Exterior materials for power storage devices

JP7583143B2Active Publication Date: 2024-11-13LISSENOK PACKAGING CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023199745
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-11-27
Publication Date
2024-11-13
Estimated Expiration
2037-03-17

AI Technical Summary

Benefits of technology

【0023】 [1]及び[2]の発明では、エージング処理後の外装材の内側表面(内側シーラント層の最内層の表面)に存在する(析出する)滑剤量の減少を抑制し得て成形時に良好なすべり性を確保できて成形性に優れるとともに、外装材の内側表面(内側シーラント層の最内層の表面)に白粉が表出し難く、十分なシール強度が得られる。また、エージング処理後の外装材の内側シーラント層における金属箔側の第1無延伸フィルム層の表面7aに存在する滑剤量が少ないものとなるので、十分なラミネート強度(金属箔と内側シーラント層とのラミネート強度)を確保できる。更に、前記エージング処理後の外装材の表面(内側シーラント層の最内層の表面)に存在する滑剤量は、輸送や保管時等に熱履歴を受けても変動しないので、優れた成形性を安定して備えた外装材の提供が可能となる。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583143000003
    Figure 0007583143000003
  • Figure 0007583143000004
    Figure 0007583143000004
  • Figure 0007583143000005
    Figure 0007583143000005
Patent Text Reader

Abstract

To provide a sealant film for a power storage device exterior material, which is superior in moldability and hard to cause white powder to appear on its surface, and by which a sufficient lamination strength and a sufficient seal strength can be achieved.SOLUTION: A sealant film for a power storage device exterior material comprises a laminate having two or more layers including a first non-stretched film layer 7 disposed on a side closest to a metal foil, and a second non-stretched film layer 8 laminated on one face of the first non-stretched film layer. The first non-stretched film layer 7 contains a random copolymer containing propylene as a copolymerization component, and another copolymerization component other than the propylene, and contains no lubricant or a lubricant of over 0 ppm and 250 ppm or less. The second non-stretched film layer 8 contains a propylene-based polymer and a lubricant, the content of the lubricant in the second non-stretched film layer 8 being 500-5,000 ppm.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a sealant film used to form an exterior material for electricity storage devices such as batteries and capacitors used in portable devices such as smartphones and tablets, and batteries and capacitors used for storing electricity in hybrid automobiles, electric automobiles, wind power generation, solar power generation, and night-time electricity, and a method for producing an exterior material for electricity storage devices using the sealant film. [Background technology]

[0002] In recent years, as mobile electrical devices such as smartphones and tablet terminals become thinner and lighter, a laminate consisting of a heat-resistant resin layer / adhesive layer / metal foil layer / adhesive layer / thermoplastic resin layer (inner sealant layer) is used as the exterior material of the electricity storage devices such as lithium ion secondary batteries, lithium polymer secondary batteries, lithium ion capacitors, and electric double layer capacitors mounted thereon, instead of the conventional metal can. In addition, power sources for electric vehicles and the like, large power sources for electricity storage, capacitors, etc. are increasingly being exteriorized with the laminate (exterior material) having the above configuration. The laminate is molded into a three-dimensional shape such as a substantially rectangular parallelepiped shape by performing stretch molding or deep drawing. By molding into such a three-dimensional shape, it is possible to secure a storage space for accommodating the main body of the electricity storage device.

[0003] Improving the slipperiness of the surface of the inner sealant layer is required to form such a three-dimensional shape in a good condition without pinholes, breaks, etc. As a laminate material for secondary battery containers that improves the slipperiness of the surface of the inner sealant layer to ensure good formability, a laminate material has been proposed in which an exterior resin film, a first adhesive layer, a chemically treated aluminum foil, a second adhesive layer, and a sealant film are laminated in this order, the sealant film being made of a random copolymer of propylene and an α-olefin with an α-olefin content of 2 to 10% by weight, and containing 1000 to 5000 ppm of a lubricant (see Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2003-288865 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, in the above-mentioned conventional technology, it is difficult to control the amount of lubricant precipitated on the surface of the innermost layer of the exterior material (the inner surface of the inner sealant layer) depending on the heating and holding time and storage period in the production process of the exterior material (laminate material), and although the slipperiness during molding is good, the lubricant precipitates excessively on the surface, and the lubricant adheres to and accumulates on the molding surface of the molding die during molding of the exterior material, generating white powder (white powder caused by the lubricant). When such white powder adheres to and accumulates on the molding surface, it becomes difficult to perform good molding, so it becomes necessary to clean and remove the white powder every time it adheres and accumulates, but there is a problem that cleaning and removing such white powder reduces the productivity of the exterior material.

[0006] In addition, a large amount of lubricant bleeds onto the surface of the inner sealant layer facing the metal foil, which reduces the laminate strength (lamination strength between the metal foil and the inner sealant layer) and makes the metal foil and the inner sealant layer prone to peeling.

[0007] Of course, if the amount of lubricant added (lubricant content) is reduced, it is possible to suppress the adhesion and accumulation of white powder and prevent a decrease in laminate strength, but in this case, the amount of surface lubricant deposition is insufficient, resulting in a problem of poor formability. Thus, in the past, it was difficult to achieve both "excellent formability" and "suppression of the appearance of white powder on the surface of the exterior material and ensuring sufficient laminate strength."

[0008] The present invention has been made in consideration of the above technical background, and aims to provide a sealant film for exterior materials of electricity storage devices, which has excellent moldability, is less likely to produce white powder on the surface, and has sufficient lamination strength and sufficient sealing strength, and an exterior material for electricity storage devices, and a method for manufacturing the same. [Means for solving the problem]

[0009] In order to achieve the above object, the present invention provides the following means.

[0010] [1] A sealant film comprising a laminate of two or more layers including a first non-stretched film layer and a second non-stretched film layer laminated on one side of the first non-stretched film layer, the first non-oriented film layer is a layer of the sealant film disposed closest to the metal foil, The first unstretched film layer contains a random copolymer containing propylene and other copolymer components other than propylene as copolymer components, The first unstretched film layer does not contain a lubricant or contains more than 0 ppm to 250 ppm of a lubricant; The second unstretched film layer contains a propylene-based polymer and a lubricant, 13. A sealant film for exterior packaging of an electricity storage device, wherein the second unoriented film layer has a lubricant content of 500 ppm to 5000 ppm.

[0011] [2] The sealant film for exterior materials of electricity storage devices according to the preceding item 1, further comprising a third non-stretched film layer laminated on a surface of the second non-stretched film layer opposite to the side on which the first non-stretched film layer is laminated, the third non-stretched film layer containing a random copolymer containing propylene and other copolymer components except propylene as copolymer components, and a lubricant, and the content concentration of the lubricant in the third non-stretched film layer is 200 ppm to 3000 ppm.

[0012] [3] The sealant film for exterior materials of electricity storage devices according to item 2, wherein the second non-oriented film layer has a lubricant concentration that is 1.0 to 5.0 times that of the third non-oriented film layer.

[0013] [4] An inner sealant layer made of the sealant film according to the preceding paragraph 1, and a metal foil layer laminated on one side of the inner sealant layer, wherein the amount of lubricant present on the surface of the second non-oriented film layer is 0.1 μg / cm 2 ~1.0μg / cm 2 The exterior material for an electricity storage device is characterized in that

[0014] [5] An inner sealant layer made of the sealant film according to the preceding paragraph 2 or 3, and a metal foil layer laminated on one side of the inner sealant layer, wherein the amount of lubricant present on the surface of the third non-oriented film layer is 0.1 μg / cm 2 ~1.0μg / cm 2 The exterior material for an electricity storage device is characterized in that

[0015] [6] A heat-resistant resin layer as an outer layer, an inner sealant layer made of the sealant film described in the preceding paragraph 1, and a metal foil layer disposed between these two layers, 2 ~1.0μg / cm 2 The exterior material for an electricity storage device is characterized in that

[0016] [7] A heat-resistant resin layer as an outer layer, an inner sealant layer made of the sealant film described in the above item 2 or 3, and a metal foil layer disposed between these two layers, wherein the amount of lubricant present on the surface of the third non-oriented film layer is 0.1 μg / cm 2 ~1.0μg / cm 2 The exterior material for an electricity storage device is characterized in that

[0017] [8] An exterior case for an electricity storage device, comprising a molded article of the exterior material according to any one of items 4 to 7 above.

[0018] [9] A step of preparing a laminate in which the sealant film according to any one of the above items 1 to 3 and a metal foil are laminated via a first adhesive; and an aging step of heat-treating the laminate to obtain an exterior material for an electricity storage device.

