Toner, developer, toner storage unit and image forming apparatus
A toner with a core-shell structure and specific glass transition temperatures addresses the challenge of achieving both low-temperature fixability and heat-resistant storage stability, enhancing image quality by preventing abnormal images and adhesion issues.
Patent Information
- Application Number
- JP2020215476
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-24
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-12-24
AI Technical Summary
Existing toners fail to achieve both high levels of low-temperature fixability and heat-resistant storage stability, leading to issues such as abnormal images due to insufficient fluidity or chargeability, and adhesion to charging members.
A toner with a core-shell structure containing polyester resin-based toner base particles and organic fine particles as external additives, where the organic fine particles are partially buried and have a specific particle size distribution, ensuring optimal glass transition temperatures for both fixability and storage stability.
The toner achieves excellent low-temperature fixability and heat-resistant storage stability, preventing abnormal images by maintaining sufficient fluidity and chargeability while minimizing adhesion to charging members.
Smart Images

Figure 0007581851000004 
Figure 0007581851000005 
Figure 0007581851000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a toner, a developer, a toner storage unit, and an image forming apparatus. [Background technology]
[0002] Image forming devices using toner, such as multi-function peripherals (MFPs) and printers, are widely used in various places, including offices. Toner is required to have low-temperature fixing property and heat-resistant storage property in order to reduce power consumption during fixing to save energy, and to improve resistance to high temperatures and high humidity during storage and transportation after production.
[0003] As a toner having low-temperature fixing property and heat-resistant storage stability, for example, a toner containing a polyester resin and having a glass transition temperature Tg1st of 45°C to 65°C in the first temperature rise of differential scanning calorimetry (DSC) is disclosed (see, for example, Patent Document 1). In the toner of Patent Document 1, the glass transition temperatures Tg1st of the components insoluble in tetrahydrofuran in the first temperature rise of DSC are -45°C to 5°C and 45°C to 70°C, and the glass transition temperature Tg2nd of the components soluble in tetrahydrofuran in the second temperature rise of DSC is 40°C to 65°C. Summary of the Invention [Problem to be solved by the invention]
[0004] However, the toner described in Patent Document 1 was insufficient to achieve both low-temperature fixability and heat-resistant storage stability, which are required at a high level in recent years. Patent Document 1 also describes that at least a part of the surface of the toner is coated with an additive to impart fluidity and chargeability to the toner, but does not describe the use of organic fine particles. When organic fine particles are used as an external additive, if the external additive is buried too deeply in the surface of the toner so that it does not separate, the toner may not be imparted with sufficient fluidity or chargeability, and abnormal images may be easily generated due to transfer failure. In addition, if the external additive is easily separated from the surface of the toner, it may adhere to a charging member such as a photoconductor drum (filming), degrading image quality and making it easier for abnormal images to occur.
[0005] An object of one aspect of the present invention is to provide a toner that has excellent low-temperature fixability and heat-resistant storage stability and is capable of suppressing the occurrence of abnormal images. [Means for solving the problem]
[0006] One embodiment of the toner according to the present invention is a toner containing toner base particles containing a polyester resin and an external additive attached to the surface of the toner base particles, the external additive containing a plurality of organic fine particles arranged in a state where at least a part of the organic fine particles is embedded in the surface of the toner base particles, the particle size distribution of the organic fine particles has two or more peaks, and the glass transition temperature Tg 1st is 30°C to 60°C, and the glass transition temperature Tga of the component of the toner that is insoluble in tetrahydrofuran at the first temperature rise measured by differential scanning calorimetry 1st is -40°C to 10°C, and the glass transition temperature Tg 2nd However, the temperature range is 45℃~65℃. Effect of the Invention
[0007] According to one aspect of the present invention, there is provided a toner which has excellent low-temperature fixing property and heat-resistant storage stability and is capable of suppressing the occurrence of abnormal images. [Brief description of the drawings]
[0008] [Figure 1] FIG. 2 is a diagram showing a DSC curve. [Diagram 2] 3A and 3B are schematic diagrams illustrating an example of a surface state of a toner base particle. [Diagram 3] FIG. 1 is a schematic diagram illustrating an example of an image forming apparatus according to an embodiment. [Figure 4] FIG. 2 is a schematic diagram illustrating an example of a process cartridge according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, the embodiments of the present invention will be described in detail. Note that the embodiments are not limited by the following description, and can be modified as appropriate without departing from the gist of the present invention. In addition, in this specification, a tilde "~" indicating a numerical range means that the numerical values before and after it are included as the lower and upper limits, unless otherwise specified.
[0010] <Toner> The toner according to one embodiment comprises toner base particles containing a polyester resin as a binder resin, and an external additive attached to the surface of the toner base particles, and contains a plurality of organic fine particles as the external additive, the organic fine particles being disposed in a state in which at least a portion of the particles is embedded in the surface of the toner base particles. The toner according to one embodiment has a core-shell structure in which at least a portion of the surface of the toner base particles is coated with a plurality of organic fine particles as the external additive.
[0011] The toner according to the embodiment includes organic fine particles present as an external additive in a state where at least a part of the particles is embedded in the surface of the toner base particles, and the particle size distribution of the organic fine particles has two or more peaks. 1stThe glass transition temperature Tga of the component insoluble in tetrahydrofuran (THF) of the toner according to one embodiment at the first temperature rise measured by DSC is 30° C. to 60° C. 1st The glass transition temperature (Tg) of the THF-soluble component in the second heating cycle measured by DSC is -40°C to 10°C. 2nd The glass transition temperature Tg of the toner is 45° C. to 65° C. Since the organic fine particles have two or more different particle size distributions, even if the organic fine particles cover at least a part of the surface of the toner base particles, the toner does not become impeded in fixing, and the toner according to the embodiment can have adhesion and storage stability. 1st , the glass transition temperature Tga of the component insoluble in THF 1st , and the glass transition temperature Tg of the THF-soluble component 2nd However, if each of these is within the above range, the toner can have sufficient fluidity and chargeability, so that the toner can suppress transfer defects. In addition, since the external additive is less likely to separate from the surface of the toner, it is possible to suppress the deterioration of image quality due to adhesion (filming) to a charging member such as a photoconductor drum. Therefore, the toner according to one embodiment can achieve both low-temperature fixability and heat-resistant storage stability at a high level, and the liberation rate of the external additive can be set within an optimal range, so that the occurrence of abnormal images can be suppressed.
[0012] Glass transition temperature Tg of the toner according to an embodiment 1st , the glass transition temperature Tga of the THF-insoluble component (THF-insoluble matter) 1st , the glass transition temperature Tg of the THF-soluble component 2nd can be measured as follows:
[0013] For example, 1 g of toner is put into 100 mL of THF, and Soxhlet extraction is performed to obtain THF-soluble and insoluble fractions. These are then dried in a vacuum dryer for 24 hours to obtain modified polyester resin from the THF-soluble fraction and amorphous polyester resin from the THF-insoluble fraction. These are used as the target samples. The glass transition temperature Tg 1st When measuring, a toner is used as a target sample.
[0014] Next, about 5.0 mg of the target sample is placed in an aluminum sample container, the sample container is placed on a holder unit, and set in an electric furnace. Next, in a nitrogen atmosphere, the sample is heated from -80°C to 150°C at a heating rate of 1.0°C / min (first heating). After that, the sample is cooled from 150°C to -80°C at a heating rate of 1.0°C / min, and further heated to 150°C at a heating rate of 1.0°C / min (second heating). During each of the first and second heating, a DSC curve is measured using a differential scanning calorimeter ("Q-200", manufactured by TA Instruments).
[0015] From the obtained DSC curves, the DSC curve at the first heating was selected using the analysis program in the Q-200 system, and the glass transition temperature Tg at the first heating of the target sample was calculated. 1st Request.
[0016] Similarly, select the DSC curve during the second heating and measure the glass transition temperature (Tg) of the sample during the second heating. 2nd Request.
[0017] Furthermore, from the obtained DSC curves, the analysis program in the Q-200 system can be used to select the DSC curve during the first heating and determine the endothermic peak top temperature during the first heating of the target sample as the melting point. Similarly, the DSC curve during the second heating can be selected and the endothermic peak top temperature during the second heating of the target sample as the melting point.
[0018] In addition, unless otherwise specified, the melting points and glass transition temperatures (Tg) of other components such as modified polyester resin, amorphous polyester resin, and release agent are the endothermic peak top temperatures and glass transition temperatures (Tg) of the second heating. 2nd are the melting point and glass transition temperature Tg of each sample.
[0019] The toner components that are insoluble in THF are heated from -80°C to 150°C at a temperature rise rate of 1.0°C / min using the modulation mode with a modulation temperature amplitude of ±1.0°C / min (first temperature rise). The obtained DSC curve is then obtained by plotting "Reversing Heat Flow" on the vertical axis using the analysis program in the Q-200 system in the same manner as above, and the onset value shown in Figure 1 is taken as the glass transition temperature Tg. This gives the glass transition temperature Tga 1st and Tg 2nd You may ask for:
[0020] [Toner base particles] As described above, the toner base particles contain a binder resin.
[0021] (Binding resin) The binder resin contains a polyester resin as a main component. The polyester resin is preferable because it can impart flexibility to the toner. In addition to the polyester resin, the binder resin may contain, for example, a styrene-acrylic resin, a polyol resin, a vinyl resin, a polyurethane resin, an epoxy resin, a polyamide resin, a polyimide resin, a silicon resin, a phenol resin, a melamine resin, a urea resin, an aniline resin, an ionomer resin, a polycarbonate resin, etc. These may be used alone or in combination of two or more.
[0022] ((Polyester resin)) The polyester resin is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include crystalline polyester resins, amorphous polyester resins, modified polyester resins, etc. These may be used alone or in combination of two or more.
[0023] The polyester resin may contain at least a trivalent or tetravalent aliphatic polyhydric alcohol component having 3 to 10 carbon atoms.
[0024] The polyester resin contains a diol component, and the diol component may contain a resin having an odd carbon number of 3 to 9 in the main chain portion and having an alkyl group in the side chain.
[0025] The polyester resin preferably contains at least one of a urethane bond and a urea bond, whereby the urethane bond or the urea bond in the polyester resin behaves like a pseudo-crosslinking point, and the polyester resin has strong rubber-like properties, resulting in more excellent heat-resistant storage stability and high-temperature offset resistance of the toner.
[0026] -Crystalline polyester- The polyester resin preferably contains a crystalline polyester. The crystalline polyester has high crystallinity and therefore exhibits a thermal melting characteristic in which the viscosity drops sharply near the fixing start temperature. By using a crystalline polyester resin having such characteristics together with an unmodified polyester resin, the heat-resistant storage stability due to the crystallinity is good up to just before the melting start temperature, and a sharp viscosity drop (sharp melt) can be caused by the melting of the crystalline polyester resin at the melting start temperature. In addition, the crystalline polyester resin is compatible with the polyester resin and is fixed by a sharp drop in viscosity, so that a toner having both good heat-resistant storage stability and low-temperature fixing ability can be obtained. In addition, the release width (the difference between the minimum fixing temperature and the high-temperature offset occurrence temperature) also shows good results.
[0027] The crystalline polyester resin (also referred to as crystalline polyester) is not particularly limited and can be appropriately selected depending on the purpose. For example, a crystalline polyester resin obtained by reacting a polyol with a polycarboxylic acid can be mentioned.
[0028] In this embodiment, the crystalline polyester resin refers to a resin obtained by reacting a polyol with a polycarboxylic acid as described above, and modified polyester resins, such as prepolymers and resins obtained by subjecting the prepolymers to a crosslinking and / or elongation reaction, do not belong to the crystalline polyester resins.
[0029] --Polyol-- The polyol is not particularly limited and can be appropriately selected depending on the purpose. Examples of the polyol include diols and trihydric or higher polyols.
[0030] The diol includes, for example, saturated aliphatic diols. Examples of the saturated aliphatic diol include linear saturated aliphatic diols and branched saturated aliphatic diols. These may be used alone or in combination of two or more. Among these, linear saturated aliphatic diols are preferred, and linear saturated aliphatic diols having a carbon number of 2 to 12 are more preferred, because they can improve crystallinity and prevent a decrease in melting point.
[0031] Examples of saturated aliphatic diols include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, and 1,14-eicosanediol. Among these, ethylene glycol, 1,4-butanediol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, and 1,12-dodecanediol are preferred because the crystalline polyester resin has high crystallinity and excellent sharp melting properties.
[0032] Examples of trihydric or higher alcohols include glycerin, trimethylolethane, trimethylolpropane, and pentaerythritol.
[0033] --Polycarboxylic acids-- The polycarboxylic acid is not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include divalent carboxylic acids and trivalent or higher carboxylic acids.
[0034] Examples of the divalent carboxylic acid include saturated aliphatic dicarboxylic acids such as oxalic acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, and 1,18-octadecanedicarboxylic acid; and aromatic dicarboxylic acids such as dibasic acids such as phthalic acid, isophthalic acid, terephthalic acid, naphthalene-2,6-dicarboxylic acid, malonic acid, and mesaconic acid; and further, anhydrides of these acids and lower (carbon number: 1 to 3) alkyl esters of these acids.
[0035] Examples of trivalent or higher carboxylic acids include 1,2,4-benzenetricarboxylic acid, 1,2,5-benzenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, and anhydrides and lower (carbon number 1 to 3) alkyl esters of these.
[0036] The polycarboxylic acid may contain a dicarboxylic acid having a sulfonic acid group in addition to a saturated aliphatic dicarboxylic acid or an aromatic dicarboxylic acid, and may further contain a dicarboxylic acid having a double bond in addition to a saturated aliphatic dicarboxylic acid or an aromatic dicarboxylic acid. These may be used alone or in combination of two or more.
[0037] The crystalline polyester resin is preferably composed of a linear saturated aliphatic dicarboxylic acid having 4 to 12 carbon atoms and a linear saturated aliphatic diol having 2 to 12 carbon atoms. That is, the crystalline polyester resin preferably has a constitutional unit derived from a saturated aliphatic dicarboxylic acid having 4 to 12 carbon atoms and a constitutional unit derived from a saturated aliphatic diol having 2 to 12 carbon atoms. This is preferable in that the resin has high crystallinity and excellent sharp melting properties, and can therefore exhibit excellent low-temperature fixability.
[0038] The presence or absence of crystallinity of the crystalline polyester resin can be confirmed by a crystal analysis X-ray diffraction device (for example, X'Pert Pro MRD, manufactured by Philips). The measurement method is described below.
[0039] First, the target sample is ground in a mortar to prepare a powdered sample, and the powdered sample is evenly applied to a sample holder.Then, the sample holder is set in the diffraction device, and measurements are performed to obtain a diffraction spectrum.
[0040] When the half-width of the peak with the greatest intensity among the diffraction peaks obtained in the range of 20°<2θ<25° is 2.0 or less, it is determined to have crystallinity.
[0041] In contrast to crystalline polyester resins, polyester resins that do not exhibit the above-mentioned state are referred to as amorphous polyester resins in this embodiment. The measurement conditions for X-ray diffraction are described below. ( Measurement conditions ) Tension kV: 45kV Current: 40mA ·MPSS Upper Gonio Scan mode: continuous Starting angle: 3° End angle: 35° Angle Step: 0.02° Lucident beam optics ·Divergence slit: Div slit 1 / 2 Diffraction beam optics ·Anti scatter slit: As Fixed 1 / 2 ·Receiving slit: Prog rec slit
[0042] The melting point of the crystalline polyester resin is not particularly limited and can be appropriately selected depending on the purpose, but is preferably from 60° C. to 80° C. If the melting point is 60° C. or higher, the crystalline polyester resin is easily melted at low temperatures, and the problem of the heat-resistant storage stability of the toner decreasing can be prevented, while if the melting point is 80° C. or lower, the problem of the crystalline polyester resin not melting sufficiently due to heating during fixing, and the problem of the low-temperature fixability decreasing can be prevented.
[0043] The molecular weight of the crystalline polyester resin is not particularly limited and can be appropriately selected depending on the purpose.
[0044] The orthodichlorobenzene soluble portion of the crystalline polyester resin preferably has a weight average molecular weight (Mw) of 3,000 to 30,000, more preferably 5,000 to 15,000, as measured by GPC.
[0045] The orthodichlorobenzene soluble portion of the crystalline polyester resin preferably has a number average molecular weight (Mn) of 1,000 to 10,000, more preferably 2,000 to 10,000, as measured by GPC.
[0046] The molecular weight ratio Mw / Mn of the crystalline polyester resin is preferably from 1.0 to 10, and more preferably from 1.0 to 5.0.
[0047] This is because a toner having a sharp molecular weight distribution and a low molecular weight has excellent low-temperature fixability, and the high heat-resistant storage stability is reduced when there are a lot of low-molecular weight components.
[0048] The acid value of the crystalline polyester resin is not particularly limited and can be appropriately selected depending on the purpose, but from the viewpoint of affinity between paper and resin, in order to achieve the desired low-temperature fixability, it is preferably 5 mgKOH / g or more, more preferably 10 mgKOH / g or more, while in order to improve high-temperature offset resistance, it is preferably 45 mgKOH / g or less.
[0049] The hydroxyl value of the crystalline polyester resin is not particularly limited and can be appropriately selected depending on the purpose. In order to achieve the desired low-temperature fixability and good charging characteristics, the hydroxyl value is preferably 0 mgKOH / g to 50 mgKOH / g, and more preferably 5 mgKOH / g to 50 mgKOH / g.
[0050] The molecular structure of the crystalline polyester resin can be confirmed by NMR measurement in solution or solid, as well as X-ray diffraction, GC / MS, LC / MS, IR measurement, etc. -1 Or 990±10cm -1 One method is to detect a crystalline polyester resin that has absorption based on the δCH (out-of-plane bending vibration) of olefin.
[0051] The content of the crystalline polyester resin is not particularly limited and can be appropriately selected according to the purpose, but is preferably 3 to 20 parts by mass, more preferably 5 to 15 parts by mass, relative to 100 parts by mass of the toner. If the content is 3 parts by mass or more, the problem of poor low-temperature fixability due to insufficient sharp melting by the crystalline polyester resin can be prevented. Also, if the content is 20 parts by mass or less, the problem of reduced heat-resistant storage stability and image fogging can be prevented.
[0052] -Amorphous polyester resin- The polyester resin preferably contains an amorphous polyester resin (also called an amorphous polyester resin or an unmodified polyester resin). The amorphous polyester resin is a polyester resin obtained by using a polyhydric alcohol and a polycarboxylic acid or a derivative thereof, such as a polycarboxylic acid, a polycarboxylic acid anhydride, or a polycarboxylic acid ester, and is not modified by an isocyanate compound or the like.
[0053] The amorphous polyester resin is not particularly limited and may be appropriately selected depending on the purpose. For example, there may be mentioned an amorphous polyester resin obtained by reacting a polyol with a polycarboxylic acid.
[0054] In the present embodiment, the amorphous polyester resin refers to a resin obtained by reacting a polyol with a polycarboxylic acid as described above. In the present embodiment, modified polyester resins, such as prepolymers described below and modified polyester resins obtained by crosslinking and / or elongating the prepolymers, are not included in the amorphous polyester resins and are treated as modified polyester resins.
[0055] The amorphous polyester resin is a polyester resin that is soluble in THF.
[0056] As the amorphous polyester, a linear polyester resin is preferred.
[0057] The polyol includes, for example, a diol.
[0058] Examples of diols include alkylene (carbon number 2-3) oxide (average added mole number 1-10) adducts of bisphenol A such as polyoxypropylene (2.2)-2,2-bis(4-hydroxyphenyl)propane and polyoxyethylene (2.2)-2,2-bis(4-hydroxyphenyl)propane; ethylene glycol, propylene glycol; hydrogenated bisphenol A, and alkylene (carbon number 2-3) oxide (average added mole number 1-10) adducts of hydrogenated bisphenol A. These may be used alone or in combination of two or more. Among these, it is preferable that the polyol contains 40 mol % or more of alkylene glycol.
[0059] The polycarboxylic acid may, for example, be a dicarboxylic acid.
[0060] Examples of dicarboxylic acids include adipic acid, phthalic acid, isophthalic acid, terephthalic acid, fumaric acid, maleic acid, dodecenylsuccinic acid, octylsuccinic acid, and other alkyl groups having 1 to 20 carbon atoms; succinic acid substituted with an alkenyl group having 2 to 20 carbon atoms. These may be used alone or in combination of two or more. Among these, the polycarboxylic acid preferably contains 50 mol % or more of terephthalic acid.
[0061] The amorphous polyester resin may contain a trivalent or higher carboxylic acid and / or a trivalent or higher alcohol, a trivalent or higher epoxy compound, etc. at the end of the resin chain in order to adjust the acid value and hydroxyl value.
[0062] Among these, it is preferable to contain a trihydric or higher aliphatic alcohol, from the viewpoint of preventing unevenness and obtaining sufficient gloss and image density.
[0063] Examples of the trivalent or higher carboxylic acid include trimellitic acid, pyromellitic acid, and acid anhydrides thereof.
[0064] Examples of trihydric or higher alcohols include glycerin, pentaerythritol, and trimethylolpropane.
[0065] The molecular weight of the amorphous polyester resin is not particularly limited and can be appropriately selected depending on the purpose, but is preferably in the following range.
[0066] The weight average molecular weight Mw of the amorphous polyester resin is preferably from 3,000 to 10,000, and more preferably from 4,000 to 7,000.
[0067] The number average molecular weight Mn of the amorphous polyester resin is preferably 1,000 to 4,000, and more preferably 1,500 to 3,000.
[0068] The molecular weight ratio (Mw / Mn) of the amorphous polyester resin is preferably from 1.0 to 4.0, and more preferably from 1.0 to 3.5.
[0069] The weight average molecular weight and the number average molecular weight can be measured, for example, by GPC (gel permeation chromatography).
[0070] The reason why the weight average molecular weight and number average molecular weight are preferred within the above ranges is that if the weight average molecular weight and number average molecular weight are too low, the toner may be inferior in heat resistant storage stability and durability against stress such as stirring in a developing machine, while if the weight average molecular weight and number average molecular weight are too high, the viscoelasticity of the toner when melted may increase and low-temperature fixability may be poor. Also, if there is too much of the component having a molecular weight of 600 or less, the toner may be inferior in heat resistant storage stability and durability against stress such as stirring in a developing machine, while if there is too little of the component having a molecular weight of 600 or less, the low-temperature fixability may be poor.
[0071] The THF soluble component having a molecular weight of 600 or less is preferably 2% by mass to 10% by mass. As a method for adjusting the content of this component, a method of extracting the amorphous polyester resin with methanol, removing the components having a molecular weight of 600 or less, and purifying the resin can be mentioned.
[0072] The acid value of the amorphous polyester resin is not particularly limited and can be appropriately selected according to the purpose, but is preferably 1 mgKOH / g to 50 mgKOH / g, more preferably 5 mgKOH / g to 30 mgKOH / g. If the acid value is 1 mgKOH / g or more, the toner tends to be negatively charged, and furthermore, the affinity between the paper and the toner is improved when fixing to the paper, and low-temperature fixing property can be improved. On the other hand, if the acid value is 50 mgKOH / g or less, the problem of the charging stability, particularly the charging stability against environmental changes, decreasing can be prevented.
[0073] The hydroxyl value of the amorphous polyester resin is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 5 mgKOH / g or more.
[0074] The glass transition temperature Tg of the amorphous polyester resin is preferably 40° C. to 65° C., more preferably 45° C. to 65° C., and even more preferably 50° C. to 60° C. If the Tg is 40° C. or higher, the toner has improved heat-resistant storage stability and durability against stress such as stirring in a developing machine, and also has improved filming resistance. On the other hand, if the Tg is 65° C. or lower, the toner is less susceptible to deformation due to heat and pressure during fixing, and low-temperature fixing ability is improved.
[0075] The content of the amorphous polyester resin is preferably 80 parts by mass to 90 parts by mass with respect to 100 parts by mass of the toner.
[0076] -Modified polyester resin- The modified polyester resin (also referred to as modified polyester) is not particularly limited and can be appropriately selected depending on the purpose. For example, there is a reaction product between an active hydrogen group-containing compound and a polyester resin (also referred to as a prepolymer or polyester prepolymer) having a site capable of reacting with the active hydrogen group-containing compound.
[0077] Modified polyester is a polyester resin that is insoluble in THF. The polyester resin component that is insoluble in THF lowers the glass transition temperature Tg and melt viscosity, and ensures low-temperature fixability. At the same time, it has a branched structure in the molecular skeleton, and the molecular chain has a three-dimensional network structure, so it has rubber-like properties in that it deforms at low temperatures but does not flow.
[0078] Since polyester resin C has an active hydrogen group-containing compound and a site capable of reacting with an active hydrogen group-containing compound, these sites behave like pseudo-crosslinking points, enhancing the rubber-like properties of amorphous polyester resin A, enabling the production of a toner with excellent heat resistance, storage stability, and high-temperature offset resistance.
[0079] --Compounds containing active hydrogen groups-- The active hydrogen group-containing compound is a compound that reacts with a polyester resin having a site capable of reacting with the active hydrogen group-containing compound.
