Method for manufacturing a semiconductor substrate, a semiconductor substrate, a method for manufacturing a composite semiconductor substrate, a composite semiconductor substrate, and a semiconductor junction substrate
The ion implantation and laser irradiation method efficiently separates semiconductor layers from seed substrates, addressing inefficiencies in existing methods by reducing manufacturing time and costs while ensuring a flat surface, suitable for various applications.
Patent Information
- Application Number
- JP2022185070
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2015-01-16
- Filing Date
- 2022-11-18
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2036-01-15
AI Technical Summary
Existing methods for separating semiconductor layers from seed substrates are inefficient, leading to increased manufacturing costs, rough surfaces, and potential cracking due to uneven laser intensity and slow etching rates, especially for large or thin substrates.
A method involving ion implantation to form a weakened ion implantation layer in the seed substrate, followed by laser irradiation to break atomic bonds without direct cleavage, allowing for rapid and flat separation of semiconductor layers.
Enables rapid separation of semiconductor layers with a smooth surface, reducing manufacturing time and costs, while avoiding thermal and electrical constraints, and allowing for a wide range of applications including AuSn-based and In-based soldering.
Smart Images

Figure 0007582284000014 
Figure 0007582284000015 
Figure 0007582284000016
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a semiconductor substrate, a semiconductor substrate, a method for manufacturing a composite semiconductor substrate, a composite semiconductor substrate, and a semiconductor junction substrate. [Background technology]
[0002] Semiconductor substrates are built into all kinds of electronics and are widely used, and wide band gap semiconductor substrates in particular are a material that is expected to be used in the future as semiconductor substrates for highly efficient devices that contribute to energy conservation, power devices, etc. Diamond substrates in particular are not only used as semiconductor substrates, but are also widely used as materials for various tools (cutting tools such as drills, end mills, milling cutters, cutters, and bits, abrasion-resistant tools such as dies, jet nozzles for water and other fluids, and stitchels), optical components (windows, lenses, etc.), and electronic components (heat dissipation substrates, etc.), and their importance is expected to increase further in the future.
[0003] Most semiconductors can be formed into thin films, plates, or bulk shapes by chemical vapor deposition (hereinafter referred to as CVD).
[0004] In the vapor phase synthesis method, a semiconductor layer is grown on a seed substrate, which is a seed crystal. The semiconductor layer can be used together with the seed substrate. Alternatively, the semiconductor layer can be separated from the seed substrate and used as a product by itself. In this case, the seed substrate can be reused, which reduces manufacturing costs.
[0005] Patent Document 1 (JP Patent Publication No. 6-234595) discloses a method in which a first diamond layer having high optical transparency and a second diamond layer having low optical transparency are alternately laminated by vapor phase synthesis, and this laminate is irradiated with laser light to cause the second diamond layer to absorb the laser light, and the first diamond layer is separated as a thin diamond plate.
[0006] Patent Document 2 (JP Patent Publication No. 2007-112637) discloses a method of obtaining a laminate by growing a first diamond layer having low optical transparency and a second diamond layer having high optical transparency on a substrate by vapor phase synthesis, modifying the first diamond layer by irradiating the upper or lower surface of the laminate with laser light, and peeling off the modified first diamond layer by a process such as heat treatment, electrochemical etching or acid etching, thereby separating the second diamond layer.
[0007] Patent Document 3 (US Pat. No. 5,587,210 specification) discloses a method in which ions are implanted into a diamond substrate to form a damage layer made of non-diamond carbon inside the substrate, diamond is then grown on the substrate by vapor phase synthesis, and the damage layer is then electrochemically etched to separate the grown diamond from the substrate.
[0008] In order to reduce the manufacturing cost, it is also effective to use a thinly sliced seed substrate.
[0009] Patent Document 4 (JP 2011-60860 A) discloses a method of forming a modified layer inside a substrate by irradiating the substrate surface with laser light, and then etching the modified layer to slice the substrate.
[0010] Patent document 5 (JP 2012-169363 A) discloses a method for processing a substrate, in which a modified layer is formed inside the substrate by irradiating the substrate surface with laser light, and then the substrate is cut at or near the modified layer.
[0011] Patent Document 6 (JP 2011-60862 A) discloses a method for slicing a substrate, in which a modified layer is formed inside the substrate by irradiating the substrate surface with laser light, and then a groove is formed in the modified layer and the substrate is peeled off using the groove as a base point. [Prior art documents] [Patent documents]
[0012] [Patent Document 1] Japanese Patent Application Publication No. 6-234595 [Patent Document 2] JP 2007-112637 A [Patent Document 3] US Patent No. 5,587,210 [Patent Document 4] JP 2011-60860 A [Patent Document 5] JP 2012-169363 A [Patent Document 6] JP 2011-60862 A Summary of the Invention [Problem to be solved by the invention]
[0013] In the method of Patent Document 1, in order to fully cleave the second diamond layer that absorbs the laser light with the laser light, it is necessary to cut the bond of diamond, which is the hardest material. For such cleavage, it is necessary to maintain the laser light intensity strong enough. At this time, on the surface of the first diamond layer, which should originally transmit the laser light, the laser light intensity may partially exceed the processing threshold due to the influence of dust or unevenness on the surface, and the first diamond layer may also be processed. In addition, since the second diamond layer is cleaved suddenly, the cleavage boundary may reach the first diamond layer due to the momentum of the cleavage, and there is a problem that the separated surface becomes rough. In addition, the entire diamond may break due to the impact during processing.
[0014] In Patent Documents 2 to 4, the thickness of the layer to be etched (hereinafter also referred to as the damaged layer) is very thin, so the penetration speed of the etching solution into the damaged layer is very slow. Therefore, when the size of the substrate increases, the diamond separation speed becomes very slow, which causes a problem of increasing manufacturing costs. In some cases, the solution does not penetrate into the damaged layer, making separation impossible.
[0015] In Patent Documents 5 and 6, the substrate is peeled off by applying a physical force to the modified layer, which causes problems in that the surface of the obtained substrate is likely to become rough. In addition, if the thickness of the substrate is not sufficiently large for its size, the substrate may crack.
[0016] Therefore, a first object of the present invention is to provide a method for manufacturing a semiconductor substrate, which enables a semiconductor layer to be separated from a part of a seed substrate in a short time, and further enables separation even when the seed substrate is thin or the size of the seed substrate is large, and results in a flat separation surface, a semiconductor substrate obtained by the method for manufacturing a semiconductor substrate, and a semiconductor junction substrate from which the semiconductor substrate can be separated.
[0017] A second object of the present invention is to provide a method for manufacturing a composite semiconductor substrate, which can thinly slice a seed substrate in a short time and produce flat sliced surfaces, and a composite semiconductor substrate obtained by the manufacturing method for the composite semiconductor substrate. [Means for solving the problem]
[0018] A method for manufacturing a semiconductor substrate according to one embodiment of the present invention includes the steps of: preparing a seed substrate containing a semiconductor material; implanting ions into the seed substrate to form an ion-implanted layer (a layer in which implanted ions remain) at a certain depth from a surface of a main surface of the seed substrate; growing a semiconductor layer on the main surface of the seed substrate by a vapor phase synthesis method; and separating a semiconductor substrate including the semiconductor layer and a part of the seed substrate by irradiating light from a surface of at least one of the main surfaces of the semiconductor layer and the seed substrate.
[0019] This method does not directly break the bond state of the semiconductor elements by light (laser light, etc.), nor does it form a modified or altered layer in the semiconductor by light. Instead, the bonds of the elements in the semiconductor are loosened by ion implantation, and the laser directly or indirectly gives energy to the ions (atoms or molecules) that remain inside by the implantation, and the expansion energy of the implanted ions (atoms or molecules) breaks the bonds of the semiconductor. In ion implantation, although the energy of each atom is high, each atom is small, so the effect is that the total energy is small. In other words, the energy of one atom is enough to loosen or break the bonds of the diamond, but is much smaller than the energy that would break the entire diamond. In such a situation, the principle of the present invention is to give energy to the atoms that remain inside by ion implantation by light, causing them to evaporate, expand, or simply expand, and to cut only the weakened part (the implantation interface). This achieves the purpose of separating the substrate and the grown semiconductor with much smaller light energy than the conventional method of cutting using only light. In the method of directly cutting the bonds of semiconductor elements with light, a focused laser applies isotropic force to the semiconductor crystal at one point, which applies force not only in the direction you want to separate but also in the direction that breaks the substrate, which can cause the substrate to crack. However, if the area where the ions will remain is formed into a planar shape by prior implantation, the weak area becomes planar, and even if the light is focused at one point, the cracking direction is not isotropic, as if there is a cutting line, but acts in a direction that tears the ion-implanted surface vertically. Even if the light is focused at one point, it can be cleanly separated by scanning.
[0020] A semiconductor substrate according to one aspect of the present invention is a semiconductor substrate obtained by the above-described method for producing a semiconductor substrate.
[0021] A semiconductor substrate according to one aspect of the present invention is a semiconductor substrate including a semiconductor layer formed by a vapor phase synthesis method, the semiconductor substrate including a first main surface and a second main surface, the first main surface including a first element different in type or bonding state from a main element constituting the semiconductor substrate, the first element including at least one element selected from the group consisting of hydrogen, oxygen, nitrogen, carbon, helium, neon and argon, and the surface roughness of the first main surface being less than 10 μm. Here, the main element constituting the semiconductor substrate means an element constituting the semiconductor lattice of the semiconductor substrate and contained at 1 atm% or more in atomic ratio. Here, the different bonding state means the following. In the case of carbon, sp 3 Bonds and sp 2 The bond is a different bond state, and when a metal is bonded to nitrogen, the bond state with oxygen or the metal bond is a different bond state. Here, the surface roughness is Ra as defined in JIS B 0601-2013, and is the arithmetic average value of the surface irregularities. The same applies below. The first element is present on the first main surface, for example, so as to form a pattern of multiple approximately circular shapes.
[0022] A method for manufacturing a composite semiconductor substrate according to one embodiment of the present invention includes the steps of: preparing a seed substrate containing a semiconductor material; forming an ion-implanted layer at a certain depth from a surface of a main surface of the seed substrate by implanting ions into the seed substrate; growing a semiconductor layer on the main surface of the seed substrate by a vapor phase synthesis method; bonding a first substrate onto the semiconductor layer; and separating a composite semiconductor substrate including the first substrate, the semiconductor layer, and a part of the seed substrate by irradiating light from a surface of a main surface of at least one of the first substrate and the seed substrate.
[0023] A method for manufacturing a composite semiconductor substrate according to one embodiment of the present invention includes the steps of: preparing a seed substrate containing a semiconductor material; forming an ion-implanted layer at a certain depth from a surface of a main surface of the seed substrate by implanting ions into the seed substrate; bonding a first substrate onto the main surface of the seed substrate; and separating a composite semiconductor substrate including the first substrate and a portion of the seed substrate by irradiating light from a surface of a main surface of at least one of the first substrate and the seed substrate.
[0024] A compound semiconductor substrate according to one aspect of the present invention is a compound semiconductor substrate obtained by the above-mentioned compound semiconductor substrate manufacturing method.
[0025] A composite semiconductor substrate according to one embodiment of the present invention is a composite semiconductor substrate including a first substrate and a semiconductor layer laminated on a main surface of the first substrate, the main surface of the composite semiconductor substrate on the semiconductor layer side contains a first element different in type or bonding state from a main element constituting the semiconductor layer, the first element contains at least one element selected from the group consisting of hydrogen, oxygen, nitrogen, carbon, helium, neon and argon, the main surface of the composite semiconductor substrate on the semiconductor layer side has a surface roughness of less than 10 μm, and the semiconductor layer has a thickness of 0.1 μm to 50 μm. Here, the main element constituting the semiconductor layer means an element constituting the semiconductor lattice of the semiconductor layer and contained at 1 atm% or more in atomic ratio. Here, the different bonding state means the following. In the case of carbon, sp 3 Bonds and sp 2 Bonding is a different bonding state, and if a metal is bonded to nitrogen, it is a different bonding state than if it is bonded to oxygen or metallic.
[0026] A semiconductor junction substrate according to one embodiment of the present invention includes a seed substrate containing a semiconductor material and a semiconductor layer disposed on a primary surface of the seed substrate, the seed substrate having an ion-implanted layer containing a first element different in type or bonding state from a main element constituting the semiconductor material, the first element being at least one element selected from the group consisting of hydrogen, oxygen, nitrogen, carbon, helium, neon and argon. Here, the main element constituting the semiconductor material means an element constituting the semiconductor lattice of the semiconductor material and contained at 1 atm% or more in atomic ratio. Here, the different bonding state means the following. In the case of carbon, sp 3 Bonds and sp 2 Bonding is a different bonding state, and if a metal is bonded to nitrogen, it is a different bonding state than if it is bonded to oxygen or metallic. Effect of the Invention
[0027] According to the above aspect, it is possible to provide a method for manufacturing a semiconductor substrate in which a semiconductor layer can be separated from a part of a seed substrate in a short time, and further, even if the seed substrate is thin or the size of the seed substrate is large, and the separation surface is flat, and a semiconductor substrate obtained by the method for manufacturing a semiconductor substrate can be provided. Furthermore, since there are no thermal or electrical constraints, the degree of freedom during separation is high, such as separation at room temperature, and a wide range of applications are possible. For example, there are applications in which AuSn-based, Sn-based, In-based, etc. can be separated after soldering.
[0028] According to the above aspect, it is possible to provide a method for manufacturing a composite semiconductor substrate that can slice a seed substrate thinly in a short time and produce flat sliced surfaces, as well as a composite semiconductor substrate obtained by the method for manufacturing the composite semiconductor substrate. In a conventional separation method that uses the principle of cutting atomic bonds in semiconductors with a laser, it is necessary to concentrate energy in an extremely small area to prevent cracks and cut bonds. However, in the present invention, it is possible to cut bonds without worrying about cracks caused by irradiation of a large area. If the area of one irradiation is large, the time required for irradiation with the scanning light (such as laser light) can be shortened. [Brief description of the drawings]
[0029] [Figure 1] 1(A) to 1(E) are diagrams that diagrammatically show a method for manufacturing a semiconductor substrate according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a flowchart showing a method for manufacturing a semiconductor substrate according to one embodiment of the present invention. [Diagram 3] 3(A) to 3(F) are diagrams illustrating a method for manufacturing a composite semiconductor substrate according to one embodiment of the present invention. [Figure 4] FIG. 4 is a flow chart illustrating a method for manufacturing a composite semiconductor substrate according to one embodiment of the present invention. [Diagram 5] 5(A) to 5(E) are diagrams illustrating a method for manufacturing a composite semiconductor substrate according to one embodiment of the present invention. [Figure 6] FIG. 6 is a flowchart showing a method for manufacturing a semiconductor substrate according to one embodiment of the present invention. [Figure 7] 7(A) to 7(D) are diagrams that diagrammatically show a method for manufacturing a semiconductor substrate according to one embodiment of the present invention. [Figure 8] FIG. 8 is a flowchart showing a method for manufacturing a semiconductor substrate according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] [Description of the embodiment of the present invention] First, the embodiments of the present invention will be listed and described.
