Sampler for collecting per- and polyfluoroalkyl compounds for personal exposure measurement
A portable sampler with activated carbon and urethane foam filters efficiently collects and quantitatively measures volatile and semi-volatile per- and polyfluoroalkyl compounds, addressing the limitations of existing technologies and enhancing personal exposure measurements.
Patent Information
- Application Number
- JP2021017506
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-02-14
- Filing Date
- 2021-02-05
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2041-02-05
AI Technical Summary
Existing samplers are unable to efficiently collect and quantitatively measure volatile and semi-volatile per- and polyfluoroalkyl compounds, which are persistent organic pollutants, due to limitations in adsorption and desorption capabilities, and they are not suitable for personal exposure measurements in work environments.
A portable sampler equipped with an activated carbon filter section using fibrous or granular activated carbon with specific surface area, pore volume, and surface oxide content, along with a urethane foam filter section, to efficiently adsorb and desorb per- and polyfluoroalkyl compounds, including volatile and semi-volatile forms.
The sampler enables comprehensive collection and accurate quantitative analysis of per- and polyfluoroalkyl compounds, improving handling and reducing the burden on workers by maintaining low pressure loss, thus facilitating personal exposure measurements.
Smart Images

Figure 0007582615000032 
Figure 0007582615000033 
Figure 0007582615000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a sampler for collecting per- and polyfluoroalkyl compounds in the atmosphere, and more particularly to a portable personal sampler for measuring personal exposure. [Background technology]
[0002] Per- and polyfluoroalkyl compounds are fluorinated aliphatic compounds with high thermal stability, high chemical stability, and high surface activity. Taking advantage of these properties, per- and polyfluoroalkyl compounds are widely used in industrial and chemical applications such as paints, packaging materials, and liquid fire extinguishing agents.
[0003] Some per- and polyfluoroalkyl compounds are very stable chemical substances and are difficult to decompose under natural conditions after being released into the environment. For this reason, in recent years, per- and polyfluoroalkyl compounds have been recognized as persistent organic pollutants (POPs), and since 2010, the Stockholm Convention on Persistent Organic Pollutants (POPs Convention) has restricted the manufacture and use of perfluorooctane sulfonate (PFOS) (IUPAC name: 1,1,2,2,3,3,4,4,5,5,6,6,7,7,8,8,8-heptadecafluorooctane-1-sulfonic acid).
[0004] Perfluoroalkyl compounds have a completely fluorinated linear alkyl group and are represented by the chemical formula (ii). Examples include perfluorooctane sulfonic acid (PFOS) and perfluorooctanoic acid (PFOA) (IUPAC name: 2,2,3,3,4,4,5,5,6,6,7,7,8,8,8-pentadecafluorooctanoic acid).
[0005]
number
[0006] A polyfluoroalkyl compound is a compound in which some of the hydrogen atoms in an alkyl group are replaced with fluorine, and is represented by the chemical formula (iii). For example, there is fluorotelomer alcohol.
[0007]
number
[0008] Thus, since per- and polyfluoroalkyl compounds continue to remain in nature (in water, soil, and air), the establishment of a quantitative test method for per- and polyfluoroalkyl compounds is being considered. The challenge in the study of a quantitative test method is the development of a sampler with high collection, adsorption, and desorption performance for per- and polyfluoroalkyl compounds. Air, which is a sample containing trace amounts of per- and polyfluoroalkyl compounds, is ventilated, and various forms of per- and polyfluoroalkyl compounds (particle-adsorbing, semi-volatile, volatile) contained in the sample air are collected or adsorbed, and the compounds are desorbed from the collector or adsorbent into an extract by an extraction process and concentrated. After concentration, quantitative measurement is performed using a measuring device such as LC-MS / MS or GC-MS / MS, making it possible to measure the concentration of per- and polyfluoroalkyl compounds contained in the sample.
[0009] A method using a high-volume air sampler is known for measuring per- and polyfluoroalkyl compounds in the air (see, for example, Non-Patent Document 1). In this method, a filter paper made of fine fibers such as quartz fiber filter paper is attached inside the high-volume air sampler, and the sampler is allowed to circulate for a certain period of time to collect airborne particles, thereby measuring the PFOS contained in the airborne particles.
[0010] However, the substances that can be collected by passing air through the filter paper are limited to non-volatile ionic compounds such as PFOS and PFOA, which are perfluoroalkyl compounds that adsorb to airborne particles. Per- and polyfluoroalkyl compounds that cannot be collected by this sampler include volatile compounds. Volatile per- and polyfluoroalkyl compounds pass through the filter paper, making it impossible to perform quantitative measurements.
[0011] For this reason, there was a demand for a sampler capable of collecting per- and polyfluoroalkyl compounds that exist in other forms, such as volatile polyfluoroalkyl compounds that are not contained in airborne particles and cannot be collected by the sampler.
[0012] In addition, silica gel-based collectors and the like are used as collectors for volatile per- and polyfluoroalkyl compounds. For example, an organic fluorine-based compound adsorbent made of cyclodextrin polymer has been proposed (Patent Document 1). This adsorbent is specialized only for adsorption and cannot desorb the compounds, so it is not suitable for use as a collector for quantitative measurement. In addition, cyclodextrin polymers are powdery or particulate, which makes them difficult to handle, and has high resistance when passing liquid or air, resulting in problems such as the risk of fine powder leaking to the secondary side. As such, there was a problem that existing adsorbents could not sufficiently collect volatile per- and polyfluoroalkyl compounds, making it impossible to perform accurate quantitative measurement.
[0013] Furthermore, in Japan today, in order to prevent health hazards for workers, the concentration of harmful substances and dust in the work environment is measured and the results are evaluated in accordance with the provisions of the Industrial Safety and Health Law. Work environment measurements are carried out by setting measurement points at equal intervals in each unit work area, so-called A and B measurements.
[0014] When conducting risk assessments, it is considered desirable to compare the airborne concentrations of chemical substances, etc. at the work site measured using this measurement method with the worker's exposure limit, and research is currently being conducted into personal exposure measurements using personal samplers.
[0015] The advantage of using a personal sampler is that accurate measurements can be made even when the source of harmful substances moves or when it is difficult to place a measurement point between the source of harmful substances and the worker. In addition, when handling highly harmful substances, the sampler can be placed near the worker's breathing zone to enable accurate measurements.
[0016] Personal exposure measurements are broadly divided into passive and active sampling methods. In the passive sampling method, a measuring device in the shape of a batch made of a collection material is attached to the worker's breathing zone, and the target substance is collected using molecular diffusion, and the target substance is extracted from the collection material in the measuring device and measured, thereby measuring the worker's exposure. In the active sampling method, the worker performs work while wearing a sampler consisting of a target substance collection filter and a suction pump, and after work, the amount of the target substance collected by the collection filter in the sampler is measured.
