Directional electromagnetic steel sheet

By employing controlled laser or electron beam treatment to create a resolidified structure with precise crystal misorientation and minimal surface unevenness, the method addresses the challenges of maintaining magnetic domain refinement and reducing noise in grain-oriented electrical steel sheets, ensuring low iron loss and consistent magnetic properties.

JP7582466B2Active Publication Date: 2024-11-13JFE STEEL CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023524268
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-01-06
Filing Date
2022-12-21
Publication Date
2024-11-13
Estimated Expiration
2042-12-21

AI Technical Summary

Technical Problem

Existing methods for refining magnetic domains in grain-oriented electrical steel sheets face issues such as loss of magnetic domain refining effect during strain relief annealing, increased noise due to harmonics, non-uniform groove shapes leading to varying iron loss values, and decreased magnetic flux density, along with problems in insulation and space factor.

Method used

The method involves linear laser irradiation or electron beam treatment on the steel sheet surface to create a resolidified structure with controlled crystal misorientation and minimal surface unevenness, forming a pseudo-grain boundary effect without grooves, using specific laser or electron beam conditions to maintain magnetic domain refinement even after strain relief annealing.

Benefits of technology

This approach maintains low iron loss and reduces transformer noise while preserving magnetic flux density, achieving improved magnetic properties without surface irregularities or insulation issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582466000001
    Figure 0007582466000001
  • Figure 0007582466000002
    Figure 0007582466000002
  • Figure 0007582466000003
    Figure 0007582466000003
Patent Text Reader

Abstract

The present invention proposes an oriented electromagnetic steel sheet in which the magnetic domain structure is controlled and iron loss is reduced, wherein an iron loss reduction effect can be maintained even when stress relief annealing is applied. The oriented electromagnetic steel sheet has, on at least one surface from among the obverse and reverse surfaces of a steel sheet having a prescribed component composition, a local region that has an orientation angle difference of 1.5° or more with respect to the surrounding crystal and that extends in a linear shape in a direction intersecting the rolling direction of the steel sheet, the local region having a volume fraction of 0.1-2.0% inclusive and a residual stress of 100 Mpa or less, and the average unevenness amount at the ferrite surface of the surface having the local region being below 5 μm.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a grain-oriented electrical steel sheet that has low iron loss and small magnetostrictive vibration and is suitable as a material for the iron core of a transformer or the like. [Background technology]

[0002] Grain-oriented electrical steel sheets are soft magnetic materials and are mainly used as materials for the iron cores of transformers and rotating machines. Therefore, grain-oriented electrical steel sheets are required to have the following magnetic properties: high magnetic flux density, low core loss, and low magnetostriction. To meet this requirement, secondary recrystallized grains in the steel sheet are aligned in the {110} <001> It is important to highly align the orientation (Goss orientation) and to reduce impurities in the product.

[0003] Here, since there are limitations to the above-mentioned control of crystal orientation and reduction of impurities, a technology has been developed in which non-uniformity is introduced into the surface of the steel sheet by physical means, thereby subdividing the width of the magnetic domains and reducing iron loss, i.e., magnetic domain subdivision technology. For example, Patent Document 1 proposes a technology in which a final product sheet is irradiated with a laser to introduce linear high dislocation density regions into the surface layer of the steel sheet, thereby narrowing the magnetic domain width and reducing iron loss. This technology is widely used because of its excellent manufacturability. When grain-oriented electrical steel sheet is magnetized with an alternating current, the amount of magnetization exhibits a change close to a sine wave, and therefore the expansion and contraction movement of the steel sheet itself based on the reciprocating motion of the magnetic walls separating the magnetic domains, i.e., the change over time in the amount of magnetostriction, exhibits a waveform that is relatively close to a sine wave.

[0004] Other effective magnetic domain refining techniques that have been disclosed include a method of mechanically forming grooves using a toothed roll or the like (Patent Document 2), and a method of electrically or chemically forming grooves by etching or the like (Patent Document 3). With these groove forming techniques, the magnetic domain refining effect is not lost and low iron loss values ​​are maintained even when heat treatments such as stress relief annealing are performed, making it possible to use this material as the core of almost all transformers, including wound core transformers.

[0005] In contrast to these groove forming methods, Patent Document 4 proposes a technology in which grooves are formed in the final cold-rolled sheet using a laser beam or a plasma flame, and the magnetic domain refining effect can be maintained even after stress relief annealing. This technology is said to be relatively simple and allows for low-cost processing. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Special Publication No. 57-2252 [Patent Document 2] Special Publication No. 03-69968 [Patent Document 3] Japanese Patent Application Laid-Open No. 61-117218 [Patent Document 4] Japanese Patent Application Publication No. 09-49024 Summary of the Invention [Problem to be solved by the invention]

[0007] However, the technology described in Patent Document 1 has an essential problem in that the magnetic domain refinement effect is lost by stress relief annealing. Therefore, in order to maintain the iron loss reduction effect, the application is limited to stacked core transformers, which are not usually subjected to stress relief annealing. On the other hand, when a magnetic domain control method utilizing residual stress, such as laser irradiation, is applied, the motion of the magnetic domain walls is strongly affected by the stress, and the time change in the amount of magnetostriction exhibits a complex waveform different from a sine wave, in which higher-order harmonics are superimposed, and it is known that when used in a transformer core, etc., this produces a lot of noise.

[0008] The technology described in Patent Document 2 requires the maintenance of a toothed roll that wears out, and the technology described in Patent Document 3 requires the application and removal of resist ink used for etching. Both technologies have many manufacturing issues, resulting in increased costs. Furthermore, when magnetic domain control is performed using these methods, the residual distortion is basically extremely small, so the magnetostrictive vibration has a waveform close to a sine wave, similar to that of steel sheets that have not been subjected to magnetic domain control, which is advantageous in reducing transformer noise.

