Toner, developer, toner storage unit, image forming apparatus, and image forming method
The core-shell structured toner with resin fine particles addresses the challenge of achieving low-temperature fixability and heat-resistant storage stability while preventing contamination, ensuring effective cleaning performance.
Patent Information
- Application Number
- JP2021030706
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-26
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2041-02-26
AI Technical Summary
Conventional toners struggle to simultaneously achieve low-temperature fixability, heat-resistant storage stability, good cleaning properties, and prevent contamination of cleaning members and photoreceptors, with external additives like inorganic fine particles causing contamination issues.
A toner with a core-shell structure where the shell part has a higher glass transition temperature than the core part, and specific elastic modulus ranges, coated with resin fine particles to reduce inorganic additives, ensuring both low-temperature fixability and heat-resistant storage stability while minimizing contamination.
The toner achieves both low-temperature fixability and heat-resistant storage stability while maintaining good cleaning properties and reducing contamination of cleaning members and photoreceptors.
Smart Images

Figure 0007581961000012 
Figure 0007581961000013 
Figure 0007581961000014
Abstract
Description
[Technical field]
[0001] The present invention relates to a toner, a developer, a toner storage unit, an image forming apparatus, and an image forming method. [Background technology]
[0002] In recent years, toners are required to have smaller particle size and high-temperature offset resistance for improving the quality of output images, low-temperature fixability for energy saving, and heat-resistant storage stability capable of withstanding high temperatures and high humidity during storage and transportation after production. In particular, since the power consumption during fixation accounts for a large portion of the power consumption in the image forming process, improving low-temperature fixability is extremely important.
[0003] In order to improve the low-temperature fixing property of a toner, it is necessary to use a material with a low melting point for the toner. However, a toner produced using a material with a low melting point has poor heat-resistant storage stability, and there is a trade-off between low-temperature fixing property and heat-resistant storage stability.
[0004] In order to achieve both low-temperature fixability and heat-resistant storage stability, a method for producing composite resin particles has been proposed that includes a step of forming composite resin particles in which resin fine particles containing two types of resin as constituents in the same particle are attached to the surface of the resin particles, and then removing part or all of the resin from the resin fine particles (see, for example, Patent Documents 1 to 3). Patent Document 4 also proposes that resin fine particles be present on the surface of toner particles. Summary of the Invention [Problem to be solved by the invention]
[0005] However, in the conventional technology, there is a demand for a technology that can simultaneously satisfy both low-temperature fixability and heat-resistant storage stability, good cleaning properties for a photoconductor (electrostatic latent image carrier), and suppression of contamination of a cleaning member or a photoconductor. For example, an external additive such as inorganic fine particles acts as a lubricant and is expected to contribute to improving cleaning properties, but on the other hand, there is a concern that such an external additive may cause contamination of a cleaning member such as a cleaning blade or a photoconductor.
[0006] An object of the present invention is to provide a toner which can achieve both low-temperature fixability and heat-resistant storage stability, and which can suppress contamination of cleaning members and photoconductors while maintaining good cleaning properties. [Means for solving the problem]
[0007] In order to achieve the above object, the toner of the present invention is a toner in which the surfaces of toner base particles containing a binder resin, a colorant, and a wax are coated with resin fine particles, the resin fine particles having a core-shell structure consisting of a shell portion and a core portion, the glass transition temperature TgA of the shell portion being higher than the glass temperature TgB of the core portion, and when the toner is measured with a rheometer, the storage modulus G'1 at 70° C. during heating is 1.0×10 5 Pa or more 1.0×10 6 Pa or less, and the storage modulus G'2 at 100°C during heating is 1.0 x 10 4 Pa or more 5.0×10 4 Pa or less The toner contains a reaction product of a polyester prepolymer having an isocyanate group, the polyester prepolymer has a structure in which a polyol and a polycarboxylic acid are polycondensed, and the polyol contains a chain alkylene glycol having 2 to 12 carbon atoms. It is characterized by: Effect of the Invention
[0008] According to the present invention, it is possible to provide a toner which can achieve both low-temperature fixability and heat-resistant storage stability, and which can suppress contamination of cleaning members and photoconductors while maintaining good cleaning properties. [Brief description of the drawings]
[0009] [Figure 1] 3A and 3B are schematic diagrams illustrating an example of a state of a toner surface. [Diagram 2] FIG. 2 is a diagram showing an example of an SEM image of a toner surface. [Diagram 3] FIG. 2 is a diagram for explaining how to determine Tg in a DSC curve. [Figure 4] FIG. 2 is a schematic view illustrating an example of a process cartridge of the present invention. [Diagram 5] 1 is a schematic diagram illustrating an example of an image forming apparatus of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The toner, developer, toner storage unit, image forming apparatus, and image forming method according to the present invention will be described below with reference to the drawings. Note that the present invention is not limited to the following embodiments, and may be modified within the scope of what a person skilled in the art can imagine, such as other embodiments, additions, modifications, and deletions, and any aspect is within the scope of the present invention as long as it achieves the functions and effects of the present invention.
[0011] (toner) The toner of the present invention is a toner in which the surfaces of toner base particles containing a binder resin, a colorant, and a wax are coated with resin fine particles, the resin fine particles having a core-shell structure consisting of a shell portion and a core portion, the glass transition temperature TgA of the shell portion being higher than the glass temperature TgB of the core portion, and when the toner is measured with a rheometer, the storage modulus G'1 at 70° C. during heating is 1.0×10 5 Pa or more 1.0×10 6 Pa or less, and the storage modulus G'2 at 100°C during heating is 1.0 x 10 4 Pa or more 5.0×10 4 It is characterized in that the tensile strength is less than or equal to Pa.
[0012] In the prior art, additives such as inorganic fine particles such as silica and titanium oxide are added to the surface of a general toner to impart fluidity and chargeability. In toner cleaning, it is known that the toner is blocked on a photoconductor (also called an image carrier or electrostatic latent image carrier) by a cleaning blade, which is an example of a cleaning member, and the additives are liberated from the blocked toner. The liberated additives are supplied to the contact portion between the cleaning blade and the image carrier, and a pool layer of the additives is formed. This acts as a lubricant between the cleaning blade and the image carrier, thereby obtaining good cleaning properties of the toner. However, if the amount of additives is large, the amount of additives liberated from the toner also increases accordingly, which causes contamination of the cleaning blade and the photoconductor, and the wear of the cleaning blade and the deterioration of the photoconductor become significant. In particular, when inorganic fine particles are used as an external additive, such problems become significant.
[0013] In contrast, the present invention can achieve both low-temperature fixability and heat-resistant storage stability, and can suppress contamination of cleaning members and photoconductors while maintaining good cleaning properties. In the present invention, the surfaces of the toner base particles are covered with resin fine particles, so that the resin fine particles do not inhibit fixing and can harden the toner, making it possible to reduce additives in inorganic fine particles. As a result, contamination of cleaning members and photoconductors can be suppressed while maintaining good cleaning properties. In addition, by making the glass transition temperatures of the shell and core parts and the storage modulus of the toner satisfy the ranges of the present invention, reliability (storability, adhesion) can be ensured even with reduced additives, and both low-temperature fixability and heat-resistant storage stability can be achieved.
[0014] <Storage modulus of toner> The toner of the present invention has a storage modulus G'1 of 1.0×10 at 70° C. during heating, as measured by a rheometer. 5 Pa or more 1.0×10 6 Pa or less, and the storage modulus G'2 at 100°C during heating is 1.0 x 10 4 Pa or more 5.0×10 4 Pa or less. When these conditions are satisfied, the above-mentioned effects can be obtained.
[0015] The storage modulus G'1 at 70°C during heating is 1.0×10 5 Less than Pa or 1.0 x 10 6 If it exceeds Pa, it becomes difficult to achieve both the fixing property and the heat-resistant storage stability of the toner. The storage modulus G'1 at 70°C during heating is 1.0×10 5 Pa or more 1.0×10 6 In order to achieve this, for example, the content ratio of the crystalline resin, the non-crystalline resin, and the resin particles may be appropriately adjusted.
[0016] The storage modulus G'2 at 100°C during heating is 1.0×10 4 Less than Pa or 5.0 x 10 4 If it exceeds Pa, it becomes difficult to achieve both the fixing property and the heat-resistant storage stability of the toner. The storage modulus G'2 at 100°C during heating is 1.0×10 4 Pa or more 5.0×10 4 In order to achieve this, for example, the content ratio of the crystalline resin, the non-crystalline resin, and the resin particles may be appropriately adjusted.
[0017] <Resin fine particles> In the present invention, the resin particles covering the surface of the toner base particle have a core-shell structure consisting of a shell portion and a core portion, and the glass transition temperature TgA of the shell portion is higher than the glass temperature TgB of the core portion. As will be described in detail later, the glass transition temperature TgA of the shell portion is higher than the glass temperature TgB of the core portion, so that high heat-resistant storage stability can be ensured.
[0018] The resin particles cover the surface of the toner base particles, and the coverage of the resin particles on the surface of the toner base particles is preferably 30% or more and 90% or less, and more preferably 30% or more and 70% or less. A coverage rate of 30% or more ensures the heat-resistant storage stability of the toner, while a coverage rate of 90% or less allows external additives to adhere easily and facilitates heat transfer during toner fixing, ensuring fixability. Furthermore, a coverage rate of 70% or less improves the above effects.
[0019] The coverage of the resin particles on the surface of the toner base particles is measured as follows. The resin particles on the surface of the toner matrix are observed under a scanning electron microscope (SEM), and the area ratio of the resin particles to the area of the toner matrix is calculated using image processing software.
[0020] The standard deviation of the distance between adjacent resin particles present on the surface of the toner base particle is preferably 500 nm or less, more preferably 250 nm or less, and even more preferably 100 nm or less. The lower limit of the standard deviation is preferably 10 nm or more. When the standard deviation is 500 nm or less, both low-temperature fixability and heat-resistant storage stability can be achieved at a high level, and the occurrence of abnormal images due to filming can be suppressed while maintaining good cleaning properties.
[0021] The average distance between the resin fine particles is preferably from 10 nm to 500 nm, and more preferably from 20 nm to 250 nm.
[0022] Examples of methods for making the standard deviation of the distance between adjacent resin particles present on the surface of a toner base particle 500 nm or less include the following: A method of designing a formulation so that the coverage rate of resin particles with respect to the target toner particle size is 90% or more, and adding the resin particles during the emulsification process to densely attach the resin particles to the toner surface, and a method of reducing the distance between resin particles by efficiently attaching the resin particles by adjusting the average circularity of the toner.
[0023] In the present invention, the distance between adjacent resin microparticles is the distance between the centers of the resin microparticles. The center of the resin microparticle refers to the center point of an image of the resin microparticles observed with a scanning electron microscope (SEM). The surface of the toner matrix is not flat but slightly rounded (curved), so the distance between the resin particles is not the distance between the resin particles on the surface of the toner matrix measured, but the shortest distance between the resin particles on the surface of the toner matrix photographed by a scanning electron microscope (SEM).
[0024] Here, Fig. 1 is a schematic diagram showing an example of the state of a toner surface. Resin fine particles 3 are attached to the surface of a toner base particle 4. The resin fine particles 3 are composed of a core resin (b2) 2 and a shell resin (b1) 1, which will be described later. C1 and C2 indicate the centers of the resin fine particles 3. M indicates the volume average primary particle diameter of the resin fine particles 3. L indicates the distance between adjacent resin fine particles 3.
[0025] 2 is an example of a SEM image of a toner surface. As shown in the figure, fine resin particles 3 are attached to the surface of a toner base particle 4.
[0026] The method for measuring the distance between the resin particles will be described below. The external additives are removed as much as possible by ultrasonic wave to separate the external additives, and the particles are made to be in a state close to the toner base particles, and the average value and standard deviation of the distance between the resin particles are obtained.
[0027] -How to separate external additives- [1] Add 50 ml of a 5% by weight aqueous solution containing a surfactant (product name: Noigen ET-165, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) to a 100 ml screw tube, add 3 g of toner to the mixture, and gently move it up and down and left and right. Then, mix with a ball mill for 30 minutes so that the toner blends with the dispersion solution.
[0028] [2] Then, using an ultrasonic homogenizer (product name homogenizer, model VCX750, CV33, manufactured by SONICS & MATERIALS LLC), set the output to 40 W and apply ultrasonic energy for 60 minutes.
[0029] [Ultrasonic conditions] Vibration time: 60 minutes continuous ·Amplitude: 40W ·Vibration start temperature: 23±1.5℃ ·Temperature during vibration: 23±1.5℃
[0030] [3](1) The dispersion liquid is suction filtered using filter paper (product name: Qualitative Filter Paper (No. 2, 110 mm), manufactured by Advantec Toyo Co., Ltd.), washed twice again with ion-exchanged water, filtered, and the liberated additives are removed, and the toner particles are then dried. (2) The toner obtained in (1) is observed with a scanning electron microscope (SEM). First, external additives and fillers containing Si are detected by observing the backscattered electron image. (3) The image of (1) is binarized using image processing software (ImageJ) to remove the external additives and fillers.
[0031] Next, a secondary electron image is observed at the same position as in (1). Since the resin fine particles cannot be observed in the reflected electron image and can only be observed in the secondary electron image, the image is compared with the image obtained in (3), and the fine particles present in the areas other than the remaining external additives and filler (areas other than those removed in (3)) are regarded as resin fine particles, and the distance between the resin fine particles (the distance connecting the centers of the particles) is measured using the image processing software. This measurement is carried out for 100 binarized images (one toner particle per image), and the average value is regarded as the average value of the distance between the resin fine particles.
[0032] The standard deviation of the distance between the resin fine particles is calculated by the following formula, where the interparticle distance is x.
[0033]
number
[0034] [Shooting conditions] Scanning electron microscope: SU-8230 (Hitachi High-Technologies Corporation) Magnification: 35,000x Image capture: SE(L): Secondary electrons, BSE (backscattered electrons) Acceleration voltage: 2.0kV ·Acceleration current: 1.0μA ·Probe current:Normal Focus mode: UHR WD:8.0mm
[0035] The volume average primary particle diameter of the resin fine particles is preferably 5 nm to 100 nm, more preferably 10 nm to 100 nm, and even more preferably 10 nm to 50 nm. When the volume average primary particle diameter satisfies the above range, low temperature fixability is improved.
[0036] The volume average primary particle size can be measured, for example, by observing images taken with a scanning electron microscope (SEM).
[0037] The resin fine particles (hereinafter, sometimes referred to as "resin fine particles (B)") preferably have a core resin (core portion) and a shell resin (outer shell portion) that covers at least a part of the surface of the core resin, more preferably consist of a core resin and a shell resin, and further preferably contain a vinyl-based unit consisting of resin (b1) and resin (b2).
[0038] The shell resin (hereinafter also referred to as "resin (b1)") and the core resin (hereinafter also referred to as "resin (b2)") are preferably polymers obtained by homopolymerizing or copolymerizing vinyl monomers.
[0039] Examples of the vinyl monomer include the following (1) to (10). (1) Vinyl hydrocarbons Examples of vinyl hydrocarbons include (1-1) aliphatic vinyl hydrocarbons, (1-2) alicyclic vinyl hydrocarbons, and (1-3) aromatic vinyl hydrocarbons. (1-1) Aliphatic vinyl hydrocarbons Aliphatic vinyl hydrocarbons include, for example, alkenes and alkadienes. Examples of the alkenes include ethylene, propylene, and α-olefins. Examples of the alkadienes include butadiene, isoprene, 1,4-pentadiene, 1,6-hexadiene, and 1,7-octadiene. (1-2) Alicyclic vinyl hydrocarbons Alicyclic vinyl hydrocarbons include mono- or di-cycloalkenes and alkadienes, and specific examples include (di)cyclopentadiene, terpene, and the like. (1-3) Aromatic vinyl hydrocarbons Examples of aromatic vinyl hydrocarbons include styrene and its hydrocarbyl (alkyl, cycloalkyl, aralkyl and / or alkenyl) substituted derivatives, and specific examples thereof include α-methylstyrene, 2,4-dimethylstyrene and vinylnaphthalene.
[0040] (2) Carboxyl-containing vinyl monomers and their salts Examples of the carboxyl group-containing vinyl monomer and its salt include unsaturated monocarboxylic acids (salts) having 3 to 30 carbon atoms, unsaturated dicarboxylic acids (salts), and anhydrides (salts) thereof, and monoalkyl (carbon number 1 to 24) esters thereof or salts thereof. Specific examples thereof include carboxyl group-containing vinyl monomers such as (meth)acrylic acid, (anhydride) maleic acid, maleic acid monoalkyl esters, fumaric acid, fumaric acid monoalkyl esters, crotonic acid, itaconic acid, itaconic acid monoalkyl esters, itaconic acid glycol monoether, citraconic acid, citraconic acid monoalkyl esters, and cinnamic acid, and metal salts thereof.
[0041] In the present invention, "(salt)" means an acid or a salt thereof. For example, an unsaturated monocarboxylic acid (salt) having 3 to 30 carbon atoms means an unsaturated monocarboxylic acid or a salt thereof. In the present invention, "(meth)acrylic" means methacrylic acid or acrylic acid. In the present invention, "(meth)acryloyl" means methacryloyl or acryloyl. In the present invention, "(meth)acrylate" means methacrylate or acrylate.
[0042] (3) Sulfonic acid group-containing vinyl monomers, vinyl sulfate monoesters, and their salts Examples of the sulfonic acid group-containing vinyl monomer, vinyl sulfate monoester, and salts thereof include alkene sulfonic acids (salts) having 2 to 14 carbon atoms, alkyl sulfonic acids (salts) having 2 to 24 carbon atoms, sulfo(hydroxy)alkyl-(meth)acrylates (salts), (meth)acrylamides (salts), and alkylarylsulfosuccinic acids (salts). Specifically, an example of an alkene sulfonic acid having 2 to 14 carbon atoms is vinyl sulfonic acid (salt), an example of an alkyl sulfonic acid (salt) having 2 to 24 carbon atoms is α-methylstyrene sulfonic acid (salt), and an example of a sulfo(hydroxy)alkyl-(meth)acrylate (salt) or (meth)acrylamide (salt) is sulfopropyl(meth)acrylate (salt), sulfuric acid ester (salt), or a sulfonic acid group-containing vinyl monomer (salt).
[0043] (4) Phosphate-containing vinyl monomers and their salts Examples of the phosphoric acid group-containing vinyl monomer and its salt include (meth)acryloyloxyalkyl (carbon number 1 to 24) phosphoric acid monoester (salt), (meth)acryloyloxyalkyl (carbon number 1 to 24) phosphonic acid (salt), and the like. Specific examples of the (meth)acryloyloxyalkyl (carbon number 1 to 24) phosphate monoester (salt) include 2-hydroxyethyl (meth)acryloyl phosphate (salt), phenyl-2-acryloyloxyethyl phosphate (salt), and the like. Specific examples of the (meth)acryloyloxyalkyl (carbon number: 1 to 24)phosphonic acid (salt) include 2-acryloyloxyethylphosphonic acid (salt).
[0044] Examples of the salts of (2) to (4) above include alkali metal salts (sodium salts, potassium salts, etc.), alkaline earth metal salts (calcium salts, magnesium salts, etc.), ammonium salts, amine salts, and quaternary ammonium salts.
[0045] (5) Hydroxyl-containing vinyl monomers Examples of the hydroxyl group-containing vinyl monomer include hydroxystyrene, N-methylol (meth)acrylamide, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, (meth)allyl alcohol, crotyl alcohol, isocrotyl alcohol, 1-buten-3-ol, 2-buten-1-ol, 2-butene-1,4-diol, propargyl alcohol, 2-hydroxyethyl propenyl ether, and sucrose allyl ether.
[0046] (6) Nitrogen-containing vinyl monomers Examples of the nitrogen-containing vinyl monomer include (6-1) amino group-containing vinyl monomers, (6-2) amide group-containing vinyl monomers, (6-3) nitrile group-containing vinyl monomers, (6-4) quaternary ammonium cation group-containing vinyl monomers, and (6-5) nitro group-containing vinyl monomers. (6-1) Examples of amino group-containing vinyl monomers include aminoethyl (meth)acrylate. (6-2) Examples of amide group-containing vinyl monomers include (meth)acrylamide and N-methyl(meth)acrylamide. (6-3) Examples of nitrile group-containing vinyl monomers include (meth)acrylonitrile, cyanostyrene, and cyanoacrylate. (6-4) Examples of the vinyl monomer containing a quaternary ammonium cation group include quaternized products of tertiary amine group-containing vinyl monomers such as dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylamide, diethylaminoethyl (meth)acrylamide, and diallylamine (which are quaternized with a quaternizing agent such as methyl chloride, dimethyl sulfate, benzyl chloride, or dimethyl carbonate). (6-5) Examples of nitro group-containing vinyl monomers include nitrostyrene.
[0047] (7) Epoxy group-containing vinyl monomer Examples of the epoxy group-containing vinyl monomer include glycidyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, and p-vinylphenyl phenyl oxide.
[0048] (8) Halogen-containing vinyl monomers Examples of the halogen-containing vinyl monomer include vinyl chloride, vinyl bromide, vinylidene chloride, allyl chloride, chlorostyrene, bromostyrene, dichlorostyrene, chloromethylstyrene, tetrafluorostyrene, and chloroprene.
