Containers and preforms thereof

A water-soluble or alkali-soluble intermediate layer between the support and polyurethane layer in containers allows for easy separation during recycling, addressing the separation challenges of polyurethane-coated containers and improving recyclability.

JP7584012B2Active Publication Date: 2024-11-15DAI NIPPON PRINTING CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020192569
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-19
Publication Date
2024-11-15
Estimated Expiration
2040-11-19

AI Technical Summary

Technical Problem

Polyurethane coatings on containers are difficult to separate from the container body during recycling due to their water resistance, hindering effective material separation and recycling processes.

Method used

Incorporating a water-soluble or alkali-soluble intermediate layer between the support and the polyurethane protective layer, allowing for easy separation through dissolution during recycling.

Benefits of technology

Enables efficient recycling of containers by facilitating the separation of the support and protective layer, maintaining the benefits of polyurethane while enhancing recyclability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007584012000003
    Figure 0007584012000003
  • Figure 0007584012000004
    Figure 0007584012000004
  • Figure 0007584012000005
    Figure 0007584012000005
Patent Text Reader

Abstract

To provide a container including a layer containing polyurethane and having excellent recyclability.SOLUTION: The inventive container includes a support body and a protective layer provided on at least one side of the support body. The protective layer contains polyurethane, and an intermediate layer, which is a water-soluble or alkaline-soluble one, is included between the support body and the protective layer.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a container and a preform thereof. [Background technology]

[0002] Conventionally, polyurethane has been used as a coating material to be applied to the surface of containers because of its excellent heat resistance, water resistance, gas barrier properties, and the like.

[0003] For example, Patent Document 1 discloses a technique for coating the surface of a container with polyurethane. Furthermore, Patent Document 2 proposes a container coated with a polyurethane coating film for the purpose of imparting gas barrier properties, water resistance, film adhesion, and the like, and a preform thereof.

[0004] In recent years, used containers have been recycled in order to reduce the environmental load, such as by reducing carbon dioxide emissions. Recycling must be done with the same type of material, so for example, when recycling used PET bottles, the collected PET bottles must be separated into the label, cap, and bottle body. In addition, when the bottle body has a multi-layer structure, for example, when the bottle body has a support and a coating layer provided on the surface of the support, it must be separated into the support and the coating layer. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2000-102763 A [Patent Document 2] JP 2014-46678 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, because polyurethane has excellent water resistance and film adhesion, containers such as bottles having a support and a layer containing polyurethane cannot be easily separated from each other, making recycling difficult.

[0007] Therefore, an object of the present invention is to provide a container that has a layer containing polyurethane and has excellent recyclability, and a preform of the container. [Means for solving the problem]

[0008] The present inventors have now discovered that the above object can be achieved by providing a water-soluble or alkali-soluble intermediate layer between a support and a layer containing polyurethane. The present invention has been made in view of the above findings.

[0009] The present invention provides a container comprising a support and a protective layer provided on at least one surface side of the support, the protective layer comprises polyurethane; The container further comprises a water-soluble or alkali-soluble intermediate layer between the support and the protective layer.

[0010] In the container according to the present invention, the polyurethane may be a reaction product of a polyurethane polyol and an organic polyisocyanate.

[0011] In the container according to the present invention, the polyurethane polyol may have a carboxy group in the molecule.

[0012] In the container according to the present invention, the protective layer may have a thickness of 0.1 μm or more and 200.0 μm or less.

[0013] In the container according to the present invention, the intermediate layer may contain a carboxy group-containing resin and a polyvinyl alcohol-based resin.

[0014] In the container according to the present invention, the mass ratio of the carboxyl group-containing resin to the polyvinyl alcohol resin may be 1 / 20 or more and 10 / 1 or less.

[0015] In the container according to the present invention, the support may comprise polyester.

[0016] The present invention relates to a preform of the container. Effect of the Invention

[0017] According to the present invention, it is possible to provide a container which has a layer containing polyurethane and has excellent recyclability, and a preform of this container. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1 is a schematic half-sectional view showing one embodiment of a bottle, which is an example of a container of the present invention. [Diagram 2] FIG. 1 is a schematic half-sectional view showing one embodiment of a bottle, which is an example of a container of the present invention. [Diagram 3] FIG. 1 is a schematic half-sectional view showing one embodiment of a bottle, which is an example of a container of the present invention. [Figure 4] FIG. 1 is a schematic half sectional view showing an embodiment of a preform, which is an example of a preform of the present invention. [Diagram 5] FIG. 1 is a schematic half sectional view showing an embodiment of a preform, which is an example of a preform of the present invention. [Figure 6] FIG. 1 is a schematic half sectional view showing an embodiment of a preform, which is an example of a preform of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] <Container> The container of the present invention includes a support and a protective layer provided on at least one surface of the support. In the container of the present invention, the protective layer contains polyurethane. The container of the present invention also includes an intermediate layer that is water-soluble or alkali-soluble between the support and the protective layer. In this specification, the term "container" refers to a molded body that contains an article. Examples of the container include molded bodies such as compression molded bodies, injection molded bodies, blow molded bodies, and thermoformed bodies. Specific examples of the container include bottles, vials, cups, trays, and packs.

[0020] First, the reason why the container having the above-mentioned structure can have advantageous physical properties due to polyurethane and excellent recyclability will be described. Since polyurethane has heat resistance, water resistance, scratch resistance, stretchability, etc., when it is coated on the surface of a support (container body), it forms a crack-free uniform film that conforms to the shape of the container, and can improve the heat resistance, water resistance, scratch resistance, etc. of the container. On the other hand, since recycling is performed for each material, if the surface of the container body is coated, it is necessary to separate the container body from the coating layer. This separation method includes chemical separation methods such as dissolution and physical separation methods such as peeling. However, since the polyurethane coating has water resistance, it is difficult to separate by dissolution. In addition, it is time-consuming and costly to separate the container body and the polyurethane coating by peeling. The container of the present invention is suitable for recycling because the support and the protective layer containing polyurethane can be easily separated from each other after use by providing a water-soluble or alkali-soluble intermediate layer between the support and the protective layer. That is, in a container whose surface is coated with a resin such as polyurethane, it is difficult to separate the container body and the protective layer, and it is difficult to recycle the container body. However, according to the container of the present invention, the intermediate layer dissolves when the container is crushed and washed after use, so that the container body and the protective layer can be easily separated. The recycling method is not particularly limited, but the following method can be exemplified. First, used containers are collected, and bottle caps and container bodies are sorted according to the type of material they are made of, and the container bodies are crushed into flakes. The flakes are washed with water or an alkaline solution, or a heated version of these if necessary, to remove dirt and foreign matter from the flake surface, and the intermediate layer is dissolved to peel off the protective layer from the support. The resulting flakes of the support are treated for a certain period of time by high-temperature drying, reduced-pressure drying, centrifugation, or the like, and then the support and protective layer are separated by air sorting, and the support is collected. Note that air sorting allows the materials that make up the support to be efficiently collected.

[0021] Hereinafter, each of the components that the container of the present invention may have will be described.

[0022] (Support) In the container of the present invention, the support is capable of maintaining the shape of the container. In one embodiment, the support contains a thermoplastic resin. Examples of the thermoplastic resin contained in the support include polyolefins such as polyethylene and polypropylene, polyesters such as polycarbonate, polyvinyl chloride, and polyethylene terephthalate, polyamides such as nylon 6 and nylon 6,6, and mixtures thereof. Among these, from the viewpoints of gas barrier properties and strength, the support preferably contains polyester. From the viewpoint of recyclability, the support preferably contains polyethylene terephthalate.

[0023] In this specification, the term "polyester" refers to a polymer that is polymerized through ester bonds. Such polyesters are usually obtained by polycondensation of a dicarboxylic acid compound and a diol compound. Examples of dicarboxylic acid compounds include malonic acid, succinic acid, glutaric acid, adipic acid, suberic acid, sebacic acid, dodecanedioic acid, eicosanedioic acid, pimelic acid, azelaic acid, methylmalonic acid, ethylmalonic acid, adamantanedicarboxylic acid, norbornenedicarboxylic acid, cyclohexanedicarboxylic acid, decalindicarboxylic acid, terephthalic acid, isophthalic acid, phthalic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 1,8-naphthalenedicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 4,4'-diphenyletherdicarboxylic acid, 5-sodiumsulfoisophthalic acid, phenylendanedicarboxylic acid, anthracenedicarboxylic acid, phenanthrenedicarboxylic acid, 9,9'-bis(4-carboxyphenyl)fluorene acid, and ester derivatives thereof. Examples of the diol compound include ethylene glycol, 1,2-propanediol, 1,3-propanediol, butanediol, 2-methyl-1,3-propanediol, hexanediol, neopentyl glycol, cyclohexanedimethanol, cyclohexanediethanol, decahydronaphthalenedimethanol, decahydronaphthalenediethanol, norbornanedimethanol, norbornanediethanol, tricyclodecanedimethanol, tricyclodecaneethanol, tetracyclododecanedimethanol, tetracyclododecanediethanol, decalindimethanol, decalindiethanol, and 5-methylol-5-ethyl -2-(1,1-dimethyl-2-hydroxyethyl)-1,3-dioxane, cyclohexanediol, bicyclohexyl-4,4'-diol, 2,2-bis(4-hydroxycyclohexylpropane), 2,2-bis(4-(2-hydroxyethoxy)cyclohexyl)propane, cyclopentanediol, 3-methyl-1,2-cyclopentadiol, 4-cyclopentene-1,3-diol, adamantanediol, paraxylene glycol, bisphenol A, bisphenol S, styrene glycol, trimethylolpropane, pentaerythritol, and bis-β-hydroxyethyl terephthalate (BHET). The polyester is preferably polyethylene terephthalate or a modified polyethylene terephthalate obtained by polymerizing a raw material monomer of polyethylene terephthalate and a copolymerizable monomer.

