content in the injection molding material can be adjusted by the mixing amount in the mixing step described below.

[0048] 1.3.2. Mixing process method In this specification, "mixing in air" refers to mixing by the action of an air current. The mixing process in the mixing step is a method (dry method) in which cellulose and starch are introduced into an air current and diffused into each other in the air current, which is a hydrodynamic mixing process.

[0049] In the mixing process, the mixture is mixed in a gas such as air or nitrogen, rather than in a large amount of liquid water. In other words, the mixing process may be performed in a completely dry state without water, or in a liquid state. Mixing may be performed in the presence of a small amount of body water or water vapor.

[0050] Water or steam may be intentionally added in the mixing step. In that case, it is preferable to add the water in an amount that does not require too much energy or time to remove the water by heating or the like in a subsequent step.

[0051] The mixing step can be carried out using a known device such as an FM mixer, a Henschel mixer, or a super mixer. The device may be one that uses a blade that rotates at high speed to stir, or one that uses the rotation of a container such as a V-type mixer. Furthermore, the device may be a batch type device or a continuous type device. An example of a continuous type device is the mixing section of the manufacturing device described below, which is preferable.

[0052] 1.4.Other processes A method for producing a material for injection molding may, for example, include the following steps.

[0053] 1.4.1.Plasticizer application process The manufacturing method of the injection molding material may include a plasticizer applying step. In the plasticizer applying step, a plasticizer is applied to the defibrated material. The plasticizer has a function of plasticizing starch, and the application of the plasticizer promotes fluidization of the injection molding material by heating, making molding easier.

[0054] The plasticizer application process is carried out at least after the defibration process. The method of the plasticizer application process is not particularly limited, as with the above-mentioned application process, but examples include a method of preparing an aqueous solution of the plasticizer and immersing the defibrated material in the solution, a method of spraying or applying the aqueous solution to the defibrated material, and a method of sprinkling the plasticizer in powder form on the defibrated material, adding water as necessary.

[0055] Examples of the plasticizer include glycerin, urea, guanidine hydrochloride, dimethyl sulfoxide, salicylate, alkali salt (sodium hydroxide, potassium hydroxide, thiocyanate, potassium iodide, ammonium nitrate, calcium chloride, etc.), acid (hydrochloric acid, sulfuric acid), sugar (sorbitol, xylitol, mannitol, erythritol, lactitol), etc. A plurality of plasticizers may be used. The amount of the plasticizer applied in the plasticizer application step is 0.01% by mass or more and 30.0% by mass or less based on the starch.

[0056] 1.4.2. Processing process The processing step may be performed after the mixing step, for example, to facilitate handling of the injection molding material. The injection molding material is obtained through the mixing step, but may be further shaped into a sheet, coarsely crushed pieces, or pellets through a processing step. That is, the processing step provides a sheet, coarsely crushed, or pellet-shaped injection molding material.

[0057] 1.4.3. Molding process The molding step can be carried out, for example, by a molding section of a manufacturing apparatus described later, in which case a sheet-like injection molding material can be obtained. If necessary, the sheet-like injection molding material can be cut by a shredder or the like, in which case a rough piece of injection molding material can be obtained. The processing step can also be carried out using a known pelletizer, in which case a pellet-like injection molding material can be obtained.

[0058] 1.5. Materials for injection molding As described above, the injection molding material according to the present embodiment includes fiberized cellulose, a water-soluble polymer, and starch. The injection molding material may be in the form of fluff, web, sheet, pellet, or the like, but should have a density of 0.001 g / cm or less. 3 More than 1.3g / cm 3 Less than or equal to 0.005 g / cm 3 More than 1.15g / cm 3 Preferably, it is equal to or less than 0. .01g / cm 3 More than 1.05g / cm 3 More preferably, it is 0.05 g / cm or less. 3 More than 0.95g / cm 3 It is even more preferable that:

[0059] If the density of the injection molding material is within the above range, the material can be easily handled during injection molding. 3 If the density is greater than 0.001 g / cm, the dispersion of the material in the subsequent kneading and injection molding processes will be incomplete (the material will not be completely loosened), and the composition of the molded product will become non-uniform, which may cause lumps or unevenness. 3 If the density is less than 0.001 g / cm, the cellulose particles will be too coarse, making it difficult to form a web, and may be difficult to transport in the subsequent kneading and injection molding processes. 3 If it is less than this, there is an increased risk that each material will fall off from the cellulose.

[0060] As described above, the injection molding material contains the water-soluble polymer and starch in addition to the fiberized cellulose, and the starch may bind the fiberized cellulose or may simply be attached thereto.

