Silicon nitride etching compositions and methods

A composition of phosphoric acid, silanes, and water with optional fluorine compounds addresses the challenge of selective silicon nitride etching in semiconductor devices, enhancing etch rates and selectivity, thereby improving the reliability and efficiency of microelectronic device manufacturing.

JP7583105B2Active Publication Date: 2024-11-13ENTEGRIS INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023078794
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-11-15
Filing Date
2023-05-11
Publication Date
2024-11-13
Estimated Expiration
2039-11-12

AI Technical Summary

Technical Problem

Conventional etching methods for silicon nitride in semiconductor devices face challenges in achieving high selectivity and etch rates while minimizing damage to underlying layers such as silicon oxide and metal silicides, leading to reliability issues and process control difficulties, especially in advanced microelectronic devices like 3D NAND structures.

Method used

A composition comprising phosphoric acid, alkylaminoalkoxysilanes or alkylaminohydroxylsilanes, water, and optionally a fluorine compound, which provides high selectivity and etch rates for silicon nitride relative to silicon oxide and metal silicides, minimizing redeposition and corrosion.

Benefits of technology

The composition achieves high selectivity (up to 2000:1) and etch rates for silicon nitride, reducing process variability and improving manufacturing yield in microelectronic devices by selectively removing silicon nitride without substantial damage to underlying layers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583105000014
    Figure 0007583105000014
  • Figure 0007583105000015
    Figure 0007583105000015
  • Figure 0007583105000016
    Figure 0007583105000016
Patent Text Reader

Abstract

To provide compositions useful particularly in the etching of 3D NAND structures.SOLUTION: A composition comprises: phosphoric acid; at least one silane compound selected from alkylamino alkoxysilanes and alkylamino hydroxyl silanes; a solvent comprising water; and optionally a fluorine compound.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to compositions and methods for selectively etching silicon nitride in the presence of silicon oxide, polysilicon and / or metal silicides, and more particularly to compositions and methods for effectively and efficiently etching layers of silicon nitride with high etch rates and high selectivity to exposed or underlying layers of silicon oxide, polysilicon and / or metal silicides, especially in multi-layer semiconductor wafer structures. [Background technology]

[0002] There is a continuing need for improvements in the performance of microelectronic devices and a continuing emphasis on reducing device dimensions, which offers the dual benefits of dramatically increasing device density while improving device performance. Reducing device dimensions improves device performance by shortening the paths that charge carriers, e.g., electrons, must travel.

[0003] For example, the gate electrode of a metal oxide semiconductor field effect transistor (MOSFET) has a gate surface and a source region and a drain region as electrical contacts. The distance between the source region and the drain region forms the channel length of the gate electrode, and therefore, by reducing the dimensions of the device, the channel length is concomitantly reduced. As a result, the switching speed of the device is increased.

[0004] It is self-evident that reducing device dimensions increases the packing density of devices on a microelectronic device chip, which in turn results in a drastic reduction in the length of the interconnect paths between devices, reducing the relative adverse effect of these interconnect paths on the overall device performance (such as resistive voltage drop, crosstalk or RC delay).

[0005] However, such requirements cause problems of increased parasitic capacitance, device contact resistance (gate, source and drain contacts of MOSFET devices), and tight tolerance of pattern definition. For very small sub-micron or sub-half micron or even sub-quarter micron modern silicon devices, conventional photolithography techniques for patterning contacts do not meet the required tolerance of critical dimensions. Methods that have been investigated to improve the resolution and feature size include the formation of self-aligned polysilicon (poly-Si) gate structures that help to solve the problem of critical dimension tolerance. Using this method, the contacts formed for the source and drain of the gate electrode are self-aligned with the poly-Si gate.

[0006] One problem encountered during the formation of self-aligned gate structures is the selective removal of silicon nitride materials relative to polysilicon, silicon oxide and / or metal silicide materials. For example, during anisotropic etching of a silicon nitride layer covering a gate electrode, the underlying silicon oxide layer and silicon substrate are often also damaged, reducing the reliability of the semiconductor device.

[0007] Conventional wet etching techniques for selectively removing silicon nitride (Si3N4) have utilized high temperature (approximately 145-180°C) aqueous phosphoric acid (H3PO4) solutions, typically 85% phosphoric acid and 15% water (by volume). Using virgin hot phosphoric acid, the typical Si3N4:SiO2 selectivity is approximately 40:1. Advantageously, as the nitride layer is removed, hydrated silicon oxide is formed, which is consistent with Le Chatelier's principle and inhibits further removal of silicon oxide from the device surface. Thus, the selectivity gradually increases with use. Drawbacks associated with the use of high temperature phosphoric acid etches include corrosion of metal silicide materials, e.g., gate contact materials, etching of silicon oxide, and process control due to the difficulties associated with maintaining a specific amount of water in the process solution. Additionally, hot phosphoric acid is a difficult medium to fit into single wafer tools that are increasingly favored by many manufacturers.

[0008] Another method for selectively removing silicon nitride involves the use of compositions containing hydrofluoric acid, which also remove silicon oxide. A Si3N4:SiO2 selectivity of about 10:1 can be achieved by dilution. However, the etch rate of silicon nitride is compromised or pressures above ambient pressure must be used. Yet another process for removing silicon nitride involves dry etch removal using halogenated gas species. However, the Si3N4:SiO2 selectivity is even worse than that obtained using the wet etch process described above.

[0009] 3D-NAND structures under development today at all major memory chip manufacturers require highly selective etching of silicon nitride (SiN) from high aspect ratio "slits" defined by oxide (PETEOS). In the usual hot phosphoric acid "hot phosphorus" process, the selectivity is controlled by pre-dissolving a certain amount of nitride. The dissolved silicon nitride is converted to a less soluble oxide. The same happens during etching, but the oxide soon starts to deposit near the opening of the slit, eventually blocking the opening. See also US Patent Application Publication No. 2017 / 0287725, especially FIG. 1D, for an explanation of how colloidal silica deposition tends to "pinch off" gaps or trenches in microelectronic devices. As a result, the process window for oxide concentration before etching is very narrow and difficult to control, and etching baths must be replaced very frequently. Therefore, the oxide redeposition rate needs to be minimized.

