Coated positive electrode active material, method for producing coated positive electrode active material, and all-solid-state battery

Coating the positive electrode active material with scandium lithium phosphate or lithium borate compounds in all-solid-state batteries suppresses the reaction with the solid electrolyte, maintaining low internal resistance and enhancing battery performance.

JP7581806B2Active Publication Date: 2024-11-13TOYOTA JIDOSHA KK
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2020199476
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-01
Publication Date
2024-11-13
Estimated Expiration
2040-12-01

AI Technical Summary

Technical Problem

The reaction between the positive electrode active material and the solid electrolyte in all-solid-state batteries generates a high resistance layer at the interface, increasing the internal resistance of the battery.

Method used

A positive electrode active material is coated with a scandium lithium phosphate compound or a lithium borate compound to suppress the reaction with the solid electrolyte, using a sputtering method to form the coating.

Benefits of technology

The coating effectively reduces the reaction between the positive electrode active material and the solid electrolyte, maintaining low internal resistance and improving cycle characteristics of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581806000004
    Figure 0007581806000004
  • Figure 0007581806000005
    Figure 0007581806000005
  • Figure 0007581806000006
    Figure 0007581806000006
Patent Text Reader

Abstract

To provide a cathode active material which can be suppressed in reaction with a solid electrolyte.SOLUTION: In the present disclosure, a coated cathode active material is provided, including a cathode active material, and a coating portion coating at least a part of a front surface of the cathode active material, wherein the coating portion includes a scandium lithium phosphate-based chemical compound or a lithium borate-based chemical compound.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a coated positive electrode active material, a method for producing a coated positive electrode active material, and an all-solid-state battery. [Background technology]

[0002] An all-solid-state battery is a battery that has a solid electrolyte layer between a positive electrode active material layer and a negative electrode active material layer, and has the advantage that it is easier to simplify safety devices compared to liquid batteries that have an electrolyte solution containing a flammable organic solvent.

[0003] Attempts to suppress the reaction between the positive electrode active material and the solid electrolyte have been known. For example, Patent Document 1 discloses a Li-ion conductive oxide (LiNbO 3-α A nonaqueous electrolyte battery is disclosed in which an intermediate layer containing

[0004] Furthermore, Patent Document 2 describes a positive electrode for an all-solid-state secondary battery, which contains a surface-treated positive electrode active material in which at least a portion of the surface of the positive electrode active material is covered with an oxide containing at least one type of Group 13 element in the periodic table.

[0005] Patent Document 3 describes a positive electrode active material for an alkaline storage battery, in which 1 to 30% of the surface area of ​​solid solution particles mainly composed of nickel hydroxide is covered with particles of at least one oxide selected from yttrium, scandium, or lanthanoids, and the outer periphery is covered with cobalt oxide having an average cobalt valence of more than 3.0.

[0006] Patent Document 4 describes a non-sintered nickel electrode for an alkaline storage battery, which comprises an inner coating layer made of cobalt or a cobalt compound that coats base particles, and an outer coating layer made of yttrium, scandium, or a lanthanoid, or a compound thereof, that coats the inner coating layer. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2011-086555 A [Patent Document 2] JP 2010-192373 A [Patent Document 3] JP 2002-298840 A [Patent Document 4] Japanese Patent Application Publication No. 11-007950 Summary of the Invention [Problem to be solved by the invention]

[0008] When the positive electrode active material and the solid electrolyte react with each other, a high-resistance layer is formed at the interface between them, increasing the internal resistance of the all-solid-state battery.

[0009] The present disclosure has been made in view of the above circumstances, and has as its main object to provide a positive electrode active material capable of suppressing a reaction with a solid electrolyte. [Means for solving the problem]

[0010] The present disclosure provides a coated positive electrode active material having a positive electrode active material and a coating portion that coats at least a portion of a surface of the positive electrode active material, the coating portion including a scandium lithium phosphate-based compound or a lithium borate-based compound.

[0011] According to the present disclosure, by providing a coating portion containing a scandium lithium phosphate-based compound or a lithium borate-based compound on the surface of a positive electrode active material, it is possible to obtain a coated positive electrode active material that is capable of suppressing reaction with a solid electrolyte.

[0012] In the above disclosure, the molar ratio of Li, Sc and P in the scandium lithium phosphate-based compound may satisfy Li:Sc:P=3.00:2.19-5.00:1.99-2.57.

[0013] In the above disclosure, in the lithium scandium phosphate-based compound, a molar ratio of Li to Sc (Li / Sc) may be 0.60 or more.

[0014] In the above disclosure, the molar ratio of Li and B in the lithium borate-based compound may satisfy Li:B=3.00:5.04 to 6.72.

[0015] In the above disclosure, in the lithium borate-based compound, the molar ratio of Li to B (Li / B) may be 0.60 or less.