[0031] A method for manufacturing a semiconductor substrate according to one aspect of the present invention includes: (1) a step of preparing a seed substrate containing a semiconductor material; a step of forming an ion-implanted layer (a layer in which the implanted ions remain) at a certain depth from the surface of a main surface of the seed substrate by implanting ions into the seed substrate; and a step of separating a semiconductor substrate including a part of the seed substrate by irradiating the surface of the main surface of the seed substrate with light; or (2) a step of preparing a seed substrate containing a semiconductor material; a step of forming an ion-implanted layer (a layer in which the implanted ions remain) at a certain depth from the surface of the main surface of the seed substrate by implanting ions into the seed substrate; a step of growing a semiconductor layer on the main surface of the seed substrate by a vapor phase synthesis method; and a step of separating a semiconductor substrate including the semiconductor layer and a part of the seed substrate by irradiating the surface of at least one of the main surfaces of the semiconductor layer and the seed substrate with light.
[0032] The ion-implanted layer does not necessarily have to be a layer with high light absorption. In the case of a semiconductor containing carbon such as diamond, when a specific ion is implanted at a specific concentration or higher, the carbon bond is broken and the carbon sp 2 The bonds increase, the material turns black, and a light absorbing layer may form. However, even if ions are implanted below a certain concentration, or if certain ions (mainly hydrogen ions) are implanted, the light absorption coefficient often does not increase if the carbon bonds are terminated. In semiconductors other than diamond, the sp 2 If no bonds are formed, there may be cases where the light absorption coefficient barely increases even above a certain concentration. However, even if the light absorption coefficient does not increase, the bonds of the elements that make up the substrate are broken or loosened, so if energy is applied to the surrounding lattice by laser irradiation or to the directly implanted ions, energy is applied to the ions or molecules that ultimately expand, vaporizing and expanding them, and sufficient strength is obtained to separate the substrate.
[0033] According to the above aspect, the semiconductor substrate can be separated from the part of the seed substrate in a short time. Furthermore, even if the seed substrate is thin or the size of the seed substrate is large, the semiconductor substrate can be separated from the part of the seed substrate. Furthermore, a semiconductor substrate having a flat separated surface can be obtained.
[0034] In the above embodiment, an ion-implanted layer having a lower crystallinity than the seed substrate is formed in the seed substrate by ion implantation. That is, an ion-implanted layer having a weak bond is formed in advance in the seed substrate. As a result, light irradiated from the main surface of the seed substrate, or from the main surface of at least one of the semiconductor layer and the seed substrate, is absorbed in the ion-implanted layer or in the vicinity thereof. The energy of the absorbed light gasifies and expands the ions (atoms or molecules) present in the ion-implanted layer, pushing out the part of the ion-implanted layer with weak bonds, and separates the semiconductor substrate including a part of the seed substrate, or the semiconductor substrate including the semiconductor layer and a part of the seed substrate. That is, the method for manufacturing a semiconductor substrate of the above embodiment can separate the semiconductor substrate without using the action of directly altering or splitting the semiconductor forming the seed substrate by irradiation with light (including laser light). Therefore, compared with the method of directly splitting the semiconductor forming the seed substrate by irradiation with light, irradiation with light can be performed with lower power and in a larger area (beam size), so that the semiconductor substrate can be separated in a short time.
[0035] According to the above aspect, instead of a method of directly cutting strong bonds between semiconductor elements, the ion-implanted layer or its vicinity is irradiated with irradiation light, and the energy is applied to the implanted layer or its vicinity to vaporize the implanted element present in the implanted layer, and the upper and lower surfaces of the ion-implanted layer are spread apart by gas pressure, making it possible to separate the semiconductor substrate from most of the seed substrate with very low power.
[0036] According to the above embodiment, the separation of the semiconductor substrate can be performed at room temperature. That is, even if the temperature required to gasify the injected element is equal to or higher than the temperature at which the semiconductor melts, the energy of the irradiated light acts on the locally injected element to generate the desired gas pressure, and there is no need to expose the entire semiconductor substrate to high temperatures. Therefore, the semiconductor constituting the seed substrate or semiconductor layer is hardly affected by melting, alteration, detachment or reconstruction of surface atoms, diffusion of doping atoms, etc. due to heat. The energy of the irradiated light acts on the surface where defects are introduced by ion implantation (the ion-implanted layer, that is, the layer where the implanted ions remain), but does not act on the crystal parts where defects are not introduced, so that cracks and the like hardly occur in places other than the ion-implanted layer. And, in the ion-implanted layer, peeling proceeds easily as if removing the cut line of the perforation.
[0037] The separation of the semiconductor substrate can also be performed by raising the temperature to a desired level. In this case, temperature constraints, ion implantation dose constraints, time constraints, equipment constraints, and other constraints can be selected and set from a much wider range of conditions than in the past separation techniques.
[0038] According to the above aspect, the irradiated light may act on the element introduced when the seed substrate is ion-implanted, the ion-implanted layer, or the vicinity thereof, and therefore, it is possible to use irradiated light with a lower power than that used in the conventional direct cleavage of semiconductor atomic bonds.
[0039] (3) The ion-implanted layer has a thickness of 50 nm to 10 μm, and an ion dose of 1×10 14 cm -2 More than 2×10 18 cm -2 The following range is preferable: This can shorten the time required to separate the semiconductor substrate from the part of the seed substrate.
[0040] (4) The ion implantation is preferably performed using ions containing at least one element selected from the group consisting of hydrogen, oxygen, nitrogen, carbon, helium, neon, and argon. These ions are easily gasified when they indirectly or directly absorb the energy of light. Therefore, the light irradiation energy can be used efficiently, and the time required to separate the semiconductor substrate from the part of the seed substrate can be shortened. In addition, the ion implantation is preferably performed using ions containing at least one molecule selected from the group consisting of hydrogen molecules, oxygen molecules, and nitrogen molecules. These molecular ions are more easily gasified than single atoms when they indirectly or directly absorb the energy of light. Therefore, the light irradiation energy can be used more efficiently, and the time required to separate the semiconductor substrate from the part of the seed substrate can be shortened.
[0041] (5) The light is pulsed light, and the irradiation fluence per pulse on the surface of the main surface to which the light is irradiated is 0.01 J / mm 2 More than 1500J / mm 2 According to this, the light does not damage the surfaces of the semiconductor layer and the main surface of the seed substrate, and does not cause cracks inside the seed substrate and the semiconductor layer, and it is possible to destroy only the ion-implanted layer.
[0042] (6) It is preferable that the light is pulsed light, and the pulse energy at the surface of the main face to which the light is irradiated is 0.05 mJ or more and 1000 mJ or less. With this, the surface of the main face to which the light is irradiated is not destroyed by the light, and when a seed substrate and a semiconductor layer are present, cracks are not generated inside the semiconductor layer, and only the ion-implanted layer can be destroyed.
[0043] (7) The light is preferably laser light, and the surface of the main surface to be irradiated with the light is preferably scanned. When laser light is used, strong light can be generated with one pulse, and the intensity and pulse width of one pulse can be easily controlled. In addition, the light can be easily focused or broadened, and the power density can be adjusted. Furthermore, the wavelength of laser light can be selected, and it is possible to select a wavelength that is difficult to absorb by semiconductors with good crystallinity and easily absorbed by ion-implanted layers or defects with poor crystallinity.
[0044] (8) The step of separating the semiconductor substrate is preferably carried out in a liquid, which can reduce the impact of light irradiation on the seed substrate and, if any, the semiconductor layer, and therefore can suppress the occurrence of cracks or breakage in the seed substrate or the semiconductor layer.
[0045] (9) The semiconductor layer preferably contains at least one selected from the group consisting of diamond, aluminum nitride, gallium nitride, silicon carbide, zinc selenide, and zinc sulfide. The semiconductor layer containing these semiconductors can be suitably used as a material for a semiconductor device. These semiconductor materials may be polycrystalline or may be used for optical purposes.
[0046] (10) A semiconductor substrate according to an aspect of the present invention is a semiconductor obtained by the method for producing a semiconductor substrate according to any one of (1) to (9) above. The semiconductor substrate can be produced at reduced cost because the time required for separation from a portion of a seed substrate is shortened.
[0047] (11) A semiconductor substrate according to one aspect of the present invention is a semiconductor substrate including a semiconductor layer formed by a vapor phase synthesis method, the semiconductor substrate including a first main surface and a second main surface, the first main surface including a first element different in type or bonding state from a main element constituting the semiconductor substrate, the first element including at least one element selected from the group consisting of hydrogen, oxygen, nitrogen, carbon, helium, neon and argon, and the surface roughness of the first main surface being less than 10 μm. The semiconductor substrate has a flat surface and can be easily processed for various applications. Here, the main element constituting the semiconductor substrate means an element constituting the semiconductor lattice of the semiconductor substrate and contained at 1 atm% or more in atomic ratio. Here, the different bonding state means the following. In the case of carbon, sp 3 Bonds and sp 2 The bond is a different bond state, and when a metal is bonded to nitrogen, the bond state with oxygen or the metal bond state is a different bond state. The elements constituting the semiconductor lattice of the semiconductor substrate are bonded to other elements constituting the semiconductor lattice. In the first main surface, the elements constituting the semiconductor lattice of the semiconductor substrate may exist in a bond state different from the bond state in the semiconductor lattice, such as when they are not bonded to other elements constituting the semiconductor lattice, or when they are bonded to elements different from the elements constituting the semiconductor lattice. The type of element can be analyzed by secondary ion mass spectrometry (SIMS), X-ray photoelectron spectroscopy (XPS), Auger electron spectroscopy (AES), energy dispersive X-ray spectroscopy (EDX), electron beam microanalysis (EPMA), etc. The elements and bond states can be analyzed by X-ray photoelectron spectroscopy (XPS), Auger electron spectroscopy (AES), etc. The bond states of the elements can be analyzed by X-ray photoelectron spectroscopy (XPS), Auger electron spectroscopy (AES), etc.
[0048] (12) The first element may be present on the first main surface to form a plurality of substantially circular patterns. This includes a case where the first element is present on the first main surface to form a plurality of substantially circular depressions, thereby forming the substantially circular pattern. The pattern formed by the elements may be subjected to mapping analysis using X-ray photoelectron spectroscopy (XPS), Auger electron spectroscopy (AES), or the like.
[0049] (13) A method for manufacturing a composite semiconductor substrate according to one embodiment of the present invention includes the steps of: preparing a seed substrate containing a semiconductor material; implanting ions into the seed substrate to form an ion-implanted layer at a certain depth from a surface of a main surface of the seed substrate; growing a semiconductor layer on the main surface of the seed substrate by a vapor phase synthesis method; bonding a first substrate onto the semiconductor layer; and separating a composite semiconductor substrate including the first substrate, the semiconductor layer, and a part of the seed substrate by irradiating light from a surface of a main surface of at least one of the first substrate and the seed substrate.
[0050] According to the above aspect, the seed substrate can be thinly sliced in a short time. Furthermore, even if the seed substrate is thin or the size of the seed substrate is large, the seed substrate can be thinly sliced. Furthermore, a composite semiconductor substrate with a flat slice surface can be obtained.
[0051] (14) A method for manufacturing a composite semiconductor substrate according to one embodiment of the present invention includes the steps of: preparing a seed substrate containing a semiconductor material; implanting ions into the seed substrate to form an ion-implanted layer at a certain depth from a surface of a main surface of the seed substrate; bonding a first substrate onto the main surface of the seed substrate; and separating a composite semiconductor substrate including the first substrate and a part of the seed substrate by irradiating light from a surface of a main surface of at least one of the first substrate and the seed substrate.
[0052] According to the above aspect, the seed substrate can be thinly sliced in a short time. Furthermore, even if the seed substrate is thin or the size of the seed substrate is large, the seed substrate can be thinly sliced. Furthermore, a composite semiconductor substrate with a flat slice surface can be obtained.
[0053] (15) A compound semiconductor substrate according to one aspect of the present invention is a compound semiconductor substrate obtained by the compound semiconductor substrate manufacturing method according to the above (13) or (14). The compound semiconductor substrate can be produced at reduced costs because the time required for separation from a portion of a seed substrate is shortened.
[0054] (16) A composite semiconductor substrate according to one embodiment of the present invention is a composite semiconductor substrate including a first substrate and a semiconductor layer laminated on a main surface of the first substrate, the main surface of the composite semiconductor substrate on the semiconductor layer side includes a first element different in type or bonding state from the main element constituting the semiconductor layer, the first element includes at least one element selected from the group consisting of hydrogen, oxygen, nitrogen, carbon, helium, neon and argon, the main surface of the composite semiconductor substrate on the semiconductor layer side has a surface roughness of less than 10 μm, and the semiconductor layer has a thickness of 0.1 μm or more and 50 μm or less. The composite semiconductor substrate has a flat surface and is easily processed for various applications. Here, the main element constituting the semiconductor layer means an element constituting the semiconductor lattice of the semiconductor layer and contained at 1 atm% or more in atomic ratio. Here, the different bonding state means the following. In the case of carbon, sp 3 Bonds and sp 2The bond is a different bond state, and when a metal is bonded to nitrogen, the bond state with oxygen or the metal bond state is a different bond state. The elements constituting the semiconductor lattice of the semiconductor layer are bonded to other elements constituting the semiconductor lattice. In the first main surface, the elements constituting the semiconductor lattice of the semiconductor layer may exist in a bond state different from the bond state in the semiconductor lattice, such as when they are not bonded to other elements constituting the semiconductor lattice, or when they are bonded to elements different from the elements constituting the semiconductor lattice. The types of elements can be analyzed by secondary ion mass spectrometry (SIMS), X-ray photoelectron spectroscopy (XPS), Auger electron spectroscopy (AES), energy dispersive X-ray spectroscopy (EDX), electron beam microanalysis (EPMA), etc. The bond state of the elements can be analyzed by X-ray photoelectron spectroscopy (XPS), Auger electron spectroscopy (AES), etc.
[0055] (17) The first element may be present on the principal surface on the semiconductor layer side so as to form a pattern of a plurality of substantially circular shapes. The pattern formed by the elements may be subjected to mapping analysis by X-ray photoelectron spectroscopy (XPS), Auger electron spectroscopy (AES), or the like.
