Hot-rolled steel sheet for non-oriented electrical steel sheet and its manufacturing method
By controlling chemical composition and physical properties at the edges of hot-rolled steel sheets, the issue of breakage during pickling is resolved, ensuring stable processing and maintaining magnetic properties.
Patent Information
- Application Number
- JP2023500455
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-19
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2041-02-19
AI Technical Summary
Hot-rolled steel sheets prone to breakage during pickling due to scratches and bumps on the edges during self-annealing, which compromises the benefits of omitting hot-rolled sheet annealing.
Control the chemical composition and physical properties of the steel sheet, particularly at the edges, by setting specific Vickers hardness, ductile-brittle transition temperature, and thickness differences across the width, along with controlled winding and cooling temperatures to prevent breakage during pickling.
Achieves stable threading without breakage and maintains magnetic properties by enhancing edge hardness and toughness, reducing scratches and bumps, and controlling thickness variations.
Smart Images

Figure 0007583323000001 
Figure 0007583323000002 
Figure 0007583323000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a hot-rolled steel sheet for a non-oriented electrical steel sheet and a manufacturing method thereof. [Background technology]
[0002] In recent years, with the increasing demand for energy saving in electrical equipment worldwide, higher performance characteristics are being demanded for non-oriented electrical steel sheets used as iron core materials for rotating machines.
[0003] High-grade non-oriented electrical steel sheets are often used for motors in electrical appliances that are considered to be highly efficient. High-grade non-oriented electrical steel sheets generally have increased Si and Al content to increase resistivity and have coarse grain size.
[0004] However, the manufacturing costs of high-grade non-oriented electrical steel sheets are high, and there is a demand for further reduction in the manufacturing costs. To reduce costs, it is important to simplify the manufacturing process.
[0005] Self-annealing, which is performed during cooling after hot rolling, is a technology that is expected to eliminate the need for hot-rolled sheet annealing. The purpose of hot-rolled sheet annealing is to promote recrystallization and grain growth in the hot-rolled sheet, which can eliminate the shape defect problem called ridging and improve magnetic properties. The so-called self-annealing technology, which aims to obtain the effects of this hot-rolled sheet annealing by using the temperature of the hot-rolled coil itself during cooling after hot rolling, is disclosed as follows.
[0006] For example, Patent Document 1 discloses a self-annealing technology for a non-oriented electrical steel sheet having good magnetic flux density, containing, by mass%, C: ≦0.005%, Si: 0.1-2.0%, Mn: 0.05-0.6%, and Al: ≦0.5%, and having a specified number density of AlN with an average diameter of 10-200 nm, and in which the coiling temperature for hot rolling is 780°C or higher.
[0007] Patent Document 2 discloses a technology for omitting hot-rolled sheet annealing in which the steel contains, in mass%, C:≦0.008%, 2%≦Si+Al≦3%, and 0.02≦Mn≦1.0%, the relationship of 0.3%≦Al / (Si+Al)≦0.5% is satisfied, the hot-rolling finish rolling temperature is 1050°C or higher, the subsequent water-free period is 1 to 7 seconds, and the hot-rolled sheet is coiled at 700°C or lower after water cooling.
[0008] Patent Document 3 discloses a method for producing a non-oriented electrical steel sheet having high magnetic flux density and low iron loss, which contains, by weight, C: 0.010% or less, Si: 0.1% or more and 2.0% or less, Mn: 0.1% or more and 1.5% or less, Al: 0.1% or more and 1.0% or less, Sn: 0.02% or more and 0.20% or less, and Cu: 0.1% or more and 1.0% or less, and is hot-rolled annealed or self-annealed at a temperature equal to or lower than the Ac1 transformation point. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] International Publication No. 2013-069754 [Patent Document 2] Japanese Patent Application Publication No. 2010-242186 [Patent Document 3] Japanese Patent Publication No. 4-6220 Summary of the Invention [Problem to be solved by the invention]
[0010] The above-mentioned conventional technology aims to promote the growth of crystal grains in hot-rolled steel sheets by self-annealing, and improve the magnetic properties while omitting hot-rolled sheet annealing. However, it has been found that when hot-rolled sheet annealing is replaced with self-annealing after hot rolling, the steel sheet is prone to breakage during the pickling process in which the steel sheet is repeatedly bent multiple times. Therefore, the above-mentioned conventional technology has a problem in that the advantage of omitting hot-rolled sheet annealing cannot be fully obtained.
[0011] The present invention has been made in consideration of the above circumstances. An object of the present invention is to provide a hot-rolled steel sheet for non-oriented electrical steel sheet, which is capable of realizing stable threading without breaking during the pickling process, and a manufacturing method thereof. [Means for solving the problem]
[0012] The gist of the present invention is as follows.