[0010] Furthermore, deep slits require long etching times (typically more than an hour). The addition of small amounts of HF increases the etch rate, but also increases the polymerization of soluble silica species and thus the rate of oxide redeposition. Furthermore, the volatility of HF and related fluorinated species makes process control difficult.

[0011] In planar NAND technology, scaling is primarily driven by lithography. Scaling 3D NAND requires extreme precision and process repeatability to create complex 3D structures with very high aspect ratio (HAR) features. Therefore, achieving success with 3D NAND requires innovative patterning solutions that minimize variability. (For more on overcoming challenges in 3D NAND volume manufacturing, see Solid State Technology's website: http: / / electroig.com / blog / 2017 / 07 / overcoming-challenges-in-3d-nand-volume-manufacturing / .)

[0012] The precision of etching the extreme HAR features is critical to optimize the channel holes and trenches for cell access, as well as its unique staircase architecture that connects the cells to the surrounding CMOS circuitry for reading, writing, and erasing data. With a vertical pitch of about 50 nm in the memory stack, the 96-layer stack is about 4.8 μm high. This corresponds to a challenging aspect ratio of about 100:1.

[0013] Additionally, as the height of the multi-layer stack increases, it becomes more difficult to achieve consistent etch and deposition profiles at the top and bottom of the memory array. For example, given a ratio of about 100:1, selective removal of Si3N4 in the memory stack becomes a wet etch challenge. The challenge is to remove the Si3N4 consistently at the top and bottom of the stack and across the wafer without etching any of the SiO2. Below 96 layers, this task is accomplished using hot phosphoric acid (about 160°C). However, above 96 layers, specially formulated wet etch chemistries are required to improve process margins. Summary of the Invention

[0014] In one aspect, the present invention provides a composition useful for etching a substrate having a surface comprising silicon nitride and silicon oxide, the composition having selectivity for etching silicon nitride relative to silicon oxide. The composition comprises phosphoric acid, at least one silane compound selected from alkylaminoalkoxysilanes and alkylaminohydroxylsilanes, a solvent comprising water, and optionally a fluorine compound.

[0015] Figures 1-4 show a comparison of several embodiments of the present invention in terms of etch rate versus Si loading. The etch rates of silicon nitride and silicon oxide were measured using CVD silicon nitride and PECVD silicon oxide films. The silicon oxide films were exposed to the etching formulation for 4 hours so that the small amount of film loss could be measured. The silicon nitride films were etched for 5 and 10 minutes. The film thicknesses before and after treatment were measured by spectroscopic ellipsometry and the etch rates were calculated using these film thicknesses.

[0016] Specifically, the figure shows: [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 shows a graph of etch rate as a function of Si loading. [Diagram 2] FIG. 1 shows a graph displaying etch rate as a function of Si loading. [Diagram 3] FIG. 1 shows a graph displaying the etch rate in 85% phosphoric acid as a function of Si loading. [Figure 4] FIG. 1 shows a graph showing selectivity in ("Example B"), ("Example A") and 85% H3PO4. [Diagram 5] 3A-3C are schematic diagrams illustrating exemplary substrate structures as described before and after a selective etching process as also described. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] One aspect of the present invention relates to a composition useful for selective removal of silicon nitride relative to deposited polysilicon (poly-Si) and silicon oxide materials from a silicon oxide precursor source, and thus useful as a wet etchant for at least partially removing silicon nitride materials from microelectronic devices. Metal silicide materials that may be present should not be substantially attacked by said removal composition.

[0019] The present invention also provides methods, processes, and systems for using the wet etching compositions to remove silicon nitride from substrates containing silicon nitride and silicon oxide, the compositions being capable of providing advantageously high etch rates of silicon nitride, advantageously high selectivity of silicon nitride over silicon oxide, or an advantageous balance of these performance characteristics.

[0020] For ease of reference, a "microelectronic device" corresponds to a semiconductor substrate, including 3D NAND structures, flat panel displays, and microelectromechanical systems (MEMS), that is manufactured for use in microelectronics, integrated circuits, or computer chip applications. It should be understood that the term "microelectronic device" is not meant to be limiting in any way and includes any substrate that contains negative channel metal oxide semiconductor (nMOS) and / or positive channel metal oxide semiconductor (pMOS) transistors and that will ultimately become a microelectronic device or microelectronic assembly.

[0021] As used herein, "suitability" for removing silicon nitride material from a microelectronic device having such nitride material corresponds to at least partial removal of the silicon nitride material from the microelectronic device.

[0022] As used herein, "silicon nitride" and "Si3N4" correspond to pure silicon nitride (Si3N4) as well as impure silicon nitride that contains hydrogen, carbon and / or oxygen impurities in its crystal structure.

[0023] As used herein, "silicon oxide" refers to silicon oxide (SiO x ), e.g. SiO2, "thermal oxide" (ThO x Silicon oxide refers to a thin film made from a silicon dioxide, such as a silicon carbide (SiO 2 ), a silicon carbide (SiO 2 ), or a silicon carbide (SiO 2 ). The silicon oxide can be placed on the substrate by any method, such as by deposition by chemical vapor deposition from TEOS or another source, or by thermal deposition. Silicon oxide generally contains commercially useful low levels of other materials or impurities. Silicon oxide may be present as a feature of a microelectronic device, such as an insulating layer, or as part of a microelectronic device substrate.

[0024] As used herein, "at least partial removal of silicon nitride material" corresponds to removal of at least a portion of the exposed silicon nitride layer. For example, partial removal of silicon nitride material includes anisotropic removal of the silicon nitride layer that covers / protects the gate electrode to form the Si3N4 sidewall. It is also contemplated herein that the compositions of the present invention may be used more generally to substantially remove silicon nitride material relative to polysilicon and / or silicon oxide layers. In those contexts, "substantial removal" is defined as in one embodiment at least 90%, in another embodiment at least 95%, and in yet another embodiment at least 99% of the silicon nitride material is removed using the compositions of the present invention.

