Photosensitive resin composition, and photosensitive film, resist pattern forming method, and printed wiring board using the same

The photosensitive resin composition addresses the challenges of heat resistance, thermal expansion, and filler residue by using a specific epoxy resin and inorganic filler, ensuring high durability and reliability in printed wiring boards.

JP7582379B2Active Publication Date: 2024-11-13RESONAC CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023092165
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-06-05
Publication Date
2024-11-13
Estimated Expiration
2036-09-14

AI Technical Summary

Technical Problem

Existing photosensitive resin compositions for printed wiring boards face challenges in achieving high heat resistance, low thermal expansion, good electrical reliability, and effective filler residue removal, particularly in high-temperature soldering processes and electroless plating environments, which can lead to poor wiring connections and cracks.

Method used

A photosensitive resin composition comprising an acid-modified vinyl group-containing epoxy resin with a specific molecular dispersity, a photopolymerizable monomer with multiple ethylenically unsaturated bonds, a photopolymerization initiator, and an inorganic filler, optimized to provide high heat resistance, low thermal expansion, and improved filler developability.

Benefits of technology

The composition achieves both high heat resistance and low thermal expansion, ensuring excellent electrical reliability and minimal filler residue, thereby enhancing the durability and performance of printed wiring boards in demanding environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582379000001
    Figure 0007582379000001
  • Figure 0007582379000002
    Figure 0007582379000002
  • Figure 0007582379000003
    Figure 0007582379000003
Patent Text Reader

Abstract

To provide a photosensitive resin composition which has excellent heat resistance and an excellent low thermal expansion coefficient and also achieves good resolution, electrical reliability (HAST resistance) and elimination of a filler residue and to provide a photosensitive film using the same, a method for forming a resist pattern and a printed wiring board.SOLUTION: There is provided a photosensitive resin composition which comprises (A) an acid-modified vinyl group-containing epoxy resin, (B) a photopolymerizable monomer having an ethylenically unsaturated bond, (C) a photopolymerization initiator and (D) an inorganic filler, wherein the acid-modified vinyl group-containing epoxy resin of the component (A) contains a resin (A'') obtained by reacting a resin (A'), which is obtained by reacting at least one epoxy resin (a) selected from the group consisting of a specific novolac type epoxy resin and a bisphenol-type novolac resin having a specific structural unit, and a vinyl group-containing monocarboxylic acid (b) with a saturated or unsaturated group-containing polybasic acid anhydride (provided that a resin has a dispersion degree of 2.0 to 5.0 as represented as Mw / Mn (weight average molecular weight / number average molecular weight) and a resin obtained by reacting an o-cresol novolac resin with acrylic acid, followed by reacting with tetrahydrophthalic anhydride and a resin obtained by reacting an o-cresol novolac resin, acrylic acid and pentaerythritol triacrylate / succinic anhydride adduct, followed by reacting succinic anhydride and tetrahydro phthalic anhydride are excluded), the inorganic filler (D) contains silica and barium sulfate and the content of the inorganic filler (D) is 30 to 70 mass% based on the total solid content.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an alkali-developable photosensitive resin composition for a protective film of a printed wiring board, and more particularly to a photosensitive resin composition for a protective film of a printed wiring board used as a permanent mask resist in the field of resists for semiconductor package substrates, as well as a photosensitive film, a method for forming a resist pattern, and a printed wiring board each using the same. [Background technology]

[0002] In the field of printed wiring boards, a permanent mask resist (protective film) has been formed on a printed wiring board. The photolithography method is the mainstream method for forming a pattern using a photosensitive resist. The photosensitive resin composition is applied to a substrate, dried, and then selectively irradiated with ultraviolet light to cure the composition. Then, only the uncured portion is developed and removed with an alkaline solution to form a pattern. This permanent mask resist has a role of preventing solder from adhering to unnecessary portions of the conductor layer of the printed wiring board, for example, in a process of flip-chip mounting a semiconductor element on a printed wiring board via solder. Furthermore, the permanent mask resist also has a role of preventing corrosion of the conductor layer and maintaining electrical reliability between the conductor layers when the printed wiring board is used.

[0003] Conventionally, permanent mask resists in the manufacture of printed wiring boards have been prepared by screen printing or roll coating a thermosetting or photosensitive resin composition.

[0004] For example, in flexible wiring boards using mounting methods such as FC, TAB, and COF, except for the rigid wiring board, IC chip, electronic components, or LCD panel and the connection wiring pattern portion, a thermosetting resin paste is screen-printed and thermally cured to form a permanent mask resist (see, for example, Patent Document 1).

[0005] In recent years, with the increasing density of wiring patterns, permanent mask resists are required to have high resolution, and photosensitive resin compositions that form patterns by photography have become widely used. Among them, alkaline development types that can be developed with weak alkaline aqueous solutions such as sodium carbonate aqueous solutions have become mainstream in terms of preserving the working environment and the global environment. In addition, with the trend toward miniaturization and high performance of electronic devices, there is a remarkable tendency for the wiring of semiconductor chips to become denser due to narrower pitches, and as a semiconductor mounting method that corresponds to this, the flip chip connection method in which the semiconductor chip and the substrate are joined by solder bumps has become mainstream. This flip chip connection method is a semiconductor mounting method using a reflow method in which solder balls are placed between the substrate and the semiconductor chip and the entire substrate is heated to melt and join them. Therefore, during solder reflow, the substrate itself is exposed to a high temperature environment, and the thermal contraction of the substrate generates large stress in the solder balls that connect the substrate and the semiconductor, which can cause poor connection of the wiring and cracks in the permanent mask resist and underfill. For this reason, insulating materials used in printed wiring boards are required to have a low thermal expansion coefficient.

[0006] As the wiring patterns and insulating patterns (permanent mask resist) on printed wiring boards become increasingly fine, the pitch between the wiring lines becomes finer, which requires excellent electrical reliability between the wiring lines (especially electrical reliability after moisture absorption (HAST (High Accelerated Stress Test) resistance)). In the manufacture of such mask resists, electroless plating methods that do not require lead wires have come to be adopted (for example, Patent Document 2). Electroless plating methods have the advantages of uniform plating thickness and high smoothness. However, the plating solution has a high pH and is strongly alkaline, and the solution temperature is raised to a high temperature of about 90° C. to improve the plating deposition rate, so that the permanent mask resist tends to be significantly damaged. For this reason, there is a demand for the permanent mask resist to be resistant to damage caused by the plating solution used in electroless plating, and further improvement in electroless plating resistance is also required.

[0007] In addition, when the amount of inorganic filler is increased to reduce the thermal expansion coefficient, the filler tends to remain after alkaline development. The occurrence of this filler residue leads to insufficient electrical connection and poor electrical reliability, so improvement of the filler residue is required. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2003-198105 A [Patent Document 2] JP 2006-190848 A Summary of the Invention [Problem to be solved by the invention]

[0009] The present invention provides a photosensitive resin composition that has excellent heat resistance and a low coefficient of thermal expansion, and further realizes good resolution, electrical reliability (HAST resistance), and filler developability, as well as a photosensitive film, a method for forming a resist pattern, and a printed wiring board each using the same. [Means for solving the problem]

[0010] The inventors have conducted extensive research into solder resist properties and compositions that can satisfy these requirements of high heat resistance, low thermal expansion coefficient, good electrical reliability (HAST resistance), good filler developability, and elimination of filler residue. As a result, they have found that a photosensitive resin composition containing (A) an acid-modified vinyl group-containing epoxy resin, (B) a photopolymerizable monomer having an ethylenically unsaturated bond, (C) a photopolymerization initiator, and (D) an inorganic filler can be used, and that the acid-modified vinyl group-containing epoxy resin of component (A) is a specific compound with high heat resistance, and has a polydispersity expressed by Mw / Mn of 2.0 to 5.0, and that the inorganic filler is contained in an amount of 30 to 70 mass %, thereby making it possible to achieve both heat resistance, electrical reliability, and filler developability (elimination of filler residue) without deteriorating the linear thermal expansion coefficient.

[0011] The photosensitive resin composition of the present invention is [1] a photosensitive resin composition comprising (A) an acid-modified vinyl group-containing epoxy resin, (B) a photopolymerizable monomer having an ethylenically unsaturated bond, (C) a photopolymerization initiator, and (D) an inorganic filler, characterized in that the acid-modified vinyl group-containing epoxy resin of component (A) contains a compound represented by general formula (1) or general formula (2) (having a polydispersity represented by Mw / Mn (weight average molecular weight / number average molecular weight) of 2.0 to 5.0), and the content of the inorganic filler (D) is 30 to 70 mass% based on the total solid content.

[0012] [ka] [In general formula (1), R 11 represents a hydrogen atom or a methyl group, and Y 1 represents a hydrogen atom or a glycidyl group, and n1 represents an integer of 1 or more. 11 and Y 1 may be the same or different, provided that at least one Y 1 In the general formula (2), R 12 represents a hydrogen atom or a methyl group, Y 2 Each of R independently represents a hydrogen atom or a glycidyl group. 12 may be the same or different, provided that Y 2 At least one of these represents a glycidyl group.]