[0049] (9) Vinyl esters, vinyl (thio)ethers, vinyl ketones Examples of vinyl esters include vinyl acetate, vinyl butyrate, vinyl propionate, vinyl butyrate, diallyl phthalate, diallyl adipate, isopropenyl acetate, vinyl methacrylate, methyl 4-vinyl benzoate, cyclohexyl methacrylate, benzyl methacrylate, phenyl (meth)acrylate, vinyl methoxyacetate, vinyl benzoate, ethyl α-ethoxyacrylate, alkyl (meth)acrylates having an alkyl group having 1 to 50 carbon atoms [methyl (meth)acrylate], ) acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, dodecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, eicosyl (meth)acrylate, behenyl (meth)acrylate, etc.)], dialkyl fumarate (wherein the two alkyl groups are linear, branched or alicyclic groups having 2 to 8 carbon atoms), dialkyl Examples of the poly(meth)allyloxyalkane include maleates (the two alkyl groups are straight-chain, branched-chain or alicyclic groups having 2 to 8 carbon atoms), poly(meth)allyloxyalkanes (diallyloxyethane, triallyloxyethane, tetraallyloxyethane, tetraallyloxypropane, tetraallyloxybutane, tetramethallyloxyethane, etc.), vinyl monomers having polyalkylene glycol chains (polyethylene glycol (molecular weight 300) mono(meth)acrylate, polypropylene glycol (molecular weight 500) monoacrylate, methyl alcohol ethylene oxide 10 mol adduct (meth)acrylate, lauryl alcohol ethylene oxide 30 mol adduct (meth)acrylate, etc.), poly(meth)acrylates (poly(meth)acrylates of polyhydric alcohols: ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, polyethylene glycol di(meth)acrylate, etc.). An example of the vinyl (thio)ether is vinyl methyl ether. An example of the vinyl ketone is vinyl methyl ketone.
[0050] (10) Other vinyl monomers Examples of other vinyl monomers include tetrafluoroethylene, fluoroacrylate, isocyanatoethyl (meth)acrylate, and m-isopropenyl-α,α-dimethylbenzyl isocyanate.
[0051] In the synthesis of the resin (b1), the vinyl monomers (1) to (10) may be used alone or in combination of two or more. As the resin (b1), from the viewpoint of low-temperature fixability, a styrene-(meth)acrylic acid ester copolymer and a (meth)acrylic acid ester copolymer are preferred, and a styrene-(meth)acrylic acid ester copolymer is more preferred. When the resin (b1) has a carboxylic acid, an acid value is imparted to the resin, and the resin fine particles (B) are easily attached to the surface of the toner particles to form the toner particles.
[0052] The vinyl monomer used in the resin (b2) may be the same as that used in the resin (b1). In synthesizing the resin (b2), the vinyl monomers (1) to (10) listed in the above resin (b1) may be used alone or in combination of two or more. As the resin (b2), from the viewpoint of low-temperature fixability, a styrene-(meth)acrylic acid ester copolymer and a (meth)acrylic acid ester copolymer are preferred, and a styrene-(meth)acrylic acid ester copolymer is more preferred.
[0053] In particular, it is preferable that the shell and core contain a styrene-acrylic resin. In this case, both heat-resistant storage stability and fixability can be achieved. As for the content of the resin in the shell and the content of the resin in the shell, it is preferable that the shell and core each contain 50% by mass or more of styrene-acrylic resin.
[0054] The loss modulus G" of the viscoelastic properties of the resin (b1) at 100° C. and a frequency of 1 Hz is preferably 1.5 MPa to 100 MPa, more preferably 1.7 MPa to 30 MPa, and even more preferably 2.0 MPa to 10 MPa. The loss modulus G" of the viscoelastic properties of the resin (b2) at 100° C. and a frequency of 1 Hz is preferably 0.01 MPa to 1.0 MPa, more preferably 0.02 MPa to 0.5 MPa, and even more preferably 0.05 MPa to 0.3 MPa. When the loss modulus G″ of the viscoelastic properties is within this range, it is easy to form toner particles in which the resin fine particles (B) containing the resin (b1) and the resin (b2) as constituent components in the same particle are adhered to the surface of the toner particle.
[0055] The loss modulus G″ of the viscoelastic properties of resins (b1) and (b2) at a frequency of 1 Hz and 100°C can be adjusted by changing the types and composition ratio of the constituent monomers or by adjusting the polymerization conditions (types and amounts of initiator and chain transfer agent, reaction temperature, etc.). Specifically, for example, by using the following composition, it is possible to adjust each G'' to be within the above-mentioned range.
[0056] (1) Regarding the glass transition temperature (Tg1) calculated from the constituent monomers of resin (b1) and the glass transition temperature (Tg2) calculated from the constituent monomers of resin (b2), Tg1 is preferably 0° C. to 150° C., more preferably 50° C. to 100° C., and Tg2 is preferably −30° C. to 100° C., more preferably 0° C. to 80° C., and most preferably 30° C. to 60° C. Tg1 corresponds to the above TgA, and Tg2 corresponds to the above TgB.
[0057] The glass transition temperature (Tg) calculated from the constituent monomers is a value that can be calculated by the Fox method. Here, the Fox method [TGFox, Phys. Rev., 86, 652 (1952)] is a method for estimating the Tg of a copolymer from the Tg of each homopolymer represented by the following formula. 1 / Tg=W1 / Tg1+W2 / Tg2++Wn / Tgn [In the formula, Tg is the glass transition temperature (expressed in absolute temperature) of the copolymer, Tg1, Tg2...Tgn are the glass transition temperatures (expressed in absolute temperature) of the homopolymers of each monomer component, and W1, W2...Wn are the weight fractions of each monomer component.]
[0058] (2) Regarding the calculated acid value (AV1) of the resin (b1) and the calculated acid value (AV2) of the resin (b2), (AV1) is preferably 75 mgKOH / g to 400 mgKOH / g, more preferably 150 mgKOH / g to 300 mgKOH / g, and (AV2) is 0 mgKOH / g to 50 mgKOH / g, more preferably 0 mgKOH / g to 20 mgKOH / g, and most preferably 0 mgKOH / g. The calculated acid value is a theoretical acid value calculated from the molar amount of acidic groups contained in the constituent monomers and the total weight of the constituent monomers.
[0059] As for the resin (b1), an example of a constituent monomer satisfying the conditions (1) and (2) is a resin that contains, as a constituent monomer, preferably 10% by mass to 80% by mass, and more preferably 30% by mass to 60% by mass of styrene, and preferably 10% by mass to 60% by mass in total, and more preferably 30% by mass to 50% by mass of methacrylic acid and / or acrylic acid, based on the total mass of the resin (b1).
[0060] Moreover, examples of the resin (b2) include a resin that contains, as a constituent monomer, preferably 10% by mass to 100% by mass, and more preferably 30% by mass to 90% by mass of styrene, based on the total mass of the resin (b2), and that contains a total of preferably 0% by mass to 7.5% by mass, and more preferably 0% by mass to 2.5% by mass of methacrylic acid and / or acrylic acid, based on the total mass of the resin (b2).
[0061] (3) Polymerization conditions (type and amount of initiator and chain transfer agent, reaction temperature, etc.) are adjusted. Specifically, regarding the number average molecular weights (Mn1) and (Mn2) of the resins (b1) and (b2), (Mn1) is preferably 2,000 to 2,000,000, and more preferably 20,000 to 200,000. (Mn2) is preferably 1,000 to 1,000,000, and more preferably 10,000 to 100,000.
[0062] The loss modulus G″ of the viscoelastic properties in the present invention is measured, for example, using the following viscoelasticity measuring device. Equipment: ARES-24A (Rheometrics) Fixture: 25mm parallel plate Frequency: 1Hz Distortion rate: 10% Heating rate: 5℃ / min
[0063] The acid value (AVb1) of the resin (b1) is preferably from 75 mgKOH / g to 400 mgKOH / g, and more preferably from 150 mgKOH / g to 300 mgKOH / g. When the acid value is within the above range, the resin fine particles (B) containing vinyl units in which the resin (b1) and the resin (b2) are contained as constituents in the same particle are easily formed into particles adhered to the surface of the toner. Resin (b1) having an acid value within the above range is a resin that contains methacrylic acid and / or acrylic acid in a total amount of preferably 10% by mass to 60% by mass, and more preferably 30% by mass to 50% by mass, based on the total mass of resin (b1).
[0064] From the viewpoint of low-temperature fixability, the acid value (AVb2) of the resin (b2) is preferably from 0 mgKOH / g to 50 mgKOH / g, more preferably from 0 mgKOH / g to 20 mgKOH / g, and even more preferably 0 mgKOH / g. Resin (b2) having an acid value within this range is a resin that contains methacrylic acid and / or acrylic acid in a total amount of preferably 0% to 7.5% by mass, and more preferably 0% to 2.5% by mass, based on the total mass of resin (b2). The acid value can be measured, for example, by the method of JIS K0070:1992.
[0065] In the present invention, the glass transition temperature TgA of the shell portion (resin b1) is higher than the glass temperature TgB of the core portion (resin b2). By having the glass transition temperature TgA of the shell portion higher than the glass temperature TgB of the core portion, high heat-resistant storage stability can be ensured.
[0066] In order to make the glass transition temperature TgA of the shell portion of the resin microparticles higher than the glass transition temperature TgB of the core portion, for example, a method of adjusting the type and ratio of monomers used in synthesizing the shell can be mentioned.
[0067] The glass transition temperature TgA of the shell portion of the resin fine particles and the glass transition temperature TgB of the core portion preferably satisfy TgA-TgB≧10[° C.], and more preferably satisfy TgA-TgB≧20[° C.]. By making the difference between TgA and TgB 10° C. or more, the ease of forming toner particles in which the resin fine particles (B) are adhered to the toner surface and the low-temperature fixability of the toner particles of the present invention are excellent in balance.
[0068] In order to set the difference in glass transition temperature within the above range, for example, a method of adjusting the type and ratio of monomers used when synthesizing the shell portion and the core portion can be mentioned.
[0069] In the present invention, Tg is measured by the method (DSC) specified in ASTM D3418-82 using "DSC60-A" [manufactured by Shimadzu Corporation]. The method for measuring the glass transition temperature TgA of the shell portion and the glass transition temperature TgB of the core portion of the resin fine particles from the toner is as follows. For example, the shell is removed by using an organic solvent or by heating to separate only the core, which is then measured by the method (DSC) specified in the above-mentioned ASTM D3418-82.
[0070] The glass transition temperature TgA of the resin (b1) is preferably 0° C. to 150° C., and more preferably 50° C. to 100° C. When the glass transition temperature TgA is 0° C. or higher, the heat-resistant storage stability can be improved, and when it is 150° C. or lower, the inhibition of low-temperature fixability can be reduced.
[0071] The glass transition temperature TgB of the resin (b2) is preferably −30° C. to 100° C., more preferably 0° C. to 80° C., and even more preferably 30° C. to 60° C. If the glass transition temperature is −30° C. or higher, the heat-resistant storage stability can be improved, and if it is 100° C. or lower, the inhibition of low-temperature fixability can be reduced.
[0072] The glass transition temperature Tg of the resin particles is preferably 40° C. or more and 70° C. or less. In this case, high heat-resistant storage stability can be ensured without inhibiting fixation. In order to set the glass transition temperature Tg of the resin particles in the above range, for example, a method of appropriately adjusting the glass transition temperatures of the shell portion and the core portion can be mentioned.
[0073] The glass transition temperature Tg of the resin particles from the toner is measured as follows: The resin particles on the toner surface are physically peeled off, or separated using an organic solvent and the solvent is removed, and then the glass transition temperature Tg is calculated by the above-mentioned measurement method.
[0074] From the viewpoint of ease of forming toner particles, the solubility parameter (hereinafter sometimes abbreviated as SP value) of the resin (b1) is set to 9 (cal / cm 3 ) 1 / 2 ~13(cal / cm 3 ) 1 / 2 is preferable, and 9.5 (cal / cm 3)1 / 2 ~12.5(cal / cm 3 ) 1 / 2 More preferably, 10.5 (cal / cm 3 ) 1 / 2 ~11.5(cal / cm 3 ) 1 / 2 is more preferred.
[0075] The SP value of the resin (b1) can be adjusted by changing the types and composition ratio of the constituent monomers. From the viewpoint of ease of forming toner particles, the SP value of the resin (b2) is set to 8.5 (cal / cm 3 ) 1 / 2 ~12.5(cal / cm 3 ) 1 / 2 is preferable, and 9 (cal / cm 3 ) 1 / 2 ~12(cal / cm 3 ) 1 / 2 More preferably, 10 (cal / cm 3 ) 1 / 2 ~11(cal / cm 3 ) 1 / 2 is more preferred. The SP value of the resin (b2) can be adjusted by changing the types and composition ratio of the constituent monomers.
[0076] The SP value in the present invention is calculated by the method by Fedors [Polym. Eng. Sci. 14(2)152, (1974)].
[0077] From the viewpoint of TgA of resin (b1) and copolymerizability with other monomers, resin (b1) preferably contains 10% by mass to 80% by mass, and more preferably 30% by mass to 60% by mass of styrene as a constituent monomer, based on the total mass of resin (b1). From the viewpoint of TgB of resin (b2) and copolymerizability with other vinyl monomers, resin (b2) preferably contains 10% by mass to 100% by mass, and more preferably 30% by mass to 90% by mass of styrene as a constituent monomer, based on the total mass of resin (b2).
[0078] The number average molecular weight (Mn) of the resin (b1) is preferably 2,000 to 2,000,000, and more preferably 20,000 to 200,000. When the number average molecular weight is 2,000 or more, the heat-resistant storage stability is improved, and when it is 2,000,000 or less, the low-temperature fixability of the toner is less hindered.
[0079] The weight average molecular weight (Mw) of the resin (b1) is preferably larger than that of the resin (b2), more preferably 1.5 times or more larger than that of the resin (b2), and even more preferably 2.0 times or more larger than that of the resin (b2). Within this range, the balance between the ease of forming toner particles and low-temperature fixability is excellent.
[0080] The weight average molecular weight (Mw) of the resin (b1) is preferably 20,000 to 20,000,000, and more preferably 200,000 to 2,000,000. When the weight average molecular weight is 20,000 or more, the heat resistant storage stability is improved, and when it is 20,000,000 or less, the low temperature fixability is less hindered.
[0081] The number average molecular weight (Mn) of the resin (b2) is preferably 1,000 to 1,000,000, and more preferably 10,000 to 100,000. When Mn is 1,000 or more, the heat-resistant storage stability of the toner is improved, and when it is 1,000,000 or less, the low-temperature fixability of the toner is less hindered.
[0082] The weight average molecular weight (Mw) of the resin (b2) is preferably 10,000 to 10,000,000, and more preferably 100,000 to 1,000,000. When Mw is 10,000 or more, the heat-resistant storage stability of the toner is improved, and when it is 10,000,000 or less, the low-temperature fixability of the toner is less hindered.
[0083] Among these, it is preferred that the Mw of resin (b1) is 200,000 to 2,000,000, the Mw of resin (b2) is 100,000 to 500,000, and the "Mw of (b1)" is greater than the "Mw of (b2)".
[0084] In the present invention, Mn and Mw can be measured by gel permeation chromatography (GPC) under the following conditions. Equipment (example): "HLC-8120" [manufactured by Tosoh Corporation] Column (example): "TSK GEL GMH6" [Tosoh Corporation] x 2 ·Measurement temperature: 40℃ Sample solution: 0.25% by weight tetrahydrofuran solution (undissolved matter was removed by filtration using a glass filter) ·Solution injection volume: 100μl Detector: Refractive index detector Reference material: 12 standard polystyrenes (TSKstandard POLYSTYRENE) (molecular weight: 500, 1,050, 2,800, 5,970, 9,100, 18,100, 37,900, 96,400, 190,000, 355,000, 1,090,000, 2,890,000) [manufactured by Tosoh Corporation]
[0085] The mass ratio of resin (b1) to resin (b2) in the resin fine particles (B) is preferably 5 / 95 to 95 / 5, more preferably 25 / 75 to 75 / 25, and even more preferably 40 / 60 to 60 / 40. When the mass ratio of resin (b1) to resin (b2) is 5 / 95 or more, the toner has excellent heat-resistant storage stability, and when the mass ratio of resin (b1) to resin (b2) is 95 / 5 or less, toner particles in which resin fine particles (B) adhere to the surfaces of the toner particles are easily formed.
[0086] Methods for producing the resin fine particles (B) include known production methods, such as the following production methods (I) to (V). (I) A method of seed polymerization of constituent monomers of resin (b2) using fine particles of resin (b1) in an aqueous dispersion as seeds. (II) A method of carrying out seed polymerization of constituent monomers of resin (b1) using fine particles of resin (b2) in an aqueous dispersion as seeds. (III) A method in which a mixture of resin (b1) and resin (b2) is emulsified in an aqueous medium to obtain an aqueous dispersion of resin fine particles. (IV) A method in which a mixture of resin (b1) and constituent monomers of resin (b2) is emulsified in an aqueous medium, and then the constituent monomers of resin (b2) are polymerized to obtain an aqueous dispersion of resin fine particles. (V) A method in which a mixture of resin (b2) and constituent monomers of resin (b1) is emulsified in an aqueous medium, and then the constituent monomers of resin (b1) are polymerized to obtain an aqueous dispersion of resin fine particles.
[0087] The fact that the resin microparticles (B) contain the shell resin (b1) and the core resin (b2) as constituent components within the same particle can be confirmed by observing an element mapping image of a cut surface of the resin microparticles (B) using a known surface elemental analysis device (TOF-SIMSEDX-SEM, etc.), and by observing an electron microscope image of a cut surface of the resin microparticles (B) stained with a stain corresponding to the functional groups contained in the resins (b1) and (b2).
[0088] Furthermore, the resin microparticles obtained by this method may be obtained as a mixture containing resin microparticles whose only constituent resin component is resin (b1) and resin microparticles whose only constituent resin component is resin (b2), in addition to resin microparticles (B) containing resin (b1) and resin (b2) as constituent components within the same particle. In the composite process described below, the mixture may be used as is, or only the resin microparticles (B) may be isolated and used.
[0089] Specific examples of (I) include a method in which the constituent monomers of (b1) are polymerized by dropwise polymerization to produce an aqueous dispersion of resin microparticles containing (b1), and then the constituent monomers of (b2) are polymerized using this as a seed; and a method in which (b1) produced in advance by solution polymerization or the like is emulsified and dispersed in water, and then the constituent monomers of (b2) are polymerized using this as a seed.
[0090] Specific examples of (II) include a method in which the constituent monomer of (b2) is polymerized by dropwise polymerization to produce an aqueous dispersion of resin microparticles containing (b2), and then the constituent monomer of (b1) is polymerized using this as a seed; and a method in which (b2) produced in advance by solution polymerization or the like is emulsified and dispersed in water, and then the constituent monomer of (b1) is polymerized using this as a seed.
[0091] A specific example of (III) is a method in which solutions or melts of (b1) and (b2) previously prepared by solution polymerization or the like are mixed together, and the mixture is then emulsified and dispersed in an aqueous medium.
[0092] Specific examples of (IV) include a method in which (b1), which has been produced in advance by solution polymerization or the like, is mixed with constituent monomers of (b2), the mixture is emulsified and dispersed in an aqueous medium, and then the constituent monomers of (b2) are polymerized; and a method in which (b1) is produced in the constituent monomers of (b2), the mixture is emulsified and dispersed in an aqueous medium, and then the constituent monomers of (b2) are polymerized.
[0093] Specific examples of (V) include a method in which (b2), which has been produced in advance by solution polymerization or the like, is mixed with the constituent monomers of (b1), the mixture is emulsified and dispersed in an aqueous medium, and then the constituent monomers of (b1) are polymerized; and a method in which (a2) is produced in the constituent monomers of (b1), the mixture is emulsified and dispersed in an aqueous medium, and then the constituent monomers of (b1) are polymerized.
[0094] In the present invention, any of the above production methods (I) to (V) is suitable.
[0095] The resin fine particles (B) are preferably used in the form of an aqueous dispersion. The substance (aqueous medium) used in the aqueous dispersion is not particularly limited as long as it dissolves in water, and can be appropriately selected depending on the purpose, and examples thereof include a surfactant (D), a buffering agent, a protective colloid, etc. These may be used alone or in combination of two or more. The aqueous medium used in the aqueous dispersion is not particularly limited as long as it is a liquid essentially containing water, and examples thereof include an aqueous solution containing water.
[0096] Examples of the surfactant (D) include nonionic surfactants (D1), anionic surfactants (D2), cationic surfactants (D3), amphoteric surfactants (D4), and other emulsifying dispersants (D5).
[0097] Examples of the nonionic surfactant (D1) include AO (alkylene oxide) addition type nonionic surfactants and polyhydric alcohol type nonionic surfactants. Examples of the AO-addition type nonionic surfactant include EO adducts of aliphatic alcohols having 10 to 20 carbon atoms, EO adducts of phenols, EO (ethylene oxide) adducts of nonylphenols, EO adducts of alkylamines having 8 to 22 carbon atoms, and EO adducts of poly(oxypropylene) glycols. Examples of the polyhydric alcohol type nonionic surfactant include fatty acid (having 8 to 24 carbon atoms) esters of polyhydric (tri- to octahydric or higher) alcohols (having 2 to 30 carbon atoms) (e.g., glycerin monostearate, glycerin monooleate, sorbitan monolaurate, sorbitan monooleate, etc.), alkyl (having 4 to 24 carbon atoms) poly(degree of polymerization 1 to 10) glycosides, and the like.
[0098] Examples of the anionic surfactant (D2) include ether carboxylic acids or salts thereof having a hydrocarbon group having 8 to 24 carbon atoms, sulfate esters or ether sulfate esters and salts thereof having a hydrocarbon group having 8 to 24 carbon atoms, sulfonates having a hydrocarbon group having 8 to 24 carbon atoms, sulfosuccinates having one or two hydrocarbon groups having 8 to 24 carbon atoms, phosphate esters or ether phosphate esters and salts thereof having a hydrocarbon group having 8 to 24 carbon atoms, fatty acid salts having a hydrocarbon group having 8 to 24 carbon atoms, and acylated amino acid salts having a hydrocarbon group having 8 to 24 carbon atoms.
[0099] Examples of ether carboxylic acids having a hydrocarbon group with 8 to 24 carbon atoms or salts thereof include sodium lauryl ether acetate, (poly)oxyethylene (number of moles added: 1 to 100) sodium lauryl ether acetate, and the like.
