Epoxy resin, curable composition, cured product, prepreg, printed wiring board, build-up film, semiconductor encapsulant, and semiconductor device

A novel epoxy resin formulation with specific structural compounds addresses the flexibility and dielectric loss issues in semiconductor materials, offering improved performance for high-speed, high-frequency applications.

JP7581784B2Active Publication Date: 2024-11-13DIC CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020190799
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-17
Publication Date
2024-11-13
Estimated Expiration
2040-11-17

AI Technical Summary

Technical Problem

Existing epoxy resins used in semiconductor applications lack sufficient flexibility and have high dielectric loss tangents, which are inadequate for high-speed, high-frequency signals, necessitating a balance of flexibility and low dielectric properties.

Method used

An epoxy resin composed of a bifunctional epoxy compound and a dihydroxy compound, characterized by specific structural parts, is developed to achieve excellent flexibility and extremely low dielectric loss tangent, using compounds represented by general formulas (1) and (1-1), with controlled molecular weights and epoxy group equivalents.

Benefits of technology

The resulting epoxy resin provides a cured product with enhanced flexibility and significantly reduced dielectric loss tangent, suitable for advanced semiconductor applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581784000015
    Figure 0007581784000015
  • Figure 0007581784000016
    Figure 0007581784000016
  • Figure 0007581784000017
    Figure 0007581784000017
Patent Text Reader

Abstract

To provide: an epoxy resin capable of forming a cured product with excellent flexibility and an extremely low dielectric loss tangent; a curable resin composition containing the same and a cured product thereof; and a prepreg, a printed wiring board, a build-up film, a semiconductor encapsulant, and a semiconductor device.SOLUTION: Reaction ingredients of the epoxy resin are a bifunctional epoxy compound (A) and a dihydroxy compound (B), where the bifunctional epoxy compound (A) and / or the dihydroxy compound (B) is a compound (X) represented by the structural formula (1) in the figure.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to an epoxy resin characterized by excellent flexibility in a cured product and an extremely low dielectric loss tangent, a curable resin composition containing the same, and a cured product thereof, a prepreg, a printed wiring board, a build-up film, a semiconductor encapsulant, and a semiconductor device. [Background technology]

[0002] In the technical field of insulating materials used in semiconductors, multilayer printed circuit boards, etc., the miniaturization and weight reduction of various electronic devices and the increasing speed and frequency of signals have led to a demand for the development of new resin materials that meet these market trends. The various properties required of resin materials include, for example, heat resistance, flexibility, low dielectric constant, low dielectric loss tangent, etc. in the cured product, and efforts are underway to develop resin materials that combine these properties in a balanced manner.

[0003] Techniques using relatively high molecular weight epoxy resins are known as techniques for improving the flexibility and film-forming properties of cured products (see Patent Documents 1 to 3 below). The high molecular weight epoxy resins described in these documents are effective in improving the flexibility, film-forming properties, impact resistance, and substrate adhesion of resin materials, but have the drawback of insufficient dielectric properties, as evaluated by dielectric constant and dielectric loss tangent. In particular, a low dielectric loss tangent has become an important performance factor in recent years in order to reduce energy losses, such as heat generation, associated with faster and higher signal speeds and frequencies, and there has been a demand for the development of resin materials that can combine flexibility with a low dielectric loss tangent. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Laid-Open No. 2003-342350 [Patent Document 2] Japanese Patent Application Laid-Open No. 2017-214529 [Patent Document 3] Japanese Patent Application Publication No. 2019-172996 Summary of the Invention [Problem to be solved by the invention]

[0005] Therefore, an object of the present invention is to provide an epoxy resin characterized by excellent flexibility in a cured product and an extremely low dielectric loss tangent, a curable resin composition containing the same, a cured product thereof, a prepreg, a printed wiring board, a build-up film, a semiconductor encapsulant, and a semiconductor device. [Means for solving the problem]

[0006] As a result of intensive research to solve the above problems, the present inventors have found that by using an epoxy resin having a specific structural moiety, a cured product having excellent flexibility and an extremely low dielectric loss tangent can be obtained, and have thus completed the present invention.

[0007] That is, the present invention relates to an epoxy resin produced from a bifunctional epoxy compound (A) and a dihydroxy compound (B) as reaction raw materials, wherein either or both of the bifunctional epoxy compound (A) and the dihydroxy compound (B) are compounds (X) represented by the following general formula (1):

[0008] [ka] [In the above general formula (1), R 1 , R 2 , R 3 each independently represents an alkyl group, alkyloxy group, or alkylthio group having 1 to 10 carbon atoms, an aryl group, aryloxy group, or arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, or a halogen atom. l is an integer value of 0 to 4, and when l is 2 or 4, R 1 may be the same or different within the same ring. m is an integer value of 0 to 3. When m is 2 or 3, R 2 may be the same or different within the same ring. n is an integer value of 0 to 4. When n is 2 to 4, R 3may all be the same or different. k is the average number of repeating units and is a number from 0.2 to 20. X is a hydrogen atom or a glycidyl group.

[0009] The present invention further relates to an epoxy resin which is produced using a dihydroxy compound (X-1) represented by the following general formula (1-1) and epihalohydrin as reaction raw materials, and which has an epoxy group equivalent in the range of 10,000 to 50,000 g / equivalent:

[0010] [ka] [In the above general formula (1-1), R 1 , R 2 , R 3 each independently represents an alkyl group, alkyloxy group, or alkylthio group having 1 to 10 carbon atoms, an aryl group, aryloxy group, or arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, or a halogen atom. l is an integer value of 0 to 4, and when l is 2 or 4, R 1 may be the same or different within the same ring. m is an integer value of 0 to 3. When m is 2 or 3, R 2 may be the same or different within the same ring. n is an integer value of 0 to 4. When n is 2 to 4, R 3 may all be the same or different. k is the average number of repeating units and is a value of 0.2 to 20.]

[0011] The present invention further relates to a curable resin composition containing the epoxy resin.

[0012] The present invention further relates to a cured product of the curable resin composition.

[0013] The present invention further relates to a prepreg using the curable resin composition.

[0014] The present invention further relates to a printed wiring board using the curable resin composition.

[0015] The present invention further relates to a build-up film using the curable resin composition.

[0016] The present invention further relates to a semiconductor encapsulant using the curable resin composition.

[0017] The present invention further relates to a semiconductor device using the semiconductor encapsulant. [Effects of the Invention]

[0018] According to the present invention, it is possible to provide an epoxy resin characterized by excellent flexibility in a cured product and an extremely low dielectric loss tangent, a curable resin composition containing the same, a cured product thereof, a prepreg, a printed wiring board, a build-up film, a semiconductor encapsulant, and a semiconductor device. [Brief explanation of the drawings]

[0019] [Figure 1] FIG. 1 is a GPC chart of the intermediate (1) obtained in Synthesis Example 1. [Figure 2] FIG. 2 is a 13C-NMR chart of the intermediate (1) obtained in Synthesis Example 1. [Figure 3] FIG. 3 is an FD-MS chart of the intermediate (1) obtained in Synthesis Example 1. [Figure 4] FIG. 4 is a GPC chart of the epoxy resin (A1) obtained in Synthesis Example 1. [Figure 5] FIG. 5 is a 13C-NMR chart of the epoxy resin (A1) obtained in Synthesis Example 1. [Figure 6] FIG. 6 is an FD-MS chart of the epoxy resin (A1) obtained in Synthesis Example 1. [Figure 7] FIG. 7 is a GPC chart of the epoxy resin (1) obtained in Example 1. [Figure 8] FIG. 8 is a GPC chart of the epoxy resin (2) obtained in Example 2. [Figure 9] FIG. 9 is a GPC chart of the epoxy resin (3) obtained in Example 3. [Figure 10] FIG. 10 is a GPC chart of the epoxy resin (4) obtained in Example 4. [Figure 11] FIG. 11 is a GPC chart of the epoxy resin (5) obtained in Example 5. [Figure 12] FIG. 12 is a GPC chart of the epoxy resin (6) obtained in Example 6. DETAILED DESCRIPTION OF THE INVENTION

[0020] The present invention will be described in detail below. The epoxy resin of the present invention is an epoxy resin produced from a bifunctional epoxy compound (A) and a dihydroxy compound (B) as reaction raw materials, characterized in that either or both of the bifunctional epoxy compound (A) and the dihydroxy compound (B) are compounds (X) represented by the following general formula (1). Such epoxy resins will be described below as epoxy resin (I).