[0056] (18) A semiconductor junction wafer according to one embodiment of the present invention includes a seed substrate containing a semiconductor material and a semiconductor layer disposed on a primary surface of the seed substrate, the seed substrate having an ion-implanted layer containing a first element different in type or bonding state from a main element constituting the semiconductor material, the first element containing at least one element selected from the group consisting of hydrogen, oxygen, nitrogen, carbon, helium, neon and argon. Here, the main element constituting the semiconductor material means an element constituting the semiconductor lattice of the semiconductor material and contained at 1 atm% or more in atomic ratio. Here, the different bonding state means the following. In the case of carbon, sp 3 Bonds and sp 2Bonds are different bonding states, and when a metal is bonded to nitrogen, it is different from bonding to oxygen or metallic bonding. The elements that make up the semiconductor lattice of the semiconductor material are bonded to other elements that make up the semiconductor lattice. In the ion implantation layer, elements that make up the semiconductor lattice of the semiconductor material may exist in a bonding state different from the bonding state in the semiconductor lattice, such as when they are not bonded to other elements that make up the semiconductor lattice, or when they are bonded to elements different from the elements that make up the semiconductor lattice. The types of elements can be analyzed by secondary ion mass spectrometry (SIMS), X-ray photoelectron spectroscopy (XPS), Auger electron spectroscopy (AES), energy dispersive X-ray spectroscopy (EDX), electron beam microanalysis (EPMA), etc. The bonding state of elements can be analyzed by X-ray photoelectron spectroscopy (XPS), Auger electron spectroscopy (AES), etc.
[0057] [Details of the embodiment of the present invention] Specific examples of a semiconductor substrate and a method for manufacturing a semiconductor substrate according to an embodiment of the present invention will be described below with reference to the drawings. Note that the present invention is not limited to these examples, but is defined by the claims, and is intended to include all modifications within the meaning and scope of the claims.
[0058] [Embodiment 1] <Method of manufacturing semiconductor substrate> Figures 1(A) to 1(E) are diagrams that typically show a method for manufacturing a semiconductor substrate according to an embodiment of the present invention, and Figure 2 is a flow chart showing the method for manufacturing a semiconductor substrate according to an embodiment of the present invention.
[0059] A method for manufacturing a semiconductor substrate according to an embodiment of the present invention includes the steps of preparing a seed substrate containing a semiconductor material (shown in FIG. 1(A) and FIG. 2 as a substrate preparation step (S1)); forming an ion-implanted layer at a certain depth from a surface of a main surface of the seed substrate by implanting ions into the seed substrate (shown in FIG. 1(B) and FIG. 2 as an ion-implanted layer formation step (S2)); growing a semiconductor layer on the main surface of the seed substrate by a vapor phase synthesis method (shown in FIG. 1(C) and FIG. 2 as a semiconductor layer growth step (S3)); and separating a semiconductor substrate containing the semiconductor layer and a part of the seed substrate by irradiating light from the surface of at least one of the main surfaces of the semiconductor layer and the seed substrate (shown in FIG. 1(D-1), (D-2), (E) and FIG. 2 as a semiconductor separation step (S4)).
[0060] (Step of Preparing Seed Substrate) First, with reference to FIG. 1(A), a seed substrate 1 including a semiconductor material is prepared.
[0061] The seed substrate 1 may be a single crystal semiconductor substrate or a polycrystalline semiconductor substrate. Generally, single crystal materials are more expensive, and from the viewpoint of exerting the effects of the embodiment of the present invention to a greater extent, a single crystal semiconductor substrate is preferable. Note that semiconductor devices are often single crystal.
[0062] The semiconductor material contained in the seed substrate 1 may be a wide band gap semiconductor such as diamond, aluminum nitride, aluminum oxide, magnesium oxide, gallium nitride, gallium oxide, silicon carbide, zinc selenide, zinc sulfide, or a semiconductor such as gallium arsenide, indium phosphide, silicon, etc. These semiconductor materials can be suitably used in various semiconductor devices.
[0063] The seed substrate 1 preferably has high crystallinity. The seed substrate 1 has high crystallinity, so that the semiconductor layer 3 formed on the seed substrate 1 can also have high crystallinity. The seed substrate 1 is preferably a method capable of synthesizing a semiconductor with high crystallinity. In the case of diamond, it is preferably a single crystal manufactured by a high-temperature, high-pressure synthesis method. In the case of silicon carbide, it is preferably a sublimation method. In the case of silicon, it is preferably a pulling method. It is preferable that aluminum nitride is produced by the sublimation method, aluminum oxide is produced by the flux method or the pulling method, magnesium oxide is produced by the flux method, gallium nitride is produced by the vapor phase growth method or the flux method, gallium oxide is produced by the melt growth method, zinc selenide is produced by the sublimation method or the chemical transport method using iodine as a transport agent, zinc sulfide is produced by the sublimation method, and gallium arsenide and indium phosphide are produced by the vertical Bridgman method. However, it may be a single crystal semiconductor produced by a vapor phase synthesis method. It may also be a semiconductor substrate obtained by the method for producing a semiconductor substrate according to an embodiment of the present invention and processed.
[0064] In order to efficiently increase the thickness of the semiconductor layer 3 (vertical direction in FIG. 1(C)), it is preferable that the main surface of the seed substrate 1 has a specific plane orientation. For example, for silicon or diamond, it is preferable that it is a (001) plane. For silicon carbide or gallium nitride, it is preferable that it is a c-plane. For zinc selenide or zinc sulfide, it is preferable that it is a (111) plane. In order to further increase the crystal homogeneity of the semiconductor layer 3, it is preferable that the main surface of the seed substrate 1 has an off angle with respect to the specific plane orientation of 0° or more and 15° or less, and more preferably 1.5° or more and 10° or less.
[0065] The thickness of the seed substrate 1 is preferably 10 μm or more and 1000 μm or less, and more preferably 100 μm or more and 800 μm or less, where the thickness of the seed substrate 1 is the thickness measured near the center of the main surface of the seed substrate 1.
[0066] 1, the seed substrate 1 is formed from one type of substrate, but as long as it does not interfere with subsequent processes, the seed substrate 1 may have a structure in which a semiconductor layer containing a seed crystal is bonded (attached) to a non-semiconductor substrate. This can prevent cracks and improve handleability even when the semiconductor layer containing a seed crystal is thin.
[0067] The shape of the main surface of the seed substrate 1 is not particularly limited, and examples thereof include a rectangle, a polygon, a circle (including those with an orientation flat), etc. The main surface of the seed substrate 1 may be a flat surface, or may be a surface having projections and recesses, such as a concave lens shape, a convex lens shape, a rectangle, a trapezoid, or a pyramid shape.
[0068] (Step of forming ion implantation layer) Next, referring to FIG. 1(B), ion implantation (downward arrow in the figure) is performed on the seed substrate 1 to form an ion-implanted layer 2 at a certain depth from the surface of the main surface of the seed substrate 1. In the ion implantation, atoms different from the semiconductor atoms forming the seed substrate are introduced into the seed substrate 1, defects are introduced, and bonds between semiconductor atoms are loosened. In the ion implantation, different atoms and defects penetrate into the inside of the seed substrate 1, so that the surface of the seed substrate 1 maintains the semiconductor crystal structure. Therefore, after the layer is formed by ion implantation, a semiconductor layer can be formed on the seed substrate 1.
[0069] The depth and thickness of the ion-implanted layer 2 from the surface of the substrate can be adjusted mainly by the type of ions used, the implantation energy, and the dose. The design of the ion-implanted layer 2 can be calculated and predicted with almost exact accuracy by a Monte Carlo simulation such as TRIM.
[0070] The implantation energy is preferably 50 keV or more and 10,000 keV or less, and more preferably 80 keV or more and 800 keV or less. The irradiation dose is 1×10 14 pieces / cm 2 More than 2×10 18 pieces / cm 2 Less than or equal to 1×10 is preferred 15 pieces / cm 2 8×10 or more17 pieces / cm 2 The following is even more preferable: When the implantation energy and the dose are within the above-mentioned ranges, the crystallinity of the main surface of the seed substrate 1 is maintained to a degree that enables epitaxial growth by a vapor phase synthesis method, while the crystal structure inside the seed substrate 1 is destroyed, and an ion-implanted layer 2 in which the bonding strength between semiconductor atoms is reduced can be formed.
[0071] When the implantation energy is high, such as 50 keV or more, atomic vacancies are generated in the ion implantation layer 2, weakening the bonding force between the atoms that make up the semiconductor. In the ion implantation layer 2, the parts where the bonding force between the atoms is weak are arranged on the same plane, so when light is irradiated from the outside to make the implanted atoms absorb energy and vaporize and expand, the force is equally applied to the parts of the ion implantation layer 2. Therefore, the separation surface, which is the fracture surface after the ion implantation layer 2 is destroyed, becomes flat. The thinner the ion implantation layer 2 is and the greater the amount of atomic vacancies, the greater the flatness, which is preferable. If the amount of ions in the ion implantation layer 2 is too small, it becomes difficult to obtain a peeling force.
[0072] If the dose is too high, the crystal structure of the semiconductor on the outermost surface may be destroyed, making it impossible to synthesize the semiconductor layer 3 on the surface of the seed substrate 1 after implantation. Even if the semiconductor layer 3 can be synthesized, the ion-implanted layer 2 may be partially lost due to the influence of the atmosphere during synthesis, making separation difficult. If the implantation energy is too high, the ion-implanted layer 2 may become too thick, making it difficult to obtain a flat separation surface. If the dose is too low, it becomes difficult to separate the semiconductor substrate by light irradiation in a later process.
[0073] It is preferable that the ion implantation layer 2 formed in the seed substrate 1 has a different absorption rate of the irradiated light from that of the seed substrate 1. This allows the semiconductor layer to be separated from the part of the seed substrate in a shorter time. Note that even if the light absorption rates of the ion implantation layer 2 and the seed substrate 1 are the same, the semiconductor layer can be separated from the part of the seed substrate. This is because the bonding force of the semiconductor substrate is not directly broken by light, but energy is locally given to the lattice of the semiconductor crystal or the implanted ions, and the energy is transmitted to the implanted atoms or molecules, which expand and act on and break the bonds weakened by the implantation.
[0074] It is preferable that the light transmittance of the ion-implanted layer 2 is 1% or more lower than that of the seed substrate 1, since the irradiated light is efficiently absorbed by the ion-implanted layer 2. It is more preferable that the light transmittance of the ion-implanted layer 2 is 5% or more lower than that of the seed substrate 1, and even more preferable that it is 20% or more lower. Even if the light transmittance of the ion-implanted layer 2 is similar to or higher than that of the seed substrate 1, the semiconductor layer can be separated from a part of the seed substrate in a short time by adjusting the light irradiation conditions. Here, the light transmittance Ta is a value expressed by the following formula (1) taking multiple internal reflections into consideration. Ta=I t / I0 expression (1) Furthermore, the reflectance Ra taking into account multiple reflections and the single reflection R are expressed by the following equations (2) and (3), respectively. Ra=I r / I0 expression (2) R = (n0-n f ) 2 / (n0+n f ) 2 Formula (3) (In equation (1), I0 is the intensity of the incident light, I t is the intensity of the emitted light after passing through the medium, I r is the intensity of reflected light after inserting a medium, n0 is the refractive index of air, n f indicates the refractive index of diamond.) However, if the energy of the irradiated light is greater than the band gap of the semiconductor, no such difference occurs. The absorption by the semiconductor itself is large, so this difference is so small that it cannot be detected. Also, when irradiating the ion-implanted layer with light, the light must pass through the semiconductor substrate to reach the ion-implanted layer, and in this case, it is better if the light is not absorbed in the semiconductor substrate. Therefore, in this embodiment, it is common and effective to use light with an energy smaller than the band gap of the semiconductor.
[0075] The light transmittance can be measured by a normal spectrophotometer. The transmittance of the ion-implanted layer 2 is a value compared to the highly light-transmitting seed substrate 1, and is measured as a value including the reflectance without subtracting the reflectance. Therefore, even if the light transmittance is 100%, the reflectance is equal to or greater than the value calculated by the refractive index of the semiconductor, so the transmittance does not exceed the transmittance obtained by subtracting the reflectance. Since the thickness of the ion-implanted layer is very thin, even if the change in light transmittance is 1%, it makes a large difference in the absorption coefficient and has a great effect. However, in the present invention, there are cases where the ion-implanted layer is too thin or does not create a clear absorption level, and is hardly reflected in the transmittance within the range of the present invention. In the present invention, even in such cases, the effect is exerted as long as the atomic bonds in the crystal are cut by ions.
[0076] At the wavelength of irradiation light used in the subsequent step of separating semiconductor substrate 3, the absorption coefficient of ion-implanted layer 2 is preferably at least 5 times, and more preferably at least 30 times, larger than the absorption coefficient of seed substrate 1. Here, the optical absorption coefficient is a value expressed by the following formula (4) taking multiple internal reflections into consideration. μ=(log e ((I t / I0) / ((I r / I0) / R-1))) / x Formula (4) (In equation (4), μ is the average optical absorption coefficient, I0 is the intensity of the incident light, and I t is the intensity of the emitted light after passing through the medium, I r is the intensity of reflected light after the medium is inserted, R is the single reflection R expressed by formula (3), and x is the thickness of the medium (the effective thickness of the ion-implanted layer 2). When a light source containing a mixed wavelength is used as the light source, the light transmittance and absorption coefficient refer to the light transmittance and absorption coefficient of the wavelength that shows the maximum absorption energy among the wavelengths and wavelength range contained in the light source.
[0077] If the relationship between the light transmittance or light absorption coefficient between the seed substrate 1 and the ion-implanted layer 2 is within the above range, when the seed substrate 1 is irradiated with light, the light passes through the seed substrate 1 and is efficiently absorbed by the ion-implanted layer 2. Therefore, the time required for the destruction of the ion-implanted layer 2 can be shortened. However, if the light transmittance of the ion-implanted layer 2 increases, the efficiency of absorbing the energy of light increases, which is convenient for shortening the time for the ion-implanted layer 2, but is not essential. This is because the main purpose of the ion implantation is to weaken the atomic bonding force described below. In that case, it is sufficient to make the crystal lattice or ions absorb the light nonlinearly. In this case, it is important to expand the implanted atoms and use their force to cut the weak bonds without directly cutting the bonds of the crystal lattice. Therefore, there is no problem even if the light transmittance is reduced by thermal annealing after the ion implantation before the process of separating with light. There is also no problem even if a wavelength of light different from the wavelength of light with absorption is used. This is because the energy is indirectly transmitted to the implanted ions, and the implanted ions eventually expand and become the energy for separation.
[0078] The type of ions to be implanted may be ions of an element capable of reducing the crystallinity of the ion-implanted layer 2. For example, ions of all elements that can be ion-implanted, such as carbon, boron, nitrogen, oxygen, phosphorus, neon, hydrogen, helium, aluminum, silicon, sulfur, and argon, can be used. Among them, it is preferable to use at least one type of ion selected from the group consisting of hydrogen ions, hydrogen molecular ions, oxygen ions, oxygen molecular ions, nitrogen ions, nitrogen molecular ions, helium ions, neon ions, and argon ions. These ions are easily gasified by the energy of light. Therefore, if the ion-implanted layer contains these ions, when light is absorbed in the ion-implanted layer 2 or in its vicinity, these ions gasify and expand, facilitating the destruction of the ion-implanted layer having weak interatomic bonds.
