Paste composition, semiconductor device and manufacturing method thereof, and electronic component and manufacturing method thereof

A silver-based paste composition with controlled crystallite growth allows low-temperature bonding in semiconductor devices, ensuring high adhesive strength and thermal resistance for reliable semiconductor and electronic components.

JP7583231B1Active Publication Date: 2024-11-13KYOCERA CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024551915
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-02-29
Publication Date
2024-11-13
Estimated Expiration
2044-02-29

AI Technical Summary

Technical Problem

Conventional pressurized sintered materials for bonding wide bandgap semiconductor devices require high temperatures, which can damage surrounding components and reduce connection reliability due to residual stress from thermal expansion, necessitating a low-temperature bonding solution with high adhesive strength and resistance to cooling/heating cycles.

Method used

A paste composition containing silver particles with specific size and crystallite diameter changes, along with a binder and solvent, allowing bonding at low temperatures (180-300°C and 1-30 MPa) with high adhesive strength and resistance to thermal cycling, achieved by optimizing silver particle sinterability through controlled crystallite growth.

Benefits of technology

The paste composition enables reliable bonding with high thermal conductivity and electrical conductivity, maintaining strong adhesion despite thermal cycles, suitable for semiconductor and electronic components in vehicles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583231000001
    Figure 0007583231000001
  • Figure 0007583231000002
    Figure 0007583231000002
Patent Text Reader

Abstract

Contains silver particles (A) and a binder (B), the content of silver particles (A1) having a particle diameter of more than 20 μm in 100% by mass of the silver particles (A) is 5% by mass or less, the content of the silver particles (A) is 95% by mass or more in 100% by mass of the total amount of the silver particles (A) and the binder (B), A paste composition having a rate of change represented by the following formula (1) of 250% or more. Rate of change = (S1 - S0) / S0 × 100(%) (1) [S0 is the crystallite size of the silver particles in the dried paste composition, as measured by Miller indices (111). S1 is the crystallite size, in Miller indices (111), of silver particles in a treated product obtained by subjecting the dried paste composition to a heating and pressurizing treatment at 15 MPa and 200° C. for 2 minutes in a nitrogen atmosphere.]
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a paste composition, a semiconductor device and a method for manufacturing the same, and an electronic component and a method for manufacturing the same. [Background technology]

[0002] In recent years, power semiconductor devices using wide band gap semiconductor elements such as silicon carbide (SiC) and gallium nitride (GaN) with low power loss have been actively developed. In such power semiconductor devices, the wide band gap semiconductor elements are bonded to other members such as a semiconductor support member by a bonding member made of a bonding material. The wide band gap semiconductor element has a characteristic that the element itself has high heat resistance and can operate at high temperatures of 250°C or more with a large current. This characteristic is exhibited by sufficient dissipation of heat generated by the element during operation. Therefore, there is a demand for a bonding material that has excellent long-term high-temperature resistance in addition to electrical conductivity and heat transfer.

[0003] Sintering materials are increasingly being used as joining materials. Sintering materials are paste compositions containing fine metal particles. The fine metal particles are sintered at temperatures significantly lower than the melting point of the metal itself, and after sintering, they can acquire thermal conductivity and heat resistance equivalent to those of bulk metals.

[0004] Sintered materials are classified into non-pressure type and pressure type depending on the joining process. Non-pressure type uses heat but no pressure during joining. Pressure type uses heat and pressure simultaneously during joining. Among these, the pressurized type is used in fields that require high connection reliability, such as automobiles (vehicle inverters, etc.) This is because the pressure applied during joining forms a dense sintered body, which provides high connection reliability. Conventional pressure-type sintering materials are generally heated to high temperatures of 250°C or higher during bonding, but there are concerns that high-temperature heating can damage surrounding components and that residual stress resulting from thermal expansion can reduce connection reliability. For these reasons, there is a demand for pressure-type sintering materials that can be bonded at low temperatures. For example, Patent Document 1 describes a technique in which pressure bonding is performed at a low bonding temperature of 200° C. by focusing on the change in crystallite size before and after heat treatment. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2020-136580 A Summary of the Invention [Means for solving the problem]

[0006] The present disclosure relates to the following [1] to

[11] .

[0007] [1] A composition comprising silver particles (A) and a binder (B); the content of silver particles (A1) having a particle diameter of more than 20 μm in 100% by mass of the silver particles (A) is 5% by mass or less, the content of the silver particles (A) is 95% by mass or more in 100% by mass of the total amount of the silver particles (A) and the binder (B), A paste composition having a rate of change represented by the following formula (1) of 250% or more. Rate of change = (S1 - S0) / S0 × 100(%) (1) [S0 is the crystallite size of the silver particles in the dried paste composition, as measured by Miller indices (111). S1 is the crystallite size, in Miller indices (111), of silver particles in a treated product obtained by subjecting the dried paste composition to a heating and pressurizing treatment at 15 MPa and 200° C. for 2 minutes in a nitrogen atmosphere.] [2] The paste composition according to the above [1], wherein the content of silver particles (A2) having a particle diameter of 1.0 to 20 μm in 100 mass% of the silver particles (A) is 50 mass% or less. [3] The paste composition according to the above [1] or [2], wherein the content of silver particles (A3) having a particle diameter of less than 1.0 μm in 100 mass% of the silver particles (A) is 50 mass% or more. [4] The specific surface area of ​​the silver particles (A) is 1.4 m 2 The paste composition according to any one of the above [1] to [3], wherein the viscosity is 100% or more. [5] The paste composition according to any one of the above [1] to [4], wherein the binder (B) contains one or more resins selected from a thermosetting resin and a thermoplastic resin. [6] The paste composition according to any one of the above [1] to [5], wherein the 5% weight loss temperature of the binder (B) is 250° C. or higher. [7] A solvent (C) is included, The paste composition according to any one of the above-mentioned [1] to [6], wherein the content of the solvent (C) is 10 to 30 mass% in the total amount of the silver particles (A), the binder (B), and the solvent (C) being 100 mass%. [8] A semiconductor device having a joint formed from the paste composition according to any one of [1] to [7] above. [9] A method for manufacturing a semiconductor device including a semiconductor element and a semiconductor support member, comprising the steps of: A step of applying the paste composition according to any one of the above [1] to [7] onto the semiconductor support member; mounting the semiconductor element on the paste composition; and a step of bonding the semiconductor element and the semiconductor support member under heat and pressure, The method for producing a semiconductor device, wherein the heat and pressure bonding is performed under conditions of 180 to 300° C. and 1 to 30 MPa for 0.5 to 10 minutes.