[0016] The present disclosure also provides a method for producing a coated cathode active material having a cathode active material and a coating portion that coats at least a portion of a surface of the cathode active material, the method including a preparation step of preparing the cathode active material, and a coating portion formation step of forming the coating portion on the surface of the cathode active material by a sputtering method using a scandium lithium phosphate-based precursor compound or a lithium borate-based precursor compound as a target.

[0017] According to the present disclosure, a coated positive electrode active material capable of suppressing reaction with a solid electrolyte can be obtained by performing a sputtering method using a lithium scandium phosphate-based precursor compound or a lithium borate-based precursor compound as a target.

[0018] In the above disclosure, the lithium scandium phosphate-based precursor compound may be Li3Sc2(PO4)3.

[0019] In the above disclosure, the lithium borate precursor compound is Li3B7O 12 may be also possible.

[0020] The present disclosure also provides an all-solid-state battery having a positive electrode active material layer, a negative electrode active material layer, and a solid electrolyte layer formed between the positive electrode active material layer and the negative electrode active material layer, wherein the positive electrode active material layer contains the above-mentioned coated positive electrode active material.

[0021] According to the present disclosure, since the positive electrode active material layer contains the above-mentioned coated positive electrode active material, it is possible to obtain an all-solid-state battery in which the reaction between the coated positive electrode active material and the solid electrolyte is suppressed.

[0022] In the above disclosure, the positive electrode active material in the coated positive electrode active material may be an oxide active material, and the positive electrode active material layer may contain a sulfide solid electrolyte. Effect of the Invention

[0023] The present disclosure has an effect of providing a positive electrode active material capable of suppressing a reaction with a solid electrolyte. [Brief description of the drawings]

[0024] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of a coated positive electrode active material according to the present disclosure. [Diagram 2] FIG. 1 is a schematic cross-sectional view showing an example of an all-solid-state battery according to the present disclosure. [Diagram 3] 4 shows the cell resistance evaluation results of Examples 1-1 to 1-3. [Figure 4] 1 shows the cell resistance evaluation results of Examples 2-1 to 2-3. [Diagram 5] 1 shows the cell resistance evaluation results of Comparative Examples 1-1 to 1-3. [Figure 6] 1 shows the results of measuring the discharge capacity after each cycle in Examples 1-1 to 1-3. [Figure 7] 1 shows the results of measuring the discharge capacity after each cycle in Examples 2-1 to 2-3. [Figure 8] 1 shows the results of measuring the discharge capacity after each cycle in Comparative Examples 1-1 to 1-3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] A. Coated Positive Electrode Active Material The coated positive electrode active material in the present disclosure will be described in detail below. Fig. 1 is a schematic cross-sectional view showing an example of the coated positive electrode active material in the present disclosure. The coated positive electrode active material 10 shown in Fig. 1 has a positive electrode active material 1 and a coating portion 2 that coats at least a part of the surface of the positive electrode active material 1, and the coating portion 2 contains a scandium lithium phosphate compound or a lithium borate compound.

[0026] According to the present disclosure, by providing a coating portion containing a scandium lithium phosphate compound or a lithium borate compound on the surface of a positive electrode active material, a coated positive electrode active material capable of suppressing a reaction with a solid electrolyte can be obtained. Specifically, the scandium lithium phosphate compound or the lithium borate compound can suppress the reaction between the positive electrode active material and the solid electrolyte, similar to conventional lithium niobate (LiNbO3). In addition, the scandium lithium phosphate compound or the lithium borate compound has a higher oxidation potential than conventional lithium niobate (LiNbO3). The high oxidation potential can suppress the coating portion from reacting with the solid electrolyte during charging. As a result, the coating portion and the solid electrolyte can be suppressed from deteriorating. In addition, the high oxidation potential can suppress the oxidative decomposition of the scandium lithium phosphate compound or the lithium borate compound during charging. As a result, the internal resistance is less likely to increase over time, and the cycle characteristics can be improved.

[0027] 1. Covering part The coating portion in the present disclosure is formed so as to cover at least a part of the surface of the positive electrode active material, and includes a scandium lithium phosphate-based compound or a lithium borate-based compound.

[0028] The scandium lithium phosphate compound usually contains Li, Sc, and PO4. The molar ratio of Li, Sc, and P in the scandium lithium phosphate compound is not particularly limited, but preferably satisfies, for example, Li:Sc:P=3.00:2.19-5.00:1.99-2.57. The scandium lithium phosphate compound may contain, for example, Li x Sc y(PO4) z It is preferable that the composition has the following formula: It is preferable that x, y, and z satisfy x:y:z=3.00:2.19-5.00:1.99-2.57.

[0029] In the lithium scandium phosphate compound, the molar ratio of Li to Sc is Li / Sc, the molar ratio of Li to P is Li / P, and the molar ratio of Sc to P is Sc / P. Li / Sc is, for example, 0.60 or more, and may be 0.63 or more, or may be 0.80 or more. Meanwhile, Li / Sc is, for example, 1.37 or less. Li / P is, for example, 1.50 or less, and may be 1.40 or less. Meanwhile, Li / P is, for example, 1.17 or more. Sc / P is, for example, 2.51 or less, and may be 2.38 or less, or may be 2.00 or less. Meanwhile, Sc / P is, for example, 0.85 or more.