[0009] In the technology described in Patent Document 4, convex parts such as sputter marks and burrs are formed around the grooves when the laser light or plasma flame is irradiated. This results in a decrease in the space factor, and the insulating properties of the insulating coating applied thereafter are reduced, which can lead to dielectric breakdown of the transformer, and this technology has not yet been put to practical use.

[0010] In any case, the method of refining magnetic domains by forming grooves in this way tends to result in uneven groove shapes, which tends to cause variations in the obtained iron loss values. Furthermore, since the cross-sectional area of ​​the steel sheet is effectively reduced in the grooved area, there is also the problem that the magnetic flux density B8 decreases by up to about 1% before and after the groove formation.

[0011] The present invention has been developed in light of the above-mentioned current situation, and aims to propose a grain-oriented electrical steel sheet that controls magnetic domain structure to reduce iron loss, which maintains the iron loss reduction effect even after stress relief annealing is performed, and which suppresses an increase in noise when used in transformer cores. [Means for solving the problem]

[0012] The inventors have newly discovered that when a laser is linearly irradiated onto the surface of a steel sheet after secondary recrystallization, which has accumulated in the Goss orientation, in a direction intersecting the rolling direction of the steel sheet (for example, a direction perpendicular to the rolling direction) and the irradiated area is locally melted, a resolidified structure different from the original Goss orientation structure can be formed, and that this resolidified structure can produce a magnetic domain refinement effect.

[0013] Further investigation revealed that, although so-called grooves can be formed depending on the laser irradiation conditions, when using the resolidified structure for magnetic domain refinement, the formation of grooves is not necessarily effective, and rather has a greater adverse effect in that the magnetic flux density decreases as the cross-sectional area of ​​the steel plate is reduced due to the grooves (depressions).

[0014] Furthermore, when grooves are formed, the steel is removed from the groove area and into the surrounding area, causing burrs that can degrade the space factor and insulation resistance. Therefore, it has become clear that conditions in which very shallow grooves, i.e. no even certain irregularities, are formed on the steel sheet surface, are more advantageous in terms of improving magnetic flux density.

[0015] Here, the resolidified structure in the present invention refers to a solidified structure formed by melting and resolidifying a structure and having an orientation different from the original crystal orientation. This differs from a structure obtained by a conventional non-heat-resistant strain-introducing type magnetic domain refinement technique as described in the above-mentioned Patent Document 1, in which a linear strain distribution caused by rapid heating and quenching by laser irradiation is left behind, and the original crystal orientation is maintained without melting the structure.

[0016] Furthermore, when using laser light, the team conducted extensive research into the irradiation conditions for laser light that would allow the incident energy to be efficiently absorbed by the base steel and melt the steel while suppressing spattering. As a result, they discovered that by irradiating the steel with a ring-mode fiber laser light that combines two or more laser lights with different energy intensities, it is possible to form a molten zone without affecting the decrease in magnetic flux density, i.e., without causing almost any unevenness on the steel plate surface. Furthermore, it is also effective to irradiate the target surface solely with a laser beam called a flat-top laser beam, which is not focused, has a uniform intensity distribution on the irradiated surface, and has a relatively large beam radius.

[0017] In addition, it was found that by using a green laser, called the second harmonic, which has half the wavelength at 0.53 μm, or a UV laser, which is the third and fourth harmonic and has wavelengths of 0.36 μm and 0.27 μm respectively, the absorption efficiency is good due to the short wavelength, and spatter is less likely to occur, so the surface flatness of the steel plate can be maintained more effectively.

[0018] A similar effect can also be obtained by electron beam irradiation. The wavelength of an electron beam is extremely short compared to laser light, and the absorption efficiency into the steel sheet is even higher. In addition, it is not necessary to combine two or more beams to obtain the above effect. It has been confirmed that there are irradiation conditions that can form a molten part that can obtain the above effect without causing large irregularities on the steel sheet surface by appropriately combining and adjusting the acceleration voltage, beam current, and radial energy distribution called the beam profile, and focusing coils that play the role of electromagnetic lenses.

[0019] Furthermore, it was confirmed that when an insulating coating was baked on both sides of the steel sheet at about 800°C after irradiation with laser light or electron beam, the residual distortion introduced by the irradiation was eliminated to a certain extent. Specifically, when the magnetostrictive vibration waveforms before and after baking of the insulating coating were compared, the magnetostrictive waveform after baking had reduced harmonic components and was closer to the waveform before irradiation, suggesting that this is advantageous for reducing noise in transformers.

[0020] The development history of the present invention will now be described in detail. The steel was cold-rolled to a final thickness of 0.23 mm and decarburized to less than 10 ppm by mass by decarburization annealing. An annealing separator mainly composed of MgO was then applied and final annealing was performed which served both as secondary recrystallization and purification, to prepare grain-oriented electrical steel samples mainly composed of 3.4% Si and 0.08% Mn and having an average magnetic flux density B8 of 1.935 T.

[0021] Next, the laser irradiation conditions were fixed at a laser scanning speed of 10 m / s, the oscillation output was varied from 100 W to 300 W, and the focus and energy profile were adjusted to create three groups of materials with different irradiation levels: Group 1, a level at which thermal residual distortion was introduced but the base steel did not melt; Group 3, a level at which linear grooves were formed in the base steel; and Group 2, a level at which melting marks were visible but no grooves were formed, with an incident energy intermediate between the two.

