Nitride semiconductor device and its manufacturing method

By incorporating a nitride semiconductor layer with controlled carbon concentration and a barrier layer with a larger bandgap, along with a strategically implanted element isolation region, the device addresses leakage current issues, enhancing reliability and performance under high voltage and temperature conditions.

JP7584050B2Active Publication Date: 2024-11-15PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD

Patent Information

Application Number
JP2021536835
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-07-31
Filing Date
2020-06-24
Publication Date
2024-11-15
Estimated Expiration
2040-06-24

AI Technical Summary

Technical Problem

The existing nitride semiconductor devices face issues with leakage currents and reduced reliability due to thin back barrier layers and improper element isolation structures, especially at high voltages and temperatures, leading to degradation in performance.

Method used

The device incorporates a nitride semiconductor layer with controlled carbon concentration and a barrier layer with a larger bandgap, along with an element isolation region implanted to reach a high carbon concentration layer, ensuring the impurity concentration at specific depths to suppress leakage currents.

Benefits of technology

This design effectively reduces leakage currents and enhances the reliability of the nitride semiconductor device, particularly under high temperature and voltage conditions, improving its operational performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007584050000001
    Figure 0007584050000001
  • Figure 0007584050000002
    Figure 0007584050000002
  • Figure 0007584050000003
    Figure 0007584050000003
Patent Text Reader

Abstract

This nitride semiconductor device has a semiconductor laminated structure comprising: a substrate (1); a channel layer (3) formed on the substrate (1) and composed of a nitride semiconductor layer; and a barrier layer (4) which is formed in direct contact on the channel layer (3) and composed of a nitride semiconductor layer, and has a band gap larger than that of the channel layer (3), wherein an element separation region (10) doped with impurities is formed in the semiconductor laminated structure, one peak (12) in the depth direction of the impurity concentration in the element separation region (10) is located deeper than the interface (13) between the barrier layer (4) and the channel layer (3), and the concentration of impurities in the element separation region (10) at the depth of the interface (13) between the barrier layer (4) and the channel layer (3) is lower than the concentration of the peak (12) in the depth direction of the impurity concentration.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a nitride semiconductor device and a method for manufacturing the same, and more particularly to a nitride semiconductor device that can be used as a field effect transistor or the like, and a method for manufacturing the same. [Background technology]

[0002] Group III nitride semiconductors have a high breakdown voltage due to their wide band gap. In addition, heterostructures such as AlGaN / GaN can be easily formed, and a high-mobility, high-concentration electron channel (two-dimensional electron gas) can be generated on the GaN layer side of the AlGaN / GaN interface due to the difference between the band gap and the piezoelectric charge generated by the difference in lattice constant between AlGaN and GaN. By controlling this two-dimensional electron gas, it is possible to form a high electron mobility transistor (HEMT). Due to these characteristics of high breakdown voltage, high speed, and large current, Group III nitride semiconductors are applied to electronic devices such as field effect transistors (FETs) and diodes for power applications.

[0003] The semiconductor device shown in FIG. 1 to FIG. 4 of Patent Document 1 uses a semiconductor laminated structure in which an i-GaN layer serving as a buffer layer, an InGaN layer serving as a back barrier, an i-GaN layer serving as an electron transport layer (channel layer), an AlN layer serving as an intermediate layer, an InAlGaN layer serving as an electron supply layer (barrier layer), and a GaN layer serving as a cap layer are epitaxially grown in this order on a SiC substrate. In the semiconductor laminated structure, a two-dimensional electron gas layer is generated on the intermediate layer side in the electron transport layer due to the band gap difference between the electron supply layer / intermediate layer and the electron transport layer and the piezoelectric charge of the electron supply layer / intermediate layer. On the electron supply layer, there are a source electrode and a drain electrode that are spaced apart from each other and in ohmic contact with the second III-nitride semiconductor layer, and a gate electrode is spaced apart from each other between the source electrode and the drain electrode. The semiconductor device is a FET that can control the drain current that flows between the source electrode and the drain electrode through the two-dimensional electron gas layer by a voltage applied to the gate electrode portion. In the inactive portion outside the active region of the FET, an element isolation structure is formed by implanting Ar or the like, which extends from the upper surface side of the semiconductor laminated structure to the substrate (see FIG. 1(b) of Patent Document 1). In addition, the InGaN layer serving as the back barrier contains carbon (hereinafter simply referred to as "C"), and the C concentration is high in some parts.

[0004] According to Patent Document 1, by including C in the back barrier layer, C acts as an acceptor level, increases the potential of the conduction band, and suppresses electron diffusion toward the buffer layer side, while suppressing the short channel effect and reducing the drain leakage current. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2018 / 180021 Summary of the Invention [Problem to be solved by the invention]

[0006] However, the semiconductor device described in Patent Document 1 has the following problems.

