Perovskite layer, method for producing perovskite layer, solar cell with perovskite layer, and solar cell module with perovskite layer

A two-step process for forming perovskite seed crystals and films addresses substrate coverage and defect issues in perovskite solar cells, enhancing efficiency and reducing defects through controlled annealing and solvent volatilization.

JP7583927B2Active Publication Date: 2024-11-14LONGI GREEN ENERGY TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023520492
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-11-25
Filing Date
2021-10-13
Publication Date
2024-11-14
Estimated Expiration
2041-10-13

AI Technical Summary

Technical Problem

Conventional methods for manufacturing perovskite solar cells result in incomplete coverage of the substrate and defects such as cracks, large grain boundaries, and pores due to slow diffusion rates and environmental control issues, leading to reduced performance and efficiency.

Method used

A two-step process involving the formation of perovskite seed crystals on a substrate, followed by immersion in a perovskite solution to grow a film, with controlled annealing to form a perovskite layer, utilizing temperature reduction and solvent volatilization to enhance grain size and reduce defects.

Benefits of technology

The method ensures complete substrate coverage with fewer defects, increasing conversion efficiency and reducing electrical leakage risks while accelerating production, resulting in higher-quality perovskite films.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583927000001
    Figure 0007583927000001
  • Figure 0007583927000002
    Figure 0007583927000002
  • Figure 0007583927000003
    Figure 0007583927000003
Patent Text Reader

Abstract

This application discloses a perovskite layer, a method for manufacturing a perovskite layer, a solar cell with a perovskite layer, and a solar cell module with a perovskite layer, which relate to the technical field of photovoltaic power generation. The method for manufacturing a perovskite layer can completely cover a substrate and has few defects. The method for manufacturing a perovskite layer includes the steps of providing a substrate, forming perovskite seed crystals on the substrate, immersing the perovskite seed crystals in a perovskite solution, growing the perovskite seed crystals into a perovskite film under the action of the perovskite seed crystals, and annealing the perovskite film to form a perovskite layer. The perovskite layer and method for manufacturing the same according to this application can be used in the manufacture of solar cells.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application relates to the technical field of photovoltaic power generation, and in particular to a perovskite layer, a method for producing a perovskite layer, a solar cell with a perovskite layer, and a solar cell module with a perovskite layer. <CROSS REFERENCE TO RELATED APPLICATIONS>

[0002] This application claims priority to a Chinese patent application filed with the China Patent Office on November 25, 2020, bearing application number 202011343679.6 and entitled "Perovskite layer, method for manufacturing perovskite layer, solar cell with perovskite layer, and solar cell module with perovskite layer," the entire contents of which are incorporated herein by reference. [Background technology]

[0003] In the process of manufacturing perovskite solar cells, the perovskite layer is usually produced by a wet chemical method, which generally involves coating a perovskite precursor solution on a substrate, followed by baking or other means to crystallize and precipitate the solute to form the perovskite layer.

[0004] In the prior art, the formed perovskite layer often cannot completely cover the substrate, and there are many defects such as cracks, large grain boundaries, holes, etc., which seriously affect the performance of the perovskite battery. In the prior art, the method of poor solvent and the method of two-stage film formation can alleviate defects such as cracks, large grain boundaries, holes, etc. in the crystallization process of the perovskite film, but in the process of crystallization and grain growth, the diffusion rate of the perovskite solute is relatively slow, and the defects caused by the inability to replenish around the perovskite seed crystal still exist. In addition, when the perovskite layer is produced by the method of poor solvent method, two-stage method, etc., it is difficult to control, there are high requirements for factors such as environment and atmosphere, and the currently used poor solvent is highly toxic. Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present application is to provide a perovskite layer that can produce a perovskite layer that completely covers a substrate and has few defects, a method for producing a perovskite layer, a solar cell with a perovskite layer, and a solar cell module with a perovskite layer. [Means for solving the problem]

[0006] In a first aspect, the present application provides a method for producing a perovskite layer, the method comprising the steps of providing a substrate, forming a perovskite seed crystal on the substrate, immersing the perovskite seed crystal in a perovskite solution to grow a perovskite film, and annealing the perovskite film to form a perovskite layer.

[0007] When adopting the above technical solution, the process of forming perovskite seed crystals and the process of growing the perovskite seed crystals into a perovskite film are divided into two steps. First, the perovskite seed crystals are formed on a substrate, and then the perovskite seed crystals are immersed in a perovskite solution to grow a perovskite film. Based on the above, the process of forming the perovskite seed crystals can be independently controlled, which can form perovskite seed crystals with large grain size and distributed over the entire substrate. The action of these perovskite seed crystals with large grain size and distributed over the entire substrate can grow a perovskite film covering the entire substrate, and reduce the defects of the perovskite film. In this case, the perovskite film can be annealed to form a perovskite layer covering the entire substrate and with fewer defects, which can increase the conversion efficiency of the perovskite layer and reduce the risk of leakage current.

[0008] In some possible embodiments, in the process of growing the above-mentioned perovskite seed crystals into a perovskite film, the solubility of the perovskite material in the perovskite solution is reduced to promote the precipitation of the perovskite material from the perovskite solution and provide the perovskite material for the growth of the perovskite seed crystals. With the reduction in the solubility of the perovskite material in the perovskite solution, the perovskite solute in the perovskite solution is nearly saturated or saturated, making it easier for the perovskite solute to precipitate from the perovskite solution. In this case, the perovskite solute can be quickly diffused and transported to the surroundings of the perovskite seed crystals, and the perovskite solute consumed by the precipitation of the crystals around the perovskite seed crystals can be timely replenished. On this basis, on the one hand, the perovskite solute can be timely supplemented, so that the defects such as crystal boundaries and holes can be reduced during the process of growing the perovskite film, and the density of the perovskite film can be improved; on the other hand, the perovskite solute can be quickly transported around the perovskite seed crystal, so that the perovskite seed crystal can be rapidly grown, and the growth rate of the perovskite film can be accelerated, thereby improving the production efficiency and saving the production time.

[0009] In some possible embodiments, the solubility of the perovskite material is reduced by decreasing the temperature. On the one hand, such a temperature reduction method is easy to implement and can reduce the difficulty of the process. On the other hand, the process of reducing the solubility of the perovskite material can be easily adjusted by adjusting the temperature, which provides greater control over the process of reducing the solubility of the perovskite material.

[0010] In some possible embodiments, the rate of temperature reduction is 0.1°C / h to 10°C / h. In this case, the rate of decrease in the solubility of the perovskite material is appropriate, and the growth rate of the perovskite film can be accelerated while ensuring the quality of the perovskite film. Not only can the problem of the perovskite crystal growing too fast resulting in an increase in defects be avoided, but also the problem of the perovskite crystal growing too slowly resulting in reduced production efficiency can be avoided.

[0011] In some possible embodiments, before the above-mentioned temperature decrease, the initial temperature of the perovskite solution is 100° C. to 150° C. In this case, since the initial temperature of the perovskite solution is high, the temperature decrease operation is easy to carry out, and the temperature decrease cost is low.