[0100] Examples of sulfates or ether sulfates having a hydrocarbon group having 8 to 24 carbon atoms and salts thereof include sodium lauryl sulfate, (poly)oxyethylene (number of moles added: 1 to 100) sodium lauryl sulfate, (poly)oxyethylene (number of moles added: 1 to 100) triethanolamine lauryl sulfate, (poly)oxyethylene (number of moles added: 1 to 100) sodium coconut oil fatty acid monoethanolamide sulfate, and the like.
[0101] An example of the sulfonate having a hydrocarbon group having 8 to 24 carbon atoms is sodium dodecylbenzenesulfonate.
[0102] Examples of the phosphate ester or ether phosphate ester having a hydrocarbon group having 8 to 24 carbon atoms and salts thereof include sodium lauryl phosphate and sodium (poly)oxyethylene (addition mole number 1 to 100) lauryl ether phosphate.
[0103] Examples of fatty acid salts having a hydrocarbon group having 8 to 24 carbon atoms include sodium laurate and triethanolamine laurate.
[0104] Examples of acylated amino acid salts having a hydrocarbon group having 8 to 24 carbon atoms include sodium methyl coconut taurate, sodium coconut sarcosine, triethanolamine coconut sarcosine, N-triethanolamine coconut acyl-L-glutamate, sodium N-sodium coconut acyl-L-glutamate, and sodium lauroylmethyl-β-alanine.
[0105] Examples of the cationic surfactant (D3) include quaternary ammonium salt types and amine salt types. Examples of the quaternary ammonium salt type include stearyl trimethyl ammonium chloride, behenyl trimethyl ammonium chloride, distearyl dimethyl ammonium chloride, lanolin fatty acid aminopropyl ethyl dimethyl ammonium ethyl sulfate, and the like. Examples of the amine salt type include stearic acid diethylaminoethylamide lactate, dilaurylamine hydrochloride, and oleylamine lactate.
[0106] Examples of the amphoteric surfactant (D4) include betaine-type amphoteric surfactants and amino acid-type amphoteric surfactants. Examples of the betaine type amphoteric surfactant include coconut oil fatty acid amidopropyl dimethylaminoacetic acid betaine, lauryl dimethylaminoacetic acid betaine, 2-alkyl-N-carboxymethyl-N-hydroxyethyl imidazolinium betaine, and lauryl hydroxysulfobetaine. An example of the amino acid type amphoteric surfactant is sodium β-laurylaminopropionate.
[0107] Other emulsifying dispersants (D5) include, for example, reactive activators. The reactive activator is not particularly limited as long as it has radical reactivity and can be appropriately selected depending on the purpose. Examples of the reactive activator include ADEKA REASOAP (registered trademark) SE-10N, SR-10, SR-20, SR-30, ER-20, and ER-30 (all manufactured by ADEKA CORPORATION), AQUALON (registered trademark), HS-10, KH-05, KH-10, and KH-1025 (all manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.), ELEMINOL (registered trademark) JS-20 (manufactured by SANYO CHEMICAL INDUSTRIES, LTD.), LATEMUL (registered trademark) D-104, PD-420, and PD-430 (all manufactured by ADEKA CORPORATION), and the like. Examples of suitable emulsifying and dispersing agents include, for example, polyvinyl alcohol, starch or a derivative thereof, cellulose derivatives such as carboxymethyl cellulose, methyl cellulose, and hydroxyethyl cellulose, carboxyl group-containing (co)polymers such as sodium polyacrylate, and emulsifying and dispersing agents having urethane groups or ester groups described in U.S. Pat. No. 5,906,704 (for example, a polycaprolactone polyol and a polyether diol linked with a polyisocyanate).
[0108] As the surfactant (D), from the viewpoint of stabilizing oil droplets during emulsification and dispersion, obtaining a desired shape, and sharpening the particle size distribution, (D1), (D2), (D5), and combinations of these are preferred, and a combination of (D1) and (D5), and a combination of (D2) and (D5) are more preferred.
[0109] Examples of the buffer include sodium acetate, sodium citrate, sodium bicarbonate, and the like. Examples of the protective colloid include water-soluble cellulose compounds and alkali metal salts of polymethacrylic acid.
[0110] The resin microparticles (B) may contain, in addition to the shell resin (b1) and the core resin (b2), other resin components, an initiator (and its residue), a chain transfer agent, an antioxidant, a plasticizer, a preservative, a reducing agent, an organic solvent, etc.
[0111] Examples of the other resin components include vinyl resins other than the resins used for the shell resin (b1) and the core resin (b2), polyurethane resins, epoxy resins, polyester resins, polyamide resins, polyimide resins, silicon resins, phenol resins, melamine resins, urea resins, aniline resins, ionomer resins, polycarbonate resins, and the like.
[0112] The initiator (and its residue) includes known radical polymerization initiators, and specific examples thereof include persulfate initiators such as potassium persulfate and ammonium persulfate; azo initiators such as azobisisobutyronitrile; organic peroxides such as benzoyl peroxide, cumene hydroperoxide, tertiary butyl hydroperoxide, tertiary butyl peroxyisopropyl monocarbonate, and tertiary butyl peroxybenzoate; and hydrogen peroxide.
[0113] Examples of the chain transfer agent include n-dodecyl mercaptan, tert-dodecyl mercaptan, n-butyl mercaptan, 2-ethylhexyl thioglycolate, 2-mercaptoethanol, β-mercaptopropionic acid, and α-methylstyrene dimer.
[0114] Examples of the antioxidant include phenol compounds, paraphenylenediamine, hydroquinone, organic sulfur compounds, and organic phosphorus compounds.
[0115] Examples of the phenol compound include 2,6-di-t-butyl-p-cresol, butylated hydroxyanisole, 2,6-di-t-butyl-4-ethylphenol, stearyl-β-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 2,2'-methylene-bis-(4-methyl-6-t-butylphenol), 2,2'-methylene-bis-(4-ethyl-6-t-butylphenol), 4,4'-thiobis-(3-methyl-6-t-butylphenol), 4,4'-butylidene ... t-butyl-6-t-butylphenol), 1,1,3-tris-(2-methyl-4-hydroxy-5-t-butylphenyl)butane, 1,3,5-trimethyl-2,4,6-tris(3,5-di-t-butyl-4-hydroxybenzyl)benzene, tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane, bis[3,3'-bis(4'-hydroxy-3'-t-butylphenyl)butyric acid]glycol ester, tocopherol, etc.
[0116] Examples of paraphenylenediamines include N-phenyl-N'-isopropyl-p-phenylenediamine, N,N'-di-sec-butyl-p-phenylenediamine, N-phenyl-N-sec-butyl-p-phenylenediamine, N,N'-di-isopropyl-p-phenylenediamine, and N,N'-dimethyl-N,N'-di-t-butyl-p-phenylenediamine.
[0117] Examples of hydroquinones include 2,5-di-t-octylhydroquinone, 2,6-didodecylhydroquinone, 2-dodecylhydroquinone, 2-dodecyl-5-chlorohydroquinone, 2-t-octyl-5-methylhydroquinone, and 2-(2-octadecenyl)-5-methylhydroquinone.
[0118] Examples of the organic sulfur compound include dilauryl-3,3'-thiodipropionate, distearyl-3,3'-thiodipropionate, and ditetradecyl-3,3'-thiodipropionate.
[0119] Examples of the organic phosphorus compound include triphenylphosphine, tri(nonylphenyl)phosphine, tri(dinonylphenyl)phosphine, tricresylphosphine, and tri(2,4-dibutylphenoxy)phosphine.
[0120] Examples of the plasticizer include phthalic acid esters, aliphatic dibasic acid esters, trimellitic acid esters, phosphate esters, and fatty acid esters. Examples of phthalate esters include dibutyl phthalate, dioctyl phthalate, butyl benzyl phthalate, and diisodecyl phthalate. Examples of the aliphatic dibasic acid ester include di-2-ethylhexyl adipate and 2-ethylhexyl sebacate. Examples of trimellitic acid esters include tri-2-ethylhexyl trimellitate and trioctyl trimellitate. Examples of the phosphate ester include triethyl phosphate, tri-2-ethylhexyl phosphate, and tricresyl phosphate. An example of the fatty acid ester is butyl oleate.
[0121] Examples of the preservatives include organic nitrogen sulfur compound preservatives and organic sulfur halide preservatives.
[0122] Examples of the reducing agent include reducing organic compounds such as ascorbic acid, tartaric acid, citric acid, glucose, and metal salts of formaldehyde sulfoxylate; and reducing inorganic compounds such as sodium thiosulfate, sodium sulfite, sodium bisulfite, and sodium metabisulfite.
[0123] Examples of organic solvents include ketone solvents such as acetone and methyl ethyl ketone (hereinafter abbreviated as MEK); ester solvents such as ethyl acetate and γ-butyrolactone; ether solvents such as THF (tetrahydrofuran); amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone and N-methylcaprolactam; alcohol solvents such as isopropyl alcohol; and aromatic hydrocarbon solvents such as toluene and xylene.
[0124] The content of the resin particles is preferably 0.2% by mass to 5% by mass relative to the toner. When the sum of the resins (b1) and (b2) is within the above range, the low-temperature fixability and heat-resistant storage stability are improved. When the content is 0.2% by mass or more relative to the toner, the problem of the heat-resistant storage stability being deteriorated can be prevented, and when the content is 5% by mass or less, the problem of the low-temperature fixability being reduced can be prevented.
[0125] <Toner base particles> The toner base particles (hereinafter, sometimes referred to as "toner base" or "base particles") contain a binder resin, a colorant, and a wax, and further contain other components as required.
[0126] <<Binding resin>> The binder resin is not particularly limited and can be appropriately selected according to the purpose. For example, polyester resin, styrene-acrylic resin, polyol resin, vinyl resin, polyurethane resin, epoxy resin, polyamide resin, polyimide resin, silicon resin, phenol resin, melamine resin, urea resin, aniline resin, ionomer resin, polycarbonate resin, etc. can be mentioned. These may be used alone or in combination of two or more. Among these, polyester resin is preferable because it can give flexibility to the toner.
[0127] <<<Polyester resin>>> The polyester resin is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include crystalline polyester resins, amorphous polyester resins, modified polyester resins, etc. These may be used alone or in combination of two or more.
[0128] -Amorphous polyester resin- The amorphous polyester resin (hereinafter, also referred to as "amorphous polyester", "amorphous polyester", "amorphous polyester resin", "unmodified polyester resin", or "polyester resin component A") is not particularly limited and can be appropriately selected depending on the purpose. For example, there is an amorphous polyester resin obtained by reacting a polyol with a polycarboxylic acid.
[0129] In the present invention, the amorphous polyester resin refers to a resin obtained by reacting a polyol with a polycarboxylic acid as described above. Modified polyester resins, such as prepolymers described below, and modified polyester resins obtained by subjecting the prepolymers to a crosslinking and / or elongation reaction, are not included in the amorphous polyester resins in the present invention, and are treated as modified polyester resins.
[0130] The amorphous polyester is a polyester resin component that is soluble in tetrahydrofuran (THF). The amorphous polyester (polyester resin component A) is preferably a linear polyester resin.
[0131] The polyol includes, for example, a diol. Examples of the diol include alkylene (carbon number 2-3) oxide (average number of added moles 1-10) adducts of bisphenol A such as polyoxypropylene(2.2)-2,2-bis(4-hydroxyphenyl)propane and polyoxyethylene(2.2)-2,2-bis(4-hydroxyphenyl)propane; ethylene glycol; propylene glycol; hydrogenated bisphenol A; and alkylene (carbon number 2-3) oxide (average number of added moles 1-10) adducts of hydrogenated bisphenol A. These may be used alone or in combination of two or more. Among these, the polyol preferably contains 40 mol % or more of alkylene glycol.
[0132] The polycarboxylic acid may, for example, be a dicarboxylic acid. Examples of the dicarboxylic acid include adipic acid, phthalic acid, isophthalic acid, terephthalic acid, fumaric acid, maleic acid, dodecenylsuccinic acid, octylsuccinic acid, and other alkyl groups having 1 to 20 carbon atoms; succinic acid substituted with an alkenyl group having 2 to 20 carbon atoms. These may be used alone or in combination of two or more. Among these, the polycarboxylic acid preferably contains 50 mol % or more of terephthalic acid.
[0133] The polyester resin component A may contain a trivalent or higher carboxylic acid and / or a trivalent or higher alcohol, a trivalent or higher epoxy compound, or the like at the end of the resin chain in order to adjust the acid value and hydroxyl value. Among these, it is preferable to contain a trihydric or higher aliphatic alcohol, from the viewpoint of preventing unevenness and obtaining sufficient gloss and image density. Examples of the trivalent or higher carboxylic acid include trimellitic acid, pyromellitic acid, and acid anhydrides thereof. Examples of the trihydric or higher alcohol include glycerin, pentaerythritol, and trimethylolpropane.
[0134] The molecular weight of the polyester resin component A is not particularly limited and can be appropriately selected depending on the purpose, but is preferably in the following range. The weight average molecular weight (Mw) of the polyester resin component A is preferably from 3,000 to 10,000, and more preferably from 4,000 to 7,000. The number average molecular weight (Mn) of the polyester resin component A is preferably from 1,000 to 4,000, and more preferably from 1,500 to 3,000. The molecular weight ratio (Mw / Mn) of the polyester resin component A is preferably from 1.0 to 4.0, and more preferably from 1.0 to 3.5.
[0135] The weight average molecular weight and number average molecular weight can be measured, for example, by GPC (gel permeation chromatography).
[0136] The reason why the weight average molecular weight and number average molecular weight are preferred within the above ranges is that if the weight average molecular weight and number average molecular weight are too low, the toner may be inferior in heat resistant storage stability and durability against stress such as stirring in a developing machine, while if the weight average molecular weight and number average molecular weight are too high, the viscoelasticity of the toner when melted may increase and low-temperature fixability may be poor. Also, if there is too much of the component having a molecular weight of 600 or less, the toner may be inferior in heat resistant storage stability and durability against stress such as stirring in a developing machine, while if there is too little of the component having a molecular weight of 600 or less, the low-temperature fixability may be poor.
[0137] The THF soluble component having a molecular weight of 600 or less is preferably 2% by mass to 10% by mass. As a method for adjusting the content of this component, there may be mentioned a method in which polyester resin component A is extracted with methanol, and components having a molecular weight of 600 or less are removed, followed by purification.
[0138] The acid value of the polyester resin component A is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1 mgKOH / g to 50 mgKOH / g, and more preferably 5 mgKOH / g to 30 mgKOH / g. When the acid value is 1 mgKOH / g or more, the toner tends to be negatively charged, and furthermore, the affinity between the paper and the toner is improved when fixed to the paper, and low-temperature fixability can be improved. On the other hand, when the acid value is 50 mgKOH / g or less, the problem of a decrease in charging stability, particularly charging stability against environmental changes, can be prevented.
[0139] The hydroxyl value of the polyester resin component A is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 5 mgKOH / g or more.
[0140] The glass transition temperature (Tg) of the polyester resin component A is preferably 40° C. to 65° C., more preferably 45° C. to 65° C., and even more preferably 50° C. to 60° C. When the Tg is 40° C. or higher, the toner has improved heat-resistant storage stability and durability against stress such as stirring in a developing machine, and also has improved filming resistance. On the other hand, when the Tg is 65° C. or lower, the toner is less susceptible to deformation due to heat and pressure during fixing, and low-temperature fixing ability is improved.
[0141] The content of the polyester resin component A is preferably 80 parts by mass to 90 parts by mass with respect to 100 parts by mass of the toner.
[0142] -Modified polyester resin- The modified polyester resin (hereinafter sometimes referred to as "modified polyester" or "polyester resin component C") is not particularly limited and can be appropriately selected depending on the purpose. For example, a reaction product of an active hydrogen group-containing compound and a polyester resin (in this specification, sometimes referred to as a "prepolymer" or "polyester prepolymer") having a site capable of reacting with the active hydrogen group-containing compound can be mentioned.
[0143] The modified polyester is a polyester resin insoluble in tetrahydrofuran (THF). The polyester resin component insoluble in tetrahydrofuran (THF) lowers Tg and melt viscosity, and ensures low-temperature fixability, while having a branched structure in the molecular skeleton and a three-dimensional network structure in the molecular chain, and thus has rubber-like properties in that it deforms but does not flow at low temperatures.
[0144] Since the polyester resin component C has an active hydrogen group-containing compound and a site capable of reacting with the active hydrogen group-containing compound, these sites behave like pseudo-crosslinking points, and the rubber-like properties of the amorphous polyester resin A are enhanced, making it possible to produce a toner having excellent heat-resistant storage stability and high-temperature offset resistance.
[0145] --Compounds containing active hydrogen groups-- The active hydrogen group-containing compound is a compound that reacts with a polyester resin having a site capable of reacting with the active hydrogen group-containing compound.
[0146] The active hydrogen group is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include a hydroxyl group (alcoholic hydroxyl group and phenolic hydroxyl group), an amino group, a carboxyl group, a mercapto group, etc. These may be used alone or in combination of two or more kinds.
[0147] The active hydrogen group-containing compound is not particularly limited and can be appropriately selected according to the purpose. When the polyester resin having a site capable of reacting with the active hydrogen group-containing compound is a polyester resin containing an isocyanate group, amines are preferred because they can increase the molecular weight of the polyester resin by elongation reaction, crosslinking reaction, etc. with the polyester resin.
[0148] The amines are not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include diamines, trivalent or higher amines, amino alcohols, amino mercaptans, amino acids, blocked amino groups of these, etc. These may be used alone or in combination of two or more. Among these, diamines and mixtures of diamines with small amounts of trivalent or higher amines are preferred.
[0149] The diamine is not particularly limited and can be appropriately selected depending on the purpose. Examples of the diamine include aromatic diamines, alicyclic diamines, and aliphatic diamines. The aromatic diamine is not particularly limited and can be appropriately selected depending on the purpose. Examples of the aromatic diamine include phenylenediamine, diethyltoluenediamine, and 4,4'-diaminodiphenylmethane. The alicyclic diamine is not particularly limited and can be appropriately selected depending on the purpose. Examples of the alicyclic diamine include 4,4'-diamino-3,3'-dimethyldicyclohexylmethane, diaminocyclohexane, and isophoronediamine. The aliphatic diamine is not particularly limited and can be appropriately selected depending on the purpose. Examples of the aliphatic diamine include ethylenediamine, tetramethylenediamine, and hexamethylenediamine.
[0150] The trivalent or higher amine is not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include diethylenetriamine and triethylenetetramine.
[0151] The amino alcohol is not particularly limited and can be appropriately selected depending on the purpose. Examples of the amino alcohol include ethanolamine and hydroxyethylaniline.
[0152] The amino mercaptan is not particularly limited and can be appropriately selected depending on the purpose. Examples of the amino mercaptan include aminoethyl mercaptan and aminopropyl mercaptan.
[0153] The amino acid is not particularly limited and can be appropriately selected depending on the purpose. Examples of the amino acid include aminopropionic acid and aminocaproic acid.
[0154] The blocked amino group is not particularly limited and may be appropriately selected depending on the purpose. For example, ketimine compounds obtained by blocking the amino group with ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone, and oxazoline compounds may be mentioned.
[0155] --Polyester resin having a site capable of reacting with an active hydrogen group-containing compound-- The polyester resin having a site capable of reacting with the active hydrogen group-containing compound is not particularly limited and can be appropriately selected depending on the purpose. For example, a polyester resin containing an isocyanate group (hereinafter, sometimes referred to as a "polyester prepolymer having an isocyanate group") can be mentioned. The polyester resin containing an isocyanate group is not particularly limited and can be appropriately selected depending on the purpose. For example, a reaction product of a polyester resin having an active hydrogen group obtained by polycondensation of a polyol and a polycarboxylic acid and a polyisocyanate can be mentioned.
[0156] The polyol is not particularly limited and can be appropriately selected depending on the purpose. Examples of the polyol include diols, trihydric or higher alcohols, and mixtures of diols and trihydric or higher alcohols. These may be used alone or in combination of two or more. Among these, diols and mixtures of diols with a small amount of trihydric or higher alcohols are preferred.
[0157] The diol is not particularly limited and can be appropriately selected depending on the purpose. Examples of the diol include linear alkylene glycols, diols having an oxyalkylene group, alicyclic diols, bisphenols, alkylene oxide adducts of alicyclic diols, and alkylene oxide adducts of bisphenols. Examples of the chain alkylene glycol include ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, and 1,6-hexanediol. Examples of the diol having an oxyalkylene group include diethylene glycol, triethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, and polytetramethylene glycol. Examples of the alicyclic diol include 1,4-cyclohexanedimethanol and hydrogenated bisphenol A. Examples of the bisphenols include bisphenol A, bisphenol F, and bisphenol S. Examples of the alkylene oxide include ethylene oxide, propylene oxide, and butylene oxide. The number of carbon atoms of the chain alkylene glycol is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 2 to 12.
[0158] Among these, at least any one of a chain alkylene glycol having 2 to 12 carbon atoms and an alkylene oxide adduct of a bisphenol is preferred, and an alkylene oxide adduct of a bisphenol and a mixture of an alkylene oxide adduct of a bisphenol and a chain alkylene glycol having 2 to 12 carbon atoms are more preferred.
[0159] The trihydric or higher alcohol is not particularly limited and can be appropriately selected depending on the purpose. Examples of the trihydric or higher alcohol include aliphatic trihydric or higher alcohols, trihydric or higher polyphenols, and alkylene oxide adducts of trihydric or higher polyphenols.
[0160] The trihydric or higher aliphatic alcohol is not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, and sorbitol. The trivalent or higher polyphenols are not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include trisphenol PA, phenol novolac, and cresol novolac. Examples of the alkylene oxide adducts of trivalent or higher polyphenols include those obtained by adding alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide to trivalent or higher polyphenols.
[0161] When the diol and the trihydric or higher alcohol are used in combination, the mass ratio of the trihydric or higher alcohol to the diol (trihydric or higher alcohol / diol) is not particularly limited and can be appropriately selected depending on the purpose. For example, the mass ratio is preferably 0.01% by mass to 10% by mass, more preferably 0.01% by mass to 1% by mass.
