Sealing material composition
A sealant composition with controlled moisture removal and inkjet applicability forms a protective barrier for organic electronic devices, addressing oxidation and moisture issues to enhance durability and longevity.
Patent Information
- Application Number
- JP2022030015
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-04-28
- Filing Date
- 2022-02-28
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2038-04-30
AI Technical Summary
Organic electronic devices, particularly OLEDs, are susceptible to oxidation and moisture penetration, which affects their durability and longevity.
A sealant composition is developed that includes specific components and manufacturing processes to effectively block moisture and oxygen ingress, using a solvent-free formulation with controlled moisture removal, inkjet applicability, and a sealing structure comprising organic and inorganic layers.
The sealant composition provides enhanced durability and longevity of organic electronic devices by preventing moisture and oxygen penetration, ensuring reliable performance and reducing chemical damage.
Smart Images

Figure 0007582574000003 
Figure 0007582574000004 
Figure 0007582574000001
Abstract
Description
[Technical field]
[0001] Cross-reference to related applications This application claims the benefit of priority based on Korean Patent Application No. 10-2017-0055075, filed on April 28, 2017, the entire contents of which are incorporated herein by reference.
[0002] Technical Field The present application relates to an encapsulant composition, a method for making the same, an organic electronic device including the same, and a method for making the organic electronic device. [Background technology]
[0003] Organic electronic device (OED) refers to a device containing layers of organic materials that generate an alternating current of charge using holes and electrons, examples of which include photovoltaic devices, rectifiers, transmitters, and organic light emitting diodes (OLEDs).
[0004] Among the organic electronic devices, organic light emitting diodes (OLEDs) d e) Compared to conventional light sources, OLEDs consume less power and have a faster response speed, which is advantageous for making displays or lighting thinner. OLEDs also have excellent space utilization, and are expected to be applied in a variety of fields, including various portable devices, monitors, laptops, and televisions.
[0005] The most important problem in commercializing and expanding the use of OLEDs is their durability. Organic materials and metal electrodes contained in OLEDs are very easily oxidized by external factors such as moisture. Therefore, products containing OLEDs are highly sensitive to environmental factors. As a result, various methods have been proposed to effectively block the penetration of external oxygen or moisture into organic electronic devices such as OLEDs. Summary of the Invention [Problem to be solved by the invention]
[0006] The present application provides a sealant composition that can effectively block moisture or oxygen from entering an organic electronic device from the outside, thereby ensuring the life of the organic electronic device, and a method for producing the same. [Means for solving the problem]
[0007] The present application relates to an encapsulant composition and a manufacturing method thereof. The encapsulant composition may be manufactured by a manufacturing method of an encapsulant described below. The encapsulant composition may be an encapsulant applied to encapsulate or seal an organic electronic device such as an OLED. In one example, the encapsulant composition of the present application may be applied to encapsulate or seal the front surface of an organic electronic device. Thus, after the encapsulant composition is applied for encapsulation, it may be in the form of an organic layer that seals the front surface of an organic electronic device. In addition, the organic layer may be laminated on the organic electronic device together with an inorganic protective film and / or an inorganic layer described below to form an encapsulation structure.
[0008] In a specific example of the present application, the present application relates to an encapsulant composition for encapsulating an organic electronic device that is applicable to an inkjet process and a manufacturing method thereof, and the composition can be designed to have appropriate physical properties when discharged onto a substrate using an inkjet printer that is capable of patterning in a non-contact manner.
[0009] As used herein, the term "organic electronic device" refers to an article or device having a structure including an organic material layer that generates an alternating current of charge using holes and electrons between a pair of opposing electrodes, examples of which include, but are not limited to, photovoltaic cells, rectifiers, transmitters, and organic light-emitting diodes (OLEDs). In one example of the present application, the organic electronic device may be an OLED.
[0010] An exemplary method for producing the encapsulant composition may include a moisture removal step. The encapsulant composition undergoes a distribution and storage step before being applied to seal the organic electronic device. If moisture is present inside the composition or inside a container storing the composition, the encapsulant composition may lose its sealing function. Therefore, the encapsulant composition of the present application may be an encapsulant composition that has undergone a moisture removal step. The moisture removal step may include injecting an inert gas of 20 to 5,000 lpm (liter per minute), 30 to 4,300 lpm, 46 to 3,200 lpm, 58 to 2,800 lpm, 68 to 1,900 lpm, 80 to 1,800 lpm, 120 to 1,700 lpm, 150 to 1,500 lpm, 180 to 1,400 lpm, 188 to 1,300 lpm, or 192 to 1,250 lpm into the encapsulant composition in the container. The inert gas may be N2, which may be used for nitrogen sparging, but is not limited thereto. In the past, the process of removing moisture was carried out by repeatedly heating and cooling the sealant composition using a circulator and injecting an inert gas to remove moisture. However, in the process, a part of the sealant composition may volatilize or harden during the heating and cooling process, and in this case, the hardening proceeds with a composition different from the intended composition, resulting in a decrease in product reliability. The present application provides a sealant composition with excellent reliability by controlling the inert gas injection flow rate to remove moisture present in the sealant composition without heating or cooling.
[0011] The moisture removal step is not limited to the above and may further include passing the sealant composition through a moisture adsorbent. The method of passing the sealant composition through is not particularly limited and may include contacting the sealant composition with the moisture adsorbent.
[0012] In one example, the moisture removal step may be performed at a constant temperature. The constant temperature state means a state in which a temperature increase or cooling step is excluded. The constant temperature state means a state in which there is substantially no temperature change, and the state in which there is substantially no temperature change may have an error range of -5°C to 5°C or -3°C to 3°C relative to the set temperature. The set temperature may be any one of 20°C to 48°C. For example, the set temperature may be 21°C to 45°C, 22°C to 43°C, 23°C to 38°C, or 24°C to 32°C. The method for producing a sealant composition of the present application maintains the moisture removal step at a constant temperature, thereby preventing partial curing or partial volatilization, and thus maintaining the intended composition of the sealant composition to provide a highly reliable product. That is, the sealing material composition according to the present application has a specific compositional formulation described later, but when heated or cooled, some side reactions are promoted or phase separation occurs, resulting in poor coating characteristics (inkjetting). As a result, after application to an element, dark spots may occur during emission, which may cause a decrease in reliability.