[0007] That is, in the structure shown in Figures 1 to 4 of Patent Document 1, the back barrier layer (InGaN with a film thickness of 5 nm or less) is very thin, so that during high-voltage and high-temperature operation such as that used in power semiconductors, drain leakage current (the sum of leakage currents between the drain and gate, between the drain and source, and between the drain and substrate) and source leakage current (leakage current between the drain and source) leak to the buffer layer side, deteriorating reliability. Also, although it is said that the element isolation structure is formed by implanting impurities (Ar), depending on the amount of implanted impurities and the depth distribution, leakage current from the drain electrode to the element isolation region occurs, particularly during high-voltage and high-temperature operation such as that used in power semiconductors, which degrades reliability.

[0008] SUMMARY OF THE PRESENT EMBODIMENTS Accordingly, an object of the present invention is to provide a nitride semiconductor device in which leakage current is suppressed, and a method for manufacturing the same. [Means for solving the problem]

[0009] In order to achieve the above object, a nitride semiconductor device according to one aspect of the present invention comprises: A substrate and a C (carbon) concentration of 1E+18 cm -3 the semiconductor laminated structure includes a high C (carbon) concentration nitride semiconductor layer as described above, a channel layer formed on the high C concentration nitride semiconductor layer and made of a nitride semiconductor layer having a lower C concentration than the high C concentration nitride semiconductor layer, and a barrier layer formed on and in direct contact with the channel layer, made of a nitride semiconductor layer and having a larger band gap than the channel layer, wherein an element isolation region into which an impurity is implanted is formed in the semiconductor laminated structure, the element isolation region reaching the high C concentration nitride semiconductor layer from an upper surface side of the semiconductor laminated structure, and a maximum concentration of the impurity at a depth of the channel layer is 70 times or less than a concentration of the impurity at a depth of an interface between the high C concentration nitride semiconductor layer and the channel layer.

[0010] In order to achieve the above object, a method for manufacturing a nitride semiconductor device according to one aspect of the present invention includes the steps of: A substrate is prepared, and a C (carbon) layer having a concentration of 1E+18 cm is placed on the substrate. -3 The method includes the steps of forming a semiconductor stacked structure by forming a nitride semiconductor layer having a high C (carbon) concentration as described above, forming a channel layer made of a nitride semiconductor layer on the high C concentration nitride semiconductor layer, and forming a barrier layer made of a nitride semiconductor layer having a larger band gap than the channel layer on the channel layer, and forming an element isolation region by injecting impurities from above the semiconductor stacked structure, wherein in the step of forming the element isolation region, the impurities are injected so that the element isolation region reaches the high C concentration nitride semiconductor layer from the upper surface side of the semiconductor stacked structure, and the impurities are injected so that the maximum concentration of the impurity in the channel layer is 70 times or less the concentration of the impurity at a depth of the interface between the high C concentration nitride semiconductor layer and the channel layer. Effect of the Invention

[0011] According to the nitride semiconductor device and the manufacturing method thereof of the present invention, leakage current is suppressed. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a diagram showing a cross-sectional structure of a nitride semiconductor device according to an embodiment, and a relationship between an impurity concentration and a depth in an isolation region. [Diagram 2] FIG. 2 is a diagram for explaining in detail the relationship between the impurity concentration and the depth in the element isolation region of the nitride semiconductor device according to the embodiment. [Diagram 3] FIG. 3 is a diagram showing cross-sectional structures of nitride semiconductor devices according to first and second modifications of the embodiment, and a relationship between the impurity concentration and the depth in an isolation region. [Figure 4] FIG. 4 is a diagram for explaining in detail the relationship between the impurity concentration and the depth in the element isolation region of the nitride semiconductor device according to the first and second modifications of the embodiment. [Diagram 5] FIG. 5 is a diagram showing characteristics of the nitride semiconductor device according to the first modification of the embodiment. [Figure 6] FIG. 6 is a diagram showing characteristics of the nitride semiconductor device according to the second modification of the embodiment. [Figure 7] FIG. 7 is a diagram showing characteristics of the nitride semiconductor device according to the third modification of the embodiment. In FIG. [Figure 8] FIG. 8 is a diagram showing characteristics of the nitride semiconductor device according to the fourth modification of the embodiment. [Figure 9] FIG. 9 is a diagram showing characteristics of the nitride semiconductor device according to the fifth modification of the embodiment. [Figure 10] FIG. 10 is a cross-sectional view showing a method for manufacturing a nitride semiconductor device according to the embodiment and its modification. [Figure 11] FIG. 11 is a plan view showing a planar structure of a nitride semiconductor device according to the embodiment and its modification. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, nitride semiconductor devices according to the embodiments will be described in detail with reference to the drawings. Each of the embodiments described below shows a specific example of the present invention. The numerical values, shapes, materials, components, arrangement positions and connection forms of the components shown in the following embodiments are merely examples and are not intended to limit the present invention. Furthermore, among the components in the following embodiments, components that are not described in the independent claims showing the highest concept will be described as optional components. Furthermore, the "above" / "below" of a certain object may include not only the "above" / "below" positions that are in contact with a certain object, but also the "above" / "below" positions that are not in contact with a certain object, unless otherwise specified, such as "in contact". Furthermore, the "above" / "below" of a certain object indicates a relative positional relationship in the illustrated state, and does not indicate an absolute positional relationship with respect to gravity.

