Irregular shaped silica-based fine particle dispersion and its manufacturing method

The controlled synthesis of irregularly shaped silica-based fine particles addresses the issues of scratches and smoothness in semiconductor wafer polishing, enhancing polishing rate and surface quality.

JP7583597B2Active Publication Date: 2024-11-14JGC CATALYSTS & CHEMICALS LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020203938
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-09
Publication Date
2024-11-14
Estimated Expiration
2040-12-09

AI Technical Summary

Technical Problem

Existing semiconductor wafer polishing methods using silica particles face issues with high polishing rates leading to scratches and reduced smoothness due to irregular particle shapes, spherical particles, and clustered structures with coarse and small particles.

Method used

A method for producing a dispersion of irregularly shaped silica-based fine particles through controlled synthesis steps, including adjusting molar ratios, ionic strength, and temperature to achieve specific particle sizes and irregularities, ensuring a high proportion of irregularly shaped particles with controlled particle distribution.

Benefits of technology

The method results in improved substrate surface smoothness and polishing rate by using irregularly shaped silica particles that minimize scratches while maintaining high polishing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583597000004
    Figure 0007583597000004
  • Figure 0007583597000001
    Figure 0007583597000001
  • Figure 0007583597000002
    Figure 0007583597000002
Patent Text Reader

Abstract

To provide a method for producing a modified silica-based fine particle dispersion capable of improving smoothness of a substrate surface and increasing a polishing speed when used as a polishing slurry.SOLUTION: A method for producing a modified silica-based fine particle dispersion comprises the following steps (a) to (f). Step (a): a step of obtaining a seed particle precursor dispersion by adjusting the ionic strength of an alkali silicate aqueous solution to 0.4 or more. Step (b): a step of heating and maturing the seed particle precursor dispersion. Step (c): a step of adding an acidic silicic acid liquid to the heated and matured seed particle precursor dispersion to obtain a seed particle dispersion. Step (d): a step of adjusting the seed particle dispersion to have an ionic strength of 0.25 or more. Step (e): a step of heating and maturing the seed particle dispersion in which the concentration of SiO2 and the ionic strength have been adjusted. Step (f): a step of adding an acidic silicic acid liquid to the heated and matured seed particle dispersion to obtain a modified silica-based fine particle dispersion containing modified silica-based fine particles.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a dispersion of irregular shaped silica-based fine particles and a method for producing the same. [Background technology]

[0002] Conventionally, silica sol, fumed silica, fumed alumina, etc. have been used as polishing particles. In the manufacture of semiconductor integrated circuit-attached substrates, aluminum wiring is formed on a silicon wafer, and an oxide film such as silica is provided thereon as an insulating film. In this case, unevenness is generated by the wiring, so this oxide film is polished to flatten it. In polishing such substrates, it is required that the surface after polishing is flat without steps or unevenness, smooth without microscopic scratches, etc., and a high polishing rate.

[0003] For example, Patent Document 1 describes a method for polishing semiconductor wafers using colloidal silica in which the number of colloidal silica particles having a major axis of 7 to 1000 nm and a minor axis / major axis ratio of 0.3 to 0.8 accounts for 50% or more of all particles. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2001-150334 A [Patent Document 2] Patent No. 6207345 Summary of the Invention [Problem to be solved by the invention]

[0005] In the method for polishing semiconductor wafers described in Patent Document 1, the polishing rate can be improved because the average irregularity of the silica particles is high, with a minor axis / major axis ratio of 0.3 to 0.8. However, if the average irregularity of the silica particles is too high, there is a problem in that scratches are likely to occur on the polished substrate, reducing the smoothness of the substrate surface. In addition, in the polishing method described in Patent Document 2, it is shown that a high polishing rate can be obtained by using irregular silica particles in which at least four or more primary silica particles are clustered. However, although the polishing rate is high because of the structure of at least four or more clusters, it was found that a flocculant is used for the purpose of forming a cluster structure, and there are many coarse particles, and furthermore, there are many small-sized spherical particles that are not clustered. As a result, it was found that there is room for improvement in that polishing scratches are easily caused by coarse particles, while small-sized particles that have a high effect of repairing polishing scratches and smoothing are spherical and have a slow polishing rate, resulting in a small repair effect.

[0006] The present invention aims to provide an irregular silica-based microparticle dispersion liquid which, when used as a polishing slurry, can improve the smoothness of a substrate surface and increase the polishing rate, as well as a method for producing the irregular silica-based microparticle dispersion liquid. [Means for solving the problem]

[0007] According to one aspect of the present invention, there is provided a method for producing a dispersion of irregular shaped silica-based fine particles, comprising the following steps (a) to (f): A method for producing a dispersion of irregular shaped silica-based fine particles, comprising the following steps (a) to (f): Step (a): A step of adjusting the molar ratio of silica to alkali metal in an aqueous alkali silicate solution to a range of 0.5 to 10, and adding an alkali as necessary to adjust the SiO2 concentration to 2% by mass to 25% by mass and the ionic strength to 0.4 or more, thereby obtaining a seed particle precursor dispersion liquid. Step (b): Heating and aging the seed particle precursor dispersion liquid obtained in step (a) at a temperature in the range of 40° C. or higher and lower than 100° C. Step (c): Following step (b), an acidic silicic acid liquid is added to the heat-aged seed particle precursor dispersion liquid so that the molar ratio of the amount of silica in the acidic silicic acid liquid to the amount of silica in the seed particle precursor dispersion liquid ([amount of silica in the acidic silicic acid liquid] / [amount of silica in the seed particle precursor dispersion liquid]) is in the range of 0.5 to 10, thereby obtaining a seed particle dispersion liquid. Step (d): A step of adjusting the SiO2 concentration to 2% by mass or more and 15% by mass or less and the ionic strength to 0.25 or more by adding an alkali as necessary to the seed particle dispersion liquid obtained in the step (c). Step (e): Following step (d), the seed particle dispersion liquid having the adjusted SiO2 concentration and ionic strength is heated and aged at a temperature in the range of 40° C. or higher and lower than 100° C. Step (f): Following step (e), an acidic silicic acid liquid is added to the heat-aged seed particle dispersion so that the molar ratio of the amount of silica in the acidic silicic acid liquid to the amount of silica in the seed particle dispersion ([amount of silica in the acidic silicic acid liquid] / [amount of silica in the seed particle dispersion]) is in the range of 5 to 20, thereby obtaining an irregular silica-based microparticle dispersion containing irregular silica-based microparticles.