[0019]

[10] The method for producing an exterior material for an electricity storage device according to item 9 above, wherein the first adhesive is a thermosetting adhesive.

[0020]

[11] A step of preparing a laminate having a configuration in which a heat-resistant resin film is laminated on one surface of a metal foil via a second adhesive, and the sealant film described in any one of items 1 to 3 is laminated on the other surface of the metal foil via a first adhesive; and an aging step of heat-treating the laminate to obtain an exterior material for an electricity storage device.

[0021]

[12] The method for producing an exterior material for an electricity storage device according to item 11 above, wherein the first adhesive is a thermosetting adhesive, and the second adhesive is a thermosetting adhesive.

[0022]

[13] The amount of lubricant present on the surface of the innermost layer of the exterior material for an electricity storage device obtained by heat treatment is 0.1 μg / cm 2 ~1.0μg / cm 2 13. The method for producing an exterior material for an electricity storage device according to any one of items 9 to 12 above, wherein the above ranges from 1 to 12. Effect of the Invention

[0023] In the inventions [1] and [2], the reduction in the amount of lubricant present (precipitated) on the inner surface of the exterior material (the surface of the innermost layer of the inner sealant layer) after the aging treatment can be suppressed, and good slipperiness can be ensured during molding, resulting in excellent moldability, and white powder is unlikely to appear on the inner surface of the exterior material (the surface of the innermost layer of the inner sealant layer), resulting in sufficient seal strength. In addition, the amount of lubricant present on the surface 7a of the first non-oriented film layer on the metal foil side of the inner sealant layer of the exterior material after the aging treatment is small, so sufficient laminate strength (lamination strength between the metal foil and the inner sealant layer) can be ensured. Furthermore, the amount of lubricant present on the surface of the exterior material after the aging treatment (the surface of the innermost layer of the inner sealant layer) does not change even when subjected to heat history during transportation, storage, etc., so it is possible to provide an exterior material with stable excellent moldability.

[0024] In the invention [3], the lubricant concentration in the second non-stretched film layer is 1.0 to 5.0 times the lubricant concentration in the third non-stretched film layer forming the innermost layer of the packaging material. When the lubricant concentration is 1.0 times or more, intensive migration of the lubricant from the third non-stretched film layer 9 of the innermost layer to the second non-stretched film layer 8 to the interface (the interface between both film layers 8 and 9) due to the lubricant concentration gradient can be suppressed during the aging treatment. When the lubricant concentration is 5.0 times or less, intensive migration of the lubricant from the second non-stretched film layer 8 to the third non-stretched film layer 9 of the innermost layer to the interface (the interface between both film layers 8 and 9) due to the lubricant concentration gradient can be suppressed. The amount of lubricant present on the surface 9a of the third non-stretched film layer forming the innermost layer of the packaging material after the aging treatment is 0.1 μg / cm 2 ~1.0μg / cm 2 This makes it possible to control the melting point within the range of 0.1 to 1.0 μm. This makes it possible to further improve the moldability.

[0025] The inventions [4], [5], [6] and [7] can provide an exterior material for an electricity storage device that has excellent moldability, is less likely to produce white powder on the surface, and has sufficient lamination strength and sufficient sealing strength.

[0026] In addition, the inventions [6] and [7] further include a heat-resistant resin layer as an outer layer, so that the insulation of the metal foil layer on the side opposite the inner sealant layer can be sufficiently ensured, and the physical strength and impact resistance of the exterior material for an electricity storage device can be improved.

[0027] The invention [8] makes it possible to provide an outer casing for an electricity storage device that can be well molded, is less likely to produce white powder on the surface of the outer casing (the surface of the innermost layer of the inner sealant layer), and has sufficient laminate strength and sufficient sealing strength.

[0028] The inventions [9] to

[12] make it possible to produce an exterior material for an electricity storage device that has excellent moldability, is less likely to produce white powder on the surface, and has sufficient laminate strength and sufficient seal strength.

[0029] In addition, the inventions

[11] and

[12] further include a heat-resistant resin layer as an outer layer, so that the insulation of the metal foil layer on the side opposite the inner sealant layer can be sufficiently ensured, and the physical strength and impact resistance of the exterior material can be improved.

[0030] In the invention of

[13] , the amount of lubricant present on the surface of the innermost layer of the exterior material is 0.1 μg / cm 2 ~ 1.0μg / cm 2 Since the range is within this range, better slip properties are exhibited during molding, and It is possible to produce an outer casing material for an electricity storage device that can ensure good moldability and can further prevent the appearance of white powder. In addition, the amount of lubricant present on the surface of the innermost layer of the obtained outer casing material for an electricity storage device (0.1 μg / cm 2 ~1.0μg / cm 2 ) does not fluctuate even when subjected to thermal history during transportation, storage, etc., so that it is possible to provide an exterior material for an electricity storage device that has excellent and stable formability. [Brief description of the drawings]

[0031] [Figure 1] 1 is a cross-sectional view showing one embodiment of an exterior material for an electricity storage device according to the present invention. [Diagram 2] FIG. 3 is a cross-sectional view showing another embodiment of an exterior material for an electricity storage device according to the present invention. [Diagram 3] 1 is a cross-sectional view showing one embodiment of an electricity storage device according to the present invention. [Figure 4] FIG. 4 is a perspective view showing an exterior material (flat), an electricity storage device main body, and an exterior case (a molded body molded into a three-dimensional shape) constituting the electricity storage device in FIG. 3 in a separated state before being heat-sealed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0032] One embodiment of a sealant film 3 for exterior materials of electricity storage devices according to the first invention is shown in Fig. 1. The sealant film 3 is composed of a laminate of two or more layers including a first non-stretched film layer 7 and a second non-stretched film layer 8 laminated on one surface of the first non-stretched film layer 7, the first non-stretched film layer 7 is the layer disposed closest to the metal foil 4 in the sealant film 3, the first non-stretched film layer contains a random copolymer containing propylene and other copolymer components except propylene as copolymer components, the first non-stretched film layer 7 does not contain a lubricant or contains a lubricant, and the second non-stretched film layer 8 contains a propylene-based polymer and a lubricant.

[0033] One embodiment of the sealant film for exterior materials of electricity storage devices according to the second invention is shown in Fig. 2. This sealant film 3 is composed of a laminate of three or more layers including a second non-stretched film layer 8, a first non-stretched film layer 7 laminated on one side of the second non-stretched film layer 8, and a third non-stretched film layer 9 laminated on the other side of the second non-stretched film layer 8, the first non-stretched film layer 7 being the layer disposed closest to the metal foil 4 in the sealant film 3, the first non-stretched film layer 7 containing a random copolymer containing propylene and other copolymer components except propylene as copolymer components, the first non-stretched film layer 7 not containing a lubricant or containing a lubricant, the second non-stretched film layer 8 containing a propylene-based polymer and a lubricant, and the third non-stretched film layer 9 containing a random copolymer containing propylene and other copolymer components except propylene as copolymer components and a lubricant.

[0034] The random copolymer constituting the first unstretched film layer 7 and the third unstretched film layer 9 is a random copolymer containing "propylene" and "other copolymer components other than propylene" as copolymer components. Regarding the random copolymer, the "other copolymer components other than propylene" are not particularly limited, and examples thereof include olefin components such as ethylene, 1-butene, 1-hexene, 1-pentene, and 4-methyl-1-pentene, as well as butadiene.

[0035] The propylene-based polymer constituting the second unstretched film layer 8 is a polymer containing at least propylene as a polymerization component. The propylene-based polymer is not particularly limited, and examples thereof include homopolypropylene and block copolymers containing "propylene" and "other copolymer components other than propylene" as copolymer components. Among them, it is preferable to use at least one resin selected from the group consisting of homopolypropylene and the block copolymers as the propylene-based polymer.

[0036] Regarding the block copolymer, the "other copolymerization components other than propylene" is not particularly limited, but examples thereof include olefin components such as ethylene, 1-butene, 1-hexene, 1-pentene, and 4-methyl-1-pentene, as well as butadiene.

[0037] The second non-oriented film layer 8 preferably contains the propylene polymer, an elastomer component, and the lubricant. In particular, it is more preferable that the propylene polymer is added with the elastomer component to exhibit a microphase-separated morphology (fine structure). That is, it is preferable that the elastomer-modified propylene polymer exhibits a sea-island structure in which the elastomer component is phase-separated into islands in the sea of ​​the propylene polymer. In this case, the whitening phenomenon can be made less likely to occur, and the insulation after sealing can be further improved. The elastomer component is not particularly limited, but examples thereof include EPR (ethylene propylene rubber), propylene-butene elastomer, propylene-butene-ethylene elastomer, EPDM (ethylene-propylene-diene rubber), and the like. Among them, it is preferable to use EPR (ethylene propylene rubber) as the elastomer component.

