Two-component room temperature fast curing organopolysiloxane composition and article

The two-component room-temperature fast-curing organopolysiloxane composition addresses slow deep curing and toxicity issues by using cyclic ketones as leaving groups, ensuring rapid curing and safety for human health and the environment, suitable for diverse applications.

JP7582341B2Active Publication Date: 2024-11-13SHIN ETSU CHEMICAL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022578265
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-01-27
Filing Date
2022-01-18
Publication Date
2024-11-13
Estimated Expiration
2042-01-18

AI Technical Summary

Technical Problem

Existing room-temperature-curable organopolysiloxane compositions using hydrolyzable organosilane compounds as crosslinking agents face issues with slow deep curing, toxicity from harmful by-products like 2-butanone oxime and methanol, and environmental hazards from tin catalysts, which are not environmentally friendly.

Method used

A two-component room-temperature fast-curing organopolysiloxane composition using a specific structure of organopolysiloxane with hydrolyzable silyl or silanol groups, combined with a hydrolyzable organosilane compound releasing cyclic ketones like cyclobutanone or cyclopentanone as leaving groups, and a curing catalyst, ensuring rapid and deep curing without health or environmental hazards.

Benefits of technology

The composition achieves fast and deep curing with improved workability, storage stability, and safety, eliminating health risks and environmental hazards, suitable for various applications including automotive, electrical, and architectural uses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582341000001
    Figure 0007582341000001
  • Figure 0007582341000002
    Figure 0007582341000002
  • Figure 0007582341000003
    Figure 0007582341000003
Patent Text Reader

Abstract

This two-component type room temperature fast-curing organopolysiloxane composition: includes a first agent containing, at a specific ratio, (A) a specific structure organopolysiloxane having a silanol group or a hydrolyzable silyl group at molecular chain ends thereof, (B) a hydrolyzable organosilane compound and / or a partially hydrolyzed condensate thereof that releases a cyclic ketone compound as a leaving group (leaving substance) by hydrolysis, and (C) a curing catalyst; and a second agent containing, in a specific amount, (A') a specific structure organopolysiloxane having a silanol group at molecular chain ends thereof; and has more excellent hardenability than one-component type room temperature-curing organopolysiloxane compositions. This composition leaves or releases a cyclic ketone compound such as cyclobutanone or cyclopentanone as a leaving group (leaving compound) at the time of curing, and thus solves hazard or safety problems with respect to human bodies or environments.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a two-component, room-temperature fast-curing organopolysiloxane composition of the condensation cure type that crosslinks (cures) through a hydrolysis and condensation reaction in the presence of moisture (water) in the air at room temperature (23°C±15°C), in particular to a two-component, room-temperature fast-curing organopolysiloxane composition that contains a crosslinking agent in which the eliminated compound that is eliminated from the crosslinking agent (curing agent) by a hydrolysis reaction during curing is a cyclic ketone compound such as cyclobutanone or cyclopentanone, and to various articles that contain the composition or a cured product thereof (silicone rubber). [Background technology]

[0002] Room temperature curable organopolysiloxane compositions that cure at room temperature to become silicone rubber have been known for some time and have been widely used in the industrial world. Known mechanisms for curing at room temperature include a mechanism for curing by hydrosilylation addition reaction, a mechanism for radical curing by ultraviolet light, and a mechanism for curing by condensation reaction between hydrolyzable groups bonded to silicon atoms and hydroxyl groups. Among these, room temperature curable organopolysiloxane compositions that cure by condensation reaction have the advantage that they can be easily cured at room temperature and are less susceptible to curing inhibition by impurities that occur in hydrosilylation addition reactions, etc. Therefore, they are widely used in the fields of automotive gaskets and sealing materials, construction sealants, electrical and electronic parts, etc.

[0003] Room temperature curable organopolysiloxane compositions that cure by condensation reactions contain a hydrolyzable organosilane compound having a hydrolyzable group in the molecule as a curing agent (crosslinking agent), and examples of curing agents that are already widely used include deoxime-type hydrolyzable organosilane compounds that release oxime compounds such as 2-butanone oxime upon curing, and dealcohol-type hydrolyzable organosilane compounds that release alcohol compounds such as methanol. The rubber-like cured products obtained by curing compositions containing these curing agents have high heat resistance, chemical resistance, and weather resistance derived from silicone (siloxane structure). On the other hand, oxime compounds such as 2-butanone oxime that are generated during curing of deoxime-type curing agents are suspected to be carcinogenic and are undesirable, and methanol and the like that are generated during curing of alcohol-free curing agents are toxic to the human body and designated as deleterious substances, which are undesirable from the viewpoint of human health. Furthermore, in some cases, these compositions use tin catalysts as curing catalysts, which are subject to stronger regulations as environmentally hazardous substances, which is undesirable from the viewpoint of environmental protection.

[0004] Furthermore, conventional one-component room temperature curable organopolysiloxane compositions that cure by a condensation reaction have the drawback that curing proceeds from the surface exposed to atmospheric moisture (water), but it takes a long time for curing to be completed in deeper areas that are less exposed to moisture. For this reason, a technology is known that significantly improves curability by making a two-component room temperature curable organopolysiloxane composition in which the base polymer, crosslinking agent, catalyst, etc. are appropriately divided.

[0005] In Japanese Patent No. 3916403 (Patent Document 1), a composition is proposed that contains an organic compound having at least one carbonyl group (C=O group) in one molecule and an organic compound having at least one primary amino group (NH2 group) in one molecule, for a diorganopolysiloxane blocked with a hydrolyzable silyl group, with both ends of the molecular chain having an oxime structure as a leaving group. This improves deep curing and fast curing properties by utilizing water produced as a by-product from a ketimine-forming reaction between a carbonyl group and a primary amino group, but has the disadvantage that a large amount of a carbonyl compound must be intentionally added to one of the two components, and a composition containing a carbonyl compound is prone to separation. In addition, since the curing properties of a dealcohol-type organopolysiloxane composition are inferior to those of a dealcohol-type organopolysiloxane composition, a sufficient curing speed cannot be obtained even if the method of Patent Document 1 is used. For this reason, JP 2011-37968 A (Patent Document 2) reports that a silanol-containing organopolysiloxane and a ketene silyl acetal compound are mixed in the presence of an organic compound having a nitrogen atom, and then mixed with a composition containing silanol groups, thereby dramatically improving curability, but this technique is inferior in terms of deep curability to the technique of Patent Document 1, which generates water from the inside. Furthermore, these techniques cannot reduce the toxicity and environmental load of the leaving groups (methanol, 2-butanone oxime) released during curing of the oxime-free and alcohol-free room temperature curable organopolysiloxane compositions as described above. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Patent No. 3916403 [Patent Document 2] JP 2011-37968 A Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention has been made in view of the above circumstances, and has an object to provide a two-component, room-temperature-curable organopolysiloxane composition which is a two-component type that has excellent fast curing properties and deep curing properties, and which has no reported health hazards, such as carcinogenicity or reproductive toxicity to the human body, or environmental hazards, such as toxicity to aquatic organisms, during curing, and which uses a hydrolyzable organosilane compound as a crosslinking agent (curing agent) that eliminates and releases a cyclic ketone compound, such as cyclobutanone or cyclopentanone, which has a relatively high flash point, as a leaving group (leaving compound); various articles containing the composition; and various articles having an elastomer molded product (cured silicone rubber product) obtained by curing the two-component, room-temperature-curable organopolysiloxane composition. [Means for solving the problem]

[0008] As a result of intensive research conducted by the present inventors in order to achieve the above-mentioned object, it has been found that a two-component, room-temperature-curable, fast-curing organopolysiloxane composition comprising a first part containing, in specific proportions, (A) an organopolysiloxane of a specific structure having a silanol group or a hydrolyzable silyl group at the molecular chain terminal, (B) a hydrolyzable organosilane compound represented by the following general formula (4) and / or a partial hydrolysis condensate thereof, and (C) a curing catalyst, and a second part containing a specific amount of (A') an organopolysiloxane of a specific structure having a silanol group at the molecular chain terminal, has superior curability to one-component, room-temperature-curing organopolysiloxane compositions and eliminates and releases a cyclic ketone compound, such as cyclobutanone or cyclopentanone, as a leaving group (leaving compound) during curing, thereby resolving problems of toxicity to the human body and the environment and safety. [ka] (In the formula, R 1 is a monovalent hydrocarbon group having 1 to 10 carbon atoms, a is an integer from 1 to 8, and b is 3 or 4.