[0080] The active hydrogen group is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include a hydroxyl group (alcoholic hydroxyl group and phenolic hydroxyl group), an amino group, a carboxyl group, a mercapto group, etc. These may be used alone or in combination of two or more kinds.
[0081] The active hydrogen group-containing compound is not particularly limited and can be appropriately selected depending on the purpose. However, when the polyester resin having a site capable of reacting with the active hydrogen group-containing compound is a polyester resin containing an isocyanate group, amines are preferred in that they can increase the molecular weight of the polyester resin by elongation reaction, crosslinking reaction, or the like with the polyester resin.
[0082] The amines are not particularly limited and can be appropriately selected according to the purpose, and examples thereof include diamines, trivalent or higher amines, amino alcohols, amino mercaptans, amino acids, and blocked amino groups thereof. These may be used alone or in combination of two or more. Among these, diamines and mixtures of diamines and small amounts of trivalent or higher amines are preferred.
[0083] The diamine is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include aromatic diamines, alicyclic diamines, and aliphatic diamines. The aromatic diamine is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include phenylenediamine, diethyltoluenediamine, and 4,4'-diaminodiphenylmethane. The alicyclic diamine is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include 4,4'-diamino-3,3'-dimethyldicyclohexylmethane, diaminocyclohexane, and isophoronediamine. The aliphatic diamine is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include ethylenediamine, tetramethylenediamine, and hexamethylenediamine.
[0084] The trivalent or higher amine is not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include diethylenetriamine and triethylenetetramine.
[0085] The amino alcohol is not particularly limited and can be appropriately selected depending on the purpose. Examples of the amino alcohol include ethanolamine and hydroxyethylaniline.
[0086] The amino mercaptan is not particularly limited and can be appropriately selected depending on the purpose. Examples of the amino mercaptan include aminoethyl mercaptan and aminopropyl mercaptan.
[0087] The amino acid is not particularly limited and can be appropriately selected depending on the purpose. Examples of the amino acid include aminopropionic acid and aminocaproic acid.
[0088] The blocked amino group is not particularly limited and can be appropriately selected depending on the purpose. Examples of the blocked amino group include ketimine compounds and oxazoline compounds obtained by blocking the amino group with ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone.
[0089] --Polyester resin having a site capable of reacting with an active hydrogen group-containing compound-- The polyester resin having a site capable of reacting with an active hydrogen group-containing compound is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include polyester resins containing isocyanate groups (also called polyester prepolymers having isocyanate groups). The polyester resins containing isocyanate groups are not particularly limited and can be appropriately selected according to the purpose, and examples thereof include reaction products of polyester resins having active hydrogen groups obtained by polycondensation of polyols and polycarboxylic acids and polyisocyanates.
[0090] The polyol is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include diols, trihydric or higher alcohols, and mixtures of diols and trihydric or higher alcohols. These may be used alone or in combination of two or more. Among these, diols and mixtures of diols and a small amount of trihydric or higher alcohols are preferred.
[0091] The diol is not particularly limited and can be appropriately selected depending on the purpose. Examples of the diol include linear alkylene glycols, diols having an oxyalkylene group, alicyclic diols, bisphenols, alkylene oxide adducts of alicyclic diols, and alkylene oxide adducts of bisphenols.
[0092] Examples of the chain alkylene glycol include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, and 1,6-hexanediol.
[0093] Examples of diols having an oxyalkylene group include diethylene glycol, triethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, and polytetramethylene glycol.
[0094] Examples of the alicyclic diol include 1,4-cyclohexanedimethanol, hydrogenated bisphenol A, and the like.
[0095] Examples of bisphenols include bisphenol A, bisphenol F, and bisphenol S.
[0096] Examples of the alkylene oxide include ethylene oxide, propylene oxide, and butylene oxide.
[0097] The number of carbon atoms of the chain alkylene glycol is not particularly limited and can be appropriately selected depending on the purpose, but 2 to 12 is preferable.
[0098] Among these, at least any one of a chain alkylene glycol having 2 to 12 carbon atoms and an alkylene oxide adduct of a bisphenol is preferred, and an alkylene oxide adduct of a bisphenol and a mixture of an alkylene oxide adduct of a bisphenol and a chain alkylene glycol having 2 to 12 carbon atoms are more preferred.
[0099] The trihydric or higher alcohol is not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include trihydric or higher aliphatic alcohols, trihydric or higher polyphenols, and alkylene oxide adducts of trihydric or higher polyphenols.
[0100] The trihydric or higher aliphatic alcohol is not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, and sorbitol.
[0101] The trivalent or higher polyphenols are not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include trisphenol PA, phenol novolac, and cresol novolac.
[0102] Examples of the alkylene oxide adducts of trivalent or higher polyphenols include those obtained by adding alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide to trivalent or higher polyphenols.
[0103] When a diol and a trihydric or higher alcohol are used in combination, the mass ratio of the trihydric or higher alcohol to the diol (trihydric or higher alcohol / diol) is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.01% by mass to 10% by mass, and more preferably 0.01% by mass to 1% by mass.
[0104] The polycarboxylic acid is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include dicarboxylic acids, trivalent or higher carboxylic acids, and mixtures of dicarboxylic acids and trivalent or higher carboxylic acids. These may be used alone or in combination of two or more. Among these, dicarboxylic acids and mixtures of dicarboxylic acids and a small amount of trivalent or higher polycarboxylic acids are preferred.
[0105] The dicarboxylic acid is not particularly limited and can be appropriately selected depending on the purpose. Examples of the dicarboxylic acid include divalent alkanoic acids, divalent alkenoic acids, and aromatic dicarboxylic acids.
[0106] The divalent alkanoic acid is not particularly limited and can be appropriately selected depending on the purpose. Examples of the divalent alkanoic acid include succinic acid, adipic acid, and sebacic acid.
[0107] The divalent alkenoic acid is not particularly limited and can be appropriately selected depending on the purpose, but is preferably a divalent alkenoic acid having 4 to 20 carbon atoms. The divalent alkenoic acid having 4 to 20 carbon atoms is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include maleic acid and fumaric acid.
[0108] The aromatic dicarboxylic acid is not particularly limited and can be appropriately selected depending on the purpose, but is preferably an aromatic dicarboxylic acid having 8 to 20 carbon atoms. The aromatic dicarboxylic acid having 8 to 20 carbon atoms is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include phthalic acid, isophthalic acid, terephthalic acid, and naphthalenedicarboxylic acid.
[0109] The tri- or higher carboxylic acid is not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include tri- or higher carboxylic acids.
[0110] The trivalent or higher aromatic carboxylic acid is not particularly limited and can be appropriately selected depending on the purpose, but is preferably a trivalent or higher aromatic carboxylic acid having 9 to 20 carbon atoms. The trivalent or higher aromatic carboxylic acid having 9 to 20 carbon atoms is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include trimellitic acid and pyromellitic acid.
[0111] As the polycarboxylic acid, anhydrides or lower alkyl esters of any of dicarboxylic acids, tri- or higher carboxylic acids, and mixtures of dicarboxylic acids and tri- or higher carboxylic acids can also be used.
[0112] The lower alkyl ester is not particularly limited and can be appropriately selected depending on the purpose. Examples of the lower alkyl ester include methyl ester, ethyl ester, and isopropyl ester.
[0113] When a dicarboxylic acid and a tri- or higher carboxylic acid are used in combination, the mass ratio of the tri- or higher carboxylic acid to the dicarboxylic acid (tri- or higher carboxylic acid / dicarboxylic acid) is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.01% by mass to 10% by mass, and more preferably 0.01% by mass to 1% by mass.
[0114] When polyol and polycarboxylic acid are polycondensed, the equivalent ratio of the hydroxyl groups of the polyol to the carboxyl groups of the polycarboxylic acid (hydroxyl groups of the polyol / carboxyl groups of the polycarboxylic acid) is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1 to 2, more preferably 1 to 1.5, and particularly preferably 1.02 to 1.3.
[0115] The content of the polyol-derived structural unit in the polyester prepolymer having an isocyanate group is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.5% by mass to 40% by mass, more preferably 1% by mass to 30% by mass, and particularly preferably 2% by mass to 20% by mass. If the content is less than 0.5% by mass, the hot offset resistance may decrease, making it difficult to achieve both the heat-resistant storage stability and low-temperature fixability of the toner, and if it exceeds 40% by mass, the low-temperature fixability may decrease.
[0116] The polyisocyanate is not particularly limited and can be appropriately selected depending on the purpose. Examples of the polyisocyanate include aliphatic diisocyanates, alicyclic diisocyanates, aromatic diisocyanates, araliphatic diisocyanates, isocyanurates, and those blocked with phenol derivatives, oximes, caprolactam, etc.
[0117] The aliphatic diisocyanate is not particularly limited and can be appropriately selected depending on the purpose. Examples of the aliphatic diisocyanate include tetramethylene diisocyanate, hexamethylene diisocyanate, methyl 2,6-diisocyanatocaproate, octamethylene diisocyanate, decamethylene diisocyanate, dodecamethylene diisocyanate, tetradecamethylene diisocyanate, trimethylhexane diisocyanate, and tetramethylhexane diisocyanate.
[0118] The alicyclic diisocyanate is not particularly limited and can be appropriately selected depending on the purpose. Examples of the alicyclic diisocyanate include isophorone diisocyanate and cyclohexylmethane diisocyanate.
[0119] The aromatic diisocyanate is not particularly limited and can be appropriately selected depending on the purpose. Examples of the aromatic diisocyanate include tolylene diisocyanate, diisocyanatodiphenylmethane, 1,5-naphthylene diisocyanate, 4,4'-diisocyanatodiphenyl, 4,4'-diisocyanato-3,3'-dimethyldiphenyl, 4,4'-diisocyanato-3-methyldiphenylmethane, and 4,4'-diisocyanato-diphenyl ether.
[0120] The aromatic aliphatic diisocyanate is not particularly limited and can be appropriately selected depending on the purpose. For example, α,α,α',α'-tetramethylxylylene diisocyanate is etc.
[0121] The isocyanurates are not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include tris(isocyanatoalkyl)isocyanurate, tris(isocyanatocycloalkyl)isocyanurate, etc. These may be used alone or in combination of two or more kinds.
[0122] When reacting a polyisocyanate with a polyester resin having a hydroxyl group, the equivalent ratio (NCO / OH) of the isocyanate group of the polyisocyanate to the hydroxyl group of the polyester resin is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1 to 5, more preferably 1.2 to 4, and particularly preferably 1.5 to 2.5. If the equivalent ratio is less than 1, the hot offset resistance may decrease, and if it exceeds 5, the low-temperature fixability may decrease.
[0123] The content of the polyisocyanate-derived structural unit in the polyester prepolymer having an isocyanate group is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.5% by mass to 40% by mass, more preferably 1% by mass to 30% by mass, and particularly preferably 2% by mass to 20% by mass. If the content is less than 0.5% by mass, the hot offset resistance may decrease, and if it exceeds 40% by mass, the low-temperature fixability may decrease.
[0124] The average number of isocyanate groups in the polyester prepolymer having an isocyanate group per molecule is not particularly limited and may be appropriately selected depending on the purpose, but is preferably at least 1, more preferably 1.5 to 3, and particularly preferably 1.8 to 2.5. If the average number is less than 1, the molecular weight of the modified polyester resin becomes low, and the hot offset resistance may decrease.
[0125] The modified polyester resin can be produced by a one-shot method, etc. As an example, a method for producing a urea-modified polyester resin will be described.
[0126] First, a polyol and a polycarboxylic acid are heated to 150°C to 280°C in the presence of a catalyst such as tetrabutoxy titanate or dibutyltin oxide, and the water generated is removed while reducing the pressure as necessary to obtain a polyester resin having hydroxyl groups. Next, the polyester resin having hydroxyl groups is reacted with a polyisocyanate at 40°C to 140°C to obtain a polyester prepolymer having an isocyanate group. Furthermore, the polyester prepolymer having an isocyanate group is reacted with amines at 0°C to 140°C to obtain a urea-modified polyester resin.
[0127] The number average molecular weight (Mn) of the modified polyester resin is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1,000 to 10,000, more preferably 1,500 to 6,000, as measured by GPC (gel permeation chromatography).
[0128] The weight average molecular weight of the modified polyester resin is not particularly limited and can be appropriately selected depending on the purpose, but is preferably from 20,000 to 1,000,000 as measured by GPC (gel permeation chromatography).
[0129] If the weight average molecular weight is 20,000 or more, the toner becomes easily fluid at low temperatures, which can prevent problems such as poor heat resistance storage stability and low viscosity when melted, which can prevent problems such as reduced high temperature offset properties.
[0130] When a polyester resin having a hydroxyl group is reacted with a polyisocyanate, and when a polyester prepolymer having an isocyanate group is reacted with an amine, a solvent can be used as necessary.
[0131] The solvent is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include aromatic solvents, ketones, esters, amides, ethers, and other solvents that are inactive to isocyanate groups. Examples of aromatic solvents include toluene and xylene. Examples of ketones include acetone, methyl ethyl ketone, and methyl isobutyl ketone. Examples of esters include ethyl acetate.
[0132] Examples of the amides include dimethylformamide, dimethylacetamide, etc. Examples of the ethers include THF, etc.
[0133] The glass transition temperature of the modified polyester resin is preferably from -60°C to 0°C, and more preferably from -40°C to -20°C.
[0134] If the glass transition temperature is -60°C or higher, the flow of the toner at low temperatures cannot be suppressed, and the problems of deterioration of heat-resistant storage stability and deterioration of filming resistance can be prevented.
[0135] If the glass transition temperature is 0° C. or lower, the toner cannot be sufficiently deformed by the application of heat and pressure during fixing, and the problem of insufficient low-temperature fixing property can be prevented.
[0136] The content of the modified polyester is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1 to 15 parts by mass, and more preferably 5 to 10 parts by mass, in 100 parts by mass of the toner.
[0137] The molecular structure of the amorphous polyester resin can be confirmed by NMR measurement of the solution or solid, as well as X-ray diffraction, GC / MS, LC / MS, IR measurement, etc.
[0138] In the infrared absorption spectrum, the -1 and 990±10cm -1 One method is to detect amorphous polyester resins that do not have absorption due to olefin δCH (out-of-plane bending vibration).
[0139] [External additives] As described above, the external additive contains organic fine particles.
[0140] (Organic fine particles) The organic fine particles are contained in a state where at least a part of them is embedded in the surface of the toner base particle. The organic fine particles are not arranged in a state where they cover the surface of the toner base particle and are layered, but are arranged in a state where they are scattered on the surface of the toner base particle.
[0141] The organic fine particles are preferably one or more kinds of styrene-acrylic resins having at least a carboxylic acid, and are obtained by homopolymerizing or copolymerizing a vinyl monomer.
[0142] In the toner according to one embodiment, the organic fine particles preferably have a peak P1 at the smallest particle size of 10 nm to 40 nm, and a peak P2 at the largest particle size of 30 nm to 100 nm in two or more particle size distributions of the organic fine particles. Peak P1 is preferably 20 nm to 40 nm, and peak P2 is preferably 50 nm to 80 nm. When peaks P1 and P2 are each within the above preferred ranges, good storage stability and low-temperature fixability can be obtained. In addition, by attaching inorganic fine particles such as silica or titanium to the surface of the toner base particles in the gaps generated by the particle size difference of the organic fine particles, the state in which the organic fine particles are attached to the surface of the toner base particles can be stabilized.
[0143] The particle size distribution of the organic fine particles may be the particle size distribution of the organic fine particles present on the surface of the toner base particle, or the particle size distribution of the organic fine particles partially embedded in the surface of the toner base particle, or the particle size distribution of these organic fine particles.
[0144] In this specification, the peak refers to the top of a waveform that appears in a particle size distribution, and the peak of the organic fine particles can be measured, for example, as follows: First, ultrasonic waves are applied to the toner according to one embodiment to remove as much of the external additives adhering to the surfaces of the toner base particles as possible, to make the toner base particles in a state close to that of the toner base particles. [How to separate external additives] (1)[1] Add 50 ml of a 5% aqueous solution containing a surfactant (product name: Noigen ET-165, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) to a 100 ml screw tube, add 3 g of toner to the mixture, and gently move it up and down and left and right. Then, mix it with a ball mill for 30 minutes so that the toner blends with the dispersion solution. [2] Then, using an ultrasonic homogenizer (product name homogenizer, model VCX750, CV33, manufactured by SONICS & MATERIALS LLC), set the output to 40 W and apply ultrasonic energy for 60 minutes. -Ultrasonic conditions- Vibration time: 60 minutes continuous Amplitude: 40W Vibration start temperature: 23±1.5℃. Temperature during vibration: 23±1.5℃ [3] The dispersion liquid is suction filtered using filter paper (product name: Qualitative Filter Paper (No. 2, 110 mm), manufactured by Advantec Toyo Co., Ltd.), washed twice again with ion-exchanged water, filtered, and the liberated additives are removed. After that, the toner base particles are dried.
[0145] (2) The toner obtained in (1) was observed with a scanning electron microscope (SEM). First, the external additives and fillers containing Si were detected by observing the backscattered electron image.
[0146] (3) The image of (1) is binarized using image processing software (ImageJ) to remove external additives and fillers.
[0147] (4) Next, observe the secondary electron image in the same position as in (1). Since organic fine particles cannot be observed in the reflected electron image, but can only be observed in the secondary electron image, compare it with the image obtained in (3) above, and determine that the fine particles present in the areas other than the remaining external additives and filler (areas other than those excluded in (3) above) are organic fine particles, and use image processing software to measure the particle size (particle diameter).
[0148] (5) Count more than 100 particles to obtain a particle size distribution. -Shooting conditions- Scanning electron microscope: SU-8230 Magnification: 35,000x Image capture: SE(L): Secondary electrons, BSE (backscattered electrons) Acceleration voltage: 2.0kV ·Acceleration current: 1.0μA ·Probe current:Normal Focus mode: UHR WD:8.0mm
[0149] In addition, when peaks are close to each other, they can be separated to identify each peak. When a peak is so broad that two peaks cannot be identified, it can be determined that there is only one peak.
[0150] The average distance between adjacent organic fine particles on the surface of the toner base particle is preferably 100 nm or less, more preferably 90 nm or less, and even more preferably 80 nm or less.
[0151] The distance between adjacent organic fine particles is the distance between the centers of the organic fine particles. The center of an organic fine particle refers to the center point of an image of an organic fine particle observed with a scanning electron microscope (SEM). The surface of a toner base particle is not flat but is slightly rounded and curved. Therefore, the distance between organic fine particles is the shortest distance between the organic fine particles on the surface of the toner base particle in an image taken with an SEM.
[0152] FIG. 2 is a schematic diagram showing an example of the surface state of a toner base particle. As shown in FIG. 2, organic fine particles 3 are attached to the surface of a toner base particle 2. The organic fine particles 3 are composed of a core resin (b2) 3-1 and a shell resin (b1) 3-2, which will be described later. C1 and C2 indicate the centers of the organic fine particles 3. M indicates the volume average primary particle diameter of the organic fine particles 3. L indicates the distance between adjacent organic fine particles 3.
[0153] The average distance between adjacent organic fine particles can be determined by removing as much of the external additive as possible using ultrasonic wave to liberate the external additive, bringing the particles closer to the toner base particles, and then determining the average distance between the organic fine particles. -How to separate external additives- [1] Add 50 ml of a 5% by weight aqueous solution containing a surfactant (product name: Noigen ET-165, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) to a 100 ml screw tube, add 3 g of toner to the mixture, and gently move it up and down and left and right. Then, mix with a ball mill for 30 minutes so that the toner blends with the dispersion solution. [2] Then, using an ultrasonic homogenizer (product name homogenizer, model VCX750, CV33, manufactured by SONICS & MATERIALS LLC), set the output to 40 W and apply ultrasonic energy for 60 minutes. -Ultrasonic conditions- Vibration time: 60 minutes continuous ·Amplitude: 40W ·Vibration start temperature: 23±1.5℃ ·Temperature during vibration: 23±1.5℃ [3](1) The dispersion liquid is suction filtered using filter paper (product name: Qualitative Filter Paper (No. 2, 110 mm), manufactured by Advantec Toyo Co., Ltd.), washed twice again with ion-exchanged water, filtered, and the liberated additives are removed, and the toner particles are then dried. (2) The toner obtained in (1) is observed with a scanning electron microscope (SEM). First, external additives and fillers containing Si are detected by observing the backscattered electron image. (3) The image of (1) is binarized using image processing software (ImageJ) to remove the external additives and fillers. Next, a secondary electron image is observed at the same position as in (1). Since organic fine particles cannot be observed in the reflected electron image, but can only be observed in the secondary electron image, the image is compared with the image obtained in (3), and the fine particles present in the areas other than the remaining external additives and filler (areas other than those removed in (3)) are regarded as organic fine particles, and the distance between the organic fine particles (the distance connecting the centers of the particles) is measured using the image processing software. This measurement was carried out for 100 binarized images (one toner particle per image). The average value of these is taken as the average distance between the organic fine particles.
[0154] Glass transition temperature Tg of organic fine particles at the first heating stage of DSC 1st The glass transition temperature Tg is preferably 30°C to 70°C. 1st If the glass transition temperature Tg is 30° C. to 70° C., the toner can have good storage stability and low-temperature fixability. 1st The glass transition temperature Tg is more preferably 30° C. to 50° C. 1st can further ensure low-temperature fixability.
[0155] The polyester resin has a function of imparting plasticity to the toner. The THF-insoluble component contained in the toner according to an embodiment lowers the glass transition temperature Tg and melt viscosity, and ensures low-temperature fixability, while having a branched structure in the molecular skeleton and a three-dimensional network structure in the molecular chain, resulting in rubber-like properties in that the toner deforms but does not flow at low temperatures.
[0156] The component insoluble in THF is preferably a polyester resin, and the glass transition temperature Tga 1st The temperature is preferably −40° C. to 10° C. This component insoluble in THF is derived from the polyester (prepolymer) which is a reactive precursor.
[0157] The glass transition temperature Tg of the toner according to one embodiment at the first temperature rise in DSC 1st The temperature is from 30° C. to 60° C., and from 30° C. to 50° C. is more preferable in terms of improving low-temperature fixability and storage stability.
[0158] The component soluble in THF is preferably a polyester resin, and the glass transition temperature Tg 2nd The temperature is preferably 45°C to 65°C.
[0159] The polyester resin insoluble in THF is a component derived from a large amorphous polyester resin having a weight average molecular weight Mw of 100,000 to 200,000, while the polyester resin soluble in THF is a component derived from an amorphous polyester resin having a weight average molecular weight Mw of 3,000 to 10,000.
[0160] In the past, the problem was solved by optimizing the ratio of polyester resin insoluble in THF to polyester resin soluble in THF. However, if too much polyester resin insoluble in THF is added, the glass transition temperature Tg decreases and storage stability cannot be guaranteed. In addition, the stress resistance of the toner deteriorates, and the fluidizing agent on the surface of the toner base particles is buried due to the thermal and mechanical stress caused by stirring in the developing device, and the adhesion of the toner increases. As a result, there is a concern that defects such as image blurring may occur in the transfer process. On the other hand, if the amount of polyester resin insoluble in THF is too small, the plasticity is not sufficiently imparted and low-temperature fixability cannot be satisfied. In addition, there is a concern that the necessary elasticity is not imparted, high-temperature offset is deteriorated, the fixable area is narrowed, and the image glossiness is too high.
[0161] The organic fine particles preferably contain one or more types of styrene-acrylic resin having a carboxylic acid. The organic fine particles preferably consist of one or more types of styrene-acrylic resin having a carboxylic acid. The organic fine particles consisting of styrene-acrylic resin are obtained by homopolymerizing or copolymerizing vinyl monomers.
[0162] The organic fine particles are preferably composed of two types of styrene-acrylic resins (a1) and (a2), and more preferably have a core-shell structure composed of a shell containing the styrene-acrylic resin (a1) and a core containing (a2).
[0163] (Resin (a1)) Of the organic fine particles containing a vinyl-based unit composed of resins (a1) and (a2), the resin (a1) may be a polymer obtained by homopolymerizing or copolymerizing a vinyl monomer.
[0164] The vinyl monomer includes the following (1) to (10).
[0165] (1) Vinyl hydrocarbons Examples of the vinyl hydrocarbon include (1-1) aliphatic vinyl hydrocarbons, (1-2) alicyclic vinyl hydrocarbons, and (1-3) aromatic vinyl hydrocarbons.
[0166] (1-1) Aliphatic vinyl hydrocarbons Aliphatic vinyl hydrocarbons include alkenes and alkadienes.
[0167] Specific examples of alkenes include ethylene, propylene, and α-olefins.
[0168] Specific examples of alkadienes include butadiene, isoprene, 1,4-pentadiene, 1,6-hexadiene, and 1,7-octadiene.
[0169] (1-2) Alicyclic vinyl hydrocarbons Alicyclic vinyl hydrocarbons include mono- or di-cycloalkenes and alkadienes, and specific examples include (di)cyclopentadiene, terpene, and the like.
[0170] (1-3) Aromatic vinyl hydrocarbons Examples of aromatic vinyl hydrocarbons include styrene and its hydrocarbyl (alkyl, cycloalkyl, aralkyl and / or alkenyl) substituted derivatives, and specific examples thereof include α-methylstyrene, 2,4-dimethylstyrene and vinylnaphthalene.