[0162] The polycarboxylic acid is not particularly limited and can be appropriately selected according to the purpose. For example, dicarboxylic acid, trivalent or higher carboxylic acid, mixture of dicarboxylic acid and trivalent or higher carboxylic acid, etc. can be mentioned. These may be used alone or in combination of two or more. Among these, dicarboxylic acid, and mixture of dicarboxylic acid and a small amount of trivalent or higher polycarboxylic acid are preferred.
[0163] The dicarboxylic acid is not particularly limited and can be appropriately selected depending on the purpose. Examples of the dicarboxylic acid include divalent alkanoic acids, divalent alkenoic acids, and aromatic dicarboxylic acids. The divalent alkanoic acid is not particularly limited and can be appropriately selected depending on the purpose. Examples of the divalent alkanoic acid include succinic acid, adipic acid, and sebacic acid. The divalent alkenoic acid is not particularly limited and can be appropriately selected depending on the purpose, but is preferably a divalent alkenoic acid having 4 to 20 carbon atoms. The divalent alkenoic acid having 4 to 20 carbon atoms is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include maleic acid and fumaric acid. The aromatic dicarboxylic acid is not particularly limited and can be appropriately selected depending on the purpose, but is preferably an aromatic dicarboxylic acid having 8 to 20 carbon atoms. The aromatic dicarboxylic acid having 8 to 20 carbon atoms is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include phthalic acid, isophthalic acid, terephthalic acid, and naphthalenedicarboxylic acid.
[0164] The tri- or higher carboxylic acid is not particularly limited and can be appropriately selected depending on the purpose. Examples of the tri- or higher carboxylic acid include aromatic tri- or higher carboxylic acids. The trivalent or higher aromatic carboxylic acid is not particularly limited and can be appropriately selected depending on the purpose, but is preferably a trivalent or higher aromatic carboxylic acid having 9 to 20 carbon atoms. The trivalent or higher aromatic carboxylic acid having 9 to 20 carbon atoms is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include trimellitic acid and pyromellitic acid.
[0165] As the polycarboxylic acid, an acid anhydride or a lower alkyl ester of any of a dicarboxylic acid, a tri- or higher carboxylic acid, and a mixture of a dicarboxylic acid and a tri- or higher carboxylic acid can also be used. The lower alkyl ester is not particularly limited and can be appropriately selected depending on the purpose. Examples of the lower alkyl ester include methyl ester, ethyl ester, and isopropyl ester. When the dicarboxylic acid and the tri- or higher carboxylic acid are used in combination, the mass ratio of the tri- or higher carboxylic acid to the dicarboxylic acid (tri- or higher carboxylic acid / dicarboxylic acid) is not particularly limited and can be appropriately selected depending on the purpose. For example, the mass ratio is preferably 0.01% by mass to 10% by mass, more preferably 0.01% by mass to 1% by mass.
[0166] When the polyol and the polycarboxylic acid are polycondensed, the equivalent ratio of the hydroxyl group of the polyol to the carboxyl group of the polycarboxylic acid (hydroxyl group of the polyol / carboxyl group of the polycarboxylic acid) is not particularly limited and can be appropriately selected depending on the purpose. For example, it is preferably 1 to 2, more preferably 1 to 1.5, and particularly preferably 1.02 to 1.3.
[0167] The content of the polyol-derived structural unit in the polyester prepolymer having an isocyanate group is not particularly limited and can be appropriately selected depending on the purpose. For example, it is preferably 0.5% by mass to 40% by mass, more preferably 1% by mass to 30% by mass, and particularly preferably 2% by mass to 20% by mass. If the content is less than 0.5% by mass, the hot offset resistance decreases, and it may be difficult to achieve both the heat resistant storage stability and the low-temperature fixability of the toner. If the content exceeds 40% by mass, the low-temperature fixability may decrease.
[0168] The polyisocyanate is not particularly limited and may be appropriately selected depending on the purpose. Examples of the polyisocyanate include aliphatic diisocyanates, alicyclic diisocyanates, aromatic diisocyanates, araliphatic diisocyanates, isocyanurates, and those blocked with phenol derivatives, oximes, caprolactams, etc.
[0169] The aliphatic diisocyanate is not particularly limited and can be appropriately selected depending on the purpose. Examples of the aliphatic diisocyanate include tetramethylene diisocyanate, hexamethylene diisocyanate, methyl 2,6-diisocyanatocaproate, octamethylene diisocyanate, decamethylene diisocyanate, dodecamethylene diisocyanate, tetradecamethylene diisocyanate, trimethylhexane diisocyanate, and tetramethylhexane diisocyanate.
[0170] The alicyclic diisocyanate is not particularly limited and can be appropriately selected depending on the purpose. Examples of the alicyclic diisocyanate include isophorone diisocyanate and cyclohexylmethane diisocyanate.
[0171] The aromatic diisocyanate is not particularly limited and can be appropriately selected depending on the purpose. Examples of the aromatic diisocyanate include tolylene diisocyanate, diisocyanatodiphenylmethane, 1,5-naphthylene diisocyanate, 4,4'-diisocyanatodiphenyl, 4,4'-diisocyanato-3,3'-dimethyldiphenyl, 4,4'-diisocyanato-3-methyldiphenylmethane, and 4,4'-diisocyanato-diphenyl ether.
[0172] The aromatic aliphatic diisocyanate is not particularly limited and may be appropriately selected depending on the purpose. For example, α,α,α',α'-tetramethylxylylene diisocyanate is exemplified.
[0173] The isocyanurates are not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include tris(isocyanatoalkyl)isocyanurate, tris(isocyanatocycloalkyl)isocyanurate, and the like. These may be used alone or in combination of two or more.
[0174] When the polyisocyanate is reacted with a polyester resin having a hydroxyl group, the equivalent ratio (NCO / OH) of the isocyanate group of the polyisocyanate to the hydroxyl group of the polyester resin is not particularly limited and can be appropriately selected according to the purpose. For example, it is preferably 1 to 5, more preferably 1.2 to 4, and particularly preferably 1.5 to 2.5. If the equivalent ratio is less than 1, the hot offset resistance may decrease, and if it exceeds 5, the low temperature fixability may decrease.
[0175] The content of the polyisocyanate-derived structural unit in the polyester prepolymer having an isocyanate group is not particularly limited and can be appropriately selected according to the purpose. For example, it is preferably 0.5% by mass to 40% by mass, more preferably 1% by mass to 30% by mass, and particularly preferably 2% by mass to 20% by mass. If the content is less than 0.5% by mass, the hot offset resistance may decrease, and if it exceeds 40% by mass, the low-temperature fixability may decrease.
[0176] The average number of isocyanate groups in the polyester prepolymer having isocyanate groups per molecule is not particularly limited and can be appropriately selected depending on the purpose. For example, it is preferably 1 or more, more preferably 1.5 to 3, and particularly preferably 1.8 to 2.5. If the average number is less than 1, the molecular weight of the modified polyester resin may be low, and the hot offset resistance may be reduced.
[0177] The modified polyester resin can be produced by a one-shot method, etc. As an example, a method for producing a urea-modified polyester resin will be described. First, a polyol and a polycarboxylic acid are heated to 150°C to 280°C in the presence of a catalyst such as tetrabutoxy titanate or dibutyltin oxide, and the water generated is removed while reducing the pressure as necessary to obtain a polyester resin having hydroxyl groups. Next, the polyester resin having hydroxyl groups is reacted with a polyisocyanate at 40°C to 140°C to obtain a polyester prepolymer having an isocyanate group. Furthermore, the polyester prepolymer having an isocyanate group is reacted with amines at 0°C to 140°C to obtain a urea-modified polyester resin.
[0178] The number average molecular weight (Mn) of the modified polyester resin is not particularly limited and can be appropriately selected depending on the purpose. For example, it is preferably 1,000 to 10,000, more preferably 1,500 to 6,000, as measured by GPC (gel permeation chromatography).
[0179] The weight average molecular weight (Mw) of the modified polyester resin is not particularly limited and can be appropriately selected depending on the purpose. For example, it is preferably 20,000 or more and 1,000,000 or less as measured by GPC (gel permeation chromatography). If the weight average molecular weight is 20,000 or more, the toner becomes easily fluid at low temperatures, which can prevent problems such as poor heat-resistant storage stability and low viscosity when melted, which can prevent problems such as reduced high-temperature offset properties.
[0180] When a polyester resin having a hydroxyl group is reacted with a polyisocyanate, and when a polyester prepolymer having an isocyanate group is reacted with an amine, a solvent can be used as necessary. The solvent is not particularly limited and can be appropriately selected depending on the purpose. Examples of the solvent include aromatic solvents, ketones, esters, amides, ethers, and other solvents that are inactive to isocyanate groups. Examples of the aromatic solvent include toluene and xylene. Examples of the ketones include acetone, methyl ethyl ketone, and methyl isobutyl ketone. The esters include, for example, ethyl acetate. Examples of the amides include dimethylformamide and dimethylacetamide. The ethers include, for example, tetrahydrofuran.
[0181] The glass transition temperature of the modified polyester resin is preferably from -60°C to 0°C, and more preferably from -40°C to -20°C. If the glass transition temperature is -60°C or higher, the flow of the toner at low temperatures cannot be suppressed, and the problems of deterioration of heat-resistant storage stability and filming resistance can be prevented. If the glass transition temperature is 0°C or lower, the toner cannot be sufficiently deformed by heating and pressure during fixing, and the problems of insufficient low-temperature fixing properties can be prevented.
[0182] The content of the modified polyester is not particularly limited and can be appropriately selected depending on the purpose. For example, the content is preferably 1 part by mass to 15 parts by mass, more preferably 5 parts by mass to 10 parts by mass, in 100 parts by mass of the toner.
[0183] The molecular structures of the polyester resin components A and C can be confirmed by NMR measurement of a solution or solid, as well as X-ray diffraction, GC / MS, LC / MS, IR measurement, and the like. In the infrared absorption spectrum, the -1 and 990±10cm -1 One method is to detect amorphous polyester resins that do not have absorption due to olefin δCH (out-of-plane bending vibration).
[0184] -Crystalline polyester- The crystalline polyester resin (hereinafter also referred to as "crystalline polyester" or "polyester resin component D") is not particularly limited and can be appropriately selected depending on the purpose. For example, a crystalline polyester resin obtained by reacting a polyol with a polycarboxylic acid can be used.
[0185] The crystalline polyester resin has high crystallinity and therefore exhibits heat melting characteristics in which the viscosity drops sharply near the fixing start temperature. By using the crystalline polyester resin having such characteristics together with the amorphous polyester resin, the heat-resistant storage stability is good due to the crystallinity until just before the melting start temperature, and at the melting start temperature, the crystalline polyester resin melts and causes a sudden viscosity drop (sharp melt), which causes it to become compatible with the amorphous polyester resin, and both of them rapidly drop in viscosity to be fixed, resulting in a toner that has both good heat-resistant storage stability and low-temperature fixing ability. Also, good results are shown in terms of the release width (the difference between the minimum fixing temperature and the high-temperature offset-resistant temperature).
[0186] In the present invention, the crystalline polyester resin refers to a resin obtained by reacting a polyol with a polycarboxylic acid as described above, and modified polyester resins, such as the prepolymer and resins obtained by subjecting the prepolymer to a crosslinking and / or elongation reaction, do not belong to the crystalline polyester resin.
[0187] --Polyol-- The polyol is not particularly limited and can be appropriately selected depending on the purpose. Examples of the polyol include diols and trihydric or higher polyols.
[0188] The diol includes, for example, saturated aliphatic diols. The saturated aliphatic diol may be a linear saturated aliphatic diol or a branched saturated aliphatic diol. These may be used alone or in combination of two or more. Among these, linear saturated aliphatic diols are preferred, and linear saturated aliphatic diols having a carbon number of 2 to 12 are more preferred, because they can improve crystallinity and prevent a decrease in melting point.
[0189] Examples of the saturated aliphatic diol include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, and 1,14-eicosanediol. Among these, ethylene glycol, 1,4-butanediol, 1,6-hexanediol, 1,8-octanediol, 1,10-decanediol, and 1,12-dodecanediol are preferred because the crystalline polyester resin has high crystallinity and excellent sharp melting properties.
[0190] Examples of the trihydric or higher alcohol include glycerin, trimethylolethane, trimethylolpropane, and pentaerythritol.
[0191] --Polycarboxylic acids-- The polycarboxylic acid is not particularly limited and can be appropriately selected depending on the purpose. Examples of the polycarboxylic acid include divalent carboxylic acids and trivalent or higher carboxylic acids.
[0192] Examples of the divalent carboxylic acid include saturated aliphatic dicarboxylic acids such as oxalic acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, and 1,18-octadecanedicarboxylic acid; and aromatic dicarboxylic acids such as dibasic acids such as phthalic acid, isophthalic acid, terephthalic acid, naphthalene-2,6-dicarboxylic acid, malonic acid, and mesaconic acid; etc. Furthermore, anhydrides of these and lower (carbon number 1 to 3) alkyl esters of these can also be mentioned.
[0193] Examples of the trivalent or higher carboxylic acid include 1,2,4-benzenetricarboxylic acid, 1,2,5-benzenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, and anhydrides and lower (carbon number 1 to 3) alkyl esters of these.
[0194] The polycarboxylic acid may contain a dicarboxylic acid having a sulfonic acid group in addition to the saturated aliphatic dicarboxylic acid and aromatic dicarboxylic acid, and may further contain a dicarboxylic acid having a double bond in addition to the saturated aliphatic dicarboxylic acid and aromatic dicarboxylic acid. These may be used alone or in combination of two or more.
[0195] The crystalline polyester resin is preferably composed of a linear saturated aliphatic dicarboxylic acid having 4 to 12 carbon atoms and a linear saturated aliphatic diol having 2 to 12 carbon atoms. That is, the crystalline polyester resin preferably has a structural unit derived from a saturated aliphatic dicarboxylic acid having 4 to 12 carbon atoms and a structural unit derived from a saturated aliphatic diol having 2 to 12 carbon atoms. This is preferable in that the resin has high crystallinity and excellent sharp melting properties, and can therefore exhibit excellent low-temperature fixability.
[0196] The presence or absence of crystallinity of the crystalline polyester resin in the present invention can be confirmed by a crystal analysis X-ray diffraction device (for example, X'Pert Pro MRD, manufactured by Philips). The measurement method will be described below. First, the target sample is ground in a mortar to prepare a powdered sample, and the powdered sample is evenly applied to a sample holder.Then, the sample holder is set in the diffraction device, and measurements are performed to obtain a diffraction spectrum. When the half-width of the peak having the greatest intensity among the peaks obtained in the range of 20°<2θ<25° among the obtained diffraction peaks is 2.0 or less, it is judged to have crystallinity. In contrast to crystalline polyester resins, polyester resins that do not show the above-mentioned state are called amorphous polyester resins in the present invention.
[0197] The conditions for the X-ray diffraction measurements are described below. [Measurement conditions] Tension kV: 45kV Current: 40mA ·MPSS Upper Gonio Scan mode: continuous Starting angle: 3° End angle: 35° Angle Step: 0.02° Lucident beam optics ·Divergence slit: Div slit 1 / 2 Diffraction beam optics ·Anti scatter slit: As Fixed 1 / 2 ·Receiving slit: Prog rec slit
[0198] The melting point of the crystalline polyester resin is not particularly limited and may be appropriately selected depending on the purpose, but is preferably 60° C. or higher and 80° C. or lower. When the melting point is 60°C or higher, the crystalline polyester resin easily melts at low temperatures, preventing the problem of a decrease in the heat-resistant storage stability of the toner. When the melting point is 80°C or lower, the crystalline polyester resin does not melt sufficiently due to heating during fixing, preventing the problem of a decrease in low-temperature fixability.
[0199] The molecular weight of the crystalline polyester resin is not particularly limited and can be appropriately selected depending on the purpose. The orthodichlorobenzene soluble portion of the crystalline polyester resin preferably has a weight average molecular weight (Mw) of 3,000 to 30,000, more preferably 5,000 to 15,000, as measured by GPC. The orthodichlorobenzene soluble portion of the crystalline polyester resin preferably has a number average molecular weight (Mn) of 1,000 to 10,000, more preferably 2,000 to 10,000, as measured by GPC. The molecular weight ratio Mw / Mn of the crystalline polyester resin is preferably from 1.0 to 10, and more preferably from 1.0 to 5.0. This is because a toner having a sharp molecular weight distribution and a low molecular weight has excellent low-temperature fixability, and the high heat-resistant storage stability is reduced when there are a lot of low-molecular weight components.
[0200] The acid value of the crystalline polyester resin is not particularly limited and can be appropriately selected depending on the purpose, but from the viewpoint of affinity between paper and resin, in order to achieve the desired low-temperature fixability, it is preferably 5 mgKOH / g or more, more preferably 10 mgKOH / g or more, while in order to improve high-temperature offset resistance, it is preferably 45 mgKOH / g or less.
[0201] The hydroxyl value of the crystalline polyester resin is not particularly limited and can be appropriately selected depending on the purpose. For example, in order to achieve the desired low-temperature fixability and good charging characteristics, the hydroxyl value is preferably 0 mgKOH / g to 50 mgKOH / g, more preferably 5 mgKOH / g to 50 mgKOH / g.
[0202] The molecular structure of the crystalline polyester resin can be confirmed by NMR measurement of a solution or solid, as well as X-ray diffraction, GC / MS, LC / MS, IR measurement, etc. -1 Or 990±10cm -1 One method is to detect a crystalline polyester resin that has absorption based on the δCH (out-of-plane bending vibration) of olefin.
[0203] The content of the crystalline polyester resin is not particularly limited and can be appropriately selected according to the purpose. For example, it is preferably 3 parts by mass to 20 parts by mass, more preferably 5 parts by mass to 15 parts by mass, relative to 100 parts by mass of the toner. When the content is 3 parts by mass or more, the problem of poor low-temperature fixability due to insufficient sharp melting by the crystalline polyester resin can be prevented. In addition, when it is 20 parts by mass or less, the problem of reduced heat-resistant storage stability and image fogging can be prevented.
[0204] <<Coloring agent>> The colorant is not particularly limited and can be appropriately selected depending on the purpose. For example, carbon black, nigrosine dye, iron black, naphthol yellow S, Hansa yellow (10G, 5G, G), cadmium yellow, yellow iron oxide, yellow ochre, yellow lead, titanium yellow, polyazo yellow, oil yellow, Hansa yellow (GR, A, RN, R), pigment yellow L, benzidine yellow (G, GR), permanent yellow (NCG), Balkan fast yellow (5G, R), tartrazine lake, quinoline yellow lake, anthrazan yellow BGL, isoindolinone yellow, red iron oxide, red lead, vermilion, Domium Red, Cadmium Mercury Red, Antimony Vermilion, Permanent Red 4R, Para Red, Phaysee Red, Parachlor Orthonitroaniline Red, Lithol Fast Scarlet G, Brilliant Fast Scarlet, Brilliant Carmine BS, Permanent Red (F2R, F4R, FRL, FRLL, F4RH), Fast Scarlet VD, Belkan Fast Rubin B, Brilliant Scarlet G, Lithol Rubin GX, Permanent Red F5R, Brilliant Carmine 6B, Pigment Scarlet 3B, Bordeaux 5B, Toluidine Maroon, Permanent Bordeaux F2K, Helio Bordeaux BL, Bordeaux 10B, Bon Maroon Light, Bon Maroon Medium, Eosin Lake, Rhodamine Lake B, Rhodamine Lake Y, Alizarin Lake, Thioindigo Red B, Thioindigo Maroon, Oil Red, Quinacridone Red, Pyrazolone Red, Polyazo Red, Chrome Vermilion, Benzidine Orange, Perinone Orange, Oil Orange, Cobalt Blue, Cerulean Blue, Alkaline Blue Lake, Peacock Blue Lake, Victoria Blue Lake, Metal-free Phthalocyanine Blue, Phthalocyanine Blue, Fast Sky Blue, Indanthrene Blue (RS, BC), Indigo, Ultramarine Blue, Prussian Blue, Anthraquinone Blue, Fast Violet B, Methyl Violet Lake, Cobalt Purple, Manganese Purple, Dioxane Violet, Anthraquinone Violet, Chrome Green, Zinc Green, Chromium Oxide, Pyridian, Emerald Green, Pigment Green B, Naphthol Green B, Green Gold, Acid Green Lake,Examples include malachite green lake, phthalocyanine green, anthraquinone green, titanium oxide, zinc oxide, and lithopone.
[0205] The content of the colorant is not particularly limited and can be appropriately selected depending on the purpose. For example, the content is preferably 1 part by mass to 15 parts by mass, and more preferably 3 parts by mass to 10 parts by mass, relative to 100 parts by mass of the toner.
[0206] The colorant can also be used as a masterbatch composited with a resin. Examples of resins to be used in the preparation of the masterbatch or kneaded with the masterbatch include, in addition to the other polyester resins, styrene or its substituted polymers such as polystyrene, poly-p-chlorostyrene, and polyvinyltoluene; styrene-p-chlorostyrene copolymer, styrene-propylene copolymer, styrene-vinyltoluene copolymer, styrene-vinylnaphthalene copolymer, styrene-methyl acrylate copolymer, styrene-ethyl acrylate copolymer, styrene-butyl acrylate copolymer, styrene-octyl acrylate copolymer, styrene-methyl methacrylate copolymer, styrene-ethyl methacrylate copolymer, styrene-butyl methacrylate copolymer, and styrene-α-chloromethyl methacrylate copolymer. styrene-based copolymers such as styrene-acrylonitrile copolymers, styrene-vinyl methyl ketone copolymers, styrene-butadiene copolymers, styrene-isoprene copolymers, styrene-acrylonitrile-indene copolymers, styrene-maleic acid copolymers, and styrene-maleic acid ester copolymers; polymethyl methacrylate, polybutyl methacrylate, polyvinyl chloride, polyvinyl acetate, polyethylene, polypropylene, polyester, epoxy resins, epoxy polyol resins, polyurethanes, polyamides, polyvinyl butyral, polyacrylic acid resins, rosin, modified rosin, terpene resins, aliphatic or alicyclic hydrocarbon resins, aromatic petroleum resins, chlorinated paraffin, and paraffin wax. These may be used alone or in combination of two or more.