[0013] The photosensitive resin composition of the present invention is the photosensitive resin composition according to the above item [1], wherein the photopolymerizable monomer having an ethylenically unsaturated bond (B) is a polyfunctional photopolymerizable monomer having three or more ethylenically unsaturated bonds in one molecule. The photosensitive resin composition of the present invention is the photosensitive resin composition according to the above item [1] or [2], further comprising [3] (E) a pigment.

[0014] The photosensitive film of the present invention includes a support [4] and a photosensitive layer formed from the photosensitive resin composition according to any one of the above [1] to [3]. Further, a method for forming a resist pattern of the present invention is characterized in that a photosensitive layer is laminated on an insulating substrate of a laminate substrate including an insulating substrate and a conductor layer having a circuit pattern formed on the insulating substrate, the photosensitive layer is laminated on the insulating substrate using the photosensitive resin composition described in any one of the above [1] to [3] so as to cover the conductor layer, a predetermined portion of the photosensitive layer is irradiated with active light rays to form an exposed portion, and then a portion of the photosensitive layer other than the exposed portion is removed. The printed wiring board of the present invention includes an insulating substrate, a conductor layer having a circuit pattern formed on the insulating substrate, and a permanent resist layer formed using the photosensitive resin composition according to any one of the above [1] to [3] so as to cover the conductor layer. Effect of the Invention

[0015] According to the present invention, it is possible to provide a photosensitive resin composition for protective films of printed wiring boards that can achieve high heat resistance, resolution, electrical reliability (HAST resistance), and filler developability without deteriorating the linear thermal expansion coefficient, a photosensitive film using the same, a method for forming a resist pattern, and a printed wiring board. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] In the present invention, (meth)acrylic acid refers to acrylic acid or methacrylic acid, (meth)acrylate refers to an acrylate or the corresponding methacrylate, and (meth)acryloyl group refers to an acryloyl group or methacryloyl group. Preferred embodiments of the present invention will now be described in detail. First, a photosensitive resin composition according to a preferred embodiment will be described.

[0017] [(A) Acid-modified vinyl group-containing epoxy resin] The acid-modified vinyl-group-containing epoxy resin (A) used in the present invention (having a dispersity represented by Mw / Mn of 2.0 to 5.0) will be described. The acid-modified vinyl-group-containing epoxy resin (A) used in the present invention has a dispersity represented by Mw / Mn of 2.0 to 5.0. From the viewpoints of alkali developability and excellent resolution and adhesion, it is preferable that the acid-modified vinyl-group-containing epoxy resin (A) is a resin (A″) obtained by reacting at least one epoxy resin (a) selected from the group consisting of novolac epoxy resins represented by the following general formula (1) and bisphenol-type novolac resins having a structural unit represented by the following general formula (2) or (3) with a vinyl-group-containing monocarboxylic acid (b), and then reacting the resulting resin (A′) with a saturated or unsaturated group-containing polybasic acid anhydride.

[0018] [ka] [In general formula (1), R 11 represents a hydrogen atom or a methyl group, Y 1 represents a hydrogen atom or a glycidyl group, and n1 represents an integer of 1 or more. 11 and Y 1 may be the same or different, provided that at least one Y 1 represents a glycidyl group.

[0019] [ka] [In general formula (2), R 12 represents a hydrogen atom or a methyl group, Y 2 Each of R independently represents a hydrogen atom or a glycidyl group. 12 may be the same or different, provided that Y 2 At least one of these represents a glycidyl group.]

[0020] [ka] [In general formula (3), R 13 represents a hydrogen atom or a methyl group, Y 3 Each of R independently represents a hydrogen atom or a glycidyl group.13 may be the same or different, provided that Y 3 At least one of these represents a glycidyl group.]

[0021] Resin (A') obtained by reacting epoxy resin (a) with vinyl group-containing monocarboxylic acid (b) is presumed to have a hydroxyl group formed by an addition reaction between the epoxy group of epoxy resin (a) and the carboxyl group of vinyl group-containing monocarboxylic acid (b).

[0022] Examples of the novolac epoxy resin represented by the general formula (1) include phenol novolac epoxy resin and cresol novolac epoxy resin. These novolac epoxy resins can be obtained, for example, by reacting phenol novolac resin or cresol novolac resin with epichlorohydrin by a known method.

[0023] As the epoxy resin (a), from the viewpoints of excellent process tolerance and improved solvent resistance, a novolac type epoxy resin represented by the general formula (1) is preferred.

[0024] Examples of the phenol novolac type epoxy resin or cresol novolac type epoxy resin represented by the general formula (1) include YDCN-701, YDCN-702, YDCN-703, YDCN-704, YDCN-704L, YDPN-638, YDPN-602 (all of which are trade names manufactured by Nippon Steel & Sumitomo Metal Chemical Co., Ltd.), DEN-431, DEN-439 (all of which are trade names manufactured by Huntsman Corporation), EOCN-120, EOCN-102S, EO CN-103S, EOCN-104S, EOCN-1012, EOCN-1025, EOCN-1027, BREN (all trade names manufactured by Nippon Kayaku Co., Ltd.), EPN-1138, EPN-1235, EPN-1299 (all trade names manufactured by Huntsman Corporation), N-730, N-770, N-865, N-870, N-665, N-673, VH-4150, VH-4240 (all trade names manufactured by DIC Corporation) are commercially available.

[0025] In addition, as the epoxy resin (a), it is preferable to use an epoxy resin having structural units represented by general formula (2) and / or general formula (3), from the viewpoint of further reducing the warpage of the thin film substrate and further improving the thermal shock resistance.

[0026] In the above general formula (3), R 13 is a hydrogen atom, and Y 3 The glycidyl group is the EXA-7376 series (manufactured by DIC Corporation), and R 13 is a methyl group, and Y 3 Those having a glycidyl group are commercially available as the EPON SU8 series (product name, formerly manufactured by Japan Epoxy Resins Co., Ltd.).

[0027] Examples of the vinyl group-containing monocarboxylic acid (b) include acrylic acid, acrylic acid dimers, methacrylic acid, β-furfurylacrylic acid, β-styrylacrylic acid, cinnamic acid, crotonic acid, α-cyanocinnamic acid and other acrylic acid derivatives, half-ester compounds which are reaction products of hydroxyl group-containing acrylates and dibasic acid anhydrides, and half-ester compounds which are reaction products of vinyl group-containing monoglycidyl ethers or vinyl group-containing monoglycidyl esters and dibasic acid anhydrides.

[0028] The half ester compound can be obtained by reacting a hydroxyl group-containing acrylate, a vinyl group-containing monoglycidyl ether, or a vinyl group-containing monoglycidyl ester with a dibasic acid anhydride in an equimolar ratio. These vinyl group-containing monocarboxylic acids (b) can be used alone or in combination of two or more.

[0029] Examples of the hydroxyl group-containing acrylate, vinyl group-containing monoglycidyl ether, and vinyl group-containing monoglycidyl ester used in the synthesis of the above-mentioned half-ester compound, which is an example of the vinyl group-containing monocarboxylic acid (b), include hydroxyethyl acrylate, hydroxyethyl methacrylate, hydroxypropyl acrylate, hydroxypropyl methacrylate, hydroxybutyl acrylate, hydroxybutyl methacrylate, polyethylene glycol monoacrylate, polyethylene glycol monomethacrylate, trimethylolpropane diacrylate, trimethylolpropane dimethacrylate, pentaerythritol triacrylate, pentaerythritol trimethacrylate, dipentaerythritol pentaacrylate, pentaerythritol pentamethacrylate, glycidyl acrylate, and glycidyl methacrylate.

[0030] The dibasic acid anhydride used in the synthesis of the above-mentioned half ester compound may be one containing a saturated group or one containing an unsaturated group.Specific examples of the dibasic acid anhydride include succinic anhydride, maleic anhydride, tetrahydrophthalic anhydride, phthalic anhydride, methyltetrahydrophthalic anhydride, ethyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, ethylhexahydrophthalic anhydride, and itaconic anhydride.

[0031] In the reaction between the epoxy resin (a) and the vinyl group-containing monocarboxylic acid (b) described above, the reaction is preferably carried out in a ratio of 0.6 to 1.05 equivalents, and more preferably 0.8 to 1.0 equivalents, of the vinyl group-containing monocarboxylic acid (b) per equivalent of the epoxy group of the epoxy resin (a).

[0032] The epoxy resin (a) and the vinyl group-containing monocarboxylic acid (b) can be dissolved in an organic solvent and reacted. Examples of the organic solvent include ketones such as ethyl methyl ketone and cyclohexanone, aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene, glycol ethers such as methyl cellosolve, butyl cellosolve, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether, esters such as ethyl acetate, butyl acetate, butyl cellosolve acetate, and carbitol acetate, aliphatic hydrocarbons such as octane and decane, and petroleum solvents such as petroleum ether, petroleum naphtha, hydrogenated petroleum naphtha, and solvent naphtha.