[0012] In some possible embodiments, in the process of growing the above-mentioned perovskite seed crystals into a perovskite film, the solvent evaporation is accelerated to promote the precipitation of the perovskite material from the perovskite solution, and to provide the perovskite material for the growth of the perovskite seed crystals. By accelerating the solvent evaporation, the perovskite material in the perovskite solution is nearly saturated or saturated, which can further reduce the occurrence of defects such as crystal boundaries and holes in the process of growing the perovskite seed crystals into a perovskite film, improve the density of the perovskite film, and accelerate the growth rate.

[0013] In some possible embodiments, the solvent evaporation is accelerated by heating, in which case the evaporation rate of the solvent can be conveniently adjusted by controlling the heating temperature, and thus the growth rate of the perovskite film can be adjusted.

[0014] In some possible embodiments, the initial temperature of the above-mentioned perovskite solution is 20°C to 30°C, and in the process of growing the perovskite seed crystal into a perovskite film, the heating temperature is 40°C to 100°C. In this case, the initial temperature of the perovskite solution is low, the perovskite solution is easy to manufacture, and the cost is low when heating to a higher temperature. In addition, the temperature difference between the heating temperature and the initial temperature is appropriate, so that the growth rate of the perovskite film can be increased and the quality of the perovskite film can be ensured.

[0015] In some possible embodiments, when the above-mentioned perovskite seed crystal is immersed in the perovskite solution, the perovskite solution is a saturated solution, in which the perovskite material is more easily precipitated from the perovskite solution, and the perovskite material is rapidly precipitated on the surface of the perovskite seed crystal by the action of the perovskite seed crystal, which promotes the growth of the perovskite seed crystal, and forms a perovskite film with fewer defects and higher density.

[0016] In some possible embodiments, the above-mentioned perovskite seed crystals are distributed discretely on the substrate. In this case, the multiple perovskite seed crystals distributed discretely on the substrate serve as multiple growth points for the growth of the perovskite film, and grow continuously to become a continuous perovskite film. In this process, the perovskite seed crystals are distributed discretely, which can avoid the problem that the perovskite seed crystals overlap and cover each other, resulting in the perovskite film grains being too small, and can form a uniform perovskite film and cover the entire substrate.

[0017] In some possible embodiments, the coverage of the above perovskite seed crystals on the substrate is 10% to 50%, and the particle size of the perovskite seed crystals is 10 nm to 200 nm. On the one hand, perovskite seed crystals with a particle size of 10 nm to 200 nm have an appropriate size, and can avoid the problem of many internal defects when the crystal grain size of the perovskite seed crystals is too large. On the other hand, when the perovskite seed crystals have the above particle size, the coverage of 10% to 50% ensures that the interval and number of the perovskite seed crystals distributed on the substrate are appropriate. By the action of these perovskite seed crystals, a perovskite film with a large crystal grain size and few defects such as crystal boundaries can be efficiently formed. In this case, the problem of the crystal grain size of the perovskite film being small and the number of crystal boundaries being large due to the spacing between the perovskite seed crystals being too small (the coverage rate being too high) can be avoided, and the problem of the growth rate of the perovskite film being slow due to the spacing between the perovskite seed crystals being too large (the coverage rate being too low) can also be avoided.

[0018] In some possible embodiments, the step of forming perovskite seeds on a substrate comprises: Applying a perovskite precursor solution onto a substrate and volatilizing a solvent of the perovskite precursor solution to form a perovskite seed crystal intermediate; and annealing the perovskite seed crystal intermediate to form a perovskite seed crystal.

[0019] In some possible embodiments, the concentration of the above-mentioned perovskite precursor solution is 0.1 mol / L or less. In this case, a large amount of solvent in the perovskite precursor solution can separate the crystallized and precipitated perovskite seed crystals to form discretely distributed perovskite seed crystals, thereby forming the above-mentioned coverage and discretely distributed perovskite seed crystals. By adjusting the concentration of the perovskite precursor solution, the degree of dispersion and coverage of the perovskite seed crystals can be adjusted.

[0020] In some possible embodiments, the time of the annealing process for forming the above-mentioned perovskite seed crystal is 1 min to 30 min. When the annealing time is in this range, the crystal grain size of the perovskite seed crystal formed by annealing is appropriate. In addition, the annealing time in this range can avoid the problem of the perovskite seed crystal growing too much due to the annealing time being too long, and further reduce the internal defects of the perovskite seed crystal.

[0021] In some possible embodiments, the general formula of the above perovskite seed crystal is ABX3, the perovskite precursor solution includes AX precursor and BX2 precursor, X is a halogen element, A and B are cations, the perovskite seed crystal is an organic-inorganic hybrid material, the substance ratio of the AX precursor to the BX2 precursor is (2-15):1, and according to the above precursor blending ratio, after annealing, the perovskite seed crystal can be formed by annealing, which is discretely distributed and has the above coverage. Based on this, the substance ratio of the AX precursor to the BX2 precursor can be adjusted to adjust the coverage of the perovskite seed crystal. The perovskite seed crystal may be a total inorganic material, and the substance ratio of the AX precursor to the BX2 precursor is (0.95-1.05):1, in which case the coverage of the perovskite seed crystal can be adjusted by the precursor concentration.

[0022] In some possible embodiments, the perovskite seed crystal is an organic-inorganic hybrid material, and the annealing temperature for forming the perovskite seed crystal is 60°C to 130°C. In the process of annealing the perovskite seed crystal intermediate to form the perovskite seed crystal, the high temperature in the annealing process can also volatilize the organic halide. It can be seen that when AX is an organic halide, the excess AX precursor can be easily removed after forming the perovskite seed crystal.

[0023] In some possible embodiments, the perovskite seed crystals are all-inorganic and the annealing temperature is between 120°C and 220°C.

[0024] In a second aspect, the present application provides a perovskite seed crystal and a perovskite film, the perovskite seed crystal and the perovskite film comprising a first interface between the perovskite seed crystal and the perovskite film, the first interface being observed under high resolution scanning electron microscope. To The interface between the perovskite seed crystal and the perovskite film is more observable under high resolution scanning electron microscope. To Because a more observable first interface is formed.

[0025] In some possible embodiments, the first interface formed between the perovskite seed crystal and the perovskite film further includes a structural transition layer, the lattice parameter of the structural transition layer changes according to a first order, and the atomic arrangement manner of the structural transition layer changes according to a second order, the first order being the order from the initial parameter to a second parameter greater than the initial parameter and then to the initial parameter along the direction away from the perovskite seed crystal, and the second order being the order from order to disorder and then to order along the direction away from the perovskite seed crystal. Since the lattice parameter of the structural transition layer changes according to a first order and the atomic arrangement manner of the structural transition layer changes according to a second order, the concentration of defects also changes according to the order from the initial concentration to a second concentration greater than the initial concentration and then to the initial concentration along the direction away from the perovskite seed crystal, so that the change of the perovskite seed crystal in the process of forming the perovskite film is more gradual, the defects of the formed first interface are reduced, and the sudden change of the perovskite film due to direct change is avoided.

