Surface treatment method, region-selective film formation method on substrate surface, and surface treatment agent

A surface treatment method using a phosphorus compound and nitrogen-containing compound adjusts water repellency on semiconductor substrates, allowing selective film formation on metal and insulator regions, addressing the challenge of region-specific film control in semiconductor manufacturing.

JP7583669B2Active Publication Date: 2024-11-14TOKYO OHKA KOGYO CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021078033
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-04-30
Publication Date
2024-11-14
Estimated Expiration
2041-04-30

AI Technical Summary

Technical Problem

The challenge in semiconductor manufacturing is achieving region-selective film formation on substrates with both metal and insulator regions, where the metal region requires water repellency while the insulator region's water repellency needs to be suppressed, which existing methods struggle to control effectively.

Method used

A surface treatment method using a specific phosphorus compound and a basic nitrogen-containing compound to alter the water contact angle, making the metal region water repellent and suppressing the insulator region, followed by atomic layer deposition to selectively form films on the substrate.

Benefits of technology

The method achieves a 10° or more difference in water contact angle between metal and insulator regions, enabling selective film deposition, enhancing film thickness control and adherence, particularly in semiconductor device manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583669000001
    Figure 0007583669000001
  • Figure 0007583669000002
    Figure 0007583669000002
  • Figure 0007583669000003
    Figure 0007583669000003
Patent Text Reader

Abstract

To provide a surface treatment method capable of imparting water repellency to a metal region and suppressing the water repellency of an insulator region with respect to a substrate surface including the metal region and the insulator region that are adjacent to each other, a region-selective film forming method for a substrate surface, and a surface treatment agent that is preferably used in the surface treatment method.SOLUTION: In a surface treatment method for a surface of a substrate, the surface includes two or more regions, the two or more regions include at least one metal region and at least one insulator region, and from among two or more of the regions, at least one metal region and at least one insulator region are adjacent to each other, the metal region is made of a metal, and the insulator region consists of one or more compounds selected from the group consisting of an oxide, a nitride, a carbide, a carbonitride, an oxynitride, an oxycarbonitride, and an insulating resin, and the contact angle of water on the metal region is caused to be 10° or more higher than the contact angle of water on the insulator region that is adjacent to the metal region by reaction between a compound (P) represented by the following general formula (P-1): R1-P(=O)(OR2)(OR3), and a basic nitrogen-containing compound (B), and the regions.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a surface treatment method, a method for selectively forming a film on a region of a substrate surface, and a surface treatment agent. [Background technology]

[0002] In recent years, there has been a growing trend toward higher integration and miniaturization of semiconductor devices. Accordingly, patterned organic films used as masks and patterned inorganic films produced by etching processes are becoming finer. For this reason, there is a demand for thickness control at the atomic layer level for organic and inorganic films formed on semiconductor substrates. Atomic layer deposition (ALD; hereafter simply referred to as "ALD") is known as a method for forming a thin film on a substrate at the atomic layer level. The ALD method is known to have both high step coverage and film thickness controllability compared to the general CVD (Chemical Vapor Deposition) method.

[0003] The ALD method is a thin-film formation technology in which two types of gases, the main components of which are the elements that make up the film to be formed, are alternately supplied onto a substrate, and a thin film is formed on the substrate in atomic layer units by repeating this process multiple times to form a film of the desired thickness. The ALD method utilizes a self-limiting growth function in which only the components of the source gas that are sufficient to form one or several atomic layers are adsorbed onto the substrate surface while the source gas is being supplied, while excess source gas does not contribute to growth. For example, when forming an Al2O3 film on a substrate, a source gas made of TMA (TriMethyl Aluminum) and an oxidizing gas containing O are used. When forming a nitride film on a substrate, a nitriding gas is used instead of the oxidizing gas.

[0004] In recent years, attempts have been made to form a film selectively on a substrate surface using the ALD method (see Patent Document 1 and Non-Patent Document 1). Accordingly, there is a demand for substrates having surfaces that are selectively modified in areas that can be suitably applied to selectively forming films on the substrate by the ALD method. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Special Publication No. 2003-508897 [Non-patent literature]

[0006] [Non-Patent Document 1] J.Phys.Chem.C 2014,118,10957-10962 Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention has been made in consideration of the above circumstances, and has an object to provide a surface treatment method that can make the metal regions water-repellent and suppress the water-repellentization of the insulator regions on a substrate surface including adjacent metal regions and insulator regions, a method for selectively forming a film on a substrate surface including the surface treatment method, and a surface treatment agent that is suitably used in the above-mentioned surface treatment method. [Means for solving the problem]

[0008] The present inventors have discovered that the above-mentioned problems can be solved by using a surface treatment method for a substrate surface, the surface including two or more regions, the two or more regions including at least one metal region and at least one insulator region, at least one of the metal region and at least one insulator region being adjacent to one another among the two or more regions, the metal region being made of metal, the insulator region being made of one or more compounds selected from the group consisting of oxides, nitrides, carbides, carbonitrides, oxynitrides, oxycarbonitrides, and insulating resins, and using a surface treatment method that involves a reaction between a compound (P), which is a phosphorus compound having a specific structure, and a basic nitrogen-containing compound (B) and the regions, and have completed the present invention.

[0009] A first aspect of the present invention is a surface treatment method for a surface of a substrate, comprising the steps of: the surface comprises two or more regions; the two or more regions include at least one metal region and at least one insulator region; At least one of the metal regions and at least one of the insulator regions are adjacent to each other, the metal region is made of a metal, and the insulator region is made of one or more compounds selected from the group consisting of oxides, nitrides, carbides, carbonitrides, oxynitrides, oxycarbonitrides, and insulating resins; The following general formula (P-1): R 1 -P(=O)(OR 2 )(OR 3 ) ···(P-1) [In the formula, R 1 is an alkyl group, a fluorinated alkyl group, an alkoxy group, or an aromatic hydrocarbon group which may have a substituent, and R 2 and R 3 each independently represents a hydrogen atom, an alkyl group, a fluorinated alkyl group, or an aromatic hydrocarbon group which may have a substituent. A compound (P) represented by the formula: A basic nitrogen-containing compound (B); This is a surface treatment method in which the contact angle of water on the metal region is made 10° or more higher than the contact angle of water on the insulator region adjacent to the metal region by reaction with the metal region.

[0010] A second aspect of the present invention includes treating the surface of the substrate by the surface treatment method according to the first aspect; forming a film on the surface of the surface-treated substrate by atomic layer deposition; A method for selectively depositing a film on a substrate surface, the method comprising depositing more of the film material on the insulating regions than on the metallic regions.

[0011] A third aspect of the present invention is a surface treatment agent used in the surface treatment method according to the first aspect, comprising: The following general formula (P-1): R 1 -P(=O)(OR 2 )(OR 3 ) ···(P-1) [In the formula, R 1 is an alkyl group, a fluorinated alkyl group, an alkoxy group, or an aromatic hydrocarbon group which may have a substituent, and R 2 and R 3 each independently represents a hydrogen atom, an alkyl group, a fluorinated alkyl group, or an aromatic hydrocarbon group which may have a substituent. A compound (P) represented by the formula: A basic nitrogen-containing compound (B); A solvent; It is a one-liquid type surface treatment agent containing the above.

