Wound cores and wound core transformers

A wound core with controlled gap length and end face roughness, combined with low-viscosity insulating oil, addresses the temperature rise issue at joints, enhancing cooling and insulation in transformers.

JP7582566B1Active Publication Date: 2024-11-13JFE STEEL CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024539828
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-07-25
Filing Date
2024-03-27
Publication Date
2024-11-13
Estimated Expiration
2044-03-27

AI Technical Summary

Technical Problem

The temperature rise around the joint portion of wound core transformers is significant due to high magnetic resistance at the joint, leading to in-plane eddy current loss and potential dielectric breakdown, which limits design freedom and insulation properties.

Method used

The solution involves manufacturing a wound core with a gap length of 0.10 mm or more at the joint, an average height of the steel plate end face of 50 μm or less, and using insulating oil with a kinematic viscosity of 50 mm²/s or less to enhance cooling capacity and suppress temperature rise.

Benefits of technology

This approach effectively suppresses temperature rise at the joint, maintains insulation properties, and increases design flexibility, including miniaturization possibilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007582566000003
    Figure 0007582566000003
  • Figure 0007582566000004
    Figure 0007582566000004
  • Figure 0007582566000005
    Figure 0007582566000005
Patent Text Reader

Abstract

Provided is a wound core that is excellent in suppressing temperature rise around joints. A wound core having a wound shape in which a plurality of grain-oriented electromagnetic steel sheets are wound and overlapped in the sheet thickness direction, the wound core having a flat portion and a corner portion adjacent to the flat portion, at least a part of the flat portion having a joint where end faces in the winding direction of the grain-oriented electromagnetic steel sheets are butted against each other, the gap length of the joint being 0.10 mm or more, and the average height Rc of the end faces being 50 μm or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to wound cores and wound core transformers. [Background technology]

[0002] The easy axis of magnetization of iron <001> Grain-oriented electrical steel sheets, which have a crystal structure in which the orientation is highly concentrated in the rolling direction of the steel sheet, are used for transformer cores. Transformers are broadly divided into stacked core transformers and wound core transformers based on their core structure. Stacked core transformers have a core in which steel sheets cut to a specific shape are stacked. On the other hand, wound core transformers have a core in which steel sheets are wound in layers. There are various characteristics required for transformer cores, but low core loss is particularly important.

[0003] Low iron loss is also an important characteristic required for grain-oriented electrical steel sheets, which are the material for iron cores. Also, in order to reduce the excitation current in transformers and thereby reduce copper loss, the grain-oriented electrical steel sheets, which are the material, must have a high magnetic flux density. In general, the higher the degree of orientation concentration in the Goss orientation, the higher the magnetic flux density of the grain-oriented electrical steel sheets. Grain-oriented electrical steel sheets with high magnetic flux density have low hysteresis loss and excellent iron loss characteristics. In order to reduce the iron loss of grain-oriented electrical steel sheets, it is effective to increase the degree of orientation concentration in the Goss orientation as well as to reduce impurities in the steel.

[0004] However, there are limitations to controlling the crystal orientation and reducing impurities. Therefore, a technology has been developed to introduce nonuniformity into the surface of grain-oriented electrical steel sheets by physical methods, subdivide the magnetic domains, and reduce iron loss, that is, a magnetic domain refining technology. For example, Patent Document 1 and Patent Document 2 describe a heat-resistant magnetic domain refining method in which linear grooves of a predetermined depth are provided on the surface of the steel sheet. Patent Document 1 describes a groove forming method using a gear-type roll. Patent Document 2 describes a groove forming method using an etching process. These methods have the advantage that the magnetic domain refining effect does not disappear even when heat treatment is performed, and can be applied even when stress relief annealing is performed during the production of the iron core.

[0005] In a wound core having a joint, by using grain-oriented electrical steel sheets in which the iron loss has been reduced by the above-mentioned physical method, it is possible to greatly reduce the iron loss in the parts other than the joint. On the other hand, it is known that the iron loss in the joint is very large regardless of the properties of the grain-oriented electrical steel sheets, which are the material, due to the structure of the wound core. This is because the magnetic resistance of the gap formed at the joint is very large, so that the magnetic flux does not pass through the gap but passes to the adjacent steel sheets in the out-of-plane direction, resulting in in-plane eddy current loss. The large iron loss in the joint is converted into thermal energy, which causes a temperature rise around the joint. The temperature rise around the joint causes a decrease in the insulation of the insulating coating applied to the surface of the grain-oriented electrical steel sheets, which are the material, and ultimately causes insulation breakdown. If insulation breakdown occurs, it will cause the transformer core to burn out, so it is necessary to reliably prevent the insulation from decreasing due to this temperature rise.