[10] An electronic component having a joint formed from the paste composition according to any one of [1] to [7] above.

[11] A method for producing an electronic component, comprising a step of forming a joint using the paste composition according to any one of [1] to [7] above. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The bonding method described in Patent Document 1 has a threshold adhesive strength, which is an evaluation standard for sinterability, of 20 MPa, and it is difficult to say that the bonding method has sufficient bondability. The present disclosure has an object to provide a paste composition that has high coatability and is capable of achieving bonding with high adhesive strength through heating and pressurizing at low temperatures and that is less susceptible to peeling due to thermal cycles, as well as a semiconductor device and a manufacturing method thereof that use the paste composition, and an electronic component and a manufacturing method thereof. The present inventors have focused on the change in crystallite size of silver particles when heated and pressurized, and have found that by selecting silver particles that have good sinterability in the pressurizing step, it is possible to provide a paste composition that has high coatability and can achieve bonding by heating and pressurizing at low temperatures, with high adhesive strength and little peeling due to thermal cycles, as well as a semiconductor device and a method for manufacturing the same that use the paste composition, and an electronic component and a method for manufacturing the same. According to the present disclosure, it is possible to provide a paste composition that has high coatability and that can perform bonding by heating and pressurizing at low temperatures, which has high adhesive strength and is unlikely to peel due to thermal cycles, as well as a semiconductor device and a manufacturing method thereof, and an electronic component and a manufacturing method thereof, which use the paste composition.

[0009] Hereinafter, embodiments of the present disclosure will be described in detail. In the following description, the description of "A to B" indicating a numerical range means "A or more and B or less," including the endpoints, and when describing "may be A to B, may be C to D, or may be E to F," the upper and lower limits can be combined in any way. In addition, in the numerical ranges described in this specification, the upper or lower limit of the numerical range may be replaced with a value shown in the examples.

[0010] [Paste composition] The paste composition of the present disclosure comprises silver particles (A) and a binder (B), in which the content of silver particles (A1) having a particle diameter of more than 20 μm in 100 mass% of the silver particles (A) is 5 mass% or less, the content of the silver particles (A) in 100 mass% of the total amount of the silver particles (A) and the binder (B) is 95 mass% or more, and a rate of change represented by the following formula (1) is 250% or more. Rate of change = (S1 - S0) / S0 × 100(%) (1) Here, S0 is the crystallite size, in Miller indices (111), of the silver particles in the dried paste composition. S1 is the crystallite size, in Miller indices (111), of silver particles in a treated product obtained by subjecting the dried paste composition to a heating and pressurizing treatment at 15 MPa and 200° C. for 2 minutes in a nitrogen atmosphere.

[0011] The paste composition of the present disclosure has good coatability, is capable of pressure bonding at low temperatures, and has high adhesive strength. The details of the reason for this are unknown, but it is speculated to be as follows. That is, crystal growth progresses inside the particles and also progresses by sintering between the particles. It is considered that the greater the degree of progress of the crystal growth, the greater the progress of sintering. In general, the smaller the crystallite diameter, the easier the crystals grow, but it is considered that the degree of crystal growth varies depending on the shape and size of the particles and the treatment conditions. In silver particles with a large rate of change in crystallite diameter due to treatment assuming a bonding process (heating and pressurizing at 15 MPa and 200°C for 2 minutes in a nitrogen atmosphere), the silver particles are densely packed together under the conditions and the frequency of contact is also high, so sintering is likely to progress. In other words, if the rate of change {((S1-S0) / S0)×100} of silver particles (A) is 250% or more, it can exhibit good sinterability during heating and pressurizing treatment at low temperatures. As described above, the silver particles (A) exhibit good sinterability during heating and pressurizing treatment at low temperatures, and therefore have high bonding performance. This allows the content of the binder (B) contained for bonding to be reduced. That is, the paste composition of the present disclosure has a content of silver particles (A) of 95% by mass or more in 100% by mass of the total amount of silver particles (A) and binder (B). As described above, the paste composition of the present disclosure has a high content of silver particles (A), and therefore can form a bonded portion that has high thermal conductivity and electrical conductivity in addition to high bonding strength.

[0012] <Silver particles (A)> The silver particles (A) have a rate of change represented by the following formula (1) of 250% or more. Rate of change = (S1 - S0) / S0 × 100(%) (1) Here, S0 is the crystallite size, in Miller index (111), of silver particles in the dried paste composition, and S1 is the crystallite size, in Miller index (111), of silver particles in a treated product obtained by subjecting the dried paste composition to a heating and pressurizing treatment at 15 MPa and 200°C for 2 minutes in a nitrogen atmosphere.

[0013] When the rate of change {((S1-S0) / S0)×100} is 250% or more, a paste composition can be obtained that can perform bonding by heating and pressurizing at low temperatures with high adhesive strength and withstands thermal cycles. There is no particular upper limit to the rate of change {((S1-S0) / S0)×100}, but it may be 500% or less from the viewpoint of reducing structural changes in the sintered layer due to thermal history after bonding. From this viewpoint, the rate of change {((S1-S0) / S0)×100} may be 255 to 475%, 270 to 450%, 285 to 425%, or 300 to 400%.

[0014] The silver particles (A) may have a crystallite size S0 of 30 to 70 nm. When in this range, crystals tend to grow easily when heated and pressurized, and sintering tends to proceed easily. From this viewpoint, the crystallite size S0 may be 40 to 60 nm. The crystallite size S0 can be measured as follows. The silver particles (A) in the dried paste composition are pressed into a cake. The crystallite size S0 can be calculated by applying the cake onto a glass plate, and calculating the crystallite size S0 from the Miller index (111) plane peak by the Scherrer formula using a focusing method with a CuKα ray source using an X-ray diffractometer. Specifically, it can be obtained by the method described in the Examples.