[0012] A fourth aspect of the present invention is a surface treatment agent used in the surface treatment method according to the first aspect, comprising: The following general formula (P-1): R 1 -P(=O)(OR 2 )(OR 3 ) ···(P-1) [In the formula, R 1 is an alkyl group, a fluorinated alkyl group, an alkoxy group, or an aromatic hydrocarbon group which may have a substituent, and R 2and R 3 each independently represents a hydrogen atom, an alkyl group, a fluorinated alkyl group, or an aromatic hydrocarbon group which may have a substituent. A first surface treatment agent containing a compound (P) represented by the formula: and a solvent; a second surface treatment agent containing a basic nitrogen-containing compound (B) and a solvent; It is a two-liquid type surface treatment agent having the above features. Effect of the Invention

[0013] According to the present invention, it is possible to provide a surface treatment method that can make the metal regions water-repellent and suppress the water-repellentization of the insulator regions on a substrate surface including adjacent metal regions and insulator regions, a method for selectively forming a film on a substrate surface including the surface treatment method, and a surface treatment agent that is preferably used in the above-mentioned surface treatment method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] <Surface treatment method> The surface treatment method is a surface treatment method for a surface of a substrate. The surface of the substrate includes two or more regions. The two or more regions include at least one metal region and at least one insulator region. Of the two or more regions, at least one of the metal regions and at least one of the insulator regions are adjacent to each other. Here, "adjacent" includes a case where at least one of the metal regions and at least one of the insulator regions are adjacent to each other while sharing a boundary line, or a case where they are adjacent to each other or spaced apart without sharing a boundary line. In the surface treatment method, the contact angle of water on the metal region is made 10° or more higher than the contact angle of water on the insulator region adjacent to the metal region by reaction of the compound (P) and the basic nitrogen-containing compound (B) described below with the region.

[0015] (Substrate and substrate surface) In the surface treatment method, the "substrate" to be surface treated is exemplified by a substrate used for manufacturing a semiconductor device. Examples of such substrates include silicon (Si) substrates, silicon nitride (SiN) substrates, silicon oxide (Ox) substrates, tungsten (W) substrates, cobalt (Co) substrates, germanium (Ge) substrates, aluminum (Al) substrates, nickel (Ni) substrates, ruthenium (Ru) substrates, copper (Cu) substrates, titanium nitride (TiN) substrates, tantalum nitride (TaN) substrates, silicon germanium (SiGe) substrates, etc. The "surface of the substrate" refers to the surface of the substrate itself, as well as the surfaces of a patterned inorganic layer and an unpatterned inorganic layer provided on the substrate, and the surface of a patterned inorganic layer essentially includes the side surface of the pattern.

[0016] Examples of the patterned inorganic layer provided on the substrate include a patterned inorganic layer formed by preparing an etching mask on the surface of an inorganic layer present on the substrate by a photoresist method and then etching the same, and a patterned inorganic layer formed on the substrate surface by an atomic layer deposition method (ALD method). The surface treatment agent of the present invention can also be used when obtaining a patterned inorganic layer formed on the substrate surface by the ALD method. By using the surface treatment agent of the present invention, the selectivity between the region corresponding to the metal region and the region corresponding to the insulator region of the inorganic layer can be ensured. Examples of inorganic layers include the substrate itself, oxide films of elements constituting the substrate, silicon nitride (SiN) formed on the surface of the substrate, silicon oxide film (SiOx), tungsten (W), cobalt (Co), germanium (Ge), aluminum (Al), nickel (Ni), ruthenium (Ru), copper (Cu), silver (Ag), titanium (Ti), gold (Au), chromium (Cr), molybdenum (Mo), aluminum oxide (Al2O3), titanium oxide (TiO2), zirconium oxide (ZrO2), hafnium oxide (HfO2), tantalum oxide (Ta2O5), titanium nitride (TiN), tantalum nitride (TaN), silicon germanium (SiGe), silicon oxide (SiO2), and other inorganic films or layers. Such films or layers are not particularly limited, but examples thereof include inorganic films or layers formed during the manufacturing process of semiconductor devices. The non-patterned inorganic layer provided on the substrate may be, for example, an inorganic film or layer made of the same material as the patterned inorganic layer provided on the substrate.

[0017] (Metal and insulator regions) The metal region is made of metal. The metal region may be defined as a conductive region in contrast to the insulator region described below. As the metal, among the above inorganic substances, copper (Cu), cobalt (Co), aluminum (Al), silver (Ag), nickel (Ni), titanium (Ti), gold (Au), chromium (Cr), molybdenum (Mo), tungsten (W), ruthenium (Ru), titanium nitride (TiN), tantalum nitride (TaN), etc. are preferable. The insulating region is made of one or more compounds selected from the group consisting of oxides, nitrides, carbides, carbonitrides, oxynitrides, oxycarbonitrides, and insulating resins, and is preferably an oxide, a nitride, a carbide, a carbonitride, an oxynitride, or an oxycarbonitride. As the oxide, aluminum oxide (Al2O3), titanium oxide (TiO2), zirconium oxide (ZrO2), hafnium oxide (HfO2), tantalum oxide (Ta2O5), silicon oxide (SiOx (1≦x≦2)), fluorine-containing silicon oxide (SiOF), and carbon-containing silicon oxide (SiOC) are preferable. As the nitride, for example, silicon nitride (SiN) and boron nitride (BN) are preferable. As the carbide, silicon carbide (SiC) is preferable. As the carbonitride, silicon carbonitride (SICN) is preferable. As the oxynitride, silicon oxynitride (SiON) is preferable. The oxycarbonitride is preferably silicon oxycarbonitride (SiOCN).The insulating resin may be polyimide, polyester, plastic resin, or the like.

[0018] In the surface treatment method, the contact angle of water on the metal region is made 10° or more higher than the contact angle of water on the insulator region adjacent to the metal region, which indicates that the metal region is made water repellent and the insulator region is prevented from becoming water repellent.

[0019] (Substrate surface consisting of two regions) An example of a substrate surface having two regions is one in which one of the two regions is a first metal region and the adjacent region is a second insulator region. Here, each of the first and second regions may or may not be divided into a plurality of regions. Examples of the first region and the second region include, for example, A mode in which the surface of the substrate itself is the metal region, which is the first region, and a layer made of an insulator formed on the surface of the substrate is the insulator region, which is the second region; A mode in which the surface of the substrate itself is an insulating region that is a first region, and a layer made of metal formed on the surface of the substrate is a metal region that is a second region; A mode in which a layer made of metal formed on the surface of the substrate is a metal region that is a first region, and a layer made of an insulator formed on the surface of the substrate is an insulator region that is a second region; Examples of such an embodiment include an embodiment in which a portion of the surface of an insulator substrate is made into a metal region, which is the first region, and a layer made of an insulator formed on at least a portion of the surface of the substrate that is not the metal region and / or at least a portion of the surface of the substrate that is not the metal region (or the entire surface of the substrate that is not the metal region) is made into an insulator region, which is the second region.