[0006] One method for suppressing the temperature rise around the joint is to improve the cooling ability of the iron core. Patent Document 3 proposes a method in which one or more of the wound electromagnetic steel sheets are wound over the entire length of the longitudinal direction so as to be shifted in the width direction perpendicular to the longitudinal direction with respect to the electromagnetic steel sheets forming the other layers, thereby increasing the contact area with the oil or air, which is a cooling medium. Another method for suppressing the temperature rise at the joint is to suppress the increase in iron loss at the joint. Patent Document 4 proposes a method in which the positions of the joints (cut parts) are dispersed in the winding direction to reduce the magnetic flux density around the joints and suppress the increase in iron loss. These methods can suppress the temperature rise around the joints to a certain extent, but in order to increase the design freedom of the magnetic flux density, the iron core shape, etc., further suppression of the temperature rise is required. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Special Publication No. 62-53579 [Patent Document 2] Patent No. 2895670 [Patent Document 3] International Publication No. 2022 / 092101 [Patent Document 4] International Publication No. 2016 / 006314 Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention has been made in consideration of the above circumstances, and has an object to provide a wound core that is excellent in the effect of suppressing temperature rise around joints. [Means for solving the problem]

[0009] The cause of the temperature rise around the joints of the wound core is that the magnetic resistance of the gap formed at the joint is very large, so the magnetic flux does not pass through the gap but passes to the adjacent steel sheets in the out-of-plane direction, resulting in in-plane eddy current loss. Eliminating the gap at the joint is a very effective way to suppress the occurrence of this in-plane eddy current loss. However, because there are errors in the processing accuracy when manufacturing the core and in the accuracy of repeated winding, it is actually difficult to eliminate the gap at the joint when productivity is taken into consideration.

[0010] Therefore, we investigated ways to improve the cooling capacity of the iron core by actively passing insulating oil, which also serves as a cooling medium, through the gap at the joint.

[0011] A wound core with a length of 250 mm, width of 250 mm, width of 100 mm, and total weight of about 20 kg was produced using a Unicore manufacturing machine manufactured by AEM Co., Ltd., with two 45-degree bends at each corner. Grain-oriented electromagnetic steel sheet with a thickness of 0.23 mm and characteristics of magnetic flux density B8 = 1.91 T and iron loss W17 / 50 = 0.88 W / kg was used as the material. Here, B8 is the magnetic flux density at a magnetizing force of 800 A / m, and W17 / 50 is the iron loss at a frequency of 50 Hz and a maximum magnetic flux density of 1.7 T. The joining method for the wound core was step lap, and only the gap length of the joint was changed in the range of 0.01 to 20 mm. The number of laminated sheets was 200, and the number of turns of the primary and secondary coils was 40 turns. The excitation conditions were a frequency of 50 Hz and a magnetic flux density of 1.7 T.

[0012] Here, the configuration of the wound core that is the subject of the present invention will be described with reference to FIG. 9. As shown in FIG. 9, the wound core 1 is formed by winding a plurality of grain-oriented electromagnetic steel sheets M in the sheet thickness direction. When viewed from the side, the wound core 1 has a wound shape. Note that, here, viewed from the side, the wound core 1 is viewed in the width direction of the grain-oriented electromagnetic steel sheets M that constitute the wound core 1. The wound core 1 has a joint C where end faces E in the winding direction of the grain-oriented electromagnetic steel sheets M (length direction of the grain-oriented electromagnetic steel sheets M) are butted against each other. A gap (gap) G is formed in the joint C. In the present invention, the length (spacing) L of the gap G formed in the joint C is referred to as the gap length of the joint.

[0013] Next, the wound core prepared above was placed in the tank of an insulating oil circulation system as shown in Figure 1, and the temperature of the insulating oil flowing into the tank and the temperature of the insulating oil discharged from the tank were measured when the insulating oil was excited under the above excitation conditions. 2 1 includes a wound core 1 and insulating oil 2. The insulating oil circulation system simulates a wound core transformer equipped with a wound core 1 and insulating oil 2.

