Carbon steel austenitic stainless steel rolled composite plate and its manufacturing method
The manufacturing method for a carbon steel austenitic stainless steel rolled composite plate achieves a balance of mechanical properties and corrosion resistance by using specific annealing and cooling processes, resulting in a composite plate with varied strength levels and improved corrosion resistance.
Patent Information
- Application Number
- JP2022529742
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-11-29
- Filing Date
- 2020-11-27
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2040-11-27
AI Technical Summary
Existing high-strength structural steels face challenges in achieving both mechanical properties and corrosion resistance due to alloying element interactions and annealing processes, leading to issues like increased costs, reduced plasticity, and poor corrosion resistance.
A manufacturing method for a carbon steel austenitic stainless steel rolled composite plate involving specific annealing temperatures, cooling rates, and chemical element compositions to create a composite plate with a high-strength carbon steel layer and an austenitic stainless steel layer, ensuring both mechanical properties and corrosion resistance.
The method produces a composite plate with strength levels from 780MPa to 1700MPa and excellent corrosion resistance, addressing the limitations of existing high-strength steels by integrating austenitic stainless steel's properties with carbon steel.
Smart Images

Figure 0007583800000001 
Figure 0007583800000002 
Figure 0007583800000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a steel plate and a manufacturing method thereof, and more particularly to a steel plate provided with an austenitic stainless steel layer and a manufacturing method thereof. [Background technology]
[0002] In the past decade, structural steels, especially automotive structural steels, have been widely used, among which high-strength automotive structural steels have become the main product for reducing the weight and improving the structural strength of automobiles. Structural steels are mainly obtained by controlling various manufacturing processes to obtain different structures and properties, and their types mainly include precipitation strengthened steels, martensitic steels, dual-phase steels, TRIP steels (QP steels), multi-phase steels, etc., and their strengths cover various strength levels from 780MPa to 1700MPa. However, although cold-rolled high-strength structural steels from 780MPa to 1180MPa have achieved considerable use performance, there are still some problems in use performance that need to be urgently solved.
[0003] Ultra-high strength steel, which is carbon steel, has a lower surface corrosion resistance than stainless steel. In order to improve the corrosion resistance, a special phosphate coating process or additional plating layers are required in the factory. These additional processes increase the cost. In addition, with the increase in strength of high strength steel, the amount of alloying elements added also increases, and the surface concentration of alloying elements during the manufacturing process affects the performance of the phosphate coating and the galvanic property, which is disadvantageous to the production of high strength steel plate with corrosion resistance. Therefore, the present invention provides a rolled composite plate of carbon steel + austenitic stainless steel, which has an austenitic stainless steel layer and a high strength carbon steel layer, which provides the basis for different specific mechanical properties of the whole steel plate.
[0004] Austenitic stainless steel has excellent corrosion resistance, heat resistance, low-temperature strength and mechanical properties, and at the same time, it has excellent workability such as press working and bending, and does not have the phenomenon of heat treatment hardening. However, austenitic stainless steel is a metastable stainless steel, which is prone to work hardening and precipitation phase transition during production and processing, resulting in improved material strength, reduced plasticity, reduced formability and reduced corrosion resistance. In order to realize austenitic stainless steel with excellent corrosion resistance and strong plastic recovery, and to eliminate the hardening stress caused by press working, current technology mainly realizes softening by annealing after cold rolling. The commonly used annealing method is: the annealing temperature is 1050-1150 ° C, the holding time is 30 seconds or more, and then cooled to room temperature.
[0005] The annealing curves of structural high-strength carbon steels are varied, and various strength levels from 780MPa to 1700MPa can be achieved through the combination of compositions. However, due to the limited alloy content of structural carbon steels, the austenitizing temperature is low, and if the same annealing soaking temperature as austenitic stainless steels is used, the grains will become coarse. At the same time, the annealing curves of structural carbon steels include various controlled cooling conditions, which is different from the manufacturing process of austenitic stainless steels, which is soaked and then quenched. For this reason, it is difficult for rolled composite steel sheets containing carbon steel layers and austenitic stainless steel layers to achieve both mechanical properties and corrosion resistance with a single annealing.
