Chain scission to produce improved polymers for 3D printing

End-capping condensation polymers with anhydrides addresses the issue of molecular weight loss and deformation in 3D printing, enhancing melt rheological properties and filler incorporation, thus improving 3D printing efficiency.

JP7583818B2Active Publication Date: 2024-11-14LUMAS POLYMERS LLC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2022544107
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-04
Filing Date
2021-02-24
Publication Date
2024-11-14
Estimated Expiration
2041-02-24

AI Technical Summary

Technical Problem

Condensation polymers face challenges in 3D printing due to uncontrolled molecular weight loss and deformation during melting and shearing, limiting their ability to achieve desired rheological properties for effective layer fusion and incorporation of additives.

Method used

End-capping condensation polymers like polyamides and polyesters by reacting them with compounds such as anhydrides to reduce molecular weight while maintaining high molecular weight fractions, enhancing melt rheological properties and allowing for higher melt flow rates.

Benefits of technology

The process results in polymers with improved melt rheological properties, enabling better layer fusion and the ability to incorporate fillers, significantly increasing melt flow rates and facilitating efficient 3D printing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583818000001
    Figure 0007583818000001
  • Figure 0007583818000002
    Figure 0007583818000002
  • Figure 0007583818000003
    Figure 0007583818000003
Patent Text Reader

Abstract

An end-capped condensation polymer can be formed by heating a condensation polymer in the presence of an end-capping compound to form a cleaved condensation polymer and reacting at least a portion of the cleaved condensation polymer with the end-capping compound to form the end-capped condensation polymer. The end-capped condensation polymer can be used to form additively manufactured articles with high solids loading and improved processability due to improved rheological behavior.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to polymers and methods to enable their use in 3D printing. In particular, the present invention relates to the cleavage of condensation polymers (e.g., polyamides and polyesters) and capping of the cleaved polymers to achieve desired stable rheological properties useful for 3D printing. [Background technology]

[0002] Condensation polymers have been used to form shaped articles by conventional methods such as extrusion, film blowing, injection molding, etc. In these processes, the polymer is melted and substantially sheared, resulting in polymer cleavage and uncontrolled loss of molecular weight, causing deformation during the formation of the shaped article (e.g., blown bottles and extruded tubing). Typically, chain extenders are added to reverse the loss of molecular weight to achieve sufficiently high melt strength and melt viscosity, as described for polyesters and polyethylene terephthalates in U.S. Pat. Nos. 5,393,323 and 5,733,633, respectively.

[0003] Additive manufacturing of thermoplastic polymers typically requires localized melting of a layered pattern that then fuses and supports subsequent layers. Fused Filament Fabrication (FFF), also commonly referred to as plastic jet printing, has been used to form 3D parts using thermoplastic filaments drawn into a heated nozzle, melted, and then extruded, with the extruded filaments fusing together upon cooling (see, for example, U.S. Patent Nos. 5,313,633 and 5,313,633).

[0004] Similarly, selective laser sintering or melting (SLS or SLM) has been used to produce 3D parts by selectively sintering powders in a powder bed (see, for example, US Pat. No. 5,399,633). In this method, a powder bed maintained at an elevated temperature is selectively sintered using a CO2 laser or other electromagnetic radiation source. Once the first layer is sintered, additional layers of powder are metered in and selective sintering is repeated until the desired 3D part is produced. Because the powder must be sintered or melted, SLS has been limited by the need for complex equipment and the use of thermoplastic polymers with very distinctive characteristics that allow sintering without warping or slumping and in particular to achieve the desired fusion between layers. This has generally limited applicability mainly to polyamide (i.e., nylon) or nylon-containing composite powders.