[0020] (Substrate surface consisting of three or more regions) Examples of substrate surface configurations consisting of three or more regions include a configuration in which one of the two or more regions is a first region, which is a metal region, a region adjacent to it is a second region, which is an insulator region, and a region adjacent to the second insulator region is a third region, which is a metal region; and a configuration in which one of the two or more regions is a first region, which is an insulator region, a region adjacent to it is a second region, which is a metal region, and a region adjacent to the second metal region is a third region, which is an insulator region. Here, the first region and the third region are made of different materials. Furthermore, each of the first region, the second region, and the third region may or may not be divided into a plurality of regions. Examples of the first region, second region, and third region include, for example, a configuration in which the surface of the substrate itself is the metal region which is the first region, the surface of an insulator region formed on the surface of the substrate close to the substrate is the second region, and the surface of a metal region formed on the surface of the substrate close to the second region is the third region; a configuration in which the surface of the substrate itself is the insulator region which is the first region, the surface of a metal region formed on the surface of the substrate close to the substrate is the second region, and the surface of an insulator region formed on the surface of the substrate close to the second region is the third region, etc. A similar approach can be applied when a fourth or more regions are present. The upper limit of the number of regions made of different materials is not particularly limited as long as the effects of the present invention are not impaired, but is, for example, 7 or less or 6 or less, and typically 5 or less.

[0021] (Compound (P)) The surface treatment method involves reacting a compound (P) represented by the following general formula (P-1) with the above region.

[0022] R 1 -P(=O)(OR 2 )(OR 3 ) ···(P-1) [In the formula, R 1 is an alkyl group, an alkoxy group, a fluorinated alkyl group, or an aromatic hydrocarbon group which may have a substituent; R 2 and R 3 each independently represents a hydrogen atom, an alkyl group, a fluorinated alkyl group, or an aromatic hydrocarbon group which may have a substituent.

[0023] In the compound (P) represented by the formula (P-1), R 1 The alkyl group is preferably a straight-chain or branched-chain alkyl group having 8 or more carbon atoms, and more preferably a straight-chain or branched-chain alkyl group having 12 or more carbon atoms.

[0024] R 1Specific preferred examples of the alkyl group as the alkyl group include an octyl group, a nonyl group, a decyl group, an undecyl group, a dodecyl group, a tridecyl group, an isotridecyl group, a tetradecyl group, a pentadecyl group, a hexadecyl group, an isohexadecyl group, a heptadecyl group, an octadecyl group, a nonadecyl group, an icosyl group, a henicosyl group, and a docosyl group, as well as alkyl groups that are structurally isomeric to these alkyl groups.

[0025] In the compound (P) represented by the formula (P-1), R 1 The alkoxy group is preferably a straight-chain or branched-chain alkoxy group having 8 or more carbon atoms, and more preferably a straight-chain or branched-chain alkoxy group having 12 or more carbon atoms.

[0026] R 1 Specific preferred examples of the alkoxy group as the alkoxy group include an octyloxy group, a nonyloxy group, a decyloxy group, an undecyloxy group, a dodecyloxy group, a tridecyloxy group, an isotridecyloxy group, a tetradecyloxy group, a pentadecyloxy group, a hexadecyloxy group, an isohexadecyloxy group, a heptadecyloxy group, an octadecyloxy group, a nonadecyloxy group, an icosyloxy group, a henicosyloxy group, and a docosyloxy group, as well as alkoxy groups that are structurally isomeric to these alkoxy groups.

[0027] In the compound (P) represented by the formula (P-1), R 1 The fluorinated alkyl group is preferably a linear or branched fluorinated alkyl group having 8 or more carbon atoms, and more preferably a linear or branched fluorinated alkyl group having 12 or more carbon atoms.

[0028] R 1 Preferable specific examples of the fluorinated alkyl group as R 1 and groups in which some or all of the hydrogen atoms of the alkyl group have been substituted with fluorine atoms.

[0029] In the compound (P) represented by the formula (P-1), R 1Examples of the aromatic hydrocarbon group which may have a substituent include a phenyl group, a naphthyl group, an anthryl group, a p-methylphenyl group, a p-tert-butylphenyl group, a p-adamantylphenyl group, a tolyl group, a xylyl group, a cumenyl group, a mesityl group, a biphenyl group, a phenanthryl group, a 2,6-diethylphenyl group, and a 2-methyl-6-ethylphenyl group.

[0030] In the compound (P) represented by the formula (P-1), R 1 The upper limit of the number of carbon atoms that the above-mentioned substituents have is not particularly limited, but is, for example, 45 or less.

[0031] In the compound (P) represented by the formula (P-1), R 2 and R 3 The alkyl group is preferably a straight-chain or branched-chain alkyl group having 8 or more carbon atoms.

[0032] R 2 and R 3 Specific preferred examples of the alkyl group as the alkyl group include an octyl group, a nonyl group, a decyl group, an undecyl group, a dodecyl group, a tridecyl group, an isotridecyl group, a tetradecyl group, a pentadecyl group, a hexadecyl group, an isohexadecyl group, a heptadecyl group, an octadecyl group, a nonadecyl group, an icosyl group, a henicosyl group, and a docosyl group, as well as alkyl groups that are structurally isomeric to these alkyl groups.

[0033] In the compound (P) represented by the formula (P-1), R 2 and R 3 The fluorinated alkyl group is preferably a linear or branched fluorinated alkyl group having 8 or more carbon atoms.

[0034] R 2 and R 3 Preferable specific examples of the fluorinated alkyl group as R 2 and R 3 and groups in which some or all of the hydrogen atoms of the alkyl group have been substituted with fluorine atoms.

[0035] In the compound (P) represented by the formula (P-1), R 2 and R 3 Examples of the aromatic hydrocarbon group which may have a substituent include a phenyl group, a naphthyl group, an anthryl group, a p-methylphenyl group, a p-tert-butylphenyl group, a p-adamantylphenyl group, a tolyl group, a xylyl group, a cumenyl group, a mesityl group, a biphenyl group, a phenanthryl group, a 2,6-diethylphenyl group, and a 2-methyl-6-ethylphenyl group.

[0036] Among them, R 2 R 3 is preferably a hydrogen atom.

[0037] The compound (P) may be used alone or in combination of two or more kinds.

[0038] (Basic nitrogen-containing compound (B)) The surface treatment method comprises reacting a basic nitrogen-containing compound (B) with the above-mentioned region.

[0039] The basic nitrogen-containing compound (B) refers to a compound that inhibits the water repellency of the insulating region by the compound (P). Although the reason for such a property of the basic nitrogen-containing compound (B) is not clear, it is presumed that it is due to the fact that the cationic species of the basic nitrogen-containing compound (B) adsorbs to the insulating region and inhibits the adsorption of the compound (P) to the insulating region. The basic nitrogen-containing compound (B) is not particularly limited as long as it has such a property, but examples thereof include quaternary ammonium compounds, pyridinium halides, pyrrolidinium halides, bipyridinium halides, and pK b Amines or their salts with a pK of 2.5 or less (hereinafter referred to as "low pK b (Also referred to as "amine").