[0013] (1) A hot-rolled steel sheet for non-oriented electrical steel sheet according to one aspect of the present invention is Chemical composition, by mass % C: 0.0050% or less, Si: 1.9% or more and 3.5% or less, Mn: 0.10% or more and 1.50% or less, Al: 0.10% or more and 1.50% or less, with the remainder being Fe and impurities, When the position 25 mm from the side edge of the steel plate along the plate width direction is defined as the plate width end, and the center position of the steel plate in the plate width direction is defined as the plate width center, The Vickers hardness at the plate width end portion is 180 Hv or more, and the value obtained by subtracting the Vickers hardness at the plate width center portion from the Vickers hardness at the plate width end portion: ΔHv is 10 Hv or more and 100 Hv or less, The ductile-brittle transition temperature at the plate width end is 0°C or less, and the value obtained by subtracting the ductile-brittle transition temperature at the plate width end from the ductile-brittle transition temperature at the plate width center: ΔDBTT is 10°C or more and 100°C or less; The value obtained by subtracting the thickness at the widthwise end portion from the thickness at the widthwise center portion is 50 μm or less. (2) A method for producing a hot-rolled steel sheet for non-oriented electrical steel sheet according to one aspect of the present invention is a method for producing a hot-rolled steel sheet for non-oriented electrical steel sheet according to the above (1), Chemical composition, by mass%, C: 0.0050% or less Si: 1.9% or more and 3.5% or less, Mn: 0.10% or more and 1.50% or less, Al: 0.10% or more and 1.50% or less, The slab is heated to 1050°C to 1180°C, with the balance being Fe and impurities. The heated slab is roughly rolled, Reheating the rough rolled material after the rough rolling, The reheated rough rolled material is finish rolled under conditions where the finishing temperature is 900°C to 1000°C, The finish rolled material after the finish rolling is coiled under conditions in which the coiling temperature at the widthwise end portions is 700°C or higher and 800°C or lower, and the coiling temperature at the widthwise end portions is 50°C or higher lower than the coiling temperature at the widthwise center portion. (3) In the method for producing a hot-rolled steel sheet for non-oriented electrical steel sheet described in (2) above, The bottom surface of the hot rolled coil may not be in contact with other hot rolled coils for at least 30 minutes after the coiling. Effect of the Invention
[0014] According to the above-mentioned aspects of the present invention, it is possible to provide a hot-rolled steel sheet for a non-oriented electrical steel sheet, which is capable of realizing stable sheet threading without breaking the steel sheet during the pickling process, and a manufacturing method thereof. Also, according to the above-mentioned aspects of the present invention, it is possible to suppress scratches and strike marks on the end faces in the sheet width direction of the hot-rolled coil. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] A preferred embodiment of the present invention will be described in detail below. However, the present invention is not limited to the configuration disclosed in this embodiment, and various modifications are possible without departing from the spirit of the present invention. In addition, the numerical ranges described below include lower and upper limits. Numerical values indicated as "more than" or "less than" are not included in the numerical range. In addition, unless otherwise specified, "%" regarding the content of each element means "mass %".
[0016] The present inventors have investigated the reason why a steel sheet is prone to breakage in the pickling process when self-annealing is performed in the hot rolling process and hot-rolled sheet annealing is omitted. In particular, the inventors have focused on the properties and material characteristics of the ends in the sheet width direction of the hot-rolled coil. As a result, they have found that scratches and strike marks caused during transportation are confirmed in the ends in the sheet width direction of the hot-rolled coil, and that bending deformation is applied to the steel sheet when the steel sheet passes through many rolls in the pickling process, and the strain generated at this time is concentrated in the scratches and strike marks, resulting in the generation and propagation of cracks, which lead to breakage.
[0017] The present inventors have conducted extensive research into methods for preventing sheet breakage (breakage of steel sheet) that occurs during the pickling process as described above, and have found the following.
[0018] When the finish-rolled material is wound into a coil after finish rolling in the hot rolling process, winding irregularities occur to a certain extent. In addition, if the coil is transported on a conveyor with the coil winding axis vertical after winding (with the coil core forming a vertical hole), scratches are likely to occur in the winding irregularities on the underside of the coil (the bottom surface of the lower coil). In addition, if the coil is hoisted by a crane with the coil winding axis horizontal (with the coil core forming a horizontal hole), the hook of the crane is likely to come into contact with the coil end, causing contact marks.
[0019] In order to prevent the steel sheet from breaking during the pickling process, it is necessary to keep the abrasion marks and strike marks on the hot-rolled coil as minor as possible. In addition, the steel sheet needs to have sufficient toughness not to break even if bending strain is concentrated at the abrasion marks or strike marks.
