Method for manufacturing a switching device

By employing non-plasma state oxidizing gases with varying concentrations to form silicon oxide gate insulating films on gallium nitride semiconductor layers, the method addresses the issue of interface oxidation, enhancing channel mobility and reducing gate leakage in switching devices.

JP7583408B2Active Publication Date: 2024-11-14DENSO CORP +3
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021029177
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-25
Publication Date
2024-11-14
Estimated Expiration
2041-02-25

AI Technical Summary

Technical Problem

Existing manufacturing methods for switching devices using oxygen plasma to form gate insulating films on gallium nitride semiconductor layers result in oxidation of the semiconductor layer, leading to the formation of a gallium oxide layer at the interface, which deteriorates device characteristics.

Method used

A method involving the use of non-plasma state oxidizing gases with varying concentrations to form silicon oxide gate insulating films, where a low-concentration oxidizing gas forms the first gate insulating film to minimize semiconductor oxidation and a high-concentration oxidizing gas forms the second gate insulating film to reduce carbon incorporation, thereby enhancing insulation properties.

Benefits of technology

This approach suppresses the formation of gallium oxide layers at the interface, improving channel mobility and reducing gate leakage in the switching device by forming gate insulating films with high insulation properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583408000001
    Figure 0007583408000001
  • Figure 0007583408000002
    Figure 0007583408000002
  • Figure 0007583408000003
    Figure 0007583408000003
Patent Text Reader

Abstract

To provide a method for manufacturing a switching device in which a gate insulating film with high insulation properties is formed while suppressing formation of a gallium oxide layer at an interface between the gate insulating film and the gallium nitride semiconductor layer.SOLUTION: A method for manufacturing a switching device comprises the steps of: forming a first gate insulating film 21 by supplying a first organic film forming material including silicon to a surface of a gallium nitride semiconductor substrate 12 and supplying a first reaction gas including an oxidizing gas to the surface of the gallium nitride semiconductor substrate in a non-plasma state; and forming a second gate insulating film 22 by supplying a second organic film forming material including silicon to the surface of the first gate insulating film and supplying a second reaction gas including oxidizing gas to the surface of the first gate insulating film in a non-plasma state. Concentration of the oxidizing gas in the first reaction gas is lower than concentration of the oxidizing gas in the second reaction gas.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The technology disclosed in this specification relates to a method for manufacturing a switching device.

[0002] Patent Document 1 discloses a method for manufacturing a switching device. This manufacturing method includes a first gate insulating film forming step and a second gate insulating film forming step. In the first gate insulating film forming step, a first gate insulating film made of silicon oxide is formed on a gallium nitride semiconductor layer by ALD (atomic layer deposition) using ozone as an oxidizing agent. In the second step, a second gate insulating film made of silicon oxide is formed on the first gate insulating film by ALD using oxygen plasma as an oxidizing agent. A gate electrode is formed on the second gate insulating film.

[0003] In the first step, ozone, which has a relatively low oxidizing power, is used as the oxidizing agent, so that the first gate insulating film can be formed on the gallium nitride semiconductor layer while suppressing the oxidation of the gallium nitride semiconductor layer. By suppressing the oxidation of the gallium nitride semiconductor layer, the characteristics of the switching device can be improved. However, in the first step, ozone, which has a relatively low oxidizing power, is used as the oxidizing agent, so that carbon is easily incorporated into the first gate insulating film. Therefore, the first gate insulating film cannot suppress gate leakage. In the second step, oxygen plasma, which has a high oxidizing power, is used as the oxidizing agent, so that carbon is unlikely to be incorporated into the second gate insulating film. Therefore, a second gate insulating film having high insulating properties can be formed, and gate leakage can be suppressed. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2019-071497 A Summary of the Invention [Problem to be solved by the invention]

[0005] In the manufacturing method of Patent Document 1, a second gate insulating film is formed on a first gate insulating film by using oxygen plasma with high oxidizing power as an oxidizing agent. Experiments conducted by the inventors have revealed that when an oxidizing gas in a plasma state with high oxidizing power such as oxygen plasma is used in the second step, the gallium nitride semiconductor layer below the first gate insulating film is oxidized. As a result, a gallium oxide layer is formed at the interface between the first gate insulating film and the gallium nitride semiconductor layer. When a gallium oxide layer is formed at the interface, the characteristics of the switching device are degraded. This specification proposes a technology for forming a gate insulating film with high insulation properties while suppressing the formation of a gallium oxide layer at the interface between the gate insulating film and the gallium nitride semiconductor layer. [Means for solving the problem]

[0006] The present specification discloses a method for manufacturing a switching device, comprising the steps of: forming a first gate insulating film made of silicon oxide on a gallium nitride semiconductor layer by supplying a first organic film forming source containing silicon to a surface of the gallium nitride semiconductor layer and supplying a first reactive gas containing an oxidizing gas to the surface of the gallium nitride semiconductor layer in a non-plasma state; and forming a second gate insulating film made of silicon oxide on the first gate insulating film by supplying a second organic film forming source containing silicon to the surface of the first gate insulating film and supplying a second reactive gas containing an oxidizing gas to the surface of the first gate insulating film in a non-plasma state. The oxidizing gas contained in the first reactive gas and the oxidizing gas contained in the second reactive gas are the same type of gas. The concentration of the oxidizing gas in the first reactive gas is lower than the concentration of the oxidizing gas in the second reactive gas.

[0007] The switching device may be any switching device having a gate insulating film, for example, a field effect transistor (FET) or a high electron mobility transistor (HEMT).

[0008] The gallium nitride semiconductor layer is a semiconductor layer mainly composed of gallium nitride. For example, the gallium nitride semiconductor layer may be made of gallium nitride (GaN), indium gallium nitride (InGaN), aluminum gallium nitride (AlGaN), or indium aluminum gallium nitride (InAlGaN).

[0009] Silicon oxide is a compound containing a bond between Si and O. For example, silicon oxide may be SiO2 or SiON.

[0010] The first organic film-forming raw material and the second organic film-forming raw material may be the same kind of raw material or different kinds of raw materials.

[0011] In this manufacturing method, in the step of forming a first gate insulating film, a first organic film forming raw material containing silicon is supplied to the surface of the gallium nitride semiconductor layer, and a first reactive gas containing an oxidizing gas is supplied to the surface of the gallium nitride semiconductor layer in a non-plasma state, thereby forming a first gate insulating film made of silicon oxide. Here, a first reactive gas having a low concentration of oxidizing gas is used. Therefore, the first gate insulating film can be formed while suppressing the formation of a gallium oxide layer at the interface between the gallium nitride semiconductor layer and the first gate insulating film. In addition, since the concentration of the oxidizing gas in the first reactive gas is low, carbon is easily incorporated into the first gate insulating film. Therefore, the insulating property of the first gate insulating film is not so high. In the step of forming a second gate insulating film, a second organic film forming raw material containing silicon is supplied to the surface of the first gate insulating film, and a second reactive gas containing an oxidizing gas is supplied to the surface of the first gate insulating film in a non-plasma state, thereby forming a second gate insulating film made of silicon oxide on the first gate insulating film. Here, a second reactive gas having a high concentration of oxidizing gas is used. Therefore, carbon is not easily incorporated into the second gate insulating film. Therefore, the second gate insulating film having high insulating properties can be formed. Therefore, the gate insulating film having the first gate insulating film and the second gate insulating film has high insulating properties as a whole. This gate insulating film can suppress gate leakage. In addition, the second reactive gas is supplied to the surface of the first gate insulating film in a non-plasma state. Since the oxidizing power of the second reactive gas in a non-plasma state is not as high as the oxidizing power of the oxidizing gas in a plasma state, the surface of the gallium nitride semiconductor layer below the first gate insulating film is suppressed from being oxidized. Therefore, the second gate insulating film can be formed while suppressing the formation of a gallium oxide layer at the interface between the gallium nitride semiconductor layer and the first gate insulating film. As described above, according to this manufacturing method, a gate insulating film having high insulating properties can be formed while suppressing the formation of a gallium oxide layer at the interface between the gate insulating film and the gallium nitride semiconductor layer. [Brief description of the drawings]