[0038] In the sealant film 3 according to the first invention, the first non-stretched film layer 7 does not contain a lubricant or contains more than 0 ppm to 250 ppm or less of a lubricant, and it is important that the concentration of the lubricant in the second non-stretched film layer is set to 500 ppm to 5000 ppm. By satisfying such conditions, the lubricant present in the second non-stretched film layer 8 can be prevented from migrating into the first non-stretched film layer 7 when an aging treatment is performed to harden the adhesive, so that the amount of lubricant precipitated on the surface 8a of the innermost layer (second non-stretched film layer) of the packaging material 1 can be secured, good slip properties can be secured during molding of the packaging material, excellent moldability can be obtained, and white powder is unlikely to appear on the surface 8a of the innermost layer (second non-stretched film layer 8), and sufficient lamination strength and sufficient seal strength can be secured. If the lubricant concentration in the first unstretched film layer 7 exceeds 250 ppm, the amount of lubricant present on the surface 7a of the first unstretched film layer 7 facing the metal foil layer 4 will be so large that sufficient laminate strength (lamination strength between the metal foil and the inner sealant layer) cannot be ensured. Furthermore, if the lubricant concentration in the second non-stretched film layer 8 is less than 500 ppm, the amount of lubricant present on the surface 8a of the innermost layer of the packaging material 1 after the aging treatment to harden the adhesive will be insufficient, and excellent formability will not be obtained. On the other hand, if the lubricant concentration exceeds 5,000 ppm, the lubricant will be likely to migrate from the second non-stretched film layer 8 to the first non-stretched film layer 7 after the aging treatment to harden the adhesive, and the amount of lubricant present on the surface 7a of the first non-stretched film layer 7 on the metal foil layer 4 side will increase, making it impossible to ensure sufficient laminate strength (lamination strength between the metal foil and the inner sealant layer) and causing noticeable white powder to form on the surface 8a of the innermost layer (second non-stretched film layer 8).

[0039] In particular, in the sealant film 3 according to the first invention, the first non-stretched film layer 7 preferably does not contain a lubricant or contains more than 0 ppm to 150 ppm of a lubricant. Furthermore, in the sealant film 3 according to the first invention, the first non-stretched film layer 7 more preferably contains 10 ppm to 90 ppm of a lubricant, and particularly preferably contains 20 ppm to 60 ppm of a lubricant. Moreover, the second non-stretched film layer 8 preferably contains 700 ppm to 4500 ppm of a lubricant, more preferably contains 800 ppm to 4000 ppm of a lubricant, and particularly preferably contains 1000 ppm to 2700 ppm of a lubricant.

[0040] Furthermore, when the configuration (second invention) in which the third non-stretched film layer is further provided is adopted, it is important that the first non-stretched film layer 7 does not contain a lubricant or contains more than 0 ppm but not more than 250 ppm of a lubricant, that the lubricant concentration in the second non-stretched film layer 8 is set to 500 ppm to 5000 ppm, and that the lubricant concentration in the third non-stretched film layer 9 is set to 200 ppm to 3000 ppm.

[0041] By satisfying these conditions, when aging treatment is performed to harden the adhesive, the lubricant present in the third non-stretched film layer 9 can be prevented from migrating into the second non-stretched film layer 8 or the first non-stretched film layer 7, so that the amount of lubricant deposited on the surface 9a of the innermost layer (third non-stretched film layer) of the packaging material 1 can be secured, and good slip properties can be secured during molding of the packaging material, resulting in excellent moldability, and the surface 9a of the innermost layer (third non-stretched film layer 9) is less likely to produce white powder, and sufficient laminate strength and sufficient seal strength can be secured. If the lubricant content in the first non-stretched film layer 7 exceeds 250 ppm, the amount of lubricant present on the surface 7a of the first non-stretched film layer 7 on the metal foil layer 4 side becomes large, making it impossible to secure sufficient laminate strength (lamination strength between the metal foil and the inner sealant layer). Furthermore, if the lubricant concentration in the second non-stretched film layer 8 is less than 500 ppm, the lubricant will tend to migrate from the innermost third non-stretched film layer 9 to the second non-stretched film layer 8 when aging treatment is performed to harden the adhesive, and the amount of lubricant present on the surface 9a of the innermost layer will be insufficient, resulting in poor slipperiness during molding.If the lubricant concentration exceeds 5,000 ppm, the lubricant will tend to migrate from the second non-stretched film layer 8 to the first non-stretched film layer 7 when aging treatment is performed to harden the adhesive, and the amount of lubricant present on the surface 7a of the first non-stretched film layer 7 on the metal foil layer 4 side will increase, making it impossible to ensure sufficient laminate strength (lamination strength between the metal foil and the inner sealant layer). Furthermore, if the lubricant concentration in the third unoriented film layer 7 is less than 200 ppm, the amount of lubricant present on the surface 9a of the innermost layer after the aging treatment for hardening the adhesive will be insufficient, making it difficult to obtain excellent formability. On the other hand, if the lubricant concentration exceeds 3000 ppm, white powder will be significantly generated on the surface 9a of the innermost layer after the aging treatment for hardening the adhesive, making it necessary to clean and remove the white powder, resulting in a problem of reduced productivity.

[0042] In particular, in the sealant film 3 according to the second invention, the first non-stretched film layer 7 preferably does not contain a lubricant or contains more than 0 ppm to 150 ppm of a lubricant. Furthermore, in the sealant film 3 according to the second invention, the first non-stretched film layer 7 more preferably contains 10 ppm to 90 ppm of a lubricant, and particularly preferably contains 20 ppm to 60 ppm of a lubricant. Furthermore, in the sealant film 3 according to the second invention, the second non-stretched film layer 8 preferably contains 700 ppm to 4500 ppm of a lubricant, more preferably contains 800 ppm to 4000 ppm of a lubricant, and particularly preferably contains 1000 ppm to 2700 ppm of a lubricant. In the sealant film 3 according to the second invention, the third non-oriented film layer 9 preferably contains 300 ppm to 2700 ppm of lubricant, more preferably 500 ppm to 2000 ppm of lubricant, and particularly preferably 800 ppm to 1200 ppm of lubricant.

[0043] In the sealant film 3 according to the second invention, the lubricant concentration in the second non-stretched film layer 8 is preferably 1.0 to 5.0 times the lubricant concentration in the third non-stretched film layer 9. When the lubricant concentration is 1.0 or more, intensive migration of the lubricant from the third non-stretched film layer 9, which is the innermost layer, to the interface (the interface between both film layers 8 and 9) due to the lubricant concentration gradient from the third non-stretched film layer 9, which is the innermost layer, to the second non-stretched film layer 8 during aging treatment can be suppressed, and when the lubricant concentration is 5.0 or less, intensive migration of the lubricant from the second non-stretched film layer 8 to the third non-stretched film layer 9, which is the innermost layer, to the interface (the interface between both film layers 8 and 9) due to the lubricant concentration gradient can be suppressed, and the amount of lubricant present on the surface 9a of the third non-stretched film layer forming the innermost layer of the exterior material after aging treatment can be 0.1 μg / cm 2 ~1.0μg / cm 2 In particular, the lubricant concentration in the second non-oriented film layer 8 is more preferably 1.0 to 4.5 times, and even more preferably 1.0 to 4.0 times, the lubricant concentration in the third non-oriented film layer 9.

[0044] The lubricant is not particularly limited, but examples thereof include saturated fatty acid amides, unsaturated fatty acid amides, substituted amides, methylol amides, saturated fatty acid bisamides, unsaturated fatty acid bisamides, fatty acid ester amides, and aromatic bisamides.

[0045] The saturated fatty acid amide is not particularly limited, but examples thereof include lauric acid amide, palmitic acid amide, stearic acid amide, behenic acid amide, hydroxystearic acid amide, etc. The unsaturated fatty acid amide is not particularly limited, but examples thereof include oleic acid amide, erucic acid amide, etc.

[0046] The substituted amide is not particularly limited, but examples thereof include N-oleyl palmitic acid amide, N-stearyl stearic acid amide, N-stearyl oleic acid amide, N-oleyl stearic acid amide, N-stearyl erucic acid amide, etc. The methylol amide is not particularly limited, but examples thereof include methylol stearic acid amide, etc.