[0026] In some possible embodiments, the thickness of the structural transition layer is between 0.5 nm and 5 nm, which provides a "gradual transition"-like effect in the perovskite seed crystals and the perovskite film.

[0027] In a third aspect, the present application provides a solar cell with a perovskite layer, the solar cell comprising a perovskite layer according to any embodiment of the first or second aspect.

[0028] The beneficial effects of the perovskite layer according to the third aspect may be referred to the beneficial effects of the perovskite layer described in any of the embodiments of the first or second aspects and will not be further described here.

[0029] In a fourth aspect, the present application provides a solar cell module with a perovskite layer, comprising the solar cell with a perovskite layer according to the third aspect.

[0030] The beneficial effects of the solar cell module with a perovskite layer according to the fourth aspect may be understood by reference to the beneficial effects of the perovskite layer described in any of the embodiments of the first or second aspect, and will not be further described here. [Brief description of the drawings]

[0031] The drawings described herein are provided to facilitate a better understanding of the present application, constitute a part of the present application, and the illustrative embodiments and the description thereof are intended to interpret the present application and are not intended to unduly limit the present application. [Figure 1-3] FIG. 1 is a schematic diagram of a manufacturing process of a perovskite layer in the prior art. [Figure 4-11] 1A to 1C are schematic diagrams illustrating the states at each stage of a method for producing a perovskite layer according to an embodiment of the present application. [Figure 12] FIG. 2 is a schematic diagram of the structure of a perovskite layer according to an embodiment of the present application. [Figure 13] FIG. 2 is a schematic diagram of the structure of another perovskite layer according to an embodiment of the present application. [Figure 14] FIG. 14 is a partially enlarged schematic diagram of part A in FIG. 13 according to an embodiment of the present application. [Figure 15] FIG. 2 is a schematic diagram of forming perovskite seed crystals by annealing when AX is an organic halide and in excess according to an embodiment of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0032] In order to clearly describe the technical solutions of the embodiments of the present application, the embodiments of the present application use terms such as "first", "second", etc. to distinguish between identical or similar items that have substantially the same functions and actions. As can be understood by those skilled in the art, the terms "first", "second", etc. do not limit the number and execution order, and the terms "first", "second", etc. do not necessarily mean different ones.

[0033] After more than a decade of development, perovskite solar cells have an energy photoelectric conversion efficiency approaching that of crystalline silicon solar cells. Perovskite solar cells have many advantages, including high conversion efficiency, simple device structure, and a manufacturing process mainly using wet chemical methods, making them the most practical next-generation solar cells.

[0034] At present, the perovskite layer of the perovskite battery is mainly manufactured by wet chemical methods. Whether it is a one-step method or two-step method, the main manufacturing process of the perovskite layer includes the steps of: pre-coating a perovskite precursor solution on a substrate 11 having an electron transport layer 12 to form a perovskite precursor solution layer 13, as shown in Figure 1; then, by means of direct baking, anti-solvent crystallization, vacuum flash and other means, volatilizing the solvent in the perovskite precursor solution layer 13, crystallizing and precipitating the solute (perovskite material) to form a perovskite film, and annealing the perovskite film to form a perovskite layer 142, as shown in Figure 2.

[0035] In the above-mentioned manufacturing process of the perovskite layer, as shown in FIG. 1, after a perovskite precursor solution layer 13 is applied onto a substrate 11 having an electron transport layer 12, extremely small perovskite crystal grains are preferentially precipitated at the contact portion between the perovskite precursor solution layer 13 and the electron transport layer 12 as the solvent evaporates, and these crystal grains become perovskite seed crystals 141 of the perovskite film.

[0036] As shown in FIG. 3, when the perovskite seed crystal 141 is formed, the concentration of the perovskite solute around it decreases, and a low-concentration region 131 is formed. In the low-concentration region 131, the concentration of the perovskite solute is lower than the concentration of the perovskite solute in the perovskite precursor solution layer 13. The perovskite solute in the perovskite precursor solution layer 13 is driven by the concentration difference and diffuses and is transported to the low-concentration region 131. The volatilization of the solvent in the perovskite precursor solution layer 13 is continuously performed at the same time as this diffusion and transport. The volatilization of the solvent in the perovskite precursor solution layer 13 increases the concentration difference between the perovskite precursor solution layer 13 and the low-concentration region 131, and the growth of the perovskite seed crystal 141 is promoted. Through this mechanism, the solute in the perovskite precursor solution layer 13 is constantly transported to the surface of the perovskite seed crystal 141, the perovskite seed crystal 141 gradually grows, and finally a perovskite film is formed on the electron transport layer 12.

[0037] In the crystallization and grain growth, the perovskite solute has a slow diffusion speed, so that the defects caused by the inability to timely replenish the surroundings of the perovskite seed crystal 141 are addressed by the embodiment of the present application, which provides a perovskite layer. The perovskite layer can not only completely cover the substrate 21, but also has high film quality and few defects. Furthermore, the perovskite layer 24 has a short manufacturing time, a fast growth rate, and a high operating efficiency. The perovskite layer can be an organic-inorganic hybrid perovskite layer, an inorganic perovskite layer, or an organic perovskite layer. Specifically, the perovskite layer can be a lead-free perovskite layer or a double perovskite layer.

[0038] The present application further provides a method for manufacturing the above-mentioned perovskite layer. Figures 4 to 11 are schematic diagrams showing the states at each stage of the method for manufacturing a perovskite solar cell according to the embodiment of the present application. As shown in Figures 4 to 11, the method for manufacturing a perovskite layer according to the embodiment of the present application is as follows.

[0039] As shown in FIG. 4, a substrate 21 is provided. The substrate 21 is a conductive substrate. Specifically, the substrate 21 can be any of the following: tin-doped indium oxide (ITO) transparent conductive glass, zinc-doped indium oxide (IZO) transparent conductive glass, tungsten-doped indium oxide (IWO) transparent conductive glass, titanium-doped indium oxide (ITIO) transparent conductive glass, fluorine-doped tin oxide (FTO) transparent conductive glass, and aluminum-doped zinc oxide (AZO) transparent conductive glass. In practical applications, the above substrate 21 can be obtained by procurement or self-manufactured by a process such as magnetron sputtering.

[0040] To facilitate processing of substrate 21 in subsequent operations, substrate 21 may be cleaned.

[0041] As shown in Fig. 5, an electron transport layer 22 is formed on a substrate 21. The material of the electron transport layer 22 may be any one of SnO2, TiO2, and [6,6]-phenyl-C61-isomethylbutyrate (PCBM), but is not limited thereto. The thickness of the electron transport layer 22 may be 50 nm to 100 nm. The manufacturing process of the electron transport layer 22 may be spin coating, deposition, or the like, but is not limited thereto.

[0042] 6, a perovskite seed crystal 23 is formed on a substrate 21 having an electron transport layer 22. The steps of forming the perovskite seed crystal 23 mainly include the following steps:

[0043] A perovskite precursor solution is applied onto the substrate 21, and the solvent of the perovskite precursor solution is volatilized to form a perovskite seed crystal intermediate 231. The perovskite seed crystal intermediate 231 is annealed to form a perovskite seed crystal 23.