[0020] First, it was discovered that a method for reducing scratches and strike marks is to make the Vickers hardness at a position 25 mm from the side edge of the hot-rolled steel sheet in the sheet width direction 180 Hv or more. It is believed that increasing the hardness at the sheet width end improves the wear resistance of the steel sheet and reduces scratches and strike marks themselves.
[0021] Next, it was discovered that, as a method for suppressing plate breakage during pickling, it is sufficient that the ductile-brittle transition temperature (DBTT) in the Charpy impact test is 0°C or lower at a position 25 mm along the plate width direction from the side edge of the hot-rolled steel plate. It was found that if this condition is satisfied, plate breakage can be effectively suppressed even in winter, when plate breakage becomes prominent during the pickling process. It is believed that by increasing the toughness of the plate width end, even if a small crack occurs from the side edge of the steel plate, the ductility of the steel plate will relieve stress at the tip of the crack, mitigating the propagation of the crack.
[0022] Furthermore, they discovered that a method for preventing sheet breakage during pickling is to keep the difference in sheet thickness (crown) between a position 25 mm from the side edge along the sheet width direction and the center position in the sheet width direction of the hot-rolled steel sheet to 50 μm or less. If this condition is met, it was found that the generation of cracks that could be the starting point for sheet breakage is suppressed and the propagation of the cracks is mitigated when the steel sheet is passed through the pickling process.
[0023] For example, the widthwise end of the plate is more likely to become thinner than the widthwise center due to the deformation of the rolling rolls. If the plate thickness becomes thinner at the widthwise end, the steel plate will try to stretch in the longitudinal direction (rolling direction) at the widthwise end as a selvedge wave in order to compensate for the reduction in the volume of the steel plate. In other words, the larger the crown, the greater the degree (amplitude) of the selvedge wave. When the selvedge wave at the widthwise end is significant, the selvedge wave is accompanied by amplitude, so that repeated bending and unbending deformation is applied to the widthwise end (especially the selvedge portion) every time the steel plate passes through the rolls during pickling. As a result, it is believed that a crack that is the starting point of the plate breakage is generated, and this crack propagates. In other words, it is believed that by making the crown smaller, the generation and propagation of the crack is suppressed, and plate breakage is suppressed.
[0024] As mentioned above, sheet breakage during pickling is mainly caused by cracks that are generated and propagate at the widthwise ends of the steel sheet. Therefore, in order to suppress sheet breakage during pickling, the steel sheet characteristics at the widthwise ends should be controlled as described above. However, the most important property required for a non-oriented electrical steel sheet is the magnetic property. For example, if the steel sheet characteristics over the entire width in the width direction are the same as the steel sheet characteristics at the widthwise ends described above, the magnetic property required for a non-oriented electrical steel sheet cannot be satisfied. In other words, in order to achieve both stable pickling during the pickling process and the magnetic properties required for a non-oriented electrical steel sheet, it is necessary to create different steel sheet characteristics at the widthwise ends and the widthwise center.
[0025] The present inventors have found that, in order to achieve both stable electrical resistance in the pickling process and the magnetic properties required for a non-oriented electrical steel sheet, in addition to controlling the steel sheet characteristics at the widthwise ends as described above, it is sufficient to control the steel sheet characteristics at the widthwise center as follows: Specifically, it has been found that the value obtained by subtracting the Vickers hardness at the widthwise center from the Vickers hardness at the widthwise ends: ΔHv should be 10 Hv to 100 Hv, and the value obtained by subtracting the ductile-brittle transition temperature at the widthwise center from the ductile-brittle transition temperature at the widthwise ends: ΔDBTT should be 10°C to 100°C.
[0026] Based on the above findings, even if self-annealing is performed during hot rolling and hot-rolled sheet annealing is omitted, it is possible to obtain a hot-rolled steel sheet for non-oriented electrical steel sheet that does not break during pickling and has satisfactory magnetic properties.
[0027] The hot-rolled steel sheet for non-oriented electrical steel sheet according to this embodiment is Chemical composition, by mass % C: 0.0050% or less, Si: 1.9% or more and 3.5% or less, Mn: 0.10% or more and 1.50% or less, Al: 0.10% or more and 1.50% or less, with the remainder being Fe and impurities, When the position 25 mm from the side edge of the steel plate along the plate width direction is defined as the plate width end, and the center position of the steel plate in the plate width direction is defined as the plate width center, The Vickers hardness at the widthwise end is 180 Hv or more, and the value obtained by subtracting the Vickers hardness at the widthwise center from the Vickers hardness at the widthwise end: ΔHv is 10 Hv or more and 100 Hv or less, The ductile-brittle transition temperature at the width end is 0°C or less, and the ductile-brittle transition temperature at the width center minus the ductile-brittle transition temperature at the width end (ΔDBTT) is 10°C or more and 100°C or less, The thickness at the widthwise center minus the thickness at the widthwise ends is 50 μm or less.