[0022] Half of the samples in each group were irradiated with a ring-mode fiber laser in a line pattern at 5 mm intervals perpendicular to the rolling direction on one side of the steel sheet at various power outputs, and then an insulating coating mainly made of magnesium phosphate and colloidal silica was applied to each side to a thickness of 2 μm and baked at 850°C for 1 minute. On the other hand, for the remaining half of the samples, an insulating coating was first baked on and then the laser was irradiated under the same conditions as the former half.

[0023] Group 1 corresponds to the well-known non-heat-resistant strain-introducing magnetic domain refinement process described in Patent Document 1 etc. Group 3 corresponds to the magnetic domain refinement process that forms linear grooves that are about 1 / 10 of the sheet thickness as disclosed in Patent Document 4 etc.

[0024] The magnetic flux density B8 and iron loss W of the steel plate thus obtained were measured using a 500 mm square SST (single plate magnetic tester). 17 / 50 The results are summarized in Table 1.

[0025] [Table 1]

[0026] As shown in Table 1, Group 1 is characterized by the fact that the magnetic flux density B8 changes very little before and after the magnetic domain refinement process. In addition, the best iron loss value was obtained on average when laser irradiation was performed after the insulating coating. Conversely, if the insulating coating is baked after the laser irradiation, the induced thermal residual strain disappears due to the baking process at 850°C, the magnetic domain refinement effect is lost, and no iron loss improvement effect can be obtained.

[0027] On the other hand, Group 3 shows a significant decrease in magnetic flux density B8 after the magnetic domain refinement process. This is because linear grooves are formed perpendicular to the rolling direction, reducing the effective cross-sectional area of ​​the magnetic flux flowing inside the steel sheet. This decrease in magnetic flux density is an unavoidable phenomenon when using the so-called heat-resistant magnetic domain refinement method. On the other hand, if the groove depth is made shallower to suppress the decrease in magnetic flux density, the iron loss reduction effect is reduced. However, unlike Group 1, it is not fundamentally affected by heat treatment. Also, in group 3, the further reduction in iron loss value was observed when laser irradiation was performed after insulation coating, which is presumably due to the overlapping effect of the thermal residual strain caused by laser irradiation in addition to the groove formation effect.In contrast, when laser irradiation was performed first and then insulation coating baking was performed, the effect of the residual strain was lost and it was confirmed that the iron loss value increased slightly.

[0028] Furthermore, group 2 has a large variation in magnetic flux density B8, generally falling between group 1 and group 3, although there are some conditions under which almost no decrease in magnetic flux density B8 is observed. The iron loss values ​​are also basically intermediate between group 1 and group 3, but the best iron loss values ​​are obtained under some conditions.

[0029] From the above test results, it was found that there exist irradiation conditions that realize ideal magnetic properties, i.e., small decrease in magnetic flux density B8 and large iron loss reduction effect. The product obtained using these irradiation conditions corresponds to the grain-oriented electrical steel sheet of the present invention, which has low iron loss and excellent noise characteristics.

[0030] The inventors clarified the characteristics of the material according to the present invention from the results of measuring the crystal orientation distribution in the vicinity of the laser irradiated area and the flatness of the base steel surface. First, the crystal orientation distribution in the vicinity of the laser irradiated portion will be described. In the above test, in order to investigate the reason why an iron loss reduction effect was observed even though no groove-like depressions were present, the local orientation distribution of secondary recrystallized grains near the irradiated area was measured using EBSD (electron backscatter diffraction).

[0031] As a result, the crystal structure of Group 2 can be regarded as a single crystal with a size of about 10 mm, i.e., the crystal grains that provide excellent magnetic properties in the rolling direction, i.e., the so-called Goss orientation grains. However, in an area of ​​about 50 μm wide and 20 μm deep, estimated to be the area affected by the laser irradiation, minute rotations with a crystal orientation misorientation angle of 0.5 to 3.0 degrees were observed. That is, it is presumed that the crystal structure of Group 2 was obtained when the base steel was locally melted by the incident energy and then solidified again. In other words, it is considered that the once-melted area solidified while being influenced by the crystal orientation of the surrounding area, resulting in a crystal orientation that was relatively close to that of the surrounding area.

[0032] Here, at the incident energy level of Group 1, the crystal lattice may be distorted by thermal strain, but crystal rotation does not occur. In other words, when the rotation of the crystal orientation (crystal misorientation angle) is less than 1.5 degrees, no significant magnetic domain refinement effect is obtained. On the other hand, although the upper limit of the rotation angle (crystal misorientation angle) has not been determined, if the incident energy is increased and the melted region is enlarged too much, the amount of unevenness on the base steel surface increases, causing localized sputtering and evaporation of the crystal structure, making it impossible to evaluate the rotation angle.

[0033] Next, the flatness of the surface of the base steel will be described. In the above test, when the average unevenness was less than 5 μm, there was almost no decrease in magnetic flux density B8. On the other hand, when the average unevenness was 5 μm or more, not only did the magnetic flux density B8 decrease due to the dents, but also the occurrence of bank-like rises around the dents caused the insulating coating to become partially thinner, reducing insulation, and in transformer cores using laminated steel sheets, it led to a decrease in the space factor. In the above test, the amount of unevenness on the surface of the base steel was evaluated by measuring the difference between the highest and lowest points on the cross section near the irradiated area using a three-dimensional laser displacement meter from the surface, and averaging the differences. From the above considerations, it was found that the two main factors of the slight crystal rotation (crystal orientation difference) mentioned above producing the magnetic domain refinement effect and the small amount of surface roughness are the main reasons why the magnetic flux density B8 of the sample does not decrease.