[0012] [Figure 1]1 is a cross-sectional view of a switching device 10. FIG. [Diagram 2] 3A to 3C are explanatory diagrams of a manufacturing method of the switching device 10. [Diagram 3] 3A to 3C are explanatory diagrams of a manufacturing method of the switching device 10. [Figure 4] 3A to 3C are explanatory diagrams of a manufacturing method of the switching device 10. [Diagram 5] 3A to 3C are explanatory diagrams of a manufacturing method of the switching device 10. [Figure 6] An explanatory diagram of the mist CVD method. [Figure 7] 1 is a graph showing the results of XPS analysis of the interface between a gate insulating film and a gallium nitride semiconductor substrate. [Figure 8] 4 is a graph showing the mobility of the switching device 10 manufactured by the manufacturing method of the first embodiment. [Figure 9] 4 is a graph showing the mobility of a switching device 10 manufactured by a manufacturing method using oxygen plasma. [Figure 10] 1 is a graph showing the carbon concentration distribution in a gate insulating film. [Figure 11] 1 is a graph showing the relationship between an electric field applied to a gate insulating film and a leakage current flowing through the gate insulating film. [Figure 12] An explanatory diagram of the spray method. [Figure 13] FIG. [Figure 14] FIG. [Figure 15] FIG. 1 is an explanatory diagram of an ALD method using a non-plasma oxidizing gas. [Figure 16] 5 is a cross-sectional view of a switching device 500. FIG. [Figure 17] 5A to 5C are explanatory diagrams of a manufacturing method of the switching device 500. [Figure 18] 5A to 5C are explanatory diagrams of a manufacturing method of the switching device 500. [Figure 19] 5A to 5C are explanatory diagrams of a manufacturing method of the switching device 500. [Figure 20] 5A to 5C are explanatory diagrams of a manufacturing method of the switching device 500. [Figure 21]5A to 5C are explanatory diagrams of a manufacturing method of the switching device 500. [Figure 22] 5A to 5C are explanatory diagrams of a manufacturing method of the switching device 500. [Diagram 23] 5A to 5C are explanatory diagrams of a manufacturing method of the switching device 500. [Figure 24] 6 is a cross-sectional view of a switching device 600. FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] In the method for manufacturing a switching device according to an example disclosed in the present specification, the first organic film forming raw material may be a first solution containing a silicon-containing film forming raw material dissolved therein and containing an organic solvent, and the second organic film forming raw material may be a second solution containing a silicon-containing film forming raw material dissolved therein and containing an organic solvent. In this case, in one configuration, a mist coating method may be used. That is, in the step of forming the first gate insulating film, a mist may be generated from the first solution, and the mist of the first solution may be supplied to the surface of the gallium nitride semiconductor layer together with the first reactive gas. Also, in the step of forming the second gate insulating film, a mist may be generated from the second solution, and the mist of the second solution may be supplied to the surface of the first gate insulating film together with the second reactive gas. Also, in another configuration, a spray coating method may be used. That is, in the step of forming the first gate insulating film, the first reactive gas may be supplied to the surface of the gallium nitride semiconductor layer while spray coating the first solution on the surface of the gallium nitride semiconductor layer. In the step of forming the second gate insulating film, the second reactive gas may be supplied to the surface of the first gate insulating film while spray-coating the second solution on the surface of the first gate insulating film. In another configuration, an inkjet method may be used. That is, in the step of forming the first gate insulating film, the first reactive gas may be supplied to the surface of the gallium nitride semiconductor layer while coating the first solution on the surface of the gallium nitride semiconductor layer by an inkjet method. In the step of forming the second gate insulating film, the second reactive gas may be supplied to the surface of the gallium nitride semiconductor layer while coating the second solution on the surface of the gallium nitride semiconductor layer by an inkjet method. In another configuration, a bubbling method may be used. That is, in the step of forming the first gate insulating film, bubbles may be generated in the first solution to generate droplets of the first solution, and the droplets of the first solution may be supplied to the surface of the gallium nitride semiconductor layer together with the first reactive gas.In the step of forming the second gate insulating film, droplets of the second solution may be generated by generating bubbles in the second solution, and the droplets of the second solution may be supplied to the surface of the first gate insulating film together with the second reactive gas.

[0014] According to these configurations, the first gate insulating film and the second gate insulating film can be formed suitably.

[0015] In the method for manufacturing a switching device according to an example disclosed herein, in the step of forming the first gate insulating film, a step of supplying a first source gas containing the first organic film formation raw material to the surface of the gallium nitride semiconductor layer and a step of supplying the first reactive gas to the surface of the gallium nitride semiconductor layer may be alternately repeated multiple times. In the step of forming the second gate insulating film, a step of supplying a second source gas containing the second organic film formation raw material to the surface of the first gate insulating film and a step of supplying the first reactive gas to the surface of the first gate insulating film may be alternately repeated multiple times.

[0016] According to this configuration, the first gate insulating film and the second gate insulating film can be preferably formed.

[0017] In any of the manufacturing methods disclosed in the present specification, the oxidizing gas contained in the first reactive gas and the oxidizing gas contained in the second reactive gas may be ozone.

[0018] In any of the manufacturing methods disclosed in the present specification, the second gate insulating film may have an average carbon concentration lower than the average carbon concentration of the first gate insulating film. In this case, the carbon concentration of at least a part of the second gate insulating film is 3×10 19 atoms / cm 3 It may be less than.

[0019] According to these configurations, gate leakage can be effectively suppressed.

[0020] Any of the manufacturing methods disclosed in this specification may not include a step of exposing the first gate insulating film and the second gate insulating film to an oxidizing gas in a plasma state after performing the step of forming the first gate insulating film.

[0021] This configuration effectively suppresses the formation of a gallium oxide layer at the interface between the gate insulating film and the gallium nitride semiconductor layer.

[0022] In one example of the manufacturing method disclosed in the present specification, after performing the step of forming the second gate insulating film, no gallium oxide layer may be present at the interface between the gallium nitride semiconductor layer and the first gate insulating film, or the gallium oxide layer present at the interface between the gallium nitride semiconductor layer and the first gate insulating film may have a thickness of 1 nm or less.

[0023] This configuration can further improve the characteristics of the switching device.

[0024] The switching device 10 of the embodiment shown in FIG. 1 is a metal oxide semiconductor field effect transistor (MOSFET). The switching device 10 has a gallium nitride semiconductor substrate 12. The gallium nitride semiconductor substrate 12 has a high-concentration n-type layer 14a, a buffer layer 14b, a drift layer 14c, a body layer 16, a source layer 18, and a drain layer 20. The high-concentration n-type layer 14a is provided in a range including the lower surface of the gallium nitride semiconductor substrate 12. The buffer layer 14b is an n-type layer having a lower n-type impurity concentration than the high-concentration n-type layer 14a, and is provided on the high-concentration n-type layer 14a. The drift layer 14c is an n-type layer having an n-type impurity concentration equivalent to that of the buffer layer 14b, and is provided on the buffer layer 14b. The body layer 16 is a p-type layer and is provided on the drift layer 14c. The source layer 18 and the drain layer 20 are n-type layers and are provided on the body layer 16. The source layer 18 and the drain layer 20 are provided in a range that partially includes the upper surface 12a of the gallium nitride semiconductor substrate 12. The source layer 18 and the drain layer 20 are separated from each other. That is, the body layer 16 is provided between the source layer 18 and the drain layer 20, and the source layer 18 is separated from the drain layer 20 by the body layer 16.

[0025] On the upper portion of the gallium nitride semiconductor substrate 12, a gate insulating film 23, a gate electrode 24, a source electrode 26, and a drain electrode 28 are disposed.

[0026] The gate insulating film 23 has a first gate insulating film 21 and a second gate insulating film 22. The first gate insulating film 21 and the second gate insulating film 22 are made of silicon oxide (for example, SiO2, SiON, etc.). The first gate insulating film 21 is disposed on the gallium nitride semiconductor substrate 12. The first gate insulating film 21 extends from the surface of the source layer 18 to the surface of the drain layer 20 on the upper surface 12a of the gallium nitride semiconductor substrate 12. The first gate insulating film 21 is in contact with the source layer 18, the body layer 16, and the drain layer 20 on the upper surface 12a of the gallium nitride semiconductor substrate 12. The second gate insulating film 22 is disposed on the first gate insulating film 21. The second gate insulating film 22 covers the entire upper surface of the first gate insulating film 21.