[0047] The saturated fatty acid bisamide is not particularly limited, but examples thereof include methylene bisstearic acid amide, ethylene biscapric acid amide, ethylene bislauric acid amide, ethylene bisstearic acid amide, ethylene bishydroxystearic acid amide, ethylene bisbehenic acid amide, hexamethylene bisstearic acid amide, hexamethylene bisbehenic acid amide, hexamethylene hydroxystearic acid amide, N,N'-distearyl adipic acid amide, and N,N'-distearyl sebacic acid amide.

[0048] The unsaturated fatty acid bisamide is not particularly limited, but examples thereof include ethylene bisoleamide, ethylene biserucamide, hexamethylene bisoleamide, and N,N'-dioleylsebacamide.

[0049] The fatty acid ester amide is not particularly limited, but examples thereof include stearamide ethyl stearate, etc. The aromatic bisamide is not particularly limited, but examples thereof include m-xylylene bisstearic acid amide, m-xylylene bishydroxystearic acid amide, N,N'-cystearyl isophthalic acid amide, etc.

[0050] The thickness of the sealant film 3 is preferably set to 10 μm to 100 μm. By setting the thickness to 10 μm or more, the occurrence of pinholes can be sufficiently prevented, and by setting the thickness to 100 μm or less, the amount of resin used can be reduced, thereby reducing costs.

[0051] When the two-layer laminate structure of FIG. 1 is adopted as the sealant film 3, the thickness ratio of the two layers is preferably set in the range of thickness of first non-stretched film layer 7 / thickness of second non-stretched film layer 8=5-90 / 95-10, and particularly preferably set in the range of thickness of first non-stretched film layer 7 / thickness of second non-stretched film layer 8=5-40 / 95-60.

[0052] Furthermore, when the sealant film 3 has the three-layer laminate structure shown in FIG. 2, the thickness ratio of the three layers is preferably set in the range of thickness of first non-stretched film layer 7 / thickness of second non-stretched film layer 8 / thickness of third non-stretched film layer 9=5-45 / 90-10 / 5-45, and particularly preferably set in the range of thickness of first non-stretched film layer 7 / thickness of second non-stretched film layer 8 / thickness of third non-stretched film layer 9=5-20 / 90-60 / 5-20.

[0053] When the two-layer laminated structure of FIG. 1 is adopted as the sealant film 3, the second non-stretched film layer 8 forming the innermost layer may further contain an antiblocking agent. When the three-layer laminated structure of FIG. 2 is adopted as the sealant film 3, the third non-stretched film layer 9 forming the innermost layer may further contain an antiblocking agent. The antiblocking agent is not particularly limited, but examples thereof include silica particles, acrylic resin particles, and aluminum silicate particles. The particle size of the antiblocking agent is preferably in the range of 0.1 μm to 10 μm in average particle size, and more preferably in the range of 1 μm to 5 μm in average particle size. When the antiblocking agent is incorporated into the second non-stretched film layer 8 forming the innermost layer or the third non-stretched film layer 9 forming the innermost layer, the content concentration thereof is preferably set to 100 ppm to 5000 ppm.

[0054] By incorporating the antiblocking agent (particles) in the innermost layer, minute protrusions are formed on the surface of the innermost layer (8a in Fig. 1, 9a in Fig. 2) to reduce the contact area between films, thereby suppressing blocking between sealant films. In addition, by incorporating the antiblocking agent (particles) together with the lubricant, the slipperiness during molding can be further improved.

[0055] The sealant film 3 is preferably produced by a molding method such as multi-layer extrusion molding, inflation molding, or T-die cast film molding.

[0056] The exterior packaging material 1 for an electricity storage device according to the present invention is produced using the sealant film 3 having the above-mentioned configuration.

[0057] A first manufacturing method (manufacturing method for an exterior material for an electricity storage device) according to the present invention will be described. First, a laminate is prepared in which the sealant film 3 of the present invention (first invention or second invention) and a metal foil 4 are laminated via a first adhesive (inner adhesive) 6. At this time, the first unstretched film layer 7 of the sealant film 3 contacts the first adhesive 6. Next, the obtained laminate is heat-treated (ageing treatment is performed) to obtain the exterior material for an electricity storage device 1 of the present invention.

[0058] Next, a second manufacturing method (manufacturing method for an exterior material for an electricity storage device) according to the present invention will be described. A laminate is prepared in which a heat-resistant resin film (outer layer) 2 is laminated on one side of a metal foil 4 via a second adhesive (outer adhesive) 5, and a sealant film 3 of the present invention (first invention or second invention) is laminated on the other side of the metal foil 4 via a first adhesive (inner adhesive) 6. At this time, the first non-stretched film layer 7 of the sealant film 3 contacts the first adhesive (inner adhesive) 6 (see Figs. 1 and 2). Next, the obtained laminate is subjected to a heat treatment (aging treatment), thereby obtaining an exterior material for an electricity storage device 1 of the present invention having the configuration shown in Figs. 1 and 2. That is, the exterior material 1 for a storage battery device of the present invention obtained through such an aging treatment has a configuration in which a heat-resistant resin layer (outer layer) 2 is laminated and integrated on one surface of a metal foil layer 4 via a second adhesive layer (outer adhesive layer) 5, and an inner sealant layer (sealant film) (inner layer) 3 is laminated and integrated on the other surface of the metal foil layer 4 via a first adhesive layer (inner adhesive layer) 6 (see Figs. 1 and 2). When the sealant film of the first invention is used as the sealant film 3, the second non-stretch film layer 8 of the sealant film 3 forms the innermost layer (see Fig. 1). When the sealant film of the second invention is used as the sealant film 3, the third non-stretch film layer 9 of the sealant film 3 forms the innermost layer (see Fig. 2).

[0059] The first adhesive (inner adhesive) 6 is not particularly limited, but may be, for example, a thermosetting adhesive. The second adhesive (outer adhesive) 5 is not particularly limited, but may be, for example, a thermosetting adhesive. The thermosetting adhesive is not particularly limited, but may be, for example, an olefin-based adhesive, an epoxy-based adhesive, an acrylic-based adhesive, etc.

[0060] The heating temperature in the aging treatment is preferably set to 65° C. or less, and from the viewpoint of maintaining the degree of hardening of the adhesive and the suitable amount of lubricant present in the innermost layer of the packaging material, it is more preferably set to 35° C. to 45° C. In addition, since the hardening time varies depending on the type of adhesive, the heating time in the aging treatment may be any time that is longer than the time that provides sufficient adhesive strength for the type of adhesive, but considering the lead time of the process, it is better that the heating time is as short as possible as long as sufficient adhesive strength is obtained.

[0061] The exterior material 1 for an electrical storage device obtained through the above-mentioned aging treatment uses the sealant film of the above-mentioned present invention (first invention or second invention) as the sealant film 3 used in its production, and therefore has excellent formability, is less likely to produce white powder on the surface, and provides sufficient lamination strength and sufficient sealing strength.

[0062] In the exterior material for an electricity storage device 1 obtained through the aging treatment, the amount of lubricant present on the surface of the innermost layer was 0.1 μg / cm 2 ~1.0μg / cm 2 That is, when the sealant film of the first invention is used as the sealant film 3, the amount of the lubricant present on the surface 8a of the second non-oriented film layer 8 is preferably in the range of 0.1 μg / cm 2 ~1.0μg / cm 2 (See FIG. 1 ), and as the sealant film 3, When the sealant film of the second invention is used, the amount of lubricant present on the surface 9a of the third non-oriented film layer 9 is 0.1 μg / cm 2~1.0μg / cm 2 (See FIG. 2.) In particular, in the electrical storage device packaging material 1 obtained through the aging treatment, the amount of lubricant present on the surfaces 8a and 9a of the innermost layer is preferably in the range of 0.1 μg / cm 2 ~0.6μg / cm 2 It is more preferable that the range is .

[0063] In the exterior packaging material 1 for an electricity storage device of the present invention, the inner sealant layer (inner layer) 3 provides excellent chemical resistance even against highly corrosive electrolytes used in lithium ion secondary batteries and the like, and also plays a role in imparting heat sealing properties to the exterior packaging material.

