Resin composition
The resin composition addresses the trade-offs of warpage, elastic modulus, and adhesion/releasability by using a balanced formulation of epoxy resin, radically polymerizable unsaturated groups, and acid anhydride, resulting in improved handling and reliability of semiconductor chip packages.
Patent Information
- Application Number
- JP2021085515
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-06-12
- Filing Date
- 2021-05-20
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2041-05-20
AI Technical Summary
Existing resin compositions for compression molding face a trade-off between achieving small warpage and high elastic modulus in cured products, as well as balancing adhesion to inorganic materials with releasability from film materials, making handling and sealing of semiconductor chips challenging.
A resin composition containing specific amounts of an epoxy resin, a radically polymerizable unsaturated group with a polyalkylene oxide structure, an acid anhydride, and a radical generator, with a balanced mass ratio of these components, to achieve small warpage, high elastic modulus, and excellent adhesion to inorganic materials while ensuring easy release from film materials.
The resin composition effectively resolves the trade-offs by producing cured products with minimal warpage, high elastic modulus, strong adhesion to inorganic materials, and easy film material releasability, enhancing the handling and reliability of semiconductor chip packages.
Smart Images

Figure 0007582065000001 
Figure 0007582065000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition, and further to a resin paste, a cured product, a resin sheet, a printed wiring board, a semiconductor chip package, a semiconductor device, a method for producing a printed wiring board, and a method for producing a semiconductor chip package. [Background technology]
[0002] In order to seal a printed wiring board or a semiconductor chip included in a semiconductor device, a liquid resin composition is sometimes used as a sealing material. Patent Document 1 discloses a liquid epoxy resin composition as a sealing material, which comprises (a) an epoxy resin, (b) a curing agent, (c) a latent catalyst, (d) a polymerizable monomer having two or more radically polymerizable double bonds, (e) a radical polymerization initiator, and (f) an inorganic filler (Claim 2). Patent Document 2 discloses a liquid epoxy resin composition as a sealing material, which comprises an epoxy resin that is liquid at room temperature, an amine curing agent, a thermosetting acrylic resin, a thermal polymerization initiator for the thermosetting acrylic resin, and an inorganic filler (Claim 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Application Publication No. 11-255864 [Patent Document 2] JP 2014-094981 A Summary of the Invention [Problem to be solved by the invention]
[0004] Incidentally, it is generally required that a resin composition for compression molding (for compression molding) can obtain a cured product with little warpage. In addition, from the viewpoint of improving the handleability of printed wiring boards and semiconductor chip packages, the obtained cured product is required to have a high elastic modulus. However, the inventors' investigations showed that cured products with little warpage tend to have a low elastic modulus. In addition, cured products with a high elastic modulus tend to have a high warpage. Thus, there is a trade-off (first trade-off) between reducing warpage and increasing the elastic modulus, and it has been difficult to achieve both.
[0005] In addition, from the viewpoint of reliability, the cured product of the resin composition as an encapsulating material is required to have high adhesion between the cured product and an inorganic material (e.g., silicon or copper) that the cured product comes into contact with (hereinafter, also referred to as "inorganic material adhesion"). On the other hand, the resin composition layer (compression molded product) obtained by performing compression molding on the resin composition is required to have excellent releasability from the release film (hereinafter, also referred to as "film material releasability"). Here, the release film generally refers to a film material having releasability that is used during compression molding. By interposing a release film between the resin composition layer and the mold during compression molding, the resin composition layer is prevented from directly contacting the mold, and it is expected that the resin composition layer will be easily removed after compression molding.
[0006] However, as a result of the inventor's research, it was found that when a cured product of a resin composition has high adhesion to an inorganic material, the resin composition layer (compression molded product) of the resin composition usually tends to have high adhesion to a release film as well (second trade-off). Therefore, after compression molding, it may not be as easy as expected to remove the resin composition layer from the mold, or even if the resin composition layer can be removed from the mold, it may be difficult to peel the release film from the resin composition layer.
[0007] For these reasons, it is required that the resin composition for compression molding eliminates both the first trade-off between the reduction of warpage in the cured product and the increase in the elastic modulus of the cured product, and the second trade-off between the high adhesion between the cured product and the inorganic material and the high peelability of the resin composition layer (compression molded product) from the film material. If these trade-offs are eliminated, it is expected that the resin composition layer (compression molded product) of the resin composition will be easy to handle, and that the sealed product in which, for example, a semiconductor chip is sealed with a cured product of the resin composition will be easy to handle.
[0008] An object of the present invention is to provide a resin composition or resin paste which can give a cured product which has little warping, a high elastic modulus, and excellent adhesion to inorganic materials, and which has excellent peelability from film materials; and to provide a cured product, a resin sheet, a printed wiring board, a semiconductor chip package, a semiconductor device, a method for producing a printed wiring board, and a method for producing a semiconductor chip package, which are obtained using the resin composition or resin paste. [Means for solving the problem]
[0009] As a result of extensive investigations, the present inventors have found that the above-mentioned problems can be solved by allowing a resin composition to contain specific components in specific blending amounts, and have thus completed the present invention.
[0010] That is, the present invention includes the following. [1] (A) an epoxy resin and (B) a compound having a radically polymerizable unsaturated group and a polyalkylene oxide structure, the compound being represented by the following formula (1): E / N-(100×N)≧50 (1) (In formula (1), E represents the equivalent (g / eq.) of the radically polymerizable unsaturated group, and N represents the number of radically polymerizable unsaturated groups in the molecule and is an integer of 1 or more.) (C) an acid anhydride, (D) a radical generator, and (E) an inorganic filler, wherein the mass ratio of the component (B) to the component (C) [b]:[c] is within the range of 0.2:1 to 1.5:1. [2] The polyalkylene oxide structure of the component (B) is represented by the formula: -(R B O) n In the formula, n is an integer of 2 or more, and R B and each independently represent an alkylene group having 1 to 6 carbon atoms which may have a substituent. [3] Multiple groups R B At least one group R B The resin composition according to [2], wherein the alkyl group contains an ethylene group. [4] The resin composition according to any one of [1] to [3], wherein the radically polymerizable unsaturated group of component (B) is one or more selected from a vinyl group, an allyl group, a 1-butenyl group, a 2-butenyl group, an acryloyl group, a methacryloyl group, a fumaroyl group, a maleoyl group, a vinylphenyl group, a styryl group, and a cinnamoyl group. [5] The resin composition according to [4], wherein the radically polymerizable unsaturated group of the component (B) includes at least one type selected from a methacryloyl group and an acryloyl group. [6] The resin composition according to [4] or [5], wherein the radically polymerizable unsaturated group of the component (B) contains a methacryloyl group. [7] The resin composition according to any one of [1] to [6], wherein the component (B) contains one or more compounds selected from the group consisting of a compound in which N in formula (1) is 1 and a compound in which N in formula (1) is 2. [8] The resin composition according to [7], wherein the compound in which N in formula (1) is 1 has a molecular weight of 150 or more. [9] The resin composition according to [7] or [8], wherein the compound in formula (1) where N is 2 has an equivalent weight (g / eq.) of the radical polymerizable unsaturated group of 500 or more.
[10] The resin composition according to any one of [1] to [9], wherein the equivalent weight of the radically polymerizable unsaturated group in component (B) is 4,500 g / eq. or less.
[11] The resin composition according to any one of [1] to
[10] , wherein the content of the (B) component is 10 mass% or more and 40 mass% or less, when the total amount of non-volatile components in the resin composition other than the (E) inorganic filler is taken as 100 mass%.
[12] The resin composition according to any one of [1] to
[11] , wherein the equivalent ratio (c) / (a) of the sum of values obtained by dividing the amount (g) of component (C) by the equivalent (g / eq.) of an acid anhydride group in component (C) to the sum of values obtained by dividing the amount (g) of component (A) by the equivalent (g / eq.) of an epoxy group in component (A) is 0.4 or more.
[13] The resin composition according to any one of [1] to
[12] , wherein the component (D) is one or more types selected from radical generators having a 10-hour half-life temperature T10 (°C) in the range of 50°C or more and 110°C or less.
[14] The resin composition according to any one of [1] to
[13] , wherein the content of the component (E) is 70 mass% or more, relative to 100 mass% of the total non-volatile components in the resin composition.
[15] The resin composition according to any one of [1] to
[14] , which is for compression molding.
[16] The resin composition according to
[15] , wherein the component (D) is one or more radical generators selected from radical generators having a difference ΔT (°C) between the mold temperature Tc (°C) during compression molding and the 10-hour half-life temperature T10 (°C) of the component (D) in the range of 20°C or more and 80°C or less.
[17] The resin composition according to any one of [1] to
[16] , which is for forming an insulating layer.
[18] A resin paste comprising the resin composition according to any one of [1] to
[17] .
[19] A cured product of the resin composition according to any one of [1] to
[17] or the resin paste according to
[18] .
[20] A resin sheet comprising a support and a resin composition layer provided on the support, the resin composition layer comprising the resin composition according to any one of [1] to
[17] or the resin paste according to
[18] .
[21] A printed wiring board comprising an insulating layer formed from the resin composition according to any one of [1] to
[17] or the cured product of the resin paste according to
[18] .
[22] A semiconductor chip package comprising the printed wiring board according to
[21] and a semiconductor chip mounted on the printed wiring board.
[23] A semiconductor chip package comprising: a semiconductor chip; and a cured product of the resin composition according to any one of [1] to
[17] or the resin paste according to
[18] that encapsulates the semiconductor chip.
[24] A semiconductor device comprising the printed wiring board according to
[21] or the semiconductor chip package according to
[22] or
[23] .
[25] A method for producing a printed wiring board, comprising: forming, on a circuit board, a resin composition layer containing the resin composition according to any one of [1] to
[17] or a resin composition layer containing the resin paste according to
[18] by a compression molding method; and curing the resin composition layer.
[26] A method for producing a semiconductor chip package, comprising: forming, on a semiconductor chip, a resin composition layer containing the resin composition described in any one of [1] to
[17] or the resin paste described in
[18] by a compression molding method; and curing the resin composition layer. Effect of the Invention
[0011] According to the present invention, it is possible to provide a resin composition or resin paste which can obtain a cured product that has little warping, a high elastic modulus, and excellent adhesion to inorganic materials, and which has excellent peelability from film materials; and a cured product, a resin sheet, a printed wiring board, a semiconductor chip package, a semiconductor device, a method for producing a printed wiring board, and a method for producing a semiconductor chip package, which are obtained using the resin composition or resin paste. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The resin composition, resin paste, cured product, resin sheet, printed wiring board, semiconductor chip package, semiconductor device, method for producing a printed wiring board, and method for producing a semiconductor chip package of the present invention will be described in detail below.
[0013] [Resin composition] The resin composition of the present invention includes (A) an epoxy resin, (B) a compound having a radical polymerizable unsaturated group and an alkylene oxide structure and satisfying a specific condition, (C) an acid anhydride, (D) a radical generator, and (E) an inorganic filler, and the mass ratio [b]:[c] of the (B) component to the (C) component is in the range of 0.2:1 to 1.5:1. This resin composition can provide a cured product with small warpage, high elastic modulus, and excellent adhesion to inorganic materials, and has excellent peelability to film materials. By using such a resin composition, it is possible to provide a resin paste, a cured product, a resin sheet, a printed wiring board, a semiconductor chip package, and a semiconductor device that can achieve such effects.
[0014] The resin composition of the present invention may further contain an optional component in combination with the components (A), (B), (C), (D) and (E). Examples of the optional component include (F) a curing accelerator, (G) a compound having a radical polymerizable unsaturated group (excluding compounds having a polyalkylene oxide structure), and (H) other additives. Each component contained in the resin composition will be described in detail below. In the present invention, the content of each component in the resin composition is a value when the non-volatile components in the resin composition are 100 mass %, unless otherwise specified.
[0015] <(A) Epoxy resin> The resin composition of the present invention contains an epoxy resin (A). An epoxy resin refers to a resin having one or more epoxy groups in the molecule. By containing the epoxy resin (A) in the resin composition, a cured product having a crosslinked structure can be obtained.
[0016] Examples of epoxy resins include bixylenol type epoxy resins, bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol S type epoxy resins, bisphenol AF type epoxy resins, dicyclopentadiene type epoxy resins, trisphenol type epoxy resins, naphthol novolac type epoxy resins, phenol novolac type epoxy resins, tert-butyl-catechol type epoxy resins, naphthalene type epoxy resins, naphthol type epoxy resins, anthracene type epoxy resins, glycidylamine type epoxy resins, glycidyl ester type epoxy resins, cresol novolac type epoxy resins, biphenyl type epoxy resins, linear aliphatic epoxy resins, epoxy resins having a butadiene structure, alicyclic epoxy resins, heterocyclic epoxy resins, spiro ring-containing epoxy resins, cyclohexane type epoxy resins, cyclohexane dimethanol type epoxy resins, naphthylene ether type epoxy resins, trimethylol type epoxy resins, tetraphenylethane type epoxy resins, and alkylene oxide type epoxy resins. The epoxy resins may be used alone or in combination of two or more.
[0017] The component (A) preferably contains an epoxy resin having two or more epoxy groups in the molecule, and when the non-volatile components of the component (A) are taken as 100 mass%, it is preferable that usually 50 mass% or more, preferably 60 mass% or more, and more preferably 70 mass% or more is an epoxy resin having two or more epoxy groups in the molecule.
[0018] The epoxy resin may be either (A-1) a liquid epoxy resin or (A-2) a solid epoxy resin. The resin composition may contain (A-1) a liquid epoxy resin and (A-2) a solid epoxy resin in combination. From the viewpoint of obtaining a resin composition having excellent flowability during molding, it is preferable that the (A) component is (A-1) a liquid epoxy resin. If necessary, the (A) component may further contain (A-2) a solid epoxy resin.
[0019] ((A-1) Liquid epoxy resin) (A-1) liquid epoxy resin refers to an epoxy resin that is liquid at a temperature of 20° C. The resin composition preferably contains (A-1) liquid epoxy resin.
[0020] The liquid epoxy resin is preferably a liquid epoxy resin having two or more epoxy groups in the molecule, and more preferably an aromatic liquid epoxy resin having two or more epoxy groups in the molecule. In the present invention, the aromatic epoxy resin means an epoxy resin having an aromatic ring in the molecule.
[0021] Preferred liquid epoxy resins are bisphenol A type epoxy resins, bisphenol F type epoxy resins, bisphenol AF type epoxy resins, naphthalene type epoxy resins, glycidyl ester type epoxy resins, glycidyl amine type epoxy resins, phenol novolac type epoxy resins, alicyclic epoxy resins having an ester skeleton, cyclohexane type epoxy resins, cyclohexane dimethanol type epoxy resins, glycidyl amine type epoxy resins, alkylene oxide type epoxy resins, and epoxy resins having a butadiene structure, and bisphenol A type epoxy resins, naphthalene type epoxy resins, and glycidyl amine type epoxy resins are more preferred.
[0022] Specific examples of liquid epoxy resins include "YX7400" manufactured by Mitsubishi Chemical Corporation; "HP4032", "HP4032D", and "HP-4032-SS" (naphthalene type epoxy resins) manufactured by DIC Corporation; "828US", "jER828EL", "825", and "828EL" (bisphenol A type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER807" and "1750" (bisphenol F type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER152" (phenol novolac type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "630" and "630LSD" (glycidylamine type epoxy resins) manufactured by Mitsubishi Chemical Corporation; ADEK Examples of such epoxy resins include "EP3950L" (glycidylamine type epoxy resin) manufactured by Company A; "ZX1059" (a mixture of bisphenol A type epoxy resin and bisphenol F type epoxy resin) manufactured by Nippon Steel & Sumitomo Metal Chemical Co., Ltd.; "EX-721" (glycidyl ester type epoxy resin) manufactured by Nagase ChemteX Corporation; "Celloxide 2021P" (alicyclic epoxy resin having an ester skeleton) manufactured by Daicel Corporation; "PB-3600" (epoxy resin having a butadiene structure) manufactured by Daicel Corporation; "ZX1658" and "ZX1658GS" (liquid 1,4-glycidylcyclohexane type epoxy resin) manufactured by Nippon Steel & Sumitomo Metal Chemical Co., Ltd. These may be used alone or in combination of two or more types. As illustrated in the examples described later, one of the preferred embodiments is to use one or more liquid epoxy resins selected from "ZX1059" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., "HP-4032-SS" manufactured by DIC Corporation, and "630LSD" manufactured by Mitsubishi Chemical Corporation. From the viewpoint of reducing the warpage of the cured body, it is more preferred to use two or more liquid epoxy resins selected from "ZX1059" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., "HP-4032-SS" manufactured by DIC Corporation, and "630LSD" manufactured by Mitsubishi Chemical Corporation. From the viewpoint of reducing the warpage of the cured body, it is also more preferred to use "ZX1059" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., and two or more liquid epoxy resins selected from "HP-4032-SS" manufactured by DIC Corporation, and "630LSD" manufactured by Mitsubishi Chemical Corporation as liquid epoxy resins.