[0040] An example of the quaternary ammonium compound is a quaternary ammonium salt represented by the following formula (b1). [ka]

[0041] In formula (b1), R a1 ~R a4 R each independently represents an alkyl group having 1 to 16 carbon atoms, an aryl group having 6 to 16 carbon atoms, an aralkyl group having 7 to 16 carbon atoms, or a hydroxyalkyl group having 1 to 16 carbon atoms. a1 ~R a4 may be bonded to each other to form a cyclic structure, and in particular, a1 and R a2 Combination with and R a3 and R a4 At least one of the combinations of may be bonded to each other to form a cyclic structure. In formula (b1), X - represents a hydroxide ion, a chloride ion, a fluoride ion, or an organic carboxylate ion which may have fluorine. Examples of the organic carboxylate ion which may have fluorine include an acetate ion and a trifluoroacetate ion.

[0042] Among the compounds represented by formula (b1), hydroxides, chlorides, or fluorides of tetramethylammonium, tetraethylammonium, tetrapropylammonium, tetrabutylammonium, methyltripropylammonium, methyltributylammonium, ethyltrimethylammonium, dimethyldiethylammonium salt, benzyltrimethylammonium, hexadecyltrimethylammonium, (2-hydroxyethyl)trimethylammonium, and spiro-(1,1')-bipyrrolidinium are preferred in terms of availability, and hydroxides or fluorides are more preferred in terms of the effects of the present invention, with hydroxides or fluorides of tetramethylammonium and benzyltrimethylammonium being even more preferred. The pyridinium halide may be pyridinium chloride or fluoride, with the fluoride being preferred. The pyrrolidinium halide may be pyrrolidinium chloride or fluoride, with the fluoride being preferred. The bipyridinium halide may be a bipyridinium chloride or fluoride, with the fluoride being preferred.

[0043] low pK b pK of amine b is preferably 2.0 or less, more preferably 1.5 or less. b The amines include, for example, guanidine derivatives.

[0044] Examples of the guanidine derivative include methylguanidine, dimethylguanidine, trimethylguanidine, tetramethylguanidine, and chloride or fluoride salts thereof. Among these, tetramethylguanidine or its fluoride salt is preferred.

[0045] (reaction) The surface treatment method involves reacting a compound (P) and a basic nitrogen-containing compound (B) with the surface of a substrate including the metal region and the insulator region. Examples of the method for reacting these compounds include a method using a one-liquid type surface treatment agent containing the compound (P), the basic nitrogen-containing compound (B), and a solvent, and a method using a two-liquid type surface treatment agent including a first surface treatment agent containing the compound (P) and a solvent, and a second surface treatment agent containing the basic nitrogen-containing compound (B) and a solvent. Examples of the surface treatment method include a method in which the surface treatment agent is exposed to the surface of the substrate by means of, for example, an immersion method, or a coating method such as a spin coating method, a roll coating method, or a doctor blade method.

[0046] From the viewpoint of making the metal region water-repellent, the content of the compound (P) in the one-component surface treatment agent is preferably from 0.001% by mass to 5% by mass, more preferably from 0.005% by mass to 4% by mass, even more preferably from 0.01% by mass to 3% by mass, and particularly preferably from 0.03% by mass to 3% by mass, relative to the total mass of the one-component surface treatment agent. The content of the compound (P) in the first surface treatment agent in the two-component surface treatment agent is, from the viewpoint of making the metal region water-repellent, preferably from 0.001% by mass to 5% by mass, more preferably from 0.005% by mass to 4% by mass, even more preferably from 0.01% by mass to 3% by mass, and particularly preferably from 0.03% by mass to 3% by mass, relative to the total mass of the first surface treatment agent.

[0047] From the viewpoint of suppressing water repellency of the insulator region, the content of the basic nitrogen-containing compound (B) in the one-component surface treatment agent is preferably from 0.0001 to 5% by mass, more preferably from 0.001 to 4% by mass, even more preferably from 0.005 to 3% by mass, and particularly preferably from 0.01 to 3% by mass, based on the total mass of the one-component surface treatment agent. The content of the basic nitrogen-containing compound (B) in the second surface treatment agent in the two-component surface treatment agent is, from the viewpoint of suppressing water repellency of the insulator region, preferably from 0.0001 mass % to 5 mass %, more preferably from 0.001 mass % to 4 mass %, even more preferably from 0.005 mass % to 3 mass %, and particularly preferably from 0.01 mass % to 3 mass %, relative to the total mass of the second surface treatment agent.

[0048] Examples of the solvent include sulfoxides, sulfones, amides, lactams, imidazolidinones, dialkyl glycol ethers, monoalcohol solvents, (poly)alkylene glycol monoalkyl ethers, (poly)alkylene glycol monoalkyl ether acetates, other ethers, ketones, other esters, lactones, linear, branched, or cyclic aliphatic hydrocarbons, aromatic hydrocarbons, and terpenes.

[0049] The sulfoxides include dimethyl sulfoxide.

[0050] Examples of sulfones include dimethyl sulfone, diethyl sulfone, bis(2-hydroxyethyl) sulfone, and tetramethylene sulfone.

[0051] Examples of amides include N,N-dimethylformamide, N-methylformamide, N,N-dimethylacetamide, N-methylacetamide, and N,N-diethylacetamide.

[0052] Examples of lactams include N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N-propyl-2-pyrrolidone, N-hydroxymethyl-2-pyrrolidone, and N-hydroxyethyl-2-pyrrolidone.

[0053] Examples of imidazolidinones include 1,3-dimethyl-2-imidazolidinone, 1,3-diethyl-2-imidazolidinone, and 1,3-diisopropyl-2-imidazolidinone.

[0054] Examples of dialkyl glycol ethers include dimethyl glycol, dimethyl diglycol, dimethyl triglycol, methyl ethyl diglycol, diethyl glycol, and triethylene glycol butyl methyl ether.

[0055] Examples of monoalcohol solvents include methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, sec-butanol, tert-butanol, n-pentanol, isopentanol, 2-methylbutanol, sec-pentanol, tert-pentanol, 3-methoxybutanol, 3-methyl-3-methoxybutanol, n-hexanol, 2-methylpentanol, sec-hexanol, 2-ethylbutanol, sec-heptanol, and 3-heptanol. Examples of alcohols include 1-octanol, 2-ethylhexanol, sec-octanol, n-nonyl alcohol, 2,6-dimethyl-4-heptanol, n-decanol, sec-pentadecyl alcohol, trimethylnonyl alcohol, sec-tetradecyl alcohol, sec-heptadecyl alcohol, phenol, cyclohexanol, methylcyclohexanol, 3,3,5-trimethylcyclohexanol, benzyl alcohol, phenylmethylcarbinol, diacetone alcohol, and cresol.

