Evaluation method for transparent aggregates for fiber reinforced plastics
A direct optical evaluation method for transparent aggregates in FRP addresses the challenge of detecting capillary voids, ensuring defect-free manufacturing by impregnating with a light-transparent resin and using optical microscopy.
Patent Information
- Application Number
- JP2020191510
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-18
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-11-18
AI Technical Summary
Existing methods for evaluating capillary voids in transparent aggregates for fiber-reinforced plastics (FRP) are indirect, time-consuming, and lack accuracy, especially for thin glass cloths with high air permeability, making it difficult to detect potential defects that can cause electrical short circuits.
A direct evaluation method involving impregnation of transparent aggregates with a light-transparent resin, followed by curing and observation using an optical microscope, either by transmission or reflection methods, under controlled conditions to identify voids.
Enables reliable and efficient detection of capillary voids before manufacturing, reducing the risk of electrical short circuits in FRP products.
Smart Images

Figure 0007581786000003 
Figure 0007581786000004 
Figure 0007581786000005
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for evaluating transparent aggregates for fiber-reinforced plastics. [Background technology]
[0002] FRP (Fiber Reinforced Plastics) is a composite material that uses highly elastic materials such as fiber as aggregate and places this aggregate in a base material (matrix) such as plastic to improve its strength. Taking advantage of its weather resistance, heat resistance, chemical resistance, and light weight, FRP is an inexpensive, lightweight, and durable composite material. Taking advantage of these properties, FRP is used in a wide range of fields. For example, because of its moldability and high strength, FRP is used as a structural material for housing equipment, ships, vehicles, aircraft, etc. Also, taking advantage of its insulating properties, FRP is used in the field of electronic parts such as electrical equipment and semiconductor chips.
[0003] The integration density of electronic components such as semiconductor chips is becoming very high, and the printed wiring boards on which they are mounted are also becoming narrower. As a result, the thickness of the copper-clad laminates used is also becoming very thin. In addition, the number of IVHs (interstitial via holes) and through holes for electrical connections above and below (thickness direction) is also increasing, and they are also becoming narrower. As a result, the spacing between conductors between lines and through holes is becoming narrower.
[0004] Since the printed wiring board is becoming narrower, it is necessary to pay close attention so that an electrical short circuit does not occur in unnecessary parts. For example, it is necessary to ensure that the aggregate and insulating material used do not contain metallic foreign matter that may cause an electrical short circuit. Woven fabric, which is an aggregate, and especially glass cloth, may contain metal fibers spun from gold contained as an impurity in the raw material quartz, and may also contain hollow fibers whose filaments are hollow (see, for example, Patent Document 1). When the glass cloth contains metal fibers, the metal fibers may cause a short circuit if they are present between conductors. Furthermore, when the glass cloth contains hollow fibers, if the hollow fibers are present between through holes, copper is precipitated in the hollow parts of the hollow fibers during copper plating, which may cause an electrical short circuit. As a method for evaluating the likelihood of these defects occurring, the presence or absence of metal fibers can be confirmed by light transmission observation, since light does not pass through metal fiber parts. As light passes through hollow fibers, their presence or absence cannot be confirmed by transmission observation, but a method is known in which the hollow parts are detected by immersing the glass cloth in a solvent with a refractive index similar to that of the glass cloth to make them stand out (see Patent Document 2).
[0005] Incidentally, since the surface of glass cloth does not have a strong chemical bond with thermosetting resins as it is, the glass cloth is generally surface-treated with a silane coupling agent or the like that is reactive with both glass and resins (see, for example, Patent Document 3 and Non-Patent Document 1). However, if the glass cloth is dried in a state where the coupling agent is excessively attached to the glass cloth during the surface treatment process, the parallel filaments will stick to each other, or if a strong force is applied to the filaments during the surface treatment process of the glass cloth, they will become densely packed. In that case, gaps 2 are formed by the adhesion of many filaments 1 as shown in Figure 1, and if the adhesion distance is long, the gaps 2 cannot be filled sufficiently even if resin flows into them from openings 3 as shown in Figure 2, so the unfilled gaps become capillary voids (note that Figures 1 and 2 show four identical filaments). Although there is no particular limitation on the capillary voids, for example, they are observed in the form of black lines as indicated by the arrows in Figure 3. When capillary voids are formed between filaments in this way, the same problems as those in the case of the glass cloth having hollow fibers described above occur.