[0061] In addition to cellulose, water-soluble polymers, and starch, the injection molding material may contain, for example, cellulose-derived glues such as natural gum glues such as etherified tamarind gum, etherified locust bean gum, etherified guar gum, and acacia arabic gum; polysaccharides such as glycogen; seaweed; animal proteins such as collagen; sizing agents; impurities derived from fiberized cellulose; impurities derived from starch; hemicellulose; lignin; and synthetic polymers such as rayon, lyocell, cupra, vinylon, acrylic, nylon, aramid, polyester, polyethylene, polypropylene, polyurethane, and polyimide.

[0062] However, the content of components other than the fiberized cellulose, the water-soluble polymer, and the starch in the injection molding material is preferably 10% by mass or less, more preferably 5.0% by mass or less, and even more preferably 2.0% by mass or less.

[0063] The injection molding material may or may not contain moisture. When the injection molding material is left in an environment of 27° C. / 98% RH for 2 hours, the moisture content is, for example, 10% by mass or more and 55% by mass or less.

[0064] The moisture content can be measured, for example, by taking 0.7 g of the injection molding material, sifting the injection molding material into a disk-like layer on cooking paper using a Raffiné stainless steel automatic powder sifter M manufactured by Pearl Metal Co., Ltd., placing the cooking sheet together on a stainless steel Pishatt mesh basket (manufactured by Shinetsu Works Co., Ltd.), and leaving it in a thermostatic chamber (Platinus (registered trademark) K series PL-3KPH thermo-hygrometer manufactured by Espec Corporation) at an environmental setting of 27°C / 98% RH for 2 hours, and then using a heat-drying moisture meter (MX-50 manufactured by A&B Corporation).

[0065] 1.6. Injection molding The injection molding material of this embodiment is used for injection molding. Injection molding can be performed by a known injection molding machine. The injection molding material of this embodiment can exhibit flowability suitable for injection molding by melting the water-soluble polymer. Furthermore, water may be added to the injection molding material during injection molding, thereby softening or gelatinizing the starch. This facilitates the formation of hydrogen bonds between cellulose and starch. Furthermore, hydrogen bonds between celluloses also facilitate the formation of hydrogen bonds.

[0066] When injection molding is performed using the injection molding material, the amount of water added to the injection molding material is about 70% by mass, preferably 60% by mass or less, and more preferably 50% by mass or less, in terms of moisture content. The temperature during injection molding is preferably 50°C or more and 200°C or less.

[0067] 1.7. Molded objects The molded product obtained by injection molding the injection molding material is molded into a predetermined shape using a predetermined mold. As a result, the molded product has excellent mechanical strength and biodegradability. In addition, the molded product has excellent recyclability, and even when recycled, the fiber length of the cellulose is unlikely to shorten, so that the decrease in mechanical strength is suppressed.

[0068] The shape of the molded product is not particularly limited, and may be any shape, such as a sheet, a block, a sphere, or a three-dimensional shape.

[0069] The molded product may be at least partially made of the above-mentioned injection molding material, and may have a portion that is not made of the injection molding material. The use of the molded product is also not particularly limited.

[0070] 2.Injection molding material manufacturing equipment Next, a manufacturing apparatus that can be suitably applied to the method for manufacturing a material for injection molding will be described. Fig. 1 is a schematic side view showing a suitable example of the manufacturing apparatus.

[0071] In the following, the upper side of FIG. 1 may be referred to as "upper" or "upper side", and the lower side may be referred to as "lower" or "lower side". FIG. 1 is a schematic diagram, and the positional relationship of each part of the manufacturing apparatus 100 may differ from the actual positional relationship. In each figure, the direction in which the cellulose raw material M1, the coarsely crushed pieces M2, the defibrated material M3, the first sorted material M4-1, the second sorted material M4-2, the first web M5, the fragmented body M6, the mixture M7, the second web M8, and the sheet S are transported, that is, the direction indicated by the arrow, is also referred to as the transport direction. The tip side of the arrow is also referred to as the downstream side of the transport direction, and the base side of the arrow is also referred to as the upstream side of the transport direction.

[0072] 1 is an apparatus that roughly crushes and defibrates a cellulose raw material M1, supplies water-soluble polymer and starch as additives from an additive supply unit 171, mixes the fibrous cellulose, water-soluble polymer and starch in air in a mixing unit 17, deposits them, and molds the deposit in a molding unit 20 to obtain a sheet-like molded product. After passing through the mixing unit 17, a material for injection molding is produced, and in the manufacturing apparatus 100, a sheet-like molded product is formed as the material for injection molding.

[0073] In the following description, a case will be mainly described in which waste paper is used as the cellulose raw material M1 and the molded product produced is a sheet S of recycled paper.

[0074] 1 includes a sheet supplying device 11, a crushing section 12, a defibrating section 13, a sorting section 14, a first web forming section 15, a fragmenting section 16, a mixing section 17, a dispersion section 18, a second web forming section 19, a forming section 20, a cutting section 21, a stocking section 22, a recovery section 27, and a control section 28 that controls the operation of these sections. Each of the crushing section 12, the defibrating section 13, the sorting section 14, the first web forming section 15, the fragmenting section 16, the mixing section 17, the dispersion section 18, the second web forming section 19, the forming section 20, the cutting section 21, and the stocking section 22 is a processing section that processes a sheet.