[0014] Figure 2 shows the relationship between the gap length at the joint in the wound core and the temperature difference between the insulating oil flowing into the tank and the insulating oil discharged from the tank (hereinafter referred to as the inflow / outflow oil temperature difference). It was observed that the inflow / outflow oil temperature difference tends to increase as the gap length at the joint increases. Figure 3 shows the relationship between the gap length at the joint and the iron loss of the wound core transformer when excited under the above excitation conditions. It was observed that the iron loss tends to increase as the gap length at the joint increases. The increase in iron loss was particularly noticeable when the gap length at the joint was 10 mm or more.

[0015] Given the increase in iron loss, the following two are considered to be the causes of the increase in the inflow / outflow oil temperature difference. (1) As the gap length of the joint increases, the iron loss of the joint increases, and this thermal energy is propagated to the insulating oil. (2) As the gap length of the joint increases, it becomes easier for the insulating oil to pass through the gap of the joint, and the thermal energy around the joint is more easily propagated to the insulating oil (improved cooling capacity). Here, taking into account cause (2), we decided to explore a method to efficiently pass the insulating oil through the gap of the joint.

[0016] In order to make it easier for air or liquid to pass through pipes, it is important to reduce energy loss (pressure loss) as much as possible, so it was thought that the unevenness of the end faces of the grain-oriented electrical steel sheets (hereinafter simply referred to as steel sheet end faces), which form the walls of the gap at the joint, would have an effect. Therefore, the steel sheet end faces were flattened and the change in the inflow / outflow oil temperature difference was investigated. Here, wire cutting was used to flatten the steel sheet end faces. In general, wire cutting processing makes it easier to obtain a flat surface than conventional shear cutting processing. Using the grain-oriented electrical steel sheets described above as the material, the end faces were processed by wire cutting and shear cutting, and then a wound core was manufactured by the method described above. The wound core manufactured was then placed in the tank of the insulating oil circulation system described above, and the relationship between the gap length at the joint and the inflow / outflow oil temperature difference when excited under the excitation conditions described above was investigated.

[0017] The relationship between the gap length at the joint and the inflow / outflow oil temperature difference for each processing method is shown in Figure 4. With wound cores made from grain-oriented electrical steel sheets processed by wire cutting, the inflow / outflow oil temperature difference increased when the gap length at the joint was 0.10 mm or more, especially compared to wound cores made from grain-oriented electrical steel sheets processed by the conventional shear cut method.

[0018] The reason for the increase in the inflow / outflow oil temperature difference is thought to be that the wire cutting process reduced the unevenness of the steel plate end surface, thereby reducing pressure loss, and that the insulating oil can more easily pass through the gap at the joint, thereby improving the cooling ability of the wound core.

[0019] Therefore, in order to improve the cooling capacity of the wound core, it is sufficient to reduce the unevenness of the steel sheet end faces that form the wall surfaces of the gap at the joint and set the gap length at the joint to 0.10 mm or more. Furthermore, when considering both the iron loss characteristics and cooling capacity of the wound core, it is considered more preferable to set the gap length at the joint to 0.10 to 10 mm.

[0020] Next, in order to clarify the relationship between the roughness of the steel sheet end surface and the inflow / outflow oil temperature difference, the roughness of the steel sheet end surface was changed. Here, the roughness of the steel sheet end surface was changed by adjusting the roughness of the emery polishing paper when polishing the steel sheet end surface, and the load and time during polishing. Using the above-mentioned grain-oriented electromagnetic steel sheet as a material, the roughness of the steel sheet end surface was changed by polishing with emery polishing paper, and then a wound core was manufactured by the above-mentioned method. Then, the wound core manufactured was placed in the tank of the above-mentioned insulating oil circulation system, and the relationship between the roughness of the steel sheet end surface and the inflow / outflow oil temperature difference when excited under the above-mentioned excitation conditions was investigated. Here, the gap length of the joint of the wound core was set to 0.10 mm. The roughness of the steel sheet end surface was measured in the area of ​​the sheet thickness × total width using a 3D laser roughness meter, and the average height Rc and arithmetic mean roughness Ra were obtained, respectively. In the present invention, the average height Rc and the arithmetic mean roughness Ra are values ​​measured in accordance with JIS B 0601:2013.

