Manufacturing method of grindstone
The method of fitting parallelogram-shaped grindstone parts with angled molds addresses uncut parts and wear issues, enhancing efficiency and reducing costs in grindstone manufacturing.
Patent Information
- Application Number
- JP2020204681
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-10
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-12-10
AI Technical Summary
Existing methods for manufacturing wide cylindrical grindstones result in uncut parts due to adhesive bonding, leading to increased grinding load and frequent truing requirements, thereby elevating grinding costs.
A method involving the fitting and fixing of cylindrical grindstone parts with a parallelogram shape onto a core member, using molds with angled closure surfaces to ensure consistent spacing and orientation, preventing uncut parts and reducing wear by limiting grinding load.
This method prevents uncut parts and excessive wear, reducing the need for traverse grinding and truing, thereby lowering grinding costs and maintaining consistent abrasive grain density.
Smart Images

Figure 0007581821000001 
Figure 0007581821000002 
Figure 0007581821000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for manufacturing a grinding wheel. [Background technology]
[0002] Wide cylindrical grinding wheels are used to grind the surfaces of long objects such as camshafts. Such wide grinding wheels are sometimes manufactured by fitting multiple cylindrical grinding wheel parts side by side on a shaft member, as in the grinding wheel described in Patent Document 1. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2005-329518 A Summary of the Invention [Problem to be solved by the invention]
[0004] In the grinding wheel obtained by the above-mentioned manufacturing method, adjacent grinding wheel parts are bonded together with an adhesive or the like, so that grinding cannot be performed at the bonded parts, and residual grinding occurs. When traverse grinding is performed to remove the residual grinding, the grinding load on the parts of the grinding wheel adjacent to the bonded parts becomes very large, and wear progresses extremely. As a result, truing becomes necessary frequently, which causes a problem of increasing grinding costs. For this reason, a manufacturing method that can suppress grinding costs as a manufacturing method for wide grinding wheels is desired. [Means for solving the problem]
[0005] The present disclosure can be realized in the following forms. [Mode 1] A method for manufacturing a grindstone in which a plurality of cylindrical grindstone portions are fitted in line in the axial direction of a columnar grindstone core member and secured to the outer periphery, the method comprising the steps of: (a) preparing a plurality of cylindrical grindstone base members that are bases for the plurality of grindstone portions, the plurality of grindstone base members having a parallelogram shape projected onto a plane parallel to a cross section including a central axis of the grindstone core member; (b) fitting the plurality of grindstone base members in line in the axial direction of the grindstone core member onto the outer periphery such that the distance between the opposing end faces of two adjacent grindstone base members is constant over the entire circumference; (c) securing the plurality of grindstone base members to the outer periphery; and (d) removing and shaping the ends of the plurality of grindstone base members as a whole in the grindstone base members located at both ends in the axial direction of the grindstone core member among the plurality of grindstone base members, thereby forming both end faces of the plurality of grindstone base members as a whole into axial directions perpendicular to the axial direction. and a step of forming a surface of the grinding wheel into which the grinding wheel is pressed, the step (a) comprising the steps of: (a1) preparing a first mold that forms a cylindrical internal space and has one axial end of the internal space closed and the other end open, and a second mold that has a fitting portion that is fitted into the internal space from the other end; (a2) arranging the first mold in a predetermined orientation and filling the internal space with a grinding wheel material containing abrasive grains and a binder; and (a3) fitting the second mold into the internal space to form a grinding wheel material containing the abrasive grains and a binder. a step of compressing a stone material, wherein in the first mold, a closing surface that closes the one end of the internal space is inclined at a predetermined angle different from 90 degrees with respect to the axial direction of the internal space, and in the fitting portion, a tip surface on the tip side that is fitted into the internal space is inclined at the predetermined angle with respect to the axial direction of the internal space, and the step (a3) includes a step of fitting the second mold into the internal space so that the tip surface is parallel to the closing surface.