[0009] In a two-component room-temperature curable organopolysiloxane composition, a first agent containing, as a base polymer, an organopolysiloxane of a specific structure whose molecular chain ends are terminated with hydrolyzable silyl groups, or an organopolysiloxane whose molecular chain ends are terminated with hydrolyzable silyl groups, produced by coexisting an organopolysiloxane whose molecular chain ends are terminated with silanol groups and a specific hydrolyzable silane compound with a curing catalyst, is mixed with a second agent containing, as a base polymer, an organopolysiloxane whose molecular chain ends are terminated with silanol groups, whereby a direct crosslinking reaction occurs between the terminal hydrolyzable silyl groups of the base polymer in the first agent and the terminal silanol groups of the base polymer in the second agent, resulting in improved curability compared to a one-component room-temperature curable organopolysiloxane composition.

[0010] Furthermore, in response to the above-mentioned curability problem, the present inventors have discovered that by using in combination a hydrolyzable organosilane compound (crosslinking agent) which uses a cyclic ketone compound such as cyclobutanone or cyclopentanone as a leaving group (leaving compound) as component (B) of the present invention, which has no reported health hazards such as carcinogenicity or reproductive toxicity to the human body and which has a relatively high flash point, and an organic compound having at least one primary amino group (NH group) in one molecule as component (D), it is possible to obtain a composition which has excellent fast-curing properties while suppressing separation of the organopolysiloxane composition by generating moisture from the inside through a ketimine reaction, without the need to add a ketone compound as in Patent Document 1, and which has led to the completion of the present invention.

[0011] That is, the present invention provides the following two-component room temperature fast-curing organopolysiloxane composition, and various articles containing the composition or a cured product thereof (automobile parts, automobile oil seals, electrical and electronic parts, building structures, civil engineering structures, adhesives, sealing agents, potting agents, coating agents, etc.). [1] (A) an organopolysiloxane represented by the following general formula (1), (2), or (3): 10 to 90 parts by mass (with the proviso that the total of the components (A) and (A') is 100 parts by mass), [ka] (In the formula, R is the same or different, and is an unsubstituted or halogen-substituted monovalent hydrocarbon group having 1 to 10 carbon atoms; n is 5. ~2,000 ) [ka] (In the formula, R and n are as defined above, and n may be the same or different, and m is an integer of 1 to 10.) [ka] (In the formula, R and n are as defined above, X is an oxygen atom or an alkylene group having 2 to 5 carbon atoms, and k is independently 0 or 1 for each silicon atom to which it is bonded.) (B) a hydrolyzable organosilane compound represented by the following general formula (4) and / or a partial hydrolysis condensate thereof: 0.1 to 30 parts by mass per 100 parts by mass of the total of the components (A) and (A'), [ka] (In the formula, R 1 is a monovalent hydrocarbon group having 1 to 10 carbon atoms, a is an integer from 1 to 8, and b is 3 or 4; and (C) Curing catalyst: 0.001 to 10 parts by mass per 100 parts by mass of the total of the components (A) and (A') A first agent comprising (A') an organopolysiloxane represented by the following general formula (1) or (2): 10 to 90 parts by mass (provided that the total of components (A) and (A') is 100 parts by mass); [ka] (In the formula, R is the same or different, and is an unsubstituted or halogen-substituted monovalent hydrocarbon group having 1 to 10 carbon atoms; n is 5~2,000 ) [ka] (In the formula, R and n are as defined above, and n may be the same or different, and m is an integer of 1 to 10.) A second agent comprising and (D) an amine compound having a primary amino group is contained as a curing accelerator in an amount of 0 to 20 parts by mass in each of the first agent and the second agent per 100 parts by mass of the total of the components (A) and (A') (however, at least one of the first agent and the second agent contains 0.1 part by mass or more). The present invention relates to a two-component room temperature fast curing organopolysiloxane composition. [ 2 ] The hydrolyzable organosilane compound and / or its partial hydrolysis condensate of component (B) is one that releases a cyclic ketone compound upon hydrolysis. [1] 2. The two-component room temperature fast curing organopolysiloxane composition according to claim 1. [ 3 ] The cyclic ketone compound to be eliminated is cyclobutanone or cyclopentanone. 2 2. The two-component room temperature fast curing organopolysiloxane composition according to claim 1 . [ 4 ] Furthermore, the inorganic filler (E) is contained in the first agent and the second agent in an amount of 0 to 1,000 parts by mass, respectively, per 100 parts by mass of the total of the components (A) and (A') (however, at least one of the first agent and the second agent contains 0.1 part by mass or more).[1] to [ 3 13. The two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 12. [ 5 ] Component (E) is one or more inorganic fillers selected from calcium carbonate, fumed silica, precipitated silica, carbon black, and aluminum oxide. 4 2. The two-component room temperature fast curing organopolysiloxane composition according to claim 1 . [ 6 ] Furthermore, the first agent and the second agent each contain 0 to 10 parts by mass of an adhesion promoter (F) relative to 100 parts by mass of the total of the components (A) and (A') (however, at least one of the first agent and the second agent contains 0.001 part by mass or more). [1] to [ 5 13. The two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 12. [ 7 ] The mixing ratio of the first agent to the second agent is 1:1 to 10:1 by mass [1] to [ 6 13. The two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 12. [ 8 ] [1]~[ 7 13. An automobile part having a cured product of the two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 12. [ 9 ] [1]~[ 7 13. An oil seal for automobiles comprising a cured product of the two-component room temperature fast-curing organopolysiloxane composition according to any one of claims 1 to 12. [ 10 ] [1]~[ 7

[0021] An electric / electronic part having a cured product of the two-component room temperature fast curing organopolysiloxane composition described in any one of the above. [ 11 ] [1]~[ 7 13. A building structure comprising a cured product of the two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 12. [ 12 ] [1]~[ 7 13. A civil engineering structure comprising a cured product of the two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 12. [ 13 ] [1]~[ 7 13. An adhesive comprising the two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 12. [ 14 ] [1]~[ 7 13. A sealant comprising the two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 12. [ 15 ] [1]~[ 7 13. A potting agent comprising the two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 12. [ 16 ] [1]~[ 713. A coating agent comprising the two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 12. Effect of the Invention

[0012] The two-component room temperature fast-curing organopolysiloxane composition of the present invention is composed of a two-component composition of a first part and a second part, which provides excellent fast curing properties and deep curing properties when the first part and the second part are mixed together.