[0027] The gate electrode 24 is made of a conductor (for example, a metal or polysilicon). The gate electrode 24 is disposed on the second gate insulating film 22. The gate electrode 24 extends from an upper portion of the source layer 18 to an upper portion of the drain layer 20. The gate electrode 24 faces the source layer 18, the body layer 16, and the drain layer 20 via the gate insulating film 23.

[0028] The source electrode 26 is made of a conductor. The source electrode 26 is disposed on the source layer 18. The source electrode 26 is in ohmic contact with the source layer 18.

[0029] The drain electrode 28 is made of a conductor. The drain electrode 28 is disposed on the drain layer 20. The drain electrode 28 is in ohmic contact with the drain layer 20.

[0030] When a potential equal to or higher than a threshold is applied to the gate electrode 24, a channel is formed in the drain layer 20 directly below the gate insulating film 23. The source layer 18 and the drain layer 20 are connected by the channel. In this state, when a potential higher than that of the source electrode 26 is applied to the drain electrode 28, electrons flow from the source layer 18 to the drain layer 20 through the channel. That is, the switching device 10 is turned on. As will be described in detail later, in the switching device 10, the interface state density at the interface 30 between the first gate insulating film 21 and the gallium nitride semiconductor substrate 12 is low. Therefore, the channel mobility of the switching device 10 is high. Also, as will be described in detail later, in the switching device 10, the second gate insulating film 22 has high insulating properties. Therefore, in the gate insulating film 23, gate leakage is unlikely to occur. EXAMPLES

[0031] Next, a method for manufacturing the switching device 10 of Example 1 will be described. Fig. 2 shows the gallium nitride semiconductor substrate 12 before processing. The switching device 10 is manufactured from the gallium nitride semiconductor substrate 12 of Fig. 2. The entire gallium nitride semiconductor substrate 12 shown in Fig. 2 is composed of a high-concentration n-type layer 14a. The high-concentration n-type layer 14a has a thickness of about 400 µm and a concentration of about 1 × 10 18 cm -3 The n-type impurity concentration is

[0032] First, as shown in FIG 3, a buffer layer 14b made of gallium nitride is epitaxially grown on a high-concentration n-type layer 14a. Here, the n-type impurity concentration of the buffer layer 14b is about 2×10 16 cm -3 The buffer layer 14b is formed so that the thickness of the buffer layer 14b is about 0.3 μm. Next, as shown in FIG. 3, the drift layer 14c made of gallium nitride is epitaxially grown on the buffer layer 14b. Here, the n-type impurity concentration of the drift layer 14c is about 2×10 16 cm -3The drift layer 14c is formed so that the thickness of the drift layer 14c is about 1.0 μm. Next, as shown in FIG. 3, the body layer 16 made of gallium nitride is epitaxially grown on the drift layer 14c. Here, the body layer 16 is doped with a p-type impurity (e.g., magnesium) at a concentration of about 5×10 17 cm -3 The body layer 16 is formed so that the p-type impurity in the body layer 16 has a concentration of 0.1 μm and the thickness of the body layer 16 is about 1.5 μm. The gallium nitride semiconductor substrate 12 is then annealed in a nitrogen atmosphere at about 850° C. for about 5 minutes to activate the p-type impurity in the body layer 16.

[0033] Next, n-type impurities (e.g., silicon) are selectively introduced into the body layer 16 from the upper surface 12a of the gallium nitride semiconductor substrate 12 at a concentration of about 3×10 15 cm -2 The gallium nitride semiconductor substrate 12 is then annealed in its entirety in a nitrogen atmosphere at about 1000° C. for about 5 minutes to activate the implanted n-type impurities. As a result, a source layer 18 and a drain layer 20 are formed in parts of the surface layer of the body layer 16, as shown in FIG.

[0034] Next, the upper surface 12a of the gallium nitride semiconductor substrate 12 is cleaned. Next, a gate insulating film forming step is performed. In the gate insulating film forming step, as shown in FIG. 5, a gate insulating film 23 made of silicon oxide is formed on the upper surface 12a. That is, a first gate insulating film 21 is formed on the upper surface 12a, and a second gate insulating film 22 is formed on the first gate insulating film 21. In the gate insulating film forming step of Example 1, the first gate insulating film 21 and the second gate insulating film 22 are formed by mist CVD (chemical vapor deposition).

[0035] 6 shows a mist CVD apparatus 80 for performing a mist CVD method. The mist CVD apparatus 80 includes a furnace 82, a mist generator 84, a carrier gas supply source 86, a first reactive gas supply source 88a, and a second reactive gas supply source 88b.

[0036] The furnace 82 has a chamber 82a. The gallium nitride semiconductor substrate 12 can be placed in the chamber 82a. The furnace 82 has a built-in heater and can heat the gallium nitride semiconductor substrate 12 in the chamber 82a.

[0037] The mist generating device 84 includes a mist generating tank 84a, a container 84b, and an ultrasonic vibrator 84c. A solution 84d is stored in the mist generating tank 84a. The solution 84d is obtained by dissolving a film-forming raw material containing silicon in an organic solvent. For example, silicon compounds such as polysilazane, tetraethoxysilane, triethoxysilane, hexamethyldisiloxane, hexamethyldisilazane, and hexamethyldisilane can be used as the film-forming raw material containing silicon. Butyl acetate, dimethyl ether, methyl acetate, acetonitrile, and dibutyl ether can be used as the organic solvent. The container 84b stores a liquid 84e (for example, water). The lower part of the mist generating tank 84a is immersed in the liquid 84e. An ultrasonic vibrator 84c is fixed to the bottom surface of the container 84b. The ultrasonic vibrator 84c applies ultrasonic waves to the liquid 84e. The ultrasonic waves applied to the liquid 84e are transmitted to the solution 84d in the mist generating tank 84a via the liquid 84e. Then, the liquid surface of the solution 84d vibrates, and mist 83 of the solution 84d is generated in the space above the solution 84d. In this manner, the mist generating device 84 generates mist 83 of the solution 84d in the mist generating tank 84a. The mist generating tank 84a is connected to the furnace 82 via a raw material supply pipe 94. The mist 83 is supplied from the mist generating tank 84a to the furnace 82 via the raw material supply pipe 94. The mist 83 that has flowed through the furnace 82 to the downstream end is discharged to the outside of the furnace 82.

[0038] The carrier gas supply source 86 is connected to the mist generating tank 84a via a carrier gas supply pipe 90. The carrier gas supply source 86 supplies a carrier gas (for example, an inert gas such as argon) to the mist generating tank 84a.

[0039] The first reactive gas supply source 88a and the second reactive gas supply source 88b are connected to the middle of the raw material supply pipe 94 via a reactive gas supply pipe 92. The first reactive gas supply source 88a supplies a first reactive gas to the raw material supply pipe 94. The second reactive gas supply source 88b supplies a second reactive gas to the raw material supply pipe 94. In the mist CVD apparatus 80, the reactive gas supply source to be used can be switched between the first reactive gas supply source 88a and the second reactive gas supply source 88b. The first reactive gas contains an oxidizing gas (ozone in this embodiment). The second reactive gas contains an oxidizing gas (ozone in this embodiment). That is, the oxidizing gas contained in the first reactive gas and the oxidizing gas contained in the second reactive gas are the same type of gas. The concentration of the oxidizing gas in the first reactive gas is lower than the concentration of the oxidizing gas in the second reactive gas. The concentration of the oxidizing gas in the first reactive gas is 10 g / m 3 and the concentration of the oxidizing gas in the second reactant gas is less than 10 g / m 3 That's all.

[0040] The gate insulating film forming step includes a first gate insulating film forming step of forming a first gate insulating film 21 and a second gate insulating film forming step of forming a second gate insulating film 22.

