SUBSTRATE PROCESSING METHOD AND SUBSTRATE PROCESSING APPARATUS
By forming a doped layer on a high dielectric film using a metal solution and repairing oxygen vacancies, the method addresses leakage current issues in semiconductor capacitors, improving their performance by reducing electron flow paths.
Patent Information
- Application Number
- JP2022579517
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-02-08
- Filing Date
- 2022-01-31
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2042-01-31
AI Technical Summary
Existing semiconductor layer capacitors with dielectric films made of alternately stacked hafnium oxide and titanium oxide suffer from high leakage current due to oxygen vacancies and metal element interactions.
A substrate processing method that includes forming a doped layer on a high dielectric film by replacing the first metal element with a second metal element having higher electronegativity or lower valence, using a metal solution, and repairing oxygen vacancies with an oxidizing agent to reduce leakage current.
The method effectively reduces leakage current while maintaining the dielectric film's thickness, enhancing the capacitor's performance by modulating the Schottky barrier and stabilizing electron flow.
Smart Images

Figure 0007582757000003 
Figure 0007582757000004 
Figure 0007582757000005
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a substrate processing method and a substrate processing apparatus. [Background technology]
[0002] The semiconductor layer capacitor described in Patent Document 1 is formed by interposing a dielectric film between an upper electrode and a lower electrode. The dielectric film includes a film in which hafnium oxide and titanium oxide are alternately laminated at the atomic layer level. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Japanese Patent Publication No. 2009-59889 Summary of the Invention [Problem to be solved by the invention]
[0004] One aspect of the present disclosure provides a technique for reducing leakage current in a high dielectric film. [Means for solving the problem]
[0005] A substrate processing method according to one embodiment of the present disclosure includes the following steps (A) to (C): (A) preparing a substrate having a high dielectric constant film having a higher dielectric constant than a SiO2 film formed thereon; (B) supplying to the substrate a metal solution containing a second metal element having a higher electronegativity or a lower valence than a first metal element contained in the high dielectric constant film; and (C) forming a doping layer on a surface of the high dielectric constant film by substituting the second metal element for the first metal element. Effect of the Invention
[0006] According to one aspect of the present disclosure, the leakage current of a high dielectric film can be reduced. [Brief description of the drawings]
[0007] [Figure 1] FIG. 1 is a cross-sectional view showing a substrate obtained by using a substrate processing method according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a flowchart showing a substrate processing method according to an embodiment. [Diagram 3] 3(A) is a cross-sectional view showing the substrate at S101 in FIG. 2, FIG. 3(B) is a cross-sectional view showing the substrate at S102 in FIG. 2, FIG. 3(C) is a cross-sectional view showing the substrate at S103 in FIG. 2, FIG. 3(D) is a cross-sectional view showing the substrate at S104 in FIG. 2, and FIG. 3(E) is a cross-sectional view showing the substrate at S105 in FIG. 2. [Figure 4] FIG. 4 is a cross-sectional view showing an example of a dipole formed on the surface of a high dielectric film. [Diagram 5] FIG. 5 is a diagram showing an example of the rise of the Schottky barrier due to a dipole. [Figure 6] FIG. 6 is a diagram showing an example of a method for testing leakage current of a high dielectric film. [Figure 7] FIG. 7 is a diagram showing the evaluation results under the processing conditions 1 and 8 in Table 1. [Figure 8] FIG. 8 is a diagram showing the evaluation results under the treatment conditions 1 to 8 in Table 1. [Figure 9] FIG. 9 is a flowchart showing a substrate processing method according to a modified example. [Figure 10] FIG. 10 is a cross-sectional view showing another example of a dipole formed on the surface of a high dielectric film. [Figure 11] FIG. 11 is a cross-sectional view showing an example of a substrate processing apparatus. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. In the drawings, the same or corresponding components are denoted by the same reference numerals, and the description thereof may be omitted.
[0009] First, before describing the substrate processing method according to the present embodiment, a substrate 10 obtained using the substrate processing method will be described with reference to Fig. 1. The substrate 10 is a semiconductor device, and includes, for example, a capacitor. The substrate 10 includes, for example, a semiconductor substrate 11, a first electrode 12, a high dielectric film 13, a doping layer 14, and a second electrode 15.
