Method for manufacturing composite particles, composite powder, and composite member using the composite powder
By distributing carbon particles on the surface of tungsten carbide composite particles, the method addresses the issue of decarburation phases in laminated carbides, enhancing structural integrity and performance.
Patent Information
- Application Number
- JP2020168655
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-05
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2040-10-05
AI Technical Summary
Existing methods for producing laminated carbides using powdered metal-melt techniques face challenges in forming large decarburation phases, which affect the structural integrity and uniformity of the final product.
Incorporating carbon particles on the surface of tungsten carbide composite particles to form a composite powder that is then used in a powdered metal-melt method, ensuring even distribution and minimizing decarburation phases.
The method reduces the formation of decarburation phases, resulting in a more uniform and structurally sound laminated carbide product with improved strength and hardness.
Smart Images

Figure 0007583248000002 
Figure 0007583248000003 
Figure 0007583248000004
Abstract
Description
[Technical field]
[0001] The present invention relates to composite particles, composite powder, and a method for producing a composite member using the composite powder, which are particularly applicable to additive manufacturing. [Background technology]
[0002] Cemented carbide has material properties of high hardness, high strength, and high rigidity, and is used in cutting tools, dies, etc. Among cemented carbide, WC-based cemented carbide, in which hard tungsten carbide is bound by a cobalt binder phase, is widely used. Usually, in the manufacture of WC-based cemented carbide, a slurry of raw powder is first prepared. A small amount of carbon and wax are added to raw powder such as tungsten carbide powder and cobalt powder to prepare a mixed powder. The prepared mixed powder is mixed with a solvent such as alcohol in an attritor or ball mill to prepare a slurry. The slurry is then dried in a spray dryer to prepare a composite powder. The composite powder is then molded into a desired shape by press molding or extrusion molding. The molded product is sintered at a temperature range of about 1350°C to 1500°C by vacuum sintering or pressure sintering for about 1 hour to obtain a WC-based cemented carbide. Carbon is lost by combining with oxygen adsorbed to the composite powder during the sintering process of the molded product. If too little carbon is added when mixing the raw powder, a decarburized phase is formed. On the other hand, if too much carbon is added when mixing the raw powder, free carbon is formed. Usually, carbon is added to the raw powder in an amount of 0.1 mass% or less of the total amount of the raw powder.
[0003] In recent years, additive manufacturing of cemented carbide by powder bed fusion using a laser or electron beam has been considered. For example, the following Patent Documents 1 and 2 propose heat-treating composite particles containing tungsten carbide and cobalt at a temperature at which cobalt becomes liquid in order to increase the strength of the composite particles and prevent them from being destroyed during additive manufacturing. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Republished WO2017 / 150340 [Patent Document 2] JP 2016-172904 A Summary of the Invention [Problem to be solved by the invention]
[0005] According to the investigations of the present inventors, it has been confirmed that coarse decarburized phases are easily formed in cemented carbide manufactured by additive manufacturing using powder bed fusion. An object of the present invention is to provide a manufacturing method of composite particles, composite powder, and a composite member using the composite powder, which makes it difficult for coarse decarburized phases to form in additively manufactured cemented carbide. [Means for solving the problem]
[0006] The inventors have confirmed that by applying a composite powder containing tungsten carbide with carbon particles dispersed on the surface and a metal to a powder bed fusion method, coarse decarburized phases are less likely to form in the additively manufactured cemented carbide, and have arrived at the present invention. One aspect of the present invention is a composite particle containing tungsten carbide and a metal, characterized in that carbon particles are dispersed on the surface of the composite particle.
[0007] It is preferable that the average circle-equivalent particle size of the carbon particles dispersed on the surface is 0.3 μm or more. The tungsten carbide content is preferably 80 mass % or more. The metal is cobalt, and the cobalt content in the composite particles is preferably 5 to 30% by mass. The composite particles preferably have a compressive strength of 100 MPa or more.
[0008] One embodiment of the present invention is a composite powder including a plurality of the composite particles. The composite powder preferably has an average circle-equivalent particle size of 10 to 150 μm.