[0015] The silver particles (A) may have a crystallite size S1 of 105 to 420 nm. When the crystallite size S1 is 105 nm or more, structural changes in the sintered layer after bonding can be reduced. When the crystallite size S1 is 420 nm or less, stress generated inside the sintered layer can be reduced. From this viewpoint, the crystallite size S1 may be from 120 to 400 nm, from 130 to 350 nm, or from 140 to 300 nm. The crystallite size S1 can be measured as follows. The silver particles (A) in the dried paste composition are pressed into a cake. The sintered body is obtained by heating the cake to 200°C at a temperature increase rate of 60°C / min under a nitrogen atmosphere while applying a pressure of 15 MPa, heating and pressurizing the cake at 15 MPa and 200°C for 2 minutes, and then cooling the cake to room temperature (25°C) at a temperature decrease rate of 110°C / min. The powder is obtained by pulverizing the sintered body in a mortar. The crystallite size S1 can be calculated by applying the powder to glass, and calculating the Miller index (111) plane peak from the Scherrer formula using an X-ray diffractometer by a focusing method with CuKα radiation as a radiation source. Specifically, it can be obtained by the method described in the Examples.

[0016] The rate of change {((S1-S0) / S0) × 100} tends to be improved by, for example, setting the particle size of silver particles (A) within the range described below and setting the crystallite size S0 of silver particles (A) within the range described below. The rate of change of silver particles {((S1-S0) / S0) x 100} can be easily measured by the above-mentioned method for measuring S0 and S1.

[0017] The average particle size of the silver particles (A) may be 0.62 to 5.0 μm. When the average particle size is 0.62 μm or more, the silver particles come into contact with each other more frequently when pressure is applied, improving sinterability. When the average particle size is 5.0 μm or less, damage to a semiconductor element or a substrate when pressure is applied can be reduced. In addition, when the average particle size of the silver particles (A) is 0.62 to 5.0 μm, the aforementioned rate of change {((S1-S0) / S0)×100} tends to be high. From this viewpoint, the average particle size of the silver particles (A) may be 0.65 to 3.0 μm, or may be 2.0 μm or less, or may be 1.75 μm or less.

[0018] The shape of the silver particles (A) is not particularly limited, and examples thereof include a spherical shape, a flake shape, etc. The shape of the silver particles (A) may be spherical. The silver particles (A) may be primary particles, or secondary particles formed by agglomeration of primary particles. The silver particles (A) may be hollow or solid, but may be hollow from the viewpoint of low-temperature sintering. Here, the hollow particles refer to particles having voids inside. When the silver particles (A) are hollow, voids may be present in the center of the silver particles. The solid particles refer to particles having substantially no space inside.

[0019] The specific surface area of ​​silver particles (A) determined by the BET method is 1.4 m 2 / g or more. The specific surface area may be 1.4 m 2 When the specific surface area is 2.0 m / g or more, the contact between the silver particles can be increased, and the proportion of highly active silver atoms on the particle surface can be increased. 2 / g or less. 2 When the silver content is 1 / g or less, the viscosity of the paste composition can be reduced, and aggregation of silver particles can be reduced. From this viewpoint, the specific surface area is 1.5 to 1.95 m 2 / g. The specific surface area of ​​the silver particles (A) can be measured by a BET single-point method using nitrogen adsorption with a specific surface area measuring device, and specifically, it can be measured by the method described in the Examples.

[0020] The content of the silver particles (A) is 95% by mass or more in the total amount (100% by mass) of the silver particles (A) and the binder (B). When the content is 95% by mass or more, it is possible to obtain a paste composition that can perform bonding by heating and pressurizing at a low temperature with high adhesive strength and that is unlikely to peel off due to thermal cycles. The content of the silver particles (A) may be 99% by mass or less in the total amount (100% by mass) of the silver particles (A) and the binder (B). When the content is 99% by mass or less, the function of the binder (B) is sufficiently exhibited, and a paste composition having high coatability and capable of reducing structural changes in the sintered layer due to thermal history after bonding can be obtained. From this viewpoint, the content may be 95 to 99 mass %, may be 95.5 to 98.7 mass %, or may be 96 to 98.5 mass %.

[0021] From the viewpoint of sinterability, the silver content in the paste composition, based on the total amount of metals present in the composition (100% by mass), may be 60% by mass or more, 80% by mass or more, 90% by mass or more, 95% by mass or more, or 99% by mass or more, and the paste composition may not contain any metals other than silver.

[0022] <<Silver particles (A1)>> In the present disclosure, the content of silver particles (A1) having a particle size of more than 20 μm is 5 mass% or less in 100 mass% of silver particles (A). The content of the silver particles (A1) may be 0 mass%. When the content is 5% by mass or less, no squeegee marks are left during printing application, and a pressure load can be uniformly applied to the bonding layer. Therefore, when the content is 5% by mass or less, a paste composition can be obtained that has high coatability, and can perform bonding by heating and pressurizing at low temperatures, with high adhesive strength and little peeling due to thermal cycles. From this viewpoint, the content may be 2.5 mass % or less, 1.5 mass % or less, or 1.0 mass % or less.

[0023] <<Silver particles (A2)>> In the present disclosure, the content of silver particles (A2) having a particle diameter of 1.0 to 20 μm in 100 mass% of silver particles (A) may be 50 mass% or less. When the content is 50% by mass or less, a uniform silver sintered layer can be formed. The content may be 5% by mass or more. When the content is 5% by mass or more, the frequency of contact between silver particles can be improved. From this viewpoint, the content may be 8 to 45% by mass, 10 to 40% by mass, or 15 to 36% by mass.

[0024] <<Silver particles (A3)>> In the present disclosure, the content of silver particles (A3) having a particle diameter of less than 1.0 μm in 100 mass% of silver particles (A) may be 50 mass% or more. When the content is 50% by mass or more, a uniform silver sintered layer can be formed. The content may be 95% by mass or less. When the content is 95% by mass or less, the frequency of contact between silver particles can be improved. From this viewpoint, the content may be 55 to 92 mass %, 60 to 90 mass %, or 64 to 85 mass %.

[0025] (Method of producing silver particles (A)) The method for producing silver particles (A) includes the steps of adding ammonia water to an aqueous solution containing a silver compound to obtain a silver ammine complex solution, and reducing the silver ammine complex in the silver ammine complex solution obtained in the above step with a reducing compound to obtain a silver particle-containing slurry.

[0026] (Step of Obtaining Silver Ammine Complex Solution) In this step, aqueous ammonia is added to an aqueous solution containing a silver compound to obtain a silver ammine complex solution. Examples of the silver compound include silver nitrate, silver chloride, silver acetate, silver oxalate, silver oxide, etc. From the viewpoint of solubility in water, the silver compound may be silver nitrate or silver acetate.

[0027] The amount of ammonia added may be 2 to 50 mol, 5 mol or more, or 10 mol or more per mol of silver in the aqueous solution containing the silver compound. When the amount of ammonia added is within the above range, the average particle size of the primary particles can be set within the above range.