[0014] FIG. 1 is a diagram showing a cross-sectional structure ((b) of FIG. 1) of a nitride semiconductor device according to an embodiment, and a relationship between impurity concentration and depth in an element isolation region ((a) of FIG. 1). As shown in (b) of FIG. 1, the nitride semiconductor device includes a semiconductor laminated structure including a substrate 1, a channel layer 3 made of a nitride semiconductor layer formed on the substrate 1, and a barrier layer 4 made of a nitride semiconductor layer formed on the channel layer 3 in direct contact therewith and having a larger band gap than the channel layer 3. In this embodiment, more specifically, the semiconductor laminated structure includes, from the bottom, a substrate 1, a buffer layer 2, a channel layer 3, a two-dimensional electron gas layer 5, a barrier layer 4, and a gate layer 8. A source electrode 6 and a drain electrode 7 are formed on the barrier layer 4. The semiconductor laminated structure has an element isolation region 10 (region hatched upward to the left) into which impurities are injected, and as shown in (a) of FIG. 1, one peak 12 of the impurity concentration in the element isolation region 10 in the depth direction from the top surface of the semiconductor laminated structure is located deeper than the depth of the interface 13 between the barrier layer 4 and the channel layer 3, and the impurity concentration at the depth of the interface 13 is lower than the concentration of peak 12.

[0015] That is, in the nitride semiconductor device, in the element isolation region 10 into which an impurity has been implanted, one of the peaks 12 of the impurity concentration in the element isolation region 10 in the depth direction is located at a position deeper (in the downward direction in FIG. 1 ) than the interface 13 between the barrier layer 4 and the channel layer 3 when viewed from the top side, and the impurity concentration in the element isolation region 10 at the depth of the interface 13 between the barrier layer 4 and the channel layer 3 is lower than the concentration of the peak 12 of the impurity concentration in the depth direction.

[0016] More specifically, the semiconductor laminated structure has an appropriate buffer layer 2 (for example, a single layer or multiple layers of III-nitride semiconductors such as GaN, AlGaN, AlN, InGaN, InN, AlInGaN, etc.) on an appropriate substrate 1 such as Si (other substrates such as sapphire, SiC, GaN, AlN, etc.), a channel layer 3 made of GaN (other substrates such as III-nitride semiconductors such as InGaN, InN, AlGaN, AlInGaN, etc.) on the buffer layer 2, and a barrier layer 4 made of AlGaN (other substrates such as III-nitride semiconductors such as GaN, InGaN, AlGaN, AlN, AlInGaN, etc.) on the buffer layer 2. The barrier layer 4 has a larger band gap than the channel layer 3. If the barrier layer 4 is AlGaN and the channel layer 3 is GaN, a high-concentration two-dimensional electron gas layer 5 is generated on the channel layer 3 side near the interface 13 between the barrier layer 4 and the channel layer 3 due to the difference in the lattice constants between AlGaN and GaN and the difference in the band gap.

[0017] When various III-nitride semiconductor layers such as the barrier layer 4 and the channel layer 3 are grown using epitaxial growth techniques such as metalorganic chemical vapor deposition (MOCVD), carbon (C) contained in organometallic raw materials such as trimethylgallium (TMG) is incorporated into the III-nitride semiconductor crystal. The C in the III-nitride semiconductor layer acts as an acceptor level in the crystal, increasing the potential of the conduction band and increasing the resistance of the III-nitride semiconductor. However, since the channel layer 3 needs to efficiently flow electrons, it is better to have fewer unnecessary levels and a lower C concentration. Specifically, the C concentration in the channel layer 3 is 1E+18 cm -3Less than 5E+17cm if possible -3 It is desirable that the value be less than or equal to nE+m. m It means that the channel layer 3 does not need to be a single layer, and may have a multi-layer structure such as a so-called double heterostructure in which, for example, an AlGaN layer with low C concentration and low Al composition is combined under a GaN layer with low C concentration. This confines carriers in the upper part of the channel layer 3, improving the pinch-off characteristics.

[0018] A source electrode 6 and a drain electrode 7 are formed on the barrier layer 4, spaced apart from each other. The source electrode 6 and the drain electrode 7 are made of one or a combination of two or more metals such as Ti, Al, Mo, and Hf, which are in ohmic contact with either the two-dimensional electron gas layer 5, the barrier layer 4, or the channel layer 3, and may be electrically connected to the two-dimensional electron gas layer 5. The source electrode 6 and the drain electrode 7 may be, for example, on the upper surface of the barrier layer 4, or may be in contact with either the two-dimensional electron gas layer 5, the barrier layer 4, or the channel layer 3 by using a known ohmic recess technique (not shown).