[0006] Therefore, just as with the evaluation of the presence or absence of hollow fibers, it is necessary to evaluate the presence or absence of capillary voids. However, because capillary voids transmit light, they cannot be observed directly by light transmission observation, just as in the case of hollow fibers. In addition, in the method of immersing the glass cloth in a solvent having the same refractive index as the glass cloth described in Patent Document 2, the solvent has an extremely low viscosity, so the solvent easily enters the gaps through the openings of the gaps, making it difficult to accurately evaluate the presence or absence of capillary voids. One possible method would be to actually impregnate glass cloth with resin, let it harden, and then observe the presence or absence of gaps in cross sections (transverse sections). However, because the observation surface is one-dimensional, the results are ambiguous, and this method is time-consuming and labor-intensive. Under such circumstances, there is a method for evaluating the air permeability of a glass cloth (see, for example, Patent Document 4). [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Japanese Patent Application Publication No. 11-021147 [Patent Document 2] JP 2004-084109 A [Patent Document 3] Patent No. 2751241 [Patent Document 4] JP 2014-070098 A [Non-patent literature]
[0008] [Non-Patent Document 1] Hitachi Hyoron, "Elucidation of the interface phenomenon between glass and resin and improvement of its properties", Vol. 56, No. 7, pp. 615-619, July 1974 Summary of the Invention [Problem to be solved by the invention]
[0009] In the method described in Patent Document 4, it is necessary to prepare a calibration curve in advance for the glass cloth to be used, which is time-consuming, and furthermore, since it is an indirect evaluation and lacks accuracy, a more direct evaluation method for the presence or absence of capillary voids is required. In addition, glass cloth with a thickness of 50 μm or less, which has been widely used in recent years, has a high degree of air permeability, so there is also the problem that even if capillary voids are present, it is difficult to detect a significant difference. Therefore, an object of the present disclosure is to provide a direct and simple method for evaluating the presence or absence of capillary voids in transparent aggregates for fiber-reinforced plastics. [Means for solving the problem]
[0010] As a result of intensive research, the present inventors have found that the above object can be achieved by the following evaluation method. That is, one aspect of this embodiment is as follows.
[0011] [1] A method for evaluating transparent aggregates for fiber-reinforced plastics, comprising: (A1) a step of impregnating a transparent aggregate for fiber-reinforced plastics with a light-transmitting resin or a light-transmitting resin composition in a state of a viscosity of 5 to 100 Pa s; (A2) a step of curing the light-transmitting resin or the light-transmitting resin composition to prepare a test piece for evaluation; (A3) observing the presence or absence of voids in the evaluation test piece by a transmission method or a reflection method using an optical microscope; A method for evaluating a transparent aggregate for fiber-reinforced plastics. [2] A method for evaluating transparent aggregates for fiber-reinforced plastics, comprising: (B1) a step of impregnating a transparent aggregate for fiber-reinforced plastics with a light-transmitting resin or a light-transmitting resin composition under heating and pressure at a temperature of 70 to 150°C, a pressurizing pressure of 0.3 to 3 MPa, and a vacuum condition at a viscosity of 50 to 5,000 Pa s; (B2) a step of preparing a test piece for evaluation of the light-transmitting resin or the light-transmitting resin composition by cooling to 35° C. or less; (B3) observing the presence or absence of voids in the evaluation test piece by a transmission method or a reflection method using an optical microscope; A method for evaluating a transparent aggregate for fiber-reinforced plastics. [3] The method for evaluating a transparent aggregate for fiber-reinforced plastics described in [1] or [2] above, wherein the voids are caused by gaps formed by contact between filaments forming the transparent aggregate. [4] The method for evaluating a transparent aggregate for fiber-reinforced plastics according to any one of the above [1] to [3], wherein the size of the voids is 10 times or more the diameter of the glass filaments. [5] The method for evaluating a transparent aggregate for fiber-reinforced plastics according to any one of the above [1] to [4], wherein the size of the test piece for evaluation is 20 to 30 mm in length × 20 to 30 mm in width. [6] The method for evaluating a transparent aggregate for fiber-reinforced plastics according to any one of the above [1] to [5], wherein the transparent aggregate is glass cloth. Effect of the Invention
[0012] The present disclosure provides a direct and simple method for evaluating the presence or absence of capillary voids in a transparent aggregate for fiber reinforced plastics (hereinafter, sometimes referred to as a transparent aggregate for FRP or simply as a transparent aggregate). The evaluation method of the present disclosure makes it possible to reliably evaluate whether or not the FRP to be manufactured is prone to defects before the FRP is actually manufactured. [Brief description of the drawings]
[0013] [Figure 1] FIG. 2 is a schematic diagram showing a cross section of a yarn in which gaps are formed by the adhesion of multiple filaments. [Diagram 2] 1 is a schematic diagram showing a cross section of a yarn in which gaps are formed by bonding together a large number of filaments, at a portion where the gaps have opened. FIG. [Diagram 3] 3 is a photograph showing capillary voids observed with an optical microscope in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] In the numerical ranges described in this specification, the upper or lower limit of the numerical range may be replaced with the values shown in the examples. In addition, the lower and upper limits of a numerical range may be arbitrarily combined with the lower or upper limit of another numerical range. In the expression of a numerical range "AA to BB", the numerical values AA and BB at both ends are included in the numerical range as the lower and upper limits, respectively. In this specification, for example, the expression "10 or more" means 10 or a numerical value exceeding 10, and the same applies when the numerical values are different. In addition, for example, the expression "10 or less" means 10 or a numerical value less than 10, and the same applies when the numerical values are different. Any combination of the descriptions in this specification is also included in this embodiment.
