Epoxy composition, composition for electronic components, material for electronic components

By adding a vertical alignment agent to an epoxy compound composition, the molecular orientation is stabilized, enhancing thermal conductivity for effective heat dissipation in electronic components.

JP7582041B2Active Publication Date: 2024-11-13JNC CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021070936
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-04-20
Publication Date
2024-11-13
Estimated Expiration
2041-04-20

AI Technical Summary

Technical Problem

Existing epoxy materials with high thermal conductivity struggle to maintain molecular orientation perpendicular to the substrate under varying environmental conditions, limiting their effectiveness in heat dissipation applications.

Method used

Incorporating a vertical alignment agent with a hydrocarbon structure and a hydroxyl or carboxy group into an epoxy compound composition, along with a curing agent, to stabilize molecular orientation and enhance thermal conductivity.

Benefits of technology

The composition achieves stable vertical molecular alignment, resulting in high thermal conductivity suitable for heat dissipation materials, particularly in electronic components like IGBTs and semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582041000047
    Figure 0007582041000047
  • Figure 0007582041000048
    Figure 0007582041000048
  • Figure 0007582041000001
    Figure 0007582041000001
Patent Text Reader

Abstract

To provide an epoxy material where the molecules are vertically aligned with respect to a substrate and which has high heat conductivity, and to provide a composition which stably imparts such a material in various environments.SOLUTION: A composition comprises an epoxy compound, exhibits mesomorphism, and further comprises a vertically aligning agent. A cured product is made by curing the composition. An electronic component uses the cured product. The vertically aligning agent comprises, for example, a compound with a structure represented by the formula (1). In the formula (1), R1 is a hydrogen or a 1-20C alkyl group or the like; each of A1, A2, and A3 is independently a single bond, a cyclohexane, a cyclohexene, or a phenylene or the like; m is 0 to 3; and each of Xs is independently a single bond, a -CH2CH2-, or the like.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composition for heat dissipation members that efficiently conducts heat generated inside electronic devices, and to a polymerizable composition having liquid crystallinity used therein. [Background technology]

[0002] In recent years, there has been a demand for packaging materials with high thermal conductivity to prevent the temperature of the internal semiconductors from becoming too high in semiconductor elements for power control in hybrid and electric vehicles, CPUs for high-speed computers, etc. In other words, the ability to efficiently dissipate heat generated by semiconductor chips to the outside has become important.

[0003] One method for solving this heat dissipation problem is to bring a highly thermally conductive material (heat dissipation component) into contact with the heat-generating area, leading the heat to the outside and dissipating it. Examples of materials with high thermal conductivity include inorganic materials such as metals and metal oxides. However, these inorganic materials have problems with processability and insulation, making it very difficult to use them alone as a filler for semiconductor packages. For this reason, development is underway to create heat dissipation components with high thermal conductivity by combining these inorganic materials with resins.

[0004] In general, the thermal conductivity of composite materials has been increased by adding a large amount of inorganic fillers, such as metal fillers, to general-purpose resins, such as polyethylene resin, polyamide resin, polystyrene resin, acrylic resin, and epoxy resin. However, the thermal conductivity of inorganic fillers is a value specific to the material and has a set upper limit. Therefore, methods for increasing the thermal conductivity of the resin to achieve this have been widely attempted. As a means for actually achieving this, for example, a method of using an epoxy compound that exhibits liquid crystallinity and controlling the molecular orientation is known (Patent Document 1).

[0005] Non-Patent Document 1 discloses an epoxy material in which the molecules are oriented vertically to the substrate by setting the surface tension of the substrate to a certain value or more. By orienting the molecules vertically, the thermal conductivity in that direction is improved. However, there was a need for a liquid crystal material that would be more stably oriented vertically when the environment or conditions of material production change, such as when a substrate with a different surface tension is used. [Prior art documents] [Non-patent literature]

[0006] [Non-Patent Document 1] ACS Omega, 3, 3562(2018). [Patent documents]

[0007] [Patent Document 1] International Publication No. WO2016 / 190260 Summary of the Invention [Problem to be solved by the invention]

[0008] The object of the present invention is to provide an epoxy material having high thermal conductivity in which the molecules are oriented perpendicular to the substrate, and further to provide a composition that can provide such a material stably under various environments. [Means for solving the problem]

[0009] The present inventors have found that the above problems can be solved by adding a vertical alignment agent to a composition containing an epoxy compound, and have completed the inventions described in the following items [1] to

[18] .

[0010] [1] A composition containing an epoxy compound, the composition exhibiting liquid crystallinity, and further containing a vertical alignment agent.

[0011] [2] The composition according to item [1], further comprising a curing agent.

[0012] [3] The composition according to item [1] or [2], wherein the vertical alignment agent contains a compound having a hydrocarbon structure having 10 to 50 carbon atoms and having a hydroxyl group, amino group, or carboxy group at one end of the structure.

[0013] [4] The composition according to item [3], wherein the vertical alignment agent contains a compound having a structure represented by the following formula (1):

[0014] TIFF0007582041000001.tif1294

[0015] In formula (1), R 1 is hydrogen or alkyl having 1 to 20 carbon atoms, in which non-adjacent -CH2- in this alkyl may be substituted with -O-, and hydrogen in this alkyl may be substituted with fluorine, A 1 , A 2 , and A 3 are independently a single bond, cyclohexane, cyclohexene, or phenylene, and hydrogen on the phenylene may be replaced by CH3, OH, and NH2; m is 0 to 3; X is independently a single bond, -CH2CH2-, -CH2O-, -CH=CH-, -C≡C-, or -COO-.

[0016] [5] The composition according to item [4], wherein the vertical alignment agent contains a compound having a structure represented by the following formula (1-1):

[0017] TIFF0007582041000002.tif31122

[0018] In formula (1-1), R 1 is hydrogen or alkyl having 1 to 20 carbon atoms, in which non-adjacent -CH2- in this alkyl may be substituted with -O-, and hydrogen in this alkyl may be substituted with fluorine, A 11 and A 12are independently cyclohexane, cyclohexene, or phenylene, and hydrogen on the phenylene may be replaced by CH3; m1 is 0 to 2, X is independently a single bond, -CH2CH2-, -CH2O-, -CH=CH-, -C≡C-, or -COO-.

[0019] [6] The composition according to any one of [1] to [5], wherein the epoxy compound comprises a compound having a structure represented by formula (2).

[0020] TIFF0007582041000003.tif31133

[0021] In formula (1), R ep are independently a group having 2 to 12 carbon atoms and having an oxiranyl group, X is independently a single bond, -CH2CH2-, -CHO-, -CH=CH-, -C≡C-, or -COO-, A 3 is 1,4-phenylene, 1,4-cyclohexenylene, or 1,4-cyclohexylene; R 2 are independently hydrogen, fluorine, alkyl having 1 to 8 carbon atoms, alkoxy having 1 to 8 carbon atoms, or R ep wherein at least one -CH2- of these alkyl and alkoxy may be replaced by -C(=O)-, and n is 0 to 2.

[0022] [7] The composition according to item [6], wherein in the epoxy compound represented by formula (2), X is a single bond or -C≡C-.

[0023] [8] The composition according to any one of [2] to [7], wherein the curing agent is a phenol having two or more -OH groups in its molecular skeleton, or a compound in which the phenol is esterified.

[0024] [9] The composition according to item [8], wherein the curing agent is at least one compound represented by formulas (3-1) to (3-6) or an esterified compound of said compound.

[0025] TIFF0007582041000004.tif42115

[0026] TIFF0007582041000005.tif56148

[0027] TIFF0007582041000006.tif10297

[0028] In formula (3-1), Ring B is benzene, naphthalene, anthracene, fluorene, or 9,9-diphenylfluorene, and in these rings B, at least one hydrogen may be replaced by alkyl having 1 to 3 carbon atoms or alkoxy having 1 to 3 carbon atoms; n31 is an integer between 2 and 4 inclusive. In formula (3-2), n32 and n33 are independently an integer of 1 to 3; Z 30 is a single bond, an alkylene having 1 to 10 carbon atoms, -CH(CH3)-, -C(CH3)2-, -C(CF3)2-, -O-, -S-, or -SO2-, At least one hydrogen atom on the benzene ring may be replaced by an alkyl group having 1 to 3 carbon atoms or an alkenyl group having 2 to 3 carbon atoms; In formula (3-3) and formula (3-4), n34 is an integer of 1 or more and 5000 or less, n35 and n36 are independently 0 or 1, and when n34 is 2 or more, they may be different for each repeat; R 10 and R 11 are independently 1,4-phenylene, 4,4'-biphenylene, or cyclopentadienylene; In formula (3-5), n34 is an integer between 1 and 5000, In formula (3-6), Z 31 is independently a single bond, -CH(CH3)-, or -C(CH3)2-, and n34 is an integer of 1 or more and 5000 or less. In addition, at least one hydrogen atom on the aromatic ring in these formulas (3-3) to (3-6) may be replaced by methyl.