[0019] The semiconductor laminated structure has a selectively formed gate layer 8 (otherwise, for example, III-nitride semiconductors such as p-InGaN, p-InN, p-AlGaN, and p-AlInGaN) containing p-type impurities (Mg, Zn, C, etc.) on the barrier layer 4, between the source electrode 6 and the drain electrode 7, and spaced apart from the source electrode 6 and the drain electrode 7. The gate layer 8 may be p-GaN containing Mg, i-GaN (insulated-GaN) containing C or the like (otherwise, for example, III-nitride semiconductors such as i-InGaN, i-InGaN, i-InN, i-AlGaN, and i-AlInGaN), or n-GaN containing n-type impurities such as Si (otherwise, for example, III-nitride semiconductors such as n-InGaN, n-AlGaN, n-InN, and n-AlInGaN). The gate layer 8 may be located other than between the source electrode 6 and the drain electrode 7 as shown in FIG. 1. A gate electrode 9 is formed on a part of the gate layer 8 in a region on the barrier layer 4, spaced apart from the source electrode 6 and the drain electrode 7. The gate electrode 9 may be on the gate layer 8 as shown in FIG. 1, or may form a so-called MES (Metal-Semiconductor) structure (not shown) in direct contact with the barrier layer 4 when the gate layer 8 is not present. In the case of the MES structure, the gate electrode is an electrode in Schottky contact with the barrier layer 4. Instead of the gate layer 8 below the gate electrode 9, a so-called MIS (Metal-Insulator-Semiconductor) structure or a MOS (Metal-Oxide-Semiconductor) structure in which an insulating film such as SiNx, SiOx, or AlOx is sandwiched may be used (not shown).

[0020] From the viewpoint of safety, normally-off operation is desired for power semiconductors. When the gate layer 8 is a p-type III-nitride semiconductor, a pn junction is formed directly below the gate layer 8, and the two-dimensional electron gas layer 5 is depleted and the normally-off state is achieved when no gate voltage is applied to the gate electrode 9. The barrier layer 4 at this time differs depending on the threshold voltage (Vth) to be set. When the barrier layer 4 is AlGaN, the thickness of the AlGaN must be within the range of 10 nm to 25 nm, preferably about 20 nm, in a part directly below the gate layer 8 when the Al composition of the AlGaN of the barrier layer 4 is 20%. Also, when the gate layer 8 is p-GaN, the thickness may be within the range of 50 nm to 500 nm, preferably about 100 nm, and when the p-type impurity is Mg, the doping concentration must be 1E+19 cm -3 More than 10E+19cm -3 Within the following range, preferably 5E+19cm -3 It is fine if Mg is 5E+19cm -3 The carrier concentration of p-GaN doped to a certain extent is essentially 1E+17 cm because the activation rate of Mg is very low, at less than a few percent. -3 Above 5E+17cm -3 It is about the following.

[0021] The gate electrode 9 may be an electrode made of one or a combination of two or more metals such as Ti, Ni, Pd, Pt, Au, W, WSi, Ta, TiN, Al, Mo, Hf, Zr, etc. When the gate layer 8 is of p-type, the gate electrode 9 may be in ohmic contact or Schottky contact with the gate layer 8, but since the gate electrode has higher reliability when in ohmic contact, it is preferable to use an electrode made of one or a combination of two or more metals having low contact resistance such as Ni, Pt, Pd, Au, Ti, Cr, In, Sn, Al, etc.

[0022] This semiconductor laminated structure has an element isolation region 10 in which an impurity is implanted into a part of the group III nitride semiconductor layer extending from the barrier layer 4 to the buffer layer 2 to cause crystal defects, inactivate the layer, and increase resistance. The element isolation region 10 is formed so as to surround the active region (FET region) of the group III nitride semiconductor device in a plan view (see FIG. 11). The impurity implanted into the element isolation region 10 is an element that increases the resistance of the group III nitride semiconductor layer. Specifically, it is preferable that the impurity is one or more elements selected from H, He, B, C, N, O, F, Mg, Cl, Ar, Ca, Ti, Cr, Fe, Cu, Zn, As, and R. Furthermore, when the impurity in the element isolation region 10 is implanted by ion implantation, the distribution in the depth direction is not uniform, and the impurity concentration has a peak 12 in the depth direction, and the distribution in the depth direction is approximately normal distribution centered on the peak 12. Furthermore, the peak 12 of the impurity concentration in the depth direction does not need to be one, and may be two or more. Rather, in order to uniformly increase the resistance from the upper surface side of the barrier layer 4 etc. to the deep region of the buffer layer 2 etc. and to inactivate the layer, it is desirable to have two or more impurity concentration peaks 12 in the depth direction. For example, when there are two impurity concentration peaks 12 in the depth direction, the impurity concentration distribution in the depth direction will be as shown in FIG. 1(a). The distribution in the depth direction will be approximately normal distribution centered on each peak, and the overlapping portion will be the sum of the impurity concentrations. In the relationship diagram between impurity concentration and depth shown in FIG. 1(a), the impurity concentration axis is on a logarithmic scale. The depth of the element isolation region 10 is defined as an impurity concentration of 1E+17 cm -3 When the depth is set to 500 nm or more, in order to form the element isolation region 10 so as to reach the buffer layer 2 from the upper surface of the gate layer 8, the element isolation region 10 needs to have a depth of at least 500 nm or more, and preferably a depth of 800 nm or more.