[0015] In one embodiment of the present invention, [A] A method for evaluating transparent aggregates for fiber-reinforced plastics (transparent aggregates for FRP), comprising: (A1) a step of impregnating a transparent aggregate for FRP with a light-transmitting resin or a light-transmitting resin composition in a state of a viscosity of 5 to 100 Pa s; (A2) a step of curing the light-transmitting resin or the light-transmitting resin composition to prepare a test piece for evaluation; (A3) observing the presence or absence of voids in the evaluation test piece by a transmission method or a reflection method using an optical microscope; The present invention relates to a method for evaluating a transparent aggregate for FRP, which has the following features (hereinafter, this may be referred to as "embodiment A").
[0016] In addition, one of the present embodiments is [B] A method for evaluating transparent aggregates for fiber-reinforced plastics (transparent aggregates for FRP), comprising: (B1) a step of impregnating a transparent aggregate for FRP with a light-transmitting resin or a light-transmitting resin composition under heating and pressure at a temperature of 70 to 150°C, a pressurizing pressure of 0.3 to 3 MPa, and a vacuum condition at a viscosity of 50 to 5,000 Pa s; (B2) a step of preparing a test piece for evaluation of the light-transmitting resin or the light-transmitting resin composition by cooling to 35° C. or less; (B3) observing the presence or absence of voids in the evaluation test piece by a transmission method or a reflection method using an optical microscope; This is a method for evaluating a transparent aggregate for FRP, which has the above-mentioned features (hereinafter, this may be referred to as "embodiment B").
[0017] As described above, embodiment A is an evaluation method that uses a liquid light-transmitting resin or a liquid light-transmitting resin composition that has a relatively low viscosity at about room temperature. Embodiment B is an evaluation method that uses a light-transmitting resin or a light-transmitting resin composition that has poor fluidity around room temperature but becomes fluid under relatively high temperature conditions. Hereinafter, the embodiments A and B will be described in detail in order.
[0018] <Embodiment A> (Transparent aggregate for FRP) The transparent aggregate for FRP that is the subject of evaluation is an aggregate used in FRP that transmits light, and from the standpoint of ease of checking for the presence or absence of capillary voids, the light transmittance of the transparent aggregate is preferably 20% or more, more preferably 30% or more, even more preferably 50% or more, and particularly preferably 85% or more (all including 100%). Examples of transparent aggregates for FRP include transparent inorganic fiber substrates such as woven and nonwoven glass fabrics; and transparent organic fiber substrates such as woven and nonwoven aramid fabrics and woven and nonwoven cellulose fabrics. This embodiment is particularly suitable for evaluating glass cloth. Glass cloth is woven from glass yarns obtained by bundling a plurality of glass filaments with a bundling agent and twisting them, and although there is no particular limitation, a plain woven glass cloth can be evaluated. There is no particular limitation on the number of strands in one yarn of the glass cloth, but it may be 10 to 1,000, 30 to 400, or 50 to 300. There is no particular limitation on the glass filament diameter of the glass cloth, but it may be 2 to 25 μm, 3 to 15 μm, or 3 to 10 μm. The type of glass of the glass cloth is not particularly limited, and examples thereof include E glass, S glass, C glass, D glass, T glass, NE glass, A glass, H glass, quartz glass, etc. In this embodiment A, although there is no particular limitation, a glass cloth of E glass can be evaluated.
[0019] There are no particular limitations on the thickness of the transparent aggregate to be evaluated, but the thickness of transparent aggregate used in the production of FRP is usually 10 to 500 μm, and from the viewpoint of ease of handling and enabling high-density wiring, it tends to be considered that the thickness is preferably 10 to 400 μm, but may also be 20 to 300 μm, 30 to 150 μm, or 60 to 130 μm, and in this embodiment, transparent aggregate of such a thickness can be evaluated. The size of the transparent aggregate to be evaluated is sufficient if it is about 20-30 mm long x 20-30 mm wide. By evaluating a portion of the transparent aggregate in a certain lot, it is possible to grasp the tendency of the entire lot.
