Non-oriented electrical steel sheet and its manufacturing method
A non-oriented electrical steel sheet with optimized alloy composition and texture improves magnetic properties and productivity, addressing brittleness and cold rolling limitations, enhancing motor efficiency.
Patent Information
- Application Number
- JP2022537548
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-20
- Filing Date
- 2020-12-09
- Publication Date
- 2024-11-14
- Estimated Expiration
- 2040-12-09
AI Technical Summary
Existing non-oriented electrical steel sheets face challenges in achieving high magnetic properties, particularly at low magnetic fields and high frequencies, due to issues with brittleness, cold rolling limitations, and increased iron loss, which affect the efficiency and productivity of motors, especially in electric vehicle drive motors.
A non-oriented electrical steel sheet composition comprising specific amounts of Si, Al, Mn, Sn, P, Ga, Bi, and other elements, along with controlled textures and an oxidized layer, optimized for improved magnetism and texture through hot and cold rolling processes.
The solution results in a steel sheet with enhanced magnetic properties, reduced iron loss, and improved productivity, contributing to more efficient drive motors for electric vehicles.
Smart Images

Figure 0007583813000009 
Figure 0007583813000001 
Figure 0007583813000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a non-oriented electrical steel sheet and a manufacturing method thereof, and more particularly to a non-oriented electrical steel sheet having improved magnetic properties by appropriately adding Sn, P, Ga, and Bi to improve the texture, and a manufacturing method thereof. [Background technology]
[0002] Non-oriented electrical steel sheets are mainly used in motors that convert electrical energy into mechanical energy, and therefore excellent magnetic properties are required for non-oriented electrical steel sheets to achieve high efficiency during their use. In particular, as environmentally friendly technologies have been attracting attention in recent years, it has become increasingly important to improve the efficiency of motors, which account for more than half of the total electrical energy consumption, and as a result, the demand for non-oriented electrical steel sheets with excellent magnetic properties is also increasing. The magnetic properties of non-oriented electrical steel sheets are mainly evaluated by iron loss and magnetic flux density. Iron loss refers to the energy loss that occurs at a specific magnetic flux density and frequency, and magnetic flux density refers to the degree of magnetization obtained under a specific magnetic field. The lower the iron loss, the more energy-efficient a motor can be manufactured under the same conditions, and the higher the magnetic flux density, the more compact the motor can be and the less copper loss can be. Therefore, it is important to manufacture non-oriented electrical steel sheets with low iron loss and high magnetic flux density.
[0003] The characteristics of non-oriented electrical steel sheets that should be considered also change depending on the operating conditions of the motor. When evaluating the characteristics of non-oriented electrical steel sheets used in motors, many motors consider W15 / 50, which is the iron loss when a 1.5T magnetic field is applied at a commercial frequency of 50Hz, to be the most important. However, not all motors for various applications consider W15 / 50 iron loss to be the most important, and iron loss at other frequencies or applied magnetic fields may be evaluated depending on the main operating conditions. In particular, for non-oriented electrical steel sheets used in the drive motors of recent electric vehicles, magnetic properties are often important at low magnetic fields of 1.0T or less and high frequencies of 400Hz or more, so the characteristics of non-oriented electrical steel sheets are evaluated at iron loss such as W10 / 400. The most commonly used method to increase the magnetic properties of non-oriented electrical steel sheets is to add alloying elements such as Si. The resistivity of the steel can be increased by adding such alloying elements, and the higher the resistivity, the lower the overall iron loss as the eddy current loss decreases. On the other hand, the more Si is added, the lower the magnetic flux density becomes and the more brittle the steel becomes. If more than a certain amount is added, cold rolling becomes impossible and commercial production becomes impossible. In particular, the thinner the electrical steel sheet is made, the lower the iron loss becomes, but the lower rollability due to brittleness becomes a fatal problem. The highest quality non-oriented electrical steel sheets with excellent magnetic properties can be produced by adding elements such as Al and Mn to further increase the resistivity of the steel.
[0004] For non-oriented electrical steel sheets used in electric vehicle drive motors, the iron loss at high frequencies of 400 Hz or more is important, but as the frequency increases, the ratio of eddy current loss to iron loss increases, so it is advantageous to increase resistivity and reduce thickness. However, as the thickness of the steel sheet becomes thinner, the cold reduction rate increases, which causes the {111} / / ND texture to develop and leads to poor magnetic properties. If the hot-rolled sheet thickness is reduced to reduce the cold reduction rate in order to improve this, the shape of the steel sheet cannot be fully controlled during the cold rolling process, and the thickness deviation in the width direction increases, resulting in defective motor core sizes. In addition, as the steel sheet becomes thinner, the length of the coil increases, which increases the working time of the continuous annealing process, causing a problem of reduced annealing productivity. In order to solve the above problems, various attempts have been made, such as thoroughly removing impurities in the steelmaking process to produce extremely clean steel, and adding specific elements to reduce inclusions and precipitates in the steel to improve magnetic properties, but these methods are limited in their practical application due to limitations in commercial production conditions. In addition, methods have been proposed to improve the texture by controlling the annealing temperature and atmosphere, and the deformation rate of the steel sheet during rolling, but the technologies that are actually used are extremely limited due to reasons such as increased manufacturing costs, reduced productivity, and limited effectiveness. Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a non-oriented electrical steel sheet and a manufacturing method thereof. More specifically, the present invention provides a non-oriented electrical steel sheet and a manufacturing method thereof in which Sn, P, Ga, and Bi are appropriately added to improve the texture, thereby improving the magnetic properties. [Means for solving the problem]
[0006] The non-oriented electrical steel sheet of the present invention is characterized in that it contains, by weight, 1.5-4.0% Si, 0.1-1.5% Al, 0.05-1.5% Mn, 0.015-0.1% Sn, 0.005-0.05% P, 0.001-0.004% Ga, 0.0005-0.003% Bi, with the balance being Fe and unavoidable impurities, and has a higher fraction of {118} / / ND orientation texture than the fraction of {111} / / ND orientation texture.