[0029]

[10] The composition according to any one of [2] to [7], wherein the curing agent is an aromatic primary amine, an aliphatic primary amine, an aromatic amine having two or more secondary amino groups in its molecular skeleton, or an aliphatic amine having two or more secondary amino groups in its molecular skeleton.

[0030]

[11] The composition according to item

[10] , wherein the curing agent is at least one compound represented by formula (4-1) or (4-2). EZ-(LZ)nE (4-1) L 1 -ZE (4-2) In formulas (4-1) and (4-2), L is independently a single bond, cyclohexylene, phenylene, or naphthalene, and at least one hydrogen atom in the ring may be replaced by an alkyl group having 1 to 10 carbon atoms; L 1 is hydrogen, cyclohexyl, phenyl, or naphthyl, and at least one hydrogen in these rings may be replaced by alkyl having 1 to 10 carbon atoms; Z is independently a single bond, -O-, -NH-, -S-, -SO2-, -CO2-, or an alkylene having 1 to 12 carbon atoms; E is independently amino, alkylamino having 1 to 10 carbon atoms, hydroxyl group, or carboxy, and at least one E is amino or alkylamino having 1 to 10 carbon atoms; n is an integer from 0 to 7.

[0031]

[12] The composition according to any one of [2] to [7], wherein the curing agent is a compound containing a cyanate ester.

[0032]

[13] The composition according to any one of [2] to [7], wherein the curing agent is a compound containing a carboxylic acid, a carboxylic acid ester, an acid anhydride, or a thiol.

[0033]

[14] The composition according to any one of [1] to

[13] , further comprising an inorganic filler.

[0034]

[15] The composition according to item

[14] , wherein the inorganic filler is aluminum oxide or boron nitride.

[0035]

[16] A cured product obtained by curing the composition described in any one of items [1] to

[15] .

[0036]

[17] An electronic component using the cured product described in

[16] .

[0037]

[18] A compound represented by formula (1-3).

[0038] TIFF0007582041000007.tif24115

[0039] In formula (1-3), R 3 is hydrogen, alkyl having 1 to 12 carbon atoms, and X 3 are independently a single bond, -CH2CH2-, -CH2O-, or -C≡C-. Effect of the Invention

[0040] The composition of the present invention exhibits liquid crystallinity, and when cured, it gives an epoxy material in which the molecular skeleton is vertically oriented under various substrates and material preparation conditions. Therefore, it has high thermal conductivity. Therefore, such an epoxy material can be suitably used as a heat dissipation material for power semiconductors, etc. [Brief description of the drawings]

[0041] [Figure 1] 1 is a polarizing microscope photograph of a cured product on a glass substrate in [Example 8]. [Diagram 2] 1 is a polarizing microscope photograph of a cured product on a glass substrate in [Comparative Example 4]. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0042] Hereinafter, an embodiment of the present invention will be described in detail. However, the present invention is not limited to the embodiment.

[0043] In the present invention, the phrase "at least one hydrogen atom in the ring may be replaced by an alkyl group having 1 to 10 carbon atoms" means, for example, an embodiment in which at least one hydrogen atom at the 2-, 3-, 5- and 6-positions of 1,4-phenylene is replaced by a substituent such as methyl. "Compound (1)" means a compound represented by formula (1), and may also mean at least one compound represented by formula (1).

[0044] In this specification, the composition is a mixture containing an epoxy compound, which gives a polymerized product by reaction with heating or the like. For example, it is a mixture of an epoxy compound and a thermal acid generator, or a mixture of an epoxy compound and a curing agent. The composition may contain other components such as a curing accelerator, a photopolymerization initiator, or a surfactant. The above mixture containing a solvent is also called a composition.

[0045] In this specification, a cured product refers to a polymeric material that contains a product of a composition that has been polymerized. When a composition becomes a cured product, it loses, for example, fluidity and tackiness.

[0046] As described above, the problem of the present invention can be solved by adding a vertical alignment agent to the composition of the present invention. In the present invention, "exhibiting liquid crystallinity" means having a liquid crystal phase between room temperature and 200°C. A composition containing a large amount of solvent loses liquid crystallinity, but a composition that has liquid crystallinity in the above temperature range due to evaporation of the solvent by heating is also said to "exhibit liquid crystallinity". In the present invention, a composition that gives a prepolymer that exhibits liquid crystallinity during the course of curing a composition containing an epoxy compound is also included in the "composition that exhibits liquid crystallinity".

[0047] The temperature range of the liquid crystal phase is preferably the entire temperature range from room temperature to 200°C, but is usually limited to a narrower range. In this case, it is preferable to cure the composition in the liquid crystal phase in order to orient the molecules in the composition and improve the thermal conductivity of the cured product. Such a temperature is usually in the range of 70 to 200°C.

[0048] [Vertical alignment agent] A vertical alignment agent is a compound that is added to a composition exhibiting liquid crystallinity to cause or facilitate the vertical alignment of the mixture relative to the substrate. There is no particular limitation on the type of vertical alignment agent, but it is added at a concentration of equimolar or less to the epoxy compound, which is the main component of the composition.

[0049] One candidate for the vertical alignment agent is a compound that has a hydrocarbon structure with 10 to 50 carbon atoms and has a hydroxyl group, amino, or carboxy at one end of the structure. By selecting a compound with such a structure, vertical alignment of the epoxy composition exhibiting liquid crystallinity is induced.

[0050] The structure of the vertical alignment agent as described above is represented by the following formula (1).

[0051] TIFF0007582041000008.tif1294

[0052] In formula (1), R 1 is hydrogen or alkyl having 1 to 20 carbon atoms, in which non-adjacent -CH2- in this alkyl may be substituted with -O-, and hydrogen in this alkyl may be substituted with fluorine, A 1 , A 2 , and A 3 are independently a single bond, cyclohexane, cyclohexene, or phenylene, and hydrogen on the phenylene may be replaced by CH3, OH, and NH2; m is 0 to 3; X is independently a single bond, -CH2CH2-, -CH2O-, -CH=CH-, -C≡C-, or -COO-.

[0053] In order to prevent the vertical alignment agent from eluting from the cured product and contaminating the electronic component materials after curing, it is preferable to select a compound that acts as a curing agent as the vertical alignment agent. Such a compound can be the compound represented by the following formula (1-1).

[0054] TIFF0007582041000009.tif30122

[0055] In formula (1-1), R 1 is hydrogen or alkyl having 1 to 20 carbon atoms, in which non-adjacent -CH2- in this alkyl may be substituted with -O-, and hydrogen in this alkyl may be substituted with fluorine, A 11 and A 12 are independently cyclohexane, cyclohexene, or phenylene, and hydrogen on the phenylene may be replaced by CH3; m1 is 0 to 2, X is independently a single bond, -CH2CH2-, -CH2O-, -CH=CH-, -C≡C-, or -COO-.

[0056] Suitable examples of the compound represented by formula (1-1) are shown below.

[0057] TIFF0007582041000010.tif118108

[0058] In formulas (1-1-1) to (1-1-4), R 11 is an alkyl group having 8 to 20 carbon atoms.

[0059] TIFF0007582041000011.tif245129

[0060] TIFF0007582041000012.tif171129

[0061] In formulas (1-1-5) to (1-1-18), R 12is a hydrogen atom or alkyl having 1 to 20 carbon atoms.

[0062] Among the compounds of the above formulas (1-1-1) to (1-1-18), it is preferable to select a compound of formulas (1-1-5) to (1-1-18) in order to maintain or improve the liquid crystallinity of the composition, and it is preferable to select one of the compounds represented by formulas (1-1-5) to (1-1-12) and formulas (1-1-16) to (1-1-18) in order to improve the heat resistance of the cured product.

[0063] In the case of vertical alignment agents other than those mentioned above, it is preferable to select a compound exhibiting liquid crystallinity in order to maintain or improve the liquid crystallinity of the composition.

[0064] Formula (1-1) includes a structure of the following formula (1-3).

[0065] TIFF0007582041000013.tif24115

[0066] In formula (1-3), R 3 is hydrogen, alkyl having 1 to 12 carbon atoms, and X 3 are independently a single bond, -CH2CH2-, -CH2O-, or -C≡C-.

[0067] Examples of the compound represented by formula (1-3) include the compounds represented by formulas (1-1-5) to (1-1-8) above.

[0068] The vertical alignment agent is added at a concentration of equimolar or less to the epoxy compound, which is the main component of the composition. At this time, most types of vertical alignment agents do not react with the epoxy compound, or if they react, they do not form a polymer, or give a linear polymer. Therefore, the heat resistance of the cured product decreases, and the vertical alignment agent may dissolve into the environment after curing. In view of such problems, it is desirable to set the content of the curing agent to the minimum amount that gives the composition vertical alignment properties. For example, when a compound represented by formula (1-1) is used as the vertical alignment agent, the content of the compound represented by formula (1-1) is preferably 1% to 50% by mole, more preferably 5% to 40% by mole, based on the total amount of the epoxy compound.

[0069] When a vertical alignment agent that reacts with the epoxy compound that is the main component of the composition is selected, the content of the curing agent in the composition is preferably adjusted according to the amount of the vertical alignment agent. In order to maintain heat resistance when the cured product is obtained, it is preferable to make the epoxy equivalent of the composition equal to the equivalent of the functional group that reacts with the epoxy of the vertical alignment agent and the curing agent.