[0008] According to one aspect of the present invention, there is provided an irregular silica-based microparticle dispersion liquid containing irregular silica-based microparticles that satisfy the following conditions [1] to [4]. [1] The average particle size measured by dynamic light scattering is 10 nm or more and 300 nm or less. [2] The average particle size calculated by the nitrogen adsorption method is 5 nm or more and 200 nm or less. [3] The average degree of irregularity determined by analyzing scanning electron micrographs is 1.2 or more and 10.0 or less. [4] In the particle size distribution obtained by analyzing scanning electron micrographs, when the average irregularity of particles whose number ratio from the smaller particle size side ([number] / [total number]) is in the range of more than 0 and not more than 1 / 10 is defined as [A], and the average irregularity of particles whose number ratio from the smaller particle size side ([number] / [total number]) is in the range of more than 9 / 10 and not more than 10 / 10 is defined as [B], the value of [B] / [A] is 1.2 or more. Effect of the Invention

[0009] According to the present invention, it is possible to provide an irregular shaped silica-based microparticle dispersion liquid which, when used as a polishing slurry, can improve the smoothness of a substrate surface and increase the polishing rate, as well as a method for producing the irregular shaped silica-based microparticle dispersion liquid. [Brief description of the drawings]

[0010] [Figure 1] 1 is a scanning electron microscope photograph showing the irregular silica-based fine particles obtained in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] [Method of manufacturing irregular silica-based fine particle dispersion] The method for producing the irregular shaped silica-based fine particle dispersion according to this embodiment will be described below. The method for producing an irregular silica-based fine particle dispersion according to this embodiment is characterized by comprising the following steps (a) to (f). In this specification, irregular silica-based particles refer to particles with irregular shapes other than spherical silica-based particles. Here, spherical silica-based particles refer to silica-based particles with a spherical shape. In addition, irregular silica-based particles include all particles with shapes other than spherical, such as primary silica particles obtained by pulverizing spherical silica-based particles, particles in which primary silica particles are connected, and particles in which primary silica particles are connected and further grown with silica. The fact that primary silica particles are connected means that adjacent primary silica particles are fixed to each other by the bond formed between them. Here, the type of bond is not particularly limited, but examples include chemical bonds such as siloxane bonds formed by condensation reaction between the surface silanol groups of adjacent primary silica particles.

[0012] [Process (a)] Step (a) is a step of adjusting the molar ratio of silica to alkali metal in an aqueous alkali silicate solution to be in the range of 0.5 or more and 10 or less, and adding an alkali as necessary to adjust the SiO2 concentration to 2% by mass or more and 25% by mass or less and the ionic strength to 0.4 or more, thereby obtaining a seed particle precursor dispersion liquid. If the molar ratio of silica to alkali metal in the seed particle precursor dispersion is less than 0.5, it is necessary to add a large amount of alkali metal, which is uneconomical. In addition, since coarse particles are likely to be generated by aggregation, sedimentation is likely to occur, and it is difficult to generate monodispersed seed particles. On the other hand, if the molar ratio of silica to alkali metal exceeds 10, the size of the generated seed particles becomes very small, and it takes a lot of effort to grow the particles to the size required for polishing, which is uneconomical, and the degree of irregularity of the obtained irregular particles decreases because the particle growth width becomes large. From the same viewpoint, the molar ratio of silica to alkali metal is preferably 1 to 5.

[0013] Examples of the alkali metal in the aqueous alkali silicate solution include potassium, sodium, and lithium. In the aqueous alkali silicate solution, the SiO2 concentration and the alkali concentration (A2O concentration) are not particularly limited. For example, the SiO2 concentration is preferably 2% by mass or more and 25% by mass or less, and more preferably 5% by mass or more and 25% by mass or less. The A2O concentration is preferably 0.5% by mass or more and 25% by mass or less, and more preferably 2% by mass or more and 20% by mass or less.

[0014] If the SiO2 concentration in the seed particle precursor dispersion is less than 2 mass%, the degree of irregularity of the resulting seed particles will decrease. On the other hand, if the SiO2 concentration exceeds 25 mass%, aggregation will proceed, causing problems in that precipitation and coarse particles will occur. From the same viewpoint, the SiO2 concentration is preferably 5 mass% or more and 20 mass% or less, and more preferably 8 mass% or more and 18 mass% or less.

[0015] If the ionic strength in the seed particle precursor dispersion is less than 0.4, the ionic strength is insufficient, and therefore the association of the seed particle precursors and the core particles generated in steps (b) and (c) etc. does not proceed, resulting in a decrease in the irregularity of the seed particles. From the same viewpoint, the ionic strength is preferably 0.8 to 2.5, more preferably 1.2 to 2.0. In this specification, the ionic strength in the dispersion liquid means a value calculated from the following formula: The elements used in the calculation of the ionic strength here are only alkali metals, alkaline earth metals, and halogens that have a significant effect on the aggregation and association of particles.

[0016]

number

[0017] In the formula, J represents ionic strength, Ci represents the molar concentration of alkali metals, alkaline earth metals, and halogens in the system, and Zi represents the valence of each ion. The molar concentration of each ion is the ion concentration of the substance that dissociates at the pH of the solution in which the substance is dissolved, and is calculated using the acid dissociation constant pKa or base dissociation constant pKb of each substance. For example, when adding a salt that dissociates in water into A(-) and B(+) to a dispersion, it is divided into acid AH and base BOH, and the ion concentrations of A(-) and H(+), and B(+) and OH(-) are calculated. The same applies to acids used for pH adjustment, etc., where AH is divided into A(-) and H(+) and the ion concentrations of each are calculated and applied to the above formula.

[0018] As the alkali, any known alkali may be used as appropriate. In addition, as the alkali, it is preferable to use at least one ionic strength adjuster selected from the group consisting of sodium hydroxide and potassium hydroxide.

[0019] [Step (b)] The step (b) is a step of heating and aging the seed particle precursor dispersion liquid obtained in the step (a) at a temperature in the range of 40°C or higher and lower than 100°C. This step (b) can homogenize the solution, such as the uniformity of silica solubility in the dispersion and the uniformity of the seed particle precursors, etc. In this specification, this stabilization operation may be referred to as "seeding."

[0020] The pH of the seed particle precursor dispersion during heat aging is preferably 10 or more, and more preferably 11 or more, from the viewpoint of increasing the ionic strength of the seed particle precursor dispersion.

[0021] If the heating temperature during heat aging is less than 40°C, the seeding effect cannot be obtained. On the other hand, if the heating temperature is 100°C or higher, the reaction liquid boils, which is problematic in that stable production cannot be achieved. From the same viewpoint, the temperature during heat aging is preferably 60°C or higher and 95°C or lower. The maturation time during heat maturation is preferably from 20 minutes to 120 minutes, more preferably from 60 minutes to 100 minutes, from the viewpoint of the seeding effect.

[0022] As the alkali, any known alkali may be used as appropriate. In addition, as the alkali, it is preferable to use at least one ionic strength adjuster selected from the group consisting of sodium hydroxide and potassium hydroxide.

