Manufacturing method of cast or forged products with bonded inserts

The method of press-fitting a tapered insert into a metal product with controlled expansion and cooling addresses the weakness of existing joint methods by forming a strong, defect-free bond without precise shaping, enhancing joint strength through concentrated pressure and grain flow lines.

JP7581926B2Active Publication Date: 2024-11-13TOYOTA JIDOSHA KK
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021014124
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-01
Publication Date
2024-11-13
Estimated Expiration
2041-02-01

AI Technical Summary

Technical Problem

Existing methods for joining metal materials with inserts, such as press-fitting or casting, rely heavily on the shape and positioning accuracy of the members, leading to weak bonds due to internal defects and gaps, which compromise the strength of the joint.

Method used

A method involving the use of a tapered insert that is press-fitted into a fitting hole of a metal product, where the fitting hole is expanded with the taper, and the metal is semi-cooled to form a strong bond without relying on precise shaping and positioning, while also removing internal defects by press-fitting and cooling.

Benefits of technology

This method creates a strong, defect-free bond between the insert and metal, enhancing the joint strength by concentrating pressure around the fitting hole and forming grain flow lines, resulting in a more robust connection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581926000001
    Figure 0007581926000001
  • Figure 0007581926000002
    Figure 0007581926000002
  • Figure 0007581926000003
    Figure 0007581926000003
Patent Text Reader

Abstract

To manufacture a metallic molded article having an insert joined thereto.SOLUTION: An insert 96 having a taper 97 is embedded in metal. The metal is semi-cooled down to a temperature which higher than a recrystallization temperature thereof and lower than a melting point thereof (thereafter called a press-fit temperature) to generate a metallic molded article MM having the insert welded thereto, where a hole in which the insert 96 is embedded (thereafter called a fitting hole 92) is formed in the metallic molded article MM. The taper 97 fits to the fitting hole 92. An undercut is not formed beyond a tip of the taper 97. At the press-in temperature, the insert 96 is pressed into the fitting hole 97, toward a direction in which the taper 97 narrows (thereafter called a press-in direction), while making the taper 97 expand the fitting hole 92, and the metallic molded article MM is further cooled with the insert pressed into the hole.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for making a casting or forging having an insert bonded thereto. [Background technology]

[0002] In Patent Document 1, a rivet made of an iron-based metal is press-fitted into a hole provided in a member made of a material other than an iron-based metal, such as carbon fiber reinforced plastic (CFRP), an aluminum alloy, or a magnesium alloy, to join the rivet and the member. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2018-089657 A [Patent Document 2] JP 2006-312192 A Summary of the Invention [Problem to be solved by the invention]

[0004] In order to strongly bond a metal material and an insert by press-fitting the insert into a hole in the metal material according to the method of Patent Document 1, the hole and the insert must be formed separately with high accuracy. Also, the position of the insert relative to the hole must be accurately determined when press-fitting. In one aspect of the present invention, a method for strongly bonding these members is provided without relying on the shape and positioning accuracy of the hole in the metal material and the insert.

[0005] In addition, in Patent Document 2, a steel insert is cast in aluminum to join them. Cast-in does not depend as much on improving the accuracy of shape processing and positioning to increase the strength of the joint as press-in. Also, since there is no gap between the insert and the casting, the strength of the joint is high. However, blowholes and other internal defects occur in the metal material around the cast-in insert. The internal defects weaken the joint between the insert and the metal material. In one aspect of the present invention, a method for removing internal defects around the insert that occur during cast-in is provided. [Means for solving the problem]

[0006] <1> A method for manufacturing a casting having an insert bonded thereto, comprising the steps of: A tapered insert made of a first material, which may be metal or nonmetal, is surrounded by molten metal made of a second material, which may be metal; The molten metal is semi-cooled to a temperature higher than the recrystallization temperature of the second material but lower than the melting point of the second material, hereinafter referred to as the pressing temperature, to produce a casting made of the second material, where a hole into which the insert is embedded, hereinafter referred to as the fitting hole, is formed in the casting, the taper fits into the fitting hole, and no undercut is formed beyond the tip of the taper, At the press-fitting temperature, the insert is press-fitted into the fitting hole of the casting while expanding the fitting hole with the taper in a direction in which the taper narrows, hereinafter referred to as the press-fitting direction; further cooling the casting while maintaining the pressing in place; method.