[0007] The non-oriented electrical steel sheet of the present invention further contains 0.005 to 0.03 wt % of Cr and can satisfy the following formula 1. [Formula 1] 0.005≦[Cr]≦0.03×[Al] (In formula 1, [Cr] and [Al] represent the Cr and Al contents (wt%) in the steel plate, respectively.)
[0008] The non-oriented electrical steel sheet of the present invention further contains 0.001 to 0.01% by weight of Mo and 0.005 to 0.04% by weight of Ni, and can satisfy the following formula 2. [Formula 2] 10×[Mo]≦([Sn]+[P])≦4×[Ni] (In formula 2, [Mo], [Sn], [P] and [Ni] respectively represent the contents (weight%) of Mo, Sn, P and Ni in the steel plate.)
[0009] The non-oriented electrical steel sheet of the present invention further contains Cu: 0.001 to 0.05% by weight, S: 0.005% by weight or less, and Ti: 0.005% by weight or less, and can satisfy the following formula 3. [Formula 3] 0.5≦[Cu] / ([Ti]+[S])≦7.5 (In formula 3, [Cu], [Ti] and [S] respectively represent the contents (wt%) of Cu, Ti and S in the steel plate.)
[0010] The non-oriented electrical steel sheet of the present invention may further contain C: 0.005% by weight or less and N: 0.005% by weight or less. It is preferable that an oxide layer is present from the surface toward the inside of the electrical steel sheet, and the thickness of the oxide layer is 10 to 50 nm. The oxide layer preferably consists of 40 to 70% by weight of O, 25 to 55% by weight of Al, 0.01 to 0.1% by weight of P, 0.01 to 0.1% by weight of Sn, with the remainder being Fe and unavoidable impurities.
[0011] The non-oriented electrical steel sheet of the present invention preferably has an average crystal grain size of 50 to 100 μm. Among the sulfides formed inside the base material, the number of sulfides having a diameter of 100 nm or more can be three times or more the number of sulfides having a diameter of less than 100 nm. The thickness is preferably 0.10 to 0.30 mm. The thickness of the steel plate at the center in the width direction (t center ) and the thickness (t 500 ) is preferably 10 μm or less.
[0012] The method for producing a non-oriented electrical steel sheet of the present invention is characterized by including a step of producing a hot-rolled sheet by hot rolling a slab consisting of, by weight, 1.5-4.0% Si, 0.1-1.5% Al, 0.05-1.5% Mn, 0.015-0.1% Sn, 0.005-0.05% P, 0.001-0.004% Ga, 0.0005-0.003% Bi, with the balance being Fe and unavoidable impurities, a step of producing a cold-rolled sheet by cold-rolling the hot-rolled sheet at a reduction ratio of 85% or more, and a step of final annealing the cold-rolled sheet.
[0013] After the step of producing the hot-rolled sheet, the method may further include a step of annealing the hot-rolled sheet at a temperature of 850 to 1150°C. The final annealing step is preferably performed in an atmosphere containing hydrogen (H2) and nitrogen (N2) at a temperature in the range of 400 to 1000° C. for 100 seconds or less. Effect of the Invention
[0014] According to one embodiment of the present invention, by specifying the optimal alloy composition of a non-oriented electrical steel sheet, it is possible to manufacture a non-oriented electrical steel sheet that has little thickness deviation in the width direction of the steel sheet and is excellent in magnetic properties, shape, and productivity. Furthermore, according to one embodiment of the present invention, by supplying a non-oriented electrical steel sheet with excellent magnetic properties, it is possible to contribute to improving the efficiency of drive motors for electric vehicles. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a schematic diagram of a cross section of a non-oriented electrical steel sheet according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Terms such as first, second and third are used to describe various parts, components, regions, layers and / or sections, but are not limited thereto. These terms are used only to distinguish one part, component, region, layer or section from another part, component, region, layer or section. Thus, a first part, component, region, layer or section described below may be referred to as a second part, component, region, layer or section without departing from the scope of the present invention. The terminology used herein is merely for the purpose of referring to particular embodiments and is not intended to limit the present invention. As used herein, the singular form includes the plural form unless the text clearly indicates otherwise. The meaning of "comprising" as used in the specification embodies certain features, regions, integers, steps, operations, elements and / or components and does not exclude the presence or addition of other features, regions, integers, steps, operations, elements and / or components.