[0033] Furthermore, it is preferable to use a catalyst to promote the reaction. As the catalyst, for example, triethylamine, benzylmethylamine, methyltriethylammonium chloride, benzyltrimethylammonium chloride, benzyltrimethylammonium bromide, benzyltrimethylmethylammonium iodide, triphenylphosphine, etc. can be used. The amount of the catalyst used is preferably 0.1 to 10 parts by mass based on 100 parts by mass of the epoxy resin (a) and the vinyl group-containing monocarboxylic acid (b) in total.

[0034] In addition, it is preferable to use a polymerization inhibitor for the purpose of preventing polymerization during the reaction. Examples of the polymerization inhibitor include hydroquinone, methylhydroquinone, hydroquinone monomethyl ether, catechol, pyrogallol, etc. The amount of the polymerization inhibitor used is preferably 0.01 to 1 part by mass per 100 parts by mass of the epoxy resin (a) and the vinyl group-containing monocarboxylic acid (b) in total. In addition, the reaction temperature is preferably 60 to 150°C, more preferably 80 to 120°C.

[0035] If necessary, the vinyl group-containing monocarboxylic acid (b) can be used in combination with a phenolic compound such as p-hydroxyphenethyl alcohol, or a polybasic acid anhydride such as trimellitic anhydride, pyromellitic anhydride, benzophenonetetracarboxylic anhydride, or biphenyltetracarboxylic anhydride.

[0036] In the present invention, it is also preferable to use, as the acid-modified vinyl group-containing epoxy resin (A) , a resin (A″) obtained by reacting the above-mentioned resin (A′) with a polybasic acid anhydride (c).

[0037] In resin (A"), it is presumed that the hydroxyl groups in resin (A') (including the hydroxyl groups originally present in epoxy resin (a)) and the acid anhydride groups of polybasic acid anhydride (c) are half-esterified.

[0038] The polybasic acid anhydride (c) may be one containing a saturated group or one containing an unsaturated group. Specific examples of the polybasic acid anhydride (c) include succinic anhydride, maleic anhydride, tetrahydrophthalic anhydride, phthalic anhydride, methyltetrahydrophthalic anhydride, ethyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, ethylhexahydrophthalic anhydride, and itaconic anhydride.

[0039] In the reaction between the resin (A') and the polybasic acid anhydride (c), the acid value of the acid-modified vinyl group-containing epoxy resin can be adjusted by reacting 0.1 to 1.0 equivalent of the polybasic acid anhydride (c) with respect to 1 equivalent of the hydroxyl group in the resin (A').

[0040] The acid value of the (A) acid-modified vinyl group-containing epoxy resin is preferably 30 to 150 mgKOH / g, more preferably 40 to 120 mgKOH / g, and even more preferably 50 to 100 mgKOH / g. If the acid value is less than 30 mgKOH / g, the solubility of the photosensitive resin composition in a dilute alkaline solution tends to decrease, while if it exceeds 150 mgKOH / g, the electrical properties of the cured film tend to decrease.

[0041] The reaction temperature between the resin (A') and the polybasic acid anhydride (c) is preferably 60 to 120°C.

[0042] If necessary, the epoxy resin (a) may be partially used in combination with, for example, a hydrogenated bisphenol A type epoxy resin. Furthermore, the acid-modified vinyl group-containing epoxy resin (A) may be partially used in combination with a styrene-maleic acid resin such as a hydroxyethyl acrylate modified product of a styrene-maleic anhydride copolymer or a hydroxyethyl acrylate modified product of a styrene-maleic anhydride copolymer.

[0043] In the photosensitive resin composition, the content of component (A) is preferably 5 to 60 mass %, more preferably 10 to 50 mass %, and even more preferably 15 to 40 mass %, based on the total solid content of the photosensitive resin composition. When the content of component (A) is within the above range, a coating film with better heat resistance, electrical properties, and chemical resistance can be obtained.

[0044] [(B) Photopolymerizable monomer having an ethylenically unsaturated bond] (B) As the photopolymerizable monomer having an ethylenically unsaturated bond, a compound having a molecular weight of 1000 or less is preferable, and examples thereof include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate, glycol mono- or di(meth)acrylates such as ethylene glycol, methoxytetraethylene glycol, and polyethylene glycol, (meth)acrylamides such as N,N-dimethyl(meth)acrylamide and N-methylol(meth)acrylamide, aminoalkyl (meth)acrylates such as N,N-dimethylaminoethyl (meth)acrylate, hexanediol, trimethylolpropane, pentaerythritol, ditrimethylolpropane, Examples of the photopolymerizable monomer include polyhydric alcohols such as dipentaerythritol and tris-hydroxyethyl isocyanurate, polyhydric (meth)acrylates of their ethylene oxide or propylene oxide adducts, (meth)acrylates of ethylene oxide or propylene oxide adducts of phenols such as phenoxyethyl (meth)acrylate and polyethoxy di(meth)acrylate of bisphenol A, (meth)acrylates of glycidyl ethers such as glycerin diglycidyl ether, trimethylolpropane triglycidyl ether, and triglycidyl isocyanurate, as well as melamine (meth)acrylate, acrylamide, acrylonitrile, diacetone acrylamide, styrene, and vinyl toluene. These (B) photopolymerizable monomers having an ethylenically unsaturated group are used alone or in combination of two or more. In addition, it is more preferable that the photopolymerizable monomer has three or more ethylenically unsaturated bonds in one molecule in order to increase the crosslink density by photocuring and improve the heat resistance and electrical reliability.Examples of such compounds having an ethylenically unsaturated bond include trimethylolpropane tri(meth)acrylate, EO-modified trimethylolpropane tri(meth)acrylate, PO-modified trimethylolpropane tri(meth)acrylate, EO·PO-modified trimethylolpropane tri(meth)acrylate, tetramethylolmethane tri(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, dipentaerythritol triacrylate, dipentaerythritol penta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate. The above "EO" stands for "ethylene oxide" and "PO" stands for "propylene oxide." Additionally, "EO-modified" means having a block structure of ethylene oxide units (-CH2-CH2-O-), and "PO-modified" means having a block structure of propylene oxide units (-CH2-CH(CH3)-O-).

[0045] [(C) Photopolymerization initiator] (C) Examples of the photopolymerization initiator include benzoins such as benzoin, benzoin methyl ether, and benzoin isopropyl ether; acetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 1-hydroxycyclohexyl phenyl ketone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2-methyl-1-[4-(methylthio)phenyl]-2-mo acetophenones such as sulfolino-1-propanone and N,N-dimethylaminoacetophenone; anthraquinones such as 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 1-chloroanthraquinone, 2-amylanthraquinone, and 2-aminoanthraquinone; thioxanthones such as 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, and 2,4-diisopropylthioxanthone; acetophenone dimethyl ketone Ketals such as tar and benzyl dimethyl ketal; benzophenones such as benzophenone, methylbenzophenone, 4,4'-dichlorobenzophenone, 4,4'-bis(diethylamino)benzophenone, Michler's ketone, and 4-benzoyl-4'-methyldiphenyl sulfide; 2-(o-chlorophenyl)-4,5-diphenylimidazole dimer, 2-(o-chlorophenyl)-4,5-di(m-methoxyphenyl)imidazole dimer, 2-(o-fluorophenyl)-4,5- 2,4,5-triarylimidazole dimers such as diphenylimidazole dimer, 2-(o-methoxyphenyl)-4,5-diphenylimidazole dimer, 2-(p-methoxyphenyl)-4,5-diphenylimidazole dimer, 2,4-di(p-methoxyphenyl)-5-phenylimidazole dimer, and 2-(2,4-dimethoxyphenyl)-4,5-diphenylimidazole dimer, acridines such as 9-phenylacridine and 1,7-bis(9,9'-acridinyl)heptane;Examples of the photopolymerization initiator (C) include acylphosphine oxides such as 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 1,2-octanedione-1-[4-(phenylthio)phenyl]-2-(O-benzoyloxime), 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone-1-(O-acetyloxime), and 1-phenyl-1,2-propanedione-2-[O-(ethoxycarbonyl)oxime]. These photopolymerization initiators (C) can be used alone or in combination of two or more. In addition, Irgacure 819 (manufactured by BASF Japan Ltd., trade name, "Irgacure" is a registered trademark), which has good bottom curing properties due to photobleaching, and Irgacure 369 (manufactured by BASF Japan Ltd., trade name), which is difficult to volatilize and therefore does not easily generate outgassing, are preferred.

[0046] Furthermore, (C) photopolymerization initiation assistants such as tertiary amines such as N,N-dimethylaminobenzoic acid ethyl ester, N,N-dimethylaminobenzoic acid isoamyl ester, pentyl-4-dimethylaminobenzoate, triethylamine, triethanolamine, etc. can be used alone or in combination of two or more kinds.