[0023] [Process (c)] Step (c) is a step of adding an acidic silicic acid liquid to the heat-aged seed particle precursor dispersion liquid subsequent to step (b) so that the molar ratio of the amount of silica in the acidic silicic acid liquid to the amount of silica in the seed particle precursor dispersion liquid ([amount of silica in the acidic silicic acid liquid] / [amount of silica in the seed particle precursor dispersion liquid]) is in the range of 0.5 or more and 10 or less, thereby obtaining a seed particle dispersion liquid. If the molar ratio of the amount of silica in the acidic silicic acid liquid to the amount of silica in the seed particle precursor dispersion is less than 0.5, the amount of silica is insufficient, so seed particles are difficult to generate, and even if seed particles are generated, they are small in size and have poor stability, which is a problem. On the other hand, if the molar ratio of the amount of silica exceeds 10, there is a problem in that the irregularity of the seed particles decreases. From the same viewpoint, the molar ratio of the amount of silica is preferably 0.7 or more and 5 or less, and more preferably 1 or more and 2 or less.

[0024] The temperature at which the acidic silicic acid liquid is added is preferably 40° C. or higher and lower than 100° C., more preferably 60° C. or higher and 95° C. or lower, from the viewpoint of dissolving the acidic silicic acid liquid and promoting deposition onto the particles. When the addition time of the acidic silicic acid liquid is less than 1 hour, the addition speed of the acidic silicic acid liquid is too fast, so that self-nucleation tends to occur. On the other hand, when the addition time exceeds 15 hours, the productivity tends to decrease. From the same viewpoint, the addition time is more preferably 2 hours or more and 8 hours or less. The retention time after the addition of the acidic silicic acid liquid is preferably 10 minutes or more and 120 minutes or less. In the obtained seed particle dispersion, the seed particles are grown to a size required for polishing in steps (d) and (e) to have an average particle size measured by dynamic light scattering. If the seed particles are less than 5 nm, the particle growth width must be significantly increased, which tends to reduce the degree of irregularity. On the other hand, if the seed particles are more than 100 nm, the size becomes too large after particle growth, which causes a problem of easy sedimentation. From the same viewpoint, the average particle size of the seed particles measured by dynamic light scattering is more preferably 10 nm or more and 50 nm or less.

[0025] The acidic silicic acid liquid may be obtained by de-alkalinizing an aqueous solution of an alkali silicate (such as an alkali metal silicate or ammonium silicate) with a cation exchange resin. The SiO2 concentration of the acidic silicic acid liquid is preferably 0.1% by mass or more and 10% by mass or less, more preferably 1% by mass or more and 7% by mass or less.

[0026] [Step (d) and Step (e)] Step (d) is a step of adjusting the SiO2 concentration to 2 mass % or more and 15 mass % or less and the ionic strength to 0.25 or more by adding an alkali as necessary to the seed particle dispersion obtained in step (c). Here, the alkali is the same as the alkali used in step (b). The step (e) is a step following the step (d) in which the seed particle dispersion liquid in which the SiO2 concentration and ionic strength have been adjusted is heated and aged at a temperature in the range of 40°C or higher and lower than 100°C.

[0027] If the SiO2 concentration in the seed particle dispersion liquid in which the SiO2 concentration has been adjusted is less than 2 mass%, the concentration is low, resulting in reduced productivity. On the other hand, if the SiO2 concentration exceeds 15 mass%, excessive aggregation occurs, resulting in problems such as precipitation and coarse particles. From the same viewpoint, the SiO2 concentration is preferably 3 mass% or more and 10 mass% or less, and more preferably 4 mass% or more and 8 mass% or less.

[0028] If the ionic strength of the seed particle dispersion liquid is adjusted to less than 0.25, the degree of irregularity decreases as the irregular silica-based fine particles grow. From the same viewpoint, the ionic strength is preferably 0.3 to 0.7.

[0029] The pH of the seed particle dispersion during heat aging is preferably 10 or more from the viewpoint of increasing the ionic strength of the seed particle dispersion.

[0030] If the heating temperature during heat aging is less than 40°C, the seeding effect cannot be obtained. On the other hand, if the heating temperature is 100°C or higher, the reaction liquid boils, which is problematic in that stable production cannot be achieved. From the same viewpoint, the temperature during heat aging is preferably 80°C or higher and lower than 100°C. The maturation time during heat maturation is preferably from 20 minutes to 120 minutes, more preferably from 20 minutes to 60 minutes, from the viewpoint of the seeding effect.

[0031] [Process (f)] Step (f) is a step of adding an acidic silicic acid liquid to the heat-aged seed particle dispersion liquid subsequent to step (e) so that the molar ratio of the amount of silica in the acidic silicic acid liquid to the amount of silica in the seed particle dispersion liquid ([amount of silica in the acidic silicic acid liquid] / [amount of silica in the seed particle dispersion liquid]) is in the range of 5 or more and 20 or less, thereby obtaining an irregular silica-based microparticle dispersion liquid containing irregular silica-based microparticles. Here, the acidic silicic acid liquid is the same as the acidic silicic acid liquid used in the step (c).

[0032] If the molar ratio of the amount of silica in the acidic silicic acid solution to the amount of silica in the seed particle dispersion is less than 5, the particles do not grow to the desired size, resulting in a slow polishing rate. On the other hand, if the molar ratio of the amount of silica exceeds 20, the particles grow too much, resulting in a problem of a decrease in particle irregularity and a slow polishing rate. From the same viewpoint, the molar ratio of the amount of silica is preferably 6 or more and 15 or less.

[0033] The temperature at which the acidic silicic acid liquid is added is preferably 40°C or higher and lower than 100°C, more preferably 80°C or higher and lower than 100°C, from the viewpoint of dissolving the acidic silicic acid liquid and promoting the deposition reaction onto the particles. When the acidic silicic acid liquid is added, if the addition time is too short, the silicic acid will self-nucleate, which is not preferable, and if the addition time is too long, the economic efficiency will decrease, so the addition time is preferably 5 hours or more and 36 hours or less, and more preferably 8 hours or more and 24 hours or less. The retention time after the addition of the acidic silicic acid liquid is preferably 10 minutes or more and 120 minutes or less.

[0034] In this step (f), the ratio of the number of moles of silica to the alkali metal is preferably from 30 to 150, more preferably from 35 to 130, and particularly preferably from 40 to 120. The ratio of the number of moles of silica to the alkali metal is the value obtained by dividing the total number of moles of silica by the total number of moles of the alkali metal at the end of step (f). When the molar ratio of silica to alkali metal is less than the lower limit, the amount of silica to alkali metal is insufficient, and the pH of reaction solution becomes too high, so that particle aggregation tends to occur.Even if aggregation does not occur, the stability over time is poor, and particle size may increase with time or aggregation may occur.On the other hand, when the molar ratio of silica to alkali metal is more than 150, the amount of silica to alkali metal is too large, and the pH of reaction solution becomes low, so that the acidic silicic acid solution added for particle growth does not contribute to particle growth, and self-nucleation tends to occur.