[0021] Figure 5 shows the relationship between the average height Rc of the steel plate end face and the inflow / outflow oil temperature difference. When the average height Rc of the steel plate end face is 50 μm or less, the inflow / outflow oil temperature difference increases significantly, and the cooling ability improves. Figure 6 shows the relationship between the arithmetic mean roughness Ra of the steel plate end face and the inflow / outflow oil temperature difference. No correlation was found between the arithmetic mean roughness Ra of the steel plate end face and the inflow / outflow oil temperature difference. From the above results, it became clear that it is very important to control the average height Rc of the steel plate end face. The reason why the average height Rc of the steel plate end face tended to correlate with the cooling ability of the wound core, while the arithmetic mean roughness Ra of the steel plate end face did not tend to correlate with the cooling ability of the wound core, is not clear, but is estimated as follows. In other words, the arithmetic mean roughness Ra is the average of the absolute values ​​of the heights of each concave and convex part from the reference plane, and is not easily affected by scratches on the measurement surface or external deposits attached during the production of the core. On the other hand, since the average height Rc uses the average height of each pair of adjacent concave and convex parts, it is possible to sensitively reflect their influence. Because pressure loss is also affected by such defects and external deposits, it is believed that only the average height Rc of the steel plate end face was found to have a correlation with the cooling capacity of the wound core.

[0022] It was thought that the kinetic viscosity of the insulating oil also had an effect on the reduction of pressure loss. A wound core was manufactured by the method described above using the grain-oriented electrical steel sheet described above as the material. The manufactured wound core was then placed in the tank of the oil circulation system described above and excited under the excitation conditions described above. Here, the kinetic viscosity of the insulating oil at 40°C was set to 1 to 100 mm. 2 / sec, and the relationship between the kinetic viscosity of the insulating oil and the inflow / outflow oil temperature difference was investigated. The gap length of the joint and the average height Rc of the steel plate end faces were set to the conditions of 0.10 mm gap length of the joint and 50 μm average height Rc of the steel plate end faces, which resulted in the greatest pressure loss among the conditions for which the effect had been confirmed to date.

[0023] Figure 7 shows the relationship between the kinetic viscosity of insulating oil and the inflow / outflow oil temperature difference. 2 / sec or less, the inflow / outflow oil temperature difference became larger. Therefore, the kinematic viscosity at 40°C was 50mm 2It can be said that a higher cooling capacity can be obtained in a wound core transformer using insulating oil with a kinetic viscosity of 10 mm / sec or less. 2 / sec or less.

[0024] There are two methods for manufacturing wound cores: one is to wind steel sheets and then press the corners to a specified curvature to form a rectangle, and the other is to form the corners by stacking steel sheets that have already been bent. Cores made using the former method are called Trancocores, and those made using the latter method are called Unicores or Duocores. Figure 10 shows schematic diagrams of Unicores and Trancocores. Here, we compared the core cooling capacity of wound core transformers using Unicores and Trancocores.

[0025] For the Unicore, an AEM Unicore manufacturing machine was used to produce two Unicores with two 45-degree bends at each corner, measuring 500 mm long x 500 mm wide x 100 mm wide, and weighing approximately 100 kg in total. One of them was annealed at 825°C for 3 hours in a DX gas atmosphere, and the other was not annealed. For the Trancocore, the core was wound around a mandrel to measure 500 mm long x 500 mm wide x 100 mm wide, weighing approximately 100 kg in total, and then pressed and annealed under the same conditions as the Unicore that had been annealed. The material used was a 0.23 mm thick grain-oriented electromagnetic steel sheet with heat-resistant magnetic domain refinement treatment and characteristics of B8=1.93T and W17 / 50=0.75W / kg. The joining method for the wound core was step lap, the gap length of the joining portion was changed in the range of 0.01 to 15 mm, and the processing conditions were adjusted so that the average height Rc of the steel sheet end face was 30 μm. The number of laminated sheets was 500, and the number of turns of the primary and secondary coils was 40 turns. The excitation conditions were a frequency of 60 Hz and a magnetic flux density of 1.7 T. As shown in Figure 1, the kinetic viscosity at 40°C was 5 mm 2 The wound core was placed in the tank of an oil circulation system using insulating oil of 10000 V / sec, and the oil temperature flowing into the tank and the oil temperature discharged from the tank were measured when the oil was excited under the above excitation conditions.