[0009] One aspect of the present invention is a method for producing a composite part by additive manufacturing of a composite part using a composite powder by powder bed fusion. Effect of the Invention
[0010] According to the present invention, it is possible to reduce the decarburized phase in a cemented carbide manufactured by additive manufacturing using a powder bed fusion method. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is an example of a photograph of the composite powder of the present invention. [Diagram 2] FIG. 2 shows an example of the carbon analysis mapping result of the composite powder of the present invention. [Diagram 3] FIG. 3 is an example of a microstructure photograph of a cemented carbide alloy produced by additive manufacturing using the composite powder of the present invention by powder bed fusion using an electron beam. [Figure 4] FIG. 4 shows an example of the X-ray diffraction results of a cemented carbide alloy additively manufactured by powder bed fusion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] <Composite particles containing tungsten carbide and metal with carbon particles dispersed on the surface> The composite particles of the present embodiment contain tungsten carbide and a metal, and carbon particles are dispersed on the surface of the composite particles. Normally, in sintering cemented carbide, the compact is held for about an hour in a temperature range where the bonding phase becomes liquid, resulting in a uniform structure. On the other hand, in powder bed fusion, the process of depositing composite powder and the process of irradiating the deposited layer with an electron beam or laser to instantly generate a liquid phase and rapidly solidify it are repeated in sequence to form an additive manufacturing process. In powder bed fusion, the carbon in the composite powder reacts with the oxygen in the furnace in the part that is instantaneously heated, resulting in a localized decrease in carbon. Therefore, it is presumed that the structure becomes non-uniform with the grain growth caused by melting and solidification, and that coarse decarburized phases are easily formed. Even if a mixed powder in which additional carbon is added to the composite powder is used to compensate for the carbon lost during melting, the carbon reacts preferentially at the high temperatures during additive manufacturing, resulting in a non-uniform structure.
[0013] Therefore, the present inventors have investigated the possibility of uniformly incorporating an excess of carbon into the composite powder in advance, and have confirmed that by using composite particles containing tungsten carbide and a metal with carbon particles dispersed on the surface in a powder bed fusion process using an electron beam or a laser, coarse decarburized phases are unlikely to form in the additively manufactured cemented carbide.
[0014] In this embodiment, the "carbon particles dispersed on the surface of the composite particle" refers to the carbon powder mixed with the raw material powder when preparing the slurry. In reality, the carbon particles are also dispersed inside the composite particle, but the carbon inside the particle cannot be confirmed without destroying the composite particle, so the term "carbon particles dispersed on the surface" is used here.
[0015] If the average particle size of the carbon particles dispersed on the surface of the composite particle is too small, the structure is likely to become non-uniform. Therefore, the average circle-equivalent particle size of the carbon particles is preferably 0.3 μm or more. On the other hand, if the average circle-equivalent particle size of the dispersed carbon particles is too large, free carbon is likely to be formed, and it is difficult to disperse uniformly on the surface and inside of the composite particle. The average circle-equivalent particle size of the dispersed carbon particles is preferably 3 μm or less, more preferably 1 μm or less.
[0016] In this embodiment, the average diameter of the carbon particles dispersed on the surface of the composite particle equivalent to a circle can be obtained by binarizing the carbon mapping result with image analysis software. At this time, if particles with a diameter of less than 0.1 μm are included, the measurement will contain a lot of noise, and the average diameter will be significantly smaller than the actual size. Therefore, when binarizing, particles with a diameter of less than 0.1 μm are excluded from the measurement result. This eliminates a lot of noise, and the average diameter can be obtained with high accuracy. It is preferable to observe the surface of the composite particle in multiple fields of view and obtain the average diameter from 100 or more carbon particles with a diameter of 0.1 μm or more.
[0017] If the amount of carbon contained in the composite particles is too small, the carbon particles will not be dispersed on the surface of the composite particles, and the effect of suppressing the formation of the decarburized phase will not be obtained. In this embodiment, the state in which "carbon particles are not dispersed on the surface of the composite particles" refers to a state in which carbon particles are dispersed at a depth of 2400 μm on the surface of the composite particles. 2 This is a state in which three or more carbon particles having an equivalent circle diameter of 0.3 μm or more are not observed in the field of view. As the carbon content of the composite particles increases, the average particle size of the carbon particles dispersed on the surface of the composite particles increases. Therefore, the suitable carbon content in the composite particles can be determined by whether the average circle-equivalent particle size of the carbon particles dispersed on the surface of the composite particles is within the range of 0.3 μm to 3 μm. The area ratio of the carbon particles dispersed on the surface of the composite particles is preferably 0.3% to 5%. The composite particles have an average particle size of 2400 μm. 2 It is preferable that the number of carbon particles having an equivalent circle diameter of 0.3 μm or more in the visual field is 5 or more, and more preferably 10 or more. In this embodiment, the "composite particles" are approximately spherical particles in which tungsten carbide, which is a hard phase, and metal and carbon particles, which are a binder phase, are mixed together three-dimensionally.