[0010] The semiconductor substrate 11 is, for example, a silicon wafer. The silicon wafer may contain a p-type dopant such as phosphorus or an n-type dopant such as boron. The semiconductor substrate 11 may be a compound semiconductor wafer. The compound semiconductor wafer is not particularly limited, but may be, for example, a GaAs wafer, a SiC wafer, a GaN wafer, or an InP wafer.
[0011] The first electrode 12 and the second electrode 15 are conductive films such as TiN films. The TiN films are formed by ALD (Atomic Layer Deposition) or CVD (Chemical Vapor Deposition). When the semiconductor substrate 11 contains a dopant, the first electrode 12 may be a part of the semiconductor substrate 11.
[0012] The high dielectric film 13 has a higher dielectric constant than a SiO2 film. The high dielectric film 13 includes, for example, a zirconium oxide film or a hafnium oxide film. The high dielectric film 13 is formed by an ALD method or a CVD method. The high dielectric film 13 has a single-layer structure in this embodiment, but may have a multi-layer structure. The multi-layer high dielectric film 13 is, for example, a ZrO2 film / Al2O3 film / ZrO2 film, a ZrO2 film / Al2O3 film, or a HfO2 film / Al2O3 film. The multi-layer high dielectric film 13 preferably includes a zirconium oxide film or a hafnium oxide film in the uppermost layer on which the doping layer 14 is formed.
[0013] As described later, the substrate processing method according to this embodiment includes forming a doped layer 14 on the surface of the high dielectric film 13 before forming a second electrode 15 on the surface of the high dielectric film 13. The doped layer 14 is a so-called monolayer. As described later in detail, by forming the doped layer 14, it is possible to modulate the Schottky barrier and reduce the leakage current while suppressing an increase in the film thickness of the high dielectric film 13.
[0014] Next, a substrate processing method according to the present embodiment will be described with reference to Fig. 2. The substrate processing method includes steps S101 to S108 shown in Fig. 2. Note that the substrate processing method does not need to include all of steps S101 to S108 shown in Fig. 2, and may further include steps not shown.
[0015] Step S101 includes preparing the substrate 10. Preparing the substrate 10 includes, for example, carrying the substrate 10 into a substrate processing apparatus 20 (see FIG. 11) described below. On the surface of the substrate 10, the second electrode 15 has not yet been formed, and the high dielectric film 13 is exposed. The high dielectric film 13 shown in FIG. 3(A) is a zirconium oxide film. The high dielectric film 13 includes oxygen vacancies 13a formed during the formation of the high dielectric film 13.
[0016] Step S102 includes repairing oxygen vacancies 13a in the high dielectric film 13 with an oxidizing agent before forming the doping layer 14. An oxidizing chemical is used as the oxidizing agent. The oxidizing chemical is, for example, ozone water, SC1 (aqueous solution containing ammonium hydroxide and hydrogen peroxide), hydrogen peroxide, or SPM (aqueous solution containing sulfuric acid and hydrogen peroxide). The oxidizing agent reduces oxygen vacancies 13a as shown in FIG. 3(B) and reduces the path of leakage current. Therefore, the leakage current can be reduced.
[0017] The above step S102 includes, for example, discharging an oxidizing chemical onto the surface of the high dielectric film 13 from a nozzle disposed above the substrate 10 while the substrate 10 is held horizontally with the high dielectric film 13 facing upward, to form a liquid film of the oxidizing chemical. At that time, the substrate 10 may be rotated. Also, the nozzle may be scanned in the radial direction of the substrate 10. The nozzle may be a two-fluid nozzle, and may supply a mist of the oxidizing chemical to the substrate 10. The oxidizing chemical is collected in a cup 26 (see FIG. 11).
[0018] The above step S102 may include immersing the substrate 10 in an oxidizing chemical solution stored inside a processing tank. When the substrate 10 is immersed in the oxidizing chemical solution, a plurality of substrates 10 can be processed at once.
[0019] Step S103 includes supplying to the substrate 10 a metal solution containing a second metal element having a higher electronegativity or a lower valence than the first metal element contained in the high dielectric film 13. As shown in Fig. 3(C), when the high dielectric film 13 is zirconium oxide, the first metal element is zirconium (Zr). When the high dielectric film 13 is hafnium oxide, the first metal element is hafnium (Hf). Both Zr and Hf have a valence of four.
[0020] As described above, the metal solution contains a second metal element having a higher electronegativity or a lower valence than the first metal element. The second metal element may have a higher electronegativity and a lower valence than the first metal element. As described later, a dipole can be formed on the surface of the high dielectric film 13 by replacing the first metal element contained in the high dielectric film 13 with the second metal element contained in the metal solution.