[0047] [(D) Inorganic filler] (D) Inorganic filler will be described. (D) Inorganic filler may be, for example, silica (SiO2), alumina (Al2O3), titania (TiO2), tantalum oxide (Ta2O5), zirconia (ZrO2), silicon nitride (Si3N4), barium titanate (BaO·TiO2), barium carbonate (BaCO3), magnesium carbonate, aluminum oxide, aluminum hydroxide, magnesium hydroxide, lead titanate (PbO·TiO2), lead zirconate titanate (PZT), lead lanthanum zirconate titanate (PLZT), gallium oxide (Ga2O3), spinel (MgO·Al2O3), mullite (3A l2O3·2SiO2), cordierite (2MgO·2Al2O3 / 5SiO2), talc (3MgO·4SiO2·H2O), aluminum titanate (TiO2-Al2O3), yttria-containing zirconia (Y2O3-ZrO2), barium silicate (BaO·8SiO2), boron nitride (BN), calcium carbonate (CaCO3), barium sulfate (BaSO4), calcium sulfate (CaSO4), zinc oxide (ZnO), magnesium titanate (MgO·TiO2), hydrotalcite, mica, calcined kaolin, carbon (C), etc. can be used. These inorganic fillers (D) can be used alone or in combination of two or more.

[0048] In order to disperse the inorganic filler (D) used in the present invention in the resin without agglomeration while keeping the primary particle size, a silane coupling agent is used.As the silane coupling agent, generally available ones can be used, for example, alkylsilane, alkoxysilane, vinylsilane, epoxysilane, aminosilane, acrylsilane, methacrylsilane, mercaptosilane, sulfidesilane, isocyanatesilane, sulfursilane, styrylsilane, alkylchlorosilane, etc. can be used.Specific compound names include methyltrimethoxysilane, dimethyldimethoxysilane, trimethylmethoxysilane, methyltriethoxysilane, methyltriphenoxysilane, ethyltrimethoxysilane, n-propyltrimethoxysilane, diisopropyldimethoxysilane, isobutyltrimethoxysilane, diisobutyldimethoxysilane, isobutyltriethoxysilane, n-hexyltrimethoxysilane, n-hexyltriethoxysilane, cyclohexylmethyldimethoxysilane, n-octyltriethoxysilane, n-Dodecylmethoxysilane, phenyltrimethoxysilane, diphenyldimethoxysilane, triphenylsilanol, methyltrichlorosilane, dimethyldichlorosilane, trimethylchlorosilane, n-Octyldimethylchlorosilane, tetraethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-(2-aminoethyl)aminopropyltrimethoxysilane, 3-(2-aminoethyl)aminopropylmethyldimethoxysilane, 3-phenylaminopropyltrimethoxysilane , 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, bis(3-(triethoxysilyl)propyl)disulfide, bis(3-(triethoxysilyl)propyl)tetrasulfide, vinyltriacetoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltriisopropoxysilane, allyltrimethoxysilane, diallyldimethylsilane, 3-methacryloyldimethylsilane, Examples of suitable silanes include acryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltriethoxysilane, N-(1,3-dimethylbutylidene)-3-aminopropyltriethoxysilane, aminosilane, monomethyltriisocyanatesilane, tetraisocyanatesilane, and γ-isocyanatepropyltriethoxysilane.The silane coupling agent used is preferably one that reacts with the carboxyl group of the (A) acid-modified vinyl group-containing epoxy resin contained in the photosensitive resin composition, and is preferably, for example, epoxy silane, acrylic silane, or methacryl silane. These silane coupling agents strengthen the bond between silica and resin, and therefore, when used as a permanent mask resist, they strengthen the strength of the film and contribute to crack resistance in a temperature cycle test. Mercaptosilane and isocyanate silane may also be used. (B) It is considered that the silane coupling agent reacts with the ethylenically unsaturated group of the photopolymerizable monomer having an ethylenically unsaturated bond to exert the same effect as when the silane coupling agent is used.

[0049] In the photosensitive resin composition, the content of the (D) component is 30 to 70% by mass based on the total solid content of the photosensitive resin composition from the viewpoint of resolution and low thermal expansion coefficient, but is preferably 40 to 65% by mass, and more preferably 45 to 60% by mass. When the content of the (D) component is within the above range, low thermal expansion coefficient, heat resistance, electrical reliability (HAST resistance), thermal shock resistance, resolution, film strength, etc. can be further improved. If the filling amount exceeds 70% by mass, it becomes difficult to disperse it in the resin, and the flowability of the photosensitive resin composition tends to decrease. If the filling amount is less than 30% by mass, it tends to be difficult to obtain crack resistance during reflow mounting.

[0050] The average particle size of the (D) inorganic filler is preferably 0.01 to 1 μm, and from the viewpoint of practicality and resolution, it is more preferably 0.1 to 1 μm, and most preferably 0.3 to 0.7 μm. The maximum particle size of the (D) inorganic filler is preferably 0.1 to 5 μm, more preferably 0.1 to 3 μm, and even more preferably 0.1 to 1 μm. If the maximum particle size exceeds 5 μm, the resolution and electrical reliability tend to be impaired.

[0051] Among (D) inorganic fillers, it is preferable to use silica fine particles from the viewpoint of improving low expansion coefficient and heat resistance. It is also preferable to use barium sulfate fine particles from the viewpoint of improving solder heat resistance, HAST property (electrical reliability), crack resistance (thermal shock resistance), and adhesive strength between the underfill material and the cured film after PCT resistance test (pressure cooker test). It is also preferable that the silica fine particles are surface-treated with alumina and / or an organic silane compound from the viewpoint of improving the aggregation prevention effect.

[0052] When the silica is used, the content is preferably 30 to 60 mass % based on the total solid content of the photosensitive resin composition, and more preferably 35 to 55 mass %. When the content of the silica fine particles is within the above range, it is possible to further improve the low expansion coefficient, solder heat resistance, and adhesive strength between the underfill material and the cured film after PCT resistance test.

[0053] The photosensitive resin composition of the present invention may further contain (E) a pigment, (F) a curing agent, and / or (G) an elastomer in addition to the above-mentioned (A) to (D) components. It may further contain (H) an epoxy resin curing agent. Each component will be described below.

[0054] [(E) Pigment] The photosensitive resin composition preferably contains a pigment as component (E). The pigment (E) is preferably used according to the desired color to improve the identification and appearance of the manufacturing equipment, and to conceal the wiring pattern, etc. The pigment (E) is used as necessary according to the desired color, and a colorant that develops the desired color may be appropriately selected and used. Preferred examples of the colorant include known colorants such as phthalocyanine blue, phthalocyanine green, iodine green, diazo yellow, and crystal violet. The content of the pigment (E) is preferably 0.1 to 5 parts by mass, and more preferably 0.1 to 3 parts by mass, based on 100 parts by mass of the total solid content in the photosensitive resin composition. When the content of the component (E) is within the above range, the wiring pattern can be concealed.

[0055] [(F) Hardener] The (F) curing agent is preferably a compound that itself cures with heat, ultraviolet light, etc., or a compound that cures by reacting with a carboxyl group or a hydroxyl group of the (A) acid-modified vinyl group-containing epoxy resin with heat, ultraviolet light, etc. Use of the (F) curing agent can improve the heat resistance, adhesiveness, chemical resistance, etc. of the cured film formed from the photosensitive resin composition.

[0056] (F) Curing agents include, for example, thermosetting compounds such as epoxy compounds, melamine compounds, urea compounds, oxazoline compounds, blocked isocyanates, etc. Epoxy compounds include, for example, bisphenol A type epoxy resins, bisphenol F type epoxy resins, hydrogenated bisphenol A type epoxy resins, brominated bisphenol A type epoxy resins, novolac type epoxy resins, bisphenol S type epoxy resins, biphenyl type epoxy resins, naphthalene type epoxy resins, dicyclo type epoxy resins, hydantoin type epoxy resins, heterocyclic epoxy resins such as triglycidyl isocyanurate, and bixylenol type epoxy resins. Examples of the melamine compound include triaminotriazine, hexamethoxymelamine, and hexabutoxylated melamine. An example of the urea compound is dimethylol urea.

[0057] The blocked isocyanate is an addition reaction product of a polyisocyanate compound and an isocyanate blocking agent. Examples of the polyisocyanate compound include polyisocyanate compounds such as tolylene diisocyanate, xylylene diisocyanate, phenylene diisocyanate, naphthylene diisocyanate, bis(isocyanatemethyl)cyclohexane, tetramethylene diisocyanate, hexamethylene diisocyanate, methylene diisocyanate, trimethylhexamethylene diisocyanate, and isophorone diisocyanate, as well as their adducts, biuret forms, and isocyanurates.