[0024] From the viewpoint of recyclability, the content of one type of thermoplastic resin in the support is preferably 90% by mass or more, and more preferably 97% by mass or more.

[0025] The support may contain additives within the range that does not impair the characteristics of the present invention. Examples of additives include oxygen absorbers, plasticizers, ultraviolet stabilizers, antioxidants, matting agents, deodorants, flame retardants, weather resistance agents, antistatic agents, friction reducers, slip agents, mold release agents, antioxidants, and ion exchange agents. These additives can be used alone or in combination of two or more.

[0026] The support may be a single-layer structure or a multi-layer structure having two or more layers. When the support is a multi-layer structure, each layer may have the same composition or different compositions as long as the characteristics of the present invention are not impaired.

[0027] The cross-sectional thickness of the support is preferably 0.01 mm or more and 0.35 mm or less, and more preferably 0.05 mm or more and 0.25 mm or less. The cross-sectional thickness of the support can be measured, for example, at the body of the container. The cross-sectional thickness of the support means the point where the cross-sectional thickness is the thinnest.

[0028] The support is preferably subjected to a surface treatment. Examples of the surface treatment include corona treatment, low-temperature plasma treatment, and flame treatment. By performing such a surface treatment, the wettability of the support surface is improved, and the adhesion between the support and a layer in contact with the support can be improved.

[0029] (protective layer) In the container of the present invention, the protective layer contains polyurethane. This makes it possible to provide the container with heat resistance, water resistance, etc. Therefore, the container of the present invention can be suitably used as a heating container, for example, a bottle. The protective layer may contain one or more types of polyurethane, which will be described later.

[0030] In the container of the present invention, the polyurethane can be obtained by a known method, and the production method is not limited. The polyurethane is, for example, a reaction product generated by reacting an organic polyol with an organic polyisocyanate (urethanization reaction).

[0031] The organic polyol may be a compound having a functional group number in one molecule of preferably 2 to 6, more preferably 2 to 4, and a number average molecular weight of preferably 500 to 100,000, more preferably 1,000 to 30,000. More specifically, polyester polyol, polyether polyol, polyether ester polyol, polyester amide polyol, acrylic polyol, polycarbonate polyol, polyhydroxyl alkane, polyurethane polyol, castor oil, or a mixture thereof (hereinafter, these may be referred to as organic polyol (1)). Among these, the organic polyol is preferably polyurethane polyol. In the present specification, the number average molecular weight can be measured by gel permeation chromatography (GPC). In GPC measurement, the number average molecular weight of a polymer is generally measured in terms of standard polystyrene.

[0032] Examples of polyester polyols include polyester polyols obtained by reacting dibasic acids such as terephthalic acid, isophthalic acid, adipic acid, azelaic acid, and sebacic acid, or dialkyl esters thereof, or mixtures thereof, with glycols such as ethylene glycol, propylene glycol, diethylene glycol, butylene glycol, neopentyl glycol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, 3,3'-dimethylolheptane, polyoxyethylene glycol, polyoxypropylene glycol, and polytetramethylene ether glycol, or mixtures thereof. Examples of polyester polyols include polyester polyols obtained by ring-opening polymerization of lactones such as polycaprolactone, polyvalerolactone, and poly(β-methyl-γ-valerolactone).

[0033] Examples of polyether polyols include polyether polyols obtained by polymerizing an oxirane compound such as ethylene oxide, propylene oxide, butylene oxide, or tetrahydrofuran using a low molecular weight polyol such as water, ethylene glycol, propylene glycol, trimethylolpropane, or glycerin as an initiator.

[0034] Examples of polyether ester polyols include polyether ester polyols obtained by reacting a dibasic acid such as terephthalic acid, isophthalic acid, adipic acid, azelaic acid, or sebacic acid, or a dialkyl ester thereof, or a mixture thereof, with the above-mentioned polyether polyol.

[0035] Examples of polyesteramide polyols include polyesteramide polyols obtained by mixing an aliphatic diamine having an amino group, such as ethylenediamine, propylenediamine, or hexamethylenediamine, with the raw materials in the esterification reaction.

[0036] Examples of acrylic polyols include acrylic polyols obtained by copolymerizing hydroxyethyl acrylate, hydroxypropyl acrylate, hydroxybutyl acrylate, etc., which contain one or more hydroxyl groups in one molecule, or corresponding methacrylic acid derivatives thereof, with, for example, acrylic acid, methacrylic acid, or an ester thereof.

[0037] Examples of polycarbonate polyols include polycarbonate polyols obtained by reacting one or more glycols selected from ethylene glycol, propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, 1,9-nonanediol, 1,8-nonanediol, neopentyl glycol, diethylene glycol, dipropylene glycol, 1,4-cyclohexanediol, 1,4-cyclohexanedimethanol, bisphenol A, and hydrogenated bisphenol A with dimethyl carbonate, diphenyl carbonate, ethylene carbonate, phosgene, or the like.

[0038] The polyhydroxyalkane is butadiene, or butadiene and acrylamide, etc. Examples of the liquid rubber include those obtained by copolymerization.

[0039] The polyurethane polyol is a polyol having a urethane bond in one molecule, and examples thereof include polyurethane polyols obtained by reacting a polyol such as a polyether polyol, a polyester polyol, or a polyether ester polyol having a number average molecular weight of 200 to 20,000 with an organic polyisocyanate so that the ratio of isocyanate groups to hydroxyl groups (NCO / OH) is less than 1, preferably 0.9 or less. In the polyurethane polyol, the polyol used is preferably a polyester polyol having a number average molecular weight of 200 to 20,000. Such a polyurethane polyol may be referred to as a polyester polyurethane polyol.

[0040] As the organic polyol, one having a carboxy group in its molecule (inside the molecule or at the molecular end) (hereinafter referred to as organic polyol (2)) can be used. The organic polyol (2) is preferably obtained by reacting the above organic polyol (1) with a polybasic acid or anhydride thereof. The organic polyol (1) used in this case is one containing two or more hydroxyl groups at the molecular end and having a number average molecular weight of preferably 1,000 to 100,000, more preferably 3,000 to 15,000.

[0041] Examples of polybasic acids or their anhydrides include aromatic polybasic acids such as phthalic acid, trimellitic acid, pyromellitic acid, etc., and their anhydrides, and particularly preferred are their anhydrides, such as phthalic anhydride, trimellitic anhydride, pyromellitic anhydride, etc. Furthermore, ethylene glycol bisanhydrotrimellitate, glycerol trisanhydrotrimellitate, ethylene glycol bisanhydropyromellitate, glycerol trisanhydropyromellitate, which are derived from these anhydrides, abietic acid, which is a rosin component, C10H16 diene compounds, and derivatives obtained by addition reaction of maleic anhydride with the mixtures thereof, etc., can be used.

[0042] The synthesis of the organic polyol (2) is carried out by adding a polybasic acid or an anhydride thereof, preferably a polybasic acid anhydride, under heating after the synthesis of the organic polyol (1). During the synthesis of the organic polyol, it is possible to obtain an organic polyol containing a carboxyl group inside or at the molecular end in a single step from a polybasic carboxylic acid and a polyhydric alcohol.

[0043] The organic polyisocyanate has two or more isocyanate groups in one molecule. Examples of the organic polyisocyanate include aliphatic diisocyanates such as linear alkylene diisocyanates such as trimethylene diisocyanate, tetramethylene diisocyanate, and hexamethylene diisocyanate, and branched alkylene diisocyanates such as 1,2-propylene diisocyanate, 1,2-butylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, and 2,2,4-trimethylhexamethylene diisocyanate. Isocyanates; alicyclic diisocyanates such as 1,4-cyclohexane diisocyanate, 1,3-cyclohexane diisocyanate, 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate, 4,4'-methylenebis(cyclohexyl isocyanate), methyl 2,4-cyclohexane diisocyanate, methyl 2,6-cyclohexane diisocyanate, 1,4-bis(isocyanatomethyl)cyclohexane, and 1,3-bis(isocyanatomethyl)cyclohexane; m-phenylene Aromatic diisocyanates such as 1,3- or 1,4-xylylene diisocyanate or mixtures thereof, ω,ω'-diisocyanate, 1,5-naphthalene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4- or 2,6-tolylene diisocyanate or mixtures thereof, 4,4'-toluidine diisocyanate, dianisidine diisocyanate, 4,4'-diphenylether diisocyanate, etc. aromatic aliphatic diisocyanates such as 1,4-diethylbenzene, 1,3- or 1,4-bis(1-isocyanato-1-methylethyl)benzene or mixtures thereof; organic triisocyanates such as triphenylmethane-4,4',4"-triisocyanate, 1,3,5-triisocyanatobenzene, 2,4,6-triisocyanatotoluene, and polyisocyanate monomers such as organic tetraisocyanates such as 4,4'-diphenyldimethylmethane-2,2'-5,5'-tetraisocyanate. In addition to the above monomers, examples of organic polyisocyanates include dimers, trimers, biurets, and allophanates derived from the above polyisocyanate monomers; polyisocyanates having a 2,4,6-oxadiazinetrione ring obtained from carbon dioxide gas and the above polyisocyanate monomers; ethylene glycol, propylene glycol, butylene glycol, hexylene glycol, neopentyl glycol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, 3,3'-dimethylolpropane, cyclohexanedimethanol, diethylene glycol, triethylene glycol, and the like. Examples of the polyisocyanate monomer include adducts of low-molecular-weight polyols having a molecular weight of less than 200, such as ethylene glycol, dipropylene glycol, glycerol, trimethylolpropane, pentaerythritol, and sorbitol, and the above-mentioned polyisocyanate monomers; and adducts of polyester polyols, polyether ester polyols, polyester amide polyols, polycaprolactone polyols, polyvalerolactone polyols, acrylic polyols, polycarbonate polyols, polyhydroxy alkanes, castor oil, polyurethane polyols, and the like having a molecular weight of 200 or more and 20,000 or less, and the above-mentioned polyisocyanate monomers. The organic polyisocyanates mentioned above may be used alone or as a mixture of two or more kinds. In one embodiment, the organic polyisocyanate is preferably an adduct as described above, more preferably an adduct of a monomeric polyisocyanate with a polyurethane polyol.