[0070] The epoxy compound used in the composition of the present invention is preferably a rod-shaped liquid crystal compound because it is easy to produce and has high heat resistance when cured. For such rod-shaped liquid crystal compounds, it is preferable that they have 3 to 5 aromatic rings as the liquid crystal core in order to expand the liquid crystal temperature range.

[0071] The liquid crystal core refers to a structure in which aromatic rings or alicyclic rings are linked by a bonding group having a relatively fixed conformation, such as a single bond, ethylene, oxymethylene, double bond, triple bond, or ester.

[0072] The rod-shaped liquid crystal compound has a structure in which aromatic rings or alicyclic rings are linearly connected as a liquid crystal core, and flexible substituents such as alkyl are bonded to both ends of the core. In this case, the linearity does not need to be strictly linear, and may be bent at an angle of about 45 degrees.

[0073] In such rod-shaped liquid crystal compounds, it is preferable that they do not contain an ester in their molecular structure in order to prevent decomposition at temperatures of 200° C. or higher.

[0074] As the rod-shaped liquid crystal compound, it is more preferable to select the compound represented by formula (2) because it shows liquid crystallinity over a wide temperature range and is easy to produce.

[0075] TIFF0007582041000014.tif31133

[0076] In formula (2), R ep are independently a group having 2 to 12 carbon atoms and having an oxiranyl group, each X is independently a single bond, -CH2CH2-, -CHO-, -CH=CH-, -C≡C-, or -COO-, and A 3 is 1,4-phenylene, 1,4-cyclohexenylene, or 1,4-cyclohexylene; R 2 are independently hydrogen, alkyl having 1 to 8 carbon atoms, alkoxy having 1 to 8 carbon atoms, or R ep wherein at least one -CH2- of these alkyl and alkoxy may be replaced by -C(=O)-, and n is 0 to 2.

[0077] In the compound of formula (2), R ep are each independently a group having 2 to 12 carbon atoms containing oxiranyl. In this case, R ep There are no particular limitations on the structure other than the oxiranyl, but in order to impart high heat resistance to the cured product, a group containing an oxiranyl having 2 to 10 carbon atoms is preferred, and a group containing an oxiranyl having 2 to 8 carbon atoms is particularly preferred. In addition, -CH2- of these groups containing oxiranyl may be substituted with -O-. Compounds having a structure in which -O- is directly bonded to an aromatic ring are particularly easy to synthesize.

[0078] In the compound of formula (2), each linking group X is independently a single bond, -CH2CH2-, -CHO-, -CH=CH-, -C≡C-, or -COO-. In these linking groups, the direction of the bond is arbitrary. In this case, in order to improve the heat resistance of the cured product, it is preferable to select a single bond, -CH2CH2-, -CHO-, or -C≡C- as X, and in order to give the compound a wide liquid crystal temperature range, it is particularly preferable to select a single bond or -C≡C-. In addition, from the viewpoint of ease of synthesis, it is most preferable to select a single bond.

[0079] In the compound of formula (2), A 3 is 1,4-phenylene, 1,4-cyclohexenylene, or 1,4-cyclohexylene. In this case, in order to enhance the liquid crystallinity of the compound, A 3 It is preferable to select 1,4-phenylene as A. 3 When 1,4-cyclohexylene is selected as the aryl group, it is desirable that the substituents at the 1,4-positions are arranged in the so-called trans positions for the same reasons as above.

[0080] In the compound of formula (2), R 1 are each independently hydrogen, fluorine, alkyl having 1 to 8 carbon atoms, alkoxy having 1 to 8 carbon atoms, or R ep In addition, one of the -CH2- in these alkyl and alkoxy groups may be replaced with -CO-. In this case, the liquid crystal temperature range of the compound can be expanded, so these R 1 As R, it is preferable to select alkyl or alkoxy, and it is particularly preferable to select alkyl. ep When R and X are not the same group, it is also preferable to select hydrogen for the same reason. 1 It is most preferable to select methyl as R. Furthermore, in order to improve the heat resistance of the cured product, 1 As R ep It is preferable to select

[0081] In the compound of formula (2), n is an integer of 0 to 2. In this case, n is preferably 1 or 2, since this can expand the liquid crystal temperature range of the compound.

[0082] Suitable examples of the epoxy compound having liquid crystallinity represented by formula (2) include the compounds represented by formulas (2-1) to (2-36).

[0083] TIFF0007582041000015.tif90111

[0084] TIFF0007582041000016.tif220126

[0085] TIFF0007582041000017.tif135144

[0086] TIFF0007582041000018.tif245135

[0087] TIFF0007582041000019.tif204142

[0088] In formulas (2-1) to (2-36), R ep each independently represents an oxiranyl group having 2 to 12 carbon atoms.

[0089] In order to solve the problems of the present invention, it is preferable to select one of the compounds represented by formulas (2-4) to (2-19) and (2-23) to (2-25) from the compounds represented by formulas (2-1) to (2-36). These compounds have a wide liquid crystal temperature range, and it is in a temperature range suitable for curing. Among these compounds, it is more preferable to select one of the compounds represented by formulas (2-6), (2-9), (2-10), and (2-23) to (2-25) for the same reason. In order to further improve the thermal stability of the cured product, it is most preferable to select one of the compounds represented by formulas (2-6), (2-9), and (2-10).

[0090] The composition of the present invention is characterized by containing an epoxy compound exhibiting liquid crystallinity, a curing agent, and a curing accelerator added as necessary. Such a composition of the present invention is likely to exhibit liquid crystallinity. Furthermore, by curing the composition while maintaining this state, the entanglement of molecular skeletons in the cured product is alleviated. As a result, a material that efficiently conducts heat is obtained.

[0091] The composition of the present invention is characterized by containing a compound represented by the above formula (2). One or more compounds of formula (2) may be used. In addition, other known epoxy compounds that do not have liquid crystallinity may be used in combination as long as they do not cause the composition to lose liquid crystallinity.

[0092] As the other epoxy compounds, non-liquid crystal epoxy compounds represented by formulae (o-7) to (o-21) are also preferably used.

[0093] TIFF0007582041000020.tif170107

[0094] In formula (o-12), Z 10 represents a single bond, -CH2-, -O-, -S-, -CH(CH3)-, -C(CH3)2-, -SO2-, or -C(CF3)2-.

[0095] TIFF0007582041000021.tif203109

[0096] In formula (o-13) and formula (o-14), Z 11 represents CH or CCH3.

[0097] TIFF0007582041000022.tif140105

[0098] As the other epoxy compounds, resins having structures represented by formulae (o-23) to (o-27) are also preferably used.

[0099] TIFF0007582041000023.tif81169

[0100] In formula (o-23), Z 12 and Z 13 is independently a single bond, -CH2-, -O-, -S-, -CH(CH3)-, -C(CH3)2-, -SO2-, or -C(CF3)2-, and n21 is an integer of 1 or more and 5,000 or less. In formula (o-24) and formula (o-25), n21 represents an integer of 1 or more and 5000 or less, n22 and n23 are independently 0 or 1, and when n21 is 2 or more, it may be different for each repeat, R 10 and R 11 are independently 1,4-phenylene, 4,4'-biphenylene, or cyclopentadienylene; In addition, hydrogen on the aromatic ring in formula (o-24) to formula (o-25) may be replaced by methyl.

[0101] TIFF0007582041000024.tif104109

[0102] In formula (o-27), Z 14 are independently a single bond, -CH(CH3)-, or -C(CH3)2-. In formulae (o-26) and (o-27), n21 represents an integer of 1 or more and 5,000 or less. In addition, hydrogen on the aromatic ring in formula (o-26) and formula (o-27) may be substituted with methyl.

[0103] The content of such known epoxy compounds relative to the compound of formula (2) is not particularly limited as long as the composition or its cured product exhibits the desired properties. That is, it can be used in an amount between 0.1% by weight and 99.9% by weight based on the total weight of the epoxy compounds. In this case, in order to exhibit the effects of the present invention, it is preferable to use between 0.1% by weight and 70% by weight, and more preferably between 0.1% by weight and 50% by weight.

[0104] [Hardening agent] As the curing agent that can be used in combination with the composition of the present invention, known compounds containing amines, phenols, cyanate esters, carboxylic acids, carboxylic esters, acid anhydrides, or thiols can be used.

[0105] As the phenol-based curing agent, at least one compound represented by the following formulae (3-1) to (3-6) or a compound in which OH of the compound is esterified is preferable, since it does not significantly impair the liquid crystallinity of the composition and is easily available.

[0106] TIFF0007582041000025.tif42115

[0107] TIFF0007582041000026.tif56148

[0108] TIFF0007582041000027.tif10297

[0109] In the above formula (3-1), Ring B is benzene, naphthalene, anthracene, fluorene, or 9,9-diphenylfluorene, and in these rings B, at least one hydrogen may be replaced by alkyl having 1 to 3 carbon atoms or alkoxy having 1 to 3 carbon atoms; n31 is an integer between 2 and 4 inclusive.