[0005] However, due to the requirement for localized heating and subsequent inter-layer fusion, standard types of thermoplastic polymers such as polyamides have limited printing speeds, for example, by low melt flow rates to achieve sufficient bonding within and between layers without deformation or slumping. The rheological properties (e.g., low melt flow rates) would limit the ability to fill SLS thermoplastic particles or FFF filaments with other ingredients (e.g., inorganic fillers) to achieve specific properties such as hardness and stiffness. And because typical 3D manufacturing (FFF and SLS) does not involve significant shear as encountered during injection molding, the desired rheological properties during processing would not result from cleavage and rebound upon cooling in a shear-free situation. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] U.S. Pat. No. 4,246,378 [Patent Document 2] U.S. Patent No. 7,544,387 [Patent Document 3] U.S. Pat. No. 5,121,329 [Patent Document 4] U.S. Patent No. 5,503,785 [Patent Document 5] U.S. Pat. No. 5,597,589 Summary of the Invention [Problem to be solved by the invention]

[0007] Therefore, it would be desirable to provide a condensation polymer that is uniquely adapted to the problems of condensation polymers when used to 3D print parts. [Means for solving the problem]

[0008] It has been discovered that condensation polymers, such as polyamides and polyesters, can be formed that have desirable melt rheological properties that can improve the fusion of the polymers within and between layers. This process can, for example, reduce the weight average molecular weight while still maintaining a desired amount of a high molecular weight fraction that achieves the desired improved melt rheological properties and maintains the desired properties of the high molecular weight fraction.

[0009] A first aspect of the invention is a method for forming an end-capped condensation polymer useful for additive manufacturing, comprising the steps of: (i) heating the condensation polymer in the presence of an end-capping compound to form a cleaved condensation polymer; and (ii) reacting at least a portion of the cleaved condensation polymer with an end-capping compound to form an end-capped condensation polymer; In one embodiment, sufficient heating can be achieved by providing a sufficient amount of mechanical energy to the condensation polymer, such as provided by a twin screw kneading extruder.

[0010] A second aspect of the invention is a method of forming an article consisting of fused layers of edge-capped condensation polymer produced according to the first aspect of the invention, the layers being deposited in succession by an additive manufacturing process and fused by the directed application of heat.

[0011] A third aspect of the invention is an article comprising an end-capped condensation polymer produced by the method of the first aspect of the invention, or an article produced by the method of the second aspect of the invention.

[0012] A fourth aspect of the invention is a polymer comprising a condensation polymer end-capped with a residue of an end-capping compound. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The explanations and illustrations presented herein are intended to acquaint those skilled in the art with the invention, its principles, and its practical application. The specific embodiments of the present disclosure described are not intended to be exhaustive or to limit the scope of the present disclosure.

[0014] The method of the present invention forms end-capped polymers useful for additive manufacturing by heating a condensation polymer in the presence of an end-capping compound to form a cleaved condensation polymer.

[0015] The condensation polymer may be any suitable condensation polymer, such as those known to those skilled in the art and commercially available. Examples of useful polymers include polyamides, polyesters, polycarbonates, polyamideimides, polyimides, polyacetals, or combinations thereof. Desirably, the polymer is a polyamide, polyester, or polycarbonate. The condensation polymer may be linear or branched. Desirably, the condensation polymer is linear. Examples of polyamides include those available from Ube Industries Ltd., such as polyamide 6, polyamide 6 / 66 copolymer, polyamide 6 / 66 / 12 copolymer, and polyamide 6 / 12 copolymer. Examples of polyesters include polyethylene terephthalate and other commercially available polyesters, such as those available from Celanese under the trade name CELANEX. Examples of polycarbonates include those available from Trinseo SA under the trade name CALIBRE.

[0016] The end-capping compound may be any end-capping compound useful for reacting with and end-capping the cleaved condensation polymer and may vary depending on the particular condensation polymer. Examples of end-capping compounds include those consisting of epoxides, carboxylic acids, alcohols, anhydrides, amines, isocyanates, aziridines, oxazolines, or phosphites. It is desirable for the end-capping compound to be an anhydride or a carboxylic acid. Examples of anhydrides that are particularly useful for end-capping polyamides and polyimides include phthalic anhydride, tetrabromophthalic anhydride, hexahydrophthalic anhydride, sulfophthalic anhydride, trimellitic anhydride, and 1,8-naphthalic anhydride. In certain embodiments, the end-capping agent may introduce useful chemical groups that impart desired properties or characteristics, such as flame retardancy, UV resistance, or other functionality such as the ability to undergo further reaction with a different polymer or reactive group. For example, the end-capping compounds (e.g., anhydrides) may have a variety of functionalities, such as: The end-capping compound (e.g., anhydride) can only react once with the polyamide (functionality of 1), but has a functionality of 2 with the polyester; therefore, the end-capping compound that caps the polyamide can have remaining functionality that allows the compound to react with the polyester, if desired.