[0021] [ka] [In the above general formula (1), R 1 , R 2 , R 3 each independently represents an alkyl group, alkyloxy group, or alkylthio group having 1 to 10 carbon atoms, an aryl group, aryloxy group, or arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, or a halogen atom. l is an integer value of 0 to 4, and when l is 2 or 4, R 1 may be the same or different within the same ring. m is an integer value of 0 to 3. When m is 2 or 3, R 2 may be the same or different within the same ring. n is an integer value of 0 to 4. When n is 2 to 4, R 3 may be the same or different. k is the average number of repeating units and is a value of 0.2 to 20. X is a hydrogen atom or a glycidyl group.

[0022] In the general formula (1), R 1, R 2 , R 3 each independently represents an alkyl group, alkyloxy group, or alkylthio group having 1 to 10 carbon atoms, an aryl group, aryloxy group, or arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, or a halogen atom. The alkyl group having 1 to 10 carbon atoms may be linear or branched. More specific examples include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, a t-butyl group, a hexyl group, a cyclohexyl group, a heptyl group, an octyl group, a nonyl group, and a decyl group. Examples of the alkyloxy group include a methoxy group, an ethoxy group, a propyloxy group, and a butoxy group. Examples of the alkylthio group include a methylthio group, an ethylthio group, a propylthio group, and a butylthio group. Examples of the aryl group having 6 to 10 carbon atoms include a phenyl group, a tolyl group, a xylyl group, a naphthyl group, and an anthryl group. Examples of the aryloxy group include a phenoxy group, a tolyloxy group, a xylyloxy group, and a naphthyloxy group. Examples of the arylthio group include a phenylthio group, a tolylthio group, a xylylthio group, and a naphthylthio group. Examples of the cycloalkyl group having 3 to 10 carbon atoms include a cyclopropyl group, a cyclopentyl group, and a cyclohexyl group. Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom.

[0023] R 1 is more preferably an alkyl group having 1 to 4 carbon atoms, since this provides an excellent balance between flexibility and dielectric properties in the cured product. The value of l is preferably an integer value of 0 to 2, more preferably 2. When l is 2, two R 1 The substitution position of R 1 is preferably at the 2-position and the 6-position relative to the oxygen atom on the aromatic ring to which it is bonded.

[0024] R 2 and R 3 In terms of ease of synthesis of the epoxy resin (I), it is preferable that m and n are 0.

[0025] The above k is the average number of repeating units and is a value of 0.2 to 20. The value of k can be calculated from the weight-average molecular weight measured using gel permeation chromatography (GPC). In particular, the value of k is preferably in the range of 1 to 20, more preferably in the range of 1 to 10, and particularly preferably in the range of 2 to 7, since this results in an excellent balance between flexibility and dielectric properties in the cured product. Note that gel permeation chromatography (GPC) was measured under the measurement conditions described in the Examples.

[0026] The epoxy resin (I) has an excellent balance between flexibility and dielectric properties in the cured product, and therefore the epoxy group equivalent is preferably in the range of 10,000 to 50,000 g / equivalent, and more preferably in the range of 10,000 to 40,000 g / equivalent.

[0027] The epoxy resin (I) preferably has a weight-average molecular weight (Mw) in the range of 10,000 to 1,000,000, since this provides an excellent balance between flexibility and dielectric properties in the cured product. In this specification, the weight-average molecular weight (Mw) of the epoxy resin (I) is measured using gel permeation chromatography (GPC) under the measurement conditions described in the Examples.

[0028] The compound (X) represented by the general formula (1), which is a reaction raw material for the epoxy resin (I), may be produced by any method as long as it has the molecular structure represented by the general formula (1). For example, for a compound in which X in the general formula (1) is a hydrogen atom (hereinafter sometimes abbreviated as "dihydroxy compound (X-1)"), a method of reacting a compound (x1) represented by the following general formula (2), a compound (x2) represented by the following general formula (3), and, if desired, a compound (x3) represented by the following general formula (4) under acid catalyst conditions can be used. For a compound in which X in the general formula (1) is a glycidyl group (hereinafter sometimes abbreviated as "bifunctional epoxy compound (X-2)"), a method of reacting the dihydroxy compound (X-1) with epihalohydrin can be used.

[0029] [ka] [In the above general formulas (2) to (4), R 1 , R 2 , R 3 R each independently represents an alkyl group, alkyloxy group, or alkylthio group having 1 to 10 carbon atoms, an aryl group, aryloxy group, or arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, or a halogen atom. 4 represents a hydrogen atom or a hydroxy-protecting group such as a benzyl group, a methanesulfonyl group, a p-toluenesulfonyl group, an acetyl group, or a benzoyl group. Z represents a halogen atom. l is an integer value of 0 to 4, and when l is 2 to 4, R 1 may all be the same or different. m is an integer value of 0 to 3. When m is 2 or 3, R 2 may all be the same or different. n is an integer value of 0 to 4. When n is 2 to 4, R 3 may all be the same or different.

[0030] In the general formulas (2) to (4), R 1 , R 2 , R 3Specific examples and preferred values ​​are the same as those in the general formula (1). The preferred values ​​of l, m, and n are also the same as those in the general formula (1). In the general formulas (3) and (4), Y is a structural moiety represented by any one of the general formulas (y1), (y2), and (y3), and two Ys in the general formula may have the same structure or different structures. Compounds (x1), (x2), and (x3) each having the same structure may be used alone, or two or more types may be used in combination.

[0031] Specific examples of the compound (x1) represented by the general formula (2) include phenol; monoalkylphenols such as cresol, ethylphenol, propylphenol, and butylphenol; dialkylphenols such as xylenol; and phenols having an aryl group such as phenylphenol. Among these, dialkylphenols such as xylenol are preferred, and those in which the substitution positions of the two alkyl groups are the 2nd and 6th positions relative to the phenolic hydroxyl group are more preferred. Furthermore, the alkyl group preferably has 1 to 4 carbon atoms.

[0032] In the compound (x2) represented by the general formula (3), as shown in the formula, at least one ortho-position of one Y is a hydrogen atom. The substitution position of the other Y is not particularly limited, but it is preferable that the two Ys are at the meta- or para-position relative to each other in terms of excellent reactivity. Specific examples of the compound (x2) include m-bis(α-hydroxyisopropyl)benzene, p-bis(α-hydroxyisopropyl)benzene, m-diisopropenylbenzene, p-diisopropenylbenzene, m-bis(α-chloroisopropyl)benzene, p-bis(α-chloroisopropyl)benzene, 1-(α-hydroxyisopropyl)-3-isopropenylbenzene, 1-(α-hydroxyisopropyl)-4-isopropenylbenzene, and compounds having R in the general formula (3) on an aromatic ring thereof. 2 Examples of the compound include compounds having one or more substituents represented by the following formula:

[0033] The compound (x3) represented by the general formula (4) is not an essential reaction component but is an optional component, and is used in combination with the compound (x2) as a compound represented by the general formula (4) and different from the compound (x2). The compound (x3) is preferably used in an amount of 50% by mass or less, more preferably 10% by mass or less, based on the total mass of the compound (x2) and the compound (x3).