[0006] Based on this, a manufacturing method for a carbon steel + austenitic stainless steel rolled composite plate is expected, which can adjust the structure and properties of the carbon steel layer without changing the structure and properties of the austenitic stainless steel layer, and realize the performance of a high-strength carbon steel + austenitic stainless steel rolled composite plate. Summary of the Invention [Problem to be solved by the invention]
[0007] One of the objectives of the present invention is to provide a method for producing a carbon steel-austenitic stainless steel rolled composite plate, which has an austenitic stainless steel layer and a high-strength carbon steel layer that provides the basis for different specific mechanical properties of the entire steel plate, and the carbon steel-austenitic stainless steel rolled composite plate has various strength levels and also has good corrosion resistance. [Means for solving the problem]
[0008] In order to achieve the above object, the present invention proposes a method for producing the above carbon steel austenitic stainless steel rolled composite plate, which includes the following steps: (1) preparing a carbon steel layer billet and a stainless steel layer billet; (2) Billet assembly; (3) Composite rolling; (4) Cold rolling; (5) First annealing: The annealing temperature is 1050-1150°C, the holding time is 30 seconds or more, and then cooled to room temperature. In the cooling process, quenching is performed in the temperature range of 900-500°C, and the cooling rate is controlled at 20-200°C / s.
[0009] (6) Double annealing: Heat to a soaking temperature of 800-950°C at a heating rate of 5°C / s or more, hold for 10-100 seconds, then cool to a rapid cooling start temperature T at a rate of v1=3-20°C / s, preferably 5-20°C / s, where T≧800-10×v1, and then cool to 150-450°C at a rate of 20-1000°C / s; then perform overaging treatment, the overaging temperature is 150-450°C, and the overaging treatment time is 100-400s.
[0010] In the manufacturing method of the present invention, in step (5), the reason for setting the annealing temperature to 1050-1150 ° C is as follows: when austenitic stainless steel is solution annealed at 1050-1150 ° C, the precipitated carbide is re-solutionized, and then rapidly cooled to room temperature. Because of the fast cooling rate in the rapid cooling process, the solutionized carbon does not have time to combine with other alloy elements and precipitate, thereby improving the resistance to intergranular corrosion. In addition, when the annealing temperature of austenitic stainless steel exceeds 1150 ° C, the crystal grains become coarse, the grain size level decreases, and the corrosion resistance of the strip steel decreases. Therefore, based on the above considerations, the process parameters of step (5) are set as follows: the annealing temperature is 1050-1150 ° C, the holding time is 30 seconds or more, and then cooled to room temperature, and rapid cooling is performed in the cooling process in the temperature range of 900-500 ° C, and the cooling rate is controlled to 20-200 ° C / s. In some embodiments, the heat-holding time in step (5) is 30-80 s. In some embodiments, the cooling rate in the temperature range of 900-500 ° C. is 20-180 ° C. / s. In step (6), the soaking temperature in the second annealing is set to 800-950 ° C. because it is lower than the austenitizing temperature and higher than the upper limit of the precipitation susceptibility temperature of the stainless steel layer. In addition, in order to prevent the precipitation of carbides and σ phase, the slow cooling rate v1 is set to 3-20 ° C. / s, and then cooled to 150-450 ° C. at a rate of 20-1000 ° C. / s; then, in order to prevent the reprecipitation of the solution-treated carbides and σ phase, overaging treatment is performed, and the overaging treatment time is 100-400 seconds. In some embodiments, the heating rate in step (6) is controlled to 5-20 ° C. / s.
[0011] Furthermore, in the manufacturing method of the present invention, in step (3), the billet is heated to 1100-1260°C and kept at that temperature for 0.6 hours or more, the final rolling temperature is controlled to 850°C or more, and after rolling, it is cooled at a rate of 30-100°C / s, and the coiling temperature is controlled to 450-600°C. In some embodiments, in step (3), the keeping time is 0.6 hours to 3 hours. In some embodiments, the final rolling temperature in step (3) is 850-920°C.