[0017] In one embodiment, the end-capping compound is a liquid or solid that has a boiling point above the temperature used to heat and cleave the condensation polymer, illustratively desirably at least about 250° C., 275° C., 300° C., or higher.

[0018] The amount of end-capping agent can be any useful amount depending on the characteristics desired for the end-capped condensation polymer. Typically, the amount can be from about 0.001%, 0.01%, 0.1% to about 5%, 3% or 1% by weight of the condensation polymer and end-capping agent.

[0019] Heating can be to any useful temperature and will depend on the particular condensation polymer to be end-capped. Illustratively, the temperature can be within about 50° C. of the melting temperature of the condensation polymer. In certain embodiments, heating can be to a temperature within about 40° C., 30° C., or 25° C. of the melting temperature of the condensation polymer. Illustratively, the temperature can generally be from about 150° C. or 200° C. to 300° C. or 250° C.

[0020] Any method useful for heating the condensation polymer and end-capping agent may be used, such as methods known for heating and blending polymers. When heated, it may also be desirable to impart shear to the polymer and end-capping agent to mix and further promote the cleavage of the condensation polymer. In one embodiment, a heated single or twin screw extruder, such as those known in the art, may be utilized. The amount of shear may be any useful amount to achieve the desired cleavage and end-capping for a particular device. The extruder may be held at one temperature or may have a gradient along the length of the extruder to promote the desired cleavage and end-capping.

[0021] To aid in forming the end-capped condensation polymer, by-products formed during the end-capping reaction, such as water, can be removed during at least a portion of the process. Any method can be used to remove such by-products, including, for example, drawing a vacuum.

[0022] To illustrate the method, a polyamide is heated with an end-capping agent represented by trimellitic anhydride as shown below: From the description, it is apparent that end-capping of the polyamide can produce water that may be desirable to remove as described herein.

[0023] [ka]

[0024] or

[0025] [ka]

[0026] In another illustration, polyesters can be end-capped using a monofunctional alcohol end-capping agent as shown below. In this example, a 13 carbon branched alcohol with the trade name EXXAL 13 was used to cleave the chains in PET (polyethylene terephthalate). Since the condensation reaction is reversible, the monofunctional alcohol can cleave the ester bond, resulting in a PET chain with reduced molecular weight and a PET chain end-capped with a short chain alcohol. Since EXXAL 13 does not have any additional functional groups, no additional reaction occurs when the chain cleavage is complete.

[0027] [ka]

[0028] In contrast, when the end-capping agent phthalic anhydride is used to end-capping a polyester, the phthalic anhydride acts as a chain extender that increases molecular weight without decreasing it.

[0029] Various factors can affect the degree of molecular weight reduction that occurs in this manner. For example, the concentration of the end-capping reactant, the residence time in the extruder (e.g., as a function of the screw speed), the temperature of the extruder, the moisture content of the polymer, the pressure (e.g., the vacuum pulled on the extruder), and / or the shear rate in the extruder can affect the degree of molecular weight reduction. Slowing the screw speed of the extruder can increase the residence time that the polymer and the end-capping reactant have to react with each other, thereby decreasing the average molecular weight, e.g., increasing the residence time until all of the end-capping reactant has reacted. Increasing the concentration of the end-capping reactant can also increase the statistical probability of an end-capping reactant binding to a reactive site on the cleaved polymer for a given residence time. Increasing the shear and increasing the temperature can increase the rate of chain cleavage that occurs in the extruder, thereby cleaving more molecules and resulting in a lower average molecular weight when the end-capping reactant is present. One or more end-capping reactants can be added sub-stoichiometrically (so that all of the end-capping reactant is consumed in the reaction), stoichiometrically, or in stoichiometric excess.