[0017] When an element is referred to as being "on" another element, it means that it is immediately on top of the other element, or there may be other elements between them. In contrast, when an element is referred to as being "directly on" another element, there are no other elements between them. Moreover, unless otherwise specified, % means % by weight, and 1 ppm is 0.0001% by weight. In an embodiment of the present invention, the term "additionally contain an additional element" means that the additional element is included in place of the remaining iron (Fe) by an amount corresponding to the additional element.
[0018] Unless otherwise defined, all terms, including technical and scientific terms, used herein have the same meaning as commonly understood by a person of ordinary skill in the art to which the present invention belongs. Terms defined in commonly used dictionaries are additionally interpreted to have a meaning consistent with the relevant technical literature and the presently disclosed content, and are not interpreted in an ideal or very formal sense unless defined. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will now be described in detail with reference to exemplary embodiments thereof, so that those skilled in the art will be able to easily practice the present invention. However, the present invention may be embodied in many different forms and is not limited to the embodiments set forth herein.
[0019] The non-oriented electrical steel sheet according to one embodiment of the present invention contains, by weight, 1.5-4.0% Si, 0.1-1.5% Al, 0.05-1.5% Mn, 0.015-0.1% Sn, 0.005-0.05% P, 0.001-0.004% Ga, 0.0005-0.003% Bi, and the remainder being Fe and unavoidable impurities. The reasons for limiting the components of the non-oriented electrical steel sheet will be explained below.
[0020] Si:1.5~4.0wt% Silicon (Si) plays a role in increasing the resistivity of the material and reducing iron loss. If too little Si is added, the iron loss improvement effect may be insufficient. If too much Si is added, the brittleness of the material increases, the rolling productivity drops sharply, and a surface oxide layer and oxides that are harmful to magnetism may form. Therefore, it is preferable to contain 1.5 to 4.0% by weight of Si. More specifically, it is preferable to contain 2.0 to 3.9% by weight. It is even more preferable to contain 3.2 to 3.7% by weight.
[0021] Al: 0.1~1.5% by weight Aluminum (Al) plays a role in increasing the resistivity of the material and reducing iron loss. If too little Al is added, fine nitrides are formed or the surface oxide layer is not densely formed, making it difficult to obtain the magnetic improvement effect. On the other hand, if too much Al is added, excessive nitrides are formed, deteriorating the magnetic property, causing problems in all processes such as steelmaking and continuous casting, and greatly reducing productivity. Therefore, it is preferable that Al is contained in an amount of 0.1 to 1.5 wt %. More preferably, it is contained in an amount of 0.3 to 1.0 wt %.
[0022] Mn:0.05~1.50wt% Manganese (Mn) increases the resistivity of the material, improves core loss, and plays a role in forming sulfides. If too little Mn is added, minute sulfides are formed, causing magnetic deterioration, and if too much Mn is added, fine MnS is excessively precipitated, promoting the formation of {111} texture, which is unfavorable to magnetism, and causing a rapid decrease in magnetic flux density. Therefore, it is preferable to contain 0.05 to 1.50 wt% Mn. More preferably, it is contained 0.1 to 1.0 wt% Mn.
[0023] Sn:0.015~0.100wt% Tin (Sn) segregates on the surface and grain boundaries of the steel sheet to suppress surface oxidation during annealing, hinder the diffusion of elements through grain boundaries, and hinder recrystallization in the {111} / / ND orientation to improve the texture. If too little Sn is added, the above effects may not be sufficient. If too much Sn is added, the amount of segregation at the grain boundaries increases, which may reduce toughness and reduce productivity compared to magnetic improvement. Therefore, it is preferable to contain 0.015 to 0.100 wt% Sn. More preferably, it is preferable to contain 0.020 to 0.075 wt% Sn.
[0024] P:0.005~0.050wt% Phosphorus (P) segregates on the surface and grain boundaries of the steel sheet to suppress surface oxidation during annealing, hinder the diffusion of elements through grain boundaries, and hinder recrystallization in the {111} / / ND orientation to improve the texture. If too little P is added, the effect may not be fully exerted. If too much P is added, there is a risk that the hot working characteristics will deteriorate and productivity will decrease compared to magnetic improvement. Therefore, it is preferable that P is contained in a range of 0.005 to 0.050% by weight. More preferably, P is contained in a range of 0.007 to 0.045% by weight.
[0025] Ga:0.001~0.004wt% Gallium (Ga) does not segregate strongly on the surface and grain boundaries, but when added in small amounts, it can promote the segregation of Sn and P, maximizing the effect of improving the texture during recrystallization annealing, and increasing the softness of the steel, making it easier to control the shape of the steel sheet. If Ga is added in an excessively small amount, the effect may not be sufficient. If Ga is added in an excessively large amount, there is a risk of defects being caused on the surface of the steel sheet, which may deteriorate the magnetic property. Therefore, Ga should be contained in an amount of 0.001 to 0.0040 wt %. More preferably, Ga should be contained in an amount of 0.0015 to 0.0035 wt %.