[0013] In a specific example of the present application, the moisture removal step can include adjusting the pressure in the container to within a range of 600 to 760 mmHg, 610 mmHg to 720 mmHg, 630 mmHg to 710 mmHg, or 640 mmHg to 690 mmHg. By adjusting the pressure range in the moisture removal step, the present application can effectively remove moisture to a desired level.
[0014] In one example, the method for producing the sealant of the present application can include storing the sealant composition in a pouch after the moisture removal step. The pouch may be, but is not limited to, an aluminum pouch. By storing the sealant composition in a pouch, the present application can prevent atmospheric moisture from penetrating into the sealant composition during distribution and storage.
[0015] An exemplary sealant composition may include an epoxy compound. The sealant composition may be in a solvent-free form. The solvent-free form refers to a composition in a form that does not contain an organic solvent. The sealant composition may have a moisture content of 1000 ppm or less, 500 ppm or less, or 100 ppm or less as measured by Karl Fischer coulometric titration. The measurement may be measured for 100 mg of the composition, but is not limited thereto. The lower limit is not particularly limited and may be 0 ppm or 10 ppm. The moisture measurement may be performed at an operating temperature of 25° C., in a sealed container, and may be adjusted to an equivalent point of 50 mV within a suitable speed range of 0.3 to 2,240 μg / min. In the coulometric method, iodine is electrically generated from a generating electrode and reacts with water. At this time, the amount of moisture in the sample is calculated from the number of moles of electrons used to generate iodine. The measurement can be performed using Karl Fischer titrators-831 KF Coulometer-coulometric manufactured by Metrohm. By controlling the moisture content of the sealant composition before curing as described above, the present application can prevent chemical damage to an organic electronic device even when the sealant composition is directly applied to the organic electronic device, and can suppress the generation and growth of dark spots in the organic electronic device.
[0016] In one example, the amount of volatile organic compounds measured after curing of the encapsulant composition of the present application may be less than 100 ppm. The lower limit is not particularly limited and may be 0 ppm or 10 ppm. In the present specification, the volatile organic compounds may be expressed as outgassing. The volatile organic compounds may be measured after the encapsulant composition is cured and a cured sample is maintained at 110° C. for 30 minutes using Purge & Trap-gas chromatography / mass spectrometry. The measurement may be performed using a Purge & Trap sampler (JAI JTD-505III)-GC / MS (Agilent 7890b / 5977a) instrument. The application controls the amount of volatile organic compounds generated by the encapsulant composition as described above, thereby preventing chemical damage to the organic electronic device even when the encapsulant composition is directly applied to the device.
[0017] In a specific example of the present application, the encapsulant composition may include a compound having an oxetane group, the compound being in the range of 45 parts by weight to 145 parts by weight relative to 100 parts by weight of the epoxy compound. The epoxy compound may be a photocurable or thermosetting compound, and may be a photocurable compound in a specific example of the present application. The compound having an oxetane group may be included in the range of 45 parts by weight to 145 parts by weight, 48 parts by weight to 144 parts by weight, 63 parts by weight to 143 parts by weight, or 68 parts by weight to 142 parts by weight relative to 100 parts by weight of the epoxy compound. In this specification, the term "parts by weight" means the weight ratio between each component. By controlling the specific composition and its content range, the present application can form an organic layer on an organic electronic device by an inkjet method, and the applied encapsulant composition can provide an organic layer having excellent spreadability within a short time and excellent curing strength after curing. In one example, the encapsulant composition of the present application may have a contact angle to glass of 30° or less, 25° or less, 20° or less, or 12° or less. The lower limit is not particularly limited, but may be 1° or 3° or more. In the present application, by adjusting the contact angle to 30° or less, it is possible to ensure the spreadability in a short time in inkjet coating, and thus to form a thin organic layer. In the present application, the contact angle may be measured by applying one droplet of the sealant composition on glass using a sessile drop measurement method, or may be measured as an average value after five applications.
[0018] In one example, the epoxy compound and / or the compound having an oxetane group may be contained in the entire components of the sealant composition at 70 wt% or more, 75 wt% or more, 80 wt% or more, 85 wt% or more, or 89 wt% or more. The upper limit is not particularly limited, and may be 99 wt% or less, 95 wt% or less, or 93 wt% or less.
[0019] In one example, the epoxy compound may be at least bifunctional, i.e., the compound may have one or more epoxy functional groups, and the upper limit is not particularly limited, but may be 10 or less. The epoxy compound provides an appropriate degree of crosslinking to the adhesive, thereby providing excellent heat resistance and durability at high temperatures and high humidity.
[0020] In a specific example of the present application, the epoxy compound may include a compound having a ring structure in its molecular structure and / or a linear or branched aliphatic compound. That is, the sealant composition of the present application may include at least one of a compound having a ring structure in its molecular structure and a linear or branched aliphatic compound as the epoxy compound, or may include both. In one example, the compound having a ring structure in its molecular structure may have 3 to 10, 4 to 8, or 5 to 7 ring-constituting atoms in its molecular structure, and the compound may have 1 or more, 2 or more, and 10 or less ring structures. When the compound having a cyclic structure and the linear or branched aliphatic compound are both included, the linear or branched aliphatic compound may be included in the sealant composition in a range of 20 parts by weight or more, less than 205 parts by weight, 23 parts by weight to 204 parts by weight, 30 parts by weight to 203 parts by weight, 34 parts by weight to 202 parts by weight, 40 parts by weight to 201 parts by weight, 60 parts by weight to 200 parts by weight, or 100 parts by weight to 173 parts by weight, based on 100 parts by weight of the compound having a cyclic structure. By controlling the content range, the present application allows the sealant composition to have suitable physical properties for front sealing of an organic electronic device, to have excellent curing strength after curing, and to realize excellent moisture blocking properties.