[0075] The sheet supplying device 11 and the crushing section 12 or the defibrating section 13 form a sheet processing device 10A. The sheet processing device 10A and the second web forming section 19 form a fibrous material depositing device 10B.

[0076] The manufacturing apparatus 100 also includes a humidifier 231, a humidifier 232, a humidifier 233, a humidifier 234, a humidifier 235, and a humidifier 236. In addition, the manufacturing apparatus 100 includes The blower 261, the blower 262, and the blower 263 are provided.

[0077] Moreover, the humidifiers 231 to 236 and the blowers 261 to 263 are electrically connected to the control unit 28, and their operation is controlled by the control unit 28. That is, in this embodiment, the operation of each part of the manufacturing apparatus 100 is controlled by one control unit 28. However, without being limited thereto, for example, the manufacturing apparatus 100 may be configured to have a control unit that controls the operation of each part of the sheet supplying device 11 and a control unit that controls the operation of parts other than the sheet supplying device 11.

[0078] Furthermore, the manufacturing apparatus 100 executes a raw material supplying process, a coarse crushing process, a defibrating process, a sorting process, a first web forming process, a dividing process, a mixing process, a releasing process, a stacking process, a sheet forming process, and a cutting process. Among these, the mixing process corresponds to the mixing process in the manufacturing method of the injection molding material.

[0079] The configuration of each part will be described below. The sheet supplying device 11 is a part that performs a raw material supplying process of supplying the cellulose raw material M1 to the crushing part 12. The cellulose raw material M1 used is one that contains cellulose. Alternatively, the cellulose raw material M1 may be a molded product of an injection molding material that contains fibrous cellulose, and water-soluble polymer and starch attached to the fibrous cellulose.

[0080] The crushing unit 12 is a section that performs a crushing step of crushing the cellulose raw material M1 supplied from the sheet supply device 11 in air or the like.

[0081] The pair of crushing blades 121 rotate in opposite directions to each other, and thereby crush the cellulose raw material M1 between them, i.e., cut it into crushed pieces M2. The shape and size of the crushed pieces M2 are preferably suitable for defibration processing in the defibration unit 13, and for example, are preferably small pieces with a side length of 100 mm or less, and more preferably 10 mm or more and 70 mm or less.

[0082] The chute 122 is disposed below the pair of crushing blades 121 and has, for example, a funnel shape. This allows the chute 122 to receive the coarsely crushed pieces M2 that have been crushed by the crushing blades 121 and dropped.

[0083] In addition, above the chute 122, a humidifying section 231 is disposed adjacent to the pair of coarse crushing blades 121. The humidifying section 231 humidifies the coarsely crushed pieces M2 in the chute 122. The humidifying section 231 is configured as an evaporation type humidifier that has a moisture-containing filter and supplies humidified air with increased humidity to the coarsely crushed pieces M2 by passing air through the filter. By supplying humidified air to the coarsely crushed pieces M2, the humidifying process described above can be performed, and the effects described above can be obtained. In addition, the coarsely crushed pieces M2 can be prevented from adhering to the chute 122, etc. due to static electricity.

[0084] The chute 122 is connected to the defibrating unit 13 via a pipe 241. The coarse crushed pieces M2 collected in the chute 122 pass through the pipe 241 and are transported to the defibrating unit 13.

[0085] When the manufacturing apparatus 100 is used in the manufacturing method of the injection molding material of this embodiment, a water-soluble polymer is applied before the material is introduced into the defibrating unit 13. The water-soluble polymer may be applied to the cellulose raw material M1, or may be applied to the coarsely crushed pieces M2. When the water-soluble polymer is applied to the coarsely crushed pieces M2, the coarsely crushed pieces M2 correspond to the cellulose raw material. In addition, the water-soluble polymer may be applied by an appropriate configuration not shown in the manufacturing apparatus 100, or the manufacturing apparatus 100 may be provided with a cellulosic raw material. A water-soluble polymer may be added outside the apparatus before the introduction of the sucrose raw material M1.

[0086] The defibrating unit 13 is a section that performs a defibrating process in which the coarsely crushed pieces M2 are defibrated in the air, i.e., in a dry manner. The defibrating process in this defibrating unit 13 can produce a defibrated material M3 from the coarsely crushed pieces M2. Here, "defibrating" refers to untangling the coarsely crushed pieces M2, which are made up of multiple fibrous cellulose particles bound together, into individual fibers. This untangled material becomes the defibrated material M3. The shape of the defibrated material M3 is linear or band-like. The defibrated material M3 may also be present in a state where it is entangled with other pieces to form a mass, i.e., in a state where it forms so-called "lumps."