[0056] Examples of (poly)alkylene glycol monoalkyl ethers include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol mono-n-propyl ether, ethylene glycol mono-n-butyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol mono-n-propyl ether, diethylene glycol mono-n-butyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-n-propyl ether, propylene glycol mono-n-butyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol mono-n-propyl ether, dipropylene glycol mono-n-butyl ether, tripropylene glycol monomethyl ether, and tripropylene glycol monoethyl ether.

[0057] Examples of the (poly)alkylene glycol monoalkyl ether acetates include ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate.

[0058] Examples of other ethers include dimethyl ether, diethyl ether, methyl ethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, diisoamyl ether, diethylene glycol dimethyl ether, diethylene glycol methyl ethyl ether, diethylene glycol diethyl ether, tetraethylene glycol dimethyl ether, and tetrahydrofuran.

[0059] Examples of ketones include methyl ethyl ketone, cyclohexanone, 2-heptanone, and 3-heptanone.

[0060] Other esters include, for example, alkyl lactate esters such as methyl 2-hydroxypropionate and ethyl 2-hydroxypropionate; ethyl 2-hydroxy-2-methylpropionate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, ethyl ethoxyacetate, ethyl hydroxyacetate, methyl 2-hydroxy-3-methylbutanoate, 3-methoxybutyl acetate, 3-methyl-3-methoxy-1-butyl acetate, 3-methyl-3-methoxybutylpropionate, ethyl acetate, n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, n-pentyl acetate, n-hexyl acetate, n-heptyl acetate, n-octyl acetate, n-pentyl formate, isopentyl acetate, n-butyl propionate, ethyl butyrate, n-propyl butyrate, isopropyl butyrate, n-butyl butyrate, methyl n-octanoate, methyl decanoate, methyl pyruvate, ethyl pyruvate, n-propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, ethyl 2-oxobutanoate, dimethyl adipate, and propylene glycol diacetate.

[0061] Examples of lactones include propylolactone, γ-butyrolactone, and 6-pentyrolactone.

[0062] Examples of linear, branched, or cyclic aliphatic hydrocarbons include n-hexane, n-heptane, n-octane, n-nonane, methyloctane, n-decane, n-pentane, n-dodecane, 2,2,4,6,6-pentamethylheptane, 2,2,4,4,6,8,8-heptamethylnonane, cyclohexane, and methylcyclohexane.

[0063] Examples of aromatic hydrocarbons include benzene, toluene, xylene, 1,3,5-trimethylbenzene, and naphthalene.

[0064] Examples of terpenes include p-menthane, diphenylmenthane, limonene, terpinene, bornane, norbornane, and pinane.

[0065] Among these, the solvent is preferably 3-methyl-3-methoxy-1-butyl acetate, ethyl acetate, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, diethylene glycol monomethyl ether, 1-octanol, or methyl ethyl ketone, and more preferably propylene glycol monomethyl ether or 1-octanol.

[0066] Examples of other components that can be incorporated into the surface treatment agent include a pH adjuster, an antioxidant, an ultraviolet absorber, a viscosity adjuster, and an antifoaming agent.

[0067] The pH of the one-liquid type surface treatment agent and the pH of the second surface treatment agent in the two-liquid type surface treatment agent are preferably 5 or more, more preferably 8 or more. If the basic nitrogen-containing compound (B) used in the present invention is contained, the pH of the one-liquid type surface treatment agent and the pH of the second surface treatment agent in the two-liquid type surface treatment agent will be in the above-mentioned suitable pH range. Therefore, in order to adjust the pH to the above-mentioned suitable pH, components other than the above-mentioned essential components are usually not required.

[0068] The exposure temperature is, for example, 10°C or higher and 90°C or lower, preferably 20°C or higher and 80°C or lower, more preferably 20°C or higher and 70°C or lower, and even more preferably 20°C or higher and 30°C or lower. The exposure time is preferably 20 seconds or more, more preferably 30 seconds or more, and even more preferably 45 seconds or more, from the viewpoint of making the metal region water-repellent and suppressing the insulator region from becoming water-repellent. The upper limit of the exposure time is not particularly limited, but is, for example, 2 hours or less, typically 1 hour or less, preferably 15 minutes or less, more preferably 5 minutes or less, and particularly preferably 2 minutes or less. After the exposure, washing and / or drying may be performed as necessary. Washing is performed, for example, by rinsing with water or rinsing with an activator, etc. Drying is performed by blowing with nitrogen, etc.

[0069] By reacting with the above region, the compound (P) can be selectively adsorbed to the metal region out of the adjacent metal region and insulator region, and as a result, the contact angle of water on the metal region can be made 10° or more, preferably 15° or more, more preferably 20° or more, and even more preferably 25° or more higher than the contact angle of water on the insulator region adjacent to the above metal region. The contact angle of the substrate surface with water after exposure to the surface treatment agent can be, for example, from 50° to 140°. By controlling the material of the substrate surface, the type and amount of the surface treatment agent used, and the exposure conditions, the contact angle with water can be set to 50° or more, preferably 60° or more, more preferably 70° or more, and even more preferably 90° or more. The upper limit of the contact angle is not particularly limited, but is, for example, 140° or less, typically 130° or less. More specifically, the water contact angle of the metal region is preferably 70° or more, more preferably 80° or more, more preferably 90° or more, and even more preferably 100° or more. The upper limit of the contact angle is not particularly limited, but is, for example, 140° or less. The contact angle of water on the insulator region is preferably equal to or less than 70°, more preferably equal to or less than 65°, and even more preferably equal to or less than 60°. The lower limit of the contact angle is not particularly limited, but is, for example, equal to or more than 50°.

[0070] <Selective film formation method on substrate surface> Next, a method for selectively forming a film on a substrate surface using the above-mentioned surface treatment method will be described. A method for selectively depositing a film on a substrate surface includes treating the surface of the substrate by the above-described surface treatment method, and forming a film on the surface-treated substrate by atomic layer deposition (ALD), depositing more material of the film on the insulating region than on the metal region.

[0071] As a result of the surface treatment, the water contact angle of the metal region can be made 10° or more higher than the water contact angle of the insulator region adjacent to the metal region. The ALD film-forming material is less likely to be adsorbed to the metal region on the substrate surface where the water contact angle is larger than that of the insulator region. As a result, a thick film can be selectively formed on the insulator region by repeating the ALD cycle.

[0072] (Film formation by ALD method) Although the film formation method using the ALD method is not particularly limited, it is preferably a thin film formation method by adsorption using at least two gas phase reactants (hereinafter simply referred to as "precursor gases"). The adsorption using the precursor gas is preferably chemical adsorption. Specifically, the method includes a method including the following steps (a) and (b), which are repeated at least once (one cycle) until a desired film thickness is obtained. (a) exposing a substrate that has been surface treated by the method according to the second aspect to a pulse of a first precursor gas; and (b) following step (a) above, exposing the substrate to a pulse of a second precursor gas.