[0030] When this method is practiced, the end-capped condensation polymer has a lower weight average molecular weight Mw than the starting condensation polymer as well as increased polydispersity and higher melt flow rate. Generally, as Mw decreases and polydispersity increases, the ratio of Mw of the condensation polymer / Mw of the end-capped condensation polymer will be greater than 1, typically at least about 1.2, 1.5, 2 to 10 or 5. Similarly, as polydispersity increases, the ratio of the end-capped condensation polymer compared to the polydispersity of the condensation polymer will be greater than 1, typically at least about 1.2, 1.5, 2 to 10 or 5.

[0031] This method is particularly useful for producing low melt flow rate (MFR) condensation polymers with desirable melt flow rate and rheological properties for producing melt blown and additively manufactured articles. Low melt flow rates at a given temperature, such as typically measured here (e.g., 2.16 kg [g / 10 min] at 235° C.), are less than about 10 or 5 (ASTM D1238). This method can increase the MFR by at least 2, 5, 10, 20, or even 50 times (e.g., up to 500 times) relative to any practically useful MFR. In some embodiments, the MFR of the end-capped condensation polymer is at least about 10, 20, 30, 50, or even 75 to 200 under the conditions described above.

[0032] The end-capped polymer may be mixed with any useful additive to produce an article, such as those known in the art. Illustratively, the end-capped polymer may be mixed with additional components that may be useful when producing an article. The additional components may be one or more dyes, pigments, toughening agents, rheology modifiers, fillers, reinforcing agents, thickeners, opacifiers, inhibitors, fluorescent markers, thermal degradation reducers, heat resistance agents, surfactants, wetting agents, or stabilizers.

[0033] In one embodiment, the end-capped condensation polymer is mixed (e.g., melted and blended) with a filler. The filler can be any useful filler, such as those known in the art. Examples of fillers include ceramic, metal, carbon (e.g., graphite, carbon black, graphene), polymeric particulates that do not melt or decompose at printing temperatures (e.g., crosslinked polymeric particulates, vulcanized rubber particulates, etc.), and plant-based fillers (e.g., wood, nut shell, grain and rice husk flours or particles). Exemplary fillers include calcium carbonate, talc, silica, wollastonite, clay, calcium sulfate, mica, inorganic glasses (e.g., silica, aluminosilicates, borosilicates, alkali aluminosilicates, etc.), oxides (e.g., alumina, zirconia, magnesia, silica "quartz", and calcia), carbides (e.g., boron carbide and silicon carbide), nitrides (e.g., silicon nitride, aluminum nitride), oxynitrides, combinations of oxycarbides, or combinations thereof. In certain embodiments, the filler comprises talc, clay minerals, chopped inorganic glasses, metals, or acicular fillers such as carbon fibers, mullite, mica, wollastonite, or combinations thereof. In particular embodiments, the filler comprises talc.

[0034] The amount of filler can be any amount useful for producing articles, such as additively manufactured articles. For example, the filler can be present in an amount of 20%, 30%, 40%, or 50% to 90% by weight of the end-capped polymer and filler. It has been found that higher loadings of filler can be utilized and still achieve good printing behavior of condensation polymers, such as polyamides, due to the ability to achieve higher MFR and desirable rheology.

[0035] In one embodiment, the end-capped polymer is formed into a powder or filament useful for additive manufacturing, such as SLS or FFF, which is then used to produce additively manufactured articles comprised of the end-capped condensation polymer. EXAMPLES

[0036] The following examples are provided to illustrate the method and polymers formed thereby, but are not intended to limit its scope. All parts and percentages are by weight unless otherwise specified.

[0037] Each of the examples and comparative examples was carried out in a 27 mm twin screw extruder / kneader at 400 revolutions per minute loaded at 60 pounds per hour (about 27 kg) with the polyamide, end capping compound, and end capping compound concentrations detailed for the example as shown below. The length / diameter ratio of the extruder was 40, and the temperature was between 280°C and 240°C along the length of the extruder from the inlet through the die to the outlet (i.e., there is a somewhat linear gradient from start to finish). The pressure (vacuum) was maintained at about 800 millibars (about 80 kPa).