[0058] Examples of the isocyanate blocking agent include phenol-based blocking agents such as phenol, cresol, xylenol, chlorophenol, and ethylphenol; lactam-based blocking agents such as ε-caprolactam, δ-valerolactam, γ-butyrolactam, and β-propiolactam; active methylene-based blocking agents such as ethyl acetoacetate and acetylacetone; methanol, ethanol, propanol, butanol, amyl alcohol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, propylene glycol monomethyl ether, benzyl ether, methyl glycolate, butyl glycolate, diacetone alcohol, and methyl lactate. oxime-based blocking agents such as formaldehyde oxime, acetaldoxime, acetoxime, methyl ethyl ketoxime, diacetyl monoxime, cyclohexane oxime, etc.; mercaptan-based blocking agents such as butyl mercaptan, hexyl mercaptan, t-butyl mercaptan, thiophenol, methylthiophenol, ethylthiophenol, etc.; acid amide-based blocking agents such as acetate amide, benzamide, etc.; imide-based blocking agents such as succinimide and maleimide; amine-based blocking agents such as xylidine, aniline, butylamine, dibutylamine, etc.; imidazole-based blocking agents such as imidazole, 2-ethylimidazole, etc.; and imine-based blocking agents such as methyleneimine, propyleneimine, etc.

[0059] From the viewpoint of further improving the heat resistance of the cured film, the (F) curing agent preferably contains an epoxy compound (epoxy resin) and / or a blocked isocyanate, and it is more preferable to use an epoxy compound and a blocked isocyanate in combination.

[0060] The (F) curing agent may be used alone or in combination of two or more. When the (F) curing agent is used, the content thereof is preferably 2 to 40 mass %, more preferably 3 to 30 mass %, and further preferably 5 to 20 mass %, based on the total solid content of the photosensitive resin composition. By setting the content of the (F) curing agent within the range of 2 to 40 mass %, it is possible to further improve the heat resistance of the formed cured film while maintaining good developability.

[0061] [(G) Elastomer] The elastomer (G) can be suitably used when the photosensitive resin composition of the present invention is used for a semiconductor package substrate. By adding the elastomer (G) to the photosensitive resin composition of the present invention, the crosslinking reaction (curing reaction) proceeds due to ultraviolet light or heat, causing the acid-modified vinyl group-containing epoxy resin (A) to cure and shrink, which causes distortion (internal stress) inside the resin and reduces flexibility and adhesiveness. This problem can be solved.

[0062] Examples of (G) elastomers include styrene-based elastomers, olefin-based elastomers, urethane-based elastomers, polyester-based elastomers, polyamide-based elastomers, acrylic-based elastomers, and silicone-based elastomers. These (G) elastomers are composed of hard segment components and soft segment components, with the former generally contributing to heat resistance and strength, and the latter generally contributing to flexibility and toughness.

[0063] Examples of the styrene-based elastomer include styrene-butadiene-styrene block copolymer, styrene-isoprene-styrene block copolymer, styrene-ethylene-butylene-styrene block copolymer, and styrene-ethylene-propylene-styrene block copolymer.

[0064] As a component constituting the styrene-based elastomer, in addition to styrene, styrene derivatives such as α-methylstyrene, 3-methylstyrene, 4-propylstyrene, and 4-cyclohexylstyrene can be used. More specifically, Tufprene, Solprene T, Asaprene T, Tuftec (all manufactured by Asahi Kasei Corporation), Elastomer AR (manufactured by Aronkasei Corporation), Kraton G, Cariflex (all manufactured by Kraton Polymer Japan Co., Ltd.), JSR-TR, TSR-SIS, Dynaron (all manufactured by JSR Corporation), Denka STR (manufactured by Denka Co., Ltd.), Quintac (manufactured by Zeon Corporation), TPE-SB series (manufactured by Sumitomo Chemical Co., Ltd.), Rabalon (manufactured by Mitsubishi Chemical Corporation), Septon, Hybra (all manufactured by Kuraray Co., Ltd.), Sumiflex (manufactured by Sumitomo Bakelite Co., Ltd.), Leostomer, Actimer (all manufactured by Riken Technos Corporation), etc. can be used.

[0065] Olefin elastomers are copolymers of α-olefins having 2 to 20 carbon atoms, such as ethylene, propylene, 1-butene, 1-hexene, and 4-methyl-pentene. Specific examples include ethylene-propylene copolymers (EPR), ethylene-propylene-diene copolymers (EPDM), copolymers of non-conjugated dienes having 2 to 20 carbon atoms, such as dicyclopentadiene, 1,4-hexadiene, cyclooctadiene, methylenenorbornene, ethylidenenorbornene, butadiene, and isoprene, and α-olefin copolymers, and carboxy-modified NBR obtained by copolymerizing butadiene-acrylonitrile copolymers with methacrylic acid. More specific examples include ethylene-α-olefin copolymer rubber, ethylene-α-olefin-non-conjugated diene copolymer rubber, propylene-α-olefin copolymer rubber, and butene-α-olefin copolymer rubber. More specifically, examples of usable materials include Mirastomer (manufactured by Mitsui Chemicals, Inc.), EXACT (manufactured by ExxonMobil Corporation), ENGAGE (manufactured by The Dow Chemical Company), hydrogenated styrene-butadiene rubber "DYNABON HSBR" (manufactured by JSR Corporation), butadiene-acrylonitrile copolymer "NBR series" (manufactured by JSR Corporation), butadiene-acrylonitrile copolymers modified with carboxyl groups at both ends "XER series" (manufactured by JSR Corporation), epoxidized polybutadiene BF-1000 (manufactured by Nippon Soda Co., Ltd.) and PB-3600 (manufactured by Daicel Corporation) in which polybutadiene is partially epoxidized.

[0066] The urethane-based elastomer is composed of structural units of a hard segment made of a low molecular weight glycol and a diisocyanate, and a soft segment made of a high molecular weight (long-chain) diol and a diisocyanate.

[0067] As the low molecular weight glycol, a short chain diol such as ethylene glycol, propylene glycol, 1,4-butanediol, or bisphenol A can be used. The number average molecular weight of the short chain diol is preferably 48 to 500.

[0068] Examples of the polymeric (long-chain) diol include polypropylene glycol, polytetramethylene oxide, poly(1,4-butylene adipate), poly(ethylene·1,4-butylene adipate), polycaprolactone, poly(1,6-hexylene carbonate), and poly(1,6-hexylene·neopentylene adipate). The number average molecular weight of the polymeric (long-chain) diol is preferably 500 to 10,000.

[0069] Specific examples of urethane-based elastomers include PANDEX T-2185 and T-2983N (manufactured by DIC Corporation), and Miractoran E790 (manufactured by Nippon Miractoran Co., Ltd.).

[0070] Examples of polyester-based elastomers include those obtained by polycondensation of dicarboxylic acid or a derivative thereof and a diol compound or a derivative thereof. Specific examples of dicarboxylic acids include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, and naphthalenedicarboxylic acid, aromatic dicarboxylic acids in which the hydrogen atoms of the aromatic nuclei are substituted with methyl groups, ethyl groups, phenyl groups, etc., aliphatic dicarboxylic acids having 2 to 20 carbon atoms such as adipic acid, sebacic acid, and dodecanedicarboxylic acid, and alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid. These compounds can be used alone or in combination of two or more. Specific examples of the diol compound include aliphatic diols and alicyclic diols such as ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,6-hexanediol, 1,10-decanediol, and 1,4-cyclohexanediol, and dihydric phenols represented by the following general formula (4).

[0071] [ka] [In general formula (4), Y 11 represents an alkylene group having 1 to 10 carbon atoms, a cycloalkylene group having 4 to 8 carbon atoms, -O-, -S-, or -SO2-; R 21 and R22 represents a halogen atom or an alkyl group having 1 to 12 carbon atoms, p and q represent integers of 0 to 4, and r represents 0 or 1.]

[0072] Specific examples of the dihydric phenol represented by the general formula (4) include bisphenol A, bis-(4-hydroxyphenyl)methane, bis-(4-hydroxy-3-methylphenyl)propane, and resorcin. These compounds can be used alone or in combination of two or more.

[0073] Also, a multiblock copolymer can be used in which an aromatic polyester (e.g., polybutylene terephthalate) portion is the hard segment component and an aliphatic polyester (e.g., polytetramethylene glycol) portion is the soft segment component. There are various grades depending on the type, ratio, and molecular weight of the hard and soft segments. Specific examples include Hytrel (manufactured by DuPont-Toray Co., Ltd.), Pelprene (manufactured by Toyobo Co., Ltd.), and Espel (manufactured by Hitachi Chemical Co., Ltd.).

[0074] Polyamide elastomers are broadly divided into two types: polyether block amide type, which uses polyamide for the hard segment and polyether or polyester for the soft segment, and polyether ester block amide type.