[0035] [Effects of each process] In steps (e) and (f), the seed particles obtained in step (c) are further aggregated, adjusted to the desired size and irregularity, and grown. In this step, an alkali metal or the like is added to the solution containing the seed particles to adjust the ionic strength in the system to a predetermined value or higher, and the concentration of the seed particles, i.e., the silica concentration in step (e), is adjusted to within a predetermined range, thereby allowing the seed particles to aggregate and controlling the degree of association. Next, in step (f), an acidic silicic acid liquid is added to this solution to fill the necks of the aggregated particles with silica, thereby reinforcing the aggregate structure and obtaining particles with the desired size and irregularity. The associated seed particles are grown in an acidic silicic acid solution, so they are strongly bonded together. Therefore, the particles do not break down when used for polishing. In addition, the rate of irregularly shaped particles is high, and the irregular shape provides a large contact area with the substrate, resulting in a high polishing rate. Furthermore, the degree of irregularity of the small particles is also high, so they are highly effective at repairing polishing scratches caused by large particles.

[0036] In this case, if the silica concentration in step (e) is less than 2%, the seed particles are difficult to aggregate, and even if they do aggregate, only particles with low irregularity are obtained. In addition, the reaction concentration is low, so the productivity is poor. If the silica concentration is more than 15%, the high concentration results in high productivity, but the seed particles tend to aggregate, resulting in the formation of coarse particles and precipitation. The ionic strength adjuster may be an alkali metal, an alkaline earth metal, a halogen, or a salt or hydroxide thereof, but the ionic strength adjuster used in step (e) is preferably an alkali metal hydroxide. This is because the alkali metal hydroxide can adjust the ionic strength and also act as a catalyst for nucleation and particle growth. NaOH or KOH may be added as the alkali metal hydroxide, or the alkali metal hydroxide brought in from the raw material alkali silicate may be used.

[0037] On the other hand, when halide salts (alkali halides) such as KCl and CaCl2 are used as ionic strength adjusters, they act as agglomerants, which tend to cause aggregation of seed particles, resulting in coarse particles and precipitation. Although irregularly shaped particles can be obtained by adding a small amount of agglomerants to prevent precipitation and allowing the reaction to proceed, the amount of agglomerants is small, so some particles become irregularly shaped, but many particles are spherical or nearly spherical and not irregularly shaped. Therefore, the irregularly shaped particles obtained tend to have a low rate of irregular particles. That is, particles with a small particle size have a low degree of irregularity, and aggregated particles with a large particle size have a high degree of irregularity, resulting in a polarization of the degree of irregularity. Normally, small particles have a high smoothing effect on the polishing substrate, but in the case of particles with a wide distribution, large and small particles coexist and the polishing speed of the small particles is low, so the smoothing effect of the surface roughness worsened by the large particles is reduced. As a result, polishing scratches tend to occur frequently. If the ionic strength is less than 0.25, the ionic strength is insufficient to prevent particle association, and even if association does occur, only particles with low irregularity are obtained. If the ionic strength is 0.7 or more, aggregation occurs, which tends to cause precipitation.

[0038] [Dispersion of irregularly shaped silica particles] Next, the irregular shaped silica-based fine particle dispersion according to this embodiment will be described. The irregular shaped silica-based microparticle dispersion according to this embodiment is characterized by containing irregular shaped silica-based microparticles that satisfy the following conditions [1] to [4]. The irregular shaped silica-based fine particle dispersion according to this embodiment can be produced by the method for producing the irregular shaped silica-based fine particle dispersion according to this embodiment described above.

[0039] [Condition 1] Condition 1 is that the average particle size measured by dynamic light scattering is 10 nm or more and 300 nm or less. If the average particle diameter measured by dynamic light scattering is less than 10nm, the polishing rate will be low when used as polishing slurry.On the other hand, if the average particle diameter is more than 300nm, the roughness, waviness, and scratches of the substrate surface will be deteriorated, which is a problem.In addition, from the same viewpoint, the average particle diameter is preferably 30nm or more and 250nm or less, and more preferably 50nm or more and 200nm or less.

[0040] [Condition 2] Condition 2 is that the average particle size calculated by the nitrogen adsorption method is 5 nm or more and 200 nm or less. If the average particle size calculated by the nitrogen adsorption method is less than 5 nm, it is difficult to obtain the required polishing speed, and furthermore, small particles are likely to remain on the substrate. On the other hand, if the average particle size exceeds 200 nm, scratches will occur, the surface roughness of the substrate after polishing will deteriorate, and waviness will deteriorate. From the same viewpoint, the average particle size is preferably 10 nm or more and 150 nm or less, more preferably 20 nm or more and 100 nm or less.

[0041] [Condition 3] Condition 3 is that the average degree of irregularity determined by analyzing a scanning electron micrograph is 1.2 or more and 10 or less. When the average irregularity obtained by analyzing scanning electron micrograph is less than 1.2, the irregularity is insufficient, and the contact area with the substrate is small, so that when used as polishing slurry, the polishing speed is low. On the other hand, when this average irregularity exceeds 10, such particles are difficult to produce industrially stably because of the complicated manufacturing process, and the economic efficiency is also poor. Even if particles with an irregularity of 10 or more are obtained, the polishing speed does not improve any more, and there is a problem in that scratches are easily generated. From the same viewpoint, this average irregularity is more preferably 1.2 or more and 5 or less.

[0042] In this specification, the average irregularity is determined by analyzing a scanning electron microscope photograph. Specifically, a scanning electron microscope photograph is observed, and the rectangle with the smallest area is determined among the circumscribing rectangles circumscribing each particle. The lengths of the long side and short side of the circumscribing rectangle are then determined, and the ratio of the long side to the short side ([long side] / [short side]) is taken as the irregularity. The irregularity is calculated for each particle, and the average of these values ​​can be calculated as the average irregularity.