[0023] The content of the (A-1) component in the resin composition is preferably 1% by mass or more, more preferably 2% by mass or more, even more preferably 3% by mass or more, and particularly preferably 5% by mass or more, based on 100% by mass of the nonvolatile components in the resin composition, from the viewpoint of obtaining the effects of including the (A-1) component (for example, improved handleability (fluidity during molding) of the resin composition, improved compatibility), and from the viewpoint of obtaining a cured product with little warping. The upper limit of the content of the (A-1) component is not particularly limited as long as the effects of the present invention are not excessively impaired, and is, for example, 30% by mass or less or 25% by mass or less, and from the viewpoint of obtaining a cured product with a high elastic modulus, may be 20% by mass or less or 15% by mass or less.
[0024] ((A-2) Solid epoxy resin) A solid epoxy resin refers to an epoxy resin that is solid at a temperature of 20° C. The resin composition may contain only the liquid epoxy resin (A-1) as the component (A), but from the viewpoint of increasing the crosslink density, it is also preferable to contain a solid epoxy resin (A-2) in combination with the liquid epoxy resin (A-1). As the solid epoxy resin, a solid epoxy resin having three or more epoxy groups in the molecule is preferable.
[0025] As the solid epoxy resin, bixylenol type epoxy resin, naphthalene type epoxy resin, naphthalene type tetrafunctional epoxy resin, cresol novolac type epoxy resin, dicyclopentadiene type epoxy resin, trisphenol type epoxy resin, naphthol type epoxy resin, biphenyl type epoxy resin, naphthylene ether type epoxy resin, anthracene type epoxy resin, bisphenol A type epoxy resin, bisphenol AF type epoxy resin, and tetraphenylethane type epoxy resin are preferred, and naphthol type epoxy resin, bisphenol AF type epoxy resin, naphthalene type epoxy resin, and biphenyl type epoxy resin are more preferred.
[0026] Specific examples of solid epoxy resins include "HP4032H" (naphthalene type epoxy resin) manufactured by DIC Corporation; "HP-4700" and "HP-4710" (naphthalene type tetrafunctional epoxy resins) manufactured by DIC Corporation; "N-690" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "N-695" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "HP7200L", "HP-7200", "HP-7200HH", and "HP-7200H" (dicyclopentadiene type epoxy resins) manufactured by DIC Corporation. type epoxy resin); "EXA-7311", "EXA-7311-G3", "EXA-7311-G4", "EXA-7311-G4S", "HP6000", "HP6000L" (naphthylene ether type epoxy resin) manufactured by DIC; "EPPN-502H" (trisphenol type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; "NC7000L" (naphthol novolac type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; "NC3000H", "NC3000", "NC3000L", "N" manufactured by Nippon Kayaku Co., Ltd. C3100 (biphenyl type epoxy resin); Nippon Steel & Sumitomo Metal Chemical's "ESN475V" (naphthol type epoxy resin); Nippon Steel & Sumitomo Metal Chemical's "ESN485" (naphthol novolac type epoxy resin); Mitsubishi Chemical's "YX4000H", "YX4000", and "YL6121" (biphenyl type epoxy resin); Mitsubishi Chemical's "YX4000HK" (bixylenol type epoxy resin); Mitsubishi Chemical's "YX8800" (anthracene type epoxy resin); Osaka Gas Examples of epoxy resins include "PG-100" and "CG-500" manufactured by Mitsubishi Chemical Corporation; "157S70" (bisphenol A novolac type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "YL7760" (bisphenol AF type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "YL7800" (fluorene type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "jER1010" (bisphenol A type epoxy resin) manufactured by Mitsubishi Chemical Corporation; and "jER1031S" (tetraphenylethane type epoxy resin) manufactured by Mitsubishi Chemical Corporation. These may be used alone or in combination of two or more.
[0027] The content of the (A-2) component in the resin composition may be 0% (i.e., not contained) when the non-volatile components in the resin composition are taken as 100% by mass, but from the viewpoint of obtaining the effects of containing the (A-2) component (for example, from the viewpoint of lowering the average linear thermal expansion coefficient, improving heat resistance, or good crosslink density), it is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, even more preferably 0.1% by mass or more, and particularly preferably 0.2% by mass or more. The upper limit of the content of the (A-2) component is preferably less than the content of the (A-1) component. The upper limit of the content of the (A-2) component may be 10% by mass or less, 5% by mass or less, 3% by mass or less, or 1% by mass or less when the non-volatile components in the resin composition are taken as 100% by mass, from the viewpoint of appropriately suppressing the crosslink density.
[0028] When the liquid epoxy resin (A-1) and the solid epoxy resin (A-2) are used in combination as the component (A), the ratio of the amounts thereof (liquid epoxy resin:solid epoxy resin) is preferably in the range of 1:0.01 to 1:0.8 by mass. By setting the ratio of the liquid epoxy resin (A-1) and the solid epoxy resin (A-2) in this range, it is possible to obtain the following effects: i) moderate fluidity is provided during molding, ii) handling is improved when used in the form of a resin composition molded product, and iii) a cured product having sufficient breaking strength can be obtained. From the viewpoint of obtaining the above effects i) to iii) and from the viewpoint of appropriately suppressing the crosslinking density, the ratio of the liquid epoxy resin (A-1) and the solid epoxy resin (A-2) (liquid epoxy resin:solid epoxy resin) is more preferably in the range of 1:0.01 to 1:0.5 by mass, and even more preferably in the range of 1:0.01 to 1:0.1.
[0029] The epoxy equivalent of the (A) component is preferably 50 g / eq. to 5000 g / eq., more preferably 50 g / eq. to 3000 g / eq., even more preferably 70 g / eq. to 2000 g / eq., and even more preferably 70 g / eq. to 1000 g / eq. When it is in this range, the crosslink density of the cured product is sufficient, and a cured product having excellent strength and heat resistance can be obtained. The epoxy equivalent can be measured according to JIS K7236, and is the mass of a resin containing one equivalent of epoxy groups.
[0030] The weight average molecular weight of the component (A) is preferably 100 to 5000, more preferably 250 to 3000, and further preferably 400 to 1500. Here, the weight average molecular weight of the epoxy resin is a polystyrene-equivalent weight average molecular weight measured by gel permeation chromatography (GPC).
[0031] From the viewpoint of enhancing the intended effects of the present invention, the content of the (A) component in the resin composition is preferably 1% by mass or more, more preferably 2% by mass or more, even more preferably 3% by mass or more, and particularly preferably 5% by mass or more, when the non-volatile components in the resin composition are taken as 100% by mass. The upper limit of the (A) component content is not particularly limited as long as the effects of the present invention are not excessively impaired, but is, for example, 30% by mass or less or 25% by mass or less, and from the viewpoint of obtaining a cured product with a high elastic modulus, it may be 20% by mass or less or 15% by mass or less.
[0032] From the viewpoint of enhancing the intended effects of the present invention, the content of the (A) component is preferably 10% by mass or more, more preferably 15% by mass or more, even more preferably 20% by mass or more, and particularly preferably 25% by mass or more, when the non-volatile components in the resin composition other than the (E) inorganic filler are taken as 100% by mass. The upper limit of the (A) component content is not particularly limited as long as the effects of the present invention are not excessively impaired, but is, for example, 70% by mass or less or 65% by mass or less, and from the viewpoint of obtaining a cured product with little warping, it may be 50% by mass or less, 48% by mass or less, or 45% by mass or less.
[0033] The content (mass) of the (A) component in the resin composition is preferably at least one-fifth, more preferably at least one-fourth, and even more preferably at least three-tenths of the total content (mass) of the (B) component and the (C) component, from the viewpoint of enhancing the intended effects of the present invention. The percentage of the mass ratio value [a] / ([b]+[c]) of the content of the (A) component to the total content of the (B) component and the (C) component in the resin composition is preferably at least 20% by mass, more preferably at least 25% by mass, and even more preferably at least 30% by mass. The upper limit of the percentage of the mass ratio value [a] / ([b]+[c]) may be 100% by mass or less, 90% by mass or less, or 80% by mass or less, from the viewpoint of further enhancing the intended effects of the present invention.
[0034] <(B) Compound Having a Radically Polymerizable Unsaturated Group and a Polyalkylene Oxide Structure and Satisfying Certain Conditions> The resin composition of the present invention contains (B) a compound having a radically polymerizable unsaturated group and a polyalkylene oxide structure and satisfying a specific condition (hereinafter, also referred to as "the radically reactive polyRO compound of the present invention"). Two or more of the radically reactive polyRO compounds of the present invention may be used. By containing the resin composition in combination with the components (A) and (C), the component (B) contributes to at least a part of the desired effects of the present invention (warping, inorganic material adhesion, elastic modulus, and film material peelability), and in particular, the flexibility provided by the polyalkylene oxide structure is considered to greatly contribute to reducing warping of the cured product and improving inorganic material adhesion.
[0035] The radical polymerizable unsaturated group of the (B) component may be a group containing an ethylenic carbon-carbon double bond. Specific examples include one or more selected from vinyl, allyl, 1-butenyl, 2-butenyl, acryloyl, methacryloyl, fumaroyl, maleoyl, vinylphenyl, styryl, and cinnamoyl groups. The (B) component may contain two or more radical polymerizable unsaturated groups in one molecule. From the viewpoint of increasing reactivity, the radical polymerizable unsaturated group of the (B) component preferably contains one or more selected from methacryloyl and acryloyl groups, and from the viewpoint of controlling reactivity, it is more preferable that the radical polymerizable unsaturated group contains a methacryloyl group. In addition, from the viewpoint of obtaining a cured product with little warping, the (B) component preferably has a radical polymerizable unsaturated group at a molecular end.
[0036] The specific condition that the component (B) must satisfy is the following formula (1): E / N-(100×N)≧50 (1) (In formula (1), E represents the equivalent (g / eq.) of the radically polymerizable unsaturated group, and N represents the number of radically polymerizable unsaturated groups in the molecule and is an integer of 1 or more.) The equivalent of the radical polymerizable unsaturated group is the mass of the resin containing one equivalent of the radical polymerizable unsaturated group. By satisfying this condition, the desired effect of the present invention can be achieved. N can be, for example, 5 or less, 4 or less, or 3 or less.
[0037] The above formula (1) means that the molecular weight per equivalent (corresponding to the term "E / N" in formula (1)) must be sufficiently large according to the number N of radically polymerizable unsaturated groups. Specifically, when N is 1, the above formula (1) means that the molecular weight of the compound must be 150 or more, and when N is 2, the equivalent (g / eq.) of the radically polymerizable unsaturated group of the compound must be 500 or more (i.e., the molecular weight is 1000 or more). In this way, it is considered that the molecular weight per equivalent of the (B) component is large according to the number of radically polymerizable unsaturated groups, which tends to suppress the increase in warpage caused by the effect of cure shrinkage of the resin composition.
[0038] Component (B) includes, for example, one or more compounds selected from a compound in which N in formula (1) is 1 and a compound in which N in formula (1) is 2. Here, as described above, a compound in which N in formula (1) is 1 is a compound whose molecular weight is 150 or more. Similarly, a compound in which N in formula (1) is 2 is a compound whose radically polymerizable unsaturated group has an equivalent weight (g / eq.) of 500 or more.
[0039] When the component (B) is a compound in which N in the above formula (1) is 1, the equivalent of the radical polymerizable unsaturated group may be 150 g / eq. or more, and the lower limit may be 250 g / eq. or more or 400 g / eq. or more. When the component (B) is a compound in which N in the above formula (1) is 2, the equivalent of the radical polymerizable unsaturated group may be 500 g / eq. or more, and the lower limit may be 510 g / eq. or more or 600 g / eq. or more. The upper limit of the equivalent of the radical polymerizable unsaturated group of the radical reactive polyRO compound of the present invention may be 4500 g / eq. or less, from the viewpoint of enhancing the intended effect of the present invention. From the viewpoint of enhancing the fluidity of the resin composition (the viscosity of the resin composition or the filling property of the inorganic filler), the upper limit of the equivalent of such radical polymerizable unsaturated group is preferably 3000 g / eq. or less, more preferably 2000 g / eq. or less, and even more preferably 1500 g / eq. or less. When the resin composition contains a plurality of types of the radically reactive polyRO compounds of the present invention as the component (B), it is preferable that the equivalent weight of the radically polymerizable unsaturated group of each compound satisfies the above range.
[0040] In this embodiment, the polyalkylene oxide structure of the component (B) is represented by the formula (2): -(R B O) n In formula (2), n is an integer of 2 or more, and R B are each independently an alkylene group having 1 to 6 carbon atoms which may have a substituent. The (B) component contains at least one polyalkylene oxide structure in one molecule, and from the viewpoint of obtaining a cured product having excellent adhesion to inorganic materials, it is preferable that the (B) component contains two or more polyalkylene oxide structures in one molecule, and in this case, the multiple polyalkylene oxide structures may be the same or different. When the radical-reactive polyRO compound of the present invention contains multiple polyalkylene oxide structures which may be the same or different, the repeat number of the alkylene oxide structure per molecule (hereinafter also referred to as the "RO number") is represented by the sum of the numerical values represented by n in the formula (2) representing each alkylene oxide structure. That is, the RO number is the number of divalent groups R in the above formula (2) contained in one molecule of the radical-reactive polyRO compound of the present invention. BIt stands for the number O.
[0041] In the above formula (2), from the viewpoint of obtaining a cured product having excellent adhesion, n is an integer of 2 or more, preferably 4 or more, more preferably greater than 9 or greater, and even more preferably greater than 11. From the viewpoint of increasing the fluidity of the resin composition (the viscosity of the resin composition or the filling property of the inorganic filler), n is usually an integer of 101 or less, preferably 90 or less, more preferably 68 or less, and even more preferably 65 or less.
[0042] In the above formula (2), R B The number of carbon atoms in the alkylene group contained in the above formula (2) is usually 1 to 6, and from the viewpoint of obtaining a cured product having excellent adhesion to inorganic materials by increasing the content ratio of oxygen atoms as polar sites contained in the polyalkylene oxide structure, the number of carbon atoms is preferably 1 to 5, more preferably 1 to 4, even more preferably 1 to 3, and particularly preferably 1 to 2, and from the viewpoint of obtaining a cured product with reduced warping due to the influence of cure shrinkage, the number of carbon atoms is preferably 2 to 5, more preferably 2 to 4, and even more preferably 2 to 3. B From the viewpoint of obtaining a cured product having excellent adhesion to inorganic materials and reduced warping due to cure shrinkage, the number of carbon atoms in the alkylene group contained in the above formula (2) is typically 2. B At least one group R B It is a particularly preferred example that contains an ethylene group.
[0043] In the above formula (2), R B The alkylene group contained in the formula (1) generally does not have a substituent, but may have a substituent. Examples of such a substituent include an alkyl group having 1 to 3 carbon atoms, a halogen atom, -OH, -OC 1-5 Alkyl group, -N(C 1-5 Alkyl group) 2, C 1-5 Alkyl group, C 6-10 Aryl groups, -NH2, -CN, -C(O)OC 1-5Examples of such substituents include an alkyl group, -COOH, -C(O)H, an epoxy group, and -NO2. From the viewpoint of increasing the reactivity with the (A) component and / or the (C) component, the epoxy group, -OH, -NH2, and -COOH are preferred as such substituents. Even if the radical-reactive polyRO compound of the present invention has an epoxy group in the molecule, it is classified as the (B) component as long as it is a compound having a radically polymerizable unsaturated group and a polyalkylene oxide structure and satisfies the above-mentioned specific conditions. Thus, the radical-reactive polyRO compound of the present invention preferably contains a group reactive with the (A) component and / or the (C) component, preferably a group reactive with the (A) component, which allows the formation of a crosslinked structure, and allows the production of a cured product with a high elastic modulus and excellent handleability. In this case, one or more radical-reactive polyRO compounds containing a group reactive with the (A) component and / or the (C) component and one or more radical-reactive polyRO compounds not containing a group reactive with the (A) component and / or the (C) component may be used in combination. In addition, R B From the viewpoint of obtaining a cured product having a low dielectric tangent, it is preferable that halogen atoms are excluded from the substituents of the alkylene groups contained in the above. The substituents may be contained alone or in combination of two or more kinds.
[0044] Specific examples of the polyalkylene oxide structure contained in component (B) include a polyethylene oxide structure (-(C2H4O) n -; where n is the same as n in formula (2). ), polypropylene oxide structure (-(CHO) n -; where n is the same as n in formula (2). ), poly n-butylene oxide structure (-(C4H8O) n-; where n is the same as n in formula (2). ), poly(ethylene oxide-co-propylene oxide) structure, poly(ethylene oxide-ran-propylene oxide) structure, poly(ethylene oxide-alt-propylene oxide) structure and poly(ethylene oxide-block-propylene oxide) structure can be mentioned. Of these, from the viewpoint of obtaining a cured product having excellent adhesion to inorganic materials, the polyalkylene oxide structure of the (B) component is preferably either the above polyethylene oxide structure or the above polypropylene oxide structure, and more preferably the above polyethylene oxide structure. However, epoxy resins having an alkylene oxide structure are excluded from the (B) component.