[0034] In addition, because the crystal orientation itself has rotated, the crystal orientation will not change unless it is heated again to a temperature at which the crystals melt. Therefore, for example, even if stress relief annealing is performed for three hours at 800°C, as required for wound transformer cores, it was thought that the magnetic domain refinement effect would continue without being lost.

[0035] Next, for the materials in Group 2 that had been laser irradiated after insulating coating, an insulating coating based on magnesium phosphate, which does not contain colloidal silica, was baked to a thickness of 0.5 μm only on the irradiated surface at various temperatures ranging from 300°C to 800°C, also in order to ensure the insulation of the irradiated area. The effects of residual stress due to laser irradiation and the effects on noise characteristics when used as transformer cores were evaluated.

[0036] In the present invention, the residual stress is determined by measuring the three-dimensional stress distribution in the rolling direction (RD), transverse direction (TD), and direction normal to the sheet surface (ND) using the Wilkinson method, which calculates the amount of lattice strain from the distortion of the diffraction pattern obtained from the crystal lattice of the base steel by applying EBSD, and taking the maximum value as the residual stress.

[0037] The sample was also sheared at an angle to the core size of 100mm wide, 300mm at the top, and 500mm at the bottom, and the four sides were combined to create a 500mm square single-phase model transformer, and the relationship between residual stress and transformer characteristics was investigated. The laminate thickness of the model transformer was approximately 30mm, and the mass of the electromagnetic steel sheets used was approximately 50kg. Noise was measured with a surface pressure of 1.0kgf / cm2 on the entire surface of the core. 2 A load of 1.7T was applied, a condenser microphone was placed 150mm above the center of the leg, and the average value of the four points was taken. The noise measurement was performed under a no-load excitation condition of 1.7T and 50Hz, and A-scale correction was applied as a hearing correction, and the overall value was compared. The above residual stresses and the magnetic and noise characteristics of the single-phase transformer are summarized in Table 2.

[0038] [Table 2]

[0039] As shown in Table 2, the lower the baking temperature, the greater the variation in the transformer's iron loss value and the louder the noise, but baking at 700°C or higher reduced the variation in the iron loss value and the noise level. The maximum residual stress near the irradiated area also showed a similar trend. This is thought to be because the thermal distortion introduced by the laser irradiation disappeared due to the baking process, and the residual stress was alleviated. It was presumed that the change in noise level was also due to the same cause.

[0040] Generally, as the harmonic components of magnetostrictive vibrations caused by AC excitation increase, transformer noise increases. However, as the baking temperature increases, the residual stress is alleviated, reducing the harmonic components and noise. Regarding transformer core loss, a low core loss value was shown under the baking condition of low temperature below 600°C, which is the best value within the variation. This is presumably because the effect of magnetic domain refinement due to thermal distortion caused by residual stress is superimposed on the effect of crystal orientation rotation.

[0041] Based on the above experimental results, the present invention has been arrived at. That is, the gist of the present invention is as follows. 1. A grain-oriented electrical steel sheet comprising, by mass, 2.0 to 8.0% Si, 0.005 to 1.000% Mn, and 0.0050% or less C, with the balance being Fe and unavoidable impurities, and on at least one of the front and back surfaces of the steel sheet, a local region which extends linearly in a direction transverse to the rolling direction of the steel sheet and has a misorientation angle of 1.5 degrees or more with surrounding crystals, the local region having a volume fraction of 0.1% or more and 2.0% or less and a residual stress of 100 MPa or less, and the average amount of unevenness on the surface of the base steel on the side having the local region is less than 5 μm.

[0042] 2. The grain-oriented electrical steel sheet according to 1 above, wherein the chemical composition further contains, by mass%, at least one selected from Ni: 0.01-1.50%, Cr: 0.01-0.50%, Cu: 0.01-0.50%, Bi: 0.01-0.50%, Sb: 0.01-0.20%, Sn: 0.01-0.20%, Mo: 0.01-0.20%, P: 0.01-0.20% and Nb: 0.001-0.015%. Effect of the Invention

[0043] According to the present invention, by forming a local region having a predetermined misorientation angle, controlling the volume fraction and residual stress of the local region, and further controlling the average amount of unevenness on the surface of the base steel having the local region, it is possible to further reduce iron loss compared to the conventional method even after stress relief annealing, and also to achieve low noise when used as a transformer core. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0044] The reasons for limiting the constituent elements of the present invention will be described below. First, the composition of the material of the grain-oriented electrical steel sheet (hereinafter also simply referred to as steel sheet or finished sheet) of the present invention will be described. Silicon is an element effective in increasing the electrical resistance of steel and improving iron loss, and a silicon content of 2.0 mass% or more is particularly effective in reducing iron loss. On the other hand, a silicon content of 8.0 mass% or less provides particularly excellent workability and magnetic flux density. Therefore, the silicon content is set to the range of 2.0 to 8.0 mass%.

[0045] Mn is an element that is advantageous in improving hot workability, but if the content is less than 0.005 mass%, the effect of adding it is small. On the other hand, if the content is 1.000 mass% or less, the magnetic flux density of the product sheet is particularly good. For this reason, the Mn content is set to the range of 0.005 to 1.000 mass%.

[0046] C content is limited to 0.0050% by mass or less, preferably 0.0030% by mass or less, because if it exceeds 0.0050% by mass, core loss increases due to magnetic aging.