[0006] (1) According to one embodiment of the present disclosure, there is provided a method for manufacturing a grinding wheel in which a plurality of cylindrical grinding wheel portions are fitted into and fixed to the outer periphery of a columnar grinding wheel core member in a line in the axial direction of the grinding wheel core member. The method for manufacturing this grinding wheel includes the steps of: (a) preparing a plurality of cylindrical grinding wheel base members that serve as the bases for a plurality of the grinding wheel portions, the plurality of grinding wheel base members having a parallelogram shape projected onto a plane parallel to a cross section including the central axis of the grinding wheel; (b) fitting the plurality of grinding wheel base members in a line in the axial direction of the grinding wheel core member onto the outer periphery such that the distance between the opposing end faces of two adjacent grinding wheel base members is constant around the entire circumference; (c) fixing the plurality of grinding wheel base members to the outer periphery; and (d) removing and shaping the ends of the plurality of grinding wheel base members as a whole, in the grinding wheel base members that are located at both ends in the axial direction of the grinding wheel core member, thereby shaping both end faces of the plurality of grinding wheel base members as a whole into surfaces perpendicular to the axial direction. According to this embodiment of the manufacturing method of the grinding wheel, a plurality of grinding wheel base members, each of which has a parallelogram projected shape on a plane parallel to the cross section including its axis, are fitted to the outer periphery of the grinding wheel core member so that the distance between the opposing end faces of two adjacent grinding wheel base members is constant over the entire circumference, and the boundaries between the grinding wheel parts in the finished grinding wheel can be arranged at an incline with respect to the direction perpendicular to the axial direction of the grinding wheel core member. Therefore, when the grinding wheel is rotated, the boundaries between the grinding wheel parts can be limited to a part of the entire circumference in the rotation direction, i.e., in the direction perpendicular to the axial direction, and it is possible to avoid the occurrence of uncut parts only at a certain position in the axial direction of the workpiece. Therefore, even if a traverse is performed using the grinding wheel, the grinding load on a specific part of the grinding wheel can be increased and the wear can be prevented from progressing excessively, and the number of times truing is performed can be reduced, thereby reducing the grinding cost. (2) In the above-mentioned method for manufacturing a grindstone, the step (b) includes the steps of: (b1) preparing a first mold that forms a cylindrical internal space and has one axial end of the internal space closed and the other end open; and (b2) preparing a second mold that has a fitting portion that is fitted into the internal space from the other end; (b3) placing the first mold in a predetermined orientation and filling the internal space with a grindstone material containing abrasive grains and a binder; and (b4) fitting the second mold into the internal space to fill the grindstone material filled in the internal space. and compressing the grinding wheel material, wherein in the first mold, a closing surface that closes the one end of the internal space is inclined at a predetermined angle different from 90 degrees with respect to the axial direction of the internal space, and in the fitting portion, a tip surface on the tip side that is fitted into the internal space is inclined at the predetermined angle with respect to the axial direction of the internal space, and the step (b3) may include a step of fitting the second mold into the internal space so that the tip surface is parallel to the closing surface. According to this form of manufacturing method for a grinding wheel, in the first mold, the closing surface that closes one end of the internal space is inclined at a predetermined angle different from 90 degrees with respect to the axial direction of the internal space, and in the fitting portion, the tip surface on the tip side that is fitted into the internal space is inclined at a predetermined angle with respect to the axial direction of the internal space. Therefore, by filling the internal space with grinding wheel material and compressing it, a grinding wheel base member whose projected shape onto a plane parallel to the cross section including its axis is a parallelogram can be easily formed. (3) In the above-described method for manufacturing a grindstone, the predetermined orientation may be an orientation in which the occluded surface is parallel to a horizontal plane. According to this embodiment of the method for manufacturing a grinding wheel, when filling the internal space with the grinding wheel material, the closing surface of the internal space in the first mold can be arranged parallel to the horizontal plane. This makes it easier to keep the height (filling amount) of the grinding wheel material along the axial direction of the internal space constant over the entire circumference when the grinding wheel material is filled in the internal space. This makes it possible to prevent pressure distribution in the circumferential direction caused by differences in the filling amount of the grinding wheel material during subsequent compression, thereby preventing the occurrence of coarse and dense abrasive grains in the finished grinding wheel.