[0034] Regarding the reaction ratio of the dihydroxy compound (X-1) with the compounds (x1) to (x3), when the compound (x3) is not used, the compound (x2) is preferably used in a range of 0.1 to 10.0 moles per mole of the compound (x1). In particular, the epoxy group equivalent and weight-average molecular weight (Mw) are favorable, so it is more preferable to use the compound (x2) in a range of 0.2 to 8.0 moles per mole of the compound (x1). When the compound (x3) is used, the total amount of the compound (x2) and the compound (x3) is preferably used in a range of 0.1 to 10.0 moles, more preferably 0.2 to 8.0 moles, per mole of the compound (x1). When reaction raw materials other than the compounds (x1) to (x3) are used as needed, the total mass of the compounds (x1) to (x3) is preferably 90 mass % or more, and more preferably 95 mass % or more, based on the total mass of the reaction raw materials.

[0035] Examples of the acid catalyst include inorganic acids such as phosphoric acid, hydrochloric acid, and sulfuric acid; organic acids such as oxalic acid, benzenesulfonic acid, toluenesulfonic acid, methanesulfonic acid, and fluoromethanesulfonic acid; solid acids such as activated clay, acid clay, silica alumina, zeolite, and strongly acidic ion exchange resins; and heteropolyhydrochloric acid. Among these, oxalic acid, benzenesulfonic acid, toluenesulfonic acid, methanesulfonic acid, and fluoromethanesulfonic acid are preferred, as they are homogeneous catalysts that can be easily removed by neutralization with a base and washing with water after the reaction. The amount of the acid catalyst used is preferably in the range of 0.001 to 10 parts by mass per 100 parts by mass of the total reaction raw materials.

[0036] The reaction temperature in the production of the dihydroxy compound (X-1) is usually in the range of 50 to 300° C., preferably 80 to 200° C. The reaction time is usually in the range of 0.5 to 24 hours in total, preferably 0.5 to 12 hours in total.

[0037] The reaction for producing the dihydroxy compound (X-1) may be carried out in an organic solvent, if necessary. The solvent used is not particularly limited, and a wide variety of solvents can be used. Specific examples include ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, and acetophenone; aprotic solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, N-methyl-2-pyrrolidone, acetonitrile, and sulfolane; cyclic ethers such as dioxane and tetrahydrofuran; esters such as ethyl acetate and butyl acetate; and aromatic solvents such as benzene, toluene, and xylene. These solvents may be used alone or in combination. The amount of these organic solvents used is preferably in the range of 30% to 300% by mass based on the total mass of the reaction raw materials for the dihydroxy compound (X-1).

[0038] After the reaction is completed, the reaction solution is neutralized, and the remaining reaction raw materials and solvent are distilled off under reduced pressure to obtain the target dihydroxy compound (X-1).

[0039] The hydroxyl equivalent of the dihydroxy compound (X-1) or a composition containing the same is preferably in the range of 200 to 20,000, more preferably in the range of 200 to 5,000, and particularly preferably in the range of 200 to 800 g / equivalent. The weight average molecular weight (Mw) is preferably in the range of 500 to 50,000, more preferably in the range of 500 to 10,000, and particularly preferably in the range of 500 to 3,000. The weight average molecular weight (Mw) was measured using gel permeation chromatography (GPC) under the measurement conditions described in the Examples.

[0040] Regarding the bifunctional epoxy compound (X-2), the reaction of the dihydroxy compound (X-1) or a composition containing the same with epihalohydrin can be carried out, for example, by using an excess amount of epihalohydrin relative to the hydroxyl groups in the reaction raw materials, and reacting in the presence of a basic catalyst at a temperature of 20 to 120°C for 0.5 to 10 hours.

[0041] Examples of the epihalohydrin include epichlorohydrin, epibromohydrin, β-methylepichlorohydrin, etc. The amount of epihalohydrin added is usually 1.5 to 30 mol, and preferably 2 to 15 mol, per mol of the total number of hydroxyl groups in the reaction raw materials.

[0042] Examples of the basic catalyst include alkaline earth metal hydroxides, alkali metal carbonates, and alkali metal hydroxides. Among these, alkali metal hydroxides are preferred because of their excellent catalytic activity, and specifically, sodium hydroxide and potassium hydroxide are more preferred. These basic catalysts may be used in a solid state or in an aqueous solution state. The amount of the basic catalyst added is preferably in the range of 0.9 to 2.0 moles per mole of the total hydroxyl groups in the reaction raw materials.

[0043] The reaction for producing the bifunctional epoxy compound (X-2) may be carried out in an organic solvent. Examples of organic solvents include ketones such as acetone and methyl ethyl ketone; alcohols such as methanol, ethanol, 1-propyl alcohol, isopropyl alcohol, 1-butanol, secondary butanol, and tertiary butanol; cellosolves such as methyl cellosolve and ethyl cellosolve; ethers such as tetrahydrofuran, 1,4-dioxane, 1,3-dioxane, and diethoxyethane; and aprotic polar solvents such as acetonitrile, dimethyl sulfoxide, and dimethylformamide. These solvents may be used alone or in combination. The amount of these organic solvents used is preferably in the range of 5% to 300% by mass based on the total mass of the reaction raw materials for the bifunctional epoxy compound (X-2).

[0044] After the reaction with epihalohydrin is completed, excess epihalohydrin can be distilled off to obtain a crude product. If necessary, the obtained crude product may be dissolved again in an organic solvent, and a basic catalyst may be added to carry out the reaction again to reduce the hydrolyzable halogen. Salts produced in the reaction can be removed by filtration, washing with water, or the like. Furthermore, when an organic solvent is used, the organic solvent may be distilled off to extract only the resin solid content, or the solution may be used as is.

[0045] The epoxy group equivalent of the bifunctional epoxy compound (X-2) or a composition containing the same is preferably in the range of 150 to 20,000 g / equivalent, more preferably in the range of 150 to 5,000 g / equivalent, and particularly preferably in the range of 150 to 1,000 g / equivalent. The weight average molecular weight (Mw) is preferably in the range of 500 to 50,000, more preferably in the range of 500 to 10,000, and particularly preferably in the range of 500 to 3,000. The weight average molecular weight (Mw) was measured using gel permeation chromatography (GPC) under the measurement conditions described in the Examples.

[0046] As long as the epoxy resin (I) uses the compound (X) represented by the general formula (1) as at least one of the bifunctional epoxy compound (A) and the dihydroxy compound (B), other compounds may be used in combination. Specific examples of combinations include, for example, when some or all of the bifunctional epoxy compound (A) is the bifunctional epoxy compound (X-2), all of the dihydroxy compound (B) may be other compounds, or some or all of the dihydroxy compound (X-1). Conversely, when some or all of the dihydroxy compound (B) is the dihydroxy compound (X-1), all of the bifunctional epoxy compound (A) may be other compounds, or some or all of the bifunctional epoxy compound (X-2). In either case, one type of other compound may be used alone, or two or more types may be used in combination. In either case, the epoxy resin has excellent flexibility in the cured product and an extremely low dielectric tangent, and therefore the proportion of the compound (X) in the reaction raw materials for the epoxy resin (I) is preferably 40% by mass or more, more preferably 50% by mass or more, and even more preferably 60% by mass or more.