[0171] (2) Carboxyl-containing vinyl monomers and their salts Examples of the carboxyl group-containing vinyl monomer and its salt include unsaturated monocarboxylic acids (salts) having 3 to 30 carbon atoms, unsaturated dicarboxylic acids (salts), and their anhydrides (salts), and their monoalkyl (carbon number 1 to 24) esters or salts.
[0172] Specific examples thereof include carboxyl group-containing vinyl monomers such as (meth)acrylic acid, (anhydride) maleic acid, maleic acid monoalkyl esters, fumaric acid, fumaric acid monoalkyl esters, crotonic acid, itaconic acid, itaconic acid monoalkyl esters, itaconic acid glycol monoether, citraconic acid, citraconic acid monoalkyl esters, and cinnamic acid, and metal salts thereof.
[0173] In the present embodiment, "(salt)" means an acid or a salt thereof. For example, an unsaturated monocarboxylic acid (salt) having 3 to 30 carbon atoms means an unsaturated monocarboxylic acid or a salt thereof.
[0174] "(Meth)acrylic" means methacrylic acid or acrylic acid. "(Meth)acryloyl" means methacryloyl or acryloyl. "(Meth)acrylate" means methacrylate or acrylate.
[0175] (3) Sulfonic acid-containing vinyl monomers, vinyl sulfate monoesters, and their salts Examples of sulfone group-containing vinyl monomers, vinyl sulfate monoesters, and salts thereof include alkene sulfonic acids (salts) having 2 to 14 carbon atoms, alkyl sulfonic acids (salts) having 2 to 24 carbon atoms, sulfo(hydroxy)alkyl-(meth)acrylates (salts) or (meth)acrylamides (salts), and alkylarylsulfosuccinic acids (salts).
[0176] Specifically, an example of an alkene sulfonic acid having 2 to 14 carbon atoms is vinyl sulfonic acid (salt), etc., an example of an alkyl sulfonic acid (salt) having 2 to 24 carbon atoms is α-methylstyrene sulfonic acid (salt), etc., and an example of a sulfo(hydroxy)alkyl-(meth)acrylate (salt) or (meth)acrylamide (salt) is sulfopropyl(meth)acrylate (salt), sulfuric acid ester (salt), or a sulfonic acid group-containing vinyl monomer (salt), etc.
[0177] (4) Phosphate-containing vinyl monomers and their salts: Examples of the phosphoric acid group-containing vinyl monomer and its salt include (meth)acryloyloxyalkyl (C1-24) phosphoric acid monoester (salt) and (meth)acryloyloxyalkyl (C1-24) phosphonic acid (salt).
[0178] Specific examples of the (meth)acryloyloxyalkyl (carbon number 1 to 24) phosphate monoester (salt) include 2-hydroxyethyl (meth)acryloyl phosphate (salt) and phenyl-2-acryloyloxyethyl phosphate (salt).
[0179] Specific examples of (meth)acryloyloxyalkyl (carbon number: 1 to 24)phosphonic acids (salts) include 2-acryloyloxyethylphosphonic acid (salts).
[0180] Examples of the salts of (2) to (4) above include alkali metal salts (sodium salts, potassium salts, etc.), alkaline earth metal salts (calcium salts, magnesium salts, etc.), ammonium salts, amine salts, and quaternary ammonium salts.
[0181] (5) Hydroxyl-containing vinyl monomers Examples of hydroxyl group-containing vinyl monomers include hydroxystyrene, N-methylol (meth)acrylamide, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, (meth)allyl alcohol, crotyl alcohol, isocrotyl alcohol, 1-buten-3-ol, 2-buten-1-ol, 2-butene-1,4-diol, propargyl alcohol, 2-hydroxyethyl propenyl ether, and sucrose allyl ether.
[0182] (6) Nitrogen-containing vinyl monomers Examples of the nitrogen-containing vinyl monomer include (6-1) an amino group-containing vinyl monomer, (6-2) an amide group-containing vinyl monomer, (6-3) a nitrile group-containing vinyl monomer, (6-4) a quaternary ammonium cation group-containing vinyl monomer, and (6-5) a nitro group-containing vinyl monomer.
[0183] (6-1) Amino group-containing vinyl monomer Examples of the amino group-containing vinyl monomer include aminoethyl (meth)acrylate.
[0184] (6-2) Amide group-containing vinyl monomer Amide group-containing vinyl monomer Examples of the acrylamide include (meth)acrylamide and N-methyl(meth)acrylamide.
[0185] (6-3) Nitrile group-containing vinyl monomer Examples of the nitrile group-containing vinyl monomer include (meth)acrylonitrile, cyanostyrene, and cyanoacrylate.
[0186] (6-4) Vinyl Monomers Containing Quaternary Ammonium Cationic Groups Examples of the vinyl monomer containing a quaternary ammonium cation group include quaternized products of tertiary amine group-containing vinyl monomers such as dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylamide, diethylaminoethyl (meth)acrylamide, and diallylamine (which are quaternized using a quaternizing agent such as methyl chloride, dimethyl sulfate, benzyl chloride, or dimethyl carbonate).
[0187] (6-5) Nitro group-containing vinyl monomer Nitro group-containing vinyl monomers include nitrostyrene.
[0188] (7) Epoxy group-containing vinyl monomer Examples of the epoxy group-containing vinyl monomer include glycidyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, and p-vinylphenyl phenyl oxide.
[0189] (8) Halogen-containing vinyl monomers Examples of halogen-containing vinyl monomers include vinyl chloride, vinyl bromide, vinylidene chloride, allyl chloride, chlorostyrene, bromostyrene, dichlorostyrene, chloromethylstyrene, tetrafluorostyrene, and chloroprene.
[0190] (9) Vinyl esters, vinyl (thio)ethers, vinyl ketones (9-1) Vinyl ester Examples of vinyl esters include vinyl acetate, vinyl butyrate, vinyl propionate, vinyl butyrate, diallyl phthalate, diallyl adipate, isopropenyl acetate, vinyl methacrylate, methyl 4-vinyl benzoate, cyclohexyl methacrylate, benzyl methacrylate, phenyl (meth)acrylate, vinyl methoxyacetate, vinyl benzoate, ethyl α-ethoxyacrylate, alkyl (meth)acrylates having an alkyl group having 1 to 50 carbon atoms [methyl (meth)acrylate], ) acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, dodecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, eicosyl (meth)acrylate, behenyl (meth)acrylate, etc.)], dialkyl fumarate (wherein the two alkyl groups are linear, branched or alicyclic groups having 2 to 8 carbon atoms), dialkyl Examples of the polyalkylene glycol include maleates (wherein the two alkyl groups are straight-chain, branched-chain or alicyclic groups having 2 to 8 carbon atoms), poly(meth)allyloxyalkanes (diallyloxyethane, triallyloxyethane, tetraallyloxyethane, tetraallyloxypropane, tetraallyloxybutane, tetramethallyloxyethane, etc.), vinyl monomers having polyalkylene glycol chains (polyethylene glycol (molecular weight 300) mono(meth)acrylate, polypropylene glycol (molecular weight 500) monoacrylate, methyl alcohol ethylene oxide 10 mol adduct (meth)acrylate, lauryl alcohol ethylene oxide 30 mol adduct (meth)acrylate, etc.), poly(meth)acrylates (poly(meth)acrylates of polyhydric alcohols: ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, polyethylene glycol di(meth)acrylate, etc.).
[0191] (9-2) Vinyl(thio)ether An example of the vinyl (thio)ether is vinyl methyl ether.
[0192] (9-3) Vinyl ketone An example of the vinyl ketone is vinyl methyl ketone.
[0193] (10) Other vinyl monomers Other vinyl monomers include tetrafluoroethylene, fluoroacrylate, isocyanatoethyl (meth)acrylate, and m-isopropenyl-α,α-dimethylbenzyl isocyanate.
[0194] For the resin (a1), the above vinyl monomers (1) to (10) may be used alone or in combination of two or more.
[0195] From the viewpoint of low-temperature fixability of organic fine particles, the resin (a1) preferably includes a styrene-(meth)acrylic acid ester copolymer and a (meth)acrylic acid ester copolymer, and more preferably includes a styrene-(meth)acrylic acid ester copolymer.
[0196] (resin (a2)) Among the organic fine particles containing a vinyl-based unit composed of resins (a1) and (a2), the resin (a2) may be a polymer obtained by homopolymerizing or copolymerizing a vinyl monomer. The vinyl monomer may be the same polymer as that used for the resin (a1).
[0197] In synthesizing the resin (a2), one of the vinyl monomers (1) to (10) listed above for the resin (a1) may be used alone, or two or more of them may be used in combination.
[0198] As the resin (a2), from the viewpoint of improving the low-temperature fixing property of the toner according to one embodiment, a styrene-(meth)acrylic acid ester copolymer and a (meth)acrylic acid ester copolymer are preferable, and a styrene-(meth)acrylic acid ester copolymer is more preferable.
[0199] (1) Glass transition temperature Tg1 calculated from the constituent monomers of resin (a1), and glass transition temperature Tg2 calculated from the constituent monomers of resin (a2) The glass transition temperature Tg1 calculated from the constituent monomers of the resin (a1) is preferably 0° C. to 150° C., and more preferably 50° C. to 100° C. The glass transition temperature Tg2 calculated from the constituent monomers of the resin (a2) is preferably −30° C. to 100° C., and more preferably 0° C. to 80° C., and even more preferably 30° C. to 60° C.
[0200] The glass transition temperature Tg calculated from the constituent monomers is a value that can be calculated by the Fox method.
[0201] Here, the Fox method [TGFox, Phys. Rev., 86, 652 (1952)] is a method for estimating the Tg of a copolymer from the Tg of each homopolymer represented by the following formula. 1 / Tg=W1 / Tg1+W2 / Tg2++Wn / Tgn (In the formula, Tg is the glass transition temperature (expressed in absolute temperature) of the copolymer, Tg1, Tg2...Tgn are the glass transition temperatures (expressed in absolute temperature) of the homopolymers of each monomer component, and W1, W2...Wn are the weight fractions of each monomer component.)
[0202] (2) Calculated acid value (AV1) of resin (a1) and calculated acid value (AV2) of resin (a2) The calculated acid value (AV1) of the resin (a1) is preferably 75 mgKOH / g to 400 mgKOH / g, and more preferably 150 mgKOH / g to 300 mgKOH / g, and the calculated acid value (AV2) of the resin (a2) is preferably 0 mgKOH / g to 50 mgKOH / g, and more preferably 0 mgKOH / g to 20 mgKOH / g, and even more preferably 0 mgKOH / g.
[0203] The calculated acid value is a theoretical acid value calculated from the molar amount of acidic groups contained in the constituent monomers and the total weight of the constituent monomers.
[0204] As a constituent monomer satisfying the above conditions (1) and (2), for the resin (a1), for example, a resin containing, as a constituent monomer, preferably 10 to 80 mass% of styrene, and preferably 10 to 60 mass% in total of at least one of methacrylic acid and acrylic acid, based on the total mass of the resin (a1). The content of styrene is more preferably 30 to 60 mass%, and the content of at least one of methacrylic acid and acrylic acid is more preferably 30 to 50 mass% in total.
[0205] The resin (a2) may, for example, contain, as a constituent monomer, preferably 10% by mass to 100% by mass, and more preferably 30% by mass to 90% by mass of styrene, and preferably a total of 0% by mass to 7.5% by mass, and more preferably a total of 0% by mass to 2.5% by mass of at least one of methacrylic acid and acrylic acid, based on the total mass of the resin (a2).
[0206] (3) By adjusting the polymerization conditions (type and amount of initiator and chain transfer agent, reaction temperature, etc.), the number average molecular weights Mn1 and Mn2 of the resin (a1) and resin (a2) are preferably set to 2,000 to 2,000,000, and more preferably 20,000 to 200,000. The number average molecular weight Mn2 is preferably set to 1,000 to 1,000,000, and more preferably 10,000 to 100,000.
[0207] The acid value (AVa1) of the resin (a1) is preferably 75 mgKOH / g to 400 mgKOH / g, more preferably 150 mgKOH / g to 300 mgKOH / g. Within this range, organic fine particles containing vinyl units, which contain the resin (a1) and the resin (a2) as constituents in the same particle, are likely to form particles adhered to the surface of the toner.
[0208] Resin (a1) having an acid value within this range is a resin that contains methacrylic acid and / or acrylic acid in a total amount of preferably 10% by mass to 60% by mass, more preferably 30% by mass to 50% by mass, based on the total mass of resin (a1).
[0209] From the viewpoint of low-temperature fixability, the resin (a2) preferably has an acid value (AVa2) of 0 mgKOH / g to 50 mgKOH / g, more preferably 0 mgKOH / g to 20 mgKOH / g, and most preferably 0 mgKOH / g. Resin (a2) having an acid value within this range is a resin that contains methacrylic acid and / or acrylic acid in a total amount of preferably 0 to 7.5 mass %, more preferably 0 to 2.5 mass %, based on the total mass of resin (a2).
[0210] The acid value in this embodiment is measured by the method of JIS K0070:1992.
[0211] The glass transition temperature of the resin (a1) is preferably higher than the glass transition temperature of the resin (a2).
[0212] Within this range, the ease of forming a toner in which the organic fine particles (A) are attached to the surface of the toner base particles and the low-temperature fixability of the toner according to one embodiment are well balanced.
[0213] The glass transition temperature of the resin (a1) is more preferably at least 10° C. higher, and particularly preferably at least 20° C. higher, than the glass transition temperature of the resin (a2).
[0214] The glass transition temperature Tg of the resin (a1) is preferably 0° C. to 150° C., and more preferably 50° C. to 100° C. When the glass transition temperature Tg is 0° C. or higher, the storage stability of the organic fine particles is excellent, and when the glass transition temperature Tg is 150° C. or lower, the low-temperature fixability of the organic fine particles is less hindered.
[0215] The glass transition temperature Tg of the resin (a2) is preferably −30° C. to 100° C., more preferably 0° C. to 80° C., and further preferably 30° C. to 60° C. When the glass transition temperature Tg is −30° C. or higher, the storage stability of the organic fine particles is excellent, and when the glass transition temperature Tg is 100° C. or lower, the low-temperature fixability of the organic fine particles is less hindered.
[0216] The glass transition temperature Tg can be measured by the method (DSC) specified in ASTM D3418-82 using "DSC20, SSC / 580 (manufactured by Seiko Instruments Inc.)".
[0217] The solubility parameter SP value of the resin (a1) is preferably 9 (cal / cm) from the viewpoint of ease of formation of a toner in which organic fine particles containing the resin (a1) and the resin (a2) as constituent components in the same particle are attached to the surface of the toner base particle. 3 ) 1 / 2 ~13(cal / cm 3 ) 1 / 2 ~, more preferably 9.5 (cal / cm 3 ) 1 / 2 ~12.5(cal / cm 3 ) 1 / 2 , and more preferably 10.5 (cal / cm 3 ) 1 / 2 ~11.5(cal / cm 3 ) 1 / 2 It is.
[0218] The solubility parameter SP of the resin (a1) can be adjusted by changing the types and composition ratio of the constituent monomers.
[0219] The solubility parameter SP value of the resin (a2) is preferably 8.5 (cal / cm) from the viewpoint of ease of formation of a toner in which organic fine particles containing the resin (a1) and the resin (a2) as constituent components in the same particle are attached to the surface of the toner base particle. 3 ) 1 / 2 ~12.5(cal / cm 3 ) 1 / 2 and more preferably 9 (cal / cm 3 ) 1 / 2 ~12(cal / cm 3 )1 / 2 , and more preferably 10 (cal / cm 3 ) 1 / 2 ~11(cal / cm 3 ) 1 / 2 It is.
[0220] The solubility parameter SP value of the resin (a2) can be adjusted by changing the types and composition ratio of the constituent monomers, similarly to the resin (a1).
[0221] The solubility parameter SP value can be calculated by the method by Fedors [Polym. Eng. Sci. 14(2)152, (1974)].
[0222] From the viewpoint of the glass transition temperature Tg of the resin (a1) and copolymerizability with other monomers, the resin (a1) contains, as a constituent monomer, preferably 10% by mass to 80% by mass, more preferably 30% by mass to 60% by mass, based on the total mass of the resin (a1).
[0223] From the viewpoint of the glass transition temperature Tg of the resin (a2) and copolymerizability with other vinyl monomers, the resin (a2) contains, as a constituent monomer, preferably 10% by mass to 100% by mass, more preferably 30% by mass to 90% by mass, based on the total mass of the resin (a2).
[0224] The number average molecular weight Mn of the resin (a1) is preferably 2000 to 2,000,000, and more preferably 20,000 to 200,000. When the number average molecular weight Mn is 2000 or more, the storage stability of the organic fine particles is excellent, and when it is 2,000,000 or less, the low-temperature fixability of the organic fine particles is less hindered.
[0225] The weight average molecular weight Mw of the resin (a1) is preferably larger than the weight average molecular weight Mw of the resin (a2).
[0226] Within this range, the ease of forming a toner in which organic fine particles are attached to the surface of the toner base particles and the low-temperature fixability of the toner according to one embodiment are well balanced.
[0227] The weight average molecular weight Mw of the resin (a1) is preferably at least 1.5 times, and more preferably at least 2.0 times, larger than the weight average molecular weight Mw of the resin (a2).
[0228] The weight average molecular weight Mw of the resin (a2) is preferably 20,000 to 20,000,000, and more preferably 200,000 to 2,000,000. When the weight average molecular weight Mw is 20,000 or more, the storage stability of the organic fine particles is excellent, and when it is 20,000,000 or less, the low-temperature fixability of the organic fine particles is less hindered.
[0229] The number average molecular weight Mn of the resin (a2) is preferably 1000 to 1,000,000, and more preferably 10,000 to 100,000. When the number average molecular weight Mn is 1000 or more, the storage stability of the organic fine particles is excellent, and when it is 1,000,000 or less, the low-temperature fixability of the organic fine particles is less hindered.
[0230] The weight average molecular weight Mw of the resin (a2) is preferably 10,000 to 10,000,000, and more preferably 100,000 to 1,000,000. When the weight average molecular weight Mw is 10,000 or more, the storage stability of the organic fine particles is excellent, and when it is 10,000,000 or less, the low-temperature fixability of the organic fine particles is less hindered.
[0231] In particular, it is preferred that the weight average molecular weight Mw of resin (a1) is 200,000 to 2,000,000, the weight average molecular weight Mw of resin (a2) is 100,000 to 500,000, and the weight average molecular weight of resin (a1) is larger than the weight average molecular weight of resin (a2) (weight average molecular weight Mw of (a1)>(weight average molecular weight Mw of resin (a2))).
[0232] The number average molecular weight Mn and the weight average molecular weight Mw can be measured by gel permeation chromatography (GPC) under the following conditions. Equipment (example): "HLC-8120", manufactured by Tosoh Corporation Column (example): "TSK GEL GMH6", Tosoh Corporation, 2 columns ·Measurement temperature: 40℃ Sample solution: 0.25% by mass tetrahydrofuran solution (undissolved matter was removed using a glass filter) ·Solution injection volume: 100μl Detector: Refractive index detector Reference material: 12 standard polystyrenes (TSKstandard POLYSTYRENE) (molecular weight: 500, 1050, 2800, 5970, 9100, 18100, 37900, 96400, 190000, 355000, 1090000, 2890000), manufactured by Tosoh Corporation
[0233] The weight ratio of resin (a1) to resin (a2) in the organic fine particles is 5 / 95 to 95 / 5, preferably 25 / 75 to 75 / 25, and more preferably 40 / 60 to 60 / 40. If the weight ratio is 5 / 95 or more, the organic fine particles have excellent heat resistance storage stability, and if the weight ratio is 95 / 5 or less, a toner in which the organic fine particles adhere to the surfaces of the toner base particles is easily formed.
[0234] The organic fine particles may be a combination of organic fine particles (A) made of two types of styrene-acrylic resins (resins (a1) and (a2)) and organic fine particles (B) made of one type of styrene-acrylic resin. The organic fine particles (A) and (B) mixed in advance during emulsification are uniformly attached to the surface of the toner base particles, and the organic fine particles (B) attached to the surface of the toner base particles and all or a part of the resin (a1) in the organic fine particles (A) are removed in a washing step described later, whereby the organic fine particles (A) can be uniformly attached with gaps therebetween.
[0235] Methods for producing organic fine particles (A) containing resin (a1) and resin (a2) as constituent components within the same particle include known production methods, such as the following production methods (I) to (V). (I) A method of seed polymerization of constituent monomers of resin (a2) using fine particles of resin (a1) in an aqueous dispersion as seeds. (II) A method of seed polymerization of constituent monomers of resin (a1) using fine particles of resin (a2) in an aqueous dispersion as seeds. (III) A method in which a mixture of the resin (a1) and the resin (a2) is emulsified in an aqueous medium to obtain an aqueous dispersion of organic fine particles. (IV) A method in which a mixture of the resin (a1) and the constituent monomers of the resin (a2) is emulsified in an aqueous medium, and then the constituent monomers of the resin (a2) are polymerized to obtain an aqueous dispersion of organic fine particles. (V) A method in which a mixture of resin (a2) and monomers constituting resin (a1) is emulsified in an aqueous medium, and then the monomers constituting resin (a1) are polymerized to obtain an aqueous dispersion of organic fine particles.
[0236] In addition, the fact that the organic microparticles (A) contain resin (a1) and resin (a2) as constituent components within the same particle can be confirmed by observing element mapping images of a cut surface of the organic microparticles (A) using a known surface elemental analysis device (TOF-SIMS, EDX-SEM, etc.) and by observing electron microscope images of a cut surface of the organic microparticles (A) stained with a stain corresponding to the functional groups contained in the resin (a1) and resin (a2).
[0237] The organic fine particles obtained by the above method may be obtained as a mixture containing organic fine particles (A) containing resin (a1) and resin (a2) as constituent components within the same particle, as well as organic fine particles (B) containing resin (a1) as the only constituent resin component and organic fine particles containing resin (a2) as the only constituent resin component. In the composite process described below, the mixture may be used as is, or only the organic fine particles (A) may be isolated and used.
[0238] Specific examples of (I) include the following methods. First, the constituent monomers of the resin (a1) are polymerized by dropwise polymerization to produce an aqueous dispersion of organic fine particles containing the resin (a1). Then, the constituent monomers of the resin (a2) are seed-polymerized using the aqueous dispersion as a seed, or the resin (a1) previously produced by solution polymerization or the like is emulsified and dispersed in water. Then, the constituent monomers of the resin (a2) are seed-polymerized using the emulsified dispersion as a seed.
[0239] Specific examples of (II) include the following methods. First, the constituent monomers of the resin (a2) are polymerized by dropwise polymerization to produce an aqueous dispersion of organic fine particles containing the resin (a2). Then, the constituent monomers of the resin (a1) are seed-polymerized using the aqueous dispersion as a seed, or the resin (a2) previously produced by solution polymerization or the like is emulsified and dispersed in water. Then, the constituent monomers of the resin (a1) are seed-polymerized using the emulsified dispersion as a seed.
[0240] A specific example of (III) is a method in which a solution or melt containing resin (a1) and resin (a2) previously produced by solution polymerization or the like is mixed, and then the mixture is emulsified and dispersed in an aqueous medium.
[0241] Specific examples of (IV) include the following methods. First, resin (a1) previously produced by solution polymerization or the like is mixed with the constituent monomers of resin (a2), and the resulting mixture is emulsified and dispersed in an aqueous medium, and the constituent monomers of resin (a2) are polymerized in the emulsion dispersion to produce resin (a1) in the constituent monomers of resin (a2). Then, the mixture is emulsified and dispersed in an aqueous medium, and the constituent monomers of resin (a2) are polymerized in the emulsion dispersion.
[0242] Specific examples of (V) include the following methods. First, resin (a2) previously produced by solution polymerization or the like is mixed with the constituent monomers of resin (a1), and the resulting mixture is emulsified and dispersed in an aqueous medium, and the constituent monomers of resin (a1) are polymerized in the emulsion dispersion to produce resin (a1) in the constituent monomers of resin (a1). After that, the mixture is emulsified and dispersed in an aqueous medium, and the constituent monomers of resin (a1) are polymerized in the emulsion dispersion.
[0243] Any of the production methods (I) to (V) is suitable.
[0244] The organic fine particles (A) are preferably used as an aqueous dispersion, and the aqueous medium of the dispersion can be any liquid containing water as an essential component. In this embodiment, since the organic fine particles and the surfactant are provided on the surface of the toner, the aqueous medium can be an aqueous solution containing the surfactant (D) described later in water.
[0245] The particle diameter of the organic fine particles is preferably 10 nm to 100 nm. If the particle diameter is less than 10 nm, the coverage rate on the toner surface increases, and low-temperature fixing performance may decrease. If the particle diameter exceeds 100 nm, the voids on the toner surface become large, and the effect of heat-resistant storage performance decreases.