[0110] In the above formula (3-2), n32 and n33 are independently an integer of 1 to 3; Z 30 is a single bond, an alkylene having 1 to 10 carbon atoms, -CH(CH3)-, -C(CH3)2-, -C(CF3)2-, -O-, -S-, or -SO2-, At least one hydrogen atom on the benzene ring may be replaced by an alkyl group having 1 to 3 carbon atoms or an alkenyl group having 2 to 3 carbon atoms;

[0111] In the above formula (3-3) and formula (3-4), n34 is an integer of 1 or more and 5000 or less, n35 and n36 are independently 0 or 1, and when n34 is 2 or more, they may be different for each repeat; R 10 and R 11 are independently 1,4-phenylene, 4,4'-biphenylene, or cyclopentadienylene; In formula (3-5), n34 is an integer between 1 and 5000, In formula (3-6), Z 31 is independently a single bond, -CH(CH3)-, or -C(CH3)2-, and n34 is an integer of 1 or more and 5000 or less. In addition, at least one hydrogen atom on the aromatic ring in these formulas (3-3) to (3-6) may be replaced by methyl.

[0112] The amine-based curing agent is preferably at least one compound represented by the following formula (4-1) or (4-2), since it does not significantly impair the liquid crystallinity of the composition and is easily available. EZ-(LZ)nE (4-1) L 1 -ZE (4-2) In formulas (4-1) and (4-2), L is independently a single bond, cyclohexylene, phenylene, or naphthalene, and at least one hydrogen atom in the ring may be replaced by an alkyl group having 1 to 10 carbon atoms; L 1 is hydrogen, cyclohexyl, phenyl, or naphthyl, and at least one hydrogen in these rings may be replaced by alkyl having 1 to 10 carbon atoms; Z is independently a single bond, -O-, -NH-, -S-, -SO2-, -CO2-, or an alkylene having 1 to 12 carbon atoms; E is independently amino, alkylamino having 1 to 10 carbon atoms, hydroxyl group, or carboxy, and at least one E is amino or alkylamino having 1 to 10 carbon atoms; n is an integer from 0 to 7.

[0113] Examples of the compound represented by formula (4-1) include aliphatic polyamines having 2 to 12 carbon atoms, such as ethylenediamine, trimethylenediamine, tetramethylenediamine, hexamethylenediamine, diethylenetriamine, triethylenetetramine, p-xylenediamine, and m-xylenediamine, p-phenylenediamine, N-methyl-p-phenylenediamine, N-ethyl-p-phenylenediamine, N-propyl-p-phenylenediamine, N-butyl-p-phenylenediamine, 2,5-diaminotoluene, m-phenylenediamine, N-methyl-m-phenylenediamine, N-ethyl-m-phenylenediamine, N-propyl-m-phenylenediamine, and N-butyl-m-phenylenediamine. aromatic polyvalent amines such as diaminodiamine, 2,4-diaminotoluene, 2,6-diaminotoluene, o-phenylenediamine, 1,5-diaminonaphthalene, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylethane, 4,4'-diaminodiphenylpropane, 4,4'-diaminodiphenylether, 1,1-bis(4-aminophenyl)cyclohexane, 4,4'-diaminodiphenylsulfone, bis(4-aminophenyl)phenylmethane, m-tolidine, and o-tolidine; and alicyclic polyvalent amines such as 1,4-cyclohexyldiamine, 1,3-cyclohexyldiamine, 1,2-cyclohexyldiamine, and 1,3-bis(aminomethyl)cyclohexane.

[0114] Among these, p-phenylenediamine, N-methyl-p-phenylenediamine, N-ethyl-p-phenylenediamine, N-propyl-p-phenylenediamine, N-butyl-p-phenylenediamine, 2,5-diaminotoluene, m-phenylenediamine, N-methyl-m-phenylenediamine, N-ethyl-m-phenylenediamine, N-propyl-m-phenylenediamine, N-butyl-m-phenylenediamine, 2,4-diaminotoluene, 2,6-diaminotoluene, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylethane, 4,4'-diaminodiphenylpropane, 4,4'-diaminodiphenyl ether, and 4,4'-diaminodiphenyl sulfone are particularly preferred because they have good compatibility when made into a composition and excellent storage stability.

[0115] Examples of the compound represented by formula (4-2) include aliphatic amines having 2 to 12 carbon atoms, such as n-propylamine, n-butylamine, n-pentylamine, n-hexylamine, n-octylamine, and n-dodecylamine; aromatic amines, such as aniline, o-toluidine, m-toluidine, p-toluidine, 2,3-dimethylaniline, 2,4-dimethylaniline, 2,6-dimethylaniline, 2,4,6-trimethylaniline, 2-ethylaniline, 1-naphthylamine, and 1-amino-2-methylnaphthalene; and alicyclic amines, such as cyclohexylamine and 2-methylcyclohexylamine. Among these, aniline, o-toluidine, m-toluidine, p-toluidine, 2,3-dimethylaniline, 2,4-dimethylaniline, 2,6-dimethylaniline, 2,4,6-trimethylaniline, and 2-ethylaniline are particularly suitable because they have good compatibility when made into a composition and excellent storage stability.

[0116] Preferred carboxy-containing curing agents include phthalic acid, terephthalic acid, isophthalic acid, 1,4-naphthalenedicarboxylic acid, 2,3-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,2'-biphenyldicarboxylic acid, 4,4'-biphenyldicarboxylic acid, benzophenone-4,4'-dicarboxylic acid, and the like.

[0117] [Cure accelerator] In the composition of the present invention, particularly when using a phenol-based curing agent, it is preferable to add a curing accelerator to the composition in order to efficiently proceed with the reaction to improve heat resistance. Examples of such curing accelerators include imidazole-based curing accelerators such as 2-ethyl-4-methyl-1H-imidazole, 2-phenyl-4-methyl-1H-imidazole, 1,2-dimethylimidazole, 2-undecylimidazole, 1-benzyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, and 1-cyanoethyl-2-ethyl-4-methylimidazole, phosphorus-based curing accelerators such as triphenylphosphine, and amine-based curing accelerators such as 2,4,6-tris(dimethylaminomethyl)phenol, triethylenediamine, benzyldimethylamine, 2-(dimethylaminomethyl)phenol, and 1,8-diazabicyclo[5.4.0]undec-7-ene. Of these curing accelerators, it is preferable to use imidazole-based curing accelerators since they have a curing temperature of 200° C. or less and have high curability.

[0118] The concentration of the curing accelerator in the composition of the present invention is preferably 0.1% by weight or more, more preferably 0.5% by weight or more, based on the weight of the solid content of the composition of the present invention, in order to efficiently proceed with the reaction to improve the heat resistance, and is preferably 10% by weight or less, more preferably 5% by weight or less, based on the weight of the solid content of the composition of the present invention, in order to avoid deterioration of reliability due to sublimation of the curing accelerator.

[0119] [Inorganic filler] The composition for electronic devices of the present invention may contain an inorganic filler. The inorganic filler contained in the composition for electronic parts may be a nitride such as aluminum nitride, boron nitride, or silicon nitride, which is a filler having high thermal conductivity. In addition, the inorganic filler may be an inorganic filler or a metal filler such as diamond, graphite, silicon carbide, silicon, beryllia, magnesium oxide, aluminum oxide, zinc oxide, silicon oxide, copper oxide, titanium oxide, cerium oxide, yttrium oxide, tin oxide, holminium oxide, bismuth oxide, cobalt oxide, calcium oxide, aluminum nitride, boron nitride, silicon nitride, magnesium hydroxide, aluminum hydroxide, gold, silver, copper, platinum, iron, tin, lead, nickel, aluminum, magnesium, tungsten, molybdenum, or stainless steel. Boron nitride, aluminum nitride, or aluminum oxide is preferable. Boron nitride and aluminum nitride are preferable because they have a very high thermal conductivity in the planar direction, a low dielectric constant, and high insulation. In particular, hexagonal boron nitride (h-BN) or aluminum nitride is preferable.

[0120] The shape of the inorganic filler may be spherical, amorphous, fibrous, rod-like, cylindrical, plate-like, or tetrapod-like. The type, shape, size, and amount of the inorganic filler may be appropriately selected according to the purpose. For example, when the cured product (material for electronic components) formed from the composition for electronic components requires insulation, the inorganic filler may be conductive as long as it maintains the desired insulation.

[0121] The average particle size of the inorganic filler is preferably, for example, 0.1 to 200 μm. More preferably, it is 1 to 100 μm. If it is 0.1 μm or more, the thermal conductivity is good, and if it is 200 μm or less, the filling rate can be increased. In this specification, the average particle size is based on particle size distribution measurement by laser diffraction / scattering method. That is, using analysis based on the Fraunhofer diffraction theory and the Mie scattering theory, when a powder is divided into two at a certain particle size by a wet method, the diameter at which the larger side and the smaller side are equal in amount (volume basis) is defined as the median diameter.