[0026] Bi: 0.0005 to 0.003% Bismuth (Bi) promotes the segregation of Sn and P at grain boundaries and crystal grain boundaries, and plays a role in reducing the deformation resistance during rolling. If too little Bi is added, the effect may be insufficient. If too much Bi is added, there is a risk that the magnetic properties may be deteriorated. Therefore, it is preferable that Bi is contained in an amount of 0.0005 to 0.0030% by weight. It is more preferable that Ga is contained in an amount of 0.0010 to 0.0030% by weight. The non-oriented electrical steel sheet according to one embodiment of the present invention further contains 0.005 to 0.03 wt % of Cr.
[0027] Cr:0.005~0.03wt% Chromium (Cr) does not have a strong tendency to form fine precipitates, but it can impede the formation of an Al-based oxide layer on the surface and form Cr-based carbides, which can deteriorate magnetic properties. If too little Cr is added, the Al-based oxide layer can be formed too thick, or round-shaped oxides or nitrides can be formed on the surface, which can deteriorate magnetic properties. If too much Cr is added, it is difficult to form a dense oxide layer, which can deteriorate magnetic properties. Therefore, if Cr is further added, it is preferable to include 0.005 to 0.03 wt %. More specifically, Cr can satisfy the following formula 1. [Formula 1] 0.005≦[Cr]≦0.03×[Al] (In formula 1, [Cr] and [Al] represent the Cr and Al contents (wt%) in the steel plate, respectively.) By adjusting the upper limit of Cr in conjunction with Al, a dense oxide layer can be formed. The non-oriented electrical steel sheet according to one embodiment of the present invention may further contain Mo: 0.001 to 0.01% by weight and Ni: 0.005 to 0.04% by weight.
[0028] Mo:0.001~0.01wt% Molybdenum (Mo) segregates on the surface and grain boundaries to improve the texture. If too little Mo is added, the {111} texture may develop and magnetic properties may deteriorate. If too much Mo is added, the segregation of Sn and P may be suppressed, and the texture improving effect may decrease. Therefore, if Mo is further added, it is recommended that it be contained in an amount of 0.001 to 0.01 wt %.
[0029] Ni: 0.005~0.04% by weight Nickel (Ni) increases the softness of steel and promotes the segregation of Sn and P. If too much Ni is added, the magnetic flux density may drop sharply. Therefore, if Ni is further added, it is recommended that it be contained at 0.005 to 0.04 wt%. More specifically, Ni and Mo can satisfy the following formula 2. [Formula 2] 10×[Mo]≦([Sn]+[P])≦4×[Ni] (In formula 2, [Mo], [Sn], [P] and [Ni] respectively represent the contents (weight%) of Mo, Sn, P and Ni in the steel plate.) As shown in formula 2, by adjusting the amounts of Mo and Ni added depending on the contents of Sn and P, the effect of improving the texture due to the grain boundary segregation of Sn and P can be maximized. A non-oriented electrical steel sheet according to one embodiment of the present invention further contains Cu: 0.001 to 0.05% by weight, S: 0.005% by weight or less, and Ti: 0.005% by weight or less, and can satisfy the following formula 3.
[0030] Cu:0.001~0.05wt% Copper (Cu) is an element that can form sulfides at high temperatures, and when added in large amounts, it can cause surface defects during slab manufacturing. When added in an appropriate amount, it has the effect of coarsening fine CuS or MnCuS precipitates and improving magnetic properties. Therefore, when Cu is included, it is recommended that it be included in an amount of 0.001 to 0.05% by weight.
[0031] S: 0.005% by weight or less Sulfur (S) forms fine precipitates such as MnS, CuS, and (Mn, Cu)S, which deteriorate the magnetic properties and the hot workability, so it is better to keep the amount low. Therefore, when S is further contained, it is better to contain 0.005 wt% or less. More preferably, it is better to contain 0.0001 to 0.005 wt%. Even more preferably, it is better to contain 0.0005 to 0.0035 wt%.
[0032] Ti: 0.005% by weight or less Ti has a strong tendency to form precipitates in steel, forming fine carbides, nitrides, or sulfides inside the base material, which inhibits grain growth and deteriorates iron loss. Therefore, the Ti content must be controlled to 0.004% or less, and more preferably 0.002% or less. Cu, Ti, and S can satisfy the following formula 3. [Formula 3] 0.5≦[Cu] / ([Ti]+[S])≦7.5 (In formula 3, [Cu], [Ti] and [S] respectively represent the contents (wt%) of Cu, Ti and S in the steel plate.) By adjusting the amounts of Cu, Ti, and S added as shown in Equation 3, the ratio of coarse sulfides to fine sulfides can be increased, thereby improving high frequency iron loss. The non-oriented electrical steel sheet according to an embodiment of the present invention may further include C: 0.005% by weight or less and N: 0.005% by weight or less.
[0033] C: 0.005% by weight or less Carbon (C) causes magnetic aging and combines with other impurity elements to form carbides that degrade the magnetic properties, so the less carbon there is the better, 0.005% or less, and more preferably 0.003% or less by weight.
[0034] N: 0.005% by weight or less Nitrogen (N) not only forms fine AlN precipitates inside the base material, but also combines with other impurities to form fine precipitates that inhibit grain growth and worsen iron loss, so the lower the N content, the better, 0.005% by weight or less, and more preferably 0.003% by weight or less.