[0087] In this embodiment, for example, the defibrating unit 13 is configured with an impeller mill having a rotary blade that rotates at high speed and a liner located on the outer periphery of the rotary blade. The coarse fragments M2 that flow into the defibrating unit 13 are sandwiched between the rotary blade and the liner and defibrated.

[0088] Furthermore, the defibrating unit 13 can generate an air flow from the crushing unit 12 toward the sorting unit 14, i.e., an airflow, by the rotation of the rotary blades. This allows the coarsely crushed pieces M2 to be sucked into the defibrating unit 13 from the pipe 241. Furthermore, after the defibrating process, the defibrated material M3 can be sent to the sorting unit 14 via the pipe 242.

[0089] A blower 261 is installed in the middle of the pipe 242. The blower 261 is an airflow generating device that generates an airflow toward the screening section 14. This promotes the sending out of the defibrated material M3 to the screening section 14.

[0090] The sorting unit 14 is a section that performs a sorting process in which the defibrated material M3 is sorted according to the length of the fibrous cellulose. In the sorting unit 14, the defibrated material M3 is sorted into a first sorted material M4-1 and a second sorted material M4-2 that is larger than the first sorted material M4-1. The first sorted material M4-1 has a size suitable for the subsequent production of the sheet S. It is preferable that the average length is 1 μm or more and 30 μm or less. On the other hand, the second sorted material M4-2 includes, for example, insufficiently defibrated material and material in which defibrated fibrous cellulose has excessively aggregated together.

[0091] The sorting unit 14 has a drum unit 141 and a housing unit 142 that houses the drum unit 141.

[0092] The drum part 141 is a sieve composed of a cylindrical mesh body and rotates around its central axis. The defibrated material M3 flows into this drum part 141. Then, as the drum part 141 rotates, the defibrated material M3 smaller than the mesh opening is sorted as the first sorted material M4-1, and the defibrated material M3 larger than the mesh opening is sorted as the second sorted material M4-2. The first sorted material M4-1 falls from the drum part 141.

[0093] Meanwhile, the second sorted material M4-2 is sent to a pipe 243 connected to the drum section 141. The pipe 243 is connected to the pipe 241 on the side opposite the drum section 141, i.e., the upstream side. The second sorted material M4-2 that passes through this pipe 243 merges with the coarsely crushed pieces M2 in the pipe 241 and flows into the defibrating section 13 together with the coarsely crushed pieces M2. As a result, the second sorted material M4-2 is returned to the defibrating section 13 and is defibrated together with the coarsely crushed pieces M2.

[0094] The first selected object M4-1 that has fallen from the drum unit 141 falls while dispersing in the air, and heads toward the first web forming unit 15 located below the drum unit 141. The first web forming unit 15 is a section in which a first web forming step is carried out to form a first web M5 from the first selected object M4-1. The first web forming unit 15 comprises a mesh belt 151 and three tension rollers 152. and a suction portion 153.

[0095] The mesh belt 151 is an endless belt on which the first sorted material M4-1 is accumulated. The mesh belt 151 is wound around three tension rollers 152. As the tension rollers 152 rotate, the first sorted material M4-1 on the mesh belt 151 is transported downstream.

[0096] The size of the first sorted material M4-1 is equal to or larger than the mesh size of the mesh belt 151. This restricts the passage of the first sorted material M4-1 through the mesh belt 151, and therefore the first sorted material M4-1 can be piled up on the mesh belt 151. Furthermore, the first sorted material M4-1 is transported downstream together with the mesh belt 151 while being piled up on the mesh belt 151, and is thus formed as a layered first web M5.

[0097] In addition, the first sorted material M4-1 may contain, for example, dust or dirt. Dust or dirt may be generated, for example, by crushing or defibrating. Such dust or dirt will be collected in the collection section 27.

[0098] The suction unit 153 is a suction mechanism that sucks air from below the mesh belt 151. This makes it possible to suck in dust and dirt that has passed through the mesh belt 151 together with the air.

[0099] In addition, the suction unit 153 is connected to the collection unit 27 via a pipe 244. The dust and dirt sucked by the suction unit 153 is collected in the collection unit 27.

[0100] A pipe 245 is further connected to the collection unit 27. A blower 262 is installed in the middle of the pipe 245. By operating the blower 262, a suction force can be generated in the suction unit 153. This promotes the formation of the first web M5 on the mesh belt 151. Dust and dirt are removed from this first web M5. By operating the blower 262, the dust and dirt pass through the pipe 244 and reach the collection unit 27.

[0101] The housing part 142 is connected to the humidifying part 232. The humidifying part 232 is configured as an evaporative humidifier. This allows humidified air to be supplied into the housing part 142. The above-mentioned humidifying process can be performed by this humidified air, and the above-mentioned effects can be obtained. In addition, the first sorted object M4-1 can be humidified, and therefore, the first sorted object M4-1 can be prevented from adhering to the inner wall of the housing part 142 due to electrostatic force.