[0044] In the urethanization reaction, at least one selected from the group consisting of a silane coupling agent, a phosphorus oxyacid, and a derivative of a phosphorus oxyacid may be further used.

[0045] As the silane coupling agent, for example, those represented by the following general formula (I) or (II) can be used. R-Si≡(X)3····(I) R-Si≡(R')(X)2 (II) In formulas (I) and (II), R represents an organic group having a vinyl group, an epoxy group, an amino group, an imino group or a mercapto group, R' represents a lower alkyl group, and X represents a methoxy group, an ethoxy group or a chlorine atom. Examples of the silane coupling agent include chlorosilanes such as vinyltrichlorosilane, aminosilanes such as N-(dimethoxymethylsilylpropyl)ethylenediamine and N-(triethoxysilylpropyl)ethylenediamine, epoxysilanes such as γ-glycidoxypropyltrimethoxysilane and γ-glycidoxypropyltriethoxysilane, vinylsilanes such as vinyltriethoxysilane, etc. The amount of the silane coupling agent added is preferably 0.1% by mass or more and 5% by mass or less based on the polyurethane obtained.

[0046] Among the phosphorus oxygen acids or derivatives thereof, the phosphorus oxygen acid may be any one having at least one free oxygen acid, and examples thereof include phosphoric acids such as hypophosphorous acid, phosphorous acid, orthophosphoric acid, and hypophosphoric acid, and condensed phosphoric acids such as metaphosphoric acid, pyrophosphoric acid, tripolyphosphoric acid, polyphosphoric acid, and ultraphosphoric acid. Examples of the derivatives of phosphorus oxygen acids include those obtained by partially esterifying the above phosphorus oxygen acids with alcohols while leaving at least one free oxygen acid. Examples of these alcohols include aliphatic alcohols such as methanol, ethanol, ethylene glycol, and glycerin, and aromatic alcohols such as phenol, xylenol, hydroquinone, catechol, and phloroglucinol. One or more types of phosphorus oxygen acids or derivatives thereof may be used. The amount of phosphorus oxygen acid or derivatives thereof added is 0.01% by mass to 10% by mass, preferably 0.05% by mass to 5% by mass, and more preferably 0.1% by mass to 1% by mass, based on the polyurethane obtained.

[0047] In one embodiment, the polyurethane is a polyurethane polyol, preferably a reaction product of a polyurethane polyol having a carboxy group in the molecule and an organic polyisocyanate. The organic polyisocyanate is preferably an adduct of a polyisocyanate monomer and a polyurethane polyol. By making the polyurethane into such a reaction product, the heat resistance of the container can be further improved.

[0048] In one embodiment, the polyurethane may be a reaction product of a polyester polyol and two or more organic polyisocyanates, at least one of which may be a linear alkylene diisocyanate. The linear alkylene diisocyanate may be hexamethylene diisocyanate.

[0049] The protective layer may contain additives within the range that does not impair the characteristics of the present invention. Examples of additives include oxygen absorbers, plasticizers, ultraviolet stabilizers, antioxidants, matting agents, deodorants, flame retardants, weather resistance agents, antistatic agents, friction reducers, slip agents, release agents, antioxidants, and ion exchange agents. These additives can be used alone or in combination of two or more.

[0050] The protective layer may be a single layer or a multi-layer consisting of two or more layers. When the protective layer is a multi-layer, each layer may have the same composition or different compositions.

[0051] The thickness of the protective layer is preferably 0.1 μm or more and 200 μm or less, and more preferably 0.7 μm or more and 70 μm or less. The thickness of the protective layer can be measured, for example, at the body of the container. The thickness of the protective layer means the part where the thickness is the thinnest. When the protective layer has multiple layers, the thickness of the protective layer is the sum of the thicknesses of all the layers.

[0052] The protective layer may be colored in red, blue, yellow, green, brown, brownish-brown, orange, black, white, or the like, and may be transparent or opaque. The colored protective layer can absorb visible light entering the container from the outside, such as sunlight, and can suppress changes in taste and color of the contents of the container. In particular, when the contents are beer, a container having such a protective layer is less susceptible to visible light having a wavelength of 400 nm or more and 500 nm or less passing through the container, and therefore can suppress the problem that the bitter components in the beer are decomposed by sunlight to produce 3-methyl-2-butene-1-thiol, which is a sunlight odor component. Since the protective layer can effectively absorb visible light having a wavelength of 400 nm or more and 500 nm or less, it is preferably colored in brown or orange. For example, a coloring agent can be used to color the protective layer.

[0053] (Middle class) In the container of the present invention, the intermediate layer is water-soluble or alkali-soluble, which allows the container to have excellent recyclability. The reason for this is as follows. In recycling used containers, the containers are first crushed into flakes, and then washed with liquids such as water and an alkaline solution. If a water-soluble or alkaline-soluble intermediate layer is present between the support and the protective layer, the intermediate layer dissolves in this washing step, and the protective layer can be peeled off from the support to separate the support. Therefore, such containers have excellent recyclability. The intermediate layer may be a layer that is both water-soluble and alkaline-soluble. In this specification, "water-soluble" means that the intermediate layer is soluble in distilled water at 20°C at a concentration of 3% by mass or more, preferably 10% by mass or more, and more preferably 20% by mass or more. In this specification, "alkali soluble" means that the intermediate layer dissolves in a 1.5 mass % aqueous sodium hydroxide solution at 90°C to a degree of 3 mass % or more, preferably 10 mass % or more, and more preferably 20 mass % or more.

[0054] The intermediate layer is preferably a layer having light-shielding properties, glossiness, color, gas barrier properties, etc. depending on the application of the container. The intermediate layer is particularly preferably a barrier layer having gas barrier properties.

[0055] In one embodiment, the intermediate layer contains a polyvinyl alcohol-based resin. The polyvinyl alcohol-based resin is a resin that is water-soluble or alkali-soluble, and has a high cohesive force, so that it has a high effect of blocking oxygen and water vapor (gas barrier property). By containing a polyvinyl alcohol-based resin, the intermediate layer can be made water-soluble or alkali-soluble, and the gas barrier property of the container can be improved.

[0056] In one embodiment, the intermediate layer includes a carboxy group-containing resin and a polyvinyl alcohol-based resin. As described above, by including a polyvinyl alcohol-based resin in the intermediate layer, the intermediate layer can be made water-soluble or alkali-soluble, and the gas barrier properties of the container can be improved. In addition, the intermediate layer contains a carboxyl group-containing resin, which improves the water solubility or alkali solubility of the intermediate layer, thereby improving the recyclability of the container. Furthermore, the carboxyl group of the carboxyl group-containing resin forms a hydrogen bond with the polyvinyl alcohol resin or the "-OH" of the solvent of the coating liquid used to form the intermediate layer (e.g., water and an organic solvent having a hydroxyl group, etc.), thereby increasing the viscosity of the coating liquid. This allows the thickness of the intermediate layer to be increased with fewer coating cycles, thereby improving the productivity of the container.

[0057] The polyvinyl alcohol resin and the carboxyl group-containing resin will be described below.

[0058] Polyvinyl alcohol resins (also called "PVA resins") are resins that contain alcoholic hydroxyl groups in the polymer structure. PVA resins are usually obtained by saponifying vinyl ester polymers.

[0059] Vinyl ester polymers are usually obtained by polymerizing vinyl ester monomers as polymerization components. Examples of vinyl ester monomers include fatty acid vinyl esters such as vinyl acetate, vinyl propionate, vinyl butyrate, vinyl caprylate, vinyl versatate, and vinyl monochloroacetate, and aromatic carboxylic acid vinyl esters such as vinyl arene carboxylates (e.g., C7-12 arene carboxylic acid vinyl esters) such as vinyl benzoate. These monomers can be used alone or in combination of two or more.

[0060] The vinyl ester polymer may have a unit derived from another polymerizable monomer (monomer copolymerizable with vinyl ester). Examples of other polymerizable monomers include ethylene; α-olefins such as propylene, 1-butene, 1-pentene, 1-hexene, and 1-octene; methacrylic acid alkyl esters such as methyl methacrylate and ethyl methacrylate; chlorine-containing vinyl monomers such as vinyl chloride and vinylidene chloride; fluorine-containing vinyl monomers such as vinyl fluoride and vinylidene fluoride; unsaturated nitriles such as acrylonitrile and methacrylonitrile; aromatic vinyl monomers such as styrene and α-methylstyrene; and itaconic acid alkyl esters. These monomers can be used alone or in combination of two or more.

[0061] The PVA-based resin may be one in which a part of the vinyl alcohol units has been modified by a reaction such as acetalization, etherification, acetoacetylation, or cationization.

[0062] The degree of polymerization of the PVA-based resin is preferably 1,000 or more and 4,000 or less, more preferably 1,500 or more and 3,500 or less, and further preferably 2,000 or more and 3,000 or less. The average degree of polymerization of the PVA resin can be measured in accordance with JIS K 6726:1994.

[0063] From the viewpoints of excellent solubility in a solvent and excellent storage stability of the composition, the saponification degree of the PVA-based resin is preferably 70 mol% or more and 99.9 mol% or less, more preferably 90 mol% or more and 99.5 mol% or less, and even more preferably 95 mol% or more and 99.5 mol% or less. The degree of saponification of the PVA-based resin can be measured in accordance with JIS K 6726:1994.

[0064] The PVA-based resin has an aqueous solution viscosity of preferably 3 mPa·s or more and 70 mPa·s or less, more preferably 50 mPa·s or more and 68 mPa·s or less, and more preferably 54 mPa·s or more and 66 mPa·s or less, when the PVA-based resin is dissolved in pure water to give a concentration of 4 mass %. The viscosity of the coating liquid can be measured at a temperature of 20° C. in accordance with JIS Z 8803:2011.