[0073] After the above step (a) and before the above step (b), a plasma treatment step, a step of removing or evacuating (purging) the first precursor gas and its reactants using a carrier gas, a second precursor gas, etc., etc. may or may not be included. After the above step (b), a plasma treatment step, a step of removing or purging the second precursor gas and its reactants with a carrier gas or the like, and the like may or may not be included. The carrier gas may be an inert gas such as nitrogen gas, argon gas, or helium gas.

[0074] Preferably, each pulse per cycle and each layer formed is self-limiting, and more preferably, each layer formed is a monolayer. The thickness of the monoatomic layer can be, for example, 5 nm or less, preferably 3 nm or less, more preferably 1 nm or less, and further preferably 0.5 nm or less.

[0075] Examples of the first precursor gas include organic metals, metal halides, and metal oxide halides, and specific examples thereof include tantalum pentaethoxide, tetrakis(dimethylamino)titanium, pentakis(dimethylamino)tantalum, tetrakis(dimethylamino)zirconium, tetrakis(dimethylamino)hafnium, tetrakis(dimethylamino)silane, copper hexafluoroacetylacetonate vinyltrimethylsilane, Zn(C2H5)2, Zn(CH3)2, TMA (trimethylaluminum), TaCl5, WF6, WOCl4, CuCl, ZrCl4, AlCl3, TiCl4, SiCl4, and HfCl4.

[0076] The second precursor gas may be a precursor gas capable of decomposing the first precursor or a precursor gas capable of removing a ligand of the first precursor, such as H2O, H2O2, O2O3, NH3, H2S, H2Se, PH3, AsH3, C2H4, or Si2H6.

[0077] The exposure temperature in step (a) is not particularly limited, but is, for example, 100°C or higher and 800°C or lower, preferably 150°C or higher and 650°C or lower, more preferably 200°C or higher and 500°C or lower, and even more preferably 225°C or higher and 375°C or lower.

[0078] The exposure temperature in step (b) is not particularly limited, but may be a temperature substantially equal to or higher than the exposure temperature in step (a). Films formed by the ALD method are not particularly limited, and examples thereof include films containing pure elements (e.g., Si, Cu, Ta, W), films containing oxides (e.g., SiO2, GeO2, HfO2, ZrO2, Ta2O5, TiO2, Al2O3, ZnO, SnO2, Sb2O5, B2O3, In2O3, WO3), films containing nitrides (e.g., Si3N4, TiN, AlN, BN, GaN, NbN), films containing carbides (e.g., SiC), films containing sulfides (e.g., CdS, ZnS, MnS, WS2, PbS), films containing selenides (e.g., CdSe, ZnSe), films containing phosphides (GaP, InP), films containing arsenides (e.g., GaAs, InAs), and mixtures thereof.

[0079] <Surface treatment agent> Next, the surface treatment agent used in the above surface treatment method will be described. The surface treatment agent is a one-liquid type surface treatment agent containing a compound (P) represented by the following general formula (P-1), a basic nitrogen-containing compound (B), and a solvent. In another embodiment, the surface treatment agent is a two-liquid type surface treatment agent including a first surface treatment agent containing a compound (P) represented by the following general formula (P-1) and a solvent, and a second surface treatment agent containing a basic nitrogen-containing compound (B) and a solvent. Whether the surface of the substrate is treated with a one-liquid type surface treatment agent or a two-liquid type surface treatment agent, the metal region can be made water repellent and the insulator region can be prevented from becoming water repellent. In addition, the above-mentioned surface treatment agent may contain components other than the compound (P), the basic nitrogen-containing compound (B), and the solvent (hereinafter also referred to as "other components"), so long as the desired effect is obtained. In the following, essential or optional components that the one-liquid type surface treatment agent and the two-liquid type surface treatment agent may contain will be described.

[0080] (Compound (P)) The compound (P) is represented by the following general formula (P-1).

[0081] R 1 -P(=O)(OR 2 )(OR 3) ···(P-1) [In the formula, R 1 is an alkyl group, an alkoxy group, a fluorinated alkyl group, or an aromatic hydrocarbon group which may have a substituent; R 2 and R 3 each independently represents a hydrogen atom, an alkyl group, a fluorinated alkyl group, or an aromatic hydrocarbon group which may have a substituent.

[0082] The compound (P) represented by the above formula (P-1) is the same as the above-mentioned compound (P) contained in the surface treatment agent used in the above-mentioned surface treatment method.

[0083] The compound (P) may be used alone or in combination of two or more kinds. From the viewpoint of making the metal region water-repellent, the content of the compound (P) in the one-component surface treatment agent is preferably from 0.001% by mass to 5% by mass, more preferably from 0.005% by mass to 4% by mass, even more preferably from 0.01% by mass to 3% by mass, and particularly preferably from 0.03% by mass to 3% by mass, relative to the total mass of the one-component surface treatment agent. The content of the compound (P) in the first surface treatment agent in the two-component surface treatment agent is, from the viewpoint of making the metal region water-repellent, preferably from 0.001% by mass to 5% by mass, more preferably from 0.005% by mass to 4% by mass, even more preferably from 0.01% by mass to 3% by mass, and particularly preferably from 0.03% by mass to 3% by mass, relative to the total mass of the first surface treatment agent.

[0084] (Basic nitrogen-containing compound (B)) The basic nitrogen-containing compound (B) is the same as the above-mentioned basic nitrogen-containing compound (B) contained in the surface treatment agent used in the above-mentioned surface treatment method.

[0085] The basic nitrogen-containing compound (B) may be used alone or in combination of two or more kinds. From the viewpoint of suppressing water repellency of the insulator region, the content of the basic nitrogen-containing compound (B) in the one-component surface treatment agent is preferably from 0.0001 to 5% by mass, more preferably from 0.001 to 4% by mass, even more preferably from 0.005 to 3% by mass, and particularly preferably from 0.01 to 3% by mass, based on the total mass of the one-component surface treatment agent. The content of the basic nitrogen-containing compound (B) in the second surface treatment agent in the two-component surface treatment agent is, from the viewpoint of suppressing water repellency of the insulator region, preferably from 0.0001 mass % to 5 mass %, more preferably from 0.001 mass % to 4 mass %, even more preferably from 0.005 mass % to 3 mass %, and particularly preferably from 0.01 mass % to 3 mass %, relative to the total mass of the second surface treatment agent.

[0086] (solvent) The solvent is the same as the above-mentioned solvent contained in the surface treatment agent used in the above-mentioned surface treatment method.

[0087] (Other ingredients) Examples of other components include a pH adjuster, an antioxidant, an ultraviolet absorber, a viscosity adjuster, and an antifoaming agent.

[0088] The surface treatment agent can be obtained by mixing the above-mentioned compound (P), compound (S), a solvent, and, if necessary, other components, by a known method.

[0089] The pH of the one-liquid type surface treatment agent and the pH of the second surface treatment agent in the two-liquid type surface treatment agent are preferably 5 or more, more preferably 8 or more. If the basic nitrogen-containing compound (B) used in the present invention is contained, the pH of the one-liquid type surface treatment agent and the pH of the second surface treatment agent in the two-liquid type surface treatment agent will be in the above-mentioned suitable pH range. Therefore, in order to adjust the pH to the above-mentioned suitable pH, components other than the above-mentioned essential components are usually not required.