[0047] Although the basic components of the present invention have been described above, the present invention can also contain other elements as optional components as described below. For the purpose of improving the magnetic flux density, at least one selected from Ni: 0.01-1.50%, Cr: 0.01-0.50%, Cu: 0.01-0.50%, Bi: 0.01-0.50%, Sb: 0.01-0.20%, Sn: 0.01-0.20%, Mo: 0.01-0.20%, P: 0.01-0.20%, and Nb: 0.001-0.015% may be contained in mass %. If the amount of each added is less than the lower limit, the effect of improving the magnetic properties is poor, while if the amount exceeds the upper limit, the development of secondary recrystallized grains is inhibited, and the magnetic properties are deteriorated. The remainder other than the above components is Fe and unavoidable impurities that may generally be mixed in during the manufacturing process.

[0048] Next, the reasons for limiting the properties of the steel sheet according to the present invention will be described. A localized region (melt-resolidified region) that extends linearly in a direction transverse to the rolling direction of the steel plate and has a misorientation angle of 1.5 degrees or more with the surrounding crystals. The grain-oriented electrical steel sheet of the present invention has a heat-resistant iron loss reduction effect even though it does not have groove-shaped depressions. To achieve this, it is necessary that at least one of the front and back surfaces of the steel sheet has a local region having a crystal misorientation angle (rotation angle) of 1.5 degrees or more with the surrounding crystals. If the crystal misorientation angle of the crystal orientation is less than 1.5 degrees, the effect of dividing the magnetic domains by the local region to generate magnetic poles is small, so no significant magnetic domain refinement effect can be obtained. On the other hand, although there is no particular upper limit for the crystal misorientation angle, if the incident energy is increased to make the melting region too large, the amount of unevenness on the steel sheet surface increases, and the crystal structure is locally sputtered and evaporated. Therefore, the upper limit of the crystal misorientation angle is about 10 degrees, which is the upper limit that can be actually measured.

[0049] In the present invention, the crystal misorientation angle can be determined as an average value by measuring the crystal orientations in a two-dimensional mesh with 0.1 μm intervals using EBSD (electron backscatter diffraction).

[0050] In the present invention, it is preferable that a plurality of the local regions extending linearly in a direction transverse to the rolling direction are present at intervals in the rolling direction. In the present invention, the term "linear" may be either a straight line or a curved line, and includes not only solid lines but also dotted lines, dashed lines, etc. Furthermore, the term "direction transverse to the rolling direction" refers to an angle range of ±30 degrees with respect to the direction perpendicular to the rolling direction.

[0051] Volume fraction of local area: 0.1% to 2.0% The volume fraction of the local region is 0.1% or more and 2.0% or less with respect to the entire steel sheet. Furthermore, if the crystal orientation difference between the local region and the surrounding area in the boundary region between the local region and the surrounding area is not discontinuous, the effect tends to be poor. In the present invention, the volume fraction is an average value determined in five or more observation regions each including two or more linearly extending local regions, and is regarded as the value for the entire steel sheet. If the volume fraction of the localized region where the crystal has rotated due to melting and resolidification and has a misorientation angle of 1.5 degrees or more from the surrounding area is less than 0.1%, the effect is poor. If it is more than 2.0%, magnetostrictive vibration under AC excitation becomes large, and the noise reduction effect is lost when used in a transformer core.

[0052] Residual stress in localized area: 100MPa or less In the present invention, from the viewpoint of achieving both low iron loss and low noise, the maximum residual stress in the localized regions, whether tensile or compressive, must be 100 MPa or less.

[0053] Average unevenness of the base metal on the surface with localized areas is less than 5 μm When the average unevenness of the base steel on the surface having the localized region is less than 5 μm, there is almost no decrease in magnetic flux density B8, and the effects of the present invention can be advantageously obtained. On the other hand, when the average unevenness is 5 μm or more, a bank-like protrusion (convex portion) occurs around the depression. When such a protrusion occurs, not only does the magnetic flux density B8 decrease due to the depression, but it can also make the insulating coating thinner in parts, reducing insulation, and in transformer cores that use laminated steel sheets, it can cause a decrease in the space factor. The average unevenness is preferably less than 3 μm. On the other hand, the average unevenness may be 0 μm, but is industrially about 0.3 μm or more.

[0054] The average unevenness of the steel substrate surface is evaluated by measuring the difference between the highest and lowest points on the cross section near the irradiated areas at five locations in an area that includes five or more irradiated areas (localized regions) using a three-dimensional laser displacement meter from the steel substrate surface, and calculating the average. Note that the vicinity of the irradiated areas refers to a range of 1.0 mm from the center of the irradiated areas.

[0055] As described above, in the present invention, it is believed that the crystal rotation produces the magnetic domain refinement effect, and the small amount of surface unevenness is the main factor in preventing a decrease in magnetic flux density B8, thereby achieving the effects of the present invention. In addition, because the crystal orientation itself rotates in the localized region, the crystal orientation will not change unless it is heated again to a temperature at which the crystals melt. Therefore, the present invention also has the effect that the magnetic domain refinement effect is maintained without being lost even when stress relief annealing is performed at 800°C for three hours during the manufacturing process of wound transformer cores.

[0056] The depth of the local region of the present invention is preferably 50 μm or less from the surface of the steel sheet in the cross-sectional direction of the steel sheet (sheet thickness direction). If it is deeper than this, the treatment will cause recesses on the surface, which will reduce the magnetic flux density and increase magnetostrictive vibration, which may increase noise when used as an iron core of a transformer. It is more preferably 30 μm or less. On the other hand, the depth is preferably 2 μm or more, and more preferably 10 μm or more.