[0017] In the active sampling method, because the work is performed with the personal sampler attached, it is desirable to use a small suction pump from the viewpoints of portability and reducing the burden on the worker, but the pressure loss caused by the collection filter has been an issue. Since the collection filter must be equipped with the necessary amount of collection material to fully demonstrate its collection performance, it is unavoidable to make the suction pump larger, which leads to problems of reduced portability and increased burden on the worker. [Prior art documents] [Patent documents]
[0018] [Patent Document 1] JP 2012-101159 A [Non-patent literature]
[0019] [Non-Patent Document 1] Michiko Kotani et al., "Weekly Changes in Perfluorooctane Sulfonate (PFOS) Concentrations in Urban Air," Journal of the Japan Society for Atmospheric Environment, Vol. 45, No. 6, November 10, 2010, pp. 279-282 Summary of the Invention [Problem to be solved by the invention]
[0020] The present invention has been made in consideration of the above points, and provides a per- and polyfluoroalkyl compound sampler for personal exposure measurement that can efficiently and releasably capture per- and polyfluoroalkyl compounds present in the air in a work environment, etc., and is portable and easy to handle. [Means for solving the problem]
[0021] That is, the first invention is a portable per- and polyfluoroalkyl compound sampler for measuring personal exposure, which has an activated carbon filter part mainly made of activated carbon that adsorbs per- and polyfluoroalkyl compounds in a releasable manner, and the BET specific surface area of the activated carbon is 900 m 2 / g or more The sum of the micropore volumes of the activated carbon of 1 nm or less (V mic ) is 0.35 cm 3 / g or more, and the sum of the mesopore volumes of 2 to 60 nm of the activated carbon (V met ) is 0.03 cm 3 / g or more, The present invention relates to a per- and polyfluoroalkyl compound sampler for personal exposure measurement, characterized in that the pressure loss in the activated carbon filter section at a wind speed of 0.5 m / sec is less than 6 kPa.
[0022] No. 2 The invention is 1 Invention The sum of the micropore volumes (V mic ) and the sum of the mesopore volume (V met ) and the volume difference (V s ) is 0.35 or more R Per- and polyfluoroalkyl compound samplers for personal exposure measurement Related to .
[0023]
number
[0024] No. 3 The invention is Invention 1 or 2 The present invention relates to a per- and polyfluoroalkyl compound sampler for personal exposure measurement, in which the amount of surface oxide of the activated carbon is 0.10 meq / g or more.
[0025] No. 4 The inventions are the first to 3 In any one of the above-mentioned inventions, the present invention relates to a per- and polyfluoroalkyl compound sampler for personal exposure measurement, wherein the activated carbon is fibrous activated carbon.
[0026] No. 5 The inventions are the first to 3 In any one of the above-mentioned inventions, the present invention relates to a per- and polyfluoroalkyl compound sampler for personal exposure measurement, wherein the activated carbon is granular activated carbon.
[0027] No. 6 The inventions are the first to 5 In any one of the above-mentioned inventions, the activated carbon filter part is contained in a disk-shaped cartridge, Disk type The present invention relates to a per- and polyfluoroalkyl compound sampler for personal exposure measurement, which is provided with a detachable cartridge.
[0028] No. 7 The inventions are the first to 6 In any one of the above-mentioned inventions, the present invention relates to a per- and polyfluoroalkyl compound sampler for personal exposure measurement, in which a urethane foam filter section made of urethane foam is disposed in front of the activated carbon filter section. Effect of the Invention
[0029] According to the first aspect of the present invention, there is provided a portable sampler for measuring personal exposure to per- and polyfluoroalkyl compounds, the sampler having an activated carbon filter section that uses activated carbon as a main adsorbent for releasably adsorbing per- and polyfluoroalkyl compounds, and the BET specific surface area of the activated carbon is 900 m 2 / g or more The sum of the micropore volumes of the activated carbon of 1 nm or less (V mic ) is 0.35 cm 3 / g or more, and the sum of the mesopore volumes of 2 to 60 nm of the activated carbon (V met ) is 0.03 cm 3 / g or more, Since the pressure loss in the activated carbon filter section is less than 6 kPa under a wind speed of 0.5 m / sec, per- and polyfluoroalkyl compounds present in the air in a work environment or the like can be efficiently captured in a desorbable manner. and the accuracy of quantitative analysis of the compound can be improved. It is also portable and easy to handle.
[0030] No. 2 According to the invention of the per- and polyfluoroalkyl compound sampler for personal exposure measurement, 1 Invention In the above, the sum of the micropore volumes (V mic ) and the sum of the mesopore volume (V met ) and the volume difference (V s ) is 0.35 or more, per- and polyfluoroalkyl compounds can be efficiently captured in a desorbable manner, and the accuracy of quantitative analysis of the compounds can be improved.
[0031] No. 3 According to the invention of the per- and polyfluoroalkyl compound sampler for personal exposure measurement, Invention 1 or 2 In this case, since the surface oxide amount of the activated carbon is 0.10 meq / g or more, the activated carbon has not only the adsorption performance due to the pores of the activated carbon but also the chemical adsorption ability, which can further improve the adsorption performance of neutral per- and polyfluoroalkyl compounds, and can increase the accuracy of the quantitative analysis of the compounds.
[0032] No. 4According to the invention of the per- and polyfluoroalkyl compound sampler for personal exposure measurement, 3 In any one of the above-mentioned inventions, since the activated carbon is fibrous activated carbon, the contact efficiency with per- and polyfluoroalkyl compounds can be increased while ensuring the breathability of the filter portion, thereby improving the adsorption performance.
[0033] No. 5 According to the invention of the per- and polyfluoroalkyl compound sampler for personal exposure measurement, 3 In any one of the above-mentioned inventions, since the activated carbon is granular activated carbon, the form of use can be appropriately determined, which makes it easy to handle, and furthermore, it is easy to obtain and highly economical.
[0034] No. 6 According to the invention of the per- and polyfluoroalkyl compound sampler for personal exposure measurement, 5 In any one of the above-mentioned inventions, the activated carbon filter part is contained in a disk-shaped cartridge, Disk type Since the cartridge is provided detachably, analysis can be performed immediately after removing the cartridge from the sampler, and the cartridge is easy to replace, allowing for continuous use and easy handling.
[0035] No. 7 According to the invention of the per- and polyfluoroalkyl compound sampler for personal exposure measurement, 6 In any of the above-mentioned inventions, a urethane foam filter section made of urethane foam is disposed in front of the activated carbon filter section, so that per- and polyfluoroalkyl compounds present in the air in various forms can be selectively collected according to their form, enabling efficient and comprehensive collection. [Brief description of the drawings]
[0036] [Figure 1] FIG. 2 is a schematic diagram showing a disk-type cartridge provided in the per- and polyfluoroalkyl compound sampler for personal exposure measurement of the present invention. [Diagram 2] FIG. 2 is a partial cross-sectional view of the disk-type cartridge of FIG. 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0037] The personal exposure measurement sampler for per- and polyfluoroalkyl compounds of the present invention is used to measure the exposure of individuals, such as workers, to per- and polyfluoroalkyl compounds in the work environment. A personal sampler for carrying and use is usually connected to a pump that draws in air on one side of a main body having a filter section, and the sample air in the work environment is drawn in from the intake opening on the other side through the filter section, and the measurement target substance in the sample is collected. The sampler of the present invention has a similar configuration.
[0038] By collecting the filter part from a worker wearing a personal sampler after a certain period of time has passed and analyzing the amount of the substance to be measured captured by the filter part, it is possible to measure the personal exposure level in the work environment.
[0039] The sampler of the present invention is intended to collect per- and polyfluoroalkyl compounds present in the atmosphere. Per- and polyfluoroalkyl compounds present in the atmosphere are roughly classified into three types.
[0040] One is particle-adsorbed per- and polyfluoroalkyl compounds, many of which are ionic compounds, that adhere to the surfaces of small airborne particles (eg, dust particles such as pollen and soil particles).
[0041] The second type is semi-volatile perfluoroalkyl compounds such as N-ethylperfluorooctanesulfonamidoethanol (hereinafter referred to as "N-EtFOSE") and N-methylperfluorooctanesulfonamidoethanol (hereinafter referred to as "N-MeFOSE"). According to the definition of the World Health Organization (WHO), semi-volatile organic compounds are compounds with a boiling point of 260 to 380°C. It is known that PFOS and PFOA are produced by the decomposition of semi-volatile perfluoroalkyl compounds. N-EtFOSE is a substance represented by the following chemical formula (iv), and N-MeFOSE is a substance represented by the chemical formula (v).