[0246] The particle size of the organic fine particles can be measured by using a laser Doppler particle size distribution measuring device and adding a sample to be measured to the measuring device using a dropper or syringe, etc. The measurement conditions are as follows. (Measurement conditions) Equipment: nanotrac UPA-150EX (manufactured by Nikkiso Co., Ltd.) Distribution display: Volume Number of channels: 52 ·Measurement time: 30sec Particle refractive index: 1.81 ·Temperature: 25℃ ·Particle shape: spherical ·Viscosity (CP): High temperature viscosity 0.797 Low temperature viscosity 1.002 Solvent refractive index: 1.333 Solvent: Water
[0247] The organic fine particles (B) are obtained by the same manufacturing method as the resin (a) composed of one type of styrene acrylic resin. The organic fine particles (B) are preferably used as an aqueous dispersion, like the organic fine particles (A), and the aqueous medium of the dispersion can be any liquid containing water as an essential component. In this embodiment, since the organic fine particles and the surfactant are provided on the surface of the toner, the aqueous medium can be an aqueous solution containing the surfactant (D) described later in water.
[0248] The surfactant (D) includes nonionic surfactants (D1), anionic surfactants (D2), cationic surfactants (D3), amphoteric surfactants (D4) and other emulsifying dispersants (D5).
[0249] Furthermore, if necessary, suitable amounts of a buffer such as sodium acetate, sodium citrate, sodium bicarbonate, etc., and a protective colloid such as a water-soluble cellulose compound and an alkali metal salt of polymethacrylic acid, etc., may be used. These may be used alone or in combination of two or more.
[0250] Examples of the nonionic surfactant (D1) include AO addition type nonionic surfactants and polyhydric alcohol type nonionic surfactants.
[0251] Examples of AO-addition type nonionic surfactants include EO adducts of aliphatic alcohols having 10 to 20 carbon atoms, EO adducts of phenols, EO adducts of nonylphenols, EO adducts of alkylamines having 8 to 22 carbon atoms, and EO adducts of poly(oxypropylene) glycols.
[0252] Examples of polyhydric alcohol-type nonionic surfactants include fatty acid (carbon number 8 to 24) esters of polyhydric (trihydric to octahydric or higher) alcohols (carbon number 2 to 30) (e.g., glycerin monostearate, glycerin monooleate, sorbitan monolaurate, sorbitan monooleate, etc.) and alkyl (carbon number 4 to 24) poly(degree of polymerization 1 to 10) glycosides.
[0253] Examples of the anionic surfactant (D2) include ether carboxylic acids or salts thereof having a hydrocarbon group having 8 to 24 carbon atoms, sulfate esters or ether sulfate esters and salts thereof having a hydrocarbon group having 8 to 24 carbon atoms, sulfonates having a hydrocarbon group having 8 to 24 carbon atoms, sulfosuccinates having one or two hydrocarbon groups having 8 to 24 carbon atoms, phosphate esters or ether phosphate esters and salts thereof having a hydrocarbon group having 8 to 24 carbon atoms, fatty acid salts having a hydrocarbon group having 8 to 24 carbon atoms, and acylated amino acid salts having a hydrocarbon group having 8 to 24 carbon atoms.
[0254] Specifically, examples of ether carboxylic acids or salts thereof having a hydrocarbon group having 8 to 24 carbon atoms include sodium lauryl ether acetate and (poly)oxyethylene (number of moles added: 1 to 100) sodium lauryl ether acetate.
[0255] Examples of sulfates or ether sulfates having a hydrocarbon group having 8 to 24 carbon atoms and salts thereof include sodium lauryl sulfate, (poly)oxyethylene (number of moles added: 1 to 100) sodium lauryl sulfate, (poly)oxyethylene (number of moles added: 1 to 100) triethanolamine lauryl sulfate, and (poly)oxyethylene (number of moles added: 1 to 100) sodium coconut oil fatty acid monoethanolamide sulfate.
[0256] Examples of sulfonates having a hydrocarbon group having 8 to 24 carbon atoms include sodium dodecylbenzenesulfonate.
[0257] Examples of sulfosuccinates having one or two hydrocarbon groups having 8 to 24 carbon atoms include sodium dodecyl sulfosuccinate, sodium sulfosuccinate, and octyl sulfosuccinate.
[0258] Examples of the phosphate ester or ether phosphate ester having a hydrocarbon group having 8 to 24 carbon atoms and salts thereof include sodium lauryl phosphate and sodium (poly)oxyethylene (addition mole number 1 to 100) lauryl ether phosphate.
[0259] Examples of the fatty acid salt having a hydrocarbon group having 8 to 24 carbon atoms include sodium laurate and triethanolamine laurate.
[0260] Examples of the acylated amino acid salts having a hydrocarbon group having 8 to 24 carbon atoms include sodium methyl coconut taurate, sodium coconut sarcosine, triethanolamine coconut sarcosine, N-triethanolamine coconut acyl-L-glutamate, sodium N-sodium coconut acyl-L-glutamate, and sodium lauroylmethyl-β-alanine.
[0261] The cationic surfactant (D3) may be a quaternary ammonium salt type or an amine salt type.
[0262] Specific examples of the quaternary ammonium salt type include stearyl trimethyl ammonium chloride, behenyl trimethyl ammonium chloride, distearyl dimethyl ammonium chloride, and lanolin fatty acid aminopropyl ethyl dimethyl ammonium ethyl sulfate.
[0263] Examples of the amine salt type include stearic acid diethylaminoethylamide lactate, dilaurylamine hydrochloride, and oleylamine lactate.
[0264] Examples of the amphoteric surfactant (D4) include betaine-type amphoteric surfactants and amino acid-type amphoteric surfactants.
[0265] Examples of the betaine type amphoteric surfactant include coconut oil fatty acid amidopropyl dimethylaminoacetic acid betaine, lauryl dimethylaminoacetic acid betaine, 2-alkyl-N-carboxymethyl-N-hydroxyethyl imidazolinium betaine, and lauryl hydroxysulfobetaine.
[0266] Examples of the amino acid type amphoteric surfactant include sodium β-laurylaminopropionate.
[0267] Other emulsifying dispersants (D5) include, for example, reactive activators, polyvinyl alcohol, starch and its derivatives, cellulose derivatives such as carboxymethyl cellulose, methyl cellulose and hydroxyethyl cellulose, carboxyl group-containing (co)polymers such as sodium polyacrylate, and emulsifying dispersants having urethane groups or ester groups as described in U.S. Pat. No. 5,906,704.
[0268] The reactive activator is not particularly limited as long as it has radical reactivity, and specific examples thereof include ADEKA REASOAP (registered trademark, manufactured by ADEKA CORPORATION), SE-10N, SR-10, SR-20, SR-30, ER-20, ER-30, AQUALON (registered trademark, manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.), HS-10, KH-05, KH-10, KH-1025, ELEMINOL (registered trademark, manufactured by Sanyo Chemical Industries, Ltd.), JS-20, LATEMUL (registered trademark, manufactured by Kao Corporation), PD-104, PD-420, PD-430, IONET (registered trademark, manufactured by Sanyo Chemical Industries, Ltd.), MO-200, and the like.
[0269] Examples of emulsifying dispersants having a urethane group or an ester group described in US Pat. No. 5,906,704 include those in which a polycaprolactone polyol and a polyether diol are linked with a polyisocyanate.
[0270] As the surfactant (D), from the viewpoint of stabilizing the oil droplets during emulsification and dispersion, obtaining a desired shape, and sharpening the particle size distribution, preferred are nonionic surfactants (D1), anionic surfactants (D2), other emulsifying dispersants (D5), and combinations thereof. More preferred are combinations of nonionic surfactants (D1) and other emulsifying dispersants (D5), and combinations of anionic surfactants (D2) and other emulsifying dispersants (D5).
[0271] In addition to the resin (a1) and the resin (a2), the organic fine particles (A) in this embodiment may contain other resin components, an initiator (and its residue), a chain transfer agent, an antioxidant, a plasticizer, a preservative, a reducing agent, an organic solvent, and the like.
[0272] Examples of other resin components include vinyl resins other than the resins used in resin (a1) and resin (a2), polyurethane resins, epoxy resins, polyester resins, polyamide resins, polyimide resins, silicon resins, phenol resins, melamine resins, urea resins, aniline resins, ionomer resins, and polycarbonate resins.
[0273] Examples of the initiator (and its residue) include known radical polymerization initiators, etc. Specific examples include persulfate initiators such as potassium persulfate and ammonium persulfate, azo initiators such as azobisisobutyronitrile, organic peroxides such as benzoyl peroxide, cumene hydroperoxide, tertiary butyl hydroperoxide, tertiary butyl peroxyisopropyl monocarbonate and tertiary butyl peroxybenzoate, and hydrogen peroxide.
[0274] Examples of the chain transfer agent include n-dodecyl mercaptan, tert-dodecyl mercaptan, n-butyl mercaptan, 2-ethylhexyl thioglycolate, 2-mercaptoethanol, β-mercaptopropionic acid, and α-methylstyrene dimer.
[0275] Examples of the antioxidant include phenol compounds, paraphenylenediamine, hydroquinone, organic sulfur compounds, and organic phosphorus compounds.
[0276] The phenolic compounds include 2,6-di-t-butyl-p-cresol, butylated hydroxyanisole, 2,6-di-t-butyl-4-ethylphenol, stearyl-β-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 2,2'-methylene-bis-(4-methyl-6-t-butylphenol), 2,2'-methylene-bis-(4-ethyl-6-t-butylphenol), 4,4'-thiobis-(3-methyl-6-t-butylphenol), 4,4'-butylidenebis-(3-methyl -6-t-butylphenol), 1,1,3-tris-(2-methyl-4-hydroxy-5-t-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane, bis[3,3'-bis(4'-hydroxy-3'-t-butylphenyl)butyric acid]glycol ester, and tocopherol.
[0277] Examples of paraphenylenediamines include N-phenyl-N'-isopropyl-p-phenylenediamine, N,N'-di-sec-butyl-p-phenylenediamine, N-phenyl-N-sec-butyl-p-phenylenediamine, N,N'-di-isopropyl-p-phenylenediamine, and N,N'-dimethyl-N,N'-di-t-butyl-p-phenylenediamine.
[0278] Examples of hydroquinone include 2,5-di-t-octylhydroquinone, 2,6-didodecylhydroquinone, 2-dodecylhydroquinone, 2-dodecyl-5-chlorohydroquinone, 2-t-octyl-5-methylhydroquinone, and 2-(2-octadecenyl)-5-methylhydroquinone.
[0279] Examples of the organic sulfur compounds include dilauryl-3,3'-thiodipropionate, distearyl-3,3'-thiodipropionate, and ditetradecyl-3,3'-thiodipropionate.
[0280] Examples of the organic phosphorus compound include triphenylphosphine, tri(nonylphenyl)phosphine, tri(dinonylphenyl)phosphine, tricresylphosphine, and tri(2,4-dibutylphenoxy)phosphine.
[0281] Examples of the plasticizer include phthalate esters, aliphatic dibasic acid esters, trimellitate esters, phosphate esters, and fatty acid esters.
[0282] Specifically, examples of phthalate esters include dibutyl phthalate, dioctyl phthalate, butyl benzyl phthalate, and diisodecyl phthalate.
[0283] Examples of the aliphatic dibasic acid ester include di-2-ethylhexyl adipate and 2-ethylhexyl sebacate.
[0284] Examples of trimellitic acid esters include tri-2-ethylhexyl trimellitate and trioctyl trimellitate.
[0285] Examples of the phosphate ester include triethyl phosphate, tri-2-ethylhexyl phosphate, and tricresyl phosphate.
[0286] The fatty acid ester may, for example, be butyl oleate.
[0287] Examples of the preservatives include organic nitrogen sulfur compound preservatives and organic sulfur halide preservatives.
[0288] Examples of reducing agents include reducing organic compounds such as ascorbic acid, tartaric acid, citric acid, glucose, and metal formaldehyde sulfoxylates, and reducing inorganic compounds such as sodium thiosulfate, sodium sulfite, sodium bisulfite, and sodium metabisulfite.
[0289] Examples of the organic solvent include ketone solvents [e.g., acetone and methyl ethyl ketone (hereinafter, abbreviated as MEK)], ester solvents (e.g., ethyl acetate and γ-butyrolactone), ether solvents (e.g., THF), amide solvents (e.g., N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone and N-methylcaprolactam), alcohol solvents (e.g., isopropyl alcohol), and aromatic hydrocarbon solvents (e.g., toluene and xylene).
[0290] (Other external additives) The external additive may contain, in addition to organic fine particles, inorganic fine particles, hydrophobically treated inorganic fine particles, fatty acid metal salts (eg, zinc stearate, aluminum stearate, etc.), fluoropolymers, and the like.
[0291] Examples of inorganic fine particles include oxides such as silica, titanium oxide, alumina, barium titanate, magnesium titanate, calcium titanate, strontium titanate, iron oxide, copper oxide, zinc oxide, tin oxide, silica sand, clay, chromium oxide, cerium oxide, red iron oxide, antimony trioxide, magnesium oxide, and zirconium oxide; barium sulfate, barium carbonate, calcium carbonate, silicon carbide, silicon nitride, mica, wollastonite, and diatomaceous earth. Among these, silica and titanium oxide are particularly preferred.
[0292] Examples of silica include R972, R974, RX200, RY200, R202, R805, and R812 (all manufactured by Nippon Aerosil Co., Ltd.). Examples of titanium oxide include P-25 (manufactured by Nippon Aerosil Co., Ltd.), STT-30, and STT-65C-S (all manufactured by Titanium Kogyo Co., Ltd.), TAF-140 (manufactured by Fuji Titanium Kogyo Co., Ltd.), MT-150W, MT-500B, MT-600B, and MT-150A (all manufactured by Teika Co., Ltd.).
[0293] Hydrophobically treated inorganic fine particles can be obtained, for example, by treating hydrophilic inorganic fine particles with a silane coupling agent such as methyltrimethoxysilane, methyltriethoxysilane, or octyltrimethoxysilane.
[0294] Examples of the hydrophobized inorganic fine particles include hydrophobized silica fine particles, titanium oxide fine particles, alumina fine particles, and the like.
[0295] Examples of hydrophobically treated titanium oxide particles include T-805 (manufactured by Nippon Aerosil Co., Ltd.), STT-30A, STT-65S-S (all manufactured by Titanium Kogyo Co., Ltd.), TAF-500T, TAF-1500T (all manufactured by Fuji Titanium Kogyo Co., Ltd.), MT-100S, MT-100T (all manufactured by Teika Corporation), and IT-S (manufactured by Ishihara Sangyo Kaisha, Ltd.).
[0296] As the hydrophobically treated inorganic fine particles, for example, silicone oil-treated inorganic fine particles obtained by treating the inorganic fine particles with silicone oil and, if necessary, applying heat thereto, can be used.
[0297] Examples of silicone oils include dimethyl silicone oil, methylphenyl silicone oil, chlorophenyl silicone oil, methylhydrogen silicone oil, alkyl-modified silicone oil, fluorine-modified silicone oil, polyether-modified silicone oil, alcohol-modified silicone oil, amino-modified silicone oil, epoxy-modified silicone oil, epoxy-polyether-modified silicone oil, phenol-modified silicone oil, carboxyl-modified silicone oil, mercapto-modified silicone oil, methacryl-modified silicone oil, and α-methylstyrene-modified silicone oil.
[0298] The average particle size of the primary particles of the inorganic fine particles is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 100 nm or less, more preferably 3 nm to 70 nm. If the average particle size is 3 nm to 70 nm, the inorganic fine particles are not embedded in the toner, and can effectively exert their functions, and can be prevented from unevenly damaging the surface of the photoconductor, which is preferable.
[0299] The average particle size of the primary particles of the hydrophobized inorganic fine particles is preferably 1 nm to 100 nm, more preferably 5 nm to 70 nm. It is also preferable that the inorganic fine particles contain at least one type of inorganic fine particles having an average particle size of 20 nm or less, and at least one type of inorganic fine particles having an average particle size of 30 nm or more. The specific surface area by the BET method is 20 m 2 / g~500m 2 It is preferable that the molecular weight is 1 / g.
[0300] The content of the external additive is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.1 to 5 parts by mass, and more preferably 0.3 to 3 parts by mass, relative to 100 parts by mass of the toner.
[0301] [Other ingredients] The toner according to an embodiment may contain other components, such as a release agent, a colorant, a charge control agent, a flowability improver, a cleaning property improver, and a magnetic material.
[0302] (Release agent) The release agent is not particularly limited and can be appropriately selected from known ones.
[0303] Examples of wax and wax release agents include natural waxes such as vegetable waxes such as carnauba wax, cotton wax, and wood wax rice wax; animal waxes such as beeswax and lanolin; mineral waxes such as ozokerite and cerusin; and petroleum waxes such as paraffin, microcrystalline, and petrolatum.
[0304] In addition to these natural waxes, synthetic hydrocarbon waxes such as Fischer-Tropsch wax, polyethylene, and polypropylene; synthetic waxes such as esters, ketones, and ethers; and the like.
[0305] Further, fatty acid amide compounds such as 12-hydroxystearic acid amide, stearic acid amide, phthalimide anhydride, and chlorinated hydrocarbons; homopolymers or copolymers of polyacrylates such as poly-n-stearyl methacrylate and poly-n-lauryl methacrylate, which are low molecular weight crystalline polymer resins (for example, copolymers of n-stearyl acrylate and ethyl methacrylate); and crystalline polymers having long alkyl groups in their side chains may be used.
[0306] Among these, hydrocarbon waxes such as paraffin wax, microcrystalline wax, Fischer-Tropsch wax, polyethylene wax, and polypropylene wax are preferred.
[0307] The melting point of the release agent is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 60° C. or more and 80° C. or less. If the melting point is less than 60° C., the release agent is likely to melt at low temperatures, and the heat resistance storage stability may be poor. If the melting point is more than 80° C., even if the resin melts and is in the fixing temperature range, the release agent may not melt sufficiently, causing fixing offset and image defects.
[0308] The content of the release agent is not particularly limited and can be appropriately selected according to the purpose, but is preferably 2 to 10 parts by mass, more preferably 3 to 8 parts by mass, relative to 100 parts by mass of the toner. If the content is less than 2 parts by mass, the high-temperature offset resistance and low-temperature fixability during fixing may be poor, and if it exceeds 10 parts by mass, the heat-resistant storage stability may decrease and image fogging may easily occur. If the content is within the above more preferred range, it is advantageous in terms of improving image quality and fixing stability.
[0309] (Coloring agent) The colorant is not particularly limited and can be appropriately selected depending on the purpose. Examples of the colorant include carbon black, nigrosine dye, iron black, naphthol yellow S, Hansa yellow (10G, 5G, G), cadmium yellow, yellow iron oxide, yellow ochre, yellow lead, titanium yellow, polyazo yellow, oil yellow, Hansa yellow (GR, A, RN, R), pigment yellow L, benzidine yellow (G, GR), permanent yellow (NCG), Balkan fast yellow (5G, R), tartrazine lake, quinoline yellow lake, and anthrazan yellow BGL. , Isoindolinone Yellow, Bengala, Red Lead, Cinnabar, Cadmium Red, Cadmium Mercury Red, Antimony Vermilion, Permanent Red 4R, Para Red, Phaysee Red, Parachlor Orthonitroaniline Red, Lithol Fast Scarlet G, Brilliant Fast Scarlet, Brilliant Kanmin BS, Permanent Red (F2R, F4R, FRL, FRLL, F4RH), Fast Scarlet VD, Belkan Fast Rubin B, Brilliant Scarlet G, Lithol Rubin GX, Permanent Red F5R, Brilliant Carmine 6B, Pigment Scarlet 3B, Bordeaux 5B, Toluidine Maroon, Permanent Bordeaux F2K, Helio Bordeaux BL, Bordeaux 10B, Bon Maroon Light, Bon Maroon Medium, Eosin Lake, Rhodamine Lake B, Rhodamine Lake Y, Alizarin Lake, Thioindigo Red B, Thioindigo Maroon, Oil Red, Quinacridone Red, Pyrazolone Red, Polyazo Red, Chrome Vermilion, Benzidine Orange, Perinone Orange, Oil Orange, Cobalt Blue, Cerulean Blue, Alkaline Blue Lake, Peacock Blue Lake, Victoria Blue Lake, Metal-free Phthalocyanine Blue, Phthalocyanine Blue, Fast Sky Blue, Indanthrene Blue (RS, BC), Indigo, Ultramarine Blue, Prussian Blue, Anthraquinone Blue, Fast Violet B, Methyl Violet Lake, Cobalt Purple, Manganese Purple, Dioxane Violet, Anthraquinone Violet, Chrome Green, Zinc Green, Chromium Oxide, Pyridian, Emerald Green, Pigment Green B, Naphthol Green B, Green Gold, Acid Green Lake,Examples include malachite green lake, phthalocyanine green, anthraquinone green, titanium oxide, zinc oxide, and lithopone.
[0310] The content of the colorant is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1 to 15 parts by mass, and more preferably 3 to 10 parts by mass, per 100 parts by mass of the toner.
[0311] The colorant can also be used as a masterbatch composited with a resin. Examples of resins to be produced by the masterbatch or kneaded with the masterbatch include, in addition to polyester resins, styrene or its substituted polymers such as polystyrene, poly-p-chlorostyrene, and polyvinyltoluene; styrene-p-chlorostyrene copolymers, styrene-propylene copolymers, styrene-vinyltoluene copolymers, styrene-vinylnaphthalene copolymers, styrene-methyl acrylate copolymers, styrene-ethyl acrylate copolymers, styrene-butyl acrylate copolymers, styrene-octyl acrylate copolymers, styrene-methyl methacrylate copolymers, styrene-ethyl methacrylate copolymers, styrene-butyl methacrylate copolymers, styrene-α-chloromethyl methacrylate copolymers, Styrene-based copolymers such as styrene-acrylonitrile copolymers, styrene-vinyl methyl ketone copolymers, styrene-butadiene copolymers, styrene-isoprene copolymers, styrene-acrylonitrile-indene copolymers, styrene-maleic acid copolymers, and styrene-maleic acid ester copolymers; polymethyl methacrylate, polybutyl methacrylate, polyvinyl chloride, polyvinyl acetate, polyethylene, polypropylene, polyester, epoxy resins, epoxy polyol resins, polyurethane, polyamide, polyvinyl butyral, polyacrylic acid resins, rosin, modified rosin, terpene resins, aliphatic or alicyclic hydrocarbon resins, aromatic petroleum resins, chlorinated paraffin, and paraffin wax. These may be used alone or in combination of two or more.
[0312] The master batch can be obtained by mixing and kneading the resin for the master batch and the colorant under high shear force. In this case, an organic solvent can be used to enhance the interaction between the colorant and the resin. In addition, a method called the flushing method, in which an aqueous paste containing water of the colorant is mixed and kneaded with the resin and the organic solvent, the colorant is transferred to the resin side, and the water and organic solvent components are removed, is also preferably used because the wet cake of the colorant can be used as it is and does not need to be dried. A high shear dispersing device such as a three-roll mill is preferably used for mixing and kneading.
[0313] (Charge control agent) The charge control agent is not particularly limited and can be appropriately selected depending on the purpose. Examples of the charge control agent include nigrosine dyes, triphenylmethane dyes, chromium-containing metal complex dyes, molybdic acid chelate pigments, rhodamine dyes, alkoxy amines, quaternary ammonium salts (including fluorine-modified quaternary ammonium salts), alkylamides, phosphorus simple substance or compounds, tungsten simple substance or compounds, fluorine-based activators, metal salicylic acid salts, and metal salts of salicylic acid derivatives.
[0314] Specific examples include the nigrosine dye Bontron 03, the quaternary ammonium salt Bontron P-51, the metal-containing azo dye Bontron S-34, the oxynaphthoic acid metal complex E-82, the salicylic acid metal complex E-84, and the phenol condensate E-89 (all manufactured by Orient Chemical Industry Co., Ltd.), the quaternary ammonium salt molybdenum complexes TP-302 and TP-415 (both manufactured by Hodogaya Chemical Co., Ltd.), LRA-901, the boron complex LR-147 (manufactured by Nippon Carlit Co., Ltd.), copper phthalocyanine, perylene, quinacridone, azo pigments, and other polymeric compounds having functional groups such as sulfonic acid groups, carboxyl groups, and quaternary ammonium salts.
[0315] The content of the charge control agent is not particularly limited and can be appropriately selected according to the purpose, but is preferably 0.1 to 10 parts by mass, more preferably 0.2 to 5 parts by mass, relative to 100 parts by mass of the toner. If the content exceeds 10 parts by mass, the chargeability of the toner is too high, the effect of the main charge control agent is reduced, and the electrostatic attraction force with the developing roller increases, which may lead to a decrease in the fluidity of the developer and a decrease in image density. These charge control agents can also be melt-kneaded together with the master batch and resin, and then dissolved and dispersed. In addition, these charge control agents may be added when directly dissolved and dispersed in an organic solvent, or may be attached to the surface of the toner base particles to prepare the toner and then fixed.
[0316] (Flow improver) The flowability improver is not particularly limited as long as it is capable of performing a surface treatment to increase hydrophobicity and prevent deterioration of flowability and charging properties even under high humidity, and can be appropriately selected according to the purpose, and examples thereof include silane coupling agents, silylating agents, silane coupling agents having a fluorinated alkyl group, organic titanate coupling agents, aluminum coupling agents, silicone oils, modified silicone oils, etc. It is particularly preferable to perform a surface treatment of silica and titanium oxide with such a flowability improver and use them as hydrophobic silica and hydrophobic titanium oxide.