[0038] Example 1 (A to D) and Comparative Example 1: In these examples and comparative examples, the polyamide used is type 6 / 66 / 12 of UBE 6434. The end-capping compound is phthalic anhydride, as shown in Table 1 along with the MFR of each of the examples and comparative examples.

[0039] [Table 1]

[0040] Example 2 (A to D) and Comparative Example 2: In these examples and comparative examples, the polyamide used is type 6 / 66 / 12 of UBE 6434. The end-capping compound is hexahydrophthalic anhydride, as shown in Table 2 along with the MFR of each of the examples and comparative examples.

[0041] [Table 2]

[0042] Example 3 (A to D) and Comparative Example 3: In these examples and comparative examples, the polyamide used is type 6 / 66 / 12 of UBE 6434. The end-capping compound is trimellitic anhydride, as shown in Table 3 along with the MFR of each of the examples and comparative examples. Even when the polyamide is branched, as in this example, this method is effective in achieving the desired MFR.

[0043] [Table 3]

[0044] Example 4 (A to D) and Comparative Example 4: In these examples and comparative examples, the polyamide used is RILSAN Polyamide 11 (Arkema). The end-capping compound is hexahydrophthalic anhydride, as shown in Table 4 along with the MFR of each of the examples and comparative examples. The MFR of the examples was too high to measure. Why the MFR increased so dramatically is not fully understood, but without being limiting in any way, it is probably due to the presence of residual monomers that act as additional plasticizers.

[0045] [Table 4]

[0046] Example 5 (A to C) and Comparative Example 5: In these examples and comparative examples, the polyamide used is NYLENE 615NP PA6 (Nylene Polymer Solutions). The end-capping compound is hexahydrophthalic anhydride, as shown in Table 5 along with the MFR of each of the examples and comparative examples.

[0047] [Table 5]

[0048] Example 6 (A to C) and Comparative Example 6: In these examples and comparative examples, the polyamide used is Shadong Guangyin's type PA 1012. The end-capping compound is hexahydrophthalic anhydride, as shown in Table 6 along with the MFR of each of the examples and comparative examples.

[0049] [Table 6]

[0050] Example 7 (A to C) and Comparative Example 7: In these examples and comparative examples, the polyamide used is EMS Grilamid L16 nat PA12 (EMS-Grivory). The end-capping compound is hexahydrophthalic anhydride, as shown in Table 7 along with the measured MFR for the end-capped polyamide.

[0051] [Table 7]

[0052] Preferred embodiments of the present invention will be described below in detail.

[0053] EMBODIMENT 1 1. A method for forming an end-capped condensation polymer, comprising: (i) heating the condensation polymer in the presence of an end-capping compound to form a cleaved condensation polymer; and (ii) reacting at least a portion of the cleaved condensation polymer with the end-capping compound to form the end-capped condensation polymer; The method comprising:

[0054] EMBODIMENT 2 2. The method of embodiment 1, wherein the end-capping compound comprises an epoxide, a carboxylic acid, an alcohol, an anhydride, an amine, an isocyanate, an aziridine, an oxazoline, or a phosphite.

[0055] EMBODIMENT 3 3. The method of embodiment 1 or 2, wherein the end-capping compound is an anhydride or a carboxylic acid.

[0056] EMBODIMENT 4 4. The method of embodiment 3, wherein the end-capping compound is an anhydride.

[0057] EMBODIMENT 5 5. The method of any one of the preceding claims, wherein the condensation polymer is a polyamide, a polyester, a polycarbonate, a polyamideimide, a polyimide, a polyacetal, or a combination thereof.

[0058] EMBODIMENT 6 6. The method of embodiment 5, wherein the condensation polymer is the polyamide, the polyester, the polycarbonate, or a combination thereof.

[0059] EMBODIMENT 7 The method of any one of the preceding claims, wherein the end-capped condensation polymer and the condensation polymer each have a weight average molecular weight (Mw) and polydispersity such that the Mw of the end-capped condensation polymer is less than the Mw of the condensation polymer and the polydispersity of the end-capped condensation polymer is greater than the polydispersity of the condensation polymer.