[0079] Furthermore, it is more preferable that these ions are inert gas ions that do not bond with the semiconductor, or hydrogen ions that, even if they do bond, are not incorporated into the matrix and serve as termination ions, because this facilitates the separation of the semiconductor.
[0080] When boron, nitrogen, silicon, and phosphorus form 4-coordinate bonds with atoms in the semiconductor, it is not efficient because it requires the same amount of energy as breaking the bonds of the semiconductor atoms. On the other hand, agglomerated nitrogen that is not 4-coordinated is easy to gasify and is effective. Whether or not it has been substituted with an atom in the matrix can be calculated by comparing the amount of ESR (Electron Spin Resonance) detected in the substitutional form with the total amount of nitrogen measured by SIMS (Secondary Ion Mass Spectrometry).
[0081] The depth of the ion-implanted layer 2 from the main surface of the seed substrate 1 is preferably 0.05 μm to 10 μm, more preferably 0.1 μm to 1 μm. This makes the thickness of the layer destroyed by the irradiated light sufficiently small, and also makes it possible to prevent separation failure. Here, the main surface of the seed substrate 1 refers to the surface where the ions are implanted. The depth from the main surface of the seed substrate 1 refers to the distance between the main surface of the seed substrate 1 and the center of the ion-implanted layer 2 closest to the main surface of the seed substrate 1 (the position where the implanted ion concentration is the highest).
[0082] The thickness of the ion-implanted layer 2 is preferably 50 nm to 10 μm, more preferably 100 nm to 1 μm, so that the thickness of the layer destroyed by the irradiated light (the layer necessary for separation) is sufficiently small and sufficient flatness of the separation surface can be ensured.
[0083] The ion-implanted layer 2 has an ion dose of 1×10 14 cm -2 More than 2×10 18 cm -2 The range is preferably 1×10 15 cm -2 8×10 or more 17 cm -2 The following range is more preferable. When the ion dose is within the above range, a sufficient amount of atomic vacancies are formed in the ion-implanted layer 2. Since no atoms exist at the positions of the atomic vacancies, the bonding force of the surrounding atoms is weakened. Therefore, when the ion-implanted layer 2 or its vicinity absorbs light, the ion-implanted layer is destroyed with the atomic vacancies as the base point. The ion dose is a value calculated from the ion current density calculated from the ion current and irradiation area during implantation and the implantation time, and it can be confirmed by secondary ion mass spectrometry (SIMS) that the implantation has been performed as designed.
[0084] The thickness and dose of the ion implantation layer are designed according to the intensity of the irradiated light (laser). In other words, if the intensity of the focused light (laser) is high, the ions can be separated even if the amount of ions implanted is small, and if the intensity of the focused light (laser) is low, the amount of ions implanted is designed to be large. It is necessary to adjust the amount of ions implanted so that the crystals on the top surface of the semiconductor being implanted do not collapse.
[0085] The ion implantation layer 2 preferably has an atomic vacancy density in the range of 0.001% to 100% at the maximum peak value, more preferably 0.01% to 100%. When the atomic vacancy density is in the above range, the destruction of the ion implantation layer 2 can be promoted. When the atomic vacancy density in the maximum peak value is less than 0.001%, the starting point of destruction of the ion implantation layer 2 is small, so the power and time required to destroy the ion implantation layer 2 increase. In such a case, even a semiconductor with high crystallinity is damaged. The atomic vacancy density is a value measured by visible or near-infrared transmittance. It can be calculated by the atomic density obtained by ion implantation simulation and a calibration curve of the measured transmittance. The atomic density is expressed as a percentage of the ideal carbon atom density at room temperature. Therefore, the atomic vacancy density can be determined without measurement once the ion implantation conditions are determined.
[0086] The ion-implanted layer 2 may be a collection of atomic vacancies or may contain an amorphous phase. It is preferable that the amorphous phase contains many dangling bonds. In this case, when the ion-implanted layer 2 or its vicinity absorbs light, the dangling bonds of the amorphous phase become the starting point and destroy the ion-implanted layer 2. On the other hand, the amorphous phase layer is formed up to the outermost surface of the seed substrate 1, so separation does not go well. This is because it becomes difficult for the semiconductor layer 3 to grow epitaxially on the upper surface of the seed substrate 1 into which the ions are implanted. Therefore, there is an upper limit to the amount of ion implantation.
[0087] (Step of growing semiconductor layer) 1(C), a semiconductor layer 3 is grown by vapor phase synthesis on the main surface of the seed substrate 1. The semiconductor layer 3 is more preferably a heteroepitaxially grown layer or a homoepitaxially grown layer.
[0088] First, an example of a growth method in which the semiconductor layer is diamond will be described. The vapor phase synthesis method is not particularly limited, and PVD, CVD, MOCVD, VPE, molecular beam epitaxy, sublimation, etc. can be used. Specifically, for example, in a microwave plasma CVD synthesis method of diamond, a seed substrate 1 is placed in a vacuum chamber, the pressure in the vacuum chamber is set to 2.66 kPa to 53.2 kPa, and the substrate temperature in the chamber is heated to 800°C to 1200°C. Then, a hydrocarbon gas such as methane, hydrogen gas, and an additive gas such as an inert gas or nitrogen are introduced to epitaxially grow a semiconductor layer 3 made of diamond on the main surface of the seed substrate 1. The additive gas is added as necessary, but may not be added. The growth direction of the semiconductor layer 3 is the upward direction in FIG. 1(C). The upper surface of the semiconductor layer 3 inherits the surface orientation of the main surface of the seed substrate 1.
[0089] Next, an example of a synthesis method in which the semiconductor layer is made of gallium nitride, aluminum nitride, or zinc selenide will be described.
[0090] In a method for growing gallium nitride by MOCVD, a seed substrate 1 (typically a substrate having a C-plane of the (0001) plane as a main surface) is placed in a furnace, the substrate temperature in the furnace is heated to 600°C to 1300°C, and then an organic gallium gas such as trimethylgallium, ammonia gas, and a carrier gas such as hydrogen are introduced to epitaxially grow a semiconductor layer 3 made of gallium nitride on the main surface of the seed substrate 1. The mixture ratio of trimethylgallium gas and ammonia gas in the source gas is preferably 1:2000 by volume. The growth direction of the semiconductor layer 3 is the upward direction in FIG. 1(C). The upper surface of the semiconductor layer 3 inherits the surface orientation of the main surface of the seed substrate 1. The vapor phase synthesis method is not limited to the above-mentioned MOCVD method, and other commonly known vapor phase synthesis methods can also be used.
[0091] In the method of growing aluminum nitride by sublimation, a seed substrate 1 (a substrate having a (0001) or (0002) plane) is placed in a furnace, the substrate temperature in the furnace is maintained at 2000°C, and an aluminum nitride raw material is sublimated at 2400°C to epitaxially grow a semiconductor layer 3 made of aluminum nitride on the main surface of the seed substrate 1. The growth direction of the semiconductor layer 3 is the upward direction in FIG. 1(C). The upper surface of the semiconductor layer 3 inherits the plane orientation of the main surface of the seed substrate 1. The vapor phase synthesis method is not limited to the sublimation method described above, and other commonly known vapor phase synthesis methods can also be used.
[0092] In the method of synthesizing zinc selenide by the sublimation method, a seed substrate 1 is placed in a furnace, the substrate temperature in the furnace is kept at 1000 to 1200°C, and the raw materials selenium and zinc are introduced into the device from polycrystalline zinc selenide, which is placed at a higher temperature, using an inert gas as a carrier gas, to epitaxially grow a semiconductor layer 3 made of zinc selenide on the main surface of the seed substrate 1. The growth direction of the semiconductor layer 3 is the upward direction in FIG. 1(C). The upper surface of the semiconductor layer 3 inherits the surface orientation of the main surface of the seed substrate 1. The vapor phase synthesis method is not limited to the sublimation method described above, and other commonly known vapor phase synthesis methods can also be used.
[0093] Next, an example of a synthesis method in which the semiconductor layer is silicon carbide will be described. A seed substrate 1 (typically, the (0001) plane is used as the main surface, but is off by 0.05 to 10°) is placed in a furnace, and the substrate temperature in the furnace is heated to 1400°C to 1600°C by high frequency, and then a silicon hydrogen gas such as monosilane gas, a hydrocarbon gas such as propane gas, and a carrier gas such as hydrogen are introduced to epitaxially grow a semiconductor layer 3 made of silicon carbide on the main surface of the seed substrate 1. The furnace is an atmospheric pressure horizontal cold wall CVD apparatus or the like. The mixture ratio of silicon and carbon gases in the raw material gas is preferably 1.5:1 or the like. The growth direction of the semiconductor layer 3 is the upward direction in FIG. 1(C). The upper surface of the semiconductor layer 3 inherits the surface orientation of the main surface of the seed substrate 1. The vapor phase synthesis method is not limited to the above method, and other commonly known vapor phase synthesis methods can also be used.
[0094] Regarding the relationship between the light transmittance of the semiconductor layer 3 and the ion-implanted layer 2, the light transmittance of the ion-implanted layer 2 is preferably 1% or more lower, and more preferably 5% or more lower, than the light transmittance of the semiconductor layer 3. Here, the light transmittance is a value represented by the above formula (1).
[0095] Regarding the relationship between the light absorption coefficients of the semiconductor layer 3 and the ion-implanted layer 2 at the wavelength of the irradiated light, the absorption coefficient of the ion-implanted layer 2 is preferably 5 times or more, and more preferably 30 times or more, larger than the absorption coefficient of the semiconductor layer 3. Here, the light absorption coefficient is a value represented by the above formula (4).
[0096] When the relationship between the light transmittance or light absorption coefficient of the ion-implanted layer 2 and the semiconductor layer 3 is within the above-mentioned range, when the semiconductor layer 3 is irradiated with light, the light passes through the irradiated semiconductor layer 3 and is efficiently absorbed by the ion-implanted layer 2. Therefore, the time required for the ion-implanted layer 2 to be destroyed can be shortened.
[0097] In order to make the semiconductor layer 3 more light-transmitting than the ion-implanted layer 2, it is effective to synthesize the semiconductor layer 3 under conditions that favor crystallinity. The light-transmittance of the ion-implanted layer 2 is reduced due to point defects resulting from atomic vacancies generated by the implantation. The order of the crystal lattice of the top surface of the ion-implanted seed substrate 1 is maintained much better than that of the ion-implanted layer 2, and most of the point defects are not carried over to the semiconductor layer 3 grown later. Therefore, the semiconductor layer 3 has higher crystallinity than the ion-implanted layer 2.
[0098] The semiconductor layer 3 may be single crystal or polycrystalline. Single crystal semiconductors are expensive and are preferable because they can more effectively reduce manufacturing costs. The semiconductor layer 3 may be conductive or insulating. The semiconductor layer 3 is preferably insulating, but may be a doped substrate in which doping atoms are ion-implanted. However, when metallic doping is performed, the light may not reach the ion-implanted layer 2 when irradiated from the semiconductor layer 3 side. Therefore, when metallic doping is performed, the light is irradiated from the main surface side of the seed substrate 1 on which the semiconductor layer is not formed, so that the light reaches the ion-implanted layer 2.
[0099] In this specification, a stacked body including a seed substrate 1 having an ion-implanted layer 2 and a semiconductor layer 3 disposed on a main surface of the seed substrate 1, as shown in Fig. 1(C), is also referred to as a "semiconductor junction substrate." A semiconductor substrate can be produced by using the semiconductor junction substrate shown in Fig. 1(C) through a separation process described below.
[0100] (Step of separating the semiconductor layer from the substrate) 1(D-1) and 1(D-2), light 4 is irradiated onto the surface of at least one of the principal surfaces of the semiconductor layer 3 and the seed substrate 1. Then, referring to Fig. 1(E), the light 4 is absorbed by the ion-implanted layer 2 or its vicinity, and the ions present in the ion-implanted layer are vaporized and expanded by the energy of the light, and the portion of the ion-implanted layer where the bonds between the semiconductors are weak are pushed out by the expansion pressure, and the semiconductor substrate 5 including the semiconductor layer 3 and a portion of the seed substrate (seed substrate 1a) is separated from the majority of the seed substrate (seed substrate 1b).
[0101] Since the ion implantation layer 2 is formed by implanting ions, it contains at least one of ions, atomic vacancies, amorphous parts, and dangling bonds of semiconductor atoms constituting the matrix. When the ion implantation layer 2 or its vicinity absorbs light 4, the temperature of the ion implantation layer 2 rises, and ion atoms present in the ion implantation layer or atoms not bonded to atoms of the semiconductor lattice vaporize and expand, and the ion implantation layer 2 is destroyed from atomic vacancies and dangling bonds, which are weak interatomic bonds in the ion implantation layer 2, as base points. At this time, it can be pushed out without affecting the semiconductor layer 3. The ion implantation layer 2 is formed by forming the surface of the seed substrate 1 into which ions are implanted into a smooth or flat surface in advance, and implanting ions through that surface, so that the interface between the ion implantation layer 2 and the seed substrate 1 has little unevenness. Therefore, the separation surface between the semiconductor substrate 5 and the seed substrate 1b after the ion implantation layer 2 or its vicinity is destroyed by absorbing light has a small surface roughness. The roughness of the separation surface is approximately the same as the thickness of the ion-implanted layer, and can be made smaller than 10 μm, or even smaller than 1 μm.
[0102] It is preferable that the light 4 is focused on the ion-implanted layer 2 and the focused point is scanned. The light 4 may be focused on the ion-implanted layer 2, or may be slightly shifted from the ion-implanted layer 2. The ion-implanted layer 2 may be a layer that easily absorbs light and absorbs energy, or the vicinity of the ion-implanted layer 2 may absorb energy and transmit it to the implanted ions. Therefore, the light can function regardless of the slight shift in the focusing distance.
[0103] The light 4 may be irradiated from the main surface side of the semiconductor layer 3 as shown in Fig. 1 (D-1). Alternatively, the light may be irradiated from the main surface side of the seed substrate 1 on which the semiconductor layer 3 is not formed as shown in Fig. 1 (D-2). The top surface to be irradiated may be a somewhat rough surface. This is because, in the same principle as that of being able to extract internal information even if the surface of a compact disc (CD) is cloudy, even if the top surface to be irradiated is somewhat rough, the light can be successfully absorbed by the ion-implanted layer or its vicinity.
[0104] As the light source of the light to be irradiated, a pulsed laser, a CW laser (Continuous Wave Laser), a flash lamp, a pulsed lamp, etc. can be used. Among them, when a light source that emits pulsed light such as a pulsed laser, a flash lamp, or a pulsed lamp is used, the light irradiation can be stopped before the temperature of the entire semiconductor increases, and the light irradiation can be resumed after the semiconductor cools down, so that the temperature of only the ion-implanted layer can be increased, which is preferable. Here, the pulsed lamp means a lamp that is a continuous irradiation type lamp, but which is substantially irradiated in a pulsed manner by a physical shielding plate that blocks the light or changes the path of the light.