[0035] The balance is composed of Fe and inevitable impurities. The inevitable impurities are impurities that are mixed in during the steelmaking stage and the manufacturing process of the grain-oriented electrical steel sheet, and are widely known in the art, so a detailed description will be omitted. The addition of elements other than the above alloy components shown in one embodiment of the present invention is not excluded, and may be included in various ways within a range that does not harm the technical idea of the present invention. When an additional element is further included, it is included in place of the balance Fe. The unavoidable impurities include, for example, B, Mg, Zr, etc., and must be controlled to B: 0.002 wt % or less, Mg: 0.005 wt % or less, and Zr: 0.005 wt % or less.
[0036] Fig. 1 shows a cross section of a non-oriented electrical steel sheet according to an embodiment of the present invention. As shown in Fig. 1, an oxide layer 20 is present from the surface to the inside of an electrical steel sheet 100. The electrical steel sheet 100 excluding the oxide layer 20 is classified as an electrical steel sheet base material 10. The electrical steel sheet 100 is exposed to oxygen during the manufacturing process, and oxygen in the atmosphere penetrates into the steel sheet, resulting in an oxygen concentration gradient from the surface to the inside. The oxide layer 20 and the base material 10 can be divided into an oxide layer 20 having an oxygen content of 40% by weight or more and a base material 10 having an oxygen content of less than 40% by weight. The thickness of the oxide layer 20 divided in this way is 10 to 50 nm. By forming an oxide layer 20 of an appropriate thickness, the diffusion of nitrogen in the atmosphere into the base material during annealing is suppressed, thereby suppressing the formation of fine nitrides, thereby improving magnetic properties. The thickness of the oxide layer 20 varies over the entire surface of the steel sheet, and in one embodiment of the present invention, the thickness of the oxide layer 20 means the average thickness within the steel sheet.
[0037] The oxide layer 20 contains a large amount of Al, Sn, and P that are diffused and concentrated in the base material 10, in addition to oxygen that is present due to oxygen penetration during the manufacturing process. Specifically, the oxide layer 20 contains 40-70% by weight of O, 25-55% by weight of Al, 0.01-0.1% by weight of P, and 0.01-0.1% by weight of Sn, with the remainder being Fe and unavoidable impurities. The formation of the oxide layer in which Al, P, and Sn are concentrated in this way can suppress the formation of round-shaped oxides and fine nitrides inside the base material, thereby improving magnetic properties. In the case of P and Sn, which are similar to O, a concentration gradient exists from the base material toward the surface. The above component ranges refer to the average contents in the oxide layer 20. In one embodiment of the present invention, the area fraction of the {118} / / ND orientation texture may be higher than the area fraction of the {111} / / ND orientation texture. The {118} / / ND orientation texture refers to a texture in which the {118} plane is parallel to the rolled surface (ND surface) of the steel sheet within 5°. The {111} / / ND orientation texture refers to a texture in which the {111} plane is parallel to the rolled surface (ND surface) of the steel sheet within 5°. The area fraction can be measured based on a plane parallel to the rolled surface (ND surface) and can be measured within the base material 10.
[0038] Generally, the higher the cold rolling reduction, the more the texture of the {111} / / ND orientation, which is detrimental to magnetic properties, increases and the texture of the {118} / / ND orientation decreases, resulting in deterioration of magnetic properties. However, in the present invention, even with a high cold rolling reduction of 85% or more, the area fraction of the texture of the {118} / / ND orientation is higher than the area fraction of the texture of the {111} / / ND orientation, resulting in improved magnetic properties. Specifically, the area fraction of the {118} / / ND orientation texture is 11-15%, and the area fraction of the {111} / / ND orientation texture is 5-10%. The non-oriented electrical steel sheet according to one embodiment of the present invention has an average crystal grain size of 50-100 μm. Within the above range, the magnetic properties of the non-oriented electrical steel sheet are even more excellent. The crystal grain size is [(measurement area ÷ number of crystal grains) 0.5 The grain size can be measured based on a plane parallel to the rolled surface (ND surface), and can be measured within the base material 10. Specifically, the average grain size is 60 to 90 μm.
[0039] In one embodiment of the present invention, by appropriately controlling the alloy components, the number of sulfides with a diameter of 100 nm or more among the sulfides formed inside the base material can be three times or more the number of sulfides with a diameter of less than 100 nm. Specifically, it can be 3.3 to 5.0 times. By forming a large number of coarse sulfides in this way, fine precipitates that hinder domain wall motion can be suppressed, contributing to improved magnetic properties. The thickness of the steel plate is 0.10 to 0.30 mm. With an appropriate thickness, the magnetic property can be improved.
[0040] The thickness of the steel plate at the center in the width direction (t center ) and the thickness (t 500 ) can be 10 μm or less. This is because the reduction ratio in cold rolling is set high, as will be explained in the manufacturing process below, and this can contribute to improving the shape quality and yield of motor cores manufactured from the non-oriented electrical steel sheet. As described above, the present invention provides an optimal alloy composition and improves the texture, thereby improving the magnetic properties. Specifically, the iron loss (W10 / 400) of the non-oriented electrical steel sheet can be 10.5 W / kg or less, and the magnetic flux density (B50) can be 1.65 T or more. The iron loss (W10 / 400) is the iron loss when a magnetic flux density of 1.0 T is induced at a frequency of 400 Hz. The magnetic flux density (B50) is the magnetic flux density induced in a magnetic field of 5000 A / m. More specifically, the iron loss (W10 / 400) of the non-oriented electrical steel sheet can be 10.0 W / kg or less, and the magnetic flux density (B50) can be 1.66 T or more.