[0065] The PVA-based resins can be used alone or in combination of two or more.

[0066] The carboxyl group-containing resin may be an existing carboxyl group-containing resin. The existing carboxyl group-containing resin is a general term for resins that contain a carboxyl group in the polymer structure. Examples of the carboxyl group-containing resin include homopolymers of carboxyl group-containing unsaturated monomers, copolymers of carboxyl group-containing unsaturated monomers, copolymers of carboxyl group-containing unsaturated monomers and other polymerizable monomers, and polysaccharides containing a carboxyl group in the molecule (also called "acidic polysaccharides"). These carboxyl group-containing resins may be used alone or in combination of two or more. The carboxy group includes not only a free carboxy group but also an acid anhydride group (specifically, a dicarboxylic acid anhydride group). The acid anhydride group may be partially opened to form a carboxy group. In the carboxy group-containing resin, a part of the carboxy group may be neutralized with an alkali.

[0067] The carboxyl group-containing unsaturated monomer is preferably an α,β-monoethylenically unsaturated carboxylic acid. Therefore, the carboxyl group-containing resin includes a homopolymer of an α,β-monoethylenically unsaturated carboxylic acid, a copolymer of two or more kinds of α,β-monoethylenically unsaturated carboxylic acids, and a copolymer of an α,β-monoethylenically unsaturated carboxylic acid and another polymerizable monomer. The other polymerizable monomer may be an ethylenically unsaturated monomer.

[0068] Examples of α,β-monoethylenically unsaturated carboxylic acids include unsaturated monocarboxylic acids such as acrylic acid, methacrylic acid, crotonic acid, etc., unsaturated dicarboxylic acids such as maleic acid, fumaric acid, itaconic acid, etc., unsaturated dicarboxylic anhydrides such as maleic anhydride, itaconic anhydride, etc. These acids can be used alone or in combination of two or more. The α,β-monoethylenically unsaturated carboxylic acid is preferably selected from one or more of acrylic acid, methacrylic acid, crotonic acid, maleic acid, fumaric acid, and itaconic acid, and more preferably selected from one or more of acrylic acid, methacrylic acid, and maleic acid.

[0069] Examples of other polymerizable monomers copolymerizable with α,β-monoethylenically unsaturated carboxylic acids, particularly ethylenically unsaturated monomers, include ethylene; α-olefins such as propylene, 1-butene, 1-pentene, 1-hexene, and 1-octene; saturated carboxylic acid vinyl esters such as vinyl acetate; acrylic acid alkyl esters such as methyl acrylate and ethyl acrylate; methacrylic acid alkyl esters such as methyl methacrylate and ethyl methacrylate; chlorine-containing vinyl monomers such as vinyl chloride and vinylidene chloride; fluorine-containing vinyl monomers such as vinyl fluoride and vinylidene fluoride; unsaturated nitriles such as acrylonitrile and methacrylonitrile; aromatic vinyl monomers such as styrene and α-methylstyrene; itaconic acid alkyl esters, etc. These monomers can be used alone or in combination of two or more.

[0070] Examples of the carboxyl group-containing polysaccharides include acidic polysaccharides having a carboxyl group in the molecule, such as alginic acid, carboxymethylcellulose, and pectin. These acidic polysaccharides can be used alone or in combination of two or more. The acidic polysaccharides can be used in combination with a (co)polymer of an α,β-monoethylenically unsaturated carboxylic acid.

[0071] When the carboxyl group-containing resin used in the present invention is a copolymer of an α,β-monoethylenically unsaturated carboxylic acid and another ethylenically unsaturated monomer, the composition of the copolymer is such that the composition of the α,β-monoethylenically unsaturated carboxylic acid monomer is preferably 60 mol % or more, more preferably 80 mol % or more, and even more preferably 90 mol % or more.

[0072] The carboxyl group-containing resin is preferably a homopolymer or copolymer obtained by polymerization of only α,β-monoethylenically unsaturated carboxylic acid. When the polycarboxylic acid polymer is a (co)polymer consisting of only α,β-monoethylenically unsaturated carboxylic acid, the carboxyl group-containing resin is preferably a homopolymer, copolymer, or mixture of two or more thereof obtained from a carboxylic acid selected from one or more of acrylic acid, methacrylic acid, crotonic acid, maleic acid, fumaric acid, and itaconic acid, and more preferably a homopolymer, copolymer, or mixture of two or more thereof obtained from a carboxylic acid selected from one or more of acrylic acid, methacrylic acid, and maleic acid.

[0073] The carboxyl group-containing resin is preferably one or more selected from polyacrylic acid, polymethacrylic acid, and maleic acid polymers. The carboxyl group-containing resin is preferably polyacrylic acid, which is relatively easy to obtain and has good recyclability and gas barrier properties.

[0074] The number average molecular weight of the carboxyl group-containing resin is preferably in the range of 2,000 to 10,000,000, more preferably in the range of 5,000 to 1,000,000, and even more preferably in the range of 10,000 to 500,000.

[0075] When the intermediate layer contains a carboxy group-containing resin and a vinyl alcohol-based resin, the mass ratio of the carboxy group-containing resin to the polyvinyl alcohol-based resin (carboxy group-containing resin / polyvinyl alcohol-based resin) is preferably 1 / 20 or more and 10 / 1 or less, more preferably 1 / 15 or more and 5 / 1 or less, and even more preferably 1 / 10 or more and 2 / 1 or less. By setting the mass ratio at 1 / 20 or more, the recyclability of the container can be further improved. By setting the mass ratio to 10 / 1 or less, the gas barrier properties of the container can be further improved. The above mass ratio is a solid content ratio.

[0076] When the intermediate layer contains a carboxy group-containing resin and a vinyl alcohol resin, the content of the carboxy group-containing resin is preferably 1 mass% or more and 80 mass% or less, more preferably 2 mass% or more and 70 mass% or less, and even more preferably 5 mass% or more and 60 mass% or less, based on all components contained in the intermediate layer. By setting the content of the carboxyl group-containing resin to 1% by mass or more, the recyclability of the container can be further improved. By setting the content of the carboxyl group-containing resin to 80 mass % or less, the gas barrier property of the container can be further improved.

[0077] When the intermediate layer contains a carboxy group-containing resin and a polyvinyl alcohol-based resin, the content of the polyvinyl alcohol-based resin is preferably 20% by mass or more and 99% by mass or less, more preferably 30% by mass or more and 98% by mass or less, and even more preferably 40% by mass or more and 95% by mass or less, based on all components contained in the intermediate layer. By setting the content of the polyvinyl alcohol-based resin to 20% by mass or more, the gas barrier property of the container can be further improved. By setting the content of the polyvinyl alcohol-based resin to 99% by mass or less, the recyclability of the container can be further improved.

[0078] In another embodiment, the intermediate layer includes a reaction product of a carboxyl group-containing resin and a polyvalent metal compound. Even if the intermediate layer is configured in this manner, the intermediate layer can be water-soluble or alkali-soluble, and the container can have improved gas barrier properties.

[0079] The polyvalent metal compound will be described below. The carboxyl group-containing resin may be the same as that described above.

[0080] The polyvalent metal compound refers to a simple polyvalent metal atom having a metal ion with a valence of two or more, and a compound thereof.

[0081] Examples of polyvalent metals include beryllium, magnesium, calcium, barium, titanium, zirconium, chromium, manganese, iron, cobalt, nickel, copper, zinc, aluminum, etc. These polyvalent metals can be used alone or in combination of two or more. The polyvalent metal is preferably selected from one or more of magnesium, calcium, and zinc. By selecting one or more of these polyvalent metals, the intermediate layer can be made transparent, so that the container can be given various designs and can be made into a container with rich designability. The polyvalent metal is particularly preferably magnesium.

[0082] Examples of polyvalent metal compounds include oxides, hydroxides, organic acid salts, inorganic acid salts, and other compounds such as ammonium complexes of polyvalent metals, secondary to quaternary amine complexes of polyvalent metals, and organic acid salts and inorganic acid salts of these complexes. Examples of organic acid salts include acetates, oxalates, citrates, lactates, stearates, and monoethylenically unsaturated carboxylates. Examples of inorganic acid salts include chlorides, nitrates, carbonates, sulfates, phosphates, phosphites, and hypophosphites. Other examples include alkyl alkoxides of polyvalent metals. These compounds can be used alone or in combination of two or more. The polyvalent metal compound is preferably selected from one or more of chlorides, nitrates, sulfates, phosphates, phosphites and hypophosphites, and more preferably is a chloride, a nitrate, or a mixture thereof.

[0083] When the intermediate layer contains a reaction product of a carboxy group-containing resin and a polyvalent metal compound, the amount of the polyvalent metal compound is preferably 0.05 chemical equivalents or more and 5.00 chemical equivalents or less, more preferably 0.1 chemical equivalents or more and 3.00 chemical equivalents or less, even more preferably 0.20 chemical equivalents or more and 2.00 chemical equivalents or less, and even more preferably 0.30 chemical equivalents or more and 1.50 chemical equivalents or less, relative to all carboxy groups of the carboxy group-containing resin. The term "all carboxy groups" is used to mean carboxy groups of the carboxy group-containing resin that were not involved in the reaction, and carboxy groups that become polyvalent metal salts of polycarboxylic acids in the reaction product obtained by reacting the carboxy group-containing resin with a polyvalent metal compound. The chemical equivalent can be calculated, for example, as follows. An example will be described in which the carboxyl group-containing resin is acrylic acid and the polyvalent metal compound is magnesium chloride. The molecular weight of the monomer unit of polyacrylic acid is 72, and since it has one carboxyl group per monomer molecule, when the mass of polyacrylic acid is 100g, the amount of carboxyl groups in 100g of polyacrylic acid is 1.39mol. At this time, 1 equivalent to 100g of polyacrylic acid is the amount of base that neutralizes 1.39mol. Therefore, when 0.2 equivalents of magnesium chloride are mixed with 100g of polyacrylic acid, it is sufficient to add magnesium chloride enough to neutralize 0.278mol of carboxyl groups. Since the valence of magnesium is divalent and the molecular weight of magnesium oxide is 95, 0.2 equivalents of magnesium chloride to 100g of polyacrylic acid is 13.2g (0.139mol).