[0028] First, with regard to the hot-rolled steel sheet for the non-oriented electrical steel sheet according to this embodiment, the reasons for limiting the chemical components of the steel will be described.
[0029] <Chemical composition of hot-rolled steel sheet> In this embodiment, the heat-rolled steel sheet contains, as its chemical components, basic elements, optional elements as necessary, and the balance being Fe and impurities.
[0030] C: 0.0050% or less C deteriorates the core loss due to magnetic aging. Therefore, the C content is 0.0050% or less. The C content may be 0.0045% or less, 0.0040% or less, or 0.0035% or less. The lower the C content, the more preferable it is, and the lower limit may be 0%. However, in consideration of industrial productivity, the C content may be more than 0%, and may be 0.0015% or more, 0.0020% or more, or 0.0025% or more.
[0031] Si: 1.9% or more and 3.5% or less Si is an element effective for increasing electrical resistance. The Si content may be adjusted as appropriate according to required properties such as core loss, magnetic flux density, and strength. However, if the Si content is less than 1.9%, the problem of this embodiment does not arise. On the other hand, if the Si content exceeds 3.5%, the toughness decreases and manufacturing becomes difficult. Therefore, the Si content is set to 1.9% or more and 3.5% or less. The Si content is preferably more than 2.0%, and more preferably 2.2% or more.
[0032] Mn: 0.10% or more and 1.50% or less Mn promotes grain growth as a sulfide generating element. Therefore, the lower limit of the Mn content is set to 0.10%. Mn also has the effect of increasing electrical resistance. The upper limit of the Mn content should be set to 1.50%, at which this effect saturates.
[0033] Al: 0.10% or more and 1.50% or less Al is an element necessary for deoxidizing steel. From the viewpoint of obtaining a stable deoxidizing effect and suppressing the generation of fine AlN, the Al content is set to 0.10% or more. Al also has the effect of increasing electrical resistance. However, excessive addition of Al deteriorates castability during steelmaking. Therefore, the upper limit of the Al content is set to 1.50%.
[0034] In this embodiment, Sn may be contained as an optional element. Sn has effects such as suppressing hot rolling scale and improving magnetic properties. Therefore, the Sn content may be set to 0% or more and 0.20% or less as necessary. The Sn content is preferably 0.03% or more and 0.20% or less.
[0035] In this embodiment, P and S may be restricted as impurities. P may deteriorate toughness. Therefore, the P content may be set to 0.020% or less, if necessary. The P content is preferably set to 0.010% or less. S may deteriorate toughness and magnetic properties. Therefore, the S content may be set to 0.003% or less, if necessary.
[0036] The term "impurities" refers to elements that do not impair the effects of the present embodiment even if contained, and refers to elements that are mixed in from raw materials such as ores and scraps, or from the manufacturing environment, etc., when industrially manufacturing steel sheets. The upper limit of the total content of impurities may be, for example, 5%.
[0037] The above chemical components may be measured by a general analysis method for steel. For example, the chemical components may be measured using ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry). Specifically, a 35 mm square test piece taken from the steel plate is measured under conditions based on a calibration curve prepared in advance using a measuring device such as Shimadzu ICPS-8100, to identify the chemical components. C may be measured using a combustion-infrared absorption method.
[0038] Next, the characteristics of the widthwise end and widthwise center of the hot-rolled steel sheet for non-oriented electrical steel sheet according to this embodiment will be described. Note that the widthwise end is the position 25 mm from the side edge of the hot-rolled steel sheet in the width direction, and the widthwise center is the center position of the hot-rolled steel sheet in the width direction.
[0039] <Vickers hardness> In the hot-rolled steel sheet for non-oriented electrical steel sheet according to this embodiment, the Vickers hardness at the sheet width end is set to 180Hv or more. If the hardness is less than 180Hv, scratches and strikes are likely to occur, and strain concentration is likely to occur during sheet passing in the pickling process. The Vickers hardness at the sheet width end is preferably 190Hv or more, and more preferably 200Hv or more. If the hardness at the sheet width end is increased, the edge portion that receives scratches and strikes will inevitably have a high hardness as well. The upper limit of the Vickers hardness at the sheet width end is not particularly limited, but may be, for example, 350Hv.