[0026] Figure 8 shows the relationship between the gap length of the joint and the inflow / outflow oil temperature difference for each wound core. The inflow / outflow oil temperature difference was larger for Unicore than for Trancocore, and the inflow / outflow oil temperature difference was larger for Unicore under the condition where stress relief annealing was not performed than under the condition where stress relief annealing was performed. The reason for this is thought to be as follows. Since Unicore introduces large strain locally, deformation twins remain even after stress relief annealing, and the magnetic permeability in the winding direction is lower than that of Trancocore. Therefore, it is thought that the amount of magnetic flux passing through the adjacent steel sheets in the out-of-plane direction increases around the joint, resulting in an increase in iron loss around the joint. When stress relief annealing is not performed, the magnetic permeability in the winding direction is lower, so the amount of magnetic flux passing through the adjacent steel sheets in the out-of-plane direction is thought to be the largest among the three conditions, and as a result, the inflow / outflow oil temperature difference is thought to be the largest. From the above results, it can be said that a wound core transformer using Unicore or Duocore with bent parts at the corners can achieve higher cooling capacity.

[0027] The present invention is based on the above findings, and the gist of the present invention is as follows. [1] A wound shape in which a plurality of grain-oriented electromagnetic steel sheets are wound in the sheet thickness direction, and the wound shape has a flat portion and a corner portion adjacent to the flat portion, A wound core, comprising: a joint in which end faces of the grain-oriented electrical steel sheets in the winding direction are butted against each other in at least a portion of the planar portion; a gap length of the joint is 0.10 mm or more; and an average height Rc of the end faces is 50 μm or less. [2] The wound core according to [1], wherein the corner portion has a bent portion. [3] A wound core transformer comprising the wound core according to [1] or [2] above and insulating oil. [4] The kinetic viscosity of the insulating oil at 40°C is 50mm 2 / sec or less. Effect of the Invention

[0028] According to the present invention, it is possible to provide a wound core that is excellent in the effect of suppressing a temperature rise around a joint.

[0029] According to the present invention, it is possible to effectively suppress temperature rise in the vicinity of the joints of the wound core and prevent a decrease in the insulating properties of the insulating coating due to temperature rise, thereby increasing the design freedom of the transformer, such as by increasing the design magnetic flux density or reducing its size. [Brief description of the drawings]

[0030] [Figure 1] FIG. 1 is a schematic diagram of the insulating oil circulation system used in the experiment. [Diagram 2] FIG. 2 is a diagram showing the relationship between the gap length of the joint and the inflow / outflow oil temperature difference. [Diagram 3] FIG. 3 is a diagram showing the relationship between the gap length of the joint and the transformer iron loss W17 / 50. [Figure 4] FIG. 4 is a diagram showing the relationship between the gap length at the joint and the inflow / outflow oil temperature difference for each wound core manufactured using grain-oriented electrical steel sheet processed by wire cutting and shear cutting. [Diagram 5] FIG. 5 is a diagram showing the relationship between the average height Rc of the steel sheet end face and the inflow / outflow oil temperature difference. [Figure 6] FIG. 6 is a diagram showing the relationship between the arithmetic mean roughness Ra of the steel sheet end face and the inflow / outflow oil temperature difference. [Figure 7] FIG. 7 is a graph showing the relationship between the kinetic viscosity of insulating oil at 40° C. and the inflow / outflow oil temperature difference. [Figure 8] FIG. 8 shows the relationship between the gap length of the joint and the inflow / outflow oil temperature difference when Unicore and Trancocore are used. [Figure 9] FIG. 9 is a schematic diagram illustrating the configuration of the wound core. [Figure 10] FIG. 10 is a schematic diagram (side view) showing the unicore and the trancocore. [Figure 11] FIG. 11 is a schematic diagram showing the positions where thermocouples were attached (temperature measurement positions) in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0031] As described above, in order to effectively suppress the temperature rise around the iron core joints, the following requirements must be met.