[0007] The present disclosure may be realized in various forms, such as an apparatus for manufacturing a grindstone, a die for forming a grindstone base member, and the like. [Brief description of the drawings]
[0008] [Figure 1] 1 is an explanatory diagram showing a schematic configuration of a grindstone manufactured by a grindstone manufacturing method according to an embodiment of the present disclosure; [Diagram 2] FIG. 4 is a process diagram showing a method for manufacturing a grindstone. [Diagram 3] FIG. 2 is a perspective view showing a schematic configuration of a first mold. [Figure 4] FIG. 4 is a perspective view showing a schematic configuration of a second mold. [Diagram 5] FIG. 11 is a cross-sectional view showing the first mold and the second mold when step P115 is being performed. [Figure 6] FIG. 11 is an explanatory diagram showing a portion to which an adhesive is applied in process P130. [Figure 7] FIG. 13 is an explanatory diagram showing the two wheel base members after completion of step P135. [Figure 8] FIG. 2 is an explanatory diagram showing a schematic configuration of a grindstone manufactured by a grindstone manufacturing method of a comparative example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] A. Embodiment: A1. Composition of Grindstone 100: FIG. 1 is an explanatory diagram showing a schematic configuration of a grindstone 100 manufactured by a grindstone manufacturing method according to an embodiment of the present disclosure. The grindstone 100 has a cylindrical external shape and is fixed to the outer periphery of a columnar grindstone core member 400. The grindstone core member 400 has a columnar shaft portion 401 and a connection portion 402 connected at their ends. The grindstone 100 is fixed to one side of the shaft portion 401 in the axial direction AD, and a part of the other side is exposed. The above-mentioned "axial direction AD" means a direction along the central axis C1 of the grindstone core member 400. In this embodiment, the grindstone 100 is fixed to the shaft portion 401 so that its central axis coincides with the central axis C1 of the grindstone core member 400. Therefore, the above-mentioned "axial direction AD" can also be said to be a direction along the central axis of the grindstone 100. The connection portion 402 is connected to the exposed end of the shaft portion 401. A screw is formed on the outer circumferential surface of the connection portion 402. The connection part 402 is screwed to the grinding wheel shaft 510, which is a rotating part of the grinding wheel head 500 of the grinding machine. As a result, the rotational force of a motor (not shown) provided in the grinding wheel head 500 is transmitted to the shaft part 401 via the connection part 402, and the grinding wheel 100 rotates to grind the outer peripheral surface of the workpiece W1. The workpiece W1 is a long object, that is, an object whose length in the longitudinal direction is much larger than its length in the lateral direction. For example, a camshaft corresponds to such a workpiece W1. The camshaft has a plurality of cam parts WC in the axial direction. The grinding wheel 100 performs cam processing on the cam parts WC. In order to grind the workpiece W1, which is such a long object, the length of the axial direction AD of the grinding wheel 100 is relatively long. For example, the length of the axial direction AD of the grinding wheel 100 is 70 cm (centimeters) or more.
[0010] The grindstone 100 has a structure in which two cylindrical grindstone parts 10a and 10b are fitted in the axial direction AD of the grindstone core member 400 and fixed to the outer circumferential surface of the grindstone core member 400 (shaft part 401). Both of the two grindstone parts 10a and 10b are formed of a material containing abrasive grains made of CBN (cubic boron nitride). As shown in FIG. 1, the boundary part 20 between the two grindstone parts 10a and 10b is inclined at an angle θ to a direction perpendicular to the central axis C1, i.e., to the rotation direction of the grindstone 100. The boundary part 20 is formed by arranging the grindstone parts 10a and 10b so that the two opposing end faces of the grindstone parts 10a and 10b have a shape inclined at an angle θ to a direction perpendicular to the central axis C1, and the distance in the axial direction AD between these two end faces is constant. These two end faces are fixed to each other with an adhesive.
[0011] The boundary portion 20 does not have any abrasive grains constituting the grinding wheel 100. Therefore, the workpiece W1 cannot be ground at the boundary portion 20. However, since the boundary portion 20 is inclined at an angle θ with respect to the direction perpendicular to the axial direction AD, i.e., the direction of rotation, as shown in FIG. 1, the portion where the boundary portion 20 exists extends over a wide range having a width wd1 along the axial direction AD. Therefore, the boundary portion 20 can be limited to a part of the entire circumference in the direction perpendicular to the axial direction AD (the direction of rotation), and it is possible to prevent the workpiece W1 from being left uncut over the entire circumference at a certain position in the axial direction AD. In addition, the uncut portion generated at the boundary portion 20 can be ground by other parts on the same circumference, so there is no need to perform traverse grinding. In addition, even if traverse grinding is performed in order to reliably remove the uncut portion or with zero cut, the grinding load on a specific portion of the grinding wheel 100 can be increased and wear can be prevented from progressing excessively, and the number of times truing is performed can be reduced, thereby reducing grinding costs.