[0075] Examples of the polyamide include polyamide-6, 11, and 12. Examples of the polyether include polyoxyethylene, polyoxypropylene, and polytetramethylene glycol. Specifically, UBE polyamide elastomer (manufactured by Ube Industries, Ltd.), DAIAMID (manufactured by Daicel-Evonik Corporation), PEBAX (manufactured by Toray Industries, Inc.), GRILLON ELY (manufactured by M-Chemie Japan Co., Ltd.), NOPAMIDT (manufactured by Mitsubishi Chemical Corporation), and GLYXLUX (manufactured by DIC Corporation) can be used.

[0076] Acrylic elastomers are mainly composed of acrylic esters, and ethyl acrylate, butyl acrylate, methoxyethyl acrylate, ethoxyethyl acrylate, etc. are used. In addition, glycidyl methacrylate, allyl glycidyl ether, etc. are used as crosslinking point monomers. Furthermore, acrylonitrile and ethylene can be copolymerized. Specifically, acrylonitrile-butyl acrylate copolymer, acrylonitrile-butyl acrylate-ethyl acrylate copolymer, acrylonitrile-butyl acrylate-glycidyl methacrylate copolymer, etc. can be used.

[0077] Silicone elastomers are mainly composed of organopolysiloxane and are divided into polydimethylsiloxane, polymethylphenylsiloxane, and polydiphenylsiloxane. Some are partially modified with vinyl groups, alkoxy groups, etc. Specific examples include the KE series (manufactured by Shin-Etsu Chemical Co., Ltd.), SE series, CY series, and SH series (all manufactured by Dow Corning Toray Silicone Co., Ltd.).

[0078] In addition to the above-mentioned elastomers, rubber-modified epoxy resins can also be used. Rubber-modified epoxy resins can be obtained by modifying, for example, a part or all of the epoxy groups of bisphenol F type epoxy resins, bisphenol A type epoxy resins, salicylaldehyde type epoxy resins, phenol novolac type epoxy resins, or cresol novolac type epoxy resins with both-end carboxylic acid-modified butadiene-acrylonitrile rubber, end amino-modified silicone rubber, or the like. Among these elastomers, in terms of shear adhesion, butadiene-acrylonitrile copolymers modified with both-end carboxyl groups, Espel (Hitachi Chemical Co., Ltd., Espel 1612, 1620), which is a polyester-based elastomer having hydroxyl groups, and epoxidized polybutadiene, or the like, are preferred. In addition, elastomers that are liquid at room temperature (25°C) are particularly preferred.

[0079] When the (G) elastomer is used, its content is preferably 1 to 20 mass%, more preferably 2 to 15 mass%, and even more preferably 3 to 10 mass%, based on the total solid content of the photosensitive resin composition. By setting the content of the (G) elastomer within the range of 1 to 20 mass%, it is possible to further improve the thermal shock resistance and the adhesive strength between the underfill material and the cured film while maintaining good developability. In addition, when used in a thin film substrate, it is possible to reduce the warpage of the thin film substrate.

[0080] [(H) Epoxy resin hardener] An epoxy resin curing agent (H) may also be added to the photosensitive resin composition of the present invention for the purpose of further improving the properties of the cured film formed, such as heat resistance, adhesiveness, and chemical resistance.

[0081] Specific examples of such epoxy resin curing agents (H) include imidazole derivatives such as 2-methylimidazole, 2-ethyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 2-phenylimidazole, and 2-phenyl-4-methyl-5-hydroxymethylimidazole; guanamines such as acetoguanamine and benzoguanamine; polyamines such as diaminodiphenylmethane, m-phenylenediamine, m-xylylenediamine, diaminodiphenylsulfone, dicyandiamide, urea, urea derivatives, melamine, and polybasic hydrazides; organic acid salts and / or epoxy adducts thereof: amine complexes of boron trifluoride; triazine derivatives such as ethyldiamino-S-triazine, 2,4-diamino-S-triazine, and 2,4-diamino-6-xylyl-S-triazine; trimethylamine, triethanolamine, N,N-dimethyloctylamine, N-benzyldimethylamine, pyridine, N-methylmonoamine ... Examples of the epoxy resin hardener include tertiary amines such as fluoroline, hexa(N-methyl)melamine, 2,4,6-tris(dimethylaminophenol), tetramethylguanidine, and m-aminophenol; polyphenols such as polyvinylphenol, polyvinylphenol bromide, phenol novolac, and alkylphenol novolac; organic phosphines such as tributylphosphine, triphenylphosphine, and tris-2-cyanoethylphosphine; phosphonium salts such as tri-n-butyl(2,5-dihydroxyphenyl)phosphonium bromide and hexadecyltributylphosphonium chloride; quaternary ammonium salts such as benzyltrimethylammonium chloride and phenyltributylammonium chloride; the above-mentioned polybasic acid anhydrides; diphenyliodonium tetrafluoroborate, triphenylsulfonium hexafluoroantimonate, and 2,4,6-triphenylthiopyrylium hexafluorophosphate. These epoxy resin hardeners (H) can be used alone or in combination of two or more.

[0082] When the (H) epoxy resin curing agent is used, the content thereof is preferably from 0.01 to 20 mass %, and more preferably from 0.1 to 10 mass %, based on the total solid content of the photosensitive resin composition.

[0083] [(I) Thermoplastic resin] In addition, in order to further improve the flexibility of the cured film, (I) a thermoplastic resin can be added to the photosensitive resin composition of the present invention.

[0084] Examples of the (I) thermoplastic resin include acrylic resin and urethane resin. The content of the (I) thermoplastic resin, when included, is preferably 1 to 30 mass % and more preferably 5 to 20 mass % based on the total solid content of the photosensitive resin composition.

[0085] Furthermore, to the photosensitive resin composition of the present invention, various known and commonly used additives can be added as necessary, such as organic fine particles such as melamine and organic bentonite, polymerization inhibitors such as hydroquinone, methylhydroquinone, hydroquinone monomethyl ether, catechol and pyrogallol, thickeners such as bentone and montmorillonite, silicone-based, fluorine-based and vinyl resin-based defoamers, silane coupling agents, diluents, etc. Furthermore, flame retardants such as brominated epoxy compounds, acid-modified brominated epoxy compounds, antimony compounds, and phosphate compounds of phosphorus-based compounds, aromatic condensed phosphate esters, halogen-containing condensed phosphate esters, etc. can also be added.

[0086] As the diluent, for example, an organic solvent can be used. As the organic solvent, for example, ketones such as ethyl methyl ketone and cyclohexanone, aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene, glycol ethers such as methyl cellosolve, butyl cellosolve, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol diethyl ether, and triethylene glycol monoethyl ether, esters such as ethyl acetate, butyl acetate, butyl cellosolve acetate, and carbitol acetate, aliphatic hydrocarbons such as octane and decane, and petroleum solvents such as petroleum ether, petroleum naphtha, hydrogenated petroleum naphtha, and solvent naphtha. The diluent is used alone or in combination of two or more. When using a diluent, the content can be appropriately adjusted from the viewpoint of the coatability of the photosensitive resin composition.

[0087] The photosensitive resin composition of the present invention can be obtained by uniformly kneading and mixing the above-mentioned components using a roll mill, a bead mill or the like.

[0088] The photosensitive resin composition of the present invention can satisfy the characteristics and reliability required for solder resists, interlayer insulating films, surface protective films for semiconductors, etc., provided on printed wiring boards such as rigid wiring boards and flexible wiring boards, package substrates, etc. The solder resist obtained from the photosensitive resin composition of the present invention is sufficiently excellent in thermal shock resistance, and, due to the same factors, is also excellent in mechanical properties such as alkali resistance, solder heat resistance, electrolytic Ni / Au plating resistance, elongation and tensile strength, as well as HAST resistance.

[0089] [Photosensitive film] A preferred embodiment of the photosensitive film of the present invention will be described below. The photosensitive film includes a support layer, a photosensitive layer containing the photosensitive resin composition formed on the support layer, and a protective film layer laminated on the photosensitive layer.

[0090] The photosensitive layer is preferably formed by dissolving the above-mentioned photosensitive resin composition in a solvent (diluent) as described above as necessary to prepare a solution with a solid content of about 30 to 70% by mass, and then coating the solution on the support layer and drying it. The coating can be performed by a known method using, for example, a roll coater, a comma coater, a gravure coater, an air knife coater, a die coater, a bar coater, or the like. The thickness of the above-mentioned photosensitive layer varies depending on the application, but is preferably 5 to 100 μm, and more preferably 10 to 60 μm, after drying in which the diluent is removed by heating and / or hot air blowing. If the thickness is less than 5 μm, industrial coating tends to be difficult, and if it exceeds 100 μm, the sensitivity and resolution of the photosensitive resin composition layer tend to decrease.

[0091] Examples of the support layer of the photosensitive film include polymer films having heat resistance and solvent resistance, such as polyesters such as polyethylene terephthalate, polypropylene, and polyethylene.