[0020] ((A1) process) The step (A1) is a step of impregnating a transparent aggregate for FRP with a light-transmitting resin or a light-transmitting resin composition having a viscosity of 5 to 100 Pa·s. From the viewpoint of facilitating confirmation of the presence or absence of capillary voids, the light transmittance of the light-transmitting resin and the light-transmitting resin composition used in step (A1) is preferably 20% or more, more preferably 30% or more, even more preferably 50% or more, and particularly preferably 85% or more (all of which include 100%). The light-transmitting resin and the light-transmitting resin composition used in step (A1) each have a low viscosity of 5 to 100 Pa·s when impregnated into the transparent aggregate for FRP, and the viscosity is preferably 5 to 50 Pa·s, more preferably 5 to 25 Pa·s, and even more preferably 8 to 20 Pa·s. The process (A1) can be carried out under normal pressure, although there are no particular limitations thereon, and it is preferable to carry out the process under normal pressure.
[0021] Examples of light-transmitting resins that can be used in step (A1) include thermosetting resins such as epoxy resins; photosetting resins such as acrylic resins, etc., provided that they have the above-mentioned viscosity. The light-transmitting resin is not particularly limited as long as it is light-transmitting and within the above-mentioned viscosity range, but from the viewpoint of making the wettability relationship between the transparent aggregate and the resin similar, it is preferable to use a resin of the same type as, similar to, or the same resin as the resin to be impregnated into the FRP to be actually manufactured. If the resin to be used is not within the above-mentioned viscosity range, embodiment B can be adopted. The epoxy resin is not particularly limited, and examples thereof include bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, phenol novolac type epoxy resin, cresol novolac type epoxy resin, α-naphthol / cresol novolac type epoxy resin, bisphenol A novolac type epoxy resin, bisphenol F novolac type epoxy resin, stilbene type epoxy resin, triazine skeleton-containing epoxy resin, fluorene skeleton-containing epoxy resin, triphenol methane type epoxy resin, biphenyl type epoxy resin, xylylene type epoxy resin, biphenyl aralkyl type epoxy resin, naphthalene type epoxy resin, dicyclopentadiene type epoxy resin, alicyclic epoxy resin, polyfunctional phenols, and diglycidyl ether compounds of polycyclic aromatics such as anthracene. These may be used alone or in combination of two or more. The acrylic resin is not particularly limited, and examples thereof include homopolymers or copolymers of acrylic acid esters, homopolymers or copolymers of methacrylic acid esters, polyacrylonitrile, polyacrylamide, and the like.
[0022] When a thermosetting resin is used as the light-transmitting resin, it is preferable to use a light-transmitting resin composition containing a curing agent together with the thermosetting resin.The curing agent can be a known one, and for example, when an epoxy resin is used as the thermosetting resin, the epoxy curing agent can be phenol resin, amine compound, acid anhydride, boron trifluoride monoethylamine, isocyanate, dicyandiamide, urea resin, etc. When a photocurable resin is used as the light-transmitting resin, it is preferable to use a light-transmitting resin composition containing a photopolymerization initiator together with the photocurable resin. As the photopolymerization initiator, a known one can be used, and examples thereof include benzoin-based photopolymerization initiators, acetophenone-based photopolymerization initiators, anthraquinone-based photopolymerization initiators, thioxanthone-based photopolymerization initiators, ketal-based photopolymerization initiators, benzophenone-based photopolymerization initiators, acridine-based photopolymerization initiators, and oxime ester-based photopolymerization initiators.
[0023] The light-transmitting resin composition may further contain other components (e.g., organic solvents, fluorescent agents, coupling agents, fillers, etc.) within a range that maintains light transmittance. However, the content of the filler in the light-transmitting resin composition is preferably 5% by volume or less, more preferably 3% by volume or less, and even more preferably 1% by volume or less (all including 0% by volume) based on the total solid content. If the content of the filler in the light-transmitting resin composition is within this range, high light transmittance can be maintained, and observation by an optical microscope tends to be easy. Examples of the filler include organic fillers such as core-shell rubber particles having a core of polybutadiene, NBR, silicone rubber, or the like and a shell of an acrylic acid derivative, crosslinked NBR particles obtained by copolymerizing acrylonitrile and butadiene, and acrylonitrile butadiene copolymers such as copolymers of acrylonitrile, butadiene, and carboxylic acids such as acrylic acid; and inorganic fillers such as silica, alumina, barium sulfate, talc, clay, mica powder, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum borate, barium titanate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, barium zirconate, and calcium zirconate. In step (A1), one of the preferred embodiments is to use a resin composition from which components that impair light transmittance have been removed, in the resin composition to be impregnated into the FRP to be actually produced.