[0025] As used herein, "about" is intended to correspond to + / - 5% of the stated value.

[0026] As used herein, "metal silicide" refers to any silicide containing the species Ni, Pt, Co, Ta, Mo, W, and Ti, including, but not limited to, TiSi2, NiSi, CoSi2, NiPtSi, tantalum silicide, molybdenum silicide, and tungsten silicide.

[0027] "Silicon" has the general formula [SiO x (OH) 4-2x ] n It is the general name for a group of chemical compounds of silicon, hydrogen, and oxygen, including metasilicic acid (H2SiO3)n ), orthosilicic acid (H4SiO4), disilicic acid (H2Si2O5), and pyrosilic acid (H6Si2O7). Silica can be obtained in many ways well known to those skilled in the art, for example by hydrating fine silica powder (preferably 1 μm in diameter or less), alkoxysilanes (e.g., tetramethoxysilane (TMOS), tetraethoxysilane (TEOS), tetra-n-propoxysilane, tetra-n-butoxysilane), alkoxysilanes having amino groups (e.g., aminotriethoxysilane, hexaethoxydisilazane), alkoxysilanes having one or more halogen or pseudohalogen groups (e.g., triethoxychlorosilane, triethoxyfluorosilane, triethoxy(isocyanato)silane, diethoxydichlorosilane), or combinations thereof. For ease of reference, hereinafter "alkoxysilane" will be used to include alkoxysilanes, alkoxysilanes bearing amino groups, and alkoxysilanes bearing one or more halogen or pseudohalogen groups.

[0028] As described herein, the silicon oxide layer may be deposited from a silicon oxide precursor source, such as TEOS, or may be thermally deposited silicon oxide. Other exemplary low-κ materials, i.e., "low-k dielectric materials," correspond to any material used as a dielectric material in layered microelectronic devices, the material having a dielectric constant less than about 3.5. In certain embodiments, the low-κ dielectric material is a low polar material, such as silicon-containing organic polymers, silicon-containing hybrid organic / inorganic materials, organosilicate glass (OSG), TEOS, fluorosilicate glass (FSG), silicon dioxide, silicon oxycarbide, silicon oxynitride, silicon nitride, carbon-doped oxide (CDO) or carbon-doped glass, such as CORAL™ from Novellus Systems, BLACK from Applied Materials, and the like. Low-κ dielectric materials include DIAMOND™ (e.g., designations BD1, BD2, and BD3 for PECVD), SiLK™ dielectric resins from Dow (polymers based on crosslinked polyphenylenes by reaction of multifunctional cyclopentadienones with acetylene-containing materials, see, e.g., U.S. Pat. No. 5,965,679, incorporated herein by reference), and NANOGLASS™ from Nanopore Corporation (silica aerogels / xerogels, also known as nanoporous silica). It should be understood that low-κ dielectric materials can have a variety of densities and a variety of porosities.

[0029] The compositions of the present invention should have good metal compatibility, e.g., low etch rates on interconnect metals and / or interconnect metal silicide materials. Metals of interest include, but are not limited to, copper, tungsten, cobalt, molybdenum, aluminum, tantalum, titanium, and ruthenium. Silicides of interest include any silicide containing the species Ni, Pt, Co, Ta, Mo, W, and Ti, including, but not limited to, TiSi2, NiSi, CoSi2, NiPtSi, tantalum silicide, molybdenum silicide, and tungsten silicide.

[0030] The compositions of the present invention may be embodied in a wide variety of specific formulations, as described in more detail below.

[0031] In all such compositions, certain components of the compositions are discussed with reference to weight percent ranges inclusive of a zero lower limit, it being understood that such components may or may not be present in various particular embodiments of the compositions, and that when present, such components may be present in concentrations as low as 0.001 weight percent, based on the total weight of the composition in which such component is employed.

[0032] The composition includes an amount of aqueous phosphoric acid (e.g., concentrated phosphoric acid) effective to produce a desired etch of silicon nitride. The term "aqueous phosphoric acid" refers to the component of the composition that is mixed or combined with other components of the composition to form the composition. The term "phosphoric acid solids" refers to the non-aqueous components of the aqueous phosphoric acid component or the non-aqueous components of the composition prepared from the aqueous phosphoric acid component.

[0033] The amount of phosphoric acid solids contained in the composition can be an amount that, in combination with other materials of the etching composition, provides the desired etching performance, including the desired silicon nitride etch rate and selectivity, and typically requires a relatively large amount (high concentration) of phosphoric acid solids. For example, the etching composition can contain an amount of phosphoric acid solids of at least about 50 weight percent based on the total weight of the composition, such as at least 70, or at least about 80 or 85 weight percent based on the total weight of the composition.

[0034] To provide the desired amount of phosphoric acid solids, the composition may contain "concentrated" phosphoric acid as a component that is mixed or combined with other components (one component that is optionally water in some forms) to produce the composition. "Concentrated" phosphoric acid refers to an aqueous phosphoric acid component that contains a large or maximum amount of phosphoric acid solids in the presence of a small or minimal amount of water and is substantially free of other components (e.g., less than 0.5 or 0.1 weight percent of any non-aqueous or non-phosphate solid materials). Concentrated phosphoric acid can typically be considered to have at least about 80 or 85 weight percent phosphoric acid solids in about 15 or 20 weight percent water. Alternatively, the composition may be considered to include an amount of concentrated phosphoric acid diluted with water, i.e., diluted with an amount of water before or after combining with other components of the etching composition, or an equivalent formed in any manner. As another alternative, the components of the composition can be concentrated or diluted phosphoric acid, and the etching composition can contain an additional amount of water provided to the composition, either as a component of a different component or as a separate water component.

[0035] As an example, when concentrated phosphoric acid is used to form the composition, the amount of concentrated phosphoric acid (85% by weight in water) can be an amount of at least 60, e.g., at least 80, or at least 90, 93, 95, or at least 98 percent by weight of the composition, based on the total weight of the composition.