[0041] In the first gate insulating film forming step, first, the gallium nitride semiconductor substrate 12 is placed in the chamber 82a of the furnace 82. Here, the gallium nitride semiconductor substrate 12 is placed in the chamber 82a in a direction in which the upper surface 12a is exposed to the mist flowing in the chamber 82a. Next, the gallium nitride semiconductor substrate 12 is heated by the furnace 82. During the first gate insulating film forming step and the second gate insulating film forming step, the temperature of the gallium nitride semiconductor substrate 12 is maintained at about 400°C. Next, the ultrasonic vibrator 84c is operated to generate the mist 83 from the solution 84d. At the same time, the supply of the carrier gas from the carrier gas supply source 86 to the mist generating tank 84a is started, and the supply of the first reaction gas from the first reaction gas supply source 88a to the raw material supply pipe 94 is started. The carrier gas flowing from the carrier gas supply pipe 90 into the mist generating tank 84a flows into the raw material supply pipe 94 together with the mist 83 in the mist generating tank 84a. In the raw material supply pipe 94, the mist 83 flows toward the furnace 82 together with the carrier gas. In the middle of the raw material supply pipe 94, the first reaction gas flows from the reaction gas supply pipe 92 into the raw material supply pipe 94. Therefore, in the part of the raw material supply pipe 94 downstream of the junction with the reaction gas supply pipe 92, the mist 83 flows toward the furnace 82 together with the carrier gas and the first reaction gas. When the mist 83, the carrier gas, and the first reaction gas reach the downstream end of the raw material supply pipe 94, they flow into the chamber 82a of the furnace 82. A part of the mist 83 flowing in the chamber 82a adheres to the upper surface 12a of the gallium nitride semiconductor substrate 12. Then, the organic solvent contained in the mist 83 adhering to the upper surface 12a volatilizes, and the film formation raw material containing silicon is fixed to the upper surface 12a. At the same time that the silicon-containing film-forming raw material is fixed to the upper surface 12a, the film-forming raw material is oxidized by the first reactive gas to become silicon oxide. Therefore, the first gate insulating film 21 made of silicon oxide grows to a thickness of, for example, 10 nm on the upper surface 12a of the gallium nitride semiconductor substrate 12.

[0042] When the first gate insulating film 21 grows to a predetermined thickness, the process moves from the first gate insulating film forming process to the second gate insulating film forming process. In the second gate insulating film forming process, the reactive gas supply source used in the mist CVD device 80 is switched from the first reactive gas supply source 88a to the second reactive gas supply source 88b. Therefore, the second reactive gas is supplied to the upper surface of the first gate insulating film 21 together with the mist 83. Since the organic solvent contained in the mist 83 attached to the upper surface of the first gate insulating film 21 volatilizes, the film forming raw material containing silicon is fixed to the upper surface of the first gate insulating film 21. At the same time, the film forming raw material fixed to the upper surface of the first gate insulating film 21 is oxidized by the second reactive gas to become silicon oxide. Therefore, the second gate insulating film 22 made of silicon oxide is grown, for example, to 90 nm on the first gate insulating film 21.

[0043] After the gate insulating film 23 (that is, the first gate insulating film 21 and the second gate insulating film 22) is formed to a thickness of 100 nm, the gallium nitride semiconductor substrate 12 is annealed in a nitrogen atmosphere at about 800° C. for about 5 minutes.

[0044] 1, contact holes 26a, 28a are formed in the gate insulating film 23 above the source layer 18 and above the drain layer 20. Next, the gate electrode 24, the source electrode 26, and the drain electrode 28 are formed. Thereafter, if necessary, a hydrogen sintering process is performed on the gallium nitride semiconductor substrate 12. Through the above steps, the switching device 10 shown in FIG. 1 is completed.

[0045] FIG. 7 shows the results of an experiment verifying the presence or absence of a gallium oxide layer in the switching device 10. Graphs A to C in FIG. 7 show the results of XPS analysis of GaLMM for three samples of the switching device 10. Graph A shows the results of XPS analysis of the surface of the body layer 16 in a state where the gate insulating film 21 is not formed (the state of FIG. 4). That is, graph A shows the results of XPS analysis of the surface of the body layer 16 in a state where no gallium oxide layer exists. Graph B shows the results of XPS analysis of the interface 30 between the gate insulating film 21 and the body layer 16 formed by the gate insulating film forming process of Example 1. Graph C shows the results of XPS analysis of the interface 30 between the gate insulating film 21 and the body layer 16 formed by the ALD method using oxygen plasma (oxygen gas in a plasma state). In the measurements of graphs B and C, the thickness of the gate insulating film 21 was reduced to about 5 nm by wet etching the gate insulating film 21, and then an XPS analysis was performed on the interface 30 between the gate insulating film 21 and the body layer 16.

[0046] As shown in FIG. 7, graph B is almost identical to graph A, whereas graph C has a clear deviation from graph A. As shown in Noritake Isomura at el (2020). X-ray photoelectron spectroscopy insights on interfaces between SiO2 films and GaN substrates: differences due to depositional technique, Jpn. J. Appl. Phys. 59, 090902 (2020), by comparing the results of XPS analysis of the interface between the gate insulating film and the gallium nitride semiconductor, it is possible to detect whether or not a gallium oxide layer is present at the interface. According to this method, a gallium oxide layer having a thickness of more than 1 nm can be detected. As described above, graph A is the result of XPS analysis performed on the surface of the body layer 16 in a state in which no gallium oxide layer is present. Since graph B is identical to graph A, in the sample of graph B, no gallium oxide layer is present at the interface 30, or the thickness of the gallium oxide layer present at the interface 30 is 1 nm or less (below the detection limit). That is, when the gate insulating film 21 is formed by the manufacturing method of Example 1, a gallium oxide layer is not formed at the interface 30, or the thickness of the gallium oxide layer formed at the interface 30 is 1 nm or less. Since the graph C is shifted from the graph A, the sample of the graph C has a gallium oxide layer with a thickness of more than 1 nm at the interface 30. That is, when the gate insulating film 21 is formed by the ALD method using oxygen plasma, a gallium oxide layer with a thickness of more than 1 nm is formed at the interface 30.

[0047] As described above, according to the manufacturing method of the first embodiment, the formation of a gallium oxide layer can be suppressed. The reason is considered as follows. When an oxidizing gas in a plasma state is used when forming a gate insulating film, the oxidizing power of the oxidizing gas in a plasma state is too high, so that the surface of the gallium nitride semiconductor substrate is oxidized. Even when an oxidizing gas in a plasma state is used in a state in which the surface of the gallium nitride semiconductor substrate is covered with a silicon oxide film, the gallium nitride semiconductor substrate below the silicon oxide film is oxidized. In this way, when an oxidizing gas in a plasma state is used, a gallium oxide layer is formed at the interface between the gate insulating film and the gallium nitride semiconductor substrate. In contrast, in the first gate insulating film forming step of the first embodiment, a first reactive gas containing an oxidizing gas is used in a non-plasma state. That is, a film forming raw material containing silicon is oxidized by the first reactive gas in a non-plasma state on the gallium nitride semiconductor substrate 12, so that the first gate insulating film 21 (i.e., a silicon oxide film) is formed. Since the concentration of the oxidizing gas in the first reactive gas is low and the first reactive gas is in a non-plasma state, the oxidizing power of the first reactive gas is not so high. Therefore, the upper surface 12a of the gallium nitride semiconductor substrate 12 can be prevented from being oxidized during the first gate insulating film forming process. In addition, in the second gate insulating film forming process of Example 1, the second reactive gas containing an oxidizing gas is used in a non-plasma state. That is, the second gate insulating film 22 (i.e., a silicon oxide film) is formed by oxidizing the film forming raw material containing silicon on the first gate insulating film 21 with the second reactive gas in a non-plasma state. Since the concentration of the oxidizing gas in the second reactive gas is higher than the concentration of the oxidizing gas in the first reactive gas, the oxidizing power of the second reactive gas is higher than the oxidizing power of the first reactive gas. However, since the second reactive gas is in a non-plasma state, the oxidizing power of the second reactive gas is not strong enough to oxidize the gallium nitride semiconductor substrate 12 below the first gate insulating film 21. Therefore, the upper surface 12a of the gallium nitride semiconductor substrate 12 can be prevented from being oxidized during the second gate insulating film forming process. Therefore, according to this manufacturing method, it is possible to prevent a gallium oxide layer from being formed at the interface 30 between the gate insulating film 23 and the gallium nitride semiconductor substrate 12.Moreover, in the manufacturing method of Example 1, no oxidizing gas in a plasma state is used in the gate insulating film formation step, and the gate insulating film 23 is not exposed to the oxidizing gas in a plasma state after the gate insulating film 23 is formed. This also makes it possible to suppress the formation of a gallium oxide layer at the interface 30. Therefore, according to the manufacturing method of Example 1, it is possible to manufacture a switching device 10 in which no gallium oxide layer is present at the interface 30, or in which the gallium oxide layer present at the interface 30 has a thickness of 1 nm or less.