[0064] Although the heat-resistant resin layer (substrate layer; outer layer) 2 is not an essential constituent layer, it is preferable to adopt a configuration in which the heat-resistant resin layer 2 is laminated on the other surface (the surface opposite to the inner sealant layer) of the metal foil layer 4 via a second adhesive layer (outer adhesive layer) 5 (see Figs. 1 and 2). By providing such a heat-resistant resin layer 2, it is possible to sufficiently ensure insulation on the other surface (the surface opposite to the inner sealant layer) of the metal foil layer 4, and it is possible to improve the physical strength and impact resistance of the exterior material 1 for an electricity storage device.

[0065] A heat-resistant resin that does not melt at the heat-sealing temperature when the exterior material is heat-sealed is used as the heat-resistant resin constituting the heat-resistant resin layer (substrate layer; outer layer) 2. In the first invention, it is preferable to use a heat-resistant resin having a melting point 10° C. or more higher than the melting point of the resin constituting the second non-oriented film layer 8 as the heat-resistant resin, and in the second invention, it is preferable to use a heat-resistant resin having a melting point 10° C. or more higher than the melting point of the resin constituting the third non-oriented film layer 9.

[0066] The heat-resistant resin layer (outer layer) 2 is not particularly limited, but examples thereof include polyamide films such as nylon films, polyester films, etc., and these stretched films are preferably used. Among them, it is particularly preferable to use biaxially stretched polyamide films such as biaxially stretched nylon films, biaxially stretched polybutylene terephthalate (PBT) films, biaxially stretched polyethylene terephthalate (PET) films, or biaxially stretched polyethylene naphthalate (PEN) films as the heat-resistant resin layer 2. The nylon film is not particularly limited, but examples thereof include 6 nylon film, 6,6 nylon film, and MXD nylon film. The heat-resistant resin layer 2 may be formed as a single layer, or may be formed as a multilayer of, for example, polyester film / polyamide film (such as a multilayer of PET film / nylon film).

[0067] The thickness of the heat-resistant resin layer (outer layer) 2 is preferably 2 μm to 50 μm. When a polyester film is used, the thickness is preferably 2 μm to 50 μm, and when a nylon film is used, the thickness is preferably 7 μm to 50 μm. By setting the thickness to be equal to or greater than the above-mentioned preferable lower limit, sufficient strength as an exterior material can be ensured, and by setting the thickness to be equal to or less than the above-mentioned preferable upper limit, stress during molding such as stretch molding and draw molding can be reduced, improving moldability.

[0068] The metal foil layer 4 plays a role of imparting gas barrier properties that prevent the intrusion of oxygen and moisture to the exterior material 1. The metal foil layer 4 is not particularly limited, but examples thereof include aluminum foil, SUS foil (stainless steel foil), copper foil, etc., and among these, it is preferable to use aluminum foil and SUS foil (stainless steel foil). The thickness of the metal foil layer 4 is preferably 5 μm to 120 μm. By having a thickness of 5 μm or more, it is possible to prevent the occurrence of pinholes during rolling in manufacturing the metal foil, and by having a thickness of 120 μm or less, it is possible to reduce stress during forming such as stretch forming and drawing, thereby improving formability. Among these, the thickness of the metal foil layer 4 is more preferably 10 μm to 80 μm.

[0069] It is preferable that at least the inner surface (the surface on the inner sealant layer 3 side) of the metal foil layer 4 is subjected to a chemical conversion treatment. By performing such a chemical conversion treatment, corrosion of the metal foil surface due to the contents (such as the electrolyte of a battery) can be sufficiently prevented. For example, the chemical conversion treatment is performed on the metal foil by carrying out the following treatment. That is, for example, the surface of the metal foil that has been subjected to a degreasing treatment is subjected to the following treatment. 1) Phosphoric acid, Chromic acid, At least one compound selected from the group consisting of metal salts of fluorides and nonmetal salts of fluorides. 2) phosphoric acid; At least one resin selected from the group consisting of acrylic resins, chitosan derivative resins, and phenolic resins; At least one compound selected from the group consisting of chromic acid and chromium (III) salts; Aqueous solution of a mixture containing 3) phosphoric acid; At least one resin selected from the group consisting of acrylic resins, chitosan derivative resins, and phenolic resins; At least one compound selected from the group consisting of chromic acid and chromium (III) salts; At least one compound selected from the group consisting of metal salts of fluorides and nonmetal salts of fluorides. The chemical conversion treatment is carried out by applying an aqueous solution of any one of the above 1) to 3) and then drying.

[0070] The chemical conversion coating has a chromium coating weight (per side) of 0.1 mg / m 2 ~50mg / m 2 is preferred, and 2 mg / m 2 ~20mg / m 2 is preferred.

[0071] The thickness of the second adhesive layer (outer adhesive layer) 5 is preferably set to 1 μm to 5 μm. In particular, from the viewpoint of making the exterior material 1 thinner and lighter, the thickness of the outer adhesive layer 5 is particularly preferably set to 1 μm to 3 μm.

[0072] The thickness of the first adhesive layer (inner adhesive layer) 6 is preferably set to 1 μm to 5 μm. In particular, from the viewpoint of making the exterior material 1 thinner and lighter, the thickness of the inner adhesive layer 6 is particularly preferably set to 1 μm to 3 μm.

[0073] The exterior material 1 for an electricity storage device of the present invention is used, for example, as an exterior material for a lithium ion secondary battery. The exterior material 1 for an electricity storage device may be used as an exterior material as it is without being subjected to molding (see FIG. 4), or may be subjected to molding such as deep drawing or stretch molding and used as an exterior case 10 (see FIG. 4).

[0074] FIG. 3 shows an embodiment of an electricity storage device 30 constructed using the exterior material 1 for an electricity storage device of the present invention. This electricity storage device 30 is a lithium ion secondary battery. In this embodiment, as shown in FIGS. 3 and 4, an exterior member 15 is constructed by an exterior case 10 obtained by molding the exterior material 1 and a planar exterior material 1. Thus, a substantially rectangular parallelepiped electricity storage device main body (electrochemical element, etc.) 31 is accommodated in the accommodation recess of the exterior case 10 obtained by molding the exterior material 1 of the present invention, and the exterior material 1 of the present invention is placed on the electricity storage device main body 31 with its inner sealant layer 3 side facing inward (lower side) without being molded, and the peripheral portion of the inner sealant layer 3 of the planar exterior material 1 and the inner sealant layer 3 of the flange portion (sealing peripheral portion) 29 of the exterior case 10 are sealed and joined by heat sealing to construct the electricity storage device 30 of the present invention (see FIGS. 3 and 4). The inner surface of the storage recess of the outer case 10 is an inner sealant layer 3, and the outer surface of the storage recess is a heat-resistant resin layer (outer layer) 2 (see Fig. 4). When the exterior material shown in Fig. 1 is used as the exterior material forming the outer case 10, the inner surface of the storage recess is the second unstretched film layer 8, which is the innermost layer, and when the exterior material shown in Fig. 2 is used as the exterior material forming the outer case 10, the inner surface of the storage recess is the third unstretched film layer 9, which is the innermost layer.

[0075] 3, reference numeral 39 denotes a heat seal portion at which the peripheral portion of the exterior material 1 and a flange portion (sealing peripheral portion) 29 of the exterior case 10 are joined (welded) to each other. In the electricity storage device 30, a tip portion of a tab lead connected to an electricity storage device main body 31 is led out to the outside of the exterior member 15, but is not shown in the figure.

[0076] The electricity storage device main body 31 is not particularly limited, but examples thereof include a battery main body, a capacitor main body, and a condenser main body.

[0077] The width of the heat-sealed portion 39 is preferably set to 0.5 mm or more. By setting the width to 0.5 mm or more, sealing can be performed reliably. In particular, the width of the heat-sealed portion 39 is preferably set to 3 mm to 15 mm.

[0078] In the above embodiment, the exterior member 15 is configured to include an exterior case 10 obtained by molding the exterior material 1 and a planar exterior material 1 (see Figures 3 and 4), but is not limited to this combination. For example, the exterior member 15 may be configured to include a pair of planar exterior materials 1, or a pair of exterior cases 10. EXAMPLES

[0079] Next, specific examples of the present invention will be described, but the present invention is not particularly limited to these examples.

[0080] <Example 1> A chemical conversion coating was formed by applying a chemical conversion solution consisting of phosphoric acid, polyacrylic acid (acrylic resin), a chromium (III) salt compound, water, and alcohol to both sides of an aluminum foil 4 having a thickness of 40 μm, and then drying at 180° C. The chromium deposition amount of this chemical conversion coating was 10 mg / m per side. 2 It was.