[0036] The composition can comprise, consist of, or consist essentially of any combination of the listed components and optional components. As a general convention throughout this specification, a described composition, or a specific component or component thereof, that is said to "consist essentially of" a group of specific components or materials refers to a composition that contains the specified component or material and has small or insignificant amounts or less, for example, 5, 2, 1, 0.5, 0.1, or 0.05 parts by weight or less, of other components or materials. For example, a composition containing a material that consists essentially of aqueous phosphoric acid, at least one silane compound selected from (i) alkylaminoalkoxysilane and (ii) alkylaminohydroxylsilane, a solvent including water, and the listed optional components means a composition that contains these components and 5, 2, 1, 0.5, 0.1, or 0.05 parts by weight or less of any other dissolved or undissolved materials (individually or collectively) other than the specified materials.

[0037] As used herein, a "fluorine compound" refers to a compound that contains the ionic fluoride ion (F -) or species containing covalently bound fluorine. It should be understood that the fluoride species may be included as a fluoride species or may be generated in situ. In certain embodiments, the compound capable of generating fluoride ions is derived from HF, monofluorophosphoric acid (MFPA), difluorophosphoric acid (DFPA) or hexafluorophosphoric acid. In concentrated phosphoric acid compositions, HF is present primarily in the form of monofluorophosphoric acid (MFPA). In certain embodiments, to simplify addition and blending, low volatility MFPA or DFPA may be used directly in the composition. In other embodiments, the fluorine compound may be selected from CsF and KF. In other embodiments, the fluorine compounds include tetramethylammonium hexafluorophosphate, ammonium hexafluorophosphate, ammonium fluoride, ammonium difluoride, quaternary ammonium tetrafluoroborates and quaternary phosphonium tetrafluoroborates having the formulas NR'4BF4 and PR'4BF4, respectively, where each R' can be the same or different from each other and can be selected from hydrogen, linear, branched or cyclic C1-C6 alkyl (e.g., methyl, ethyl, propyl, butyl, pentyl, hexyl), and linear or branched C6 ... 10 aryl (e.g., selected from benzyl), tetrabutylammonium tetrafluoroborate (TBA-BF4), and combinations thereof. In certain embodiments, the fluorine compound is selected from ammonium fluoride, ammonium difluoride, quaternary ammonium tetrafluoroborate (e.g., tetramethylammonium tetrafluoroborate, tetraethylammonium tetrafluoroborate, tetrapropylammonium tetrafluoroborate, tetrabutylammonium tetrafluoroborate), quaternary phosphonium tetrafluoroborate, or combinations thereof. In certain embodiments, the fluorine compound comprises ammonium difluoride, ammonium fluoride, or combinations thereof.

[0038] As used in this specification and the appended claims, the singular forms "a," "an," and "the" include their plural referents unless the context clearly dictates otherwise. The terms "containing" or "including" are intended to be synonymous with the term "comprising" and mean that at least the specified compounds, elements, particles, method steps, etc. are present in a composition or article or method, but do not exclude the presence of other compounds, materials, particles, method steps, etc., even if they have the same function as the specified ones, unless expressly excluded in the claims.

[0039] In one aspect, the present invention provides a method for producing a method for treating a cancer cell comprising: (a) phosphoric acid; (b) at least one silane selected from (i) alkylaminoalkoxysilanes and (ii) alkylaminohydroxylsilanes, the at least one silane having at least one moiety selected from alkoxy, hydroxyl, and fluoro; (c) a solvent comprising water, and optionally (d) a fluorine compound other than hexafluorosilicic acid; A composition comprising:

[0040] In certain embodiments, the phosphoric acid is present in the composition at about 50 to about 95 weight percent, in other embodiments, the phosphoric acid is present at about 70 to about 90 weight percent, and in other embodiments, at about 85 weight percent.

[0041] In certain embodiments of the present invention, the composition may further comprise a fluorine compound. In one embodiment, the fluorine compound is selected from HF and monofluorophosphoric acid. In another embodiment, the fluorine compound is selected from cesium fluoride and potassium fluoride. In another embodiment, the fluorine compound is selected from ammonium hexafluorophosphate, tetramethylammonium hexafluorophosphate, ammonium fluoride, ammonium difluoride, fluoroboric acid, quaternary ammonium tetrafluoroborate and quaternary phosphonium tetrafluoroborate having the formulas NR'4BF4 and PR'4BF4, respectively, where R' may be the same or different from each other and is selected from hydrogen, linear, branched or cyclic C1-C6 alkyl, and linear or branched C6-C7 alkyl. 10 aryl), tetramethylammonium tetrafluoroborate (TMA-BF4), and combinations thereof.

[0042] In certain embodiments, the alkylaminoalkoxysilane and alkylaminohydroxylsilane compounds have the formula TIFF0007583105000001.tif26170 (wherein each X is independently selected from fluorine, a C1-C8 alkyl group, or a group of formula -OR, where R is hydrogen or a C1-C8 alkyl group, n is an integer from 1 to 6, and each R 1 is hydrogen, a C1-C8 alkyl group, or a C1-C8 alkoxy group of the formula (CH2) n-- are independently selected from It is expressed by:

[0043] In certain embodiments, the alkylaminoalkoxysilane and alkylaminohydroxylsilane compounds are selected from (3-aminopropyl)triethoxysilane (CAS No. 919-30-2), (3-aminopropyl)silanetriol (CAS No. 58160-99-9), 3-aminopropyldimethylethoxysilane (CAS No. 18306-79-1), 3-aminopropylmethyldiethoxysilane (CAS No. 3179-76-8), N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane (CAS No. 3069-29-2), (N,N-dimethyl-3-aminopropyl)trimethoxysilane (CAS No. 2530-86-1), and 3-aminopropyldimethylfluorosilane (CAS No. 153487-58-2).