[0042]
number
[0043]
number
[0044] The third type is volatile per- and polyfluoroalkyl compounds that exist as gases in the atmosphere, such as fluorotelomer alcohols (hereinafter referred to as "FTOHs") as shown in the above-mentioned chemical formula (iii). Volatile organic compounds are defined by the World Health Organization (WHO) as compounds with a boiling point of 50 to 160°C.
[0045] The per- and polyfluoroalkyl compounds, which are the measurement objects of the present invention, exist in the atmosphere in three forms as described above. The sampler of the present invention is mainly intended to collect volatile per- and polyfluoroalkyl compounds in the activated carbon filter section, and furthermore, by disposing a urethane foam filter section in front of the activated carbon filter section, it is possible to collect semi-volatile perfluoroalkyl compounds as well.
[0046] The sampler of the present invention comprises a syringe-type or disk-type cartridge having an intake opening through which sample air is introduced and sucked in, and an activated carbon filter section using activated carbon as an adsorbent, and a pump that sucks in the sample air through the cartridge. Furthermore, depending on the form of the per- and polyfluoroalkyl compounds to be measured, a cartridge having a urethane foam filter section made of urethane foam can also be attached to the intake side of the cartridge.
[0047] First, the urethane foam (PUF) of the urethane foam filter section arranged on the upstream side can capture semi-volatile perfluoroalkyl compounds. Furthermore, a known sampler for capturing fine particles may be installed on the upstream side of the urethane foam filter section. The sampler for capturing fine particles can be appropriately selected from an inertial impactor, a filter device using filter paper, and the like.
[0048] The activated carbon filter section is intended to mainly capture volatile per- and polyfluoroalkyl compounds. The adsorption performance of the activated carbon in the activated carbon filter section is, as will be explained in the examples below, a specific surface area of 900 m 2 / g or more. By forming a certain number of pores in the activated carbon, the adsorption performance of the compound is ensured.
[0049] Activated carbon is also defined by the pore size. In the case of an adsorbent such as activated carbon, there are micropores, mesopores, and macropores. The adsorption target and performance of activated carbon change depending on which range of pores is developed more. In the present invention, the performance desired for activated carbon is to effectively and releasably adsorb molecules of per- and polyfluoroalkyl compounds.
[0050] By collecting semi-volatile perfluoroalkyl compounds with a urethane foam filter section arranged in front of the activated carbon filter section, the micropores of the activated carbon are prevented from being blocked, and the deterioration of the adsorption performance can be expected to be reduced. In addition, by attaching a filter for collecting fine particles to the urethane foam filter section or the front of the urethane foam filter section, fine particles can be removed in front of the activated carbon filter section, and the deterioration of the performance of the activated carbon can be further suppressed. In addition, since the sampler for personal exposure measurement is not expected to be used for long periods of time, it is possible to sufficiently sample the measurement target without attaching a urethane foam filter section or the like.
[0051] In this way, since it is possible to comprehensively collect particles (per- and polyfluoroalkyl compounds adsorbed thereon), semi-volatile perfluoroalkyl compounds, and volatile per- and polyfluoroalkyl compounds, it is possible to comprehensively and highly accurately measure the amount of personal exposure to atmospheric per- and polyfluoroalkyl compounds in the work environment. In particular, it is possible to measure the amount of personal exposure to volatile per- and polyfluoroalkyl compounds, which was previously difficult to do.
[0052] Since the sampler of the present invention is used for personal exposure measurement and is therefore constructed to be portable, a small pump is preferably used as the suction power source from the viewpoint of ease of handling for the sampler user (operator). Since a small pump does not have a large suction force, it is necessary to reduce the load on the pump. For these reasons, it is desirable for the pressure loss in the filter section to be small, and it is preferable for the pressure loss to be less than 6 kPa under conditions of a wind speed of 0.5 m / sec.
[0053] The per- and polyfluoroalkyl compound-adsorbing activated carbon is made of fibrous activated carbon or granular activated carbon. The fibrous activated carbon is activated carbon obtained by carbonizing and activating appropriate fibers, such as phenolic resin-based, acrylic resin-based, cellulose-based, and coal pitch-based activated carbon. The fiber length and cross-sectional diameter are appropriate. If the fiber cross-sectional diameter is too large, the surface area is reduced and the contact efficiency is reduced, so in terms of improving the adsorption capacity, it is preferable that the fiber cross-sectional diameter is 30 μm or less.
[0054] The fibrous activated carbon can be formed into a felt-like shape to form an activated carbon filter section. Forming it into a felt-like shape improves breathability. Activated carbon filter sections using fibrous activated carbon tend to have a high adsorption rate because of their large surface area. For these reasons, it is possible to improve breathability while enhancing adsorption performance.
[0055] The raw materials for granular activated carbon include wood (waste wood, thinning wood, sawdust), coffee bean residue, rice husks, coconut shells, bark, and fruit. These naturally derived raw materials are prone to developing pores through carbonization and activation. In addition, since it is a secondary use of waste, it can be procured at low cost. Other raw materials that can be used include tires, petroleum pitch, burned products derived from synthetic resins such as urethane resins and phenolic resins, and even coal. If the particle size of the activated carbon is small, the density of the filter body increases, and the adsorption amount of per- and polyfluoroalkyl compounds increases. On the other hand, if the particle size is large, the density of the filter body decreases, and the breathability improves. For these reasons, if the average particle size of the granular activated carbon is in the range of 200 μm or more, breathability can be ensured.
[0056] Since the present invention is a sampler for personal exposure, it is unlikely that the activated carbon installed in the device will adsorb per- and polyfluoroalkyl compounds to the limit of its adsorption performance. For this reason, no upper limit for the average particle size is specified. However, since increasing the breathability too much may cause leakage of the target substance, the adsorption performance is guaranteed by the physical properties, and the possibility of leakage can be reduced by adjusting the thickness of the filter part as desired.
[0057] The activated carbon filter section is preferably housed in a disk-type cartridge 10 as shown in Figures 1 and 2, and is detachably attached to the sampler. By housing the activated carbon filter section 20 in the cartridge, the cartridge can be removed from the sampler and immediately analyzed. It is believed that the disk-type cartridge 10 improves adsorption efficiency because the sample air spreads and ventilates from the intake opening 11 to the main body section 12. The activated carbon filter section 20 is easy to handle if it is formed into, for example, a felt-like filter section 21 as shown in Figure 2. In addition, since it is easy to attach and detach, it is easy to replace, can be used continuously, and is easy to handle.
[0058] The activated carbon raw material is heated and carbonized at a temperature range of 200°C to 600°C as necessary to form micropores. The activated carbon raw material is then exposed to steam and carbon dioxide gas at a temperature range of 600°C to 1200°C for activation. As a result, activated carbon with various types of developed pores is produced. Other activation methods include activation with zinc chloride. Sequential washing is also performed.
[0059] As mentioned above, an index that specifies the physical properties of the activated carbon itself is also added. This specification is controlled by the activation conditions mentioned above. The specific surface area of the activated carbon is 900 m 2 / g or more. In this specification, the specific surface area of each prototype is measured by the BET method (Brunauer, Emmett and Teller method). 2 When the specific surface area is less than 1 / g, the pore volume becomes small, and the types of substances that can be adsorbed by a single activated carbon are limited. For this reason, the above range of specific surface area is derived as being appropriate for the per- and polyfluoroalkyl compound-adsorbing activated carbon according to the present invention.