[0018] The composite particles of this embodiment contain 80% by mass or more of tungsten carbide. By containing 80% by mass or more of tungsten carbide in the composite particles, the strength and hardness of the composite member obtained by additive manufacturing are preferably further increased. The composite particles of the present embodiment may contain ceramics other than tungsten carbide. For example, ceramics selected from carbides, nitrides, carbonitrides, oxides, and borides of at least one element selected from Cr (chromium), Mo (molybdenum), V (vanadium), Zr (zirconium), Al (aluminum), Si (silicon), Nb (niobium), Ta (tantalum), and Ti (titanium). In the composite particles of this embodiment, when the content ratio (mass %) of ceramics other than tungsten carbide and metals constituting the metal phase in the composite particles is taken as 100%, the content ratio (mass %) of ceramics can be 50% or more and 95% or less, and the content ratio (mass %) of metals can be 5% or more and 50% or less.
[0019] The metal contained in the composite particles of this embodiment is preferably selected from at least one of Co (cobalt), Ni (nickel), Fe (iron), W (tungsten), and Mo (molybdenum). The metal contained in the composite particles is preferably cobalt, and when the cobalt content in the composite particles is 5 to 30 mass %, the toughness of the composite member is increased, which is preferable.
[0020] The composite particles preferably have a compressive strength of 100 MPa or more. By using high-strength composite particles, deformation and destruction of the particles during additive manufacturing can be effectively suppressed. Furthermore, the composite particles preferably have a compressive strength of 200 MPa or more. To obtain such composite particles, it is preferable to set the sintering temperature (Ts) at which the residual porosity measured in accordance with TAS0055-2017 is A04 or less, and the sintering temperature is preferably set to 0.85Ts to 1.0Ts. Specifically, Ts is preferably set to 1200 to 1450°C, and more preferably to 1250 to 1400°C.
[0021] The composite powder of this embodiment is characterized by containing a plurality of the composite particles described above. If the composite powder contains 60% or more by volume of the composite particles of the above embodiment, advantageous effects are likely to be obtained during additive manufacturing. The content of the composite particles may be 80% or more by volume of the entire powder. The composite powder of this embodiment may be composed only of the composite particles of the above embodiment. Powders that can be added to the composite powder of this embodiment other than the composite particles of this embodiment include, for example, metal powder and carbon powder.
[0022] The composite powder of this embodiment preferably has a diameter d of D50 in the volume cumulative particle size distribution of 10 to 150 μm. In other words, the average circle-equivalent particle diameter of the composite powder is preferably in the range of 10 μm to 150 μm. If the diameter d is less than 10 μm, the powder is likely to scatter during, for example, layered manufacturing. If the diameter d is greater than 150 μm, coarse residual pores tend to be easily generated in the layered manufactured product. The average particle diameter of the composite powder can be measured, for example, by laser diffraction.
[0023] The composite powder of this embodiment is preferably applied to a powder bed fusion method in which the composite powder is deposited, and then instantaneously irradiated with an electron beam or laser to melt and solidify the composite powder and form layers by repeating this process. There are two types of powder bed fusion methods: a laser method and an electron beam method. However, it is preferable to use the electron beam method because the shaping is performed in a vacuum, preheating by an electron beam is possible, and the operation speed can be increased. EXAMPLES
[0024] The raw material powders were WC powder (average particle size 0.6 μm), Co powder (average particle size 0.6 μm), Cr3C2 powder (average particle size 1 μm), and TaC powder (average particle size 1 μm), and were mixed to give a composition of WC-10 mass% Co-0.8 mass% Cr3C2-0.25 mass% TaC. For sample No. 1, approximately 0.5% by mass of carbon powder and a small amount of paraffin wax were added to the weighed powder, and the mixture was wet-mixed with ethanol in an attritor to obtain a mixed powder slurry. The slurry was then granulated using a spray dryer to obtain a granulated powder. The obtained granulated powder was sintered at 1260°C in a vacuum atmosphere (1 to 2 Pa) to obtain a composite powder consisting of a plurality of composite particles. The obtained composite powder consisting of a plurality of composite particles was classified using a 150 μm sieve.
[0025] A very small amount of carbon powder was added to Sample No. 2, as in the case of manufacturing conventional cemented carbide. Specifically, while about 0.5% by mass of carbon powder was added to Sample No. 1, about 0.05% by mass of carbon powder was added to Sample No. 2, and the rest was the same as Sample No. 1.
[0026] It was confirmed that when the composite powder made of multiple composite particles of sample No. 1 was used and subjected to the normal process of press molding, followed by vacuum sintering in the same manner as for normal cemented carbide, a large amount of free carbon was precipitated. Also, when the composite powder made of multiple composite particles of sample No. 2 was used and subjected to the normal process of vacuum sintering in the same manner as for No. 1, it was confirmed that a healthy structure without decarburized phases or free carbon was formed.