[0090] The method of using the one-liquid type surface treatment agent includes, for example, a method of reacting the one-liquid type surface treatment agent with the surface of the substrate including the metal region and the insulator region. The reaction method includes, for example, a method of exposing the one-liquid type surface treatment agent to the surface of the substrate by means of a dipping method, or a coating method such as a spin coating method, a roll coating method, or a doctor blade method. The reaction conditions such as the exposure temperature are the same as those in the above-mentioned surface treatment method. An example of a method for using the two-liquid surface treatment agent is a method in which the second surface treatment agent is reacted with the surface of the substrate including the metal region and the insulator region, and then the first surface treatment agent is reacted with the surface of the substrate including the metal region and the insulator region. By using the above method, the metal region can be made water-repellent and the insulator region can be prevented from becoming water-repellent. EXAMPLES

[0091] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0092] [Examples 1 to 4 and Comparative Examples 1 to 3] (Preparation of Surface Treatment Agent) The following compound (P) and the following basic nitrogen-containing compound (B) were uniformly mixed in the following solvent in the amounts shown in Table 1 below to prepare the surface treatment agents of Examples 1 to 4 and Comparative Examples 1 to 3. As the compound (P), the following P1 was used. P1: Octadecylphosphonic acid As the basic nitrogen-containing compound (B), the following B1 to B6 were used. B2: Triethylamine (pK b =3.85) B3: Pyrrolidine (pK b =3.03) B4: 1,1,3,3-tetramethylguanidine (pK b =1.24) B5: Tetramethylammonium hydroxide B6: Benzyltrimethylammonium hydroxide In Example 2, a propylene glycol solution containing 15 mass % of B5 was used, in Example 3, an aqueous solution containing 25 mass % of B5 was used, and in Example 4, an ethanol solution containing 40 mass % of B6 was used. As the solvent, the following A1 was used. A1: Propylene glycol monomethyl ether

[0093] (Pretreatment, surface treatment) Using the obtained surface treatment agents of Examples 1 to 4 and Comparative Examples 1 to 3, surface treatments were carried out on Al2O3 substrates and Cu substrates according to the following method. Specifically, each substrate was pretreated by immersing it in an aqueous HF solution with a concentration of 25 ppm at 25° C. for 10 seconds. After the pretreatment, each substrate was washed with deionized water for 1 minute. After washing with water, each substrate was dried with a nitrogen stream. Each substrate after drying was immersed in the above-mentioned surface treatment agent at 25° C. for 1 minute to perform surface treatment for each substrate. Each substrate after surface treatment was washed with isopropanol for 1 minute, and then washed with deionized water for 1 minute. Each washed substrate was dried with a nitrogen gas flow to obtain each surface-treated substrate.

[0094] (Measurement of water contact angle) After the above surface treatment, the contact angle of water was measured for each substrate. The water contact angle was measured using a Dropmaster700 (Kyowa Interface Science Co., Ltd.) by dropping a droplet of pure water (2.0 μL) onto the surface of each substrate and measuring the contact angle 2 seconds after dropping. In addition, the "difference in water contact angle" was calculated by subtracting the water contact angle of the Al2O3 substrate from the water contact angle of the Cu substrate. The results are shown in Table 1.

[0095] [Table 1]

[0096] From Table 1, when each substrate was surface-treated with the surface treatment agents of Comparative Examples 1 to 3, the maximum difference in water contact angle was only 1.0° in Comparative Example 2. On the other hand, when the surface treatment agent of Example 1 was used, the difference in water contact angle exceeded 10°. Furthermore, the water contact angles of Cu were roughly the same between Example 1 and Comparative Examples 1 to 3. From these experimental results, it can be seen that by using an amine having a pKb of 2.5 or less in combination with compound (P) as the basic nitrogen-containing compound (B), the difference in water contact angle becomes 10° or more, and water repellency of the Al2O3 substrate, which is the insulating region, is selectively suppressed. Furthermore, when each substrate was surface-treated with the surface treatment agents of Examples 2 to 4, the difference in water contact angle was at least 32.3° in Example 2. These experimental results show that the use of a quaternary ammonium compound as the basic nitrogen-containing compound (B) further suppresses the water repellency of the Al2O3 substrate.

[0097] [Examples 5A to 5C] (Preparation of Surface Treatment Agent) The following compound (P) and the following basic nitrogen-containing compound (B) were uniformly mixed in the following solvent in the amounts shown in Table 4 below, and oxalic acid (100% solid) was added in amounts of 0.001 mass %, 0.005 mass %, and 0.010 mass %, respectively, to adjust the pH, thereby preparing surface treatment agents of Examples 5A to 5C, each having a pH of 10.97, 10.69, and 10.10, respectively. As the compound (P), the following P1 was used. P1: Octadecylphosphonic acid As the basic nitrogen-containing compound (B), the following B4 was used. B4: 1,1,3,3-tetramethylguanidine As the solvent, the following A1 was used. A1: Propylene glycol monomethyl ether

[0098] (Measurement of water contact angle) Using the obtained surface treatment agents, an Al2O3 substrate and a Cu substrate were pretreated with an HF aqueous solution and surface-treated with each surface treatment agent in the same manner as in Examples 1 to 4 and Comparative Examples 1 to 3, and the water contact angle of each substrate after surface treatment was measured. In addition, the difference between the water contact angle of the Cu substrate and the water contact angle of the Al2O3 substrate was calculated. The results are shown in Table 4.

[0099] (Etching rate measurement) The etching rates (nm / min) of the Al2O3 substrate and Cu substrate were calculated from the change in film thickness of each substrate before and after surface treatment with each surface treatment agent, and changes of ±0.5 nm / min or less were evaluated as "Good." The results are shown in Table 2.

[0100] [Table 2]

[0101] The results of the water contact angle in Table 2 show that in the surface treatment agent based on Example 1, the difference in water contact angle is 10° or more in the pH range of 10.10 to 10.97. Furthermore, from the etching rate results in Table 2, it is clear that damage to each substrate was suppressed, and that the difference in water contact angle is not due to substrate damage.

[0102] [Examples 6 to 7] (Preparation of Surface Treatment Agent) The following compound (P) and the following basic nitrogen-containing compound (B) were uniformly mixed in the following solvent in the amounts shown in Table 3 below to prepare the surface treatment agents of Examples 6 to 7. As the compound (P), the following P1 was used. P1: Octadecylphosphonic acid As the basic nitrogen-containing compound (B), the following B7 to B8 were used. B7: Tetramethylammonium fluoride B8: Tetrabutylammonium fluoride As the solvent, the following A1 was used. A1: Propylene glycol monomethyl ether

[0103] (Measurement of water contact angle) Using the obtained surface treatment agents, an Al2O3 substrate and a Cu substrate were pretreated with an HF aqueous solution and surface-treated with each surface treatment agent in the same manner as in Examples 1 to 4 and Comparative Examples 1 to 3, and the water contact angle of each substrate after surface treatment was measured. In addition, the difference between the water contact angle of the Cu substrate and the water contact angle of the Al2O3 substrate was calculated. The results are shown in Table 3.