[0041] A method for producing a non-oriented electrical steel sheet according to an embodiment of the present invention includes the steps of hot rolling a slab to produce a hot-rolled sheet, cold rolling the hot-rolled sheet to produce a cold-rolled sheet, and final annealing the cold-rolled sheet. First, the slab is heated. The alloy composition of the slab has been described above in relation to the alloy composition of the non-oriented electrical steel sheet, so a duplicated description will be omitted. Since the alloy composition does not substantially change during the manufacturing process of the non-oriented electrical steel sheet, the alloy composition of the non-oriented electrical steel sheet and the slab are substantially the same.
[0042] Specifically, the slab contains, by weight, 1.5-4.0% Si, 0.1-1.5% Al, 0.05-1.5% Mn, 0.015-0.1% Sn, 0.005-0.05% P, 0.001-0.004% Ga, 0.0005-0.003% Bi, and the remainder is Fe and unavoidable impurities. Other additional elements have been explained in the alloy components of the non-oriented electrical steel sheet, so duplicate explanations will be omitted.
[0043] The slab may be heated before hot rolling. There is no restriction on the heating temperature of the slab, but the slab may be heated to 1200°C or less. If the slab heating temperature is excessively high, precipitates such as AlN and MnS present in the slab may be redissolved and then finely precipitated during hot rolling and annealing, suppressing grain growth and reducing magnetic properties. Next, the slab is hot rolled to produce a hot rolled sheet. The thickness of the hot rolled sheet is 2 to 2.3 mm. In the stage of producing the hot rolled sheet, the finish rolling temperature is 800°C or higher, specifically 800 to 1000°C. The hot rolled sheet is coiled at a temperature of 700°C or lower.
[0044] After the step of producing the hot-rolled sheet, the method further includes a step of annealing the hot-rolled sheet. At this time, the annealing temperature of the hot-rolled sheet is 850 to 1150°C. If the annealing temperature of the hot-rolled sheet is too low, the structure does not grow or grows finely, making it difficult to obtain a texture favorable for magnetic properties during annealing after cold rolling. If the annealing temperature is too high, the magnetic crystal grains grow excessively, and the sheet may have excessive surface defects. The hot-rolled sheet annealing is performed to increase the orientation favorable for magnetic properties as necessary, and may be omitted. The annealed hot-rolled sheet may be pickled. Next, the hot rolled sheet is cold rolled to produce a cold rolled sheet. The cold rolling is final rolling to a thickness of 0.1 mm to 0.3 mm. The reduction ratio in the cold rolling stage can be adjusted to 85% or more. More specifically, the reduction ratio is 85% to 95%. If the reduction ratio is too low, there is a risk of thickness differences occurring in the width direction of the steel sheet.
[0045] Next, the cold-rolled sheet is subjected to final annealing. The annealing temperature in the process of annealing the cold-rolled sheet is not significantly limited as long as it is a temperature normally applied to non-oriented electrical steel sheets. Since the core loss of non-oriented electrical steel sheets is closely related to the grain size, a temperature of 400 to 1000°C is appropriate. In addition, the annealing time can be as short as 100 seconds or less. The annealing atmosphere may contain hydrogen (H2) and nitrogen (N2). Specifically, the annealing is performed in an atmosphere containing 5 to 50 volume % of hydrogen and 95 to 50 volume % of nitrogen.
[0046] During the final annealing process, the average grain size can be 50~100μm, and the processed structure formed during the previous cold rolling step is completely (99% or more) recrystallized. After the final annealing, an insulating coating can be formed, which can be made of organic, inorganic, or organic-inorganic composite coatings, or other insulating coating materials. Hereinafter, the present invention will be described in more detail with reference to the following embodiments. However, these embodiments are merely for the purpose of illustrating the present invention, and the present invention is not limited thereto.
[0047] Example 1 A slab was produced with the components shown in Tables 1 and 2, Cu: 200 ppm, the remainder being Fe and unavoidable impurities. This was heated at 1150°C and hot rolled at a finishing temperature of 830°C to produce a hot rolled sheet with a thickness of 2.3 mm. The hot rolled sheet was annealed at 1030°C for 100 seconds, then cold rolled to the thickness shown in Table 3, and recrystallization annealed at 950°C for 88 seconds. The thickness of the oxide layer for each specimen, whether or not Relational Formulas 1 and 2 are satisfied, whether or not the oxide layer contains Al, P, or Sn, the average crystal grain diameter, the area fraction of {118} / / ND and {111} / / ND orientations, the W10 / 400 core loss, and the B50 magnetic flux density are shown in Tables 3 and 4.