[0021] The second metal element includes, for example, one or more selected from Co, Ni, Mo, W, V, Cr, and Nb. From the viewpoint of substitution with the first metal element, the second metal element is preferably one having a small difference in ionic radius from the first metal element. Therefore, the second metal element preferably includes one or more selected from Co, Ni, and Nb. Co, Ni, and Nb have a small difference in ionic radius from Zr and Hf. The second metal element shown in FIG. 3(C) is Co.
[0022] The metal solution is, for example, an aqueous solution of an inorganic acid salt containing the second metal element. The inorganic acid salt is not particularly limited, but may be, for example, a sulfate, a nitrate, or a nitrate.
[0023] The metal solution may contain an organic solvent with excellent hydration properties in order to improve the wettability with respect to the high dielectric film 13. IPA, acetone, or the like is used as the organic solvent. By improving the wettability of the metal solution, it is possible to improve the rate at which the first metal element contained in the high dielectric film 13 is substituted with the second metal element contained in the metal solution.
[0024] The above step S103 includes, for example, discharging the metal solution from a nozzle disposed above the substrate 10 while the substrate 10 is held horizontally with the high dielectric film 13 facing upward, to form a liquid film of the metal solution. At this time, the substrate 10 may be rotated. Also, the nozzle may be scanned in the radial direction of the substrate 10. The nozzle may be a two-fluid nozzle, and may supply a mist of the metal solution to the substrate 10. The metal solution is collected in a cup 26 (see FIG. 11).
[0025] The above step S103 may include immersing the substrate 10 in a metal solution stored inside a processing tank. When the substrate 10 is immersed in the metal solution, a plurality of substrates 10 can be processed at once.
[0026] Step S104 includes forming a doped layer 14 by substituting a first metal element with a second metal element on the surface of the high dielectric film 13. As shown in FIG. 3(D), the first metal element contained in the high dielectric film 13 is substituted with the second metal element contained in the metal solution. As a result, a doped layer 14 is formed at a predetermined depth from the surface of the high dielectric film 13. The doped layer 14 is a monolayer, and its thickness is, for example, 1 to 5 times the atomic radius of the second metal element. Doping to form a monolayer is generally called MLD (Monolayer Doping).
[0027] As described above, the second metal element has a higher electronegativity or a lower valence than the first metal element. Therefore, a dipole can be formed on the surface of the high dielectric film 13 as shown in Fig. 4. As a result, the Schottky barrier can be modulated as shown by the arrow A1 in Fig. 5, and the flow of electrons can be stopped as shown by the arrow A2 in Fig. 5. Therefore, the leakage current can be reduced while suppressing an increase in the film thickness of the high dielectric film 13.
[0028] The surface density of the second metal element on the surface of the high dielectric film 13 is, for example, 1×10 10 atoms / cm 2 More than 1×10 15 atoms / cm 2 The surface density of the second metal element is measured by SIMS (secondary ion mass spectrometry), ICP-MS (inductively coupled plasma mass spectrometry), or TXRF (total reflection X-ray fluorescence spectrometry).
[0029] If the surface density of the second metal element on the surface of the high-dielectric film 13 is within a desired range, post-cleaning such as rinsing is not necessary after step S104. Note that if the second metal element is excessive, post-cleaning is performed.
[0030] As described above, step S104 includes replacing the first metal element contained in the high dielectric film 13 with a second metal element having a higher electronegativity or a lower valence than the first metal element. As a result, new oxygen vacancies 13a may be generated as shown in FIG. 3(D) so that the charges are balanced.
[0031] Step S105 includes repairing oxygen vacancies 13a in the high-dielectric film 13 with an oxidizing agent after forming the doped layer 14. As in step S102, an oxidizing chemical is used as the oxidizing agent, and the chemical is supplied to the substrate 10. The oxidizing agent reduces oxygen vacancies 13a as shown in FIG. 3(E), thereby reducing paths of leakage current.
[0032] The oxidizing chemical solution may be supplied to the substrate 10 simultaneously with the metal solution. That is, the formation of the doped layer 14 (step S104) and the repair of the oxygen vacancies 13a (step S102 or S105) may be performed simultaneously.