[0023] As shown in FIG. 1, when the element isolation region 10 is also formed in the gate layer 8, it is desirable to inject impurities into the gate layer 8 to cause crystal defects, inactivate the gate layer 8, and increase its resistance from the viewpoint of reducing the gate-source (substrate) capacitance and reducing the gate leakage current. Reducing the gate-source (substrate) capacitance enables the device to operate at a high speed. In addition, when the gate layer 8 is present, the impurity is injected from above the gate layer 8 to the buffer layer 2 in a lump, which reduces costs by performing the injection process once. In this case, the injection depth of the impurity in the element isolation region 10 is the same as that in the area directly below the gate layer 8 and in the area without the gate layer 8 (FIG. 1) because the injection is performed in a lump. Here, the "same depth" means a depth within the range of variation in the injection depth of the impurity at different locations when the impurity is injected in one process, and specifically, one depth is ±20% or less of the other depth, preferably ±10% or less, and more preferably ±5% or less. In addition, in FIG. 1, the gate layer 8 of the element isolation region 10 is depicted as being on the same cross section, but the gate layer 8 of the element isolation region 10 does not need to be on the same cross section, and may be rotated 90 degrees as shown in FIG. 11, or may be rotated at another angle.

[0024] Regarding the impurity concentration at the depth of the channel layer 3 of the element isolation region 10, it is necessary to suppress the amount of impurity injection to a certain extent to reduce crystal defects. If there are too many crystal defects in the channel layer 3, a leakage path is formed through the crystal defects in the channel layer 3 during high-voltage operation or high-temperature operation, and the leakage current flowing therethrough increases over time, causing reliability problems. Therefore, it is necessary to suppress the amount of impurity injection in the element isolation region 10 at a depth in the channel layer 3, particularly on the channel layer 3 side (i.e., the upper side of the channel layer 3) near the interface 13 between the barrier layer 4 where the two-dimensional electron gas layer 5 is formed and the channel layer 3. However, if the amount of impurity injection in the buffer layer 2 is reduced too much, then the drain leakage current (the sum of the leakage currents between the drain and gate, between the drain and source, and between the drain and substrate) and the source leakage current (the leakage current between the drain and source) increase through the buffer layer 2 or through a portion of the element isolation region 10 corresponding to the depth of the lower part of the channel layer 3. In order to solve these conflicting problems, the peak 12 of the impurity concentration in the depth direction is set at a position deeper than the interface 13 between the barrier layer 4 and the channel layer 3, the impurity concentration of the element isolation region 10 at the depth of the interface 13 between the barrier layer 4 and the channel layer 3 is made lower than the impurity concentration of the peak 12 of the impurity concentration in the depth direction, and a certain level of impurity concentration is maintained in the buffer layer 2.

[0025] Fig. 2 is a diagram for explaining in detail the relationship between the impurity concentration and the depth in the element isolation region of the nitride semiconductor device according to the embodiment. One of the peaks 12 of the impurity concentration in the depth direction may be in the channel layer 3 as shown in Fig. 2(b) or in the buffer layer 2 below the channel layer 3 as shown in Fig. 2(c), but it is not desirable for it to be above the interface 13 between the barrier layer 4 and the channel layer 3 as shown in Fig. 2(a). With a distribution such as Fig. 2(a), the amount of impurity implanted in the buffer layer 2 is too low, and the drain leakage current and source leakage current through the buffer layer 2 increase.

[0026] Next, the operation of the present nitride semiconductor device will be described. When the nitride semiconductor device is a normally-off FET using p-GaN for the gate layer 8, the two-dimensional electron gas layer 5 does not exist and the nitride semiconductor device is in an off state when the voltage applied to the gate electrode 9 is 0V because a depletion layer due to the pn junction spreads directly under the gate layer 8 (FIG. 1). When a positive gate voltage is applied to the gate electrode 9 with the source electrode 6 grounded and a positive voltage applied to the drain electrode 7, the depletion layer due to the pn junction directly under the gate layer 8 shrinks, and when the gate voltage exceeds the threshold voltage (Vth), a source-drain current begins to flow, and the nitride semiconductor device is in an on state (not shown). In other words, the source-drain current can be controlled by the voltage applied to the gate electrode 9.

[0027] Next, the effects of the present nitride semiconductor device will be described. The semiconductor stack structure of the present nitride semiconductor device suppresses an increase in drain leakage current or source leakage current through the buffer layer 2 or through the lower part of the channel layer 3 in the element isolation region 10 during high voltage operation or high temperature operation. In addition, it is possible to suppress the leakage current that increases over time through crystal defects in the channel layer 3, thereby improving the reliability characteristics of the nitride semiconductor device.