[0007] <2> The fitting hole penetrates the casting at least after the insert is pressed into the casting. <1> How to.

[0008] <3> The method is carried out using a mold having a first surface and a second surface facing each other across a cavity inside the mold, the first surface having a first opening, and the second surface having a second opening. <1> or <2> The method of claim 1, placing the insert in the cavity; The insert is sandwiched between an advance pin arranged on the first surface side and a retreat pin arranged on the second surface side, blocking the first opening with the insert or the advance pin and blocking the second opening with the insert or the retract pin; The insert is surrounded by the molten metal by injecting the molten metal into the cavity. The press-fitting is performed by the forward movement pin, the insert and the retraction pin moving in a row along the press-fitting direction. method.

[0009] <4> The second opening is blocked by the retraction pin; The insert is pushed by the forward pin, so that the molten metal penetrates between the head of the insert and the top of the retraction pin and is pushed out around the insert and solidified. further cooling the casting while maintaining the extrusion; <3> How to.

[0010] <5> blocking the second opening with the retraction pin, wherein a top of the retraction pin is larger than the tip of the taper; The head of the insert presses the retreat pin to create a space in the second opening, and the insert is pressed into the space beyond the second surface to displace excess volume of the casting; further cooling the casting while maintaining the displacement; <3> How to.

[0011] <6> The top of the retract pin further includes a protrusion at its center; The second opening is closed by an outer edge of the retraction pin; The molten metal is further injected into the cavity to cover the protrusion with the molten metal; By press-fitting the insert, at least a portion of the space occupied by the protrusion is replaced by the head of the insert. <5> How to.

[0012] <7> The insert further has a columnar surface extending to the head at a location beyond the tip and parallel to the press-fitting direction, The cylindrical surface fits into the fitting hole. <6> How to.

[0013] <8> the melting point of the first material is higher than the melting point of the second material; The Young's modulus of the first material is higher than the Young's modulus of the second material at the pressing temperature. The above method.

[0014] <9> The first material is iron or an alloy thereof; The second material is aluminum or an alloy thereof; The pressing temperature is higher than 150°C; The above method.

[0015] <10> A method for manufacturing a forged product having an insert bonded thereto, comprising the steps of: The metal block is molded by pressing the metal block with a die at a temperature higher than its recrystallization temperature and lower than its melting point (hereinafter referred to as the forging temperature). Further, at the forging temperature, a hole into which the insert is embedded (hereinafter, referred to as a fitting hole) is formed in the metal block by pressing a tapered insert into the metal block, the taper fitting into the fitting hole; The metal ingot is semi-cooled to a temperature higher than its recrystallization temperature and lower than the forging temperature (hereinafter referred to as the re-pressing temperature) to produce the forged product made of the metal ingot; At the re-pressing temperature, the insert is re-pressed into the fitting hole of the forging in the direction in which the taper narrows while pressing the periphery of the fitting hole of the forging with the die and expanding the fitting hole with the taper; Further cooling the forged product while maintaining the re-pressing. Manufacturing method. Effect of the Invention

[0016] In one aspect of the present invention, a method for strongly joining a hole in a metal material and an insert without relying on the accuracy of the shape and positioning of these members is provided. In another aspect of the present invention, a method for removing internal defects around an insert that occur in a cast-in insert is provided. [Brief description of the drawings]

[0017] [Figure 1] Schematic diagram of joining of insert and metal molded part. [Diagram 2] FIG. [Diagram 3] FIG. [Figure 4] FIG. 2 is a cross-sectional view of the insert and the casting. [Diagram 5] Cross-sectional views of various inserts. [Figure 6] Cross-sectional views of various inserts. [Figure 7] Cross-sectional views of various tapers. [Figure 8] 4A to 4C are cross-sectional views of various protrusions. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] FIG. 1 shows a cross-sectional view of the state of joining the insert 96 and the metal molded product MM. In this embodiment, unless otherwise specified, the cross section is a longitudinal cross section. The metal molded product MM is a cast or forged product. The insert 96 and the metal molded product MM are made of different materials. The upper part shows a state in which the insert 96 is inserted into the metal molded product MM. The lower part shows a state in which the insert 96 is further inserted into the metal molded product MM 92.