[0021] In one example, the epoxy compound may have an epoxy equivalent ranging from 50 to 350 g / eq, 73 to 332 g / eq, 94 to 318 g / eq, or 123 to 298 g / eq. The compound having an oxetane group may have a weight average molecular weight ranging from 150 to 1,000 g / mol, 173 to 980 g / mol, 188 to 860 g / mol, 210 to 823 g / mol, or 330 to 780 g / mol. The present application improves the degree of curing completion after curing of the sealant by controlling the epoxy equivalent of the epoxy compound to be low or by controlling the weight average molecular weight of the compound having an oxetane group to be low, thereby preventing the composition from becoming too viscous and making the inkjet process impossible, and at the same time, provides moisture barrier properties and excellent curing sensitivity. In this specification, the weight average molecular weight means a value converted to standard polystyrene measured by GPC (Gel Permeation Chromatograph). In one example, a column made of a metal tube having a length of 250-300 mm and an inner diameter of 4.5-7.5 mm is filled with polystyrene beads of 3-20 mm. When a diluted solution of the substance to be measured dissolved in THF solvent is passed through the column, the weight average molecular weight can be indirectly measured according to the time of effluent. The amount of the substances separated by size and discharged from the column can be detected by plotting it against time. In addition, the epoxy equivalent in this specification is the number of grams of resin containing 1 gram equivalent of epoxy groups (g / eq), and can be measured by the method specified in JIS K 7236.
[0022] In addition, the boiling point of the compound having an oxetane group may be within the range of 90 to 300°C, 98 to 270°C, 110 to 258°C, or 138 to 237°C. By controlling the boiling point of the compound within the above range, the present application can provide a sealant that realizes excellent printability even at high temperatures in an inkjet process, has excellent moisture barrier properties from the outside, and prevents damage to elements by suppressing outgassing. In this specification, the boiling point may be measured at 1 atmosphere, unless otherwise specified.
[0023] In one example, compounds having a ring structure within their molecular structure include, but are not limited to, 3,4-epoxycyclohexylmethyl 3',4'-epoxycyclohexanecarboxylate (EEC) and derivatives, dicyclopentadiene dioxide and derivatives, vinylcyclohexene dioxide and derivatives, and 1,4-cyclohexanedimethanol bis(3,4-epoxycyclohexanecarboxylate) and derivatives.
[0024] In one example, the structure of the compound containing the oxetane group is not limited as long as it has the functional group, and examples thereof include OXT-221, CHOX, OX-SC, OXT101, OXT121, OXT221, and OXT212 manufactured by Toagosei Co., Ltd., and EHO, OXBP, OXTP, and OXMA manufactured by ETERNACOLL Co., Ltd. In addition, linear or branched aliphatic epoxy compounds may include, but are not limited to, alphatic glycidyl ether, 1,4-butanediol diglycidyl ether, ethylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, propylene glycol diglycidyl ether, diethylene glycol diglycidyl ether, butyl glycidyl ether, 2-ethylhexyl glycidyl ether, and neopentyl glycol diglycidyl ether.
[0025] In a specific example of the present application, the encapsulant composition may further include a surfactant. The encapsulant composition may be provided as a liquid-phase ink having improved spreadability by including a surfactant. In one example, the surfactant may include a polar functional group, and the polar functional group may be present at the end of the compound structure of the surfactant. The polar functional group may include, for example, a carboxyl group, a hydroxyl group, a phosphate, or a sulfonate. In addition, in a specific example of the present application, the surfactant may be a non-silicon-based surfactant or a fluorine-based surfactant. The non-silicon-based surfactant or the fluorine-based surfactant is applied together with the epoxy compound and / or the compound having an oxetane group to provide excellent coating properties on the organic electronic device. In addition, in the case of a surfactant including a polar reactive group, since it has high affinity with other components of the encapsulant composition, it is possible to realize an excellent effect in terms of adhesion. In a specific example of the present application, a hydrophilic fluorine-based surfactant or a non-silicon-based surfactant may be used to improve coating properties on the substrate.
[0026] Specifically, the surfactant may be a polymer or oligomer type fluorosurfactant. The surfactant may be a commercially available product, such as Glide 100, Glide 110, Glide 130, Glide 460, Glide 440, Glide 450, or RAD2500 from TEGO, Megaface F-251, F-281, F-552, F554, F-560, F-561, F-562, F-563, F-565, F-568, F-570, or F-571 from DIC (Dainippon Ink and Chemicals), or Surflon S-111, S-112, S-113, S-121, S-131, S-132, S-141, or S-145 from Asahi Glass Co., Ltd., or Fluorad from Sumitomo 3M Co., Ltd. It is possible to use those selected from the group consisting of FC-93, FC-95, FC-98, FC-129, FC-135, FC-170C, FC-430 and FC-4430 or Zonyl FS-300, FSN, FSN-100 and FSO from DuPont and BYK-350, BYK-354, BYK-355, BYK-356, BYK-358N, BYK-359, BYK-361N, BYK-381, BYK-388, BYK-392, BYK-394, BYK-399, BYK-3440, BYK-3441, BYKETOL-AQ, BYK-DYNWET 800, etc.
[0027] The surfactant may be included in an amount of 0.01 to 10 parts by weight, 0.05 to 10 parts by weight, 0.1 to 10 parts by weight, 0.5 to 8 parts by weight, or 1 to 4 parts by weight, based on 100 parts by weight of the epoxy compound. Within the above content range, the present application allows the sealant composition to be applied in an inkjet manner to form a thin organic layer.