[0060] It was also found that the pore distribution formed in the activated carbon also contributes to the adsorption of per- and polyfluoroalkyl compounds. In this specification, the term "micropore" refers to a pore having a diameter of 1 nm or less, and as will be derived from the examples described later, the pore volume (Vmic ) total is 0.35cm 3 / g or more, the adsorption performance of per- and polyfluoroalkyl compounds is improved. In this specification, the micropore volume of 1 nm or less in each prototype is measured by the MP method (Micropore method). It is considered that the formation of a certain number of micropores or more makes it easier for the compound to be captured in the pores.
[0061] In this specification, the term "mesopores" refers to pores having a pore diameter in the range of 2 to 60 nm, and as will be explained in the examples below, the pore volume (V met ) is 0.03cm 3 / g or more, the adsorption performance of per- and polyfluoroalkyl compounds is improved. In this specification, the mesopore volume in the range of 2 to 60 nm in each prototype is measured by the DH method (Dollimore-Heal method). Since the measurement is by the DH method, the measurement targets were pores of 2.43 to 59.72 nm. It is considered that the formation of a certain number of mesopores or more allows the compound to easily penetrate into the micropores.
[0062] In addition, the difference between the pore volume of the micropores and the pore volume of the mesopores is also thought to contribute to the efficient adsorption of per- and polyfluoroalkyl compounds. As will be explained in the examples below, the sum of the micropore volumes (V mic ) and the sum of the mesopore volume (V met ) and the volume difference (V s By making the ratio of the adsorption capacity of the activated carbon to be 0.35 or more, the per- and polyfluoroalkyl compounds can be adsorbed efficiently and desorbed. By making the activated carbon have well-developed micropores in addition to not overdeveloping the mesopores, it is believed that the adsorption performance of the per- and polyfluoroalkyl compounds can be improved while the compounds can be smoothly desorbed during the subsequent extraction operation, thereby enabling good quantitative measurement.
[0063] The activated carbon thus produced also has acidic functional groups on its surface. The acidic functional groups that increase due to the surface oxidation of the activated carbon are mainly hydrophilic groups such as carboxyl groups and phenolic hydroxyl groups. The acidic functional groups on the surface of the activated carbon affect the collection capacity. The amount of these acidic functional groups can be understood as the amount of surface oxide. It is believed that an increase in the amount of surface oxide of the activated carbon increases the hydrophilicity of the surface of the activated carbon, and improves the collection performance of per- and polyfluoroalkyl compounds, particularly hydrophilic fluorotelomer compounds.
[0064] The following methods can be used to increase the surface oxide of activated carbon. One method is to promote the oxidation of the surface residue by passing through a heating process again, thereby increasing the acidic functional groups. That is, oxidation in an air or oxygen atmosphere. Alternatively, air at a temperature of 25 to 40°C and a humidity of 60 to 90% is also introduced at the same time under an air atmosphere. Then, the activated carbon is heated at 150 to 900°C for 1 to 10 hours, and the adsorbent activated carbon of the present invention is completed. It is considered that the acidic functional groups increase because the hydrocarbon groups such as alkyl groups present on the activated carbon surface are oxidized by heating with moist air, or the hydroxyl groups of water are introduced to the surface.
[0065] Another method is to oxidize the surface of activated carbon with an oxidizing agent to increase the amount of surface oxide. Examples of oxidizing agents include hypochlorous acid and hydrogen peroxide. Activated carbon with an increased amount of surface oxide can be obtained by immersing the activated carbon in a liquid containing such an oxidizing agent and then drying it.
[0066] The amount of acidic functional groups on the surface of the activated carbon can be measured as the amount of surface oxide, as shown in each prototype example below. Specifically, the amount of surface oxide is preferably 0.10 meq / g or more. If it is less than 0.10 meq / g, the hydrophobicity of the activated carbon increases, and the collection performance of the per- and polyfluoroalkyl compounds to be collected, particularly fluorotelomer compounds, tends to decrease. By making the amount of surface oxide 0.10 meq / g or more, the hydrophilicity of the activated carbon surface can be increased, and per- and polyfluoroalkyl compounds can be efficiently adsorbed. EXAMPLES
[0067] [Study of adsorption performance and breathability] In order to prepare a sampler for personal exposure measurement, the inventors prepared filter parts of prototypes 1 to 19 to be provided in the sampler, and carried out adsorption tests and air permeability tests.
[0068] [Activated carbon used] The inventors used the following raw materials when producing the filter portion of the prototype. · Fibrous activated carbon Futamura Chemical Co., Ltd.: Fibrous activated carbon "FE3010" (average fiber diameter: 15 μm) Futamura Chemical Co., Ltd.: Fibrous activated carbon "FE3012" (average fiber diameter: 15 μm) Futamura Chemical Co., Ltd.: Fibrous activated carbon "FE3015" (average fiber diameter: 15 μm) Futamura Chemical Co., Ltd.: Fibrous activated carbon "FE3018" (average fiber diameter: 15 μm) ·Granular activated carbon Futamura Chemical Co., Ltd.: Granular activated carbon "CW240SZ" (average particle size: 620 μm) Futamura Chemical Co., Ltd.: Granular activated carbon "CW480SZ" (average particle size: 260 μm) Futamura Chemical Co., Ltd.: Granular activated carbon "CW8150SZ" (average particle size: 200 μm) Futamura Chemical Co., Ltd.: Granular activated carbon "SZ100M" (average particle size: 100 μm)
[0069] [Preparation of activated carbon] <Activated carbon C1> 10 g of fibrous carbonized material, which is made by carbonizing phenolic resin fiber, the same raw material as Futamura Chemical's fibrous activated carbon "FE3010," at 600°C, was immersed in 500 ml of a 4.0% hydrogen peroxide solution and left to stand for 70 hours. The fibrous carbonized material was then taken out and dried to obtain activated carbon C1.
[0070] <Activated carbon C2> 10 g of fibrous activated carbon "FE3010" manufactured by Futamura Chemical Co., Ltd. was immersed in 500 ml of a 4.0% hydrogen peroxide solution, left to stand for 150 hours, then taken out and dried to obtain the fibrous activated carbon, designated as activated carbon C2.
[0071] <Activated carbon C3> 10 g of fibrous activated carbon "FE3012" manufactured by Futamura Chemical Co., Ltd. was immersed in 500 ml of a 4.0% hydrogen peroxide solution, left to stand for 150 hours, then taken out and dried to obtain the fibrous activated carbon, designated as activated carbon C3.
[0072] <Activated carbon C4> The fibrous activated carbon "FE3015" manufactured by Futamura Chemical was used as activated carbon C4.
[0073] <Activated carbon C5> 10 g of fibrous activated carbon "FE3015" manufactured by Futamura Chemical Co., Ltd. was immersed in 500 ml of a 1.5% hydrogen peroxide solution, left to stand for 70 hours, then taken out and dried to obtain the fibrous activated carbon, designated as activated carbon C5.
[0074] <Activated carbon C6> 10 g of fibrous activated carbon "FE3015" manufactured by Futamura Chemical Co., Ltd. was immersed in 500 ml of a 4.0% hydrogen peroxide solution, left to stand for 70 hours, then taken out and dried to obtain the fibrous activated carbon, designated as activated carbon C6.
[0075] <Activated carbon C7> 10 g of fibrous activated carbon "FE3015" manufactured by Futamura Chemical Co., Ltd. was immersed in 500 ml of a 14.0% hydrogen peroxide solution, left to stand for 350 hours, then taken out and dried to obtain fibrous activated carbon C7.