[0012] Through research, the inventors of the present application have found that the lower the final rolling temperature, the higher the coiling temperature, and the more precipitated carbides and σ phases will be precipitated at the grain boundaries. When other rolling process parameters are the same, a lower final rolling temperature and a higher coiling temperature are more likely to precipitate carbides and σ phases and cause grain boundary corrosion. Therefore, it is necessary to control the final rolling temperature to be high and the coiling temperature to be low. However, considering that a final rolling temperature that is too high and a coiling temperature that is too low cannot be stably controlled, in the manufacturing method of the present invention, the final rolling temperature is controlled to be 850°C or higher, and after rolling, the steel is quenched at a rate of 30 to 100°C / s, and the coiling temperature is controlled to be 450 to 600°C.
[0013] Furthermore, in the manufacturing method of the present invention, in step (4), the cold rolling reduction is controlled to 40-70%.
[0014] The manufacturing method of the present invention also includes planarization in step (7). Furthermore, the mass percentage contents of chemical elements in the austenitic stainless steel layer billet for assembling the billet are: C: 0.02%~0.15%, Si: 0.3%~1.0%, Mn: 1.0%~10.5%, Cr: 14.0~20.0%, Ni: 0.2~14.0%, N≦0.25%, Cu≦0.6%, Mo≦3.0%, and the balance is Fe and other unavoidable impurities.
[0015] Furthermore, the mass percent contents of the chemical elements of the carbon steel layer billet for assembling the billet are: C: 0.05%-0.35%, Si: 0.1%-2.0%, Mn: 0.5%-3.0%, Al: 0.01%-0.08%, the balance being Fe and other unavoidable impurities. Furthermore, the carbon steel layer billet further contains one or more elements of B, Nb, Ti, V, Cr and Mo; preferably, the mass percents of each chemical element are: B≦0.005%, Nb≦0.1%, Ti≦0.15%, V≦0.15%, Cr≦0.6%, Mo≦0.3%. In some embodiments, the mass percent of Ti is 0.01-0.15%.
[0016] Furthermore, during assembly of the billet, the ratio of thickness of the carbon steel layer to each of the austenitic stainless steel layers is 5-30:1, preferably 7-10:1.
[0017] The present invention further provides a rolled composite plate of carbon steel and austenitic stainless steel obtained by the above-mentioned production method.
[0018] It should be noted that in the technical solution of the present invention, the carbon steel layer is the base layer, and the austenitic stainless steel is the coating layer, and the carbon steel layer may be combined with the austenitic stainless steel coating layer on one side or both sides.
[0019] Furthermore, in the carbon steel-austenitic stainless steel rolled composite plate of the present invention, the mass percent content of the chemical elements in the austenitic stainless steel layer is: C: 0.02%~0.15%, Si: 0.3%~1.0%, Mn: 1.0%~10.5%, Cr: 14.0~20.0%, Ni: 0.2~14.0%, N≦0.25%, Cu≦0.6%, Mo≦3.0%, and the balance is Fe and other unavoidable impurities.
[0020] In the carbon steel-austenitic stainless steel rolled composite plate of the present invention, the design principles of each chemical element of the austenitic stainless steel layer are as follows: C: Carbon is an element that strongly forms, stabilizes, and expands the austenite phase region, and plays an important role in the austenite structure and strength at room temperature; especially when the Ni content is relatively low, C plays an important role in stabilizing the austenite structure; however, if the C content is too high, it will affect the plasticity and corrosion resistance of the steel, so the mass percentage of C in the austenitic stainless steel layer of the carbon steel-austenitic stainless steel rolled composite plate of the present invention is controlled to 0.02-0.15%.
[0021] Si: Si is a ferrite-forming element. If the Si content is too high, the corrosion resistance of chromium-nickel austenitic stainless steel will decrease, and the intergranular corrosion susceptibility of the steel in solid solution state will increase. Therefore, in order to ensure that the steel has an austenitic structure and corrosion resistance at room temperature, it is necessary to control the Si content in the steel; However, in the smelting process of austenitic stainless steel, Si is used as a deoxidizing agent, so a certain amount of Si must be contained; And the mass percentage of Si in the austenitic stainless steel layer of the carbon steel-austenitic stainless steel rolled composite plate of the present invention is controlled to 0.3-1.0%.