[0012] A2. Manufacturing method of grinding wheel 100: FIG. 2 is a process diagram showing a manufacturing method of the grinding wheel 100. First, in step P105, a material for the grinding wheel base member (hereinafter, simply referred to as "grinding wheel material") that is the base of the grinding wheel 100 is prepared. The grinding wheel base member is a member that becomes the grinding wheel parts 10a and 10b through a process (step P140) of removing and shaping the end parts, which will be described later. Therefore, the material of the grinding wheel base member is the material of the grinding wheel parts 10a and 10b, and can also be said to be the material of the grinding wheel 100. Hereinafter, the grinding wheel base member that is the base of the grinding wheel part 10a is called the grinding wheel base member 11a, and the grinding wheel base member that is the base of the grinding wheel part 10b is called the grinding wheel base member 11b. Specifically, the material prepared in step P105 is obtained by mixing abrasive grains made of CBN, a binder, and a filler. The grinding wheel 100 is a so-called vitrified grinding wheel, and has a structure in which an inorganic binder such as glass or ceramic is melted during sintering to fix the abrasive grains.
[0013] In step P110, the mold is tilted and positioned so as to assume a predetermined posture, and in step P115, the grinding wheel material is filled into the mold. The mold positioned in step P110 is a mold for forming the grinding wheel base member, and is made up of two molds (a first mold 200 and a second mold 300) that are used in combination with each other.
[0014] FIG. 3 is a perspective view showing a schematic configuration of the first mold 200. In FIG. 3, three mutually orthogonal axes (X1 axis, Y1 axis, Z1 axis) are shown. The Z1 axis is parallel to the central axis C2. The same three axes (X1 axis, Y1 axis, Z1 axis) are shown in FIG. 4 described later. The first mold 200 has a configuration in which a cavity 211, which is an internal space filled with a grinding wheel material, is formed inside a mold body 201 having an external shape of a substantially rectangular parallelepiped. The cavity 211 has an external shape of a substantially cylindrical shape. In the cylindrical internal space provided along the central axis C2 of the mold body 201, a columnar portion 220 having a central axis coinciding with the central axis of the internal space is provided, and the cavity 211 is, so to speak, formed as a gap between the outer peripheral surface of the columnar portion 220 and the outer diameter surface of the internal space. The lower end 212 (annular virtual surface) of the cavity 211 in the Z1 axis direction is closed. In other words, the mold body 201 has a closing surface S202 that closes the end 212 of the cavity 211. On the other hand, the upper end of the cavity 211 in the Z1 axis direction is open. A virtual surface S2 including the closing surface S202 is inclined with respect to the bottom surface S201 of the mold body 201. Specifically, the angle θ between the perpendicular line L20 of the surface S2 and the perpendicular line L2 of the bottom surface S201 of the mold body 201 is greater than 0 degrees. This angle θ coincides with the angle θ in FIG. 1.
[0015] FIG. 4 is a perspective view showing a schematic configuration of the second mold 300. The second mold 300 includes a fitting portion 301 and a pressing portion 302. The fitting portion 301 is fitted into the cavity 211 (internal space) of the first mold 200 from one end of the cavity 211 that is open. The fitting portion 301 has a substantially cylindrical external shape. A surface S301 (hereinafter referred to as a "tip surface S301") on the lower side in the Z1 axis direction of the fitting portion 301 is inclined with respect to a plane perpendicular to the central axis C3 of the second mold 300. Specifically, the angle θ between a perpendicular line L30 of an imaginary surface S3 including the tip surface S301 and a perpendicular line L3 of an imaginary surface perpendicular to the central axis C3 is the same as the angle θ shown in FIG. 3. A cylindrical internal space 320 along the central axis C3 is formed in the center of the fitting portion 301, and the columnar portion 220 of the first mold 200 can be fitted into the internal space 320. The pressing portion 302 is connected to the upper end of the fitting portion 301 in the Z1 axis direction. The pressing portion 302 has an external shape of a substantially rectangular parallelepiped, and is disposed so that the largest surface of the pressing portion 302 is perpendicular to the central axis C3. The pressing portion 302 is a portion to which force is applied when the grinding wheel material filled in the cavity 211 of the first mold 200 is pressed by the second mold 300.