[0019] <Cast products>

[0020] When the metal molded product MM shown in the upper part of Fig. 1 is a casting, an insert 96 is cast in advance with molten metal. The insert 96 has a taper 97. In the upper part of the figure, a fitting hole 92 is formed in the metal molded product MM by casting. The taper 97 fits into the fitting hole 92.

[0021] In the upper part of Fig. 1, it is preferable that no undercut is formed beyond the tip of the taper 97, which is the lower end in the drawing. In this embodiment, the tip of the taper refers to the narrow side. It is preferable that the fitting hole 92 penetrates the metal molded product MM. In another embodiment, the fitting hole 92 does not penetrate the metal molded product MM.

[0022] In the upper part of Fig. 1, the metal molded product MM is produced by semi-cooling to the pressing temperature. The pressing temperature is higher than the recrystallization temperature of the metal molded product MM. The insert 96 is pressed into the fitting hole 92 of the metal molded product MM while the taper 97 expands the fitting hole 92 in the direction in which the taper 97 narrows. The pressing is performed by pushing the insert 96, which was originally inserted into the fitting hole 92, further into the fitting hole 92. The pressing generates a strong expansion pressure on the surface of the fitting hole 92. It also generates a strong tightening pressure on the surface of the taper 97.

[0023] In the lower part of Figure 1, new grain flows 94 are created around the fitting hole 92 due to the press-fit. Furthermore, even if there are internal defects around the fitting hole 92, these are crushed by the plastic flow of the semi-cooled metal and the pressure of the press-fit. Since semi-cooled metal has poor fluidity, the pressure of the press-fit is concentrated around the fitting hole 92. The metal molded product MM is further cooled while maintaining the press-fit of the insert 96. In this way, a bond is formed between the insert 96 and the metal molded product MM. The bond created by press-fitting is stronger than the bond achieved by insert casting alone.

[0024] 1, the fitting hole 92 preferably passes through the metal molded part MM. In another embodiment, the fitting hole 92 does not pass through the metal molded part MM.

[0025] <Forged products>

[0026] When the metal molded product MM shown in the upper part of Fig. 1 is a forged product, the metal block is pressed with a die 91 and an insert 96 is pressed into the metal block to perform forging. Forging is performed at a temperature higher than the recrystallization temperature and lower than its melting point, hereinafter referred to as the forging temperature. In the upper part of the figure, a fitting hole 92 is formed in the metal molded product MM by pressing the insert 96. The taper 97 fits into the fitting hole 92.

[0027] In the upper part of Fig. 1, the fitting hole 92 preferably passes through the metal part MM. In another embodiment, the fitting hole 92 does not pass through the metal part MM. The metal part MM is produced by semi-cooling to a re-pressing temperature that is lower than the forging temperature. The re-pressing temperature is higher than the recrystallization temperature of the metal part MM.

[0028] 1, the insert 96 is press-fitted again into the fitting hole 92 of the metal molded product MM while expanding the fitting hole 92 with the taper 97 in the direction in which the taper 97 narrows. The press-fitting again is performed by thrusting the insert 96, which was originally inserted into the fitting hole 92, further into the fitting hole 92.

[0029] 1, since the metal at the re-pressing temperature is less fluid than the metal at the forging temperature, the re-pressing pressure is concentrated especially around the fitting hole 92. The re-pressing generates a strong expansion pressure on the surface of the fitting hole 92. It also generates a strong clamping pressure on the surface of the taper 97. The re-pressing of the insert 96 is performed while the periphery of the fitting hole 92 is held down by the die 91.

[0030] 1, the metal molded product MM is further cooled while maintaining the insert 96 pressed in again. As a result, a bond is formed between the insert 96 and the metal molded product MM. The bond formed by the press-in again is stronger than the bond obtained by only pressing at the forging temperature.

[0031] 1, the fitting hole 92 preferably passes through the metal molded part MM. In another embodiment, the fitting hole 92 does not pass through the metal molded part MM. EXAMPLES

[0032] The invention will be further illustrated in the following examples with reference to cast articles, although the following examples may also be applied to the forged articles mentioned above.