[0060] EMBODIMENT 8 8. The method of embodiment 7, wherein the ratio of the Mw of the condensation polymer to the Mw of the end-capped condensation polymer is greater than 1, and the ratio of the polydispersity of the end-capped condensation polymer to the polydispersity of the condensation polymer is greater than 1.

[0061] EMBODIMENT 9 The method of any one of the preceding claims, wherein the end-capped condensation polymer has a melt flow rate of at least 20 g / 10 min (2.16 kg at 235°C).

[0062] EMBODIMENT 10 10. The method of embodiment 9, wherein the end-capped condensation polymer is a polyamide, a polyester, a polycarbonate, a polyamideimide, a polyimide, a polyacetal, or a combination thereof.

[0063] EMBODIMENT 11 11. The method of embodiment 10, wherein the end-capped condensation polymer is the polyamide, the polyester, or a combination thereof.

[0064] EMBODIMENT 12 12. The method of any one of embodiments 9 to 11, wherein the end-capped condensation polymer has a MFR of at least 20 g / 10 min (2.16 kg at 235° C.).

[0065] EMBODIMENT 13 13. The method of any one of the preceding claims, further comprising shearing the condensation polymer during the heating step.

[0066] EMBODIMENT 14 14. The method of any one of the preceding claims, wherein the heating step is carried out at a temperature above the melting temperature and below the decomposition temperature of the condensation polymer.

[0067] EMBODIMENT 15 15. The method of any one of the preceding embodiments, wherein the heating step is carried out in a screw extruder.

[0068] EMBODIMENT 16 16. The method of any one of the preceding claims, further comprising removing water during at least a portion of the method.

[0069] EMBODIMENT 17 17. The method of embodiment 16, wherein water is removed by carrying out the method under reduced pressure.

[0070] EMBODIMENT 18 18. The method of any one of the preceding claims, wherein the end-capping compound comprises one or more of tetrabromophthalic anhydride, hexahydrophthalic anhydride, trimellitic anhydride, 1,8-naphthalic anhydride, phthalic anhydride, or sulfophthalic anhydride.

[0071] EMBODIMENT 19 19. The method of any one of the preceding claims, wherein the end-capped condensation polymer is formed into a powder or filaments.

[0072] EMBODIMENT 20 20. The method of any one of the preceding claims, wherein the amount of the end-capping compound is from 0.01% to 5% by weight of the condensation polymer and the end-capping compound.

[0073] EMBODIMENT 21 21. A method of forming an article consisting of fused layers of the edge-capped condensation polymer produced by the method of any one of claims 1 to 20, wherein the layers are deposited in succession by an additive manufacturing method and fused by the directed application of heat.

[0074] EMBODIMENT 22 22. The method of embodiment 21, wherein the additive manufacturing method is SLS or FFF.

[0075] EMBODIMENT 23 23. The method of embodiment 21 or 22, wherein the end-capped condensation polymer has a filler in an amount of at least about 25% to 90% by weight of the polymer and the filler.

[0076] EMBODIMENT 24 21. An article comprising an end-capped condensation polymer produced by the method of any one of claims 1 to 20.

[0077] EMBODIMENT 25 21. A polymer consisting of the end-capped condensation polymer according to any one of the preceding embodiments.

[0078] EMBODIMENT 26 24. An article produced by the method of any one of claims 21 to 23.

[0079] EMBODIMENT 27 26. The polymer of embodiment 25, wherein the end-capped condensation polymer has an MFR of at least 10.

[0080] EMBODIMENT 28 The article of claim 26, wherein the end-capped condensation polymer is end-capped with a reaction product of an epoxide, a carboxylic acid, an alcohol, an anhydride, an amine, an isocyanate, an aziridine, an oxazoline, or a phosphite.

[0081] EMBODIMENT 29 29. The article of claim 28, wherein the end-capped condensation polymer is end-capped with a reaction product of the carboxylic acid or the anhydride.

[0082] EMBODIMENT 30 30. The article of claim 29, wherein the end-capped condensation polymer is the anhydride end-capped polyamide.

[0083] EMBODIMENT 31 A polymer comprising a condensation polymer end-capped with the residue of an end-capping compound.