[0022] Mn: Mn is a weak austenite forming element, but a strong austenite stabilizing element in stainless steel, Mn can greatly improve the solubility of N in steel; when the N content is high and the Ni content is low, a part of Ni will be replaced by the combined action of Mn, N and C, and a certain amount of Mn element is required to stabilize the austenite structure; however, Mn has a negative effect on the corrosion resistance of stainless steel, so if the Mn content is too high, the pitting corrosion resistance and crevice corrosion resistance of steel will decrease, so the mass percentage of Mn in the austenitic stainless steel layer of the carbon steel-austenitic stainless steel rolled composite plate of the present invention is controlled to be 1.0-10.5%.
[0023] Cr: Cr is the most important alloying element of stainless steel and the most fundamental element for ensuring the corrosion resistance of stainless steel; With increasing Cr content in steel, the susceptibility of stainless steel to intergranular corrosion decreases, and the strength increases, but the plasticity and cold forming properties decrease; At the same time, if Cr is too high, a correspondingly high Ni equivalent is required to obtain the austenitic structure at room temperature. Therefore, taking the above into consideration, the mass percentage of Cr in the austenitic stainless steel layer of the carbon steel-austenitic stainless steel rolled composite plate of the present invention is controlled to be 14.0-20.0%.
[0024] Ni: Ni is an important austenite forming and stabilizing element, which can promote the stability of the passive film of stainless steel, reduce the ductile-brittle transition temperature, and improve the cold formability and weldability; at the same time, Ni is also an expensive element, which has an important impact on the cost of austenitic stainless steel; therefore, the mass percentage of Ni in the austenitic stainless steel layer of the carbon steel-austenitic stainless steel rolled composite plate of the present invention is controlled to be 0.2-14.0%.
[0025] N: N is a very powerful element that forms, stabilizes and expands the austenite phase region of austenitic stainless steel; Through solution strengthening, N can significantly improve the room temperature and high temperature strength of austenitic stainless steel, and does not significantly reduce the plastic toughness of the steel, but at the same time, N can improve the acid corrosion resistance and local corrosion resistance of austenitic stainless steel; Since the solubility of N in stainless steel is limited, it is necessary to ensure that N exists in a solution state in coordination with other elements to avoid the generation of subcutaneous pores during the solidification process; Considering the mass percentage of alloying elements such as Mn and C in the present invention, the austenitic stainless steel layer of the carbon steel-austenitic stainless steel rolled composite plate of the present invention is controlled to N≦0.25%.
[0026] Cu: Cu can improve the rust resistance and corrosion resistance of austenitic stainless steel, especially in reducing media such as sulfuric acid, and tends to greatly reduce the strength and cold work hardening tendency of stainless steel; however, when Cu is added to chromium-manganese austenitic stainless steel using Mn and N instead of Ni, the delayed fracture sensitivity of the austenitic stainless steel is much lower than that of chromium-nickel austenitic stainless steel, and the thermoplasticity of the austenitic stainless steel decreases with increasing Cu content in the steel; therefore, the percentage of Cu in the austenitic stainless steel layer of the carbon steel-austenitic stainless steel rolled composite plate of the present invention is controlled to be not more than 0.6%.
[0027] Mo: The addition of Mo element can greatly improve the corrosion resistance and high temperature strength of austenitic stainless steel, especially it can achieve high temperature resistance of 1200-1300 degrees, and can be used under severe conditions. Therefore, the mass percentage of Mo in the austenitic stainless steel layer of the carbon steel-austenitic stainless steel rolled composite plate of the present invention is controlled to be ≦3.0%.
[0028] In the carbon steel austenitic stainless steel rolled composite plate of the present invention, it is necessary to reduce the amount of unavoidable impurities as much as possible, but considering the limitations of technology and manufacturing costs, the mass percentage of unavoidable impurity elements such as P and S is controlled to the range of P≦0.035% and S≦0.015%. P is an impurity element in steel, which has a negative effect on the plasticity, toughness, and corrosion resistance of stainless steel, so the content needs to be reduced as much as possible during manufacturing, so the austenitic stainless steel layer of the carbon steel austenitic stainless steel rolled composite plate of the present invention is controlled to P≦0.035%; S is an impurity element in steel, which has a negative effect on the high-temperature plasticity, toughness, and corrosion resistance of stainless steel, so the content needs to be reduced as much as possible during manufacturing, so the austenitic stainless steel layer of the carbon steel austenitic stainless steel rolled composite plate of the present invention is controlled to S≦0.015%.