[0030] The lithium borate compound usually contains Li, B and O. The molar ratio of Li and B in the lithium borate compound is not particularly limited, but preferably satisfies, for example, Li:B=3.00:5.04 to 6.72. The lithium borate compound may contain, for example, Li a B b O c It is preferable that the composition has the following formula: It is preferable that a, b, and c satisfy a:b:c=3.00:5.04-6.72:9.06-12.0.

[0031] In the lithium borate compound, the molar ratio of Li to B is Li / B. Li / B is, for example, 0.60 or less, may be 0.58 or less, or may be 0.50 or less. On the other hand, Li / B is, for example, 0.45 or more.

[0032] The coating portion preferably contains a scandium lithium phosphate compound or a lithium borate compound as a main component. The ratio of the scandium lithium phosphate compound or the lithium borate compound in the coating portion is, for example, 50% by weight or more, or may be 70% by weight or more, or may be 90% by weight or more. The coating portion may contain only the scandium lithium phosphate compound or only the lithium borate compound. The coating portion may contain at least the scandium lithium phosphate compound or the lithium borate compound, and may contain both the scandium lithium phosphate compound and the lithium borate compound.

[0033] The thickness of the covering portion is, for example, 5 nm or more, and may be 10 nm or more. On the other hand, the thickness of the covering portion is, for example, 100 nm or less, and may be 50 nm or less, or may be 20 nm or less. If the covering portion is too thin, the effect of the present disclosure may not be obtained, and if the covering portion is too thick, the internal resistance of the all-solid-state battery may be high. For example, the thickness of the covering portion can be measured using a transmission electron microscope (TEM) or the like.

[0034] The coating portion covers at least a part of the surface of the positive electrode active material. The coating portion may be formed on a part of the surface of the positive electrode active material, or may be formed on the entire surface. The coverage of the coating portion is, for example, 50% or more, 70% or more, or 90% or more. On the other hand, the coverage of the coating portion may be 100% or less than 100%. The coverage can be determined by X-ray photoelectron spectroscopy (XPS) measurement. The positive electrode active material and the coating portion may be in direct contact with each other, or may be disposed via another layer.

[0035] The method for forming the coating portion will be described in detail in "B. Method for producing coated positive electrode active material" below, and therefore description thereof will be omitted here.

[0036] 2.Cathode active material The positive electrode active material may be, for example, an oxide active material. Specific examples of the oxide active material include LiCoO2, LiMnO2, LiNiO2, LiVO2, and LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, etc., rock salt layered active materials, LiMn2O4, LiNi 0.5 Mn 1.5 Examples of the active material include spinel-type active materials such as O4, and olivine-type active materials such as LiFePO4, LiMnPO4, LiNiPO4, and LiCuPO4. In particular, when the positive electrode active material is an oxide active material and the positive electrode active material layer contains a sulfide solid electrolyte, a high resistance layer is likely to be formed at the interface between the oxide active material and the sulfide solid electrolyte. Even in such a case, the reaction between the oxide active material and the sulfide solid electrolyte can be suppressed by providing the above-mentioned covering portion.

[0037] The shape of the positive electrode active material may be, for example, particulate. 50 ) is not particularly limited, but may be, for example, 10 nm or more, and may be 100 nm or more. On the other hand, the average particle diameter (D 50 ) is, for example, 50 μm or less, and may be 20 μm or less. 50 ) can be calculated, for example, from measurements using a laser diffraction particle size distribution analyzer or a scanning electron microscope (SEM).

[0038] 3.Coated positive electrode active material The coated positive electrode active material in the present disclosure is generally used in an all-solid-state battery. The all-solid-state battery will be described in detail in "C. All-solid-state battery" below, and therefore will not be described here.

[0039] B. Method for producing coated positive electrode active material The method for producing a coated positive electrode active material in the present disclosure is a method for producing a coated positive electrode active material having a positive electrode active material and a coating portion that coats at least a portion of a surface of the positive electrode active material, and includes a preparation step of preparing the positive electrode active material, and a coating portion formation step of forming the coating portion on the surface of the positive electrode active material by a sputtering method using a scandium lithium phosphate-based precursor compound or a lithium borate-based precursor compound as a target.

[0040] According to the present disclosure, a coated positive electrode active material capable of suppressing reaction with a solid electrolyte can be obtained by performing a sputtering method using a lithium scandium phosphate-based precursor compound or a lithium borate-based precursor compound as a target.

[0041] The preparation step in the present disclosure is a step of preparing a positive electrode active material. The positive electrode active material may be prepared by self-synthesis or may be prepared by purchasing a commercially available product. The positive electrode active material is the same as "A. Coated positive electrode active material", so the description here is omitted.