[0033] In this embodiment, the oxygen vacancies 13a are repaired by a wet process, but may be repaired by a dry process. For example, step S105 may include, after forming the doped layer 14, performing a heat treatment on the substrate 10 in an atmosphere containing oxygen gas, thereby repairing the oxygen vacancies 13a in the high dielectric film 13. The heating temperature of the substrate 10 is, for example, 80°C to 500°C, and preferably 100°C to 350°C. As long as oxygen gas is contained, the majority of the atmosphere may be an inert gas such as nitrogen gas. The atmosphere may be an air atmosphere.
[0034] Step S105 may also include, after forming the doped layer 14, irradiating the substrate 10 with ultraviolet light in an atmosphere containing oxygen gas to repair the oxygen vacancies 13a in the high dielectric film 13. Ozone is generated by the irradiation of the ultraviolet light, and the ozone repairs the oxygen vacancies 13a. The wavelength of the ultraviolet light is not particularly limited, but is, for example, 172 nm or 365 nm.
[0035] Step S105 may include a plurality of processes for repairing the oxygen vacancies 13a, and the combination of the processes is not particularly limited.
[0036] Step S106 includes cleaning the substrate 10. For example, step S106 includes cleaning the back surface (e.g., the lower surface) or the bevel of the substrate 10 opposite the doping layer 14 with a cleaning liquid to remove the second metal element attached to the back surface or the bevel. Both the back surface and the bevel may be cleaned. The cleaning liquid includes an inorganic acid. The cleaning liquid is, for example, hydrofluoric acid, dilute hydrochloric acid, SC2 (aqueous solution containing hydrochloric acid and hydrogen peroxide), SPM, aqua regia, or the like. It is possible to prevent the second metal element from adhering to a transport device that transports the substrate 10, or the like.
[0037] The above step S106 includes, for example, discharging the cleaning liquid from a nozzle disposed below the substrate 10 while the substrate 10 is held horizontally with the high dielectric film 13 facing upward. At that time, the substrate 10 may be rotated. The nozzle may be a two-fluid nozzle, and may supply a mist of the cleaning liquid to the substrate 10. The cleaning liquid is collected in a cup 26 (see FIG. 11).
[0038] Step S107 includes drying the substrate 10. The method for drying the substrate 10 is, for example, spin drying, supercritical drying, or Marangoni drying. In these drying methods, an organic solvent such as IPA is used. Compared with pure water, the organic solvent can reduce the surface tension acting on the substrate surface, and can suppress pattern collapse on the substrate surface. The organic solvent is supplied to the substrate 10 in a liquid or gas state. Nitrogen gas or the like may be supplied to the substrate 10 together with the organic solvent. In supercritical drying, the substrate 10 is dried by replacing a liquid film of the organic solvent formed in advance on the upper surface of the substrate 10 with a supercritical fluid.
[0039] Before drying the substrate 10, the substrate 10 may be made water-repellent with a water-repellent agent to reduce the surface tension of the organic solvent acting on the substrate surface. The water-repellent agent is not particularly limited, but may be, for example, (trimethylsilyl)dimethylamine (N,N-Dimethyltrimethylsilylamine: TMSDMA) or hexamethyldisilazane (1,1,1,3,3,3-Hexamethyldisilazane: HMDS).
[0040] Step S108 includes unloading the substrate 10 from the substrate processing apparatus 20. Thereafter, a second electrode 15 is formed on the doped layer 14 of the substrate 10.
[0041] 2. For example, the substrate processing method may include cleaning the cup 26 or the processing vessel 21 to remove the second metal element adhering to the cup 26 or the processing vessel 21. The cup 26 is cleaned using an aqueous solution of an inorganic acid. The processing vessel 21 is cleaned using a gas.
[0042] Next, experimental data will be described with reference to Table 1 etc. Table 1 shows the processing conditions of Examples 1 to 8. In Examples 1 to 8, a TiN film, a ZrO2 film, and a TiN film were formed in this order on a silicon wafer under the same processing conditions except for the processing conditions shown in Table 1. The thickness of the ZrO2 film was 5 nm. Example 1 is a comparative example, and Examples 2 to 8 are working examples.