[0028] In a specific example of the present application, the sealant composition may further include a photosensitizer to complement the curability of the sealant composition in the presence of active energy rays having a wavelength of 300 nm or more. The photosensitizer may be a compound that absorbs light having a wavelength in the range of 200 nm to 400 nm.
[0029] The photosensitizer may be an anthracene-based compound such as anthracene, 9,10-dibutoxyanthracene, 9,10-dimethoxyanthracene, 9,10-diethoxyanthracene, or 2-ethyl-9,10-dimethoxyanthracene; benzophenone, 4,4-bis(dimethylamino)benzophenone, 4,4-bis(diethylamino)benzophenone, 2,4,6-trimethylaminobenzophenone, methyl-o-benzoylbenzoate, 3,3-dimethyl-4-methoxybenzophenone, or 3,3,4,4-tetra(t-butylperoxy)benzophenone; benzophenone compounds such as dicarbonyl)benzophenone; acetophenone; ketone compounds such as dimethoxyacetophenone, diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, and propanone; perylene; fluorenone compounds such as 9-fluorenone, 2-chloro-9-fluorenone, and 2-methyl-9-fluorenone; thioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, 1-chloro-4-propyloxythioxanthone, and isopropylthioxanthone ( Thioxanthone compounds such as ITX, diisopropyl thioxanthone; xanthone compounds such as xanthone, 2-methyl xanthone; anthraquinone compounds such as anthraquinone, 2-methyl anthraquinone, 2-ethyl anthraquinone, t-butyl anthraquinone, 2,6-dichloro-9,10-anthraquinone; acridine compounds such as 9-phenyl acridine, 1,7-bis(9-acridinyl)heptane, 1,5-bis(9-acridinylpentane, 1,3-bis(9-acridinyl)propane; benzyl, 1, Dicarbonyl compounds such as 7,7-trimethyl-bicyclo[2,2,1]heptane-2,3-dione and 9,10-phenanthrenequinone; phosphine oxide compounds such as 2,4,6-trimethylbenzoyldiphenylphosphine oxide and bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide; benzoate compounds such as methyl-4-(dimethylamino)benzoate, ethyl-4-(dimethylamino)benzoate, and 2-n-butoxyethyl-4-(dimethylamino)benzoate;Amino synergists such as 2,5-bis(4-diethylaminobenzal)cyclopentanone, 2,6-bis(4-diethylaminobenzal)cyclohexanone, and 2,6-bis(4-diethylaminobenzal)-4-methyl-cyclopentanone; 3,3-carbonylvinyl-7-(diethylamino)coumarin, 3-(2-benzothiazolyl)-7-(diethylamino)coumarin, 3-benzoyl-7-(diethylamino)coumarin, and 3-benzoyl-7-methyl The compound may be one or more selected from the group consisting of coumarin compounds such as 10,10-carbonylbis[1,1,7,7-tetramethyl-2,3,6,7-tetrahydro-1H,5H,11H-C1]-benzopyrano[6,7,8-ij]-quinolizin-11-one; chalcone compounds such as 4-diethylaminochalcone and 4-azidobenzalacetophenone; 2-benzoylmethylene; and 3-methyl-b-naphthothiazoline.
[0030] The photosensitizer may be included in the range of 28 to 40 parts by weight, 31 to 38 parts by weight, or 32 to 36 parts by weight, based on 100 parts by weight of the photoinitiator described below. By adjusting the content of the photosensitizer, the present application can realize the effect of increasing the curing sensitivity at a desired wavelength, while preventing the photosensitizer from being dissolved and reducing the adhesive strength.
[0031] In an embodiment of the present application, the sealant composition may further include a photoinitiator. The photoinitiator may be an ionic photoinitiator. The photoinitiator may also be a compound that absorbs light in the wavelength range of 200 nm to 400 nm.
[0032] In one example, the photoinitiator may be a cationic photoinitiator. In the case of the cationic photoinitiator, a material known in the art may be used, for example, a cationic moiety including an aromatic sulfonium, an aromatic iodonium, an aromatic diazonium, or an aromatic ammonium, and AsF6 - , SbF6 - , PF6 -or a compound having an anion moiety including tetrakis(pentafluorophenyl)borate. In addition, as the cationic photopolymerization initiator, an onium salt or organometallic salt-based ionized cationic initiator, an organic silane or latent sulfonic acid-based or non-ionized cationic photopolymerization initiator can be used. Examples of the onium salt initiator include diaryliodonium salt, triarylsulfonium salt, and aryldiazonium salt. Examples of the organometallic salt initiator include iron arene. Examples of the organosilane initiator include o-nitrobenzyl triaryl silyl ether, triaryl silyl peroxide, and acyl silane. Examples of the latent sulfonic acid initiator include α-sulfonyloxyketone and α-hydroxymethylbenzoin sulfonate, but are not limited thereto.
[0033] In one example, the encapsulant composition of the present application may include a photoinitiator containing a sulfonium salt as a photoinitiator in the above-mentioned specific composition so as to be suitable for use in sealing an organic electronic device using an inkjet method. The encapsulant composition according to the above composition is directly sealed on an organic electronic device, but generates a small amount of outgas, so that chemical damage to the device can be prevented. In addition, the photoinitiator containing a sulfonium salt has excellent solubility and can be applied to be suitable for an inkjet process.
[0034] In the specific example of the present application, the photoinitiator may be included in an amount of 1 to 15 parts by weight, 3 to 14 parts by weight, or 7 to 13.5 parts by weight based on 100 parts by weight of the epoxy compound.
[0035] The sealant composition of the present application may further include a coupling agent. The present application may improve the adhesion of the cured product of the sealant composition to an adherend and the moisture permeability resistance of the cured product. The coupling agent may include, for example, a titanium-based coupling agent, an aluminum-based coupling agent, or a silane coupling agent.