[0029] Furthermore, in the carbon steel-austenitic stainless steel rolled composite plate of the present invention, the mass percent content of the chemical elements in the austenitic carbon steel layer is: C: 0.05% to 0.35%, Si: 0.1% to 2.0%, Mn: 0.5% to 3.0%, Al: 0.01% to 0.08%, and the balance is Fe and other unavoidable impurities.
[0030] C: The addition of C element plays an important role in improving the strength of steel, ensuring that bainite or martensite phase transformation occurs and produces phase transformation strengthening. C, together with alloying elements, precipitates finely dispersed metal carbides, resulting in fine grain strengthening and precipitation strengthening. Considering the weldability of the carbon steel austenitic stainless steel rolled composite plate of the present invention, the mass percentage of C in the carbon steel layer of the carbon steel austenitic stainless steel rolled composite plate of the present invention is controlled to 0.05% to 0.35%.
[0031] Si: Si is an element that strengthens ferrite and can effectively increase the strength of ferrite. In addition, Si is an element that forms non-carbides. In the isothermal process, Si can strongly inhibit the formation of Fe3C, and concentrate carbon in untransformed austenite, greatly improving the stability of austenite, and can maintain room temperature to produce the TRIP effect. Based on this, the mass percentage of Si in the carbon steel austenitic stainless steel rolled composite plate of the present invention is controlled to be 0.1% to 2.0%.
[0032] Mn: Mn is a carbide-forming element, which can dissolve carbon, delay the transformation of pearlite, lower the Bs point, inhibit the transformation of bainite, and play an important role in the formation window of martensite. The addition of Mn reduces the martensite transformation temperature and increases the content of retained austenite, while Mn has little effect on the toughness of the steel plate, and the steel containing 1.5-2.5 mass% Mn can effectively improve the resistance to the decomposition of retained austenite. However, Mn significantly lowers the Ms point and has a negative effect on weldability, so the amount of Mn needs to be appropriate, and in the carbon steel austenitic stainless steel rolled composite plate of the present invention, the mass percentage of Mn in the carbon steel layer is controlled to 0.5%-3.0%.
[0033] Al: The addition of Al plays a role in deoxidation and grain refinement. Like Si, Al is also a non-carbide forming element, which can strongly inhibit the formation of Fe3C and concentrate carbon in untransformed austenite. Although the solution strengthening effect of Al is weaker than that of Si, in the technical solution of the present invention, Al element can be added to reduce the side effect of silicon. In the carbon steel austenitic stainless steel rolled composite plate of the present invention, the mass percentage of Al in the carbon steel layer is controlled to 0.01%-0.08%.
[0034] Furthermore, in the carbon steel-austenitic stainless steel rolled composite plate of the present invention, the carbon steel layer contains at least one of the chemical elements B≦0.005%, Nb≦0.1%, Ti≦0.15%, V≦0.15%, Cr≦0.6%, and Mo≦0.3%.
[0035] B: Boron can improve the hardenability of steel, because in the process of austenite transformation, the nucleation of new phase (ferrite) is most likely to occur at the grain boundary. However, steel containing more than 0.005% boron exhibits the phenomenon of thermal embrittlement. Based on this, in the carbon steel austenitic stainless steel rolled composite plate of the present invention, the mass percentage of B in the carbon steel layer is controlled to B≦0.005%.
[0036] Nb: In the process of controlled rolling, the strain-induced precipitates of Nb can greatly reduce the recrystallization temperature of deformed austenite through grain pinning and subgrain boundary, provide nucleation grains, and have obvious effect on grain refinement. Based on this, in the carbon steel austenitic stainless steel rolled composite plate of the present invention, the mass percentage of Nb in the carbon steel layer is controlled to be Nb≦0.1%.
[0037] Ti: Ti is the main compound element of Ti-Mo-C nano-precipitates, and at the same time, Ti also has a strong effect of inhibiting the growth of austenite grains and refining grains at high temperatures. Based on this, in the carbon steel-austenitic stainless steel rolled composite plate of the present invention, the mass percentage of Ti in the carbon steel layer is controlled to Ti≦0.15%. In some embodiments, the mass percentage of Ti is 0.01-0.15%.