[0076] <Activated carbon C8> 10 g of fibrous activated carbon "FE3015" manufactured by Futamura Chemical Co., Ltd. was immersed in 500 ml of a solution with a hydrogen peroxide concentration of 18.9%, left to stand for 480 hours, then taken out and dried. This fibrous activated carbon was designated as activated carbon C8.
[0077] <Activated carbon C9> 10 g of fibrous activated carbon "FE3018" manufactured by Futamura Chemical Co., Ltd. was immersed in 500 ml of a 4.0% hydrogen peroxide solution, left to stand for 50 hours, then taken out and dried to obtain fibrous activated carbon C9.
[0078] <Activated carbon C10> 10 g of Futamura Chemical granular activated carbon "CW240SZ" was immersed in 500 ml of a 4.0% hydrogen peroxide solution, left to stand for 70 hours, then removed and dried to obtain granular activated carbon, designated as activated carbon C10.
[0079] <Activated carbon C11> 10 g of Futamura Chemical granular activated carbon "CW480SZ" was immersed in 500 ml of a 4.0% hydrogen peroxide solution, left to stand for 70 hours, then removed and dried to obtain granular activated carbon, designated as activated carbon C11.
[0080] <Activated carbon C12> 10 g of Futamura Chemical granular activated carbon "CW8150SZ" was immersed in 500 ml of a 4.0% hydrogen peroxide solution, left to stand for 70 hours, then removed and dried to obtain granular activated carbon, designated as activated carbon C12.
[0081] <Activated carbon C13> 10 g of Futamura Chemical granular activated carbon "SZ100M" was immersed in 500 ml of a 4.0% hydrogen peroxide solution, left to stand for 70 hours, then removed and dried to obtain granular activated carbon, designated as activated carbon C13.
[0082] [Measurement of the physical properties of activated carbon] Specific surface area (m 2 / g) was determined by measuring the nitrogen adsorption isotherm at 77K using an automatic specific surface area / pore distribution analyzer "BELSORP-miniII" manufactured by Microtrack-BEL Corporation and using the BET method (BET specific surface area).
[0083] The amount of surface oxide (meq / g) was determined by applying the Boehm method, in which the adsorbent activated carbon of each example was shaken in a 0.05N aqueous solution of sodium hydroxide, filtered, and the filtrate was neutralized and titrated with 0.05N hydrochloric acid to obtain the amount of sodium hydroxide.
[0084] The average pore diameter (nm) is calculated by multiplying the pore volume (ml / g) and specific surface area (m2) obtained from the above measurement, assuming that the pores are cylindrical. 2 / g) according to formula (vi).
[0085]
number
[0086] [Micropore volume] The pore volume was measured by nitrogen adsorption using an automatic specific surface area / pore distribution measuring device (BELSORP-miniII, manufactured by Microtrack Bell Co., Ltd.). The sum of the micropore volumes (V mic )(cm 3 / g) was calculated by analyzing the dV / dD value in the range of pore diameters of 1 nm or less from the t-plot of the nitrogen gas adsorption isotherm using the MP method.
[0087] [Mesopore volume] The value of dV / dD in the pore diameter range of 2 to 60 nm was analyzed by the DH method from the nitrogen gas adsorption isotherm. The diameter range of pore diameters of 2 to 60 nm in the analysis software is 2.43 to 59.72 nm. From the analysis results, the sum of the mesopore volumes (V met )(cm 3 / g) was calculated.
[0088] [Volume difference] Volume difference of activated carbon C1 to C13 (V s ) is the sum of the micropore volumes (V mic )(cm 3 / g) to the sum of mesopore volumes (V met )(cm 3 / g) and was calculated using the above formula (i).
[0089] The physical properties of activated carbons C1 to C13 are shown in Tables 1 to 3. The BET specific surface area (m 2 / g), surface oxide amount (meq / g), average pore diameter (nm), micropore volume (V mic )(cm 3 / g), mesopore volume (V met )(cm 3 / g), volume difference (V s )(cm 3 / g).
[0090] [Table 1]
[0091] [Table 2]
[0092] [Table 3]
[0093] [Creating the filter section] In order to evaluate the adsorption performance, an adsorption test was carried out using Prototype Examples 1 to 10. In addition, in order to evaluate the breathability performance, an air permeability test was carried out using Prototype Examples 11 to 19.
[0094] <Prototype 1> A fibrous carbon felt (thickness 2.0 mm, diameter 25 mm, weight 110 mg) using activated carbon C1 as the main raw material was prepared and used as the filter part of Prototype Example 1. The filter part was set in a polypropylene disk-shaped cartridge having an inner diameter of 25 mm.
[0095] <Prototype Example 2> A fibrous activated carbon felt (thickness 2.0 mm, diameter 25 mm, weight 110 mg) was prepared using activated carbon C2 as the main raw material, and used as the filter part of Prototype Example 2. The filter part was set in a polypropylene disk-shaped cartridge having an inner diameter of 25 mm.
[0096] <Prototype 3> A fibrous activated carbon felt (thickness 2.0 mm, diameter 25 mm, weight 100 mg) was prepared using activated carbon C3 as the main raw material, and used as the filter part of Prototype Example 3. The filter part was set in a polypropylene disk-shaped cartridge with an inner diameter of 25 mm.
[0097] <Prototype 4> A fibrous activated carbon felt (thickness 2.0 mm, diameter 25 mm, weight 90 mg) was prepared using activated carbon C4 as the main raw material, and used as the filter part of Prototype Example 4. The filter part was set in a polypropylene disk-shaped cartridge with an inner diameter of 25 mm.
[0098] <Prototype 5> A fibrous activated carbon felt (thickness 2.0 mm, diameter 25 mm, weight 90 mg) was prepared using activated carbon C5 as the main raw material, and used as the filter part of Prototype Example 5. The filter part was set in a polypropylene disk-shaped cartridge having an inner diameter of 25 mm.
[0099] <Prototype Example 6> A fibrous activated carbon felt (thickness 2.0 mm, diameter 25 mm, weight 90 mg) was prepared using activated carbon C6 as the main raw material, and used as the filter part of Prototype Example 6. The filter part was set in a polypropylene disk-shaped cartridge having an inner diameter of 25 mm.
[0100] <Prototype 7> A fibrous activated carbon felt (thickness 2.0 mm, diameter 25 mm, weight 90 mg) was prepared using activated carbon C7 as the main raw material, and used as the filter part of Prototype Example 7. The filter part was set in a polypropylene disk-shaped cartridge having an inner diameter of 25 mm.
[0101] <Prototype Example 8> A fibrous activated carbon felt (thickness 2.0 mm, diameter 25 mm, weight 90 mg) was prepared using activated carbon C8 as the main raw material, and used as the filter part of Prototype Example 8. The filter part was set in a polypropylene disk-shaped cartridge having an inner diameter of 25 mm.
[0102] <Prototype Example 9> A fibrous activated carbon felt (thickness 2.0 mm, diameter 25 mm, weight 70 mg) was prepared using activated carbon C9 as the main raw material, and used as the filter part of Prototype Example 9. The filter part was set in a polypropylene disk-shaped cartridge having an inner diameter of 25 mm.
[0103] <Prototype Example 10> 150 mg of activated carbon C11 was packed into a 12 ml syringe so as to form a filter part of a 2 mm-thick packed bed, to prepare the filter part of Prototype Example 10. Sintered polyethylene sheets (manufactured by Dikma, the same applies below) that do not allow particles of 10 μm or more to pass were placed before and after the packed bed to fix the activated carbon.