[0033] <Summary>

[0034] 2 is a cross-sectional view of the insert 16 and other tools. The other tools include a mold 10, an advance pin 15a, and a retreat pin 15b. The mold 10 has an upper die 11a and a lower die 11b. The mold 10 has a cavity 13 between the upper die 11a and the lower die 11b. Using these tools, a casting with the insert 16 bonded thereto is manufactured by insert fitting and press-fitting.

[0035] Fig. 3 shows a cross section of the molten metal 20 poured into the mold 10. Casting is performed by die casting. Fig. 4 shows a cross section of the casting 25 formed in the cavity 13. An insert 16 is pressed into the casting 25 that is retained in the cavity 13.

[0036] <insert>

[0037] Returning to FIG. 2, the insert 16 shown in FIG. 2 is made of a material different from the casting metal. In this embodiment, the material constituting the insert 16 is referred to as a first material. The first material is a metal or a non-metal. In one aspect, the metal is any one of iron, copper, titanium, and nickel, or an alloy thereof. In one aspect, the iron alloy is steel. In one aspect, the non-metal is a ceramic. Also, in this embodiment, the casting metal is referred to as a second material. The insert 16 is cast-in with the second material.

[0038] As shown in Figure 2, insert 16 is placed in cavity 13. Insert 16 has taper 17 in its center. As mentioned above, press-fitting is performed in the direction in which taper 17 narrows. This direction is called the press-fitting direction. In the figure, the press-fitting direction is downward. The tip of taper 17 is at the leading side of the press-fitting direction.

[0039] As shown in Figure 2, the insert 16 further has a cylindrical surface 18a parallel to the press-fit direction on the thicker side of the taper 17. The cylindrical surface 18b extends to the tail of the insert 16. In this embodiment, the "tail" of the insert refers to the rear end in the press-fit direction. In other embodiments, the insert 16 does not have the cylindrical surface 18a. The end face of the insert 16 that contacts the forward movement pin 15a is flat.

[0040] As shown in Figure 2, the insert 16 further has a columnar surface 18b parallel to the press-fit direction on the narrow side of the taper 17. The columnar surface 18b extends to the head of the insert 16. In this embodiment, the "head" of the insert refers to the front end in the press-fit direction. In other embodiments, the insert 16 does not have the columnar surface 18b. The end face of the insert 16 that contacts the retract pin 15b is flat.

[0041] The shape of the insert 16 shown in Fig. 2 is an example. The tail of the insert 16 may extend to the inside of the upper die 11a. The head of the insert 16 may extend to the inside of the upper die 11b. The inside of the insert 16 may have a cavity.

[0042] <Mold>

[0043] As shown in Fig. 2, the mold 10 has a first surface 12a and a second surface 12b. The first surface 12a is located on an upper mold 11a. The second surface 12b is located on a lower mold 11b. The first surface 12a and the second surface 12b face each other with a cavity 13 therebetween. The first surface 12a has a first opening 14a. The second surface 12b has a second opening 14b.

[0044] <Pin>

[0045] As shown in Fig. 2, the advance pin 15a is disposed on the first surface 12a side. The retract pin 15b is disposed on the second surface 12b side. The advance pin 15a and the retract pin 15b are disposed in a pair so as to sandwich the insert 16. In one embodiment, the tail of the insert 16 contacts the top of the advance pin 15a, and the head of the insert 16 contacts the top of the retract pin 15b. In this embodiment, the "top" of each pin refers to the end closest to the insert.

[0046] The top of the retraction pin 15b shown in FIG. 2 is preferably larger than the head of the insert 16 when viewed in plan. The top of the retraction pin 15b is preferably larger than the tip of the taper 17 when viewed in plan. The top of the retraction pin 15b preferably further has a protrusion 19 at its center. In one embodiment, the protrusion 19 is equal in size to the head of the insert 16 when viewed in plan. In one embodiment, the protrusion 19 is equal in size to the columnar surface 18b of the insert 16 when viewed in plan. In one embodiment, the protrusion 19 is equal in size to the tip of the taper 17 when viewed in plan.