[0045] When the radical-reactive polyRO compound of the present invention contains one or more polyethylene oxide structures in one molecule, the number of repeating ethylene oxide structures per molecule (hereinafter also referred to as "EO number") is 2 or more, and from the viewpoint of obtaining a cured product with excellent adhesion, it is preferably an integer of 4 or more, more preferably an integer greater than or equal to 9, even more preferably an integer of 11 or more, and usually is 101 or less, and from the viewpoint of increasing the fluidity of the resin composition (the viscosity of the resin composition or the filling property of the inorganic filler), it is preferably an integer of 90 or less, more preferably 68 or less, and even more preferably 65 or less. The EO number refers to the number of repeating ethylene oxide structures per molecule in the radical-reactive polyRO compound of the present invention, which is represented by the formula 1 above. B The number of POs refers to the number of divalent groups R in the above formula 1 contained in one molecule of the radical-reactive polyRO compound of the present invention. B This means the number when O is represented by -(C3H6O)-.
[0046] Specific examples of the component (B) include one or more radically polymerizable unsaturated groups selected from the group consisting of vinyl groups, allyl groups, 1-butenyl groups, 2-butenyl groups, acryloyl groups, methacryloyl groups, fumaroyl groups, maleoyl groups, vinylphenyl groups, styryl groups, and cinnamoyl groups, and a polyethylene oxide structure (-(C2H4O) n-; where n is the same as n in formula (2). ), polypropylene oxide structure (-(CHO) n -; where n is the same as n in formula (2). ), poly n-butylene oxide structure (-(C4H8O) n -; where n is the same as n in formula (2).) and a polyalkylene oxide structure selected from a poly(ethylene oxide-co-propylene oxide) structure, a poly(ethylene oxide-ran-propylene oxide) structure, a poly(ethylene oxide-alt-propylene oxide) structure, and a poly(ethylene oxide-block-propylene oxide) structure, which satisfies the above formula (1), can be mentioned. From the viewpoint of obtaining a cured product with excellent heat resistance, the (B) component preferably contains one or more monovalent or divalent aromatic hydrocarbon groups in the molecule, and preferably contains two or more monovalent or divalent aromatic hydrocarbon groups in the molecule. Examples of the monovalent or divalent aromatic hydrocarbon group include a phenyl group, a 1-naphthyl group, a 2-naphthyl group, a phenylene group, a 1-naphthylene group, and a 2-naphthylene group. Two or more monovalent or divalent aromatic hydrocarbon groups may be bonded to each other directly or via a linking group, and such bonds may form, for example, a bisphenol structure, preferably a bisphenol A structure.
[0047] As the component (B), commercially available products can be used. Commercially available products include monofunctional acrylates "AM-90G" (EO number: 9), "AM-130G" (EO number: 13), and "AMP-20GY" (EO number: 2) manufactured by Shin-Nakamura Chemical Co., Ltd.; bifunctional acrylates "A-1000" (EO number: 23), "A-B1206PE" (EO number: 6, PO number: 12, RO number: 18), "A-BPE-20" (EO number: 17), and "A-BPE-30" (EO number: 30); Monofunctional methacrylates "M-20G" (EO number: 2), "M-40G" (EO number: 4), "M-90G" (EO number: 9), "M-130G" (EO number: 13), "M-230G" (EO number: 23); and bifunctional methacrylates "23G" (EO number: 23), "BPE-900" (EO number: 17), "BPE-1300N" (EO number: 30), "1206PE" (EO number: 6, RO number: 18), etc. Other examples include "Light Ester BC" (EO number: 2), "Light Ester 041MA" (EO number: 30), "Light Acrylate EC-A" (EO number: 2), "Light Acrylate EHDG-AT" (EO number: 18) manufactured by Kyoeisha Chemical Co., Ltd., "FA-023M" manufactured by Hitachi Chemical Co., Ltd., and NOF Corporation's "Blenmer (registered trademark) PME-4000" (EO number: 90), "Blenmer (registered trademark) 50POEO-800B" (EO number: 8, PO number: 7), "Blenmer (registered trademark) PLE-200" (EO number: 4), "Blenmer (registered trademark) PLE-1300" (EO number: 30), "Blenmer (registered trademark) PSE-1300" (EO number: 30), "Blenmer (registered trademark) 43PAPE-600B" (EO number: 6, PO number: 6), and "Blenmer (registered trademark) ANP-300" (PO number: 5). Of these, from the viewpoint of enhancing the intended effects of the present invention, for example, one or more commercially available products selected from "M-230G", "M-130G", "23G", "M-40G", "M-90G" and "BPE-1300N" can be used.
[0048] The molecular weight of the radical-reactive polyRO compound of the present invention is 150 or more, 250 or more, or 400 or more in the case of a compound in which N in the above formula (1) is 1. The molecular weight of the radical-reactive polyRO compound of the present invention (B) is 1000 or more, 1020 or more, or 1200 or more in the case of a compound in which N in the above formula (1) is 2. From the viewpoint of increasing the fluidity of the resin composition (the viscosity of the resin composition or the filling property of the inorganic filler), the upper limit of the molecular weight of the radical-reactive polyRO compound of the present invention is, for example, 5000 or less, preferably 3000 or less, more preferably 2500 or less, more preferably 2000 or less, and even more preferably 1500 or less. When the (B) component is a commercially available product, it is preferable that the molecular weight as a nominal value is within the above range. When the (B) component is a polymer, it is preferable that the weight average molecular weight or number average molecular weight is within the above range. Here, when the component (B) is a polymer, the weight average molecular weight or number average molecular weight is the weight average molecular weight or number average molecular weight in terms of polystyrene measured by gel permeation chromatography (GPC).
[0049] The content of the (B) component is not limited as long as the mass ratio of the (B) component to the (C) component is within the range described below, but when the non-volatile components in the resin composition are taken as 100 mass%, from the viewpoint of enhancing the intended effects of the present invention, it is 0.1 mass% or more, 0.2 mass% or more, or 0.3 mass% or more, and from the viewpoint of further enhancing the intended effects of the present invention, it is preferably 1 mass% or more, more preferably 1.5 mass% or more, and even more preferably 2 mass% or more. The upper limit is not particularly limited, but is, for example, 20 mass% or less, 15 mass% or less, and is preferably less than the content of the (A) component when the non-volatile components in the resin composition are taken as 100 mass%.
[0050] The content of the (B) component is not limited as long as the mass ratio of the (B) component to the (C) component is within the range described below, but when the non-volatile components in the resin composition other than the (E) inorganic filler are taken as 100 mass%, from the viewpoint of enhancing the intended effects of the present invention, the content is preferably 10 mass% or more, more preferably 13 mass% or more, even more preferably 15 mass% or more, and particularly preferably 16 mass% or more. The upper limit is not particularly limited, but from the viewpoint of enhancing the intended effects of the present invention, it is preferably 40 mass% or less, more preferably 39 mass% or less, even more preferably 38 mass% or less, and from the viewpoint of obtaining a cured product with a higher elastic modulus, it may be 35 mass% or less or 30 mass% or less.
[0051] <(C) Acid anhydride> The resin composition contains an acid anhydride (C). An acid anhydride refers to a compound having an acid anhydride group. The (C) component may be an acid anhydride that is liquid at a temperature of 20° C. (hereinafter also referred to as a "liquid acid anhydride"), or may be an acid anhydride that is solid at a temperature of 20° C. (hereinafter also referred to as a "solid acid anhydride"), or may be a combination of these. From the viewpoint of increasing the fluidity of the resin composition (the viscosity of the resin composition or the filling property of the inorganic filler), the (C) component is preferably a liquid acid anhydride. If necessary, the (C) component may further contain a solid acid anhydride. By the resin composition containing the (C) component in combination with the (A) component and the (B) component, the (C) component contributes to at least a part of the desired effects of the present invention (warping, inorganic material adhesion, elastic modulus, and film material peelability), and in particular, as illustrated in the section of examples, the resin composition containing the (C) component tends to have excellent film material releasability.
[0052] The acid anhydride (C) can react with the component (A) to cure the resin composition. Specific examples of the acid anhydride include phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, hydrogenated methylnadic anhydride, trialkyltetrahydrophthalic anhydride, dodecenyl succinic anhydride, 5-(2,5-dioxotetrahydro-3-furanyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic anhydride, trimellitic anhydride, pyromellitic anhydride, and benzophenonetetracarboxylic dianhydride. Examples of such anhydrides include styrene-maleic acid resins, biphenyltetracarboxylic dianhydride, naphthalenetetracarboxylic dianhydride, oxydiphthalic dianhydride, 3,3'-4,4'-diphenylsulfonetetracarboxylic dianhydride, 1,3,3a,4,5,9b-hexahydro-5-(tetrahydro-2,5-dioxo-3-furanyl)-naphtho[1,2-C]furan-1,3-dione, ethylene glycol bis(anhydrotrimellitate), and polymeric acid anhydrides such as styrene-maleic acid resins, which are copolymers of styrene and maleic acid.
[0053] Commercially available acid anhydrides include "HNA-100", "MH-700", "MTA-15", "DDSA", and "OSA" manufactured by New Japan Chemical Co., Ltd., "YH-306" and "YH-307" manufactured by Mitsubishi Chemical Corporation, and "HN-2200" and "HN-5500" manufactured by Hitachi Chemical Co., Ltd.
[0054] In the present invention, the mass ratio of the (B) component to the (C) component, [b]:[c], is within the range of 0.2:1 to 1.5:1, preferably 0.25:1 to 1.35:1, and more preferably 0.3:1 to 1.3:1, from the viewpoint of achieving the desired effects of the present invention.
[0055] The ratio (equivalent ratio) (c) / (a) of the sum of values obtained by dividing the amount (g) of component (C) by the equivalent (g / eq.) of the acid anhydride groups in component (C) to the sum of values obtained by dividing the amount (g) of component (A) by the equivalent (g / eq.) of the epoxy groups in component (A) is preferably 0.4 or more, more preferably 0.5 or more, and even more preferably 0.6 or more, from the viewpoint of achieving the intended effects of the present invention, and is preferably 1.6 or less, more preferably 1.5 or less, and even more preferably 1.4 or less, from the viewpoint of obtaining a cured product with little warping.
[0056] The content of the (C) component is not limited as long as the mass ratio of the (B) component to the (C) component is within the above-mentioned range, but when the non-volatile components in the resin composition other than the (E) inorganic filler are taken as 100 mass%, it may be 10 mass% or more or 15 mass% or more from the viewpoint of enhancing the expected effects of the present invention. From the viewpoint of obtaining a resin composition layer (compression molded product) having excellent film material release properties, the content of the (C) component is preferably 17 mass% or more, more preferably 20 mass% or more, and even more preferably 23 mass% or more, when the non-volatile components in the resin composition other than the (E) inorganic filler are taken as 100 mass%. The upper limit is not particularly limited, but is, for example, 60 mass% or less, and from the viewpoint of enhancing the expected effects of the present invention, it is preferably 58 mass% or less, more preferably 55 mass% or less, and from the viewpoint of obtaining a cured product with less warping, it may be 49 mass% or less or 48 mass% or less.
[0057] The content of the (C) component is not limited as long as the mass ratio of the (B) component to the (C) component is within the above-mentioned range, but when the non-volatile components in the resin composition are taken as 100 mass%, from the viewpoint of enhancing the intended effect of the present invention, it is preferably 0.5 mass% or more, more preferably 1 mass% or more, and even more preferably 2 mass% or more or 3 mass% or more. The upper limit is not particularly limited, but is, for example, 40 mass% or less, 30 mass% or less, or 20 mass%, and is preferably less than twice the content of the (A) component when the non-volatile components in the resin composition are taken as 100 mass%.
[0058] <(D) Radical Generator> The resin composition of the present invention contains a radical generator (D). As the component (D), it is preferable to use a thermal radical generator. The thermal radical generator usually generates radicals by applying thermal energy.
[0059] Examples of the thermal radical generator include dialkyl peroxides such as di-t-butyl peroxide, dicumyl peroxide, and t-hexylperoxy-2-ethylhexanoate; diacyl peroxides such as lauroyl peroxide, benzoyl peroxide, benzoyltoluyl peroxide, and toluyl peroxide; peroxyesters such as t-butyl peracetate, t-butyl peroxyoctoate, and t-butyl peroxybenzoate; ketone peroxides; peroxycarbonates; peroxyketals such as 1,1-di(t-amylperoxy)cyclohexane; 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2-methylbutyronitrile), and the like. azonitrile compounds such as 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), azoamide compounds such as 2,2'-azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propionamide}; azoamidine compounds such as 2,2'-azobis(2-amidinopropane) dihydrochloride and 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride; azoalkane compounds such as 2,2'-azobis(2,4,4-trimethylpentane) and 4,4'-azobis(4-cyanopentanoic acid); azo compounds having an oxime skeleton such as 2,2'-azobis(2-methylpropionamide oxime), and azo compounds such as dimethyl 2,2'-azobis(isobutyrate). The thermal radical generator may be used alone or in combination of two or more kinds at any ratio. Azo compounds usually generate nitrogen when decomposed, and therefore tend to generate voids in the cured product of the resin composition, but can be preferably used in the present invention. As the thermal radical generator, of the peroxide-based thermal radical generator and the azo compound-based thermal radical generator exemplified above, it is more preferable to use the peroxide-based thermal radical generator from the viewpoint of suppressing the generation of voids.
[0060] The thermal radical generator is preferably one that is active at medium temperature. Specifically, the (D) component is preferably one or more selected from thermal radical generators whose 10-hour half-life temperature T10 (℃) is in the range of 50℃ to 110℃, more preferably one or more selected from thermal radical generators whose 10-hour half-life temperature T10 (℃) is in the range of 50℃ to 100℃, and from the viewpoint of obtaining a cured product with less warping, it is even more preferable that the (D) component is one or more selected from thermal radical generators whose 10-hour half-life temperature T10 (℃) is in the range of 50℃ to 80℃. Examples of such commercially available products include "Luperox 531M80" manufactured by Arkema Fuji Co., Ltd., "Perhexyl (registered trademark) O" manufactured by NOF Corporation, and "MAIB" manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.
[0061] Also, preferably, the (D) component is one or more selected from radical generators in which the difference ΔT (°C) between the mold temperature Tc (°C) during compression molding and the 10-hour half-life temperature T10 (°C) of the (D) component is in the range of 20°C to 80°C, more preferably 30°C to 80°C. In other words, when the mold temperature Tc (°C) used during compression molding is known, it is preferable to select a thermal radical generator whose difference ΔT (°C) satisfies the above range as the (D) component to be contained in the resin composition of the present invention. This makes it possible to obtain a cured product with less warping.
[0062] The content of the (D) component is not limited as long as the desired effect of the present invention is achieved, but when the non-volatile components in the resin composition are taken as 100 mass%, it may be, for example, 0.02 mass% to 5 mass%, 0.03 mass% to 4 mass%, or 0.04 mass% to 3 mass%. The content of the (D) component is not limited as long as the desired effect of the present invention is achieved, but when the non-volatile components in the resin composition other than the (E) inorganic filler are taken as 100 mass%, it may be, for example, 0.02 mass% to 5 mass%, 0.1 mass% to 4 mass%, or 0.2 mass% to 3 mass%.
[0063] <(E) Inorganic filler> The resin composition of the present invention contains an inorganic filler (E). When the resin composition contains the component (E), a cured product with little warping can be obtained.
[0064] The material of the inorganic filler is not particularly limited as long as it is an inorganic compound, and examples thereof include silica, alumina, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium titanate zirconate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate. Among these, silica is particularly suitable. Examples of silica include amorphous silica, fused silica, crystalline silica, synthetic silica, and hollow silica. As the silica, spherical silica is preferable. The inorganic filler may be used alone or in combination of two or more. Commercially available silica products include "SO-C2" and "SO-C1" manufactured by Admatechs Co., Ltd., and "UFP-30" and "UFP-40" manufactured by Denka Co., Ltd.
[0065] The average particle size of the inorganic filler is usually 30 μm or less, and from the viewpoint of enhancing the intended effects of the present invention, it is preferably 25 μm or less, more preferably 20 μm or less, and even more preferably 18 μm or less. The lower limit of the average particle size may be 1 nm (0.001 μm) or more, 5 nm or more, or 10 nm or more, etc., but from the viewpoint of enhancing the intended effects of the present invention, it is preferably 1.0 μm or more, more preferably 1.2 μm or more, and even more preferably 1.4 μm or more.
[0066] The average particle size of the inorganic filler can be measured by a laser diffraction / scattering method based on the Mie scattering theory. Specifically, the particle size distribution of the inorganic filler is created on a volume basis using a laser diffraction / scattering particle size distribution measuring device, and the median diameter is used as the average particle size. The measurement sample can be prepared by weighing 100 mg of the inorganic filler and 10 g of methyl ethyl ketone into a vial and dispersing the mixture by ultrasonic waves for 10 minutes. The measurement sample is measured using a laser diffraction particle size distribution measuring device with blue and red light wavelengths as the light source, and the particle size distribution of the inorganic filler on a volume basis is measured using a flow cell method. The average particle size is calculated as the median diameter from the particle size distribution obtained. An example of a laser diffraction particle size distribution measuring device is the "LA-960" manufactured by Horiba, Ltd.