[0105] When pulsed light is used as the light source, the irradiation fluence per pulse on the main surface of at least one of the semiconductor layer 3 and the seed substrate 1 to which the light is irradiated is 0.01 J / mm 2 More than 1500J / mm 2 It is preferable that the value is less than 0.1 J / mm 2 More than 500J / mm 2 It is more preferable that the irradiation fluence per pulse of the pulsed light is 0.01 J / mm or less. This allows the light to raise the temperature of only the ion-implanted layer without raising the temperature of the semiconductor layer and the substrate. Therefore, only the ion-implanted layer can be destroyed without destroying the surfaces of the principal faces of the semiconductor layer and the seed substrate, and without causing cracks inside the seed substrate and the semiconductor layer. 2 If the irradiation fluence per pulse of the pulsed light is less than 1500 J / mm, the number of pulses required to destroy the ion-implanted layer may increase, or the pulsed light may not be able to destroy the ion-implanted layer. 2 If the temperature exceeds this range, the crystal structure of the seed substrate or the surface or inside of the semiconductor layer may be damaged.
[0106] The pulse width of the pulsed light is preferably 0.01 psec to 10 msec. Furthermore, 0.01 nsec to 10 msec is more preferable, and 0.1 nsec to 1 msec is even more preferable. If the pulse width is smaller than 0.01 nsec, the energy of the pulsed light reaches an energy level that breaks the bonds of the atoms of the semiconductor, which may cause the surfaces of the semiconductor layer and the main surface of the seed substrate to become rough or crack. Furthermore, if the pulse width is less than 0.01 nsec, it is difficult to control the pulse width with a light irradiation device. On the other hand, if the pulse width exceeds 10 msec, it affects not only the ion-implanted layer but also the entire temperature rise including the seed substrate and the semiconductor. However, since the increase in the entire temperature also depends on the irradiation fluence, it is necessary to increase the irradiation fluence to 0.01 J / mm. 2 If it is less than this, up to 100 msec is permitted.
[0107] The pulse interval of the pulsed light is preferably 0.1 nsec to 100 msec. That is, the lower limit is 0.1 nsec or more, preferably 10 nsec or more, more preferably 1 μsec or more, and even more preferably 10 μsec or more, and the upper limit is 100 msec or less, preferably 10 msec or less, and even more preferably 1 msec or less. (The lower limit of the repetition frequency is preferably 1 Hz or more, more preferably 10 Hz or more, even more preferably 100 Hz or more, and even more preferably 1 kHz or more. The upper limit is preferably 1000 MHz or less, more preferably 1000 kHz or less, and even more preferably 100 kHz or less.) The ratio of the pulse width to the pulse interval is the interval / width ratio of 10 to 10 9 is preferable. 6 It is more preferable that the number is 10 to 1,000.
[0108] The pulsed light preferably has a pulse energy of 0.05 mJ or more and 1000 mJ or less on the surface of the principal surface of at least one of the semiconductor layer 3 and the seed substrate 1 to which the light is irradiated. This allows the light to destroy only the ion-implanted layer 2 without destroying the principal surfaces of the semiconductor layer 3 and the seed substrate 1, and without causing cracks inside the seed substrate 1 and the semiconductor layer 3. If the pulse energy is less than 0.05 mJ, the irradiated light cannot destroy the ion-implanted layer. On the other hand, if the pulse energy exceeds 1000 mJ, the irradiated light may destroy the semiconductor layers and the substrate other than the ion-implanted layer. The pulse energy is more preferably 0.1 mJ or more and 50 mJ or less, and even more preferably 0.3 mJ or more and 30 mJ or less.
[0109] The light to be irradiated is preferably laser light. When laser light is used, in addition to making it easy to vary the pulse width and intensity, it is possible to obtain the effect of being able to select a wavelength suitable for absorption. As the laser, a solid laser, a liquid laser, a gas laser, or the like can be used according to the absorption wavelength of the ion-implanted layer. Specifically, a glass laser, a YAG laser (YAG: Yttrium Aluminum Garnet), a YLF laser (YLF: Yttrium Lithium Fluoride), a CO2 laser, an excimer laser, a Yb-doped fiber laser, or the like can be used. In addition, the wavelengths of these double waves, triple waves, or the like may be obtained by SHG (Second Harmonic Generation) or the like and used.
[0110] The wavelength of the laser light can be appropriately selected within the range of 250 nm to 10.6 μm according to the absorption wavelength of the ion-implanted layer 2. For example, 250 nm to 400 nm is preferable, and 450 nm to 550 nm is more preferable. Furthermore, 1 μm to 2 μm is even more preferable. In other words, a longer wavelength of the laser light is preferable because it increases the proportion of implanted ions that are thermally gasified to generate expansion energy, rather than the proportion of semiconductor atomic bonds that form the matrix are broken by multilattice absorption.
[0111] The laser light is preferably scanned over the surface of the semiconductor layer 3 or the main surface of the seed substrate 1. The scanning speed is determined by the pulse interval (frequency) and the size of the light (laser beam size). The scanning speed is preferably at least twice the pulse frequency x beam size and not more than 30 times the pulse frequency x beam size, and more preferably between 5 and 20 times. This allows the surface to be processed more flatly, and separation can be performed efficiently and without waste in a short time.
[0112] The step of separating the semiconductor substrate 5 and the seed substrate 1b is preferably carried out in a liquid. This can reduce the impact of light irradiation on the semiconductor substrate 5 and the seed substrate 1b, thereby suppressing the occurrence of cracks in the seed substrates 1a, 1b and the semiconductor layer 3. The liquid is not particularly limited as long as it can reduce the impact of the laser light, and for example, pure water, various aqueous solutions, various oils, or soft solids such as solid gels can be used.
[0113] The step of separating the semiconductor substrate 5 from the seed substrate 1b is preferably performed while cooling the ambient temperature. This can reduce thermal expansion of the seed substrates 1a, 1b and the semiconductor layer 3 due to the irradiated light, and can suppress the occurrence of cracks in the seed substrates 1a, 1b and the semiconductor layer 3. Cooling can be performed, for example, by introducing a refrigerant atmosphere or by using cooled liquids such as pure water, various aqueous solutions, and various oils, or solid gels.
[0114] As shown in FIG. 1(E), the surface roughness of the separated seed substrate 1b and the separated surface of the semiconductor substrate 5 is small. When the semiconductor substrate 5 including the seed substrate 1a and the semiconductor layer 3 is used as a substrate for devices or other applied products, it may be necessary to flatten the surface. Since the surface roughness of the separated surface of the seed substrate 1a included in the semiconductor substrate 5 is small, it can be easily processed into applied products such as substrates for devices. In addition, in order to use the separated seed substrate 1b again as a substrate for epitaxial growth, it is necessary to flatten the surface. Since the surface roughness of the separated surface of the seed substrate 1b is small, it can be easily processed into a seed substrate. Ultimately, laser separation after ion implantation and CVD epi can be performed through the same process without reprocessing the substrate.
[0115] The surface roughness (Ra) of the separated surface of the separated seed substrate 1b and the semiconductor substrate 5 is preferably less than 10 μm, more preferably 1 μm or less, and even more preferably less than 0.3 μm. This facilitates processing to flatten the surface. Here, the surface roughness (Ra) means the arithmetic mean roughness according to the provisions of JIS B 0601-2013, and refers to the value in micrometers (μm) obtained by extracting only a reference length from a roughness curve in the direction of the mean line, taking the X-axis in the direction of the mean line of this extracted portion and the Y-axis in the direction of the longitudinal magnification, and expressing the roughness curve as y=f(x) using the following formula (5).
[0116]
number
[0117] The separated seed substrate 1b can be planarized by ordinary mechanical polishing, and Ra can be set to 0.1 nm. If ions are implanted into the surface of the seed substrate 1 to form an ion-implanted layer 2 and then the ion-implanted layer 2 is destroyed by irradiation with light, the planarity of the separated surface decreases. However, the planarity of the separated surface can be improved by reducing the thickness of the ion-implanted layer 2, slowing down the scanning speed of light, using low power, or other measures.
[0118] [Embodiment 2] The semiconductor substrate according to the embodiment of the present invention is a semiconductor substrate 5 obtained by the semiconductor substrate manufacturing method of the embodiment 1. The semiconductor substrate 5 is separated from the seed substrate 1b in a short time, and therefore the manufacturing cost is reduced.
[0119] A semiconductor substrate according to an embodiment of the present invention is a semiconductor substrate 5 including a semiconductor layer 3 formed by a vapor phase synthesis method, the semiconductor substrate 5 including a first main surface and a second main surface, the first main surface including a first element different in type or bonding state from a main element constituting the semiconductor substrate, the first element including at least one element selected from the group consisting of hydrogen, oxygen, nitrogen, carbon, helium, neon and argon, and the surface roughness of the first main surface being less than 10 μm. The semiconductor substrate has a flat surface and is easily processed for various applications. The surface roughness of the first main surface is preferably 1 μm or less, more preferably less than 0.3 μm. The semiconductor substrate of this embodiment can be manufactured by the semiconductor substrate manufacturing method of the first embodiment. In this case, in the semiconductor substrate of this embodiment, the surface of the first main surface corresponds to the surface of the seed substrate 1a. Moreover, the at least one element selected from the group consisting of hydrogen, oxygen, nitrogen, carbon, helium, neon and argon, which is the first element included in the first main surface, is derived from ions implanted by ion implantation. Most of the ions implanted by ion implantation are removed when the semiconductor substrate is separated, but remain in a portion of the ion-implanted layer with few defects. The element distribution by ion implantation is known, and since it has the characteristic that the type or bonding state is different from the main element that constitutes the semiconductor substrate, it is possible to determine that the ions implanted by ion implantation are present on the first main surface. There is no problem with this surface as long as it is not used as a surface for forming semiconductor substrate devices. When used as the back surface of the substrate, if the implanted ions remain, they will exist between the carbon bonds, so only the outermost surface is formed with a layer that is not very hard, and there is an advantage that it acts as a cushion when bonding to a different substrate. This layer can be later removed by plasma etching or chemical etching (if possible), polishing, or mechanically, so it can also be used as a surface for forming semiconductor devices. However, it also has disadvantages such as the generation of etch pits, accumulation of mechanical strain, and extra costs, so it is necessary to go through a process such as forming a clean epitaxial film again. Since the growth surface opposite the separation surface is an epitaxially formed surface, there is no problem as a surface for forming semiconductor devices.
[0120] It is preferable that the cracks contained in the surface of the first main surface are 100 μm or less in length, and that the maximum diameter of the altered layer contained in the surface is 100 μm or less. The cracks can be observed under an optical microscope as linear black shadows, and are caused by localized, instantaneous expansion. However, since they are minute and remain on the surface, there is no particular problem unless the substrate is used as a surface for forming semiconductor devices. The altered layer refers to the amorphous layer, and can be confirmed by the presence of a ring pattern using RHEED. The cracks have already been released from strain, and the altered layer is amorphous, so that cleavage does not occur here. Therefore, when the substrate is used as a back surface to be bonded to a different substrate, it has the advantage of stopping the extension of new cracks and exhibiting durability against cracking. These layers can be later removed by plasma etching, chemical etching (if possible), polishing, or mechanically, and can also be used as a surface for forming semiconductor devices. However, this method also has drawbacks such as the generation of etch pits, accumulation of mechanical strain, and additional costs, so it is necessary to go through a process of forming a clean epitaxial film again. The growth surface opposite the separation surface is an epitaxially formed surface, so there is no problem as a surface for forming semiconductor devices.
[0121] It is preferable that the first element, which is at least one of the main elements constituting the semiconductor substrate, exists on the surface of the first main surface in an atomic bonding state different from that of the semiconductor lattice of the semiconductor substrate. The presence of an element with a different bonding state on the surface can be confirmed by observation with XPS or AES. Since the first element remains on the surface, there is no problem in using the substrate unless it is used as a device formation surface of a semiconductor substrate. Since it remains loosely on a strong surface, it has the advantage of preventing cracks and acting as a cushion when used as a back surface to be bonded to a heterogeneous substrate. This layer can be later removed by plasma etching or chemical etching (if possible), polishing, or mechanically, and can also be used as a semiconductor device formation surface. However, it also has disadvantages such as the generation of etch pits, accumulation of mechanical strain, and extra costs, so it is necessary to go through a process such as forming a clean epitaxial film again. Since the growth surface opposite the separation surface is an epitaxially formed surface, there is no problem as a semiconductor device formation surface.
[0122] On the surface of the first main surface, it is preferable that the first element, which is at least one of the main elements constituting the semiconductor substrate, is present in a different atomic bonding state from the semiconductor lattice of the semiconductor substrate, forming a plurality of approximately circular patterns. The presence of elements with different bonding states on the surface and the pattern can be confirmed by observing by mapping with XPS or AES. The first element may expand instantaneously and form a plurality of approximately circular patterns due to the physical energy applied when separating the semiconductor substrate 5 from the seed substrate 1b. The plurality of approximately circular patterns may also form an envelope. There is no problem with using this surface as a substrate unless it is used as a device formation surface of the semiconductor substrate. Since it is loose and partially retained on a solid surface, it has the advantage of acting as a cushion when bonding to a different substrate. This layer can be later removed by plasma etching or chemical etching (if possible), polishing, or mechanically, and can also be used as a device formation surface of the semiconductor. However, it also has disadvantages such as the generation of etch pits, accumulation of mechanical strain, and extra costs, so it is necessary to go through a process of forming a clean epitaxial film again. The growth surface opposite to the separation surface is an epitaxially formed surface, and therefore presents no problem as a surface for forming semiconductor devices.
[0123] The semiconductor substrate according to the present embodiment can be used for device substrates and other application products that use substrates. The device substrates and application products include the semiconductor substrate, and therefore the manufacturing costs are reduced.
[0124] Specific examples of application products when the semiconductor layer 3 is diamond include cutting tools such as diamond cutting tools, drills, end mills, replaceable cutting tips for drills, replaceable cutting tips for end mills, replaceable cutting tips for milling, replaceable cutting tips for cutting, metal saws, gear cutting tools, reamers, and taps. In addition to cutting tools, examples of application products include grinding tools, wear-resistant tools, and parts. Examples of grinding tools include dressers. Examples of wear-resistant tools and parts include dies, scribers, water or powder ejection nozzles, and guides such as wires. In addition, examples of thermal applications include heat sinks for semiconductor devices such as high-power laser diodes (LDs) and high-power semiconductor light-emitting devices (LEDs), and examples of optical applications include window materials for high-power lasers and X-ray targets.
[0125] When the semiconductor layer 3 is made of gallium nitride, application products include, for example, substrates for blue LEDs and white LEDs, and substrates for highly efficient switching devices.