[0122] When used in a heat dissipation member, the amount of inorganic filler added is preferably 20 to 95% by weight, more preferably 50 to 95% by weight. A content of 20% by weight or more is preferable because it increases the thermal conductivity. In order to prevent the material from becoming brittle, the amount of inorganic filler added is preferably 95% by weight or less, and more preferably 90% by weight or less.

[0123] The inorganic filler may be used as it is without modification. Alternatively, the inorganic filler may be used after its surface has been treated with a coupling agent. For example, boron nitride (h-BN) is treated with a silane coupling agent. In the case of boron nitride, since there is no reactive group on the plane of the particle, the silane coupling agent is bonded only to the periphery. Boron nitride treated with a coupling agent can form a bond with a polymerizable compound in the composition for electronic components, and this bond is thought to contribute to thermal conduction. Therefore, the coupling agent is preferably one that reacts with oxiranyl, oxetanyl, or a group possessed by a curing agent. For example, an amine-based one or one having oxiranyl or oxetanyl is preferable. Specifically, Sila Ace S310, S320, S330, S360, S510, S530, etc., manufactured by JNC Corporation, can be mentioned.

[0124] The inorganic filler may be treated with a coupling agent and then surface-modified with a compound having a polymerizable group such as epoxy (polymerizable compound). For example, boron nitride (h-BN) treated with a silane coupling agent is surface-modified with a polymerizable compound. If boron nitride surface-modified with a polymerizable compound can form a bond with the polymerizable compound or a curing agent in the composition for electronic components, this bond is thought to contribute to thermal conduction. For example, the polymerizable compound may be the polymerizable compound of the present invention represented by formula (1), or may be any other polymerizable compound.

[0125] [Other components] Other components that may be contained in the composition of the present invention are not particularly limited, and examples thereof include a polymerizable compound having a polymerizable group other than epoxy, a non-polymerizable compound, a polymerization initiator, and a solvent.

[0126] The polymerizable compound having a polymerizable group other than epoxy is not particularly limited, and any known polymerizable compound can be used as long as it does not deteriorate the properties of the electronic material of the present invention. Among them, compounds that undergo radical polymerization, such as acrylic compounds and styrene-based compounds, can be preferably used, and these compounds that have liquid crystal properties can be more preferably used. Examples of the polymerization initiator include a thermal polymerization initiator, a photocationic polymerization initiator, and a photoanionic polymerization initiator. Examples of the thermal cationic polymerization initiator include a sulfonium salt type, a boron trifluoride-amine complex, a dicyan azide, an organic acid hydrazide, and a toluenesulfonic acid ester. Examples of the photocationic initiator include a sulfonium salt type, an iodonium salt type, and a nonionic type. Examples of the photoanionic initiator include an oxime type, a carbamate type, a guanidinium-carboxylate type, and a nifedipine type.

[0127] When the composition of the present invention contains a compound capable of radical polymerization, such as an acrylic compound or a styrene-based compound, a radical polymerization initiator may be used.

[0128] The composition of the present invention may contain a solvent. Preferred solvents include, for example, 1,4-dioxane, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, ethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monobutyl ether, 3-methoxy-3-methyl-1-butanol, dipropylene glycol methyl ether, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, ethylene glycol diethyl ether, diethylene glycol diethyl ether, and ethylene glycol diethyl ether. Examples of the solvent include ethyl ether, dipropylene glycol dimethyl ether, N-methyl-2-pyrrolidone, dimethylformamide, dimethylacetamide, dimethyl sulfoxide, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether propionate, diethyl carbonate, ethyl methyl carbonate, γ-butyrolactone, methyl lactate, ethyl lactate, butyl lactate, 2-ethylhexanol, 1-propanol, isobutyl alcohol, n-butanol, 2-pentanone, methyl isobutyl ketone, diisobutyl ketone, cyclopentanone, cyclohexanone, diacetone alcohol, and ethylene glycol. The solvent may be used alone or in combination of two or more.

[0129] Since the composition of the present invention has high polymerizability, a stabilizer may be added to facilitate handling. As such a stabilizer, any known stabilizer can be used without limitation. For example, hydroquinone, 4-ethoxyphenol, and 3,5-di-t-butyl-4-hydroxytoluene (BHT) can be used.

[0130] Furthermore, additives (oxides, etc.) may be added to adjust the viscosity or color of the composition for electronic parts. Examples include titanium oxide for whitening, carbon black for blackening, and silica fine powder for adjusting the viscosity. In addition, to further increase the mechanical strength, inorganic fibers such as glass and carbon fiber, cloths thereof, synthetic fibers such as polyvinyl formal, polyvinyl butyral, polyester, polyamide, and polyimide, or supramolecules may be added.

[0131] [Materials for electronic components] The material for electronic parts of the present invention is obtained by molding a cured product obtained by curing the composition for electronic parts according to the second embodiment according to the present invention according to the present invention according to the present invention. For example, the material for electronic parts can be used as a heat dissipation member.

[0132] The material for electronic parts is a polymer (cured product) obtained by polymerizing (curing) the composition of the present invention. This polymer has high thermal conductivity and is excellent in chemical stability, heat resistance, hardness, mechanical strength, etc. The mechanical strength includes Young's modulus, tensile strength, tear strength, bending strength, bending modulus, impact strength, etc.

[0133] The composition of the present invention is a thermosetting resin. The thermosetting resin is cured by heating the raw material composition to polymerize the monomer contained in the composition and further three-dimensionally crosslinking. The heating temperature at this time is preferably within a temperature range in which the composition of the present invention exhibits a liquid crystal phase. In addition, the composition of the present invention may have a liquid crystal temperature range that is increased by proceeding with the curing to a certain extent. In such a case, the composition may be cured in the increased liquid crystal temperature range.

[0134] The curing temperature may be constant or may be increased or decreased stepwise. In the latter case, the initial curing temperature is preferably a temperature at which the composition or its cured product exhibits a liquid crystal phase in order to improve the heat dissipation characteristics of the material. In addition, it is preferable to heat the composition at a temperature higher than the initial curing temperature in order to improve heat resistance.

[0135] The heat curing temperature by thermal polymerization is in the range of 20°C to 350°C, preferably 20°C to 250°C, and more preferably 50°C to 200°C. The curing time is in the range of 5 seconds to 10 hours, preferably 1 minute to 8 hours, and more preferably 5 minutes to 5 hours. After polymerization, it is preferable to slowly cool the product in order to suppress stress distortion. Also, a reheating treatment may be performed to relieve distortion.

[0136] A crosslinking agent may be added to further crosslink the polymer. This makes it possible to obtain a polymer (cured product) that is extremely excellent in chemical resistance and heat resistance. As such a crosslinking agent, any known agent may be used without limitation, and examples thereof include trimethylolpropane tris(3-mercaptopropionate).

[0137] The electronic component material of the present invention can be used in the form of a sheet, film, thin film, fiber, molded product, etc. Preferred forms are a film and a thin film. A film and a thin film can be obtained by polymerizing the composition for electronic components in a state where the composition is applied to a substrate or sandwiched between substrates. Alternatively, the composition for electronic components containing a solvent can be applied to a substrate and the solvent removed. Furthermore, a film can be obtained by press molding a polymer. In this specification, the thickness of the sheet is 1 mm or more, the thickness of the film is 5 μm or more, preferably 10 to 900 μm, and more preferably 20 to 800 μm, and the thickness of the thin film is less than 5 μm. The thickness may be appropriately changed depending on the application.

[0138] The material for electronic parts of the present invention has excellent properties such as high thermal conductivity, chemical stability, heat resistance, hardness, mechanical strength, etc. Therefore, it is useful for heat sink plates, heat sink sheets, heat sink films, heat sink coatings, heat sink adhesives, heat sink molded products, etc.

[0139] Although the electronic component material formed from the polymerizable compound of the present invention is described above as being used as a heat dissipation material, the use of the electronic component material is not limited to being a heat dissipation material. For example, the electronic component material may be used as a sealing material or an adhesive material.

[0140] [Method of manufacturing composition for electronic parts] The composition for electronic parts refers to the heat dissipation material which is the composition of the present invention, and may contain an inorganic filler to enhance thermal conductivity, and the inorganic filler may or may not be subjected to a coupling treatment. As an example of the production of the composition for electronic parts, a production method in which the inorganic filler is subjected to a coupling treatment will be described below. The coupling treatment can be performed by a known method.

[0141] As an example, first add inorganic filler particles and a coupling agent to a solvent. Stir using a stirrer or similar device and then leave to stand. After the solvent dries, heat treatment is performed under vacuum conditions using a vacuum dryer or similar device. Solvent is added to the inorganic filler particles, and the particles are pulverized by ultrasonic treatment. The solution is separated and refined using a centrifuge. After discarding the supernatant, solvent is added and the same operation is performed several times. The refined inorganic filler particles are dried in an oven.

[0142] Next, the inorganic filler particles that have been subjected to the coupling treatment and the polymerizable compound are mixed using an agate mortar or the like, and then kneaded using a two-axis roll or the like. After that, the mixture is separated and refined by ultrasonic treatment and centrifugation.