[0081] Next, a biaxially oriented nylon 6 film 2 having a thickness of 25 μm was dry laminated (attached) to one surface of the aluminum foil 4 that had been subjected to the chemical conversion treatment via a two-liquid curing urethane adhesive 5 .

[0082] Next, a first unstretched film 7 having a thickness of 12 μm containing an ethylene-propylene random copolymer and 100 ppm of erucic acid amide and a second unstretched film 8 having a thickness of 28 μm containing an ethylene-propylene block copolymer, 2500 ppm of erucic acid amide, and 2000 ppm of silica particles (antiblocking agent; average particle size: 2 μm) were co-extruded using a T-die so as to form a two-layer laminate, thereby forming a sealant film (first unstretched film) having a thickness of 40 μm formed by laminating these two layers. After obtaining the film layer 7 / second non-oriented film layer 8) 3, the first non-oriented film layer 7 side of the sealant film 3 was overlapped on the other side of the dry-laminated aluminum foil 4 via a two-component curing type maleic acid-modified polypropylene adhesive 6, and dry-laminated by being sandwiched and pressed between a rubber nip roll and a laminating roll heated to 100°C, and then aged (heated) at 40°C for 10 days to obtain an exterior material 1 for an electricity storage device having the configuration shown in Figure 1.

[0083] The two-component curing maleic acid-modified polypropylene adhesive used was an adhesive solution containing 100 parts by mass of maleic acid-modified polypropylene (melting point 80° C., acid value 10 mgKOH / g) as a base agent, 8 parts by mass of an isocyanurate of hexamethylene diisocyanate (NCO content: 20% by mass) as a curing agent, and a solvent. The adhesive solution was applied at a solid content of 2 g / m 2 The coating was applied to the other surface of the aluminum foil 4 so as to become 100%. The coating was then dried by heating, and the sealant film 3 was then laminated onto the surface of the first non-oriented film layer 7 .

[0084] In the obtained packaging material 1 for an electricity storage device, the amount of lubricant present on the surface 8a of the innermost layer (second unstretched film layer 8) of the packaging material 1 was 0.27 μg / cm 2 The sealant for the exterior material The amount of lubricant present on the surface (surface of the first unstretched film layer 7) 7a of the film 3 on the metal foil layer 4 side is 0.38 μg / cm 2 (See Table 1).

[0085] <Example 2> An exterior material for an electricity storage device 1 having the configuration shown in FIG. 1 was obtained in the same manner as in Example 1, except that the content concentration of erucamide in the first unstretched film layer 7 before lamination was set to 0 ppm, and the content concentration of erucamide in the second unstretched film layer 8 before lamination was set to 3000 ppm.

[0086] <Example 3> A chemical conversion treatment solution consisting of phosphoric acid, polyacrylic acid (acrylic resin), chromium (III) salt compound, water, and alcohol is applied to both sides of an aluminum foil 4 having a thickness of 40 μm, and then heated at 180° C. The coating had a chromium content of 10 mg / m2 per side. 2 It was.

[0087] Next, a biaxially oriented nylon 6 film 2 having a thickness of 25 μm was dry laminated (attached) to one surface of the aluminum foil 4 that had been subjected to the chemical conversion treatment via a two-liquid curing urethane adhesive 5 .

[0088] Next, a first unstretched film 7 having a thickness of 6 μm containing an ethylene-propylene random copolymer and 100 ppm of erucic acid amide, a second unstretched film 8 having a thickness of 28 μm containing an ethylene-propylene block copolymer and 2500 ppm of erucic acid amide, and a third unstretched film 9 having a thickness of 6 μm containing an ethylene-propylene random copolymer, 1000 ppm of erucic acid amide, and 2000 ppm of silica particles (antiblocking agent; average particle size 2 μm) were co-extruded using a T-die so that the three layers were laminated in this order. After obtaining a sealant film (first non-stretched film layer 7 / second non-stretched film layer 8 / third non-stretched film layer 9) 3 having a thickness of 40 μm, the first non-stretched film layer 7 side of the sealant film 3 was overlapped on the other side of the dry-laminated aluminum foil 4 via a two-component curing type maleic acid-modified polypropylene adhesive 6, and the resulting film was sandwiched between a rubber nip roll and a laminating roll heated to 100° C. and pressed to be dry laminated, and then aged (heated) at 40° C. for 10 days to obtain an exterior material for an electricity storage device 1 having the configuration shown in FIG. 2.

[0089] The two-component curing maleic acid-modified polypropylene adhesive used was an adhesive solution containing 100 parts by mass of maleic acid-modified polypropylene (melting point 80° C., acid value 10 mgKOH / g) as a base agent, 8 parts by mass of an isocyanurate of hexamethylene diisocyanate (NCO content: 20% by mass) as a curing agent, and a solvent. The adhesive solution was applied at a solid content of 2 g / m 2 The coating was applied to the other surface of the aluminum foil 4 so as to become 100%. The coating was then dried by heating, and the sealant film 3 was then laminated onto the surface of the first non-oriented film layer 7 .

[0090] In the obtained packaging material 1 for an electricity storage device, the amount of lubricant present on the surface 9a of the innermost layer (third unstretched film layer 9) of the packaging material was 0.25 μg / cm 2 The amount of lubricant present on the surface (surface of the first unstretched film layer 7) 7a of the sealant film 3 of the exterior material on the side of the metal foil layer 4 is 0.25 μg / cm2 (See Table 1).

[0091] <Example 4> An exterior material for an electricity storage device 1 having the configuration shown in FIG. 2 was obtained in the same manner as in Example 3, except that the content concentration of erucamide in the first unstretched film layer 7 before lamination was set to 60 ppm, and the content concentration of erucamide in the second unstretched film layer 8 before lamination was set to 1000 ppm.

[0092] <Example 5> An outer casing material for an electricity storage device 1 having the configuration shown in FIG. 2 was obtained in the same manner as in Example 3, except that the content concentration of erucamide in the third unoriented film layer 9 before lamination was set to 500 ppm.

[0093] <Example 6> An exterior material for a power storage device 1 having the configuration shown in FIG. 2 was obtained in the same manner as in Example 3, except that the erucamide concentration in the first unstretched film layer 7 before lamination was set to 60 ppm, the erucamide concentration in the second unstretched film layer 8 before lamination was set to 1000 ppm, and the erucamide concentration in the third unstretched film layer 9 before lamination was set to 2000 ppm.

[0094] <Example 7> An exterior material for an electricity storage device 1 having the configuration shown in FIG. 2 was obtained in the same manner as in Example 3, except that behenic acid amide was used instead of erucic acid amide as the lubricant in the first unstretched film layer 7, the second unstretched film layer 8, and the third unstretched film layer 9, and the content concentration of behenic acid amide in the first unstretched film layer 7 before lamination was set to 50 ppm.

[0095] <Example 8> An outer casing material for an electricity storage device 1 having the configuration shown in FIG. 2 was obtained in the same manner as in Example 7, except that oleic acid amide was used instead of erucic acid amide as the lubricant in the first unstretched film layer 7, the second unstretched film layer 8, and the third unstretched film layer 9.

[0096] <Example 9> An exterior material for an electricity storage device 1 having the configuration shown in FIG. 2 was obtained in the same manner as in Example 7, except that stearic acid amide was used instead of erucic acid amide as the lubricant in the first unstretched film layer 7, the second unstretched film layer 8, and the third unstretched film layer 9.

[0097] <Example 10> An outer casing material for an electricity storage device 1 having the configuration shown in FIG. 2 was obtained in the same manner as in Example 3, except that the content concentration of erucamide in the second unoriented film layer 8 before lamination was set to 4500 ppm.

[0098] <Example 11> An exterior material for a power storage device 1 having the configuration shown in FIG. 2 was obtained in the same manner as in Example 3, except that the content concentration of erucamide in the first unstretched film layer 7 before lamination was set to 0 ppm, and the content concentration of erucamide in the second unstretched film layer 8 before lamination was set to 2000 ppm.

[0099] <Comparative Example 1> An outer casing material for an electricity storage device was obtained in the same manner as in Example 1, except that the content concentration of erucamide in the first unoriented film layer 7 before lamination was set to 400 ppm.

[0100] <Comparative Example 2> An exterior material for a power storage device was obtained in the same manner as in Example 1, except that the erucamide content in the first unstretched film layer 7 before lamination was set to 50 ppm, and the erucamide content in the second unstretched film layer 8 before lamination was set to 6000 ppm.

[0101] <Comparative Example 3> An outer casing material for an electricity storage device was obtained in the same manner as in Example 3, except that the content concentration of erucamide in the first unoriented film layer 7 before lamination was set to 500 ppm.