[0102] The humidifying section 235 is disposed downstream of the sorting section 14. The humidifying section 235 is configured with an ultrasonic humidifier that sprays water. This allows moisture to be supplied to the first web M5, and thus the moisture content of the first web M5 is adjusted. This adjustment allows the humidifying process to be performed, and the above-mentioned effects can be obtained. In addition, the adhesion of the first web M5 to the mesh belt 151 due to electrostatic force can be suppressed. This allows the first web M5 to be easily peeled off from the mesh belt 151 at the position where the mesh belt 151 is folded back by the tension roller 152.

[0103] The segmentation unit 16 is disposed downstream of the humidification unit 235. The segmentation unit 16 is a portion that performs a segmentation step of segmenting the first web M5 peeled off from the mesh belt 151. The segmentation unit 16 has a rotatably supported propeller 161 and a housing portion 162 that houses the propeller 161. The first web M5 is segmented by the rotating propeller 161. The divided first web M5 becomes a segmented body M6. The segmented body M6 moves down inside the housing portion 162.

[0104] The housing part 162 is connected to the humidifying part 233. The humidifying part 233 is configured as an evaporation type humidifier. This allows humidified air to be supplied into the housing part 162. The humidifying process can be performed by this humidified air, and the above-mentioned effects can be obtained. In addition, it is also possible to prevent the fragmented bodies M6 from adhering to the propeller 161 and the inner wall of the housing part 162 due to electrostatic force.

[0105] A mixing section 17 is disposed downstream of the subdivision section 16. The mixing section 17 is a section in which a mixing step is performed to mix the subdivision bodies M6 with an additive. The mixing section 17 has an additive supply section 171, a pipe 172, and a blower 173.

[0106] The pipe 172 connects the housing portion 162 of the subdivision portion 16 and the housing 182 of the dispersion portion 18, and is a flow path through which the mixture M7 of the subdivision bodies M6 and the additive passes.

[0107] An additive supply unit 171 is connected to the middle of the pipe 172. The additive supply unit 171 has a housing portion 170 in which an additive is accommodated, and a screw feeder 174 provided in the housing portion 170. By rotation of the screw feeder 174, the additive in the housing portion 170 is pushed out from the housing portion 170 and supplied into the pipe 172. The additive supplied into the pipe 172 is mixed with the fragmented bodies M6 to become a mixture M7.

[0108] Here, examples of additives supplied from the additive supply unit 171 include a binder for binding fibers together, a colorant for coloring the fibers, an aggregation inhibitor for inhibiting aggregation of the fibers, a flame retardant for making the fibers less flammable, a paper strength enhancer for enhancing the paper strength of the sheet S, defibrated materials, etc., and one or a combination of a plurality of these can be used. The following describes the case where the additive is starch P1.

[0109] By supplying starch P1 from the additive supply unit 171, a suitable injection molding material can be obtained even when the starch content in the cellulose raw material M1 is relatively low or when a relatively large proportion of the starch contained in the cellulose raw material M1 is removed by the treatment using the production apparatus 100. In other words, the contents of the water-soluble polymer and starch in the injection molding material can be set within a predetermined range.

[0110] In addition, a blower 173 is installed in the middle of the pipe 172 downstream of the additive supply section 171. The action of the rotating part such as a blade of the blower 173 promotes the mixing of the fragmented bodies M6 and the starch P1. In addition, the blower 173 can generate an airflow toward the dispersion section 18. This airflow can agitate the fragmented bodies M6 and the starch P1 in the pipe 172. The fragmented bodies M6 in the mixture M7 are loosened in the process of passing through the pipe 172 and become finer fibrous. As a result, the mixture M7 is in a state in which the fragmented bodies M6 are loosened and the starch P1 is uniformly dispersed. That is, by passing through the mixing section 17, an injection molding material in which starch is uniformly distributed in an aggregate of fibrous cellulose is produced.

[0111] In this embodiment, the mixture M7, which is an injection molding material, is formed into a sheet shape, so the mixture M7 is further transported to a dispersion section 18. In this embodiment, the mixture M7, the second web M8, and the sheet S all correspond to the injection molding material.

[0112] The blower 173 is electrically connected to the control unit 28, and the operation thereof is controlled by the control unit 28. By adjusting the airflow rate of the blower 173, the amount of air sent into the drum 181 can be adjusted.

[0113] Although not shown in the figure, the end of pipe 172 on the drum 181 side is branched into two, and the branched ends are each connected to an inlet port (not shown) formed on the end face of drum 181.

[0114] 1 is a section that performs a discharging step of loosening and discharging entangled fibers in the mixture M7. The dispersing section 18 has a drum 181 that introduces and discharges the mixture M7, a housing 182 that contains the drum 181, and a drive source 183 that drives the drum 181 to rotate.