[0207] The master batch can be obtained by mixing and kneading the resin for the master batch and the colorant under high shear force. In this case, an organic solvent can be used to enhance the interaction between the colorant and the resin. In addition, a method called the flushing method, in which an aqueous paste containing water of the colorant is mixed and kneaded with the resin and the organic solvent, the colorant is transferred to the resin side, and the water and organic solvent components are removed, is also preferably used because the wet cake of the colorant can be used as it is and does not need to be dried. A high shear dispersion device such as a three-roll mill is preferably used for mixing and kneading.
[0208] <<Wax>> The wax (releasing agent) is not particularly limited and can be appropriately selected from known waxes, for example, natural waxes, synthetic waxes, etc. These may be used alone or in combination of two or more kinds.
[0209] Examples of the natural waxes include vegetable waxes such as carnauba wax, cotton wax, and wood wax; animal waxes such as beeswax and lanolin; mineral waxes such as ozokerite and cerusin; and petroleum waxes such as paraffin, microcrystalline, and petrolatum. Examples of the synthetic wax include synthetic hydrocarbon waxes such as Fischer-Tropsch wax, polyethylene, and polypropylene; fatty acid amide compounds such as esters, ketones, ethers, 12-hydroxystearic acid amide, stearic acid amide, phthalic anhydride imide, and chlorinated hydrocarbons; low molecular weight crystalline polymer resins, such as polyacrylate homopolymers and copolymers (e.g., n-stearyl acrylate-ethyl methacrylate copolymers); and crystalline polymers having long alkyl groups in their side chains. Among these, hydrocarbon waxes such as paraffin wax, microcrystalline wax, Fischer-Tropsch wax, polyethylene wax, and polypropylene wax are preferred.
[0210] The melting point of the release agent is not particularly limited and can be appropriately selected according to the purpose. For example, it is preferably 60°C or more and 80°C or less. When the melting point is 60°C or more, the release agent is easily melted at low temperatures, and the problem of poor heat resistance storage stability can be prevented. When the melting point is 80°C or less, even when the resin is melted and in the fixing temperature range, the release agent does not melt sufficiently, causing fixing offset and preventing defects in the image.
[0211] The content of the release agent is not particularly limited and can be appropriately selected according to the purpose. For example, it is preferably 2 to 10 parts by mass, more preferably 3 to 8 parts by mass, relative to 100 parts by mass of the toner. When the content is 2 parts by mass or more, the problems of poor high-temperature offset resistance and poor low-temperature fixability during fixing can be prevented, and when it is 10 parts by mass or less, the problems of poor heat-resistant storage stability and image fogging can be prevented.
[0212] <<Other ingredients>> The toner base particles are not particularly limited as long as they are used in ordinary toner base particles, and may contain other components appropriately selected depending on the purpose. The content of the other components is not particularly limited as long as it does not impair the properties of the toner, and can be appropriately selected depending on the purpose.
[0213] The other components are not particularly limited as long as they are used in ordinary toners and can be appropriately selected depending on the purpose. For example, a charge control agent, an external additive, a flowability improver, a cleaning property improver, a magnetic material, etc. can be mentioned.
[0214] -Charge control agent- The charge control agent is not particularly limited and can be appropriately selected according to the purpose. For example, Nigrosine dyes, triphenylmethane dyes, chromium-containing metal complex dyes, molybdic acid chelate pigments, rhodamine dyes, alkoxy amines, quaternary ammonium salts (including fluorine-modified quaternary ammonium salts), alkylamides, phosphorus simple substance or compounds, tungsten simple substance or compounds, fluorine-based activators, salicylic acid metal salts, salicylic acid derivative metal salts, etc. can be mentioned.
[0215] Examples of commercially available charge control agents include the nigrosine dye Bontron 03, the quaternary ammonium salt Bontron P-51, the metal-containing azo dye Bontron S-34, the oxynaphthoic acid metal complex E-82, the salicylic acid metal complex E-84, and the phenol condensate E-89 (all manufactured by Orient Chemical Industry Co., Ltd.), the quaternary ammonium salt molybdenum complexes TP-302 and TP-415 (all manufactured by Hodogaya Chemical Co., Ltd.), LRA-901, and the boron complex LR-147 (all manufactured by Nippon Carlit Co., Ltd.).
[0216] The content of the charge control agent is determined by the type of the binder resin, the presence or absence of additives used as necessary, and the toner manufacturing method including the dispersion method. Therefore, it is not uniquely limited, but for example, it is preferably 0.1 parts by mass to 10 parts by mass, more preferably 0.2 parts by mass to 5 parts by mass, relative to 100 parts by mass of the binder resin. If the content exceeds 10 parts by mass, the chargeability of the toner is too high, the effect of the main charge control agent is reduced, and the electrostatic attraction force with the developing roller increases, which may lead to a decrease in the fluidity of the developer and a decrease in image density.
[0217] These charge control agents can be melt-kneaded together with the master batch and the resin and then dissolved and dispersed. Of course, they may be added when directly dissolving or dispersing in an organic solvent, or they may be fixed on the toner surface after the toner particles are produced.
[0218] -External additives- Examples of the external additive include silica fine particles, hydrophobic silica, fatty acid metal salts (e.g., zinc stearate, aluminum stearate, etc.), metal oxides (e.g., titania, alumina, tin oxide, antimony oxide, etc.), and fluoropolymers. These may be used alone or in combination of two or more. Among these, hydrophobized inorganic fine particles are preferred.
[0219] Examples of silica fine particles include R972, R974, RX200, RY200, R202, R805, and R812 (all manufactured by Nippon Aerosil Co., Ltd.). Examples of titania microparticles include P-25 (manufactured by Nippon Aerosil Co., Ltd.), STT-30, STT-65C-S (all manufactured by Titanium Kogyo Co., Ltd.), TAF-140 (manufactured by Fuji Titanium Kogyo Co., Ltd.), MT-150W, MT-500B, MT-600B, MT-150A (all manufactured by Teika Corporation).
[0220] Examples of hydrophobically treated titanium oxide particles include T-805 (manufactured by Nippon Aerosil Co., Ltd.), STT-30A, STT-65S-S (all manufactured by Titanium Kogyo Co., Ltd.), TAF-500T, TAF-1500T (all manufactured by Fuji Titanium Kogyo Co., Ltd.), MT-100S, MT-100T (all manufactured by Teika Corporation), and IT-S (manufactured by Ishihara Sangyo Co., Ltd.).
[0221] Hydrophobized oxide particles, hydrophobized silica particles, hydrophobized titania particles, and hydrophobized alumina particles can be obtained by treating hydrophilic particles with a silane coupling agent such as methyltrimethoxysilane, methyltriethoxysilane, octyltrimethoxysilane, etc. Silicone oil-treated oxide particles and inorganic particles, which are treated with silicone oil by heating if necessary, are also suitable.
[0222] Examples of the silicone oil include dimethyl silicone oil, methylphenyl silicone oil, chlorophenyl silicone oil, methylhydrogen silicone oil, alkyl-modified silicone oil, fluorine-modified silicone oil, polyether-modified silicone oil, alcohol-modified silicone oil, amino-modified silicone oil, epoxy-modified silicone oil, epoxy-polyether-modified silicone oil, phenol-modified silicone oil, carboxyl-modified silicone oil, mercapto-modified silicone oil, methacryl-modified silicone oil, and α-methylstyrene-modified silicone oil.
[0223] The average particle size of the primary particles of the external additive is not particularly limited and can be appropriately selected according to the purpose. For example, it is preferably 100 nm or less, more preferably 1 nm to 100 nm, even more preferably 3 nm to 70 nm, and particularly preferably 5 nm to 70 nm. When the average particle size of the primary particles is within this range, it is possible to prevent the inorganic fine particles from being buried in the toner, making it difficult to effectively exert their functions, and the photoreceptor surface from being unevenly damaged.
[0224] The external additive preferably contains at least one type of inorganic fine particles that have been hydrophobized and have an average primary particle size of 20 nm or less, and at least one type of inorganic fine particles that have an average primary particle size of 30 nm or more.
[0225] The specific surface area of the external additive by the BET method is 20 m 2 / g~500m 2 / g is preferred.
[0226] The content of the external additive is not particularly limited and can be appropriately selected depending on the purpose. For example, the content is preferably 0.1 parts by mass to 5 parts by mass, and more preferably 0.3 parts by mass to 3 parts by mass, relative to 100 parts by mass of the toner.
[0227] -Flow improver- The flowability improver is not particularly limited, and can be appropriately selected according to purpose, as long as it can be surface-treated to increase hydrophobicity and prevent deterioration of flowability and charging properties even under high humidity.For example, silane coupling agent, silylating agent, silane coupling agent having fluorinated alkyl group, organic titanate coupling agent, aluminum coupling agent, silicone oil, modified silicone oil, etc. can be mentioned. It is particularly preferable that the silica and titanium oxide are surface-treated with such a flowability improving agent and used as hydrophobic silica and hydrophobic titanium oxide.
[0228] -Cleaning improver- The cleaning property improver is not particularly limited as long as it is added to the toner to remove the developer remaining on the photoconductor or the primary transfer medium after transfer, and can be appropriately selected according to the purpose. For example, it may be a fatty acid metal salt such as zinc stearate, calcium stearate, or stearic acid, or a polymer fine particle produced by soap-free emulsion polymerization such as polymethyl methacrylate fine particle or polystyrene fine particle.
[0229] The polymer fine particles preferably have a relatively narrow particle size distribution, and the volume average particle size is preferably 0.01 μm to 1 μm.
[0230] -Magnetic materials- The magnetic material is not particularly limited and may be appropriately selected depending on the purpose, and examples thereof include iron powder, magnetite, ferrite, etc. Among these, those that are white in color are preferred.
[0231] <Toner glass transition temperature> The glass transition temperature (Tg1st) of the toner at the first temperature rise in differential scanning calorimetry (DSC) is preferably 20°C or more and 65°C or less, more preferably 20°C or more and 50°C or less, and even more preferably 40°C or more and 50°C or less. The glass transition temperature (Tga1st) in the first temperature rise of the DSC of the component of the toner insoluble in tetrahydrofuran (THF) is preferably -45°C or more and 10°C or less, and more preferably -40°C or more and 10°C or less. It is particularly preferable that Tg1st is 20° C. or more and 50° C. or less, and Tga1st is −40° C. or more and 10° C. or less. In this case, good low-temperature fixability can be obtained while maintaining heat-resistant storage stability.
[0232] The glass transition temperature (Tg2nd) of the THF-soluble component of the toner at the second temperature rise in DSC is preferably 20°C to 65°C.
[0233] It is preferable that the glass transition temperature (Tg1st) during the first temperature rise and the glass transition temperature (Tg2nd) during the second temperature rise in differential scanning calorimetry (DSC) of the toner satisfy Tg1st-Tg2nd≧10[°C], since this improves the low-temperature fixability and heat-resistant storage stability.
[0234] Here, the glass transition temperature of the toner can be measured, for example, by using a differential scanning calorimeter (DSC-60, Q-200, manufactured by Shimadzu Corporation). For example, a DSC curve is measured using the above-mentioned differential scanning calorimeter. From the obtained DSC curves, a DSC curve at the first heating is selected using an analysis program, and the glass transition temperature Tg1st at the first heating is obtained using the endothermic shoulder temperature in the analysis program. A DSC curve at the second heating is selected, and the glass transition temperature Tg2nd at the second heating is obtained using the endothermic shoulder temperature.
[0235] The method for determining the glass transition temperature is as follows: In the present invention, the onset value shown in Fig. 3 is calculated as Tg. A DSC curve is obtained by applying an analysis program to the obtained DSC curve, and the onset value shown in the figure is taken as Tg in the present invention.
[0236] For the toner components insoluble in THF, the glass transition temperature (Tg1st) during the first temperature rise can be separated into two points, so that the following modulation temperature amplitude is applied to the temperature rise measurement. Using the modulation mode, heat from -80°C to 150°C at a temperature increase rate of 1.0°C / min while applying a modulation temperature amplitude of ±1.0°C / min (first temperature increase). Using the analysis program as above, obtain a DSC curve by plotting "Reversing Heat Flow" on the vertical axis, and use the onset value shown in the figure as Tg.
[0237] (Developer) The developer of the present invention contains at least the toner of the present invention, and contains other components, such as a carrier, which are appropriately selected as necessary. The developer may be a one-component developer or a two-component developer, but when used in a high-speed printer or the like that corresponds to the recent improvement in information processing speed, a two-component developer is preferred because of its improved lifespan.
[0238] <Career> The carrier is not particularly limited and may be appropriately selected depending on the purpose, but it is preferable that the carrier has a core material and a resin layer that covers the core material.
[0239] -Core material- The material of the core material is not particularly limited and can be appropriately selected according to the purpose. For example, manganese-strontium-based materials of 50 emu / g to 90 emu / g and manganese-magnesium-based materials of 50 emu / g to 90 emu / g can be mentioned. In order to ensure image density, it is preferable to use high magnetization materials such as iron powder of 100 emu / g or more and magnetite of 75 emu / g to 120 emu / g. In addition, it is preferable to use low magnetization materials such as copper-zinc-based materials of 30 emu / g to 80 emu / g because it can reduce the impact of the developer in a standing state on the photoconductor and is advantageous for high image quality. These materials may be used alone or in combination of two or more.
[0240] The volume average particle diameter of the core material is not particularly limited and can be appropriately selected according to the purpose. For example, 10 μm to 150 μm is preferable, and 40 μm to 100 μm is more preferable. If the volume average particle diameter is less than 10 μm, the amount of fine powder in the carrier increases, and the magnetization per particle decreases, which may cause the carrier to scatter. On the other hand, if it exceeds 150 μm, the specific surface area decreases, which may cause the toner to scatter, and in full color with many solid parts, the reproduction of the solid parts may be particularly poor.
[0241] The toner of the present invention can be mixed with the above-mentioned carrier and used in a two-component developer. The content of the carrier in the two-component developer is not particularly limited and can be appropriately selected depending on the purpose. For example, the content is preferably 90 parts by mass to 98 parts by mass, more preferably 93 parts by mass to 97 parts by mass, relative to 100 parts by mass of the two-component developer.
[0242] The developer of the present invention can be suitably used for image formation by various known electrophotographic methods such as a magnetic one-component development method, a non-magnetic one-component development method, and a two-component development method.
[0243] (Toner manufacturing method) The toner production method of the present invention is a method for producing the above-mentioned toner. The method for producing the toner includes a composite particle forming step and a removing step, and further includes other steps as necessary.
[0244] <Composite particle formation process> The composite particle forming step is a step of forming composite particles by adhering resin fine particles to the surfaces of toner base particles. Examples of the method for forming the composite particles include a known dissolution suspension method in which an oil phase containing components of the toner base particles, such as the binder resin, colorant, and wax, is dispersed in an aqueous medium containing resin fine particles to form granules.
[0245] As an example of the dissolution suspension method, a method of forming composite particles while generating a polyester resin by an elongation reaction and / or a crosslinking reaction between the prepolymer and the curing agent will be described. In this method, an aqueous medium is prepared, an oil phase containing a toner base particle material is prepared, the toner base particle material is emulsified or dispersed, and the organic solvent is removed.
[0246] - Preparation of aqueous medium (aqueous phase) - The aqueous medium can be prepared, for example, by dispersing resin fine particles in the aqueous medium. The amount of the resin fine particles added to the aqueous medium is not particularly limited and can be appropriately selected according to the purpose. For example, it is preferably 0.5 parts by mass to 10 parts by mass with respect to 100 parts by mass of the aqueous medium.
[0247] The aqueous medium is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include water, a solvent miscible with water, and a mixture thereof. These may be used alone or in combination of two or more. Among these, water is preferred.
[0248] The water-miscible solvent is not particularly limited and may be appropriately selected depending on the purpose. Examples of the water-miscible solvent include alcohol, dimethylformamide, tetrahydrofuran, cellosolves, and lower ketones. Examples of the alcohol include methanol, isopropanol, and ethylene glycol. Examples of the lower ketones include acetone and methyl ethyl ketone.
[0249] - Preparation of oil phase - The oil phase can be prepared by dissolving or dispersing the toner base particle material, which contains a binder resin, a colorant, and a wax, and further contains a hardener, etc., as required, in an organic solvent.
[0250] The organic solvent is not particularly limited and can be appropriately selected depending on the purpose. For example, an organic solvent having a boiling point of less than 150° C. is preferred because it is easy to remove.
[0251] Examples of the organic solvent having a boiling point of less than 150° C. include toluene, xylene, benzene, carbon tetrachloride, methylene chloride, 1,2-dichloroethane, 1,1,2-trichloroethane, trichloroethylene, chloroform, monochlorobenzene, dichloroethylidene, methyl acetate, ethyl acetate, methyl ethyl ketone, and methyl isobutyl ketone. These may be used alone or in combination of two or more. Among these, ethyl acetate, toluene, xylene, benzene, methylene chloride, 1,2-dichloroethane, chloroform, carbon tetrachloride, and the like are preferred, and ethyl acetate is more preferred.
[0252] -Emulsification or dispersion- The toner materials can be emulsified or dispersed by dispersing an oil phase containing the toner materials in the aqueous medium, and when the toner materials are emulsified or dispersed, the curing agent and the prepolymer can undergo an elongation reaction and / or a crosslinking reaction.
[0253] The reaction conditions (reaction time, reaction temperature) for producing the prepolymer are not particularly limited and can be appropriately selected depending on the combination of the curing agent and the prepolymer. The reaction time is preferably 10 minutes to 40 hours, more preferably 2 to 24 hours. The reaction temperature is preferably 0°C to 150°C, more preferably 40°C to 98°C.
[0254] The method for stably forming a dispersion liquid containing the prepolymer in the aqueous medium is not particularly limited and can be appropriately selected depending on the purpose. For example, there is a method in which an oil phase prepared by dissolving or dispersing a toner material in a solvent is added to an aqueous medium phase, and the mixture is dispersed by shear force.
[0255] The dispersing machine for the dispersion is not particularly limited and can be appropriately selected according to the purpose. For example, low-speed shear dispersing machine, high-speed shear dispersing machine, friction dispersing machine, high-pressure jet dispersing machine, ultrasonic dispersing machine, etc. can be mentioned. Among these, high-speed shear dispersing machine is preferable because it can control the particle size of the dispersion (oil droplets) to 2 μm to 20 μm.
[0256] When using the high-speed shear type disperser, the conditions such as the rotation speed, dispersion time, and dispersion temperature can be appropriately selected depending on the purpose. The rotation speed is preferably 1,000 rpm to 30,000 rpm, and more preferably 5,000 rpm to 20,000 rpm. In the case of a batch method, the dispersion time is preferably 0.1 minutes to 5 minutes. The dispersion temperature is preferably 0°C to 150°C under pressure, and more preferably 40°C to 98°C. Generally, the higher the dispersion temperature, the easier the dispersion.
[0257] The amount of the aqueous medium used when emulsifying or dispersing the toner materials is not particularly limited, and can be appropriately selected according to the purpose. For example, it is preferably 50 parts by mass to 2,000 parts by mass, more preferably 100 parts by mass to 1,000 parts by mass, relative to 100 parts by mass of the toner materials. If the amount of the aqueous medium used is less than 50 parts by mass, the dispersion state of the toner materials may be poor, and toner base particles of a predetermined particle size may not be obtained, and if it exceeds 2,000 parts by mass, the production cost may be high.
[0258] When the oil phase containing the toner materials is emulsified or dispersed, it is preferable to use a dispersant from the viewpoints of stabilizing the dispersion such as oil droplets, forming a desired shape, and sharpening the particle size distribution.
[0259] The dispersant is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include surfactants, poorly water-soluble inorganic compound dispersants, polymer-based protective colloids, etc. These may be used alone or in combination of two or more. Among these, surfactants are preferred.
[0260] The surfactant is not particularly limited and can be appropriately selected depending on the purpose, and for example, anionic surfactants, cationic surfactants, nonionic surfactants, amphoteric surfactants, etc. can be used. Examples of the anionic surfactant include alkylbenzene sulfonates, α-olefin sulfonates, and phosphate esters. Among these, those having a fluoroalkyl group are preferred.
[0261] -Removal of organic solvents- The method for removing the organic solvent from the dispersion liquid such as the emulsified slurry is not particularly limited and can be appropriately selected depending on the purpose. Examples of the method include a method in which the temperature of the entire reaction system is gradually increased to evaporate the organic solvent in the oil droplets, and a method in which the dispersion liquid is sprayed in a dry atmosphere to remove the organic solvent in the oil droplets. Once the organic solvent is removed, composite particles are formed.
[0262] <Removal process> The removing step is a step of removing at least a part of the resin fine particles from the composite particles, and it is preferable to remove a part or the whole of the shell resin (resin (b1)) in the resin fine particles. An example of the step of removing at least a portion of the resin fine particles is a washing step of washing the composite particles. For this reason, the removing step can also be called a washing step.
[0263] In the washing step, the method for removing a part or all of the resin (b1) includes a method for removing a part or all of (b1) by a chemical method. The chemical method may, for example, be a step of washing the composite particles with a basic aqueous solution, which can dissolve a part or all of the shell resin (b1).
[0264] The basic aqueous solution is not particularly limited as long as it is basic and can be appropriately selected depending on the purpose, and examples thereof include aqueous solutions of hydroxides of alkali metals such as potassium hydroxide and sodium hydroxide, ammonia, etc. These may be used alone or in combination of two or more. Among these, potassium hydroxide and sodium hydroxide are preferred from the viewpoint of easiness in dissolving the shell resin (b1). The pH of the basic aqueous solution is preferably 8 to 14, and more preferably 10 to 12.