[0016] FIG. 5 is a cross-sectional view showing the first mold 200 and the second mold 300 during the execution of the process P115. In FIG. 5, three mutually orthogonal axes (X2 axis, Y2 axis, Z2 axis) are shown. The Z2 axis is parallel to the vertical direction. As shown in FIG. 5, a work table 600 is placed on a horizontal plane S0, and the first mold 200 is placed so that the bottom surface S201 of the mold body 201 is in contact with the upper surface S600 of the work table 600. Here, the upper surface S600 of the work table 600 is inclined at an angle θ with respect to the horizontal plane S0. Therefore, the bottom surface S201 of the mold body 201 is also inclined at an angle θ with respect to the horizontal plane S0. As a result, the end 212 (closed surface S202) of the cavity 211, which was inclined at an angle θ with respect to the bottom surface S201, is arranged parallel to the horizontal plane S0. In this manner, in process P110, the first mold 200 is placed on the upper surface S600 of the workbench 600, so that the posture of the first mold 200 is a predetermined posture in which the central axis C2 of the first mold 200 is inclined at an angle θ with respect to the vertical direction.
[0017] In the first mold 200 arranged in the posture shown in Fig. 5, a predetermined amount of grinding wheel material is filled into the cavity 211. As a result, the upper surface S15 of the filled grinding wheel material 15 becomes parallel to the horizontal plane S0. By filling the cavity 211 with the grinding wheel material 15 with the first mold 200 arranged in such a posture, the height of the grinding wheel material 15 along the central axis C2, in other words, the filling amount of the grinding wheel material 15 in the cavity 211, can be made substantially equal at any position in the circumferential direction.
[0018] As shown in FIG. 2, in step P120, the fitting portion 301 of the second mold 300 is fitted into the cavity 211 of the first mold 200 to compress the grindstone material 15 filled in the cavity 211, and then the compressed grindstone material 15 is released from the first mold 200. The first mold 200 is arranged in a posture as shown in FIG. 5, and the grindstone material 15 is filled into the cavity 211 in that state. In step P120, the fitting portion 301 of the second mold 300 is inserted into the cavity 211 in that state. Then, a compressive force is applied in the direction of the central axis C3 using the pressing portion 302, and the grindstone material 15 is compressed in the direction of the central axis C3. When the fitting portion 301 is fitted into the cavity 211, the fitting portion 301 is fitted so that the tip surface S301 of the fitting portion 301 is parallel to the closing surface S202 of the mold body 201.
[0019] 2, in step P125, the released grinding wheel material 15 is fired under a predetermined temperature profile. By repeating the above steps P105 to P125 twice, or by preparing two sets of the first mold 200 and the second mold 300 and performing steps P110 to P120 in parallel for these two mold sets, two grinding wheel base members 11a and 11b are obtained. In step P130, adhesive is applied to predetermined locations of the two obtained grinding wheel base members 11a and 11b.
[0020] FIG. 6 is an explanatory diagram showing a portion to which an adhesive is applied in step P130. FIG. 6 shows a cross section along the central axis C1 of the grindstone base member 11a. As shown in FIG. 6, the grindstone base member 11a has a shape in which a projection shape onto a plane parallel to the cross section including the central axis C1 is a parallelogram. The grindstone base member 11b also has a similar shape. An axial hole 14 along the central axis C1 is formed inside the grindstone base member 11a. In step P130, an adhesive is applied to the surface of the axial hole 14 and one end face 13 of both end faces in the direction of the central axis C1 of the axial hole 14. The end face 13 is a surface that will face the grindstone base member 11b in the axial direction AD in a later step.
[0021] As shown in Fig. 2, in step P135, a plurality of grindstone base members, i.e., in this embodiment, two grindstone base members 11a and 11b, are attached to the shaft portion 401 in phase with each other and fixed to the outer circumferential surface of the shaft portion 401. "Attaching the two grindstone base members 11a and 11b to the shaft portion 401 in phase with each other" means that the shaft portion 401 is inserted into the shaft holes of the two grindstone base members 11a and 11b, respectively, and in this state, the two grindstone base members 11a and 11b are arranged so that the distance between the opposing end faces is constant over the entire circumference (constant at any position in the circumferential direction perpendicular to the central axis C1). In addition, in step P135, the two grindstone base members 11a and 11b are pressed against each other in the direction of the central axis C1. As a result, the two grindstone base members 11a, 11b are also fixed to each other, and a boundary portion 20 is formed at the boundary between the two grindstone base members 11a, 11b.