[0024] In the step (A1), since a light-transmitting resin or a light-transmitting resin composition having a low viscosity of 5 to 100 Pa·s can be used during impregnation, the step can be carried out under normal pressure as described above. For example, the light-transmitting resin or light-transmitting resin composition is poured onto a flat plate or into a container at normal pressure and at a temperature of about 15 to 40°C, preferably by a method that does not introduce bubbles, and transparent aggregate is placed on the light-transmitting resin or light-transmitting resin composition, and the transparent aggregate is allowed to sink into the light-transmitting resin or light-transmitting resin composition under its own weight, thereby impregnating the transparent aggregate with the light-transmitting resin or light-transmitting resin composition.
[0025] ((A2) process) The step (A2) is a step of preparing a test piece for evaluation by curing the light-transmitting resin or the light-transmitting resin composition impregnated into the transparent aggregate in the step (A1). There is no particular restriction on the method for curing the light-transmitting resin or light-transmitting resin composition impregnated into the transparent aggregate in step (A1), but when a thermosetting resin is used, it can be cured by leaving it at room temperature, or by heating it to a temperature at which the organic solvent is easily volatilized, for example, 80°C or higher, to promote curing to a degree where the resin is not sticky. When a photocurable resin is used, it can be cured by irradiating it with active energy rays such as ultraviolet rays, electron beams, α rays, β rays, and γ rays. In either case, it is sufficient that the resin is cured to a degree where it is not sticky. The size of the test piece for evaluation is about 20 to 30 mm in length × 20 to 30 mm in width, which allows for sufficiently accurate evaluation.
[0026] ((A3) process) Step (A3) is a step of observing the presence or absence of voids in the evaluation test piece prepared in step (A2) using an optical microscope by a transmission method or a reflection method. The voids that can be observed in the step (A3) are due to gaps formed by contact between the filaments that form the transparent aggregate, and when voids are present, the voids have different refractive indices, and can be observed as shadows, for example, as shown by the arrows in Fig. 3. Therefore, the size of the voids is usually 10 times or more the length of the glass filament diameter, and may be 15 times or more, 50 times or more, or 100 times or more. There is no particular upper limit to the size of the voids, but they are often 100,000 times or less the glass filament diameter, and may be 10,000 times or less. Observation with an optical microscope can be performed using either a transmission method or a reflection method, but the voids tend to be easier to observe using a transmission method. As the light source, a commonly used light source can be used, including natural light (white light), a halogen lamp, a xenon lamp, a tungsten lamp, an LED, infrared light, and ultraviolet light. A light source that is easy to observe can be selected as appropriate. Observation with an optical microscope can utilize bright-field observation, phase contrast observation, polarized light observation, etc. Among these, bright-field observation is preferred from the viewpoint of ease of observation of voids.
[0027] <Embodiment B> The transparent aggregate for FRP to be evaluated in embodiment B is explained in the same manner as in embodiment A. Steps (B1) to (B3) in embodiment B will be described in detail below in order.
[0028] ((B1) process) Step (B1) is a step of impregnating a transparent aggregate for FRP with a light-transmitting resin or a light-transmitting resin composition under heating and pressure at a temperature of 70 to 150°C, a pressurizing pressure of 0.3 to 3 MPa, and a vacuum condition with a viscosity of 50 to 5,000 Pa·s. From the viewpoint of facilitating confirmation of the presence or absence of capillary voids, the light transmittance of the light-transmitting resin and the light-transmitting resin composition used in step (B1) is preferably 20% or more, more preferably 30% or more, even more preferably 50% or more, and particularly preferably 85% or more (all including 100%). The light-transmitting resin and light-transmitting resin composition used in step (B1) are solid or highly viscous at 25°C, but have the property of softening to an extent that allows impregnation into aggregate under the above-mentioned heating and pressure impregnation conditions. From the viewpoint of impregnation properties, the viscosity of the light-transmitting resin and light-transmitting resin composition when impregnating transparent aggregate for FRP under heating and pressure is preferably 50 to 5,000 Pa s, may be 80 to 3,000 Pa s, or may be 100 to 1,500 Pa s.
[0029] The heating and impregnation conditions in the step (B1) are 70 to 150°C, 0.3 to 3 MPa, and vacuum conditions. The heating temperature may be 80 to 130°C, 80 to 110°C, or 85 to 100°C. The pressurizing pressure may be 0.3 to 1.5 MPa, 0.4 to 1.3 MPa, or 0.5 to 1.0 MPa. The vacuum conditions are not particularly limited, but are preferably 10 5 ~10 -5 Pa (the so-called low, medium and high vacuum ranges) and 10 5 ~10 2 Pa (so-called low vacuum range). By setting such heating and impregnation conditions, the aggregate is sufficiently impregnated with the light-transmitting resin or the light-transmitting resin composition.