[0067] From the viewpoint of improving embeddability, the inorganic filler is preferably treated with a surface treatment agent, more preferably with one or more surface treatment agents such as fluorine-containing silane coupling agents, aminosilane coupling agents, epoxysilane coupling agents, mercaptosilane coupling agents, silane coupling agents, alkoxysilane compounds, organosilazane compounds, acryloylsilane compounds, methacryloylsilane compounds, titanate coupling agents, etc., and even more preferably with an aminosilane silane coupling agent. The surface treatment agent preferably has a functional group that reacts with other components, such as resins, such as an epoxy group, an amino group, or a mercapto group, and more preferably the functional group is bonded to the terminal group. Commercially available surface treatment agents include, for example, the silane coupling agent "KBM403" (3-glycidoxypropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., the silane coupling agent "KBM803" (3-mercaptopropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., the silane coupling agent "KBE903" (3-aminopropyltriethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., the silane coupling agent "KBM573" (N-phenyl-3-aminopropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd. Examples of suitable surface treatment agents include silane coupling agents "KBM573", "KBM-4803", and "KBM403" manufactured by Shin-Etsu Chemical Co., Ltd. As surface treatment agents, it is preferable to use silane coupling agents "KBM573", "KBM-4803", and "KBM403" manufactured by Shin-Etsu Chemical Co., Ltd. From the viewpoint of obtaining a cured product with less warpage, long-chain silane coupling agents are preferred, and long-chain epoxy silane coupling agents having an epoxy group are particularly preferred.
[0068] With regard to the degree of surface treatment with the surface treatment agent, from the viewpoint of improving embeddability, etc., the surface treatment is preferably performed with 0.2 parts by mass to 5 parts by mass of the surface treatment agent per 100 parts by mass of component (E), more preferably with 0.2 parts by mass to 4 parts by mass, and even more preferably with 0.3 parts by mass to 3 parts by mass.
[0069] The degree of surface treatment with a surface treatment agent can be evaluated by the amount of carbon per unit surface area of the inorganic filler. From the viewpoint of improving embeddability, the amount of carbon per unit surface area of the inorganic filler is 0.02 mg / m 2 More than 0.1 mg / m is preferable. 2 More preferably, 0.2 mg / m or more 2 On the other hand, from the viewpoint of suppressing an increase in the melt viscosity of the resin varnish and the melt viscosity in the form of a sheet, it is more preferable that the content is 1 mg / m 2 Less than 0.8 mg / m is preferred. 2 Less than 0.5 mg / m is more preferable. 2 The following is even more preferred:
[0070] The amount of carbon per unit surface area of the inorganic filler can be measured after the surface-treated inorganic filler is washed with a solvent (e.g., methyl ethyl ketone (MEK)). Specifically, a sufficient amount of MEK as a solvent is added to the inorganic filler that has been surface-treated with a surface treatment agent, and ultrasonic cleaning is performed at 25°C for 5 minutes. After removing the supernatant and drying the non-volatile components, the amount of carbon per unit surface area of the inorganic filler can be measured using a carbon analyzer. The carbon analyzer that can be used is the "EMIA-320V" manufactured by Horiba, Ltd.
[0071] The specific surface area of component (E) is preferably 0.3 m 2 / g or more, more preferably 0.5m 2 / g or more, particularly preferably 0.7m 2 / g or more. There is no particular upper limit, but it is preferably 60m 2 / g or less, 50m 2 / g or less or 40m 2The specific surface area is determined according to the BET method by adsorbing nitrogen gas onto the surface of the sample using a BET fully automatic specific surface area measuring device ("Macsorb HM-1210" manufactured by Mountech Co., Ltd.) and calculating the specific surface area using the BET multipoint method.
[0072] The content of the (E) component in the resin composition is preferably high. When the non-volatile components in the resin composition are taken as 100% by mass, from the viewpoint of obtaining a cured product with less warping, the content is preferably 70% by mass or more, more preferably 71% by mass or more, and even more preferably 72% by mass or more. The upper limit will naturally be determined depending on the contents of the other components, but may be, for example, 95% by mass or less, 93% by mass or less, or 90% by mass or less.
[0073] <(F) Curing accelerator> The resin composition may contain (F) a curing accelerator. Examples of the curing accelerator include phosphorus-based curing accelerators, amine-based curing accelerators, guanidine-based curing accelerators, imidazole-based curing accelerators, and metal-based curing accelerators. Phosphorus-based curing accelerators and imidazole-based curing accelerators are preferred, and imidazole-based curing accelerators are more preferred. The curing accelerator may be used alone or in combination of two or more.
[0074] Examples of the phosphorus-based curing accelerator include triphenylphosphine, phosphonium borate compounds, tetraphenylphosphonium tetraphenylborate, n-butylphosphonium tetraphenylborate, tetrabutylphosphonium decanoate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, butyltriphenylphosphonium thiocyanate, and the like, with triphenylphosphine and tetrabutylphosphonium decanoate being preferred.
[0075] Examples of the amine-based curing accelerator include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine (DMAP), benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 1,8-diazabicyclo(5,4,0)-undecene, and 4-dimethylaminopyridine and 1,8-diazabicyclo(5,4,0)-undecene are preferred. Examples of commercially available amine-based curing accelerators include "DMP-30" manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.
[0076] Examples of the guanidine curing accelerator include dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, and 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene. Examples of the guanidine-based hardening accelerator include 1-methyl biguanide, 1-ethyl biguanide, 1-n-butyl biguanide, 1-n-octadecyl biguanide, 1,1-dimethyl biguanide, 1,1-diethyl biguanide, 1-cyclohexyl biguanide, 1-allyl biguanide, 1-phenyl biguanide, and 1-(o-tolyl) biguanide. Dicyandiamide and 1,5,7-triazabicyclo[4.4.0]dec-5-ene are preferred. As a commercially available product of the guanidine-based hardening accelerator, for example, one or more selected from pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, and 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene can be used.
[0077] Examples of the imidazole curing accelerator include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2, 4-Diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-furan Examples of the imidazole compounds include imidazole compounds such as 2-ethyl-4-methyl-5-hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, and 2-phenylimidazoline, as well as adducts of imidazole compounds and epoxy resins. Of these, 2-ethyl-4-methylimidazole and 1-benzyl-2-phenylimidazole are preferred.
[0078] As the imidazole-based curing accelerator, commercially available products may be used, for example, imidazole compounds "1B2PZ" and "2E4MZ" manufactured by Shikoku Chemical Industry Co., Ltd., "P200-H50" manufactured by Mitsubishi Chemical Corporation, and "2MA-OK-PW" manufactured by Shikoku Chemical Industry Co., Ltd.
[0079] Examples of metal-based curing accelerators include organometallic complexes or organometallic salts of metals such as cobalt, copper, zinc, iron, nickel, manganese, and tin. Specific examples of organometallic complexes include organocobalt complexes such as cobalt(II) acetylacetonate and cobalt(III) acetylacetonate, organocopper complexes such as copper(II) acetylacetonate, organozinc complexes such as zinc(II) acetylacetonate, organoiron complexes such as iron(III) acetylacetonate, organonickel complexes such as nickel(II) acetylacetonate, and organomanganese complexes such as manganese(II) acetylacetonate. Examples of organometallic salts include zinc octylate, tin octylate, zinc naphthenate, cobalt naphthenate, tin stearate, and zinc stearate.
[0080] When the resin composition contains the (F) component, the content of the (F) component may be, for example, 0.01% to 5% by mass, 0.05% to 4% by mass, or 0.08% to 3% by mass, when the nonvolatile components in the resin composition are taken as 100% by mass. The content of the (F) component may be, for example, 0.05% to 10% by mass, 0.1% to 5% by mass, or 0.2% to 3% by mass, when the nonvolatile components in the resin composition other than the (E) inorganic filler are taken as 100% by mass.
[0081] <(G) Compound having a radically polymerizable unsaturated group (excluding compounds having a polyalkylene oxide structure)> It is also preferable that the resin composition of the present invention further contains (G) a compound having a radically polymerizable unsaturated group (excluding compounds having a polyalkylene oxide structure). Two or more kinds of (G) components may be used as the (G) component. It is considered that the resin composition further contains the (G) component in addition to the (B) component, so that the radical polymerization reaction proceeds in an accelerated or competitive manner, and the (G) component exerts part of the function of the (B) component, thereby enhancing the intended effect of the present invention.
[0082] The radical polymerizable unsaturated group of the (G) component may be a group containing an ethylenic carbon-carbon double bond. Specific examples include one or more selected from a vinyl group, an allyl group, a 1-butenyl group, a 2-butenyl group, an acryloyl group, a methacryloyl group, a fumaroyl group, a maleoyl group, a vinylphenyl group, a styryl group, a cinnamoyl group, and a maleimide group. The (G) component may contain two or more radical polymerizable unsaturated groups in one molecule. From the viewpoint of increasing reactivity, the radical polymerizable unsaturated group of the (G) component preferably contains one or more selected from a methacryloyl group and an acryloyl group, and from the viewpoint of controlling reactivity, it is more preferable that the radical polymerizable unsaturated group contains a methacryloyl group.
[0083] Specific examples of the (G) component include compounds containing one or more radically polymerizable unsaturated groups selected from vinyl, allyl, 1-butenyl, 2-butenyl, acryloyl, methacryloyl, fumaroyl, maleoyl, vinylphenyl, styryl, cinnamoyl, and maleimide groups. From the viewpoint of obtaining a cured product with excellent heat resistance, the (G) component preferably contains one or more monovalent or divalent aromatic hydrocarbon groups in the molecule, and preferably contains two or more monovalent or divalent aromatic hydrocarbon groups in the molecule. Examples of the monovalent or divalent aromatic hydrocarbon groups include phenyl, 1-naphthyl, 2-naphthyl, phenylene, 1-naphthylene, and 2-naphthylene groups. Two or more monovalent or divalent aromatic hydrocarbon groups may be bonded to each other directly or via a linking group, and such bonds may form, for example, a bisphenol structure, preferably a bisphenol A structure.
[0084] It is also preferable that the (G) component is a compound containing a group reactive with the (A) component in the molecule. This allows a crosslinked structure to be formed, and warpage in the cured product to be further reduced. Examples of the group reactive with the (A) component include an epoxy group, -OH, -NH2, and -COOH. Even if the (G) component is a compound having an epoxy group in the molecule, it is classified as the (G) component as long as it is a compound having a radical polymerizable unsaturated group (excluding compounds having a polyalkylene oxide structure). As the (G) component, one or more compounds containing a group reactive with the (A) component in the molecule and one or more compounds not containing a group reactive with the (A) component in the molecule may be used in combination.
[0085] The component (G) may be a compound having an alkylene oxide structure in the molecule. The alkylene oxide structure of the component (G) may be, for example, a compound represented by the formula (3): -(R C O) n -, where in formula (3), n is an integer equal to 1, and R C represents an alkylene group having 1 to 6 carbon atoms which may have a substituent.
[0086] The content of the (G) component is arbitrary as long as it does not excessively impair the radical polymerization of the (B) component, but when the non-volatile components in the resin composition other than the (E) inorganic filler are taken as 100 mass%, it can be, for example, 20 mass% or less, 19.5 mass% or less, or 19 mass% or less. From the viewpoint of enhancing the intended effects of the present invention, the lower limit is preferably 1 mass% or more, more preferably 1.3 mass% or more, even more preferably 1.5 mass% or more, and particularly preferably 1.6 mass% or more.
[0087] <(H) Optional Additives> In one embodiment, the resin composition may further contain other additives (H) as necessary, and examples of such other additives include curing agents other than the component (C), thermoplastic resins, organic fillers, organometallic compounds such as organocopper compounds, organozinc compounds, and organocobalt compounds, as well as resin additives such as thickeners, defoamers, leveling agents, adhesion promoters, and colorants, solvents, etc. The content of the component (H) is arbitrary as long as it does not excessively impair the intended effects of the present invention, but when the non-volatile components in the resin composition are taken as 100 mass%, it can be, for example, 0.1 mass% or more, 0.3 mass% or more, or 0.5 mass% or more, and can be, for example, 15 mass% or less, 13 mass% or less, or 10 mass% or less.
[0088] As the curing agent other than the component (C), one or more types of curing agents selected from active ester curing agents, phenolic curing agents, naphthol curing agents, carbodiimide curing agents, benzoxazine curing agents, amine curing agents, guanidine curing agents, and cyanate ester curing agents can be mentioned, and for example, commercially available products can be used. From the viewpoint of obtaining a resin composition layer (compression molded body) having excellent film material release properties, it is preferable to use one or more types of curing agents selected from the group consisting of active ester curing agents, phenolic curing agents, naphthol curing agents, carbodiimide curing agents, benzoxazine curing agents, and cyanate ester curing agents as the curing agent other than the component (C). One or more types of curing agents selected from amine curing agents (e.g., "Kayahard AA" manufactured by Nippon Kayaku Co., Ltd.) and guanidine curing accelerators (e.g., dicyandiamide ("DICY7" manufactured by Mitsubishi Chemical Corporation)) can be used as long as they do not excessively impair the intended effects of the present invention.
[0089] Examples of the thermoplastic resin include phenoxy resin, polyvinyl acetal resin, polyolefin resin, polyimide resin, polyamideimide resin, polyetherimide resin, polysulfone resin, polyethersulfone resin, polyphenylene ether resin, polyetheretherketone resin, polyester resin, etc. The thermoplastic resin preferably has a reactive functional group, which allows it to be incorporated into the crosslinked structure composed of the (A) component. The reactive functional group may be one that exhibits reactivity upon heating or light irradiation. The content of the thermoplastic resin is arbitrary as long as it does not excessively impair the intended effect of the present invention, but when the non-volatile components in the resin composition are taken as 100% by mass, it may be, for example, 0.1% by mass or more, 0.2% by mass or more, or 0.3% by mass or more, and from the viewpoint of increasing the crosslink density, it may be 5% by mass or less, 3% by mass or less, or 1% by mass or less.
[0090] As the organic filler, any organic filler that can be used when forming an insulating layer of a printed wiring board may be used, for example, rubber particles, polyamide fine particles, silicone particles, etc. As the rubber particles, commercially available products may be used, for example, "EXL2655" manufactured by Dow Chemical Japan, "AC3401N" and "AC3816N" manufactured by Aica Kogyo Co., Ltd. The content of the organic filler is arbitrary as long as it does not excessively impair the intended effect of the present invention, but when the non-volatile components in the resin composition are taken as 100 mass%, it can be, for example, 0.1 mass% or more, 0.3 mass% or more, or 0.5 mass% or more, and for example, 10 mass% or less, 7 mass% or less, or 5 mass% or less.
[0091] When the resin composition contains a solvent, the amount of the solvent is preferably small. The content of the solvent is more preferably 0.5% by mass or less, more preferably 0.1% by mass or less, and particularly preferably 0% by mass (absent), when the non-volatile components of the resin composition are 100% by mass. In order to reduce the amount of the solvent, it is preferable to use a liquid component as at least one component selected from the (A) component, the (C) component, the (D) component, the (F) component, and the (G) component.
[0092] <Characteristics of resin composition> (Warpage and elasticity) The resin composition of the present invention has a small warpage of the cured product obtained by curing at 150°C for 60 minutes. Specifically, as evaluated in the Examples section, the measured warpage of a laminate including a silicon wafer and a cured product formed on the silicon wafer is, for example, less than 2300 μm, more preferably less than 2000 μm, and even more preferably less than 1500 μm. In addition, the resin composition of the present invention has a large elastic modulus of the cured product obtained by curing at 150°C for 60 minutes. Specifically, as evaluated in the Examples section, the elastic modulus of the cured product at 25°C is, for example, 7 GPa or more, more preferably 9 GPa or more. Therefore, the resin composition of the present invention can obtain a cured product in which the first trade-off is eliminated.
[0093] (Adhesion to inorganic materials and release properties of film materials) The resin composition of the present invention has excellent adhesion to inorganic materials in the cured product obtained by curing at 150° C. for 60 minutes. Specifically, as evaluated in the Examples section, in a laminate including a copper foil and a cured product formed on the copper foil, the measured adhesion strength (copper foil peel strength) is, for example, 100 kgf / cm 2 That's all. In addition, the resin composition of the present invention has excellent film material releasability of the resin composition layer (compression molded product) obtained by curing at 130 ° C for 10 minutes. Specifically, as evaluated in the Examples section, after compression molding such a resin composition layer (compression molded product), it is observed that the mold opens with a normal operating force and the resin composition layer peels off from the release film and is on the silicon wafer. Therefore, the resin composition of the present invention can obtain a resin composition layer (compression molded product) and a cured product in which the second trade-off is eliminated.
[0094] As described above, the resin composition of the present invention has the effect of obtaining a cured product with small warpage, large elastic modulus, and excellent adhesion to inorganic materials, and has excellent peelability to film materials. Although the reasons for such effects have not been fully clarified, it has been found that the resin composition of the present invention contains components (A) to (E) and the mass ratio of component (B) to component (C) is within a predetermined range, which unexpectedly tends to eliminate the first and second trade-offs described above. In addition, the resin composition of the present invention has a large elastic modulus of its cured product, specifically, the elastic modulus at 25°C, so that it can improve the handleability of an encapsulation product containing, for example, a semiconductor chip and a cured product in which the semiconductor chip is embedded. Furthermore, the resin composition of the present invention has excellent inorganic material adhesion of the cured product, so that it is highly reliable as an encapsulation material used for encapsulating semiconductor chips. In addition, the resin composition of the present invention has excellent film material releasability of the resin composition layer (compression molded product), so that it can be easily removed from a mold after compression molding.