[0022] Fig. 7 is an explanatory diagram showing the two grindstone base members 11a, 11b after completion of step P135. As shown in Fig. 7, the two grindstone base members 11a, 11b each having a parallelogram projected shape are attached to the shaft portion 401 in phase with each other in the direction of the central axis C1.
[0023] As shown in FIG. 2, in step P140, the grindstone base members at both ends in the direction of the central axis C1, in this embodiment, the two grindstone base members 11a and 11b, are removed and shaped to form both end faces of the grindstone 100 as a whole, so that both end faces of the grindstone 100 are formed into planes perpendicular to the axial direction AD. In step P140, a truing device 700 shown in FIG. 7 is used. The truing device 700 has a configuration in which a grindstone 702 is supported by a shaft member 703. The truing device 700 is a so-called diamond truer, and the grindstone 702 has a configuration in which a large amount of diamond abrasive grains 701 are dispersed in a high-strength bond. As shown in FIG. 7, the end EP1 far from the grindstone base member 11b among both ends in the axial direction AD of the grindstone base member 11a is cut off from the grindstone base member 11a at the cutting line ct1 by the truing device 700. Similarly, of both ends of the grindstone base member 11b in the axial direction AD, the end EP2 farther from the grindstone base member 11a is cut off from the grindstone base member 11b at the cutting line ct2 by the truing device 700. Upon completion of this process P140, the grindstone base member 11a is formed into the grindstone portion 10a, and the grindstone base member 11b is formed into the grindstone portion 10b. In this way, the grindstone 100 shown in FIG. 1 is completed.
[0024] FIG. 8 is an explanatory diagram showing a schematic configuration of a grindstone 900 manufactured by a method for manufacturing a grindstone of a comparative example. The grindstone 900 is different from the grindstone 100 of the present embodiment shown in FIG. 1 in that the grindstone 900 includes two grindstone parts 90a and 90b instead of the two grindstone parts 10a and 10b. The two grindstone parts 90a and 90b have a cylindrical external shape and are fitted into the grindstone core member 400 (shaft part 401) in line with the axial direction AD parallel to the central axis C10 of the grindstone parts 90a and 90b. The end faces of the two grindstone parts 90a and 90b facing each other are formed so as to be perpendicular to the axial direction AD. Therefore, the boundary part 80 between the grindstone parts 90a and 90b coincides with the direction perpendicular to the axial direction AD. Such a grindstone 900 is manufactured by using a grindstone base member having a shape different from that of the grindstone base members 11a and 11b. The grindstone base member of the comparative example has a shape almost equal to that of the grindstone parts 90a and 90b. That is, it has a cylindrical external shape. Therefore, in the comparative example, the step P140 is omitted. Also, unlike the present embodiment, the mold of the comparative example has a cavity closing surface parallel to the bottom surface of the mold body, and the line end surface of the fitting part perpendicular to its own central axis. And, in the comparative example, the mold is not tilted in the step P110. In the comparative example, the grindstone material is filled into the mold placed without tilting it on the horizontal plane, and then pressed and demolded, and then sintered to obtain the grindstone parts 90a and 90b. Then, the two grindstone parts 90a and 90b are coated with adhesive and attached to the grindstone core member 400 as shown in FIG. 8.
[0025] In the grindstone 900 manufactured by the manufacturing method of the comparative example, since the boundary portion 80 is perpendicular to the axial direction AD, the uncut portion is generated around the entire circumference of the workpiece W1 at the boundary portion 80. Therefore, in the comparative example, it is necessary to relatively move the grindstone 900 and the workpiece W1 in the axial direction AD and perform traverse grinding to remove the uncut portion. In this case, the grindstone portion 90a and the grindstone portion 90b are subjected to a grinding load concentrated on the portion adjacent to the boundary portion 80, and wear progresses. Therefore, truing is performed more frequently, and the grinding cost using the grindstone 900 increases.
[0026] On the other hand, according to the grinding wheel 100 obtained by the manufacturing method of the present embodiment described above, the boundary portion 20 can be limited to a part of the entire circumference in the direction perpendicular to the axial direction AD (rotation direction), and it is possible to avoid the occurrence of uncut portions only at a certain position in the axial direction AD of the workpiece. In addition, the uncut portions occurring at the boundary portion 20 can be ground by other portions in the circumferential direction. Therefore, it is possible to suppress the need for traverse grinding to grind the surface of the workpiece W1. Therefore, even if traverse grinding is performed, it is possible to suppress the grinding load on a specific portion of the grinding wheel 100 from increasing and causing extreme wear, and it is possible to reduce the number of times truing is performed and suppress the grinding cost.