[0042] The coating portion forming step in the present disclosure is a step of forming the coating portion on the surface of the positive electrode active material by a sputtering method using a scandium lithium phosphate-based precursor compound or a lithium borate-based precursor compound as a target.

[0043] The lithium scandium phosphate precursor compound usually contains Li, Sc, and PO4. An example of the lithium scandium phosphate precursor compound is Li3Sc2(PO4)3. On the other hand, the lithium borate precursor compound contains Li, B, and O. An example of the lithium borate precursor compound is Li3B7O 12 As the sputtering method, for example, barrel sputtering is preferable because it is possible to form a uniform film on the surface of the positive electrode active material. By adjusting the sputtering time, etc., the thickness of the coating portion can be adjusted.

[0044] In the coating portion forming step, a heat treatment may or may not be performed after the sputtering, but the latter is preferred. This is because the reaction with the solid electrolyte can be further suppressed. On the other hand, in the former case, the heat treatment temperature is, for example, 300°C or higher, and may be 400°C or higher. The heat treatment atmosphere may be, for example, an argon atmosphere. The heat treatment time is, for example, 1 hour or more and 10 hours or less, and preferably about 5 hours.

[0045] C. All-solid-state battery Fig. 2 is a schematic cross-sectional view of an all-solid-state battery according to the present disclosure. The all-solid-state battery 20 shown in Fig. 2 has a positive electrode active material layer 11 containing the coated positive electrode active material described above, a negative electrode active material layer 12, a solid electrolyte layer 13 formed between the positive electrode active material layer 11 and the negative electrode active material layer 12, a positive electrode current collector 14 that collects current from the positive electrode active material layer 11, and a negative electrode current collector 15 that collects current from the negative electrode active material layer 12.

[0046] According to the present disclosure, since the positive electrode active material layer contains the above-mentioned coated positive electrode active material, it is possible to obtain an all-solid-state battery in which the reaction between the coated positive electrode active material and the solid electrolyte is suppressed.

[0047] 1.Cathode active material layer The positive electrode active material layer is a layer containing at least the coated positive electrode active material described above, and may have at least one of a solid electrolyte, a conductive material, and a binder as necessary. The content of the coated positive electrode active material in the positive electrode active material layer is not particularly limited, and may be appropriately determined according to the performance of the intended battery. The ratio of the coated positive electrode active material in the positive electrode active material layer is, for example, 20% by weight or more, may be 30% by weight or more, or may be 40% by weight or more. On the other hand, the ratio of the coated positive electrode active material is, for example, 80% by weight or less, may be 70% by weight or less, or may be 60% by weight or less.

[0048] The positive electrode active material layer preferably contains a solid electrolyte. The solid electrolyte may be a conventionally known solid electrolyte that is usually used in all-solid-state lithium ion batteries, and may be, for example, a sulfide solid electrolyte, an oxide solid electrolyte, a nitride solid electrolyte, a halide, or the like, among which a sulfide solid electrolyte is preferred. In particular, in the positive electrode active material layer, it is preferred that the sulfide solid electrolyte is in contact with the coated positive electrode active material. This is because the effects of the present disclosure can be enjoyed more.

[0049] Examples of sulfide solid electrolytes include solid electrolytes containing Li, X (X is at least one of P, As, Sb, Si, Ge, Sn, B, Al, Ga, and In), and S. The sulfide solid electrolyte may further contain at least one of O and halogen elements. Examples of halogen elements include F, Cl, Br, and I.

[0050] The sulfide solid electrolyte has an anion structure with an ortho composition (PS4 3- Structure: SiS4 4- Structure, GeS4 4- Structure: AlS3 3- Structure, BS3 3- It is preferable that the anion has an ortho-composition structure) as the main component of the anion. This is because the anion has high chemical stability. The ratio of the anion structure of the ortho-composition is, for example, 70 mol% or more, and may be 90 mol% or more, based on the total anion structures in the sulfide solid electrolyte. The ratio of the anion structure of the ortho-composition can be determined, for example, by Raman spectroscopy, NMR, or XPS. Specific examples of the sulfide solid electrolyte include xLi2S·(100-x)P2S5 (70≦x≦80), yLiI·zLiBr·(100-yz)Li3PS4 (0≦y≦30, 0≦z≦30).

[0051] The sulfide solid electrolyte may be a glass-based sulfide solid electrolyte or a glass ceramic-based sulfide solid electrolyte. The glass-based sulfide solid electrolyte can be obtained by vitrifying the raw material. The glass ceramic-based sulfide solid electrolyte can be obtained, for example, by heat treating the above-mentioned glass-based sulfide solid electrolyte. In addition, the sulfide solid electrolyte preferably has a predetermined crystal structure. Examples of the crystal structure include a Thio-LISICON type crystal structure, a LGPS type crystal structure, and an Argyrodite type crystal structure.