[0040] In addition, in the hot-rolled steel sheet for non-oriented electrical steel sheet according to this embodiment, the value obtained by subtracting the Vickers hardness at the center of the sheet width from the Vickers hardness at the sheet width end: ΔHv is set to 10 Hv or more and 100 Hv or less. When the Vickers hardness satisfies the above condition, both stable hardness in the pickling process and magnetic properties as a non-oriented electrical steel sheet can be achieved. The above value is preferably 10 Hv or more, and more preferably 20 Hv or more. The above value is preferably 100 Hv or less, more preferably 90 Hv or less, and more preferably 50 Hv or less.
[0041] The Vickers hardness may be measured in accordance with JIS Z 2244 (2009). The measurement load can be set appropriately to a load that produces the largest indentation, allowing for more accurate measurement. For example, the measurement load is 9.8×10 -5 ~9.8×10 0 The Vickers hardness may be measured in N. In measuring the Vickers hardness, the indentation diameter is usually measured using an optical microscope, but for more accurate measurements, an electron microscope such as a SEM may also be used. The Vickers hardness may be measured at the center of the plate thickness direction.
[0042] <Ductile-brittle transition temperature> In the hot-rolled steel sheet for non-oriented electrical steel sheet according to the present embodiment, the ductile-brittle transition temperature at the sheet width end is set to 0°C or less. If the DBTT at the sheet width end is higher than 0°C, cracks are likely to occur and grow due to strain concentrated in scratches and strike scratches, and the sheet is likely to break, especially in winter when the outside air temperature is low. The DBTT at the sheet width end is preferably -5°C or less, and more preferably -10°C or less. Since the unevenness of the bottom surface of the coil caused by the winding irregularity of the hot-rolled coil is about 10 mm, if the toughness of the sheet width end is increased, the crack generated at the side edge of the steel sheet is unlikely to grow toward the sheet width center. The lower limit of the DBTT at the sheet width end is preferably lower and is not particularly limited, but may be, for example, -100°C.
[0043] In addition, in the hot-rolled steel sheet for non-oriented electrical steel sheet according to this embodiment, ΔDBTT, which is the value obtained by subtracting DBTT at the end of the sheet width from DBTT at the center of the sheet width, is set to 10°C or more and 100°C or less. When ΔDBTT satisfies the above condition, both stable pickling in the pickling process and magnetic properties as a non-oriented electrical steel sheet can be achieved. The above value is preferably 10°C or more, and more preferably 20°C or more. The above value is preferably 100°C or less, more preferably 90°C or less, and more preferably 50°C or less.
[0044] DBTT can be obtained from the results of a Charpy impact test. The Charpy impact test may be performed in accordance with JIS Z 2242 (2018). For example, the measurement conditions may include providing a V-shaped notch in the test piece, performing an impact test, and measuring the absorbed energy. Note that the test piece for the Charpy impact test may have the same thickness as the hot-rolled steel plate.
[0045] <Crown> In the hot-rolled steel sheet for the non-oriented electrical steel sheet according to the present embodiment, the value (crown) obtained by subtracting the thickness at the widthwise end from the thickness at the widthwise center is set to 50 μm or less. When the crown is 50 μm or less, it is possible to reduce sheet breakage during the pickling process. The crown is preferably 40 μm or less, and more preferably 30 μm or less. Since the unevenness of the bottom surface of the coil caused by the winding irregularity of the hot-rolled coil is about 10 mm, if the crown is low at the widthwise end and widthwise center, repeated bending and unbending deformation that would cause cracks generated at the side edges of the steel sheet to progress toward the widthwise center is rarely applied.
[0046] The crown may be measured, for example, using a commercially available thickness measuring device. In cases where the oxidation state in the sheet width direction significantly differs during hot rolling and / or after coiling, the crown may be measured after removing the scale (surface oxide layer) of the hot-rolled steel sheet by pickling or the like. Alternatively, the cross section of the hot-rolled steel sheet may be polished, observed using an optical microscope or an electron microscope such as SEM, and the thickness of the steel sheet portion may be measured, thereby eliminating the effect of the scale and measuring the crown.
[0047] <Method of manufacturing hot-rolled steel sheets> Next, a method for producing a hot-rolled steel sheet for a non-oriented electrical steel sheet according to this embodiment will be described.
[0048] The manufacturing method of the hot-rolled steel sheet for non-oriented electrical steel sheet according to the present embodiment is the manufacturing method of the above-mentioned hot-rolled steel sheet, Chemical composition, by mass % C: 0.0050% or less, Si: 1.9% or more and 3.5% or less, Mn: 0.10% or more and 1.50% or less, Al: 0.10% or more and 1.50% or less, The slab is heated to 1050°C to 1180°C, with the balance being Fe and impurities. The heated slab is roughly rolled, The rough rolled material after the rough rolling is reheated, The reheated rough rolled material is finish rolled under the condition that the finishing temperature is 900°C to 1000°C, The finish rolled material after the finish rolling is coiled under conditions such that the coiling temperature at the widthwise end portion is 700°C or higher and 800°C or lower, and the coiling temperature at the widthwise end portion is 50°C or higher lower than the coiling temperature at the widthwise center portion.