[0044] In certain embodiments, the alkylaminoalkoxysilane and alkylaminohydroxylsilane compounds have the formula TIFF0007583105000002.tif26170 (wherein each X is independently selected from fluorine, a C1-C8 alkyl group, or a group of formula -OR, where R is hydrogen or a C1-C8 alkyl group, n is an integer from 1 to 6, y is an integer from 1 to 6, and z is an integer from 1 to 6) It is expressed by:

[0045] In certain embodiments, the alkylaminoalkoxysilane and alkylaminohydroxylsilane compounds are selected from N-(3-trimethoxysilylpropyl)diethylenetriamine (CAS No. 35141-30-1), N-(2-aminoethyl)-3-aminopropyltriethoxysilane (CAS No. 5089-72-5), N-(2-aminoethyl)-3-aminopropylsilanetriol (CAS No. 1760-24-3), (3-trimethoxysilylpropyl) ethylenetriamine (CAS No. 35141-30-1), and N-(6-aminohexyl)aminopropyltrimethoxysilane (CAS No. 51895-58-0).

[0046] In certain embodiments, two alkylamino groups are linked to a silicon atom bearing two X groups (as defined above) or one X group and one alkyl group, such as, for example, 3,3'-(dimethoxysilylene)bis-(1-propanamine) (CAS number 51749-36-1). The file is TIFF0007583105000003.tif38170.

[0047] In certain embodiments, one or more aminoalkyl groups are branched from an alkyl or aminoalkyl chain linked to a silicon atom having three X groups (as defined above) or two X groups and one alkyl group, such as, for example, 2-[(dimethoxymethylsilyl)methyl]-1,4-butanediamine (CAS number 1019109-96-6). The file is TIFF0007583105000004.tif27170.

[0048] In certain embodiments, two or more silicon atoms linked by oxygen bridges have at least one aminoalkyl group and at least one of all of the above "X" groups, with the remaining silicon substituents being alkylamines, "X" or alkyls, such as 1,3-bis(3-aminopropyl)-1,1,3,3-tetraethoxydisiloxane (CAS number 17907-78-7). TIFF0007583105000005.tif37170, and its methoxy analogue, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethoxydisiloxane (CAS number 76712-65-7). The file is TIFF0007583105000006.tif38170.

[0049] The amount of alkylaminoalkoxysilane and alkylaminohydroxylsilane compounds in the composition of the present invention can be an amount that, in combination with other materials of the etching composition, provides the desired etching performance, including the desired silicon nitride etch rate and selectivity. For example, the etching composition can contain an amount ranging from about 20 to 10,000 ppm (i.e., 0.0020 to 1.0 weight percent) based on the total weight of the composition, or about 20 to 2,000, 4,000, or 5,000 ppm (i.e., 0.002 to 0.2, 0.4, or 0.5 weight percent) based on the total weight of the composition, of alkylaminoalkoxysilane and alkylaminohydroxylsilane compounds, which may be a single species or a combination of two or more species.

[0050] Component (c) is a solvent that includes water. In some cases, the solvent may further include one or more water-miscible solvents, such as pyrrolidinones, glycols, amines, and glycol ethers. Examples of water-miscible solvents include methanol, ethanol, isopropanol, butanol, and higher alcohols (C2-C4 diols and C3-C4 triols), tetrahydrofurfuryl alcohol (THFA), halogenated alcohols (3-chloro-1,2-propanediol, 1-chloro-2-propanol, 2-chloro-1-propanol, 3-chloro-1-propanol, 3-bromo-1,2-propanediol, 1-bromo-2-propanol, 3-bromo-1-propanol, 3-iodo-1-propanol, 4-chloro-1-butanol, 2-chloro-1-propan ...1-propanol, 1-bromo-1-propanol, 1-bromo-1-propanol, 1-bromo-1-propanol, 1-bromo-1-propanol, 1-bromo-1-propanol, 1-bromo-1-propanol, 1-bromo-1-propanol, 1- ethanol, etc.), acetic acid, propionic acid, trifluoroacetic acid, N-methylpyrrolidinone (NMP), cyclohexylpyrrolidinone, N-octylpyrrolidinone, N-phenylpyrrolidinone, methyldiethanolamine, dimethylformamide (DMF), dimethylsulfoxide (DMSO), tetramethylene sulfone (sulfolane), phenoxy-2-propanol (PPh), propiophenone, ethyl lactate, ethyl acetate, ethyl benzoate, acetonitrile, ethylene glycol, propylene glycol (PG), 1,3-propanediol, butyryllactone, butylene carbonate, ethylene carbonate, propylene carbonate, dipropylene glycol, diethylene glycol monomethyl ether, triethylene glycol monomethyl ether, diethylene glycol monoethyl ether, triethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether (i.e., butyl carbitol), triethylene glycol monobutyl ether, ethylene glycol monohexyl ether, diethylene glycol monohexyl ether, ethylene glycol phenyl ether, propylene glycol methyl ether, dipropylene glycol methyl ether (DPGME ), tripropylene glycol methyl ether (TPGME), dipropylene glycol dimethyl ether, dipropylene glycol ethyl ether, propylene glycol n-propyl ether, dipropylene glycol n-propyl ether (DPGPE), tripropylene glycol n-propyl ether, propylene glycol n-butyl ether, dipropylene glycol n-butyl ether, tripropylene glycol n-butyl ether, propylene glycol phenyl ether, dipropylene glycol methyl ether acetate, tetraethylene glycol dimethyl ether (TEGDE), dibasic esters, glycerin carbonate, N-formylmorpholine, triethyl phosphate, and combinations thereof. When an alkoxysilane additive is used, its hydrolysis produces small amounts of alcohol, such as methanol or ethanol, which is incorporated into the formulation as the alcohol itself or as its phosphoric acid monoester and which mostly evaporates at typical process temperatures. Additionally, the organic solvent may contain other amphiphilic species, i.e., species that contain both hydrophilic and hydrophobic moieties similar to surfactants. ,

[0051] In certain embodiments, the compositions of the present invention further comprise low molecular weight amines and amine phosphates. In other embodiments, the low molecular weight amines and amine phosphates are primary, secondary or tertiary C 1~C6 alkylamines or their phosphates. Examples include dimethylamine, trimethylamine, triethylamine, tripropylamine, tributylamine, etc. It will be appreciated that when such amines or their aqueous solutions are added to a concentrated H3PO4 composition, an amine phosphate will be formed.