[0052] The shape of the solid electrolyte may be, for example, particulate. The average particle size of the solid electrolyte is, for example, 0.05 μm or more, and may be 0.1 μm or more. On the other hand, the average particle size of the solid electrolyte is, for example, 50 μm or less, and may be 20 μm or less. The average particle size of the solid electrolyte is D 50 and can be calculated, for example, from measurements using a laser diffraction particle size distribution analyzer or a scanning electron microscope (SEM).

[0053] The positive electrode active material layer may contain a conductive material. By using the conductive material, the electronic conductivity in the positive electrode active material layer can be improved. Examples of the conductive material include carbon materials, metal particles, and conductive polymers. Examples of the carbon material include particulate carbon materials such as acetylene black (AB) and ketjen black (KB), and fibrous carbon materials such as carbon fibers, carbon nanotubes (CNT), and carbon nanofibers (CNF).

[0054] The positive electrode active material layer may contain a binder. The use of the binder can improve the denseness of the positive electrode active material layer. Examples of the binder include rubber-based binders such as butylene rubber (BR) and styrene butadiene rubber (SBR), and fluorine-based binders such as polyvinylidene fluoride (PVDF) and polytetrafluoroethylene (PTFE). The thickness of the positive electrode active material layer is, for example, 0.1 μm or more and 1000 μm or less. Examples of the method for forming the positive electrode active material layer include a method of coating a composite material containing at least a coated positive electrode active material and a dispersion medium, and drying the coated composite material.

[0055] 2.Negative electrode active material layer The negative electrode active material layer is a layer containing at least a negative electrode active material, and may contain at least one of a solid electrolyte, a conductive material, and a binder, as necessary.

[0056] The negative electrode active material is not particularly limited, but examples thereof include metal active materials, carbon active materials, and oxide active materials. Examples of the metal active material include simple metals and metal alloys. Examples of the metal elements contained in the metal active material include Si, Sn, In, and Al. The metal alloy is preferably an alloy containing the above metal elements as a main component.

[0057] On the other hand, examples of the carbon active material include mesocarbon microbeads (MCMB), highly oriented graphite (HOPG), hard carbon, and soft carbon. Examples of the oxide active material include Li4Ti5O 12 Lithium titanates such as those mentioned above are also included.

[0058] The ratio of the negative electrode active material in the negative electrode active material layer is, for example, 20% by weight or more, or may be 30% by weight or more, or may be 40% by weight or more, while the ratio of the negative electrode active material is, for example, 80% by weight or less, or may be 70% by weight or less, or may be 60% by weight or less.

[0059] The solid electrolyte, conductive material, and binder are the same as those described in "1. Positive electrode active material layer" above, and therefore the description thereof will be omitted here. The thickness of the negative electrode active material layer is, for example, 0.1 μm or more and 1000 μm or less.

[0060] 3.Solid electrolyte layer The solid electrolyte layer is a layer formed between the positive electrode active material layer and the negative electrode active material layer, and contains at least a solid electrolyte. The solid electrolyte layer may contain only a solid electrolyte, or may further contain a binder.

[0061] The solid electrolyte layer preferably contains a sulfide solid electrolyte as a solid electrolyte. In particular, it is preferable that the sulfide solid electrolyte contained in the solid electrolyte layer is in contact with the coated positive electrode active material contained in the positive electrode active material layer. The sulfide solid electrolyte and the binder are the same as those described in "1. Positive electrode active material layer" above, and therefore the description here is omitted. The thickness of the solid electrolyte layer is, for example, 0.1 μm or more and 1000 μm or less.

[0062] 4.Other The all-solid-state battery of the present disclosure preferably has a positive electrode current collector that collects the current of the positive electrode active material layer, and a negative electrode current collector that collects the current of the negative electrode active material layer. Examples of the material of the positive electrode current collector include SUS, aluminum, nickel, iron, titanium, and carbon. On the other hand, examples of the material of the negative electrode current collector include SUS, copper, nickel, and carbon.

[0063] The type of all-solid-state battery in the present disclosure is not particularly limited, but is typically a lithium-ion battery. The all-solid-state battery in the present disclosure may be a primary battery or a secondary battery, but is preferably a secondary battery, because it can be repeatedly charged and discharged and is useful, for example, as an in-vehicle battery.

[0064] The all-solid-state battery in the present disclosure may be a single cell or a stacked battery. The stacked battery may be a monopolar stacked battery (a parallel-connected stacked battery) or a bipolar stacked battery (a series-connected stacked battery). The shape of the battery may be, for example, a coin type, a laminate type, a cylindrical type, or a square type.

[0065] The present disclosure is not limited to the above-described embodiments. The above-described embodiments are merely examples, and anything that has substantially the same configuration as the technical idea described in the claims of the present disclosure and exhibits similar effects is included in the technical scope of the present disclosure. EXAMPLES

[0066] The all-solid-state battery of the present disclosure will be described more specifically below using examples and comparative examples.