[0044] The above-mentioned perovskite seed crystals 23 are distributed discretely on the substrate 21. The particles of the multiple perovskite seed crystals 23 are distributed over the entire substrate 21, and the perovskite seed crystals 23 have a certain interval between each other, and do not overlap and cover each other. In this case, the multiple perovskite seed crystals 23 distributed discretely on the substrate 21 become multiple growth points for the growth of the perovskite film, and grow continuously to form a continuous perovskite film. In this process, the discretely distributed perovskite seed crystals 23 can avoid the problem that the crystal grains of the perovskite film are too small due to the perovskite seed crystals 23 overlapping and covering each other, and can form a uniform perovskite film to completely cover the substrate 21.

[0045] The coverage of the perovskite seed crystals 23 on the substrate 21 may be 10% to 50%, and the particle size of the perovskite seed crystals 23 may be 10 nm to 200 nm. On the one hand, the perovskite seed crystals 23 with a particle size of 10 nm to 200 nm have an appropriate size, and can avoid the problem of many internal defects when the crystal grain size of the perovskite seed crystals 23 is too large, and can also avoid the problem of slow growth rate of the perovskite film when the crystal grain size of the perovskite seed crystals 23 is too small. On the other hand, when the perovskite seed crystals 23 have the above particle size, the coverage of 10% to 50% makes the interval and number of the perovskite seed crystals 23 distributed on the substrate 21 appropriate. These actions of the perovskite seed crystals 23 make it possible to efficiently form a perovskite film with large crystal grain size and few defects such as crystal boundaries. In this case, the problem of the perovskite film having a small crystal grain size and many crystal boundaries due to the spacing between the perovskite seed crystals 23 being too small (the coverage rate being too high) can be solved, and the problem of the perovskite film growing at a slow rate due to the spacing between the perovskite seed crystals 23 being too large (the coverage rate being too low) can be avoided.

[0046] As an example, the coverage of the perovskite seed crystals 23 on the substrate 21 may be 10%, 18%, 20%, 25%, 30%, 34%, 40%, 45%, 50%, etc. The particle size of the perovskite seed crystals 23 may be 10 nm, 20 nm, 50 nm, 70 nm, 90 nm, 100 nm, 120 nm, 150 nm, 175 nm, 185 nm, 190 nm, 200 nm, etc.

[0047] In practical applications, the above-mentioned perovskite seed crystals 23 can be obtained by adjusting the concentration of the perovskite precursor solution. Specifically, the concentration of the perovskite precursor solution may be 0.1 mol / L or less. Usually, the concentration of the perovskite precursor solution for producing a perovskite layer is 0.5 mol / L to 1.5 mol / L, and in the embodiment of the present application, the concentration of the perovskite precursor solution is much lower than the concentration usually used. The perovskite seed crystals 23 crystallized and precipitated by a large amount of solvent are separated to form the perovskite seed crystals 23 that are distributed discretely, thereby forming the perovskite seed crystals 23 that have the above-mentioned coverage and are distributed discretely. In this case, the concentration of the perovskite precursor solution can be adjusted to adjust the degree of dispersion and coverage of the perovskite seed crystals 23. The lower the concentration of the perovskite precursor solution, the smaller the coverage of the perovskite seed crystals 23 becomes, and the higher the dispersion degree of the perovskite seed crystals 23 becomes.

[0048] As an example, the concentration of the perovskite precursor solution may be 0.1 mol / L, 0.09 mol / L, 0.08 mol / L, 0.07 mol / L, 0.06 mol / L, 0.05 mol / L, 0.04 mol / L, 0.03 mol / L, 0.02 mol / L, 0.01 mol / L, etc. In order to obtain perovskite seed crystals 23 with good coverage, the concentration of the perovskite precursor solution may be between 0.02 mol / L and 0.05 mol / L.

[0049] In practical applications, the above-mentioned perovskite seed crystal 23 can also be obtained by adjusting the compounding ratio of the perovskite precursor solution. The general formula of the perovskite material is ABX3, and the perovskite precursor solution includes AX precursor and BX2 precursor, where X is a halogen element, and A and B are cations. The perovskite material may be an organic-inorganic hybrid material, and the substance ratio of the AX precursor to the BX2 precursor may be (2-15):1. In the perovskite precursor solution used for manufacturing the perovskite layer, the substance ratio of the AX precursor to the BX2 precursor is usually 1:1, and even if one of the precursors is overdosed in consideration of passivation defects, the ratio of AX:BX2 is between (0.9-1.1):1. In the embodiment of the present application, as shown in FIG. 15, since the substance amount of the AX precursor is large, a large amount of the AX precursor remains after the solvent of the perovskite precursor solution is volatilized to form the perovskite seed crystal intermediate 231. These excess AX precursors can separate a plurality of perovskite seed crystal intermediates 231, and after annealing, form perovskite seed crystals 23 that are discretely distributed and have the above coverage. Based on this, the coverage of the perovskite seed crystals 23 can be adjusted by adjusting the substance ratio of the AX precursor to the BX2 precursor. The larger the substance amount of the AX precursor is relative to the substance amount of the BX2, the lower the coverage of the perovskite seed crystals 23 and the higher the dispersion degree of the perovskite seed crystals 23. When the perovskite material is a total inorganic material, the substance amount ratio of the AX precursor to the BX2 precursor can be (0.95-1.05):1, and in this case, the coverage of the perovskite seed crystals can be adjusted by the concentration of the precursors.

[0050] For example, the mass ratio of the AX precursor to the BX2 precursor may be 2:1, 3:1, 5:1, 7:1, 9:1, 10:1, 11:1, 12.5:1, 13:1, 13.4:1, 15:1, etc. In order to obtain a perovskite seed crystal 23 with an appropriate coverage, the mass ratio of the AX precursor to the BX2 precursor may be (5 to 10):1.

[0051] The method of applying the above-mentioned perovskite precursor solution may be any of blade coating, spin coating, drop coating, inkjet, rotogravure coating, spray coating, and roll coating. The method of volatilizing the solvent of the perovskite precursor solution may be, but is not limited to, natural volatilization, volatilization by baking, vacuum flash, and crystallization acceleration by a poor solvent, as long as the solvent of the perovskite precursor solution can be volatilized.

[0052] The time of the annealing treatment may be 1 min to 30 min. For example, the annealing time may be 1 min, 10 min, 12 min, 17 min, 20 min, 25 min, 28 min, 30 min, etc. In this case, the crystal grain size of the perovskite seed crystal 23 formed by annealing is appropriate. Furthermore, with the annealing time in this range, the problem of the perovskite seed crystal 23 growing too much due to the annealing time being too long can be avoided, and the internal defects of the perovskite seed crystal 23 can be reduced.