[0043] [Condition 4] Condition 4 is that, in the particle size distribution obtained by analyzing a scanning electron microscope photograph, when the average irregularity of particles whose number ratio from the smaller particle size side ([number] / [total number]) is in the range of more than 0 and not more than 1 / 10 is defined as [A], and the average irregularity of particles whose number ratio from the smaller particle size side ([number] / [total number]) is in the range of more than 9 / 10 and not more than 10 / 10 is defined as [B], the value of [B] / [A] is 1.2 or more. The particle diameter used in calculating the number ratio of particle diameters was the diameter of the area-equivalent circle. The area-equivalent circle diameter was determined by analyzing a scanning electron microscope photograph. Specifically, a scanning electron microscope photograph was observed to determine the area of ​​each particle, and the diameter of a circle equal to this area was used as the area-equivalent circle diameter. If the value of [B] / [A] is 1.2 or more, the polishing rate can be improved while suppressing scratches. Here, [A] is the average irregularity of a relatively small particle group, and [B] is the average irregularity of a relatively large particle group. Therefore, a value of [B] / [A] of 1 or more indicates that the larger the particle, the greater the irregularity tends to be. In addition, when the average irregularity is within a specified range (1.2 or more and 10 or less) and the B / A ratio is 1.2 or more, this indicates that the overall irregularity is high and that the irregularities of both the small particle component and the large particle component are also high. Generally, small and large particles have a large effect on polishing performance. Large particles have a very high polishing rate, and as the irregularity increases, the polishing rate also increases, so they make a large contribution to improving the polishing rate of the entire abrasive. However, on the other hand, large particles tend to worsen the roughness of the substrate surface and cause polishing scratches. On the other hand, small-sized particles have a low polishing rate, so they have a large impact in the sense that they reduce the polishing rate of the entire abrasive grain. On the other hand, they contribute greatly to the smoothing of the substrate surface, and have the effect of repairing and smoothing scratches caused by coarse particles, etc. Therefore, if the irregularity of small-sized particles is moderately high, the effect of repairing surface roughness and scratches, etc. will be improved, and the polishing rate will also be raised, so it is desirable for the irregularity of small particles to be high. Therefore, when the degree of irregularity of the small particles is high and the B / A ratio is also high, the polishing rate is sufficiently high and a smoother substrate surface with fewer scratches can be obtained. The present inventors presume that due to this mechanism, if the value of [B] / [A] is 1.2 or more, it is possible to improve the polishing rate while suppressing sludge. From the same viewpoint, the value of [B] / [A] is preferably 1.2 or more and 2 or less, and more preferably 1.2 or more and 1.80 or less. From the above viewpoint, the value of [A] is preferably 1.13 or more, and more preferably 1.15 to 1.8. When the value of [A] is less than 1.13, the irregularity is low and the polishing speed is slow, resulting in a small surface smoothing effect. On the other hand, when the value of [A] is more than 1.8, the irregularity is high and the polishing speed is high, but the effect of worsening roughness is greater than the smoothing effect.

[0044] [Condition 5] Condition 5 is that, when the degree of irregularity of particles is determined by analyzing a scanning electron micrograph, the rate of irregular particles to all particles ([number of particles with an irregularity of 1.2 or more] / [total number of particles]×100%) is 45% or more. In this embodiment, it is more preferable to satisfy this condition 5. If the ratio of irregular particles to the total particles is 45% or more, the polishing rate can be further improved. From the same viewpoint, the ratio of irregular particles is preferably 48% or more and 95% or less, and more preferably 50% or more and 90% or less. If the ratio of irregular particles is more than 95%, the polishing rate is high, but the substrate surface roughness tends to deteriorate and scratches tend to occur easily. If the ratio of irregular particles is less than 45%, the polishing rate decreases due to the increase in spherical particles.

[0045] [Condition 6] Condition 6 is that, when a scanning electron microscope photograph is analyzed, the number of particles having a three-dimensional structure is T, and the total number of particles is S, the three-dimensional structure rate (T / S×100%) is 10% or more. In this embodiment, it is more preferable to satisfy condition 6. When particles have a three-dimensional structure, the presence of three-dimensional parts makes it possible to concentrate stress on the substrate and improve the polishing rate, compared to spherical or planar particles. If the three-dimensional structure ratio is 10% or more, the polishing speed can be improved. From the same viewpoint, the three-dimensional structure ratio is preferably 12% or more and 95% or less, and more preferably 15% or more and 90% or less. If the three-dimensional structure ratio exceeds 95%, although the polishing speed is high, polishing scratches tend to occur frequently and the surface smoothness tends to deteriorate. Here, whether or not a particle has a three-dimensional structure can be judged based on the color of the particle in a scanning electron microscope photograph. The three-dimensional portion of the particle can also be identified by using a transmission electron microscope photograph in combination.

[0046] [Application] When the irregular silica-based microparticle dispersion according to this embodiment is used as polishing slurry, it can improve the smoothness of the substrate surface and increase the polishing speed.Therefore, the irregular silica-based microparticle dispersion according to this embodiment can be suitably used as a component of polishing composition or polishing slurry. The polishing composition and the polishing slurry may further contain other components, such as one or more components selected from a polishing accelerator, a surfactant, a hydrophilic compound, a heterocyclic compound, a pH adjuster, and a pH buffer. EXAMPLES

[0047] The present invention will be described in more detail below by showing examples and comparative examples, but the present invention is not limited to these examples. [Example 1] (Preparation of seed particle dispersion) 1.0 kg of potassium silicate aqueous solution (Fuji Chemical Industry Co., Ltd. No. 2 potassium silicate aqueous solution, SiO2 concentration 20.5 mass%, K2O concentration 9.4 mass%, ratio of molar number of silica to alkali metal 2.04) was added to 329 g of pure water, and 157 g of potassium hydroxide aqueous solution (Toa Gosei Co., Ltd. "Super Kali R" KOH concentration 48.0 mass%) was added and stirred until it became uniform (step (a)). The pH of this solution was 12.9, the electrical conductivity was 92.3 mS / cm, the SiO2 concentration was 13.8 mass%, and the ionic strength was 1.305. Then, this solution was heated to 72 ° C while stirring and held for 80 minutes to obtain a heat-aged seed particle precursor dispersion (step (b)). Next, while maintaining the temperature of this solution, 6.51 kg of acidic silicic acid liquid (SiO2 concentration 4.55 mass%) was added over 5 hours. The molar ratio of the amount of silica in the acidic silicic acid liquid to the amount of silica in this seed particle precursor dispersion ([silica amount in acidic silicic acid liquid] / [silica amount in seed particle precursor dispersion]) was 1.44. After the addition was completed, the mixture was stirred for 1 hour while maintaining the temperature at 72°C, and then allowed to cool to room temperature to obtain a seed particle dispersion (step (c)). In the obtained seed particle dispersion, the molar ratio of silica to alkali metal was 5.0. The average particle size of the obtained seed particles was 27 nm as measured by dynamic light scattering.