[0028] (Step of obtaining silver particle-containing slurry) In this step, the silver ammine complex in the silver ammine complex solution obtained in the previous step is reduced with a reducing compound to obtain a silver particle-containing slurry. By reducing the silver ammine complex with a reducing compound, the primary particles of the silver particles in the silver ammine complex are aggregated to form secondary particles (hollow particles) having a void in the center.

[0029] By appropriately adjusting the amount of silver in the silver ammine complex and the content of the reducing compound, it is possible to control the aggregation of the primary particles and to set the average particle size of the obtained secondary particles within the above-mentioned range.

[0030] The reducing compound is not particularly limited as long as it has the reducing power to reduce the silver ammine complex and precipitate silver. Examples of the reducing compound include hydrazine derivatives. Examples of hydrazine derivatives include hydrazine monohydrate, methylhydrazine, ethylhydrazine, n-propylhydrazine, i-propylhydrazine, n-butylhydrazine, i-butylhydrazine, sec-butylhydrazine, t-butylhydrazine, n-pentylhydrazine, i-pentylhydrazine, neo-pentylhydrazine, t-pentylhydrazine, n-hexylhydrazine, i-hexylhydrazine, n-heptylhydrazine, n-octylhydrazine, n-nonylhydrazine, n-decylhydrazine, n-undecylhydrazine, n-dodecylhydrazine, cyclohexylhydrazine, phenylhydrazine, 4-methylphenylhydrazine, benzylhydrazine, 2-phenylethylhydrazine, 2-hydrazinoethanol, acetohydrazine, etc. These may be used alone or in combination of two or more.

[0031] The content of the reducing compound may be 0.25 to 20.0 mol per mol of silver in the silver ammine complex, or may be 10.0 mol or less, or may be 5.0 mol or less. When the content of the reducing compound is within the above range, the average particle size of the obtained secondary particles can be within the above range.

[0032] Furthermore, the temperature of the silver ammine complex solution when reducing the silver ammine complex may be less than 30° C., or may be 0 to 20° C. If the temperature of the silver ammine complex solution is within this range, the aggregation of the primary particles can be controlled, and the average particle size of the obtained secondary particles can be within the above-mentioned range.

[0033] <Binder (B)> The binder (B) may contain one or more resins selected from thermosetting resins and thermoplastic resins.

[0034] <<Thermosetting resin>> The thermosetting resin can be any thermosetting resin that is generally used for adhesive applications, without any particular limitations. The thermosetting resin may be a resin that is liquid at room temperature (25°C), or a resin that becomes a paste when diluted with a solvent or the like. The thermosetting resin may include at least one selected from cyanate resins, epoxy resins, acrylic resins, and maleimide resins. These may be used alone, or two or more may be used in combination.

[0035] Cyanate resins are compounds that have an -NCO group in the molecule, and the -NCO group reacts when heated. Specific examples include 1,3-dicyanatobenzene, 1,4-dicyanatobenzene, 1,3,5-tricyanatobenzene, 1,3-dicyanatonaphthalene, 1,4-dicyanatonaphthalene, 1,6-dicyanatonaphthalene, 1,8-dicyanatonaphthalene, 2,6-dicyanatonaphthalene, 2,7-dicyanatonaphthalene, 1,3,6-tricyanatonaphthalene, 4,4'-dicyanatobiphenyl, bis(4-cyanatophenyl)methane, bis(3,5-dimethyl-4-cyanatophenyl)methane, and bis(2,3-dimethyl-4-cyanatophenyl)methane. Examples of the cyanates include 2,2-bis(4-cyanatophenyl)methane, 2,2-bis(4-cyanatophenyl)propane, 2,2-bis(3,5-dibromo-4-cyanatophenyl)propane, bis(4-cyanatophenyl)ether, bis(4-cyanatophenyl)thioether, bis(4-cyanatophenyl)sulfone, tris(4-cyanatophenyl)phosphite, tris(4-cyanatophenyl)phosphate, and cyanates obtained by reacting novolak resin with cyanogen halide. Also usable are prepolymers having a triazine ring formed by trimerizing the cyanate groups of these polyfunctional cyanate resins. The prepolymers are obtained by polymerizing the above polyfunctional cyanate resin monomers using, for example, acids such as mineral acids and Lewis acids, bases such as sodium alcoholates and tertiary amines, and salts such as sodium carbonate as catalysts.

[0036] As the curing accelerator for the cyanate resin, generally known ones can be used. For example, organometallic complexes such as zinc octylate, tin octylate, cobalt naphthenate, zinc naphthenate, and iron acetylacetonate; metal salts such as aluminum chloride, tin chloride, and zinc chloride; and amines such as triethylamine and dimethylbenzylamine, but are not limited thereto. These curing accelerators can be used alone or in combination of two or more.

[0037] An epoxy resin is a compound having one or more glycidyl groups in a molecule, and the glycidyl group reacts by heating. The epoxy resin may be a compound having two or more glycidyl groups in one molecule. For example, bifunctional epoxy resins obtained by epoxidizing bisphenol compounds such as bisphenol A, bisphenol F, biphenol, or derivatives thereof; diols having an alicyclic structure such as hydrogenated bisphenol A, hydrogenated bisphenol F, hydrogenated biphenol, cyclohexanediol, cyclohexanedimethanol, cyclohexanediethanol, or derivatives thereof; aliphatic diols such as butanediol, hexanediol, octanediol, nonanediol, decanediol, or derivatives thereof; trifunctional epoxy resins obtained by epoxidizing compounds having a trihydroxyphenylmethane skeleton or an aminophenol skeleton; polyfunctional epoxy resins obtained by epoxidizing phenol novolac resins, cresol novolac resins, phenol aralkyl resins, biphenyl aralkyl resins, naphthol aralkyl resins, polybutadiene, etc., but are not limited thereto. The epoxy resin may be liquid at room temperature (25°C) either alone or as a mixture. It is a compound containing one glycidyl group in one molecule, and can be used as a reactive diluent as is commonly used. Examples of reactive diluents include monofunctional aromatic glycidyl ethers such as phenyl glycidyl ether and cresyl glycidyl ether, and aliphatic glycidyl ethers.