[0032] <Wound core> [A] A wound shape in which multiple grain-oriented electromagnetic steel sheets are wound and stacked in the sheet thickness direction, and has a flat portion and a corner portion adjacent to the flat portion. [B] At least a part of the flat portion has a joint where end faces of the grain-oriented electrical steel sheets in the winding direction are butted against each other, and the gap length of the joint is 0.10 mm or more, more preferably 0.10 to 10 mm. [C] The average height Rc of the end faces is 50 μm or less, and more preferably 10 μm or less.

[0033] The method for manufacturing the wound core is not particularly limited, and for example, a known method can be used. More specifically, Unicore and Duocore, which have bent corners, can be manufactured using a Unicore manufacturing machine manufactured by AEM. In this case, when a design drawing is loaded into the manufacturing machine, processed steel sheets are sheared and bent to the size according to the design drawing, and the processed steel sheets (material) are wound and stacked in the thickness direction to manufacture the wound core. After the wound core is manufactured, stress relief annealing may or may not be performed.

[0034] On the other hand, Trancocore, which has curved corners, is made by rolling out a coil of directional electromagnetic steel sheet, cutting each turn, winding it around a circular winding die, and winding it in the thickness direction. After that, a forming die is pressed against the inside and outside of the wound core material to give it the desired winding shape, and then stress relief annealing is performed.

[0035] In either manufacturing method, the method of controlling the gap length of the joint is not particularly limited. For example, when the grain-oriented electromagnetic steel sheet as the material is sheared for each turn, the gap length of the joint can be controlled within the range of the present invention by setting the length in the winding direction slightly shorter than the designed length of one turn. In addition, the gap length of the joint can be controlled within the range of the present invention by a method of adjusting the binding force or tightening force of a cable tie or tightening jig that integrally fixes the wound grain-oriented electromagnetic steel sheets. As described above, in the present invention, the gap length of the joint is 0.10 mm or more. The gap length of the joint is preferably 0.50 mm or more. In addition, the gap length of the joint is preferably 20 mm or less, more preferably 15 mm or less, even more preferably 10 mm or less, and even more preferably 5 mm or less.

[0036] The method of controlling the average height Rc of the steel plate end face is not particularly limited. For example, in the case of shear processing, which is a general processing method, the average height Rc of the steel plate end face can be controlled within the range of the present invention by adjusting the clearance, adjusting the surface roughness of the shear blade, brush grinding after shearing, etc. In addition, even in the case of processing using a laser beam, etc., the average height Rc of the steel plate end face can be controlled within the range of the present invention by changing the laser output and scanning speed to adjust the thermal energy introduced into the steel plate. It is more preferable to incorporate a process of measuring the average height Rc of the steel plate end face into the manufacturing process of the wound core. As described above, in the present invention, the average height Rc of the steel plate end face is 50 μm or less. The average height Rc of the steel plate end face is preferably 25 μm or less, more preferably 10 μm or less, and even more preferably 5 μm or less. On the other hand, the lower limit of the average height Rc of the steel plate end face is not particularly limited, but as an example, the average height Rc of the steel plate end face is 0.5 μm or more.

[0037] In the present invention, as long as the gap length of the joint and the average height Rc of the steel sheet end faces are controlled within the ranges of the present invention when producing a wound core, there are no particular limitations on the core structure, such as the core size and joining method. In addition, when the wound core has bent portions at the corners, there are no particular limitations on the core structure, such as the bending angle of the bent portions at the corners and the number of bent portions.

[0038] As an example, a method for manufacturing a wound core of the present invention can include the steps of measuring the average height Rc of the end faces of grain-oriented electromagnetic steel sheets, preparing as raw materials a plurality of grain-oriented electromagnetic steel sheets whose average end face height Rc is within the range of the present invention, and winding and stacking the grain-oriented electromagnetic steel sheets prepared as raw materials in the above steps to form a wound core. In the step of forming the wound core, the gap length of the joint is controlled within the range of the present invention, for example as described above.

[0039] <Grain-oriented electrical steel sheet> In the present invention, the grain-oriented electromagnetic steel sheet used as the material for the wound core is not particularly limited. The thickness of the grain-oriented electromagnetic steel sheet may be appropriately selected depending on the application. The thickness may be, for example, 0.15 mm or more, and may be 0.18 mm or more. The thickness may be, for example, 0.35 mm or less, and may be 0.27 mm or less. The thickness may be, for example, in the range of 0.15 to 0.35 mm, and may be in the range of 0.18 to 0.27 mm.