[0317] (Cleaning improver) The cleaning property improver is not particularly limited as long as it is added to the toner to remove the developer remaining on the photoconductor or primary transfer medium after transfer, and can be appropriately selected depending on the purpose, and examples thereof include fatty acid metal salts such as zinc stearate, calcium stearate, and stearic acid, polymer fine particles produced by soap-free emulsion polymerization such as polymethyl methacrylate fine particles and polystyrene fine particles. The polymer fine particles preferably have a relatively narrow particle size distribution, and are preferably those having a volume average particle size of 0.01 μm to 1 μm.
[0318] (Magnetic material) The magnetic material is not particularly limited and may be appropriately selected depending on the purpose, and examples thereof include iron powder, magnetite, ferrite, etc. Among these, a white material is preferred in terms of color tone.
[0319] As described above, the toner according to the embodiment includes a plurality of organic fine particles at least partially embedded as an external additive on the surface of the toner base particle containing a polyester resin to form a core-shell structure, and the particle size distribution of the organic fine particles has two or more peaks. The toner according to the embodiment can improve the adhesion and storage stability of the toner and increase the reliability of the toner by covering at least a part of the surface of the toner base particle with organic fine particles having two or more different particle size distributions without inhibiting the fixing of the toner. That is, the organic fine particles include two types of organic fine particles, large particle size organic fine particles and small particle size organic fine particles. The large particle size organic fine particles can have a sharp particle size distribution, so that the adhesion and storage stability of the toner can be improved. On the other hand, when the large particle size organic fine particles cover the surface of the toner base particle, the surface of the toner becomes hard, and additives and the like are difficult to adhere to. The small particle size organic fine particles can reduce the fixing inhibition of the toner. In addition, the small particle size organic fine particles can fill the gaps between the large particle size organic fine particles, so that they can stably adhere to the surface of the toner base particle, so that the storage stability and adhesion of the toner are further improved, and the reliability of the toner is further increased. In addition, since large and small organic fine particles are present on the surface of the toner base particle, the toner according to one embodiment can have minute irregularities on the surface of the toner base particle due to the particle size difference between the large and small organic fine particles, and therefore additives other than the organic fine particles, such as inorganic fine particles, can be effectively attached.
[0320] In the toner according to one embodiment, the glass transition temperature Tg 1st The glass transition temperature Tga of the THF-insoluble component contained in the toner at the first heating step measured by DSC is 30°C to 60°C. 1st The glass transition temperature Tg of the THF-soluble component contained in the toner at the second heating time measured by DSC is -40°C to 10°C. 2ndThe glass transition temperature Tg of the toner is 45°C to 65°C. 1st , the glass transition temperature Tga of the component insoluble in THF 1st and the glass transition temperature Tg of the component soluble in THF 2nd However, if each of these is within the above range, the liberation rate of the external additive can be set to an optimal range, which makes it possible to achieve both high levels of low-temperature fixability and high-temperature storage stability while suppressing transfer defects and adhesion (filming) to charging members such as photoconductor drums, thereby suppressing deterioration in image quality.
[0321] Therefore, the toner according to the embodiment has excellent low-temperature fixing property and heat-resistant storage stability, and can suppress the occurrence of abnormal images. Therefore, the toner according to the embodiment can reduce power consumption during fixing, improve resistance to high temperature and high humidity during storage and transportation, and form good images.
[0322] In the toner according to the embodiment, the position of the peak P1 at the position where the particle diameter is the smallest among the two or more peaks can be set to 10 nm to 40 nm, and the position of the peak P2 at the position where the particle diameter is the largest can be set to 30 nm to 100 nm. This allows the large particle size organic fine particles and the small particle size organic fine particles to easily exert their respective functions, so that the storage stability and adhesive force of the toner can be further improved. In addition, since minute irregularities are more easily formed on the surface of the toner base particles, additives other than the organic fine particles can be more effectively attached. Therefore, the toner according to the embodiment has better low-temperature fixing property and heat-resistant storage stability, and can more effectively suppress the occurrence of abnormal images.
[0323] In the toner according to an embodiment, the average distance between adjacent organic fine particles on the surface of the toner base particle can be set to 100 nm or less, which ensures the adhesion and storage stability of the toner according to an embodiment, thereby ensuring low-temperature fixability and heat-resistant storage stability.
[0324] In the toner according to an embodiment, the organic fine particles can contain one or more kinds of styrene acrylic resins having carboxylic acid. This makes it possible to easily obtain two or more kinds of organic fine particles having different particle sizes while containing the same raw material. Therefore, the toner according to an embodiment has excellent low-temperature fixing property and heat-resistant storage stability more reliably, and can more reliably suppress the occurrence of abnormal images.
[0325] In the toner according to an embodiment, the organic fine particles are composed of two kinds of resins, and the organic fine particles can have a core layer containing one of the two kinds of resins and a shell layer that covers at least a part of the core layer and contains the other resin. If the organic fine particles have a core-shell structure composed of two kinds of resins, organic fine particles with different particle sizes can be easily formed. Therefore, the particle size distribution of the organic fine particles is likely to have two or more peaks. Therefore, the toner according to an embodiment can more reliably have unevenness on the surface.
[0326] The toner according to the embodiment has a glass transition temperature Tg 1st can be set to 30° C. to 70° C. This allows the toner according to one embodiment to have better low-temperature fixability and heat-resistant storage stability.
[0327] The toner according to the embodiment has a glass transition temperature Tg 1st and the glass transition temperature Tg in the second heating 2nd The difference between the glass transition temperature (Tg) and the 1st and glass transition temperature Tg 2nd When the organic fine particles have a core-shell structure composed of two types of resins, the toner can maintain its low-temperature fixability while maintaining the amount of the organic fine particles adhering to the surface of the toner base particle, if the difference between the temperature is 10° C. or more. Therefore, the toner according to one embodiment has low-temperature fixability and heat-resistant storage stability, and can also have improved filming resistance.
[0328] The toner according to the embodiment has a peak P1 of 20 nm to 40 nm and a peak P2 of 50 nm to 80 nm. This allows the large organic particles and the small organic particles to be more clearly separated, and each particle can reliably perform its function. Therefore, the toner according to the embodiment can further improve low-temperature fixing property and heat-resistant storage stability, and can further reliably suppress the occurrence of abnormal images.
[0329] In the toner according to an embodiment, the component insoluble in THF may have at least one of a urethane bond and a urea bond, which enhances the rubber-like properties of the polyester resin, thereby allowing the toner according to an embodiment to have better heat-resistant storage stability and high-temperature offset resistance.
[0330] In the toner according to an embodiment, the polyester resin may contain a crystalline polyester, which may enable the toner according to an embodiment to have better low-temperature fixability and heat-resistant storage stability.
[0331] <Toner manufacturing method> The method for producing the toner according to the embodiment is not particularly limited and may be appropriately selected depending on the purpose, and examples thereof include a wet granulation method, a pulverization method, and the like. Examples of the wet granulation method include a dissolution suspension method, an emulsion aggregation method, and the like. In view of molecular scission due to kneading of the binder resin and the difficulty of uniformly kneading high molecular weight resin and low molecular weight resin, the dissolution suspension method or the emulsion aggregation method, which is a production method that does not involve kneading of the binder resin, is preferred, and in view of increasing the uniformity of the resin contained in the toner, the dissolution suspension method is more preferred. A case where the dissolution suspension method is used as the method for producing the toner according to the embodiment will be described.
[0332] The toner manufacturing method according to one embodiment preferably includes a granulation step of granulating toner base particles and adhering organic fine particles to the surfaces thereof by dispersing an oil phase containing a polyester resin and, if necessary, a release agent, a colorant, etc., in an aqueous medium containing organic fine particles.
[0333] The polyester resin may include a non-crystalline polyester resin which is a prepolymer having a urethane bond and / or a urea bond, and a non-crystalline polyester resin which does not have a urethane bond and / or a urea bond, and preferably a crystalline polyester resin.
[0334] In the toner manufacturing method according to an embodiment, in the granulation step, it is more preferable to use an oil phase containing a modified polyester, a hardener, and the like, in addition to a release agent and a colorant, as necessary.
[0335] Furthermore, in the toner manufacturing method according to an embodiment, in the above-mentioned granulation step, for example, a method can be used in which toner base particles are manufactured while the amorphous polyester resin is elongated by an elongation reaction and / or a crosslinking reaction between a prepolymer and a curing agent.
[0336] A method for producing a toner according to one embodiment includes a step of preparing an aqueous medium (aqueous medium preparation step), a step of preparing an oil phase containing toner materials (oil phase preparation step), a step of emulsifying or dispersing the toner materials (emulsifying or dispersing step), and a step of removing an organic solvent (organic solvent removal step).
[0337] (Preparation of aqueous medium) The aqueous medium (aqueous phase) can be prepared, for example, by dispersing resin particles and organic fine particles in the aqueous medium. The amount of resin particles added to the aqueous medium is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0.5 parts by mass to 10 parts by mass relative to 100 parts by mass of the aqueous medium.
[0338] The aqueous medium is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include water, a solvent miscible with water, and a mixture thereof. These may be used alone or in combination of two or more. Among these, water is preferred.
[0339] The solvent miscible with water can be appropriately selected depending on the purpose, and examples thereof include alcohol, lower ketones, dimethylformamide, tetrahydrofuran, cellosolves, etc. The alcohol is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include methanol, isopropanol, ethylene glycol, etc. The lower ketones can be appropriately selected depending on the purpose, and examples thereof include acetone, methyl ethyl ketone, etc.
[0340] (Oil phase preparation process) The oil phase containing the toner materials includes a crystalline polyester resin, a non-crystalline polyester resin which is a prepolymer having at least one of a urethane bond and a urea bond, and a non-crystalline polyester resin which does not have a urethane bond or a urea bond, and can be prepared by dissolving or dispersing the toner materials, which further include, as necessary, a crystalline polyester resin, a hardener, a release agent, a colorant, and the like, in an organic solvent.
[0341] The organic solvent is not particularly limited and can be appropriately selected depending on the purpose, but an organic solvent having a boiling point of less than 150° C. is preferred in terms of ease of removal.
[0342] The organic solvent having a boiling point of less than 150° C. is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include toluene, xylene, benzene, carbon tetrachloride, methylene chloride, 1,2-dichloroethane, 1,1,2-trichloroethane, trichloroethylene, chloroform, monochlorobenzene, dichloroethylidene, methyl acetate, ethyl acetate, methyl ethyl ketone, methyl isobutyl ketone, etc. These may be used alone or in combination of two or more.
[0343] Among these, ethyl acetate, toluene, xylene, benzene, methylene chloride, 1,2-dichloroethane, chloroform, carbon tetrachloride, etc. are preferable, and ethyl acetate is more preferable.
[0344] (Emulsification or dispersion process) The toner materials can be emulsified or dispersed by dispersing the oil phase containing the toner materials in an aqueous medium, and organic fine particles can be arranged on the surfaces of the toner base particles.
[0345] Furthermore, when the toner materials are emulsified or dispersed, an elongation reaction and / or a crosslinking reaction occurs between the curing agent and the prepolymer, thereby producing an amorphous polyester resin.
[0346] The reaction conditions (reaction time, reaction temperature) for producing the prepolymer are not particularly limited, and can be appropriately selected depending on the combination of the curing agent and the prepolymer.
[0347] The reaction time is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 10 minutes to 40 hours, more preferably 2 hours to 24 hours.
[0348] The reaction temperature is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 0°C to 150°C, more preferably 40°C to 98°C.
[0349] The method for stably forming a dispersion liquid containing a prepolymer in an aqueous medium is not particularly limited and may be appropriately selected depending on the purpose. For example, there is a method in which an oil phase prepared by dissolving or dispersing a toner material in a solvent is added to an aqueous medium phase, and the oil phase is dispersed by shear force.
[0350] The dispersing machine for dispersion is not particularly limited and can be appropriately selected depending on the purpose. Examples of the dispersing machine include a low-speed shear type dispersing machine, a high-speed shear type dispersing machine, a friction type dispersing machine, a high-pressure jet type dispersing machine, and an ultrasonic dispersing machine.
[0351] Among these, a high-speed shear type disperser is preferred because it is possible to control the particle size of the dispersion (oil droplets) to 2 μm to 20 μm.
[0352] When a high-speed shear type dispersing machine is used, the conditions such as the rotation speed, dispersing time, and dispersing temperature can be appropriately selected depending on the purpose.
[0353] The rotation speed is preferably from 1000 rpm to 30000 rpm, and more preferably from 5000 rpm to 20000 rpm.
[0354] The dispersion time can be appropriately selected depending on the purpose, but in the case of a batch method, it is preferably 0.1 to 5 minutes.
[0355] The dispersion temperature can be appropriately selected depending on the purpose, but is preferably from 0° C. to 150° C. under pressure, and more preferably from 20° C. to 98° C. In general, the higher the dispersion temperature, the easier the dispersion.
[0356] The amount of the aqueous medium used when emulsifying or dispersing the toner material is not particularly limited and can be appropriately selected according to the purpose, but is preferably 50 parts by mass to 2000 parts by mass, more preferably 100 parts by mass to 100 parts by mass of the toner material. If the amount of the aqueous medium used is less than 50 parts by mass, the dispersion state of the toner material may become poor, and toner base particles of a predetermined particle size may not be obtained. If the amount of the aqueous medium used is more than 2000 parts by mass, the production cost may increase.
[0357] When emulsifying or dispersing the oil phase containing the toner materials, it is preferable to use a dispersant from the viewpoints of stabilizing the dispersion such as oil droplets, forming a desired shape, and sharpening the particle size distribution.
[0358] The dispersant is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include surfactants, poorly water-soluble inorganic compound dispersants, polymer-based protective colloids, etc. These may be used alone or in combination of two or more. Among these, surfactants are preferred.
[0359] The surfactant is not particularly limited and can be appropriately selected depending on the purpose. For example, anionic surfactants, cationic surfactants, nonionic surfactants, amphoteric surfactants, etc. can be used.
[0360] The anionic surfactant is not particularly limited and may be appropriately selected depending on the purpose, and examples thereof include alkylbenzene sulfonate, α-olefin sulfonate, phosphate, etc. Among these, those having a fluoroalkyl group are preferred.
[0361] (Organic solvent removal process) Toner base particles are obtained by removing the organic solvent from the dispersion liquid such as the emulsified slurry. The method for removing the organic solvent from the dispersion liquid is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include a method of gradually increasing the temperature of the entire reaction system to evaporate the organic solvent in the oil droplets, and a method of spraying the dispersion liquid in a dry atmosphere to remove the organic solvent in the oil droplets.
[0362] Once the organic solvent is removed, toner base particles are formed.
[0363] The toner manufacturing method may include at least one of a washing step for washing the toner base particles, a drying step for drying the toner base particles, a classification step for classifying the toner base particles, an addition step for mixing an external additive, a charge control agent, etc. with the toner base particles, etc. This allows the toner base particles to be washed, dried, classified, have external additives added, etc.
[0364] (Cleaning process) A part or all of the resin (a1) covering at least a part of the surface of the toner base particle can be removed by washing. In the washing step, a method for removing a part or all of the resin (a1) can be a method for removing a part or all of (a1) by a chemical method. Among the removal steps by chemical methods, a preferred method is a method in which an alkaline aqueous solution is added to the toner base particle and mixed to dissolve a part or all of the resin (a1).
[0365] Examples of the alkali in the alkaline aqueous solution include hydroxides of alkali metals such as potassium hydroxide and sodium hydroxide, and ammonia, etc. From the viewpoint of easiness in dissolving the resin (a1), potassium hydroxide and sodium hydroxide are preferred.
[0366] The pH of the alkali contained in the alkaline aqueous solution is preferably 8-14, and more preferably 10-12.
[0367] In the washing step, the toner base particles and the alkaline aqueous solution can be mixed by, for example, dropping the alkaline aqueous solution into the toner base slurry under stirring. An acid aqueous solution may also be dropped to neutralize the mixture.
[0368] (drying process) The toner base particles after washing are dried. There are no particular limitations on the method for drying the toner base particles, and any method that can dry the toner base particles can be used.
[0369] (Classification process) The toner base particles after drying are classified to recover toner base particles having a desired particle size. Classification may be performed by removing fine particles in a liquid using a cyclone, a decanter, centrifugal separation, or the like.
[0370] Next, the mixture is passed through a sieve of 250 mesh or more to remove coarse particles and agglomerated particles.
[0371] (addition process) The toner base particles obtained by classification are mixed with external additives, charge control agents, etc. At this time, by applying a mechanical impact force, it is possible to suppress the particles of the external additives, etc. from being detached from the surfaces of the toner base particles.
[0372] The method of applying the mechanical impact force can be appropriately selected depending on the purpose, and examples thereof include a method of applying an impact force to the mixture using a blade rotating at high speed, a method of introducing the mixture into a high-speed air current to accelerate it, and causing particles to collide with each other or with an appropriate collision plate, etc.
[0373] The device used in the method of applying a mechanical impact force can be appropriately selected depending on the purpose, and examples include an Angmill (manufactured by Hosokawa Micron Corporation), a device obtained by modifying an I-type mill (manufactured by Japan Pneumatic Mfg. Co., Ltd.) to reduce the grinding air pressure, a Hybridization System (manufactured by Nara Machinery Works, Ltd.), a Cryptron System (manufactured by Kawasaki Heavy Industries, Ltd.), an automatic mortar, and the like.
[0374] The toner according to one embodiment is obtained by adhering particles of an external additive or the like to the surfaces of the toner base particles.
[0375] <Developer> The developer according to an embodiment includes the toner according to an embodiment, and may include other appropriately selected components such as a carrier, etc., as necessary. As a result, the developer according to an embodiment has excellent low-temperature fixing properties and heat-resistant storage stability, can suppress the occurrence of abnormal images, and can form high-quality images.
[0376] The developer may be a one-component developer or a two-component developer. However, when used in high-speed printers that correspond to the improvement of information processing speed, a two-component developer is preferable from the viewpoint of improving the developer life.
[0377] When the toner according to one embodiment is used in a one-component developer, even if the toner is balanced, there is little variation in the particle size of the toner, there is little filming of the toner on the developing roller, and there is little melting of the toner to components such as blades that thin the toner layer, and good and stable developability and images can be obtained even with long-term stirring in the developing device.
[0378] When the toner according to the embodiment is used as a two-component developer, it can be mixed with a carrier and used as a developer. When the developer is used as a two-component developer, even if the toner is balanced over a long period of time, the particle size of the toner is less likely to fluctuate, and good and stable developability and images can be obtained even when the toner is stirred for a long period of time in a developing device.
[0379] The content of the carrier in the two-component developer can be appropriately selected depending on the purpose, but is preferably 90 parts by mass to 98 parts by mass, and more preferably 93 parts by mass to 97 parts by mass, relative to 100 parts by mass of the two-component developer.
[0380] The developer according to an embodiment can be suitably used for image formation by various known electrophotographic methods such as a magnetic one-component development method, a non-magnetic one-component development method, and a two-component development method.
[0381] [Career] The carrier is not particularly limited and can be appropriately selected depending on the purpose, but it is preferable that the carrier has a core material and a resin layer (coating layer) that coats the core material.
[0382] (Core material) The material of the core material is not particularly limited and can be appropriately selected according to the purpose. For example, manganese-strontium-based material of 50 emu / g to 90 emu / g, manganese-magnesium-based material of 50 emu / g to 90 emu / g, etc. can be mentioned. In order to ensure image density, it is preferable to use high magnetization materials such as iron powder of 100 emu / g or more, magnetite of 75 emu / g to 120 emu / g. In addition, it is preferable to use low magnetization materials such as copper-zinc-based materials of 30 emu / g to 80 emu / g, because it can reduce the impact of the developer in a standing state on the photoconductor and is advantageous for high image quality. These materials may be used alone or in combination of two or more.
[0383] The volume average particle diameter of the core material is not particularly limited and can be appropriately selected according to the purpose, but is preferably 10 μm to 150 μm, more preferably 40 μm to 100 μm. If the volume average particle diameter is 10 μm or more, the increase in fine powder in the carrier can be suppressed, so that the decrease in magnetization per particle can be suppressed and the scattering of the carrier can be suppressed. On the other hand, if the volume average particle diameter is 150 μm or less, the specific surface area can be secured, so that the scattering of the toner can be suppressed, and the deterioration of the reproduction of the solid parts can be suppressed, especially in full color with many solid parts.
[0384] (Resin layer) The resin layer can contain a resin and other components as necessary. The resin used in the resin layer can be a known material that can impart the necessary electrostatic property. Specifically, it is preferable to use a silicone resin, an acrylic resin, or a combination of these. In addition, the composition for forming the resin layer preferably contains a silane coupling agent.
[0385] The average thickness of the resin layer is preferably 0.05 μm to 0.50 μm.
[0386] <Developer container> The developer storage container according to the embodiment stores the developer according to the embodiment. The developer storage container is not particularly limited and can be appropriately selected from known containers, and examples of the developer storage container include a container body and a cap.
[0387] In addition, the size, shape, structure, material, etc. of the container body are not particularly limited, but the shape is preferably cylindrical or the like, and a spiral-shaped irregularity is formed on the inner surface so that, by rotating, the developer content can move to the discharge outlet side, and it is particularly preferable that some or all of the spiral-shaped irregularity has a bellows function.
[0388] The material of the container body is not particularly limited, but it is preferable that the material has good dimensional accuracy, and examples of the material include resin materials such as polyester resin, polyethylene resin, polypropylene resin, polystyrene resin, polyvinyl chloride resin, polyacrylic acid, polycarbonate resin, ABS resin, and polyacetal resin.
[0389] The developer storage container is easy to store, transport, and the like, and has excellent handleability, and therefore can be detachably attached to an image forming apparatus, a process cartridge, and the like, which will be described later, and used for replenishing the developer.
[0390] <Toner storage unit> The toner storage unit according to the embodiment can store the toner according to the embodiment. The toner storage unit according to the embodiment refers to a unit having a function of storing toner and storing the toner. Here, examples of the toner storage unit include a toner storage container, a developing unit, and a process cartridge.
[0391] The toner storage container refers to a container that stores toner.
[0392] The developing device has a means for containing toner and developing the toner.
[0393] The process cartridge is a cartridge that integrates at least an electrostatic latent image carrier (also called an image carrier) and a developing means, contains toner, and is detachable from an image forming apparatus. The process cartridge may further include at least one selected from a charging means, an exposure means, a cleaning means, etc.
[0394] The toner storage unit according to the embodiment stores the toner according to the embodiment. By mounting the toner storage unit according to the embodiment on an image forming apparatus and forming an image, the toner storage unit according to the embodiment is used to form an image. Therefore, the toner storage unit according to the embodiment has excellent low-temperature fixing properties and heat-resistant storage stability, can suppress the occurrence of abnormal images, and can form high-quality images.
[0395] <Image forming device> An image forming apparatus according to one embodiment has an electrostatic latent image carrier, an electrostatic latent image forming unit that forms an electrostatic latent image on the electrostatic latent image carrier, and a developing unit that develops the electrostatic latent image formed on the electrostatic latent image carrier with toner to form a toner image, and may further have other components as necessary.
[0396] More preferably, the image forming apparatus according to one embodiment includes, in addition to the electrostatic latent image carrier, electrostatic latent image forming unit, and developing unit described above, a transfer unit that transfers the toner image onto the recording medium, and a fixing unit that fixes the transferred image onto the surface of the recording medium.
[0397] In the developing section, the toner according to the embodiment is used. Preferably, a developer containing the toner according to the embodiment and, if necessary, other components such as a carrier may be used to form a toner image.
[0398] (Electrostatic latent image carrier) The material, shape, structure, size, etc. of the electrostatic latent image carrier (sometimes called "electrophotographic photoreceptor" or "photoreceptor") are not particularly limited and can be appropriately selected from known materials. Examples of materials for the electrostatic latent image carrier include inorganic photoreceptors such as amorphous silicon and selenium, and organic photoreceptors (OPC) such as polysilane and phthalopolymethine. Among these, amorphous silicon is preferred in terms of long life.
[0399] As the amorphous silicon photoreceptor, for example, a photoreceptor having a photoconductive layer made of a-Si formed on the support by heating the support to 50° C. to 400° C. and forming a film on the support by a vacuum deposition method, a sputtering method, an ion plating method, a thermal CVD (chemical vapor deposition) method, a photo CVD method, a plasma CVD method, etc. Among these, the plasma CVD method, that is, a method in which a raw material gas is decomposed by a direct current, a high frequency wave, or a microwave glow discharge to form an a-Si deposition film on the support, is preferable.
[0400] The shape of the electrostatic latent image carrier is not particularly limited and can be appropriately selected depending on the purpose, but is preferably cylindrical. The outer diameter of the cylindrical electrostatic latent image carrier is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 3 mm to 100 mm, more preferably 5 mm to 50 mm, and particularly preferably 10 mm to 30 mm.