[0030] The light-transmitting resin usable in step (B1) may be, provided that it has the above-mentioned viscosity, a thermosetting resin such as an epoxy resin; an aliphatic saturated hydrocarbon such as paraffin, etc. Examples of the epoxy resin include the same ones as those exemplified in the explanation of step (A1) of embodiment A, and it is sufficient to select one that satisfies the above-mentioned viscosity condition. Examples of the paraffin include n-paraffin, isoparaffin, etc. The light-transmitting resin composition may further contain other components (e.g., a fluorescent agent, a coupling agent, a filler, etc.) within a range that maintains light transmittance. However, the content of the filler in the light-transmitting resin composition is preferably 5% by volume or less, more preferably 3% by volume or less, and even more preferably 1% by volume or less (all including 0% by volume) based on the total solid content. If the content of the filler in the light-transmitting resin composition is within this range, high light transmittance can be maintained, and observation by an optical microscope tends to be easy. Specific examples of the filler are explained in the same manner as in the step (A1) above. In addition, in step (B1), one of the preferred embodiments is to use a resin composition from which components that impair light transmittance have been removed in the resin composition to be impregnated into the FRP to be actually manufactured.
[0031] There is no particular limitation on the embodiment of step (B1). For example, the optically transparent resin or optically transparent resin composition is made to have a low viscosity (liquified) on a flat plate such as a glass plate, and then cooled to form a resin layer having a substantially flat surface. This is then superimposed on aggregate, and heated and pressurized to impregnate the aggregate. This has the advantage that the resin layer can be easily and uniformly impregnated into the aggregate.
[0032] ((B2) process) The step (B2) is a step of preparing a test piece for evaluation of the light-transmitting resin or light-transmitting resin composition by cooling to 35° C. or lower. In this step, if the light-transmitting resin or light-transmitting resin composition impregnated into the transparent aggregate under heating and pressure in the step (B1) is not yet cured, it is solidified by the cooling. There is no particular limitation on the cooling temperature as long as it is 35°C or lower, and it is sufficient that the light-transmitting resin or light-transmitting resin composition is solidified, but there is little need to cool to 0°C or lower. Therefore, it is sufficient to prepare a test piece for evaluation by generally cooling to preferably 0 to 35°C, more preferably 5 to 30°C, and even more preferably 10 to 30°C. In the step (B1), the light-transmitting resin or light-transmitting resin composition may be cured. Even in this case, the light-transmitting resin or the light-transmitting resin composition is cooled to 35° C. or less (preferably within the above-mentioned temperature range) in the step (B2) to obtain a test piece for evaluation. The size of the test piece for evaluation should be about 20 to 30 mm in length × 20 to 30 mm in width to ensure sufficiently accurate evaluation.
[0033] ((B3) process) Step (B3) is a step of observing the presence or absence of voids in the evaluation specimen by a transmission method or a reflection method using an optical microscope. The details are the same as those of step (A3) in embodiment A.
[0034] Capillary voids that can be observed by the evaluation method of this embodiment, if they exist between through-holes, can cause copper to precipitate at the capillary voids during copper plating, which can cause electrical shorts. According to the evaluation method of this embodiment, it is possible to reliably evaluate whether or not the FRP to be manufactured is prone to such defects before actually manufacturing the FRP. EXAMPLES
[0035] The present embodiment will now be described in more detail with reference to the following examples, but these examples are not intended to limit the present embodiment.
[0036] Prior to the following Examples and Comparative Examples, the following glass cloths for evaluation were prepared and manufactured. (Glass Cloth 1) IPC style #2116 (glass cloth manufactured by Nitto Boseki Co., Ltd.) was prepared. (Glass Cloth 2) A silane coupling agent "Shin-Etsu Silicone (registered trademark) KBM-053" (manufactured by Shin-Etsu Chemical Co., Ltd., product name) was added to pure water at a concentration of 1% by mass, and the mixture was stirred at room temperature for 60 minutes. After confirming that the solution was transparent, the solution was filtered through a 200 mesh filter to obtain a silane coupling treatment solution. Next, the glass cloth 1 was immersed in this silane coupling solution, and then the glass cloth was pulled out and dried with hot air at 120° C. to obtain a glass cloth designated as glass cloth 2. (Glass Cloth 3) In the production of the glass cloth 2, the operation of immersing the glass cloth in the silane coupling solution and then drying was repeated three times to obtain a glass cloth designated as glass cloth 3.