[0126] When the semiconductor 3 is silicon carbide, application products include, for example, substrates for power control or high-efficiency power devices mounted on vehicles.
[0127] [Embodiment 3] <Method of manufacturing composite semiconductor substrate> 3(A) to 3(F) are schematic diagrams illustrating a method for manufacturing a composite semiconductor substrate according to an embodiment of the present invention, and FIG 4 is a flowchart illustrating a method for manufacturing a composite semiconductor substrate according to an embodiment of the present invention.
[0128] A method for producing a composite semiconductor substrate according to an embodiment of the present invention includes a step of preparing a seed substrate containing a semiconductor material (shown in FIG. 3(A) and a substrate preparation step (S21) in FIG. 4), a step of forming an ion-implanted layer at a certain depth from the surface of a main surface of the seed substrate by implanting ions into the seed substrate (shown in FIG. 3(B) and an ion-implanted layer formation step (S22) in FIG. 4), and a step of growing a semiconductor layer on the main surface of the seed substrate by a vapor phase synthesis method (shown in FIG. 3(C) and a semiconductor layer growth step (S23) in FIG. 4). The method includes a step of bonding a first substrate onto the semiconductor layer (shown as a first substrate bonding step (S23) in FIG. 3(D) and FIG. 4), and a step of separating a composite semiconductor substrate including the first substrate, the semiconductor layer, and a part of the seed substrate by irradiating light from a main surface of at least one of the first substrate and the seed substrate (shown as a composite semiconductor substrate separation step (S25) in FIG. 3(E-1), (E-2), (F) and FIG. 4).
[0129] In the manufacturing method of the composite semiconductor substrate according to the third embodiment, the substrate preparation step (S21), the ion-implanted layer formation step (S22), the semiconductor layer growth step (S23), and the composite semiconductor substrate separation step (S25) can be the same as the substrate preparation step (S1), the ion-implanted layer formation step (S2), the semiconductor layer growth step (S3), and the semiconductor substrate separation step (S4) in the manufacturing method of the semiconductor substrate according to the first embodiment. Therefore, the step of bonding the first substrate (S24), which is different from the first embodiment, will be described below.
[0130] (Step of bonding the first substrate) 3(D), first substrate 25 is bonded onto semiconductor layer 23. In this way, even if semiconductor layer 23 is formed so thin that it cannot stand on its own, composite semiconductor substrate 26 including semiconductor layer 23 and first substrate 25 can stand on its own and has good handleability. That is, in the third embodiment, expensive semiconductor layer 23 can be made thinner than in the first embodiment, and therefore the manufacturing cost of composite semiconductor substrate 26 can be reduced.
[0131] The first substrate 25 may be, for example, a silicon oxide (SiO2) substrate. The silicon oxide substrate may be formed by forming a SiO2 layer on the semiconductor substrate 23 that has been polished very flat, and then pasted onto the SiO2 layer. A plurality of first substrates 25 may be used. For example, a SiO2 layer may be formed on the first substrate 25, and a plurality of SiO2 substrates may be pasted onto the SiO2 layer. The material of the first substrate is not limited to SiO2, and other materials (metals, etc.) may be used as long as they can form a clean, flat film on the surface. Examples of other materials include gold (Au), titanium (Ti), molybdenum (Mo), tantalum (Ta), and tungsten (W). The material may be a semiconductor, ceramic, single crystal, or polycrystal. Examples include silicon (Si), germanium (Ge), and alumina (Al2O3). In any combination, it is preferable that the substrate is less expensive than the semiconductor substrate to be separated.
[0132] The first substrate 25 can be a substrate made of resin. This is realized for the first time because the present invention is a technology that allows separation at room temperature. When the semiconductor layer 23 is to be used in a high-temperature process, the main surface of the seed substrate 21 of the composite semiconductor substrate 26 is bonded to another heat-resistant substrate using an adhesive, and then the first substrate 25 made of resin can be removed in an appropriate liquid such as alcohol, or the adhesive between the first substrate 25 and the semiconductor layer 23 can be removed, and the first substrate 25 can be removed. When the first substrate 25 is made of resin, the surface of the first substrate 25 may be somewhat less flat than when the first substrate 25 is made of SiO2. This is because an adhesive layer made of a soft and thin adhesive can be placed between the first substrate 25 and the semiconductor layer 23.
[0133] [Embodiment 4] <Method of manufacturing composite semiconductor substrate> 5(A) to 5(E) are schematic diagrams illustrating a method for manufacturing a composite semiconductor substrate according to an embodiment of the present invention, and FIG 6 is a flowchart illustrating a method for manufacturing a composite semiconductor substrate according to an embodiment of the present invention.
[0134] A method for manufacturing a composite semiconductor substrate according to an embodiment of the present invention includes the steps of preparing a seed substrate containing a semiconductor material (shown in FIG. 5(A) and the substrate preparation step (S31) in FIG. 6), forming an ion-implanted layer at a certain depth from the surface of a main surface of the seed substrate by implanting ions into the seed substrate (shown in FIG. 5(B) and the ion-implanted layer formation step (S32) in FIG. 6), bonding a first substrate onto the main surface of the seed substrate (shown in FIG. 5(C) and the first substrate bonding step (S33) in FIG. 6), and separating a composite semiconductor substrate containing a part of the first substrate and the seed substrate by irradiating light from the surface of at least one of the main surfaces of the first substrate and the seed substrate (shown in FIG. 5(D-1), (D-2), (E) and the composite semiconductor substrate separation step (S34) in FIG. 6).
[0135] The method for manufacturing a compound semiconductor substrate according to the fourth embodiment includes the same steps as those of the third embodiment, except that the method for manufacturing a compound semiconductor substrate according to the third embodiment does not include the semiconductor layer growing step (S23).
[0136] In the manufacturing method of the composite semiconductor substrate according to the fourth embodiment, the first substrate 35 is directly bonded onto the main surface of the seed substrate 31. The resulting composite semiconductor substrate 36 has a thin layer of the seed substrate 31a formed on the surface of the first substrate 35. Even if the seed substrate 31a is sliced thin enough that it cannot stand on its own, the composite semiconductor substrate 26 can stand on its own and has good handleability. Furthermore, since no expensive semiconductor layer is formed, the manufacturing cost of the composite semiconductor substrate 36 in the fourth embodiment is lower than that in the third embodiment.
[0137] [Embodiment 5] The composite semiconductor substrate according to the embodiment of the present invention is a composite semiconductor substrate 26, 36 obtained by the composite semiconductor substrate manufacturing method according to the third or fourth embodiment. The composite semiconductor substrate 26, 36 can be manufactured at a reduced cost because the time required for separation from the seed substrate 21b or 31b is shortened. In addition, the composite semiconductor substrate 26, 36 can be obtained without thinning the expensive semiconductor layer 23 or fabricating a semiconductor layer, thereby reducing the manufacturing cost.
[0138] A composite semiconductor substrate according to one embodiment of the present invention includes a first substrate and a semiconductor layer laminated on a main surface of the first substrate, the main surface of the composite semiconductor substrate on the semiconductor layer side includes a first element different in type or bonding state from the main element constituting the semiconductor layer, the first element includes at least one element selected from the group consisting of hydrogen, oxygen, nitrogen, carbon, helium, neon and argon, the surface roughness of the main surface on the semiconductor layer side is less than 10 μm, and the semiconductor layer has a thickness of 0.1 μm to 50 μm. The semiconductor substrate has a flat surface and can be easily processed for various applications. The composite semiconductor substrate contains the first element inside, but is preferably a light-transmitting substrate.
[0139] The composite semiconductor substrates 26 and 36 can be used in the same application products as the semiconductor substrate of the second embodiment.
[0140] [Embodiment 6] The semiconductor junction substrate of the sixth embodiment of the present invention can be fabricated as follows. The manufacturing method used in the first embodiment is performed in the same manner up to the "step of preparing a seed substrate", the "step of forming an ion-implanted layer", and the "step of growing a semiconductor layer". Next, the growth surface is polished flat without separating the semiconductor substrate. The flatness Ra is preferably 100 nm or less, more preferably 10 nm or less, and even more preferably 1 nm or less. This flatness allows direct bonding or bonding after a very thin coating of SOG during bonding. In addition, the parallelism of the polished surface with the ion-implanted layer is preferably 1° or less, more preferably 0.1° or less, and even more preferably 0.03° or less. This is because the higher the parallelism, the greater the effect on the thickness distribution of the semiconductor layer when separated later. This is because the thinner the semiconductor layer, the greater the effect. The more uniform the thickness distribution, the better the semiconductor characteristics. Thus, the semiconductor junction substrate is in a state where the semiconductor layer is not separated from the seed substrate at the ion-implanted layer, but it is characterized in that it can be separated later at room temperature or at a low temperature of 500° C. or less and used. The ion implantation conditions are the same as those described in the first embodiment. In addition, the dose of ions in the present semiconductor junction wafer is 1×10 15 cm -2 More than 3×10 16 cm -2 It is preferable that the thickness is less than 100 nm, because this is within the range where transparency is ensured and separation is possible with the energy of irradiated light.
[0141] Furthermore, the semiconductor junction substrate can be effectively used when the semiconductor layer is thin, for example, when the thickness of the semiconductor layer is 200 μm or less. This is because a thin semiconductor layer is easily broken when separated and made to stand on its own. The thickness of the semiconductor layer in the semiconductor junction substrate is preferably 140 μm or less, more preferably 90 μm or less, and even more preferably 50 μm or less. The semiconductor layer is preferably 1 μm or more, and can function as a semiconductor layer with this thickness. The semiconductor junction substrate can be bonded to a substrate or circuit that cannot be heat treated, and then the seed substrate can be separated. For example, this junction substrate can be bonded to a circuit board on which an electronic circuit is formed using solder at room temperature, and then the seed substrate can be separated by irradiating light, leaving the thin semiconductor layer attached to the circuit board. If the semiconductor layer is a diamond layer, a bare GaN chip (laser diode chip) can be bonded on top of it to form a heat sink for the laser diode. If the semiconductor layer is a GaN layer, a light emitting diode (LED) or laser diode (LD) can be mounted inside to form a hybrid device.
[0142] [Embodiment 7] <Method of manufacturing semiconductor substrate> 7(A) to 7(D) are diagrams that typically show a method for manufacturing a semiconductor substrate according to an embodiment of the present invention, and Fig. 8 is a flowchart that shows the method for manufacturing a semiconductor substrate according to an embodiment of the present invention.
[0143] A method for manufacturing a semiconductor substrate according to an embodiment of the present invention includes a step of preparing a seed substrate containing a semiconductor material (shown in FIG. 7(A) and the substrate preparation step (S41) in FIG. 8), a step of forming an ion-implanted layer at a certain depth from the surface of a main surface of the seed substrate by implanting ions into the seed substrate (shown in FIG. 7(B) and the ion-implanted layer formation step (S42) in FIG. 8), and a step of separating a semiconductor substrate including a part of the seed substrate by irradiating light from the surface of the main surface of the seed substrate (shown in FIG. 7(C-1), (C-2), (D), and the semiconductor separation step (S43) in FIG. 8).
[0144] The method for manufacturing a semiconductor substrate according to the seventh embodiment includes the same steps as those of the first embodiment, except that the method for manufacturing a semiconductor substrate according to the first embodiment does not include the semiconductor layer growing step (S3). EXAMPLES
[0145] The embodiments of the present invention will be described in more detail below with reference to examples, but the embodiments of the present invention are not limited to these.
[0146] In Example 1, the method for manufacturing a semiconductor substrate according to the first embodiment was examined. [Samples 1-1 and 1-2] (Seed substrate preparation) First, a seed substrate 1 was prepared, which was a high-temperature, high-pressure synthesized type IIa single crystal diamond substrate having a size of 6 mm × 6 mm and a thickness of 1 mm. After mechanically polishing the surface of the seed substrate 1, the surface of the seed substrate 1 was etched to a thickness of 1 μm to 2 μm by reactive ion etching.
[0147] (Formation of ion implantation layer) Next, hydrogen ions were implanted into the main surface of the seed substrate 1 to form an ion-implanted layer 2. The implantation energy was 200 keV and the dose was 1×10 15 pieces / cm 2 (Sample 1-1) and 1×10 16 pieces / cm 2 (Sample 1-2) Ion-implanted layer 2 had a depth of about 0.34 μm from the surface of the principal surface of seed substrate 1 and a thickness of about 0.06 μm.
[0148] The optical transmittance of the ion-implanted layer 2 was visually confirmed. All samples were transparent, and no clear difference between the optical transmittance of the seed substrate 1 and the optical transmittance of the ion-implanted layer 2 could be confirmed.
[0149] (Diamond layer formation) Next, the seed substrate 1 on which the ion-implanted layer 2 was formed was placed in a vacuum chamber of a microwave plasma CVD apparatus so that the surface on which the ions were implanted was exposed. The seed substrate 1 was then heated to a temperature of 800°C, and the pressure in the vacuum chamber was set to 13.3 kPa. Then, hydrogen gas, methane gas, and nitrogen gas were introduced into the vacuum chamber to perform the microwave plasma CVD method, and a semiconductor layer 3 made of a single crystal diamond layer having a thickness of 500 μm was formed on the seed substrate 1. The mixing ratio (volume %) of each gas at this time was hydrogen gas:methane gas:nitrogen gas=92:8:0.005.
[0150] In the samples of Sample 1-1 and Sample 1-2, the light transmittance (T1) of the seed substrate 1, the light transmittance (T2) of the ion-implanted layer 2, and the light transmittance (T3) of the diamond layer (semiconductor layer 3) were measured using a general ultraviolet, visible, and near-infrared spectrophotometer. In all samples, the ratio (T2 / T1) of the light transmittance (T1) of the substrate to the light transmittance (T2) of the ion-implanted layer for light with a wavelength of 800 nm was 99% or more. The ratio (T2 / T3) of the light transmittance (T2) of the ion-implanted layer to the light transmittance (T3) of the diamond layer for light with a wavelength of 800 nm was 99% or more.
[0151] (Separation of semiconductor substrate) Next, a YAG laser beam with a wavelength of 1.06 μm was irradiated from the surface of the principal surface of the diamond layer (semiconductor layer 3). The laser beam was focused and irradiated so that the pulse interval was 40 μsec, the pulse width was 10 nsec, and the diameter was 30 μm on the principal surface. At this time, the focus of the laser beam was located inside the ion-implanted layer. The scanning speed of the laser beam was 25 mm / sec. The pulse energy (A) of the laser beam was selected in the range of 0.01 mJ or more and 10 mJ or less. The irradiation fluence per pulse on the principal surface of the diamond layer (semiconductor layer 3) was 1410 mJ / mm 2 The laser light was irradiated in air at room temperature (25°C), in cooled air (-5°C), in pure water (25°C), or in commercially available engine oil (25°C). As a result, the seed substrate 1b was separated from the semiconductor substrate 5 including the diamond layer (semiconductor layer 3) and the seed substrate 1a. The time required for separation in air at room temperature was 11 minutes for sample 1-1 and 7 minutes for sample 1-2.