[0028] Next, a nitride semiconductor device according to a first modification of the embodiment will be described. FIG. 3 is a diagram showing a cross-sectional structure ((b) of FIG. 3) of the nitride semiconductor device according to the first modification of the embodiment, and a relationship between the impurity concentration and the depth in the element isolation region ((a) of FIG. 3). The nitride semiconductor device according to this modification basically includes a semiconductor laminated structure including a substrate 1, a nitride semiconductor layer (high C layer) 11 having a high C (carbon) concentration formed on the substrate 1, a channel layer 3 formed on the high C layer 11 and made of a nitride semiconductor layer having a lower C concentration than the high C layer 11, and a barrier layer 4 formed on the channel layer 3 in direct contact with the channel layer 3, having a larger band gap than the channel layer 3, and made of a nitride semiconductor layer, as shown in FIG. 3(b). In this embodiment, more specifically, the semiconductor laminated structure includes, from the bottom, the substrate 1, the buffer layer 2, the high C layer 11, the channel layer 3, the two-dimensional electron gas layer 5, the barrier layer 4, and the gate layer 8. An element isolation region 10 into which impurities are injected is formed in the semiconductor laminated structure. 3(a), the element isolation region 10 reaches the high C layer 11 from the upper surface side of the semiconductor laminated structure, and is characterized in that the maximum impurity concentration at the depth of the channel layer 3 is 70 times or less than the impurity concentration at the depth of the interface 14 between the high C layer 11 and the channel layer 3. Note that "high C concentration" is a relative expression and means a C concentration higher than the C concentration in the channel layer.

[0029] That is, the high C layer 11, which is a III-nitride semiconductor layer with a high C concentration, is between the buffer layer 2 and the channel layer 3, the element isolation region 10 reaches the high C layer 11 from the upper surface side, and the maximum impurity concentration at the depth of the channel layer 3 is 70 times or less than the impurity concentration at the depth of the interface 14 between the high C layer 11 and the channel layer 3. Note that, although this modification is described using a III-nitride semiconductor, the present invention is not limited thereto. Also, this semiconductor laminated structure shows a minimum configuration, and is not limited thereto.

[0030] This semiconductor laminated structure is different from the embodiment shown in Figs. 1 and 2 in that it has a high C layer 11 (a single layer or multiple layers of high C group III nitride semiconductors such as GaN, AlGaN, AlN, InGaN, InN, AlInGaN, etc.) between the buffer layer 2 and the channel layer 3. C in the group III nitride semiconductor layer acts as an acceptor level in the crystal, increasing the potential of the conduction band and increasing the resistance of the group III nitride semiconductor. Therefore, this high C layer 11 has high resistance. In addition, this semiconductor laminated structure is different from the embodiment shown in Figs. 1 and 2 in that the element isolation region 10, which is made high-resistance by implanting impurities, reaches the high C layer 11 from the upper surface side, and the "maximum impurity concentration at the depth of the channel layer 3" is 70 times or less than the "impurity concentration at the depth of the interface 14 between the high C layer 11 and the channel layer 3".

[0031] As shown in the embodiment shown in FIGS. 1 and 2, the channel layer 3 needs to efficiently pass electrons, so it is preferable that there are fewer unnecessary levels and that the C concentration is low. Specifically, the C concentration in the channel layer 3 is 1E+18 cm -3 Less than 5E+17cm if possible -3 On the other hand, in order to reduce the drain-substrate leakage current, the high C layer 11 has a C concentration of 1E+18 cm -3 Above, 1E+19cm if possible -3 It is preferable that the above value is satisfied. This makes it possible to suppress leakage current to the buffer layer 2 side. Furthermore, the high C layer 11 may be made of a group III nitride semiconductor having a larger band gap than the channel layer 3. This allows carriers to be confined in the channel layer 3, improving the pinch-off characteristics.

[0032] FIG. 4 is a diagram for explaining in detail the relationship between the impurity concentration and the depth in the element isolation region of the nitride semiconductor device according to the first modified example of the embodiment. One of the peaks 12 of the impurity concentration in the element isolation region 10 in the depth direction may be in the channel layer 3 as shown in FIG. 4(b) or in the high C layer 11 below the channel layer 3 as shown in FIG. 4(c). However, it is not desirable to be above the interface 13 between the barrier layer 4 and the channel layer 3 as shown in FIG. 4(a). In the distribution as shown in FIG. 4(a), the amount of impurity implanted in the high C layer 11 is too low, and the drain leakage current and the source leakage current through the high C layer 11 and the buffer layer 2 increase. The bottom surface of the element isolation region 10 does not need to stop at the high C layer 11, and may reach the buffer layer 2 as shown in FIG. 4(c). In that case, the drain leakage current and the source leakage current can be further reduced.