[0013] The two-component room temperature fast curing organopolysiloxane composition of the present invention is particularly excellent in fast curing in air at room temperature and has good workability. Furthermore, it has storage stability. Therefore, even after long-term storage, for example, 6 months, the two-component room temperature fast curing organopolysiloxane composition of the present invention quickly cures when the first and second components are mixed and exposed to air, and exhibits excellent physical properties. Furthermore, the crosslinking agent used in the present invention has no reported health hazards such as carcinogenicity and reproductive toxicity to the human body, or environmental hazards such as toxicity to aquatic organisms, during curing, and releases cyclic ketone compounds such as cyclobutanone and cyclopentanone, which have a relatively high flash point, as leaving groups (leaving substances), so that it can be suitably used as various adhesives, sealing agents, potting agents, coating agents, etc., taking into consideration human health and safety and environmental protection (load reduction). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The present invention will now be described in further detail. <Two-component room temperature fast curing organopolysiloxane composition> The two-component room temperature curable organopolysiloxane composition of the present invention comprises a first part containing specific amounts of components (A), (B), and (C) described below, and a second part containing component (A'). Note that the second part does not contain components (B) and (C). Each component will be described in detail below. In the present invention, the viscosity is a value measured at 23°C using a rotational viscometer in accordance with the method specified in JIS Z-8803. Unless otherwise specified, "room temperature" refers to a state where the temperature is 23°C ± 15°C and the humidity is 50% RH ± 5% RH.

[0015] [Component (A) and Component (A'): Organopolysiloxane] Component (A) is an organopolysiloxane represented by general formula (1), (2) or (3) described below, which is blended into the first agent, and component (A') is an organopolysiloxane represented by general formula (1) or (2) described below, which is blended into the second agent. These components (A) and (A') act as the main component (base polymer) in the two-component room-temperature fast-curing organopolysiloxane composition of the present invention.

[0016] Component (A) used in the two-component room temperature curable organopolysiloxane composition of the present invention is an organopolysiloxane represented by the following general formula (1), (2), or (3) and preferably having a viscosity at 23°C of 20 to 1,000,000 mPa s, and component (A') is an organopolysiloxane represented by the following general formula (1) or (2) and preferably having a viscosity at 23°C of 20 to 1,000,000 mPa s. [ka] (In the formula, R is the same or different, and is an unsubstituted or halogen-substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and n is an integer of 5 or greater.) [ka] (In the formula, R and n are as defined above, and n may be the same or different, and m is an integer of 1 to 10.) [ka] (In the formula, R and n are as defined above, X is an oxygen atom or an alkylene group having 2 to 5 carbon atoms, and k is independently 0 or 1 for each silicon atom to which it is bonded.)

[0017] In the general formulae (1), (2), and (3), R is a monovalent hydrocarbon group having 1 to 10 carbon atoms that is unsubstituted or substituted with a halogen atom, such as alkyl groups such as methyl, ethyl, and propyl; cycloalkyl groups such as cyclohexyl; alkenyl groups such as vinyl and allyl; aryl groups such as phenyl and tolyl; and groups in which the hydrogen atoms bonded to the carbon atoms of these groups are partially substituted with halogen atoms, such as 3,3,3-trifluoropropyl. Among these, methyl, vinyl, phenyl, and 3,3,3-trifluoropropyl are preferred, and methyl is particularly preferred. The multiple Rs in the general formulae (1), (2), and (3) may be the same or different groups.

[0018] Furthermore, n is an integer of 5 or more, and in particular an integer that provides a viscosity of this diorganopolysiloxane at 23° C. in the range of 20 to 1,000,000 mPa·s, and preferably in the range of 100 to 300,000 mPa·s. The value of n that provides such a viscosity may be, specifically, an integer of usually 5 to 2,000, preferably 20 to 1,500, and more preferably about 50 to 1,000. In the present invention, the degree of polymerization (or molecular weight) can usually be determined as the number average degree of polymerization (number average molecular weight) in terms of polystyrene in gel permeation chromatography (GPC) analysis using toluene or the like as a developing solvent.

[0019] In addition, in formula (2), m represents the number of branched chains and is an integer from 1 to 10, preferably an integer from 1 to 5, and more preferably an integer from 1 to 3. In formula (2), the repeating units may be bonded randomly.

[0020] In addition, in the general formula (3), X is an oxygen atom or an alkylene group having 2 to 5 carbon atoms, and examples of the alkylene group having 2 to 5 carbon atoms include an ethylene group, a propylene group, a butylene group, etc. Among these, an oxygen atom or an ethylene group is preferable as X. k is independently 0 or 1 for each silicon atom to which it is bonded.

[0021] The organopolysiloxanes of components (A) and (A') preferably have a viscosity at 23°C of 20 to 1,000,000 mPa·s, more preferably 100 to 300,000 mPa·s, even more preferably 1,000 to 200,000 mPa·s, and particularly preferably 10,000 to 100,000 mPa·s. If the viscosity of the organopolysiloxane is less than the lower limit (20 mPa·s), a large amount of component (B), which will be described later, is required, which is economically disadvantageous. If the viscosity of the organopolysiloxane exceeds the upper limit (1,000,000 mPa·s), workability decreases, which is not preferable.

[0022] The organopolysiloxanes of components (A) and (A') may each be used alone or in combination of two or more kinds. Furthermore, the organopolysiloxanes of components (A) and (A') may be the same or different.

[0023] [Component (B): Hydrolyzable organosilane compound and / or partial hydrolysis condensate thereof] The component (B) used in the two-component, room-temperature-curable organopolysiloxane composition of the present invention is a hydrolyzable organosilane compound represented by the following general formula (4) and / or a partial hydrolysis condensate thereof, which is used as a crosslinking agent (curing agent) and is characterized in that it releases a cyclic ketone compound such as cyclobutanone or cyclopentanone as a leaving group (leaving substance) upon hydrolysis. The cyclic ketone compound, which is the leaving group (leaving substance), reacts with the curing accelerator (D) described below to generate water, thereby imparting fast curing properties and deep curing properties to the two-component, room-temperature-curable organopolysiloxane composition. In the present invention, the term "partial hydrolysis condensate" refers to an organosiloxane oligomer having 3 or more, preferably 4 or more, residual hydrolyzable groups in the molecule, which is produced by partial hydrolysis and condensation of the hydrolyzable organosilane compound.

[0024] [ka] (In the formula, R 1 is a monovalent hydrocarbon group having 1 to 10 carbon atoms, a is an integer from 1 to 8, and b is 3 or 4.

[0025] In the above general formula (4), R 1 is a monovalent hydrocarbon group having 1 to 10 carbon atoms, preferably 1 to 6 carbon atoms, and more preferably an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an aryl group having 6 to 10 carbon atoms, or an aralkyl group having 7 to 10 carbon atoms; 1 Examples of the alkyl group include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, pentyl, hexyl, octyl, 2-ethylhexyl, nonyl, and decyl, alkenyl groups such as vinyl, allyl, propenyl, isopropenyl, butenyl, and hexenyl, aryl groups such as phenyl and tolyl, and aralkyl groups such as benzyl and phenylethyl. Among these, methyl, ethyl, vinyl, and phenyl groups are preferred, and methyl, vinyl, and phenyl groups are particularly preferred.

[0026] In the above general formula (4), a is an integer of 1 to 8, preferably an integer of 2 to 6, more preferably an integer of 2 to 4, and even more preferably 2 or 3. When a is 0, a cyclic structure is not formed. When a is an integer of 9 or more, the molecular weight of the hydrolyzable organosilane compound becomes large, making purification by distillation difficult and increasing the amount added to ensure storage stability, which is disadvantageous in terms of cost.

[0027] As mentioned above, b is 3 or 4. If this number is less than 3, rubber hardening by crosslinking reaction does not occur, and the compound is unsuitable as a crosslinking agent for two-component room temperature fast curing organopolysiloxane compositions.