[0053] The temperature of the annealing treatment may be set according to the perovskite seed crystals. Since the perovskite seed crystals 23 are small, discontinuous crystal grains that are scattered, the annealing temperature for forming the perovskite seed crystals 23 should be 20°C to 50°C lower than the annealing temperature for forming the perovskite film. When the perovskite seed crystals are all inorganic materials, the annealing temperature may be 120°C to 220°C. In this case, it is possible to avoid stoichiometric mismatch and decomposition of the perovskite seed crystals 23 while ensuring that the perovskite seed crystals 23 formed after the annealing treatment have few defects. Preferably, the annealing temperature may be 160°C to 200°C. For example, when the perovskite seed crystals are all inorganic materials, the annealing temperature may be 120°C, 130°C, 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, etc.

[0054] When the perovskite seed crystal is an organic-inorganic hybrid perovskite material, i.e., AX is an organic halide, the annealing temperature may be 60° C. to 130° C. Preferably, the annealing temperature may be 90° C. to 110° C. For example, when the perovskite seed crystal is an organic-inorganic material, the annealing temperature may be 60° C., 70° C., 80° C., 90° C., 95° C., 100° C., 108° C., 110° C., 120° C., 130° C., etc.

[0055] As shown in Figure 7, the perovskite seed crystal 23 is immersed in a perovskite solution 30. The perovskite solution 30 may be a solution of a dissolved perovskite material or a perovskite precursor solution. As shown in Figure 8, the perovskite seed crystal 23 is grown into a perovskite film by the action of the perovskite seed crystal 23, and the perovskite film is annealed to form a perovskite layer 24.

[0056] In order to reduce defects such as cracks, crystal boundaries, and holes in the perovskite film, the solubility of the perovskite material can be reduced in the process of growing the above-mentioned perovskite seed crystals 23 into a perovskite film. With the reduction in the solubility of the perovskite material in the perovskite solution 30, the perovskite solute in the perovskite solution 30 becomes nearly saturated or saturated, and the perovskite solute is easily precipitated from the perovskite solution 30. In this case, the perovskite solute is quickly diffused and transported to the periphery of the perovskite seed crystals 23, and the perovskite solute consumed by the precipitation of crystals around the perovskite seed crystals 23 can be timely replenished. On the basis of this, on the one hand, since the perovskite solute is timely replenished, defects such as crystal boundaries and holes can be reduced in the process of growing the perovskite film, and the density of the perovskite film can be improved. On the other hand, since the perovskite solute can be quickly transported around the perovskite seed crystals 23, the perovskite seed crystals 23 can be grown quickly and the growth rate of the perovskite film can be increased, thereby improving the production efficiency and saving the production time.

[0057] There are various ways to reduce the solubility of the perovskite material, for example, by reducing the pressure, or by reducing the temperature. When the solubility of the perovskite material is reduced by reducing the temperature, on the one hand, the temperature reduction is easy to carry out, and the process difficulty is reduced. On the other hand, the process of reducing the solubility of the perovskite material can be easily adjusted by adjusting the temperature, which allows the process of reducing the solubility of the perovskite material to have greater control.

[0058] The rate of temperature drop is positively correlated with the rate of decrease in the solubility of the perovskite material in the perovskite solution 30, while the rate of decrease in the solubility of the perovskite material is positively correlated with the growth rate of the perovskite film. Based on this, the rate of temperature drop may be 0.1°C / h to 10°C / h. In this case, the rate of decrease in the solubility of the perovskite material is appropriate, and the growth rate of the perovskite film can be accelerated while ensuring the quality of the perovskite film. This not only avoids the problem of too many defects due to the growth rate of the perovskite crystal being too fast, but also avoids the problem of reduced production efficiency due to the growth rate of the perovskite crystal being too slow.

[0059] As an example, the temperature drop rate may be 0.1°C / h, 0.5°C / h, 1°C / h, 3°C / h, 4.5°C / h, 5°C / h, 6.2°C / h, 7°C / h, 8.2°C / h, 9°C / h, 10°C / h, etc.

[0060] Before the temperature drop, the initial temperature of the perovskite solution 30 may be 100°C to 150°C. For example, the initial temperature of the perovskite solution 30 may be 100°C, 110°C, 121°C, 135°C, 146°C, 150°C, 160°C, 180°C, 192°C, 200°C, etc. In this case, since the initial temperature of the perovskite solution 30 is high, the temperature drop operation is easy to carry out, and the temperature drop cost is low. Before immersing the substrate 21 having the perovskite seed crystal 23 in the perovskite solution 30, the substrate 21 may be preheated to the initial temperature in order to keep the initial temperature of the entire system constant. According to such a perovskite film growth method, when preparing the perovskite solution 30, first, the solvent may be heated to the initial temperature, and then the perovskite solute may be added while stirring. The solvent for the perovskite solution 30 may be one or a combination of N,N-dimethylformamide (DMF, boiling point 153° C.), dimethylsulfoxide (DMSO, boiling point 189° C.), N-methylpyrrolidone (NMP, boiling point 202° C.), and γ-butyrolactone (boiling point 204° C.). A high initial temperature can provide a highly soluble perovskite solution 30, and is always lower than the boiling point of the solvent.

[0061] In order to reduce defects such as cracks, crystal boundaries, and holes in the perovskite film, the saturation of the perovskite material can be increased by accelerating the solvent evaporation in the process of growing the above-mentioned perovskite seed crystals 23 into a perovskite film. By accelerating the solvent evaporation, the perovskite solute in the perovskite solution 30 is brought to a nearly saturated state or a saturated state, and defects such as crystal boundaries and holes in the process of growing the perovskite seed crystals 23 into a perovskite film can be reduced, the density of the perovskite film can be improved, and the growth rate can be increased.

[0062] Specifically, the evaporation of the solvent can be accelerated by heating, and in this case, the rate of evaporation of the solvent can be easily adjusted by controlling the heating temperature, and thus the growth rate of the perovskite film can be adjusted.

[0063] The initial temperature of the above-mentioned perovskite solution 30 may be 20°C to 30°C, and the heating temperature during the process of growing the perovskite seed crystal 23 into a perovskite film may be 40°C to 100°C. Preferably, the heating temperature may be 50°C to 70°C. In this case, the initial temperature of the perovskite solution 30 is low, the perovskite solution 30 is easy to manufacture, and the cost is low when the solution is heated to a higher temperature. In addition, since the temperature difference between the heating temperature and the initial temperature is appropriate, the growth rate of the perovskite film can be increased and the quality of the perovskite film can be ensured. As an example, the initial temperature of the perovskite solution 30 may be 20°C, 21.5°C, 22°C, 23°C, 24.5°C, 25.1°C, 26°C, 27°C, 28°C, 29°C, 30°C, etc. The heating temperature may be 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, etc. Based on this, the perovskite solution 30 may be prepared at room temperature. After the substrate 21 having the perovskite seed crystals 23 is immersed in the perovskite solution 30, the perovskite solution 30 can be heated to accelerate the evaporation of the solvent.