[0048] When the formation of a gallium oxide layer at the interface 30 is suppressed, the interface state density at the interface 30 can be reduced. In the switching device 10, a channel is formed along the interface 30, so that the channel mobility can be improved by reducing the interface state density at the interface 30. FIG. 8 shows the results of measuring the channel mobility of the switching device 10 manufactured by the manufacturing method of Example 1. As shown in FIG. 8, in this case, the channel mobility of 150 cm 2 A mobility exceeding 1000 .mu.m / Vs was obtained. FIG. 9 shows the results of measuring the channel mobility of the switching device 10 when the gate insulating film 23 was formed by the ALD method using oxygen plasma. As shown in FIG. 9, in this case, the mobility was about 56 cm.sup.2 at most. 2 / Vs. Thus, according to the manufacturing method of Example 1, the formation of a gallium oxide layer at the interface 30 can be suppressed, and a switching device 10 with high channel mobility can be manufactured.

[0049] FIG. 10 also shows the carbon concentration inside the gate insulating film. Graph D in FIG. 10 shows the result of measuring the carbon concentration in a sample in which the first gate insulating film 21 is formed on the gallium nitride semiconductor substrate 12 (i.e., a sample in which a silicon oxide film is formed using a first reactive gas having a low concentration of oxidizing gas). Graph E in FIG. 10 shows the result of measuring the carbon concentration in a sample in which the second gate insulating film 22 is formed on the gallium nitride semiconductor substrate 12 (i.e., a sample in which a silicon oxide film is formed using a second reactive gas having a high concentration of oxidizing gas). As shown in FIG. 10, a lower average carbon concentration was obtained in graph E (i.e., the second gate insulating film 22) than in graph D (i.e., the first gate insulating film 21). In particular, as shown in graph E, in most part of the second gate insulating film 22 (a range of more than half of the thickness), the average carbon concentration was 3×10 19 atoms / cm 3 Thus, an extremely low carbon concentration of less than 1000 ppm was obtained. The reason why the carbon concentration in the second gate insulating film 22 is lower than that in the first gate insulating film 21 is considered to be as follows. When the gate insulating film (i.e., silicon oxide film) is grown, carbon contained in the organic solvent is incorporated into the silicon oxide film. When the second gate insulating film 22 is formed using the second reactive gas having a high concentration of oxidizing gas, the growth rate of the silicon oxide film is faster than when the first gate insulating film 21 is formed using the first reactive gas having a low concentration of oxidizing gas. For this reason, it is considered that carbon is less likely to be incorporated into the silicon oxide film in the second gate insulating film forming process than in the first gate insulating film forming process. Also, most of the carbon attached to the upper surface of the gallium nitride semiconductor substrate 12 is oxidized and removed by the oxidizing gas. When the second gate insulating film is formed using the second reactive gas having a high concentration of oxidizing gas, carbon is more likely to be removed by oxidation than when the first gate insulating film is formed using the first reactive gas having a low concentration of oxidizing gas. Therefore, it is considered that carbon is less likely to be incorporated into the silicon oxide film in the second gate insulating film forming process than in the first gate insulating film forming process. It is believed that the carbon concentration in the second gate insulating film 22 is lower than the carbon concentration in the first gate insulating film 21 for the above reasons.

[0050] Moreover, Fig. 11 shows the leakage current occurring in the gate insulating film. Graph D in Fig. 11 shows the measurement results for the sample of graph D in Fig. 10 (i.e., the first gate insulating film 21), and graph E in Fig. 11 shows the measurement results for the sample of graph E in Fig. 10 (i.e., the second gate insulating film 22). As shown in Fig. 11, at any electric field strength, gate leakage is less likely to occur in the second gate insulating film 22 (i.e., graph E) than in the first gate insulating film 21 (i.e., graph D). In this way, the second gate insulating film 22 with a low carbon concentration has higher insulation properties than the first gate insulating film 21 with a high carbon concentration.

[0051] According to the manufacturing method of the first embodiment, the second gate insulating film 22 having high insulating properties can be formed on the first gate insulating film 21, and therefore the gate insulating film 23 having high insulating properties can be formed. Therefore, gate leakage in the gate insulating film 23 can be suppressed.

[0052] As described above, according to the manufacturing method of Example 1, it is possible to form the gate insulating film 23 having high insulating properties including the second gate insulating film 22 while suppressing the formation of a gallium oxide layer at the interface 30. Therefore, according to the manufacturing method of Example 1, it is possible to manufacture a switching device 10 having low channel resistance and low gate leakage.

[0053] Next, a description will be given of the manufacturing methods of Examples 2 to 5. Note that in the manufacturing methods of Examples 2 to 5, only the gate insulating film formation step is different from the manufacturing method of Example 1. Therefore, the gate insulating film formation step of Examples 2 to 5 will be described below. EXAMPLES

[0054] In the gate insulating film forming process of Example 2, the first gate insulating film 21 and the second gate insulating film 22 are formed by a spray coating method. That is, here, while the gallium nitride semiconductor substrate 12 is heated, as shown in FIG. 12, a solution 84d is spray-coated on the upper surface 12a of the gallium nitride semiconductor substrate 12. At the same time, a reaction gas containing an oxidizing gas (here, ozone) is supplied to the upper surface 12a of the gallium nitride semiconductor substrate 12. The organic solvent evaporates from the solution 84d attached to the upper surface 12a, and the film forming raw material containing silicon is fixed to the upper surface 12a. At the same time that the film forming raw material is fixed to the upper surface 12a, the film forming raw material is oxidized by the reaction gas. The oxidized film forming raw material becomes silicon oxide. Therefore, silicon oxide grows on the upper surface 12a of the gallium nitride semiconductor substrate 12. In the first gate insulating film forming process, a first reaction gas having a low concentration of an oxidizing gas is supplied to the upper surface 12a while the solution 84d is spray-coated on the upper surface 12a. Therefore, a first gate insulating film 21 having a high carbon concentration is formed on the upper surface 12a. In the second gate insulating film forming step, a second reactive gas having a high concentration of an oxidizing gas is supplied to the upper surface 12a while the solution 84d is spray-applied onto the upper surface of the first gate insulating film 21. Therefore, a second gate insulating film 22 having a low carbon concentration is formed on the first gate insulating film 21. EXAMPLES

[0055] In the gate insulating film forming process of Example 3, the first gate insulating film 21 and the second gate insulating film 22 are formed by the inkjet method. That is, here, while the gallium nitride semiconductor substrate 12 is heated, droplets of a solution 84d are discharged from an inkjet head 300 toward the upper surface 12a of the gallium nitride semiconductor substrate 12 as shown in FIG. 13. At the same time, a reaction gas containing an oxidation gas (here, ozone) is supplied to the upper surface 12a of the gallium nitride semiconductor substrate 12. The organic solvent is evaporated from the solution 84d attached to the upper surface 12a, and the film forming raw material containing silicon is fixed to the upper surface 12a. At the same time that the film forming raw material is fixed to the upper surface 12a, the film forming raw material is oxidized by the reaction gas. The oxidized film forming raw material becomes silicon oxide. Therefore, silicon oxide grows on the upper surface 12a of the gallium nitride semiconductor substrate 12. In the first gate insulating film forming process, a first reactive gas having a low concentration of oxidizing gas is supplied to the upper surface 12a while the solution 84d is applied to the upper surface 12a by the inkjet method. Thus, a first gate insulating film 21 having a high carbon concentration is formed on the upper surface 12a. In the second gate insulating film forming process, a second reactive gas having a high concentration of oxidizing gas is supplied to the upper surface 12a while the solution 84d is applied to the upper surface 12a by the inkjet method. Thus, a second gate insulating film 22 having a low carbon concentration is formed on the first gate insulating film 21. EXAMPLES