[0084] When the intermediate layer contains a reaction product of a carboxyl group-containing resin and a polyvalent metal compound, the intermediate layer may contain components other than the reaction product, such as unreacted carboxyl group-containing resin, unreacted polyvalent metal compound, by-products produced by the reaction of the carboxyl group-containing resin and the polyvalent metal compound, and other resin components.

[0085] The intermediate layer may contain additives within the range that does not impair the characteristics of the present invention. Examples of additives include oxygen absorbers, plasticizers, ultraviolet stabilizers, antioxidants, matting agents, deodorants, flame retardants, weather resistance agents, antistatic agents, thread friction reducing agents, slip agents, mold release agents, antioxidants, and ion exchange agents. These additives can be used alone or in combination of two or more.

[0086] The intermediate layer may be a single layer or a multi-layer structure having two or more layers. When the intermediate layer is a multi-layer structure, each layer may have the same composition or different compositions.

[0087] The thickness of the intermediate layer is preferably 0.1 μm or more and 200 μm or less, and more preferably 1 μm or more and 50 μm or less. The thickness of the intermediate layer can be measured, for example, at the body of the container. The thickness of the intermediate layer means the part where the thickness is the thinnest. When the intermediate layer is a multi-layered layer, the thickness of the intermediate layer is the sum of the thicknesses of all the layers.

[0088] The intermediate layer may be colored in a color such as red, blue, yellow, green, brown, reddish brown, orange, black, or white, and may be transparent or opaque. By coloring the intermediate layer, it is possible to absorb light such as sunlight that enters the container from the outside, as in the case of coloring the intermediate layer, and to suppress changes in taste and color of the contents of the container. Since it can effectively absorb visible light having a wavelength of 400 nm or more and 500 nm or less, the intermediate layer is preferably colored in a color such as reddish brown or orange. For example, a coloring agent can be used to color the intermediate layer.

[0089] (evaporated film) The container of the present invention may have a vapor-deposited film in order to further improve the gas barrier properties.

[0090] Examples of the vapor-deposited film include vapor-deposited films composed of metals such as aluminum, inorganic oxides such as aluminum oxide, silicon oxide, magnesium oxide, calcium oxide, zirconium oxide, titanium oxide, boron oxide, hafnium oxide, and barium oxide, organic silicon compounds such as hexamethyldisiloxane, and hard carbon films such as DLC (Diamond Like Carbon) films. In addition, the hard carbon film made of DLC is also called i-carbon film or hydrogenated amorphous carbon film (aC:H), and is a hard carbon film. 3 It is an amorphous carbon film that is mainly composed of bonds.

[0091] The thickness of the deposited film is not particularly limited, and can be, for example, 1 nm or more and 150 nm or less. The thickness of the deposited film can be measured, for example, at the body of the container, and refers to the location where the thickness is the thinnest.

[0092] The deposition film can be formed by a conventional method, for example, physical vapor deposition methods (PVD methods) such as vacuum deposition, sputtering, and ion plating, and chemical vapor deposition methods (CVD methods) such as plasma chemical vapor deposition, thermal chemical vapor deposition, and photochemical vapor deposition.

[0093] Hereinafter, one embodiment of the container structure according to the present invention will be described by taking a bottle as an example.

[0094] 1 to 3 are schematic half-sectional views showing one embodiment of a bottle, which is an example of a container of the present invention. As shown in Figs. 1 to 3, a bottle 10 has a mouth 11, a neck 12 provided below the mouth 11, a shoulder 13 provided below the neck 12, a body 14 provided below the shoulder 13, and a bottom 15 provided below the body 14.

[0095] The mouth portion 11 includes a threaded portion 16 to which a cap (not shown) is screwed, a cap 17 provided below the threaded portion 16, and a support ring 18 provided below the cap 17. The shape of the mouth portion 11 may be any conventional shape. In this specification, "upper" and "lower" refer to the upper and lower sides, respectively, of the bottle 10 when it is held upright (FIGS. 1 to 3).

[0096] The neck 12 is located between the support ring 18 and the shoulder 13, and has a generally cylindrical shape with a generally uniform diameter. The shoulder 13 is located between the neck 12 and the body 14, and has a shape whose diameter gradually increases from the neck 12 side toward the body 14 side.

[0097] The body 14 has a cylindrical shape with a generally uniform diameter as a whole. However, this is not limited thereto, and the body 14 may have a polygonal cylindrical shape such as a rectangular cylindrical shape or an octagonal cylindrical shape. Alternatively, the body 14 may have a cylindrical shape with a non-uniform horizontal cross section from top to bottom. Furthermore, the body 14 has a generally flat surface without any irregularities, but this is not limited thereto. For example, the body 14 may have irregularities such as panels or grooves.

[0098] The bottom 15 has a recess 19 located in the center and a grounding portion 20 provided around the recess 19. The shape of the bottom 15 is not particularly limited, and may be any conventionally known bottom shape (for example, a petaloid bottom shape or a rounded bottom shape).

[0099] 1 to 3, the bottle 10 includes a support 21 and a protective layer 23 provided on one surface of the support 21. In addition, the bottle 10 includes an intermediate layer 22 between the support 21 and the protective layer 23, as shown in FIGS.

[0100] In one embodiment, as shown in Fig. 1, the mouth 11 of the bottle 10 is formed by a support 21, and the neck 12, shoulder 13, body 14, and bottom 15 are formed by the support 21, an intermediate layer 22, and a protective layer 23. As shown in Fig. 1, in the neck 12, shoulder 13, body 14, and bottom 15, the intermediate layer 22 is provided on the entire outer area of ​​the support 21 so as to surround the support 21, and the protective layer 23 is provided on the entire outer area of ​​the intermediate layer 22 so as to surround the intermediate layer 22.

[0101] In one embodiment, as shown in Fig. 2, the mouth 11 and the neck 12 of the bottle 10 are formed by a support 21, and the shoulder 13, the body 14 and the bottom 15 are formed by the support 21, an intermediate layer 22 and a protective layer 23. As shown in Fig. 2, in the shoulder 13, the body 14 and the bottom 15, the intermediate layer 22 is provided on the entire outer area of ​​the support 21 so as to surround the support 21. As shown in Fig. 2, the protective layer 23 is provided on the entire outer area of ​​the intermediate layer 22 so as to surround the intermediate layer 22.

[0102] In one embodiment, bottle 10 may not have intermediate layer 22 and protective layer 23 in a range of 1 mm to 10 mm downward from the lower end of support ring 18. When filling bottle 10 with contents, the portion below the lower end of support ring 18 (neck portion 12, etc.) is grasped and transported, and if intermediate layer 22 and protective layer 23 are provided in this portion, there is a risk of poor grasping. A bottle that does not have intermediate layer 22 and protective layer 23 provided in a range of 1 mm to 10 mm downward from the lower end of support ring 18 can prevent such poor grasping. This range is preferably 2 mm to 5 mm. It should be noted that this range is the distance from the lower end of the support ring 18 in a direction perpendicular to a plane when the bottle 10 is standing on the plane.

[0103] In one embodiment, the intermediate layer 22 and the protective layer 23 may be provided in the entirety or a part of one or more regions selected from the neck portion 12 , the shoulder portion 13 , the body portion 14 and the bottom portion 15 . In one embodiment, the bottle 10 is preferably provided with an intermediate layer 22 and a protective layer 23 over the entire exterior area of ​​the body 14. More preferably, the bottle 10 is provided with an intermediate layer 22 and a protective layer 23 over the entire exterior area of ​​the shoulder 13 and body 14.

[0104] 3, when the bottom end of the mouth portion 11 is defined as "0L" and the ground portion 20 is defined as "1L", the intermediate layer 22 and the protective layer 23 are provided over the entire outer area of ​​at least 0.4 L to 0.6 L. With this configuration, when the intermediate layer 22 is a barrier layer, the gas barrier property can be efficiently improved. The bottle 10 is preferably provided with an intermediate layer 22 and a protective layer 23 over the entire outer area of ​​at least 0.1 L to 0.8 L, and more preferably provided with an intermediate layer 22 and a protective layer 23 over the entire outer area of ​​at least 0.05 L to 0.95 L.

[0105] An intermediate layer 22 and a protective layer 23 may be provided on the inside of the bottle 10 (not shown). The bottle 10 may have a vapor-deposited film on at least one selected from the group consisting of the inside and the outside of the bottle 10 (not shown).

[0106] In one embodiment, the container of the present invention may be a blow molded product of a preform. As the preform, the preform of the present invention described below may be used. When the container of the present invention is a bottle, a preform may be used as the preform.

[0107] When the bottle of the present invention is a blow molded product of a preform, the volume increase rate of the bottle relative to the preform is preferably 2 or more and 45 or less, more preferably 5 or more and 40 or less, and further preferably 8 or more and 35 or less. The volume increase rate of the bottle relative to the preform means the volume increase rate of the blow-molded portion, for example, the volume increase rate "V2 / V1" when the volume of the preform excluding the mouth portion is V1 and the volume of the bottle excluding the mouth portion after blow molding is V2.

[0108] In the bottle of the present invention, the oxygen permeability is preferably 0.100 cc / day·bottle·0.21 atm or less, more preferably 0.075 cc / day·bottle·0.21 atm or less, even more preferably 0.050 cc / day·bottle·0.21 atm or less, and even more preferably 0.020 cc / day·bottle·0.21 atm or less. In the present invention, the oxygen permeability is a value measured in accordance with JIS K 7126-2:2006 using an oxygen permeability measuring device (e.g., product name: OX-TRAN 2 / 20 manufactured by MOCON) under conditions of 23°C and humidity of 40% RH, and is a value measured over the entire bottle with the mouth sealed with a jig and divided by the surface area of ​​the entire bottle excluding the mouth.