[0092] The thickness of the support layer is preferably 5 to 100 μm, more preferably 10 to 30 μm. If the thickness is less than 5 μm, the support tends to be easily torn when peeled off from the photosensitive film before development, and if the thickness exceeds 100 μm, the resolution and flexibility tend to decrease. In this embodiment, since the photosensitive layer is formed using the polyester resin as described above, even if the thickness of the support layer is thicker than that of the conventional one, for example, more than 25 μm and 100 μm or less, the flexibility and resolution can be maintained.

[0093] Examples of the protective film layer include a polyethylene film, a polypropylene film, a polyethylene terephthalate film, surface-treated paper, etc. It is preferable that the adhesive strength between the photosensitive layer and the protective film layer is smaller than the adhesive strength between the photosensitive layer and the support layer.

[0094] The photosensitive film consisting of three layers, namely, the support layer, the photosensitive layer, and the protective film layer, as described above, may be stored as is, or may be wound up in a roll on a core with a protective film layer interposed therebetween and then stored.

[0095] [Method of forming resist pattern, printed wiring board] The method for forming a resist pattern of the present invention is characterized in that a photosensitive layer is laminated on the insulating substrate of a laminated substrate comprising an insulating substrate and a conductor layer having a circuit pattern formed on the insulating substrate, using a photosensitive resin composition, so as to cover the conductor layer, predetermined parts of the photosensitive layer are irradiated with active light rays to form exposed parts, and then parts of the photosensitive layer other than the exposed parts are removed.

[0096] In an embodiment, the photosensitive layer of the photosensitive film is used as the photosensitive layer using the photosensitive resin composition. A photosensitive layer made of the photosensitive resin composition is formed on a substrate on which a resist is to be formed. The protective film of the photosensitive film is peeled off from the photosensitive resin composition layer, and the exposed surface is adhered by lamination or the like. From the viewpoint of improving adhesion and followability, a method of laminating under reduced pressure is also preferred. The photosensitive resin composition can also be applied to a substrate by a known method such as a method of applying a varnish of the photosensitive resin composition by a screen printing method or a roll coater. Next, an exposure process is performed in which a predetermined portion of the photosensitive resin composition layer is irradiated with active light through a mask pattern, and the photosensitive resin composition layer in the irradiated portion is photocured.

[0097] As the light source of the actinic rays, known light sources that effectively radiate ultraviolet rays, such as carbon arc lamps, mercury vapor arc lamps, extra-high pressure mercury lamps, high pressure mercury lamps, xenon lamps, etc. Also usable are light sources that effectively radiate visible light or ultraviolet light, such as photographic flood lamps and sun lamps.

[0098] Furthermore, if a support is present on the photosensitive layer, the support is removed, and then the non-photocured portion (unexposed portion) is removed by wet or dry development, followed by development to form a resist pattern. In the case of wet development, the developer used is, for example, an alkaline aqueous solution such as sodium hydroxide, an aqueous developer, or an organic solvent, which is safe, stable, and easy to operate. Development methods include the dip method, the bath method, the spray method, the high-pressure spray method, brushing, and slapping.

[0099] After completion of the above-mentioned development step, it is preferable to irradiate with ultraviolet light using a high-pressure mercury lamp or heat the film in order to improve solder heat resistance, chemical resistance, etc. When irradiating with ultraviolet light, the amount of irradiation can be adjusted as necessary, for example, 0.05 to 10 J / cm. 2 In addition, when the resist pattern is heated, it is preferable to heat the resist pattern at a temperature in the range of about 130 to 200° C. for about 15 to 90 minutes.

[0100] Both ultraviolet irradiation and heating may be performed. In this case, both may be performed simultaneously, or one may be performed after the other. When ultraviolet irradiation and heating are performed simultaneously, it is preferable to heat the material to 60 to 150° C. in order to provide better solder heat resistance and chemical resistance.

[0101] The permanent resist thus formed also serves as a protective film for wiring after soldering to the board, and has various properties of a solder resist, and can be used as a solder resist for printed wiring boards, semiconductor package boards, flexible wiring boards, etc. The above-mentioned solder resist is used as a plating resist or an etching resist, for example, when plating or etching is performed on the board, and is also used as a protective film for protecting wiring, etc., by being left on the board as it is.

[0102] The substrate provided with the permanent resist is then subjected to mounting (for example, wire bonding or soldering) of semiconductor elements and the like, and is then installed in an electronic device such as a personal computer.

[0103] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to the above-described embodiments.

[0104] For example, in another embodiment of the photosensitive film of the present invention, the photosensitive film may have only a photosensitive layer and a support layer without having a protective film layer. The printed wiring board of the present invention may be a multilayer printed wiring board in which a conductive layer and an insulating layer are alternately laminated on an insulating substrate or on both sides of the insulating substrate, and in this case, the cured product of the photosensitive resin composition of the present invention functions as an interlayer insulating film for reliably insulating the conductive layers from each other.

[0105] The photosensitive resin composition of the present invention may also be used in a method for producing a printed wiring board. For example, the method includes a method for producing a printed wiring board comprising an insulating substrate, a conductor layer having a circuit pattern formed on the insulating substrate, and a permanent resist layer formed so as to cover the conductor layer, in which a photosensitive layer is laminated on the insulating substrate so as to cover the conductor layer using the photosensitive resin composition of the present invention, a predetermined portion of the photosensitive layer is irradiated with active light to form an exposed portion, and then a portion other than the exposed portion is removed. EXAMPLES

[0106] The present invention will be described in more detail below based on examples and comparative examples, but the present invention is not limited to the following examples.

[0107] [Synthesis Example: Production of Acid-Modified Vinyl Group-Containing Epoxy Resins (A-1, 2, 3, 4)] The structural unit represented by the general formula (3) (R 13 = hydrogen atom, Y 3= glycidyl group), 350 parts by mass of bisphenol F novolac type epoxy resin (EXA-7376, manufactured by DIC Corporation), 70 parts by mass of acrylic acid, 0.5 parts by mass of methyl hydroquinone, 120 parts by mass of carbitol acetate, and a catalyst (triphenylphosphine) were charged, and reacted by heating to 90°C and stirring to completely dissolve the mixture. Next, the resulting solution was cooled to 60°C, 2 parts by mass of triphenylphosphine was added, and the mixture was heated to 100°C and reacted until the acid value of the solution reached 1 mgKOH / g. To the reaction solution, 98 parts by mass of tetrahydrophthalic anhydride (THPAC) and 85 parts by mass of carbitol acetate were added, and the mixture was heated to 80°C and reacted for about 6 hours, followed by cooling to obtain a solution of THPAC-modified bisphenol F-type novolac epoxy acrylate (hereinafter referred to as "acid-modified vinyl-containing epoxy resin (A-1, 2, 3, 4) (dispersity; A-1 = 6.0, A-2 = 4.5, A-3 = 3.5, A-4 = 2.5)) as component (A) with a solid content concentration of 73% by mass. Here, resins with different dispersities were obtained by changing the amount of catalyst (0 to 2 parts by mass), heating temperature (80 to 120°C), and time.

[0108] (Measurement of Dispersion Degree) The number average molecular weight (Mn), weight average molecular weight (Mw) and Mw / Mn (dispersity) of the THPAC-modified bisphenol F-type novolac epoxy acrylate were determined by measuring the chromatogram of the molecular weight distribution of the THPAC-modified bisphenol F-type novolac epoxy acrylate by GPC (gel permeation chromatography) and converting it from the elution time of standard polystyrene at 25° C. The measurement device used was EcoSEC, HLC-8320GPC manufactured by Tosoh Corporation, the eluent used was tetrahydrofuran, and the column used was a Gelpack GL-A-150 and a Gelpack GL-A-10 (manufactured by Hitachi High-Technologies Corporation, product name) directly connected together.

[0109] (Examples 1 to 3, Comparative Examples 1 to 4) The materials shown in Table 1 below were mixed in the amounts (unit: parts by mass) shown in the table, then kneaded with a three-roll mill, and carbitol acetate was added so that the solid content concentration became 70% by mass to obtain a photosensitive resin composition. The amount of each material in Table 1 below indicates the amount of solid content.