[0056] In the gate insulating film forming process of Example 4, the first gate insulating film 21 and the second gate insulating film 22 are formed by a bubbling method. FIG. 14 shows a bubbling film forming apparatus 400 used in the bubbling method. The bubbling film forming apparatus 400 is obtained by replacing the mist generating device 84 of the mist CVD apparatus 80 of FIG. 6 with a bubbling tank 310. A solution 84d is stored in the bubbling tank 310. The downstream end of the carrier gas supply pipe 90 is immersed in the solution 84d in the bubbling tank 310. The upstream end of the raw material supply pipe 94 is disposed above the liquid surface of the solution 84d in the bubbling tank 310. When the gate insulating film 23 is formed by the bubbling film forming apparatus 400, a carrier gas is supplied from the carrier gas supply source 86 to the carrier gas supply pipe 90 while the gallium nitride semiconductor substrate 12 is heated, and a reaction gas containing an oxidizing gas (here, ozone) is supplied from the first reaction gas supply source 88a or the second reaction gas supply source 88b to the reaction gas supply pipe 92. The carrier gas supplied to the bubbling tank 310 passes through the solution 84d as bubbles. This generates droplets of the solution 84d in the carrier gas. The droplets of the solution 84d are supplied to the upper surface 12a of the gallium nitride semiconductor substrate 12 in the furnace 82 together with the carrier gas and the reaction gas. When the droplets of the solution 84d adhere to the upper surface 12a, the organic solvent volatilizes from the solution 84d, and the film forming raw material containing silicon is fixed to the upper surface 12a. At the same time that the film forming raw material is fixed to the upper surface 12a, the film forming raw material is oxidized by the reaction gas. The oxidized film-forming raw material becomes silicon oxide. Therefore, a gate insulating film made of silicon oxide grows on the upper surface 12a of the gallium nitride semiconductor substrate 12. In the first gate insulating film forming step, the first gate insulating film 21 is grown in the bubbling film-forming apparatus 400 while the first reactive gas is supplied from the first reactive gas supply source 88a to the furnace 82. Since the concentration of the oxidizing gas in the first reactive gas is low, the first gate insulating film 21 having a high carbon concentration is formed on the upper surface 12a. In the second gate insulating film forming step, the second gate insulating film 22 is grown in the bubbling film-forming apparatus 400 while the second reactive gas is supplied from the second reactive gas supply source 88b to the furnace 82. Since the concentration of the oxidizing gas in the second reactive gas is high, the second gate insulating film 22 having a low carbon concentration is formed on the first gate insulating film 21.

[0057] As described above, the manufacturing methods of Examples 2 to 4 are all techniques for supplying the solution 84d containing the film-forming raw material dissolved therein and the organic solvent to the upper surface 12a of the heated gallium nitride semiconductor substrate 12, as in Example 1. In any of the manufacturing methods of Examples 2 to 4, the gate insulating film 23 is formed using a non-plasma oxidizing gas. In addition, none of the manufacturing methods of Examples 2 to 4 includes a step of exposing the gate insulating film 23 to a plasma oxidizing gas after the gate insulating film 23 is formed. Therefore, in any of the manufacturing methods of Examples 2 to 4, the formation of a gallium oxide layer at the interface 30 between the gate insulating film 23 and the body layer 16 can be suppressed. In any of the manufacturing methods of Examples 2 to 4, the switching device 10 having high channel mobility can be manufactured. In any of the manufacturing methods of Examples 2 to 4, the gate insulating film 23 including the second gate insulating film 22 having a low carbon concentration can be formed. Therefore, the switching device 10 in which gate leakage is unlikely to occur can be manufactured.

[0058] In Examples 1 to 4, a common solution 84d was used in the first gate insulating film forming step and the second gate insulating film forming step. However, the solution used in the first gate insulating film forming step (hereinafter referred to as the first solution) and the solution used in the second gate insulating film forming step (hereinafter referred to as the second solution) may be different. For example, the film forming raw material dissolved in the first solution may be different from the film forming raw material dissolved in the second solution. Also, the organic solvent dissolved in the first solution may be different from the organic solvent dissolved in the second solution. EXAMPLES

[0059] In the gate insulating film forming process of Example 5, a first gate insulating film 21 and a second gate insulating film 22 are formed by the ALD method using a non-plasma state reactive gas. FIG. 15 shows the gate insulating film forming process of Example 5. As shown in FIG. 15, in the first gate insulating film forming process, step S2 and step S4 are alternately repeated multiple times. In step S2, an organic raw material gas containing silicon as an element is supplied to the upper surface 12a of the gallium nitride semiconductor substrate 12 while heating the gallium nitride semiconductor substrate 12. As a result, a raw material containing silicon is deposited on the upper surface 12a of the gallium nitride semiconductor substrate 12. In step S4, a first reactive gas containing a low concentration of an oxidizing gas (here, ozone) is supplied to the upper surface 12a of the gallium nitride semiconductor substrate 12 while heating the gallium nitride semiconductor substrate 12. As a result, the raw material containing silicon deposited on the upper surface 12a of the gallium nitride semiconductor substrate 12 is oxidized to become silicon oxide. By repeating step S2 and step S4, a silicon oxide film grows on the upper surface 12a of the gallium nitride semiconductor substrate 12. In the first gate insulating film forming process, carbon in the organic raw material gas is incorporated into the silicon oxide film. Since the concentration of the oxidizing gas in the first reactive gas is low, a silicon oxide film with a high carbon concentration (i.e., the first gate insulating film 21) is formed in the first gate insulating film forming process. As shown in FIG. 15, in the second gate insulating film forming process, steps S6 and S8 are alternately repeated multiple times. In step S6, an organic raw material gas containing silicon as an element is supplied to the upper surface of the first gate insulating film 21 while heating the gallium nitride semiconductor substrate 12. As a result, a raw material containing silicon is deposited on the upper surface of the first gate insulating film 21. In step S8, a second reactive gas containing a high concentration of an oxidizing gas (here, ozone) is supplied to the upper surface of the first gate insulating film 21 while heating the gallium nitride semiconductor substrate 12. As a result, the raw material containing silicon deposited on the upper surface of the first gate insulating film 21 is oxidized to become silicon oxide. By repeating steps S6 and S8, a silicon oxide film grows on the first gate insulating film 21. In the second gate insulating film forming step, carbon in the organic source gas is incorporated into the silicon oxide film.Since the concentration of the oxidizing gas in the second reactive gas is high, in the second gate insulating film forming step, a silicon oxide film with a low carbon concentration (i.e., second gate insulating film 22) is formed on first gate insulating film 21. Therefore, gate leakage is suppressed.

[0060] In the manufacturing method of Example 5, the gate insulating film 23 is formed using an oxidizing gas in a non-plasma state. In the manufacturing method of Example 5, the gate insulating film 23 is not exposed to an oxidizing gas in a plasma state after the gate insulating film 23 is formed. Therefore, the manufacturing method of Example 5 can also suppress the formation of a gallium oxide layer at the interface 30 between the gate insulating film 23 and the body layer 16. In the manufacturing method of Example 5, the switching device 10 with high channel mobility can also be manufactured. However, since this method is a film formation method at the atomic level in principle, it takes 10 hours or more to form a film of 100 nm, for example. Considering that the film formation time is at most several tens of minutes in a general CVD film formation method, even if an oxidizing gas in a plasma state is not used, a gallium oxide film is formed at the interface 30 during long film formation in the ALD method, so Example 5 is particularly effective when forming a film of 10 nm or less.

[0061] In the fifth embodiment, the organic source gas used in the first gate insulating film forming step and the organic source gas used in the second gate insulating film forming step may be the same or different.

[0062] (Variation 1) Next, a switching device 500 according to a modified example shown in Fig. 16 will be described. The switching device 500 is a vertical MOSFET. Among the components of the switching device 500, those having the same functions as the switching device 10 are given the same reference numerals as the switching device 10.