[0067] [Example 1-1] (Preparation of Positive Electrode Active Material Layer) NCM(LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 A coating was performed on 10 g of the cathode active material (10 g of 02, cathode active material) by barrel sputtering using a Li3Sc2(PO4)3 target. This resulted in a coated cathode active material having a coating part with a thickness of 10 nm.

[0068] PVDF, the coated positive electrode active material obtained above, a solid electrolyte (Li2S-P2S5-based glass ceramics), and a conductive material (vapor-grown carbon fiber, VGCF, manufactured by Showa Denko) were added to a polypropylene (PP) container, and the PP container was stirred for 30 seconds with an ultrasonic dispersion device (UH-50 manufactured by SMT). Next, the PP container was shaken for 3 minutes with a shaker (TTM-1 manufactured by Shibata Scientific Co., Ltd.), and further stirred for 30 seconds with an ultrasonic dispersion device to obtain a coating liquid. The obtained coating liquid was applied to an Al foil (manufactured by Nippon Foil Co., Ltd.) substrate by the blade method using an applicator. The coating layer was naturally dried, and then dried on a hot plate at 100 ° C. for 30 minutes to form a positive electrode active material layer on one surface of the Al foil substrate.

[0069] (Preparation of positive electrode current collector) Carbon black and a PVDF-based binder (manufactured by Kureha) were weighed out to a weight ratio of 30:70, and an organic solvent was added to obtain a coating solution. The solution was applied to an Al foil (thickness: 15 μm) by a blade method using an applicator, naturally dried, and then dried on a hot plate at 100° C. for 30 minutes. This formed a positive electrode current collector having a 2 μm-thick carbon layer on one surface of the Al foil.

[0070] (Preparation of negative electrode) A PVDF-based binder (Kureha), a negative electrode active material (lithium titanate (LTO)), and the above-mentioned solid electrolyte were added to a PP container, and the PP container was stirred for 30 seconds with an ultrasonic dispersion device (UH-50 manufactured by SMT) to obtain a coating liquid. Next, a Cu foil (negative electrode current collector) was prepared, and the obtained coating liquid was applied by a blade method using an applicator. The coated electrode was naturally dried, and then dried on a hot plate at 100°C for 30 minutes. This formed a negative electrode active material layer on one surface of the Cu foil (negative electrode current collector). Thereafter, the same treatment was performed to form a negative electrode active material layer on the other surface of the Cu foil (negative electrode current collector), and a negative electrode was obtained.

[0071] (Preparation of solid electrolyte layer) Butyl butyrate and the above-mentioned solid electrolyte were added to a PP container, and the PP container was stirred for 30 seconds with an ultrasonic dispersion device (UH-50, manufactured by SMT). Next, the PP container was shaken for 30 minutes with a shaker (TTM-1, manufactured by Shibata Scientific) and further stirred for 30 seconds with an ultrasonic dispersion device to obtain a coating liquid. The obtained coating liquid was applied to an Al foil (manufactured by Nippon Foil Co., Ltd.) substrate by a blade method using an applicator, and after natural drying, it was dried on a hot plate at 100°C for 30 minutes to obtain a transfer member having an Al foil and a solid electrolyte layer.

[0072] The two obtained transfer members were placed on the negative electrode active material layers formed on both sides of the negative electrode current collector, respectively, and pressed, and the Al foil base material of the transfer member was peeled off. As a result, a solid electrolyte layer was formed on the negative electrode active material layer. The obtained laminate was punched out so as to have a size larger than the positive electrode current collector obtained above. Next, the two obtained positive electrode active material layers were placed on the solid electrolyte layers formed on both sides of the negative electrode, respectively, and pressed, and the Al foil base material on which the positive electrode active material layer was formed was peeled off from the positive electrode active material layer and pressed. As a result, an electrode laminate having a negative electrode active material layer, a solid electrolyte layer, and a positive electrode active material layer on both sides of the negative electrode current collector was obtained.

[0073] Next, a positive electrode current collector was attached to both sides of the obtained electrode laminate using a binder. As a result, a two-layer cell structure all-solid-state battery in which a positive electrode current collector was formed on both sides of the electrode laminate was obtained. At this time, the carbon layer side of the positive electrode current collector was arranged so as to contact the positive electrode active material layer of the electrode laminate. Furthermore, a plurality of the obtained two-layer cell structures were stacked, terminals were welded, and then the stacked cells were sealed with a laminate film to obtain a battery for evaluation.

[0074] [Example 1-2] After coating by barrel sputtering, a coated positive electrode active material was obtained in the same manner as in Example 1-1, except that a heat treatment was performed in an Ar atmosphere at 300° C. for 5 hours. A battery for evaluation was obtained in the same manner as in Example 1-1, except that the coated positive electrode active material obtained was used.