[0038] Examples of the curing agent for the epoxy resin include aliphatic amines, aromatic amines, dicyandiamide, dihydrazide compounds, acid anhydrides, phenolic resins, and organic peroxides. Examples of the dihydrazide compound include carboxylic acid dihydrazides such as adipic acid dihydrazide, dodecanoic acid dihydrazide, isophthalic acid dihydrazide, and p-oxybenzoic acid dihydrazide. Examples of the acid anhydride include phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, endomethylenetetrahydrophthalic anhydride, dodecenylsuccinic anhydride, a reaction product of maleic anhydride and polybutadiene, and a copolymer of maleic anhydride and styrene. Examples of organic peroxides include hydroperoxides, dialkyl peroxides, dicumyl peroxide, benzoyl peroxide, lauroyl peroxide, acetyl peroxide, acyl peroxides, and peroxyketals such as cumene peroxide, 1,1-di-t-butylperoxycyclohexane, and peroxyesters such as t-butyl peroxybenzoate, as well as so-called room temperature curing organic peroxides, for example, methyl ethyl ketone peroxide.

[0039] Furthermore, a curing accelerator can be added to accelerate curing. Examples of the curing accelerator for epoxy resin include imidazoles, triphenylphosphine or tetraphenylphosphine and their salts, and amine compounds such as diazabicycloundecene and their salts. Examples of the curing accelerator include 2-methylimidazole, 2-ethylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 2-C 11 H 23 The imidazole compound may be an imidazole compound such as 2-imidazole, an adduct of 2-methylimidazole and 2,4-diamino-6-vinyltriazine, etc. The imidazole compound may have a melting point of 180° C. or higher.

[0040] Examples of acrylic resins include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 1,2-cyclohexanediol mono(meth)acrylate, 1,3-cyclohexanediol mono(meth)acrylate, 1,4-cyclohexanediol mono(meth)acrylate, 1,2-cyclohexanedimethanol mono(meth)acrylate, 1,3-cyclohexanedimethanol mono(meth)acrylate, 1,4-cyclohexanedimethanol mono(meth)acrylate, 1,2-cyclohexanediethanol mono(meth)acrylate, Examples of the hydroxyl group-containing (meth)acrylate include (meth)acrylates having a hydroxyl group such as tert-butyl ether mono(meth)acrylate, 1,3-cyclohexanediethanol mono(meth)acrylate, 1,4-cyclohexanediethanol mono(meth)acrylate, glycerin mono(meth)acrylate, glycerin di(meth)acrylate, trimethylolpropane mono(meth)acrylate, trimethylolpropane di(meth)acrylate, pentaerythritol mono(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, and neopentyl glycol mono(meth)acrylate, as well as (meth)acrylates having a carboxyl group obtained by reacting these hydroxyl group-containing (meth)acrylates with dicarboxylic acid or a derivative thereof. Examples of dicarboxylic acids that can be used herein include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, maleic acid, fumaric acid, phthalic acid, tetrahydrophthalic acid, hexahydrophthalic acid, and derivatives thereof.

[0041] Examples of the acrylic resin include polyethers, polyesters, polycarbonates, and poly(meth)acrylates having a molecular weight of 100 to 10,000, which are compounds having a (meth)acrylic group; (meth)acrylates having a hydroxy group; and (meth)acrylamides having a hydroxy group.

[0042] The maleimide resin is a compound containing one or more maleimide groups in one molecule, and the maleimide groups react when heated. Examples of the maleimide resin include bismaleimide resins such as N,N'-(4,4'-diphenylmethane)bismaleimide, bis(3-ethyl-5-methyl-4-maleimidophenyl)methane, and 2,2-bis[4-(4-maleimidophenoxy)phenyl]propane. The maleimide resin may be a compound obtained by the reaction of dimer acid diamine with maleic anhydride; or a compound obtained by the reaction of maleimide amino acid such as maleimide acetic acid or maleimide caproic acid with a polyol. The maleimide amino acid is obtained by reacting maleic anhydride with amino acetic acid or amino caproic acid. The polyol may be polyether polyol, polyester polyol, polycarbonate polyol, or poly(meth)acrylate polyol, or may not contain an aromatic ring.

[0043] <<Thermoplastic resin>> The thermoplastic resin can be any thermoplastic resin that is generally used for adhesive applications, without any particular limitations. Examples include acrylic resins, methacrylic resins, vinyl resins, carbonate resins, cellulose, polyolefin resins, ethylene-vinyl acetate copolymers, and polyamide resins. At least one selected from the thermoplastic resins listed above may be included. These may be used alone, or two or more may be used in combination.

[0044] The content of the binder (B) is 5.0% by mass or less in the total amount (100% by mass) of the silver particles (A) and the binder (B). When the content is 5.0% by mass or less, it is possible to fill voids in the structure formed by silver sintering without inhibiting the sintering of the silver particles. The content of the binder (B) may be 0.1% by mass or more in the total amount (100% by mass) of the silver particles (A) and the binder (B). When the content is 0.1% by mass or more, the resin fills the voids in the structure formed by silver sintering, thereby making it possible to relieve the stress applied to the sintered layer. From this viewpoint, the content may be 0.1 to 5.0 mass%, 0.5 to 4.8 mass%, 1.0 to 4.5 mass%, or 1.5 to 4.0 mass%.

[0045] <<Physical properties etc.>> The 5% weight loss temperature of the binder (B) may be 250° C. or higher. If the temperature is 250° C. or higher, the thermal decomposition of the resin during bonding can be reduced. There is no particular upper limit to the 5% weight loss temperature of the binder (B), but it may be 450° C. or lower in terms of the availability of the binder, compatibility with the solvent, and the like. From this viewpoint, the 5% by mass weight loss temperature of the binder (B) may be 250 to 450°C, 300 to 425°C, or 350 to 400°C. The 5% weight loss temperature of the binder (B) can be measured by a thermogravimetric and differential thermal analyzer, specifically, by the method described in the examples.

[0046] <Solvent (C)> From the viewpoint of workability, the paste composition of the present disclosure may further contain a solvent (C). Examples of the solvent (C) include butyl carbitol, cellosolve acetate, ethyl cellosolve, butyl cellosolve, butyl cellosolve acetate, butyl carbitol acetate, diethylene glycol dimethyl ether, diacetone alcohol, N-methyl-2-pyrrolidone (NMP), dimethylformamide, N,N-dimethylacetamide (DMAc), γ-butyrolactone, 1,3-dimethyl-2-imidazolidinone, 3,5-dimethyl-1-adamantanamine (DMA), and terpene ethers such as dihydroterpinyloxyethanol. These may be used alone or in combination of two or more.