[0040] The method of manufacturing the grain-oriented electrical steel sheet is not particularly limited. For example, a slab having a known chemical composition is heated at 1150 to 1450 ° C., hot-rolled, and then annealed at 900 to 1150 ° C. as necessary. Then, cold rolling is performed once or twice or more times with intermediate annealing, decarburization annealing is performed in a wet hydrogen atmosphere at 700 to 900 ° C., and nitriding is performed as necessary. Then, an annealing separator is applied, finish annealing is performed at 1000 to 1200 ° C., and an insulating coating is formed at about 900 ° C. As an example, the grain-oriented electrical steel sheet can be manufactured by the above method. It is also possible to perform a magnetic domain refining treatment using distortions or grooves on the grain-oriented electrical steel sheet by a known method. When performing distortion relief annealing during the production of a wound core, it is preferable to perform a groove-type magnetic domain refining treatment.

[0041] <Wound core transformer> The wound core transformer of the present invention includes the wound core and insulating oil. As described above, the insulating oil has a kinetic viscosity of 50 mm at 40° C. 2The insulating oil preferably has a kinetic viscosity of 10 mm / sec or less at 40°C. 2 The lower limit of the kinetic viscosity is not particularly limited, but as an example, the kinetic viscosity is 1 mm 2 / sec or more. EXAMPLES

[0042] Next, the present invention will be specifically described based on examples. The following examples are preferred examples of the present invention, and the present invention is not limited by these examples. The embodiments of the present invention can be appropriately modified within the scope of the gist of the present invention, and all of these modifications are included in the technical scope of the present invention.

[0043] [Example 1] A wound core with a weight of approximately 40 kg and a capacity of 30 kVA was produced using a 0.23 mm thick grain-oriented electromagnetic steel sheet (heat-resistant magnetic domain refinement material) with magnetic properties of B8 = 1.88 T and W17 / 50 = 0.68 W / kg and grooves formed on the surface of the steel sheet. The wound core was produced as follows. A coil-shaped grain-oriented electromagnetic steel sheet was dispensed and wound up on a circular winding mold while being cut into individual turns. Here, the steel sheet was cut 0.03 to 13.00 mm shorter than the designed circumference length during cutting, and the gap length of the joint was changed. Cutting was performed using a laser, and the laser processing conditions were a single mode fiber laser, a deflection speed of 10 m / sec, and the average height Rc of the steel sheet end surface was changed by changing the laser output from 0.5 to 10.0 kW. After that, the steel sheet was wound up, and the inside and outside of the core material that was wound in the thickness direction were pressed with a forming die to form the final wound shape, and then stress relief annealing was performed at 800°C for 3 hours in a N2 gas atmosphere to form a wound core. Table 1 shows the difference between the designed circumference length and the actual cut length, the gap length of the joint of each wound core, the laser output, and the average height Rc of the steel sheet end face that forms the joint of each wound core. After that, the wound core was once loosened and the coil was assembled, and at the same time, a thermocouple was attached around the joint to measure the temperature around the joint. The thermocouple was attached at the center of the width of the center joint of the wound core (the joint at the center of the thickness of the wound core), 5 mm from the steel sheet end face that forms the joint (see Figure 11). After the coil was assembled, the wound core was set in a tank and insulating oil was poured into it to form a wound core transformer. At this time, the kinetic viscosity of the insulating oil was changed by using different insulating oils. The kinetic viscosity of the insulating oil, the transformer loss, and the temperature around the joint are also shown in Table 1. The transformer was excited at 50 Hz and 1.7 T. The transformer loss and the temperature around the joint were measured by monitoring the temperature of the insulating oil and after the temperature became constant (after thermal equilibrium).