[0027] According to the manufacturing method of the grinding wheel 100 of the first embodiment described above, the two grinding wheel base members 11a, 11b, each of which has a parallelogram projected shape on a plane parallel to the cross section including the central axis C1, are fitted into the outer periphery of the grinding wheel core member 400 so that the distance between the opposing end faces is constant over the entire circumference, and are fixed to the outer periphery, so that the boundary portion 20 between the grinding wheel portions 10a, 10b in the finished product of the grinding wheel 100 can be arranged at an incline with respect to the direction perpendicular to the axial direction AD of the grinding wheel core member 400. Therefore, when the grinding wheel 100 is rotated, the boundary portion 20 between the grinding wheel portions 10a, 10b can be limited to a part of the entire circumference in the rotation direction, i.e., in the direction perpendicular to the axial direction AD, and it is possible to avoid the occurrence of uncut portions only at a certain position in the axial direction AD in the workpiece W1. Therefore, even if traversing is performed using the grinding wheel 100, the grinding load on a specific part of the grinding wheel 100 can be prevented from increasing and causing extreme wear, and the number of times truing is performed can be reduced, thereby reducing grinding costs.
[0028] In the first mold 200, the closing surface S202 closing one end of the internal space is inclined at a predetermined angle different from 90 degrees with respect to the axial direction of the cavity 211, and in the fitting portion 301, the tip surface S301 on the tip side that is fitted into the cavity 211 is inclined at a predetermined angle with respect to the axial direction of the cavity 211. Therefore, by filling the cavity 211 with the grinding wheel material 15 and compressing it, it is possible to easily form the grinding wheel base members 11a, 11b whose projected shape onto a plane parallel to a cross section including their own central axis C1 is a parallelogram.
[0029] Furthermore, when filling the grinding wheel material 15 into the cavity 211, the closing surface S202 of the cavity 211 in the first mold 200 is arranged parallel to the horizontal plane S0. This makes it easier to keep the height (filling amount) of the grinding wheel material 15 along the axial direction of the cavity 211 constant over the entire circumference when the grinding wheel material 15 is filled into the cavity 211. Therefore, when compressed thereafter, pressure distribution occurs in the circumferential direction due to differences in the filling amount of the grinding wheel material 15, which can prevent uneven distribution of abrasive grains in the finished grinding wheel.
[0030] B. Other embodiments: (B1) In the above embodiment, the grinding wheel 100 was made of a material containing abrasive grains made of CBN. However, it is not limited to CBN and may be made of a material containing any type of abrasive grains, such as diamond particles.
[0031] (B2) In step P130, adhesive is applied to the surface of the shaft hole 14 in the grindstone base member 11a, but the present disclosure is not limited to this. Instead of or in addition to the surface of the shaft hole 14, adhesive may also be applied to the surface of the shaft portion 401. With this configuration as well, the grindstone base member 11a can be fixed to the shaft portion 401. The same may be done with the grindstone base member 11b.
[0032] (B3) In the above embodiment, the grinding wheel 100 has two grinding wheel portions 10a, 10b, but the number is not limited to two, and the grinding wheel 100 may have any number of grinding wheel portions equal to or greater than two. In such a configuration, the grinding wheel base members to be ground in step P140 are the two grinding wheel base members located at both ends in the axial direction AD, and the other grinding wheel base members sandwiched between the two grinding wheel base members are not ground.
[0033] (B4) In the above embodiment, the first mold 200 is inclined by using the work table 600, but such inclination may be omitted and the first mold 200 may be arranged so that the horizontal plane S0 and the bottom surface S201 of the first mold 200 are parallel to each other. Even in such a configuration, at least on the closed surface S202 side of the cavity 211, the surface can be inclined at an angle other than 90 degrees with respect to the direction perpendicular to the axial direction. Therefore, by using such a surface as a surface facing the adjacent grinding wheel portions in the grinding wheel 100, the same effect as the above embodiment can be achieved.