[0033] FIG. 5 is a diagram showing the characteristics of a nitride semiconductor device according to a first modified example of the embodiment. More specifically, FIG. 5 shows the correlation between the ratio of the "maximum impurity concentration at the depth of the channel layer 3" to the "impurity concentration at the depth of the interface 14 between the high C layer 11 and the channel layer 3" (the numerator is the maximum impurity concentration at the depth of the channel layer 3) and the reliability life. The smaller this ratio is, the lower the "maximum impurity concentration at the depth of the channel layer 3" is compared with the "impurity concentration at the depth of the interface 14 between the high C layer 11 and the channel layer 3". The reliability life here is the life in an accelerated test at high temperature operation (for example, 150° C. or higher) and high voltage operation (for example, drain voltage 600 V or higher) in an off state (a state in which a part of the two-dimensional electron gas layer 5 immediately below the gate layer 8 is depleted). From FIG. 5, it can be seen that the smaller this impurity concentration ratio is, the longer the reliability life is, and when it is 70 times or less, it is significantly improved. This indicates that by suppressing the amount of impurities injected into the channel layer 3, crystal defects in the channel layer 3 can be suppressed, and the leakage current that increases over time through the crystal defects in the channel layer 3 can be suppressed, thereby improving the reliability characteristics of the nitride semiconductor device.

[0034] By using this semiconductor laminated structure, it is possible to obtain the same effect as that of the first embodiment. In addition, in this semiconductor laminated structure, since the element isolation region 10 reaches the high-resistance high-C layer 11 from the upper surface side, the active region other than the element isolation region 10 is surrounded by the element isolation region 10 in the horizontal direction and the high-resistance high-C layer 11 in the vertical (downward) direction, and is completely surrounded in all directions. Therefore, compared to the embodiment, it is possible to further suppress the drain leakage current and the source leakage current through the buffer layer 2 and the high-C layer 11, or through the lower part of the channel layer 3 of the element isolation region 10. In addition, since the maximum impurity concentration at the depth of the channel layer 3 is 70 times or less than the impurity concentration at the depth of the interface between the high-C layer 11 and the channel layer 3, it is possible to suppress the crystal defects of the channel layer 3. As a result, it is possible to suppress the leakage current that increases over time through the crystal defects of the channel layer 3 in the element isolation region 10, and it is possible to further improve the reliability characteristics of the nitride semiconductor device compared to the first embodiment.

[0035] Next, a nitride semiconductor device according to a second modification of the embodiment will be described. The same drawings as those of the first modification will be used for the description. FIG. 3 shows a cross-sectional structure ((b) of FIG. 3) of the nitride semiconductor device according to the second modification of the embodiment, and a relationship between the impurity concentration and the depth in the element isolation region ((a) of FIG. 3). The nitride semiconductor device according to this modification basically has the same configuration as the nitride semiconductor device according to the first modification of the embodiment. However, the element isolation region 10 of the nitride semiconductor device reaches the high C layer 11 from the upper surface side of the semiconductor laminated structure as shown in (a) of FIG. 3, and is characterized in that the maximum impurity concentration at the depth of the interface 13 between the barrier layer 4 and the channel layer 3 is 40 times or less than the impurity concentration at the depth of the interface 14 between the high C layer 11 and the channel layer 3.

[0036] That is, the high C layer 11 is between the buffer layer 2 and the channel layer 3, the element isolation region 10 reaches the high C layer 11 from the upper surface side, and the impurity concentration at the depth of the interface 13 between the barrier layer 4 and the channel layer 3 is 40 times or less than the impurity concentration at the depth of the interface 14 between the high C layer 11 and the channel layer 3. In addition, although the present modification is described using a Group III nitride semiconductor, the present invention is not limited thereto. In addition, the present semiconductor laminated structure shows a minimum configuration, and is not limited thereto.

[0037] The present semiconductor laminated structure is different from the embodiment shown in Figs. 1 and 2 in that it has a high C layer 11 (a single layer or multiple layers of high C group III nitride semiconductors such as GaN, AlGaN, AlN, InGaN, InN, AlInGaN, etc.) between the buffer layer 2 and the channel layer 3. C in the group III nitride semiconductor layer acts as an acceptor level in the crystal, increasing the potential of the conduction band and increasing the resistance of the group III nitride semiconductor. Therefore, the high C layer 11 has high resistance. In addition, the present semiconductor laminated structure is different from the embodiment shown in Figs. 1 and 2 in that the element isolation region 10, which is made high-resistance by doping impurities, reaches the high C layer 11 from the upper surface side, and the impurity concentration at the depth of the interface 13 between the barrier layer 4 and the channel layer 3 is 40 times or less than the impurity concentration at the depth of the interface 14 between the high C layer 11 and the channel layer 3.