[0152] [Table 1]
[0153] (evaluation) The obtained seed substrate 1b and the semiconductor substrate 5 including the seed substrate 1a and the diamond layer (semiconductor layer 3) were evaluated according to the following criteria.
[0154] A: When observed at 20x magnification with a normal optical microscope, no cracks were found in either the seed substrates 1a, 1b or the diamond layer (semiconductor layer 3), and the surface roughness (Ra) of the separation surface was Ra≦1 μm.
[0155] B: No cracks are generated in either the substrates 1a and 1b or the diamond layer (semiconductor layer 3), and the surface roughness (Ra) of the separation surface is 1 μm or less. <Ra<10μmであった。
[0156] C: Cracks occurred in at least one of the substrates 1a, 1b and the diamond layer (semiconductor layer 3), or the surface roughness (Ra) of the separated surface was Ra ≧ 10 μm.
[0157] The occurrence of cracks was observed under a normal optical microscope at 20x magnification. Surface roughness was measured using a 3D profiler (model: NEW VIEW200, manufactured by ZYGO) of an optical microscope that uses the principle of white light interference.
[0158] (result) The laser irradiation performed in room temperature air was rated B, while the laser irradiation performed in cooled air, pure water, and oil was rated A. The results are summarized in Table 2.
[0159] [Table 2]
[0160] When the separated surface of the sample rated A was observed by SIMS, it was confirmed that the amount of hydrogen element was clearly greater than that in the bulk. When the separated surface of the sample rated B was observed by SIMS, it was confirmed that the amount of hydrogen element was clearly greater than that in the bulk, and when the surface was further analyzed by XPS, it was confirmed that sp 3 Not only the carbon element of the bond, but also the sp 2 The carbon element in the bond was confirmed.
[0161] Samples under the same conditions as Sample 1-1 and Sample 1-2 were irradiated with laser light under the following conditions: pulse width 0.02psec, 1psec, 10psec, pulse interval 1msec (repetition frequency 1kHz), pulse energy 0.01μJ, 0.03μJ, 0.06μJ, respectively, in pure water at room temperature. The results were the same for Sample 1-1 and Sample 1-2, with the 0.02psec and 1psec conditions receiving a C rating in the above-mentioned evaluation, and the 10psec condition receiving a B rating. The energy required to break the bonds was high, making it difficult to receive an A rating, but even under these laser light irradiation conditions, the diamond layer could be separated from the seed substrate.
[0162] [Sample 2 to Sample 35] In Samples 2 to 35, the semiconductor substrate 5 and the seed substrate 1b were separated using the same method as Sample 1-1, except that the type of ion implanted in the ion implantation, the dose of the ion implanted layer, and the laser light irradiation conditions were set to the conditions shown in Tables 1 and 2. Note that in Samples 11, 25, and 32, the laser light was irradiated from the main surface side of the seed substrate 1, not from the main surface side of the diamond layer (semiconductor layer 3). The time required for separation in air at room temperature is shown in Table 1.
[0163] The obtained seed substrate 1b and semiconductor substrate 5 including seed substrate 1a and diamond layer (semiconductor layer 3) were evaluated according to the same criteria as those for sample 1-1.
[0164] The samples where the laser irradiation was performed in air at room temperature were rated as B or C, while the samples where the laser irradiation was performed in cooled air, aqueous solution, and oil were rated as A or B, except for sample 19 where the laser irradiation was performed in cooled air. The results are summarized in Table 2.
[0165] When the separated surfaces of the samples rated A were observed by SIMS, it was confirmed that the amount of the implanted element was clearly greater than that in the bulk, except for the case where carbon ions were implanted. The separated surfaces of the samples rated B were also confirmed by SIMS to have a greater amount of the implanted element than that in the bulk, except for the case where carbon ions were implanted. Furthermore, when the surfaces were analyzed by XPS, it was confirmed that the amount of the implanted element was greater than that in the bulk, including the case where carbon ions were implanted.3 Not only the carbon element of the bond, but also the sp 2 The carbon element of the bond was confirmed. On the separated surface of the sample rated C, the amount of the implanted element was confirmed to be greater than that in the bulk by SIMS, and the sp 2 It was confirmed that carbon elements in a bonded state were present, forming at least one approximately circular pattern with a diameter of 30 μm or more. In addition, the surface roughness was evaluated using a three-dimensional profiler, and it was confirmed that the approximately circular pattern portion was recessed. When at least two or more of the approximately circular patterns were confirmed, they were lined up in a line. The line direction coincided with the scanning direction of the laser during separation. In this specification, the approximately circular pattern does not mean a perfect circle, but refers to a pattern whose outline has an arc of at least 1 / 5 of a perfect circle. The circle includes not only a perfect circle, but also an elliptical shape. EXAMPLES
[0166] In Example 2, the method for manufacturing the semiconductor substrate according to the first embodiment was examined. [Sample 36] (Preparation of seed substrate, formation of ion implantation layer, formation of diamond layer) A seed substrate 1 similar to that of sample 1-1 was prepared, and an ion-implanted layer 2 and a diamond layer (semiconductor layer 3) were formed in the same manner as sample 1-1. In the sample of sample 36, the light transmittance (T1) of the seed substrate 1, the light transmittance (T2) of the ion-implanted layer 2, and the light transmittance (T3) of the diamond layer (semiconductor layer 3) were measured using a general ultraviolet-visible-near infrared spectrophotometer. The ratio (T2 / T1) of the light transmittance (T1) of the substrate to the light transmittance (T2) of the ion-implanted layer for light with a wavelength of 800 nm was 99% or more. The ratio (T2 / T3) of the light transmittance (T2) of the ion-implanted layer to the light transmittance (T3) of the diamond layer for light with a wavelength of 800 nm was 99% or more.
[0167] (Diamond layer separation) Next, flash lamp light was irradiated from the surface of the main surface of the diamond layer (semiconductor layer 3). The flash lamp light was used by concentrating the light to a diameter of 5 mm from a xenon flash lamp, and light with a wavelength of less than 500 nm and more than 1.25 μm was cut, and light with a wavelength of 500 nm to 1.25 μm was selectively used. The flash lamp light was physically cut to have a pulse interval of 8 msec, a pulse width of 1 μsec, and a diameter of 1 mm on the main surface, and was further concentrated to 0.1 mm for irradiation. At this time, the focus of the flash lamp light was located inside the ion-implanted layer 2. The scanning speed of the flash lamp light (actually the sample moved) was 10 mm / sec. The pulse output (A) of the flash lamp light was changed in the range of more than 3 mJ and less than 30 mJ. In other words, the radiation fluence per pulse width of 1 msec on the main surface of the diamond layer (semiconductor layer 3) was 1900 mJ / mm 2 The irradiation of the flash lamp light was performed in air at room temperature (25°C), in cooled air (-5°C), in pure water (25°C), or in commercially available engine oil (25°C). The seed substrate 1b was separated from the semiconductor substrate 5 including the diamond layer (semiconductor layer 3) and the seed substrate 1a. The time required for separation in air at room temperature was 14 minutes.
[0168] [Table 3]
[0169] (evaluation) The obtained seed substrate 1b and the semiconductor substrate 5 including the seed substrate 1a and the diamond layer (semiconductor layer 3) were evaluated according to the same criteria as in Example 1.
[0170] (result) The flash lamp light irradiation performed in room temperature air was rated B, while the flash lamp light irradiation performed in cooled air, pure water and oil was rated A. The results are shown in Table 4.
[0171] [Table 4]
[0172] When the separated surface of the sample rated A was observed by SIMS, it was confirmed that the amount of hydrogen element was clearly greater than that in the bulk. When the separated surface of the sample rated B was observed by SIMS, it was confirmed that the amount of hydrogen element was clearly greater than that in the bulk, and when the surface was further analyzed by XPS, it was confirmed that sp 3 Not only the carbon element of the bond, but also the sp 2 The carbon element in the bond was confirmed.
[0173] [Sample 37 to Sample 49] (Sample Preparation) In Samples 37 to 49, semiconductor substrate 5 and seed substrate 1b were separated using the same method as Sample 36, except that the type of ion implanted in the ion implantation, the dose of the ion implanted layer, and the flash lamp light irradiation conditions were set to the conditions shown in Table 3. The time required for separation in air at room temperature is shown in Table 3.
[0174] (evaluation) The obtained substrate and diamond layer were evaluated according to the same criteria as in Example 1. The results are summarized in Table 4.
[0175] (result) Those subjected to flash lamp light irradiation in room temperature air were rated B or C, those subjected to irradiation in cooled air and pure water were rated A or B, and those subjected to irradiation in oil were rated A.
[0176] When the separated surfaces of the samples rated A were observed by SIMS, it was confirmed that the amount of the implanted element was greater than that in the bulk, except for the case where carbon ions were implanted. The separated surfaces of the samples rated B were also confirmed by SIMS to have a greater amount of the implanted element than that in the bulk, except for the case where carbon ions were implanted, and furthermore, the surfaces were analyzed by XPS to confirm the sp 3 Not only the carbon element of the bond, but also the sp 2 The carbon element of the bond was confirmed. On the separated surface of the sample rated C, the amount of the implanted element was confirmed to be greater than that in the bulk by SIMS, and the sp 2The carbon elements in a bonded state were present, and could be confirmed as at least one roughly circular pattern with a diameter of 30 μm or more. In addition, the surface roughness was evaluated with a 3D profiler, and it was confirmed that the roughly circular pattern portion was depressed. When at least two or more of these roughly circular patterns were confirmed, they were arranged in a line. The line direction matched the laser scanning direction during division. EXAMPLES
[0177] In Example 3, the method for manufacturing the semiconductor substrate according to the first embodiment was examined. [Samples 101-1, 101-2, 201-1, 201-2, 301-1, 301-2, 401-1, 401-2] (Seed substrate preparation) First, seed substrates 1 were prepared, each consisting of a semiconductor substrate of gallium nitride substrate (samples 101-1, 101-2), aluminum nitride substrate (samples 201-1, 201-2), zinc selenide substrate (samples 301-1, 301-2), and silicon carbide substrate (samples 401-1, 401-2), each having a size of 20 mm × 20 mm and a thickness of 2 mm. After mechanically polishing the surface of the seed substrate 1, the surface of the seed substrate 1 was etched to a thickness of 3 to 5 μm by a thermal, plasma, or chemical treatment appropriate for each seed substrate 1.
[0178] (Formation of ion implantation layer) Next, hydrogen ions were implanted into the main surface of the seed substrate 1 to form an ion-implanted layer 2. The implantation energy was 200 keV and the dose was 7×10 15 pieces / cm 2 (Samples 101-1, 201-1, 301-1, 401-1) or 7×10 16 pieces / cm 2 The depth of the ion-implanted layer 2 from the surface of the main surface of the substrate could be simulated almost accurately, and was 1 μm or less, and the thickness was 0.5 μm or less.
[0179] (Formation of semiconductor layer) Next, a semiconductor layer 3 was grown on the ion-implanted surface of the seed substrate 1 on which the ion-implanted layer 2 had been formed. The formation of the semiconductor layer 3 will be described below for each type of semiconductor layer 3.
[0180] When the semiconductor layer 3 was a gallium nitride layer, the gallium nitride layer was grown by MOCVD. First, a seed substrate 1 made of gallium nitride with a (0001) plane as the main surface was placed in a furnace, and the temperature of the seed substrate 1 in the furnace was heated to 1030°C. Trimethylgallium and ammonia gas, as well as hydrogen gas as a carrier gas, were then introduced to epitaxially grow a gallium nitride layer (semiconductor layer 3) on the main surface of the seed substrate 1. The mixture ratio of trimethylgallium gas:ammonia gas was 1:2000 by volume. As a result, a gallium nitride layer (semiconductor layer 3) could be epitaxially grown to a thickness of 0.8 mm on the seed substrate 1 made of a gallium nitride substrate.
[0181] When the semiconductor layer 3 was an aluminum nitride layer, the aluminum nitride layer was grown by a sublimation method. First, a seed substrate 1 made of aluminum nitride with a (0001) plane as the main surface was placed in a furnace, and the temperature of the seed substrate 1 in the furnace was kept at 2000° C., and the aluminum nitride raw material was sublimated at 2380° C. to epitaxially grow an aluminum nitride layer (semiconductor layer 3) to a thickness of 1 mm on the main surface of the seed substrate 1.
[0182] When the semiconductor layer 3 is zinc selenide, the zinc selenide layer is synthesized by a sublimation method. First, a seed substrate 1 made of zinc selenide with a (111) plane as the main surface is placed in a furnace, and the temperature of the seed substrate 1 in the furnace is maintained at 1100°C. Then, selenium and zinc obtained by decomposing a polycrystalline zinc selenide raw material at about 1130°C are introduced into the device using an inert gas as a carrier gas, and the zinc selenide layer 3 is epitaxially grown on the main surface of the seed substrate 1.
[0183] When the semiconductor layer 3 was silicon carbide, a silicon carbide layer was grown using a normal pressure horizontal cold wall CVD apparatus. First, a seed substrate 1 that was 2° off from the (0001) plane of a 4C-SiC substrate was placed in a furnace, and the temperature of the seed substrate 1 in the furnace was set to 1500°C by high frequency heating. Monosilane gas, propane gas, and hydrogen gas as a carrier gas were introduced, and a silicon carbide layer 3 was epitaxially grown on the main surface of the seed substrate 1. The mixture ratio of monosilane gas:propane gas was 1.5:1 by volume.
[0184] The light transmittance (T1) of the seed substrate 1, the light transmittance (T2) of the ion-implanted layer 2, and the light transmittance (T3) of each semiconductor layer 3 were measured using a general ultraviolet, visible, and near-infrared spectrophotometer. The ratios (T2 / T1) of the light transmittance (T1) of the seed substrate 1 to the light transmittance (T2) of the ion-implanted layer 2 for light with a wavelength of 800 nm all exceeded 90%. The ratios (T2 / T3) of the light transmittance (T2) of the ion-implanted layer to the light transmittance (T3) of the semiconductor layer for light with a wavelength of 800 nm all exceeded 90%.
[0185] (Separation of semiconductor substrate) Next, a YAG laser beam having a wavelength of 1.06 μm was irradiated from the main surface of the semiconductor layer 3. The laser beam was focused and irradiated so that the pulse interval was 40 μsec, the pulse width was 10 nsec, and the diameter was 30 μm on the main surface. At this time, the focus of the laser beam was located inside the light absorption layer. The scanning speed of the laser beam was 25 mm / sec. The pulse energy (A) of the laser beam was selected in the range of 0.01 mJ or more and 10 mJ or less. In other words, the irradiation fluence per pulse on the main surface of the semiconductor layer was 1410 mJ / mm. 2 The laser light was irradiated in room temperature air (25°C), in cooled air (-5°C), in pure water (25°C), or in commercially available engine oil (25°C). As a result, the substrate and the semiconductor layer were separated.