[0047] Among the other compounds, specific examples of the dihydroxy compound (B) include compounds represented by any of the following general formulas (5-1) to (5-17), ring-opening polymers of these compounds with lactone compounds, and polyoxyalkylene-modified products.

[0048] [ka]

[0049] [ka] [In general formulas (5-1) to (5-17), R 1 R is a structural moiety that is an aliphatic hydrocarbon group having 2 to 10 carbon atoms or has one or more alkoxy groups or halogen atoms on its carbon atoms.2 R are each independently an aliphatic hydrocarbon group having 1 to 6 carbon atoms, an alkoxy group, a halogen atom, an aryl group, or an aralkyl group. 3 are each independently an aliphatic hydrocarbon group having 1 to 10 carbon atoms, an alkoxy group, a halogen atom, an aryl group, or an aralkyl group. 3 may form an alicyclic structure. k is an integer of 1 to 4, l is 0 or an integer of 1 to 4, m is 0 or an integer of 1 to 6, p is 0 or an integer of 1 to 3, and q is 0 or an integer of 1 to 5. Ar 1 is an aryl group which may have a substituent, Ar 2 represents a monohydroxyaryl group which may have a substituent. In the above general formula (5-13) and the above general formula (5-14), x and y are bonded to adjacent carbon atoms to form a xanthene structure or a dinaphthofuran structure, respectively. In the above general formula (5-17), Z is any one of a hydrocarbon group, an oxygen atom, and a carbonyl group.

[0050] Among these, the compounds represented by any one of the general formulae (5-2), (5-3), (5-4), and (5-6) are preferred, and the compounds represented by any one of the general formulae (5-3), (5-4), and (5-6) are particularly preferred, since they result in epoxy resins characterized by excellent flexibility in the cured product and an extremely low dielectric loss tangent.

[0051] Among the other compounds, specific examples of the bifunctional epoxy compound (A) include compounds represented by any one of the general formulae (5-1) to (5-17), or diglycidyl ethers such as ring-opening polymers of these compounds with lactone compounds, and polyoxyalkylene-modified products. Among these, diglycidyl ethers of compounds represented by any one of the general formulae (5-2), (5-3), (5-4), and (5-6) are preferred, and diglycidyl ethers of compounds represented by any one of the general formulae (5-3), (5-4), and (5-6) are particularly preferred, since they result in epoxy resins characterized by excellent flexibility in the cured product and an extremely low dielectric tangent.

[0052] The reaction conditions for producing the epoxy resin (I) include, for example, a method in which the reaction raw materials are reacted in the presence of a catalyst at a temperature of 50 to 230°C, preferably 120 to 200°C, for about 1 to 12 hours.

[0053] The charging ratio of the reaction raw materials for the epoxy resin (I) may be any ratio so long as the epoxy groups are in excess relative to the hydroxyl groups in the raw materials, and from the standpoint of reaction efficiency, the molar ratio of the two, (epoxy groups) / (hydroxyl groups), is preferably in the range of 1.01 to 1.10.

[0054] Examples of the catalyst include alkali metal compounds, organic phosphorus compounds, tertiary amines, quaternary ammonium salts, cyclic amine compounds, imidazole compounds, etc. The amount of catalyst added is preferably in the range of 100 to 10,000 ppm relative to the total mass of the raw materials for the epoxy resin (I).

[0055] When producing the epoxy resin (I), an organic solvent may be used as needed. Examples of the organic solvent include ketone solvents such as acetone, methyl ethyl ketone, and cyclohexanone; acetate ester solvents such as ethyl acetate, butyl acetate, cellosolve acetate, propylene glycol monomethyl ether acetate, and carbitol acetate; carbitol solvents such as cellosolve and butyl carbitol; aromatic hydrocarbon solvents such as toluene and xylene; dimethylformamide, dimethylacetamide, and N-methylpyrrolidone. These solvents may be used alone or in combination. The amount of these organic solvents used is preferably in the range of 30% by mass to 300% by mass based on the total mass of the reaction raw materials for the epoxy resin.

[0056] The epoxy resin of the present invention may be produced by a method using the dihydroxy compound (X-1) and epihalohydrin as reaction raw materials. That is, the epoxy resin of the present invention may be an epoxy resin characterized by using the dihydroxy compound (X-1) represented by the following general formula (1-1) and epihalohydrin as reaction raw materials, and having an epoxy group equivalent in the range of 10,000 to 50,000 g / equivalent. Such an epoxy resin will be referred to as epoxy resin (II) hereinafter.

[0057] [ka] [In the above general formula (1-1), R 1 , R 2 , R 3 each independently represents an alkyl group, alkyloxy group, or alkylthio group having 1 to 10 carbon atoms, an aryl group, aryloxy group, or arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, or a halogen atom. l is an integer value of 0 to 4, and when l is 2 or 4, R 1 may be the same or different within the same ring. m is an integer value of 0 to 3. When m is 2 or 3, R 2 may be the same or different within the same ring. n is an integer value of 0 to 4. When n is 2 to 4, R 3 may all be the same or different. k is the average number of repeating units and is a value of 0.2 to 20.]

[0058] In the general formula (1-1), R 1 , R 2 , R 3 Specific examples and preferred values ​​are the same as those in the general formula (1). Preferred values ​​of k, l, m, and n are also the same as those in the general formula (1).

[0059] The epoxy resin (II) has an excellent balance between flexibility and dielectric properties in the cured product, and therefore the epoxy group equivalent is preferably in the range of 10,000 to 50,000 g / equivalent, and more preferably in the range of 10,000 to 40,000 g / equivalent.

[0060] The epoxy resin (II) preferably has a weight-average molecular weight (Mw) in the range of 10,000 to 1,000,000, since this provides an excellent balance between flexibility and dielectric properties in the cured product. In this specification, the weight-average molecular weight (Mw) of the epoxy resin is measured using gel permeation chromatography (GPC) under the measurement conditions described in the Examples.

[0061] The dihydroxy compound (X-1) used as a reaction raw material for the epoxy resin (II) is the same as the dihydroxy compound (X-1) used as a reaction raw material for the epoxy resin (I). The epoxy resin (II) may use other dihydroxy compounds in addition to the dihydroxy compound (X-1) as a reaction raw material. Examples of other dihydroxy compounds include compounds represented by any of the general formulae (5-1) to (5-17), ring-opening polymers of these compounds with lactone compounds, and polyoxyalkylene-modified compounds. When these other dihydroxy compounds are used in combination, the resulting epoxy resin exhibits excellent flexibility in the cured product and an extremely low dielectric loss tangent. Therefore, the proportion of the dihydroxy compound (X-1) in the dihydroxy raw materials for the epoxy resin (II) is preferably 40% by mass or more, more preferably 50% by mass or more, and even more preferably 60% by mass or more.

[0062] The epoxy resin (II) can be produced by reacting a dihydroxy compound starting material containing the dihydroxy compound (X-1) as an essential component with epihalohydrin. The reaction between the dihydroxy compound starting material and epihalohydrin can be carried out, for example, by using an excess amount of epihalohydrin relative to the hydroxyl groups in the reaction starting materials, in the presence of a basic catalyst, at a temperature of 20 to 120°C for 0.5 to 10 hours.

[0063] Examples of the epihalohydrin include epichlorohydrin, epibromohydrin, β-methylepichlorohydrin, etc. The amount of epihalohydrin added is usually 1.5 to 30 mol, and preferably 2 to 15 mol, per mol of the total number of hydroxyl groups in the reaction raw materials.