[0048] The thickness of the oxide layer was determined by processing the specimen with FIB to produce a smooth cross section, photographing this with a high magnification TEM, and measuring the thickness of the oxide layer at more than 10 points on the surface of the base material, and averaging this. The TEM-EDS measurement function was then used to area analyze the chemical composition of the oxide layer on the surface of the base material, and if Al, P, or Sn was detected at 0.5% by weight or more at the same time, it was determined that the oxide layer contained the relevant elements. The grain size was determined by polishing and etching the cross section of the specimen perpendicular to the rolling direction (TD direction), photographing an area sufficient to contain more than 1,500 grains with an optical microscope, and calculating the average value of [(measured area ÷ number of grains)]. 0.5 〕 was calculated. The texture was measured by EBSD in the normal direction (ND direction) of the rolling surface of the specimen, and the measurement area of each specimen was 100 mm 2 In the above, a step size of 2 μm was applied, V118 is the fraction of the measurement area where the ND plane is parallel to the {118} plane in the entire measurement area, V111 is the fraction of the measurement area where the ND plane is parallel to the {111} plane in the entire measurement area, and the error angle was always 5°.
[0049] Magnetic properties such as magnetic flux density and core loss were measured by cutting 5 pieces of 60mm wide x 60mm long for each specimen, measuring the rolling direction and the vertical direction with a single sheet tester, and showing the average value. At this time, W10 / 400 is the core loss when a magnetic flux density of 1.0T is induced at a frequency of 400Hz, and B50 means the magnetic flux density induced in a magnetic field of 5000A / m.
[0050] [Table 1]
[0051] [Table 2]
[0052] [Table 3]
[0053] [Table 4]
[0054] As shown in Tables 1 to 4, it can be confirmed that A3, A4, B3, B4, C3, C4, D3, D4, E3, E4, and F4, in which the alloy components and texture are appropriately controlled, have excellent magnetic properties. On the other hand, it can be seen that A1, A2, B1, B2, C1, C2, D1, D2, E1, E2, F1, F2, and F3, in which the alloy components or texture are not appropriately controlled, have inferior magnetic properties. Also, in the cases of A3, A4, B3, B4, C3, C4, D3, D4, E3, E4, and F4, the oxide layer is of an appropriate thickness and the Al, P, and Sn in the oxide layer are appropriately concentrated, resulting in excellent magnetic properties. On the other hand, in the cases of A1, A2, B1, B2, C1, C2, D1, D2, E1, E2, F1, F2, and F3, the oxide layer is not of an appropriate thickness or the Al, P, and Sn in the oxide layer are not appropriately concentrated, resulting in inferior magnetic properties.
[0055] Example 2 Slabs were produced from the alloy compositions shown in Tables 5 and 6, plus 20 ppm C, 20 ppm N, 200 ppm Cr, 20 ppm Mo, with the balance being Fe and unavoidable impurities. These were reheated at 1170°C, hot rolled at a finishing temperature of 860°C, and rolled at the cold reduction shown in Table 7 to produce hot-rolled sheets of various thicknesses. The hot-rolled sheets were annealed at 1020°C for 80 seconds, and then cold rolled to produce the thicknesses shown in Table 7. These were then subjected to final recrystallization annealing at a maximum temperature of 960°C for the time shown in Table 7 to produce coils having a width of 1100 mm.
[0056] The cold reduction ratio, final annealing time, whether or not Relational Formula 3 was satisfied, crystal grain size, number ratio of coarse sulfides and fine sulfides, thickness deviation in the width direction, W10 / 400 iron loss, and B50 magnetic flux density for each specimen are shown in Tables 7 and 8. The cold reduction ratio was calculated using the formula [(hot-rolled sheet thickness - cold-rolled sheet thickness) / hot-rolled sheet thickness]. The final annealing time refers to the time during annealing in a continuous annealing furnace during which the atmospheric temperature passes through a section of 400°C or higher. The number ratio of coarse sulfides and fine sulfides was determined by preparing specimens using the TEM replica method and measuring the number of 2500μm 2 The diameter and number of all sulfides in the above area are measured, and the number of sulfides with a diameter of 100 nm or more is divided by the number of sulfides with a diameter of less than 100 nm. center -t 500 The magnetic properties were measured using a single sheet tester in the same manner as in Example 1.
[0057] [Table 5]
[0058] [Table 6]
[0059] [Table 7]
[0060] [Table 8]
[0061] The component contents, microstructural characteristics, and manufacturing methods of specimens A11, A12, B11, B12, C11, and C12 all satisfied the ranges of the present invention, and the grain size, sulfide size, thickness deviation in the width direction, and magnetic properties all showed excellent values. On the other hand, in the cases of A5~8, B5~8, and C5~8, the rolling reduction was insufficient, resulting in excessive thickness deviation in the width direction. In the cases of A9 and C10, the Ga and Bi contents were low, so although the rolling reduction was sufficiently high, the thickness deviation was severe and the sheet shape was poor. In A6, A10, C5, and C9, the Cu content was outside the range of the present invention, so the sulfides were not sufficiently coarsened, the crystal grain size was small, and the magnetic properties were not good. In B5, B6, B9, and B10, the Ga or Bi content was too high, which caused excessive segregation, resulting in surface defects, fine sulfides, and poor grain growth, resulting in poor magnetic properties.