[0043] [Table 1]
[0044] In Table 1, in the "doping treatment", before forming a TiN film on the surface of the ZrO2 film, the substrate was immersed in an aqueous solution containing 10 ppm Co ions by mass for 30 minutes, and then dried with compressed air. In the "pretreatment", after forming the ZrO2 film and before the doping treatment, SPM was supplied to the surface of the ZrO2 film for 1 minute, and then DHF (dilute hydrofluoric acid) was supplied for 1 minute. The SPM used had a mass ratio of sulfuric acid and hydrogen peroxide of 6:1 (H2SO4:H2O2=6:1). The DHF used had a mass ratio of hydrofluoric acid and water of 1:100 (H2O2:H2O=1:100). In the "first post-treatment", after the doping treatment and before forming the TiN film, the substrate was heated at 100°C in an air atmosphere. In the "second post-treatment", after the doping process and before the formation of the TiN film, the substrate was immersed in hydrogen peroxide water for 10 seconds, and then dried with compressed air. The hydrogen peroxide water used contained 1.5 mass% H2O2.
[0045] In Examples 1 to 8, 60 test pieces were prepared under the treatment conditions shown in Table 1. A voltage was applied to each test piece as shown in FIG. 6, and the leakage current was measured. In Example 1, as shown in Table 1, no doping treatment was performed. Therefore, the test piece prepared in Example 1 did not have the doping layer 14 shown in FIG. 6.
[0046] FIG. 7 shows the measurement results for Example 1 and Example 8. In FIG. 7, the vertical axis shows cumulative probability (%), and the horizontal axis shows leakage current (A / cm 2 ) is shown. The leakage current is expressed in logarithm. In addition, in FIG. 7, the horizontal line B1 indicates that the cumulative probability is 50%. The median value of the leakage current of the test pieces prepared in Example 1 was set as the reference value of the leakage current.
[0047] As is clear from Fig. 7, in Example 8, unlike Example 1, doping treatment, pretreatment, first post-treatment, and second post-treatment were performed, and therefore the leakage current could be reduced compared to Example 1. For example, in Example 8, the median value of the leakage current could be reduced to about 1 / 20 of the reference value. Furthermore, in Example 8, the variation in leakage current could be reduced, and the leakage current of most of the test pieces could be reduced below the reference value.
[0048] The measurement results for Examples 1 to 8 are shown in a bar graph in Figure 8. In Figure 8, "less than 1 / 10 of the reference value" indicates the percentage of test pieces in which the leakage current was less than 1 / 10 of the reference value, and "short circuit" indicates the percentage of test pieces in which the leakage current was less than 10 A / cm 2 The percentage of test specimens exceeding the limit is shown.
[0049] As is clear from FIG. 8, in Example 2, unlike Example 1, a doping process was performed, so the percentage of test pieces whose leakage current was 1 / 10 of the reference value could be increased compared to Example 1. Also, in Examples 3 to 5, unlike Example 2, at least one of the first post-processing and the second post-processing was performed, so the percentage of short-circuited test pieces could be reduced compared to Example 2. Furthermore, in Example 6, unlike Example 2, a pre-processing was performed, so the percentage of test pieces whose leakage current was 1 / 10 of the reference value could be increased compared to Example 2, and the percentage of short-circuited test pieces could be reduced. Furthermore, in Examples 7 to 8, unlike Example 6, not only the pre-processing but also at least the second post-processing was performed, so the percentage of test pieces whose leakage current was 1 / 10 of the reference value could be increased compared to Example 6, and the percentage of short-circuited test pieces could be reduced.
[0050] Next, a substrate processing method according to a modified example will be described with reference to Fig. 9. The substrate processing method according to the modified example includes steps S101 to S102, S105 to S108, and S201 to S202 shown in Fig. 9. Differences will be mainly described below.
[0051] Step S201 includes supplying a polar organic solvent to the substrate. The polar organic solvent includes, for example, a carbonyl compound or an amine compound. The carbonyl compound is, but is not limited to, for example, acetone, formaldehyde, or cyclohexanone. The amine compound is, but is not limited to, for example, triethylamine or trimethylamine.
[0052] The above step S201 includes, for example, discharging an organic solvent from a nozzle disposed above the substrate 10 while the substrate 10 is held horizontally with the high dielectric film 13 facing upward, to form a liquid film of the organic solvent. At that time, the substrate 10 may be rotated. Also, the nozzle may be scanned in the radial direction of the substrate 10. The nozzle may be a two-fluid nozzle, and may supply a mist of the organic solvent to the substrate 10. The organic solvent is collected in a cup 26 (see FIG. 11).