[0064] Examples of the basic catalyst include alkaline earth metal hydroxides, alkali metal carbonates, and alkali metal hydroxides. Among these, alkali metal hydroxides are preferred because of their excellent catalytic activity, and specifically, sodium hydroxide and potassium hydroxide are more preferred. These basic catalysts may be used in a solid state or in an aqueous solution state. The amount of the basic catalyst added is preferably in the range of 0.9 to 2.0 moles per mole of the total hydroxyl groups in the reaction raw materials.

[0065] The reaction for producing the epoxy resin (II) may be carried out in an organic solvent. Examples of the organic solvent include ketones such as acetone and methyl ethyl ketone; alcohols such as methanol, ethanol, 1-propyl alcohol, isopropyl alcohol, 1-butanol, secondary butanol, and tertiary butanol; cellosolves such as methyl cellosolve and ethyl cellosolve; ethers such as tetrahydrofuran, 1,4-dioxane, 1,3-dioxane, and diethoxyethane; and aprotic polar solvents such as acetonitrile, dimethyl sulfoxide, and dimethylformamide. These solvents may be used alone or in combination. The amount of these organic solvents used is preferably in the range of 5% to 300% by mass based on the total mass of the reaction raw materials for the epoxy resin (I).

[0066] After the reaction is complete, excess epihalohydrin can be distilled off to obtain a crude product of epoxy resin (II). If necessary, the resulting crude product may be dissolved again in an organic solvent, and a basic catalyst may be added to the reaction mixture to reduce the hydrolyzable halogen. Salts produced in the reaction can be removed by filtration, washing with water, or the like. When an organic solvent is used, the organic solvent may be distilled off to extract only the resin solids, or the resulting solution may be used as is.

[0067] The epoxy resin of the present invention may be blended with a curing agent or a curing accelerator to form a curable resin composition. The curing agent may be any compound capable of reacting with the epoxy resin of the present invention, and various compounds may be used without particular limitation. Examples of curing agents include amine compounds such as diaminodiphenylmethane, diethylenetriamine, triethylenetetramine, diaminodiphenylsulfone, isophoronediamine, imidazole, BF3-amine complex, and guanidine derivatives; amide compounds such as dicyandiamide and polyamide resins synthesized from a linoleic acid dimer and ethylenediamine; acid anhydrides such as phthalic anhydride, trimellitic anhydride, pyromellitic anhydride, maleic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylnadic anhydride, hexahydrophthalic anhydride, and methylhexahydrophthalic anhydride; phenol novolac resins, cresol, and the like. The resin composition may contain phenolic resins such as phenol novolac resins, naphthol novolac resins, bisphenol novolac resins, biphenyl novolac resins, dicyclopentadiene-phenol adduct resins, phenol aralkyl resins, naphthol aralkyl resins, triphenol methane resins, tetraphenol ethane resins, and aminotriazine-modified phenolic resins; active ester resins; cyanate ester resins; bismaleimide resins; benzoxazine resins; styrene-maleic anhydride resins; allyl group-containing resins such as diallyl bisphenol and triallyl isocyanurate; polyphosphate esters; and phosphate ester-carbonate copolymers. These may be used alone or in combination of two or more. Among these, active ester resins are preferred because of their excellent dielectric properties in the cured product.

[0068] Specifically, the active ester resin is prepared by reacting a phenolic hydroxyl group-containing compound with an aromatic carboxylic acid or its acid halide as reactant materials. In particular, from the viewpoint of reactivity and physical properties of the cured product, an active ester resin is preferably prepared by reacting a compound (e1) having one phenolic hydroxyl group, a compound (e2) having two or more phenolic hydroxyl groups, and an aromatic dicarboxylic acid or its acid halide (e3) as reactant materials.

[0069] Examples of the compound (e1) having one phenolic hydroxyl group include phenol, naphthol, anthracenol, and compounds having one or more substituents such as alkyl groups, alkoxy groups, halogen atoms, and aryl groups on the aromatic nucleus thereof.

[0070] Examples of the compound (e2) having two or more phenolic hydroxyl groups include polyhydroxybenzene, polyhydroxynaphthalene, polyhydroxyanthracene, and compounds having one or more substituents such as alkyl groups, alkoxy groups, halogen atoms, and aryl groups on the aromatic nucleus thereof, as well as novolac-type phenolic resins obtained by reacting various phenolic hydroxyl group-containing compounds with formaldehyde as reaction raw materials, and compounds represented by the following general formula (6).

[0071] [ka] [In the formula, p is 1 or 2, and q is an integer of 1 to 4. Each Ar is independently a structural moiety such as a benzene ring, a naphthalene ring, an anthracene ring, or an aromatic ring having one or more substituents such as a hydrocarbon group, an alkoxy group, or a halogen atom on the aromatic ring. R is an alkylene group having 2 to 6 carbon atoms, or a structural moiety represented by any of the following general formulae (R-1) to (R-5). When q is an integer of 2 to 4, the multiple Rs may have the same structure or different structures.]

[0072] [ka] (wherein h is 0 or 1. R 3 are each independently an aliphatic hydrocarbon group, an alkoxy group, a halogen atom, an aryl group, or an aralkyl group, and i is 0 or an integer of 1 to 4. 4 is a hydrogen atom or a methyl group. Y is an alkylene group having 1 to 4 carbon atoms, an oxygen atom, a sulfur atom, or a carbonyl group. j is an integer of 1 to 4.

[0073] Examples of the aromatic dicarboxylic acid or acid halide thereof (e3) include benzenedicarboxylic acids such as isophthalic acid and terephthalic acid, naphthalene-1,4-dicarboxylic acid, naphthalene-2,3-dicarboxylic acid, naphthalene-2,6-dicarboxylic acid, and naphthalene-2,7-dicarboxylic acid, acid halides thereof, and compounds in which the aliphatic hydrocarbon group, alkoxy group, halogen atom, or the like is substituted on the aromatic nucleus of these.

[0074] The curable resin composition of the present invention may contain other epoxy resins in addition to the above-mentioned epoxy resins. Examples of other epoxy resins include phenol novolac epoxy resins, cresol novolac epoxy resins, naphthol novolac epoxy resins, bisphenol novolac epoxy resins, biphenol novolac epoxy resins, bisphenol epoxy resins, biphenyl epoxy resins, triphenolmethane epoxy resins, tetraphenolethane epoxy resins, dicyclopentadiene-phenol addition reaction epoxy resins, phenol aralkyl epoxy resins, and naphthol aralkyl epoxy resins.

[0075] The blending ratio of the epoxy resin of the present invention, the curing agent, and the other epoxy resins is not particularly limited and can be adjusted appropriately depending on the desired performance of the cured product, etc. As an example of blending, a preferred ratio is such that the total amount of functional groups in the curing agent is 0.7 to 1.5 moles per mole of the total amount of epoxy groups in the curable resin composition.

[0076] The curable resin composition of the present invention may contain various additives such as a curing accelerator, a flame retardant, an inorganic filler, a silane coupling agent, a mold release agent, a pigment, an emulsifier, etc., as needed.

[0077] Examples of the curing accelerator include phosphorus compounds, tertiary amines, imidazole compounds, pyridine compounds, organic acid metal salts, Lewis acids, amine complex salts, etc. Among them, from the viewpoint of excellent curability, heat resistance, electrical properties, moisture resistance reliability, etc., preferred are triphenylphosphine as a phosphorus compound, 1,8-diazabicyclo-[5.4.0]-undecene (DBU) as a tertiary amine, 2-ethyl-4-methylimidazole as an imidazole compound, and 4-dimethylaminopyridine as a pyridine compound.