[0044] In Nos. 1 to 12, the gap length of the joint is short and outside the range of the present invention, so the temperature around the joint is high under all conditions. The reason why the average height Rc of the steel plate end face changes with the laser output is thought to be because when the output increases, the amount of melting on the steel plate end face, which is the laser processed surface, increases, and the molten material scatters and adheres to the processed surface again. In Nos. 13 to 24 and Nos. 25 to 36, it can be seen that the temperature rise around the joint is suppressed when the average height Rc of the steel plate end face is within the range of the present invention compared to those outside the range of the present invention. It can also be seen that the temperature around the joint is lower and the cooling capacity is higher when the average height Rc of the steel plate end face and the kinetic viscosity of the insulating oil are lower. Furthermore, the increase in transformer loss due to the increase in the gap length of the joint is also minimized, and it can be seen that both the transformer characteristics and the cooling capacity have been achieved. In Nos. 37 to 48, the gap length of the joint is large, so the transformer loss is inferior to Nos. 13 to 36. However, it is clear that when the average height Rc of the steel sheet end faces is within the range of the present invention, the temperature rise around the joint is sufficiently suppressed, and the object of the present invention is achieved.

[0045] [Table 1]

[0046] [Example 2] A wound core with a weight of about 500 kg and a capacity of 500 kVA was manufactured using a grain-oriented electromagnetic steel sheet with a thickness of 0.30 mm and magnetic properties of B8 = 1.93 T and W17 / 50 = 1.05 W / kg. The wound core was manufactured as follows. Using a Unicore manufacturing machine manufactured by AEM, the steel sheet was sheared according to the designed circumference length by shearing, the corner parts were bent in advance, and this was wound in the thickness direction to manufacture a wound core. Here, each corner part of the wound core was shaped to have two 45-degree bent parts. In addition, the average height Rc of the steel sheet end face was changed by changing the clearance during shearing. After that, the core was once loosened and the coil was installed, and then cable ties were installed to fix the wound grain-oriented electromagnetic steel sheet together. At this time, the tightening pressure of the cable ties was set to 0.01 to 1.00 kg / mm 2 The gap length of the joint was changed within the range. In addition, the core was loosened and the coil was assembled, and at the same time, a thermocouple was attached around the joint to measure the temperature around the joint in the same manner as in Example 1. After assembling the coil, the wound core was set in the tank and insulating oil was poured in to make a wound core transformer. At this time, the dynamic viscosity was changed by using different insulating oil. Table 2 shows the tightening pressure of the cable tie and the gap length of the joint, the clearance during shearing and the average height Rc of the steel plate end face, the dynamic viscosity of the insulating oil, the transformer loss, and the temperature around the joint. Here, the transformer was excited in the same manner as in Example 1, and the transformer loss and the temperature around the joint were measured.

[0047] In Nos. 37 to 48, the gap length of the joint is short and outside the range of the present invention, so the temperature around the joint is high under all conditions. For Nos. 13 to 24 and Nos. 25 to 36, it can be seen that the temperature rise around the joint is suppressed when the average height Rc of the steel plate end face is within the range of the present invention, compared to those outside the range of the present invention. It can also be seen that the temperature around the joint is lower and the cooling capacity is higher when the average height Rc of the steel plate end face and the kinetic viscosity of the insulating oil are low. Furthermore, it can be seen that the increase in transformer loss due to the increase in the gap length of the joint is also minimized, and it can be seen that both the transformer characteristics and the cooling capacity are achieved. For Nos. 1 to 12, the gap length of the joint is large, so the transformer loss is inferior to Nos. 13 to 36. However, it can be seen that the temperature rise around the joint is sufficiently suppressed when the average height Rc of the steel plate end face is within the range of the present invention, and the object of the present invention is achieved.

[0048] [Table 2]

Claims

1. The coil has a wound shape in which a plurality of grain-oriented electromagnetic steel sheets are wound in a thickness direction, and has a flat portion and a corner portion adjacent to the flat portion. a joint in which end faces in the winding direction of the grain-oriented electrical steel sheets are butted against each other in at least a part of the planar portion, a gap length of the joint being 0.10 mm or more, and an average height Rc of the end faces being 50 μm or less.

2. The wound core according to claim 1 , wherein the corner portion has a bent portion.

3. A wound core transformer comprising the wound core according to claim 1 or 2 and insulating oil.

4. The kinetic viscosity of the insulating oil at 40°C is 50 mm 2 4. The wound core transformer according to claim 3, wherein the winding current is equal to or less than 1000 Hz / sec.

Citation Information

Patent Citations

  • Three-phase three-dimensional non-circular open type wound iron core structure

    CN110136933A

  • Three-dimensional wound iron core heat radiation structure

    CN204155717U

  • Method and device for cutting iron core

    JP2002224916A