[0036] In a specific example of the present application, the silane coupling agent may be specifically an epoxy-based silane coupling agent such as 3-glycidyloxypropyltrimethoxysilane, 3-glycidyloxypropyltriethoxysilane, 3-glycidyloxypropyl(dimethoxy)methylsilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; a mercapto-based silane coupling agent such as 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropylmethyldimethoxysilane, and 11-mercaptoundecyltrimethoxysilane; a 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropyldimethoxymethylsilane, N-phenyl-3-aminopropyltrimethoxysilane, N-methylaminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, and N-(2-aminoethyl)-3-aminopropyltrimethoxysilane; amino-based silane coupling agents such as (3-aminopropyl)-3-aminopropyldimethoxymethylsilane; ureido-based silane coupling agents such as 3-ureidopropyltriethoxysilane, vinyl-based silane coupling agents such as vinyltrimethoxysilane, vinyltriethoxysilane, and vinylmethyldiethoxysilane; styryl-based silane coupling agents such as p-styryltrimethoxysilane; acrylate-based silane coupling agents such as 3-acryloxypropyltrimethoxysilane and 3-methacryloxypropyltrimethoxysilane; isocyanate-based silane coupling agents such as 3-isocyanatepropyltrimethoxysilane, sulfide-based silane coupling agents such as bis(triethoxysilylpropyl)disulfide and bis(triethoxysilylpropyl)tetrasulfide; phenyltrimethoxysilane, methacryloxypropyltrimethoxysilane, imidazole silane, and triazine silane.
[0037] In the present application, the coupling agent may be included in an amount of 0.1 to 10 parts by weight or 0.5 to 5 parts by weight based on 100 parts by weight of the epoxy compound. In the present application, the effect of improving adhesion due to the addition of the coupling agent within the above range may be realized.
[0038] The sealant composition of the present application may contain a moisture adsorbent, if necessary. The term "moisture adsorbent" can be used as a general term for a component that can adsorb or remove moisture or humidity entering from the outside through a physical or chemical reaction, etc. That is, it means a moisture-reactive adsorbent or a physical adsorbent, and a mixture thereof can also be used.
[0039] The specific type of moisture adsorbent that can be used in the present application is not particularly limited, and examples of the moisture-reactive adsorbent include one or a mixture of two or more of metal oxides, metal salts, phosphorus pentoxide (P2O5), etc., and examples of the physical adsorbent include zeolite, zirconia, montmorillonite, etc.
[0040] The sealant composition of the present application may contain the moisture adsorbent in an amount of 5 to 100 parts by weight, 5 to 80 parts by weight, 5 to 70 parts by weight, or 10 to 30 parts by weight, based on 100 parts by weight of the epoxy compound. The sealant composition of the present application preferably controls the content of the moisture adsorbent to 5 parts by weight or more, so that the sealant composition or its cured product can exhibit excellent moisture and humidity barrier properties. In addition, the present application controls the content of the moisture adsorbent to 100 parts by weight or less, so that a thin film sealing structure can be provided.
[0041] In one example, the sealant composition may further include an inorganic filler, if necessary. The specific type of filler that may be used in the present application is not particularly limited, and may be, for example, one or a mixture of two or more of clay, talc, alumina, calcium carbonate, or silica.
[0042] The sealant composition of the present application may contain 0 to 50 parts by weight, 1 to 40 parts by weight, 1 to 20 parts by weight, or 1 to 10 parts by weight of an inorganic filler relative to 100 parts by weight of an epoxy compound. The present application can provide a sealing structure having excellent moisture or humidity barrier properties and mechanical properties by controlling the content of the inorganic filler to preferably 1 part by weight or more. In addition, the present invention can provide a cured product that exhibits excellent moisture barrier properties even when formed into a thin film by controlling the content of the inorganic filler to 50 parts by weight or less.
[0043] In addition to the above-mentioned components, the sealant composition according to the present application may contain various additives within a range that does not affect the effects of the above-mentioned invention. For example, the sealant composition may contain an antifoaming agent, a tackifier, an ultraviolet stabilizer, an antioxidant, etc. in an appropriate range depending on the desired physical properties.
[0044] In one example, the encapsulant composition may be in a liquid phase at room temperature, for example, about 25°C. In a specific example of the present application, the encapsulant composition may be in a liquid phase in a solvent-free form. The encapsulant composition may be applied to encapsulate an organic electronic device, specifically, to encapsulate a front surface of an organic electronic device. In the present application, since the encapsulant composition has a liquid phase at room temperature, the device can be encapsulated by applying the composition to the side surface of the organic electronic device. In addition, since the present application has a solvent-free form, the volatile organic compound and / or moisture content can be adjusted to the above-mentioned range.
[0045] The sealant composition of the present application may also be an ink composition. The sealant composition of the present application may also be an ink composition capable of being ink-jet processed. The sealant composition of the present application may have a specific composition and physical properties so that it may be ink-jet capable.
[0046] In addition, in a specific example of the present application, the encapsulant composition may have a light transmittance of 90% or more, 92% or more, or 95% or more in the visible light region after curing. In the above range, the present application provides an organic electronic device with high resolution, low power consumption, and long life by applying the encapsulant composition to a top-emitting organic electronic device. In addition, the encapsulant composition of the present application may have a haze of 3% or less, 2% or less, or 1% or less according to a JIS K7105 standard test after curing, and the lower limit is not particularly limited, but may be 0%. Within the above haze range, the encapsulant composition may have excellent optical properties after curing. In the present specification, the above-mentioned light transmittance or haze may be measured in a state in which the encapsulant composition is cured in an organic layer, or may be an optical property measured when the organic layer has a thickness of 2 μm to 50 μm. In a specific example of the present application, the above-mentioned moisture adsorbent or inorganic filler may not be included in order to realize the optical properties.