[0095] The resin composition of the present invention can provide an insulating layer formed of a cured product having small warpage, excellent inorganic material adhesion, and a large elastic modulus. Therefore, the resin composition of the present invention can be suitably used as a resin composition for forming an insulating layer of a printed wiring board (resin composition for forming an insulating layer of a printed wiring board), and can be more suitably used as a resin composition for forming an interlayer insulating layer of a printed wiring board (resin composition for forming an interlayer insulating layer of a printed wiring board). In addition, since the resin composition of the present invention provides an insulating layer having small warpage, excellent inorganic material adhesion, and a large elastic modulus, it can be suitably used even when the printed wiring board is a circuit board with built-in components. Furthermore, since the resin composition of the present invention provides an insulating layer formed of a cured product having small warpage, excellent inorganic material adhesion, and a large elastic modulus, it can be more suitably used as a resin composition for forming a solder resist layer (resin composition for forming a solder resist layer of a printed wiring board). In addition, the resin composition of the present invention provides an insulating layer formed of a cured product with small warpage, excellent adhesion to inorganic materials, and high elastic modulus, and therefore can be suitably used as a resin composition for forming an encapsulation layer for encapsulating a semiconductor chip for a semiconductor chip package (a resin composition for forming an encapsulation layer for a semiconductor chip package). In addition, the resin composition of the present invention can be suitably used as a resin composition for forming a rewiring formation layer for a semiconductor chip package (a resin composition for forming a rewiring formation layer for a semiconductor chip package).
[0096] The semiconductor chip package including the redistribution layer can be manufactured, for example, by the manufacturing method described below. When the semiconductor chip package including the sealing layer is manufactured, a redistribution layer may be further formed on the sealing layer.
[0097] <Method of producing resin composition> The method for producing the resin composition of the present invention is not particularly limited, and examples thereof include a method in which the components are mixed with a solvent as necessary, and dispersed using a rotary mixer or the like.
[0098] The resin composition can be obtained as a resin varnish by, for example, containing a solvent. In one embodiment, the amount of the solvent is preferably small, and the amount of the solvent is more preferably 0.5% by mass or less, and further preferably 0.1% by mass or less, when the non-volatile components of the resin composition are 100% by mass.
[0099] <Physical properties and uses of the resin composition layer or the cured product of the resin composition> (Warpage and elasticity) The cured product obtained by thermally curing the resin composition of the present invention usually has a small warpage. For example, the cured product of the resin composition having a thickness of 100 μm has a measured warpage of, for example, less than 2300 μm, more preferably less than 2000 μm, and even more preferably less than 1500 μm in a laminate including a silicon wafer and a cured product formed on the silicon wafer. In addition, the cured product obtained by thermally curing the resin composition of the present invention usually has a large elastic modulus. For example, the cured product of the resin composition usually has an elastic modulus of 7 GPa or more, preferably 9 GPa or more at 25° C. Therefore, the first trade-off is usually eliminated in the cured product of the resin composition of the present invention.
[0100] (Adhesion to inorganic materials) The cured product obtained by thermally curing the resin composition of the present invention usually has excellent adhesion to inorganic materials. For example, a 300 μm thick cured product of the resin composition usually has an adhesion strength (copper foil peel strength) of 100 kgf / cm when measured in a laminate including a copper foil and the cured product formed on the copper foil. 2 That is all. In addition, since the resin composition layer (compression molded product) of the resin composition of the present invention has excellent film material releasability as described above, the cured product obtained by thermally curing the resin composition of the present invention is usually easily removed from the mold used during compression molding. Therefore, in the cured product of the present invention, the second trade-off is usually eliminated.
[0101] The cured product of the resin composition of the present invention has small warpage, excellent inorganic material adhesion, and a large elastic modulus. Therefore, the cured product of the resin composition of the present invention can be suitably used as an insulating layer of a printed wiring board, and can be more suitably used as an interlayer insulating layer of a printed wiring board. In addition, the cured product of the resin composition of the present invention provides an insulating layer with small warpage, excellent inorganic material adhesion, and a large elastic modulus, so it can be suitably used even when the printed wiring board is a circuit board with built-in components. Furthermore, the cured product of the resin composition of the present invention provides an insulating layer formed of a cured product with small warpage, excellent inorganic material adhesion, and a large elastic modulus, so it can be more suitably used as a solder resist layer. In addition, the cured product of the resin composition of the present invention provides an insulating layer with small warpage, excellent inorganic material adhesion, and a large elastic modulus, so it can be suitably used as an encapsulating layer for encapsulating a semiconductor chip for a semiconductor chip package. In addition, the cured product of the resin composition of the present invention can be suitably used as a rewiring formation layer (insulating layer) for forming a rewiring layer of a semiconductor chip package.
[0102] [Resin paste] The resin paste of the present invention contains the resin composition described above. The resin paste of the present invention usually contains only the resin composition described above. The viscosity of the resin paste at 25°C is preferably within a range of 20 Pa·s to 1000 Pa·s. In order to suppress the generation of voids, the heat loss of the resin paste is preferably 5% or less.
[0103] [Resin composition molded article] The resin composition of the present invention may be made into a resin composition molded product by compression molding or the like. The shape of the resin composition molded product is not limited to a sheet shape, and the resin composition may be processed into any shape. In addition, the resin composition of the present invention may be formed into a powder-like, granular, or pellet-like resin composition molded product (which may be referred to as resin powder, resin granules, or resin pellets, respectively) by compression molding or a method other than compression molding.
[0104] [Resin sheet] The resin sheet of the present invention includes a support and a resin composition layer provided on the support, the resin composition of the present invention.
[0105] The thickness of the resin composition layer of the resin sheet is usually 600 μm or less, preferably 500 μm or less, and may be 400 μm or less or 300 μm or less from the viewpoint of thinning the printed wiring board. The thickness may be further reduced. The lower limit of the thickness of the resin composition layer is not particularly limited, but may usually be 1 μm or more, 10 μm or more, 50 μm or more, etc.
[0106] Examples of the support include films made of plastic materials, metal foils, and release papers, with films made of plastic materials and metal foils being preferred.
[0107] When a film made of a plastic material is used as the support, examples of the plastic material include polyesters such as polyethylene terephthalate (hereinafter sometimes abbreviated as "PET") and polyethylene naphthalate (hereinafter sometimes abbreviated as "PEN"), polycarbonate (hereinafter sometimes abbreviated as "PC"), acrylics such as polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, polyimide, etc. Among these, polyethylene terephthalate and polyethylene naphthalate are preferred, and inexpensive polyethylene terephthalate is particularly preferred.
[0108] When a metal foil is used as the support, examples of the metal foil include copper foil, aluminum foil, etc., and copper foil is preferred. As the copper foil, a foil made of a single metal, copper, or an alloy of copper and another metal (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.) may be used.
[0109] The surface of the support to be bonded to the resin composition layer may be subjected to a matte treatment, a corona treatment, or an antistatic treatment.
[0110] In addition, as the support, a support with a release layer having a release layer on the surface to be bonded to the resin composition layer may be used. The release agent used in the release layer of the support with a release layer may be, for example, one or more release agents selected from the group consisting of alkyd resins, polyolefin resins, urethane resins, and silicone resins. The support with a release layer may be a commercially available product, for example, "SK-1", "AL-5", and "AL-7" manufactured by Lintec Corporation, "Lumirror T60" manufactured by Toray Industries, Inc., "Purex" manufactured by Teijin Limited, and "Unipeel" manufactured by Unitika Limited, which are PET films having a release layer mainly composed of an alkyd resin-based release agent.
[0111] The thickness of the support is not particularly limited, but is preferably in the range of 5 μm to 75 μm, and more preferably in the range of 10 μm to 60 μm. When a support with a release layer is used, it is preferable that the total thickness of the support with a release layer is in the above range.
[0112] In one embodiment, the resin sheet may further include other layers as necessary. Examples of such other layers include a protective film equivalent to the support provided on the surface of the resin composition layer that is not bonded to the support (i.e., the surface opposite to the support). The thickness of the protective film is not particularly limited, but is, for example, 1 μm to 40 μm. By laminating the protective film, adhesion of dirt and the like to the surface of the resin composition layer and scratches can be suppressed.
[0113] The resin sheet can be produced, for example, by preparing a resin varnish by dissolving a resin composition in an organic solvent, applying this resin varnish onto a support using a die coater or the like, and then drying the same to form a resin composition layer.
[0114] Examples of organic solvents include ketones such as acetone, methyl ethyl ketone (MEK) and cyclohexanone; acetates such as ethyl acetate, butyl acetate, cellosolve acetate, propylene glycol monomethyl ether acetate and carbitol acetate; carbitols such as cellosolve and butyl carbitol; aromatic hydrocarbons such as toluene and xylene; and amide solvents such as dimethylformamide, dimethylacetamide (DMAc) and N-methylpyrrolidone. The organic solvent may be used alone or in combination of two or more. In one embodiment, the amount of organic solvent is preferably as small as possible (for example, 0.5% by mass or less, 0.1% by mass or less, or 0.01% by mass or less when the non-volatile components in the resin composition are taken as 100% by mass), and it is particularly preferable that no organic solvent is contained.
[0115] Drying may be performed by a known method such as heating or hot air blowing. Drying conditions are not particularly limited, but drying is performed so that the content of organic solvent in the resin composition layer becomes 10 mass % or less, preferably 5 mass % or less. Although it varies depending on the boiling point of the organic solvent in the resin varnish, for example, when a resin varnish containing 30 mass % to 60 mass % of organic solvent is used, the resin composition layer can be formed by drying at 50°C to 150°C for 3 minutes to 10 minutes.
[0116] The resin sheet can be stored in a rolled state. When the resin sheet has a protective film, it can be used by peeling off the protective film.
[0117] The resin sheet of the present invention provides an insulating layer formed of a cured product having small warpage, excellent inorganic material adhesion, and a large elastic modulus. Therefore, the resin sheet of the present invention can be suitably used as a resin sheet for forming an insulating layer of a printed wiring board (resin sheet for forming an insulating layer of a printed wiring board), and can be more suitably used as a resin sheet for forming an interlayer insulating layer of a printed wiring board (resin sheet for forming an interlayer insulating layer of a printed wiring board). The resin sheet of the present invention can also be suitably used as a resin sheet for forming a solder resist layer of a printed wiring board (resin sheet for forming a solder resist layer of a printed wiring board). In addition, since the resin sheet of the present invention provides an insulating layer formed of a cured product having small warpage, excellent inorganic material adhesion, and a large elastic modulus, it can be suitably used as a resin composition for forming an encapsulating layer for encapsulating a semiconductor chip for a semiconductor chip package (resin sheet for forming an encapsulating layer of a semiconductor chip package). In addition, the resin sheet of the present invention can also be suitably used as a resin sheet for forming a rewiring forming layer (insulating layer) of a semiconductor chip package (resin sheet for forming a rewiring forming layer for a semiconductor chip package).
[0118] <Printed wiring board> The printed wiring board of the present invention includes an insulating layer formed containing a cured product of the resin composition of the present invention. The printed wiring board can be produced, for example, by a production method including the following steps (1) and (2). (1) A step of forming a resin composition layer containing a resin composition of the present invention on a substrate using the resin composition of the present invention. (2) A step of thermally curing the resin composition layer to form an insulating layer. For example, a method for producing a printed wiring board of the present invention includes a step of forming a resin composition layer containing the resin composition of the present invention or a resin composition layer containing the resin paste of the present invention on a circuit board by a compression molding method, and a step of curing the resin composition layer.
[0119] In step (1), a substrate is prepared. Examples of the substrate include glass epoxy substrates, metal substrates (such as stainless steel and cold-rolled steel sheet (SPCC)), polyester substrates, polyimide substrates, BT resin substrates, and thermosetting polyphenylene ether substrates. The substrate may have a metal layer such as copper foil on the surface as a part of the substrate. For example, a substrate having a peelable first metal layer and a peelable second metal layer on both surfaces may be used. When such a substrate is used, a conductor layer as a wiring layer that can function as a circuit wiring is usually formed on the surface of the second metal layer opposite to the first metal layer. Examples of substrates having such a metal layer include "Micro Thin", an ultra-thin copper foil with a carrier copper foil manufactured by Mitsui Mining & Smelting Co., Ltd.
[0120] A conductor layer may be formed on one or both surfaces of the substrate. In the following description, a member including a substrate and a conductor layer formed on the substrate surface may be referred to as a "substrate with wiring layer" as appropriate. Examples of the conductor material included in the conductor layer include materials including one or more metals selected from the group consisting of gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin, and indium. The conductor material may be a single metal or an alloy. Examples of the alloy include alloys of two or more metals selected from the above group (e.g., nickel-chromium alloy, copper-nickel alloy, and copper-titanium alloy). Among them, from the viewpoints of versatility, cost, and ease of patterning in the formation of the conductor layer, chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper as single metals; and alloys of nickel-chromium alloy, copper-nickel alloy, and copper-titanium alloy as alloys; are preferred. Among these, the single metals chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver and copper; and nickel-chromium alloys; are more preferable, and the single metal copper is particularly preferable.
[0121] The conductor layer may be patterned, for example, to function as a wiring layer. In this case, the line (circuit width) / space (width between circuits) ratio of the conductor layer is not particularly limited, but is preferably 20 / 20 μm or less (i.e., pitch is 40 μm or less), more preferably 10 / 10 μm or less, even more preferably 5 / 5 μm or less, even more preferably 1 / 1 μm or less, and particularly preferably 0.5 / 0.5 μm or more. The pitch does not need to be the same throughout the conductor layer. The minimum pitch of the conductor layer may be, for example, 40 μm or less, 36 μm or less, or 30 μm or less.
[0122] The thickness of the conductor layer depends on the design of the printed wiring board, but is preferably 3 μm to 35 μm, more preferably 5 μm to 30 μm, further preferably 10 μm to 20 μm, and particularly preferably 15 μm to 20 μm.
[0123] The conductor layer can be formed, for example, by a method including a step of laminating a dry film (photosensitive resist film) on a substrate, a step of forming a pattern by exposing and developing the dry film under predetermined conditions using a photomask to obtain a patterned dry film, a step of forming a conductor layer by a plating method such as electrolytic plating using the developed patterned dry film as a plating mask, and a step of peeling off the patterned dry film. As the dry film, a photosensitive dry film made of a photoresist composition can be used, and for example, a dry film formed of a resin such as a novolac resin or an acrylic resin can be used. The lamination conditions of the substrate and the dry film can be the same as the lamination conditions of the substrate and the resin sheet described later. The peeling off of the dry film can be carried out using, for example, an alkaline peeling solution such as a sodium hydroxide solution.
[0124] After preparing the substrate, a resin composition layer is formed on the substrate. When a conductor layer is formed on the surface of the substrate, the resin composition layer is preferably formed so that the conductor layer is embedded in the resin composition layer.
[0125] The resin composition layer is formed, for example, by laminating a resin sheet and a substrate. This lamination can be performed, for example, by bonding the resin sheet to the substrate from the support side under heat and pressure, thereby laminating the resin composition layer to the substrate. Examples of the member for heat-pressing the resin sheet to the substrate (hereinafter, sometimes referred to as a "heat-pressing member") include a heated metal plate (such as a SUS plate) or a metal roll (such as a SUS roll). It is preferable to press the heat-pressing member through an elastic material such as heat-resistant rubber so that the resin sheet can sufficiently follow the surface irregularities of the substrate, rather than directly pressing the resin sheet.
[0126] The lamination of the substrate and the resin sheet may be carried out, for example, by a vacuum lamination method. In the vacuum lamination method, the thermocompression temperature is preferably in the range of 60°C to 160°C, more preferably in the range of 80°C to 140°C. The thermocompression pressure is preferably in the range of 0.098MPa to 1.77MPa, more preferably in the range of 0.29MPa to 1.47MPa. The thermocompression time is preferably in the range of 20 seconds to 400 seconds, more preferably in the range of 30 seconds to 300 seconds. The lamination is preferably carried out under reduced pressure conditions of a pressure of 13hPa or less.
[0127] After lamination, the laminated resin sheets may be smoothed under normal pressure (atmospheric pressure), for example, by pressing the support side with a thermocompression member. The pressing conditions for the smoothing treatment may be the same as the thermocompression conditions for the lamination. The lamination and smoothing treatment may be performed successively using a vacuum laminator.
[0128] The resin composition layer can be formed, for example, by compression molding. The molding conditions may be the same as those of the method for forming the resin composition layer in the step of forming the sealing layer of the semiconductor chip package described later.
[0129] After forming the resin composition layer on the substrate, the resin composition layer is thermally cured to form an insulating layer. The thermal curing conditions for the resin composition layer vary depending on the type of resin composition, but the curing temperature is usually in the range of 120°C to 240°C (preferably in the range of 130°C to 220°C, more preferably in the range of 140°C to 200°C), and the curing time is in the range of 5 minutes to 120 minutes (preferably in the range of 10 minutes to 100 minutes, more preferably in the range of 15 minutes to 90 minutes).