[0143] Further, an amine-based curing agent is added, and the mixture is mixed using an agate mortar or the like, and then kneaded using a two-axis roll or the like. This produces a solvent-free composition for electronic devices.

[0144] [Method of manufacturing materials for electronic components] As an example, a method for producing a film as a material for electronic parts using a solvent-free composition will be described below.

[0145] The composition containing no solvent is sandwiched between heating plates using a compression molding machine and molded by compression molding. The polymerizable compound is polymerized at a specified temperature and time to form a polymer. Post-curing may be further performed at an appropriate time and temperature. The pressure during compression molding is 50 to 500 kgf / cm. 2 is preferable, and more preferably 70 to 250 kgf / cm 2Generally, the higher the pressure during curing, the better. However, it is best to adjust the pressure appropriately depending on the fluidity of the mold and the desired physical properties (such as which direction of thermal conductivity is most important).

[0146] In addition, the composition becomes easier to handle when it is partially cured (semi-cured state). For example, the composition in a semi-cured state may be formed into a sheet, cut into a desired shape, and placed between suitable members and pasted together.

[0147] A method for producing a film as a material for electronic parts using a composition containing a solvent will be described below.

[0148] The composition is applied onto a substrate, and the solvent is dried and removed to form a coating layer of uniform thickness. Examples of the coating method include spin coating, roll coating, caten coating, flow coating, printing, microgravure coating, gravure coating, wire bar coating, dip coating, spray coating, and meniscus coating.

[0149] The solvent can be removed by drying, for example, air drying at room temperature, drying on a hot plate, drying in a drying oven, blowing warm or hot air, etc. The conditions for removing the solvent are not particularly limited, and drying may be performed until the solvent is mostly removed and the coating layer loses its fluidity.

[0150] [Electronic components] The composition of the present invention or a cured product thereof can be used, for example, as a heat dissipation member for electronic components. Examples of such electronic components include electronic devices having a heat generating part. When the composition of the present invention or a cured product thereof is used as a heat dissipation member, the heat dissipation member is placed on the electronic device so as to contact the heat generating part. The shape of the heat dissipation member may be any of a heat dissipation plate, a heat dissipation sheet, a heat dissipation film, a heat dissipation adhesive, a heat dissipation molded product, and the like. In this way, the heat generated in the electronic device is dissipated by the heat dissipation member, and failure due to heat is avoided, thereby extending the life of the electronic device equipped with the electronic device.

[0151] Examples of electronic devices include semiconductor elements. The heat dissipation material has high thermal conductivity, high heat resistance, and high insulation. Therefore, it is particularly effective for insulated gate bipolar transistors (IGBTs), which require a more efficient heat dissipation mechanism due to their high power consumption. IGBTs are a type of semiconductor element, a bipolar transistor with a MOSFET built into the gate, and are used for power control. Examples of electronic devices equipped with IGBTs include the main conversion element of a high-power inverter, an uninterruptible power supply, a variable voltage variable frequency control device for an AC motor, a control device for a railway vehicle, electric transport equipment such as hybrid cars and electric cars, and an induction cooker.

[0152] [Method for synthesizing the compound represented by formula (1)] The compound of formula (1) can be synthesized by combining known methods in organic synthetic chemistry. Methods for introducing the desired polymerizable group and ring structure into the starting material are described in, for example, Houben-Weyl, Methods of Organic Chemistry, Georg Thieme Verlag, Stuttgart, Organic Syntheses, John Wiley & Sons, Inc., Organic Reactions, John Wiley & Sons, Inc., Comprehensive Organic Synthesis, Pergamon Press, New Experimental Chemistry Course (Maruzen), and other publications. Also, JP 2006-265527 A may be referenced. EXAMPLES

[0153] The present invention will be described in detail below using examples. However, the present invention is not limited to the contents described in the examples. Unless otherwise stated, measurements were performed at 23°C.

[0154] [Measurement of phase transition points of compounds and identification of liquid crystal phases] Measurements were performed using a polarizing microscope and a differential scanning calorimeter. The polarizing microscope was a VHX5000 digital microscope (KEYENCE) equipped with a polarizing plate. The temperature was adjusted using a hot stage system HS1 (Mettler Toledo). The polarizing microscope measurements were performed under crossed Nicols. The magnifications of the eyepiece and objective lens were 10x20, respectively. The differential scanning calorimeter used was a Diamond DSC manufactured by Perkin Elmer. During the measurements, the heating and cooling rates were both 3°C / min. In the examples, C indicates crystal, N indicates nematic phase, I indicates isotropic liquid, and () indicates monotropic liquid crystal phase.

[0155] [NMR measurement] NMR was measured using a VARIAN NMR SYSTEM manufactured by VARIAN. 1 The magnetic field strength for H NMR measurements was 500 MHz, the sample was dissolved in a deuterated solvent such as CDCl3, and the measurements were performed at room temperature. The number of integrations was 8. The internal standard was tetramethylsilane. In the NMR symbols, s means singlet, d means doublet, t means triplet, m means multiplet, and br means broad.

[0156] [Confirmation of liquid crystal properties of the composition] A few drops of the composition were placed on a slide glass and kept at 80°C for 5 minutes to evaporate the solvent. The sample was observed under a polarizing microscope in the same manner as above. Some types of compositions were vertically aligned, so the dark field area occupied most of the area, but the observation was made in the area where alignment defects characteristic of the liquid crystal state existed, and if the defects existed, it was determined that the liquid crystal property existed.

[0157] [Confirmation of orientation of cured product] The retardation was confirmed using a polarizing microscope and an OPTIPRO ellipsometer manufactured by Shintech Co., Ltd. In the OPTIPRO ellipsometer, the substrate coated with the cured material was irradiated with light having a wavelength of 550 nm, and the retardation was measured. The retardation (also called retardation) is expressed as Δn×d. The symbol Δn is the optical anisotropy value, and the symbol d is the thickness of the polymer film. When the angle of incidence of the measurement light is decreased from 90° to the substrate surface, the retardation value is almost 0 nm at 90° in the case of vertically aligned liquid crystals or materials in a cured state, and a curve gradually increases as the angle decreases.

[0158] [Measurement of thermal conductivity] A sample consisting of resin only: NETZSCH LFA467 HyperFlash was used to measure the thermal diffusivity (α, m 2 The thermal diffusivity was measured in the vertical and horizontal directions of the sample. The specific heat (c, J / (Kg)) and density (ρ, g / m 3 ) and the thermal conductivity (W / (Km)) was calculated according to the following formula. κ = α x c x ρ At this time, the specific heat was measured using a DSC type high sensitivity differential scanning calorimeter Thermo Plus EVO2 DSC-8231 manufactured by Rigaku Corp. The specific gravity was measured using a specific gravity scale type specific gravity meter DME-220 manufactured by Shinko Denshi Co., Ltd. Filler-containing sample: The thermal diffusivity in the thickness direction of the sample was measured using an ai-Phase Mobile 1u thermal diffusivity measuring device manufactured by ai-Phase Co., Ltd. The specific heat and density of the sample were also measured in the same manner as above. From these values, the thermal conductivity was calculated in the same manner as above.

[0159] [Compound used] As the vertical alignment agent represented by formula (1-1), the compound represented by the following formula (1-1-8-1) was used in the examples. These compounds were synthesized as described below. As the epoxy compound represented by formula (2), compounds represented by the following formulas (2-10-1) and (2-10-2) were used in the examples. These compounds were synthesized as described below. In addition, a compound represented by formula (2-21-1) was used in the examples. This compound was synthesized according to ACS Omega, 3, 3562 (2018) and the literature described therein. The curing agent used was a compound represented by formula (3-2-1), which was synthesized as described below.

[0160] TIFF0007582041000028.tif28138

[0161] TIFF0007582041000029.tif124146

[0162] [Example 1] Synthesis of compound represented by formula (1-1-8-1)

[0163] TIFF0007582041000030.tif54159

[0164] A mixture of 3.30g (9.26mmol) of 1-iodo-4-trans(4-n-pentyl)cyclohexylbenzene, 1.50g (9.25mmol) of 4-ethynyl-1,2-dimethoxybenzene, 130mg (0.185mmol) of dichlorobistriphenylphosphinepalladium(II), and 35.2mg (0.185mmol) of CuI was refluxed in Et3N (30ml) under N2 flow for 4 hours. After cooling the reaction solution, toluene (60ml) and pure water (50ml) were added to the reaction solution, and the organic layer was separated. The organic layer was dried over MgSO4, filtered, and the solvent was distilled off under reduced pressure. The residue was purified by column chromatography (silica gel, toluene / ethyl acetate = 10 / 1) and recrystallization (EtOH) to obtain compound (1-1-8-1-a). Yield 2.72g (75%).

[0165] The above 1-iodo-4-trans(4-n-pentyl)cyclohexylbenzene and 4-ethynyl-1,2-dimethoxybenzene were synthesized according to J. Am. Chem. Soc., 131, 6763 (2009) and J. Org. Chem., 73, 4241 (2008), respectively.