[0078] Examples of the flame retardant include inorganic phosphorus compounds such as red phosphorus, ammonium phosphates such as monoammonium phosphate, diammonium phosphate, triammonium phosphate, and ammonium polyphosphate, and phosphoric acid amides; phosphoric acid ester compounds, phosphonic acid compounds, phosphinic acid compounds, phosphine oxide compounds, phosphorane compounds, organic nitrogen-containing phosphorus compounds, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, and 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide. and organic phosphorus compounds such as cyclic organic phosphorus compounds such as 10-(2,7-dihydroxynaphthyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide and derivatives thereof obtained by reacting them with compounds such as epoxy resins and phenolic resins; nitrogen-based flame retardants such as triazine compounds, cyanuric acid compounds, isocyanuric acid compounds, and phenothiazine; silicone-based flame retardants such as silicone oil, silicone rubber, and silicone resin; and inorganic flame retardants such as metal hydroxides, metal oxides, metal carbonate compounds, metal powders, boron compounds, and low-melting-point glass. When these flame retardants are used, their content in the curable resin composition is preferably in the range of 0.1 to 20 mass %.

[0079] The inorganic filler is blended, for example, when the curable resin composition of the present invention is used as a semiconductor encapsulation material. Examples of the inorganic filler include fused silica, crystalline silica, alumina, silicon nitride, and aluminum hydroxide. Among these, fused silica is preferred because it allows for a larger amount of inorganic filler to be blended. While either crushed or spherical fused silica can be used, it is preferable to primarily use spherical silica in order to increase the blending amount of fused silica and suppress an increase in the melt viscosity of the curable composition. Furthermore, to increase the blending amount of spherical silica, it is preferable to appropriately adjust the particle size distribution of the spherical silica. The filler is preferably blended in at a rate of 0.5 to 95 parts by mass per 100 parts by mass of the curable resin composition.

[0080] In addition, when the curable resin composition of the present invention is used for applications such as a conductive paste, a conductive filler such as silver powder or copper powder can be used.

[0081] As described above in detail, the epoxy resin of the present invention is characterized by excellent flexibility in the cured product and an extremely low dielectric loss tangent. In addition, it satisfies the general requirements for resin materials, such as solubility in general organic solvents and curability with various curing agents, and can be widely used in a wide range of applications, including electronic materials such as printed wiring boards, semiconductor encapsulation materials, and resist materials, as well as paints, adhesives, and molded products.

[0082] When the curable resin composition of the present invention is used for printed wiring boards or build-up adhesive films, it is generally preferable to dilute it with an organic solvent. Examples of the organic solvent include methyl ethyl ketone, acetone, dimethylformamide, methyl isobutyl ketone, methoxypropanol, cyclohexanone, methyl cellosolve, ethyl diglycol acetate, and propylene glycol monomethyl ether acetate. The type and amount of the organic solvent can be adjusted appropriately depending on the environment in which the curable resin composition is used. For example, for printed wiring boards, polar solvents with a boiling point of 160°C or less, such as methyl ethyl ketone, acetone, dimethylformamide, and cyclohexanone, are preferred, and they are preferably used in a proportion such that the nonvolatile content is 25 to 80% by mass. For build-up adhesive film applications, it is preferable to use ketone solvents such as acetone, methyl ethyl ketone, cyclohexanone, etc.; acetate ester solvents such as ethyl acetate, butyl acetate, cellosolve acetate, propylene glycol monomethyl ether acetate, carbitol acetate, etc.; carbitol solvents such as cellosolve and butyl carbitol, aromatic hydrocarbon solvents such as toluene and xylene, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, etc., and it is preferable to use them in a proportion such that the non-volatile content is 25 to 60 mass%.

[0083] Furthermore, a method for producing a printed wiring board using the curable resin composition of the present invention includes, for example, impregnating a reinforcing substrate with the curable resin composition, curing the composition to obtain a prepreg, and then laminating the prepreg on a copper foil and heat-pressing the laminate. Examples of the reinforcing substrate include paper, glass cloth, glass nonwoven fabric, aramid paper, aramid cloth, glass mat, and glass roving cloth. The amount of the curable resin composition impregnated is not particularly limited, but it is generally preferable to adjust the resin content in the prepreg to 20 to 60 mass%.

[0084] When the curable resin composition of the present invention is used for semiconductor encapsulation materials, it is generally preferable to blend an inorganic filler. The semiconductor encapsulation material can be prepared by mixing the blend using, for example, an extruder, a kneader, a roll, or the like. A method for molding a semiconductor package using the obtained semiconductor encapsulation material includes, for example, molding the semiconductor encapsulation material using a casting or transfer molding machine, an injection molding machine, etc., and further heating it at a temperature of 50 to 200 °C for 2 to 10 hours. By such a method, a semiconductor device as a molded product can be obtained.

Examples

[0085] Next, the present invention will be specifically described with reference to Examples and Comparative Examples, but the present invention is not limited thereto.

[0086] <Measurement conditions for GPC> Measuring device: "HLC-8320 GPC" manufactured by Tosoh Corporation, Column: Guard column "HXL-L" manufactured by Tosoh Corporation + "TSK-GEL G4000HXL" manufactured by Tosoh Corporation + "TSK-GEL G3000HXL" manufactured by Tosoh Corporation + "TSK-GEL G2000HXL" manufactured by Tosoh Corporation + "TSK-GEL G2000HXL" manufactured by Tosoh Corporation Detector: RI (differential refractometer) Data processing: "GPC Workstation EcoSEC-WorkStation" manufactured by Tosoh Corporation Measurement conditions: Column temperature 40 °C Developing solvent: Tetrahydrofuran Flow rate: 1.0 ml / min Standard: In accordance with the measurement manual of the above "GPC-8320", the following monodisperse polystyrene with a known molecular weight was used. (Polystyrene used) "A-500" manufactured by Tosoh Corporation "A-1000" manufactured by Tosoh Corporation "A-2500" manufactured by Tosoh Corporation "A-5000" manufactured by Tosoh Corporation "F-1" manufactured by Tosoh Corporation "F-2" manufactured by Tosoh Corporation "F-4" manufactured by Tosoh Corporation "F-10" manufactured by Tosoh Corporation "F-20" manufactured by Tosoh Corporation "F-40" manufactured by Tosoh Corporation "F-80" manufactured by Tosoh Corporation "F-128" manufactured by Tosoh Corporation Sample: A 1.0 mass% tetrahydrofuran solution in terms of resin solids content, filtered through a microfilter (50 μl)

[0087] < 13 Measurement conditions of C-NMR Apparatus: JNM-ECA500 manufactured by JEOL Ltd. Measurement mode: Inverse-gated decoupling Solvent: Deuterated dimethyl sulfoxide Pulse angle: 30° pulse Sample concentration: 30 mass% Number of integrations: 4000 times Reference of chemical shift: Peak of dimethyl sulfoxide: 39.5 ppm

[0088] <Measurement of FD-MS FD-MS was measured using a double focusing mass spectrometer AX505H (FD505H) manufactured by JEOL Ltd.

[0089] Synthesis Example 1 Production of epoxy resin (A1) <Synthesis of intermediate (1)>[[]] A flask equipped with a stirrer, a Dean-Stark apparatus, a condenser, and a nitrogen inlet was charged with 377.4 parts by mass of 2,6-xylenol, 300.0 parts by mass of m-bis(α-hydroxyisopropyl)benzene, 677.4 parts by mass of toluene, and 3.77 parts by mass of p-toluenesulfonic acid monohydrate, and heated while nitrogen gas was blown in. The temperature was raised to 120°C, and the reaction was continued at that temperature for 15 hours, while the water generated during the reaction was removed using a Dean-Stark apparatus. The reaction mixture was cooled and then neutralized using a 49% aqueous sodium hydroxide solution. The volatiles were distilled off under reduced pressure to obtain intermediate (1). The hydroxyl equivalent of the obtained intermediate (1) was 329 g / equivalent, the weight-average molecular weight (Mw) was 994, and the softening point was 69°C. The GPC chart of intermediate (1) is shown in Figure 1. 13 The C-NMR chart is shown in Figure 2, and the FD-MS chart is shown in Figure 3.