[0130] Before the resin composition layer is thermally cured, the resin composition layer may be subjected to a preheating treatment at a temperature lower than the curing temperature. For example, prior to thermally curing the resin composition layer, the resin composition layer may be preheated at a temperature of usually 50° C. or more and less than 120° C. (preferably 60° C. or more and 110° C. or less, more preferably 70° C. or more and 100° C. or less) for usually 5 minutes or more (preferably 5 minutes to 150 minutes, more preferably 15 minutes to 120 minutes).
[0131] In the manner described above, a printed wiring board having an insulating layer can be manufactured. The method for manufacturing a printed wiring board may further include any optional step. For example, when a printed wiring board is manufactured using a resin sheet, the method for manufacturing a printed wiring board may include a step of peeling off the support of the resin sheet. The support may be peeled off before or after the resin composition layer is thermally cured.
[0132] The method for manufacturing a printed wiring board may include, for example, a step of polishing the surface of an insulating layer after forming the insulating layer. The polishing method is not particularly limited. For example, the surface of the insulating layer can be polished using a surface grinder.
[0133] The method for manufacturing a printed wiring board may include, for example, a step (3) of connecting the conductor layers to each other, for example, a step of drilling holes in the insulating layer. This allows holes such as via holes and through holes to be formed in the insulating layer. Examples of the method for forming the via holes include laser irradiation, etching, and mechanical drilling. The size and shape of the via holes may be appropriately determined depending on the design of the printed wiring board. In addition, the step (3) may also be performed by polishing or grinding the insulating layer to perform the interlayer connection.
[0134] After the via holes are formed, it is preferable to carry out a step of removing smears in the via holes. This step is sometimes called a desmear step. For example, when the conductive layer is formed on the insulating layer by a plating step, the via holes may be subjected to a wet desmear process. When the conductive layer is formed on the insulating layer by a sputtering step, a dry desmear process such as a plasma treatment process may be carried out. Furthermore, the insulating layer may be roughened by the desmear process.
[0135] Furthermore, before forming the conductor layer on the insulating layer, the insulating layer may be subjected to a roughening treatment. This roughening treatment usually roughens the surface of the insulating layer including the inside of the via hole. The roughening treatment may be either a dry or wet roughening treatment. An example of the dry roughening treatment is a plasma treatment. An example of the wet roughening treatment is a method in which a swelling treatment using a swelling liquid, a roughening treatment using an oxidizing agent, and a neutralization treatment using a neutralizing liquid are performed in this order.
[0136] After the via holes are formed, a conductor layer may be formed on the insulating layer. By forming a conductor layer at the position where the via holes are formed, the newly formed conductor layer and the conductor layer on the surface of the substrate are electrically connected to each other, and interlayer connection is performed. Examples of the method for forming the conductor layer include plating, sputtering, and vapor deposition, among which plating is preferred. In a preferred embodiment, the surface of the insulating layer is plated by an appropriate method such as a semi-additive method or a full-additive method to form a conductor layer having a desired wiring pattern. In addition, when the support in the resin sheet is a metal foil, a conductor layer having a desired wiring pattern can be formed by a subtractive method. The material of the conductor layer to be formed may be a single metal or an alloy. In addition, this conductor layer may have a single layer structure, or may have a multi-layer structure including two or more layers of different types of materials.
[0137] Here, an example of an embodiment in which a conductor layer is formed on an insulating layer will be described in detail. A plating seed layer is formed on the surface of the insulating layer by electroless plating. Then, a mask pattern is formed on the formed plating seed layer, exposing a part of the plating seed layer corresponding to a desired wiring pattern. After forming an electrolytic plating layer on the exposed plating seed layer by electrolytic plating, the mask pattern is removed. Thereafter, unnecessary plating seed layer is removed by a process such as etching, and a conductor layer having a desired wiring pattern can be formed. Note that, when forming the conductor layer, the dry film used to form the mask pattern is the same as the above-mentioned dry film.
[0138] The method for producing a printed wiring board may include a step (4) of removing the substrate. By removing the substrate, a printed wiring board having an insulating layer and a conductor layer embedded in the insulating layer is obtained. This step (4) can be carried out, for example, when a substrate having a peelable metal layer is used.
[0139] <Semiconductor chip package> The semiconductor chip package according to the first embodiment of the present invention includes the above-mentioned printed wiring board and a semiconductor chip mounted on the printed wiring board. The semiconductor chip package can be manufactured by bonding the semiconductor chip to the printed wiring board. The manufacturing method of the semiconductor chip package of the present invention may include a step of forming a resin composition layer containing the resin composition of the present invention or a resin composition layer containing the resin paste of the present invention on the semiconductor chip by a compression molding method, and a step of curing the resin composition layer.
[0140] The bonding conditions between the printed wiring board and the semiconductor chip may be any conditions that allow conductive connection between the terminal electrodes of the semiconductor chip and the circuit wiring of the printed wiring board. For example, the conditions used in flip-chip mounting of the semiconductor chip may be used. Also, for example, the semiconductor chip and the printed wiring board may be bonded via an insulating adhesive.
[0141] An example of a bonding method is a method in which a semiconductor chip is pressure-bonded to a printed wiring board. Pressure-bonding conditions are a pressure-bonding temperature usually in the range of 120°C to 240°C (preferably in the range of 130°C to 200°C, more preferably in the range of 140°C to 180°C), and a pressure-bonding time usually in the range of 1 second to 60 seconds (preferably in the range of 5 seconds to 30 seconds).
[0142] Another example of the bonding method is a method of bonding a semiconductor chip to a printed wiring board by reflow. The reflow conditions may be in the range of 120°C to 300°C.
[0143] After the semiconductor chip is bonded to the printed wiring board, the semiconductor chip may be filled with a molded underfill material. As the molded underfill material, the above-mentioned resin composition or the above-mentioned resin sheet may be used.
[0144] The semiconductor chip package according to the second embodiment of the present invention includes a semiconductor chip and a cured product of the resin composition that encapsulates the semiconductor chip. In such a semiconductor chip package, the cured product of the resin composition usually functions as an encapsulating layer. For example, the manufacturing method of the semiconductor chip package of the present invention may include a step of forming a resin composition layer containing the resin composition of the present invention or a resin composition layer containing the resin paste of the present invention on a semiconductor chip by a compression molding method, and a step of curing the resin composition layer.
[0145] The method for manufacturing such a semiconductor chip package includes: (A) a step of laminating a temporary fixing film on a substrate; (B) a step of temporarily fixing a semiconductor chip on a temporary fixing film; (C) forming an encapsulation layer on the semiconductor chip; (D) peeling the substrate and the temporary fixing film from the semiconductor chip; (E) a step of forming a rewiring formation layer as an insulating layer on the surface of the semiconductor chip from which the base material and the temporary fixing film have been peeled off; (F) forming a rewiring layer as a conductor layer on the rewiring formation layer; and (G) forming a solder resist layer on the rewiring layer; The method for manufacturing the semiconductor chip package may further include: (H) A process of dicing and separating multiple semiconductor chip packages into individual semiconductor chip packages. may also include
[0146] (Process (A)) Step (A) is a step of laminating a temporary fixing film on a substrate. The lamination conditions for the substrate and the temporary fixing film can be the same as the lamination conditions for the substrate and the resin sheet in the method for producing a printed wiring board.
[0147] Examples of the substrate include silicon wafers; glass wafers; glass substrates; metal substrates such as copper, titanium, stainless steel, and cold-rolled steel (SPCC); substrates such as FR-4 substrates in which glass fibers are impregnated with epoxy resin or the like and then heat-cured; and substrates made of bismaleimide triazine resins such as BT resin.
[0148] The temporary fixing film may be made of any material that can be peeled off from the semiconductor chip and can temporarily fix the semiconductor chip. Commercially available products include "Riva Alpha" manufactured by Nitto Denko Corporation.
[0149] (Process (B)) Step (B) is a step of temporarily fixing the semiconductor chip on the temporary fixing film. The temporary fixing of the semiconductor chip can be performed using, for example, a device such as a flip chip bonder or a die bonder. The layout and number of the semiconductor chips can be appropriately set depending on the shape and size of the temporary fixing film, the number of semiconductor chip packages to be produced, etc. For example, the semiconductor chips may be temporarily fixed by arranging them in a matrix shape of multiple rows and multiple columns.
[0150] (Process (C)) Step (C) is a step of forming an encapsulating layer on the semiconductor chip. The encapsulating layer is formed by a cured product of the above-mentioned resin composition. The encapsulating layer is usually formed by a method including a step of forming a resin composition layer on the semiconductor chip and a step of thermally curing the resin composition layer to form the encapsulating layer.
[0151] The resin composition layer is preferably formed by a compression molding method, in which a semiconductor chip and a resin composition are usually placed in a mold, and pressure and, if necessary, heat are applied to the resin composition in the mold to form a resin composition layer covering the semiconductor chip.
[0152] A specific operation of the compression molding method can be, for example, as follows. An upper mold and a lower mold are prepared as molds for compression molding. A resin composition is applied to the semiconductor chip temporarily fixed on the temporary fixing film as described above. The semiconductor chip to which the resin composition is applied is attached to the lower mold together with the substrate and the temporary fixing film. Then, the upper mold and the lower mold are clamped, and heat and pressure are applied to the resin composition to perform compression molding.
[0153] In addition, the specific operation of the compression molding method may be, for example, as follows. An upper mold and a lower mold are prepared as molds for compression molding. A resin composition is placed on the lower mold. Also, a semiconductor chip is attached to the upper mold together with a substrate and a temporary fixing film. Then, the upper mold and the lower mold are clamped so that the resin composition placed on the lower mold contacts the semiconductor chip attached to the upper mold, and heat and pressure are applied to perform compression molding. Generally, in the compression molding method, a release film is provided on the surface of the mold. Therefore, the resin composition can be molded in a state of contact with the release film. The resin composition containing the components (A) to (E) in combination as described above has excellent releasability from the release film, so that the molded resin composition layer or the cured product can be smoothly removed from the mold.
[0154] The molding conditions vary depending on the composition of the resin composition, and appropriate conditions can be adopted so that good sealing is achieved. For example, the temperature of the mold during molding (mold temperature Tc) is preferably 70°C or higher, more preferably 80°C or higher, particularly preferably 90°C or higher, and preferably 200°C or lower, more preferably 170°C or lower, particularly preferably 150°C or lower. The pressure applied during molding is preferably 1 MPa or higher, more preferably 2 MPa or higher, particularly preferably 3 MPa or higher, preferably 50 MPa or lower, more preferably 30 MPa or lower, particularly preferably 20 MPa or lower. The cure time is preferably 1 minute or higher, more preferably 2 minutes or higher, particularly preferably 3 minutes or higher, preferably 60 minutes or lower, more preferably 30 minutes or lower, particularly preferably 20 minutes or lower. Usually, the mold is removed after the formation of the resin composition layer. The mold may be removed before or after the resin composition layer is thermally cured.
[0155] The resin composition layer may be formed by laminating a resin sheet and a semiconductor chip. For example, the resin composition layer of the resin sheet and the semiconductor chip are heated and pressed to form a resin composition layer on the semiconductor chip. The lamination of the resin sheet and the semiconductor chip is usually performed in the same manner as the lamination of the resin sheet and the substrate in the method for producing a printed wiring board, using a semiconductor chip instead of a substrate.
[0156] After forming a resin composition layer on the semiconductor chip, the resin composition layer is thermally cured to obtain an encapsulation layer that covers the semiconductor chip. This encapsulates the semiconductor chip with a cured product of the resin composition. The thermal curing conditions of the resin composition layer may be the same as the thermal curing conditions of the resin composition layer in the method for producing a printed wiring board. Furthermore, before thermally curing the resin composition layer, a preheating treatment may be performed on the resin composition layer at a temperature lower than the curing temperature. The treatment conditions of this preheating treatment may be the same as the preheating treatment in the method for producing a printed wiring board.
[0157] (Process (D)) Step (D) is a step of peeling off the substrate and the temporary fixing film from the semiconductor chip. It is desirable to adopt an appropriate peeling method according to the material of the temporary fixing film. For example, the peeling method may be a method of heating, foaming or expanding the temporary fixing film to peel it off. In addition, for example, the peeling method may be a method of irradiating the temporary fixing film with ultraviolet light through the substrate to reduce the adhesive strength of the temporary fixing film to peel it off.
[0158] In the method of peeling off the temporary fixing film by heating, foaming or expanding it, the heating conditions are usually 100° C. to 250° C. for 1 second to 90 seconds or 5 minutes to 15 minutes. In the method of peeling off the temporary fixing film by reducing the adhesive strength of the temporary fixing film by irradiating it with ultraviolet light, the irradiation amount of ultraviolet light is usually 10 mJ / cm 2 ~1000mJ / cm 2 It is.
[0159] (Process (E)) Step (E) is a step of forming a rewiring formation layer as an insulating layer on the surface of the semiconductor chip from which the base material and the temporary fixing film have been peeled off.
[0160] The material of the rewiring formation layer can be any material having insulating properties. Among them, photosensitive resins and thermosetting resins are preferred from the viewpoint of ease of manufacturing the semiconductor chip package. The resin composition of the present invention may be used as the thermosetting resin.
[0161] After forming the rewiring formation layer, via holes may be formed in the rewiring formation layer to provide interlayer connection between the semiconductor chip and the rewiring layer.
[0162] In the method of forming a via hole when the material of the rewiring formation layer is a photosensitive resin, the surface of the rewiring formation layer is usually irradiated with active energy rays through a mask pattern to photocure the rewiring formation layer in the irradiated portion. Examples of active energy rays include ultraviolet rays, visible rays, electron beams, X-rays, etc., and ultraviolet rays are particularly preferred. The irradiation amount and irradiation time of the ultraviolet rays can be appropriately set according to the photosensitive resin. Examples of the exposure method include a contact exposure method in which a mask pattern is attached to the rewiring formation layer and exposed, and a non-contact exposure method in which a mask pattern is not attached to the rewiring formation layer and exposed using parallel rays.
[0163] After the rewiring formation layer is photocured, the rewiring formation layer is developed to remove the unexposed portion to form a via hole. The development may be performed by either wet development or dry development. Examples of the development method include a dip method, a paddle method, a spray method, a brushing method, and a scraping method, and the paddle method is preferable from the viewpoint of resolution.
[0164] When the material of the rewiring formation layer is a thermosetting resin, the method of forming the via hole may be, for example, laser irradiation, etching, mechanical drilling, etc. Among them, laser irradiation is preferable. The laser irradiation can be performed using an appropriate laser processing machine using a light source such as a carbon dioxide laser, a UV-YAG laser, or an excimer laser.
[0165] The shape of the via hole is not particularly limited, but is generally circular (approximately circular). The top diameter of the via hole is preferably 50 μm or less, more preferably 30 μm or less, and further preferably 20 μm or less. Here, the top diameter of the via hole refers to the diameter of the opening of the via hole on the surface of the rewiring formation layer.
[0166] (Process (F)) Step (F) is a step of forming a rewiring layer as a conductor layer on the rewiring formation layer. The method of forming the rewiring layer on the rewiring formation layer can be the same as the method of forming a conductor layer on an insulating layer in the method of manufacturing a printed wiring board. Steps (E) and (F) may be repeated to alternately stack (build up) the rewiring layers and the rewiring formation layers.
[0167] (Process (G)) Step (G) is a step of forming a solder resist layer on the rewiring layer. Any material having insulating properties can be used as the material of the solder resist layer. Among them, photosensitive resins and thermosetting resins are preferred from the viewpoint of ease of manufacturing the semiconductor chip package. The resin composition of the present invention may be used as the thermosetting resin.
[0168] In step (G), bumping processing may be performed to form bumps, if necessary. The bumping processing can be performed by a method such as solder balls or solder plating. In addition, the formation of via holes in the bumping processing can be performed in the same manner as in step (E).
[0169] (Process (H)) The method for manufacturing a semiconductor chip package may include a step (H) in addition to the steps (A) to (G). The step (H) is a step of dicing a plurality of semiconductor chip packages into individual semiconductor chip packages to separate them. The method for dicing the semiconductor chip packages into individual semiconductor chip packages is not particularly limited.
[0170] <Semiconductor device> The semiconductor device includes a semiconductor chip package. Examples of the semiconductor device include a printed wiring board, a semiconductor chip package, a multi-chip package, a package-on-package, a wafer-level package (e.g., a fan-out type WLP), a panel-level package, and a system-in-package. Examples of the semiconductor device include various semiconductor devices used in electrical products (e.g., computers, mobile phones, smartphones, tablet devices, wearable devices, digital cameras, medical devices, and televisions) and vehicles (e.g., motorcycles, automobiles, trains, ships, and aircraft). EXAMPLES
[0171] The present invention will be specifically described below with reference to examples. However, the present invention is not limited to the following examples. In the following description, "parts" and "%" representing amounts mean "parts by mass" and "% by mass", respectively, unless otherwise specified. Furthermore, the operations described below were performed in an environment of normal temperature and pressure, unless otherwise specified.