[0166] 2.20 g (5.75 mmol) of compound (1-1-8-1-a) was subjected to hydrogenation reaction in an autoclave in toluene / ethanol = 20 / 20 ml using Pd / C 320 m as a catalyst. At this time, the hydrogen pressure was 0.7 MPa. After the reaction, the catalyst was filtered off and the solvent was distilled off under reduced pressure. The residue was purified by recrystallization (EtOH) to obtain compound (1-1-8-1-b). Yield 1.70 g (75%).

[0167] To a solution of 1.10 g (2.79 mmol) of compound (1-1-8-1-b) in CH2Cl2 (10 ml), 5.8 ml of a solution of BBr3 in CH2Cl2 (1 M) was added at -10°C. After stirring overnight at room temperature, the reaction solution was added to pure water (30 ml). To this mixture, AcOEt (40 ml) was added and extracted. The organic layer was washed twice with pure water (15 ml) and then dried over MgSO4. The solution was filtered and the solvent was distilled off under reduced pressure. The residue was purified by column chromatography (silica gel, toluene / ethyl acetate = 1 / 1) and recrystallization (toluene) to obtain compound (1-1-8-1). Yield 870 mg (85%).

[0168] Phase transition temperature (℃); C·147.4·N·161.4·I. 1 H-NMR(ppm,CDCl3);7.14-7.09(AA'BB',4H),6.78(d,1H,J=8.00Hz),6.72(d,1H,J=2.00Hz),6.64( dd,1H,J=8.00,2.00Hz),4.98,4.86(s,1H),2.84-2.79,2.48-2.39,1.89-1.84,1.49-0.88(m,25H).

[0169] [Example 2] Synthesis of compound represented by formula (2-10-1)

[0170] TIFF0007582041000031.tif47160

[0171] A mixture of 10.0 g (53.5 mmol) of 4-bromo-o-cresol, 8.70 g (58.4 mmol) of 5-bromopentene, and 8.9 g (64 mmol) of K2CO3 was refluxed in acetone (100 ml) under nitrogen atmosphere for 78 hours. After cooling the reaction solution, pure water (100 ml) and toluene (120 ml) were added and the organic layer was separated. The organic layer was washed twice with pure water (50 ml) and then dried over MgSO4. The solution was filtered and the solvent was distilled off under reduced pressure. The residue was purified by column chromatography (silica gel, toluene) to obtain 4-bromo-2-methyl-(4-pentenyloxy)benzene. Yield 13.4 g (98%).

[0172] Mg1.42g (58.8mmol) was added to THF (15ml) and a piece of iodine crystal was added. The above 4-bromo-2-methyl-(4-pentenyloxy)benzene in THF (85ml) solution was added to this solution under a nitrogen atmosphere to prepare a Grignard reagent. The above Grignard reagent was added to a THF (50ml) solution of B(OMe)37.5ml (67.1mmol) at a rate not exceeding -30℃, and stirred at -60℃ for 1 hour. The reaction temperature was set to 0℃, 30ml of 3N hydrochloric acid was added, and stirred at room temperature for 1 hour. Pure water (60ml) and toluene (200ml) were added to this reaction solution, and the organic layer was separated. The organic layer was washed twice with pure water (50ml) and then dried with MgSO4. The solution was filtered and the solvent was distilled off under reduced pressure. The residue was purified by recrystallization (heptane) to give 4-(4-pentenyloxy)-3-methylphenylboronic acid in an amount of 8.12 g (yield 67%).

[0173] Compound (1-10-1-b) was synthesized using 4-(4-pentenyloxy)-3-methylphenylboronic acid and compound (2-10-1-a) in the same manner as in Example 4 above. The product was purified by column chromatography (silica gel, toluene) and recrystallization (heptane). Yield 9.5 g (82%).

[0174] Compound (2-10-1) was synthesized using compound (1-10-1-b) in the same manner as in Example 1. The product was purified by column chromatography (silica gel, toluene:ethyl acetate=10:1) and recrystallization (ethanol). Yield: 6.6 g (64%).

[0175] Phase transition point (℃); C·118.9·N·174.7·I 1 H-NMR(ppm,CDCl3);7.64-7.60(m,4H),7.57,7.43(AA'BB',4H),7.31-7.25(m,2H),6.89(d,1H,J=8.00 Hz),4.11-4.04(m,2H),3.04-2.99,2.93-2.78,2.53-2.51,1.90-1.86,1.78-1.67(m,16H)2.30(s,3H).

[0176] [Example 3] Synthesis of compound represented by formula (2-10-2)

[0177] TIFF0007582041000032.tif20169

[0178] Compound (2-10-2-a) was synthesized in the same manner as in Example 2 above, using 4-(3-methyl-3-butenyloxy)-3-methylphenylboronic acid and compound (2-10-1-a) which were synthesized in the same manner as in Example 2. The product was purified by column chromatography (silica gel, toluene) and recrystallization (heptane). Yield 6.5 g (yield 86%).

[0179] Compound (2-10-2) was synthesized using compound (2-10-2-a) in the same manner as in Example 1. The product was purified by column chromatography (silica gel, toluene:ethyl acetate=10:1) and recrystallization (ethanol). Yield 6.9 g (yield 85%).

[0180] Phase transition point (℃); C 122.0 N 153.3 I 1 H-NMR(ppm,CDCl3);7.63-7.62(m,4H),7.57,7.29(AA'BB',4H),7.45-7.42(m,2H),6.90(d,1H,9 .00Hz),3.00-2.77,2.67-2.66,2.51-2.50(m,7H),2.29(s,3H),2.17-1.83(m,4H),1.55(s,3H).

[0181] [Example 4] Synthesis of compound represented by formula (3-2-1)

[0182] TIFF0007582041000033.tif51133

[0183] A mixture of 2.00g (9.34mmol) of 3-formyl-4,4'-dihydroxybiphenyl, 4.7g (56mmol) of 3,4-dihydro-2H-pyran, and 0.47g (1.9mmol) of PPTS was stirred overnight at room temperature in 20ml of CHCl. ​​30ml of saturated sodium bicarbonate solution was added to the reaction solution, and the organic layer was separated. The organic layer was dried over anhydrous magnesium sulfate and then filtered. The solvent was removed under reduced pressure, and the resulting product was purified by column chromatography (toluene:ethyl acetate=10:1) to obtain compound (3-2-1-a). Yield 244mg (7.9%).

[0184] Compound (3-2-1-a) was converted to compound (3-2-1-b) in the same manner as in Example 5. The crude product was purified by column chromatography (heptane:toluene=1:1→toluene). Yield: 86%.

[0185] Compound (3-2-1-b) was converted to compound (3-2-1) in the same manner as in Example 5. The crude product was purified by column chromatography (toluene:ethyl acetate=2:1). Yield: 100%.

[0186] Melting point(℃):138.0-145.7. 1H-NMR(ppm,CDCl3);7.54(d,1H,J=2.50Hz),7.44-7.41(AA'BB',2H),7.31(dd,1H,J=8.00,2.50Hz),6.97(dd,1H,J=17.50,10.50 Hz),6.91-6.87(AA'BB',2H),6.85(d,1H,J=8.50Hz),5.80(d,1H,J=18.00Hz),5.41(d,1H,J=11.00Hz),4.99(s,1H),4.76(s,1H).

[0187] [Example 5] Preparation of composition and confirmation of liquid crystal properties 0.0900g (0.2455mmol) of the compound represented by formula (1-1-8-1) synthesized in Example 1, 0.5000g (1.206mmol) of the compound represented by formula (2-10-1) synthesized in Example 2, and 0.2050g (0.9658mmol) of the compound represented by formula (3-2-1) synthesized in Example 4 were placed in a sample bottle, and cyclopentanone (2.9ml) was added to dissolve the solid content. When this composition was observed on a hot plate with a polarizing microscope, it showed nematic liquid crystal properties in the range of 78 to 100°C. This composition is designated as S1.

[0188] [Examples 6 to 7] The compositions shown in Table 1 were prepared in the same manner as in Example 5. In Table 1, the molar ratio is shown in parentheses. Example 5 is also shown again.

[0189] [Table 1]

[0190] The liquid crystal temperature range of each composition is shown in Table 2.

[0191] [Table 2]

[0192] [Comparative Examples 1 to 3] Preparation of compositions not containing a vertical alignment agent and confirmation of liquid crystal properties The compositions shown in Table 3 were prepared in the same manner as in Example 5. In Table 3, the numbers in parentheses indicate mol %, and numbers without parentheses indicate a molar ratio of 100.

[0193] [Table 3]

[0194] [Example 8] Confirmation of the orientation of the composition on a glass substrate To the S1 prepared in Example 5, 0.0380 g of imidazole and 10 μl of a 10% cyclopentanone solution of TEGOFLOW370 (sold by Evonik Japan Co., Ltd.) were added. This composition was designated S1C. This S1C was spin-coated (700 rpm) onto a glass substrate (40 × 40 mm, Eagle XG, Corning). This substrate was left standing on a hot plate at 90 ° C for 1 hour to cure the composition. The resulting cured product had no tackiness.

[0195] When this substrate was observed under a polarizing microscope, a dark field was observed in all observed regions (polarizing microscope photograph in FIG. 1 [Example 8]). In addition, retardation measurements confirmed that the skeleton molecules in this cured product were vertically aligned.