[0048] (Preparation of irregular silica-based fine particle dispersion) 144 g of pure water was added to 700 g of the obtained seed particle dispersion, and the mixture was stirred until it became uniform. In this seed particle dispersion, the SiO2 concentration was 5.2 mass% and the ionic strength was 0.368 (step (d)). Furthermore, the temperature of this seed particle dispersion was raised to 97.5°C while stirring, and was kept at 97.5°C for 30 minutes (step (e)). Next, while keeping the temperature at 97.5°C, 8.96 kg of 4.55 mass% acidic silicic acid solution was added over 12 hours. The molar ratio of the amount of silica in the acidic silicic acid solution to the amount of silica in this seed particle dispersion ([silica amount in acidic silicic acid solution] / [silica amount in seed particle dispersion]) was 9.3. After the addition, the mixture was continued to stir while keeping the temperature at 97.5°C for 1 hour, and then cooled to room temperature to obtain an irregular silica-based fine particle dispersion (step (f)). In the obtained irregular silica-based fine particle dispersion, the molar ratio of silica to alkali metal was 51.2. The obtained irregular silica-based microparticle dispersion was concentrated using an ultrafiltration membrane until the silica concentration became 12% by mass. Then, it was concentrated to 20% by mass using a rotary evaporator. The obtained irregular silica-based microparticles had a specific surface area converted particle diameter of 49 nm and a dynamic light scattering particle diameter of 124 nm. Table 1 shows the conditions for producing this irregular shaped silica-based fine particle dispersion.

[0049] [Examples 2 to 3] Each step was carried out according to the conditions shown in Table 1 to obtain a dispersion of irregular shaped silica-based fine particles.

[0050] [Comparative Example 1] (Seed particle (a) preparation) 1,127g of pure water was added to 87.8g of potassium silicate (SiO2 concentration 20.5% by mass, K2O concentration 9.37% by mass), 31.4g of potassium hydroxide aqueous solution (KOH concentration 3% by mass) was added, stirred, and then heated to 83°C and held at 83°C for 30 minutes to obtain a precursor dispersion. The SiO2 concentration of this solution was 1.45% by mass. Next, 1,494 g of acidic silicic acid solution with a SiO2 concentration of 4.6 mass% was added continuously over 3 hours. Then, 8,963 g of acidic silicic acid solution was added continuously over 12 hours. After the addition was completed, the mixture was kept at 83°C for 1 hour and then cooled to room temperature. The particle diameter of the obtained seed particles (a) was 35 nm by dynamic light scattering method. The obtained silica sol was concentrated using an ultrafiltration membrane until the silica concentration became 12% by mass, and then concentrated to 20% by mass with a rotary evaporator.

[0051] (Preparation of Particles (A)) 26.0 g of potassium hydroxide aqueous solution with a KOH concentration of 48.5% by mass was added to 1,692 g of pure water and stirred until it became uniform. While continuing stirring, 460.7 g of 4.6% by mass acidic silicic acid solution was added, and then 355 g of seed particles (a) was added. The SiO2 concentration of this solution was 6.5% by mass. The temperature was further increased to 87°C and maintained at 87°C for 30 minutes. Next, 11,388 g of 4.6% by mass acidic silicic acid solution was added over 14 hours while maintaining the temperature at 87°C. After the addition was completed, stirring was continued while maintaining the temperature at 87°C for 1 hour, and the mixture was allowed to cool to room temperature to obtain a silica sol containing particles (A). Next, this silica was concentrated to 12% by mass using an ultrafiltration membrane, and then concentrated to 20% by mass using a rotary evaporator. The particle diameter of the obtained particles (A) measured by dynamic light scattering was 64 nm, and the particle diameter calculated by specific surface area was 43 nm.

[0052] [Comparative Example 2] (Preparation of Particles (B)) 274.7 g of potassium hydroxide aqueous solution with a KOH concentration of 48.5% by mass was added to 23,142 g of pure water and stirred until it was uniform. 4,951 g of 4.52% by mass acidic silicic acid solution was added while continuing stirring, and then 3,336.8 g of silica sol obtained in the same manner as the preparation of particles (A) in Comparative Example 1 was added. The SiO2 concentration of this solution was 5.0% by mass. The temperature was further increased to 98°C and maintained at 98°C for 30 minutes. Next, 128.65 kg of 4.52% by mass acidic silicic acid solution was added over 18 hours while maintaining the temperature at 98°C. After the addition was completed, stirring was continued while maintaining the temperature at 98°C for 1 hour, and the mixture was allowed to cool to room temperature to obtain a silica sol containing particles (B). Next, this silica was concentrated to 12% by mass using an ultrafiltration membrane, and then concentrated to 20% by mass using a rotary evaporator. The particle diameter of the obtained particles (B) measured by dynamic light scattering was 110 nm, and the particle diameter calculated by specific surface area was 80 nm.

[0053] [Comparative Example 3] A dispersion of irregular shaped silica-based microparticles was obtained by the same procedure as in Example 1, except that the seed particle dispersion obtained in the same manner as in Example 1 was used and the amount of pure water added to the seed particle dispersion in step (d) of Example 1 was changed to 1909 g. The obtained irregular silica-based microparticle dispersion was concentrated using an ultrafiltration membrane until the silica concentration became 12% by mass. Then, it was concentrated to 20% by mass using a rotary evaporator. The particle diameter of the obtained irregular silica-based microparticles measured by dynamic light scattering was 47 nm, and the particle diameter calculated by specific surface area was 27 nm.

[0054] [Comparative Example 4] (Preparation of Particles (D)) 3,294g of sodium silicate aqueous solution (SiO2 concentration 24.3% by mass) was added to 9,483g of pure water and stirred until homogeneous, then 347g of 4.5% by mass acidic silicic acid solution and 254g of 20% by mass KCl (flocculant) were added and mixed for 5 minutes (step (a)). The SiO2 concentration of this solution was 6.1% by mass. The mixture was then heated to 97° C. and held at 97° C. for 30 minutes. (Step (b)) The rotation speed of the stirring blade in steps (a) and (b) was set to 2.5 / sec. Then, 281.8 kg of acidic silicic acid liquid was added over 15 hours, and after the addition was completed, the mixture was left at 97°C for 30 minutes. The Reynolds number at this time was calculated to be 1.36 x 10 5 It was calculated that the solid content of the particles (D) was 10% by mass. The solid content of the particles (D) was 10% by mass. The solid content of the particles (D) was 10% by mass. The solid content of the particles (D) was 10% by mass. The particle diameter of the particles (D) was 155 nm by dynamic light scattering method, and the particle diameter of the particles (D) was 65 nm by specific surface area.

[0055] [Comparative Example 5] (Preparation of potassium silicate solution) 2.766 kg of potassium hydroxide aqueous solution (KOH concentration 48.7% by mass) was added to 3.699 kg of ultrapure water and stirred until homogenous. 2.82 kg of silica powder (water content 20% by mass) was added to this potassium hydroxide aqueous solution and mixed. This mixture was heated to 95°C and held for 4 hours to obtain a potassium silicate solution. In the obtained potassium silicate solution, the SiO2 concentration was 24.5 mass%, the K2O concentration was 12.4 mass%, and the SiO2 / K2O (molar ratio) was 3.10 (hereinafter, this potassium silicate solution or an equivalent potassium silicate solution will be referred to as "potassium silicate solution (1)"). (Preparation of Precursor Dispersion) 0.88 kg of potassium silicate solution (1) was added to 2.344 kg of ultrapure water and stirred until homogeneous to obtain an alkaline aqueous solution. 0.15 kg of acidic silicic acid solution was added to this alkaline aqueous solution and mixed. This mixture was heated to 98.5°C and held for 1.3 hours to obtain a precursor dispersion. The precursor dispersion had a SiO2 concentration of 6.6 mass% and a SiO2 / A2O (molar ratio) of 3.2.