[0057] In addition, the local region of the present invention preferably has a width in the rolling direction of 10 μm or more and 500 μm or less. Outside this range, the iron loss reduction effect decreases. More preferably, it is 20 μm or more, and even more preferably, it is 50 μm or more. On the other hand, the width in the rolling direction is more preferably 250 μm or less, and even more preferably 200 μm or less. In addition, since the local regions may not be a simple rectangle or semicircle, in the present invention, the longest distance in the rolling direction in each local region is applied as the width in the rolling direction.

[0058] Furthermore, the local regions of the present invention preferably have a repeat interval in the rolling direction of about 0.5 mm to 20 mm, because if the repeat interval is less than 0.5 mm, the frequency of the local regions is too high, causing adverse effects on magnetic properties and noise properties, whereas if the repeat interval is more than 20 mm, the effect of the present invention cannot be clearly obtained.

[0059] In the present invention, an insulating coating may be formed on the surface of the base steel, if necessary. The insulating coating in the present invention may be a known tensile coating, for example, a glass coating mainly composed of a phosphate such as magnesium phosphate or aluminum phosphate and a low thermal expansion oxide such as colloidal silica. By forming the coating at a baking temperature of 700°C or higher and reducing the residual stress in the local region to 100 MPa or less, it is possible to achieve both low iron loss and low noise. The upper limit of the baking temperature is not particularly limited as long as it is within the range of conventional methods, but it is generally preferable to set the baking temperature at about 900°C, at which the glass coating does not fuse.

[0060] If an insulating coating is not applied, the residual stress in the local region cannot be reduced to 100 MPa or less by baking at a temperature of 700° C. or more. In that case, the residual stress in the local region can be reduced to 100 MPa or less by replacing the baking temperature with an annealing treatment at 500° C. for 1 minute or more.

[0061] It is also possible to combine this with a method to suppress the formation of the forsterite film, such as lowering the dew point during decarburization annealing, suppressing the generation of surface oxides mainly composed of SiO2 by using a non-decarburization atmosphere, adding chlorides to the additive assistants of the annealing separator, or changing the main component of the annealing separator itself to Al2O3 or CaO, thereby preventing the formation of the forsterite film.

[0062] In the present invention, the process for producing the grain-oriented electrical steel sheet can basically follow a conventionally known production process. The steel material adjusted to the above-mentioned composition may be made into a slab by a normal ingot casting method or continuous casting method, or a thin cast piece having a thickness of 100 mm or less may be produced directly by a continuous casting method. The slab is heated by a normal method and subjected to hot rolling, but it may also be subjected to hot rolling immediately after casting without heating. In the case of a thin cast piece, it may be hot rolled, or hot rolling may be omitted and the piece may be directly advanced to the subsequent process.

[0063] The preferred conditions are to anneal the hot-rolled sheet as necessary, and then cold roll it once or two or more times with intermediate annealing to obtain the final sheet thickness. Next, after decarburization annealing, an annealing separator mainly composed of MgO is applied, and then final annealing is performed to obtain a secondary recrystallized structure mainly composed of Goss orientation. If necessary, an insulating coating is applied to produce the product.

[0064] As a method for generating a crystal misorientation angle to obtain a magnetic domain refinement effect, it is effective to irradiate the steel sheet surface with the above-mentioned laser light or electron beam. This process can be performed either before or after baking of the insulating coating. Furthermore, even if a crystal misorientation angle is imparted before secondary recrystallization, the misorientation angle is alleviated during secondary recrystallization, so it is preferable to impart it after secondary recrystallization. However, since a certain degree of magnetic domain refinement effect can be expected, there is no problem with imparting it before secondary recrystallization.

[0065] The present invention is characterized in that there is no decrease in magnetic flux density after stress relief annealing, and low iron loss and good noise characteristics are obtained. The purpose of this stress relief annealing is to remove the strain introduced by slitting, bending, and other processes performed when manufacturing transformer cores, and in order to achieve this, annealing is generally performed for about 1 to 5 hours at a temperature in the range of about 700°C to 900°C.

[0066] Next, preferred irradiation conditions for a laser beam or an electron beam for locally melting and resolidifying the steel sheet surface to obtain the localized region will be described.

[0067] First, known magnetic domain refinement techniques using laser light include a so-called strain introduction type in which thermal strain is applied to the surface of a steel sheet to form regions with extremely high dislocation density and thereby narrow the magnetic domain width, and a groove introduction type in which grooves are directly formed on the surface of the base steel by irradiating it with high-energy laser light or the like, and magnetic poles are generated on the side surfaces of the grooves to narrow the magnetic domain width. The irradiation conditions of the present invention are intermediate between these two.

[0068] Under these irradiation conditions, the resolidified structure obtained by irradiating the base steel with laser light and locally melting the area near the surface has a crystal orientation different from the main Goss orientation of the secondary recrystallized grain group, and this resolidified structure creates a pseudo grain boundary effect, making it possible to narrow the magnetic domain width.

[0069] If the irradiation energy of the laser light is too large, the base metal on the surface of the steel sheet will be evaporated or sputtered, forming grooves. Even if grooves are not formed, if recesses are formed, burrs or convex banks will form around them, causing a decrease in the space factor, and the insulating coating formed thereon will become locally thin, causing a decrease in insulation and corrosion resistance. Therefore, it is preferable to avoid the formation of grooves and unevenness as much as possible.