[0196] [Examples 9 and 10] A glass substrate on which a cured product was formed by curing the composition was obtained in the same manner as in Example 8, except that S1 was changed to S2 and S3. The orientation of the molecules constituting this cured product was examined, and the results are shown in Table 4 below. Example 8 is also shown in the table.

[0197] [Table 4]

[0198] [Comparative Example 4] A glass substrate on which the composition was cured was obtained in the same manner as in Example 8, except that composition S1 was changed to R1. The cured product had no tackiness. When this substrate was observed with a polarizing microscope, light leakage was observed in some observation areas (Figure 2). In addition, retardation measurements confirmed that the majority of the area was vertically aligned.

[0199] [Comparative Examples 5 and 6] A glass substrate on which a cured composition was formed was obtained in the same manner as in Example 8, except that R1 was changed to R2 and R3. The orientation of the molecules constituting this cured product was examined, and the results are shown in Table 5 below. Comparative Example 4 is also shown in the table.

[0200] [Table 5]

[0201] A comparison of the above Examples 8 to 10 and Comparative Examples 4 to 6 shows that the addition of a vertical alignment agent to the composition can improve the vertical alignment of the composition. In other words, the technology of the present invention makes it possible to stably obtain an epoxy material with a vertically oriented molecular skeleton even when the substrate and material preparation conditions are changed in various ways.

[0202] [Example 11] Measurement of thermal conductivity of cured product prepared from composition S1C Composition S1C was placed in an aluminum container with a diameter of 2.4 cm, and held on a hot plate heated to 150°C for 120 minutes, and a circular piece with a thickness of 0.6 mm was taken out. The thermal conductivity of this cured material was 1.07 W / m K and 0.69 W / m K in the planar and perpendicular directions, respectively.

[0203] [Examples 12 to 13] The thermal conductivity of the cured products prepared in the same manner as in Example 11 above, except that composition S1C was replaced with composition S2C and S3C, is shown in Table 6. Example 11 is also shown in the table.

[0204] [Table 6]

[0205] [Example 14] Preparation of a sample containing filler 0.100 g of composition S1C and 0.9000 g of boron nitride particles (PolarTherm PTX-25, Momentive Performance Materials Japan, Ltd.) were weighed out and mixed thoroughly, sandwiched between stainless steel plates, and held for 45 minutes at a pressure of 20 MPa in a compression molding machine (IMC-19EC, Imoto Machinery Co., Ltd.) heated to 150°C, to obtain a square piece with a thickness of 683 μm as a heat dissipation member. The thermal conductivity of this heat dissipation member was 12.7 W / m K.

[0206] [Examples 15 to 16] Except for using compositions S2C and S3C instead of composition S1C, heat dissipation members were prepared and their thermal conductivity was measured in the same manner as in Example 14. The results are shown in Table 7, which also includes Example 14.

[0207] [Table 7]

[0208] As described above, it is understood that the technology disclosed in the present invention provides high thermal conductivity. [Industrial Applicability]

[0209] The technology of the present invention can be suitably used for packaging materials for semiconductor devices, and can also be used as an alternative to other epoxy resins, such as adhesives.

Claims

1. A composition containing an epoxy compound, the composition exhibiting liquid crystallinity, and further containing a vertical alignment agent, the vertical alignment agent containing a compound having a structure represented by the following formula (1-1): In formula (1-1), R 1 is hydrogen or alkyl having 1 to 20 carbon atoms, in which non-adjacent —CH 2 — in the alkyl may be substituted with —O—, and hydrogen in the alkyl may be substituted with fluorine; A 11 and A 12 are independently cyclohexane, cyclohexene, or phenylene, and hydrogen on the phenylene may be replaced by CH 3 ; m1 is an integer from 0 to 2; X is independently a single bond, -CH 2 CH 2 -, -CH 2 O-, -CH=CH-, -C≡C-, or -COO-.

2. The composition of claim 1 further comprising a curing agent.

3. The composition according to claim 1 or 2, wherein the epoxy compound comprises a compound having a structure of formula (2). In formula (1), R ep are independently a C2 to C12 group having an oxiranyl group, and X is independently a single bond, -CH 2 CH 2 --, --CH 2 O-, -CH=CH-, -C≡C-, or -COO-; 3 is 1,4-phenylene, 1,4-cyclohexenylene, or 1,4-cyclohexylene; R 2 are independently hydrogen, fluorine, alkyl having 1 to 8 carbon atoms, alkoxy having 1 to 8 carbon atoms, or R ep and at least one of these alkyl and alkoxy groups is —CH 2 - may be replaced by -C(=O)-, and n is an integer from 0 to 2.

4. The composition according to claim 3, wherein in the epoxy compound represented by formula (2), X is a single bond or -C≡C-.

5. 3. The composition according to claim 2, wherein the curing agent is a phenol having two or more --OH groups in the molecular skeleton, or a compound obtained by esterifying the phenol.

6. The composition according to claim 5, wherein the curing agent is at least one compound represented by formulas (3-1) to (3-6) or an esterified compound of said compound. In formula (3-1), Ring B is benzene, naphthalene, anthracene, fluorene, or 9,9-diphenylfluorene, and in these rings B, at least one hydrogen may be replaced by alkyl having 1 to 3 carbon atoms or alkoxy having 1 to 3 carbon atoms; n31 is an integer of 2 or more and 4 or less. In formula (3-2), n32 and n33 are independently an integer of 1 to 3; Z 30 represents a single bond, an alkylene having 1 to 10 carbon atoms, -CH(CH 3 ) -, -C(CH 3 ) 2 -, -C(CF 3 ) 2 -, -O-, -S-, or -SO 2 - and At least one hydrogen atom on the benzene ring may be replaced by an alkyl group having 1 to 3 carbon atoms or an alkenyl group having 2 to 3 carbon atoms; In formula (3-3) and formula (3-4), n34 is an integer of 1 or more and 5000 or less, n35 and n36 are independently 0 or 1, and when n34 is 2 or more, it may be different for each repetition, R 10 and R 11 are independently 1,4-phenylene, 4,4'-biphenylene, or cyclopentadienylene; In formula (3-5), n34 is an integer of 1 or more and 5000 or less, In formula (3-6), Z 31 are independently a single bond, -CH(CH 3 ) - or -C(CH 3 ) 2 -, and n34 is an integer between 1 and 5000. In addition, at least one hydrogen atom on the aromatic ring in the formulae (3-3) to (3-6) may be replaced by methyl.

7. The composition according to claim 2 , wherein the curing agent is an aromatic primary amine, an aliphatic primary amine, an aromatic amine having two or more secondary amino groups in its molecular skeleton, or an aliphatic amine having two or more secondary amino groups in its molecular skeleton.

8. The composition according to claim 7, wherein the curing agent is at least one compound represented by formula (4-1) or (4-2). E-Z-(L-Z)n-E (4-1) L 1 -Z-E (4-2) In formulas (4-1) and (4-2), L is independently a single bond, cyclohexylene, phenylene, or naphthalene, and at least one hydrogen atom in the ring may be replaced by alkyl having 1 to 10 carbon atoms; L 1 is hydrogen, cyclohexyl, phenyl, or naphthyl, and at least one hydrogen in these rings may be replaced by alkyl having 1 to 10 carbon atoms; Z is independently a single bond, -O-, -NH-, -S-, or -SO 2 --, --CO 2 - or alkylene having 1 to 12 carbon atoms; E is independently amino, alkylamino having 1 to 10 carbon atoms, hydroxyl group, or carboxy, and at least one E is amino or alkylamino having 1 to 10 carbon atoms; n is an integer from 0 to 7.

9. The composition of claim 2 , wherein the curing agent is a compound comprising a cyanate ester.

10. The composition of claim 2 , wherein the curing agent is a compound containing a carboxylic acid, a carboxylic ester, an acid anhydride, or a thiol.

11. The composition according to any one of claims 1 to 10, further comprising an inorganic filler.

12. The composition of claim 11, wherein the inorganic filler is aluminum oxide or boron nitride.

13. A cured product obtained by curing the composition according to any one of claims 1 to 11.

14. An electronic part using the cured product according to claim 13.

15. A compound, wherein the compound having a structure represented by formula (1-1) according to claim 1 has a structure represented by formula (1-3). In formula (1-3), R 3 is hydrogen or alkyl having 1 to 12 carbon atoms; X 3 are independently a single bond, -CH 2 CH 2 --, --CH 2 It is -O-, or -C≡C-.

Citation Information

Patent Citations

  • Optical anisotropy film, liquid crystal display device, and compound for use in them

    JP2006276821A

  • Polymerizable compound, composition for electronic component and material for electronic component

    JP2022008092A

  • Process for preparing a planographic printing plate

    US4221858A

  • Liquid crystal resin composition, heat dissipation material precursor, and heat dissipation material

    WO2012098735A1

  • Epoxy resin composition, thermoconductive material precursor, b-stage sheet, prepreg, heat-dissipating material, laminated plate, metal substrate, and printed circuit board

    WO2016190260A1