[0265] In the washing step, the composite particles and the alkaline aqueous solution can be mixed by, for example, dropping the basic aqueous solution into the composite slurry under stirring. After the basic aqueous solution has been added dropwise, an acidic aqueous solution may be added dropwise to neutralize the mixture.
[0266] <Other processes> The other steps are not particularly limited and can be appropriately selected depending on the purpose. Examples of the other steps include a drying step and a classification step. The drying step is not particularly limited as long as it can remove the solvent from the composite particles, and can be appropriately selected depending on the purpose. The classification step may be carried out by removing fine particles in a liquid using a cyclone, decanter, centrifugal separation, or the like, or the classification operation may be carried out after drying.
[0267] The obtained composite particles may be mixed with particles of the external additive, the charge control agent, etc. In this case, by applying a mechanical impact force, it is possible to suppress the particles of the external additive, etc. from being detached from the surface of the toner base particle. The method of applying the mechanical impact force is not particularly limited and can be appropriately selected depending on the purpose. Examples of the method include a method of applying an impact force to the mixture using a blade rotating at high speed, a method of introducing the mixture into a high-speed air stream and accelerating it to collide the particles with each other or with a suitable collision plate, etc.
[0268] The apparatus used in the above method is not particularly limited and can be appropriately selected depending on the purpose. Examples include Angmill (manufactured by Hosokawa Micron Corporation), an apparatus obtained by modifying I-type mill (manufactured by Japan Pneumatic Co., Ltd.) to reduce the grinding air pressure, Hybridization System (manufactured by Nara Machinery Works, Ltd.), Cryptron System (manufactured by Kawasaki Heavy Industries, Ltd.), and automatic mortar.
[0269] (Toner storage unit) The toner storage unit in the present invention refers to a unit having a function of storing toner and storing the toner. Examples of the toner storage unit include a toner storage container, a developing unit, and a process cartridge. The toner storage container refers to a container that stores toner. The developing device has a means for storing toner and developing the toner. The process cartridge is a cartridge which integrates at least an image carrier and a developing means, contains toner, and is detachably mountable to an image forming apparatus. The process cartridge may further include at least one selected from a charging means, an exposure means, and a cleaning means.
[0270] By mounting the toner storage unit of the present invention in an image forming apparatus and forming an image, the image is formed using the toner of the present invention, so that low-temperature fixing properties and heat-resistant storage stability can be achieved at the same time, and contamination of the cleaning member and photosensitive member can be suppressed while maintaining good cleaning properties.
[0271] Next, one embodiment of the process cartridge is shown in Fig. 4. As shown in the figure, the process cartridge of this embodiment has a built-in latent image carrier 101, a charging device 102, a developing device 104, and a cleaning unit 107, and further has other means as necessary. In the figure, reference numeral 103 denotes exposure from an exposure device, and reference numeral 105 denotes recording paper.
[0272] The latent image carrier 101 may be the same as an electrostatic latent image carrier in an image forming apparatus described later. The charging device 102 may be any charging member.
[0273] In the image forming process using the process cartridge shown in FIG. 4, while the latent image carrier 101 rotates in the direction of the arrow, an electrostatic latent image corresponding to the exposed image is formed on its surface by charging the latent image carrier 101 with a charging device 102 and exposing the latent image carrier 101 to light with light 103 by an exposure means (not shown).
[0274] This electrostatic latent image is developed with toner by a developing device 104, and the toner development is transferred to a recording paper 105 by a transfer roller 108 and printed out. Next, the surface of the latent image carrier after the image transfer is cleaned by a cleaning unit 107, and further discharged by a discharge means (not shown), and the above operations are repeated again.
[0275] (Image forming apparatus and image forming method) The image forming apparatus of the present invention has an electrostatic latent image carrier, an electrostatic latent image forming unit, a developing unit, a transfer unit, a fixing unit, and a cleaning unit. It may have the toner storage unit described above, and preferably has other units as necessary. The image forming method according to the present invention includes an electrostatic latent image forming step, a developing step, a transferring step, a fixing step, and a cleaning step, and may further include other steps as required.
[0276] <Electrostatic latent image carrier> The material, structure, and size of the electrostatic latent image carrier (also called photoconductor) are not particularly limited and can be appropriately selected from known materials. Examples of the material include inorganic photoconductors such as amorphous silicon and selenium, and organic photoconductors such as polysilane and phthalopolymethine. Among these, amorphous silicon is preferred in terms of long life. The linear speed of the electrostatic latent image bearing member is preferably 300 mm / s or more.
[0277] <Electrostatic latent image forming means and electrostatic latent image forming process> The electrostatic latent image forming unit is not particularly limited as long as it is a unit that forms an electrostatic latent image on the electrostatic latent image carrier, and can be appropriately selected depending on the purpose. For example, it may be a unit having at least a charging member that charges the surface of the electrostatic latent image carrier and an exposure member that exposes the surface of the electrostatic latent image carrier to light in an imagewise manner.
[0278] The electrostatic latent image forming step is not particularly limited as long as it is a step of forming an electrostatic latent image on the electrostatic latent image bearing member, and can be appropriately selected depending on the purpose. For example, it can be performed by charging the surface of the electrostatic latent image bearing member and then exposing it imagewise, and can be performed using the electrostatic latent image forming unit.
[0279] -Charging materials and charging- The charging member is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include a contact charger having a conductive or semiconductive roller, brush, film, rubber blade, etc., which is known per se, and a non-contact charger using corona discharge such as a corotron or scorotron.
[0280] The charging can be carried out, for example, by applying a voltage to the surface of the electrostatic latent image bearing member using the charging member. The shape of the charging member may be any shape, such as a roller, a magnetic brush, a fur brush, etc., and can be selected according to the specifications and shape of the image forming apparatus.
[0281] The charging member is not limited to the contact-type charging member, but it is preferable to use a contact-type charging member because an image forming apparatus in which the amount of ozone generated from the charging member is reduced can be obtained.
[0282] <<Exposure materials and exposure>> The exposing member is not particularly limited and may be appropriately selected depending on the purpose as long as it can expose the surface of the electrostatic latent image carrier charged by the charging member in the form of an image to be formed, and examples of the exposing member include various exposing members such as a copying optical system, a rod lens array system, a laser optical system, and a liquid crystal shutter optical system.
[0283] The light source used in the exposure member is not particularly limited and can be appropriately selected depending on the purpose. For example, fluorescent lamps, tungsten lamps, halogen lamps, mercury lamps, sodium lamps, light-emitting diodes (LEDs), semiconductor lasers (LDs), electroluminescence (EL), and other light-emitting materials in general can be mentioned.
[0284] In order to irradiate only light in a desired wavelength range, various filters such as a sharp cut filter, a band pass filter, a near infrared cut filter, a dichroic filter, an interference filter, and a color temperature conversion filter can be used.
[0285] The exposure can be carried out, for example, by exposing the surface of the electrostatic latent image bearing member imagewise using the exposure member. In the present invention, a light back system may be adopted in which exposure is performed imagewise from the back side of the electrostatic latent image bearing member.
[0286] <Developing means and developing process> The developing unit is not particularly limited as long as it is a developing unit that develops the electrostatic latent image formed on the electrostatic latent image carrier to form a toner image, which is a visible image, and is equipped with a toner, and can be appropriately selected depending on the purpose. The developing step is not particularly limited as long as it is a step of developing the electrostatic latent image formed on the electrostatic latent image carrier with a toner to form a toner image, which is a visible image, and can be appropriately selected depending on the purpose. For example, the developing step can be performed by the developing means. The developing means is preferably a developing device having an agitator that frictionally stirs the toner to charge it, a magnetic field generating means fixed inside, and a developer carrier that can rotate and carries a developer containing the toner on its surface.
[0287] <Transfer means and transfer process> The transfer means is not particularly limited as long as it is a means for transferring a visible image onto a recording medium, and can be appropriately selected according to the purpose. For example, a preferred embodiment has a first transfer means for transferring a visible image onto an intermediate transfer body to form a composite transfer image, and a second transfer means for transferring the composite transfer image onto a recording medium. The transfer step is not particularly limited as long as it is a step of transferring a visible image to a recording medium, and can be appropriately selected according to the purpose. For example, it is preferable to use an intermediate transfer body, and after the visible image is primarily transferred onto the intermediate transfer body, the visible image is secondarily transferred onto the recording medium. The transfer step can be carried out by, for example, charging the visible image on the photoconductor using a transfer charger, and can be carried out by the transfer unit.
[0288] Here, when the image to be secondarily transferred onto the recording medium is a color image made up of toners of multiple colors, the transfer means can be configured to sequentially overlay toners of each color on the intermediate transfer body to form an image on the intermediate transfer body, and the intermediate transfer means can be configured to secondarily transfer the image on the intermediate transfer body onto the recording medium all at once. The intermediate transfer body is not particularly limited and can be appropriately selected from known transfer bodies depending on the purpose. For example, a transfer belt is preferably used.
[0289] The transfer means (the primary transfer means and the secondary transfer means) preferably has at least a transfer device that peels and charges the visible image formed on the photoreceptor onto the recording medium. Examples of the transfer device include a corona transfer device that uses corona discharge, a transfer belt, a transfer roller, a pressure transfer roller, and an adhesive transfer device. The recording medium is typically plain paper, but is not particularly limited as long as it is capable of transferring an unfixed image after development, and can be appropriately selected according to the purpose. A PET base for overhead projectors can also be used.
[0290] <Fixing means and fixing process> The fixing means is not particularly limited as long as it is a means for fixing the transferred image transferred to the recording medium, and can be appropriately selected according to the purpose. For example, a known heating and pressing member is preferable. Examples of the heating and pressing member include a combination of a heating roller and a pressing roller, and a combination of a heating roller, a pressing roller, and an endless belt. The fixing step is not particularly limited as long as it is a step of fixing the visible image transferred to the recording medium, and can be appropriately selected according to the purpose. For example, the fixing step may be performed for each color toner transferred to the recording medium, or may be performed simultaneously for each color toner in a laminated state.
[0291] The fixing step can be carried out by the fixing means. The heating temperature in the heating and pressing member is preferably 80°C to 200°C. In the present invention, depending on the purpose, for example, a known optical fixing device may be used together with or instead of the fixing means. The surface pressure in the fixing step is not particularly limited and can be appropriately selected depending on the purpose. 2 ~80N / cm 2 It is preferable that:
[0292] <Cleaning means and cleaning process> The cleaning means is not particularly limited as long as it can remove the toner remaining on the photoreceptor, and can be appropriately selected depending on the purpose, for example, a magnetic brush cleaner, an electrostatic brush cleaner, a magnetic roller cleaner, a blade cleaner, a brush cleaner, a web cleaner, etc. The cleaning step is not particularly limited as long as it can remove the toner remaining on the photoconductor, and can be appropriately selected depending on the purpose. For example, the cleaning step can be performed by the cleaning unit.
[0293] <Other means and other steps> Examples of the other means include a static elimination means, a recycling means, and a control means. Examples of the other steps include a static elimination step, a recycling step, and a control step.
[0294] -Static charge removal means and static charge removal process- The charge removing means is not particularly limited as long as it is a means for removing electricity by applying a charge removing bias to the photoconductor, and may be appropriately selected depending on the purpose. For example, a charge removing lamp may be used. The charge removing step is not particularly limited as long as it is a step of removing electricity by applying a charge removing bias to the photoconductor, and can be appropriately selected depending on the purpose. For example, it can be performed by the charge removing unit.
[0295] -Recycling methods and processes- The recycling means is not particularly limited as long as it is a means for recycling the toner removed in the cleaning step to the developing device, and can be appropriately selected depending on the purpose. For example, a known transport means can be used. The recycling step is not particularly limited as long as it is a step of recycling the toner removed by the cleaning step to the developing device, and can be appropriately selected depending on the purpose. For example, it can be performed by the recycling means.
[0296] <An example of an image forming apparatus> Next, one embodiment of a method for forming an image by the image forming apparatus of the present invention will be described with reference to Fig. 5. Although a printer is shown as an example of the image forming apparatus of this embodiment, the image forming apparatus is not particularly limited as long as it is capable of forming an image using toner, such as a copier, facsimile, or multifunction machine. The image forming apparatus includes a paper feed section 210, a conveying section 220, an image creating section 230, a transfer section 240, and a fixing unit 250. The paper feed section 210 includes a paper feed cassette 211 in which the paper P to be fed is stacked, and a paper feed roller 212 that feeds the paper P stacked in the paper feed cassette 211 one sheet at a time.
[0297] The conveying section 220 includes a roller 221 that conveys the paper P fed by the paper feed roller 212 toward the transfer section 240, a pair of timing rollers 222 that hold the leading end of the paper P conveyed by the roller 221 and wait to send the paper to the transfer section 240 at a predetermined timing, and a paper discharge roller 223 that discharges the paper P with the color toner image fixed thereto onto a paper discharge tray 224.
[0298] The image creating section 230 includes, spaced at a predetermined interval from left to right in the figure, an image forming unit Y that forms an image using a developer containing yellow toner, an image forming unit C that uses a developer containing cyan toner, an image forming unit M that uses a developer containing magenta toner, an image forming unit K that uses a developer containing black toner, and an exposure device 233.
[0299] Incidentally, when referring to any one of the image forming units (Y, C, M, K), it is referred to as an image forming unit.
[0300] The developer contains toner and carrier. The four image forming units (Y, C, M, K) have substantially the same mechanical configuration, except for the developer used in each unit.
[0301] The image forming units (Y, C, M, K) are provided so as to be rotatable clockwise in the drawing. They include photoconductor drums (231Y, 231C, 231M, 231K) on which electrostatic latent images and toner images are formed, chargers (232Y, 232C, 232M, 232K) for uniformly charging the surfaces of the photoconductor drums (231Y, 231C, 231M, 231K), developers (180Y, 180C, 180M, 180K) for developing the electrostatic latent images formed on the surfaces of the photoconductor drums (231Y, 231C, 231M, 231K) by the exposure device 233 into toner images using toners of each color, and cleaners (236Y, 236C, 236M, 236K) for removing toner remaining on the surfaces of the photoconductor drums (231Y, 231C, 231M, 231K).
[0302] In addition, the image forming units (Y, C, M, K) are equipped with toner cartridges (234Y, 234C, 234M, 234K) that contain toner of each color, and sub-hoppers (160Y, 160C, 160M, 160K) for replenishing the toner supplied from the toner cartridges (234Y, 234C, 234M, 234K).
[0303] The toner contained in the toner cartridge 234 is discharged by a suction pump and supplied to the sub hopper 160 via a supply pipe. The sub hopper 160 transports the toner supplied from the toner cartridge 234 and supplies it to the developing device 180. The developing device 180 develops the electrostatic latent image formed on the photosensitive drum 231 using the toner supplied by the sub hopper 160.
[0304] The transfer unit 240 includes a drive roller 241 and a driven roller 242, an intermediate transfer belt 243 that can rotate counterclockwise in the figure as the drive roller 241 is driven, primary transfer rollers (244Y, 244C, 244M, 244K) arranged opposite the photosensitive drum 231 across the intermediate transfer belt 243, and secondary opposing roller 245 and secondary transfer roller 246 arranged opposite each other across the intermediate transfer belt 243 at the transfer position of the toner image to paper.
[0305] The fixing unit 250 has a heater installed inside and is equipped with a pressure roller 252 that forms a nip by rotatably pressing a fixing belt 251, which heats the paper P, against the fixing belt 251. This applies heat and pressure to the color toner image on the paper P, fixing the color toner image. The paper P with the fixed color toner image is discharged to a paper discharge tray 224 by a paper discharge roller 223, completing a series of image formation processes. EXAMPLES
[0306] The present invention will be described in more detail below by way of examples, but the present invention is not limited to these examples.
[0307] (Production Example 1) [Production of Aqueous Dispersion (W0-1) of Resin Fine Particles (A)] In a reaction vessel equipped with a stirrer, a heating / cooling device, and a thermometer, 3710 parts by mass of water and 200 parts by mass of polyoxyethylene-1-(allyloxymethyl) alkyl ether sulfate ester ammonium (Aqualon KH-1025, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) were charged and homogenized by stirring at 200 rpm. The homogenized mixture was heated to raise the temperature inside the system to 75° C., after which 90 parts by mass of a 10% by mass aqueous ammonium persulfate solution was added, and then a mixture consisting of 450 parts by mass of styrene, 250 parts by mass of butyl acrylate, and 300 parts by mass of methacrylic acid was added dropwise over 4 hours. After the dropwise addition, the mixture was aged at 75° C. for 4 hours to obtain a fine particle dispersion (W0-1) containing a resin (a1-1) that is a polymer in which the monomer and polyoxyethylene-1-(allyloxymethyl) alkyl ether sulfate ester ammonium were copolymerized. The volume average particle size of the microparticles in the microparticle dispersion (W0-1) was 15 nm when measured by dynamic light scattering (light scattering electrophoresis apparatus: ELS-8000, manufactured by Otsuka Electronics Co., Ltd.). A part of the fine particle dispersion (W0-1) was dried to isolate resin (a1-1), which had a glass transition temperature (TgA) of 75° C. and an acid value of 195 mg KOH / g.
[0308] (Production Example 2) [Production of Aqueous Dispersion (W0-2) of Resin Fine Particles (A)] In a reaction vessel equipped with a stirrer, a heating / cooling device, and a thermometer, 3760 parts by mass of water and 150 parts by mass of polyoxyethylene-1-(allyloxymethyl) alkyl ether sulfate ester ammonium (Aqualon KH-1025, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) were charged and homogenized by stirring at 200 rpm. The homogenized mixture was heated to raise the temperature inside the system to 75° C., after which 90 parts by mass of a 10% by mass aqueous ammonium persulfate solution was added, and then a mixture consisting of 430 parts by mass of styrene, 270 parts by mass of butyl acrylate, and 300 parts by mass of methacrylic acid was added dropwise over 4 hours. After the dropwise addition, the mixture was aged at 75° C. for 4 hours to obtain a fine particle dispersion (W0-2) containing a resin (a2-1) that is a polymer in which the monomer and polyoxyethylene-1-(allyloxymethyl) alkyl ether sulfate ester ammonium were copolymerized. The volume average particle size of the microparticles in the microparticle dispersion (W0-2) was measured in the same manner as in Production Example 1 and was found to be 30 nm. A part of the fine particle dispersion (W0-2) was dried to isolate a resin (a2-1). The resin had a glass transition temperature (TgA) of 85° C. and an acid value of 195 mg KOH / g.
[0309] (Production Example 3) [Production of Aqueous Dispersion (W0-3) of Resin Fine Particles (A)] In a reaction vessel equipped with a stirrer, a heating / cooling device, and a thermometer, 3810 parts by mass of water and 100 parts by mass of polyoxyethylene-1-(allyloxymethyl) alkyl ether sulfate ester ammonium (Aqualon KH-1025, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) were charged and homogenized by stirring at 200 rpm. The homogenized mixture was heated to raise the temperature inside the system to 75° C., after which 90 parts by mass of a 10% by mass aqueous ammonium persulfate solution was added, and then a mixture consisting of 400 parts by mass of styrene, 300 parts by mass of butyl acrylate, and 300 parts by mass of methacrylic acid was added dropwise over 4 hours. After the dropwise addition, the mixture was aged at 75° C. for 4 hours to obtain a fine particle dispersion (W0-3) containing a resin (a3-1) that is a polymer in which the monomer and polyoxyethylene-1-(allyloxymethyl) alkyl ether sulfate ester ammonium were copolymerized. The volume average particle size of the microparticles in the microparticle dispersion (W0-3) was measured in the same manner as in Production Example 1 and was found to be 45 nm. A part of the fine particle dispersion (W0-3) was dried to isolate a resin (a3-1). The resin had a glass transition temperature (TgA) of 65° C. and an acid value of 195 mg KOH / g.
[0310] Table 1 shows the contents of the aqueous dispersions (W0-1) to (W0-3) of the resin fine particles (A).
[0311] [Table 1]
[0312] (Production Example 4) <Production of Aqueous Dispersion (W-1) of Resin Fine Particles (A-1)> Next, 667 parts by mass of the aqueous dispersion (W0-1) of resin microparticles (A) and 248 parts by mass of water were charged into a reaction vessel equipped with a stirrer, a heating / cooling device, and a thermometer, and 0.267 parts by mass of tertiary butyl hydroperoxide (Perbutyl H, manufactured by NOF Corporation) was added and heated to raise the temperature inside the system to 70°C. After that, 43.3 parts by mass of styrene, 23.3 parts by mass of butyl acrylate, and 18.0 parts by mass of a 1% by mass aqueous ascorbic acid solution were added dropwise over 2 hours. After the dropwise addition, the mixture was matured at 70°C for 4 hours to obtain an aqueous dispersion (W-1) of resin microparticles (A-1) containing resin (a2-1), which is a polymer formed by copolymerizing the monomer using the resin microparticles in (W0-1) as seeds, and resin (a1-1) as constituent components within the same particle. The volume average particle size of the resin fine particles (A-1) was measured in the same manner as in Production Example 1 and was found to be 17.3 nm. The aqueous dispersion (W-1) of the resin fine particles (A-1) was neutralized with 10% by weight of ammonia aqueous solution to pH 9.0, and the precipitate obtained by centrifugation was dried to isolate the resin (a2-1). The glass transition temperature (Tg) of the resin was 61°C.
[0313] It was confirmed as follows that the aqueous dispersion (W-1) of the resin fine particles (A-1) contains the resin fine particles (A-1) containing the resin (a1-1) and the resin (a2-1) as constituent components in the same particle. Specifically, 2 parts by weight of gelatin (Cook Gelatin, Morinaga Milk Industry Co., Ltd.) was added to and dissolved in 15 parts by weight of water heated to 95°C to 100°C, and the gelatin solution was cooled to 40°C by air cooling. An aqueous dispersion (W-1) of resin microparticles (A-1) was then mixed with the aqueous solution in a 1:1 mass ratio, thoroughly stirred, and then cooled to 10°C for 1 hour to produce a hardened gel. This gel was sliced into 80 nm-thick sections using an ultramicrotome (Ultramicrotome UC7, FC7, Leica Microsystems) while controlling the temperature at -80°C. The sections were then subjected to gas-phase staining with a 2% by mass aqueous solution of ruthenium tetroxide for 5 minutes, and then observed with a transmission electron microscope (Hitachi Technologies, H-7100) to confirm the results.