[0064] The perovskite solution 30 used to grow the perovskite film may be an unsaturated solution or a saturated solution. When a saturated solution is used to grow the perovskite film, the perovskite solution 30 is a saturated solution when the perovskite seed crystal 23 is immersed in the perovskite solution 30, and the perovskite solution 30 remains saturated throughout the process of growing the perovskite film. In the saturated perovskite solution 30, the perovskite material is more easily precipitated from the perovskite solution 30, and is rapidly precipitated on the surface of the perovskite seed crystal 23 by the action of the perovskite seed crystal 23, which promotes the growth of the perovskite seed crystal 23, and a perovskite film with fewer defects and higher density is formed.

[0065] When the perovskite solution 30 is a saturated solution, the driving force for growing the perovskite film comes from the supersaturation of the solution. When the perovskite solution 30 is in a supersaturated state, the solutes in the perovskite solution 30 tend to precipitate thermodynamically. When the perovskite seed crystals 23 are present, the perovskite solutes are rapidly precipitated on the surface of the perovskite seed crystals 23 by the action of the perovskite seed crystals 23, which promotes the growth of the perovskite seed crystals 23 and forms a perovskite film.

[0066] In preparing the saturated perovskite solution 30, a predetermined amount of perovskite solute is added to the solvent while stirring, and then the mixture is stirred until the solute is completely dissolved. Next, the solute is added again, and this process is repeated until the solute does not dissolve even after stirring for 30 minutes, thereby completing the saturated perovskite solution 30.

[0067] In the process of growing the perovskite film, the perovskite solute may also precipitate on the side and back surface of the substrate 21. In such a case, the side and back surface of the substrate 21 may be coated before growing the perovskite film, or may be wiped off with a mixed solvent of acetonitrile and DMF or another polar solvent after growing the perovskite film.

[0068] As shown in Fig. 9, a hole transport layer 25 is formed on the perovskite layer 24. The material of the hole transport layer 25 may be 2,2',7,7'-tetrakis[N,N-bis(4-methoxyphenyl)amino]-9,9'-spirobifluorene (Spiro-OMeTAD), (poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] (PTAA), 2,2',7,7'-tetrakis(di-p-tolylamino)spiro-9,9'-bifluorene (Spiro-TTB), or the like. The process for forming the hole transport layer 25 is The deposition process may be any of, but is not limited to, spin coating, spray coating, magnetron sputtering process, and thermal evaporation deposition process. However, in the above-mentioned manufacturing of the perovskite solar cell, the electron transport layer 22 is manufactured first, and then the perovskite layer 24 and the hole transport layer 25 are manufactured. In some perovskite layers, the hole transport layer 25 may be manufactured first, and then the perovskite layer 24 and the electron transport layer 22 may be manufactured.

[0069] As shown in FIG. 10, a transparent conductive layer 26 is formed on the hole transport layer 25, and the material of the transparent conductive layer 26 may be one or more of tin-doped indium oxide (ITO), zinc-doped indium oxide (IZO), tungsten-doped indium oxide (IWO), titanium-doped indium oxide (ITIO), fluorine-doped tin oxide (FTO), and aluminum-doped zinc oxide (AZO). The process of forming the transparent conductive layer 26 may be a magnetron sputtering process, a thermal evaporation process, etc. However, in some perovskite layers, the transparent conductive layer 26 may be omitted.

[0070] 11, an electrode 27 is formed on the transparent conductive layer 26. Specifically, the material of the electrode 27 may be a metal with excellent conductivity, such as silver or copper. The process for manufacturing the electrode 27 may be screen printing, deposition, sputtering, or the like.

[0071] Based on the above manufacturing method, in the embodiment of the present application, the process of forming the perovskite seed crystals 23 and the process of growing the perovskite seed crystals 23 into a perovskite film are divided into two steps. First, the perovskite seed crystals 23 are formed on the substrate 21, and then the perovskite seed crystals 23 are immersed in the perovskite solution 30, and the perovskite seed crystals 23 are grown into a perovskite film by the action of the perovskite seed crystals 23. Based on this, the process of forming the perovskite seed crystals 23 can be independently adjusted to form perovskite seed crystals 23 with large crystal grain size distributed over the entire substrate 21. The action of these perovskite seed crystals 23 with large crystal grain size distributed over the entire substrate 21 can grow a perovskite film that covers the entire substrate 21, and the defects of the perovskite film can be reduced. In this case, such a perovskite film undergoes an annealing process to become a perovskite layer 24 that covers the entire substrate 21 and has fewer defects, further increasing the conversion efficiency of the perovskite layer and reducing the risk of electrical leakage.

[0072] In order to verify the performance of the perovskite solar cell manufactured by the method for manufacturing a perovskite layer according to the embodiments of the present application, a comparison between several embodiments will be described below.

[0073] <Example 1> Specifically, the method for producing the perovskite layer according to this embodiment is as follows.

[0074] First step, provide clean FTO conductive glass.

[0075] Second, an electron transport layer made of SnO2 and having a thickness of 100 nm is formed on the FTO conductive glass by spin-coating process.

[0076] In the third step, 1032 mg of FAI and 461 mg of PbI2 are dissolved in 20 ml of DMF, and the mixture is heated and stirred at 60°C for 2 h to obtain a transparent perovskite precursor solution. Here, the molar ratio of FAI:PbI2 is 6:1, and the solution concentration is 0.05 mol / L. The perovskite precursor solution is spin-coated on the electron transport layer, with a spin-coating speed of 3000 rpm and a spin-coating time of 30 s. After spin-coating, the mixture is annealed at 100°C for 10 to 20 min to volatilize the solvent and excess FAI, and discretely distributed FAPbI3 seed crystals are formed on the electron transport layer.

[0077] Step 4: Heat 50ml of DMF in a beaker and keep it at 120℃, add 0.6g of FAPbI3 perovskite to completely dissolve, and when the solution becomes clear, add another 0.6g of FAPbI3 perovskite to dissolve. Repeat the above dissolution process until no more perovskite can be dissolved, to obtain a saturated DMF solution of FAPbI3 perovskite.

[0078] The substrate with perovskite seed crystals is preheated to 120°C, and then immersed in the above 120°C saturated solution of FAPbI3 perovskite in DMF. After sealing the beaker, it is placed in a precision oven preheated to 120°C. A program is set to lower the perovskite saturated solution to room temperature at a rate of 5°C / h. The growth thickness of the perovskite film is controlled by the temperature drop width of the perovskite saturated solution. In the process of lowering from 120°C to room temperature, the amount of perovskite solute precipitated due to the difference in solubility is approximately equal to the amount of perovskite deposited on the electron transport layer. In the process of lowering the temperature, the solute in the perovskite saturated solution tends to precipitate, driven by the degree of supersaturation. Due to the action of the perovskite seed crystals, they crystallize on the surface of the perovskite seed crystals, and the perovskite seed crystals gradually grow, forming a high-quality and complete FAPbI3 perovskite film.

[0079] Fifth step, a hole transport layer made of Spiro-OMeTAD and having a thickness of 50 nm is formed on the perovskite layer by a spin-coating process.