[0037] [Example 1] Embodiment A 10 parts by mass of triethylenetetramine was added to 100 parts by mass of a bis-A type epoxy resin (EPICLON (registered trademark) 840S: product name manufactured by DIC Corporation) and stirred. After stirring was completed, the mixture was degassed at a vacuum degree of 680 mmHg to obtain a mixed resin A (resin viscosity: 11 Pa s / 25°C). About 10 g of the mixed resin A was poured onto a glass plate having a thickness of 1 mm under atmospheric pressure conditions at 25°C, while being careful not to introduce bubbles. A glass cloth having a size of about 50 mm square was placed on the mixed resin A, and the glass cloth was left to stand so that the resin was impregnated by its own weight (step (A1)). This operation was carried out for each of the glass cloths 1 to 3. The epoxy resin was allowed to harden by leaving it as it was for 24 hours, and evaluation samples a1 to a3 were obtained (step (A2)). Using the obtained evaluation samples a1 to a3, light was applied from below the evaluation samples to an area of 25.4 mm square using an optical microscope and transmission observation was performed (step (A3)). Voids with a length of 15 times or more the filament diameter were recognized as capillary voids (see Figure 3) and counted. The results are shown in Table 1.
[0038] [Example 2] Embodiment B A bis-A type epoxy resin "jER (registered trademark) 1004" (product name, manufactured by Mitsubishi Chemical Corporation) (resin viscosity: solid / 25°C, 1,500 Pa·s / 95°C, 50 Pa·s / 120°C) was prepared. Approximately 10 g of the bis-A type epoxy resin was placed on a glass plate with a thickness of 1 mm, and the resin was made low-viscosity (liquefied) in a dryer at 120°C. It was then cooled, resulting in a state in which the resin (in a solidified state) was evenly applied onto the glass plate. Next, a glass cloth of about 50 mm square was placed on the resin on the glass plate, and a stain-preventing PET film "Lumirror (registered trademark) #75S10" (product name, manufactured by Toray Industries, Inc.) was placed on top of the glass cloth, and the glass cloth was evacuated with a flat pressure vacuum laminator (product name, manufactured by Meiki Seisakusho, Inc.), and pressurized and heated at 95°C for 30 seconds at a pressure of 0.5 MPa to impregnate the glass cloth with the resin (step (B1)). This operation was performed for each of the glass cloths 1 to 3. Thereafter, the mixture was cooled to 25° C. and solidified to obtain evaluation samples b1 to b3, respectively (step (B2)). Using the obtained evaluation samples b1 to b3, light was applied from below the evaluation sample to an area of 25.4 mm square using an optical microscope and transmission observation was performed (step (B3)). Voids with a length of 15 times or more the filament diameter were recognized as capillary voids and counted. The results are shown in Table 1.
[0039] [Comparative Example 1] Method of immersing in a solvent with a refractive index similar to that of glass cloth (method of Patent Document 2) Benzyl alcohol (viscosity 6 mPa·s / 25° C., refractive index: 1.5396 / 20° C.) was placed in a petri dish, and the glass cloths 1 to 3 were each separately immersed in the benzyl alcohol to obtain evaluation samples c1 to c3, respectively. Using the obtained evaluation samples c1 to c3, transmission observation was performed in the same manner as in Example 1. The results are shown in Table 1.
[0040] [Comparative Example 2] Evaluation after actually producing prepreg To 100 parts by mass of phenol novolac epoxy resin (EPICLON (registered trademark) N-660; manufactured by DIC Corporation) and 60 parts by mass of cresol novolac resin (PHENOLITE (registered trademark) KA-1165; manufactured by DIC Corporation), 15 parts by mass of cyclohexane and 130 parts by mass of methyl ethyl ketone were added and dissolved by stirring thoroughly. To this, 180 parts by mass of aluminum hydroxide (CL-303; manufactured by Sumitomo Chemical Co., Ltd.) as a filler, 1 part by mass of a coupling agent (Silquest A-187; manufactured by Momentive Performance Materials Co., Ltd.), and 2.5 parts by mass of socyanate mask imidazole (G8009L; manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) as a curing accelerator were added, and the mixture was dissolved and dispersed by stirring to prepare a thermosetting resin varnish X with a non-volatile content of 70% by mass. This thermosetting resin varnish X was adjusted to a resin content of 58% by mass and applied to each of the glass cloths 1 to 3, then dried and heated at 171°C to bring them to the B stage, producing prepregs d1 to d3 (volatile content of 1% or less). At this time, the viscosity was measured with a rheometer "AR-200ex" (manufactured by TA Instruments Japan, Inc., heating rate: 3°C / min, jig diameter 20 mm), and the prepregs were produced while adjusting the minimum melt viscosity to 800 to 1,200 Pa s. Five sheets each of the prepregs d1 to d3 prepared as described above were stacked, and copper foil “F2-WS-12” (12 μm electrolytic copper foil, manufactured by Furukawa Electric Co., Ltd.) was placed on the top and bottom. The stack was then sandwiched between SUS mirror plates and heat-molded for 90 minutes under conditions of a product pressure of 3.0 MPa and a product temperature of 185°C or higher to produce copper-coated laminates (evaluation samples d1 to d3) having copper foil on both sides. The cross sections of the evaluation samples d1 to d3 thus obtained within a 25.4 mm square range were observed under a scanning electron microscope (SEM: magnification 5,000 times) to count the voids in the filaments. The results are shown in Table 1.