[0063] As shown in FIG. 16, the gallium nitride semiconductor substrate 12 of the switching device 500 has a high-concentration n-type layer 14a, a buffer layer 14b, and a drift layer 14c, similar to the switching device 10. A plurality of body layers 16 are provided on the drift layer 14c. Each body layer 16 is provided in a range that partially includes the upper surface 12a of the gallium nitride semiconductor substrate 12. The plurality of body layers 16 are separated from each other. A drift layer 14c is provided between the two body layers 16, and the two body layers 16 are separated from each other by the drift layer 14c. Hereinafter, the drift layer 14c located between the two body layers 16 is referred to as a JFET layer 14d (junction field effect transistor layer). Each body layer 16 has a p-type high-concentration layer 16a and a p-type low-concentration layer 16b having a p-type impurity concentration lower than that of the high-concentration layer 16a. The high-concentration layer 16a is in contact with the drift layer 14c from above. The low concentration layer 16b contacts the high concentration layer 16a from above. A source layer 18 and a contact layer 510 are provided within an area surrounded by each low concentration layer 16b. Each source layer 18 is provided in an area that partially includes the upper surface 12a. Each source layer 18 is separated from the drift layer 14c by the body layer 16. Each contact layer 510 is a p-type layer having a higher p-type impurity concentration than the high concentration layer 16a. Each contact layer 510 is provided in an area that partially includes the upper surface 12a.

[0064] A gate insulating film 23, a gate electrode 24, a source electrode 26, and an interlayer insulating film 520 are disposed on the upper part of the gallium nitride semiconductor substrate 12. The gate insulating film 23 covers a part of the upper surface 12a of the gallium nitride semiconductor substrate 12. The gate insulating film 23 has a first gate insulating film 21 and a second gate insulating film 22. The first gate insulating film 21 covers a range of the upper surface 12a that spans the surface of the source layer 18, the surface of the low concentration layer 16b, and the surface of the JFET layer 14d. The second gate insulating film 22 is disposed on the first gate insulating film 21. The second gate insulating film 22 covers the entire upper surface of the first gate insulating film 21. The gate electrode 24 is disposed on the second gate insulating film 22. The gate electrode 24 faces the source layer 18, the body layer 16, and the JFET layer 14d via the gate insulating film 23. The upper part of the gate electrode 24 is covered by the interlayer insulating film 520. The source electrode 26 covers the interlayer insulating film 520, and is in ohmic contact with the source layer 18 and the contact layer 510. A drain electrode 28 is provided on the lower surface of the gallium nitride semiconductor substrate 12. The drain electrode 28 is in ohmic contact with the high-concentration n-type layer 14a.

[0065] When a potential equal to or higher than the threshold is applied to the gate electrode 24, a channel is formed in the low-concentration layer 16b directly below the gate insulating film 23. The channel connects the source layer 18 and the JFET layer 14d. In this state, when a potential higher than that of the source electrode 26 is applied to the drain electrode 28, electrons flow from the source layer 18 through the channel, the drift layer 14c, and the buffer layer 14b to the high-concentration n-type layer 14a. In other words, the switching device 500 is turned on.

[0066] The switching device 500 is manufactured from the gallium nitride semiconductor substrate 12 (the substrate entirely made up of the high-concentration n-type layer 14a) shown in FIG.

[0067] First, as shown in Fig. 17, a buffer layer 14b made of gallium nitride is epitaxially grown on a high-concentration n-type layer 14a. Here, the n-type impurity concentration of the buffer layer 14b is about 2 x 10 16 cm-3 The buffer layer 14b is formed so that the thickness of the buffer layer 14b is about 0.3 μm. Next, as shown in FIG. 17, the drift layer 14c made of gallium nitride is epitaxially grown on the buffer layer 14b. Here, the n-type impurity concentration of the drift layer 14c is about 2×10 16 cm -3 The drift layer 14c is formed so that the thickness of the drift layer 14c is about 5.0 μm. Next, as shown in FIG. 17, the high concentration layer 16a made of gallium nitride is epitaxially grown on the drift layer 14c. Here, the p-type impurity concentration of the high concentration layer 16a is about 5×10 19 cm -3 The high concentration layer 16a is formed so that its thickness is about 0.5 μm. Next, as shown in FIG. 17, the low concentration layer 16b made of gallium nitride is epitaxially grown on the high concentration layer 16a. Here, the p-type impurity concentration of the low concentration layer 16b is about 5×10 17 cm -3 The low-concentration layer 16b is then formed to a thickness of about 1.5 μm. The gallium nitride semiconductor substrate 12 is then annealed in a nitrogen atmosphere at about 850° C. for about 5 minutes to activate the impurities in the gallium nitride semiconductor substrate 12.

[0068] 18, the upper surface 12a of the gallium nitride semiconductor substrate 12 is selectively dry-etched using an etching mask to form a recess 530 in the upper surface 12a. Here, the recess 530 is formed so that the width of the recess 530 is about 4 μm and the depth of the recess 530 reaches the drift layer 14c.

[0069] 19, an n-type layer 540 is epitaxially grown on the gallium nitride semiconductor substrate 12. Here, the n-type impurity concentration of the n-type layer 540 is about 2×10 16 cm -3The n-type layer 540 is formed so that the thickness of the n-type layer 540 is about 3.0 μm. When the n-type layer 540 is formed in this manner, the recess 530 is filled with the n-type layer 540. The n-type layer 540 in the recess 530 forms the JFET layer 14d.

[0070] 20, the upper surface 12a of the gallium nitride semiconductor substrate 12 is planarized by CMP (chemical mechanical polishing). Here, the upper surface 12a is planarized so that the low concentration layer 16b is exposed on the upper surface 12a.

[0071] Next, n-type impurities (e.g., silicon) are selectively introduced into the low concentration layer 16b from the upper surface 12a of the gallium nitride semiconductor substrate 12 at a concentration of about 3×10 15 cm -2 The ions are implanted at a dose of 1000° C. Thereafter, the entire gallium nitride semiconductor substrate 12 is annealed in a nitrogen atmosphere at about 1000° C. for about 5 minutes to activate the implanted n-type impurities. As a result, a source layer 18 is formed in a part of the surface layer of the low concentration layer 16b, as shown in FIG.

[0072] 22, a gate insulating film 23 (i.e., a first gate insulating film 21 and a second gate insulating film 22) is formed on the upper surface 12a of the gallium nitride semiconductor substrate 12. Here, the first gate insulating film 21 and the second gate insulating film 22 are formed so as to cover the entire upper surface 12a. The first gate insulating film 21 and the second gate insulating film 22 can be formed by the gate insulating film formation process of any one of the above-mentioned Examples 1 to 5.

[0073] 22, the gate electrode 24 is formed on the second gate insulating film 22. Here, the gate electrode 24 is formed so as to cover the entire upper surface of the second gate insulating film 22.

[0074] Next, as shown in Fig. 23, the gate insulating film 23 and the gate electrode 24 are partially removed to expose the source layer 18 and a part of the low concentration layer 16b. Next, p-type impurities are ion-implanted into the low concentration layer 16b, and then activation annealing is performed to form a contact layer 510, as shown in Fig. 23. Thereafter, an interlayer insulating film 520 and a source electrode 26 are formed on the upper part of the gallium nitride semiconductor substrate 12, and a drain electrode 28 is formed on the lower part of the gallium nitride semiconductor substrate 12, thereby completing the switching device 500 shown in Fig. 16.

[0075] As described above, the gate insulating film 23 of the switching device 500 of the first modification is formed by the gate insulating film forming process of any one of the first to fifth embodiments described above. Therefore, the gate insulating film 23 having high insulating properties is formed. Furthermore, the formation of a gallium oxide layer at the interface 30 between the gate insulating film 23 and the gallium nitride semiconductor substrate 12 is suppressed. That is, in the switching device 500 of the first modification, no gallium oxide layer is present at the interface 30, or the thickness of the gallium oxide layer present at the interface 30 is 1 nm or less. Therefore, in the switching device 500 of the first modification, the interface state density at the interface 30 is low. Therefore, the switching device 500 of the first modification has high channel mobility.