[0034] (B5) In the above embodiment, the two dies 200, 300 are used to form the two grinding wheel base members 11a, 11b, but the present disclosure is not limited to this. For example, the two dies may be two dies having cavities of the same shape as the semi-cylindrical members obtained when the grinding wheel base members 11a, 11b are divided at a cross section including the central axis. Also, three or more dies may be used instead of two. That is, in general, any shape and any number of dies capable of forming a grinding wheel base member whose projected shape onto a plane parallel to a cross section including its axis is a parallelogram may be used in the manufacturing method of the grinding wheel of the present disclosure.
[0035] The present disclosure is not limited to the above-mentioned embodiments, and can be realized in various configurations without departing from the spirit of the present disclosure. For example, the technical features in each embodiment corresponding to the technical features in each form described in the Summary of the Invention column can be appropriately replaced or combined in order to solve some or all of the above-mentioned problems or to achieve some or all of the above-mentioned effects. Furthermore, if a technical feature is not described as essential in this specification, it can be appropriately deleted. [Explanation of symbols]
[0036] 10a...grindstone portion, 10b...grindstone portion, 11a...grindstone base member, 11b...grindstone base member, 13...end surface, 14...shaft hole, 15...grindstone material, 20...boundary portion, 80...boundary portion, 90a...grindstone portion, 90b...grindstone portion, 100...grindstone, 200...first mold, 201...mold body, 211...cavity, 212...end portion, 220...cylindrical portion, 300...second mold, 301...fitting portion, 302...pressing portion, 320...internal space, 400...grindstone core member, 401...shaft portion, 402...connecting portion, 500...grinding table, 600...work table, 60 1...top surface, 700...truing device, 702...grinding wheel, 703...shaft member, 900...grinding wheel, C1...center axis, AX...axial direction, C10...center axis, C2...center axis, C3...center axis, EP1...end, EP2...end, L2...perpendicular line, L20...perpendicular line, L3...perpendicular line, L30...perpendicular line, S0...horizontal surface, S2...surface, S3...surface, S15...top surface, S201...bottom surface, S202...closed surface, S301...tip surface, S600...top surface, W1...workpiece, WC...cam portion, ct1...cutting line, ct2...cutting line, n600...work table, wd1...width
Claims
1. A method for manufacturing a grindstone in which a plurality of cylindrical grindstone portions are fitted in an outer periphery of a columnar grindstone core member and fixed to the outer periphery, the method comprising the steps of: (a) preparing a plurality of cylindrical grindstone base members which are bases for the plurality of grindstone portions, each of which has a parallelogram shape projected onto a plane parallel to a cross section including a central axis of the grindstone base member; (b) fitting a plurality of the grindstone base members to the outer periphery of the grindstone core member in a line in an axial direction thereof such that a distance between opposing end faces of two adjacent grindstone base members is constant over the entire circumference; (c) fixing a plurality of the wheel base members to the outer periphery; (d) removing and shaping the ends of each of the plurality of grindstone base members located at both ends in the axial direction of the grindstone core member, thereby shaping both end faces of the plurality of grindstone base members as a whole into surfaces perpendicular to the axial direction; Equipped with The step (a) (a1) preparing a first mold that forms a cylindrical internal space and has one axial end of the internal space closed and the other axial end open, and a second mold that has a fitting portion that is fitted into the internal space from the other end; (a2) placing the first die in a predetermined orientation and filling the internal space with a grinding wheel material including abrasive grains and a binder; (a3) fitting the second die into the internal space to compress the grindstone material filled in the internal space; having In the first mold, a closing surface that closes the one end of the internal space is inclined at a predetermined angle different from 90 degrees with respect to an axial direction of the internal space, In the fitting portion, a tip surface on a tip side that is fitted into the internal space is inclined at the predetermined angle with respect to an axial direction of the internal space, The step (a3) includes a step of fitting the second mold into the internal space so that the tip surface is parallel to the closing surface. Manufacturing method of grinding wheels.
2. The method for manufacturing a grindstone according to claim 1, The predetermined orientation is an orientation in which the occlusion surface is parallel to a horizontal plane. Manufacturing method of grinding wheels.
Citation Information
Patent Citations
JP1981094265U
The wide wheel
JP1983070868U
Grinding wheel
JP1988074570A
Polishing method and grinding tool for polishing
JP2005329518A
Cylindrical resin grinding wheel and its manufacturing method
JP2008221430A