[0104] <Prototype Example 11> 32 mg of activated carbon C1 was packed into a 6 ml syringe to form a filter part of a 2 mm-thick packed layer, to prepare the filter part of Prototype Example 11. Sintered polyethylene sheets with an average pore size of 10 μm were placed in front of and behind the filter part (packed layer) to fix the activated carbon.
[0105] <Prototype Example 12> 30 mg of activated carbon C2 was packed into a 6 ml syringe so as to form a filter part of a 2 mm-thick packed layer, to prepare the filter part of Prototype Example 12. Sintered polyethylene sheets with an average pore size of 10 μm were placed in front of and behind the filter part (packed layer) to fix the activated carbon.
[0106] <Prototype Example 13> 28 mg of activated carbon C3 was packed into a 6 ml syringe to form a filter part of a 2 mm-thick packed layer, to prepare the filter part of Prototype Example 13. Sintered polyethylene sheets with an average pore size of 10 μm were placed in front of and behind the filter part (packed layer) to fix the activated carbon.
[0107] <Prototype Example 14> 24 mg of activated carbon C6 was packed into a 6 ml syringe to form a filter part of a 2 mm-thick packed layer, to prepare the filter part of Prototype Example 14. Sintered polyethylene sheets with an average pore size of 10 μm were placed in front of and behind the filter part (packed layer) to fix the activated carbon.
[0108] <Prototype Example 15> 20 mg of activated carbon C9 was packed into a 6 ml syringe to form a filter part of a 2 mm-thick packed layer, to prepare the filter part of Prototype Example 15. Sintered polyethylene sheets with an average pore size of 10 μm were placed in front of and behind the filter part (packed layer) to fix the activated carbon.
[0109] <Prototype Example 16> 150 mg of activated carbon C10 was packed into a 6 ml syringe to form a filter part of a 2 mm-thick packed layer, to prepare the filter part of Prototype Example 16. When packing, the packing was loosely packed so that the activated carbon surface was horizontal. Sintered polyethylene sheets with an average pore size of 10 μm were placed in front of and behind the filter part (packed layer) to fix the activated carbon.
[0110] <Prototype Example 17> A 6 ml syringe cartridge was filled with 180 mg of activated carbon C11 to form a filter part with a 2 mm-thick packed layer, to prepare the filter part of Prototype Example 17. When filling, the activated carbon was loosely packed so that the surface of the activated carbon was horizontal. Sintered polyethylene sheets with an average pore size of 10 μm were placed in front of and behind the filter part (packed layer) to fix the activated carbon.
[0111] <Prototype Example 18> 200 mg of activated carbon C12 was packed into a 6 ml syringe cartridge so as to form a filter part with a 2 mm thick packed layer, to prepare the filter part of Prototype Example 18. When packing, the packing was loosely packed so that the activated carbon surface was horizontal. Sintered polyethylene sheets with an average pore size of 10 μm were placed in front of and behind the filter part (packed layer) to fix the activated carbon.
[0112] <Prototype Example 19> Activated carbon C13 was packed in a 6 ml syringe cartridge at 230 mg to form a filter part with a 2 mm-thick packed layer, to prepare the filter part of Prototype Example 19. When packing, the packing was loosely packed so that the activated carbon surface was horizontal. Sintered polyethylene sheets with an average pore size of 10 μm were placed in front of and behind the filter part (packed layer) to fix the activated carbon.
[0113] [Measurement of adsorption performance] Using Prototype Examples 1 to 10, the collection efficiency of per- and polyfluoroalkyl compounds was measured. As per- and polyfluoroalkyl compounds, evaluation was performed using fluorotelomer alcohols (hereinafter referred to as "FTOHs"), iodinated fluorine compounds, and brominated fluorine compounds. FTOHs is a substance represented by the above chemical formula (iii), and the substance name varies depending on the number of carbon atoms. For example, C8F 17 In the case of CH2CH2OH, it is named 8:2FTOH (IUPAC name: 3,3,4,4,5,5,6,6,7,7,8,8,9,9,10,10,10-heptadecafluoro-1-decanol). N-EtFOSA is the substance represented by the following chemical formula (vii).
[0114]
number
[0115] A 20 ml syringe (manufactured by AS ONE Corporation, diameter 20 mm) filled with polyurethane foam (PUF) (manufactured by Shibata Scientific Co., Ltd., diameter 20 mm, length 50 mm) was directly connected to the front stage of the cartridge equipped with the filter part of Prototype Example 1 to Prototype Example 10. In addition, a sampling pump (manufactured by Shibata Scientific Co., Ltd., "MP-Σ500N II") was connected to the rear stage of each cartridge via a polypropylene tube using vinyl tape to prevent leaks.
[0116] Each standard substance was diluted with methanol to 100 ppb, and 100 μl of the diluted solution was added to polyurethane foam (PUF), and 25°C air was passed through it at a rate of 2.0 L / min for 8 hours. After the aeration, 15 ml of a mixed solvent mainly composed of dichloromethane and ethyl acetate was passed through each cartridge at a rate of 1 drop / sec, and the extract was collected.
[0117] The extract was quantitatively measured in MRM mode using a GC-MS / MS ("GCMS-TQ8050", manufactured by Shimadzu Corporation) to confirm the collection performance.
[0118] Tables 4 to 8 show the recovery rates (%) of fluoro iodide compounds and brominated fluoride compounds in addition to fluoro telomer alcohol (FTOH) for each standard substance for Prototype Examples 1 to 10. The target substances were 4:2 FTOH (IUPAC name: 3,3,4,4,5,5,6,6,6-nonafluoro-1-hexanol), 6:2 FTOH (IUPAC name: 3,3,4,4,5,5,6,6,7,7,8,8,8-tridecafluoro-1-octanol), 8:2 FTOH, and 10:2 FTOH (IUPAC name: 3,3,4,4,5,5,6,6,7,7,8,8,9,9,10,10,11,11,12,12,12-heneicosafluoro-1-dodecanol). ), 6:2FTI (IUPAC name: 1,1,1,2,2,3,3,4,4,5,5,6,6-tridecafluoro-8-iodooctane), 8:2FTI (IUPAC name: 1,1,1,2,2,3,3,4,4,5,5,6,6,7,7,8,8-heptadecafluoro-12-iodododecane), 10:2FTI (IUPAC name: 1,1,1,2,2,3,3,4,4,5,5,6,6,7,7,8,8,9,9,10,10-heneicosafluoro-12-iodo dodecane), PFDeI (IUPAC name: 1,1,1,2,2,3,3,4,4,5,5,6,6,7,7,8,8,9,9,10,10-pentacosafluoro-10-iodododecane), PFDoI (IUPAC name: 1,1,1,2,2,3,3,4,4,5,5,6,6,7,7,8,8,9,9,10,10,11,11,12,12-pentacosafluoro-12-iodododecane), PFBuDiI (IUPAC name: 1,1,2,2,3,3,4,4- octafluoro-1,4-diiodobutane), PFHxDiI (IUPAC name: 1,1,2,2,3,3,4,4,5,5,6,6-dodecafluoro-1,6-diiodohexane), PFoDiI (IUPAC name: 1,1,2,2,3,3,4,4,5,5,6,6,7,7,8,8-hexadecafluoro-1,8-diiodooctane), and C8H3BrF6 (IUPAC name: 1-bromo-3,5-bis(trifluoromethyl)benzene).
[0119] The fluorine iodo compound (FTI) is a substance represented by the following chemical formula (viii), PFDeI and PFDoI are represented by the chemical formula (ix), PFBuDiI, PFHxDiI and PFoDiI are represented by the chemical formula (x), and the fluorine bromide compound (C8H3BrF6) is represented by the chemical formula (xi).