[0109] The cross-sectional thickness of the container is preferably 0.1 mm or more and 0.4 mm or less, and more preferably 0.15 mm or more and 0.3 mm or less. The cross-sectional thickness of the container can be measured, for example, at the body of the container having at least the support, the intermediate layer, and the protective layer. The cross-sectional thickness of the container means the point where the cross-sectional thickness is the thinnest.

[0110] The container of the present invention has a volume / mass of preferably 5 mL / g or more and 50 mL / g or less, and more preferably 8 mL / g or more and 45 mL / g or less. By setting the volume / mass of the container to 5 mL / g or more, the weight of the container can be reduced. Furthermore, by setting the volume / mass of the container to 50 mL / g or less, the strength of the container can be improved.

[0111] The container of the present invention may have a full capacity of, for example, 100 mL or more and 2000 mL or less. The full capacity of the container is preferably 280 mL or more and 750 mL or less. Furthermore, the container of the present invention may be a large one having a full filling capacity of, for example, 10 L or more and 60 L or less.

[0112] In the container of the present invention, the transmittance of visible light having a wavelength of 400 nm or more and 500 nm or less is preferably 20% or less. This can suppress changes in taste and color of the contents. In particular, when the contents is beer, the problem of odor caused by sunlight can be suppressed. The transmittance is more preferably 15% or less, even more preferably 5% or less, and even more preferably 1% or less. Such a transmittance can be adjusted by appropriately coloring at least one layer selected from the group consisting of the protective layer and the intermediate layer. The transmittance of visible light having a wavelength of 400 nm or more and 500 nm or less can be obtained by measuring the light transmittance of visible light wavelengths at 0.5 nm intervals using a spectrophotometer. As the spectrophotometer, an ultraviolet-visible spectrophotometer manufactured by Shimadzu Corporation can be used. The transmittance of the container is measured, for example, in the body of the container having at least the support, the intermediate layer, and the protective layer.

[0113] The container of the present invention may be printed on its surface. The image formed by printing is not particularly limited, and examples thereof include patterns and letters. From the viewpoint of not being affected by the color tone of the container, the printing is preferably applied to the outer surface of the container. Printing can be carried out by a known method, such as an inkjet method, a gravure printing method, an offset printing method, a flexographic printing method, a thermal transfer method, a silk screen method, a pad method, a hot stamp method, or a cold stamp method. Furthermore, a printed container can be obtained by blow molding a preform on which a print has been applied.

[0114] <Container manufacturing method> The method for producing a container of the present invention will be described below with reference to a bottle as an example.

[0115] In one embodiment, the bottle 10 shown in FIG. 1 can be manufactured by the following procedure. First, a support 21 having a mouth portion 11, a neck portion 12, a shoulder portion 13, a body portion 14, and a bottom portion 15 is prepared by a conventionally known method. Next, an intermediate layer coating liquid containing the material constituting the intermediate layer 22 and a solvent is prepared. Next, the coating liquid for the intermediate layer is applied to the neck portion 12, the shoulder portion 13, the body portion 14 and the bottom portion 15 of the support 21 to form a coating film. The coated film is then dried to remove the solvent, thereby forming the intermediate layer 22. Next, a coating liquid for the protective layer containing polyurethane and a solvent is prepared. Next, the protective layer coating liquid is applied to the surface of the intermediate layer 22 to form a coating film. Next, the coating film is dried to remove the solvent, thereby forming the protective layer 23, and the bottle 10 shown in FIG. 1 can be produced. The bottle 10 shown in Figs. 2 and 3 can be manufactured by appropriately selecting the locations to which the intermediate layer coating fluid and the protective layer coating fluid are applied.

[0116] In one embodiment, the bottle 10 shown in Figures 1 to 3 can be produced by blow molding a preform 30 shown in Figures 4 to 6, which will be described later. The blow molding can be carried out by a conventionally known method.

[0117] The solvent used in the intermediate layer coating liquid is one that can dissolve or emulsify and disperse the material that constitutes the intermediate layer. Examples of the solvent include water; alcohols such as methyl alcohol, ethyl alcohol, isopropyl alcohol, n-propyl alcohol, n-butyl alcohol, and n-pentyl alcohol; and polar organic solvents such as dimethyl sulfoxide, N,N-dimethylformamide, and N,N-dimethylacetamide. These solvents can be used alone or in combination of two or more. The solvent is preferably water, alcohols, or a mixture thereof, more preferably a mixed solvent of water and isopropyl alcohol, which improves the viscosity of the intermediate layer coating liquid and reduces the number of coating cycles, thereby improving the productivity of the container.

[0118] In the intermediate layer coating solution, the total concentration of solids of the materials constituting the intermediate layer is preferably 2% by mass or more and 15% by mass or less, more preferably 3% by mass or more and 10% by mass or less, which allows the formation of an intermediate layer with a uniform thickness.

[0119] The viscosity of the intermediate layer coating liquid is preferably from 150 mPa·s to 4000 mPa·s, and more preferably from 200 mPa·s to 2500 mPa·s, which can further improve the productivity of containers. The viscosity of the intermediate layer coating liquid can be measured using a rotational viscometer at a temperature of 20° C. in accordance with JIS Z 8803:2011.

[0120] The intermediate layer coating liquid can be applied by a conventional method, for example, a method of applying the intermediate layer coating liquid by a brush, a method of immersing a container in the intermediate layer coating liquid, a method of spraying the intermediate layer coating liquid on the surface of a container, etc.

[0121] The drying temperature of the coating film formed from the intermediate layer coating liquid is a temperature at which the solvent can be removed, and is preferably 20°C or higher and 80°C or lower, more preferably 50°C or higher and 70°C or lower.

[0122] The solvent used in the coating liquid for the protective layer is one that can dissolve or emulsify and disperse the polyol, polyisocyanate, and polyurethane, and examples of the solvent that can be used include acetone, ethyl methyl ketone, methyl isobutyl ketone, and ethyl acetate.

[0123] The coating liquid for the protective layer can be applied by a conventionally known method, such as a method of applying the coating liquid by a brush, a method of immersing a container in the coating liquid for the protective layer, or a method of spraying the coating liquid for the protective layer on the surface of a container.

[0124] The coating film formed from the protective layer coating liquid is dried at a temperature at which the solvent can be removed, preferably from 20° C. to 80° C., more preferably from 40° C. to 70° C.

[0125] The method for manufacturing a container of the present invention may include a step of printing images such as patterns and letters on the surface of the container. Printing can be performed by a known method. Examples of printing methods include inkjet printing, gravure printing, offset printing, flexographic printing, thermal transfer printing, silk screen printing, pad printing, hot stamping, and cold stamping. For example, when printing is performed by the inkjet method, a UV-curable ink is applied to the container, and then irradiated with UV light to harden the ink. Printing may also be performed using a thermal transfer sheet.

[0126] <Preform> As described above, the container of the present invention can also be manufactured by forming an intermediate layer and a protective layer on the surface of a support obtained by various methods such as compression molding, injection molding, blow molding, and thermoforming. In particular, when the support is obtained by blow molding, an intermediate layer and a protective layer can be formed on the surface of the support of a preform before blow molding, and the preform can be blow molded to form a container. In this specification, the preform is a molded body before blow molding the container of the present invention, and is used to manufacture the container of the present invention. The shape of the preform can be appropriately selected depending on the shape of the container after blow molding. The preform of the present invention comprises a support and a protective layer provided on at least one side of the support, and comprises an intermediate layer having water solubility or alkali solubility between the support and the protective layer.

[0127] Each of the components of the preform of the present invention will be described below.

[0128] (Support) In the preform of the present invention, the material constituting the support may be the same as the material constituting the support of the container of the present invention. By using such a material for the support, the container of the present invention can be obtained, and a preform with excellent blow moldability can be obtained.

[0129] The support may have a single layer structure or a multi-layer structure of two or more layers. When the support has a multi-layer structure, each layer may have the same composition or different compositions.

[0130] The cross-sectional thickness of the support is preferably 1.3 mm or more and 4.3 mm or less, and more preferably 1.9 mm or more and 2.9 mm or less. The cross-sectional thickness of the support can be measured, for example, at the body portion of the preform, and refers to the location where the cross-sectional thickness is the thinnest.

[0131] The support of the preform is preferably subjected to a surface treatment. Examples of the surface treatment include corona treatment, low-temperature plasma treatment, and flame treatment. By performing such a surface treatment, the wettability of the support surface is improved, and the adhesion between the support and the layer in contact with the support can be improved.

[0132] (protective layer) In the preform of the present invention, the protective layer contains polyurethane, which makes it possible to obtain a container with improved durability. In the preform of the present invention, the material constituting the protective layer may be the same as the material constituting the protective layer in the container of the present invention. By using such a material for the protective layer, the container of the present invention can be obtained, and a preform with excellent blow moldability can be obtained.

[0133] The protective layer may be a single layer or a multi-layer consisting of two or more layers. When the protective layer is a multi-layer, each layer may have the same composition or different compositions.

[0134] The thickness of the protective layer is preferably 0.5 μm or more and 1000 μm or less, and more preferably 0.7 μm or more and 500 μm or less. The thickness of the protective layer can be measured, for example, at the body of the preform. The thickness of the protective layer means the part where the thickness is the thinnest. When the protective layer has multiple layers, the thickness of the protective layer is the sum of the thicknesses of all the layers.

[0135] The protective layer may be colored in a color such as red, blue, yellow, green, brown, reddish brown, orange, black, or white, and may be transparent or opaque. By forming such a protective layer, a container having a colored protective layer can be manufactured. For example, a coloring agent can be used to color the protective layer.