[0080] Sixth step, a transparent conductive layer made of FTO and having a thickness of 100 nm is formed on the hole transport layer by thermal evaporation process.

[0081] Seventh step, form silver electrodes on the transparent conductive layer by deposition process.

[0082] <Example 2> The method for producing the perovskite layer according to this embodiment is almost the same as the method for producing the perovskite layer described in embodiment 1, except for the following points.

[0083] In the third step, 688 mg of FAI and 461 mg of PbI2 are added to 20 ml of DMF, and the mixture is heated and stirred at 60°C for 2 h to obtain a transparent perovskite precursor solution. Here, the molar ratio of FAI:PbI2 is 4:1, and the solution concentration is 0.05 mol / L. The perovskite precursor solution is spin-coated on the electron transport layer, with a spin-coating speed of 3000 rpm and a spin-coating time of 30 s. After spin-coating, the mixture is annealed at 105°C for 10 to 20 min to volatilize the solvent and excess FAI, and FAPbI3 seed crystals are obtained on the electron transport layer.

[0084] Step 4: Put 50ml of γ-butyrolactone into a beaker at room temperature (about 25°C), add 0.6g of FAPbI3 perovskite to completely dissolve, and when the solution becomes clear, add another 0.6g of FAPbI3 perovskite to dissolve. Repeat the above dissolution process until no more perovskite can be dissolved, and obtain a saturated solution of FAPbI3 perovskite in γ-butyrolactone. Due to the high boiling point of γ-butyrolactone, the volatilization rate of the γ-butyrolactone solvent is slow, the film growth rate is slow, and a higher quality perovskite film is obtained.

[0085] The substrate with the FAPbI3 seed crystals is immersed in the above-mentioned saturated solution of FAPbI3 perovskite in γ-butyrolactone, and the beaker is left open. The entire system (beaker) is placed in a strictly temperature-controlled environment, heated from room temperature to 60°C at a rate of 10°C / h, and kept at that temperature for 6h to 12h. During this process, the solvent in the saturated solution is constantly evaporated, the perovskite seed crystals gradually grow, and finally, a high-quality FAPbI3 perovskite film is obtained.

[0086] <Example 3> The method for producing the perovskite layer according to this embodiment is almost the same as the method for producing the perovskite layer described in embodiment 1, except for the following points.

[0087] In the third step, 259.8 mg of CsI and 461 mg of PbI2 are added to 50 ml of DMF and stirred at 80°C for 2 h to obtain a transparent and clear perovskite precursor solution. Here, the molar ratio of CsI:PbI2 is 1.05:1, and the perovskite concentration is 0.02 mol / L. The above perovskite precursor solution is spin-coated on the electron transport layer, with a spin-coating speed of 4000 rpm and a spin-coating time of 45 s. After spin-coating, the solution is annealed at 160°C for 10 min to 30 min to obtain CsPbI3 seed crystals on the electron transport layer.

[0088] Put 50ml of DMSO into a beaker and heat it to 130℃, then add 0.6g of CsPbI3 perovskite to completely dissolve it, and when the solution becomes clear, add another 0.6g of CsPbI3 perovskite and dissolve it. Repeat the above dissolution process until no more perovskite can be dissolved, to obtain a saturated DMSO solution of CsPbI3 perovskite.

[0089] The substrate with CsPbI3 seed crystals is preheated to 130℃, and then immersed in a saturated solution of CsPbI3 perovskite in DMSO, which is kept at 130℃. The beaker is sealed and placed in a precision oven preheated to 130℃. A program is set to cool the whole system to room temperature at a rate of 6℃ / h. During the cooling process, the solute in the saturated solution tends to precipitate, driven by supersaturation. Under the action of the seed crystals, the perovskite seed crystals slowly crystallize on their surfaces, and the perovskite seed crystals gradually grow, forming a high-quality and complete CsPbI3 perovskite film.

[0090] <Example 4> The method for producing the perovskite layer according to this embodiment is almost the same as the method for producing the perovskite layer described in embodiment 1, except for the following points.

[0091] In the third step, 259.8 mg of CsI and 461 mg of PbI2 are added to 50 ml of DMF and stirred at 80°C for 2 h to obtain a transparent and clear perovskite precursor solution. Here, the molar ratio of CsI:PbI2 is 1:1, and the perovskite concentration is 0.02 mol / L. The above perovskite precursor solution is spin-coated on the electron transport layer, with a spin-coating speed of 4000 rpm and a spin-coating time of 45 s. After spin-coating, the solution is annealed at 160°C for 10 to 30 min to obtain CsPbI3 seed crystals on the electron transport layer.

[0092] Put 50ml of γ-butyrolactone into a beaker at room temperature, add 0.6g of CsPbI3 perovskite and dissolve it completely. When the solution becomes clear, add another 0.6g of CsPbI3 perovskite and dissolve it. Repeat the above dissolution process until no more perovskite can be dissolved, and obtain a saturated solution of CsPbI3 perovskite in γ-butyrolactone.

[0093] The substrate with CsPbI3 seed crystals is immersed in the above-mentioned CsPbI3 perovskite gamma-butyrolactone saturated solution, and the beaker is left open. The whole system is placed in a strictly temperature-controlled environment, heated from room temperature to 70°C at a heating rate of 10°C / h, and kept at that temperature for 8-16 hours, so that the solvent in the perovskite saturated solution is constantly evaporated, the perovskite seed crystals are gradually grown, and finally, a CsPbI3 perovskite film is obtained.

[0094] <Example 5> The method for producing the perovskite layer according to this embodiment is almost the same as the method for producing the perovskite layer described in embodiment 1, except for the following points.

[0095] In the fourth step, 50 ml of DMF is heated in a beaker and kept at 120°C, 3 g of FAPbI3 perovskite is added and completely dissolved, and when the solution becomes clear, an unsaturated solution of FAPbI3 perovskite in DMF is obtained.

[0096] As a result of observing the microstructure of the perovskite layers produced in Examples 1 to 5, it was found that the perovskite layers produced in Examples 1 to 5 had few cracks, crystal boundaries, and holes in the perovskite layers and were highly dense.

[0097] Although the present application has been described herein with reference to embodiments, in the course of prosecuting the present application by practice, those skilled in the art will understand and realize other variations of the disclosed embodiments based on the drawings, the disclosure, and the appended claims.

[0098] figure As shown in FIG. 12, in a second aspect, the present application may be produced by the method for producing a perovskite layer according to any of the above examples, comprising a perovskite seed crystal and a perovskite film, comprising a first interface between the perovskite seed crystal and the perovskite film, and the first interface is observed by a high resolution scanning electron microscope. To The interface between the perovskite seed crystal and the perovskite film is more observable under high resolution scanning electron microscope. To Because a more observable first interface is formed.