[0084] EMBODIMENT 32 32. The polymer of embodiment 31, wherein the condensation polymer is a polyamide, a polyester, a polycarbonate, a polyamideimide, a polyimide, a polyacetal, or a combination thereof.

[0085] EMBODIMENT 33 33. The polymer of embodiment 32, wherein the condensation polymer is a polyamide, a polyester, or a polycarbonate.

[0086] EMBODIMENT 34 34. The polymer of embodiment 33, wherein the condensation polymer is a polyamide.

[0087] EMBODIMENT 35 The polymer of any one of embodiments 31 to 34, wherein the end-capping compound is an epoxide, a carboxylic acid, an alcohol, an anhydride, an amine, an isocyanate, an aziridine, an oxazoline, or a phosphite.

[0088] EMBODIMENT 36 The polymer of embodiment 35, wherein the end-capping compound is an anhydride and the condensation polymer is a polyamide.

[0089] EMBODIMENT 37 37. The polymer of embodiment 36, wherein the anhydride is tetrabromophthalic anhydride, hexahydrophthalic anhydride, trimellitic anhydride, 1,8-naphthalic anhydride, phthalic anhydride, or sulfophthalic anhydride.

[0090] EMBODIMENT 38 38. The polymer of embodiment 36 or 37, wherein the polymer has a melt flow rate of at least about 10 g / 10 min (2.16 kg at 235° C.).

[0091] EMBODIMENT 39 2. The method of embodiment 1, wherein the end-capping compounds have variable functionality.

Claims

1. 1. A method for forming an end-capped polyamide polymer, comprising: (i) heating a polyamide polymer, which may be branched or linear and has a melt flow rate of at most 5 g / 10 min (2.16 kg at 235° C.), in the presence of end-capping compounds, each end-capping compound having a functionality of 1, to form a cleaved polyamide polymer; and (ii) reacting at least a portion of the cleaved polyamide polymer with the end capping compound to form the end capped polyamide polymer, the cleaved polyamide polymer having a melt flow rate of from 20 g to 200 g / 10 min (2.16 kg at 235° C.) and an amount of filler of from 30% to 90% by weight of the cleaved polyamide polymer and filler, the end capping compound comprising an anhydride or a carboxylic acid; The method comprising:

2. The method of claim 1 , wherein the end-capping compound comprises an anhydride.

3. The method of claim 2 wherein the end-capping compound is an anhydride.

4. 2. The method of claim 1, wherein the polyamide polymer is polyamide 6, copolyamide (6 / 66), copolyamide (6 / 66 / 12), polyamide 1012, polyamide 11, or copolyamide (6 / 12).

5. The method of claim 1 , wherein the end-capped polyamide polymer has a melt flow rate of at least 50 g / 10 min (2.16 kg at 235° C.).

6. 2. The method of claim 1, wherein the end capped polyamide polymer has a filler in an amount of at least about 50% to 90% by weight of the polymer and the filler, the cleaved polyamide polymer has a polydispersity 1.2 to 10 times greater than the polydispersity of the polyamide polymer, and the polyamide polymer has a weight average molecular weight 1.2 to 10 times greater than the weight average molecular weight of the cleaved polyamide polymer.

7. 7. The process of any one of claims 1 to 6, further comprising the steps of shearing the polyamide polymer in a screw extruder during the heating step, which is conducted at a temperature above the melting temperature and below the decomposition temperature of the polyamide polymer, and removing water under reduced pressure during at least a portion of the process.

8. The method of any one of claims 1 to 6, wherein the end-capping compound comprises one or more of tetrabromophthalic anhydride, hexahydrophthalic anhydride, 1,8-naphthalic anhydride, or phthalic anhydride.

9. 7. The method of claim 1, wherein the amount of the end capping compound is from 0.7% to 5% by weight of the polyamide polymer and the end capping compound.

Citation Information

Patent Citations

  • Thermoplastic blends with end-group controlled polyamide resin

    EP0285692A1

  • Process for Making Inorganic-Filled Polyamide and Polyester Compositions Exhibiting Increased Melt Flow and Articles Formed Therefrom

    JP2009529602A

  • Thermoplastic polyester resinous composition

    US4246378A

  • Apparatus and method for creating three-dimensional objects