[0070] Here, in order to efficiently melt the base steel locally without forming unevenness in the irradiated area of ​​the laser light, it is effective to combine two or more laser lights. Specifically, if the laser light is irradiated concentrically, the evaporation and sputtering of the base steel can be suppressed from spreading by increasing the intensity of the laser light in the center and decreasing the intensity of the laser light in the periphery, and only the central part can be efficiently melted. In addition to changing the energy density of the laser light, it is also effective to use laser lights with different wavelengths as a means of creating a difference in irradiation energy between the center and periphery of the laser light. In general, it is difficult to limit the energy range of the high-energy and low-energy laser lights, but a combination of laser lights with an energy range is selected such that a molten part is formed on the surface of the base steel and the unevenness of the surface of the base steel is 5 μm or less on average. It is also possible to use a laser beam called a flat-top laser beam, which has a uniform intensity distribution on the irradiated surface and a relatively large beam radius, by itself. Laser beams are usually focused to increase the energy density at the focal position, but by using a technology that converts the energy profile into a flat shape using optical techniques such as a beam shaper, the irradiated area can be melted uniformly. The use of such laser beams is also advantageous in suppressing surface irregularities.

[0071] Regarding the wavelength of the laser light, the shorter the wavelength, the higher the energy, which reduces reflection on the surface of the material and improves absorption by the material. Specifically, by using a laser light with a wavelength of 0.9 μm or less, the reflectance decreases and the absorption increases, making it easier to form a local molten part while suppressing sputtering. A laser light with a short wavelength is more effective when suppressing the formation of a forsterite film or when applying such a laser light irradiation technique to a steel sheet that has been subjected to a mirror finish treatment. On the other hand, the lower limit of the wavelength of the laser light is preferably set to 0.15 μm due to equipment restrictions.

[0072] The wavelength of the YAG laser, which is widely used because it is easy to narrow the laser beam, is 1.03 to 1.07 μm, and can be used in the present invention. However, green lasers, which are the second harmonic and have half the wavelength of 0.53 μm, and UV lasers, which are the third and fourth harmonic and have wavelengths of 0.36 μm and 0.27 μm, respectively, have good absorption efficiency and are less likely to produce sputter, so they are more advantageous from the viewpoint of maintaining surface flatness. Similarly, blue lasers with wavelengths of 0.44 to 0.49 μm using blue semiconductors, excimer lasers with wavelengths of 0.19 to 0.31 μm using halogen gas, etc. are also effective. On the other hand, with typical laser light with a wavelength of around 1 μm, if the steel plate surface is mirror-like or otherwise highly reflective, the laser light will be reflected, making it extremely difficult to have the base steel (inside the steel plate) absorb the energy and form a locally molten area.

[0073] The laser light output is a combination of two or more laser lights with different intensities, so it is difficult to specify the optimum conditions, but in general, the total heat per unit length is preferably 2 J / m or more and 50 J / m or less. The spot diameter of the laser beam is preferably 100 μm or less.

[0074] Meanwhile, with regard to the preferred conditions for the electron beam, as with laser light, a magnetic domain refining technique is known in which thermal distortion is introduced to control the magnetic domain structure, but in order to locally melt the Goss-oriented crystal grains inside the base steel, it is preferable to irradiate with a higher energy density than before. The penetration depth of the electron beam into the base steel depends on the electron acceleration voltage, and in the case of the present invention, an acceleration voltage of 60 kV or more is preferable.

[0075] The optimum condition for the beam current varies depending on the speed at which the beam is scanned along the steel sheet surface. One way to suppress the formation of burrs and grooves on the surface and reduce the amount of unevenness is to combine multiple focusing coils, which are equivalent to lenses in an optical system that converge the electron beam. This makes it possible to adjust the beam profile, which is the energy distribution of the electron beam, suppress the evaporation and sputtering of the base steel, and reduce the amount of unevenness on the surface.

[0076] Electron beams have an extremely short wavelength, and because increasing the acceleration voltage allows the electrons to penetrate deeper into the base steel, they are less likely to create unevenness on the surface compared to laser light, making it easier to form only a molten zone. Furthermore, with electron beams, less care needs to be taken with the forsterite coating than with laser light. Electrons are more strongly scattered by heavier elements than by lighter elements, resulting in interactions. Because the forsterite coating is composed of the light elements Mg, Si, and O (oxygen), the electron beam incident from the surface has little interaction with the forsterite coating. On the other hand, it interacts strongly with Fe, a heavy element that makes up the base steel, transferring energy between them, allowing the base steel to melt efficiently.

[0077] Regarding the manufacturing conditions for the grain-oriented electrical steel sheet not described above, any of them may be in accordance with conventional methods. The present invention will be further described below using examples, but the scope of the present invention is not limited to these examples. EXAMPLES

[0078] The grain-oriented electrical steel sheet, which had the composition shown in Table 3, the remainder being Fe and unavoidable impurities, and had a finish thickness of 0.23 mm and had completed secondary recrystallization by final annealing, was used as the sample steel sheet. One side of the sample steel sheet was continuously irradiated with various incident energies by changing the irradiation interval perpendicular to the rolling direction using a ring mode fiber laser with a wavelength of 1.07 μm and a green laser with a wavelength of 0.53 μm. Since the incident energy depends on the laser output and scanning speed, it was organized in terms of energy per unit length. For the ring mode fiber laser, the balance of the strength on the inside and outside was adjusted to find the condition that would minimize the amount of surface unevenness, and irradiation was performed. After that, an insulating coating consisting of 50% colloidal silica and aluminum phosphate was applied and an insulating coating treatment was performed by baking at 850°C.