[0099] As shown in Figures 13 and 14, in some possible embodiments, the first interface formed between the above-mentioned perovskite seed crystal and the perovskite film is a structural transition layer, the lattice parameters of the structural transition layer change according to a first order, and the atomic arrangement manner of the structural transition layer changes according to a second order, the first order being a order from an initial parameter to a second parameter greater than the initial parameter and then back to the initial parameter along a direction away from the perovskite seed crystal, and the second order being a order from ordered to disordered and then back to ordered along a direction away from the perovskite seed crystal. Since the lattice parameters of the structural transition layer change according to a first sequence and the atomic arrangement manner of the structural transition layer changes according to a second sequence, the concentration of defects also changes in the order of changing from an initial concentration to a second concentration greater than the initial concentration and then back to the initial concentration along the direction away from the perovskite seed crystal, so that the change of the perovskite seed crystal in the process of forming the perovskite film is more gradual, the formed first interface defects are reduced, and the sudden change of the perovskite film due to direct change is avoided.

[0100] In some possible embodiments, the thickness of the structural transition layer is greater than a certain value of atomic layer thickness, typically only 10 atomic layers thick, and the thickness of said structural transition layer 233 is 0.5 nm to 5 nm, thereby achieving a "soft transition"-like effect in the perovskite seed crystal 23 and the perovskite film 24.

[0101] It should be noted that terms such as "by way of example" or "for example" are used herein to exemplify, validate, or explain. Any embodiment or design described herein as "by way of example" or "for example" should not be construed as preferred or advantageous over other embodiments or designs. In particular, the use of "by way of example" or "for example" is intended to specifically refer to the relevant concept.

[0102] In this application, "at least one" refers to one or more, and "multiple" refers to two or more. "And / or" describes the relationship between related objects, and indicates that there may be three types of relationship, for example, A and / or B means that A exists alone, A and B exist simultaneously, and B exists alone, where A and B may be singular or plural. The symbol " / " usually indicates that the related objects before and after have an "OR" relationship. "At least one of the following" or similar expressions refers to any combination of these, and represents any combination of one or more. For example, at least one of a, b, or c may represent a, b, c, a combination of a and b, a combination of a and c, a combination of b and c, or a combination of a, b, and c, where a, b, and c may be one or more.

[0103] Although the present application has been described with reference to specific features and embodiments thereof, it is apparent that various modifications and combinations of the present application are possible without departing from the spirit and scope of the present application. In such a case, the present specification and drawings are exemplary descriptions of the present application as defined by the appended claims, and cover any and all modifications, variations, combinations or equivalents within the scope of the present application. Obviously, those skilled in the art can make various changes and modifications to the present application without departing from the spirit and scope of the present application. Thus, if these modifications and variations of the present application are within the scope of the claims of the present application and their equivalent technologies, the present application is intended to include these changes and variations. [Explanation of symbols]

[0104] In Figures 1 to 3, 11 is a substrate, 12 is an electron transport layer, 13 is a perovskite precursor solution layer, 131 is a low concentration region, 141 is a perovskite seed crystal, and 142 is a perovskite layer. In Figures 4 to 14, 21 - substrate, 22 - electron transport layer, 23 - perovskite seed crystal, 230 - AX precursor, 231 - perovskite seed crystal intermediate, 232 - first interface, 233 - structural transition layer, 24 - perovskite layer, 25 - hole transport layer, 26 - transparent conductive layer, 27 - electrode, 30 - perovskite solution.

Claims

1. Providing a substrate; preparing a perovskite precursor solution by adjusting the concentration or the compounding ratio of the perovskite precursor solution; Coating the prepared perovskite precursor solution on the substrate, volatilizing the solvent of the perovskite precursor solution to form a perovskite seed crystal intermediate, and annealing the perovskite seed crystal intermediate to form discretely distributed perovskite seed crystals; immersing the perovskite seed crystal in a perovskite solution to grow the perovskite seed crystal into a perovskite film by the guiding effect of the perovskite seed crystal; and annealing the perovskite film to form a perovskite layer. In the process of growing the perovskite seed crystals into a perovskite film, promoting precipitation of the perovskite material from the perovskite solution by reducing the solubility of the perovskite material in the perovskite solution to provide the perovskite material for the growth of the perovskite seed crystals; or A method for producing a perovskite solar cell, characterized in that in the process of growing the perovskite seed crystals into a perovskite film, precipitation of a perovskite material from the perovskite solution is promoted by accelerating solvent volatilization, thereby supplying a perovskite material for the growth of the perovskite seed crystals.

2. 2. The method for producing a perovskite solar cell according to claim 1, characterized in that the solubility of the perovskite material in the perovskite solution is reduced to promote precipitation of the perovskite material from the perovskite solution, and the solubility of the perovskite material is reduced by lowering the temperature when providing the perovskite material for growth of perovskite seed crystals.

3. The temperature drop rate is 0.1 ° C. / h to 10 ° C. / h, and / or The method for producing a perovskite solar cell according to claim 2, characterized in that the initial temperature of the perovskite solution before the temperature drop is 100°C to 150°C.

4. Accelerating the precipitation of perovskite material from the perovskite solution by accelerating solvent evaporation, and accelerating solvent evaporation by heating when providing perovskite material for the growth of perovskite seed crystals; the initial temperature of the perovskite solution is between 20° C. and 30° C.; The method for producing a perovskite solar cell according to claim 1, characterized in that in the process of growing the perovskite seed crystal into a perovskite film, the heating temperature is 40°C to 100°C.

5. The method for producing a perovskite solar cell according to any one of claims 1 to 4, characterized in that when the perovskite seed crystal is immersed in the perovskite solution, the perovskite solution is a saturated solution.

6. The method for producing a perovskite solar cell according to any one of claims 1 to 4, characterized in that the coverage of the perovskite seed crystals on the substrate is 10% to 50%, and the particle size of the perovskite seed crystals is 10 nm to 200 nm.

7. The general formula of the perovskite seed crystal is ABX 3 and The perovskite precursor solution is a mixture of AX precursor and BX 2 A precursor, wherein X is a halogen element; The perovskite seed crystal is an organic-inorganic hybrid material, and is a precursor of AX and BX 2 The mass ratio of the AX precursor to the BX precursor is (2-15):1, or the perovskite seed crystal is an all-inorganic material, and the AX precursor and the BX precursor are 2 The method for producing a perovskite solar cell according to any one of claims 1 to 4, characterized in that the mass ratio of the precursor to the perovskite solar cell is (0.95 to 1.05):

1.

8. The concentration of the perovskite precursor solution is 0.1 mol / L or less, and / or The method for producing a perovskite solar cell according to any one of claims 1 to 4, characterized in that the time for the annealing treatment for forming the perovskite seed crystals is 1 min to 30 min.

9. The perovskite seed crystal is an organic-inorganic hybrid material, and the temperature of the annealing treatment for forming the perovskite seed crystal is 60°C to 130°C; or The method for producing a perovskite solar cell according to claim 8, characterized in that the perovskite seed crystal is an all-inorganic material, and the temperature of the annealing treatment for forming the perovskite seed crystal is 120°C to 220°C.

Citation Information

Patent Citations

  • Manufacturing method of multi-stimulus response actuator and multi-stimulus response actuator

    CN109595132A

  • Solar cell, light-absorbing layer, and method for forming light-absorbing layer

    WO2018123402A1