[0120]
number
[0121]
number
[0122]
number
[0123]
number
[0124] The recovery rate of each standard substance was evaluated as follows: 70% or more was marked with "◎", less than 70% and more than 50% was marked with "〇", less than 50% and more than 40% was marked with "△", and less than 40% was marked with "×". The overall evaluation was given to those with 7 or less "〇" (half) and no "△" or "×" in the evaluation of the recovery rate of each standard substance, "A", those with no "×" were marked with "B", and those with at least one "×" were marked with "C".
[0125] [Table 4]
[0126] [Table 5]
[0127] [Table 6]
[0128] [Table 7]
[0129] [Table 8]
[0130] In the table, "ND" indicates that the level was below the detection limit.
[0131] In addition, to confirm that none of the standard substances added to the PUF remained without volatilizing, the remaining rate (%) in the PUF was also measured. If the remaining rate in the PUF was 10% or less, it could be confirmed that the volatilized standard substances had sufficiently come into contact with each prototype.
[0132] Furthermore, in Tables 9 to 11, as semi-volatile target substances, ethyl perfluorooctanesulfamide (IUPAC name: N-ethyl-1,1,2,2,3,3,4,4,5,5,6,6,7,7,8,8,8-heptadecafluorooctane-1-sulfamide) (hereinafter referred to as "N-EtFOSA"), N-methylperfluorooctanesulfonamide (IUPAC name: 1,1,2,2,3,3,4,4,5,5,6,6,7,7,8,8,8-heptadecafluoro-N-methyl-1-octanesulfonamide) (hereinafter referred to as "N-MeFOSA"), and N-methylperfluorooctanesulfonamidoethanol (IUPAC name: The recovery rate (%) was measured in the urethane foam filter section attached to the front stage of prototypes 1 to 10 using 1,1,2,2,3,3,4,4,5,5,6,6,7,7,8,8,8-heptadecafluoro-N-(2-hydroxyethyl)-N-methyl-1-octanesulfonamide) (hereinafter referred to as "N-MeFOSE") and N-ethylperfluorooctanesulfonamideethanol (IUPAC name: N-ethyl-1,1,2,2,3,3,4,4,5,5,6,6,7,7,8,8,8-heptadecafluoro-N-(2-hydroxyethyl)-1-octanesulfonamide) (hereinafter referred to as "N-EtFOSE").
[0133] N-EtFOSA is a substance represented by the above-mentioned chemical formula (vii), and N-MeFOSA is a substance represented by the following chemical formula (xii).
[0134]
number
[0135] [Table 9]
[0136] [Table 10]
[0137] [Table 11]
[0138] [Results and Discussion] For Prototype Examples 3 to 10, the recovery rates of all the standard substances were good. For Prototype Examples 1 and 2, the recovery rates were below the detection limit or very low, indicating that adsorption was not possible and that they did not have sufficient collection performance. It is presumed that Prototype Examples 1 and 2 did not have the specific surface area required for collection, and therefore did not fully demonstrate collection performance.
[0139] For prototypes 3 to 10, good results were obtained for the recovery rates of all standard substances, and the samples had excellent collection performance. 2 It was shown that the target substances can be adsorbed when the concentration is 0.015g / g or more.
[0140] Furthermore, when Prototype 4, which uses the same activated carbon raw material, is compared with Prototypes 5 to 8, which have an increased amount of surface oxide, it is shown that Prototypes 5 to 8 have better adsorption performance for the target substance. It can be seen that increasing the amount of surface oxide on the activated carbon improves the affinity with FTOH, which has a hydrophilic group, and improves the adsorption performance of FTOH.
[0141] The polyurethane foam filter showed stable and good recovery rates for semi-volatile target substances. In addition, considering that all fluorotelomer alcohols were below the detection limit, it was shown that it is possible to selectively collect semi-volatile perfluoroalkyl compounds.
[0142] [Measurement of breathability] Next, the inventors conducted an air permeability test using the filter parts of prototypes 11 to 19. The reason why the thickness of the packed layer was set to 2 mm is that if the packed layer is less than 2 mm, it is difficult to pack the packed layer uniformly in the cartridge, and there may be some places that cannot sufficiently contact the target substance, which may cause a short pass.
[0143] The pressure difference between the front and rear of the cartridges of prototypes 11 to 19 was measured, and the ventilation performance was evaluated by measuring the pressure loss. Polypropylene tubes for measuring the differential pressure gauge were connected to the front and rear of the cartridges of each prototype using vinyl tape to prevent leaks. Air at 25°C was ventilated using a sampling pump (manufactured by Shibata Scientific Co., Ltd., "SIP-32L type") at five airflow rates of 1.0, 2.0, 3.0, 4.0, and 5.0 L / min to measure the pressure difference between the front and rear of the cartridges of each prototype.
[0144] Tables 12 and 13 show the differential pressure (kPa) before and after the cartridges of prototypes 11 to 19 and a cartridge filled with only two sintered polyethylene sheets and not equipped with an activated carbon filter section as a "BLANK". In the tables, each prototype is filled in a 6 ml syringe, so the five levels of air volume are converted to the air speed in the right column of the table. Since the pressure loss is roughly proportional to the air speed, the cartridges of each prototype were evaluated based on the pressure loss at an air speed of 0.5 m / sec. In addition, Tables 14 and 15 show the difference between the pressure loss in each prototype and the pressure loss in "BLANK", and the pressure loss in the activated carbon filter section of each prototype was calculated. A pressure loss in the activated carbon filter section of less than 5 kPa was evaluated as "◯", a pressure loss of 5 kPa or more but less than 6 kPa was evaluated as "△", and a pressure loss of 6 kPa or more was evaluated as "×".
[0145] [Table 12]
[0146] [Table 13]
[0147] [Table 14]
[0148] [Table 15]
[0149] [Results and Discussion] In prototype 19, the particle size of the adsorbent activated carbon was too small, causing a large pressure loss, and when the suction pump air volume was increased to 4.0 L / min (air speed 0.5 m / sec) or more, the load became too large and it became impossible to operate safely, resulting in a "- (impossible to measure)." In the cartridge of prototype 18, the pressure loss was at a level that allowed it to operate without problems, given the performance of a general small pump, so when the adsorbent is granular activated carbon, it is desirable for the average particle size to be 200 μm or more.
[0150] In prototypes 11 to 16, which used fibrous activated carbon or granular activated carbon with an average particle size of more than 200 μm, there was almost no pressure loss even when the filter layer was thick enough to take short paths into account, and it can be said that the target substance can be measured sufficiently even when a small pump is used as the suction power source.
[0151] [Treatment experiments of per- and polyfluoroalkyl compounds in real environments] Using the activated carbon filter part of Prototype Example 5, a collection experiment of per- and polyfluoroalkyl compounds in a real environment was carried out. A 20 ml syringe (manufactured by AS ONE Corporation, diameter 20 mm) filled with polyurethane foam (PUF) (manufactured by Shibata Scientific Co., Ltd., diameter 20 mm, length 50 mm) was directly connected to the front stage of the cartridge equipped with the filter part of Prototype Example 5. In addition, a sampling pump (manufactured by Shibata Scientific Co., Ltd., "MP-Σ500N II") was connected to the rear stage of each cartridge via a polypropylene tube using vinyl tape to prevent leaks.
[0152] The samplers with the above configuration were installed in the living room and bedroom of the inventor's home (January 2020). In consideration of actual usage conditions, they were installed at a height of approximately 140 cm from the floor to approximate the height of the human respiratory zone. In this experiment, in order to improve the measurement sensitivity, the air was ventilated for 11 hours at a ventilation rate of 10.0 ml / min. The temperature in the living room of the inventor's home was 12.9 to 23.0 ° C (average 22 ° C), and the temperature in the bedroom was 12.9 to 23.0 ° C (average 22 ° C).