[0115] The drum 181 is a sieve that is composed of a cylindrical mesh body and rotates around its central axis. As the drum 181 rotates, fibers and the like of the mixture M7 that are smaller than the mesh openings can pass through the drum 181. At that time, the mixture M7 is further loosened and discharged together with air. That is, the drum 181 functions as a discharge section that discharges the material containing fibers.

[0116] Although not shown, the driving source 183 has a motor, a reducer, and a belt. The motor is electrically connected to the control unit 28 via a motor driver. Furthermore, the rotational force output from the motor is reduced by the reducer. The belt is, for example, an endless belt, and is wound around the output shaft of the reducer and the outer periphery of the drum. As a result, the rotational force of the output shaft of the reducer is transmitted to the drum 181 via the belt.

[0117] In addition, the housing 182 is connected to the humidifying section 234. The humidifying section 234 is configured as an evaporative humidifier. This allows humidified air to be supplied into the housing 182. The inside of the housing 182 can be humidified by this humidified air, and the humidifying process can be performed, thereby obtaining the above-mentioned effects. In addition, it is also possible to prevent the mixture M7 from adhering to the inner wall of the housing 182 due to electrostatic force.

[0118] Furthermore, the mixture M7 discharged from the drum 181 falls while being dispersed in the air, and heads toward the second web forming unit 19 located below the drum 181. The second web forming unit 19 is a section where a deposition step is carried out in which the mixture M7 is deposited to form a second web M8, which is a deposit. The second web forming unit 19 has a mesh belt 191, a tension roller 192, and a suction unit 193.

[0119] The mesh belt 191 is a mesh member, and in the illustrated configuration, is configured as an endless belt. The mixture M7 dispersed and discharged by the dispersion unit 18 is accumulated on the mesh belt 191. The mesh belt 191 is wound around four tension rollers 192. The mixture M7 on the mesh belt 191 is transported downstream by the rotational drive of the tension rollers 192.

[0120] In the illustrated configuration, the mesh belt 191 is used as an example of the mesh member, but the present invention is not limited to this, and the mesh member may be, for example, a flat plate-like member.

[0121] Moreover, most of the mixture M7 on the mesh belt 191 has a size equal to or larger than the mesh openings of the mesh belt 191. This prevents the mixture M7 from passing through the mesh belt 191, and therefore the mixture M7 can be accumulated on the mesh belt 191. Moreover, the mixture M7 is transported downstream together with the mesh belt 191 while being accumulated on the mesh belt 191, and is thus formed as a layered second web M8.

[0122] The suction unit 193 is a suction mechanism that sucks air from below the mesh belt 191. This allows the mixture M7 to be sucked onto the mesh belt 191, thereby facilitating deposition of the mixture M7 on the mesh belt 191.

[0123] A pipe 246 is connected to the suction unit 193. A blower 263 is provided midway through the pipe 246. By operating the blower 263, the suction unit 193 can generate a suction force.

[0124] The humidifying section 236 is disposed downstream of the dispersion section 18. The humidifying section 236 is configured with an ultrasonic humidifier similar to the humidifying section 235. This allows moisture to be supplied to the second web M8, and thus the moisture content of the second web M8 is adjusted. This adjustment allows the humidifying process to be performed, and the above-mentioned effects can be obtained. In addition, the adhesion of the second web M8 to the mesh belt 191 due to electrostatic force can be suppressed. This allows the second web M8 to be easily peeled off from the mesh belt 191 at the position where the mesh belt 191 is folded back by the tension roller 192.

[0125] The total amount of moisture added from the humidifying units 231 to 236 is not particularly limited, but the moisture content of the mixture at the end of the humidifying process, i.e., the ratio of the mass of moisture contained in the second web M8 to the mass of the second web M8 in a state humidified by the humidifying unit 236, is preferably 15% by mass to 50% by mass, more preferably 18% by mass to 45% by mass, and even more preferably 20% by mass to 40% by mass. The humidifying units 234 and 236 are operated as necessary so that the second web M8 and the sheet S as injection molding materials have properties suitable for injection molding.

[0126] A forming section 20 is disposed downstream of the second web forming section 19. The forming section 20 is a section in which a sheet forming step is performed to form a sheet S from the second web M8, which is a mixture. The forming section 20 has a pressurizing section 201 and a heating section 202.

[0127] The pressurizing unit 201 has a pair of calender rollers 203, and can pressurize the second web M8 between the calender rollers 203 without heating it. This increases the density of the second web M8. The second web M8 is transported toward the heating unit 202. Note that one of the pair of calender rollers 203 is a driven roller driven by the operation of a motor (not shown), and the other is a driven roller.

[0128] The heating section 202 has a pair of heating rollers 204, and can heat and pressurize the second web M8 between the heating rollers 204. This forms a sheet S. Then, this sheet S is transported toward the cutting section 21. Note that one of the pair of heating rollers 204 is a driven roller that is driven by the operation of a motor (not shown), and the other is a driven roller.