[0102] <Comparative Example 4> An exterior material for a power storage device was obtained in the same manner as in Example 3, except that the erucamide content in the first unstretched film layer 7 before lamination was set to 400 ppm, and the erucamide content in the second unstretched film layer 8 before lamination was set to 1000 ppm.

[0103] <Comparative Example 5> An exterior material for a power storage device was obtained in the same manner as in Example 3, except that the erucamide content in the first unstretched film layer 7 before lamination was set to 500 ppm, and the erucamide content in the third unstretched film layer 9 before lamination was set to 500 ppm.

[0104] <Comparative Example 6> An exterior material for a power storage device was obtained in the same manner as in Example 3, except that the erucamide content in the first unstretched film layer 7 before lamination was set to 360 ppm, the erucamide content in the second unstretched film layer 8 before lamination was set to 1000 ppm, and the erucamide content in the third unstretched film layer 9 before lamination was set to 2000 ppm.

[0105] <Comparative Example 7> An exterior material for a storage battery device was obtained in the same manner as in Example 3, except that behenic acid amide was used instead of erucic acid amide as the lubricant in the first unstretched film layer 7, the second unstretched film layer 8, and the third unstretched film layer 9, and the content concentration of behenic acid amide in the first unstretched film layer 7 before lamination was set to 320 ppm.

[0106] <Comparative Example 8> An exterior material for an electricity storage device was obtained in the same manner as in Comparative Example 7, except that oleic acid amide was used instead of erucic acid amide as the lubricant in the first unstretched film layer 7, the second unstretched film layer 8 and the third unstretched film layer 9.

[0107] <Comparative Example 9> An exterior material for an electricity storage device was obtained in the same manner as in Comparative Example 7, except that stearic acid amide was used instead of erucic acid amide as the lubricant in the first unstretched film layer 7, the second unstretched film layer 8, and the third unstretched film layer 9.

[0108] <Comparative Example 10> An exterior material for a power storage device was obtained in the same manner as in Example 3, except that the erucamide content in the first unstretched film layer 7 before lamination was set to 400 ppm, and the erucamide content in the second unstretched film layer 8 before lamination was set to 4500 ppm.

[0109] <Comparative Example 11> An exterior material for a power storage device was obtained in the same manner as in Example 3, except that the erucamide content in the first unstretched film layer 7 before lamination was set to 60 ppm, and the erucamide content in the second unstretched film layer 8 before lamination was set to 100 ppm.

[0110] <Comparative Example 12> An outer casing material for an electricity storage device was obtained in the same manner as in Example 3, except that the content concentration of erucamide in the second unoriented film layer 8 before lamination was set to 5500 ppm.

[0111] <Comparative Example 13> An outer casing material for an electricity storage device was obtained in the same manner as in Example 3, except that the content concentration of erucamide in the third unoriented film layer 9 before lamination was set to 100 ppm.

[0112] <Comparative Example 14> An exterior material for a power storage device was obtained in the same manner as in Example 3, except that the erucamide content in the first unstretched film layer 7 before lamination was set to 60 ppm, the erucamide content in the second unstretched film layer 8 before lamination was set to 1000 ppm, and the erucamide content in the third unstretched film layer 9 before lamination was set to 4000 ppm.

[0113] [Table 1]

[0114] [Table 2]

[0115] Each of the exterior materials for electricity storage devices (after aging treatment) obtained as described above was evaluated according to the following evaluation methods. The results are shown in Tables 1 and 2.

[0116] The dynamic friction coefficients shown in Tables 1 and 2 were measured on the surface of the innermost layer of each electrical storage device exterior material (after aging treatment) in accordance with JIS K7125-1995 (see Figs. 1 and 2). The surface of the innermost layer was surface 8a of the second unstretched film layer in Examples 1 and 2 and Comparative Examples 1 and 2, and surface 9a of the third unstretched film layer in Examples 3 to 11 and Comparative Examples 3 to 14 (see Figs. 1 and 2).

[0117] <Method for evaluating the amount of lubricant present on the surface of the innermost layer of exterior material> Two rectangular test pieces measuring 100 mm long x 100 mm wide were cut out from each exterior material for power storage devices, and these two test pieces were then overlapped and the periphery of the inner sealant layer was heat sealed at a heat seal temperature of 200°C to produce a bag. 1 mL of acetone was injected into the internal space of this bag using a syringe, and the bag was left for 3 minutes with the surface of the innermost layer of the inner sealant layer in contact with the acetone, after which the acetone was removed from the bag. The amount of lubricant contained in the removed liquid was measured and analyzed using a gas chromatograph to determine the amount of lubricant (μg / cm) present on the surface of the innermost layer of the exterior material. 2 ) was calculated. 2 The amount of lubricant per unit was determined.

[0118] <Method for Evaluating the Amount of Lubricant Present on Surface 7a of First Unstretched Film Layer in Exterior Material> In each of the examples and comparative examples, the sealant film 3 produced by coextrusion was cut into a rectangular shape of 200 mm long x 200 mm wide, and then aged at 40°C for 10 days. Two rectangular test pieces of 100 mm long x 100 mm wide were cut out from the aged film, and these two test pieces were overlapped so that the first non-stretched film layers 7 were in contact with each other, and the periphery was covered with a nylon film, and the periphery was heat-sealed at a heat-sealing temperature of 200°C to produce a bag. 1 mL of acetone was injected into the internal space of this bag using a syringe, and the bag was left for 3 minutes in a state in which the surface of the first non-stretched film layer (the inner surface of the bag) was in contact with the acetone, and then the acetone in the bag was removed. The amount of lubricant contained in the extracted liquid was measured and analyzed using a gas chromatograph to determine the amount of lubricant (μg / cm 2 ) present on the surface 7a of the first non-stretched film layer. 2 That is, the first unstretched film layer Surface of 1cm 2 The amount of lubricant per unit was determined.

[0119] <Moldability evaluation method> A single-stage deep drawing process was performed on the exterior material using a depth-free straight mold under the following molding conditions, and the moldability was evaluated for each molding depth (9mm, 8mm, 7mm, 6mm, 5mm, 4mm, 3mm, 2mm), and the maximum molding depth (mm) at which good molding without any pinholes at the corners could be performed was investigated. The maximum molding depth of 5mm or more was judged as "○", the maximum molding depth of 2mm or more but less than 5mm was judged as "△", and the maximum molding depth of less than 2mm was judged as "×". The presence or absence of pinholes was checked by visually observing the presence or absence of transmitted light passing through the pinholes. (Molding conditions) Mold: Punch: 33.3mm x 53.9mm, Die: 80mm x 120mm, Corner R: 2mm, Punch R: 1.3mm, Die R: 1mm Wrinkle holding pressure: Gauge pressure: 0.475MPa, Actual pressure (calculated value): 0.7MPa Material: SC (carbon steel), punch R only chrome plated.

[0120] <Method for assessing the presence or absence of white powder> After cutting out a rectangular test piece of 600 mm long x 100 mm wide from each exterior material for electric storage devices, the obtained test piece was placed on a test stand with the three inner sealant layers (i.e., the surface 8a or 9a of the innermost layer) facing up, and a SUS weight (mass 1.3 kg, contact surface size 55 mm x 50 mm) with a black cloth wrapped around it and its surface black was placed on the upper surface of the test piece, and the weight was pulled in a horizontal direction parallel to the upper surface of the test piece at a pulling speed of 4 cm / sec, so that the weight was pulled over a length of 400 mm in contact with the upper surface of the test piece. The cloth (black) on the contact surface of the weight after the pulling movement was visually observed, and a case in which white powder was noticeably generated on the surface of the cloth (black) was marked as "x", a case in which white powder was generated to a certain degree (moderate degree) was marked as "△", and a case in which there was little or no white powder was recognized was marked as "○". The black cloth used was "Static Electricity Removal Sheet S SD2525 3100" manufactured by TRUSCO.

[0121] <Seal strength evaluation method> Two test pieces measuring 15 mm in width and 150 mm in length were cut out from the obtained exterior material, and then these two test pieces were overlapped so that their inner sealant layers were in contact with each other. In this state, heat sealing was performed by heating one side using a heat sealing device (TP-701-A) manufactured by Tester Sangyo Co., Ltd. under the following conditions: heat sealing temperature: 200°C, sealing pressure: 0.2 MPa (gauge pressure), sealing time: 2 seconds.