[0027] The composite powder samples No. 1 and No. 2 were subjected to surface observation, average particle size measurement, and composite particle strength measurement. The flowability of the composite powder was measured in accordance with JIS Z 2502. The compression strength of the composite particles was determined using a micro compression strength tester (MCT510, manufactured by Shimadzu Corporation) at a loading speed of 207.4 mN / sec. The average particle size of the composite powder was measured using Microtrac's laser diffraction / scattering particle size distribution measuring device "Microtrac MT3000II" in the volume cumulative particle size distribution, measured in dry mode for 30 seconds, with particle conditions of granulated powder and solvent of air, as D50.
[0028] For sample No. 1, surface observation was performed using an electron probe microanalyzer (model number: JXA-8500F) manufactured by JEOL Ltd., and composition mapping analysis was performed using wavelength dispersive electron probe microanalysis (WDS-EPMA). Figure 1 shows an example of an observation photograph (magnification 2000x) of the surface of a composite particle of sample No. 1. Figure 2 shows an example of the carbon analysis results of the surface of a composite particle. It can be seen that carbon is dispersed on the surface of the composite particle. Using the image processing software Image-Pro, the carbon mapping results were binarized to determine the circle-equivalent carbon particle diameter. Ten or more composite particles were then observed to determine the circle-equivalent average particle diameter D50 of the carbon dispersed on the surface of the composite particles and the area ratio of carbon on the surface of the composite particles. At this time, carbon particles smaller than 0.1 μm were excluded from the measurement as noise to determine the average particle diameter. In addition, from the area of the observation region in each composite particle and the number of carbon particles located within the observation region, a diameter of 2400 μm was determined. 2 The number of carbon particles having an equivalent circle diameter of 0.3 μm or more per unit area was calculated. The measurement results are summarized in Table 1.
[0029] [Table 1]
[0030] Using an electron beam additive manufacturing device manufactured by Arcam, the composite powders of samples No. 1 and No. 2 were used to fabricate cemented carbide specimens measuring 20 mm x 10 mm x 35 mm.
[0031] Figure 3 shows an example of a microstructure photograph of a cemented carbide alloy produced by additive manufacturing using powder bed fusion with an electron beam. Unlike ordinary cemented carbide alloys, voids can be seen inside the tungsten carbide particles. The relative density was about 97%. Voids other than those inside the tungsten carbide can be reduced by performing HIP processing after additive manufacturing.
[0032] The cross section of the obtained sintered body (laminated product) was polished, and the amount of decarburized phase (Co3W3C) was evaluated using an X-ray diffractometer EMPUREAN manufactured by PANalytical under the conditions of 45 kV-40 mA, 2θ: 34 to 50°, and scan speed: 0.5° / min. The evaluation method was based on the peak height ratio (%) of the WC (101) plane to the Co3W3C (511) plane. Figure 4 shows a part of the X-ray diffraction results. Figure 4 shows the range of 42° to 43°, including the Co3W3C (511) peak. It can be seen from Figure 4 that sample No. 1 has less decarburized phase than sample No. 2. As described above, it is clear that by using the composite powder according to an embodiment of the present invention, it is possible to reduce the decarburized phase (Co3W3C), which was difficult to reduce using conventional methods, in cemented carbide manufactured by electron beam additive manufacturing.
Claims
1. A composite particle comprising tungsten carbide and a metal, A composite particle, characterized in that carbon particles are dispersed on the surface of the composite particle.
2. 2. The composite particle according to claim 1, wherein the average circle-equivalent particle size of the carbon particles dispersed on the surface is 0.3 μm or more.
3. 3. The composite particle according to claim 1, wherein the tungsten carbide content is 80 mass % or more.
4. 4. The composite particle according to claim 1, wherein the metal is cobalt, and the content of cobalt in the composite particle is 5 to 30 mass %.
5. 5. The composite particle according to claim 1, wherein the composite particle has a compressive strength of 100 MPa or more.
6. A composite powder comprising a plurality of composite particles according to any one of claims 1 to 5.
7. 7. The composite powder according to claim 6, characterized in that the average particle diameter equivalent to a circle is 10 to 150 μm.
8. A method for producing a composite member, comprising additively manufacturing a composite member by powder bed fusion using the composite powder according to claim 6 or 7.
9. The method of claim 8, wherein the powder bed fusion process uses an electron beam.
Citation Information
Patent Citations
Tungsten carbide-base sintered hard alloy
JP1992202738A
Hard composite sintered compact, hard structure and production method therefor
JP2004353047A
WC-based cemented carbide and manufacturing method therefor
JP2007191741A
Hard mold suitable for energization heating and material therefor
JP2012246537A
Granule for lamination molding, and method for producing the same
JP2016172904A