[0028] In addition, the leaving group (leaving compound) generated by hydrolysis of the hydrolyzable organosilane compound represented by the above general formula (4) is a cyclic ketone compound such as cyclopropanone, cyclobutanone, cyclopentanone, cyclohexanone, cycloheptanone, cyclooctanone, cyclononanone, cyclodecanone, etc., preferably cyclobutanone and cyclopentanone, more preferably cyclopentanone. There are no reports of cyclobutanone and cyclopentanone being harmful to human health, such as carcinogenicity or reproductive toxicity, or environmentally harmful, such as toxicity to aquatic organisms. In addition, cyclopentanone is mass-produced industrially, is easily available, and is highly cost-competitive, so it is also advantageous for producing the hydrolyzable organosilane compound of the component (B), as described below.

[0029] The hydrolyzable organosilane compound of component (B) can be produced, for example, by reacting a chlorosilane compound corresponding to the product hydrolyzable organosilane compound represented by general formula (4) with a cyclic ketone compound in the presence of a catalyst and a basic substance (e.g., dehydrochlorination reaction). The reaction formula is, for example, represented by the following formula [1].

[0030] [ka] (In the formula, R 1 , a, and b are as defined above.)

[0031] Examples of the chlorosilane compound include the following. [ka]

[0032] Examples of the cyclic ketone compound include the following. [ka]

[0033] The amount of the cyclic ketone compound to be reacted with the chlorosilane compound is preferably 0.95 to 3.0 mol, more preferably 0.99 to 2.5 mol, and even more preferably 1.0 to 2.0 mol, per mol of chlorine atoms in the chlorosilane compound. If the amount of the cyclic ketone compound is too small, the reaction may not be completed, whereas if the amount of the cyclic ketone compound is too large, purification may take a long time, resulting in an increase in production time.

[0034] The catalyst used in the reaction includes monovalent or divalent metallic copper compounds, such as, but not limited to, copper chloride, copper bromide, copper iodide, copper sulfate, copper nitrate, copper carbonate, basic copper carbonate, copper formate, copper acetate, and copper butyrate. The amount of catalyst (metallic copper compound) added is preferably 0.001 to 0.5 mol, more preferably 0.002 to 0.2 mol, and even more preferably 0.003 to 0.1 mol, per mol of chlorosilane. If the amount of catalyst added is too small, the reaction may not be completed, whereas if the amount of catalyst added is too large, it is disadvantageous in terms of cost.

[0035] The basic substance used in the reaction may be a basic substance having low nucleophilicity, such as trimethylamine, triethylamine, tripropylamine, tributylamine, urea, diazabicycloundecene, diazabicyclononene, etc. Among these, trimethylamine, triethylamine, and tributylamine are preferred, and triethylamine is particularly preferred. The amount of the basic substance added is preferably 0.95 to 2.5 mol, more preferably 0.99 to 2.0 mol, and even more preferably 1.0 to 1.5 mol, per mol of chlorine atoms in the chlorosilane. If the amount of the basic substance added is too small, the reaction may not be completed, whereas if the amount of the basic substance added is too large, it is economically disadvantageous.

[0036] A commonly used solvent may be used in the production of the hydrolyzable organosilane compound of component (B). Examples of the solvent include organic solvents such as aromatic hydrocarbons, such as toluene, xylene, and benzene; aliphatic hydrocarbons, such as pentane, hexane, heptane, nonane, octane, and decane; ethers, such as dimethyl ether, methyl ethyl ether, tetrahydrofuran, and dioxane; halogenated hydrocarbons, such as perchloroethane, perchloroethylene, trichloroethane, chloroform, and carbon tetrachloride; amides, such as dimethylformamide; and esters, such as ethyl acetate, methyl acetate, and butyl acetate. The amount of the solvent used is not particularly limited, but is usually in the range of 10 to 500 parts by mass, preferably 30 to 400 parts by mass, and more preferably 50 to 300 parts by mass, per 100 parts by mass of the cyclic ketone compound used.

[0037] The reaction conditions of the chlorosilane compound and the cyclic ketone compound are usually 0 to 120°C, preferably 0 to 100°C, at which the cyclic ketone compound is dropped into the chlorosilane, and the reaction is carried out at 50 to 120°C, preferably 60 to 100°C, for 1 to 48 hours, more preferably 3 to 30 hours. If the reaction temperature is too low, the reaction may not be completed, and if the reaction temperature is too high, the product may become significantly colored. If the reaction time is too short, the reaction may not be completed, and if the reaction time is too long, the reaction may be disadvantageous to productivity. After the reaction is complete, the product can be purified by distillation under reduced pressure. The degree of reduction is preferably 1×10 -5 ~3,000 Pa, more preferably 1×10 -5 The pressure during the purification is preferably 100 to 250° C., and more preferably 120 to 230° C. If the pressure during the purification (degree of reduction in pressure) is too high, distillation may become difficult. If the temperature during the purification is too low, purification by distillation may become difficult, and if it is too high, coloration or decomposition of the reaction product may occur.

[0038] Specific examples of the hydrolyzable organosilane compound of component (B) include those represented by the following formula: In this case, Me represents a methyl group. [ka]

[0039] The hydrolyzable organosilane compound and / or partial hydrolysis condensate thereof as the component (B) may use either a single compound or a combination of two or more different compounds. Component (B) is blended in the first agent in an amount of 0.1 to 30 parts by mass, and preferably 0.5 to 25 parts by mass, per 100 parts by mass of components (A) and (A') combined. If the blending amount of component (B) is too small, sufficient crosslinking is not obtained when the composition is cured, whereas if the blending amount is too large, the mechanical properties (rubber physical properties) of the resulting cured product (silicone rubber) will decrease, which may be economically disadvantageous.

[0040] [Component (C): Curing catalyst] The curing catalyst of component (C) is used to accelerate the hydrolysis and condensation reaction and is generally called a curing catalyst. Any known catalyst that is commonly used in room temperature curable silicone resin compositions that cure in the presence of moisture can be used.

[0041] Of the curing catalysts of component (C), the non-metallic organic catalyst is not particularly limited, but any known curing accelerator for condensation curing organopolysiloxane compositions can be used. Examples include phosphazene-containing compounds such as N,N,N',N',N'',N''-hexamethyl-N'''-(trimethylsilylmethyl)-phosphorimidic triamide; quaternary ammonium salts such as benzyltriethylammonium acetate; dialkylhydroxylamines such as dimethylhydroxylamine and diethylhydroxylamine; silanes and siloxanes containing guanidyl groups such as γ-(N,N,N',N'-tetramethylguanidyl)propyltrimethoxysilane, γ-(N,N,N',N'-tetramethylguanidyl)propylmethyldimethoxysilane, and γ-(N,N,N',N'-tetramethylguanidyl)propyltris(trimethylsiloxy)silane. The non-metallic organic catalysts may be used alone or in combination of two or more.

[0042] Among the curing catalysts of component (C), the metal catalyst is not particularly limited, but those known as curing catalysts for condensation curing organopolysiloxanes can be used. For example, alkyltin ester compounds such as dibutyltin diacetate, dibutyltin dilaurate, dibutyltin dioctoate, dimethyltin dineodecanoate, dioctyltin dineodecanoate, and di-n-butyl-dimethoxytin; titanate esters or titanium chelate compounds such as tetraisopropoxytitanium, tetra-n-butoxytitanium, tetrakis(2-ethylhexoxy)titanium, dipropoxybis(acetylacetonato)titanium, and titanium isopropoxyoctylene glycol; zinc naphthenate, zinc stearate, and zinc-2-ethyloctoate; aluminum isopropylate, aluminum Examples of suitable metal catalysts include alcoholate aluminum compounds such as aluminum alkyl acetate diisopropylate and aluminum bisethylacetoacetate monoacetylacetonate; organometallic compounds such as bismuth neodecanoate (III), bismuth 2-ethylhexanoate (III), bismuth citrate (III), bismuth octylate, iron 2-ethylhexoate, cobalt 2-ethylhexoate, manganese 2-ethylhexoate, and cobalt naphthenate; and lower fatty acid salts of alkali metals such as potassium acetate, sodium acetate, and lithium oxalate. Metal catalysts are not limited to these. Metal catalysts may be used alone or in combination of two or more.