[0090] <Epoxidation reaction of intermediate (1)> A flask equipped with a thermometer, a condenser, and a stirrer was charged with 250.0 parts by mass of the intermediate (1) obtained above, 281.2 parts by mass of epichlorohydrin, and 75.9 parts by mass of isopropyl alcohol, and dissolved while purging with nitrogen gas. The mixture was heated to 40°C, and 9.30 parts by mass of 49 wt% aqueous sodium hydroxide solution was added over 4 hours. Further, while raising the temperature from 40°C to 60°C, 62.0 parts by mass of 49 wt% sodium hydroxide solution was added over 4 hours to allow the reaction to proceed. After the reaction was completed, the mixture was heated to 150°C under reduced pressure, and unreacted epichlorohydrin was distilled off to obtain a crude product. 438.8 parts by mass of methyl isobutyl ketone and 1.46 parts by mass of benzyl tributylammonium chloride were added to the obtained crude product and dissolved. Furthermore, 50.9 parts by mass of 5 wt% aqueous sodium hydroxide solution was added, and the reaction was allowed to proceed at 80°C for 1 hour. Thereafter, the mixture was repeatedly washed with water until the pH of the washings became neutral, and the system was dehydrated by azeotropy. After microfiltration, the solvent was distilled off under reduced pressure to obtain epoxy resin (A1). The obtained epoxy resin (A1) had a softening point of 63°C, an epoxy group equivalent of 465 g / equivalent, and a weight-average molecular weight (Mw) of 1,138. The GPC chart of epoxy resin (A1) is shown in Figure 4. 13The C-NMR chart is shown in Figure 5, and the FD-MS chart is shown in Figure 6. The value of k in the general formula (1) calculated from the weight average molecular weight was 5.4.

[0091] Example 1: Preparation of epoxy resin (1) The epoxy resin (A1) obtained in Synthesis Example 1 and bisphenol A were charged into a flask equipped with a thermometer, condenser, and stirrer in such a ratio that the epoxy group equivalent to hydroxyl group equivalent ratio (epoxy group equivalent) / (hydroxyl group equivalent) was 1.03. Cyclohexanone was added to the mixture to achieve a nonvolatile content of 70% by mass, and the mixture was heated to 150°C for dissolution. 1-benzyl-2-methylimidazole (Curezol 1B2MZ, manufactured by Shikoku Chemicals Co., Ltd.) was added in an amount of 1,000 ppm relative to the total mass of the epoxy resin (A1) and bisphenol A, and the mixture was allowed to react for 8.5 hours. Additional cyclohexanone was added to obtain an epoxy resin (1) solution with a nonvolatile content of 29.6% by mass. The GPC chart of the resulting epoxy resin (1) is shown in Figure 7. The epoxy group equivalent of the epoxy resin (1) was 30,930 g / eq, and the weight-average molecular weight (Mw) was 482,319.

[0092] Example 2: Preparation of epoxy resin (2) The epoxy resin (A1) obtained in Synthesis Example 1 and bisphenolacetophenone were charged into a flask equipped with a thermometer, condenser, and stirrer at a ratio of 1.03 (epoxy group equivalent / hydroxyl group equivalent). Cyclohexanone was added to achieve a nonvolatile content of 70% by weight, and the mixture was heated to 150°C for dissolution. 1-benzyl-2-methylimidazole (Curezol 1B2MZ, manufactured by Shikoku Chemical Industries, Ltd.) was added in an amount of 1,000 ppm relative to the total weight of the epoxy resin (A1) and bisphenolacetophenone, and the mixture was allowed to react for 3 hours. Cyclohexanone was then added to adjust the nonvolatile content to 50% by weight, and the mixture was allowed to react for 7 hours. Additional cyclohexanone was added to obtain an epoxy resin (2) solution with a nonvolatile content of 31.1% by weight. The GPC chart of the resulting epoxy resin (2) is shown in Figure 8. The epoxy resin (2) had an epoxy group equivalent of 15,677 g / equivalent and a weight average molecular weight (Mw) of 481,765.

[0093] Example 3: Preparation of epoxy resin (3) The epoxy resin (A1) obtained in Synthesis Example 1 and biphenol were charged into a flask equipped with a thermometer, condenser, and stirrer at a ratio of 1.03 (epoxy group equivalent / hydroxyl group equivalent). Cyclohexanone was added to achieve a nonvolatile content of 70% by weight, and the mixture was heated to 150°C to dissolve. 1-benzyl-2-methylimidazole (Curezol 1B2MZ, manufactured by Shikoku Chemical Industries, Ltd.) was added in an amount of 1,000 ppm relative to the total weight of the epoxy resin (A1) and biphenol, and the mixture was allowed to react for 4 hours. Cyclohexanone was further added to adjust the nonvolatile content to 50% by weight, and the mixture was allowed to react for 6 hours. Additional cyclohexanone was added to obtain an epoxy resin (3) solution with a nonvolatile content of 30.4% by weight. The GPC chart of the resulting epoxy resin (3) is shown in Figure 9. The epoxy resin (3) had an epoxy group equivalent of 18,443 g / equivalent and a weight average molecular weight (Mw) of 25,880.

[0094] Example 4 Preparation of epoxy resin (4) The epoxy resin (A1) obtained in Synthesis Example 1 and a bisphenol compound ("S-BOC" manufactured by Honshu Chemical Industry Co., Ltd.) represented by the following structural formula were charged into a flask equipped with a thermometer, condenser, and stirrer, in a ratio of 1.03, where the ratio of epoxy group equivalent to hydroxyl group equivalent (epoxy group equivalent) / (hydroxyl group equivalent) was 1.03. Cyclohexanone was added to achieve a nonvolatile content of 70% by weight, and the mixture was heated to 150°C for dissolution. 1-benzyl-2-methylimidazole ("Curezol 1B2MZ" manufactured by Shikoku Chemical Industry Co., Ltd.) was added in an amount of 1,000 ppm based on the total weight of the epoxy resin (A1) and the bisphenol compound, and the mixture was allowed to react for 4 hours. Further cyclohexanone was added to adjust the nonvolatile content to 50% by weight, and the mixture was allowed to react for 6 hours. Additional cyclohexanone was added to obtain an epoxy resin (4) solution with a nonvolatile content of 31.2% by weight. The GPC chart of the obtained epoxy resin (4) is shown in Figure 10. The epoxy group equivalent of the epoxy resin (4) was 13,193 g / equivalent, and the weight average molecular weight (Mw) was 21,265.

[0095] [ka]

[0096] Example 5 Preparation of epoxy resin (5) The epoxy resin (A1) obtained in Synthesis Example 1 and a bisphenol compound represented by the following structural formula ("BisP-HTG" manufactured by Honshu Chemical Industry Co., Ltd.) were charged into a flask equipped with a thermometer, condenser, and stirrer, in a ratio of 1.03, where the ratio of epoxy group equivalent to hydroxyl group equivalent (epoxy group equivalent) / (hydroxyl group equivalent) was 1.03. Cyclohexanone was added to achieve a nonvolatile content of 70% by weight, and the mixture was heated to 150°C for dissolution. 1-benzyl-2-methylimidazole ("Curezol 1B2MZ" manufactured by Shikoku Chemical Industry Co., Ltd.) was added in an amount of 1,000 ppm based on the total weight of the epoxy resin (A1) and the bisphenol compound, and the mixture was allowed to react for 4 hours. Further cyclohexanone was added to adjust the nonvolatile content to 50% by weight, and the mixture was allowed to react for 6 hours. Additional cyclohexanone was added to obtain an epoxy resin (5) solution with a nonvolatile content of 31.7% by weight. The GPC chart of the obtained epoxy resin (5) is shown in Figure 11. The epoxy group equivalent of the epoxy resin (5) was 27,028 g / equivalent, and the weight average molecular weight (Mw) was 154,901.