[0314] (Production Example 5) <Production of Aqueous Dispersion (W-2) of Resin Fine Particles (A-2)> Next, 667 parts by mass of the aqueous dispersion (W0-2) of resin microparticles (A) and 248 parts by mass of water were charged into a reaction vessel equipped with a stirrer, a heating / cooling device, and a thermometer, and 0.267 parts by mass of tert-butyl hydroperoxide (NOF Corp., Perbutyl H) was added and the system was heated to raise the temperature inside the system to 70°C. After that, 43.3 parts by mass of styrene, 23.3 parts by mass of butyl acrylate, and 18.0 parts by mass of a 1% by mass aqueous ascorbic acid solution were added dropwise over 2 hours. After the dropwise addition, the mixture was matured at 70°C for 4 hours to obtain a microparticle dispersion (W-2) of resin microparticles (A-2) containing resin (a2-2), which is a polymer copolymerized from the monomers using the resin microparticles in (W0-2) as seeds, and resin (a1-2) as constituent components within the same particle. The volume average particle size of the resin fine particles (A-2) was measured in the same manner as in Production Example 1 and was found to be 34.3 nm. The aqueous dispersion (W-2) of the resin fine particles (A-2) was neutralized with 10% by weight of ammonia aqueous solution to pH 9.0, and the precipitate obtained by centrifugation was dried to isolate the resin (a2-2). The glass transition temperature (Tg) of the resin was 69°C. It was confirmed by a method similar to that in Production Example 4 that the aqueous dispersion (W-2) of resin microparticles (A-2) contained resin microparticles (A-2) containing resin (a1-2) and resin (a2-2) as constituent components within the same particle.
[0315] (Production Example 6) <Production of Aqueous Dispersion (W-3) of Resin Fine Particles (A-3)> Next, 667 parts by mass of the aqueous dispersion (W0-3) of resin microparticles (A) and 248 parts by mass of water were charged into a reaction vessel equipped with a stirrer, a heating / cooling device, and a thermometer, and 0.267 parts by mass of tertiary butyl hydroperoxide (Perbutyl H, manufactured by NOF Corporation) was added and heated to raise the temperature inside the system to 70°C. After that, 43.3 parts by mass of styrene, 23.3 parts by mass of butyl acrylate, and 18.0 parts by mass of a 1% by mass aqueous ascorbic acid solution were added dropwise over 2 hours. After the dropping, the mixture was aged at 70°C for 4 hours to obtain a fine particle dispersion (W-3) of resin fine particles (A-3) containing resin (a2-3) and resin (a1-3) as constituents in the same particle, which are polymers obtained by copolymerizing the monomers using the resin fine particles in (W0-3) as seeds. The volume average particle size of the resin fine particles (A-3) was measured in the same manner as in Production Example 1 and was found to be 51.5 nm. The aqueous dispersion (W-3) of the resin fine particles (A-3) was neutralized with 10% by weight of ammonia aqueous solution to pH 9.0, and the precipitate obtained by centrifugation was dried to isolate the resin (a2-3). The glass transition temperature (Tg) of the resin was 55°C. It was confirmed by a method similar to that in Production Example 4 that the aqueous dispersion (W-3) of resin microparticles (A-3) contained resin microparticles (A-3) containing resin (a1-3) and resin (a2-3) as constituent components within the same particle.
[0316] The details of the resin particles (A-1) to (A-3) are summarized in Table 2.
[0317] [Table 2]
[0318] (Production Example 7) <Synthesis of non-crystalline polyester resin (b-1)> Into a reaction vessel equipped with a cooling tube, a stirrer, a heating / cooling device, a thermometer, and a nitrogen inlet tube, 425 parts by mass of bisphenol A·PO 2-mol adduct, 100 parts by mass of propylene glycol, 634 parts by mass of terephthalic acid·propylene glycol 2-mol adduct, and 0.5 parts by mass of titanium diisopropoxybistriethanolamine as a condensation catalyst were placed and reacted at 230°C for 12 hours. Then, the reaction was carried out under a reduced pressure of 10 to 15 mmHg. The amount of propylene glycol recovered was 195 parts by mass. Next, after cooling to 180° C., 30 parts by mass of trimellitic anhydride was added and reacted at 180° C. for 1 hour, and then the mixture was taken out. The resin was cooled to room temperature to obtain amorphous polyester (b-1). The resin had a glass transition temperature (Tg) of 42°C, a number average molecular weight (Mn) of 2400, a weight average molecular weight (Mw) of 5400, a hydroxyl value of 32 mgKOH / g, and an acid value of 18 mgKOH / g.
[0319] (Production Example 8) <Production of Colorant Dispersion> Into a reaction vessel equipped with a cooling tube, a stirrer, a heating / cooling device, a thermometer, and a nitrogen inlet tube, 557 parts by mass of propylene glycol, 569 parts by mass of dimethyl terephthalate, 184 parts by mass of adipic acid, and 3 parts by mass of tetrabutoxychinate as a condensation catalyst were charged, and the mixture was reacted for 8 hours under a nitrogen stream at 180° C. while distilling off the produced methanol. Next, while gradually increasing the temperature to 230° C., the reaction was carried out for 4 hours under a nitrogen stream while distilling off the produced propylene glycol and water, and further for 1 hour under a reduced pressure of 0.007 MPa to 0.026 MPa. The amount of propylene glycol recovered was 175 parts by mass. Next, the mixture was cooled to 180°C, 121 parts by mass of trimellitic anhydride was added, and the mixture was reacted for 2 hours under normal pressure in a sealed state. The mixture was then heated to 220°C under normal pressure and reacted until the softening point reached 180°C, yielding a polyester resin (number average molecular weight (Mn) = 8500). 20 parts by mass of copper phthalocyanine, 4 parts by mass of colorant dispersant (Solsperse 28000, manufactured by Avecia), 20 parts by mass of the obtained polyester resin, and 56 parts by mass of ethyl acetate were added to a beaker and stirred to uniformly disperse, and then the copper phthalocyanine was finely dispersed using a bead mill to obtain a [colorant dispersion]. The volume average particle size of the resulting [colorant dispersion] was 0.2 μm.
[0320] (Production Example 9) <Production of Modified Wax (d)> A pressure-resistant reaction vessel equipped with a stirrer, a heating / cooling device, a thermometer, and a dropping bomb was charged with 454 parts by mass of xylene and 150 parts by mass of low-molecular-weight polyethylene (Sunwax LEL-400, manufactured by Sanyo Chemical Industries, Ltd.). After replacing the atmosphere with nitrogen, the temperature was raised to 170°C with stirring, and a mixed solution of 595 parts by mass of styrene, 255 parts by mass of methyl methacrylate, 34 parts by mass of di-t-butylperoxyhexahydroterephthalate, and 119 parts by mass of xylene was added dropwise at the same temperature over a period of 3 hours, and the vessel was then maintained at the same temperature for a further 30 minutes. Next, the xylene was distilled off under a reduced pressure of 0.039 MPa to obtain a modified wax (d). The SP value of the graft chain of the modified wax (d) is 10.35 (cal / cm 3 ) 1 / 2 The number average molecular weight (Mn) was 1,900, the weight average molecular weight (Mw) was 5,200, and the glass transition temperature (Tg) was 57°C.
[0321] (Production Example 10) <Production of release agent dispersion> Into a reaction vessel equipped with a cooling tube, a stirrer, a heating / cooling device, and a thermometer, 10 parts by mass of paraffin wax (HNP-9, manufactured by Nippon Seiro Co., Ltd.), 1 part by mass of the modified wax (d), and 33 parts by mass of ethyl acetate were added, and the mixture was heated to 78°C and stirred at the same temperature for 30 minutes. The mixture was then cooled to 30°C over one hour to crystallize the paraffin wax into fine particles, and further wet-pulverized with an Ultraviscomill (manufactured by Imex) to obtain a [release agent dispersion]. The volume average particle size of the release agent dispersion was 0.25 μm.
[0322] (Production Example 11) <Production of reactive prepolymer (α2b-1)> Into a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube, 3-methyl-1,5-pentanediol, isophthalic acid, adipic acid, and trimellitic anhydride were added together with titanium tetraisopropoxide (1,000 ppm relative to the resin component) so that the molar ratio of hydroxyl groups to carboxyl groups, OH / COOH, was 1.5, the diol component was 100 mol% 3-methyl-1,5-pentanediol, the dicarboxylic acid component was 40 mol% isophthalic acid and 60 mol% adipic acid, and the amount of trimellitic anhydride in all monomers was 1 mol%. Thereafter, the temperature was raised to 200°C over about 4 hours, and then to 230°C over 2 hours, and the reaction was continued until no water was discharged. Thereafter, the mixture was further reacted for 5 hours under a reduced pressure of 10 mmHg to 15 mmHg to obtain [intermediate polyester C-1]. Next, [intermediate polyester C-1] and isophorone diisocyanate (IPDI) were added to a reaction vessel equipped with a cooling tube, a stirrer, and a nitrogen inlet tube in a molar ratio (isocyanate group of IPDI / hydroxyl group of intermediate polyester) of 2.0, and the mixture was diluted with ethyl acetate to become a 50% ethyl acetate solution. The mixture was reacted at 100°C for 5 hours to obtain [reactive prepolymer (α2b-1)].
[0323] Example 1 <Production of Composite Resin Particles (C-1)> A beaker was charged with 165 parts by mass of ion-exchanged water, a mixture of 5 parts by mass of microparticle dispersion (W-1) and 10 parts by mass of microparticle dispersion (W0-1), 1 part by mass of sodium carboxymethylcellulose, 26 parts by mass of sodium dodecyl diphenyl ether disulfonate (Eleminol MON-7, manufactured by Sanyo Chemical Industries, Ltd.), and 15 parts by mass of ethyl acetate to obtain a mixed dispersion. Next, 71 parts by mass of the amorphous polyester resin (b-1), 40 parts by mass of the [colorant dispersion], 39 parts by mass of the [release agent dispersion], and 54 parts by mass of ethyl acetate were added to another beaker and mixed, and then 18 parts by mass of the reactive prepolymer (α2b-1) solution and 0.3 parts by mass of isophoronediamine as a curing agent (β) were further added and mixed to obtain a mixed liquid. The entire amount of this mixture was added to the dispersion prepared above, and the mixture was stirred for 2 minutes using a TK Auto Homomixer to obtain a mixture. Next, this mixture was transferred to a reaction vessel equipped with a stirrer and a thermometer, and the ethyl acetate was distilled off at 50° C. until the concentration became 0.5% by mass or less to carry out a composite process, thereby obtaining an aqueous dispersion of composite resin particles.
[0324] The aqueous dispersion of the composite resin particles is a composite resin particle in which fine particles including resin fine particles (A-1) are adhered to resin particles (B'-1) including a non-crystalline polyester resin (b-1) and a non-crystalline polyurethane resin (b-2) consisting of a reaction product of a reactive prepolymer (α2b-1) and isophoronediamine. It was confirmed that the resin particles contained in the aqueous dispersion of the composite resin particles were composite resin particles (C-1) in which fine particles containing resin fine particles (A-1) were attached to resin particles (B'-1) by magnifying and observing the shapes of the particles contained in the aqueous dispersion of the composite resin particles with an electron microscope (scanning electron microscope: SU-8230 (manufactured by Hitachi High-Technologies Corporation)).
[0325] Next, sodium hydroxide was added so that the pH of the aqueous dispersion of composite resin particles became 12, and the mixture was stirred for 1 hour with a three-one motor. After that, the mixture was centrifuged and ion-exchanged water was added again to make a reslurry. After repeating the process of centrifugal filtration and reslurrying several times, the mixture was filtered by suction using a membrane filter (hereinafter referred to as the "washing and filtering process") and dried at 40°C for 18 hours to reduce the volatile content to 0.5% by mass or less, to obtain composite resin particles (C-1).
[0326] Next, 100 parts by mass of the composite resin particles (C-1) was mixed with 1.0 part by mass of colloidal silica (Aerosil R972, manufactured by Nippon Aerosil Co., Ltd.) as an external additive in a sample mill to obtain a toner (T-1) after external additive treatment.
[0327] Example 2 <Preparation of Toner (T-2)> In Example 1, 15 parts by mass of a mixture of 5 parts by mass of microparticle dispersion (W-1) and 10 parts by mass of microparticle dispersion (W0-1) was changed to 15 parts by mass of a mixture of 7.5 parts by mass of microparticle dispersion (W-1) and 7.5 parts by mass of microparticle dispersion (W0-1), and an aqueous dispersion of composite resin particles (C-2) in which microparticles containing resin microparticles (A-2) are attached to resin particles (B'-1) was obtained in the same manner as in Example 1, except for the resin microparticles A-2. Next, the obtained aqueous dispersion was subjected to washing and filtration steps in the same manner as in Example 1, and then dried at 40° C. for 18 hours to reduce the volatile content to 0.5% by mass or less, thereby obtaining composite resin particles (C-2). Next, external addition treatment was carried out in the same manner as in Example 1 to obtain toner (T-2).
[0328] Example 3 <Preparation of toner (T-3)> In Example 1, 15 parts by mass of a mixture of 5 parts by mass of microparticle dispersion (W-1) and 10 parts by mass of microparticle dispersion (W0-1) was changed to 15 parts by mass of a mixture of 10 parts by mass of microparticle dispersion (W-1) and 5 parts by mass of microparticle dispersion (W0-1). In the same manner as in Example 1, an aqueous dispersion of composite resin particles (C-3) in which microparticles containing resin microparticles (A-3) are attached to resin particles (B'-1) was obtained. Next, the obtained aqueous dispersion was subjected to washing and filtration steps in the same manner as in Example 1, and then dried at 40° C. for 18 hours to reduce the volatile content to 0.5% by mass or less, thereby obtaining composite resin particles (C-3). Next, external addition treatment was carried out in the same manner as in Example 1 to obtain toner (T-3).
[0329] Example 4 <Preparation of toner (T-4)> In Example 1, except that 15 parts by mass of a mixture of 5 parts by mass of microparticle dispersion (W-1) and 10 parts by mass of microparticle dispersion (W0-1) was changed to 15 parts by mass of a mixture of 5 parts by mass of microparticle dispersion (W-2) and 10 parts by mass of microparticle dispersion (W0-2), an aqueous dispersion of composite resin particles (C-4) in which microparticles including resin microparticles (A-4) are attached to resin particles (B'-1) was obtained in the same manner as in Example 1. Next, the obtained aqueous dispersion was subjected to washing and filtration steps in the same manner as in Example 1, and then dried at 40° C. for 18 hours to reduce the volatile content to 0.5% by mass or less, thereby obtaining composite resin particles (C-4). Next, external addition treatment was carried out in the same manner as in Example 1 to obtain toner (T-4).
[0330] Example 5 <Preparation of toner (T-5)> In Example 1, except that 15 parts by mass of a mixture of 5 parts by mass of microparticle dispersion (W-1) and 10 parts by mass of microparticle dispersion (W0-1) was changed to 15 parts by mass of a mixture of 7.5 parts by mass of microparticle dispersion (W-2) and 7.5 parts by mass of microparticle dispersion (W0-2), an aqueous dispersion of composite resin particles (C-5) in which microparticles containing resin microparticles (A-5) are attached to resin particles (B'-1) was obtained in the same manner as in Example 1. Next, the obtained aqueous dispersion was subjected to washing and filtration steps in the same manner as in Example 1, and then dried at 40° C. for 18 hours to reduce the volatile content to 0.5% by mass or less, thereby obtaining composite resin particles (C-5). Next, external addition treatment was carried out in the same manner as in Example 1 to obtain toner (T-5).
[0331] Example 6 <Preparation of toner (T-6)> In Example 1, except that 15 parts by mass of a mixture of 5 parts by mass of microparticle dispersion (W-1) and 10 parts by mass of microparticle dispersion (W0-1) was changed to 15 parts by mass of a mixture of 10 parts by mass of microparticle dispersion (W-2) and 5 parts by mass of microparticle dispersion (W0-2), an aqueous dispersion of composite resin particles (C-6) in which microparticles including resin microparticles (A-6) are attached to resin particles (B'-1) was obtained in the same manner as in Example 1. Next, the obtained aqueous dispersion was subjected to washing and filtration steps in the same manner as in Example 1, and then dried at 40° C. for 18 hours to reduce the volatile content to 0.5% by mass or less, thereby obtaining composite resin particles (C-6). Next, external addition treatment was carried out in the same manner as in Example 1 to obtain toner (T-6).
[0332] Example 7 <Preparation of toner (T-7)> In Example 1, 15 parts by mass of a mixture of 5 parts by mass of microparticle dispersion (W-1) and 10 parts by mass of microparticle dispersion (W0-1) was changed to 15 parts by mass of a mixture of 5 parts by mass of microparticle dispersion (W-3) and 10 parts by mass of microparticle dispersion (W0-3). In the same manner as in Example 1, an aqueous dispersion of composite resin particles (C-7) in which microparticles including resin microparticles (A-7) are attached to resin particles (B'-1) was obtained. Next, the obtained aqueous dispersion was subjected to washing and filtration steps in the same manner as in Example 1, and then dried at 40° C. for 18 hours to reduce the volatile content to 0.5% by mass or less, thereby obtaining composite resin particles (C-7). Next, external addition treatment was carried out in the same manner as in Example 1 to obtain toner (T-7).
[0333] Example 8 <Preparation of toner (T-8)> In Example 1, except that 15 parts by mass of a mixture of 5 parts by mass of microparticle dispersion (W-1) and 10 parts by mass of microparticle dispersion (W0-1) was changed to 15 parts by mass of a mixture of 7.5 parts by mass of microparticle dispersion (W-3) and 7.5 parts by mass of microparticle dispersion (W0-3), an aqueous dispersion of composite resin particles (C-8) in which microparticles containing resin microparticles (A-8) are attached to resin particles (B'-1) was obtained in the same manner as in Example 1. Next, the obtained aqueous dispersion was subjected to washing and filtration steps in the same manner as in Example 1, and then dried at 40° C. for 18 hours to reduce the volatile content to 0.5% by mass or less, thereby obtaining composite resin particles (C-8). Next, external addition treatment was carried out in the same manner as in Example 1 to obtain toner (T-8).
[0334] Example 9 <Preparation of Toner (T-9)> In Example 1, except that 15 parts by mass of a mixture of 5 parts by mass of microparticle dispersion (W-1) and 10 parts by mass of microparticle dispersion (W0-1) was changed to 15 parts by mass of a mixture of 10 parts by mass of microparticle dispersion (W-3) and 5 parts by mass of microparticle dispersion (W0-3), an aqueous dispersion of composite resin particles (C-9) in which microparticles including resin microparticles (A-9) are attached to resin particles (B'-1) was obtained in the same manner as in Example 1. Next, the obtained aqueous dispersion was subjected to washing and filtration steps in the same manner as in Example 1, and then dried at 40° C. for 18 hours to reduce the volatile content to 0.5% by mass or less, thereby obtaining composite resin particles (C-9). Next, external addition treatment was carried out in the same manner as in Example 1 to obtain toner (T-9).
[0335] Example 10 <Preparation of toner (T-10)> In Example 1, an aqueous dispersion of composite resin particles (C-10) in which fine particles containing resin fine particles (A-10) are attached to resin particles (B'-1) was obtained in the same manner as in Example 1, except that the amount of resin fine particles added was reduced. Next, the obtained aqueous dispersion was subjected to washing and filtration steps in the same manner as in Example 1, and then dried at 40° C. for 18 hours to reduce the volatile content to 0.5% by mass or less, thereby obtaining composite resin particles (C-10). Next, the external addition treatment was carried out in the same manner as in Example 1 to obtain a toner (T-10).
[0336] Example 11 <Preparation of toner (T-11)> In Example 1, an aqueous dispersion of composite resin particles (C-11) in which fine particles containing resin fine particles (A-11) are attached to resin particles (B'-1) was obtained in the same manner as in Example 1, except that the amount of resin fine particles added was increased. Next, the obtained aqueous dispersion was subjected to washing and filtration steps in the same manner as in Example 1, and then dried at 40° C. for 18 hours to reduce the volatile content to 0.5% by mass or less, thereby obtaining composite resin particles (C-11). Next, external addition treatment was carried out in the same manner as in Example 1 to obtain toner (T-11).
[0337] Example 12 <Preparation of toner (T-12)> In Example 1, the same procedure as in Example 1 was repeated to obtain an aqueous dispersion of composite resin particles (C-12) in which fine particles containing resin fine particles (A-12) adhere to resin particles (B'-1), except that the amount of styrene in the production of the aqueous dispersion (W-1) of resin fine particles (A-1) was changed to 50.3 parts by mass. Next, the obtained aqueous dispersion was subjected to washing and filtration steps in the same manner as in Example 1, and then dried at 40° C. for 18 hours to reduce the volatile content to 0.5% by mass or less, thereby obtaining composite resin particles (C-12). Next, the external addition treatment was carried out in the same manner as in Example 1 to obtain a toner (T-12).
[0338] Example 13 <Preparation of toner (T-13)> In Example 1, in the production of the aqueous dispersion (W-1) of resin microparticles (A-1), the amount of styrene was changed to 37.5 parts by mass, and the amount of microparticle dispersion (W-1) was changed to 15 parts by mass and the amount of microparticle dispersion (W0-1) was changed to 5 parts by mass. In the same manner as in Example 1, an aqueous dispersion of composite resin particles (C-13) in which microparticles containing resin microparticles (A-13) are attached to resin particles (B'-1) was obtained. Next, the obtained aqueous dispersion was subjected to washing and filtration steps in the same manner as in Example 1, and then dried at 40° C. for 18 hours to reduce the volatile content to 0.5% by mass or less, thereby obtaining composite resin particles (C-13). Next, external addition treatment was carried out in the same manner as in Example 1 to obtain a toner (T-13).