[0043] The (C) component is blended in the first agent, and its blending amount is 0.001 to 10 parts by mass, preferably 0.005 to 8 parts by mass, and more preferably 0.01 to 5 parts by mass, per 100 parts by mass of the total of the (A) and (A') components. If the amount is less than 0.001 part by mass, good curing properties cannot be obtained, resulting in a problem of a slow curing speed. Conversely, if the amount exceeds 10 parts by mass, the composition cures too quickly, shortening the allowable range of working time after application of the composition and deteriorating the mechanical properties (rubber physical properties) of the resulting cured product (silicone rubber).

[0044] [Component (D): Curing accelerator] Component (D) is an amine compound having a primary amino group (i.e., an amino group having an -NH2 structure, excluding guanidyl groups) and reacts with a cyclic ketone compound produced by hydrolysis of component (B) to produce water, thereby significantly improving the deep curing properties of the composition. The component (D) is not particularly limited as long as it has a primary amino group, but specific examples include aliphatic amines such as methylamine, ethylamine, butylamine, pentylamine, hexylamine, heptylamine, octylamine, nonylamine, and dodecylamine; aliphatic polyamines such as ethylenediamine and triethylenetetramine; aromatic amines such as aniline; cyclic amines such as cyclopentylamine, cyclohexylamine, and 2-ethylcyclohexylamine; primary amino group-containing silane coupling agents such as aminosilanes such as γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, and 3-2-(aminoethylamino)propyltrimethoxysilane [also known as N-2-(aminoethyl)-3-aminopropyltrimethoxysilane]; and primary amino group-containing organosilicon compounds such as primary amino group-containing polysiloxanes. These may be used alone or in combination of two or more.

[0045] When the (D) component is blended, it may be blended in the first agent, the second agent, or both, and the blending amount is preferably 0 to 20 parts by mass in each of the first agent and the second agent relative to 100 parts by mass of the total of the (A) and (A') components (however, at least 0.1 parts by mass or more is contained in either the first agent or the second agent), and more preferably 0 to 10 parts by mass (however, at least 0.1 parts by mass or more is contained in either the first agent or the second agent). That is, when the (D) component is blended, the total blending amount in the composition is preferably 0.1 to 20 parts by mass, particularly 0.5 to 10 parts by mass, relative to 100 parts by mass of the total of the (A) and (A') components. When the (D) component is added in an amount of less than 0.1 parts by mass, the amount of water generated by reaction with the cyclic ketone compound generated by hydrolysis of the (B) component is small, and sufficient deep curing is not expressed, and when it exceeds 20 parts by mass, it is disadvantageous in terms of the characteristics and storage stability of the obtained cured product.

[0046] [Component (E): Inorganic filler] The two-component room temperature fast-curing organopolysiloxane composition of the present invention may optionally contain an inorganic filler (E) as required. The inorganic filler (E) is a reinforcing or non-reinforcing filler for imparting rubber properties to the two-component room temperature fast-curing organopolysiloxane composition of the present invention. Examples of the inorganic filler (E) include silica-based fillers such as dry silica such as calcined silica and fumed silica, wet silica such as precipitated silica and sol-gel silica, which have been surface-treated or not to be hydrophobized, carbon black, talc, bentonite, calcium carbonate, zinc carbonate, magnesium carbonate, calcium oxide, zinc oxide, magnesium oxide, aluminum oxide, aluminum hydroxide, which have been surface-treated or not to be treated, and among these, calcium carbonate, fumed silica, precipitated silica, carbon black, and aluminum oxide are preferred, and more preferred are calcium carbonate, fumed silica, precipitated silica, carbon black, and aluminum oxide, which have been surface-treated or not to be hydrophobized. In this case, it is preferable that the inorganic filler has a small water content. There are no particular limitations on the type, amount, treatment method, etc. of the surface treatment agent (hydrophobic treatment agent). Representative examples of the surface treatment agent that can be used include organosilicon compounds such as chlorosilanes, alkoxysilanes, and organosilazanes, fatty acids, paraffins, silane coupling agents, and titanium coupling agents. The inorganic filler of component (E) may use one type alone, or two or more types in combination.

[0047] When the (E) component is blended, it may be blended in the first agent, the second agent, or both, and the blending amount is preferably 0 to 1,000 parts by mass in each of the first agent and the second agent (provided that at least 0.1 parts by mass or more is contained in at least one of the first agent and the second agent) relative to 100 parts by mass of the total of the (A) and (A') components, and more preferably 0 to 500 parts by mass (provided that at least 0.1 parts by mass or more is contained in at least one of the first agent and the second agent). That is, when the (E) component is blended, the total blending amount in the composition is preferably 0.1 to 1,000 parts by mass, particularly 1 to 500 parts by mass, relative to 100 parts by mass of the total of the (A) and (A') components. If more than 1,000 parts by mass is used, not only does the viscosity of the composition increase, resulting in poor workability, but the rubber strength after curing decreases, making it difficult to obtain rubber elasticity.

[0048] [Component (F): Adhesion promoter] Component (F) is an adhesion promoter, which is an optional component that can be added as needed, and is used to impart sufficient adhesion to the cured product formed from the two-component room temperature curable organopolysiloxane composition of the present invention. As the adhesion promoter, a known one is suitably used, and examples thereof include silane coupling agents such as functional group-containing hydrolyzable silanes (excluding aminosilanes having a primary amino group described in the above component (B) and curing accelerator (D)), specifically, vinyl silane coupling agents, (meth)acrylic silane coupling agents, epoxy silane coupling agents, mercapto silane coupling agents, isocyanate silane coupling agents, etc., specifically, vinyl tris(β-methoxyethoxy)silane, γ-acryloxypropyl trimethoxysilane, γ-methacryloxypropyl trimethoxysilane, β-(3,4-epoxycyclohexyl)ethyl trimethoxysilane, γ-glycidoxypropyl trimethoxysilane, γ-glycidoxypropyl methyl diethoxysilane, γ-mercaptopropyl trimethoxysilane, 3-isocyanate propyl triethoxysilane, etc. Among these, particularly preferred are (meth)acrylic silanes such as γ-methacryloxypropyltrimethoxysilane and γ-acryloxypropyltrimethoxysilane, epoxy silanes such as γ-glycidoxypropyltrimethoxysilane and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and isocyanate silanes such as 3-isocyanatepropyltriethoxysilane.

[0049] When the (F) component is blended, it may be blended in the first agent, the second agent, or both, and the blending amount is preferably 0 to 10 parts by mass in each of the first agent and the second agent relative to 100 parts by mass of the total of the (A) and (A') components (however, at least one of the first agent and the second agent contains 0.001 parts by mass or more), and particularly preferably 0.1 to 10 parts by mass. That is, when the (F) component is blended, the total blending amount in the composition is preferably 0.001 to 10 parts by mass, particularly preferably 0.1 to 10 parts by mass, relative to 100 parts by mass of the total of the (A) and (A') components. When the adhesion promoter is not used depending on the inorganic filler and the adherend, it is not necessary to use the adhesion promoter.