[0047] When the paste composition of the present disclosure contains a solvent (C), the content of the solvent (C) in 100% by mass of the paste composition may be 5 to 50% by mass. When the content is 5% by mass or more, good coatability can be imparted. When the content is 50% by mass or less, it is possible to reduce settling of silver particles when the paste composition is allowed to stand, and the pot life is improved. From this viewpoint, the content may be 10 to 40% by mass, 12 to 30% by mass, or 15 to 25% by mass.

[0048] When the paste composition of the present disclosure contains a solvent (C), the content of the solvent (C) in the total amount of the silver particles (A), the binder (B), and the solvent (C) (100% by mass) may be 10 to 30% by mass. When the content is 10% by mass or more, good coatability can be imparted, and when the content is 30% by mass or less, sedimentation of silver particles when the paste composition is left to stand can be reduced, and the usable time can be improved. From this viewpoint, the content may be 12 to 25% by mass.

[0049] <Other ingredients> In addition to the above components, the paste composition of the present disclosure may contain various additives, such as stress reducing agents such as rubber and silicone, coupling agents, antifoaming agents, surfactants, colorants such as pigments and dyes, various polymerization inhibitors, antioxidants, solvents, fluxing agents, and other additives that are generally blended in this type of composition, as necessary. Each of these additives may be used alone or in combination of two or more. The paste composition of the present disclosure may or may not contain a resin containing an aromatic amine skeleton.

[0050] The total content of the silver particles (A), binder (B), and solvent (C) in 100 mass% of the paste composition of the present disclosure may be 80 to 100 mass%, 90 to 99.95 mass%, or 95 to 99.9 mass%. The total content of the silver particles (A) and the binder (B) in 100% by mass of the solid content of the paste composition of the present disclosure may be 80 to 100% by mass, 90 to 100% by mass, or 95 to 99.9% by mass. The solid content here refers to the components remaining after excluding the solvent (C) from the paste composition.

[0051] The paste composition of the present disclosure can be prepared by thoroughly mixing the above-mentioned silver particles (A), binder (B), solvent (C) which is contained as necessary, and various additives, followed by a kneading treatment using a disperse, kneader, three-roll mill, or the like, and then degassing.

[0052] <Physical properties of paste composition> (viscosity) From the viewpoint of coatability, the viscosity of the paste composition of the present disclosure may be 1 to 200 Pa·s, 10 to 100 Pa·s, 12 to 50 Pa·s, or 15 to 25 Pa·s. The viscosity is a value measured using an E-type viscometer (3° cone) at 25° C. and a rotation speed of 2.0 rpm. Specifically, it can be measured by the method described in the examples.

[0053] (Thixotropy index) The thixotropic index of the paste composition of the present disclosure may be 1-20, 2-10, or 3.5-7, from the viewpoint of coatability. The above thixotropy index was measured using an E-type viscometer (3°) at a temperature of 25°C and a rotation speed of 2.0 rpm (V 2.0 ) and viscosity at 20 rpm (V 20 ) and measure the viscosity ratio (V 2.0 / V 20 Specifically, it can be measured by the method described in the Examples.

[0054] (shear strength) The shear strength of the cured product of the paste composition of the present disclosure may be 80 MPa or more. If it is 80 MPa or more, bonding can be performed by heating and pressurizing at a low temperature, with high adhesive strength and resistance to peeling due to thermal cycles. From this viewpoint, the shear strength of the cured product of the paste composition may be 85 MPa or more, 90 MPa or more, or 92 MPa or more. The shear strength of the cured product of the paste composition can be measured by applying the paste composition to a copper frame, mounting a backside gold chip with a gold vapor deposition layer on a 2 mm x 2 mm bonding surface, and curing the paste composition under heat and pressure at 200°C and 15 MPa for 2 minutes, and then measuring the hot die shear strength at 260°C using a mount strength measuring device. Specifically, the measurement can be performed by the method described in the Examples.

[0055] (Volume resistivity) The volume resistivity of the cured product of the paste composition of the present disclosure may be 4.0 μΩ·cm or less. When the volume resistivity is 4.0 μΩ·cm or less, resistance heating at the joints can be reduced. From this viewpoint, the volume resistivity of a cured product of the paste composition may be 3.5 μΩ·cm or less, 3.4 μΩ·cm or less, or 3.0 μΩ·cm or less. The volume resistivity of the cured product of the paste composition can be measured by applying the paste composition to a glass substrate to a thickness of 30 μm, drying, and curing the resulting wiring at 200° C. and 15 MPa for 2 minutes, and measuring the electrical resistivity of the wiring using a resistivity meter by a four-terminal method. Specifically, the measurement can be performed by the method described in the Examples.

[0056] [Semiconductor device and its manufacturing method] The semiconductor device of the present disclosure has a joint formed by the above-mentioned paste composition. Since the semiconductor device of the present disclosure has a joint formed by the above-mentioned paste composition, it is possible to provide a semiconductor device for an in-vehicle component with good heat dissipation properties and connection reliability. The semiconductor device may have a semiconductor element, a substrate, and a joint that joins the semiconductor element and the substrate, The joint is formed from the paste composition described above.

[0057] The method for manufacturing a semiconductor device according to the present disclosure is a method for manufacturing a semiconductor device including a semiconductor element and a semiconductor support member, the method including the steps of applying the paste composition to the semiconductor support member, mounting the semiconductor element on the paste composition, and bonding the semiconductor element and the semiconductor support member under heat and pressure, the heat and pressure bonding being performed under conditions of 180 to 300°C and 1 to 30 MPa for 0.5 to 10 minutes.

[0058] When the heating temperature in the heat and pressure bonding is 180° C. or higher, sintering proceeds sufficiently and the bonding strength of the bonded portion is improved. When the heating temperature is 300° C. or lower, thermal deterioration of members such as the semiconductor element and the semiconductor support member is reduced. From this viewpoint, the heating temperature may be 180 to 300°C, 185 to 250°C, or 190 to 210°C.

[0059] When the pressure in the heat and pressure bonding is 1 MPa or more, sintering proceeds sufficiently and the bonding strength of the bonded portion is improved, and when the pressure is 30 MPa or less, damage to members such as the semiconductor element and the semiconductor support member due to pressure is reduced. From this viewpoint, the pressure may be from 1 to 30 MPa, may be from 5 to 25 MPa, or may be from 10 to 20 MPa.