[0075] [Examples 1-3] A coated positive electrode active material was obtained in the same manner as in Example 1-1, except that after coating by barrel sputtering, heat treatment was performed in an Ar atmosphere at 400° C. for 5 hours. A battery for evaluation was obtained in the same manner as in Example 1-1, except that the obtained coated positive electrode active material was used.

[0076] [Example 2-1] Li3B7O as target 12A coated positive electrode active material was obtained in the same manner as in Example 1-1, except that the coated positive electrode active material was used. A battery for evaluation was obtained in the same manner as in Example 1-1, except that the coated positive electrode active material was used.

[0077] [Example 2-2] After coating by barrel sputtering, a coated positive electrode active material was obtained in the same manner as in Example 2-1, except that a heat treatment was performed in an Ar atmosphere at 300° C. for 5 hours. A battery for evaluation was obtained in the same manner as in Example 2-1, except that the obtained coated positive electrode active material was used.

[0078] [Example 2-3] After coating by barrel sputtering, a coated positive electrode active material was obtained in the same manner as in Example 2-1, except that a heat treatment was performed in an Ar atmosphere at 400° C. for 5 hours. A battery for evaluation was obtained in the same manner as in Example 2-1, except that the obtained coated positive electrode active material was used.

[0079] [Comparative Example 1-1] A coated positive electrode active material was obtained in the same manner as in Example 1-1, except that LiNbO3 was used as the target. A battery for evaluation was obtained in the same manner as in Example 1-1, except that the obtained coated positive electrode active material was used.

[0080] [Comparative Example 1-2] After coating by barrel sputtering, a coated positive electrode active material was obtained in the same manner as in Comparative Example 1-1, except that a heat treatment was performed in an Ar atmosphere at 300° C. for 5 hours. A battery for evaluation was obtained in the same manner as in Comparative Example 1-1, except that the obtained coated positive electrode active material was used.

[0081] [Comparative Example 1-3] After coating by barrel sputtering, a coated positive electrode active material was obtained in the same manner as in Comparative Example 1-1, except that a heat treatment was performed in an Ar atmosphere at 400° C. for 5 hours. A battery for evaluation was obtained in the same manner as in Comparative Example 1-1, except that the obtained coated positive electrode active material was used.

[0082] [Composition analysis] In order to determine the composition of the coating of the coated positive electrode active material produced in Example 1-1, Example 2-1, and Comparative Example 1-1, Li3Sc2(PO4)3, Li3B7O 12 After deposition for 24 hours using a LiNbO3 sputtering target, the composition of the coating was determined using ICP measurement.

[0083] In order to determine the composition of the coating of the coated positive electrode active material formed in Example 1-2 and Example 2-2, Li3Sc2(PO4)3, Li3B7O 12 After deposition for 24 hours using the sputtering target, heat treatment was performed at 300°C for 5 hours in an Ar atmosphere, and the composition of the coating was determined using ICP measurement.

[0084] In order to determine the composition of the coating of the coated positive electrode active material formed in Examples 1-3 and 2-3, Li3Sc2(PO4)3, Li3B7O 12 After deposition for 24 hours using the sputtering target, heat treatment was performed at 400°C for 5 hours in an Ar atmosphere, and the composition of the coating was determined using ICP measurement.

[0085] The results of the composition analysis of Examples 1-1 to 1-3 and Examples 2-1 to 2-3 are shown in Tables 1 and 2. The result of the composition analysis of Comparative Example 1-1 was Li:Nb=1:0.99.

[0086] [Table 1]

[0087] [Table 2]

[0088] [Cell resistance evaluation] The cell resistance was measured for the evaluation battery obtained above. The measurement was performed by constant current-constant voltage charging at 25°C and 0.33C in the range of 1.5 to 3.0V, followed by constant current-constant voltage discharging to SOC40%, and the resistance was calculated from the voltage drop (ΔV) when discharging at a rate of 3C for 5 seconds. The resistance obtained from the voltage drop when discharging from 0 to 0.1 seconds was calculated as the reaction resistance, and the resistance obtained from the voltage drop when discharging from 0.1 seconds to 5 seconds was calculated as the diffusion resistance. 1 to 10 cycles of charge and discharge were repeated, with constant current charging and constant current discharging at 0.33C being one cycle, and the resistance of the all-solid-state battery was measured after each cycle. The results at SOC40% are shown in Figures 3 to 5 and Table 3.