[0050] [Other ingredients] The two-component room temperature fast-curing organopolysiloxane composition of the present invention preferably contains components (A), (A'), (B), and (C) as essential components, and further contains components (D), (E), and (F). In addition, known additives such as pigments, dyes, antioxidants, antioxidants, antistatic agents, antimony oxide, and flame retardants such as chlorinated paraffin can be added. Polyethers as thixotropy improvers, fungicides, and antibacterial agents can also be added.

[0051] In addition, the two-component room temperature fast curing organopolysiloxane composition of the present invention may contain an organic solvent as necessary. Examples of the organic solvent include aliphatic hydrocarbon compounds such as n-hexane, n-heptane, isooctane, and isododecane; aromatic hydrocarbon compounds such as toluene and xylene; linear siloxanes such as hexamethyldisiloxane, octamethyltrisiloxane, decamethyltetrasiloxane, dodecamethylpentasiloxane, and 2-(trimethylsiloxy)-1,1,1,2,3,3,3-heptamethyltrisiloxane; and cyclic siloxanes such as octamethylcyclopentasiloxane and decamethylcyclopentasiloxane. The amount of the organic solvent may be appropriately adjusted within a range that does not impede the effects of the present invention.

[0052] [Preparation of two-component room temperature fast curing organopolysiloxane composition] The two-component room temperature fast-curing organopolysiloxane composition of the present invention comprises a first part containing components (A), (B), and (C), and a second part containing component (A') but not components (B) or (C). By forming the composition into a two-component composition consisting of the first part and second part, the composition has excellent fast-curing properties and deep curing properties. This is presumably due to a direct hydrolysis / condensation reaction (crosslinking reaction) occurring when the first and second agents are mixed together between the hydrolyzable silyl groups in the organopolysiloxane of a specific structure in which the molecular chain ends of component (A), the base polymer in the first agent, are blocked with hydrolyzable silyl groups, or between the hydrolyzable silyl groups in the organopolysiloxane in which the molecular chain ends are blocked with hydrolyzable silyl groups, which is produced by coexisting the organopolysiloxane in which the molecular chain ends of component (A) are blocked with silanol groups and the specific hydrolyzable silane compound in component (B), with the curing catalyst in component (C), and the silanol groups in the organopolysiloxane in which the molecular chain ends of component (A'), the base polymer in the second agent, are blocked with silanol groups.

[0053] The first agent can be prepared by mixing all of the components (A), (B), and (C) and, if necessary, some or all of the components (D), (E), and (F) and other components in a conventional manner. The second agent can be prepared by mixing all of the component (A') and, if necessary, the remainder or all of the components (D), (E), and (F) and other components in a conventional manner.

[0054] In the base polymers, component (A) and component (A'), component (A) is blended into the first agent and component (A') is blended into the second agent. 10 to 90 parts by mass, particularly 30 to 70 parts by mass of component (A) is blended into the first agent, and 10 to 90 parts by mass, particularly 30 to 70 parts by mass of component (A') is blended into the second agent (however, the total of components (A) and (A') is 100 parts by mass). In addition, the optional components (D), (E), (F) and other components may be blended into either the first agent or the second agent, or into one or both. However, it is particularly preferable to blend the (D), (E), and (F) components into the first agent and the (D) and (E) components into the second agent. When the (D) component is blended into the first and second agents, it is preferable from the viewpoint of the storage stability of the composition to blend the first and second agents in a mass ratio of 1:99 to 99:1, and particularly 30:70 to 70:30. Furthermore, when the (E) component is blended into the first and second agents, the mass ratio of the first and second agents is preferably 80:20 to 20:80, and particularly preferably 60:40 to 40:60, from the viewpoint of uniformity of the composition (ease of mixing) when mixed. The ratio of the first agent to the second agent is preferably 100:10 to 100:100 by mass, particularly 100:25 to 100:100, from the viewpoints of workability and uniformity of the composition (ease of mixing) when the first agent and the second agent are mixed.

[0055] The two-component room temperature curable organopolysiloxane composition of the present invention can be obtained by uniformly mixing the above-mentioned components and the various additives in the prescribed amounts in a dry atmosphere. Furthermore, because the two-component room temperature curable organopolysiloxane composition of the present invention has storage stability, the first and second parts produced as described above can be stored in an atmosphere free from moisture.

[0056] [Method of curing two-component room temperature fast curing organopolysiloxane composition] The two-component room temperature curable organopolysiloxane composition of the present invention is prepared by mixing these components in an appropriate ratio, specifically, the mass ratio of the first component to the second component is 1:1 to 10:1, and particularly 1:1 to 4:1, and generally cures at room temperature in 10 minutes to 5 days. The two-component room temperature fast-curing organopolysiloxane composition of the present invention has fast curing properties; when molded into a sheet of 2 mm thickness at 23°C and 50% RH, the composition normally cures in 3 to 5 days but cures in a short time of 10 minutes to 3 days. Furthermore, the two-component room temperature fast-curing organopolysiloxane composition of the present invention has deep curing properties; when cured in a glass petri dish having an inner diameter of 10 mm and a depth of 20 mm at 23°C and 50% RH, the composition cures deep within a short period of 30 minutes, whereas a composition that would normally cure deep within (to a measurable thickness) takes two hours.

[0057] The two-component room-temperature curable organopolysiloxane composition of the present invention cures when allowed to stand at room temperature. The molding method, curing conditions, and the like can be any known method and condition suited to a variety of applications and purposes, such as for use in electronic components, on-vehicle applications, and construction applications.

[0058] In the two-component room temperature fast curing organopolysiloxane composition of the present invention, the compound generated from the crosslinking agent by the hydrolysis reaction during curing is a highly safe cyclic ketone compound such as cyclobutanone or cyclopentanone, and is therefore considered to be safe for the human body and the environment. Furthermore, cyclopentanone has a flash point of 35°C, which is higher than that of a dealcohol type that releases an alcohol compound such as methanol during curing of the composition, and is therefore highly safe. Such a two-component room temperature fast curing organopolysiloxane composition of the present invention shows good curability by using various existing catalysts, and the cured product (silicone rubber) also has excellent adhesion.

[0059] Therefore, the two-component room-temperature-curable organopolysiloxane composition of the present invention is useful as an adhesive, sealing agent, potting agent, coating agent, etc. The method for using the two-component room-temperature-curable organopolysiloxane composition of the present invention as an adhesive, sealing agent, potting agent, or coating agent may follow a conventionally known method.

[0060] Examples of target articles include automobile parts, automobile oil seals, electrical and electronic parts, building structures, and civil engineering structures. EXAMPLES

[0061] Synthesis examples, examples and comparative examples are given below to specifically explain the present invention, but the present invention is not limited to the following examples. In the following examples, the viscosity is measured at 23°C using a rotational viscometer in accordance with the method specified in JIS Z 8803.