[0041] [Table 1]
[0042] [Evaluation of electrolytic corrosion resistance of glass cloths 1 to 3] In order to evaluate the results in Table 1, the glass cloths 1 to 3 were evaluated for their respective levels of galvanic corrosion resistance. If the number of capillary voids observed in Table 1 shows a similar tendency to the evaluation results of galvanic corrosion resistance, it can be judged that the evaluation method is excellent for transparent aggregates for FRP. Specifically, using the evaluation samples d1 to d3 produced in Comparative Example 2, holes with a drill hole diameter of 0.3 mm and a drill pitch of 0.45 mm (wall spacing 0.15 mm) were drilled in two rows of 250 holes each (i.e., a total of 500 holes), and 10 of these were arranged to produce evaluation panels d1 to d3. After that, the evaluation panels d1 to 3 were subjected to desmear treatment, electroless copper plating treatment, and electric copper plating (15 μm), and then a circuit for a through-hole insulation reliability test was formed. An electrolytic corrosion test was performed for 1,000 hours in a constant temperature and humidity chamber at 85°C and 85% RH with an applied voltage of 50 V. The same electrolytic corrosion test was performed 10 times for each panel d1 to d3, and the resistance in the chamber was 10 7 We defined a test result of Ω or more as a "pass" and counted the number of tests that passed. The results are shown in Table 2. [Table 2]
[0043] From the results in Table 2, it can be seen that Glass Cloth 1 has the best performance, followed by Glass Cloth 2, and then Glass Cloth 3. For Examples 1 and 2 in Table 1, in which this tendency is clearly shown, it can be said that the evaluation methods therefor are excellent. On the other hand, in Comparative Example 1 in Table 1, the evaluation results are unstable, and it is also clear that voids are not counted as compared to the Examples, making it clearly an inferior evaluation method to the Examples. Also, in Comparative Example 2, the inorganic filler contained in the prepreg prevents light from passing through, so the light transmission method cannot be used, and therefore cross-sections are observed with an SEM. However, the results of Comparative Example 2 in Table 1 show that this is a time-consuming method to evaluate, and it hardly counts any voids, making it an evaluation method inferior to the Examples. [Explanation of symbols]
[0044] 1 filament 2 gap 3 Opening
Claims
1. A method for evaluating a transparent aggregate for fiber reinforced plastics, comprising: (B1) A step of impregnating a transparent aggregate for fiber-reinforced plastics with a light-transmitting resin or a light-transmitting resin composition under heating and pressure at a temperature of 70 to 150° C., a pressurizing pressure of 0.3 to 3 MPa, and a vacuum condition at a viscosity of 50 to 5,000 Pa s; (B2) a step of preparing a test piece for evaluation of the light-transmitting resin or the light-transmitting resin composition by cooling to 35° C. or less; (B3) observing the presence or absence of voids in the evaluation test piece using an optical microscope by a transmission method or a reflection method; A method for evaluating a transparent aggregate for fiber-reinforced plastics.
2. 2. The method for evaluating a transparent aggregate for fiber-reinforced plastics according to claim 1, wherein the voids are caused by gaps formed by contact between filaments forming the transparent aggregate.
3. 3. The method for evaluating a transparent aggregate for fiber-reinforced plastics according to claim 1, wherein the size of the voids is 10 times or more the diameter of the glass filaments.
4. The method for evaluating a transparent aggregate for fiber-reinforced plastics according to any one of claims 1 to 3, wherein the size of the evaluation test piece is 20 to 30 mm in length x 20 to 30 mm in width.
5. The method for evaluating a transparent aggregate for fiber-reinforced plastics according to any one of claims 1 to 4, wherein the transparent aggregate is glass cloth.
Citation Information
Patent Citations
Electronic-grade glass cloth and method for testing holes of monofilaments of yarns
CN101864665A
Production of glass cloth for reinforcing resin
JP1993140873A
Composition for high strength glass fiber
JP1999021147A
Test method for detecting hollow fiber of glass cloth for laminated plate
JP2004084109A
Insulative resin sheet containing glass woven fabric, laminate plate, multilayer printed wiring board, and semiconductor device
JP2011216892A