[0047] The present application also relates to a sealant composition. The sealant composition may have a moisture content of 1,000 ppm or less, 500 ppm or less, or 100 ppm or less as measured by Karl Fischer coulometric titration. The measurement may be performed on 100 mg of the composition, but is not limited thereto. The lower limit is not particularly limited and may be 0 ppm or 10 ppm. The moisture measurement may be performed at an operating temperature of 25° C., in a sealed container, and may be adjusted to an equivalence point of 50 mV within a suitable speed range of 0.3 to 2,240 μg / min. In the coulometric method, iodine is electrically generated from a generating electrode and reacts with water. At this time, the amount of moisture in the sample is calculated from the number of moles of electrons used to generate iodine. The measurement may be performed using Karl fischer titrators-831 KF Coulometer-coulometric manufactured by Metrohm. In the present application, by controlling the moisture content of the encapsulant composition before curing as described above, even if the encapsulant composition is directly applied to an organic electronic device, chemical damage to the device can be prevented and the generation and growth of dark spots in the organic electronic device can be suppressed. The encapsulant composition may be an encapsulant composition for encapsulating an organic electronic device prepared by the above-mentioned preparation method.
[0048] The present application also relates to an organic electronic device. An exemplary organic electronic device 3, as shown in FIG. 1, may include a substrate 31, an organic electronic element 32 formed on the substrate 31, and an organic layer 33 that seals the front surface of the organic electronic element 32 and includes the above-mentioned sealant composition.
[0049] In a specific example of the present application, the organic electronic device may include a first electrode layer, an organic layer formed on the first electrode layer and including at least an emitting layer, and a second electrode layer formed on the organic layer. The first electrode layer may be a transparent electrode layer or a reflective electrode layer, and the second electrode layer may also be a transparent electrode layer or a reflective electrode layer. More specifically, the organic electronic device may include a reflective electrode layer formed on a substrate, an organic layer formed on the reflective electrode layer and including at least an emitting layer, and a transparent electrode layer formed on the organic layer.
[0050] In this application, the organic electronic element 23 may be an organic light emitting diode.
[0051] In one example, the organic electronic device according to the present application may be a top emission type, but is not limited thereto, and may be applied to a bottom emission type.
[0052] The organic electronic device may further include a protective film 35 for protecting the electrodes and the light-emitting layer of the device. The protective film 35 may be an inorganic protective film. The protective film may be a protective layer formed by chemical vapor deposition (CVD), and the material may be a known inorganic material, for example, silicon nitride (SiNx). In one example, silicon nitride (SiNx) used in the protective film may be deposited to a thickness of 0.01 μm to 50 μm.
[0053] In a specific example of the present application, the organic electronic device 3 may further include an inorganic layer 34 formed on the organic layer 33. The material of the inorganic layer 34 is not limited and may be the same as or different from the protective film described above. In one example, the inorganic layer may be one or more metal oxides or nitrides selected from the group consisting of Al, Zr, Ti, Hf, Ta, In, Sn, Zn, and Si. The thickness of the inorganic layer may be 0.01 μm to 50 μm, 0.1 μm to 20 μm, or 1 μm to 10 μm. In one example, the inorganic layer of the present application may be an inorganic material that does not contain a dopant or an inorganic material that contains a dopant. The dopant that may be doped may be one or more elements selected from the group consisting of Ga, Si, Ge, Al, Sn, Ge, B, In, Tl, Sc, V, Cr, Mn, Fe, Co, and Ni, or oxides of the elements, but is not limited thereto.
[0054] In one example, the thickness of the organic layer may be in the range of 2 μm to 20 μm, 2.5 μm to 15 μm, or 2.8 μm to 9 μm. The present application provides a thin organic layer to provide a thin-film organic electronic device.
[0055] The organic electronic device 3 of the present application may include a sealing structure including the organic layer 33 and inorganic layer 34 described above, and the sealing structure may include at least one or more organic layers and at least one or more inorganic layers, and the organic layers and the inorganic layers may be repeatedly laminated. For example, the organic electronic device may have a structure of substrate / organic electronic element / protective film / (organic layer / inorganic layer)n, where n may be a number within a range of 1 to 100. FIG. 1 is a cross-sectional view illustrating an example where n is 1.
[0056] In one example, the organic electronic device 3 of the present application may further include a cover substrate on the organic layer 33. The material of the substrate and / or cover substrate is not particularly limited, and any material known in the art may be used. For example, the substrate or cover substrate may be glass, a metal substrate, or a polymer film. The polymer film may be, for example, a polyethylene terephthalate film, a polytetrafluoroethylene film, a polyethylene film, a polypropylene film, a polybutene film, a polybutadiene film, a vinyl chloride copolymer film, a polyurethane film, an ethylene-vinyl acetate film, an ethylene-propylene copolymer film, an ethylene-ethyl acrylate copolymer film, an ethylene-methyl acrylate copolymer film, or a polyimide film.
[0057] 2, the organic electronic device 3 of the present application may further include a sealing film 37 disposed between the cover substrate 38 and the substrate 31 on which the organic electronic element 32 is formed. The sealing film 37 may be used to attach the substrate 31 on which the organic electronic element 32 is formed to the cover substrate 38, and may be, for example, but is not limited to, an adhesive film or a bonding film. The sealing film 37 may seal the front surface of the sealing structure 36 of the organic layer and inorganic layer laminated on the organic electronic element 32.
[0058] The present application also relates to a method for manufacturing an organic electronic device.
[0059] In one example, the manufacturing method may include forming an organic layer 33 on a substrate 31 having an organic electronic element 32 formed thereon, so that the encapsulant composition described above encapsulates the front surface of the organic electronic element 32.
[0060] The organic electronic device 32 may be manufactured by forming a reflective electrode or a transparent electrode on a substrate 31 such as glass or a polymer film by a method such as vacuum deposition or sputtering, and then forming an organic material layer on the reflective electrode. The organic material layer may include a hole injection layer, a hole transport layer, a light emitting layer, an electron injection layer, and / or an electron transport layer. Then, a second electrode is further formed on the organic material layer. The second electrode may be a transparent electrode or a reflective electrode.