[0110] [Table 1]

[0111] The details of each material in Table 1 are as follows: [(A) Acid-modified vinyl group-containing epoxy resin] *1 (Acid-modified vinyl group-containing epoxy resin (A-1)): THPAC-modified bisphenol F-type novolac epoxy acrylate (dispersity Mw / Mn = 6.0) prepared in the synthesis example. *2 (Acid-modified vinyl group-containing epoxy resin (A-2)): THPAC-modified bisphenol F-type novolac epoxy acrylate (dispersity Mw / Mn = 4.5) prepared in the synthesis example. *3 (Acid-modified vinyl group-containing epoxy resin (A-3)): THPAC-modified bisphenol F-type novolac epoxy acrylate (dispersity Mw / Mn = 3.5) prepared in the synthesis example. *4 (Acid-modified vinyl group-containing epoxy resin (A-4)): THPAC-modified bisphenol F-type novolac epoxy acrylate (dispersity Mw / Mn=2.5) prepared in the synthesis example. [(B) Photopolymerizable monomer having an ethylenically unsaturated bond] *5 (Aronix M402): Dipentaerythritol hexaacrylate (manufactured by Toagosei Co., Ltd.) [(C) Photopolymerization initiator)] *6 (Irgacure 907): (2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one, manufactured by BASF Japan Ltd.) [(D) Inorganic filler] *7 (SFP-20M): Silica microparticles (ultrafine spherical silica, average particle size 0.3 μm, manufactured by Denka Co., Ltd.) *8 (B-34): Barium sulfate microparticles (average particle size 0.3 μm, manufactured by Sakai Chemical Industry Co., Ltd.) [(F) Hardener] *9 (YSLV-80XY): Epoxy resin (Tetramethylbisphenol F type, epoxy equivalent = 192g / eq, melting point = 72℃, manufactured by Nippon Steel & Sumikin Chemical Co., Ltd.) *10 (RE-306): Epoxy resin (phenol novolac type epoxy resin, manufactured by Nippon Kayaku Co., Ltd.) [(G) Elastomer] *11 (PB-3600): Epoxidized polybutadiene (manufactured by Daicel Corporation)

[0112] [Silica residue] The photosensitive resin compositions of the Examples and Comparative Examples were applied to a copper-clad laminate substrate (MCL-E-67, glass cloth-based epoxy resin substrate, manufactured by Hitachi Chemical Co., Ltd.) by screen printing so that the film thickness after drying would be 15 μm, and then dried at 75° C. for 30 minutes using a hot air circulation dryer. The resulting coating film was exposed to an integrated exposure of 100 mJ / cm through a negative film having a dotted light-nontransmitting area of ​​80 μm in diameter over an area of ​​1×1 cm. 2 UV light of 1.8 kgf / cm2 for 60 seconds, and a 1% by mass sodium carbonate aqueous solution was applied. 2 The unexposed areas were then developed by spraying at a pressure of 10,000 x 1000, and the unexposed areas were dissolved and developed to form an image. The openings were then observed at 10,000 x 1000 using a SEM (High Technologies Corporation, Model S4200, field emission scanning electron microscope), and the degree of remaining silica residue was evaluated according to the following criteria. The evaluation results are shown in Table 2. A: Less than one silica residue in one field of view B: 2 or more but less than 10 silica residues in one field of view C: 10 or more silica residues in one field of view

[0113] [HAST resistance evaluation] A copper surface of a printed wiring board substrate (MCL-E-679, glass cloth base high Tg epoxy resin substrate, Hitachi Chemical Co., Ltd., product name) in which 12 μm thick copper foil was laminated on a glass epoxy base material was etched to form a comb-shaped electrode with a line / space of 28 μm / 32 μm. This substrate was used as an evaluation substrate, and a cured resist was formed on the substrate as described above, and then exposed to conditions of 135°C, 85% RH, and DC5V for 200 hours. The degree of migration was then observed with a 100x metallurgical microscope and evaluated according to the following criteria. In other words, a permanent resist film in which no migration occurred and no decrease in resistance was rated as "3," a film in which no decrease in resistance occurred but migration occurred was rated as "2," and a film in which significant migration occurred and resistance decreased was rated as "1." The evaluation results are shown in Table 2.

[0114] [Thermal expansion coefficient / glass transition temperature (Tg) evaluation] The photosensitive resin composition solution was uniformly applied onto a 16 μm thick polyethylene terephthalate film (G2-16, Teijin Ltd., product name) that was a support layer so that the film thickness after drying was 30 μm, and it was dried at 75 ° C. for about 30 minutes using a hot air convection dryer. Then, a polyethylene film (NF-15, Tamapoly Co., Ltd., product name) was attached as a protective film to the surface opposite to the side in contact with the support of the photosensitive resin composition layer to obtain a photosensitive film. The entire surface of the photosensitive film was exposed to light, and then it was left to stand at room temperature (25 ° C.) for 1 hour, after which the polyethylene film was peeled off and spray-developed with a 1% by mass aqueous solution of sodium carbonate at 30 ° C. After spray development, it was irradiated with ultraviolet light at 2 J / cm2 using an ultraviolet light irradiation device manufactured by Oak Seisakusho Co., Ltd., and further heated at 170 ° C. for 60 minutes. Next, the laminate was cut into a piece 3 mm wide and 30 mm long with a cutter knife, and the polyethylene terephthalate film supporting the laminate was peeled off to obtain a photosensitive resin cured product (test piece) for evaluating the thermal expansion coefficient. The thermal expansion coefficient (10 -6The glass transition point and thermal expansion coefficient (Tg / °C, ppm) were measured. The tensile load was 5g, the span (distance between chucks) was 15mm, and the heating rate was 10°C / min. First, the test piece was attached to the device and heated from room temperature (25°C) to 160°C and left for 15 minutes. It was then cooled to -60°C and measurements were made under conditions of a heating rate of 10°C / min from -60°C to 250°C, to measure the glass transition point and thermal expansion coefficient. The evaluation results are shown in Table 2.

[0115] [Table 2]

[0116] As is clear from Table 2, Examples 1 to 3 are excellent in general properties such as silica residue, electrical reliability (HAST resistance), low thermal expansion coefficient, and high Tg. Also, it is clear that the acid-modified vinyl group-containing epoxy resin with a dispersity of 3.5 or less has particularly low silica residue and is excellent in thermal expansion coefficient and heat resistance. In contrast, as is clear from Table 2, Comparative Examples 1 to 4 have insufficient silica residue and electrical reliability. Therefore, according to the photosensitive resin composition of the present invention, a permanent mask resist that achieves a low thermal expansion coefficient while maintaining a low level of silica residue, is excellent in HAST resistance, and has a high Tg can be obtained.

Claims

1. A photosensitive resin composition comprising (A) an acid-modified vinyl group-containing epoxy resin, (B) a photopolymerizable monomer having an ethylenically unsaturated bond, (C) a photopolymerization initiator, and (D) an inorganic filler, wherein the acid-modified vinyl group-containing epoxy resin of component (A) is a resin (A″) obtained by reacting a bisphenol-type novolak resin having a structural unit represented by the following general formula (2) or (3) with a vinyl group-containing monocarboxylic acid (b) to obtain a resin (A′), with a saturated or unsaturated group-containing polybasic acid anhydride (wherein Mw / Mn (weight average molecular weight / Mw / Mn) is: (A) is a photosensitive resin composition having a polydispersity of 2.0 to 5.0, represented by the number average molecular weight. Also excluding a resin obtained by reacting an o-cresol novolac resin with acrylic acid, followed by reaction with tetrahydrophthalic anhydride, and a resin obtained by reacting an o-cresol novolac resin with acrylic acid and a pentaerythritol triacrylate-succinic anhydride adduct, followed by reaction with succinic anhydride and tetrahydrophthalic anhydride.), and wherein (D) the inorganic filler comprises silica and barium sulfate, and the content of the inorganic filler is 40 to 70 mass% based on the total solid content. [Case 1] [Case 2] [In general formula (2), R 12 represents a hydrogen atom or a methyl group; Y 2 Each of R independently represents a hydrogen atom or a glycidyl group. 12 may be the same or different. 2 At least one of R represents a glycidyl group. 13 represents a hydrogen atom or a methyl group; Y 3 Each of R independently represents a hydrogen atom or a glycidyl group. 13 may be the same or different. 3 At least one of these represents a glycidyl group.

2. 2. The photosensitive resin composition according to claim 1, wherein the photopolymerizable monomer having an ethylenically unsaturated bond (B) is a polyfunctional photopolymerizable monomer having three or more ethylenically unsaturated bonds in one molecule.

3. The photosensitive resin composition according to claim 1 or 2, further comprising (E) a pigment.

4. A photosensitive film comprising a support and a photosensitive layer formed from the photosensitive resin composition according to any one of claims 1 to 3.

5. A method for forming a resist pattern, comprising: laminating a photosensitive layer on a laminate substrate including an insulating substrate and a conductor layer having a circuit pattern formed on the insulating substrate, using the photosensitive resin composition according to any one of claims 1 to 3, so as to cover the conductor layer; irradiating a predetermined portion of the photosensitive layer with active light to form an exposed portion; and then removing a portion of the photosensitive layer other than the exposed portion.

6. A printed wiring board comprising an insulating substrate, a conductor layer having a circuit pattern formed on the insulating substrate, and a permanent resist layer formed using the photosensitive resin composition according to any one of claims 1 to 3 so as to cover the conductor layer.

Citation Information

Patent Citations

  • Resin paste and flexible wiring board using the same

    JP2003198105A

  • Photosensitive resin composition and method for manufacturing its hardened product

    JP2005115187A

  • Photosetting / thermosetting one-liquid type solder resist composite and printed wiring board using the same

    JP2006190848A

  • Circuit board with electromagnetic wave shield film, and production method of the same

    JP2016149388A