[0129] The cutting unit 21 is disposed downstream of the forming unit 20. The cutting unit 21 is a portion that performs a cutting step of cutting the sheet S. The cutting unit 21 has a first cutter 211 and a second cutter 212.

[0130] The first cutter 211 cuts the sheet S in a direction intersecting the conveying direction of the sheet S, particularly in a direction perpendicular to the conveying direction.

[0131] The second cutter 212 is located downstream of the first cutter 211 and cuts the sheet S in a direction parallel to the conveying direction of the sheet S. This cutting is performed to remove unnecessary portions on both side edges of the sheet S in the width direction to adjust the width of the sheet S, and the cut and removed portions are so-called "selvages."

[0132] A sheet S having a desired shape and size is obtained by such cutting by the first cutter 211 and the second cutter 212. Then, this sheet S is conveyed further downstream and accumulated in the stock unit 22.

[0133] The molding unit 20 is not limited to the above-described configuration for molding the sheet S, and may be configured to mold a block-shaped, spherical, or other shaped object. The molding unit 20 may also include a shredder (not shown), and the sheet S may be made into shredded pieces of injection molding material.

[0134] Each unit included in the manufacturing apparatus 100 is electrically connected to a control unit 28. The operation of each unit is controlled by the control unit 28.

[0135] Each component of the manufacturing apparatus used to manufacture the injection molding material may be replaced with any component that can exert a similar function. In addition, any component may be added.

[0136] Furthermore, the method for producing a material for injection molding may include the above-mentioned mixing step, and may be performed using any apparatus, not limited to the case where the production apparatus 100 is used.

[0137] 3. Examples and Comparative Examples The present invention will be further described below with reference to examples and comparative examples, but the present invention is not limited to the following examples in any way.

[0138] 3.1. Example 1 A 0.5% aqueous solution of PVA (Denka Poval B-05, Denka Company, Ltd.) was sprayed onto softwood pulp (NBKP: BRATSK International Pulp Trading Co., Ltd.) at 0.07 wt% relative to the pulp, dried, and coarsely crushed using a shredder, then introduced into a modified Paper Labo A-8000 machine manufactured by Seiko Epson Corporation for defibration. The modified Paper Labo A-8000 machine was configured as shown in Figure 1, and was configured so that defibrated material M3 could be taken out from between the defibration section 13 and the sorting section 14.

[0139] 3.2. Comparative Example 1 Defibration was carried out in the same manner as in Example 1, except that softwood pulp (NBKP:BRATSK) was used without being sprayed with the aqueous solution of PVA.

[0140] 3.3. Measurement of average fiber length For the defibrated materials obtained in Example 1 and Comparative Example 1, the average length and average thickness of the cellulose were measured using a Fiber Tester: 912plus manufactured by L&W.

[0141] 3.4.Measurement results The average length and average thickness of the defibrated cellulose were as follows. Example 1: Average length 1.5 mm, average thickness 27.1 μm Comparative Example 1: Average length 1.3 mm, average thickness 26.3 μm

[0142] 3.5. Summary It was found that the average fiber length of the cellulose in the defibrated material can be maintained long by adding a water-soluble polymer to the cellulose raw material. As a result, it is expected that the mechanical strength of the molded product obtained by injection molding the injection molding material manufactured using the defibrated material of Example 1 will be better than that of Comparative Example 1.

[0143] The present invention includes configurations that are substantially the same as the configurations described in the embodiments, for example, configurations with the same functions, methods, and results, or configurations with the same purpose and effects. The present invention also includes configurations in which non-essential parts of the configurations described in the embodiments are replaced. The present invention also includes configurations that achieve the same effects as the configurations described in the embodiments, or configurations that can achieve the same purpose. The present invention also includes configurations in which publicly known technology is added to the configurations described in the embodiments.

[0144] The following can be derived from the above-described embodiment and modified examples.

[0145] The method for producing the injection molding material comprises the steps of: An application step of applying a water-soluble polymer to a cellulose raw material; a defibration step of defibrating the cellulose raw material to which the water-soluble polymer has been applied to produce a defibrated material; a mixing step of mixing the defibrated material and starch in air; Includes.

[0146] According to this manufacturing method, the cellulose raw material is defibrated together with the water-soluble polymer, so the fiber length of the cellulose in the defibrated material is unlikely to become short. In addition, because the defibrated material and starch are mixed in air, an injection molding material in which the starch is uniformly dispersed in the cellulose aggregate can be obtained. Furthermore, the injection molding material obtained in this way can be easily injection molded by adding a small amount of water, and a molded product with good strength can be formed.

[0147] In the above manufacturing method, a depositing step of depositing the mixture mixed in the mixing step to form a web; a molding step of pressurizing and heating the web to form a molded product; It may further include.

[0148] According to this manufacturing method, it is possible to manufacture an injection molding material which is easier to handle and more suitable for injection molding than a fluff-like material.