[0038] V: After V controls the occurrence of rolling phase transition, it remains in austenite and further precipitates in ferrite, which brings about significant precipitation strengthening effect. Based on this, in the carbon steel austenitic stainless steel rolled composite plate of the present invention, the mass percentage of V in the carbon steel layer is controlled to be V≦0.15%.
[0039] Cr: Mn and Cr are both carbide forming elements, and can be interchanged to ensure strength when considering hardenability. However, adding Cr can delay the pearlite transition more, shift the bainite transition region to the left, and reduce the Ms point less than Mn. However, if low carbon steel contains too many carbonitride forming elements such as Nb, Ti, and V, it will affect the subsequent phase transition, so the content of the alloying elements must be controlled to an upper limit. Elements such as Cr and Mo that improve hardenability also need to be controlled to an upper limit because the weldability will decrease when they reach a certain amount. Based on this, in the carbon steel austenitic stainless steel rolled composite plate of the present invention, the mass percentage of Cr in the carbon steel layer is controlled to Cr≦0.6%.
[0040] Mo: Mo can greatly improve hardenability. Mo significantly delays the pearlite transformation by pulling carbon into solution, but has little retarding effect on the precipitation of ferrite that precipitated before. Mo has a greater effect of lowering the Bs point than Cr, but less than Mn, so Mo's metastabilizing effect on austenite is also greater than Cr. In addition, Mo is the most important compound element that affects the formation of nano-precipitates. Mo can improve the degree of solution of Ti(C,N) into austenite, and can retain a large amount of Ti in solid solution and disperse and precipitate at low temperature transition, resulting in a higher strengthening effect.
[0041] If the low carbon steel contains too many carbonitride forming elements such as Nb, Ti, V, etc., it will affect the subsequent phase transformation, so the content of the alloying elements must be controlled to an upper limit. Elements such as Cr and Mo, which improve hardenability, also need to be controlled to an upper limit because the weldability will decrease when they reach a certain amount. Based on this, in the carbon steel austenitic stainless steel rolled composite plate of the present invention, the mass percentage of Mo in the carbon steel layer is controlled to Mo≦0.3%.
[0042] Furthermore, in the carbon steel austenitic stainless steel rolled composite plate of the present invention, the tensile strength of the carbon steel austenitic stainless steel rolled composite plate is 780-1710MPa, for example 780-1700MPa. Furthermore, the yield strength of the carbon steel austenitic stainless steel rolled composite plate of the present invention is 500-1400MPa. Furthermore, the pitting corrosion potential of the carbon steel austenitic stainless steel rolled composite plate of the present invention is 0.25-0.45V, for example 0.29-0.42V, and the intergranular corrosion is 0.25-0.40Ra. Effect of the Invention
[0043] Compared with the prior art, the manufacturing method of the carbon steel austenitic stainless steel rolled composite plate of the present invention has the following advantages and beneficial effects: The carbon steel austenitic stainless steel rolled composite plate of the present invention comprises an austenitic stainless steel layer and at the same time a high strength carbon steel layer which provides the basis for different specific mechanical properties of the whole steel plate, so that the final steel plate has various strength levels from 780 MPa to 1700 MPa and has excellent corrosion resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0044] Hereinafter, the carbon steel-austenitic stainless steel rolled composite plate and the manufacturing method thereof according to the present invention will be further explained based on specific examples, but the explanations and interpretations are not intended to unduly limit the technical solution of the present invention.