[0401] (Electrostatic latent image forming section) The electrostatic latent image forming unit is not particularly limited as long as it is a means for forming an electrostatic latent image on an electrostatic latent image carrier, and can be appropriately selected according to the purpose. The electrostatic latent image forming unit includes, for example, a charging member (charger) that uniformly charges the surface of the electrostatic latent image carrier, and an exposure member (exposure device) that imagewise exposes the surface of the electrostatic latent image carrier.
[0402] The charger is not particularly limited and can be appropriately selected depending on the purpose. Examples of the charger include a contact charger equipped with a conductive or semiconductive roll, brush, film, rubber blade, etc., and a non-contact charger that utilizes corona discharge such as a corotron or scorotron.
[0403] The shape of the charger may be any shape, such as a roller, a magnetic brush, a fur brush, etc., and can be selected according to the specifications and shape of the image forming apparatus.
[0404] The charger is preferably one that is arranged in contact or non-contact with the electrostatic latent image carrier and charges the surface of the electrostatic latent image carrier by applying superimposed DC and AC voltages to the electrostatic latent image carrier. Also, the charger is preferably a charging roller that is arranged in close proximity to the electrostatic latent image carrier in a non-contact manner via a gap tape and charges the surface of the electrostatic latent image carrier by applying superimposed DC and AC voltages to the charging roller.
[0405] The charger is not limited to a contact type charger, but it is preferable to use a contact type charging member since it provides an image forming apparatus in which the amount of ozone generated from the charger is reduced.
[0406] The exposure device is not particularly limited as long as it can expose the surface of the electrostatic latent image carrier charged by the charger in the shape of an image to be formed, and can be appropriately selected depending on the purpose. Examples of the exposure device include various exposure devices such as a copying optical system, a rod lens array system, a laser optical system, and a liquid crystal shutter optical system.
[0407] The light source used in the exposure device is not particularly limited and can be appropriately selected depending on the purpose. Examples of the light source include fluorescent lamps, tungsten lamps, halogen lamps, mercury lamps, sodium lamps, light-emitting diodes (LEDs), semiconductor lasers (LDs), electroluminescence (EL), and other light-emitting materials in general.
[0408] In order to irradiate only light in a desired wavelength range, various filters such as a sharp cut filter, a band pass filter, a near infrared cut filter, a dichroic filter, an interference filter, and a color temperature conversion filter can be used.
[0409] It is also possible to employ a backlight system in which exposure is performed imagewise from the back side of the electrostatic latent image bearing member.
[0410] (Developing section) The developing unit is not particularly limited as long as it can develop the electrostatic latent image formed on the electrostatic latent image carrier to form a visible image, and can be appropriately selected according to the purpose. For example, the developing unit can be suitably used one that contains toner and has a developing device that can apply the toner to the electrostatic latent image in a contact or non-contact manner, and a developing device equipped with a toner container is preferable.
[0411] The developing device may be a single-color developing device or a multi-color developing device. As the developing device, for example, a developing device having an agitator that frictionally agitates the toner to charge it, a magnetic field generating unit fixed inside, and a rotatable developer carrier that carries a developer containing toner on its surface is preferable.
[0412] (Transfer section) The transfer section preferably has a first transfer section that transfers a visible image onto an intermediate transfer body to form a composite transfer image, and a second transfer section that transfers the composite transfer image onto a recording medium. The intermediate transfer body is not particularly limited and can be appropriately selected from known transfer bodies depending on the purpose, and a transfer belt or the like is preferably used.
[0413] The transfer section (first transfer means and secondary transfer section) preferably has at least a transfer device that peels and charges a visible image formed on an electrostatic latent image carrier (photoconductor) onto a recording medium. The number of transfer sections may be one or more.
[0414] Examples of the transfer device include a corona transfer device using corona discharge, a transfer belt, a transfer roller, a pressure transfer roller, and an adhesive transfer device.
[0415] The recording medium is typically plain paper, but there are no particular limitations as long as it is capable of transferring the unfixed image after development, and it can be selected appropriately according to the purpose. A PET base for overhead projectors can also be used.
[0416] (Fixing part) The fixing unit is not particularly limited and can be appropriately selected depending on the purpose, but a known heating and pressing unit is suitable. Examples of the heating and pressing unit include a combination of a heating roller and a pressure roller, and a combination of a heating roller, a pressure roller, and an endless belt.
[0417] The fixing section is preferably a heating and pressurizing section having a heating element having a heat generating element, a film in contact with the heating element, and a pressure member in pressure contact with the heating element via the film, and capable of heat-fixing the recording medium on which an unfixed image has been formed by passing the recording medium between the film and the pressure member.
[0418] The heating temperature in the heating and pressurizing section is usually preferably 80°C to 200°C.
[0419] The surface pressure in the heating and pressing section is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 10 N / cm 2 ~80N / cm 2 It is preferable that:
[0420] In this embodiment, depending on the purpose, for example, a known optical fixing device may be used together with or instead of the fixing unit.
[0421] (others) The image forming apparatus according to the first embodiment may further include, for example, a static eliminator, a recycle unit, a controller, and the like.
[0422] ((Static charge removal section)) The charge removing section is not particularly limited as long as it can apply a charge removing bias to the electrostatic latent image bearing member, and can be appropriately selected from among known charge removers. For example, a charge removing lamp or the like is preferably used.
[0423] (Cleaning section) The cleaning unit may be any type capable of removing the toner remaining on the electrostatic latent image carrier, and may be appropriately selected from among known cleaners. Examples of the cleaning unit include a magnetic brush cleaner, an electrostatic brush cleaner, a magnetic roller cleaner, a blade cleaner, a brush cleaner, and a web cleaner.
[0424] The image forming apparatus according to the first embodiment has a cleaning section, which improves the cleaning performance. That is, by controlling the adhesion between toner particles, the fluidity of the toner is controlled, and the cleaning performance can be improved. In addition, by controlling the characteristics of the toner after deterioration, it is possible to maintain excellent cleaning quality even under severe conditions such as a long life or high temperature and humidity. Furthermore, since the external additive can be sufficiently liberated from the toner on the photoreceptor, a deposition layer (dam layer) of the external additive in the cleaning blade nip can be formed, thereby achieving high cleaning performance.
[0425] (Recycling Department) The recycling section is not particularly limited, and examples thereof include known conveying means.
[0426] ((Control Unit)) The control unit can control the movement of each of the above-mentioned parts. The control unit is not particularly limited as long as it can control the movement of each of the above-mentioned parts, and can be appropriately selected depending on the purpose. For example, the control unit can be a control device such as a sequencer or a computer.
[0427] The image forming apparatus according to one embodiment can form images using the toner according to one embodiment, and therefore has excellent low-temperature fixing properties and heat-resistant storage properties, can suppress the occurrence of abnormal images, and can provide high-quality images.
[0428] <Image forming method> An image forming method according to an embodiment includes an electrostatic latent image forming step of forming an electrostatic latent image on an electrostatic latent image carrier, and a developing step of developing the electrostatic latent image with toner to form a toner image, and may further include other steps as necessary. The image forming method can be suitably performed by the image forming apparatus, the electrostatic latent image forming step can be suitably performed by the electrostatic latent image forming unit, the developing step can be suitably performed by the developing unit, and the other steps can be suitably performed by the other units.
[0429] Furthermore, the image forming method according to one embodiment more preferably includes, in addition to the electrostatic latent image forming process and the developing process described above, a transfer process of transferring the toner image onto a recording medium, and a fixing process of fixing the transferred image onto the surface of the recording medium.
[0430] In the developing step, the toner according to an embodiment is used. Preferably, a developer containing the toner according to an embodiment and, if necessary, other components such as a carrier may be used to form a toner image.
[0431] The electrostatic latent image forming process is a process of forming an electrostatic latent image on an electrostatic latent image carrier, and includes a charging process of charging the surface of the electrostatic latent image carrier and an exposure process of exposing the charged surface of the electrostatic latent image carrier to light to form an electrostatic latent image. Charging can be performed, for example, by applying a voltage to the surface of the electrostatic latent image carrier using a charger. Exposure can be performed, for example, by exposing the surface of the electrostatic latent image carrier to light in an imagewise manner using an exposure device. The electrostatic latent image can be formed, for example, by uniformly charging the surface of the electrostatic latent image carrier and then exposing it to light in an imagewise manner, and can be performed by an electrostatic latent image forming unit.
[0432] The developing process is a process of sequentially developing the electrostatic latent image with toners of multiple colors to form a visible image. The formation of the visible image can be performed, for example, by developing the electrostatic latent image with toners, and can be performed by a developing device.
[0433] In the developing device, for example, toner and carrier are mixed and stirred, and the toner becomes charged by friction during this process and is held in a standing state on the surface of the rotating magnet roller, forming a magnetic brush. Since the magnet roller is disposed near an electrostatic latent image carrier (photoconductor), a part of the toner constituting the magnetic brush formed on the surface of the magnet roller moves to the surface of the electrostatic latent image carrier (photoconductor) by electrical attraction. As a result, the electrostatic latent image is developed by the toner, and a visible image made of the toner is formed on the surface of the electrostatic latent image carrier (photoconductor).
[0434] The transfer step is a step of transferring a visible image to a recording medium. The transfer step is preferably performed using an intermediate transfer body, and after the visible image is primarily transferred onto the intermediate transfer body, the visible image is secondarily transferred onto the recording medium. The transfer step is more preferably performed using toner of two or more colors, preferably full-color toner, and includes a primary transfer step of transferring the visible image onto the intermediate transfer body to form a composite transfer image, and a secondary transfer step of transferring the composite transfer image onto the recording medium. The transfer can be performed, for example, by charging an electrostatic latent image carrier (photoconductor) with a transfer charger, and can be performed by a transfer section.
[0435] The fixing process is a process in which the visible image transferred to the recording medium is fixed using a fixing device, and may be performed for each color developer each time it is transferred to the recording medium, or may be performed simultaneously for each color developer in a stacked state.
[0436] The image forming method according to the first embodiment may further include other steps appropriately selected as necessary, such as a static elimination step, a cleaning step, a recycling step, and the like.
[0437] The charge removing step is a step of removing electricity by applying a charge removing bias to the electrostatic latent image bearing member, and can be suitably performed by the charge removing unit.
[0438] The cleaning step is a step of removing the toner remaining on the electrostatic latent image carrier, and can be suitably performed by a cleaning unit.
[0439] The recycling step is a step in which the toner removed in the cleaning step is recycled to the developing unit, and can be suitably carried out by the recycling unit.
[0440] The image forming method according to one embodiment can form an image using the toner according to one embodiment, and therefore has excellent low-temperature fixing properties and heat-resistant storage stability, can suppress the occurrence of abnormal images, and can provide high-quality images.
[0441] [One embodiment of the image forming apparatus] One aspect of an image forming apparatus according to an embodiment will be described with reference to Fig. 3. The image forming apparatus is not particularly limited as long as it is an apparatus that forms an image using toner, such as a printer, a copier, a facsimile, or a multifunction machine, and Fig. 3 will be used to explain the case where the image forming apparatus according to this embodiment is a printer.
[0442] 4 is a schematic diagram showing an example of an image forming apparatus according to an embodiment. As shown in FIG. 4, an electrophotographic image forming apparatus (printer) 1 includes a paper feed section 10, a conveyance section 20, an image forming section 30, a transfer section 40, a fixing section 50, and a toner cartridge 60.
[0443] The paper feed section 10 includes a paper feed cassette 11 in which paper P to be fed is stacked, and a paper feed roller 12 that feeds the paper P stacked in the paper feed cassette 11 one sheet at a time.
[0444] The paper feed cassettes 11 are disposed below the exposure unit 32. Each paper feed cassette 11 contains a stack of transfer paper P, which is a recording medium.
[0445] The paper feed roller 12 is disposed so as to come into contact with the topmost sheet of transfer paper P in the paper feed cassette 11 .
[0446] In the paper feed section 10, when the paper feed roller 12 is driven to rotate counterclockwise in the figure by the driving means, the topmost transfer sheet P in the paper feed cassette 11 is discharged from the right side of the paper feed cassette 11 in Figure 4 toward the conveying section 20. The discharged transfer sheet P is sandwiched between the rollers of the conveying roller 21 and conveyed from the bottom to the top in Figure 4.
[0447] The conveying section 20 includes a conveying roller 21 that conveys the transfer paper P fed by the paper feed roller 12 toward the transfer section 40, a pair of timing rollers 22 that hold the leading edge of the transfer paper P conveyed by the conveying roller 21 and wait, and send the paper to the transfer section 40 at a predetermined timing, a paper discharge roller 23 that discharges the paper P with the fixed color toner image onto a paper discharge tray 24, and a paper discharge tray 124 into which the paper P discharged from the paper discharge roller 23 is fed.
[0448] The transport rollers 21 are disposed so as to sandwich the transfer sheet P, and transport the transfer sheet P from the lower side to the upper side in FIG.
[0449] The timing roller 22 is disposed at the downstream end in the transport direction of the transport roller 21. As soon as the timing roller 22 sandwiches the transfer paper P sent from the transport roller 21 between the rollers, the timing roller 22 temporarily stops the rotation of both rollers. Then, the timing roller 22 sends the transfer paper P sandwiched between the rollers toward the secondary transfer nip at a timing that allows the transfer paper P to be synchronized with the four-color toner image on the intermediate transfer belt 43.
[0450] The paper discharge roller 23 is a roller that discharges the transfer paper P to the outside of the printer 100 after the fixing process has been performed.
[0451] The paper discharge tray 24 is provided on the upper surface of the housing of the main body of the printer 100, and stacks the transfer paper P discharged to the outside of the printer 100 by the paper discharge rollers 23.
[0452] The image forming section 30 includes four imaging units 31Y, 31C, 31M and 31K for yellow, magenta, cyan and black (hereinafter referred to as Y, C, M and K, respectively), and an exposure device 32 which is a latent image forming section.
[0453] The imaging units 31Y, 31C, 31M, and 31K are arranged in order from left to right in the drawing at a predetermined interval, and are arranged side by side so as to face the intermediate transfer belt 141. The imaging units 31Y, 31C, 31M, and 31K form images using developers containing Y toner, C toner, M toner, and K toner, respectively. The developers contain toner and carrier. The four imaging units 31Y, 31C, 31M, and 31K each use a different type of developer.
[0454] The configurations of the imaging units 31Y, 31C, 31M, and 31K will be described. Note that the imaging units 31Y, 31C, 31M, and 31K are similar except for the toner colors, so only the configuration of the imaging unit 31Y will be described, and the configurations of the other imaging units 31C, 31M, and 31K will not be described.
[0455] The imaging unit 31Y incorporates a drum-shaped photoconductor 311Y, a charging device 312Y, a developing device 313Y, a photoconductor cleaning device 314, a lubricant application device (not shown), a cleaning roller, a static electricity removal lamp, etc. into one unit as a process cartridge, which is detachable from the image forming apparatus 1. Around the photoconductor 11Y, the photoconductor 311Y, the charging device 312Y, the developing device 313Y, the photoconductor cleaning device 314, a lubricant application device (not shown), a cleaning roller, a static electricity removal lamp, etc. are arranged.
[0456] Although the photoconductor 311Y is shown to have a drum shape, it may also be in the form of a sheet or an endless belt.
[0457] The charging device 312Y may be a known device such as a corotron, a scorotron, or a solid-state charger. Of these charging methods, the contact charging method and the non-contact close-by arrangement method are more preferable, and have the advantages of increasing charging efficiency, reducing the amount of ozone generated, and enabling the device to be made smaller. In this embodiment, the charging device 312Y includes a charging roller 3121Y, which is a charging member, and uses a non-contact close-by arrangement method in which the charging roller 3121Y is placed close to the photoconductor 311Y at a predetermined distance and in a non-contact manner. The charging roller 3121Y is placed in a non-contact manner with the photoconductor 311Y, and charges the photoconductor 311Y to a predetermined polarity and a predetermined potential. The surface of the photoconductor 311Y, which is uniformly charged by the charging roller 3121Y, is irradiated with a laser beam L from the exposure device 32 based on image information, and an electrostatic latent image is formed.
[0458] The developing device 313Y converts the latent image formed on the surface of the photoconductor 311Y into a toner image. The developing device 313Y has a developing roller 3131Y as a developer carrier. A developing bias is applied to the developing roller 3131Y from a power source.
[0459] In the developing device 13Y, the toner in the developer is charged to a predetermined polarity. Then, the developer is pumped up onto the surface of the developing roller 3131Y, and the toner of the pumped up developer adheres to the latent image on the photoconductor 311Y in a developing area facing the photoconductor 311Y.
[0460] The photoconductor cleaning device 314 cleans the toner remaining on the photoconductor 311Y after the toner image is transferred to the intermediate transfer belt 43 included in the transfer unit 40. The photoconductor cleaning device 314Y may have a fur brush, a cleaning blade, or the like.
[0461] A lubricant application device (not shown) applies a lubricant onto the surface of the photoconductor 311Y after it has been cleaned by the photoconductor cleaning device 314Y.
[0462] The cleaning roller (not shown) cleans the charging roller 3121Y.
[0463] A charge removing lamp (not shown) removes the surface potential of the photoconductor 311Y after cleaning.
[0464] The exposure device 32 is disposed below the imaging units 31Y, 31C, 31M, and 31K. The exposure device 32 irradiates the photoconductors 311Y, 311C, 311M, and 311K with laser light L emitted based on image information. As a result, electrostatic latent images for Y, C, M, and K are formed on the photoconductors 311Y, 311C, 311M, and 311K.
[0465] The exposure unit 32 includes a polygon mirror 321 that is rotated by a motor to irradiate laser light L emitted from a light source. The exposure unit 32 irradiates the laser light L onto photoconductors 311Y, 311C, 311M, and 311K via a plurality of optical lenses and mirrors while deflecting the laser light L by the polygon mirror 321. Note that the exposure unit 32 may include an LED array for optical scanning instead of the above configuration.
[0466] The light source for the laser light L of the exposure device 32 and the light source for the discharge lamp can be any light-emitting material such as a fluorescent lamp, a tungsten lamp, a halogen lamp, a mercury lamp, a sodium lamp, a light-emitting diode (LED), a semiconductor laser (LD), an electroluminescence (EL), etc.
[0467] In order to irradiate only light in a desired wavelength range, various filters such as a sharp cut filter, a band pass filter, a near infrared cut filter, a dichroic filter, an interference filter, and a color temperature conversion filter can be used.
[0468] Of these light sources, light emitting diodes and semiconductor lasers are preferably used since they have high irradiation energy and emit light with a long wavelength of 600 to 800 nm.
[0469] The transfer section 40 is disposed above the four image forming units 1Y, 1C, 1M, and 1K. The transfer section 40 includes a drive roller 41, a driven roller 42, an intermediate transfer belt 43 that is an intermediate transfer body that can rotate counterclockwise in the figure as the drive roller 41 is driven, primary transfer rollers 44Y, 44C, 44M, and 44K that are provided facing the photoconductors 311Y, 311C, 311M, and 311K across the intermediate transfer belt 43, and a secondary opposing roller 45 and a secondary transfer roller 46 that are provided facing each other across the intermediate transfer belt 43 at a transfer position of the toner image to paper. The transfer section 40 transfers the toner images of each color formed on the surfaces of the photoconductors 311Y, 311C, 311M, and 311K onto the surface of the intermediate transfer belt 43 in a superimposed manner.
[0470] The driving roller 41 is a roller that drives the intermediate transfer belt 43 to rotate.
[0471] The driven roller 42 is disposed inside the intermediate transfer belt 43 and is a roller for moving the intermediate transfer belt 43 endlessly.
[0472] The intermediate transfer belt 43 is an endless belt that is stretched around seven rollers arranged on the inside, and is designed to be endlessly movable in the direction of the arrow by the rotational drive of the drive roller 41.
[0473] The primary transfer rollers 44Y, 44C, 44M, and 44K are primary transfer members provided in a primary transfer device that is a primary transfer section that transfers the toner images on the surfaces of the photoconductors 311Y, 311C, 311M, and 311K to the intermediate transfer belt 43. The primary transfer rollers 44Y, 44C, and 44M, and 44K sandwich the intermediate transfer belt 43 between the photoconductors 311Y, 311C, 311M, and 311K to form primary transfer nips. The primary transfer rollers 44Y, 44C, and 44M, and 44K apply a transfer bias of the opposite polarity (e.g., positive) to that of the toner to the back surface (inner peripheral surface of the loop) of the intermediate transfer belt 43. As the intermediate transfer belt 43 moves endlessly, the Y, C, M, and K toner images on the photoconductors 311Y, 311C, 311M, and 311K are sequentially passed through the primary transfer nips for Y, C, M, and K, and are primarily transferred in a superimposed manner onto the surface of the intermediate transfer belt 43. As a result, a four-color superimposed toner image (hereinafter referred to as a four-color toner image) is formed on the intermediate transfer belt 43.
[0474] The secondary opposing roller 45 sandwiches the intermediate transfer belt 43 with a secondary transfer roller 46 disposed outside the loop of the intermediate transfer belt 43 to form a secondary transfer nip.
[0475] A secondary transfer bias is applied to the secondary transfer roller 46. The secondary transfer roller 46 is a secondary transfer member that performs secondary transfer of the four-color toner image on the intermediate transfer belt 43 all at once onto the transfer paper P. The four-color toner image on the intermediate transfer belt 43 is secondarily transferred all at once onto the transfer paper P in the secondary transfer nip due to the influence of the secondary transfer electric field and nip pressure formed between the secondary transfer roller 46 and the secondary opposing roller 45. This results in a color toner image.
[0476] After passing through the secondary transfer nip, residual toner that has not been transferred to the transfer paper P adheres to the intermediate transfer belt 43. The residual toner is cleaned by a belt cleaning unit (not shown).
[0477] When forming a monochrome image, the printer 100 revolves the primary transfer rollers 44Y, 44C, 44M, and 44K for Y, C, and M counterclockwise around the rotation axis of the driven roller 42 to separate the intermediate transfer belt 43 from the photoconductors 311Y, 311C, and 311M for Y, C, and M. Then, of the four imaging units 31Y, 31C, 31M, and 31K, only the imaging unit 31K for K is driven to form a monochrome image. This makes it possible to avoid wear and tear on the members constituting the imaging units due to unnecessary driving of the imaging units 31Y, 31C, and 31M when forming a monochrome image.
[0478] The fixing section 50 is disposed above the secondary transfer nip in the drawing. The fixing section 50 includes a fixing belt unit 51 that contains a heat source such as a halogen lamp and heats the transfer paper P, and a pressure roller 52 that rotatably presses the fixing belt unit 51 to form a fixing nip in contact with the fixing belt 621.
[0479] The transfer paper P that has passed through the secondary transfer nip described above is separated from the intermediate transfer belt 43 and then sent into the fixing section 50. Then, in the process of being conveyed from the bottom to the top in the figure while being sandwiched in the fixing nip inside the fixing section 50, the transfer paper P is heated and pressed by the fixing belt unit 51, so that heat and pressure are applied to the color toner image on the transfer paper P, and the color toner image is fixed to the transfer paper P.
[0480] The transfer paper P which has been subjected to the fixing process in this manner passes between the rollers of the paper discharge roller 23, and is then discharged onto the paper discharge tray 24. This completes a series of image forming processes.
[0481] The toner cartridge 60 is provided above the transfer unit 40 and includes toner cartridges 60Y, 60C, 60M, and 60K. The toner cartridges 60Y, 60C, 60M, and 60K accommodate Y, C, M, and K toners, respectively. The Y, C, M, and K toners in the toner cartridges 60Y, 60C, 60M, and 60K are appropriately supplied to the developing devices 313Y, 313C, 313M, and 313K of the image forming units 31Y, 31C, 31M, and 31K. These toner cartridges 60Y, 60C, 60M, and 60K are detachable from the printer body independently of the image forming units 31Y, 31C, 31M, and 31K.
[0482] <Process cartridge> The process cartridge according to one embodiment is molded so as to be detachably attached to various image forming devices, and has an electrostatic latent image carrier that carries an electrostatic latent image, and a developing unit that develops the electrostatic latent image carried on the electrostatic latent image carrier with a developer according to the above-mentioned one embodiment to form a toner image, and may have other configurations as necessary.
[0483] The electrostatic latent image carrier is the same as the electrostatic latent image carrier of the image forming apparatus described above, and therefore details thereof will be omitted.
[0484] The developing unit includes a developer container that contains the developer according to an embodiment, and a developer carrier that carries and transports the developer contained in the developer container. The developing unit may further include a regulating member or the like to regulate the thickness of the developer carried by the developer container.
[0485] FIG. 4 shows an example of a process cartridge according to an embodiment. As shown in FIG. 4, the process cartridge 200 has a photoconductor drum 210, a corona charger 220 as a charging unit, a developing device 230, a transfer roller 240, and a cleaning device 250. An exposure device 260 is provided above the process cartridge 200. These members constituting the process cartridge 200 are the same as the photoconductors 311Y, 311C, 311M, and 311K, the charging devices 312Y, 312C, 312M, and 312K, the developing devices 313Y, 313C, 313M, and 313K, the photoconductor cleaning devices 314, 314C, 314M, and 314K, and the primary transfer rollers 44Y, 44C, 44M, and 44K shown in FIG. 4, so details are omitted.