[0049] In the method for producing a hot-rolled steel sheet for a non-oriented electrical steel sheet according to this embodiment, it is preferable that the bottom surface of the hot-rolled coil is not brought into contact with other hot-rolled coils for at least 30 minutes after the coiling.
[0050] Unless otherwise specified, the heating temperature (e.g., slab heating temperature, finish rolling temperature, etc.) refers to the surface temperature at the center of the plate width. The plate width end is the position 25 mm from the side edge along the plate width direction, and the center position of the plate in the plate width direction is the plate width center.
[0051] The chemical composition of the slab is the same as that of the hot-rolled steel sheet described above. In the production of non-oriented electrical steel sheets, the chemical composition hardly changes during the process from slab to hot-rolled steel sheet. The chemical composition of the slab described above corresponds to ferritic single-phase steel in which no α-γ transformation occurs during the manufacturing process.
[0052] The slab heating temperature is set to 1050°C to 1180°C. Since the ferritic single-phase steel targeted in this embodiment has low high-temperature strength, if the slab heating temperature is high, the slab may sag, which may cause problems in rolling. For this reason, the slab heating temperature is set to 1180°C or lower. On the other hand, if the slab heating temperature is less than 1050°C, the deformation resistance becomes too large, which increases the rolling load, so the lower limit of the slab heating temperature is set to 1050°C.
[0053] The conditions for the rough rolling are not particularly limited, and known rough rolling conditions may be applied.
[0054] The ferritic single-phase steel targeted in this embodiment has a small deformation resistance, so the temperature drop during rough rolling is significant. Therefore, the rough rolled material after rough rolling is reheated. The rough rolled material after rough rolling may be reheated so that the finishing temperature of the finish rolling falls within the range of 900°C to 1000°C.
[0055] The reheated rough rolled material is finish-rolled. Finish rolling may be performed under conditions where the finishing temperature is 900°C to 1000°C. If the finishing temperature is lower than 900°C, it becomes difficult to control the coiling temperature at the width end to 700°C or higher during the coiling process, and it becomes difficult to control the coiling temperature at the width end to be 50°C or lower than the coiling temperature at the width center. Therefore, the lower limit of the finishing temperature is set to 900°C. On the other hand, if the finishing temperature exceeds 1000°C, the cooling capacity after the finish rolling is insufficient, so that it becomes difficult to control the coiling temperature at the width end to 800°C or lower during the coiling process, which is the later process. Therefore, the upper limit of the finishing temperature is set to 1000°C.
[0056] The finish-rolled material after finish rolling is coiled under conditions where the coiling temperature at the widthwise ends is 700°C to 800°C and is 50°C or more lower than the coiling temperature at the widthwise center.
[0057] In general, increasing the hardness of a hot-rolled steel sheet and decreasing the DBTT are contradictory. However, the present inventors have found that if the coiling temperature of the finish-rolled material is lowered and the strain introduced into the steel sheet by the finish hot rolling is allowed to remain appropriately, both the hardness and the DBTT can be achieved. The reason why both the hardness and the DBTT can be achieved is considered to be that the hardness is increased by the remaining strain, and the low coiling temperature leaves a non-recrystallized structure, which improves toughness. In order to leave the strain appropriately, the coiling temperature at the width end is set to 800°C or less. On the other hand, if the coiling temperature at the width end is less than 700°C, the hardness is further increased, but the remaining strain becomes excessive, and the DBTT exceeds 0°C. Therefore, the coiling temperature at the width end is set to 700°C or more.
[0058] In addition, the coiling temperature at the widthwise ends is set to be at least 50°C lower than the coiling temperature at the widthwise center. If the entire width of the steel sheet were to be cooled to the same temperature as the widthwise ends, the magnetic properties would deteriorate. To achieve both stable pickling during the pickling process and the magnetic properties required for a non-oriented electrical steel sheet, the coiling temperatures at the widthwise ends and the widthwise center must be controlled separately. Note that the area of 25 mm from the side edge of the steel sheet in the widthwise direction is trimmed during pickling and when it is formed into a product. Therefore, even if the coiling temperature at the widthwise ends is set to be at least 50°C lower than the coiling temperature at the widthwise center, it will not affect the magnetic properties of the final product.