[0062] [Synthesis Example 1] Synthesis of vinyltris(1-cyclopenten-1-yloxy)silane Cyclopentanone 834g (9.9mol), triethylamine 825g (8.2mol), copper(I) chloride 5g (0.05mol), and hexane 1,500ml were charged into a 5,000mL four-necked separable flask equipped with a mechanical stirrer, a thermometer, a reflux condenser, and a dropping funnel, and vinyltrichlorosilane 400g (2.47mol) was added dropwise over about 2 hours at 40-60℃. After stirring at 80℃ for 12 hours, the triethylamine hydrochloride formed was removed by filtration, and hexane was distilled from the filtrate at 100℃ and normal pressure, and then vinyltris(1-cyclopenten-1-yloxy)silane was obtained by distillation at 180℃ and 300Pa (yield 532g, 69%). This reaction formula is represented by the following formula [2]. [ka]

[0063] [Example 1] Preparation of first agent a (Component (A)) 50 parts by mass of dimethylpolysiloxane having a viscosity of 20,000 mPa s at 23°C and both ends of the molecular chain blocked with silanol groups (hydroxyl groups bonded to silicon atoms), and (Component (E)) a dimethylpolysiloxane having a BET specific surface area of ​​130 m 2 The first agent a was prepared by uniformly mixing under reduced pressure 5 parts by mass of fumed silica (fumed silica) surface-treated with dimethyldichlorosilane (1.0 g / g), 3.5 parts by mass of vinyltris(1-cyclopenten-1-yloxy)silane (component (B)), 0.4 parts by mass of γ-(N,N,N',N'-tetramethylguanidyl)propyltrimethoxysilane (component (C)), and 0.5 parts by mass of γ-aminopropyltrimethoxysilane (component (D)).

[0064] Preparation of second agent a (Component (A')) 50 parts by mass of dimethylpolysiloxane having a viscosity of 20,000 mPa s at 23°C and both ends of the molecular chain are blocked with silanol groups (hydroxyl groups bonded to silicon atoms); (Component (E)) a dimethylpolysiloxane having a BET specific surface area of ​​130 m 2The second agent a was prepared by uniformly mixing 5 parts by mass of fumed silica (fumed silica) having a surface treated with dimethyldichlorosilane (having a molecular weight of 1.0 to 1.2 g) at 200 nm under reduced pressure.

[0065] The first agent a and the second agent a were uniformly mixed at a mixing ratio (mass ratio) of 1:1 to produce composition 1. Composition 1 was left to stand for 1 day and 3 days, respectively, under conditions of 23°C and 50% RH to cure, and these were designated as cured products 1-1 and 1-2.

[0066] [Example 2] Preparation of second agent b (Component (A')) 50 parts by mass of dimethylpolysiloxane having a viscosity of 20,000 mPa s at 23°C and both ends of the molecular chain are blocked with silanol groups (hydroxyl groups bonded to silicon atoms); (Component (E)) a dimethylpolysiloxane having a BET specific surface area of ​​130 m 2 A second agent b was prepared by uniformly mixing 5 parts by mass of fumed silica (fumed silica) having a surface treated with dimethyldichlorosilane (having a molecular weight of 1.0 to 1.2 g) and 2 parts by mass of octylamine (component (D)) under reduced pressure.

[0067] The first agent a prepared in Example 1 and the second agent b described above were uniformly mixed at a mixing ratio (mass ratio) of 1:1 to produce composition 2. Furthermore, composition 2 was left to stand under conditions of 23°C and 50% RH for 1 day and 3 days, respectively, to cure, to give cured products 2-1 and 2-2.

[0068] [Example 3] Preparation of first agent b (Component (A)) 50 parts by mass of dimethylpolysiloxane having a viscosity of 20,000 mPa s at 23°C and both ends of the molecular chain blocked with silanol groups (hydroxyl groups bonded to silicon atoms), and (Component (E)) a dimethylpolysiloxane having a BET specific surface area of ​​130 m 2A first agent b was prepared by uniformly mixing under reduced pressure 5 parts by mass of fumed silica (fumed silica) surface-treated with dimethyldichlorosilane (component (B)), 3.5 parts by mass of vinyltris(1-cyclopenten-1-yloxy)silane (component (C)), 0.4 parts by mass of γ-tetramethylguanidylpropyltrimethoxysilane (component (D)), 0.5 parts by mass of γ-aminopropyltrimethoxysilane (component (D)), and 0.5 parts by mass of γ-glycidoxypropyltrimethoxysilane (component (F)).

[0069] The first agent b and the second agent b prepared in Example 2 were uniformly mixed at a mixing ratio (mass ratio) of 1:1 to produce composition 3. Furthermore, composition 3 was left to stand for 1 day and 3 days, respectively, under conditions of 23°C and 50% RH to cure, and these were designated as cured products 3-1 and 3-2.

[0070] [Comparative Example 1] Preparation of first agent c (Component (A)) 50 parts by mass of dimethylpolysiloxane having a viscosity of 20,000 mPa s at 23°C and both ends of the molecular chain blocked with silanol groups (hydroxyl groups bonded to silicon atoms), and (Component (E)) a dimethylpolysiloxane having a BET specific surface area of ​​130 m 2 A first agent c was prepared by uniformly mixing under reduced pressure 5 parts by mass of fumed silica (fumed silica) surface-treated with dimethyldichlorosilane (1.0 g / g), 2.5 parts by mass of vinyltrimethoxysilane, 0.05 parts by mass of dioctyltin dilaurate (component (C)), 0.5 parts by mass of γ-aminopropyltrimethoxysilane (component (D)), and 0.5 parts by mass of γ-glycidoxypropyltrimethoxysilane (component (F)).

[0071] The first agent c and the second agent b prepared in Example 2 were uniformly mixed at a mixing ratio (mass ratio) of 1:1 to produce composition 4. Furthermore, composition 4 was left to stand for 1 day and 3 days, respectively, under conditions of 23°C and 50% RH to cure, and these were designated as cured products 4-1 and 4-2.

[0072] [Comparative Example 2] Preparation of first agent d (Component (A)) 50 parts by mass of dimethylpolysiloxane having a viscosity of 20,000 mPa s at 23°C and both ends of the molecular chain blocked with silanol groups (hydroxyl groups bonded to silicon atoms), and (Component (E)) a dimethylpolysiloxane having a BET specific surface area of ​​130 m 2 A first agent d was prepared by uniformly mixing under reduced pressure 5 parts by mass of fumed silica (fumed silica) surface-treated with dimethyldichlorosilane (1.0 g / g), 3.5 parts by mass of vinyltris(methylethylketoxime)silane, 0.05 parts by mass of dioctyltin dilaurate (component (C)), 0.5 parts by mass of γ-aminopropyltrimethoxysilane (component (D)), and 0.5 parts by mass of γ-glycidoxypropyltrimethoxysilane (component (F)).

[0073] The first agent d and the second agent b prepared in Example 2 were uniformly mixed at a mixing ratio (mass ratio) of 1:1 to produce composition 5. Furthermore, composition 5 was left to stand for 1 day and 3 days, respectively, under conditions of 23°C and 50% RH to cure, and these were designated as cured products 5-1 and 5-2.

[0074] [Test Method] The compositions prepared in Examples 1 to 3 and Comparative Examples 1 and 2 were used to evaluate the curability, rubber properties, and adhesion by the methods described below.

[0075] [Curability] Tuck Free Time: Using each of the compositions prepared in Examples 1 to 3 and Comparative Examples 1 and 2, the tack-free time (touch-dry time) was measured according to the method specified in JIS A-5758.

[0076] Deep hardening: Each composition prepared in Examples 1 to 3 and Comparative Examples 1 and 2 was filled into a glass petri dish having an inner diameter of 10 mm and a depth of 20 mm, and after 20 minutes at 23°C and 50% RH, the thickness from the surface exposed to air to the hardened part was measured to evaluate deep curability.