[0079] The average value of the properties in the vicinity of the laser irradiated area of ​​the steel sheet thus obtained was measured. Regarding the crystal misorientation angle distribution, the KAM map method of EBSD was used to extract the area (local area) where the crystal misorientation angle differed from the surroundings by 1.5 degrees or more, and the volume fraction was calculated at the same time. In addition, the residual stress was evaluated by the Wilkinson method of EBSD, and the surface unevenness was evaluated by a three-dimensional laser displacement meter. Note that the condition where the laser irradiation energy was too large and grooves were dug was outside the scope of the present invention, and the crystal misorientation angle could not be measured, and the volume fraction of the area could not be calculated, so it is indicated as -* in Table 3.

[0080] The magnetic properties are AC iron loss W 17 / 50 The B8 value and the magnetic flux density B8 value were measured. In order to evaluate the noise characteristics, the transformer was cut into a bevel size of 100 mm wide, 300 mm at the top, and 500 mm at the bottom, and a 500 mm square single-phase model transformer was created by combining the four sides, and noise measurements were performed under AC excitation of 1.7 T and 50 Hz. The measurement results were A-scaled for hearing correction and evaluated as an overall value. The above results are summarized in Table 3.

[0081] [Table 3]

[0082] As is clear from Table 3 above, good core loss and noise characteristics are obtained under conditions within the range of the present invention.

[0083] Nos. 1, 6, 11, and 13 are cases where the irradiation energy is too high, and residual stress of 100 MPa or more remains, so the iron loss value is relatively low, but the noise characteristics are poor due to the influence of residual distortion caused by the residual stress. No. 2 also has too high irradiation energy, so the average unevenness is high, and the noise characteristics are similarly poor.

[0084] On the other hand, Nos. 4, 5, 9, 10, 17, and 20 had insufficient irradiation energy and had excellent noise characteristics, but the azimuth angle difference was small due to insufficient melting of the structure, and the volume fraction of the obtained local area was insufficient, so the magnetic domain refinement effect was small and sufficient reduction in iron loss was not achieved.In addition, Nos. 8, 14, and 18, which had an excessively narrow irradiation interval and an excessively large volume fraction of the local area, both iron loss and noise were deteriorated. EXAMPLES

[0085] The sample steel sheet used was a grain-oriented electrical steel sheet with the composition shown in Table 4, the balance being Fe and unavoidable impurities, with a finished thickness of 0.23 mm, in which secondary recrystallization had been completed by final annealing. Both sides of the sample steel sheet were coated with a chromium-free insulating coat consisting of 40% colloidal silica and magnesium phosphate, and then baked at 900°C for an insulating coating treatment. One side of the sample steel sheet was then irradiated with electrons at 5 mm intervals perpendicular to the rolling direction, either continuously or in dot patterns with a pitch of 0.1 to 0.7 mm, using electron guns with accelerating voltages of 60 kV and 150 kV. In this example, for Nos. 3, 12, and 19, the irradiation interval was set to 2 mm.

[0086] Thereafter, the specimen was sheared to a sample size for various evaluations and stress relief annealed in a nitrogen atmosphere at 800°C for 3 hours. The obtained specimen was subjected to evaluation of properties in the vicinity of the electron beam irradiated region and evaluation of magnetism and noise using a single-phase model transformer in the same manner as in Example 1, and the results are summarized in Table 4. Note that conditions in which grooves were dug due to the electron beam irradiation energy being too large were outside the scope of the present invention, and the crystal orientation misorientation angle could not be measured, and the volume fraction of that region could not be calculated, so this is indicated as -* in Table 4.

[0087] [Table 4]

[0088] As shown in Table 4 above, regardless of whether the electron beam is irradiated continuously or in dots, good core loss and noise characteristics are obtained under conditions that have a crystal orientation angle, residual stress, and surface roughness that satisfy the requirements of the present invention. That is, in the invention examples Nos. 2, 4, 7, 8, 13, 14, and 20, the surface irregularities are all less than 5 μm, and no so-called grooves are formed, but a significant iron loss reduction effect is obtained even after stress relief annealing.

[0089] From the above, it can be seen from this embodiment that the present invention is significantly different from the previously known technology of forming physical grooves to maintain the magnetic domain refinement effect after stress relief annealing, and that the present invention is a completely new technique that utilizes the crystal rotated structure formed during melting and resolidification to obtain an advantageous iron loss reduction effect even after stress relief annealing.

Claims

1. A grain-oriented electrical steel sheet having a component composition containing, by mass%, 2.0 to 8.0% Si, 0.005 to 1.000% Mn, and 0.0050% or less C, with the balance being Fe and unavoidable impurities, the steel sheet having, on at least one of its front and back surfaces, a localized region which extends linearly in a direction transverse to the rolling direction of the steel sheet and has a misorientation angle of 1.5 degrees or more with surrounding crystals, the localized region having a volume fraction of 0.1% or more and 2.0% or less and a residual stress of 100 MPa or less, the average unevenness on the surface of the base steel on the side having the localized region being less than 5 μm.

2. The grain-oriented electrical steel sheet according to claim 1, wherein the chemical composition further contains, in mass%, at least one selected from Ni: 0.01 to 1.50%, Cr: 0.01 to 0.50%, Cu: 0.01 to 0.50%, Bi: 0.01 to 0.50%, Sb: 0.01 to 0.20%, Sn: 0.01 to 0.20%, Mo: 0.01 to 0.20%, P: 0.01 to 0.20%, and Nb: 0.001 to 0.015%.

Citation Information

Patent Citations

  • Novel precursor drug of biological activator containing mercapto group

    JP1982002252A

  • Manufacture of grain oriented magnetic steel sheet of low iron loss

    JP1986117218A

  • Copying device

    JP1991069968A

  • Production of grain oriented silicon steel sheet with low iron loss

    JP1997049024A

  • Low core loss grain-oriented electrical steel sheet and method for producing the same

    JP2007002334A