[0052] In one embodiment, the composition comprises (a) phosphoric acid, (b) N-(2-aminoethyl)-3-aminopropyl silanetriol, and (c) a solvent comprising water. In a further embodiment, the composition further comprises HF or monofluorophosphoric acid. In a further embodiment, the composition further comprises triethylamine or a dihydrogen phosphate salt thereof.

[0053] The composition may optionally include a surfactant (different from other optional or required components herein) to improve the performance of the composition. As used herein, the term "surfactant" refers to an organic compound, typically an organic amphiphilic compound that contains a hydrophobic group (e.g., a hydrocarbon (e.g., alkyl) "tail") and a hydrophilic group, that reduces the surface tension (or interfacial tension) between two liquids or between a liquid and a solid. Preferred surfactants are thermally stable and remain ionic under strongly acidic conditions, such as those of the etching process of the present invention. Examples include perfluoroalkylsulfonic acids and long-chain quaternary ammonium compounds (e.g., dodecyltrimethylammonium hydrogen sulfate). Fluorinated nonionic surfactants, such as Chemours' Capstone® FS-31 / FS-35, can also be used. Nonionic nonfluorinated surfactants, such as poly(ethylene glycol)-poly(propylene glycol) copolymers ("PEG-PPG"), can also be used and are more suitable for low acid compositions (e.g., 75% H3PO4 or less) and operation at 130°C or less.

[0054] The amount of surfactant in the composition can be an amount that, in combination with the other materials of the etching composition, provides the desired overall performance. For example, the composition can contain an amount of surfactant that can range from about 0.001 to about 10 weight percent, such as from about 0.01 to about 0.5, 1, 2, 7, or 7 weight percent, based on the total weight of the composition.

[0055] In some cases, the composition can contain a certain amount of carboxylic acid compound, i.e., organic compound containing at least one carboxylic acid group.According to the present invention, the presence of carboxylic acid compound in the described composition can improve performance by inhibiting the redeposition of silicon oxide or the formation of particles thereof.In certain embodiments, the carboxylic acid compound for use in the composition includes acetic acid, malonic acid, succinic acid, 2-methylsuccinic acid, glutaric acid, adipic acid, salicylic acid, 1,2,3-propanetricarboxylic acid (also known as tricarballylic acid), 2-phosphonoacetic acid, 3-phosphonopropanoic acid, and 2-phosphonobutane-1,2,4-tricarboxylic acid (PBTCA), any of which can be used alone, in combination with each other, or in combination with different carboxylic acid compounds.

[0056] The amount of carboxylic acid compound (including derivatives thereof) contained in the composition can be an amount that, in combination with other materials of the composition, provides the desired etching performance without affecting the performance or chemical stability of the etching composition. For example, the composition can contain an amount of carboxylic acid compound ranging from about 0.01 to about 10 weight percent based on the total weight of the composition, or from about 0.1 to about 5 or 8 weight percent based on the total weight of the composition, and the carboxylic acid compound can be a single species or a combination of two or more species.

[0057] The composition may contain water from one or more sources. For example, water is present in the aqueous phosphoric acid component. Additionally, water may be used as a carrier for one or more other components of the etching composition, or water may be added alone as a component in its own right. The amount of water must be low enough to enable the composition to exhibit desired or preferred or advantageous etching performance characteristics, including a useful (sufficiently high) silicon nitride etch rate. Increasing the presence of water tends to increase the silicon nitride etch rate, but may also be counterproductive by lowering the boiling point of the etching composition, thereby reducing the operating temperature of the etching composition. Examples of the amount of water from all sources in the etching composition may be less than about 50, 40, or 30 weight percent, for example, in the range of about 5 weight percent to about 25 weight percent based on the total weight of the composition, or in the range of about 10 to 20 weight percent based on the total weight of the composition.

[0058] In some cases, these and other exemplary compositions described can contain, consist of, or consist essentially of phosphoric acid, aminohydroxylsilane or aminoalkoxysilane, and any one or any combination of the specified optional components. Certain embodiments of the compositions of the present invention do not require or can eliminate other types of components (other than the acids mentioned as possible components herein) that are not typically included in etching compositions, such as pH adjusters and solid materials such as abrasive particles.

[0059] The following table contains exemplary compositions, by weight percent, believed to be useful in the practice of this invention. TIFF0007583105000007.tif140170

[0060] As used herein, (3-aminopropyl)triethoxysilane (CAS number 919-30-2) is "APTES", (3-aminopropyl)silanetriol (CAS number 58160-99-9) is "APST", N-(2-aminoethyl)-3-aminopropylsilanetriol (CAS number 1760-24-3) is "N2APST", N 1 These compounds are often abbreviated as "N3APTMS" for N-(3-trimethoxysilylpropyl)diethylenetriamine, "N3APTMS" for 3,3'-(dimethoxysilylene)bis-(1-propanamine) (CAS number 51749-36-1) for DMSBP, "BAPTEDS" for 1,3-bis(3-aminopropyl)-1,1,3,3-tetraethoxydisiloxane (CAS number 17907-78-7), "AHAPTMS" for N-(6-aminohexyl)aminopropyltrimethoxysilane (CAS number 51895-58-0) for AHAPTMS, and "BC" for diethylene glycol monobutyl ether (butyl carbitol).

[0061] In yet another aspect, the present invention provides a method for removing silicon nitride from a microelectronic device, the method comprising contacting the microelectronic device with a composition of the present invention under conditions and for a time sufficient to at least partially remove the silicon nitride material from the microelectronic device.