[0061] The manufacturing method of the present application may further include a step of forming a protective film 35 on the first electrode, the organic material layer, and the second electrode formed on the substrate 31. Then, the organic layer 33 described above is applied to the substrate 31 to cover the front surface of the organic electronic device 32. At this time, the step of forming the organic layer 33 is not particularly limited, and the sealing material composition described above may be applied to the front surface of the substrate 31 by a process such as inkjet printing, gravure coating, spin coating, screen printing, or reverse offset coating.
[0062] In addition, the method may further include a step of irradiating the organic layer with light. In the present invention, a curing process may be performed on the organic layer that encapsulates the organic electronic device, and the curing process may be performed, for example, in a heating chamber or a UV chamber, and preferably in a UV chamber.
[0063] In one example, the above-mentioned sealant composition is applied to form a front organic layer, and then the composition is irradiated with light to induce crosslinking. The light irradiation may be performed by applying light having a wavelength range of 250 nm to 450 nm or 300 nm to 450 nm at a dose of 0.3 to 6 J / cm. 2 or 0.5~5J / cm 2 The method can include irradiating the substrate with an amount of light of
[0064] In addition, the manufacturing method of the present application may further include a step of forming an inorganic layer 34 on the organic layer 33. The step of forming the inorganic layer may be performed by a method known in the art, and may be the same as or different from the above-mentioned method of forming a protective layer. Effect of the Invention
[0065] The present application provides a sealant composition capable of effectively blocking moisture or oxygen from entering an organic electronic device from the outside to ensure the life of the organic electronic device, and an organic electronic device including the same. [Brief description of the drawings]
[0066] [Figure 1] 1 is a cross-sectional view showing an organic electronic device according to an embodiment of the present invention. [Diagram 2] 1 is a cross-sectional view showing an organic electronic device according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0067] The present invention will be described in more detail below through examples according to the present invention and comparative examples not according to the present invention, but the scope of the present invention is not limited to the following examples.
[0068] Example 1 At room temperature, an alicyclic epoxy compound (Daicel, Celloxide 2021P) and an aliphatic epoxy compound (HAJIN CHEM TECH, DE203) were added as epoxy compounds to a mixing vessel in a weight ratio of 23.8:28.7:37.5:5.0:1.0 (Celloxide 2021P:DE203:OXT-221:I290:F552), respectively.
[0069] The mixing vessel was mixed with a planetary mixer (Kurabo, KK-250s) to prepare a uniform sealant composition ink.
[0070] The composition ink is subjected to a moisture removal step. Nitrogen sparging of 200 lpm is started for the sealant composition prepared in the mixing vessel having an internal pressure of 660 mmHg, and the sparging is continued for 3 hours while maintaining a constant temperature of 25° C. The sealant composition that has undergone the moisture removal step is sealed in an aluminum pouch.
[0071] Example 2 A sealant composition was prepared in the same manner as in Example 1, except that nitrogen sparging of 1,000 lpm was started for the sealant composition prepared in a mixing vessel having an internal pressure of 660 mmHg, and the sparging was continued for 3 hours while maintaining a constant temperature of 25° C., and the sealant composition was sealed in an aluminum pouch.
[0072] Example 3 A sealant composition was prepared in the same manner as in Example 1, except that nitrogen sparging of 200 lpm was started for the sealant composition prepared in a mixing vessel having an internal pressure of 660 mmHg, and the sparging was continued for 3 hours while maintaining a constant temperature of 45° C., and the sealant composition was sealed in an aluminum pouch.
[0073] Comparative Example 1 A sealant composition was prepared in the same manner as in Example 1, except that sparging with nitrogen at 5 lpm was started for the sealant composition prepared in a mixing vessel having an internal pressure of 660 mmHg, and the sparging was continued for 3 hours while maintaining a constant temperature of 25° C., and the sealant composition was sealed in an aluminum pouch.
[0074] Comparative Example 2 A sealant composition was prepared in the same manner as in Example 1, except that nitrogen sparging of 15 lpm was started for the sealant composition prepared in a mixing vessel having an internal pressure of 660 mmHg, and the sparging was continued for 3 hours while maintaining a constant temperature of 25° C., and the sealant composition was sealed in an aluminum pouch.
[0075] Comparative Example 3 The sealant composition ink was prepared and stored in the same manner as in Example 1, except that the temperature was heated from 25° C. to 50° C. in the moisture removal step.
[0076] Comparative Example 4 The sealant composition ink was prepared and stored in the same manner as in Example 1, except that the temperature was cooled from 25°C to 10°C during the moisture removal step.
[0077] The physical properties in the examples and comparative examples were evaluated by the following methods.
[0078] 1. Moisture content measurement The moisture content of the sealing material compositions prepared in the examples and comparative examples was measured using Karl Fischer titrators-831 KF Coulometer-coulometric of Metrohm. The moisture content was measured using Karl Fischer coulometric titration for 100 mg of the composition. The titration was carried out at an operating temperature of 25° C. in a closed container, and the equivalence point was adjusted to 50 mV within the appropriate speed range of 0.3 to 2240 μg / min.
[0079] In addition to the above measurements, the moisture content of the sealant composition before the moisture removal step was performed in each of the examples and comparative examples was measured and is shown in Ref. of Table 1 below.
[0080] 2. Outgassing Measurement The sealing material compositions prepared in the examples and comparative examples were subjected to 1000 mW / cm 2 At an intensity of 1 J / cm 2 After curing by irradiating with UV, 50 mg of the cured sample was kept at 110°C for 30 minutes and the amount of volatile organic compounds was measured using Purge & Trap sampler (JAI JTD-505III) - GC / MS (Agilent 7890b / 5977a). If the amount measured is 100 ppm or less, it can be classified as good, and if it exceeds, it can be classified as bad.