[0047] As shown in FIG. 2, the first opening 14a is blocked by an insert 16. In another embodiment, the first opening 14a is blocked by an advance pin 15a. Also, the second opening 14b is blocked by a retract pin 15b. In another embodiment, the second opening 14b is blocked by an insert 16. Preferably, the second opening 14b is blocked by the outer edge of the top of the retract pin 15b. In one embodiment, the outer edge of the retract pin 15b is flush with the second surface 12b of the lower mold 11b, so that no step is created between them. In another embodiment, the second opening 14b is blocked by a protrusion 19.

[0048] <Cast doll>

[0049] As shown in Fig. 3, a molten metal 20 made of the second material is poured into the cavity in the mold 10. The insert 16 is surrounded by the molten metal 20. It is preferable that the protrusion 19 is also surrounded by the molten metal 20. The molten metal 20 is semi-cooled to a predetermined injection temperature to produce a molded product made of the second material.

[0050] 3 is higher than the recrystallization temperature of the second material constituting the molten metal 20 and is lower than the melting point of the second material. In one embodiment, the melting point of the first material of the molten metal 20 is higher than the melting point of the second material of the molten metal 20.

[0051] 3, a molded product produced from molten metal 20 has a hole, a fitting hole 22, into which insert 16 is embedded. Taper 17 fits into fitting hole 22. Columnar surfaces 18a and 18b also fit into fitting hole 22. It is preferable that no undercut is formed beyond the tip of taper 17 in the molded product.

[0052] In one embodiment, the second material that is the molten metal 20 shown in FIG. 3 is any one of aluminum, magnesium, and zinc, and alloys thereof.

[0053] In one example, the second material of the molten metal 20 shown in FIG. 3 is pure aluminum or an aluminum alloy. In one embodiment, the pressing temperature is higher than 150° C. These second materials exhibit high ductility at temperatures above 150° C. Therefore, the fitting hole 22 is less likely to crack when the insert 16 is pressed into the casting in the process described below.

[0054] <Press-fit>

[0055] As shown in Fig. 4, the insert 16 is press-fitted into the fitting hole 22 at the press-fitting temperature. The press-fitting is performed in the direction in which the taper 17 narrows, that is, the press-fitting direction. The press-fitting is performed by thrusting the insert 16 into the fitting hole 22 while pushing the fitting hole 22 open with the taper 17. The press-fitting generates pressure that expands the surface of the fitting hole 22 and pressure that tightens the surface of the taper 17.

[0056] As shown in Fig. 4, the press-fit is performed by pushing the insert 16 and the retraction pin 15b with the advancement pin 15a. The advancement pin 15a and the insert 16 slide on the first opening 14a in the press-fit direction. The retraction pin 15b slides on the second opening 14b in the press-fit direction.

[0057] 4, the forward pin 15a, the insert 16, and the retract pin 15b advance in a row along the press-fit direction. As the retract pin 15b escapes from the cavity 13, the insert 16 advances into the area where the retract pin 15b is no longer present. The retract pin 15b relieves the pressure acting on the head of the insert 16 to push the insert 16 back.

[0058] In one embodiment, the advance pin 15a and the insert 16 shown in Figure 4 are both rotationally symmetrical and have the same center of rotation. In another embodiment, the advance pin 15a is rotated by the insert 16 around the center of rotation as an axis while being thrust in. A strong shear force acts on the surface of the fitting hole 22, further hardening the surface of the fitting hole 22 and providing a strong joint.

[0059] In one embodiment, the recrystallization temperature of the second material of the casting 25 shown in Fig. 4 is higher than room temperature. In one example, the room temperature is 5 to 35°C (JIS standard). Furthermore, the Young's modulus of the first material of the insert 16 is higher than the Young's modulus of the second material of the casting 25 at the pressing temperature. Therefore, the metal structure around the fitting hole 22 has a state in which it has been forged by the insert 16. Grain flows 24 are formed in the metal structure around the fitting hole 22 of the casting 25 by the pressing.

[0060] In one embodiment shown in Figure 4, it is preferable that the fitting hole 22 penetrates the casting 25 after press-fitting. Since a non-through hole has a bottom at which stress is concentrated and is prone to cracking, it is advantageous for the fitting hole 22 not to have such a bottom. In another embodiment, the fitting hole 22 does not penetrate the casting 25.