[0486] In the process cartridge 200, the surface of the photosensitive drum 210 is uniformly charged using a corona charger 220, and after the surface of the photosensitive drum 210 is uniformly charged, the exposure device 260 is used to expose the photosensitive drum 210 to exposure light L to form an electrostatic latent image. The electrostatic latent image formed on the photosensitive drum 210 is then developed with toner supplied from a developing device 230 to form a toner image. The toner image formed on the photosensitive drum 210 is then transferred to the transfer paper P conveyed by the transfer roller 240 by a transfer bias applied by the roller. EXAMPLES
[0487] The embodiments will be described in more detail below with reference to examples and comparative examples, but the embodiments are not limited to these examples and comparative examples.
[0488] <Production of fine particle dispersion containing organic fine particles> [Production Example 1: Production of microparticle dispersion (W-1) containing organic microparticles (A1-1)] (Production of Microparticle Dispersion (W0-1) Containing Organic Microparticles (A1)) In a reaction vessel equipped with a stirrer, a heating / cooling device, and a thermometer, 3785 parts by mass of water and 125 parts by mass of polyoxyethylene-1-(allyloxymethyl) alkyl ether sulfate ammonium (Aqualon KH-1025, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) were charged, and the mixture was homogenized by stirring at 200 rpm. After the mixture was heated to raise the temperature inside the system to 75°C, 90 parts by mass of a 10% by mass aqueous solution of ammonium persulfate was added, and then a mixture consisting of 415 parts by mass of styrene, 285 parts by mass of butyl acrylate, and 300 parts by mass of methacrylic acid was dropped over 4 hours. After the dropwise addition, the mixture was aged at 75°C for 4 hours to obtain a fine particle dispersion (W0-1) containing organic fine particles (A1) consisting of a resin (a1-1) which is a polymer in which styrene, butyl acrylate, and methacrylic acid are copolymerized with polyoxyethylene-1-(allyloxymethyl) alkyl ether sulfate ammonium.
[0489] A part of the fine particle dispersion (W0-1) was dried to isolate the resin (a1-1) which was the organic fine particles (A1). The glass transition temperature Tg of this resin (a1-1) was 53° C., and the acid value was 195 mg KOH / g.
[0490] (Production of Microparticle Dispersion (W-1) Containing Organic Microparticles (A1-1)) Next, 667 parts by mass of the microparticle dispersion (W0-1) and 248 parts by mass of water were charged into a reaction vessel equipped with a stirrer, a heating / cooling device, and a thermometer, and 0.267 parts by mass of tertiary butyl hydroperoxide (Perbutyl H, manufactured by NOF Corp.) was added, and the mixture was heated to raise the temperature in the system to 70° C. Then, 43.3 parts by mass of styrene, 23.3 parts by mass of butyl acrylate, and 18.0 parts by mass of a 1% by mass aqueous ascorbic acid solution were dropped into the mixture over 2 hours. After the dropping, the mixture was aged at 70° C. for 4 hours to obtain a microparticle dispersion (W-1) containing organic microparticles (A1-1) containing resin (a2-1), which is a polymer in which styrene and butyl acrylate are copolymerized, and resin (a1-1) as constituents in the same particle, using the microparticles in the microparticle dispersion (W0-1) as seeds.
[0491] The organic fine particles (A1-1) had a volume average particle size of 42 nm, which was measured using a laser Doppler particle size distribution measuring device (nanotrac UPA-150EX, manufactured by Nikkiso Co., Ltd.).
[0492] The fine particle dispersion (W-1) was neutralized with 10% by weight aqueous ammonia to pH 9.0, and the precipitate was centrifuged and dried to isolate the resin (a2-1) contained in the organic fine particles (A1-1). The glass transition temperature Tg of this resin (a2-1) was 53°C.
[0493] [Production Example 2: Production of Microparticle Dispersion (W-2) of Organic Microparticles (A2-1)] (Production of Microparticle Dispersion (W0-2) of Organic Microparticles (A2)) In a reaction vessel equipped with a stirrer, a heating / cooling device, and a thermometer, 3820 parts by mass of water and 90 parts by mass of polyoxyethylene-1-(allyloxymethyl) alkyl ether sulfate ammonium (Aqualon KH-1025, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) were charged, and the mixture was homogenized by stirring at 200 rpm. After the mixture was heated to raise the temperature inside the system to 75°C, 90 parts by mass of a 10% by mass aqueous solution of ammonium persulfate was added to the mixture, and then a mixture consisting of 390 parts by mass of styrene, 310 parts by mass of butyl acrylate, and 300 parts by mass of methacrylic acid was dropped over 4 hours. After the dropwise addition, the mixture was aged at 75°C for 4 hours to obtain a fine particle dispersion (W0-2) containing organic fine particles (A2) consisting of a resin (a1-2) which is a polymer in which styrene, butyl acrylate, and methacrylic acid are copolymerized with polyoxyethylene-1-(allyloxymethyl) alkyl ether sulfate ammonium.
[0494] A part of the fine particle dispersion (W0-2) was dried to isolate the resin (a1-2) which is the organic fine particles (A2). The resin (a1-2) had a glass transition temperature Tg of 53° C. and an acid value of 195 mg KOH / g.
[0495] (Production of Microparticle Dispersion (W-2) Containing Organic Microparticles (A2-1)) Next, 667 parts by mass of the microparticle dispersion (W0-2) and 248 parts by mass of water were charged into a reaction vessel equipped with a stirrer, a heating / cooling device, and a thermometer, and 0.267 parts by mass of tertiary butyl hydroperoxide (NOF Corp., Perbutyl H) was added, and the temperature in the system was raised to 70°C by heating, and then 43.3 parts by mass of styrene, 23.3 parts by mass of butyl acrylate, and 18.0 parts by mass of 1% by mass aqueous ascorbic acid solution were dropped over 2 hours. After dropping, the mixture was aged at 70°C for 4 hours to obtain a microparticle dispersion (W-2) containing organic microparticles (A2-1) containing resin (a2-2), which is a polymer in which styrene and butyl acrylate are copolymerized, and resin (a1-2) as constituents in the same particle, using the microparticles in the microparticle dispersion (W0-2) as seeds.
[0496] The volume average particle diameter of the organic fine particles (A2-1) was 57 nm. The volume average particle diameter was measured in the same manner as for the organic fine particles (A1-1).
[0497] In addition, the fine particle dispersion (W-2) was neutralized with a 10% by mass aqueous ammonia solution to a pH of 9.0, and then centrifuged to separate the precipitate, which was then dried to isolate resin (a2-2). The glass transition temperature Tg of resin (a2-2) was 53°C.
[0498] [Production Example 3: Production of microparticle dispersion (W-3) of organic microparticles (A3-1)] (Production of Microparticle Dispersion (W0-3) of Organic Microparticles (A3)) In a reaction vessel equipped with a stirrer, a heating / cooling device, and a thermometer, 3710 parts by mass of water and 200 parts by mass of polyoxyethylene-1-(allyloxymethyl) alkyl ether sulfate ammonium (Aqualon KH-1025, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) were charged, and the mixture was homogenized by stirring at 200 rpm. After the mixture was heated to raise the temperature inside the system to 75°C, 90 parts by mass of a 10% by mass aqueous solution of ammonium persulfate was added, and then a mixture consisting of 450 parts by mass of styrene, 250 parts by mass of butyl acrylate, and 300 parts by mass of methacrylic acid was dropped over 4 hours. After the dropwise addition, the mixture was aged at 75°C for 4 hours to obtain a fine particle dispersion (W0-3) containing organic fine particles (A3) consisting of a resin (a1-3) which is a polymer in which styrene, butyl acrylate, and methacrylic acid are copolymerized with polyoxyethylene-1-(allyloxymethyl) alkyl ether sulfate ammonium.
[0499] A part of the fine particle dispersion (W0-3) was dried to isolate the resin (a1-3) which was the organic fine particles (A3). The resin (a1-3) had a glass transition temperature Tg of 53° C. and an acid value of 195 mg KOH / g.
[0500] (Production of Microparticle Dispersion (W-3) Containing Organic Microparticles (A3-1)) Next, 667 parts by mass of the microparticle dispersion (W0-3) and 248 parts by mass of water were charged into a reaction vessel equipped with a stirrer, a heating / cooling device, and a thermometer, and 0.267 parts by mass of tertiary butyl hydroperoxide (NOF Corp., Perbutyl H) was added, and the system was heated to raise the temperature to 70°C. Then, 43.3 parts by mass of styrene, 23.3 parts by mass of butyl acrylate, and 18.0 parts by mass of 1% by mass aqueous ascorbic acid solution were dropped into the mixture over 2 hours. After the dropping, the mixture was aged at 70°C for 4 hours to obtain a microparticle dispersion (W-3) containing organic microparticles (A3-1) containing resin (a2-3), which is a polymer in which styrene and butyl acrylate are copolymerized, and resin (a1-3) as constituents in the same particle, using the microparticles in the microparticle dispersion (W0-3) as seeds.
[0501] The volume average particle diameter of the organic fine particles (A3-1) was 17 nm. The volume average particle diameter was measured in the same manner as for the organic fine particles (A1-1).
[0502] The fine particle dispersion (W-3) was neutralized with a 10% by mass aqueous ammonia solution to a pH of 9.0, and the precipitate was centrifuged and dried to isolate resin (a2-3). The glass transition temperature Tg of resin (a2-3) was 53°C.
[0503] [Production Example 4: Production of aqueous dispersion (W0-4) of organic fine particles (B1-1)] (Production of Microparticle Dispersion (W0-4) Containing Organic Microparticles (B1)) In a reaction vessel equipped with a stirrer, a heating / cooling device, and a thermometer, 3860 parts by mass of water and 50 parts by mass of polyoxyethylene-1-(allyloxymethyl) alkyl ether sulfate ammonium (Aqualon KH-1025, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) were charged, and the mixture was homogenized by stirring at 200 rpm. After the mixture was heated to raise the temperature inside the system to 75°C, 90 parts by mass of a 10% by mass aqueous solution of ammonium persulfate was added, and then a mixture consisting of 350 parts by mass of styrene, 350 parts by mass of butyl acrylate, and 300 parts by mass of methacrylic acid was dropped over 4 hours. After the dropwise addition, the mixture was aged at 75°C for 4 hours to obtain a fine particle dispersion (W0-4) containing organic fine particles (B1) consisting of a resin (b1-1) which is a polymer in which styrene, butyl acrylate, and methacrylic acid are copolymerized with polyoxyethylene-1-(allyloxymethyl) alkyl ether sulfate ammonium.
[0504] A part of the fine particle dispersion (W0-4) was dried to isolate the resin (b1-1) which is the organic fine particles (B1). The glass transition temperature Tg of this resin (b1-1) was 53° C., and the acid value was 195 mg KOH / g.
[0505] (Production of Microparticle Dispersion (W-4) Containing Organic Microparticles (B1-1)) Next, 667 parts by mass of the microparticle dispersion (W0-4) and 248 parts by mass of water were charged into a reaction vessel equipped with a stirrer, a heating / cooling device, and a thermometer, and 0.267 parts by mass of tertiary butyl hydroperoxide (NOF Corp., Perbutyl H) was added, and the temperature in the system was raised to 70°C by heating, and then 43.3 parts by mass of styrene, 23.3 parts by mass of butyl acrylate, and 18.0 parts by mass of 1% by mass aqueous ascorbic acid solution were dropped over 2 hours. After dropping, the mixture was aged at 70°C for 4 hours to obtain a microparticle dispersion (W-4) containing organic microparticles (B1-1) containing resin (b2-1), which is a polymer in which styrene and butyl acrylate are copolymerized, and resin (b1-1) as constituents in the same particle, using the microparticles in (W0-4) as seeds.
[0506] The volume average particle diameter of the organic fine particles (B1-1) was 86 nm. The volume average particle diameter was measured in the same manner as for the organic fine particles (A1-1).
[0507] The fine particle dispersion (W-4) was neutralized with 10% by weight aqueous ammonia to pH 9.0, and the precipitate was centrifuged and dried to isolate the organic fine particles (B1-1) as resin (b2-1). The glass transition temperature Tg of this resin (b2-1) was 53°C.
[0508] [Production Example 5: Production of microparticle dispersion (W-5) of organic microparticles (B2-1)] (Production of fine particle dispersion (W0-5) of organic fine particles (B2)) In a reaction vessel equipped with a stirrer, a heating / cooling device, and a thermometer, 3840 parts by mass of water and 70 parts by mass of polyoxyethylene-1-(allyloxymethyl) alkyl ether sulfate ammonium (Aqualon KH-1025, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) were charged, and the mixture was homogenized by stirring at 200 rpm. After the mixture was heated to raise the temperature inside the system to 75°C, 90 parts by mass of a 10% by mass aqueous solution of ammonium persulfate was added to the mixture, and then a mixture consisting of 370 parts by mass of styrene, 330 parts by mass of butyl acrylate, and 300 parts by mass of methacrylic acid was dropped over 4 hours. After the dropwise addition, the mixture was aged at 75°C for 4 hours to obtain a fine particle dispersion (W0-5) containing organic fine particles (B2) consisting of a resin (b1-2) which is a polymer in which styrene, butyl acrylate, and methacrylic acid are copolymerized with polyoxyethylene-1-(allyloxymethyl) alkyl ether sulfate ammonium.
[0509] A part of the fine particle dispersion (W0-5) was dried to isolate the resin (b1-2) which was the organic fine particles (B2). The resin (b1-2) had a glass transition temperature Tg of 53° C. and an acid value of 195 mg KOH / g.
[0510] (Production of Microparticle Dispersion (W-5) Containing Organic Microparticles (B2-1)) Next, 667 parts by mass of the microparticle dispersion (W0-5) and 248 parts by mass of water were charged into a reaction vessel equipped with a stirrer, a heating / cooling device, and a thermometer, and 0.267 parts by mass of tertiary butyl hydroperoxide (NOF Corp., Perbutyl H) was added, and the temperature in the system was raised to 70°C by heating, and then 43.3 parts by mass of styrene, 23.3 parts by mass of butyl acrylate, and 18.0 parts by mass of 1% by mass aqueous ascorbic acid solution were dropped over 2 hours. After dropping, the mixture was aged at 70°C for 4 hours to obtain a microparticle dispersion (W-5) of organic microparticles (B2-1) containing resin (b2-2), which is a polymer in which styrene and butyl acrylate are copolymerized, and resin (b1-2) as constituents in the same particle, using the microparticles in the microparticle dispersion (W0-5) as seeds.
[0511] The volume average particle diameter of the organic fine particles (B2-1) was 69 nm. The volume average particle diameter was measured in the same manner as for the organic fine particles (A1-1).
[0512] In addition, the fine particle dispersion (W-5) was neutralized with a 10% by mass aqueous ammonia solution to a pH of 9.0, and the precipitate obtained by centrifugation was dried to isolate resin (b2-2). The glass transition temperature Tg of resin (b2-2) was 53°C.
[0513] [Production Example 6: Production of microparticle dispersion (W-6) of organic microparticles (B3-1)] (Production of Microparticle Dispersion (W0-6) of Organic Microparticles (B3)) In a reaction vessel equipped with a stirrer, a heating / cooling device, and a thermometer, 3880 parts by mass of water and 30 parts by mass of polyoxyethylene-1-(allyloxymethyl) alkyl ether sulfate ammonium (Aqualon KH-1025, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) were charged, and the mixture was homogenized by stirring at 200 rpm. After the mixture was heated to raise the temperature inside the system to 75°C, 90 parts by mass of a 10% by mass aqueous solution of ammonium persulfate was added, and then a mixture consisting of 330 parts by mass of styrene, 370 parts by mass of butyl acrylate, and 300 parts by mass of methacrylic acid was dropped over 4 hours. After the dropwise addition, the mixture was aged at 75°C for 4 hours to obtain a fine particle dispersion (W0-6) containing organic fine particles (B3) consisting of a resin (b1-3) which is a polymer in which styrene, butyl acrylate, and methacrylic acid are copolymerized with polyoxyethylene-1-(allyloxymethyl) alkyl ether sulfate ammonium.
[0514] A part of the fine particle dispersion (W0-6) was dried to isolate the resin (b3-1) which is the organic fine particles (B3). The resin (b1-3) had a glass transition temperature Tg of 53° C. and an acid value of 195 mg KOH / g.
[0515] (Production of Microparticle Dispersion (W-6) Containing Organic Microparticles (B3-1)) Next, 667 parts by mass of the microparticle dispersion (W0-6) and 248 parts by mass of water were charged into a reaction vessel equipped with a stirrer, a heating / cooling device, and a thermometer, and 0.267 parts by mass of tertiary butyl hydroperoxide (NOF Corp., Perbutyl H) was added, and the temperature in the system was raised to 70°C by heating. Then, 43.3 parts by mass of styrene, 23.3 parts by mass of butyl acrylate, and 18.0 parts by mass of 1% by mass aqueous ascorbic acid solution were dropped into the mixture over 2 hours. After the dropping, the mixture was aged at 70°C for 4 hours to obtain a microparticle dispersion (W-6) containing organic microparticles (B3) containing resin (b2-3), which is a polymer in which styrene and butyl acrylate are copolymerized, and resin (b1-3) as constituents in the same particle, using the microparticles in the microparticle dispersion (W0-6) as seeds.
[0516] The volume average particle diameter of the organic fat particles (B3) was 103 nm. The volume average particle diameter was measured in the same manner as for the organic particles (A1-1).
[0517] In addition, the fine particle dispersion (W-6) was neutralized with a 10% by mass aqueous ammonia solution to a pH of 9.0, and the precipitate obtained by centrifugation was dried to isolate resin (b2-3). The glass transition temperature Tg of resin (b2-3) was 53°C.
[0518] The type of organic fine particles contained in the fine particle dispersions (W-1) to (W-3), the type of resin (a1) constituting the resin (a), and the glass transition temperature Tg 1st and oxidation, type of resin (a2) and glass transition temperature Tg 1st The types of organic fine particles contained in the fine particle dispersions (W-4) to (W-6), the type of resin (b1) constituting the resin (b), and the glass transition temperature Tg 1st and oxidation, type of resin (b2) and glass transition temperature Tg 1st is shown in Table 2.
[0519] [Table 1]
[0520] [Table 2]
[0521] <Synthesis of non-crystalline polyester resin> In a reaction vessel equipped with a cooling tube, a stirrer, a heating / cooling device, a thermometer, and a nitrogen inlet tube, 425 parts by mass of bisphenol A·PO 2-mol adduct, 100 parts by mass of propylene glycol, 634 parts by mass of terephthalic acid·propylene glycol 2-mol adduct, and 0.5 parts by mass of titanium diisopropoxy bistriethanolamine as a condensation catalyst were added and reacted at 230°C for 12 hours. Then, the reaction was carried out under a reduced pressure of 10 to 15 mmHg. The amount of propylene glycol recovered was 195 parts by mass. Then, after cooling to 180°C, 30 parts by mass of trimellitic anhydride were added and reacted at 180°C for 1 hour, and then taken out. After cooling the taken out resin to room temperature, amorphous polyester (b-1) was obtained. The amorphous polyester (b-1) had a glass transition temperature Tg of 42° C., a number average molecular weight Mn of 2,400, a weight average molecular weight Mw of 5,400, a hydroxyl value of 32 mg KOH / g, and an acid value of 18 mg KOH / g.
[0522] <Production of Colorant Dispersion> In a reaction vessel equipped with a cooling tube, a stirrer, a heating / cooling device, a thermometer, and a nitrogen inlet tube, 557 parts by mass of propylene glycol, 569 parts by mass of dimethyl terephthalate, 184 parts by mass of adipic acid, and 3 parts by mass of tetrabutoxychinanate as a condensation catalyst were added, and the mixture was reacted for 8 hours under a nitrogen stream at 180°C while distilling off the methanol produced. Next, the mixture was gradually heated to 230°C, and reacted for 4 hours under a nitrogen stream while distilling off the propylene glycol and water produced, and further reacted for 1 hour under a reduced pressure of 0.007 MPa to 0.026 MPa. The amount of propylene glycol recovered was 175 parts by mass. Next, the mixture was cooled to 180°C, and 121 parts by mass of trimellitic anhydride was added, and the mixture was reacted for 2 hours under a sealed normal pressure, and then reacted at 220°C and normal pressure until the softening point reached 180°C, to obtain a polyester resin (Mn=8500).
[0523] 20 parts by mass of copper phthalocyanine, 4 parts by mass of colorant dispersant (Solsperse 28000, manufactured by Avecia), 20 parts by mass of the obtained polyester resin, and 56 parts by mass of ethyl acetate were put into a beaker, and after stirring to uniformly disperse, the copper phthalocyanine was finely dispersed using a bead mill to obtain a colorant dispersion. The volume average particle size of the colorant dispersion was 0.2 μm.
[0524] <Production of modified wax> In a pressure-resistant reaction vessel equipped with a stirrer, a heating / cooling device, a thermometer, and a dropping bomb, 454 parts by mass of xylene and 150 parts by mass of low molecular weight polyethylene (Sunwax LEL-400, manufactured by Sanyo Chemical Industries) were added and replaced with nitrogen. The mixed solution was then heated to 170°C under stirring, and a mixed solution containing 595 parts by mass of styrene, 255 parts by mass of methyl methacrylate, 34 parts by mass of di-t-butylperoxyhexahydroterephthalate, and 119 parts by mass of xylene was added dropwise at the same temperature over a period of 3 hours, and the mixture was maintained at the same temperature for another 30 minutes. Next, the xylene was distilled off under a reduced pressure of 0.039 MPa to obtain a modified wax. The sp value of the graft chain of the modified wax was 10.35 (cal / cm 3 ) 1 / 2 The number average molecular weight Mn was 1,900, the weight average molecular weight Mw was 5,200, and the glass transition temperature Tg was 57°C.
[0525] <Production of release agent dispersion> In a reaction vessel equipped with a cooling tube, a stirrer, a heating / cooling device, and a thermometer, 10 parts by mass of paraffin wax (HNP-9, manufactured by Nippon Seiro Co., Ltd.), 1 part by mass of modified wax, and 33 parts by mass of ethyl acetate were added, heated to 78°C, and stirred at the same temperature for 30 minutes. The mixed solution was then cooled to 30°C over one hour to crystallize the paraffin wax into fine particles. The mixture was then wet-pulverized using an Ultraviscomill (manufactured by Imex Co., Ltd.) to obtain a release agent dispersion. The volume average particle size of the release agent dispersion was 0.25 μm.
[0526] <Production of reactive prepolymer (α2b-1)> In a reaction vessel equipped with a cooling tube, a stirrer, a heating / cooling device, a thermometer, and a nitrogen inlet tube, 439 parts by mass of bisphenol A·PO 2-mol adduct, 329 parts by mass of bisphenol A·PO 3-mol adduct, 206 parts by mass of terephthalic acid, 90 parts by mass of adipic acid, and 0.5 parts by mass of titanium diisopropoxy bistriethanolamine as a condensation catalyst were added, and the temperature was gradually raised to 230°C while reacting for 10 hours under a reduced pressure of 0.5 to 2.5 kPa. When the acid value became less than 1, the mixture was taken out to obtain polyester (α2b). The glass transition temperature Tg of polyester (α2b) was 45°C, the number average molecular weight Mn was 3900, the weight average molecular weight Mw was 11000, and the hydroxyl value was 25 mgKOH / g.
[0527] Next, 448 parts by mass of polyester (α2b), 52 parts by mass of isophorone diisocyanate, and 500 parts by mass of ethyl acetate were added to a pressure-resistant reaction vessel equipped with a stirrer, a heating / cooling device, and a thermometer, and the mixture was reacted at 80°C for 10 hours in a sealed state to obtain a reactive prepolymer (α2b-1) solution containing isocyanate groups at the molecular terminals. The reactive prepolymer (α2b-1) had a urethane group concentration of 2.0, a number average molecular weight Mn of 6900, and a weight average molecular weight Mw of 25000.
[0528] <Example 1: Production of toner (T-1)> [Production of toner (C-1)] In a beaker, 165 parts by mass of ion-exchanged water, a mixture of 7.5 parts by mass of microparticle dispersion (W-1) and 7.5 parts by mass of microparticle dispersion (W-4), 1 part by mass of sodium carboxymethyl cellulose, 26 parts by mass of sodium dodecyl diphenyl ether disulfonate (Sanyo Chemical Industries, Eleminol MON-7) and 15 parts by mass of ethyl acetate were added and mixed to obtain a dispersion. Next, 71 parts by mass of amorphous polyester resin, 40 parts by mass of coloring dispersion, 39 parts by mass of release agent dispersion and 54 parts by mass of ethyl acetate were added and mixed in another beaker, and then 18 parts by mass of reactive prepolymer (α2b-1) solution and 0.3 parts by mass of isophorone diamine as a curing agent β were further added and mixed to obtain a mixture. The entire amount of this mixture was added to the dispersion prepared earlier and stirred for 2 minutes with a TK auto homomixer to obtain a mixture. The mixture was then transferred to a reactor equipped with a stirrer and a thermometer, and a composite treatment was carried out by distilling off ethyl acetate at 50°C until the concentration became 0.5 mass% or less, to obtain an aqueous dispersion containing toner base particles to which organic fine particles were attached. The aqueous dispersion is toner (C-1) which is a composite resin particle in which organic fine particles (A1-1) and (B1-1) are attached to toner base particles which are resin particles containing a non-crystalline polyester resin and a non-crystalline polyurethane resin (b-2) composed of a reaction product of a reactive prepolymer (α2b-1) and isophoronediamine.