[0062] For example, silicon nitride materials can be removed without substantially damaging metal and metal silicide interconnect materials. Thus, the present invention provides a method for selectively and substantially removing silicon nitride materials relative to polysilicon and / or silicon oxide materials from a surface of a microelectronic device having the same using the compositions described herein. Present metal silicide materials are not substantially attacked by the removal compositions using the method.

[0063] In an etching application, the composition is applied to the surface of the microelectronic device having a silicon nitride material thereon in any suitable manner, for example, by spraying the removal composition on the surface of the device, by dipping the device containing the silicon nitride material (into a static or dynamic volume of the removal composition), by contacting the device with another material, such as a pad or fibrous sorbent applicator element, on which the removal composition has been absorbed, by contacting the device containing the silicon nitride material with a circulating removal composition, or by any other suitable means, manner or technique that brings the removal composition into removal contact with the silicon nitride material. The application may be performed in a batch or single wafer apparatus for dynamic or static cleaning. In one embodiment, the application of the removal composition to the surface of the microelectronic device is with controlled agitation, whereby the composition is circulated in a vessel containing said composition.

[0064] The compositions of the present invention achieve highly efficient and selective removal of at least a portion of the silicon nitride material due to their selectivity for silicon nitride material over other materials, such as metallization, polysilicon, silicon oxide, that may be present on the microelectronic device structure and exposed to the composition.

[0065] In using the compositions of the present invention to remove silicon nitride material from a microelectronic device structure having the silicon nitride material, the composition is typically contacted with the microelectronic device structure for a sufficient time, for a single wafer tool, from about 1 minute to about 200 minutes, in one embodiment from about 15 minutes to about 100 minutes, or from about 1 minute to about 3 minutes, and in one embodiment, under sufficient conditions, including, but not limited to, at a temperature in the range of from about 120° C. to about 180° C. Such contact times and temperatures are exemplary, and any other suitable time and temperature conditions effective to at least partially remove the silicon nitride material from the device structure may be employed within the practice of the present invention.

[0066] Following achievement of the desired removal effect, the removal composition is easily removed from the previously coated microelectronic device, for example, by rinsing, washing, or other removal step, as may be desired and effective for a given end use application of the inventive composition. For example, the device may be rinsed with a rinse solution including deionized water and / or dried (e.g., spin dry, N2, steam dry, etc.).

[0067] The removal compositions of the present invention selectively etch silicon nitride materials relative to poly-Si and silicon oxide from the surface of a microelectronic device without causing substantial corrosion of the metal and / or metal silicide interconnect materials. For example, the selectivity of silicon nitride relative to silicon oxide in the presence of the removal compositions of the present invention ranges from about 10:1 to about 7,000:1 in one embodiment, from about 30:1 to about 3,000:1 in another embodiment, and from about 100:1 to about 2000:1 in another embodiment, at temperatures of 40-100° C. in one embodiment, 60-95° C. in another embodiment, and 75-90° C. in yet another embodiment. When the silicic acid source includes an alkoxysilane, such as TEOS, the selectivity of silicon nitride relative to silicon oxide can be adjusted from about 20:1 to infinity in one embodiment, and from about 20:1 to about 7,000:1 in another embodiment. In fact, in some usable formulations the selectivity is formally negative, reflecting the fact that the oxide film thickness is increased very slightly but measurably by silica precipitation.

[0068] The etching process herein may be useful for etching silicon nitride material from the surface of any type of substrate. According to certain embodiments, the substrate may include alternating thin layers of silicon nitride, including alternating thin layers of silicon nitride and silicon oxide, as structural features of the substrate. The silicon oxide layers are high aspect ratio structures containing silicon nitride layers disposed between layers of silicon oxide.

[0069] Yet another aspect of the invention relates to a method of manufacturing an article comprising a microelectronic device, said method comprising contacting the microelectronic device with a composition of the invention for a time sufficient to etch away silicon nitride material from a surface of the microelectronic device having silicon nitride material thereon, and incorporating said microelectronic device into said article.

[0070] The compositions described herein are easily formulated by simple addition of each component and mixing to a uniform state. Furthermore, the compositions can be easily formulated as single package formulations or multi-part formulations, preferably multi-part formulations, that are mixed at the point of use. The individual parts of the multi-part formulation can be mixed at the tool or in a storage tank upstream of the tool. The concentration of each component can vary widely, i.e., more dilute or more concentrated, at a particular multiple of the composition. It will be understood that the compositions described herein can variously and alternatively comprise, consist of, or consist essentially of any combination of components consistent with the disclosure herein.

[0071] Another aspect of the invention relates to a kit comprising one or more components adapted to form a composition as described herein in one or more containers. In one embodiment, the kit comprises at least one combination of components (a)-(c) above in one or more containers for combination with water at the manufacturing plant or at the point of use. The container of the kit should be suitable for storing and transporting said cleaning composition components, for example, a NOWPak.® container (Advanced Technology Materials, Inc., Danbury, Connecticut, USA). The one or more containers housing the first cleaning composition components preferably include a means for fluidly communicating the components in said one or more containers for blending and dispensing. For example, referring to the NOWPak.® container, gas pressure can be applied to the outside of the liner in said one or more containers to expel at least a portion of the contents of the liner, thus enabling fluid communication for blending and dispensing. Alternatively, gas pressure can be applied to the headspace of a conventional pressurized container, or a pump can be used to enable fluid communication. Additionally, the system preferably includes a dispense port for dispensing the admixed cleaning composition to a process tool.

[0072] Substantially chemically inert, impurity-free, flexible and resilient polymeric film materials, such as high density polyethylene, may be used to manufacture liners for the one or more containers. Desirable liner materials are processed without the need for coextrusion or barrier layers and without pigments, UV inhibitors, or processing agents that may adversely affect the purity requirements of the components disposed within the liner. A list of desirable liner materials includes films comprising virgin (unadded) polyethylene, virgin polytetrafluoroethylene (PTFE), polypropylene, polyurethane, polyvinylidene chloride, polyvinyl chloride, polyacetal, polystyrene, polyacrylonitrile, polybutylene, and the like. Exemplary thicknesses of such liner materials range from about 5 mils (0.005 inches) to about 30 mils (0.030 inches), such as a thickness of 20 mils (0.020 inches).