[0136] (Middle class) In the preform of the present invention, the material constituting the intermediate layer can be the same as the material constituting the intermediate layer in the container of the present invention. By using such a material for the intermediate layer, the container of the present invention can be obtained, and a preform with excellent blow moldability can be obtained.

[0137] The intermediate layer is preferably a layer having light-shielding properties, glossiness, color, gas barrier properties, etc., depending on the application of the container produced from the preform. The intermediate layer is particularly preferably a barrier layer having gas barrier properties.

[0138] The intermediate layer may be a single layer or a multi-layer structure having two or more layers. When the intermediate layer is a multi-layer structure, each layer may have the same composition or different compositions.

[0139] The thickness of the intermediate layer is preferably 2.0 μm or more and 1000 μm or less, and more preferably 20 μm or more and 500 μm or less. The thickness of the intermediate layer can be measured, for example, at the body of the preform. The thickness of the intermediate layer means the portion where the thickness is the thinnest. When the intermediate layer has multiple layers, the thickness of the intermediate layer is the sum of the thicknesses of all the layers.

[0140] The intermediate layer or protective layer may be colored in a color such as red, blue, yellow, green, brown, dark brown, orange, black, or white, and may be transparent or opaque. By forming the intermediate layer in this manner, a container having a colored intermediate layer can be manufactured. For example, a coloring agent can be used to color the intermediate layer.

[0141] Hereinafter, one embodiment of the structure of the preform according to the present invention will be described by taking a preform as an example.

[0142] 4 to 6 are schematic half-sectional views showing one embodiment of a preform according to the present invention. As shown in Figs. 4 to 6, the preform 30 includes a mouth 31, a body 32 connected to the mouth 31, and a bottom 33 connected to the body 32. The mouth 31 corresponds to the mouth 11 of the bottle 10 described below, and has substantially the same shape as the mouth 11. The body 32 corresponds to the neck 12, shoulder 13, and body 14 of the bottle 10, and has a substantially cylindrical shape. The bottom 33 corresponds to the bottom 15 of the bottle 10, and has a substantially hemispherical shape.

[0143] Mouth portion 31 is provided with a threaded portion 34 corresponding to threaded portion 16 of bottle 10 (described below) to which a cap (not shown) is screwed, a cap 35 provided below threaded portion 34 and corresponding to cap 17 of bottle 10, and a support ring 36 provided below cap 35 and corresponding to support ring 18 of bottle 10. Mouth portion 31 may have a conventionally known shape.

[0144] As shown in Figures 4 to 6, the preform 30 includes a support 37 and a protective layer 39 provided on one surface of the support 37. In addition, the preform 30 includes an intermediate layer 38 between the support 37 and the protective layer 39, as shown in Figures 4 to 6.

[0145] In one embodiment, as shown in Fig. 4, the mouth portion 31 of the preform 30 is formed by the support 37, and the body portion 32 and the bottom portion 33 are formed by the support 37, an intermediate layer 38, and a protective layer 39. As shown in Fig. 4, the intermediate layer 38 is provided on the entire outer area of ​​the support 37 so as to surround the support 37. As shown in Fig. 4, the protective layer 39 is provided on the entire outer area of ​​the intermediate layer 38 so as to surround the intermediate layer 38.

[0146] In one embodiment, as shown in Fig. 5, the mouth portion 31 and a part of the body portion 32 of the preform 30 are formed by the support 37, and the remaining portion of the body portion 32 and the bottom portion 33 are formed by the support 37, an intermediate layer 38, and a protective layer 39. As shown in Fig. 5, the intermediate layer 38 is provided on the entire outer area of ​​the support 37 so as to surround the support 37. As shown in Fig. 5, the protective layer 39 is provided on the entire outer area of ​​the intermediate layer 38 so as to surround the intermediate layer 38. In the above, "a part of the body 32" refers to the part corresponding to the neck 12 of the bottle 10 shown in FIG. 2, and "the remaining part of the body 32" refers to the parts corresponding to the shoulder 13, the body 14, and the bottom 15 of the bottle 10 shown in FIG. 2.

[0147] In one embodiment, the preform 30 may not have the intermediate layer 38 and the protective layer 39 in a range of 1 mm to 10 mm below the lower end of the support ring 36. This makes it possible to manufacture a bottle that is less likely to be gripped when being transported when filling the bottle with contents. The range is preferably 2 mm to 5 mm.

[0148] In one embodiment, the intermediate layer 38 and the protective layer 39 may be provided over the entire area or a partial area in the vertical direction of at least one portion selected from the group consisting of the body portion 32 and the bottom portion 33. In one embodiment, as shown in Fig. 6, when the lower end of the mouth portion 31 is "0L" and the lower end of the bottom portion 33 is "1L", the preform 30 has an intermediate layer 38 and a protective layer 39 provided over the entire outer area of ​​at least 0.4L to 0.6L. By configuring the preform in this way, when the intermediate layer 38 is a barrier layer, a container with efficiently improved gas barrier properties can be obtained. The preform 30 is preferably provided with an intermediate layer 38 and a protective layer 39 over the entire outer area of ​​at least 0.2L to 0.7L, and more preferably provided with an intermediate layer 38 and a protective layer 39 over the entire outer area of ​​at least 0.1L to 0.9L.

[0149] An intermediate layer 38 and a protective layer 39 may be provided on the inside of the preform 30 (not shown).

[0150] The cross-sectional thickness of the preform is preferably 1.4 mm or more and 4.5 mm or less, and more preferably 2.0 mm or more and 3.0 mm or less. The cross-sectional thickness of the preform can be measured, for example, at a body portion of the preform having at least the support, the intermediate layer, and the protective layer. The cross-sectional thickness of the preform means the point where the cross-sectional thickness is the thinnest.

[0151] In the preform of the present invention, the transmittance of visible light having a wavelength of 400 nm or more and 500 nm or less is preferably 20% or less. This makes it possible to produce a container in which changes in taste and color of the contents of the container are suppressed. The transmittance is more preferably 15% or less, even more preferably 5% or less, and even more preferably 1% or less. Such a transmittance can be adjusted by appropriately coloring at least one layer selected from the group consisting of the protective layer and the intermediate layer. The transmittance of visible light having a wavelength of 400 nm or more and 500 nm or less can be obtained by measuring the light transmittance of visible light wavelengths at 0.5 nm intervals using a spectrophotometer. As the spectrophotometer, an ultraviolet-visible spectrophotometer manufactured by Shimadzu Corporation can be used. The transmittance of the preform is measured, for example, in the body portion of the preform having at least the support, the intermediate layer, and the protective layer.

[0152] The surface of the preform of the present invention may be printed. The image formed by printing is not particularly limited, and examples thereof include patterns and letters. From the viewpoint of not being affected by the color tone of the preform, the printing is preferably performed on the outer surface of the preform. Printing can be carried out by a known method, such as an inkjet method, a gravure printing method, an offset printing method, a flexographic printing method, a thermal transfer method, a silk screen method, a pad method, a hot stamp method, and a cold stamp method.

[0153] <Method of manufacturing preform> The method for producing a preform according to the present invention will be described below with reference to an example of a preform.

[0154] In one embodiment, the preform 30 depicted in FIG. 4 can be manufactured by the following procedure. First, the material constituting the support is injection molded using a conventionally known device to produce support 37 having mouth portion 31, body portion 32, and bottom portion 33. Next, an intermediate layer coating liquid containing the material for forming the intermediate layer 38 and a solvent is prepared. Next, the intermediate layer coating liquid is applied to the body 32 and bottom 33 of the support 37 to form a coating film. The coated film is then dried to remove the solvent, thereby forming the intermediate layer 38. Next, a coating liquid for the protective layer containing polyurethane and a solvent is prepared. Next, the protective layer coating liquid is applied to the surface of the intermediate layer 38 to form a coating film. Next, the coating film is dried to remove the solvent, thereby forming a protective layer 39, and the preform 30 shown in FIG. 4 can be manufactured. The preform 30 shown in Figs. 5 and 6 can be manufactured by appropriately selecting the locations to which the intermediate layer coating fluid and the protective layer coating fluid are applied.

[0155] The intermediate layer coating fluid and protective layer coating fluid in the method for producing a preform can be the same as the intermediate layer coating fluid and protective layer coating fluid in the method for producing a container.

[0156] The intermediate layer coating liquid and the protective layer coating liquid can be applied by a conventionally known method, such as a method of applying the coating liquid by a brush, a method of immersing a preformed body in the intermediate layer coating liquid, or a method of spraying the intermediate layer coating liquid on the surface of a preformed body.

[0157] The method for producing a preform of the present invention may include a step of printing images such as patterns and characters on the surface of the preform. Printing can be performed by a known method. Examples of printing methods include inkjet printing, gravure printing, offset printing, flexographic printing, thermal transfer printing, silk screen printing, pad printing, hot stamping, and cold stamping. For example, when printing is performed by the inkjet method, printing can be performed by applying a UV-curable ink to the preform, irradiating it with UV light, and curing it. Also, printing may be performed using a thermal transfer sheet. EXAMPLES

[0158] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples.

[0159] [Example 1] Pellets of polyethylene terephthalate (PET) were prepared. The PET was melted and injected into an injection molding machine to produce a support having a mouth, a body, and a bottom. The mouth of the support has a screw portion, a cap, and a support ring in that order from above the mouth.

[0160] 7 parts by mass of polyacrylic acid (trade name: AS-58, number average molecular weight: 106,000) manufactured by Nippon Shokubai Co., Ltd. was added to 93 parts by mass of water while stirring, and then heated to 80°C to completely dissolve, to obtain a 7% by mass aqueous solution of polyacrylic acid. Separately, 7 parts by mass of polyvinyl alcohol (trade name: PVA-124, polymerization degree: 2400, saponification degree: 98 to 99%) manufactured by Kuraray Co., Ltd. was added to 93 parts by mass of water while stirring, and then heated to 90°C to completely dissolve, to obtain a 7% by mass aqueous solution of PVA. These two solutions were mixed at room temperature in a mass ratio of 1:1 to prepare a coating liquid for the intermediate layer (viscosity: 230 mPa·s (20°C)). This coating liquid for the intermediate layer was applied to the trunk and bottom of the support to form a coating film, and the coating film was dried at 50°C for 10 minutes. This coating film formation and drying were performed a total of three times to form an intermediate layer.