[0529] The fact that the aqueous dispersion is toner (T-1) in which organic fine particles (A1-1) and (B1-1) are attached to the surface of the toner base particle was confirmed by magnifying the shape of the particles contained in the aqueous dispersion with an electron microscope. From the observation results, it was confirmed that the toner (T-1) had a core-shell structure in which organic fine particles (A1-1) and (B1-1) were attached to the surface of the toner base particle. It was also confirmed that the two organic fine particles (A1-1) and (B1-1) formed a core-shell structure composed of them.
[0530] [Production of toner (T-1)] Next, 100 parts by mass of the toner (C-1) was mixed with 1.0 part by mass of colloidal silica (Aerosil R972, manufactured by Nippon Aerosil Co., Ltd.) as an external additive in a sample mill for external addition treatment, toner (T-1) after external addition treatment was obtained.
[0531] <Example 2: Production of toner (T-2)> [Production of toner (C-2)] In Example 1, the mixture of 7.5 parts by mass of the fine particle dispersion (W-1) and 7.5 parts by mass of the fine particle dispersion (W-4) was changed to a mixture of 7.5 parts by mass of the fine particle dispersion (W-1) and 7.5 parts by mass of the fine particle dispersion (W-5). Otherwise, the same procedure as in Example 1 was carried out to obtain an aqueous dispersion containing a toner (C-2) which is a composite resin particle in which organic fine particles (A1-1) and organic fine particles (B2-1) are attached to a toner base particle which is a resin particle. This aqueous dispersion was washed and filtered, and dried at 40°C for 18 hours to reduce the volatile content to 0.5% by mass or less, thereby obtaining a toner (C-2). Next, an external addition treatment was carried out in the same manner as in Example 1 to obtain a toner (T-2) after the external addition treatment.
[0532] It was confirmed that the toner (T-2), like the toner (T-1), had a core-shell structure formed by the organic fine particles (A1-1) and (B2-1) adhering to the surface of the toner base particle. It was also confirmed that the organic fine particles (A1-1) and (B2-1) formed a core-shell structure composed of these.
[0533] <Example 3: Production of toner (T-3)> In Example 1, the mixture of 7.5 parts by mass of the fine particle dispersion (W-1) and 7.5 parts by mass of the fine particle dispersion (W-4) was changed to a mixture of 7.5 parts by mass of the fine particle dispersion (W-1) and 7.5 parts by mass of the fine particle dispersion (W-6). Otherwise, the same procedure as in Example 1 was carried out to obtain an aqueous dispersion containing a toner (T-3) which is a composite resin particle in which organic fine particles (A1-1) and organic fine particles (B3-1) are attached to a toner base particle which is a resin particle. This aqueous dispersion was washed and filtered, and dried at 40°C for 18 hours to reduce the volatile content to 0.5% by mass or less, thereby obtaining a toner (C-3). Next, an external addition treatment was carried out in the same manner as in Example 1 to obtain a toner (T-3) after the external addition treatment.
[0534] It was confirmed that the toner (T-3), like the toner (T-1), had a core-shell structure formed by the organic fine particles (A1-1) and (B3-1) adhering to the surface of the toner base particle. It was also confirmed that the organic fine particles (A1-1) and (B3-1) formed a core-shell structure composed of these.
[0535] <Example 4: Production of toner (T-4)> In Example 1, the mixture of 7.5 parts by mass of the fine particle dispersion (W-1) and 7.5 parts by mass of the fine particle dispersion (W-4) was changed to a mixture of 7.5 parts by mass of the fine particle dispersion (W-2) and 7.5 parts by mass of the fine particle dispersion (W-4). Otherwise, the same procedure as in Example 1 was carried out to obtain an aqueous dispersion containing a toner (T-4) which is a composite resin particle in which organic fine particles (A2-1) and organic fine particles (B1-1) are attached to a toner base particle which is a resin particle. This aqueous dispersion was washed and filtered, and dried at 40° C. for 18 hours to reduce the volatile content to 0.5% by mass or less, thereby obtaining a toner (C-4). Next, an external addition treatment was carried out in the same manner as in Example 1 to obtain a toner (T-4) after the external addition treatment.
[0536] It was confirmed that the toner (T-4), like the toner (T-1), had a core-shell structure formed by the organic fine particles (A2-1) and (B1-1) adhering to the surface of the toner base particle. It was also confirmed that the organic fine particles (A2-1) and (B1-1) formed a core-shell structure composed of these.
[0537] <Example 5: Production of toner (T-5)> In Example 1, the mixture of 7.5 parts by mass of fine particle dispersion (W-1) and 7.5 parts by mass of fine particle dispersion (W-4) was changed to a mixture of 7.5 parts by mass of fine particle dispersion (W-2) and 7.5 parts by mass of fine particle dispersion (W-5). Otherwise, the same procedure as in Example 1 was carried out to obtain an aqueous dispersion containing toner (T-5) which is a composite resin particle in which organic fine particles (A2-1) and organic fine particles (B2-1) are attached to toner base particles which are resin particles. This aqueous dispersion was washed, filtered, and dried at 40°C for 18 hours to reduce the volatile content to 0.5% by mass or less, thereby obtaining toner (C-5). Next, the same procedure as in Example 1 was carried out to obtain toner (T-5) after external addition treatment.
[0538] It was confirmed that the toner (T-5), like the toner (T-1), had a core-shell structure formed by the organic fine particles (A2-1) and (B2-1) adhering to the surface of the toner base particle. It was also confirmed that the organic fine particles (A2-1) and (B2-1) formed a core-shell structure composed of these.
[0539] <Example 6: Production of toner (T-6)> In Example 1, the mixture of 7.5 parts by mass of the fine particle dispersion (W-1) and 7.5 parts by mass of the fine particle dispersion (W-4) was changed to a mixture of 7.5 parts by mass of the fine particle dispersion (W-2) and 7.5 parts by mass of the fine particle dispersion (W-6). Otherwise, the same procedure as in Example 1 was carried out to obtain an aqueous dispersion containing a toner (T-6) which is a composite resin particle in which organic fine particles (A2-1) and organic fine particles (B3-1) are attached to a toner base particle which is a resin particle. This aqueous dispersion was washed and filtered, and dried at 40°C for 18 hours to reduce the volatile content to 0.5% by mass or less, thereby obtaining a toner (C-6). Next, an external addition treatment was carried out in the same manner as in Example 1 to obtain a toner (T-6) after the external addition treatment.
[0540] It was confirmed that the toner (T-6), like the toner (T-1), had a core-shell structure formed by the organic fine particles (A2-1) and (B3-1) adhering to the surface of the toner base particle. It was also confirmed that the organic fine particles (A2-1) and (B3-1) formed a core-shell structure composed of these.
[0541] <Example 7: Production of toner (T-7)> In Example 1, the mixture of 7.5 parts by mass of the fine particle dispersion (W-1) and 7.5 parts by mass of the fine particle dispersion (W-4) was changed to a mixture of 7.5 parts by mass of the fine particle dispersion (W-3) and 7.5 parts by mass of the fine particle dispersion (W-5). Otherwise, the same procedure as in Example 1 was carried out to obtain an aqueous dispersion containing a toner (C-7) which is a composite resin particle in which organic fine particles (A3-1) and organic fine particles (B2-1) are attached to a toner base particle which is a resin particle. This aqueous dispersion was washed and filtered, and dried at 40°C for 18 hours to reduce the volatile content to 0.5% by mass or less, thereby obtaining a toner (C-7). Next, an external addition treatment was carried out in the same manner as in Example 1 to obtain a toner (T-7) after the external addition treatment.
[0542] It was confirmed that the toner (T-7), like the toner (T-1), had a core-shell structure formed by the organic fine particles (A3-1) and (B2-1) adhering to the surface of the toner base particles. It was also confirmed that the organic fine particles (A3-1) and (B2-1) formed a core-shell structure composed of these.
[0543] <Comparative Example 1: Production of Toner (T'-1)> In Example 1, the mixture of 7.5 parts by mass of the fine particle dispersion (W-1) and 7.5 parts by mass of the fine particle dispersion (W-4) was changed to a mixture of 7.5 parts by mass of the fine particle dispersion (W-4) and 7.5 parts by mass of the fine particle dispersion (W-6). Otherwise, the same procedure as in Example 1 was carried out to obtain an aqueous dispersion containing a toner (C'-1) which is a composite resin particle in which organic fine particles (B1-1) and organic fine particles (B3-1) are attached to a toner base particle which is a resin particle. This aqueous dispersion was washed and filtered, and dried at 40°C for 18 hours to reduce the volatile content to 0.5% by mass or less, thereby obtaining a toner (C'-1). Next, an external addition treatment was carried out in the same manner as in Example 1 to obtain a toner (T'-1) after the external addition treatment.
[0544] Observation of the toner (T'-1) with an electron microscope confirmed that the toner (T'-1) had a core-shell structure formed by organic fine particles (B1-1) and (B3-1) adhering to the surface of the toner base particle. It was also confirmed that the organic fine particles (B1-1) and the organic fine particles (B3-1) each existed independently and formed a single structure.
[0545] <Comparative Example 2: Production of Toner (T'-2)> In Example 1, the mixture of 7.5 parts by mass of the fine particle dispersion (W-1) and 7.5 parts by mass of the fine particle dispersion (W-4) was changed to a mixture of 7.5 parts by mass of the fine particle dispersion (W-1) and 7.5 parts by mass of the fine particle dispersion (W-2). Otherwise, the same procedure as in Example 1 was carried out to obtain an aqueous dispersion containing a toner (C'-2) which is a composite resin particle in which organic fine particles (A1-1) and organic fine particles (A2-1) are attached to a toner base particle which is a resin particle. This aqueous dispersion was washed and filtered, and dried at 40°C for 18 hours to reduce the volatile content to 0.5% by mass or less, thereby obtaining a toner (C'-2). Next, an external addition treatment was carried out in the same manner as in Example 1 to obtain a toner (C'-2) after the external addition treatment.
[0546] Observation of the toner (T'-1) with an electron microscope confirmed that the toner (T-1) had a core-shell structure formed by organic fine particles (A1-1) and (A2-1) adhering to the surface of the toner base particle. It was also confirmed that the organic fine particles (A1-1) and the organic fine particles (A2-1) each existed independently and constituted a single structure.
[0547] Table 3 shows the type of toner, the structure, type and volume average particle size of the organic fine particles, and the type and volume average particle size of the composite resin particles B in each of the examples and comparative examples.
[0548] <Measurement of peaks P1 and P2 of organic particles A and B contained in toner> Peaks P1 and P2 of organic fine particles A and B contained in the toner of each Example and Comparative Example were measured. First, ultrasonic waves were applied to the toner of each Example and Comparative Example to remove as much of the external additives adhering to the surface of the toner base particles as possible, to make the toner base particles in a state close to that of the toner base particles. [How to separate external additives] (1)[1] 50 ml of a 5% aqueous solution containing a surfactant (product name: Noigen ET-165, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) was added to a 100 ml screw tube, and 3 g of toner was added to the mixture and gently moved up and down and left and right. After that, the mixture was stirred in a ball mill for 30 minutes so that the toner was mixed into the dispersion solution. [2] Then, using an ultrasonic homogenizer (product name homogenizer, model VCX750, CV33, manufactured by SONICS & MATERIALS LLC), the output was set to 40 W and ultrasonic energy was applied for 60 minutes. -Ultrasonic conditions- Vibration time: 60 minutes continuous Amplitude: 40W Vibration start temperature: 23±1.5℃. Temperature during vibration: 23±1.5℃ [3] The dispersion liquid is suction filtered using filter paper (product name: Qualitative Filter Paper (No. 2, 110 mm), manufactured by Advantec Toyo Co., Ltd.), washed twice again with ion-exchanged water, filtered, and the liberated additives are removed. After that, the toner base particles are dried.
[0549] (2) The toner obtained in (1) was observed with a scanning electron microscope (SEM). First, the external additives and fillers containing Si were detected by observing the backscattered electron image.
[0550] (3) The image of (1) was binarized using image processing software (ImageJ), and external additives and fillers were removed.
[0551] (4) Next, a secondary electron image was observed at the same position as in (1). Since organic fine particles cannot be observed in a backscattered electron image, but can only be observed in a secondary electron image, the image was compared with the image obtained in (3) above, and fine particles present in areas other than the remaining external additives and filler (areas other than those excluded in (3) above) were determined to be organic fine particles, and the particle size (particle diameter) was measured using image processing software.
[0552] (5) More than 100 particles were counted to obtain the particle size distribution. -Shooting conditions- Scanning electron microscope: SU-8230 Magnification: 35,000x Image capture: SE(L): Secondary electrons, BSE (backscattered electrons) Acceleration voltage: 2.0kV ·Acceleration current: 1.0μA ·Probe current:Normal Focus mode: UHR WD:8.0mm
[0553] <Toner glass transition temperature Tg 1st , glass transition temperature Tga of THF insoluble matter 1st , Tg of THF soluble matter 2nd > 1 g of toner was put into 100 mL of THF and subjected to Soxhlet extraction to obtain THF soluble and insoluble fractions. These were then dried in a vacuum dryer for 24 hours to obtain modified polyester resin from the THF soluble fraction and amorphous polyester resin from the THF insoluble fraction. These were used as the target samples. The glass transition temperature Tg 1st When measuring, a toner was used as a target sample.
[0554] Next, about 5.0 mg of the target sample was placed in an aluminum sample container, the sample container was placed on a holder unit, and set in an electric furnace. Next, under a nitrogen atmosphere, the sample was heated from -80°C to 150°C at a heating rate of 1.0°C / min (first heating). After that, the sample was cooled from 150°C to -80°C at a heating rate of 1.0°C / min, and further heated to 150°C at a heating rate of 1.0°C / min (second heating). In each of the first and second heating, a DSC curve was measured using a differential scanning calorimeter ("Q-200", manufactured by TA Instruments).
[0555] From the obtained DSC curves, the DSC curve at the first heating was selected using the analysis program in the Q-200 system, and the glass transition temperature Tg at the first heating of the target sample was calculated. 1st asked for.
[0556] Similarly, select the DSC curve during the second heating and measure the glass transition temperature (Tg) of the sample during the second heating. 2nd asked for.
[0557] The THF insoluble portion of the toner was heated from -80°C to 150°C at a temperature rise rate of 1.0°C / min using the modulation mode with a modulation temperature amplitude of ±1.0°C / min (first temperature rise). The obtained DSC curve was obtained by plotting "Reversing Heat Flow" on the vertical axis using the analysis program in the Q-200 system in the same manner as above, and the onset value shown in Figure 1 was taken as the glass transition temperature Tg. As a result, the glass transition temperature Tga of the THF insoluble portion was calculated. 1st and Tg 2nd asked for.
[0558] The glass transition temperature Tg of the toner 1st , the glass transition temperature Tg of the THF insoluble matter of the toner 1st , Tg of the THF-soluble portion of the toner 2nd is shown in Table 3.
[0559] <Toner Evaluation> The toners (T-1) to (T-7) and (T'-1) to (T'-2) after the external additive treatment were evaluated for low temperature fixability, heat resistance storage stability, and liberation rate of additives by the following methods. The evaluation results are shown in Table 1.
[0560] [Low temperature fixability] Composite resin particles are applied to the paper surface at 0.8 mg / cm 2 The powder was placed evenly on the paper surface using a color multifunction printer (imagio MP C4500, manufactured by Ricoh Co., Ltd.) with the thermal fixing unit removed. The paper with the powder placed on it was placed on the pressure roller at a fixing speed (heat roller peripheral speed) of 213 mm / sec and a fixing pressure (pressure roller pressure) of 10 kg / cm. 2 The temperature at which cold offset occurred (MFT) when the toner was passed through the above conditions was measured and evaluated based on the following evaluation criteria. The lower the temperature at which cold offset occurred, the better the low-temperature fixing ability. (Cold offset evaluation criteria) ◎: Minimum fixing temperature is 130℃ or less ○: The minimum fixing temperature is greater than 130°C and less than or equal to 135°C. △: The minimum fixing temperature is greater than 135°C and less than 140°C ×: The minimum fixing temperature is higher than 140° C.
[0561] [Heat-resistant storage stability] After storing the toner at 50° C. for 8 hours, it was sieved through a 42 mesh sieve for 2 minutes, and the residual ratio on the wire screen was measured and evaluated based on the following evaluation criteria. At this time, the better the heat resistance storage stability of the toner, the smaller the residual ratio. (Evaluation Criteria) ◎: Residual rate is less than 5% ○: Residual rate is 5% or more and less than 15% △: Residual rate is between 15% and 30% ×: Residual rate is 30% or more
[0562] [Free rate of additives] The occurrence rate of abnormal images was evaluated based on the liberation rate of additives adhering to the toner. The amount of additives released from the toner was measured as follows. (1) 3 g of a toner sample was dispersed in 50 mL of a 0.5% by mass polyoxyalkylene alkyl ether (Noigen ET-165, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) dispersion in a 110 mL vial. (2) Using an ultrasonic homogenizer (product name: homogenizer, model VCX750, CV33, manufactured by SONICS & MATERIALS), ultrasonic waves were irradiated for 100 seconds at a frequency of 20 kHz and an output of 40 W. The amount of energy applied at this time was calculated from the product of the output and the irradiation time (40 W x 100 seconds = 4 kJ). At this time, the toner dispersion was cooled as necessary to prevent the liquid temperature from exceeding 40°C. (3) The obtained dispersion liquid was suction filtered using filter paper (product name: Qualitative Filter Paper (No. 2, 110 mm), manufactured by Advantec Toyo Co., Ltd.), washed twice again with ion-exchanged water, filtered, and the liberated additives were removed, and the toner was then dried. (4) The amount of additive in the toner before and after additive removal was quantified by calculating the mass % from the intensity according to the calibration curve (or the difference in intensity before and after additive removal) using a fluorescent X-ray analyzer (ZSX-100e, manufactured by Rigaku Corporation), and the amount of released additive was calculated using the following formula (1). Released amount = (mass of additive before dispersion) - (mass of residual additive after dispersion) Equation (1)
[0563] The liberation rate of the additive (mass%) was calculated from the following formula (2) and evaluated based on the following evaluation criteria: The smaller the liberation rate of the additive, the lower the occurrence rate of abnormal images. Freedom rate = [free amount / total amount of additives added] × 100 Formula (2) (Evaluation Criteria) ◎: Free rate is 10% or more and less than 30% ○: Free rate is 5% or more and less than 45% △: Free rate is 5% or more and less than 60% ×: Free rate is 60% or more
[0564] In this case, the total amount of additives added was defined as follows. Using an ultrasonic homogenizer, the amount of additives in the toner irradiated with ultrasonic waves at irradiation energy amounts of 1000 kJ and 1500 kJ in the same manner as above was quantified with a fluorescent X-ray analyzer, and it was confirmed that there was no decrease in the amount of additives at 1000 kJ and 1500 kJ. If there was no decrease, it could be determined that all of the additives had been released. If a change was observed, the irradiation energy amount was increased by 500 kJ each time, and the same treatment was repeated. As described above, the total amount of additives added was calculated from the difference between the amount of additives in the toner from which all the additives had been released and the untreated toner.
[0565] After all the additives have been removed as described above, if the "amount of additives in the toner from which all the additives have been removed" is measured using fluorescent X-rays, the amount of additives will be zero, or if the toner base particles contain the same substance as the additives, it will be affected and will be a constant value. On the other hand, if the amount of additives in the untreated toner is measured using fluorescent X-rays, if the toner base particles use a material that contains the same substance as the additives as described above, the amount of additives will be added by the amount of the additives. Therefore, the total amount of additives added was calculated from the difference between the amount of additives in the toner from which all the additives have been removed as calculated above and the amount of additives in the untreated toner.
[0566] In addition, the liberation rate of the additives in the toner is preferably 20% by mass to 50% by mass when the amount of irradiation energy is 4 kJ. If the liberation rate is less than 20% by mass when the amount of irradiation energy is 4 kJ, the cleaning efficiency decreases. If the liberation rate is more than 50% by mass when the amount of irradiation energy is 4 kJ, the liberated additives adhere to the transfer body, causing image defects such as filming. By setting the irradiation energy to 4 kJ, the amount of additives with weak adhesion that are easily liberated from the toner in the image forming apparatus was measured.
[0567] [Table 3]
[0568] From Table 3, it was confirmed that the toners of Examples 1 to 7 all exhibited excellent performance in terms of low-temperature fixability, heat-resistant storage stability, and additive liberation rate, and met the conditions for use. On the other hand, the toner of Comparative Example 1 had poor low-temperature fixability and additive liberation rate. The toner of Comparative Example 2 had poor additive liberation rate and insufficient heat-resistant storage stability. Therefore, it was confirmed that the toners of Comparative Examples 1 and 2 did not meet the conditions for use in terms of at least one of low-temperature fixability, heat-resistant storage stability, and additive liberation rate, and thus had practical problems.
[0569] Therefore, the toners of Examples 1 to 7, unlike the toners of Comparative Examples 1 and 2, have a plurality of organic fine particles on the surface of the toner, and the glass transition temperature Tg 1st , the glass transition temperature Tga of the component insoluble in THF 1st , and the glass transition temperature Tg of the THF-soluble component 2nd By setting each of these to within a specific range, the toner can be said to be of high quality, since it has excellent low-temperature fixing property and heat-resistant storage stability and can suppress the occurrence of abnormal images.
[0570] Although the embodiment has been described above, the above embodiment is presented as an example, and the present invention is not limited to the above embodiment. The above embodiment can be implemented in various other forms, and various combinations, omissions, substitutions, modifications, etc. can be made without departing from the gist of the invention. These embodiments and their modifications are included in the scope and gist of the invention, and are included in the scope of the invention and its equivalents described in the claims. [Explanation of symbols]
[0571] 1. Image forming device 311Y, 311C, 311M, 311K photoreceptor 312Y, 312C, 312M, 312K Charging device 313Y, 313C, 313M, 313K developing device (developing section) 40 Transcription section 50 Fixing unit [Prior art documents] [Patent documents]
[0572] [Patent Document 1] JP 2018-180515 A
Claims
1. A toner comprising toner base particles containing a polyester resin and an external additive attached to the surface of the toner base particles, the external additive includes a plurality of organic fine particles arranged in a state where at least a part of the organic fine particles is embedded in the surface of the toner base particle, The particle size distribution of the organic fine particles has two or more peaks, Among the two or more peaks, a peak P1 at a position where the particle size is smallest is 10 nm to 40 nm, and a peak P2 at a position where the particle size is largest is 30 nm to 100 nm, The glass transition temperature Tg of the toner at the first temperature rise measured by differential scanning calorimetry 1st is between 30°C and 60°C, The glass transition temperature Tga of the component of the toner that is insoluble in tetrahydrofuran during the first heating cycle measured by differential scanning calorimetry 1st is −40° C. to 10° C., The glass transition temperature Tg of the tetrahydrofuran-soluble component of the toner measured by differential scanning calorimetry 2nd The toner has a temperature of 45°C to 65°C.
2. 2. The toner according to claim 1, wherein an average distance between adjacent organic fine particles on the surface of the toner base particle is 100 nm or less.
3. The toner according to claim 1 or 2, wherein the organic fine particles contain one or more kinds of styrene-acrylic resins having a carboxylic acid.
4. The organic fine particles are composed of two types of resins, 4. The toner according to claim 3, wherein the organic fine particles have a core layer containing one of the two types of resins, and a shell layer covering at least a portion of the core layer and containing the other of the two types of resins.
5. The glass transition temperature Tg of the organic fine particles at the first heating step measured by differential scanning calorimetry 1st The toner according to any one of claims 1 to 4, wherein the temperature is from 30°C to 70°C.
6. The glass transition temperature Tg of the toner at the first temperature rise measured by differential scanning calorimetry 1st and the glass transition temperature Tg in the second heating 2nd The toner according to any one of claims 1 to 5, wherein the difference between the temperature and the viscosity is 10°C or more.
7. A developer comprising the toner according to any one of claims 1 to 6 and a carrier.
8. A toner storage unit containing the toner according to any one of claims 1 to 6.
9. An electrostatic latent image carrier; an electrostatic latent image forming unit for forming an electrostatic latent image on the electrostatic latent image carrier; a developing section for developing the electrostatic latent image with toner to form a visible image; a transfer section for transferring the visible image onto a recording medium; a fixing unit that fixes the transferred image on the recording medium, 7. An image forming apparatus, wherein the toner is the toner according to claim 1.
Citation Information
Patent Citations
Electrophotographic developing toner
JP2002055481A
Electrostatic charge image developing toner, and process cartridge and image forming apparatus using the same, and method for manufacturing electrostatic charge image developing toner
JP2005092024A
Toner for electrostatic charge image development and production method of the toner
JP2012194327A
Toner and production method of toner
JP2012194470A
Toner, developer, and image forming apparatus
JP2018180515A