[0062] The present invention is not limited to the above-described embodiment, but can be manufactured in various different forms, and a person having ordinary skill in the art to which the present invention pertains should understand that the present invention can be embodied in other specific forms without changing the technical concept or essential features of the present invention. Therefore, it should be understood that the above-described embodiment is illustrative in all respects and is not limiting.
Claims
1. In weight percent, Si: 1.5-4.0%, Al: 0.1-1.5%, Mn: 0.05-1.5%, Sn: 0.015-0.1%, P: 0.005-0.05%, Ga: 0.001-0.004%, Bi: 0.0005-0.003%, and the balance being Fe and unavoidable impurities. A non-oriented electrical steel sheet, characterized in that the area fraction of a {118} / / ND orientation texture is 11 to 15% and is higher than the area fraction of a {111} / / ND orientation texture.
2. Cr: 0.005 to 0.03 wt %; 2. The non-oriented electrical steel sheet according to claim 1, which satisfies the following formula 1: [Formula 1] 0.005≦[Cr]≦0.03×[Al] (In formula 1, [Cr] and [Al] represent the Cr and Al contents (wt%) in the steel plate, respectively.)
3. Further comprising Mo: 0.001 to 0.01 wt % and Ni: 0.005 to 0.04 wt %; The non-oriented electrical steel sheet according to claim 1 or 2, which satisfies the following formula 2: [Formula 2] 10×[Mo]≦([Sn]+[P])≦4×[Ni] (In formula 2, [Mo], [Sn], [P] and [Ni] respectively represent the contents (wt%) of Mo, Sn, P and Ni in the steel plate.)
4. Further comprising Cu: 0.001 to 0.05 wt %, S: 0.005 wt % or less, and Ti: 0.005 wt % or less; The non-oriented electrical steel sheet according to any one of claims 1 to 3, which satisfies the following formula 3: [Formula 3] 0.5≦[Cu] / ([Ti]+[S])≦7.5 (In formula 3, [Cu], [Ti] and [S] respectively represent the contents (wt%) of Cu, Ti and S in the steel plate.)
5. The non-oriented electrical steel sheet according to any one of claims 1 to 4, further comprising C: 0.005% by weight or less and N: 0.005% by weight or less.
6. 6. The non-oriented electrical steel sheet according to claim 1, characterized in that an oxide layer is present from the surface of the electrical steel sheet toward the inside, and the thickness of the oxide layer is 10 to 50 nm.
7. 7. The non-oriented electrical steel sheet according to claim 6, wherein the oxide layer is composed of 40 to 70% by weight of O, 25 to 55% by weight of Al, 0.01 to 0.1% by weight of P, 0.01 to 0.1% by weight of Sn, and the remainder being Fe and unavoidable impurities.
8. The non-oriented electrical steel sheet according to any one of claims 1 to 7, characterized in that the average crystal grain size is 50 to 100 µm.
9. 9. The non-oriented electrical steel sheet according to claim 1, wherein, among the sulfides formed inside the base material, the number of sulfides having a diameter of 100 nm or more is three times or more the number of sulfides having a diameter of less than 100 nm.
10. The non-oriented electrical steel sheet according to any one of claims 1 to 9, characterized in that the thickness is 0.10 to 0.30 mm.
11. The thickness of the steel plate at the center in the width direction (t center ) and the thickness (t 500 The non-oriented electrical steel sheet according to any one of claims 1 to 10, characterized in that the difference between the grain size and the grain boundary size is 10 µm or less.
12. a step of producing a hot-rolled sheet by hot rolling a slab containing, in weight percent, 1.5-4.0% Si, 0.1-1.5% Al, 0.05-1.5% Mn, 0.015-0.1% Sn, 0.005-0.05% P, 0.001-0.004% Ga, 0.0005-0.003% Bi, and the balance being Fe and unavoidable impurities; cold rolling the hot rolled sheet at a rolling reduction of 83% or more to produce a cold rolled sheet; and final annealing of the cold rolled sheet; A method for producing a non-oriented electrical steel sheet, characterized in that the produced steel sheet has an area fraction of {118} / / ND orientation texture of 11-15% and is higher than the area fraction of {111} / / ND orientation texture.
13. The method of claim 12, further comprising the step of annealing the hot-rolled sheet at a temperature of 850 to 1150° C. after the step of producing the hot-rolled sheet.
14. The final annealing step is carried out in a hydrogen atmosphere (H 2 ) and nitrogen (N 2 14. The method for producing a non-oriented electrical steel sheet according to claim 12 or 13, characterized in that the steel sheet is annealed in an atmosphere containing 100% by weight of the alloy at a temperature in the range of 400 to 1000° C. for 100 seconds or less.
Citation Information
Patent Citations
Nonoriented silicon steel sheet having excellent magnetic property and its production method
JP2006241563A
Non-oriented electromagnetic steel sheet for rotor, and its manufacturing method
JP2007016278A
Nonoriented electromagnetic steel sheet
JP2019183185A
Non-oriented electrical steel sheet and method for manufacturing the same
KR1020180070949A
Non-oriented electrical steel sheet and method for manufacturing the same
KR1020190078155A