[0339] Example 14 <Preparation of toner (T-14)> In Example 1, the production of the aqueous dispersion (W-1) of resin microparticles (A-1) was changed to 50.5 parts by mass of styrene, and the amounts of microparticle dispersion (W-1) and microparticle dispersion (W0-1) were changed to 5 parts by mass. In the same manner as in Example 1, an aqueous dispersion of composite resin particles (C-14) in which microparticles containing resin microparticles (A-14) are attached to resin particles (B'-1) was obtained. Next, the obtained aqueous dispersion was subjected to washing and filtration steps in the same manner as in Example 1, and then dried at 40° C. for 18 hours to reduce the volatile content to 0.5% by mass or less, thereby obtaining composite resin particles (C-14). Next, the external addition treatment was carried out in the same manner as in Example 1 to obtain a toner (T-14).
[0340] Example 15 <Preparation of toner (T-15)> In Example 1, the production of the aqueous dispersion (W-1) of resin microparticles (A-1) was changed to 50.5 parts by mass of styrene, and the amounts of microparticle dispersion (W-1) and microparticle dispersion (W0-1) were changed to 5 parts by mass. In the same manner as in Example 1, an aqueous dispersion of composite resin particles (C-15) in which microparticles containing resin microparticles (A-15) are attached to resin particles (B'-1) was obtained. Next, the obtained aqueous dispersion was subjected to washing and filtration steps in the same manner as in Example 1, and then dried at 40° C. for 18 hours to reduce the volatile content to 0.5% by mass or less, thereby obtaining composite resin particles (C-15). Next, external addition treatment was carried out in the same manner as in Example 1 to obtain a toner (T-15).
[0341] (Example 16) <Preparation of toner (T-16)> In Example 1, except for changing the amount of reactive prepolymer (α2b-1) solution to 3 parts by mass, the same procedure as in Example 1 was repeated to obtain an aqueous dispersion of composite resin particles (C-16) in which microparticles containing resin microparticles (A-16) were attached to resin particles (B'-1). Next, the obtained aqueous dispersion was subjected to washing and filtration steps in the same manner as in Example 1, and then dried at 40° C. for 18 hours to reduce the volatile content to 0.5% by mass or less, thereby obtaining composite resin particles (C-16). Next, external addition treatment was carried out in the same manner as in Example 1 to obtain a toner (T-16).
[0342] Comparative Example 1 <Preparation of Toner (T'-1)> In Example 1, except that 15 parts by mass of a mixture of 5 parts by mass of microparticle dispersion (W-1) and 10 parts by mass of microparticle dispersion (W0-1) was changed to 15 parts by mass of microparticle dispersion (W0-2), an aqueous dispersion of composite resin particles (C'-1) in which microparticles containing resin microparticles (A'-1) adhere to resin particles (B'-1) was obtained in the same manner as in Example 1. Next, the obtained aqueous dispersion was subjected to washing and filtration steps in the same manner as in Example 1, and then dried at 40° C. for 18 hours to reduce the volatile content to 0.5 mass % or less, thereby obtaining composite resin particles (C'-1). Next, external addition treatment was carried out in the same manner as in Example 1 to obtain toner (T'-1).
[0343] Comparative Example 2 <Preparation of Toner (T'-2)> In Example 1, except that 15 parts by mass of a mixture of 5 parts by mass of microparticle dispersion (W-1) and 10 parts by mass of microparticle dispersion (W0-1) was changed to 15 parts by mass of microparticle dispersion (W0-2), an aqueous dispersion of composite resin particles (C'-2) in which microparticles containing resin microparticles (A'-2) adhere to resin particles (B'-1) was obtained in the same manner as in Example 1. Next, the obtained aqueous dispersion was subjected to washing and filtration steps in the same manner as in Example 1, and then dried at 40° C. for 18 hours to reduce the volatile content to 0.5 mass % or less, thereby obtaining composite resin particles (C'-2). Next, external addition treatment was carried out in the same manner as in Example 1 to obtain toner (T'-2).
[0344] Comparative Example 3 <Preparation of Toner (T'-3)> In Example 1, 15 parts by mass of a mixture of 5 parts by mass of microparticle dispersion (W-1) and 10 parts by mass of microparticle dispersion (W0-1) was changed to 15 parts by mass of a mixture of 3 parts by mass of microparticle dispersion (W-1) and 12 parts by mass of microparticle dispersion (W0-1). In the same manner as in Example 1, an aqueous dispersion of composite resin particles (C'-3) in which microparticles containing resin microparticles (A'-3) are attached to resin particles (B'-1) was obtained. Next, the obtained aqueous dispersion was subjected to washing and filtration steps in the same manner as in Example 1, and then dried at 40° C. for 18 hours to reduce the volatile content to 0.5 mass % or less, thereby obtaining composite resin particles (C'-3). Next, external addition treatment was carried out in the same manner as in Example 1 to obtain toner (T'-3).
[0345] Comparative Example 4 <Preparation of Toner (T'-4)> In Example 1, except that 15 parts by mass of a mixture of 5 parts by mass of microparticle dispersion (W-1) and 10 parts by mass of microparticle dispersion (W0-1) was changed to 15 parts by mass of a mixture of 2.5 parts by mass of microparticle dispersion (W-3) and 12.5 parts by mass of microparticle dispersion (W0-3), an aqueous dispersion of composite resin particles (C'-4) in which microparticles containing resin microparticles (A'-4) are attached to resin particles (B'-1) was obtained in the same manner as in Example 1. Next, the obtained aqueous dispersion was subjected to washing and filtration steps in the same manner as in Example 1, and then dried at 40° C. for 18 hours to reduce the volatile content to 0.5 mass % or less, thereby obtaining composite resin particles (C'-4). Next, external addition treatment was carried out in the same manner as in Example 1 to obtain toner (T'-4).
[0346] (Creating the carrier) To 100 parts by mass of toluene, 100 parts by mass of silicone resin (organo straight silicone), 5 parts by mass of γ-(2-aminoethyl)aminopropyltrimethoxysilane, and 10 parts by mass of carbon black were added, and dispersed for 20 minutes using a homomixer to prepare a resin layer coating liquid. Using a fluidized bed type coating device, the resin layer coating liquid was applied to the surface of 1,000 parts by mass of spherical magnetite having a volume average particle size of 50 μm to prepare a [carrier].
[0347] (Preparation of developer) Using a ball mill, 5 parts by weight of each of the toners and 95 parts by weight of the carrier were mixed to prepare each of the developers.
[0348] (measurement) Next, the Tg1st of each toner, the Tga1st of the THF insoluble matter, the distance between the resin particles, the storage modulus of the toner, the glass transition temperature TgA of the shell portion, and the glass transition temperature TgB of the core portion were measured as follows. The results are shown in Tables 3 to 6.
[0349] <Measurement of toner Tg1st and Tga1st of THF insoluble matter> 1 g of toner was put into 100 mL of THF, and Soxhlet extraction was performed to obtain THF soluble and insoluble fractions. This was dried in a vacuum dryer for 24 hours, and polyester resin component A was obtained from the THF soluble fraction, and polyester resin component C was obtained from the THF insoluble fraction. These were used as the target samples. In addition, the toner was used as the target sample when measuring the toner Tg1st. Note that, here, the above-mentioned non-crystalline polyester (b-1) is considered to be polyester resin component A, and the above-mentioned reactive prepolymer (α2b-1) is considered to be polyester resin component C.
[0350] Next, 5.0 mg of the target sample was placed in an aluminum sample container, the sample container was placed on a holder unit, and set in an electric furnace. Next, under a nitrogen atmosphere, the sample was heated from -80°C to 150°C at a heating rate of 1.0°C / min (first heating). After that, the sample was cooled from 150°C to -80°C at a heating rate of 1.0°C / min, and further heated to 150°C at a heating rate of 1.0°C / min (second heating). In each of the first and second heating, a DSC curve was measured using a differential scanning calorimeter ("Q-200", manufactured by TA Instruments).
[0351] From the obtained DSC curves, the DSC curve at the first heating was selected using the analysis program in the Q-200 system, and the glass transition temperature Tg1st at the first heating of the target sample was determined.
[0352] For the toner components insoluble in THF, the toner was heated from -80°C to 150°C at a temperature rise rate of 1.0°C / min while applying a modulation temperature amplitude of ±1.0°C / min using the modulation mode (first temperature rise). The obtained DSC curve was obtained by plotting "Reversing Heat Flow" on the vertical axis using the analysis program in the Q-200 system in the same manner as above, and the onset value was taken as Tg. This allowed the Tga1st to be calculated.
[0353] <Measurement of distance between resin particles> Next, for each of the obtained toners, the external additives were removed as much as possible by a process for liberating the external additives using ultrasonic waves in the following manner, to bring the toner particles closer to the toner base particles, and the average value and standard deviation of the distance between the resin particles were calculated.
[0354] -How to separate external additives- [1] 50 ml of a 5% by weight aqueous solution containing a surfactant (product name: Noigen ET-165, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) was added to a 100 ml screw tube, and 3 g of toner was added to the mixture and gently moved up and down and left and right. After that, the mixture was stirred for 30 minutes in a ball mill so that the toner was mixed into the dispersion solution.
[0355] [2] Then, using an ultrasonic homogenizer (product name homogenizer, model VCX750, CV33, manufactured by SONICS & MATERIALS LLC), the output was set to 40 W and ultrasonic energy was applied for 60 minutes.
[0356] [Ultrasonic conditions] Vibration time: 60 minutes continuous ·Amplitude: 40W ·Vibration start temperature: 23±1.5℃ ·Temperature during vibration: 23±1.5℃
[0357] [3](1) The dispersion liquid was suction filtered using filter paper (product name: Qualitative Filter Paper (No. 2, 110 mm), manufactured by Advantec Toyo Co., Ltd.), washed twice again with ion-exchanged water, filtered, and the liberated additives were removed, and the toner particles were then dried. (2) The toner obtained in (1) was observed with a scanning electron microscope (SEM). First, external additives and fillers containing Si were detected by observing the backscattered electron image. (3) The image of (1) was binarized using image processing software (ImageJ) to remove the external additives and fillers. Next, a secondary electron image was observed at the same position as in (1). Since the resin fine particles are not observed in the reflected electron image but only in the secondary electron image, the image was compared with the image obtained in (3), and the fine particles present in the areas other than the remaining external additives and filler (areas other than those removed in (3)) were determined to be resin fine particles, and the distance between the resin fine particles (the distance connecting the centers of the particles) was measured using the image processing software. This measurement was carried out for 100 binarized images (one toner particle per image), and the average value was taken as the average value of the distance between the resin particles. The standard deviation of the distance between the resin fine particles was calculated by the following formula, where the interparticle distance is x.
[0358]
number
[0359] [Shooting conditions] Scanning electron microscope: SU-8230 (Hitachi High-Technologies Corporation) Magnification: 35,000x Image capture: SE(L): Secondary electrons, BSE (backscattered electrons) Acceleration voltage: 2.0kV ·Acceleration current: 1.0μA ·Probe current:Normal Focus mode: UHR WD:8.0mm
[0360] <Measurement of storage modulus of toner> Pellets were prepared as follows, and the storage modulus of the toner was measured. [Pellet preparation conditions] The measurement sample is prepared by pressurizing the toner into a disk shape having a diameter of 8.0 mm±0.3 mm and a thickness of 1.0 mm±0.3 mm using a tablet molding machine in an environment of 25° C. [Measurement conditions] Rotating disk rheometer: ARES-G2 Manufacturer: TA Instruments The sample is attached to a parallel plate with a diameter of 8.0 mm and stabilized at 40°C. Then, the temperature is raised to 200°C at 2.0°C / min with a frequency of 10 Hz (6.28 rad / s) and a strain of 0.1% (strain control mode).
[0361] <Glass transition temperature TgA of the shell and glass transition temperature TgB of the core> As described above, the glass transition temperature TgA of the shell portion was determined by drying a part of the microparticle dispersion (W0) to isolate the resin (a-1) and determining the glass transition temperature of the resin component. The glass transition temperature TgB of the core portion was measured by drying up the microparticle dispersion (W0) to extract the resin microparticles, and then removing the shell portion with an organic solvent or by heating to separate only the core portion.
[0362] (evaluation) Next, the toners (T-1) to (T-16), and (T'-1) to (T'-4) and the developer were evaluated for "low-temperature fixability," "heat-resistant storage stability," "cleanability," and "contamination of the blade and photoreceptor" as follows. The results are shown in Tables 7 to 9.
[0363] <Low temperature fixability> Each toner is applied on the paper at 0.8 mg / cm 2The powder was evenly placed on the paper surface using a printer with the heat fixing unit removed. Other methods may be used as long as the powder can be evenly placed at the weight density described above. The paper was then placed on the pressure roller at a fixing speed (heat roller peripheral speed) of 213 mm / sec and a fixing pressure (pressure roller pressure) of 10 kg / cm. 2 The temperature at which cold offset occurs (MFT) was measured when the sheet was passed through the above conditions. The lower the temperature at which cold offset occurs, the better the low-temperature fixing ability.
[0364] [Cold offset evaluation criteria] ◎: Minimum fixing temperature is 130℃ or less ○: The minimum fixing temperature is greater than 130°C and less than or equal to 135°C. △: The minimum fixing temperature is greater than 135°C and less than 140°C ×: The minimum fixing temperature is higher than 140° C.
[0365] <Heat-resistant storage stability> After storing each toner at 50°C for 8 hours, it was sieved through a 42 mesh sieve for 2 minutes, the residual ratio on the wire mesh was measured, and the heat-resistant storage stability was evaluated according to the following criteria. Note that the better the heat-resistant storage stability of the toner, the smaller the residual ratio.
[0366] [Evaluation Criteria] ◎: Residual rate is less than 5% ○: Residual rate is 5% or more and less than 15% △: Residual rate is between 15% and 30% ×: Residual rate is 30% or more
[0367] <Cleaning ability (photoreceptor contamination)> Using an image forming apparatus (imageo MP C5002, manufactured by Ricoh Co., Ltd.), 50,000 sheets (A4 size landscape) of a 5% image area ratio chart were output at 3 prints / job in a laboratory environment of 21°C and 65% RH, and the 50,000 sheets were passed through as follows. The apparatus configuration was as shown in Figure 5. Thereafter, in a laboratory environment of 32°C and 54% RH, 100 sheets of A4 size landscape printouts of 3 charts with a vertical band pattern width of 43 mm (relative to the paper travel direction) were printed as evaluation images, and the resulting images were visually observed. The cleaning performance was evaluated based on the following criteria, depending on whether or not there were any image abnormalities due to poor cleaning.
[0368] [Evaluation Criteria] ⊚: Toner that has slipped through due to poor cleaning cannot be visually confirmed on either the printed paper or the photoconductor, and no streaks of toner can be confirmed even when observing the photoconductor in the longitudinal direction with a microscope. ◯: The toner that has slipped through due to poor cleaning cannot be visually confirmed on the printed paper or on the photoconductor. ×: Toner that has slipped through due to poor cleaning can be visually confirmed on the printed paper and on the photoconductor.
[0369] <Blade contamination> Using an image forming device (imageo MP C5002, manufactured by Ricoh Co., Ltd.), 5,000 sheets (A4 size horizontal) of a vertical band chart with an image area ratio of 30% were output at 3 prints / job in a laboratory environment of 27°C and 90% RH. Next, 5,000 sheets (A4 size horizontal) of blank paper were output at 3 prints / job, and then one halftone image was printed. The blade (cleaning blade) and photoconductor were visually observed to evaluate blade contamination. The evaluation criteria are as follows:
[0370] [Evaluation Criteria] ◎: No contamination on the photoconductor and blade. No quality issues. ○: There is a thin layer of toner on either the photoconductor or the blade, but the image is not of a quality that is of concern. ×: Toner adhesion is clearly observed on both the photoconductor and blade, and there is a problem with the image quality.
[0371] <Overall Judgment> The four evaluation results of "low-temperature fixability," "heat-resistant storage stability," "cleanability," and "blade contamination" were comprehensively judged based on the following criteria.
[0372] [Evaluation Criteria] 〇: One or more ◎ and no △ or × △: No △ or × ×: △ or ×
[0373] [Table 3]
[0374] [Table 4]
[0375] [Table 5]
[0376] [Table 6]
[0377] [Table 7]
[0378] [Table 8]
[0379] [Table 9]
[0380] From the above results, it can be seen that Examples 1 to 16 gave superior results compared to Comparative Examples 1 to 4. In contrast, the toner (T'-1) of Comparative Example 1, which uses composite resin particles (A'-1) consisting only of resin microparticles (B-2), had good low-temperature fixing properties and resistance to filming due to external additives, but had poor cleaning properties and heat-resistant storage stability. In addition, the toner (T'-2) of Comparative Example 2, which uses composite resin particles (A'-1) consisting only of resin microparticles (B-2) and (A'-2) that have not been subjected to a washing process, has good heat-resistant storage properties and cleaning properties but poor low-temperature fixing properties and resistance to filming due to external additives. In addition, the toner (T'-3) of Comparative Example 3, which uses composite resin particles (A'-3) with a reduced ratio of resin microparticles (A-1), and the toner (T'-4) of Comparative Example 4, which uses composite resin particles (A'-4) with a reduced ratio of resin microparticles (A-3), have good low-temperature fixing properties, but are poor in heat-resistant storage stability, cleaning properties, and resistance to filming due to additives. [Explanation of symbols]
[0381] 10 Photoconductor drum 40 Developer 58 Corona charger 80 Transfer roller 90 Cleaning Equipment 110 Process cartridge 210 Paper feed section 211 Paper feed cassette 212 Paper feed roller 220 Conveyor 221 Lola 222 Timing roller 223 Paper ejection roller 224 Paper output tray 230 Image creation section 233 Exposure device 240 Transcription Unit 241 Drive roller 242 Driven roller 243 Intermediate transfer belt 244 Primary transfer roller 245 Secondary opposing roller 246 Secondary transfer roller 250 Fixing unit 251 Fixing belt 252 Pressure roller [Prior art documents] [Patent documents]
[0382] [Patent Document 1] JP 2002-284881 A [Patent Document 2] JP 2019-099809 A [Patent Document 3] JP 2019-143128 A [Patent Document 4] JP 2007-233030 A
Claims
1. A toner in which the surface of a toner base particle containing a binder resin, a colorant and a wax is coated with resin fine particles, The resin fine particles have a core-shell structure consisting of a shell portion and a core portion, the glass transition temperature TgA of the shell portion is higher than the glass transition temperature TgB of the core portion; When the toner was measured with a rheometer, the storage modulus G′1 at 70° C. during heating was 1.0×10 5 Pa or more 1.0×10 6 Pa or less, and the storage modulus G'2 at 100°C during heating is 1.0 x 10 4 Pa or more 5.0×10 4 Pa or less, The toner comprises a reaction product of a polyester prepolymer having an isocyanate group, The polyester prepolymer has a structure obtained by polycondensation of a polyol and a polycarboxylic acid, The toner is characterized in that the polyol contains a chain alkylene glycol having 2 to 12 carbon atoms.
2. 2. The toner according to claim 1, wherein the coverage of the resin particles is 30% or more and 90% or less.
3. 3. The toner according to claim 2, wherein the coverage of the resin particles is 30% or more and 70% or less.
4. 4. The toner according to claim 1, wherein a glass transition temperature TgA of the shell portion and a glass transition temperature TgB of the core portion of the resin fine particles satisfy the relationship TgA-TgB≧10° C.
5. 5. The toner according to claim 1, wherein the shell and the core of the resin particles contain a styrene-acrylic resin.
6. 6. The toner according to claim 1, wherein the resin fine particles have a volume average primary particle diameter of 10 nm or more and 100 nm or less.
7. 7. The toner according to claim 1, wherein the resin fine particles have a glass transition temperature Tg of 40° C. or more and 70° C. or less.
8. 8. The toner according to claim 1, wherein the standard deviation of the distance between adjacent resin particles present on the surface of the toner base particle is 500 nm or less.
9. the toner has a glass transition temperature Tg1st at the first temperature rise in differential scanning calorimetry (DSC) of 20° C. or higher and 50° C. or lower; 9. The toner according to claim 1, wherein the component of the toner insoluble in tetrahydrofuran (THF) has a glass transition temperature Tga1st in a first DSC temperature rise of -40° C. or more and 10° C. or less.
10. A developer comprising the toner according to any one of claims 1 to 9.
11. A toner storage unit, comprising the toner according to any one of claims 1 to 9 stored therein.
12. An electrostatic latent image carrier; an electrostatic latent image forming means for forming an electrostatic latent image on the electrostatic latent image bearing member; a developing means for developing the electrostatic latent image with a toner to form a visible image; a transfer means for transferring the visible image onto a recording medium; A fixing means for fixing the transferred image on the recording medium; a cleaning means for cleaning the electrostatic latent image carrier; 10. An image forming apparatus, comprising the toner according to claim 1.
13. an electrostatic latent image forming step of forming an electrostatic latent image on an electrostatic latent image carrier; a developing step of developing the electrostatic latent image with a toner to form a visible image; a transfer step of transferring the visible image onto a recording medium; a fixing step of fixing the transferred image on the recording medium; a cleaning step of cleaning the electrostatic latent image carrier, 10. An image forming method, comprising the toner according to claim 1.
Citation Information
Patent Citations
Resin dispersion having uniform particle size, resin particle and their manufacturing method
JP2002284881A
Toner and method for manufacturing the same, and developer, toner-containing vessel, process cartridge, image forming apparatus and image forming method
JP2005055498A
Toner for electrostatic charge image development
JP2007233030A
Manufacturing method of composite resin particle
JP2019099809A
Composite resin particle
JP2019143128A