[0076] (Variation 2) The above-described switching devices 10 and 500 are MOSFETs. However, the technology disclosed in this specification may be applied to other switching devices. For example, the technology disclosed in this specification may be applied to a HEMT. FIG. 24 shows a switching device 600 of Modification 2 as an example of a HEMT. In FIG. 24, a gallium nitride semiconductor substrate 612 has a carrier travel layer 618 and a carrier supply layer 620. The carrier travel layer 618 is made of n-type gallium nitride (i.e., n-GaN). The carrier supply layer 620 is provided on the carrier travel layer 618. The carrier supply layer 620 is made of i-type aluminum gallium nitride (i.e., i-AlGaN). An interface 640 between the carrier travel layer 618 and the carrier supply layer 620 is a heterojunction surface, and two-dimensional electron gas is generated along the interface 640. A recess 650 is provided on the upper surface of the carrier supply layer 620, and a gate insulating film 623 and a gate electrode 624 are provided in the recess 650. The gate insulating film 623 has a first gate insulating film 621 in contact with the carrier supply layer 620, and a second gate insulating film 622 disposed on the first gate insulating film 621. The gate electrode 624 faces the carrier supply layer 620 via the gate insulating film 623. In addition, a source electrode 626 and a drain electrode 628 are provided on both sides of the gate electrode 624 on the upper surface of the gallium nitride semiconductor substrate 612.

[0077] At the interface 640 directly below the gate electrode 624, two-dimensional electron gas is generated or disappeared depending on the potential of the gate electrode 624. When two-dimensional electron gas is generated at the interface 640 directly below the gate electrode 624, electrons flow from the source electrode 626 to the drain electrode 628 through the two-dimensional electron gas. When the two-dimensional electron gas disappears at the interface 640 directly below the gate electrode 624, the flow of electrons from the source electrode 626 to the drain electrode 628 stops. In this way, the switching device 600 is turned on and off depending on the potential of the gate electrode 624.

[0078] In the switching device 600 (i.e., HEMT) of FIG. 24, the gate insulating film 623 (i.e., the first gate insulating film 621 and the second gate insulating film 622) can be formed by any of the gate insulating film forming steps of the above-mentioned Examples 1 to 5. Therefore, the gate insulating film 623 having high insulating properties is formed. Also, the formation of a gallium oxide layer at the interface 630 between the first gate insulating film 621 and the carrier supply layer 620 can be suppressed. That is, in the switching device 600 of the second modification, no gallium oxide layer exists at the interface 630, or the thickness of the gallium oxide layer existing at the interface 630 is 1 nm or less. Therefore, the interface state density at the interface 630 is low. The interface state density at the interface 630 has a large effect on the behavior of the two-dimensional electron gas directly below the interface 630. Therefore, by reducing the interface state density at the interface 630, the characteristics of the switching device 600 can be improved.

[0079] In the gate insulating film forming process of the above-mentioned Examples 1 to 5, ozone was used as the oxidizing gas. However, other gases capable of oxidizing silicon (for example, oxygen, water vapor, etc.) may be used as the oxidizing gas. However, since ozone has a higher oxidizing power than oxygen and water vapor, even if the heating temperature of the gallium nitride semiconductor substrate in the gate insulating film forming process is relatively low, the gate insulating film can be suitably formed. Furthermore, by setting the heating temperature of the gallium nitride semiconductor substrate to a relatively low temperature in this way, it is possible to suppress the diffusion of gallium from the gallium nitride semiconductor substrate to the gate insulating film during the gate insulating film forming process. This makes it possible to prevent the characteristics of the switching device from deteriorating.

[0080] Although the embodiments have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and changes to the specific examples exemplified above. The technical elements described in this specification or drawings exhibit technical utility alone or in various combinations, and are not limited to the combinations described in the claims at the time of filing. In addition, the technology exemplified in this specification or drawings achieves multiple objectives simultaneously, and achieving one of the objectives itself has technical utility. [Explanation of symbols]

[0081] 10: switching device, 12: gallium nitride semiconductor substrate, 16: body layer, 18: source layer, 20: drain layer, 21: first gate insulating film, 22: second gate insulating film, 24: gate electrode

Claims

1. A method for manufacturing a switching device (10, 500, 600), comprising the steps of: a step of supplying a first organic film-forming source containing silicon to a surface of the gallium nitride semiconductor layer (12, 612) and supplying a first reactive gas containing an oxidizing gas in a non-plasma state to the surface of the gallium nitride semiconductor layer, thereby forming a first gate insulating film (21, 621) made of silicon oxide on the gallium nitride semiconductor layer; a step of forming a second gate insulating film (22, 622) made of silicon oxide on the first gate insulating film by supplying a second organic film-forming material containing silicon to the surface of the first gate insulating film and supplying a second reactive gas containing an oxidizing gas to the surface of the first gate insulating film in a non-plasma state; and the oxidizing gas contained in the first reactive gas and the oxidizing gas contained in the second reactive gas are the same type of gas, the concentration of the oxidizing gas in the first reactive gas is lower than the concentration of the oxidizing gas in the second reactive gas; Manufacturing method.

2. the first organic film-forming raw material is a first solution (84d) containing a silicon-containing film-forming raw material dissolved therein and an organic solvent; the second organic film-forming raw material is a second solution (84d) containing a silicon-containing film-forming raw material dissolved therein and an organic solvent; The method of claim 1.

3. In the step of forming the first gate insulating film, a mist (83) is generated from the first solution, and the mist of the first solution is supplied to the surface of the gallium nitride semiconductor layer together with the first reactive gas; In the step of forming the second gate insulating film, a mist (83) is generated from the second solution, and the mist of the second solution is supplied to the surface of the first gate insulating film together with the second reactive gas. The method of claim 2.

4. In the step of forming the first gate insulating film, the first solution is spray-coated onto the surface of the gallium nitride semiconductor layer while the first reactive gas is supplied to the surface of the gallium nitride semiconductor layer; In the step of forming the second gate insulating film, the second solution is spray-coated onto the surface of the first gate insulating film while the second reactive gas is supplied to the surface of the first gate insulating film. The method of claim 2.

5. In the step of forming the first gate insulating film, the first solution is applied to the surface of the gallium nitride semiconductor layer by an inkjet method while the first reactive gas is supplied to the surface of the gallium nitride semiconductor layer; In the step of forming the second gate insulating film, the second solution is applied to the surface of the gallium nitride semiconductor layer by an inkjet method while the second reactive gas is supplied to the surface of the gallium nitride semiconductor layer. The method of claim 2.

6. In the step of forming the first gate insulating film, droplets of the first solution are generated by generating bubbles in the first solution, and the droplets of the first solution are supplied to the surface of the gallium nitride semiconductor layer together with the first reactive gas; In the step of forming the second gate insulating film, droplets of the second solution are generated by generating bubbles in the second solution, and the droplets of the second solution are supplied to the surface of the first gate insulating film together with the second reactive gas. The method of claim 2.

7. the step of forming the first gate insulating film comprises alternately repeating a step of supplying a first source gas containing the first organic film-forming raw material to the surface of the gallium nitride semiconductor layer and a step of supplying the first reactive gas to the surface of the gallium nitride semiconductor layer multiple times; In the step of forming the second gate insulating film, a step of supplying a second source gas containing the second organic film-forming raw material to the surface of the first gate insulating film and a step of supplying the first reactive gas to the surface of the first gate insulating film are alternately repeated multiple times. The method of claim 1 .

8. 8. The manufacturing method according to claim 1, wherein the oxidizing gas contained in the first reactive gas and the oxidizing gas contained in the second reactive gas are ozone.

9. 9. The manufacturing method according to claim 1, wherein the average carbon concentration of the second gate insulating film is lower than the average carbon concentration of the first gate insulating film.

10. The carbon concentration of at least a part of the second gate insulating film is 3×10 19 atoms / cm 3 The method of claim 9, wherein the

11. 11. The manufacturing method according to claim 1, wherein the method does not include a step of exposing the first gate insulating film and the second gate insulating film to an oxidizing gas in a plasma state after the step of forming the second gate insulating film is performed.

12. 12. The manufacturing method according to claim 1, wherein after the step of forming the first gate insulating film is performed, no gallium oxide layer is present at the interface between the gallium nitride semiconductor layer and the first gate insulating film, or the thickness of the gallium oxide layer present at the interface between the gallium nitride semiconductor layer and the first gate insulating film is 1 nm or less.

Citation Information

Patent Citations

  • Fabrication of semiconductor device

    JP1995273194A

  • Manufacture of semiconductor device and the semiconductor device

    JP2000183051A

  • Semiconductor device and method of manufacturing the same

    JP2016018888A

  • Processing method

    JP2018142637A

  • Gate switching element and manufacturing method thereof

    JP2019021753A