[0089] [Table 3]

[0090] As shown in FIG. 3 to FIG. 5 and Table 3, it was confirmed that Examples 1-1 to 1-3 and Examples 2-1 to 2-3 have the same internal resistance as Comparative Examples 1-1 to 1-3. Although Comparative Example 1-3 had a low internal resistance, as described later, it did not obtain a good evaluation in terms of cycle characteristics. The reason is presumed to be that the formed coating portion has oxygen deficiency, which causes electronic conductivity, and oxidative decomposition of the solid electrolyte occurs at the interface between the positive electrode active material and the solid electrolyte. In addition, as shown in FIG. 3, it was confirmed that, comparing Examples 1-1 to 1-3, the higher the heat treatment temperature, the higher the internal resistance in each cycle tends to increase. This is presumed to be because the Li and P deficiency caused by the heat treatment affected the conductivity and oxidation resistance of the coating portion. In addition, it was confirmed that, in each of Examples 1-1 to 1-3, the internal resistance tends to increase as the number of cycles increases. In addition, as shown in FIG. 4, in Examples 2-1 to 2-3, the same tendency as in Examples 1-1 to 1-3 was confirmed.

[0091] [Cycle characteristic evaluation] The above charge / discharge cycle was carried out 50 times for the evaluation battery obtained above, and the measurement results of the discharge capacity after each cycle are shown in FIGS.

[0092] As shown in FIG. 6, the cycle characteristics were better in the order of Example 1-1, Example 1-2, and Example 1-3. As shown in FIG. 3, the internal resistance was lower in the order of Example 1-1, Example 1-2, and Example 1-3, suggesting that the cycle characteristics are better as the internal resistance is lower. Also, as shown in FIG. 7, the cycle characteristics were better in the order of Example 2-1, Example 2-2, and Example 2-3. As shown in FIG. 4, the internal resistance was lower in the order of Example 2-1, Example 2-2, and Example 2-3, suggesting that the cycle characteristics are better as the internal resistance is lower. On the other hand, as shown in FIG. 8, the cycle characteristics were better in the order of Comparative Example 1-1, Comparative Example 1-2, and Comparative Example 1-3, but the cycle characteristics were significantly lower in Comparative Example 1-3. [Explanation of symbols]

[0093] 1 … Cathode active material 2 … Covering part 10... Coated positive electrode active material 11... Positive electrode active material layer 12... Negative electrode active material layer 13…Solid electrolyte layer 14... Positive electrode current collector 15… Negative electrode current collector 20… All-solid-state battery

Claims

1. A positive electrode active material layer containing a coated positive electrode active material and a solid electrolyte, The coated positive electrode active material has a particulate positive electrode active material and a coating portion that coats at least a portion of a surface of the positive electrode active material, the coating portion contains a scandium lithium phosphate compound, The positive electrode active material layer, wherein the molar ratio of Li, Sc and P in the scandium lithium phosphate compound satisfies Li:Sc:P=3.00:2.19-5.00:1.99-2.

57.

2. A positive electrode active material layer containing a coated positive electrode active material and a solid electrolyte, The coated positive electrode active material has a particulate positive electrode active material and a coating portion that coats at least a portion of a surface of the positive electrode active material, the coating portion contains a scandium lithium phosphate compound, In the positive electrode active material layer, in the lithium scandium phosphate-based compound, a molar ratio of Li to Sc (Li / Sc) is 0.60 or more and 1.37 or less.

3. The thickness of the coating portion is 5 nm or more and 20 nm or less, The positive electrode active material layer according to claim 1 or 2, wherein a coverage rate of the covering portion is 90% or more.

4. A method for producing a coated positive electrode active material having a particulate positive electrode active material and a coating portion that coats at least a portion of a surface of the positive electrode active material and contains a scandium lithium phosphate compound, comprising: A preparation step of preparing the positive electrode active material; and forming a coating portion on a surface of the positive electrode active material by a sputtering method using Li 3 Sc 2 (PO 4 ) 3 as a target. The coated positive electrode active material satisfies at least one of the following (i) and (ii): (i) the molar ratio of Li, Sc, and P in the scandium lithium phosphate-based compound satisfies Li:Sc:P=3.00:2.19-5.00:1.99-2.57; and (ii) The method for producing a coated positive electrode active material, wherein in the scandium lithium phosphate-based compound, a molar ratio of Li to Sc (Li / Sc) is 0.60 or more and 1.37 or less.

5. The thickness of the coating portion is 5 nm or more and 20 nm or less, The method for producing a coated positive electrode active material according to claim 4 , wherein a coverage rate of the coating portion is 90% or more.

6. a positive electrode active material layer, a negative electrode active material layer, and a solid electrolyte layer formed between the positive electrode active material layer and the negative electrode active material layer, The positive electrode active material layer according to claim 1 or 2,

7. The positive electrode active material in the coated positive electrode active material is an oxide active material, The all-solid-state battery according to claim 6 , wherein the positive electrode active material layer contains a sulfide solid electrolyte as the solid electrolyte.

Citation Information

Patent Citations

  • Non-sintered nickel electrode for alkali storage battery

    JP1999007950A

  • Positive electrode active material for alkaline storage battery, and the alkaline storage battery using the same

    JP2002298840A

  • Nonaqueous electrolyte secondary battery

    JP2007103339A

  • All-solid battery

    JP2010135090A

  • All-solid secondary battery

    JP2010192373A