[0045] Examples 1 to 6 The carbon steel austenitic stainless steel rolled composite plates of Examples 1 to 6 are obtained by the following steps: (1) Prepare a carbon steel layer billet and an austenitic stainless steel layer billet according to the chemical compositions shown in Table 1; (2) Billet assembly; (3) Combined rolling: the billet is heated to 1150-1260°C, kept at that temperature for more than 0.6 hours, and the final rolling temperature is controlled to be above 850°C. After rolling, the billet is cooled at a rate of 30-100°C / s, and the coiling temperature is controlled to be 450-750°C; (4) Cold rolling: control the cold rolling reduction rate at 40-70%; (5) First annealing: the annealing temperature is 1050-1150°C, the holding time is more than 30 seconds, and then cooled to room temperature. In the cooling process, quenching is carried out in the temperature range of 900-500°C, and the cooling rate is controlled at 20-200°C / s; (6) Double annealing: Heat to a soaking temperature of 800-950℃ at a heating rate of 5℃ / s or more, hold for 10-100 seconds, then cool to the rapid cooling start temperature T at a rate of v1=3-20℃ / s, and the rapid cooling start temperature T≧800-10×v1, then cool to 150-450℃ at a rate of 20~1000℃ / s; then perform overaging treatment, the overaging temperature is 150~450℃, and the overaging treatment time is 100~400s.
[0046] In some other embodiments, step (7) includes planarizing. Table 1 shows the mass percentage ratio of each chemical element in the rolled composite plates of carbon steel 1 to 6 and austenitic stainless steel.
[0047] [Table 1]
[0048] Tables 2-1 and 2-2 show the specific process parameters for the carbon steel austenitic stainless steel rolled composite plates of Examples 1-6.
[0049] [Table 2-1]
[0050] [Table 2-2]
[0051] In order to verify the practical effect of the present invention and prove its superior effect in comparison with the prior art, the carbon steel austenitic stainless steel rolled composite plates of Examples 1 to 6 were tested, and the test results are shown in Table 3.
[0052] [Table 3]
[0053] From Table 3, it can be seen that the tensile strength of the carbon steel austenitic stainless steel rolled composite plate of each example of the present application is 802-1710MPa, the yield strength is 514-1390MPa, and the elongation is 7.3-15.4%. The pitting corrosion test is performed according to GB / T 17899-1999 stainless steel pitting potential measurement method, and the intergranular corrosion performance test is performed according to ASTM G108-94. From Table 3, it can be seen that the pitting corrosion potential of each example of the present application is 0.29-0.42V, and the intergranular corrosion is 0.26-0.4Ra, and each example of the present application has excellent corrosion resistance.
[0054] That is, the carbon steel-austenitic stainless steel rolled composite plate produced by the method of the present invention has an austenitic stainless steel layer that ensures corrosion resistance, and at the same time has a high-strength carbon steel layer that provides the basis for different specific mechanical properties of the entire steel plate, so that the final steel plate has various strength levels from 780 MPa to 1700 MPa and has excellent corrosion resistance.
[0055] It should be noted that the prior art within the scope of protection of the present invention is not limited to the examples described in this application, and all prior art that is not inconsistent with the solution of the present invention (including but not limited to prior patent documents, prior public publications, prior public use, etc.) is incorporated into the scope of protection of the present invention.
[0056] Furthermore, the combinations of the technical features in this application are not limited to the combinations described in the claims of this application or the combinations described in the specific examples, and all technical features described in this application can be freely combined or combined in any form, as long as they are not mutually contradictory.
[0057] It is apparent that the present invention is not limited to the above embodiments, and any similar changes or modifications that can be directly derived or easily conceived by those skilled in the art from the disclosure of the present invention are included in the scope of protection of the present invention.