[0077] Initial sealability: To compare the curing properties, the initial sealability was measured. The initial sealability was tested by using a pressure vessel similar to the flange pressure vessel for pressure test specified in JIS K-6820 as a test device and performing a pressure test. The pressure vessel was composed of an upper vessel having an upper flange with an inner diameter of 58 mm, an outer diameter of 80 mm, and a thickness of 10 mm, and a lower vessel having a lower flange with the same dimensions as the upper flange, and a ring-shaped notch with a width of 3 mm and a depth of 3 mm was provided along the circumference at the inner side edge of the seal surface of the lower flange. The seal surface of this lower flange was washed with toluene. Then, the composition was applied in a bead shape to the center of the lower seal surface in an amount sufficient to fully fill the seal surface. Immediately after application, the upper vessel was placed on the lower vessel so that the seal surfaces of the upper and lower flanges were in contact with each other, and an iron spacer with a height of 21 mm (in the thickness direction of the flange) was installed to define the distance between the seal surfaces of the upper and lower flanges, and four tightening bolts were installed. The spacer creates a gap of 1 mm between the sealing surfaces, which is intended to make the pressure resistance test for the sealant more severe, i.e., to make it an accelerated test. After curing for 30 minutes at 23°C and 50% RH, gas was introduced from the upper pressure port to measure the gas pressure that the sealant, which is the cured product of the composition, could withstand. Those with a pressure of 400 kPa or more were judged to pass.

[0078] [Rubber properties] Immediately after preparation, each composition prepared in Examples 1 to 3 and Comparative Examples 1 and 2 was extruded into a sheet having a thickness of 2 mm and exposed to air at 23°C and 50% RH, and the sheet was then left in the same atmosphere for 1 or 3 days to obtain a cured product, whose rubber properties (hardness, elongation at break, tensile strength) were measured in accordance with JIS K-6249. The hardness was measured using a JIS K-6249 durometer A hardness tester.

[0079] [Adhesiveness] The compositions prepared in Examples 1 to 3 and Comparative Examples 1 and 2 were used to bond aluminum or glass specimens measuring 25 mm in width and 100 mm in length to each other, and the adhesive bonded the specimens to each other with the same adhesive. 2Shear adhesion test specimens were prepared with a bond thickness of 1 mm and aged at 23°C and 50% RH for one or three days. After this, the shear adhesive strength of these test specimens to aluminum or glass was measured in accordance with the method specified in JIS K-6249.

[0080] The test results of Examples 1 to 3 are shown in Table 1, and the test results of Comparative Examples 1 and 2 are shown in Table 2. Tables 1 and 2 also show the compounds that are released from the curing agent during curing, and whether or not the compounds are harmful to health and the environment.

[0081] [Table 1]

[0082] [Table 2]

[0083] From the above results, it can be seen that the two-component, room temperature fast-curing organopolysiloxane compositions of the present invention (the compositions of Examples 1 to 3) exhibit high values ​​for deep curing ability and initial sealability, and there is little difference in the rubber properties and adhesive strength between the one-day and three-day cure periods, thereby having high curing ability compared to the conventional dealcohol-free (composition of Comparative Example 1) and oxime-free (composition of Comparative Example 2) cure forms. The compound released during curing from the compositions of the examples is cyclopentanone, a highly safe compound with no reported health hazards, such as carcinogenicity or reproductive toxicity, to the human body, or environmental hazards, such as toxicity to aquatic organisms. On the other hand, the compounds released during curing from the compositions of the comparative examples are all designated as hazardous substances, and are highly harmful to the human body, and are 2-butanone oxime, which may be carcinogenic and is toxic to aquatic organisms, and their health hazards are indicated in SDS (Safety Data Sheet) or the like. Methanol has a lower flash point and boiling point than cyclopentanone, and therefore the two-component room temperature fast curing organopolysiloxane composition of the present invention is superior in terms of human health and safety and environmental protection.

Claims

1. (A) an organopolysiloxane represented by the following general formula (1), (2), or (3): 10 to 90 parts by mass (provided that the total of components (A) and (A′) is 100 parts by mass); [Formula 1] (In the formula, R is the same or different, and is an unsubstituted or halogen-substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and n is an integer from 5 to 2,000.) [Case 2] (In the formula, R and n are as defined above, and n may be the same or different. m is an integer of 1 to 10.) [C3] (In the formula, R and n are as defined above, X is an oxygen atom or an alkylene group having 2 to 5 carbon atoms, and k is independently 0 or 1 for each silicon atom to which it is bonded.) (B) a hydrolyzable organosilane compound represented by the following general formula (4) and / or a partial hydrolysis condensate thereof: 0.1 to 30 parts by mass per 100 parts by mass of the total of the components (A) and (A′), [C4] (In the formula, R 1 is a monovalent hydrocarbon group having 1 to 10 carbon atoms, a is an integer from 1 to 8, and b is 3 or 4; and (C) Curing catalyst: 0.001 to 10 parts by mass per 100 parts by mass of the total of the components (A) and (A'). A first agent comprising (A') an organopolysiloxane represented by the following general formula (1) or (2): 10 to 90 parts by mass (the total of components (A) and (A') is 100 parts by mass); [C5] (In the formula, R is the same or different, and is an unsubstituted or halogen-substituted monovalent hydrocarbon group having 1 to 10 carbon atoms, and n is an integer from 5 to 2,000.) [C6] (In the formula, R and n are as defined above, n may be the same or different, and m is an integer of 1 to 10.) and further comprising 0 to 20 parts by mass of an amine compound having a primary amino group as a curing accelerator in each of the first and second agents, relative to 100 parts by mass of the total of the components (A) and (A') (with the proviso that at least one of the first and second agents contains 0.1 part by mass or more).

2. 2. The two-component room temperature fast-curing organopolysiloxane composition according to claim 1, wherein the hydrolyzable organosilane compound and / or partial hydrolysis condensate thereof, component (B), is a compound that releases a cyclic ketone compound upon hydrolysis.

3. 3. The two-component room temperature fast-curing organopolysiloxane composition according to claim 2, wherein the cyclic ketone compound which is eliminated is cyclobutanone or cyclopentanone.

4. The two-component room-temperature fast-curing organopolysiloxane composition according to any one of claims 1 to 3, further comprising 0 to 1,000 parts by mass of an inorganic filler (E) in each of the first and second agents, relative to 100 parts by mass of the total of the components (A) and (A') (with the proviso that at least 0.1 part by mass or more is contained in at least one of the first and second agents).

5. 5. The two-component room temperature fast-curing organopolysiloxane composition according to claim 4, wherein component (E) is one or more inorganic fillers selected from the group consisting of calcium carbonate, fumed silica, precipitated silica, carbon black, and aluminum oxide.

6. The two-component room-temperature fast-curing organopolysiloxane composition according to any one of claims 1 to 5, further comprising 0 to 10 parts by mass of an adhesion promoter (F) in each of the first and second agents, relative to 100 parts by mass of the total of the components (A) and (A') (with the proviso that at least one of the first and second agents contains 0.001 part by mass or more).

7. 7. The two-component room temperature fast-curing organopolysiloxane composition according to any one of claims 1 to 6, wherein the blending ratio of the first agent to the second agent is from 1:1 to 10:1 by mass.

8. 8. An automobile part comprising a cured product of the two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 7.

9. 8. An oil seal for automobiles comprising a cured product of the two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 7.

10. 8. An electric or electronic part comprising a cured product of the two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 7.

11. 8. A building structure comprising a cured product of the two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 7.

12. 8. A civil engineering structure comprising a cured product of the two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 7.

13. An adhesive comprising the two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 7.

14. A sealant comprising the two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 7.

15. A potting agent comprising the two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 7.

16. A coating agent comprising the two-component room temperature fast curing organopolysiloxane composition according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Two-part mixing type organopolysiloxane composition

    JP2011037968A

  • Method for producing room temperature-curable organopolysiloxane composition, sealant, and article

    JP2015113377A

  • Room temperature curing organopolysiloxane composition and production method thereof, and long life coolant sealant for automobile

    JP2019073670A

  • Curable silicone rubber compounds

    JP2020517771A

  • Room-temperature-curing sealant composition for automobiles

    JP3916403B2