[0059] There are no particular limitations on the method for controlling the coiling temperature at the widthwise end portions to be at least 50° C. lower than the coiling temperature at the widthwise center portion. For example, the coiling temperatures at the widthwise end portions and the widthwise center portion may be controlled by spraying a liquid such as water, spraying a gas such as air or nitrogen, or contacting a solid with the end portions or the vicinity of the end portions during or after hot rolling, during or after coiling.
[0060] In addition, in the manufacturing method of the hot-rolled steel sheet for non-oriented electrical steel sheet according to the present embodiment, it is preferable that the bottom surface of the hot-rolled coil is not brought into contact with other hot-rolled coils for at least 30 minutes after the coiling. For example, if the bottom surfaces of the coils are stacked in a state where the coil cores are in a vertical hole within 30 minutes after the coiling, that is, stacking is performed, the temperature of the hot-rolled coil is still high and the strength of the steel sheet is low, so that the bottom surface of the coil is likely to be scratched. In addition, if the bottom surface of the hot-rolled coil comes into contact with other hot-rolled coils, the temperature of the bottom surface of the coil increases and the strain introduced in the finish hot rolling is alleviated, making it difficult to achieve both hardness and DBTT. Therefore, it is preferable that the bottom surface of the hot-rolled coil is not brought into contact with other hot-rolled coils for at least 30 minutes after the coiling.
[0061] The hot-rolled steel sheet manufactured under the above-mentioned manufacturing conditions has excellent hardness and toughness. The properties of this hot-rolled steel sheet can be evaluated by whether or not the sheet breaks when repeatedly bent. For example, a strip-shaped test piece is prepared by shearing a width of 30 mm and a length of 300 mm from the end of the width of the hot-rolled steel sheet, and while immersed in a bath at 0°C, it is bent 90° clockwise from the 6 o'clock position to the 9 o'clock position with a curvature radius of 40 mm, and then returned to the 6 o'clock position, bent 90° counterclockwise to the 3 o'clock position, and returned to the 6 o'clock position again. This is regarded as one cycle, and the number of cycles until the test piece breaks is measured. In the hot-rolled steel sheet for non-oriented electrical steel sheet according to this embodiment, this number of cycles is 10 or more. EXAMPLES
[0062] The effects of one embodiment of the present invention will be described in more detail with reference to the following examples, but the conditions in the examples are merely examples of conditions adopted to confirm the feasibility and effects of the present invention, and the present invention is not limited to these examples. Various conditions may be adopted in the present invention as long as they do not deviate from the gist of the present invention and the object of the present invention is achieved.
[0063] <Example 1> A slab having the chemical composition shown in Table 1 was hot rolled to a thickness of 2.5 mm under the manufacturing conditions of the hot rolling code shown in Table 2, and a hot-rolled steel sheet was coiled. Note that between hot rolling and coiling, the coiling temperature at the widthwise end and the widthwise center were controlled by selectively spraying a coolant near the widthwise end.
[0064] [Table 1]
[0065] [Table 2]
[0066] The chemical composition of the produced hot-rolled steel plate was equivalent to that of the slab. Test pieces were cut out from the produced hot-rolled steel plate, and the Vickers hardness at the plate width end and the plate width center, the ductile-brittle transition temperature at the plate width end and the plate width center, and the crown (the difference in plate thickness between the plate width end and the plate width center of the hot-rolled steel plate) were measured based on the above-mentioned method.
[0067] Furthermore, test pieces were prepared from the produced hot-rolled steel sheets, and a repeated bending test was carried out based on the above-mentioned method, and the number of cycles until the test pieces broke was measured.
[0068] The hot-rolled steel sheets were then pickled, cold-rolled to 0.5 mm, and finish-annealed to obtain non-oriented electrical steel sheets. During the pickling process, care was taken to avoid breaking the steel sheets, if necessary. Test pieces were cut out from the non-oriented electrical steel sheets after the finish-annealing, and the magnetic properties were measured according to the single sheet magnetic property test method of JIS C 2556 (2015).
[0069] [Table 3]
[0070] As shown in Table 3, the examples of the present invention had excellent repeated bending properties. In addition, although not shown in the table, the examples of the present invention also satisfied the magnetic properties. On the other hand, the comparative examples did not satisfy the chemical composition or manufacturing conditions, and therefore failed in at least one of manufacturability, repeated bending properties, or magnetic properties.
[0071] Although not shown in the table, steels with a Si content of less than 1.9% by mass were not tested because they do not have the above-mentioned problems. In addition, in steels with a Mn content of more than 1.5% by mass, the effect of Mn was saturated.