[0061] <Removal of the casting>

[0062] 4, while maintaining the insert 16 pressed in as described above, the casting 25 is further cooled, preferably to a temperature lower than the recrystallization temperature of the second material. The upper die 11a, the lower die 11b, the forward pin 15a, and the backward pin 15b are removed from the casting 25, and the casting 25 with the insert 16 joined thereto is taken out.

[0063] <Application example: Removing burrs>

[0064] Returning to Fig. 3, as shown in the figure, the molten metal 20 may seep into the gap between the head of the insert 16 and the top of the retraction pin 15b. Specifically, the molten metal seeps into the gap between the head of the insert 16 and the protrusion 19. The seeped molten metal 20 solidifies and becomes a burr. In one embodiment, the burr is removed during press-fitting.

[0065] As shown in FIG. 4, the insert 16 is pushed in by the forward pin 15a. The retraction pin 15b is supported in the second opening 14b. The head of the insert 16 reaches the top of the retraction pin 15b. The insert 16 and the retraction pin 15b push aside any burrs that may have formed between them. This burr removal is performed simultaneously with the joining of the insert 16 and the casting 25 by press-fitting.

[0066] 4, while maintaining the state in which the burrs are removed from between the insert 16 and the retraction pin 15b, the casting 25 is further cooled, preferably to a temperature lower than the recrystallization temperature of the second material.

[0067] 4, the flash between the insert 16 and the retraction pin 15b may remain in the casting 25. The flash may be removed after the casting 25 is removed from the mold 10 and the retraction pin 15b is separated from the casting 25.

[0068] <Application example: Relieving excess volume>

[0069] As shown in Figures 3 and 4, by pressing the insert 16 into the casting 25, the metal around the fitting hole 22 is pushed out. Furthermore, the metal between the insert 16 and the retract pin 15b is also pushed out. Since the casting 25 is in a semi-cooled state, the resulting pressure remains around the fitting hole 22. If the pressure is too high, it becomes difficult to press the insert 16 in. Therefore, the retract pin 15b and others are designed as follows to release the excess volume of the casting 25 and weaken the press-in.

[0070] 4, the top of the retraction pin 15b is larger than the tip of the taper 17. Therefore, by pushing the retraction pin 15b with the tip of the taper 17, a space 23 is created in the second opening 14b. This allows the excess volume of the casting 25 to be pushed out into the space 23 beyond the second surface 12b.

[0071] As shown in FIG. 4, the casting 25 is further cooled while maintaining the state in which the excess volume of the casting 25 is pushed aside.

[0072] <Application example: Adjusting the amount of insert protrusion>

[0073] Returning to FIG. 2, the top of the retraction pin 15b has a protrusion 19 at its center. Also, the outer edge of the retraction pin 15b closes the second opening 14b. Molten metal is poured into the cavity 13, so that the protrusion 19 is enveloped in molten metal 20 as shown in FIG. 3. After the molten metal 20 is cooled to the pressing temperature, the insert 16 is pressed in to a depth not exceeding the height of the protrusion 19 as shown in FIG. 4.

[0074] As shown in FIG. 4, by press-fitting the insert 16, at least a part of the space occupied by the projection 19, and preferably the entirety of the space, is replaced by the head of the insert 16.

[0075] 2 to 4, the projection 19 has the same size as the head of the insert 16 when viewed in a plan view. In one embodiment, the projection 19 has the same size as the columnar surface 18b of the insert 16 when viewed in a plan view. In one embodiment, the projection 19 has the same size as the tip of the taper 17 when viewed in a plan view. The head of the insert 16 smoothly enters the space previously occupied by the projection 19.

[0076] As shown in Fig. 4, it is preferable that the head of the insert 16 does not protrude from the surface of the casting 25. The casting 25 is further cooled while maintaining this pressed-in state. By adjusting the height of the protrusion 19, the protruding height or recessed depth of the head of the insert 16 relative to the second surface 12b of the mold 10 can be set to any desired value. In a preferred embodiment, the height of the end face of the head of the insert 16 is aligned with the second surface 12b of the mold 10 when the pressing is completed.

[0077] <Modifications: Variations in insert shape>

[0078] FIG. 5 shows the cross-sectional shapes of variations of the insert 96 (FIG. 1) and the insert 16 (FIGS. 2-4). The inserts 26a-26g are pressed into the metal molded product MM by moving downward in the figure. For convenience, the lower part of the figure is the head of the insert, and the upper part of the figure is the tail of the insert. Unless otherwise specified, the taper of the insert becomes narrower from the tail side toward the head side.