[0056] (Preparation of seed particles (e)) To the entire amount of the obtained precursor particle dispersion, 6.97 kg of acidic silicic acid liquid was added over 4.9 hours at 98.5° C. After the addition was completed, the mixture was left at 98.5° C. for 0.5 hours to obtain a dispersion of seed particles (e). The SiO2 concentration of this seed particle dispersion was 5.2 mass % and the K2O concentration was 1.1 mass %. The average particle size measured by a dynamic light scattering particle size measuring device was 105 nm. (Preparation of Particles (E)) 0.006 kg of potassium silicate solution (1) was added to 0.113 kg of ultrapure water. 10.34 kg of seed particle dispersion liquid containing seed particles (e) was added to this and mixed. The SiO2 concentration of this solution was 5.2 mass%. Next, this was heated to 97.5°C and held for 0.5 hours. Then, 142.94 kg of acidic silicic acid liquid was added over 12 hours at 97.5°C. After the addition was completed, the mixture was left at 97.5°C for 1 hour, and then cooled to room temperature to obtain a silica particle dispersion containing particles (E). In the obtained silica particle dispersion, the SiO2 concentration was 4.6 mass% and the K2O concentration was 0.07 mass%. The mixture was then concentrated using an ultrafiltration module to prepare a silica particle dispersion with a SiO2 concentration of 11.7% by mass. It was then concentrated to 20% by mass using a rotary evaporator. The particle diameter calculated based on the specific surface area of ​​the resulting particles (E) was 41 nm, and the particle diameter measured by dynamic light scattering was 131 nm.

[0057] [Evaluation of irregular silica-based microparticle dispersion and its manufacturing method] First, Table 1 shows the various conditions for the production method of the irregular shaped silica-based fine particle dispersion. The physical properties of the irregular silica-based microparticles and the irregular silica-based microparticle dispersion were measured by the following methods, and the results are shown in Table 2. A scanning electron microscope photograph of the irregular silica-based microparticles obtained in Example 1 is shown in Figure 1. (1) Measurement of average particle size The average particle diameters of the obtained seed particle dispersion and irregular shaped silica-based fine particle dispersion were measured by dynamic light scattering. The average particle diameter of the irregular shaped silica-based fine particle dispersion was also measured by nitrogen adsorption.

[0058] (2) Analysis of irregularly shaped silica particles using scanning electron microscopy (2-1) Average degree of anomaly The average irregularity was determined by analyzing scanning electron micrographs. Specifically, scanning electron micrographs were observed, and the minimum circumscribing rectangle with the smallest area was determined from the circumscribing rectangles circumscribing any 100 or more particles. The lengths of the long and short sides of the minimum circumscribing rectangle were then determined, and the ratio of the long side to the short side ([long side] / [short side]) was taken as the irregularity. The irregularity was calculated for each particle, and the average of these was calculated as the average irregularity. (2-2) Area-equivalent circular mean particle size The area-equivalent circular particle diameter is determined by observing a scanning electron microscope photograph and finding the diameter of a circle having an area equal to the projected area of ​​any 100 or more particles, which is taken as the particle diameter of each particle. (2-3) Average irregularity of particle group [A], [B], and [B] / [A] value Scanning electron micrographs were analyzed to determine the particle size distribution of 100 or more random particles. The particle size here is the area-equivalent circular average particle size. In this particle size distribution, the average irregularity [A] of particles whose number ratio ([number] / [total number]) from the small particle size side is in the range of more than 0 and not more than 1 / 10 was determined, and the average irregularity [B] of particles whose number ratio ([number] / [total number]) from the small particle size side is in the range of more than 9 / 10 and not more than 10 / 10 was determined, and the value of [B] / [A] was further calculated. (2-4) Irregular particle rate Scanning electron micrographs were analyzed to determine the degree of irregularity for each of 100 or more random particles, and the rate of irregular particles in the total number of particles ([number of particles with an irregularity of 1.2 or more] / [total number of particles] x 100%) was calculated. (2-5) Three-dimensional structure ratio Scanning electron micrographs were analyzed to determine the number S of particles having a three-dimensional structure among 100 or more random particles. The ratio of the number S to the total number T of particles was calculated as T / S×100% to determine the three-dimensional structure rate. (2-6) Number of coarse particles The number of coarse particles in the irregular silica-based microparticle dispersion was measured using an Accusizer 780APS manufactured by Particle Sizing System Inc. The measurement sample was diluted to 1% by mass with pure water, and then 5 mL was injected into the measuring device and measured under the following conditions. After three measurements, the average value of the number of coarse particles of 0.51 μm or more was calculated from the obtained measurement data. The average value was then multiplied by 100 to obtain the number of coarse particles in the irregular silica-based microparticle dispersion calculated on a dry basis. The measurement conditions were as follows: <System Setup> ·Stir Speed ​​Control / Low Speed ​​Factor 1500 / High Speed ​​Factor 2500 <System Menu> ·Data Collection Time 60 Sec. Syringe Volume 2.5mL Sample Line Number: Sum Mode ·Initial 2nd-Stage Dilution Factor 350 ·Vessel Fast Flush Time 35 Sec. ·System Flush Time / Before Measurement 60 Sec. / After Measurement 60 Sec. ·Sample Equilibration Time 30 Sec. / Sample Flow Time 30 Sec.

[0059] (3) Polishing characteristics of irregular silica-based fine particle dispersion (3-1) Preparation of polishing slurry for evaluation Pure water was added to the irregular silica-based fine particle dispersion liquid to adjust the SiO2 concentration to 1.0 mass %, and 5% nitric acid was further added dropwise to adjust the pH to 6.0 to prepare a polishing slurry for evaluation. (3-2) TEOS film polishing speed The polishing device used was a Nanofactor NF-300, and the polishing pad was a two-layer IC-1000 / SUBA400 pad. The substrate used was an 8-inch plasma TEOS film (film thickness 2 μm) cut into 29 mm squares. The polishing load was 0.08 MPa, the rotation speeds of the head and platen were 93 rpm and 87 rpm, respectively, and polishing was performed for 15 minutes with a slurry flow rate of 50 g / min. The polishing thickness was calculated as the difference in substrate weight before and after polishing.