[0081] 3. Measurement of viscosity change The sealant compositions prepared in the Examples and Comparative Examples were sealed in pouches, and after 10 days had passed, the viscosity of the sealant compositions was measured using a Brookfield viscometer DV-3 as follows.
[0082] The sealant composition was measured at a temperature of 25° C., a torque of 90%, and a shear rate of 100 rpm. Specifically, the viscosity was measured by injecting 0.5 ml of a sample using a Brookfield viscometer in a cone / plate mode.
[0083] The measurement was carried out by measuring the viscosity V1 immediately before sealing and the viscosity V2 after 10 days, and determining the rate of change. If the rate of change was within ±10%, it was classified as good, if it exceeded 10%, it was increased, and if it exceeded -10%, it was decreased.
[0084] If a side reaction occurs within the sealant composition during long-term storage, the viscosity increases. A higher rate of change indicates that some side reaction occurs within the composition.
[0085] 4. Determining reliability (checking for dark spots) The sealant compositions prepared in the examples and comparative examples were applied (inkjet process) onto an organic electronic device on which an inorganic deposition film (chemical vapor deposition film) was formed. Then, a 1,000 mW / cm 2 At an intensity of 1 J / cm 2 The cured organic layer was left in an environment of 85℃ and 85% RH for 300 hours, and then the luminescence form was observed. If there were no dark spots, it was classified as O; if 1-2 dark spots were observed, it was △; if 3 or more dark spots were observed and luminescence was impossible, it was classified as X.
[0086] [Table 1]
[0087] [Table 2] [Explanation of symbols]
[0088] 3 Organic electronic devices 31 Substrate 32 Organic Electronic Devices 33 Organic layer 34 Inorganic layer 35 Protective film 36 Sealing structure 37 Sealing film 38 Cover Board
Claims
1. a moisture removing step of injecting 20 to 5,000 lpm (liters per minute) of inert gas into the sealant composition in the container so that the moisture content per 100 mg of the sealant composition is 1,000 ppm or less as determined by Karl Fischer coulometric titration; The moisture removal step is carried out at constant temperature, The sealant composition includes an epoxy compound, The epoxy compound includes a compound having a ring structure in its molecular structure and a linear or branched aliphatic compound, the linear or branched aliphatic compound is contained in an amount of 120 parts by weight or more and less than 173 parts by weight based on 100 parts by weight of the compound having a cyclic structure, The sealant composition is a solvent-free ink composition. A method for making a sealant composition.
2. The set temperature of the constant temperature state is any one of 20°C to 48°C. A method for producing the sealant composition of claim 1.
3. The constant temperature state has an error range of −5° C. to 5° C. compared to the set temperature. A method for producing the sealant composition of claim 2.
4. The moisture removal step includes adjusting the pressure in the container to within the range of 600 to 760 mmHg. A method for producing the sealant composition according to any one of claims 1 to 3.
5. storing the sealant composition in a pouch after the moisture removal step. A method for producing the sealant composition according to any one of claims 1 to 4.
6. The sealant composition has a moisture content of 1,000 ppm or less per 100 mg of the sealant composition as determined by Karl Fischer coulometric titration method. A method for producing the sealant composition according to any one of claims 1 to 5.
7. Further comprising a compound having an oxetane group in a range of 45 parts by weight to 145 parts by weight based on 100 parts by weight of the epoxy compound; A method for producing the sealant composition according to any one of claims 1 to 6.
8. The epoxy compound has two or more epoxy functional groups. A method for producing the sealant composition according to any one of claims 1 to 7.
9. The compound having a ring structure in its molecular structure has a number of ring-constituting atoms in the molecular structure within the range of 3 to 10. A method for producing the sealant composition according to any one of claims 1 to 8.
10. The sealant composition further comprises a surfactant. A method for producing the sealant composition according to any one of claims 1 to 9.
11. The sealant composition further comprises a photoinitiator. A method for producing the sealant composition according to any one of claims 1 to 10.
12. A sealant composition for sealing an organic electronic element, which is in the form of a solvent-free ink composition containing an epoxy compound and a fluorine-based surfactant, The sealing material composition for encapsulating an organic electronic element has a moisture content of 1,000 ppm or less per 100 mg of the sealing material composition for encapsulating an organic electronic element, as determined by Karl Fischer coulometric titration method; The epoxy compound includes a compound having a ring structure in its molecular structure and a linear or branched aliphatic compound, The sealing material composition for sealing an organic electronic element, wherein the linear or branched aliphatic compound is contained in an amount within a range of 120 parts by weight or more and less than 173 parts by weight based on 100 parts by weight of the compound having a cyclic structure.
13. A method for producing a sealing material composition for sealing an organic electronic element, comprising the steps of: The sealing material composition for encapsulating an organic electronic element is produced by the method for producing the sealing material composition according to any one of claims 1 to 11. A method for producing a sealing material composition for sealing an organic electronic element.
14. A substrate; An organic electronic device formed on a substrate; an organic layer that seals the front surface of the organic electronic element and includes the sealant composition for sealing the organic electronic element; Includes 1. A method for manufacturing an organic electronic device, comprising the steps of: The method for producing the sealing material composition for encapsulating an organic electronic element according to claim 13, A method for manufacturing an organic electronic device.
15. forming an organic layer on a substrate having an organic electronic element formed thereon, the organic electronic element encapsulant composition according to claim 12 so as to encapsulate the organic electronic element on the substrate, the organic electronic element encapsulant composition comprising: A method for manufacturing an organic electronic device.
Citation Information
Patent Citations
Preserving method of organic material for organic electroluminescent element
JP2005135735A
Curable resin composition and method for producing the same
JP2007169337A
Curable composition for optical parts, adhesive agent for optical parts, and sealing agent for organic electroluminescence element
JP2010018797A
Photocurable resin compositon for sealing of electric device
KR101693265B1
Indicating film
KR1020170037571A