[0097] [ka]

[0098] Example 6 Preparation of epoxy resin (6) The epoxy resin (A1) obtained in Synthesis Example 1 and 2,6-dihydroxynaphthalene represented by the following structural formula were charged into a flask equipped with a thermometer, condenser, and stirrer, in a ratio of 1.03 (epoxy group equivalent / hydroxyl group equivalent). Cyclohexanone was added to achieve a nonvolatile content of 70% by weight, and the mixture was heated to 150°C for dissolution. 1-benzyl-2-methylimidazole (Curezol 1B2MZ, manufactured by Shikoku Chemicals Co., Ltd.) was added in an amount of 1,000 ppm relative to the total weight of the epoxy resin (A1) and biphenol compound, and the reaction was allowed to proceed for 4 hours. Further cyclohexanone was added to adjust the nonvolatile content to 50% by weight, and the reaction was allowed to proceed for 7 hours. Additional cyclohexanone was added to obtain an epoxy resin (6) solution with a nonvolatile content of 31.4% by weight. The GPC chart of the resulting epoxy resin (6) is shown in Figure 12. The epoxy resin (6) had an epoxy group equivalent of 26,699 g / equivalent and a weight average molecular weight (Mw) of 44,349.

[0099] Comparative Production Example 1 Production of Epoxy Resin (1') A flask equipped with a stirrer was charged with 100 parts by weight of 3,3',5,5'-tetramethyl-4,4'-biphenol diglycidyl ether (Mitsubishi Chemical Corporation "YX4000"), 77.2 parts by weight of bisphenolacetophenone, 0.4 parts by weight of 50% aqueous tetramethylammonium chloride solution, and 55 parts by weight of cyclohexanone, and the mixture was reacted at 180°C for 5 hours under a nitrogen gas atmosphere. Additional cyclohexanone was added to obtain an epoxy resin (1') solution with a non-volatile content of 30.9% by weight. The epoxy group equivalent of the epoxy resin (1') was 17,698 g / equivalent.

[0100] Examples 7 to 12 and Comparative Example 1 <Production of Curable Resin Composition> 50 parts by mass, in terms of resin solids, of any of the epoxy resins (1) to (6) or (1') obtained in Examples 1 to 6 and Comparative Production Example, 23 parts by mass of bisphenol A type epoxy resin ("EPICLON850-S" manufactured by DIC Corporation), 27 parts by mass, in terms of resin solids, of activated ester resin ("EPICLON HPC-8000-65T" manufactured by DIC Corporation), and 0.25 parts by mass of 4-(dimethylamino)pyridine were blended and mixed, and the mixture was diluted with toluene to a non-volatile content of 30% by mass, to obtain a curable resin composition.

[0101] <Production of cured product> The curable resin composition obtained above was applied to a mirror-finished aluminum substrate using an applicator and cured at 80°C for 1 hour, 100°C for 30 minutes, 120°C for 30 minutes, and 180°C for 1 hour to obtain a cured coating film with a thickness of approximately 30 μm.

[0102] <Measurement of dielectric loss tangent> The cured coating film obtained above was peeled off from the aluminum substrate, heated and vacuum dried, and then stored for 24 hours in a room at 23°C and 50% humidity. The dielectric loss tangent of the epoxy resin film was then measured in accordance with JIS-C-6481 using an Agilent Technologies Impedance Material Analyzer "HP4291B." The measurement conditions were two points: 1 GHz and 10 GHz. The absolute value of the difference between the two measurements was evaluated as frequency dependency.

[0103] <Flexibility evaluation> The cured coating film obtained above was peeled off from the aluminum substrate, and a tensile test was performed at a speed of 10 mm / min using an AGS-X made by Shimadzu Corporation, to determine the elongation of the cured coating film. The evaluation criteria are as follows: 3% or more: A Less than 3%: B

[0104] [Table 1]

Claims

1. A curable resin composition comprising an epoxy resin which is prepared from a bifunctional epoxy compound (A) and a dihydroxy compound (B) as reaction raw materials, and in which either or both of the bifunctional epoxy compound (A) and the dihydroxy compound (B) are a compound (X) represented by the following general formula (1), an epoxy resin other than the bifunctional epoxy compound (A), and a curing agent. [Formula 1] [In the above general formula (1), R 1 , R 2 , R 3 each independently represents an alkyl group, an alkyloxy group, or an alkylthio group having 1 to 10 carbon atoms, an aryl group, an aryloxy group, or an arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, or a halogen atom. l is an integer value of 0 to 4, and when l is 2 to 4, R 1 may be the same or different in the same ring. m is an integer value of 0 to 3. When m is 2 to 3, R 2 may be the same or different in the same ring. n is an integer value of 0 to 4. When n is 2 to 4, R 3 may be the same or different; k is the average number of repeating units and is a value from 0.2 to 20; and X is a hydrogen atom or a glycidyl group.

2. The curable resin composition according to claim 1, wherein the epoxy group equivalent of the epoxy resin (not the other epoxy resin) is in the range of 10,000 to 50,000 g / equivalent.

3. A curable resin composition comprising a dihydroxy compound (X-1) represented by the following general formula (1-1) and epihalohydrin as reaction raw materials, an epoxy resin having an epoxy group equivalent in the range of 10,000 to 50,000 g / equivalent, another epoxy resin, and a curing agent. [Formula 1] [In the above general formula (1-1), R 1 , R 2 , R 3each independently represents an alkyl group, an alkyloxy group, or an alkylthio group having 1 to 10 carbon atoms, an aryl group, an aryloxy group, or an arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, or a halogen atom. l is an integer value of 0 to 4, and when l is 2 to 4, R 1 may be the same or different in the same ring. m is an integer value of 0 to 3. When m is 2 to 3, R 2 may be the same or different in the same ring. n is an integer value of 0 to 4. When n is 2 to 4, R 3 may be the same or different. k is the average number of repeating units and is a value from 0.2 to 20.

4. The curable resin composition according to claim 1 or 3, wherein the weight average molecular weight (Mw) of the epoxy resin (not the other epoxy resin) is in the range of 10,000 to 1,000,000.

5. A curable resin composition according to any one of claims 1 to 4, wherein the curing agent is an active ester resin.

6. A cured product of the curable resin composition according to any one of claims 1 to 5.

7. A prepreg using the curable resin composition according to any one of claims 1 to 5.

8. A printed wiring board using the curable resin composition according to any one of claims 1 to 5.

9. A build-up film using the curable resin composition according to any one of claims 1 to 5.

10. A semiconductor encapsulant using the curable resin composition according to any one of claims 1 to 5.

11. A semiconductor device using the semiconductor encapsulation material according to claim 10.

Citation Information

Patent Citations

  • Polyhydroxy compound, thermosetting compound derived therefrom and composition thereof

    JP1994172242A

  • Copper plated epoxy resin laminated plate

    JP1994246871A

  • Epoxy resin composition and semiconductor device

    JP2003160635A

  • High-molecular weight epoxy resin, resin composition for electrical laminate, and electrical laminate

    JP2003342350A

  • Epoxy resin, epoxy resin composition, and cured product

    JP2017214529A