[0060] The semiconductor element may be a known semiconductor element, such as a transistor or a diode. The semiconductor element may further include a light-emitting element such as an LED. The type of the light-emitting element is not particularly limited, and may include, for example, a light-emitting layer formed of a nitride semiconductor such as InN, AlN, GaN, InGaN, AlGaN, or InGaAlN on a substrate by MOCVD (metal organic chemical vapor deposition) or the like. Examples of the semiconductor support member include support members made of materials such as copper, copper-plated copper, PPF (preplating lead frame), glass epoxy, and ceramics.

[0061] By using the die attach material of this embodiment, the semiconductor element can be bonded to a base material that is not metal plated. The semiconductor device thus obtained has improved connection reliability against temperature cycles after mounting compared to conventional devices. In addition, since the electrical resistance is sufficiently small and changes little over time, there is an advantage in that the output does not decrease much over time even when driven for a long time, resulting in a long life.

[0062] [Electronic components and their manufacturing methods] The electronic component of the present disclosure has a joint formed by the above-mentioned paste composition. Since the electronic component of the present disclosure has a joint formed by the above-mentioned paste composition, it is possible to provide an electronic component for use in an automobile, which has good heat dissipation properties and connection reliability. The electronic component may have an electronic element, a substrate, and a joint that joins the electronic element and the substrate. The joint is formed from the paste composition described above. The method for producing an electronic component according to the present disclosure includes a step of forming a joint using the above-described paste composition. EXAMPLES

[0063] Next, the present disclosure will be described in detail by showing examples, but the present disclosure is not limited to these examples.

[0064] The raw materials used were those shown in Table 1 and below.

[0065] (1) Silver particles

[0066] [Table 1]

[0067] (2) Binder (resin) jER1009 (Bisphenol A type solid epoxy resin, manufactured by Mitsubishi Chemical Corporation, molecular weight: 3800, 5% weight loss temperature: 359°C) JP-100 (epoxidized solid epoxy resin, manufactured by Nippon Soda Co., Ltd., molecular weight: 1300, 5% weight loss temperature: 377°C) (3) Solvent TOE-100 (Dihydroterpinyloxyethanol, manufactured by Nippon Terpene Chemical Co., Ltd., molecular weight 198.31) (4) Other ingredients Hardener: Percumyl D (dicumyl peroxide, NOF Corp., molecular weight 270.37) Fluxing agent: KE-604 (product name "Pine Crystal KE-604", hydrogenated acrylic acid modified rosin, manufactured by Arakawa Chemical Industries, Ltd.)

[0068] [Examples 1 to 7 and Comparative Examples 1 to 10] The components were mixed according to the formulation shown in Table 2 and kneaded with a roll to obtain a paste composition. The obtained paste compositions were evaluated as described below, and the results are shown in Table 2.

[0069] [evaluation] (1) Crystallite size S0, S1 and their rate of change {((S1-S0) / S0)×100} The obtained paste composition was dried at 80° C. for 30 minutes to obtain a cake. The obtained cake was applied to a glass plate to a thickness of 200 μm, and the crystallite size S0 (nm) was calculated using the Scherrer formula for the Miller index (111) plane peak by the focusing method using an X-ray diffractometer (product name: SmartLab SE, manufactured by Rigaku Corporation) with CuKα radiation as the radiation source. The fitting function used was a divided pseudo-Voigt function, the width was FWHD, and the Scherrer constant was 0.94.

[0070] The cake was heated to 200°C at a heating rate of 60°C / min under a nitrogen atmosphere while applying a pressure of 15 MPa, and then heated and pressurized at 15 MPa and 200°C for 2 minutes, and then cooled to room temperature (25°C) at a cooling rate of 110°C / min to obtain a sintered body. The sintered body was pulverized in a mortar to obtain a powder. The powder was applied to a glass plate, and the crystallite size S1 (nm) was calculated from the Miller index (111) plane peak by the Scherrer formula using an X-ray diffractometer (product name: SmartLab SE, manufactured by Rigaku Corporation) by the focusing method with CuKα radiation as the radiation source. The fitting function used was a divided pseudo-Voigt function, the width was FWHD, and the Scherrer constant was 0.94. Furthermore, the rate of change {((S1-S0) / S0) x 100} (%) was calculated from the above S0 and S1.

[0071] (2) Viscosity The viscosity of the obtained paste composition was measured at a temperature of 25°C and a rotation speed of 2.0 rpm using an E-type viscometer (manufactured by Toki Sangyo Co., Ltd., product name: VISCOMETER-TV22, applicable cone-plate type rotor: 3°×R14) (3° cone).

[0072] (3) Thixotropic index The viscosity (V) of the obtained paste composition was measured at a temperature of 25° C. and a rotation speed of 2.0 rpm using an E-type viscometer (manufactured by Toki Sangyo Co., Ltd., product name: VISCOMETER-TV22, applicable cone-plate type rotor: 3°×R14). 2.0 ) and viscosity at 20 rpm (V 20 The viscosity V 20 Viscosity V 2.0 Viscosity ratio (V 2.0 / V 20 ) was used as the thixotropy index.

[0073] (4) Volume resistivity The obtained paste composition was applied to a glass substrate (thickness 1 mm) by screen printing to a thickness of 30 μm, dried at 120°C for 10 minutes, heated to 200°C at a heating rate of 60°C / min, and cured at 200°C and 15 MPa for 2 minutes to obtain wiring. The electrical resistivity of the obtained wiring was measured by a four-terminal method using a resistivity meter (product name "MCP-T600", manufactured by Mitsubishi Chemical Corporation).

[0074] (5) Shear strength The obtained paste composition was applied by stencil printing to a copper frame and dried at 120°C for 10 minutes, after which a backside gold chip with a gold vapor deposition layer on a 2 mm x 2 mm bonding surface was mounted, the temperature was raised to 200°C at a heating rate of 60°C / min, and heat-pressure curing was performed at 200°C and 15 MPa for 2 minutes. The hot die shear strength at 260°C was measured using a mount strength measuring device.

[0075] (6) Heat and cold cycle (Manufacturing of Joints) The obtained paste composition was applied by stencil printing to a copper frame and dried at 120°C for 10 minutes. After that, a gold-backed silicon chip with a gold vapor deposition layer on a 5 mm x 5 mm bonding surface was mounted on it. The temperature was increased to 200°C at a rate of 60°C / min, and the material was heated and pressurized for 2 minutes at 200°C and 15 MPa to obtain a bonded body.