[0079] The inserts 26a to 26g shown in Fig. 5 have tapers. These tapers become thinner mainly from the tail side to the head side. The insert 26a has a taper at the head and a columnar surface at the tail that continues from the base of the taper. The insert 26b is formed with a taper all the way from the end of the head to the end of the tail. The insert 26c has a taper that is rounded on the head side.

[0080] The insert 26d shown in Figure 5 has a taper at the head and a taper at the tail, but the taper at the tail narrows in the direction opposite to the press-fitting direction.

[0081] The insert 26e shown in FIG. 5 has a cylindrical surface at the head and a taper at the tail. The insert 26f has a taper at the head and a cylindrical surface at the tail. The diameter of the cylindrical surface is larger than the diameter at the base of the taper. It also has a table surface connecting the taper and the cylindrical surface. The insert 26g has a cylindrical surface at the head and a taper at the tail. The taper of the tail is rounded on the head side.

[0082] Figure 6 shows the cross section of another insert. Inserts 36a to 36c and 36e to 36g have a taper. These tapers are so-called reverse tapers, which become thicker from the tail side toward the head side. Even if these inserts are pressed into the fitting hole of the metal molded product MM from the head side, no tightening pressure is generated on the reverse tapered surface. Therefore, it is preferable to use inserts with tapers as shown in Figures 1 to 5 for joining the inserts and the metal molded product MM.

[0083] The insert 36d shown in FIG. 6 has a reverse taper at the head and a constricted type with a reverse taper at the tail. However, the reverse taper at the tail narrows along the press-fit direction. Therefore, at first glance, it is expected that tightening pressure will be applied to the taper at the tail when the insert is pressed into the fitting hole. However, in this example, a pocket is formed between the reverse taper at the head and the surface of the fitting hole, which may promote fretting failure. Therefore, as shown in FIGS. 1 to 5, it is preferable that no undercut is formed beyond the tip of the taper.

[0084] <Modification: Variation of the position of the insert after press-fitting>

[0085] Figure 7 shows cross-sectional views of variations in the position of the insert after press-fitting. The metal molded product MM has a mating hole that runs through it. The mating hole has a reverse taper. The surface on the thicker side of the reverse taper of the mating hole is the first surface. The surface on the thinner side of the reverse taper is the second surface.

[0086] As shown in FIG. 7, the end face of the tail portion of the insert 27a is flush with the first surface of the metal molded product MM. The end face of the head portion of the insert 27a is flush with the second surface of the metal molded product MM. The tail portion of the insert 27b protrudes from the first surface of the metal molded product MM. The end face of the head portion of the insert 27b is flush with the second surface of the metal molded product MM. The tail portion of the insert 27c protrudes from the first surface of the metal molded product MM, and the head portion of the insert 27c protrudes from the second surface. The end face of the tail portion of the insert 27d is lower than the first surface of the metal molded product MM, but the head portion of the insert 27c protrudes from the second surface. The end face of the tail portion of the insert 27e is lower than the first surface of the metal molded product MM, and the end face of the head portion of the insert 27e is lower than the second surface of the metal molded product MM.

[0087] In this embodiment, the position of the insert relative to the metal molded product can be set as desired. The desired position can be obtained by adjusting the height of the insert, the height of the projection of the retraction pin, and the depth of the press fit. By adjusting these, the step between the end face of the insert and the surface of the metal molded product can be reduced.

[0088] <Variations in the shape of the retract pin protrusion>

[0089] Fig. 8 shows variations in the cross-sectional shape of the protrusion on the top surface of the retraction pin. Like the retraction pin 15b shown in Fig. 2, the retraction pins 28a to 28d shown in Fig. 8 also close the openings of the lower die 11b.