[0073] With respect to kit containers, the disclosures of the following patents and patent applications are each incorporated herein by reference in their entirety: No. 7,188,644, entitled "APPARATUS AND METHOD FOR MINIMIZING THE GENERATION OF PARTICLES IN ULTRAPURE LIQUIDS," U.S. patent application Ser. No. 6,698,619, entitled "RETURNABLE AND REUSABLE, BAG-IN-DRUM FLUID STORAGE AND DISPENSING CONTAINER SYSTEM," and U.S. patent application Ser. No. 60 / 916,966, entitled "SYSTEMS AND METHODS FOR MATERIAL BLENDING AND DISTRIBUTION," filed May 9, 2007 in the name of John E. Q. Hughes, and PCT Application No. PCT / US08 / 63276, entitled "SYSTEMS AND METHODS FOR MATERIAL BLENDING AND DISTRIBUTION," filed May 9, 2008 in the name of Advanced Technology Materials, Inc.

[0074] Thus, in a further aspect, the present invention provides a kit comprising one or more containers having components therein suitable for removing silicon nitride from a microelectronic device, the one or more containers of the kit containing (a) phosphoric acid, (b) at least one silane compound selected from (i) alkylaminoalkoxysilanes and (ii) alkylaminohydroxylsilanes as described herein, and (c) a solvent comprising water, and optionally (d) a fluorine compound other than hexafluorosilicic acid.

[0075] The present invention can be further illustrated by the following examples of specific embodiments thereof, however, it will be understood that these examples are included for illustrative purposes only and are not intended to limit the scope of the invention unless specifically stated. EXAMPLES

[0076] The high aspect ratio structures were treated to first remove the oxide from the exposed silicon nitride. The structures were then treated in the formulations with stirring in a boiling flask at the desired temperature. For conditions where a silicate loading was specified, either tetramethylammonium silicate (TMAS) or silica nanoparticles were added. In Examples 16 and 17, TMAS was used and the loading is provided as ppm Si. In all other examples, SiO2 nanoparticles were used and the silicate loading is provided as ppm SiO2. The structures were treated for a time sufficient to completely remove the SiN, typically 45 minutes to 2 hours. After treatment in the formulations, the structures were rinsed with hot deionized water and dried with flowing nitrogen. The etch rates shown were similarly obtained by treating blanket films and the thicknesses were measured by spectroscopic ellipsometry. TIFF0007583105000008.tif56170TIFF0007583105000009.tif51170TIFF0007583105000010.tif64170

[0077] It should be noted that compared to Examples 12-14, 85% H3PO4 either has low selectivity to oxides (about 40:1 at 0 ppm silica, Table 3) or causes excessive oxide redeposition (at 100 and 200 ppm silica, Table 2). TIFF0007583105000011.tif113170

[0078] The addition of dissolved silicate during processing reduces the silicon oxide etch rate without substantially changing the nitride etch rate.

[0079] At sufficiently high dissolved silicate concentrations, silica-rich precipitates redeposit on the SiO2 surface within the 3D NAND structure.

[0080] In this case the load window is defined on the low end by when the selectivity is above 1000 and on the high end by the onset of redeposition. Different selectivity targets result in load windows of different widths.

Claims

1. 1. A method for removing silicon nitride from a microelectronic device, comprising: The method includes contacting the microelectronic device with a composition under conditions and for a time sufficient to at least partially remove silicon nitride material from the microelectronic device; The composition, (a) phosphoric acid; (b) at least one silane selected from (i) alkylaminoalkoxysilanes and (ii) alkylaminohydroxylsilanes, the at least one silane having at least one moiety selected from alkoxy, hydroxyl, and fluoro; (c) a solvent comprising water; (d) a fluorine compound other than hexafluorosilicic acid; and (e) an alkylamine which is dimethylamine, trimethylamine, triethylamine, tripropylamine, or tributylamine, or a phosphate thereof, or a phosphate thereof; A composition comprising: method.

2. The method according to claim 1, wherein the alkylamine or its phosphate is triethylamine or its dihydrogen phosphate.

3. The method of claim 1, wherein the phosphoric acid is present in the range of 50 to 95 weight percent based on the total weight of the composition.

4. The alkylaminoalkoxysilane and alkylaminohydroxylsilane compounds are represented by the formula (wherein each X is fluorine, C 1 ~C 8 an alkyl group, or a group of formula -OR, where R is hydrogen or C 1 ~C 8 is an alkyl group, n is an integer from 1 to 6, and each R 1 is hydrogen, C 1 ~C 8 an alkyl group or a group of formula C 1 ~C 8 Alkoxy (CH 2 ) n - groups). The method of claim 1 , wherein the

5. 5. The method of claim 4, wherein the alkylaminoalkoxysilane and alkylaminohydroxylsilane compounds are selected from (3-aminopropyl)triethoxysilane, (3-aminopropyl)silane-triol, 3-aminopropyldimethylethoxysilane, 3-aminopropylmethyldiethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, (N,N-dimethyl-3-aminopropyl)trimethoxysilane, and 3-aminopropyldimethylfluorosilane.

6. The alkylaminoalkoxysilane and alkylaminohydroxylsilane compounds are represented by the formula (wherein each X is fluorine, C 1 ~C 8 an alkyl group, or a group of formula -OR, where R is hydrogen or C 1 ~C 8 an alkyl group, n is an integer from 1 to 6, y is an integer from 1 to 6, and z is an integer from 1 to 6. The method of claim 1 , wherein the

Citation Information

Patent Citations

  • Etching composition and etching method

    JP2009021538A

  • Compositions and methods for selective removal of silicon nitride

    JP2010515245A

  • Etchant for silicon nitride

    JP2012033561A

  • Etchant for silicon nitride

    JP2012099550A

  • Etching composition and manufacturing method of semiconductor element using the same

    JP2016029717A