Claims
1. A method for producing a carbon steel austenitic stainless steel rolled composite plate, comprising the steps of: (1) A carbon steel layer billet and an austenitic stainless steel layer billet are prepared; (2) Billet assembly; (3) A composite rolling method in which the billet is heated to 1150-1260°C, kept at that temperature for 0.6 hours or more, the final rolling temperature is controlled to 850°C or more, and after rolling, the billet is cooled at a rate of 30-100°C / s, and the coiling temperature is controlled to 450-600°C; (4) cold rolling; (5) First annealing: the annealing temperature is 1050-1150°C, the holding time is 30 seconds or more, and then cooled to room temperature. In the cooling process, quenching is performed in the temperature range of 900-500°C, and the cooling rate is controlled at 20-200°C / s; (6) double annealing: heating to a soaking temperature of 800-950 ° C. at a heating rate of 5 ° C. / s or more, holding for 10-100 seconds, then cooling to a rapid cooling start temperature T at a rate of v1 = 3-20 ° C. / s, the rapid cooling start temperature T ≧ 800-10 × v1 ° C., and then cooling to 150-450 ° C. at a rate of 20-1000 ° C. / s; then carrying out overaging treatment, the overaging temperature is 150-450 ° C., and the overaging treatment time is 100-400 s; The carbon steel layer is a base layer and the austenitic stainless steel is a coating layer, The mass percent contents of the chemical elements of the austenitic stainless steel layer billet are: C: 0.02%-0.15%, Si: 0.3%-1.0%, Mn: 1.0%-10.5%, Cr: 14.0-20.0%, Ni: 0.2-14.0%, N≦0.25%, Cu≦0.6%, Mo≦3.0%, and the balance being Fe and other inevitable impurities; 1. The method for producing the carbon steel austenitic stainless steel rolled composite plate, wherein the mass percent contents of the chemical elements of the carbon steel layer are: C: 0.05%-0.35%, Si: 0.1%-2.0%, Mn: 0.5%-3.0%, Al: 0.01%-0.08%, and at least one of the chemical elements B≦0.005%, Nb≦0.1%, Ti≦0.15%, V≦0.15%, Cr≦0.6%, Mo≦0.3%, with the balance being Fe and other unavoidable impurities.
2. The method according to claim 1, characterized in that in step (4), the cold rolling reduction is controlled to be 40-70%.
3. 2. The method of claim 1 further comprising the step (7) of planarizing.
4. 2. The method according to claim 1, wherein in step (5), the heat-holding time is 30-80 s, and the cooling rate in the temperature range of 900-500° C. is 20-180° C. / s.
5. 2. The method according to claim 1, wherein in step (6), the heating rate is 5-20° C. / s, and v1=5-20° C. / s.
6. 2. The method according to claim 1, wherein in step (3), the heat-holding time is 0.6-3 hours and the final rolling temperature is 850-920°C.
7. 2. A method according to claim 1, characterized in that the carbon steel layer is composited on one or both sides with a coating layer of austenitic stainless steel.
8. 2. The method of claim 1, wherein, upon assembly of the billet, said carbon steel layers have a thickness ratio to each austenitic stainless steel layer of 5-30:
1.
9. 2. The method of claim 1, wherein, upon assembly of the billet, said carbon steel layers have a thickness ratio of 7-10:1 to each austenitic stainless steel layer.
10. A rolled carbon steel austenitic stainless steel composite plate, comprising: The carbon steel-austenitic stainless steel rolled composite plate includes an austenitic stainless steel layer and a carbon steel layer, the carbon steel layer being a base layer and the austenitic stainless steel layer being a coating layer, the carbon steel layer being composited with the coating layer, which is made of austenitic stainless steel, on one or both sides; The mass percent contents of the chemical elements of the austenitic stainless steel layer billet are: C: 0.02%-0.15%, Si: 0.3%-1.0%, Mn: 1.0%-10.5%, Cr: 14.0-20.0%, Ni: 0.2-14.0%, N≦0.25%, Cu≦0.6%, Mo≦3.0%, and the balance being Fe and other inevitable impurities; the carbon steel layer has a mass percent content of chemical elements of: C: 0.05%-0.35%, Si: 0.1%-2.0%, Mn: 0.5%-3.0%, Al: 0.01%-0.08%, and at least one of the following chemical elements: B≦0.005%, Nb≦0.1%, Ti≦0.15%, V≦0.15%, Cr≦0.6%, Mo≦0.3%, with the balance being Fe and other inevitable impurities; The carbon steel-austenitic stainless steel rolled composite plate has a tensile strength of 780 to 1700 MPa.
11. The carbon steel-austenitic stainless steel rolled composite plate according to claim 10, characterized in that the yield strength of said carbon steel-austenitic stainless steel rolled composite plate is 500-1400 MPa, the pitting potential is 0.25-0.45 V, and the intergranular corrosion is 0.25-0.40 Ra.
Citation Information
Patent Citations
Method for quenching stainless clad steel plate
JP1989136931A
Production of stainless steel clad steel plate
JP1993255758A
Multilayer steel, and method for producing the same
JP2009235492A
Multilayer steel and method for producing multilayer steel
WO2008013233A1
Clad steel plate
WO2019132039A1