[0104] [Table 3]

[0105] From the results in Table 3, when each substrate was surface-treated with the surface treatment agents of Examples 6 to 7, the difference in water contact angle was as small as 72.9° in Example 7. These experimental results show that the use of a fluoride salt of a quaternary ammonium compound as the basic nitrogen-containing compound (B) extremely selectively inhibits the Al2O3 substrate from becoming water repellent.

[0106] [Surface treatment and ALD deposition test 1 and comparison test 1-2] Using the surface treatment agent of Example 6, which had a large difference in water contact angle, Test 1 was performed on a SiO2 substrate and a Cu substrate by the following procedure, using the surface treatment and ALD film formation. The results of each test piece were evaluated assuming that they were the results when a metal region and an insulator region were included on the same substrate. Comparative Test 1 was performed by carrying out surface treatment and ALD film formation in the same procedure as Test 1 above, except that the surface treatment agent of Comparative Example 1 was used instead of the surface treatment agent of Example 6. Comparative Test 2 was performed by carrying out immersion in the surface treatment agent of the following procedure 3 only once before the first ALD cycle treatment in Comparative Test 1. (procedure) 1. A test piece having a SiO2 region and a Cu region was cleaned with dilute hydrofluoric acid for 1 minute. 2. After the treatment, the test piece was rinsed with pure water and then blown with nitrogen. 3. After blowing, the test piece was immersed in the surface treatment agent of Example 6 for 1 minute, then thoroughly washed with isopropanol for 1 minute, rinsed with pure water, and then blown with nitrogen. 4. ALD cycle processing was performed 18 times under the following conditions. Atomic layer deposition (ALD) equipment: AT-410 (manufactured by Anric Technologies) Chamber temperature: 150℃ Precursor: Trimethylaluminum and H2O 5. The above steps 2 to 4 were repeated for each 18 cycle treatment, and a total of 144 ALD cycles (18 times x 8) were performed. 6. The amount of Al2O3 deposited on each test piece after 18, 36, and 144 cycles was confirmed by X-ray fluorescence analysis. The results are shown in Table 4.

[0107] [Table 4]

[0108] As shown in Table 4, even after 144 cycles, the selectivity of the ALD film was well maintained by performing treatment with the surface treatment agent of Example 6, suggesting that it is possible to provide a contrast of nearly 10 nm. On the other hand, with the composition of Comparative Example 1, it was not possible to form a thick film even after repeated cycles, and the contrast was lost even when the surface treatment conditions were changed. From these test results, it is evident that the use of the surface treatment agent according to the present invention not only enables selective ALD film formation on a patterned substrate having a Cu region (pattern) and an Al2O3 region (pattern), but also enables selective thickening of an Al2O3 film on a patterned substrate having a Cu region and a SiO2 region.

Claims

1. A surface treatment method for a surface of a substrate, comprising the steps of: the surface comprises two or more regions; the two or more regions include at least one metal region and at least one insulator region; At least one of the metal regions and at least one of the insulator regions are adjacent to each other, the metal region is made of a metal, and the insulator region is made of one or more compounds selected from the group consisting of oxides, nitrides, carbides, carbonitrides, oxynitrides, oxycarbonitrides, and insulating resins; The following general formula (P-1): R 1 -P(=O)(OR 2 )(OR 3 ) ・・・(P-1) [In the formula, R 1 is an alkyl group, an alkoxy group, a fluorinated alkyl group, or an aromatic hydrocarbon group which may have a substituent, R 2 and R 3 each independently represents a hydrogen atom, an alkyl group, a fluorinated alkyl group, or an aromatic hydrocarbon group which may have a substituent. Compound (P) represented by the formula: A basic nitrogen-containing compound (B); A surface treatment method, comprising: reacting with said region to cause a contact angle of water on said metal region to be at least 10° higher than a contact angle of water on said insulator region adjacent to said metal region.

2. 2. The surface treatment method according to claim 1, wherein the basic nitrogen-containing compound (B) is selected from the group consisting of quaternary ammonium compounds, pyridinium halides, pyrrolidinium halides, bipyridinium halides, and amines or salts thereof having a pKb of 2.5 or less.

3. 3. The surface treatment method according to claim 1, wherein the metal is at least one selected from the group consisting of copper, cobalt, aluminum, silver, nickel, titanium, gold, chromium, molybdenum, tungsten, ruthenium, titanium nitride, and tantalum nitride, and the insulator is at least one selected from the group consisting of aluminum oxide, titanium oxide, zirconium oxide, hafnium oxide, tantalum oxide, silicon oxide, fluorine-containing silicon oxide, carbon-containing silicon oxide, silicon nitride, boron nitride, silicon carbide, silicon carbonitride, silicon oxynitride, and silicon oxycarbonitride.

4. The surface treatment method according to any one of claims 1 to 3, wherein after the reaction, the metal region has a contact angle with water of 70° or more.

5. treating the surface of the substrate by the surface treatment method according to any one of claims 1 to 4; forming a film on the surface of the surface-treated substrate by atomic layer deposition; A method for selectively depositing a film on a surface of a substrate, the method comprising depositing more of the film material on the insulating regions than on the metallic regions.

6. A surface treatment agent used in the surface treatment method according to any one of claims 1 to 4, The following general formula (P-1): R 1 -P(=O)(OR 2 )(OR 3 ) ・・・(P-1) [In the formula, R 1 is an alkyl group, an alkoxy group, a fluorinated alkyl group, or an aromatic hydrocarbon group which may have a substituent, R 2 and R 3 each independently represents a hydrogen atom, an alkyl group, a fluorinated alkyl group, or an aromatic hydrocarbon group which may have a substituent. A compound (P) represented by the formula: A basic nitrogen-containing compound (B); A solvent; A one-component surface treatment agent containing the compound.

7. A surface treatment agent used in the surface treatment method according to any one of claims 1 to 4, The following general formula (P-1): R 1 -P(=O)(OR 2 )(OR 3 ) ・・・(P-1) [In the formula, R 1 is an alkyl group, an alkoxy group, a fluorinated alkyl group, or an aromatic hydrocarbon group which may have a substituent, R 2 and R 3 each independently represents a hydrogen atom, an alkyl group, a fluorinated alkyl group, or an aromatic hydrocarbon group which may have a substituent. A first surface treatment agent containing a compound (P) represented by the formula: and a solvent; a second surface treatment agent containing a basic nitrogen-containing compound (B) and a solvent; A two-component surface treatment agent comprising:

Citation Information

Patent Citations

  • A bottomless deposition method for barrier layers in integrated circuit metallization schemes

    JP2003508897A

  • Surface treatment agent, surface treatment method and area selective film production method for substrate surface

    JP2021014631A

  • Pattern formation method

    WO2019139043A1

  • Polymerizable self-assembled monolayers for use in atomic layer deposition

    WO2019202418A1