[0161] Separately, 42.1 parts by mass of a base material of a urethane-based coating material (product name: EL-540) manufactured by Toyo-Morton Co., Ltd., 7.9 parts by mass of a curing agent, and 50 parts by mass of ethyl acetate were mixed to prepare a coating liquid for a protective layer. This coating liquid for a protective layer was applied to the surface of the intermediate layer to form a coating film, and the coating film was dried at 50° C. for 10 minutes. This formation and drying of the coating film was performed a total of three times to form a protective layer and obtain a preform. The cross-sectional thickness of the body of the preform was 2 mm, the thickness of the intermediate layer was 50 μm, and the thickness of the protective layer was 80 μm. The weight of the preform was 18.3 g.

[0162] The preform was then heated to 110°C and biaxially stretched and blow molded in a blow molding die to obtain a bottle having a mouth, neck, shoulder, body, and bottom and a capacity of 600 mL. The intermediate layer was formed on the outer surfaces of the neck, shoulder, body, and bottom of the bottle. The cross-sectional thickness of the bottle body was 0.15 mm, the intermediate layer was 5 μm, and the protective layer was 7 μm.

[0163] [Example 2] A preform was obtained in the same manner as in Example 1, except that EL-540 was changed to EL-510, which is the main component of the same urethane-based coating material. The cross-sectional thickness of the body of the preform was 2 mm, the thickness of the intermediate layer was 50 μm, and the thickness of the protective layer was 80 μm. The weight of the preform was 18.3 g.

[0164] Next, in the same manner as in Example 1, a bottle was obtained from the preform of this example. The cross-sectional thickness of the body of the bottle was 0.15 mm, the thickness of the intermediate layer was 5 μm, and the thickness of the protective layer was 7 μm.

[0165] [Example 3] A preform was obtained in the same manner as in Example 1, except that the number of times the protective layer coating liquid was applied and dried was one, and the weight of the preform was 18.3 g. The cross-sectional thickness of the body of the preform was 2 mm, the thickness of the intermediate layer was 50 μm, and the thickness of the protective layer was 20 μm.

[0166] Next, in the same manner as in Example 1, a bottle was obtained from the preform of this example. The cross-sectional thickness of the body of the bottle was 0.15 mm, the thickness of the intermediate layer was 5 μm, and the thickness of the protective layer was 2 μm.

[0167] [Example 4] A preform was obtained in the same manner as in Example 3, except that the intermediate layer coating liquid was applied and dried a total of three times, the protective layer coating liquid was applied and dried a total of four times, and the preform had a basis weight of 21.8 g. The cross-sectional thickness of the body of the preform was 2 mm, the intermediate layer was 50 μm, and the protective layer was 110 μm.

[0168] Next, a bottle was obtained from the preform of this example in the same manner as in Example 1, except that the bottle had an internal volume of 280 mL. The cross-sectional thickness of the body of the bottle was 0.15 mm, the thickness of the intermediate layer was 7 μm, and the thickness of the protective layer was 15 μm.

[0169] [Comparative Example 1] Polyvinyl butyral A (Mowital (registered trademark) B30H, Mn: 28,000 to 38,000, manufactured by Kuraray Co., Ltd.) and ethyl acetate were mixed to prepare a coating liquid for a protective layer containing 11% polyvinyl butyral A. A preform and a bottle were prepared in the same manner as in Example 3, except that the protective layer was formed using this coating liquid for the protective layer. The thickness of the protective layer in the preform was 7.4 μm, and the thickness of the protective layer in the bottle was 0.7 μm.

[0170] [Comparative Example 2] A preform and a bottle were produced in the same manner as in Comparative Example 1, except that the number of times the protective layer coating solution was applied and dried was set to five in total. The thickness of the protective layer in the preform was 59 μm, and the thickness of the protective layer in the bottle was 5.3 μm.

[0171] [Comparative Example 3] Polyvinyl butyral B (Mowital (registered trademark) B60H, Mn: 50,000 or more and 60,000 or less, manufactured by Kuraray Co., Ltd.) and ethyl acetate were mixed to prepare a coating liquid for a protective layer containing 7 mass% of polyvinyl butyral B, and a preform and a bottle were produced in the same manner as in Comparative Example 1, except that a protective layer was formed using this coating liquid for a protective layer. The thickness of the protective layer in the preform was 3.4 μm, and the thickness of the protective layer in the bottle was 0.3 μm.

[0172] [Comparative Example 4] A preform and a bottle were produced in the same manner as in Comparative Example 3, except that the number of times the protective layer coating solution was applied and dried was 10 in total. The thickness of the protective layer in the preform was 44 μm, and the thickness of the protective layer in the bottle was 3.9 μm.

[0173] [Comparative Example 5] A preform and a bottle were obtained in the same manner as in Example 4, except that the intermediate layer and the protective layer were not formed.

[0174] [Comparative Example 6] A preform and a bottle were obtained in the same manner as in Comparative Example 5, except that the support had a multilayer structure consisting of three layers, the first layer on the inside and the third layer on the outside were formed of PET, and the second layer located between the first and third layers was formed of nylon.

[0175] <<Recyclability evaluation>> The bottles obtained in Examples 1 and 2 were crushed into flakes, and the flakes were then placed in a 1.5% by mass aqueous sodium hydroxide solution at 90°C and stirred for 15 minutes. The flakes were then filtered off, and the alkaline aqueous solution on the flake surfaces was washed away with distilled water at 20°C. The recyclability of the bottles was evaluated based on the following criteria. The evaluation results are shown in Table 1. The recyclability evaluation was performed by mixing a small amount of red colorant into the protective layer coating liquid to color the protective layer. (Evaluation Criteria) A: The flakes became colorless and transparent. B: The colored protective layer remained on the flakes.

[0176] [Table 1]

[0177] <<Heat resistance rating A>> Water was filled into the bottles obtained in Examples 1 and 3 and Comparative Examples 1 to 4. The bottles were heated on a hot plate at 200° C., and the surfaces of the bottles were observed during heating. In the bottles of Comparative Examples 1 to 4, stickiness occurred at the bottom of the bottle when the water temperature reached approximately 56°C. In the bottles of Examples 1 and 3, the bottom of the bottle did not become sticky even when the water temperature reached about 64°C.

[0178] <<Heat resistance rating B>> The bottles obtained in Example 4 and Comparative Examples 5 and 6 were filled with water. The bottles were heated on a hot plate and the water temperature in the bottle was adjusted to 70°C. The bottles were left in this state for 3 weeks, and the occurrence of buckling was confirmed. Buckling refers to the phenomenon in which the concave portion of the bottom of the bottle is inverted and becomes convex. In the bottles of Comparative Examples 5 and 6, buckling occurred. In the bottle of Example 4, no buckling occurred.

[0179] As is clear from the results of heat resistance evaluations A and B, the container having a protective layer containing polyurethane has better heat resistance than the container having a protective layer not containing polyurethane.

[0180] <<Gas barrier property evaluation>> The oxygen permeability of the bottles obtained in Example 4 and Comparative Examples 5 and 6 was measured to evaluate the gas barrier properties of the bottles. The oxygen permeability was measured in accordance with JIS K 7126-2:2006 using an oxygen gas permeability measuring device (manufactured by MOCON, product name: OX-TRAN2 / 20) under conditions of 23°C and 40% RH. The oxygen permeability value was measured for the entire bottle with the mouth closed with a jig, and was divided by the surface area of ​​the entire bottle excluding the mouth. In addition, the oxygen transmission rate of the bottle of Example 4 was measured even after the above heat resistance evaluation B (after heating). The measurement results are shown in Table 2.

[0181] [Table 2]

[0182] As is clear from Table 2, the bottle of Example 4 has gas barrier properties equivalent to those of the bottle of Comparative Example 6, which has a layer made of nylon having gas barrier properties. Moreover, the bottle of Example 4 maintains its gas barrier properties even after heating. [Explanation of symbols]

[0183] 10: Bottle 11: Mouth 12: Neck 13:Shoulder 14: Torso 15: Bottom 16: Screw part 17: Turnip 18: Support ring 19: Recess 20: Grounding part 21:Support 22: Middle class 23:Protective layer 30: Preform 31: Mouth 32: Torso 33: Bottom 34: Screw part 35: Turnip 36: Support ring 37:Support 38: Middle class 39:Protective layer

Claims

1. A preform comprising a support and a protective layer provided on at least one surface side of the support, the protective layer comprises polyurethane; a water-soluble or alkali-soluble intermediate layer is provided between the support and the protective layer; The intermediate layer comprises a carboxyl group-containing resin and a polyvinyl alcohol-based resin.

2. 10. The preform of claim 1, wherein the polyurethane is the reaction product of a polyurethane polyol and an organic polyisocyanate.

3. The preform according to claim 2 , wherein the polyurethane polyol has a carboxy group in the molecule.

4. The preform according to any one of claims 1 to 3, wherein the protective layer has a thickness of 0.5 µm or more and 1000 µm or less.

5. The preform according to any one of claims 1 to 4, wherein a mass ratio of the carboxyl group-containing resin to the polyvinyl alcohol-based resin is 1 / 20 or more and 10 / 1 or less.

6. The preform of any one of claims 1 to 5, wherein the support comprises polyester.

7. A container which is a blow molded article made of the preform according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Treatment of container made of thermoplastic polyester

    JP1984152929A

  • Easily peelable label and method for removing this label

    JP1992350892A

  • Thermoplastic resin container with polyurethane layer on external surface, which can be compressed, and its manufacture

    JP1996324572A

  • Production of coated container

    JP2000102763A

  • Gas barrier film

    JP2002307601A