[0053] The above step S201 may include immersing the substrate 10 in an organic solvent stored inside a processing tank. When the substrate 10 is immersed in the organic solvent, a plurality of substrates 10 can be processed at once. The organic solvent may be supplied to the substrate 10 in a gaseous state instead of a liquid state.
[0054] Step S202 includes adsorbing an organic solvent onto the surface of the high dielectric film 13 to form an adsorption layer containing the organic solvent. When a carbonyl compound is supplied as the organic solvent, the carbonyl group is adsorbed onto the surface of the high dielectric film 13 as shown in Fig. 10, and an adsorption layer 16 is formed. The adsorption layer 16 is a monolayer, and its thickness is, for example, 1 to 5 times the thickness of one molecule of the organic solvent.
[0055] By forming the adsorption layer 16, a dipole is formed on the surface of the high-dielectric film 13. As a result, similar to the case where the doping layer 14 is formed instead of the adsorption layer 16, the Schottky barrier can be modulated as shown by the arrow A1 in Fig. 5, and the flow of electrons as shown by the arrow A2 in Fig. 5 can be stopped. Therefore, the leakage current can be reduced while suppressing an increase in the film thickness of the high-dielectric film 13.
[0056] Next, the experimental data will be described with reference to Table 2 and the like. Table 2 shows the experimental results of Example 1 and Example 9. In Example 9, a TiN film, a ZrO2 film, and a TiN film were formed in this order on a silicon wafer under the same conditions as Example 2, except that an "adsorption treatment" was performed instead of a "doping treatment". In the adsorption treatment, the substrate was immersed in acetone for 30 seconds, and then dried with compressed air. Example 1 is a comparative example, and Example 9 is an embodiment.
[0057] [Table 2]
[0058] As is clear from Table 2, in Example 9, unlike Example 1, an adsorption treatment was performed, and therefore the leakage current was reduced compared to Example 1. Specifically, in Example 9, the median leakage current was reduced to about 2 / 5 of the reference value.
[0059] Next, the substrate processing apparatus 20 according to this embodiment will be described with reference to FIG. 11. The substrate processing apparatus 20 includes, for example, a processing vessel 21, a gas supply mechanism 22, a chuck 23, a chuck drive mechanism 24, a liquid supply mechanism 25, a cup 26, and a control unit 29. The processing vessel 21 accommodates the substrate 10. The gas supply mechanism 22 is a fan filter unit or the like, and supplies gas to the inside of the processing vessel 21. The chuck 23 is a substrate holding unit that holds the substrate 10 inside the processing vessel 21. The chuck drive mechanism 24 rotates the chuck 23. The liquid supply mechanism 25 supplies a processing liquid to the substrate 10 held by the chuck 23. The cup 26 collects the processing liquid that is shaken off from the rotating substrate 10. The control unit 29 controls the gas supply mechanism 22, the chuck drive mechanism 24, and the liquid supply mechanism 25.
[0060] The liquid supply mechanism 25 has a nozzle 251 that discharges a processing liquid. The nozzle 251 discharges the processing liquid from above onto the substrate 10 held by the chuck 23. The processing liquid is supplied to the radial center of the rotating substrate 10, and spreads over the entire radial direction of the substrate 10 by centrifugal force to form a liquid film. The number of nozzles 251 is one or more. A plurality of nozzles 251 may discharge a plurality of types of processing liquid, or a single nozzle 251 may discharge a plurality of types of processing liquid.
[0061] Examples of the multiple types of processing liquids include an oxidizing chemical liquid used in step S102 or S105, a metal solution used in steps S103 and S104, a cleaning liquid used in step S106, an organic solvent used in step S201, etc. The liquid supply mechanism 25 corresponds to a liquid supply unit or an organic solvent supply unit described in the claims.
[0062] The liquid supply mechanism 25 has a flow path for each processing liquid, which supplies the processing liquid toward the nozzle 251. The liquid supply mechanism 25 also has a flow meter, a flow controller, and an opening / closing valve in the flow path. The flow meter measures the flow rate of the processing liquid. The flow controller controls the flow rate of the processing liquid. The opening / closing valve opens and closes the flow path.
[0063] Furthermore, the liquid supply mechanism 25 has a nozzle drive unit 252 that moves the nozzle 251. The nozzle drive unit 252 moves the nozzle 251 in a horizontal direction perpendicular to the rotation center line of the chuck 23. The nozzle drive unit 252 may also move the nozzle 251 in a vertical direction. While the nozzle 251 is ejecting liquid onto the substrate surface, the nozzle drive unit 252 may move the nozzle 251 in a radial direction of the substrate surface.