[0172] [Example 1] <Preparation of Resin Paste A> 10 parts of epoxy resin (Nippon Steel Chemical & Material Co., Ltd. "ZX-1059", epoxy group equivalent: 165 g / eq.) as component (A), 5 parts of a compound having a methacryloyl group and a polyethylene oxide structure (Shin-Nakamura Chemical Co., Ltd. "M-130G", methacryloyl group equivalent: 628 g / eq.) as component (B), and 5 parts of an acid anhydride-based curing agent (Shin-Nippon Rika Co., Ltd. "MH-700", acid anhydride-based curing agent) as component (C). (equivalent: 163 g / eq.), 0.1 parts of a thermal radical generator (Arkema Fuji's "Luperox 531M80", 10-hour half-life temperature T10: 93.0°C, hydrocarbon solution with 80% peroxide content) as component (D), 0.15 parts of an imidazole-based curing accelerator (Shikoku Kasei's "1B2PZ") as component (F), and inorganic filler A (average particle size: 1.8 μm, specific surface area: 3.6 m) as component (E). 2 85 parts of "KBM573" (spherical silica treated with N-phenyl-3-aminopropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd., with a particle size of 1 / g and a maximum cut diameter of 5 μm, were uniformly dispersed using a mixer. This resulted in the preparation of a liquid resin composition. Hereinafter, the liquid resin composition prepared in this manner is also referred to as "resin paste A."
[0173] <Evaluation of the cured product of Resin Paste A> The obtained resin paste A was used to obtain a compression molded body (resin composition layer), or a cured product, or a substrate for evaluation containing the cured product. The obtained compression molded body (resin composition layer), or the cured product, or the substrate for evaluation was evaluated in terms of warpage, elastic modulus, adhesion to inorganic materials, and peelability from film materials, as described below.
[0174] [Examples 2 to 6] In Example 1, 5 parts of a compound having a methacryloyl group and a polyethylene oxide structure ("M-130G" manufactured by Shin-Nakamura Chemical Co., Ltd.) as component (B) were used, and in Examples 2 to 6, 5 parts of a compound having a methacryloyl group and a polyethylene oxide structure ("M-230G" manufactured by Shin-Nakamura Chemical Co., Ltd., methacryloyl group equivalent: 1068 g / eq.) as component (B), 5 parts of a compound having a methacryloyl group and a polyethylene oxide structure ("M-23G" manufactured by Shin-Nakamura Chemical Co., Ltd., methacryloyl group equivalent: 568 g / eq.) as component (B), and The compound having a methacryloyl group and a polyethylene oxide structure as component (B) ("M-90G" manufactured by Shin-Nakamura Chemical Co., Ltd., methacryloyl group equivalent: 468 g / eq.) was changed to 5 parts, the compound having a methacryloyl group and a polyethylene oxide structure as component (B) ("M-40G" manufactured by Shin-Nakamura Chemical Co., Ltd., methacryloyl group equivalent: 276 g / eq.) was changed to 5 parts, and the compound having a methacryloyl group and a polyethylene oxide structure as component (B) ("BPE-1300N" manufactured by Shin-Nakamura Chemical Co., Ltd., methacryloyl group equivalent: 842 g / eq.) was changed to 5 parts.
[0175] Except for the above, resin paste A was prepared in the same manner as in Example 1. Then, using resin paste A, a compression molded body (resin composition layer), or a cured product or a substrate for evaluation containing a cured product was obtained in the same manner as in Example 1, and these were subjected to evaluation in the same manner as in Example 1.
[0176] [Example 7] In Example 6, 85 parts of inorganic filler A as component (E) was replaced with inorganic filler B (average particle size: 2.6 μm, specific surface area: 1.4 m) as component (E). 2 / g, maximum cut diameter: 10 μm, and 140 parts of "KBM573" (spherical alumina treated with N-phenyl-3-aminopropyltrimethoxysilane) manufactured by Shin-Etsu Chemical Co., Ltd.
[0177] Except for the above, resin paste A was prepared in the same manner as in Example 6. Then, using resin paste A, a compression molded body (resin composition layer), or a cured product or a substrate for evaluation containing a cured product was obtained in the same manner as in Example 6, and these were subjected to evaluation in the same manner as in Example 6.
[0178] [Examples 8 and 9] In Example 6, 0.1 parts of the thermal radical generator as component (D) ("Luperox 531M80" manufactured by Arkema Fuji, a hydrocarbon solution with a peroxide content of 80%) was used. In Example 8, this was changed to 0.1 parts of the thermal radical generator as component (D) ("Perhexyl (registered trademark) O" manufactured by NOF Corporation, 10-hour half-life temperature T10: 69.9°C). In Example 9, this was changed to 0.1 parts of the thermal radical generator as component (D) ("MAIB" (2,2'-azobis(isobutyric acid) dimethyl) manufactured by Fujifilm Wako Pure Chemical Industries, 10-hour half-life temperature T10: 67.0°C).
[0179] Except for the above, resin paste A was prepared in the same manner as in Example 6. Then, using resin paste A, a compression molded body (resin composition layer), or a cured product or a substrate for evaluation containing a cured product was obtained in the same manner as in Example 6, and these were subjected to evaluation in the same manner as in Example 6.
[0180] [Example 10] In Example 6, 8 parts of an acid anhydride curing agent as component (C) ("MH-700" manufactured by New Japan Chemical Co., Ltd.) was changed to 8 parts of an acid anhydride curing agent as component (C) ("HNA-100" manufactured by New Japan Chemical Co., Ltd., acid anhydride group equivalent: 179 g / eq.).
[0181] Except for the above, resin paste A was prepared in the same manner as in Example 6. Then, using resin paste A, a compression molded body (resin composition layer), or a cured product or a substrate for evaluation containing a cured product was obtained in the same manner as in Example 6, and these were subjected to evaluation in the same manner as in Example 6.
[0182] [Example 11] In Example 6, 8 parts of the acid anhydride curing agent ("MH-700" manufactured by New Japan Chemical Co., Ltd.) as component (C) was changed to 15 parts of the acid anhydride curing agent ("MH-700" manufactured by New Japan Chemical Co., Ltd.) as component (C), and 85 parts of the inorganic filler A as component (E) was changed to 100 parts of the inorganic filler A as component (E).
[0183] Except for the above, resin paste A was prepared in the same manner as in Example 6. Then, using resin paste A, a compression molded body (resin composition layer), or a cured product or a substrate for evaluation containing a cured product was obtained in the same manner as in Example 6, and these were subjected to evaluation in the same manner as in Example 6.
[0184] [Example 12] In Example 6, 5 parts of a compound having a methacryloyl group and a polyethylene oxide structure ("BPE-1300N" manufactured by Shin-Nakamura Chemical Co., Ltd.) as component (B) was changed to 10 parts of a compound having a methacryloyl group and a polyethylene oxide structure ("BPE-1300N" manufactured by Shin-Nakamura Chemical Co., Ltd.) as component (B), and 85 parts of inorganic filler A as component (E) was changed to 95 parts of inorganic filler A as component (E).
[0185] Except for the above, resin paste A was prepared in the same manner as in Example 6. Then, using resin paste A, a compression molded body (resin composition layer), or a cured product or a substrate for evaluation containing a cured product was obtained in the same manner as in Example 6, and these were subjected to evaluation in the same manner as in Example 6.
[0186] [Example 13] In Example 6, for the component (A), 10 parts of epoxy resin ("ZX-1059" manufactured by Nippon Steel Chemical & Material Co., Ltd.) was changed to 5 parts of epoxy resin ("ZX-1059" manufactured by Nippon Steel Chemical & Material Co., Ltd.) and 5 parts of epoxy resin ("HP-4032SS" manufactured by DIC Corporation, epoxy group equivalent: 143 g / eq.), for the component (C), 8 parts of acid anhydride curing agent ("MH-700" manufactured by New Japan Chemical Co., Ltd.) was changed to 9 parts of acid anhydride curing agent ("MH-700" manufactured by New Japan Chemical Co., Ltd.), and 85 parts of inorganic filler A as component (E) was changed to 90 parts of inorganic filler A as component (E).
[0187] Except for the above, resin paste A was prepared in the same manner as in Example 6. Then, using resin paste A, a compression molded body (resin composition layer), or a cured product or a substrate for evaluation containing a cured product was obtained in the same manner as in Example 6, and these were subjected to evaluation in the same manner as in Example 6.
[0188] [Example 14] In Example 6, for the component (A), 10 parts of epoxy resin ("ZX-1059" manufactured by Nippon Steel Chemical & Material Corporation) was changed to 5 parts of epoxy resin ("ZX-1059" manufactured by Nippon Steel Chemical & Material Corporation) and 5 parts of epoxy resin ("630LSD" manufactured by Mitsubishi Chemical Corporation, epoxy group equivalent: 98 g / eq.), for the component (C), 8 parts of acid anhydride curing agent ("MH-700" manufactured by New Japan Chemical Co., Ltd.) was changed to 11 parts of acid anhydride curing agent ("MH-700" manufactured by New Japan Chemical Co., Ltd.), and 85 parts of inorganic filler A as the component (E) was changed to 95 parts of inorganic filler A as the component (E).
[0189] Except for the above, resin paste A was prepared in the same manner as in Example 6. Then, using resin paste A, a compression molded body (resin composition layer), or a cured product or a substrate for evaluation containing a cured product was obtained in the same manner as in Example 6, and these were subjected to evaluation in the same manner as in Example 6.
[0190] [Example 15] In Example 6, 85 parts of inorganic filler A as component (E) was replaced with inorganic filler C (average particle size: 1.8 μm, specific surface area: 3.6 m) as component (E). 2 / g, maximum cut diameter: 5 μm, Shin-Etsu Chemical Co., Ltd. "KBM-4803" (spherical silica treated with glycidoxyoctyltrimethoxysilane) was changed to 95 parts.
[0191] Except for the above, resin paste A was prepared in the same manner as in Example 6. Then, using resin paste A, a compression molded body (resin composition layer), or a cured product or a substrate for evaluation containing a cured product was obtained in the same manner as in Example 6, and these were subjected to evaluation in the same manner as in Example 6.
[0192] [Example 16] In Example 6, 85 parts of inorganic filler A as component (E) was replaced with inorganic filler D (average particle size: 1.8 μm, specific surface area: 3.6 m) as component (E). 2 / g, maximum cut diameter: 5 μm, Shin-Etsu Chemical Co., Ltd.'s "KBM403" (spherical silica treated with 3-glycidoxypropyltrimethoxysilane) was changed to 85 parts.
[0193] Except for the above, resin paste A was prepared in the same manner as in Example 6. Then, using resin paste A, a compression molded body (resin composition layer), or a cured product or a substrate for evaluation containing a cured product was obtained in the same manner as in Example 6, and these were subjected to evaluation in the same manner as in Example 6.
[0194] [Comparative Example 1] In Example 1, 5 parts of a compound having a methacryloyl group and a polyethylene oxide structure ("M-130G" manufactured by Shin-Nakamura Chemical Co., Ltd.) as component (B) was changed to 5 parts of a compound having a methacryloyl group and a polyethylene oxide structure ("BPE-500" manufactured by Shin-Nakamura Chemical Co., Ltd., methacryloyl group equivalent: 402 g / eq.) as component (B'). That is, in Comparative Example 1, component (B) was not used.
[0195] Except for the above, resin paste A was prepared in the same manner as in Example 1. Then, using resin paste A, a compression molded body (resin composition layer), or a cured product or a substrate for evaluation containing a cured product was obtained in the same manner as in Example 1, and these were subjected to evaluation in the same manner as in Example 1.
[0196] [Comparative Example 2] In Example 6, 8 parts of an acid anhydride curing agent ("MH-700" manufactured by New Japan Chemical Co., Ltd.) as component (C) was changed to 0.5 parts of an amine curing agent ("Kayahard AA" manufactured by Nippon Kayaku Co., Ltd.) as component (H). In other words, in Comparative Example 2, component (C) was not used. In addition, in Example 6, 0.15 parts of the imidazole curing accelerator ("1B2PZ" manufactured by Shikoku Chemical Industries, Ltd.) as component (F) was changed to 0.2 parts of the imidazole curing accelerator ("2E4MZ" manufactured by Shikoku Chemical Industries, Ltd.) as component (F), and 85 parts of the inorganic filler A as component (E) was changed to 60 parts of the inorganic filler A as component (E).
[0197] Except for the above, resin paste A was prepared in the same manner as in Example 6. Then, using resin paste A, a compression molded body (resin composition layer), or a cured product or a substrate for evaluation containing a cured product was obtained in the same manner as in Example 6, and these were subjected to evaluation in the same manner as in Example 6.
[0198] [Comparative Example 3] In Comparative Example 2, 0.5 parts of the amine-based curing agent ("KAYAHARD AA" manufactured by Nippon Kayaku Co., Ltd.) as component (H) was changed to 1 part of dicyandiamide ("DICY7" manufactured by Mitsubishi Chemical Corporation) as component (H). That is, in Comparative Example 3, like Comparative Example 2, component (C) was not used.
[0199] Except for the above, resin paste A was prepared in the same manner as in Comparative Example 2. Then, using resin paste A, a compression molded body (resin composition layer), or a cured product or a substrate for evaluation containing a cured product was obtained in the same manner as in Comparative Example 2, and these were subjected to evaluation in the same manner as in Comparative Example 2.
[0200] [Comparative Example 4] In Comparative Example 2, 0.5 parts of an amine-based curing agent ("Kayahard AA" manufactured by Nippon Kayaku Co., Ltd.) as the component (H) was not used. That is, in Comparative Example 4, like Comparative Example 2, the component (C) was not used.
[0201] Except for the above, resin paste A was prepared in the same manner as in Comparative Example 2. Then, using resin paste A, a compression molded body (resin composition layer), or a cured product or a substrate for evaluation containing a cured product was obtained in the same manner as in Comparative Example 2, and these were subjected to evaluation in the same manner as in Comparative Example 2.
[0202] [Comparative Example 5] In Example 1, 5 parts of a compound having a methacryloyl group and a polyethylene oxide structure ("M-130G" manufactured by Shin-Nakamura Chemical Co., Ltd.) as component (B) was not used. That is, component (B) was not used in Comparative Example 5. In addition, 85 parts of inorganic filler A as component (E) in Example 1 was changed to 65 parts of inorganic filler A as component (E).
[0203] Except for the above, resin paste A was prepared in the same manner as in Example 1. Then, using resin paste A, a compression molded body (resin composition layer), or a cured product or a substrate for evaluation containing a cured product was obtained in the same manner as in Example 1, and these were subjected to evaluation in the same manner as in Example 1.
[0204] [Comparative Example 6] In Example 6, 8 parts of the acid anhydride curing agent ("MH-700" manufactured by New Japan Chemical Co., Ltd.) as component (C) was changed to 3 parts of the acid anhydride curing agent ("MH-700" manufactured by New Japan Chemical Co., Ltd.) as component (C). Also, in Example 6, 85 parts of the inorganic filler A as component (E) was changed to 65 parts of the inorganic filler A as component (E).
[0205] Except for the above, resin paste A was prepared in the same manner as in Example 6. Then, using resin paste A, a compression molded body (resin composition layer), or a cured product or a substrate for evaluation containing a cured product was obtained in the same manner as in Example 6, and these were subjected to evaluation in the same manner as in Example 6.
[0206] [Comparative Example 7] In Example 6, 5 parts of a compound having a methacryloyl group and a polyethylene oxide structure ("BPE-1300N" manufactured by Shin-Nakamura Chemical Co., Ltd.) as component (B) was changed to 1 part of a compound having a methacryloyl group and a polyethylene oxide structure ("BPE-1300N" manufactured by Shin-Nakamura Chemical Co., Ltd.) as component (B). Also, in Example 6, 85 parts of inorganic filler A as component (E) was changed to 70 parts of inorganic filler A as component (E).
[0207] Except for the above, resin paste A was prepared in the same manner as in Example 6. Then, using resin paste A, a compression molded body (resin composition layer), or a cured product or a substrate for evaluation containing a cured product was obtained in the same manner as in Example 6, and these were subjected to evaluation in the same manner as in Example 6.
[0208] [Comparative Example 8] In Example 6, 5 parts of a compound having a methacryloyl group and a polyethylene oxide structure ("BPE-1300N" manufactured by Shin-Nakamura Chemical Co., Ltd.) as component (B) was changed to 13 parts of a compound having a methacryloyl group and a polyethylene oxide structure ("BPE-1300N" manufactured by Shin-Nakamura Chemical Co., Ltd.) as component (B). Also, in Example 6, 85 parts of inorganic filler A as component (E) was changed to 110 parts of inorganic filler A as component (E).
[0209] Except for the above, resin paste A was prepared in the same manner as in Example 6. Then, using resin paste A, a compression molded body (resin composition layer), or a cured product or a substrate for evaluation containing a cured product was obtained in the same manner as in Example 6, and these were subjected to evaluation in the same manner as in Example 6.
[0210] [Evaluation method] The compression molded product (resin composition layer) or the cured product of the resin paste A obtained in the above-mentioned Examples and Comparative Examples, or the evaluation substrate containing the cured product, was obtained, and was evaluated in terms of warpage, elastic modulus, adhesion to inorganic materials, and peelability from film materials according to the following methods. Tables 1 and 2 show the evaluation results.
[0211] <Evaluation of peelability from film material> A compression molded product (resin composition layer) was obtained from resin paste A, and its peelability from the film material was evaluated as follows.