[0076] (Cold-heat cycle treatment) The ten bonded bodies thus obtained were subjected to a thermal cycle treatment, which consisted of holding the body at -55°C for 30 minutes, increasing the temperature from -55°C to 150°C at a heating rate of 30°C / min, holding the body at 150°C for 30 minutes, and then decreasing the temperature at a rate of 30°C / min. This cycle was repeated 2000 times. The bonded bodies that had been subjected to the thermal cycle treatment were observed using an ultrasonic microscope (product name "FineSAT II", manufactured by Hitachi Power Solutions Corp.) to check for peeling of the silicon chip, and were evaluated according to the following criteria.

[0077] OK: 0 out of 10 silicon chips peeled off NG: 1 or more of the silicon chips peeled off out of 10

[0078] (7) Particle size distribution For each paste composition shown in Table 2, only silver particles among the components of the paste composition were blended in the ratio shown in Table 2 to obtain a sample for measuring the particle size distribution of the silver particles. For example, for the paste composition of Example 2, 90 parts by mass of TC-728 and 10 parts by mass of TC-905 were mixed to obtain a measurement sample. The particle size distribution of each measurement sample was measured using a laser diffraction particle size distribution analyzer (product name "SALAD-7500nano", manufactured by Shimadzu Corporation). From the particle size distribution, the average particle diameter (D50) was calculated from the particle size at which the cumulative volume was 50% (50% particle size D50). Based on the particle size distribution, the proportions of particles in three ranges of 1.0 μm or less, 1.0 to 20 μm, and over 20 μm were calculated from the frequency of the particle size distribution.

[0079] (8) Specific surface area A sample for measuring the specific surface area of ​​silver particles was prepared by carrying out the following procedure: For each paste composition shown in Table 2, only silver particles among the components of the paste composition were blended in the ratio shown in Table 2 to obtain a sample for measuring the specific surface area of ​​silver particles. For example, for the paste composition of Example 2, 90 parts by mass of TC-728 and 10 parts by mass of TC-905 were mixed to obtain a measurement sample. Each of the obtained measurement samples was degassed at 60° C. for 10 minutes, and then the specific surface area was measured by the BET single point method using nitrogen adsorption using a specific surface area measuring device (Monosorb, manufactured by Quanta Chrome).

[0080] (9)5% weight loss temperature Each resin (jER-1009 and JP-100) was placed in a thermogravimetric and differential thermal analyzer (product name "TG / DTA6200", manufactured by Hitachi High-Tech Science Corp.) The resin was heated from room temperature (25°C) at a heating rate of 10°C / min, and the temperature at which the weight of the resin was reduced by 5% by mass was defined as the 5% weight reduction temperature of the resin.

[0081] [Table 2]

[0082] The paste composition of the examples has a rate of change in crystallite size on the (111) plane ({((S1-S0) / S0)×100} of 250% or more, and the content of silver particles with a particle size of more than 20 μm in 100% by mass of silver particles is 5% by mass or less. Therefore, the paste composition has good coatability, can be pressure-bonded at low temperatures, and has high adhesive strength. On the other hand, the paste compositions of Comparative Examples 1 to 3 and 5 to 8 had a rate of change {((S1-S0) / S0)×100} of less than 250%, and therefore had poor at least one of the properties of coatability, pressure bonding property at low temperatures, and adhesive strength. The paste composition of Comparative Example 4 had poor at least one of the properties of coatability, dispersibility, pressure bonding property at low temperatures, and adhesive strength because the content of silver particles having a particle diameter of more than 20 μm exceeded 5 mass% relative to 100 mass% of silver particles. The paste compositions of Comparative Examples 9 to 10 had a content of silver particles (A) of less than 95 mass% in the total amount of silver particles (A) and binder (B) of 100 mass%, and therefore had poor at least one of the properties among coatability, dispersibility, pressure bonding property at low temperatures, and adhesive strength.

Claims

1. Contains silver particles (A) and a binder (B), the content of silver particles (A1) having a particle diameter of more than 20 μm in 100% by mass of the silver particles (A) is 5% by mass or less, the content of the silver particles (A) is 95% by mass or more in the total amount of the silver particles (A) and the binder (B) (100% by mass), A paste composition having a rate of change represented by the following formula (1) of 250% or more. Rate of change = (S1 - S0) / S0 x 100 (%) (1) [S0 is the crystallite size of the silver particles in the dried paste composition in Miller index (111). S1 is the crystallite size, in Miller indices (111), of silver particles in a treated product obtained by subjecting a dried product of the paste composition to a heating and pressurizing treatment at 15 MPa and 200° C. for 2 minutes in a nitrogen atmosphere.

2. 2. The paste composition according to claim 1, wherein a content of silver particles (A2) having a particle diameter of 1.0 to 20 μm in 100 mass% of the silver particles (A) is 50 mass% or less.

3. 2. The paste composition according to claim 1, wherein a content of silver particles (A3) having a particle diameter of less than 1.0 μm in 100 mass% of the silver particles (A) is 50 mass% or more.

4. The specific surface area of ​​the silver particles (A) is 1.4 m 2 The paste composition according to claim 1, wherein the molecular weight of the paste composition is 1 / g or more.

5. The paste composition according to claim 1 , wherein the binder (B) comprises at least one selected from a thermosetting resin and a thermoplastic resin.

6. The paste composition according to claim 1 , wherein the binder (B) has a 5% by mass weight loss temperature of 250° C. or higher.

7. Contains a solvent (C), 2. The paste composition according to claim 1, wherein a content of the solvent (C) is 10 to 30 mass% based on 100 mass% total of the silver particles (A), the binder (B), and the solvent (C).

8. A semiconductor device having a joint formed from the paste composition according to any one of claims 1 to 7.

9. A method for manufacturing a semiconductor device including a semiconductor element and a semiconductor support member, comprising: A step of applying the paste composition according to any one of claims 1 to 7 to the semiconductor support member; mounting the semiconductor element on the paste composition; and a step of bonding the semiconductor element and the semiconductor support member under heat and pressure, The heat and pressure bonding is performed under conditions of 180 to 300° C. and 1 to 30 MPa for 0.5 to 10 minutes.

10. An electronic component having a joint formed by the paste composition according to any one of claims 1 to 7.

11. A method for producing an electronic component, comprising a step of forming a joint using the paste composition according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Conductive adhesive and method for manufacturing electronic substrate

    JP2019052237A

  • Bonding method by using conductive adhesive

    JP2020136580A

  • Fine silver particles, method for producing same, conductive paste containing the fine silver particles, conductive film, and electronic device

    WO2011040521A1

  • Conductive paste and die bonding method

    WO2014069074A1