[0064] Cup 26 accommodates substrate 10 held by chuck 23 and collects processing liquid shaken off from rotating substrate 10. A drain pipe 261 and an exhaust pipe 262 are provided at the bottom of cup 26. Drain pipe 261 discharges liquid that accumulates inside cup 26. Exhaust pipe 262 discharges gas inside cup 26. Cup 26 does not rotate together with chuck 23, but may rotate.
[0065] The control unit 29 is, for example, a computer, and includes a CPU (Central Processing Unit) 291 and a storage medium 292 such as a memory. The storage medium 292 stores programs for controlling various processes executed in the substrate processing apparatus 20. The control unit 29 causes the CPU 291 to execute the programs stored in the storage medium 292, thereby controlling the operation of the substrate processing apparatus 20 and implementing the substrate processing method shown in FIG. 2 or FIG.
[0066] Although the embodiments of the substrate processing method and substrate processing apparatus according to the present disclosure have been described above, the present disclosure is not limited to the above-mentioned embodiments. Various changes, modifications, substitutions, additions, deletions, and combinations are possible within the scope of the claims. These naturally fall within the technical scope of the present disclosure.
[0067] This application claims priority based on Patent Application No. 2021-018133 filed with the Japan Patent Office on February 8, 2021, and the entire contents of Patent Application No. 2021-018133 are incorporated by reference into this application. [Explanation of symbols]
[0068] 10 Substrate 13 High dielectric film 14 Doping layer
Claims
1. SiO 2 preparing a substrate on which a high dielectric film having a higher dielectric constant than the film is formed; supplying a metal solution containing a second metal element having a higher electronegativity or a lower valence than a first metal element contained in the high dielectric film to the substrate; forming a doping layer on a surface of the high dielectric film by substituting the first metal element with the second metal element; A method for processing a substrate, comprising:
2. The substrate processing method according to claim 1 , wherein the second metal element includes one or more selected from the group consisting of Co, Ni, Mo, W, V, Cr, and Nb.
3. 3. The substrate processing method according to claim 1, wherein the metal solution is an aqueous solution of an inorganic acid salt containing the second metal element.
4. The surface density of the second metal element on the surface of the high dielectric film is 1×10 10 atoms / cm 2 Above 1 x 10 15 atoms / cm 2 The substrate processing method according to any one of claims 1 to 3, wherein:
5. 5. The substrate processing method according to claim 1, further comprising repairing oxygen vacancies in the high dielectric film with an oxidizing agent before forming the doped layer.
6. 6. The substrate processing method according to claim 1, further comprising repairing oxygen vacancies in the high dielectric film with an oxidizing agent after forming the doped layer.
7. 7. The substrate processing method according to claim 5, wherein the oxidizing agent is an oxidizing chemical liquid.
8. 8. The substrate processing method according to claim 1, further comprising: after forming the doping layer, heating the substrate in an atmosphere containing oxygen gas to repair oxygen vacancies in the high dielectric film.
9. 9. The substrate processing method according to claim 1, further comprising: after forming the doping layer, irradiating the substrate with ultraviolet light in an atmosphere containing oxygen gas to repair oxygen vacancies in the high dielectric film.
10. The substrate processing method according to any one of claims 1 to 9, further comprising, after forming the doping layer, washing a back surface of the substrate opposite to the doping layer or a bevel of the substrate with a cleaning solution to remove the second metal element adhering to the back surface or the bevel.
11. 11. The substrate processing method according to claim 1, wherein the high dielectric film includes a zirconium oxide film or a hafnium oxide film.
12. The high dielectric film is formed on a first electrode, The substrate processing method according to any one of claims 1 to 11, further comprising forming a second electrode on the high dielectric film.
13. SiO 2 a substrate holder for holding a substrate on which a high dielectric film having a higher dielectric constant than the film is formed; a liquid supply unit that supplies a metal solution containing a second metal element having a higher electronegativity or a lower valence than a first metal element contained in the high dielectric film to the substrate, and forms a doping layer on a surface of the high dielectric film by substituting the first metal element with the second metal element; The substrate processing apparatus includes:
Citation Information
Patent Citations
Capacitor and its manufacturing method
JP2009059889A
Method of manufacturing semiconductor device and method of forming metal oxide film
JP2019016778A