[0060] (3-3) Polishing scratches [Polishing test] ·Substrate to be polished The substrate to be polished was a nickel-plated aluminum substrate for hard disks (nickel-plated substrate manufactured by Toyo Kohan Co., Ltd.) This substrate was a doughnut-shaped substrate (outer diameter 95 mmφ, inner diameter 25 mmφ, thickness 1.27 mm). Polishing test 344 g of a 9% by mass silica-based particle dispersion was prepared, to which 5.65 g of a 31% by mass hydrogen peroxide solution was added, and then the pH was adjusted to 1.5 with 10% by mass nitric acid to prepare a polishing slurry. The above substrate to be polished was set in a polishing apparatus (NF300 manufactured by Nanofactor), and a polishing pad (Bellatrix NO178 manufactured by FILWEL) was used to polish the substrate by 1 μm while supplying polishing slurry at a rate of 40 g / min at a substrate load of 0.05 MPa, a platen rotation speed of 50 rpm, and a head rotation speed of 50 rpm. Polishing scratches on the circuit board The polished substrate obtained from the polishing test was observed using an ultrafine defect visualization macro device (manufactured by VISION PSYTEC, product name: Micro-Max VMX-3100) with the white light of MME-250W adjusted to 10% and LA-180Me adjusted to 0%. In this observation, if there are defects such as scratches on the substrate surface, the white light is diffusely reflected and the defective parts are observed as white. On the other hand, the white light is specularly reflected in parts without defects and the whole surface is observed as black. Observations were made in this way, and the area of ​​defects (area of ​​the substrate observed as white) caused by scratches (linear marks) on the substrate surface was evaluated according to the following criteria. "Very Few": The defect area is less than 3%. "Few": The area of ​​defects is 3% or more and less than 20%. "Many": The area of ​​defects is 20% or more but less than 40%. "Very Many": The defective area is 40% or more.

[0061] [Table 1]

[0062] [Table 2]

Claims

1. A method for producing a dispersion of irregular shaped silica-based fine particles, comprising the steps of: (a) preparing a dispersion of irregular shaped silica-based fine particles; Step (a): In the aqueous alkali silicate solution, the molar ratio of silica to alkali metal is adjusted to be in the range of 0.5 to 10, and an alkali is added as necessary to obtain SiO 2 A step of adjusting the concentration to 2% by mass or more and 25% by mass or less and adjusting the ionic strength to 0.4 or more to obtain a seed particle precursor dispersion liquid. Step (b): A step of heat-aging the seed particle precursor dispersion liquid obtained in the step (a) at a temperature in the range of 40° C. or more and less than 100° C. Step (c): Following step (b), an acidic silicic acid liquid is added to the heat-aged seed particle precursor dispersion liquid so that the molar ratio of the amount of silica in the acidic silicic acid liquid to the amount of silica in the seed particle precursor dispersion liquid ([silica amount in the acidic silicic acid liquid] / [silica amount in the seed particle precursor dispersion liquid]) is in the range of 0.5 to 10, thereby obtaining a seed particle dispersion liquid. Step (d): The seed particle dispersion liquid obtained in the step (c) is, if necessary, added with an alkali to form a SiO 2 A step of adjusting the concentration to 2% by mass or more and 15% by mass or less and the ionic strength to 0.25 or more. Step (e): Following step (d), SiO 2 A step of heating and aging the seed particle dispersion liquid whose concentration and ionic strength have been adjusted at a temperature in the range of 40° C. or more and less than 100° C. Step (f): Following step (e), an acidic silicic acid liquid is added to the heat-aged seed particle dispersion so that the molar ratio of the amount of silica in the acidic silicic acid liquid to the amount of silica in the seed particle dispersion ([amount of silica in the acidic silicic acid liquid] / [amount of silica in the seed particle dispersion]) is in the range of 5 to 20, thereby obtaining an irregular silica-based microparticle dispersion containing irregular silica-based microparticles.

2. In the step (a), an alkali is added to the seed particle precursor dispersion liquid as necessary to form a SiO 2 2. The method for producing a dispersion liquid of irregular shaped silica-based fine particles according to claim 1, wherein the concentration is adjusted to 5% by mass or more and 20% by mass or less, and the ionic strength is adjusted to 0.4 or more.

3. 3. The method for producing a dispersion of irregular shaped silica-based fine particles according to claim 1, wherein the average irregularity of the irregular shaped silica-based fine particles is 1.2 or more and 10 or less.

4. The method for producing a dispersion liquid of irregular shaped silica-based microparticles according to any one of claims 1 to 3, wherein the alkali used in the steps (b) and (d) is at least one ionic strength adjuster selected from the group consisting of sodium hydroxide and potassium hydroxide.

5. The method for producing a dispersion liquid of irregular shaped silica-based fine particles according to any one of claims 1 to 4, wherein an alkali halide is not used in any of the steps (a) to (f).

6. The irregular shaped silica-based microparticle dispersion liquid contains irregular shaped silica-based microparticles that satisfy the following conditions [1] to [4]: [1] The average particle size as measured by dynamic light scattering is 10 nm or more and 300 nm or less. [2] The average particle size calculated by a nitrogen adsorption method is 5 nm or more and 200 nm or less. [3] The average degree of deformation determined by analyzing a scanning electron microscope photograph is 1.2 or more and 10 or less. [4] In a particle size distribution obtained by analyzing a scanning electron microscope photograph, when the average irregularity of particles whose number ratio from the smaller particle size side ([number] / [total number]) is in the range of more than 0 and not more than 1 / 10 is defined as [A], and the average irregularity of particles whose number ratio from the smaller particle size side ([number] / [total number]) is in the range of more than 9 / 10 and not more than 10 / 10 is defined as [B], the value of [B] / [A] is 1.2 or more.

7. 7. The irregular shaped silica-based fine particle dispersion according to claim 6, wherein in the condition [4], the value of [A] is 1.13 or more.

8. 8. The irregular shaped silica-based fine particle dispersion according to claim 6 or 7, wherein the irregular shaped silica-based fine particles satisfy the following condition [5]: [5] When the degree of irregularity of particles is determined by analyzing a scanning electron microscope photograph, the rate of irregular particles to the total number of particles ([number of particles with an irregularity of 1.2 or more] / [total number of particles]×100%) is 45% or more.

9. The irregular shaped silica-based fine particles dispersion according to any one of claims 6 to 8, wherein the irregular shaped silica-based fine particles satisfy the following condition [6]: [6] When a scanning electron microscope photograph is analyzed, where the number of particles having a three-dimensional structure is T and the total number of particles is S, the three-dimensional structure rate (T / S×100%) is 10% or more.

Citation Information

Patent Citations

  • Manufacture of multilayer seat coil

    JP1987007345A

  • Semiconductor wafer polishing method and abrasive

    JP2001150334A

  • Konpeito-like inorganic oxide sol, its production method, and abrasive including the oxide sol

    JP2008137822A

  • Nonspherical silica sol, method for producing the same and polishing composition

    JP2009149493A

  • Method for producing chain-like particle dispersion, and dispersion of chain-like particles