[0212] (Preparation of Evaluation Substrate Bb Including Resin Composition Layer Ba) First, a compression molding device equipped with a mold was prepared. A release film (AGC Corporation's double-sided matte finish film "Aflex (registered trademark) 50MW") was attached to the surface of the mold. Using this compression molding device, resin paste A was compression molded on a 12-inch silicon wafer (substrate) under the conditions of mold temperature Tc: 130 ° C., pressure: 6 MPa, and cure time: 10 minutes. As a result, an evaluation substrate was produced in the mold, consisting of a silicon wafer and a resin composition layer having a thickness of 150 μm as a compression molded body of resin paste A formed on the silicon wafer. The resin composition layer and evaluation substrate produced in this way are hereinafter also referred to as "resin composition layer Ba" and "evaluation substrate Bb", respectively.
[0213] (Evaluation of Resin Composition Layer Ba) After the compression molding was completed, it was confirmed whether the molds opened (i.e., whether the pair of opposing molds separated with the normal operating force set in the compression molding device). Furthermore, when the molds opened, it was observed whether the resin composition layer Ba peeled off from the release film and was on the silicon wafer. The results of these confirmations and observations were evaluated according to the following criteria. "○": As a result of the test, it was observed that the mold opened with normal operating force, and the resin composition layer B peeled off from the release film and was located on the silicon wafer. Therefore, the resin composition layer B was evaluated as having excellent releasability from the film material. "X": As a result of the test, the mold did not open with the normal operating force. Or, since the resin composition layer B did not peel off from the release film, (i) the entire evaluation substrate Bb was in a state of being adhered to the release film, or (ii) a part or the whole of the resin composition layer Ba was observed to have detached from the silicon wafer. Therefore, the resin composition layer Ba was evaluated as not having excellent releasability from the film material.
[0214] <Warpage evaluation> The resin composition layer Ba contained in the evaluation substrate Bb prepared for evaluating peelability from the film material was cured to obtain an evaluation substrate containing a cured product, and the warpage of the cured product was evaluated by measuring the amount of warpage of the evaluation substrate as described in detail below.
[0215] (Preparation of Evaluation Substrate Cb Including Cured Product Ca of Resin Composition Layer Ba) The resin composition layer Ba contained in the evaluation substrate Bb prepared for evaluation in the evaluation of the peelability from the film material was heated together with the silicon wafer at 150°C for 60 minutes. As a result, the resin composition layer Ba was thermally cured on the silicon wafer to form a cured product. The cured product of the resin composition layer and the evaluation substrate thus prepared are hereinafter also referred to as the "cured product Ca" and the "evaluation substrate Cb", respectively. In addition, in Comparative Examples 2 to 4 and 6, as a result of the evaluation of the peelability from the film material, the mold could not be opened with a normal operating force, so first, the release film was detached from the compression molding device, and then the evaluation substrate Bb with the release film attached thereto was taken out of one of the molds, and further, the release film was peeled off from the resin composition layer Ba to obtain the evaluation substrate Bb. In addition, in Comparative Examples 2 to 4 and 6, no interfacial peeling was observed between the resin composition layer Ba and the silicon wafer and between the resin composition layer Ba and the release film. Therefore, in Comparative Examples 2 to 4 and 6 as well, the evaluation substrate Cb containing the cured product Ca of the resin composition layer Ba was obtained as described above.
[0216] (Measurement and evaluation of warpage) The amount of warpage of each evaluation substrate Cb was measured indoors at 25°C using a shadow moire measurement device ("ThermoireAXP" manufactured by Akorometrix). The measurement was performed in accordance with the JEITA EDX-7311-24 standard of the Japan Electronics and Information Technology Industries Association. Specifically, a virtual plane calculated by the least squares method of all data on the substrate surface in the measurement area was used as the reference plane, and the difference between the minimum and maximum values in the vertical direction from the reference plane was calculated as the amount of warpage.
[0217] The amount of warpage was evaluated according to the following criteria. "Excellent": The amount of warping was less than 1500 μm, and was evaluated as being particularly small. "Good": The amount of warping was 1500 μm or more and less than 2000 μm, and was evaluated as being sufficiently small. "△": The amount of warping was 1500 μm or more and less than 2000 μm, and the amount of warping was evaluated as being small. "X": The amount of warping was 2300 μm or more, and was evaluated as being large.
[0218] <Evaluation of adhesion to inorganic materials> A cured product was obtained using Resin Paste A, and the adhesion to inorganic materials was evaluated by measuring the adhesive strength between the product and copper foil, as described in detail below.
[0219] (Preparation of Laminate Db Including Resin Composition Layer Da of Resin Paste A) First, a compression molding device equipped with a mold was prepared. Using this compression molding device, the resin paste A placed on the glossy surface (shiny surface) of the copper foil having a thickness of 18 μm on a SUS plate (12 inches) coated with a release agent was compression molded under the conditions of a mold temperature Tc: 130° C., a pressure: 6 MPa, and a cure time: 10 minutes. After compression molding, the resin composition layer was peeled off from the SUS plate. As a result, a laminate consisting of a resin composition layer having a thickness of 300 μm as a compression molded body of the resin paste A and the copper foil provided on the resin composition layer was obtained. In this laminate, the non-glossy surface (matte surface) of the copper foil was exposed. The resin composition layer and laminate thus prepared are hereinafter also referred to as "resin composition layer Da" and "laminate Db", respectively.
[0220] (Preparation of Laminate Eb Including Cured Product Ea of Resin Composition Layer Da) Subsequently, the laminate Db was heated at 150° C. for 60 minutes. As a result, the resin composition layer Da was thermally cured with the copper foil still attached to form a cured product. The cured product of the resin composition layer and the laminate thus produced are hereinafter also referred to as the “cured product Ea” and the “laminate Eb”, respectively.
[0221] (Preparation of test piece F) Next, the laminate Eb was cut into 1 cm squares, thereby obtaining a number of test piece materials each having a size of 1 cm square and a thickness of 318 μm.
[0222] Further, one adhesive-attached stud pin (φ5.8 mm) was vertically set up on the matte surface of the copper foil of each test piece material. Then, an adhesive-attached backing plate was placed on the surface of the cured product (cured product Ea) of the resin composition layer of the test piece material. This resulted in a laminate having the backing plate, the test piece material, and the stud pin in this order. Then, this laminate was heated at 150°C for 60 minutes. As a result, the adhesive solidified, and the copper foil and the stud pin were fixed, and a laminate in which the test piece material and the backing plate were fixed was obtained. Then, at the bonding portion of the copper foil with the stud pin, a cutter was used to make a cut only in the copper foil along the peripheral surface (φ5.8 mm) of the stud pin. The laminate obtained in this manner is also referred to as "test piece F" below.
[0223] (Measurement and evaluation of adhesive strength between cured material Ea and inorganic materials) A vertical tensile test was performed on each of the obtained test pieces F at a test speed of 0.1 kg / sec using a vertical tensile tester "ROMULUS" manufactured by QUAD GROUP, and a measured value indicating the peel strength of the copper foil (hereinafter also simply referred to as "adhesive strength") was obtained. Specifically, this measured value usually indicates the adhesive strength between the cured product Ea and the copper foil as an inorganic material. Measurements were performed on five test pieces F, and the average measured value of the adhesive strength was calculated. The average value of the calculated measured values of adhesive strength was then evaluated according to the following criteria. "○": The average measured value of adhesive strength is 100kgf / cm 2 As described above, the cured product Ea was evaluated as having excellent adhesion to inorganic materials. "X": The average measured value of adhesive strength is 100kgf / cm 2 The cured product Ea was evaluated as not having excellent adhesion to inorganic materials.
[0224] <Evaluation of elastic modulus> The elastic modulus of the cured product obtained using Resin Paste A was evaluated as described in detail below.
[0225] (Preparation of Laminate Gb Including Resin Composition Layer Ga of Resin Paste A) Using a compression molding device (mold temperature Tc: 130°C, pressure: 6 MPa, cure time: 10 minutes), resin paste A placed on a SUS plate with a release treatment on its surface was compression molded in a mold. This resulted in a laminate consisting of a SUS plate and a 300 μm thick resin composition layer as a compression molded body of resin paste A provided on the SUS plate. The resin composition layer and laminate produced in this way are hereinafter also referred to as "resin composition layer Ga" and "laminate Gb", respectively.
[0226] (Preparation of cured product H of resin composition layer Ga) Next, the laminate Gb was heated at 150°C for 60 minutes. As a result, the resin composition layer Ga was thermally cured on the SUS plate to form a cured product. Then, this cured product was peeled off from the SUS plate. The cured product of the resin composition layer thus produced is hereinafter also referred to as "cured product H".
[0227] (Preparation of test piece I and measurement and evaluation of elastic modulus at 25℃) Next, three test pieces of No. 1 shape, which is a dumbbell shape when viewed from above, were cut out from the cured product H. Each test piece thus obtained is hereinafter also referred to as "test piece I". Next, a tensile test was performed on each test piece I in a room at 25°C using a tensile tester "RTC-1250A" manufactured by Orientec Co., Ltd., to measure the elastic modulus (GPa) at 25°C. The measurement was performed in accordance with JIS K7127:1999. The average value of the measured values of the elastic modulus at 25°C of the three test pieces I was calculated. The calculated average value of the measured elastic modulus at 25° C. was then evaluated according to the following criteria. "◯": The average measured value of the elastic modulus at 25° C. was 9 GPa or more, and the elastic modulus was evaluated as being high. "△": The average measured value of the elastic modulus at 25° C. was 7 GPa or more and less than 9 GPa, and the elastic modulus was evaluated as being sufficiently high. "X": The average measured value of the elastic modulus at 25° C. was less than 7 GPa, and the elastic modulus was evaluated as being low.
[0228] [result] The results of the above-mentioned Examples and Comparative Examples are shown in Tables 1 and 2 below.
[0229] In Tables 1 and 2 below, the amount of each component is expressed in terms of non-volatile components. Furthermore, the "resin component" shown in Tables 1 and 2 refers to the non-volatile components in the resin composition other than the (E) inorganic filler. The "mass ratio [b]:[c]" indicates the mass ratio of the (B) component to the (C) component. The "content of the (B) component in the resin components" indicates the content of the (C) component when the resin component is taken as 100 mass% of the non-volatile components in the resin composition. "Equivalent ratio (c) / (a)" refers to the equivalent ratio (c) / (a) of the sum of the amount (g) of component (C) divided by the equivalent (g / eq.) of the acid anhydride groups in component (C) divided by the equivalent (g / eq.) of the epoxy groups in component (A). "Content of component (E) in resin composition" refers to the content of component (E) when the content of non-volatile components in the resin composition is taken as 100 mass%. "ΔT of component (D)" refers to the difference (°C) between the mold temperature Tc (130°C) during compression molding and the 10-hour half-life temperature T10 (°C) of component (D).
[0230] [Table 1]
[0231] [Table 2]
[0232] <Consideration> As can be seen from Tables 1 and 2, by comparing the Examples and Comparative Examples, the resin composition in the Examples is (A) an epoxy resin, and (B) a compound having a radical polymerizable unsaturated group and an alkylene oxide structure, and represented by the following formula (1): E / N-(100×N)≧50 (1) (In formula (1), E represents the equivalent (g / eq.) of the radically polymerizable unsaturated group, and N represents the number of radically polymerizable unsaturated groups in the molecule and is an integer of 1 or more.) It has been found that by containing a compound satisfying the above condition, (C) an acid anhydride, (D) a radical generator, and (E) an inorganic filler, and the mass ratio of the (B) component to the (C) component, [b]:[c], is within the range of 0.2:1 to 1.5:1, a cured product having small warpage, a high elastic modulus, and excellent adhesion to inorganic materials can be obtained, and a resin composition or resin paste having excellent peelability from film materials can be provided.
[0233] Furthermore, it has been found that it is also possible to provide a cured product, a resin sheet, a printed wiring board, a semiconductor chip package, and a semiconductor device obtained by using the resin composition or resin paste according to the examples.
Claims
1. (A) an epoxy resin, (B) A compound having a radical polymerizable unsaturated group and a polyalkylene oxide structure in the molecule, which is represented by the following formula (1): E / N-(100×N)≧50...(1) (In formula (1), E represents the equivalent (g / eq.) of the radically polymerizable unsaturated group, and N represents the number of radically polymerizable unsaturated groups in the molecule and is an integer of 1 or more.) A compound that satisfies (C) acid anhydride, (D) a radical generator, and (E) containing an inorganic filler, the mass ratio of the component (B) to the component (C), [b]:[c], is within the range of 0.2:1 to 1.5:1; A resin composition, wherein the polyalkylene oxide structure of component (B) is represented by the formula -(R B O) n -, in which n is an integer of 2 or more, and each R B is independently an alkylene group having 2 to 4 carbon atoms.
2. A plurality of groups R B At least one group R B The resin composition according to claim 1 , wherein contains an ethylene group.
3. The resin composition according to claim 1 or 2, wherein the radically polymerizable unsaturated group contained in the component (B) is at least one selected from the group consisting of a vinyl group, an allyl group, a 1-butenyl group, a 2-butenyl group, an acryloyl group, a methacryloyl group, a fumaroyl group, a maleoyl group, a vinylphenyl group, a styryl group, and a cinnamoyl group.
4. The resin composition according to claim 3, wherein the radically polymerizable unsaturated group contained in the component (B) includes at least one type selected from the group consisting of a methacryloyl group and an acryloyl group.
5. The resin composition according to claim 3 or 4, wherein the radically polymerizable unsaturated group contained in the component (B) includes a methacryloyl group.
6. The resin composition according to any one of claims 1 to 5, wherein the component (B) comprises one or more compounds selected from the group consisting of a compound in which N in formula (1) is 1 and a compound in which N in formula (1) is 2.
7. The resin composition according to claim 6, wherein the compound in which N in formula (1) is 1 has a molecular weight of 150 or more.
8. The resin composition according to claim 6 or 7, wherein the compound in which N is 2 in formula (1) has an equivalent weight (g / eq.) of the radically polymerizable unsaturated group of 500 or more.
9. The resin composition according to any one of claims 1 to 8, wherein the equivalent weight of the radically polymerizable unsaturated group of component (B) is 4500 g / eq. or less.
10. The content of the component (B) is 10 mass% or more and 40 mass% or less, when the content of the components other than the inorganic filler (E) among the non-volatile components in the resin composition is 100 mass%. The resin composition according to any one of claims 1 to 9.
11. The resin composition according to any one of claims 1 to 10, wherein the equivalent ratio (c) / (a) of the sum of values obtained by dividing the amount (g) of the component (C) by the equivalent (g / eq.) of an acid anhydride group contained in the component (C) to the sum of values obtained by dividing the amount (g) of the component (A) by the equivalent (g / eq.) of an epoxy group contained in the component (A) is 0.4 or more.
12. The resin composition according to any one of claims 1 to 11, wherein the component (D) is one or more selected from radical generators having a 10-hour half-life temperature T10 (°C) in the range of 50°C or more and 110°C or less.
13. The resin composition according to any one of claims 1 to 12, wherein the content of the component (E) is 70 mass% or more when the content of the non-volatile components in the resin composition is 100 mass%.
14. The resin composition according to any one of claims 1 to 13, which is for compression molding.
15. 15. The resin composition according to claim 14, wherein the component (D) is one or more radical generators selected from radical generators having a difference ΔT (°C) between the mold temperature Tc (°C) during compression molding and the 10-hour half-life temperature T10 (°C) of the component (D) in the range of 20°C to 80°C.
16. The resin composition according to any one of claims 1 to 15, which is for forming an insulating layer.
17. A resin paste comprising the resin composition according to any one of claims 1 to 16.
18. A cured product of the resin composition according to any one of claims 1 to 16 or the resin paste according to claim 17.
19. A resin sheet having a support and a resin composition layer comprising the resin composition according to any one of claims 1 to 16 or the resin paste according to claim 17 provided on the support.
20. A printed wiring board comprising an insulating layer formed from the resin composition according to any one of claims 1 to 16 or the cured product of the resin paste according to claim 17.
21. 21. A semiconductor chip package comprising the printed wiring board according to claim 20 and a semiconductor chip mounted on the printed wiring board.
22. A semiconductor chip package comprising a semiconductor chip and a cured product of the resin composition according to any one of claims 1 to 16 or the resin paste according to claim 17 that encapsulates the semiconductor chip.
23. A semiconductor device comprising the printed wiring board according to claim 20 or the semiconductor chip package according to claim 21 or 22.
24. A step of forming a resin composition layer containing the resin composition according to any one of claims 1 to 16 or a resin composition layer containing the resin paste according to claim 17 on a circuit board by a compression molding method; curing the resin composition layer; A method for manufacturing a printed wiring board, comprising:
25. A step of forming a resin composition layer containing the resin composition according to any one of claims 1 to 16 or a resin composition layer containing the resin paste according to claim 17 on a semiconductor chip by a compression molding method; curing the resin composition layer; A method for manufacturing a semiconductor chip package, comprising:
Citation Information
Patent Citations
Liquid epoxy rein composition and resin-sealed type semiconductor apparatus
JP1999255864A
Resin composition of electrically insulating material and electrically insulating laminate material
JP2005015639A
Resin composition, optical member using the same and its manufacturing method
JP2006307088A
Resin composition, optical member using the same, and method for producing the same
JP2007138126A
Thermosetting resin composition with excellent coating and recoating properties
JP2013536275A