[0072] <Example 2> A slab having the chemical composition shown in Table 1 was hot rolled to a thickness of 2.5 mm under the manufacturing conditions of the hot rolling code shown in Table 2, and a hot-rolled steel sheet was coiled. Note that between hot rolling and coiling, the coiling temperature at the widthwise end and the widthwise center were controlled by selectively spraying a coolant near the widthwise end. Thereafter, the same evaluation as in Example 1 was performed. The chemical composition of the produced hot-rolled steel sheet was equivalent to that of the slab.
[0073] The hot-rolled steel sheets thus produced were subjected to pickling, cold rolling to 0.5 mm, and finish annealing to obtain non-oriented electrical steel sheets. In the pickling process, the steel sheets were pickled, if necessary, while paying attention not to break the steel sheets. Thereafter, the same evaluation as in Example 1 was performed.
[0074] [Table 4]
[0075] As shown in Table 4, the examples of the present invention had excellent repeated bending properties. In addition, although not shown in the table, the examples of the present invention also satisfied the magnetic properties. On the other hand, the comparative examples did not satisfy the chemical composition or manufacturing conditions, and therefore failed in at least one of manufacturability, repeated bending properties, or magnetic properties.
[0076] In addition, "defective hot rolling roll" shown in the table indicates that the thickness of the strip was thinner at the strip width end portion than at the strip width center portion due to deformation of the hot rolling roll. [Industrial Applicability]
[0077] According to the above-mentioned aspect of the present invention, it is possible to provide a hot-rolled steel sheet for non-oriented electrical steel sheet, which can realize stable sheet threading without breaking the steel sheet during the pickling process, and a manufacturing method thereof. Also, according to the above-mentioned aspect of the present invention, it is possible to suppress scratches and strike marks on the end faces in the sheet width direction of the hot-rolled coil. Therefore, it has a high industrial applicability.
Claims
1. Chemical composition, by mass percent C: 0.0050% or less, Si: 1.9% or more and 3.5% or less, Mn: 0.10% or more and 1.50% or less, Al: 0.10% or more and 1.50% or less, with the remainder being Fe and impurities; When the position 25 mm from the side edge of the steel plate along the plate width direction is defined as the plate width end portion, and the center position of the steel plate in the plate width direction is defined as the plate width center portion, The Vickers hardness at the sheet width end portion is 180 Hv or more, and the value obtained by subtracting the Vickers hardness at the sheet width center portion from the Vickers hardness at the sheet width end portion: ΔHv is 10 Hv or more and 100 Hv or less, The ductile-brittle transition temperature at the plate width end is 0° C. or less, and the value obtained by subtracting the ductile-brittle transition temperature at the plate width end from the ductile-brittle transition temperature at the plate width center: ΔDBTT is 10° C. or more and 100° C. or less; The value obtained by subtracting the thickness at the widthwise end portion from the thickness at the widthwise center portion is 50 μm or less. A hot-rolled steel sheet for non-oriented electrical steel sheet, characterized in that
2. A method for producing a hot-rolled steel sheet for non-oriented electrical steel sheet according to claim 1, Chemical composition, by mass%, C: 0.0050% or less Si: 1.9% or more and 3.5% or less, Mn: 0.10% or more and 1.50% or less, Al: 0.10% or more and 1.50% or less, and the balance being Fe and impurities, the slab is heated to 1050°C to 1180°C, The heated slab is roughly rolled, Reheating the rough rolled material after the rough rolling, The reheated rough rolled material is finish rolled under conditions where the finishing temperature is 900°C to 1000°C, The finish-rolled material after the finish rolling is coiled under the condition that the coiling temperature at the widthwise end portion is 700° C. or more and 800° C. or less, and the coiling temperature at the widthwise end portion is 50° C. or more lower than the coiling temperature at the widthwise center portion. The present invention relates to a method for producing a hot-rolled steel sheet for use as a non-oriented electrical steel sheet.
3. The bottom surface of the hot-rolled coil is not allowed to come into contact with other hot-rolled coils for at least 30 minutes after the coiling. The method for producing a hot-rolled steel sheet for a non-oriented electrical steel sheet according to claim 2 .
Citation Information
Patent Citations
Production of nonoriented silicon steel sheet having high magnetic flux density and reduced in iron loss
JP1992006220A
Production of silicon steel sheet and hot rolled sheet stock for silicon steel sheet
JP2000226616A
Non-oriented magnetic steel sheet with high strength
JP2008050685A
Method of manufacturing nondirectional electromagnetic steel sheet excellent in magnetic property
JP2010242186A
Hot rolled sheet for nonoriented magnetic steel sheet and production method therefor, and nonoriented magnetic steel sheet excellent in magnetic property and production method therefor