[0122] Next, for a pair of exterior packaging materials whose inner sealant layers had been heat-sealed together as described above, the exterior packaging materials (test specimens) were peeled at an angle of 90 degrees between the inner sealant layers of the sealed portions at a tensile speed of 100 mm / min using a Strograph (AGS-5kNX) manufactured by Shimadzu Access Co., Ltd. in accordance with JIS Z0238-1998, and the peel strength was measured, which was taken as the seal strength (N / 15 mm width).

[0123] A seal strength of 30 N / 15 mm width or more was rated as "◯" (pass), and a seal strength of less than 30 N / 15 mm width was rated as "×".

[0124] <Method for evaluating the cohesion of peeled interface> After measuring the above-mentioned seal strength (peel strength), both sides of the peeled portion (destroyed portion) of the inner sealant layer of the exterior material were visually observed, and the presence or absence and the degree of whitening on both sides of the peeled portion (destroyed portion) (the stronger the whitening, the greater the degree of cohesion) were evaluated based on the following criteria. (Judgment criteria) The samples in which significant whitening occurred and the degree of aggregation was high were marked with "◯", those in which some whitening occurred and the degree of aggregation was medium were marked with "Δ", and those in which no or almost no whitening was observed and the degree of aggregation was low were marked with "×".

[0125] <Laminate strength evaluation method> A test specimen measuring 15 mm wide x 150 mm long was cut out from the obtained exterior material, and the end of the test specimen in the longitudinal direction was immersed in an alkaline peeling solution to peel off the inner sealant layer 3 and the metal foil layer (aluminum foil layer) 4. In accordance with JIS K6854-3 (1999), a Shimadzu Strograph (AGS-5kNX) was used to clamp and fix a laminate including the metal foil layer (aluminum foil layer) 4 with one chuck, and the peeled sealant layer 3 was clamped and fixed with the other chuck, and the peel strength was measured when T-type peeling was performed in this state at a tensile speed of 100 mm / min, and this was taken as the laminate strength (adhesive strength) (N / 15 mm width) between the inner sealant layer 3 and the metal foil layer 4. The measurement of this peel strength was performed in a 25°C environment. Evaluation was based on the following criteria. (Judgment criteria) Those having a laminate strength of "5.0 N / 15 mm width" or more were rated "◯", and those having a laminate strength of less than "5.0 N / 15 mm width" were rated "X".

[0126] As is clear from Table 1, the exterior packaging materials for electrical storage devices of the present invention in Examples 1 to 11, which were constructed using the sealant film of the present invention, had excellent moldability, were less likely to produce white powder on the surface of the innermost layer of the exterior packaging material, and had sufficient laminate strength and sufficient seal strength.

[0127] In contrast, in Comparative Examples 1 to 10, which are outside the range specified by the present invention, sufficient laminate strength was not obtained. Furthermore, in Comparative Examples 2 and 8, the seal strength was also insufficient. Furthermore, in Comparative Examples 11 and 13, which are outside the range specified by the present invention, the moldability was poor, in Comparative Example 14, white powder was generated on the surface of the innermost layer, and in Comparative Example 12, white powder was generated on the surface of the innermost layer, and the seal strength and laminate strength were also insufficient. [Industrial Applicability]

[0128] Specific examples of the electrical storage device exterior material produced using the sealant film according to the present invention, the electrical storage device exterior material according to the present invention, and the electrical storage device exterior material obtained by the manufacturing method of the present invention include, for example, - Energy storage devices such as lithium secondary batteries (lithium ion batteries, lithium polymer batteries, etc.) Lithium-ion capacitor Electric double layer capacitor ·All-solid-state battery It is used as an exterior material for various electricity storage devices such as those mentioned above. [Explanation of symbols]

[0129] 1. Exterior materials for power storage devices 2...Heat-resistant resin layer (outer layer) 3...Inner sealant layer (sealant film) (inner layer) 4…Metal foil layer 5...Second adhesive layer (outer adhesive layer) 6...First adhesive layer (inner adhesive layer) 7...First non-oriented film layer (metal foil layer side) 7a…Surface of the inner sealant layer on the metal foil layer side 8...Second non-oriented film layer 8a…Surface of the innermost layer 9…Third non-oriented film layer 9a…Surface of the innermost layer 10...Outer case for power storage device (molded body)

Claims

1. An exterior material for an electricity storage device, comprising an inner sealant layer made of a sealant film and a metal foil layer laminated on one side of the inner sealant layer, The sealant film is composed of a laminate of two or more layers including a first non-stretched film layer and a second non-stretched film layer laminated on one surface of the first non-stretched film layer, the first non-oriented film layer is a layer of the sealant film disposed closest to the metal foil, the first unstretched film layer contains a random copolymer containing propylene and other copolymer components other than propylene as copolymer components, The first unstretched film layer does not contain a lubricant or contains more than 0 ppm to 250 ppm of a lubricant; The second unstretched film layer contains a propylene-based polymer and a lubricant, The packaging material for an electrical storage device, wherein the second unoriented film layer has a lubricant content of 2500 ppm to 5000 ppm.

2. An exterior material for an electricity storage device as described in claim 1, wherein the thickness of the first unstretched film layer / the thickness of the second unstretched film layer is in the range of 5-90 / 95-10.

3. An exterior material for an electricity storage device as described in claim 1 or 2, wherein the second unstretched film layer further contains an antiblocking agent.

4. The exterior material for an electricity storage device according to claim 1, wherein the amount of lubricant present on the surface of the second unoriented film layer is in the range of 0.1 μg / cm 2 to 1.0 μg / cm 2 .

5. An exterior material for an electricity storage device described in any one of claims 1 to 4, further comprising a heat-resistant resin layer as an outer layer laminated on the side of the metal foil layer opposite to the side on which the inner sealant layer is laminated.

6. An exterior case for an electricity storage device, comprising a molded body of the exterior material described in any one of claims 1 to 5.

7. A step of preparing a laminate in which a sealant film and a metal foil are laminated via a first adhesive; An aging step of heat-treating the laminate to obtain an exterior material for an electricity storage device, The sealant film is composed of a laminate of two or more layers including a first non-stretched film layer and a second non-stretched film layer laminated on one surface of the first non-stretched film layer, the first non-oriented film layer is a layer of the sealant film disposed closest to the metal foil, the first unstretched film layer contains a random copolymer containing propylene and other copolymer components other than propylene as copolymer components, The first unstretched film layer does not contain a lubricant or contains more than 0 ppm to 100 ppm of a lubricant; The second unstretched film layer contains a propylene-based polymer and a lubricant, The method for producing an exterior material for an electrical storage device, wherein the second unoriented film layer has a lubricant content of 2500 ppm to 5000 ppm.

8. A method for manufacturing an exterior material for an electricity storage device as described in claim 7, wherein the first adhesive is a thermosetting adhesive.

9. A process for preparing a laminate having a heat-resistant resin film laminated on one side of a metal foil via a second adhesive and a sealant film laminated on the other side of the metal foil via a first adhesive; An aging step of heat-treating the laminate to obtain an exterior material for an electricity storage device, the sealant film is composed of a laminate of two or more layers including a first non-stretched film layer and a second non-stretched film layer laminated on one surface of the first non-stretched film layer, the first non-stretched film layer being a layer disposed closest to the metal foil in the sealant film; the first unstretched film layer contains a random copolymer containing propylene and other copolymer components other than propylene as copolymer components, The first unstretched film layer does not contain a lubricant or contains more than 0 ppm to 100 ppm of a lubricant; The second unstretched film layer contains a propylene-based polymer and a lubricant, The method for producing an exterior material for an electrical storage device, wherein the second unoriented film layer has a lubricant content of 2500 ppm to 5000 ppm.

10. A method for manufacturing an exterior material for an electricity storage device as described in claim 9, wherein the first adhesive is a thermosetting adhesive and the second adhesive is a thermosetting adhesive.

11. The method for producing an exterior material for an electricity storage device according to claim 9 or 10, wherein the amount of lubricant present on the surface of the innermost layer of the exterior material for an electricity storage device obtained by heat treatment is in the range of 0.1 μg / cm 2 to 1.0 μg / cm 2 .

Citation Information

Patent Citations

  • Laminated material for secondary battery container and secondary battery container

    JP2003288865A

  • External facing material for secondary battery and secondary battery

    JP2013101764A

  • Packaging material for battery

    JP2014170720A

  • Packaging material for battery

    JP2014170721A

  • Outer casing material for electricity storage devices, electricity storage device and method for producing embossed outer casing material

    WO2015156327A1