[0186] [Table 5]
[0187] [Table 6]
[0188] [Table 7]
[0189] [Table 8]
[0190] (evaluation) The obtained seed substrate 1b and semiconductor substrate 5 including seed substrate 1a and semiconductor layer 3 were evaluated according to the same criteria as in Example 1.
[0191] (result) For samples 101-1 and 101-2 in which the semiconductor layer 3 is made of gallium nitride, those in which the laser irradiation was performed in air at room temperature were rated B, and those in which the laser irradiation was performed in cooled air, pure water, and oil were rated A.
[0192] For the samples 201-1 and 201-2 in which the semiconductor layer 3 is aluminum nitride, those in which the laser irradiation was performed in air at room temperature were rated B, and those in which the laser irradiation was performed in cooled air, pure water, and oil were rated A.
[0193] For samples 301-1 and 301-2 in which the semiconductor layer 3 is zinc selenide, the samples in which the laser irradiation was performed in air at room temperature were rated C, the samples in which the laser irradiation was performed in cooled air were rated B, and the samples in which the laser irradiation was performed in pure water and oil were rated A.
[0194] For the samples 401-1 and 401-2 in which the semiconductor layer 3 is silicon carbide, those in which the laser irradiation was performed in air at room temperature were rated B, and those in which the laser irradiation was performed in cooled air, pure water, and oil were rated A.
[0195] The results are summarized in Tables 9 to 12.
[0196] [Table 9]
[0197] [Table 10]
[0198] [Table 11]
[0199] [Table 12]
[0200] When the separated surface of the sample rated A was observed by SIMS, it was confirmed that the amount of hydrogen element was clearly greater than that in the bulk. When the separated surface of the sample rated B was observed by SIMS, it was confirmed that the amount of hydrogen element was greater than that in the bulk, and furthermore, when the surface was analyzed by XPS, it was confirmed that the main elements were in a different bond state than in the semiconductor substrate. Specifically, it was confirmed that the Ga element was in the case of the GaN substrate, the Al element was in the case of the AlN substrate, the Zn element was in the case of the ZnSe substrate, and the Si element was in the case of the SiC substrate, each in a different bond state than in the substrate. When the separated surface of the sample rated C was observed by SIMS, it was confirmed that the amount of hydrogen element was greater than that in the bulk, and the main elements were in a different bond state than in the semiconductor substrate by XPS analysis, and the surface roughness was evaluated by a 3D profiler, and it was confirmed that the depressions with a diameter of 30 μm or more were in a roughly circular pattern.
[0201] Samples with the same conditions as Sample 101-1, Sample 101-2, Sample 201-1, Sample 201-2, Sample 301-1, Sample 301-2, Sample 401-1, and Sample 401-2 were irradiated with laser light under the following conditions: pulse width 0.02psec, 1psec, and 10psec, pulse interval 1msec (repetition frequency 1kHz), pulse energy 0.008μJ, 0.02μJ, and 0.05μJ, respectively, in pure water at room temperature. The results were the same for all samples, with the 0.02psec and 1psec conditions receiving a C rating in the above-mentioned evaluation, and the 10psec condition receiving a B rating. The energy required to break the bonds was high, making it difficult to receive an A rating, but even under these laser light irradiation conditions, the diamond layer could be separated from the seed substrate.
[0202] [Sample 102 to Sample 120] In Samples 102 to 120, the substrate and the semiconductor layer were separated using the same method as Sample 101-1, except that the type of ions implanted in the ion implantation, the dose of the ion implanted layer, and the laser light irradiation conditions were set to the conditions shown in Table 5. Note that in Sample 111, the laser light irradiation was performed from the main surface side of the substrate, not from the main surface side of the semiconductor layer.
[0203] [Sample 202 to Sample 220] (Sample Preparation) In Samples 202 to 220, the substrate and the semiconductor layer were separated using the same method as Sample 201-1, except that the type of ion implanted in the ion implantation, the dose of the ion implanted layer, and the laser light irradiation conditions were set to the conditions shown in Table 6. Note that, in Sample 211, the laser light irradiation was performed from the main surface side of the substrate, not from the main surface side of the semiconductor layer.
[0204] [Sample 302 to Sample 320] In Samples 302 to 320, the substrate and the semiconductor layer were separated using the same method as Sample 301-1, except that the type of ions implanted in the ion implantation, the dose amount in the ion implantation layer, and the laser light irradiation conditions were set to the conditions shown in Table 7. Note that, in Sample 311, the laser light irradiation was performed from the principal surface side of the substrate, not from the principal surface side of the semiconductor layer.
[0205] [Sample 102 to Sample 120] In Samples 402 to 420, the substrate and the semiconductor layer were separated using the same method as Sample 401-1, except that the type of ions implanted in the ion implantation, the dose amount in the ion implantation layer, and the laser light irradiation conditions were set to the conditions shown in Table 8. Note that in Sample 411, the laser light irradiation was performed from the principal surface side of the substrate, not from the principal surface side of the semiconductor layer.
[0206] (evaluation) The obtained seed substrate 1b and semiconductor substrate 5 including seed substrate 1a and semiconductor layer 3 were evaluated according to the same criteria as in Example 1.
[0207] (result) For samples 102 to 120 in which the semiconductor layer 3 is made of gallium nitride, those in which the laser irradiation was performed in room temperature air or in cooled air were rated A or B, and those in which the laser irradiation was performed in pure water or oil were rated A.
[0208] For samples 202 to 220 in which the semiconductor layer 3 is aluminum nitride, those in which the laser irradiation was performed in room temperature air or cooled air were rated A or B, and those in which the laser irradiation was performed in pure water or oil were rated A.
[0209] For samples 302 to 320 in which the semiconductor layer 3 is zinc selenide, those in which the laser irradiation was performed in room temperature air were rated B or C, those in which the laser irradiation was performed in cooled air were rated A or B, and those in pure water and oil were rated A.
[0210] For samples 402 to 420 in which the semiconductor layer 3 is silicon carbide, those in which the laser irradiation was performed in air at room temperature were rated A or B, and those in which the laser irradiation was performed in cooled air, pure water, and oil were rated A.
[0211] When the separated surface of the sample rated A was observed by SIMS, it was confirmed that the amount of the implanted element was clearly greater than that in the bulk. When the separated surface of the sample rated B was observed by SIMS, it was confirmed that the amount of the implanted element was greater than that in the bulk, and furthermore, when the surface was analyzed by XPS, it was confirmed that the main element was in a different bond state than that in the semiconductor substrate. Specifically, it was confirmed that the Ga element was in the case of the GaN substrate, the Al element was in the case of the AlN substrate, the Zn element was in the case of the ZnSe substrate, and the Si element was in the case of the SiC substrate, each in a different bond state than that in the substrate. When the separated surface of the sample rated C was observed by SIMS, it was confirmed that the implanted element was in a greater amount than that in the bulk, and the main element was in a different bond state than that in the semiconductor substrate by XPS analysis, and the surface roughness was evaluated by a 3D profiler, and it was confirmed that the depressions with a diameter of 30 μm or more were in a roughly circular pattern. EXAMPLES
[0212] In Example 4, the manufacturing method of the semiconductor substrate according to the fourth embodiment was examined. Specifically, in this example, in the manufacturing process of samples 101-120 in Example 3, instead of forming a semiconductor layer, a first substrate 35 made of SiO2 was bonded to seed substrate 31 after ion implantation into the seed substrate, and composite semiconductor substrate 36 and seed substrate 31b were separated using the same method as in Example 3. Evaluation of the separation surface showed a tendency that was almost consistent with Table 9 in Example 3, although the surface roughness became slightly larger in some areas.
[0213] In the composite semiconductor substrate 36, the first substrate 35 made of SiO2 can be easily formed to a thickness of 0.3 mm or more, so that even if the semiconductor substrate is thin, it will not crack and can be easily carried around. EXAMPLES
[0214] In Example 5, the manufacturing method of the semiconductor substrate according to the fourth embodiment was examined. Specifically, in this example, in the manufacturing process of Samples 1 to 35 in Example 1, instead of forming a diamond layer, a first substrate 35 made of SiO2 was bonded to the seed substrate 31 after ion implantation into the seed substrate, and the composite semiconductor substrate 36 and the seed substrate 31b were separated using the same method as in Example 1. Evaluation of the separation surface showed a tendency that was almost consistent with Table 2 in Example 1, although the surface roughness was slightly increased in some areas.
[0215] In the composite semiconductor substrate 36, the first substrate 35 made of SiO2 can be easily formed to a thickness of 0.3 mm or more, so that even if the semiconductor substrate is thin, it will not crack and can be easily carried around. EXAMPLES
[0216] In Example 6, the semiconductor junction substrate of the sixth embodiment was fabricated as follows. A seed substrate was prepared by the same manufacturing method as Sample 1-1 and Sample 1-2 used in Example 1, an ion-implanted layer was formed, and then a diamond layer (semiconductor layer) was formed. Next, the semiconductor substrate was not separated, and the growth surface was polished flat to Ra of 0.1 μm or less to obtain a semiconductor junction substrate. If Ra is 1 μm or less, polishing is not necessary. At this time, the semiconductor layer was 150 μm thick when fabricated under the same conditions as Sample 1-1, and 50 μm thick when fabricated under the same conditions as Sample 1-2. The substrate with the ion-implanted layer of the appropriate conditions and processed flat is the semiconductor junction substrate. This semiconductor junction substrate was bonded to a circuit board (bare semiconductor board) on which an electronic circuit was formed, using AuSn solder. Then, as in Example 1, it was irradiated with laser light in cooled air to separate it from the seed substrate, and a thin diamond layer was attached to the circuit board. Next, a bare GaN chip (laser diode chip) was attached to the thin diamond layer via a thin layer of Sn at room temperature using the principle of friction that utilizes ultrasonic vibrations, and then wired to a laser diode and operated. When comparing the output of laser diodes with and without a diamond layer, the one with the diamond layer was able to produce a 20-30% higher output. EXAMPLES
[0217] In Example 7, the semiconductor junction substrate of the sixth embodiment was fabricated as follows. A seed substrate was prepared by the same manufacturing method as that of Sample 101-1 and Sample 101-2 used in Example 3, an ion-implanted layer was formed, and then a diamond layer (semiconductor layer) was formed. Next, the semiconductor substrate was not separated, and a planarization process was performed as a semiconductor substrate to obtain a semiconductor junction substrate. A necessary epitaxial layer was formed on this semiconductor junction substrate to fabricate an LED element, and SiO2 was formed on it as a cap layer, and the surface was polished to a flat surface with Ra of 10 nm or less. Up to this point, it was performed on a 2-inch wafer. After this, it was cut into 3 mm squares, and this semiconductor junction substrate with LED was bonded to a circuit board (a bare Si semiconductor board) on which a flat SiO2 layer was provided. Then, in the same manner as in Example 1, a laser beam was irradiated in cooling air to separate it from the seed substrate, and a circuit board on which only a thin semiconductor layer was mounted was fabricated. After that, when it was wired to a laser diode, it was possible to operate it. In this example, a hybrid type electronic circuit was fabricated.
[0218] The embodiments and examples disclosed herein should be considered to be illustrative and not restrictive in all respects. The scope of the present invention is defined by the claims, not the above description, and is intended to include all modifications within the meaning and scope of the claims. [Industrial Applicability]
[0219] The semiconductor substrate and composite semiconductor substrate of the present invention are useful for use in tools such as cutting tools, grinding tools, and wear-resistant tools, as well as in various products such as optical components, semiconductors, and electronic components, substrates for blue LEDs and white LEDs, substrates for highly efficient switching devices, substrates for power control or highly efficient power devices mounted on vehicles, optical substrates, and optical lenses. [Explanation of symbols]
[0220] 1, 21, 31, 41 seed substrate; 1a, 1b, 21a, 21b, 31a, 31b, 41a, 41b part of seed substrate; 2, 22, 32 ion implanted layer; 3, 23 semiconductor layer; 4, 24, 34, 44 light; 5 semiconductor substrate; 25, 35 first substrate; 26, 36 composite semiconductor substrate.
Claims
1. A semiconductor substrate comprising a substrate made of a semiconductor material and a semiconductor layer provided on the substrate, the semiconductor substrate includes a first major surface and a second major surface; the first main surface is a main surface exposed to the outside of the substrate, the first main surface contains a first element having a different kind or bonding state from a main element constituting the semiconductor substrate; the first element includes at least one element selected from the group consisting of hydrogen, oxygen, nitrogen, carbon, helium, neon, and argon; the first element is present in the first main surface so as to form a plurality of substantially circular depressions, The surface roughness Ra of the first main surface as defined in JIS B 0601-2013 is less than 10 μm, The semiconductor layer is made of diamond, gallium nitride, aluminum nitride, zinc selenide or silicon carbide. Semiconductor substrate.
2. A composite semiconductor substrate including a substrate made of a semiconductor material, a semiconductor layer provided on one main surface of the substrate, and a first substrate provided on a main surface of the semiconductor layer opposite to the main surface on the substrate side, the composite semiconductor substrate includes a third major surface; the third main surface is a main surface exposed to an outside of the substrate, the third principal surface contains a first element different in kind or bonding state from a main element constituting the semiconductor layer, the first element includes at least one element selected from the group consisting of hydrogen, oxygen, nitrogen, carbon, helium, neon, and argon; the first element is present on the third main surface so as to form a plurality of substantially circular patterns, The third main surface of the composite semiconductor substrate has a surface roughness Ra of less than 10 μm as defined in JIS B 0601-2013; The semiconductor layer has a thickness of 0.1 μm or more and 50 μm or less, The semiconductor layer is made of diamond, gallium nitride, aluminum nitride, zinc selenide or silicon carbide. Compound semiconductor substrate.
3. A semiconductor layer is disposed on a main surface of the seed substrate and in contact with the main surface of the seed substrate. the seed substrate has an ion-implanted layer including a first element having a different kind or bonding state from a main element constituting the semiconductor material, the first element includes at least one element selected from the group consisting of hydrogen, oxygen, nitrogen, carbon, helium, neon, and argon; The ion-implanted layer has a thickness of 50 nm to 10 μm, and the ion dose is 1×10 14 cm -2 Above 2 x 10 18 cm -2 is as follows: The semiconductor layer is a heteroepitaxially grown layer or a homoepitaxially grown layer that inherits the plane orientation of the seed substrate. Semiconductor junction substrate.
Citation Information
Patent Citations
Production of diamond thin plate
JP1994234595A
Method of manufacturing substrate for semiconductor device, substrate for semiconductor device and semiconductor device
JP2004026624A
Diamond single crystal substrate and its manufacturing method
JP2005219962A
Method for processing diamond
JP2007112637A
Substrate slicing method
JP2011060860A