[0153] In the activated carbon filter of Prototype Example 5, measurements were performed on per- and polyfluoroalkyl compounds, including fluorotelomer alcohols (FTOHs) such as 4:2FTOH, 6:2FTOH, 8:2FTOH, and 10:2FTOH, iodine fluoride compounds such as 6:2FTI, 8:2FTI, 10:2FTI, PFDeI, PFDoI, PFBuDi, PFHxDiI, and PFoDiI, and bromine fluoride compounds such as C8H3BrF6. FTI is a substance represented by the above-mentioned chemical formula (viii). In addition, the recovery rate (%) was also measured using 4:2FTOH, 6:2FTOH, 8:2FTOH, and 10:2FTOH as surrogates.
[0154] In the polyurethane foam filter part made of polyurethane foam (PUF), the recovery rate (%) was measured using N-MeFOSA and N-EtFOSA as perfluorooctanoic acids, and N-MeFOSE and N-EtFOSE as perfluorooctane sulfonic acids. The recovery rate (%) was also measured using N-MeFOSA, N-EtFOSA, N-MeFOSE, and N-EtFOSE as surrogates.
[0155] After the aeration, 15 ml of a mixed solvent mainly composed of dichloromethane and ethyl acetate was passed through each cartridge and urethane foam filter at a rate of 1 drop / sec to collect an extract. The extract was quantitatively measured in MRM mode using a GC-MS / MS ("GCMS-TQ8050", Shimadzu Corporation).
[0156] Table 16 shows the concentration of per- and polyfluoroalkyl compounds in the sample air at the activated carbon filter and Table 17 shows the concentration of per- and polyfluoroalkyl compounds in the sample air at the urethane foam filter (pg / m 3 The concentration of per- and polyfluoroalkyl compounds is calculated by multiplying the amount (pg) of per- and polyfluoroalkyl compounds (target substances) collected by the cumulative flow rate (m 3 ) and was calculated using the following formula (xiii). In the table, "BLANK" indicates the value detected by performing the same measurement on the activated carbon filter part and the urethane foam filter part before the experiment, and "LOQ" indicates the lower limit at which each substance can be quantitatively measured by the measuring device. "-" indicates that it is below the lower limit of quantification, and "ND" indicates that it is below the detection limit.
[0157]
number
[0158] [Table 16]
[0159] [Table 17]
[0160] [Results and considerations of collection experiments of per- and polyfluoroalkyl compounds in real environments] In the experimental results of the activated carbon filter shown in Table 16, three types of fluorotelomer alcohols (FTOHs), 6:2FTOH, 8:2FTOH, and 10:2FTOH, were detected in both the living room and bedroom of the developer's house. It is known that FTOHs are used in carpets, clothing, and interior decorations, and it is considered reasonable that the FTOHs were detected in the living room and bedroom where various furniture is installed. In addition, although the target substances detected in the living room and bedroom were the same type, a clear difference in concentration was confirmed and the recovery rate of the surrogate was also good, so that it can be said that the sampler is useful for measuring per- and polyfluoroalkyl compounds. Furthermore, it was also shown that advanced analysis is possible even under aeration conditions of 10.0 ml / min for 11 hours.
[0161] In the experimental results for the urethane foam filter part shown in Table 17, the target substances were not detected in the living room and bedroom. However, because the recovery rate of the surrogate was good, the accuracy of the sampler for semi-volatile per- and polyfluoroalkyl compounds was good, and it is believed that there were almost no semi-volatile per- and polyfluoroalkyl compounds in the living room and bedroom that were the subject of the measurement.
[0162] As described above, by using activated carbon having the physical property of adsorbing per- and polyfluoroalkyl compounds in a detachable manner, an activated carbon filter part that can efficiently collect the compounds in the air can be obtained. In addition, by using the activated carbon as an adsorbent and forming a filter with a certain degree of breathability, it is possible to make a portable per- and polyfluoroalkyl compound sampler for personal exposure measurement that can perform high-precision measurements.
[0163] In addition, by disposing a urethane foam filter section in front of the activated carbon filter section, it is possible to separate and collect semi-volatile perfluoroalkyl compounds in the urethane foam filter section and volatile per- and polyfluoroalkyl compounds in the activated carbon filter section. In addition, it is also possible to reduce the deterioration of the adsorption performance of the activated carbon, which is an adsorbent. Furthermore, by disposing an inertial impactor or the like that collects particles in front of the urethane foam filter section, it is possible to sample per- and polyfluoroalkyl compounds by form, and it is possible to comprehensively collect and measure per- and polyfluoroalkyl compounds. [Industrial Applicability]
[0164] The per- and polyfluoroalkyl compound sampler for personal exposure measurement of the present invention is highly portable and can be worn by an individual, and can efficiently and releasably collect per- and polyfluoroalkyl compounds in the working environment, making it possible to measure the personal exposure to the compounds, which was not possible with existing samplers. This makes it possible to effectively and efficiently quantitatively evaluate the exposure of workers to regulated persistent organic pollutants, and can significantly prevent health damage to workers. [Explanation of symbols]
[0165] 10 Disk-type cartridge 11 Intake opening 12 Main body 20 Activated carbon filter section 21 Felt filter part
Claims
1. A portable per- and polyfluoroalkyl compound sampler for measuring personal exposure, comprising an activated carbon filter portion having activated carbon as a main adsorbent for releasably adsorbing per- and polyfluoroalkyl compounds, The BET specific surface area of the activated carbon is 900 m 2 / g or more, the sum of the micropore volumes of the activated carbon having a size of 1 nm or less (V mic ) is 0.35 cm 3 / g or more; the sum of mesopore volumes of 2 to 60 nm of the activated carbon (V met ) is 0.03 cm 3 / g or more; The pressure loss in the activated carbon filter section at a wind speed of 0.5 m / sec is less than 6 kPa. A sampler for measuring personal exposure to per- and polyfluoroalkyl compounds, characterized in that:
2. The sum of the micropore volumes of the activated carbon (V mic ) and the sum of the mesopore volume (V met ) and the volume difference (V s 2. The per- and polyfluoroalkyl compound sampler for personal exposure measurement according to claim 1, wherein the value of (I) is 0.35 or more. [Equation 1]
3. 3. The per- and polyfluoroalkyl compound sampler for measuring personal exposure according to claim 1, wherein the amount of surface oxides of the activated carbon is 0.10 meq / g or more.
4. 4. A sampler for measuring personal exposure to per- and polyfluoroalkyl compounds according to claim 1, wherein the activated carbon is fibrous activated carbon.
5. 5. The sampler for measuring personal exposure to per- and polyfluoroalkyl compounds according to claim 1, wherein the activated carbon is granular activated carbon.
6. 6. A sampler for measuring personal exposure to per- and polyfluoroalkyl compounds according to claim 1, wherein the activated carbon filter portion is housed in a disk-shaped cartridge, and the disk-shaped cartridge is detachably provided.
7. 7. A sampler for measuring personal exposure to per- and polyfluoroalkyl compounds according to claim 1, wherein a urethane foam filter section made of urethane foam is disposed in front of said activated carbon filter section.
Citation Information
Patent Citations
Method and apparatus for purging unwanted substances from air
CN106110766A
Active sampling sleeve for persistent organic pollutant in atmosphere
CN107843463A
JP1988094527U
Sheet-shaped material and filter
JP1999226393A
Analytical sampler for analyzing chlorinated organic compound
JP2000035386A