[0090] Retract pin 28a shown in Figure 8 has a tapered protrusion 29a. Retract pin 28b has a rounded tapered protrusion 29b. Retract pin 28c has a columnar protrusion 29c. Retract pins with these protrusions are easily detached from semi-cooled casting 25. Retract pin 28d has a reverse tapered protrusion 29d. Because protrusion 29d is an undercut shape relative to casting 25, retract pin 28d is less likely to detach from semi-cooled casting 25. [Explanation of symbols]

[0091] 10 mold, 11a upper mold, 11b lower mold, 12a first surface, 12b second surface, 13 cavity, 14a first opening, 14b second opening, 15a forward pin, 15b retract pin, 16 insert, 17 taper, 18a-b columnar surface, 19 protrusion, 20 molten metal, 22 mating hole, 23 space, 24 grain flow line, 25 casting, 26a-g insert, 27a-e insert, 28a-d retract pin, 29a-d protrusion, 36a-g insert, 91 mold, 92 mating hole, 94 grain flow line, 96 insert, 97 taper, MM metal forming product

Claims

1. A method for manufacturing a casting having an insert bonded thereto, comprising using a mold having a first surface and a second surface facing each other across a cavity inside the mold, the first surface having a first opening, and the second surface having a second opening, disposing an insert in the cavity, the insert being made of a first material, which may be metallic or non-metallic, and having a taper; The insert is sandwiched between an advance pin arranged on the first surface side and a retreat pin arranged on the second surface side, blocking the first opening with the insert or the advance pin and blocking the second opening with the insert or the retract pin; Injecting a molten metal of a second material, which is a metal, into the cavity to surround the insert; The molten metal is semi-cooled to a temperature higher than the recrystallization temperature of the second material but lower than the melting point of the second material, hereinafter referred to as the pressing temperature, to produce a casting made of the second material, where a hole into which the insert is embedded, hereinafter referred to as the fitting hole, is formed in the casting, the taper fits into the fitting hole, and no undercut is formed beyond the tip of the taper, At the press-fitting temperature, the forward movement pin, the insert and the retraction pin advance in a row along a direction in which the taper narrows, hereinafter referred to as a press-fitting direction, so that the insert is press-fitted into the fitting hole of the casting while the taper expands the fitting hole; further cooling the casting while maintaining the pressing in place; A method for manufacturing a casting having a bonded insert.

2. The fitting hole penetrates the casting at least after the insert is pressed into the casting. A method for producing a casting having the insert of claim 1 bonded thereto.

3. The second opening is blocked by the retraction pin; The insert is pushed by the forward pin, so that the molten metal penetrates between the head of the insert and the top of the retraction pin and is pushed out around the insert and solidifies. further cooling the casting while maintaining the extrusion; A method for producing a casting having the insert according to claim 1 or 2 bonded thereto.

4. blocking the second opening with the retraction pin, wherein a top of the retraction pin is larger than the tip of the taper; The head of the insert is used to push the retraction pin into the second opening, creating a space within the second opening, and the insert is pressed into the second opening to displace excess volume of the casting beyond the second surface into the space; further cooling the casting while maintaining the displacement; A method for producing a casting having the insert according to claim 1 or 2 bonded thereto.

5. The top of the retract pin further includes a protrusion at its center; The second opening is blocked by an outer edge of the retraction pin; The molten metal is further injected into the cavity to cover the protrusion with the molten metal; By press-fitting the insert, at least a portion of the space occupied by the protrusion is replaced by the head of the insert. A method for producing a casting having the insert bonded thereto according to claim 4.

6. The insert further has a columnar surface extending to the head at a location beyond the tip and parallel to the press-fitting direction, The cylindrical surface fits into the fitting hole. A method for producing a casting having the insert bonded thereto according to claim 5.

7. the melting point of the first material is higher than the melting point of the second material; The Young's modulus of the first material is higher than the Young's modulus of the second material at the pressing temperature. A method for producing a casting having the insert according to any one of claims 1 to 6 bonded thereto.

8. The first material is iron or an alloy thereof, The second material is aluminum or an alloy thereof; The pressing temperature is higher than 150°C; A method for producing a casting having the insert according to any one of claims 1 to 6 bonded thereto.

Citation Information

Patent Citations

  • JP1975125927A

  • Insert bonding method and insert bonding device of object to be bonded by dieecasting

    JP1980117552A

  • Method of producing metal composite component

    JP2004237298A

  • Method for joining dissimilar metal product

    JP2006312192A

  • Cast-in structure of vehicle component and cast-in mold

    JP2013132676A