[0149] In the above manufacturing method, The water-soluble polymer may be selected from polyvinyl alcohol, polyacrylic acid, ethylene-acrylic acid copolymers, polyethylene glycol, polypropylene glycol, polysaccharides, modified celluloses, glue, and casein.

[0150] According to this manufacturing method, the fiber length of the cellulose can be maintained longer during defibration, making it possible to produce an injection molding material that is more suitable for injection molding and can give injection molded articles with better strength.

[0151] In the above manufacturing method, The starch may be selected from starches of vegetable origin.

[0152] According to this manufacturing method, a molded product can be formed in which the cellulose particles are better bonded together, and an injection molding material that is also environmentally friendly can be produced.

[0153] In the above manufacturing method, The amount of the water-soluble polymer applied in the application step may be 0.01% by mass or more based on the cellulose raw material.

[0154] According to this manufacturing method, the fiber length of the cellulose can be maintained longer during defibration, which makes it possible to obtain an injection molded product having better strength and is more suitable for injection molding. A molding material can be produced.

[0155] In the above manufacturing method, The method may include a plasticizer applying step of applying a plasticizer to the defibrated material.

[0156] According to this manufacturing method, since starch is more easily fluidized during injection molding, it is possible to manufacture a material for injection molding that can be easily injection molded.

[0157] Injection molding materials include: Fiberized cellulose; A water-soluble polymer; Starch and Including, Density: 0.001g / cm 3 More than 1.3g / cm 3 The following is the result.

[0158] This injection molding material is easier to handle than a dust-like material, and by adding a small amount of water, it is easy to injection mold and can form molded products with good strength. [Explanation of symbols]

[0159] 100... manufacturing apparatus, 10A... sheet processing apparatus, 10B... fibrous body depositing apparatus, 11... sheet supplying apparatus, 12... coarse crushing section, 13... defibrating section, 14... sorting section, 15... first web forming section, 16... fine division section, 17... mixing section, 18... dispersion section, 19... second web forming section, 20... molding section, 21... cutting section, 22... stock section, 27... recovery section, 28... control section, 121... coarse crushing blade, 122... chute, 141... drum section, 142... housing section, 151... mesh belt, 152... tension roller, 153... suction section, 161... propeller, 162... housing section, 170... housing section, 171... additive supply section, 172... pipe, 173... blower, 174... screw feeder, 181... drum, 182... housing, 183... drive source , 191... mesh belt, 192... tension roller, 193... suction section, 201... pressure section, 202... heating section, 203... calendar roller, 204... heating roller, 211... first cutter, 212... second cutter, 231... humidification section, 232... humidification section, 233... humidification section, 234... humidification section, 235... humidification section, 236... humidification section, 241... pipe, 242... pipe, 2 43...pipe, 244...pipe, 245...pipe, 246...pipe, 261...blower, 262...blower, 263...blower, 281...CPU, 282...memory unit, M1...cellulose raw material, M2...coarsely crushed pieces, M3...defibrated material, M4-1...first sorted material, M4-2...second sorted material, M5...first web, M6...fine body, M7...mixture, M8...second web, S...sheet, P1...starch

Claims

1. An application step of applying a water-soluble polymer to a cellulose raw material; a defibration step of defibrating the cellulose raw material to which the water-soluble polymer has been applied to produce a defibrated material; a mixing step of mixing the defibrated material and starch in air; A method for producing a material for injection molding, comprising:

2. In claim 1, a depositing step of depositing the mixture mixed in the mixing step to form a web; a molding step of pressurizing and heating the web to form a molded product; The method for producing the injection molding material further comprises:

3. In claim 1 or 2, The method for producing a material for injection molding, wherein the water-soluble polymer is selected from the group consisting of polyvinyl alcohol, polyacrylic acid, ethylene-acrylic acid copolymer, polyethylene glycol, polypropylene glycol, polysaccharides, modified celluloses, glue, and casein.

4. In any one of claims 1 to 3, The method for producing an injection molding material, wherein the starch is selected from starches of plant origin.

5. In any one of claims 1 to 4, A method for producing a material for injection molding, wherein the amount of the water-soluble polymer applied in the application step is 0.01 mass% or more with respect to the cellulose raw material.

6. In any one of claims 1 to 5, A method for producing an injection molding material, comprising: a plasticizer applying step of applying a plasticizer to the defibrated material.

Citation Information

Patent Citations

  • Method for adjusting molding material composed mainly of paper fiber

    JP2001079815A

  • Particle for cushioning material and method for production thereof, and cushioning material and method for production thereof

    JP2001098078A

  • Pellet for foam, and process of producing the same

    JP2010229322A

  • Molding material for manufacturing fibrous molded article and molded article using the same

    JP2018016745A

  • Manufacturing method of fibrillated cellulose fiber, and manufacturing method of resin composition

    JP2019001938A