[0038] As shown in the embodiment shown in FIGS. 1 and 2, the channel layer 3 needs to efficiently pass electrons, so it is preferable that there are fewer unnecessary levels and that the C concentration is low. Specifically, the C concentration in the channel layer 3 is 1E+18 cm -3 Less than 5E+17cm if possible -3 On the other hand, in order to reduce the drain-substrate leakage current, the high C layer 11 has a C concentration of 1E+18 cm -3 Above, 1E+19cm if possible -3It is preferable that the above value is satisfied. This makes it possible to suppress leakage current to the buffer layer 2 side. Furthermore, the high C layer 11 may be made of a group III nitride semiconductor having a larger band gap than the channel layer 3. This allows carriers to be confined in the channel layer 3, improving the pinch-off characteristics.

[0039] One of the peaks 12 of the impurity concentration in the depth direction of the element isolation region 10 may be in the channel layer 3 as shown in FIG. 4(b) or in the high C layer 11 below the channel layer 3 as shown in FIG. 4(c). However, it is not desirable for the peak to be above the interface 13 between the barrier layer 4 and the channel layer 3 as shown in FIG. 4(a). In the distribution as shown in FIG. 4(a), the amount of impurity implanted in the high C layer 11 is too low, and the drain leakage current and source leakage current through the high C layer 11 and the buffer layer 2 increase. The bottom surface of the element isolation region 10 does not need to stop at the high C layer 11, and may reach the buffer layer 2 as shown in FIG. 4(c). In that case, the drain leakage current and source leakage current can be further reduced.

[0040] FIG. 6 is a diagram showing the characteristics of a nitride semiconductor device according to a second modified example of the embodiment. More specifically, FIG. 6 shows the correlation between the ratio of "impurity concentration at the depth of interface 13 between barrier layer 4 and channel layer 3" to "impurity concentration at the depth of interface 14 between high C layer 11 and channel layer 3" (the numerator is the impurity concentration at interface 13 between barrier layer 4 and channel layer 3) and the reliability life. The smaller this ratio is, the lower the "impurity concentration at the depth of interface 13 between barrier layer 4 and channel layer 3" is compared with the "impurity concentration at the depth of interface 14 between high C layer 11 and channel layer 3". The reliability life here is the life in an accelerated test at high temperature operation (for example, 150° C. or higher) and high voltage operation (for example, drain voltage 600 V or higher) in an off state (a state in which a part of the two-dimensional electron gas layer 5 immediately below the gate layer is depleted). From FIG. 6, it can be seen that the smaller this impurity concentration ratio is, the longer the reliability life is, and when it is 40 times or less, it is significantly improved. This indicates that by suppressing the amount of impurities injected into the channel layer 3, particularly into the region of the channel layer 3 close to the barrier layer 4, i.e., the region of the two-dimensional electron gas layer 5 where electrons easily flow, crystal defects in this region can be suppressed, and as a result, the leakage current that increases over time through crystal defects in the channel layer 3 in the element isolation region 10 is suppressed, thereby improving the reliability characteristics of the nitride semiconductor device.

[0041] The semiconductor laminated structure of the present invention can provide the same effect as that of the embodiment. In addition, in the semiconductor laminated structure of the present invention, the element isolation region 10 reaches the high-C layer 11 having high resistance from the upper surface side, so that the active region other than the element isolation region 10 is surrounded by the element isolation region 10 in the horizontal direction and the high-C layer 11 in the vertical (downward) direction, and is completely surrounded in all directions. Therefore, compared to the embodiment, it is possible to further suppress the drain leakage current and the source leakage current through the buffer layer 2 or the high-C layer 11, or through the lower part of the channel layer 3 of the element isolation region 10. In addition, since the impurity concentration at the depth of the interface 13 between the barrier layer 4 and the channel layer 3 is 40 times or less than the impurity concentration at the depth of the interface between the high-C layer 11 and the channel layer 3, it is possible to suppress the crystal defects in the region of the channel layer 3 close to the barrier layer 4. As a result, it is possible to effectively suppress the leakage current that increases over time through the crystal defects in the channel layer 3, and it is possible to further improve the reliability characteristics of the nitride semiconductor device compared to the embodiment.

[0042] Next, a nitride semiconductor device according to a third modification of the embodiment will be described. In the present semiconductor stacked structure, in the embodiment shown in FIGS. 1 to 4, the maximum impurity concentration at the depth of the channel layer 3 in the element isolation region 10 is 6E+19 cm -3 The present invention is characterized by the following. In addition, although the present modification is described using a group III nitride semiconductor, the present invention is not limited thereto. In addition, the present semiconductor laminated structure shows a minimum configuration, and is not limited thereto.

[0043] 7 is a diagram showing the characteristics of a nitride semiconductor device according to a third modified example of the embodiment. More specifically, FIG. 7 shows the correlation between the maximum impurity concentration at the depth of the channel layer 3 in the element isolation region 10 and the reliability life. As can be seen from FIG. 7, the smaller the maximum impurity concentration at the depth of the channel layer 3, the longer the reliability life. -3It can be seen that the reliability is significantly improved below 1000 V. This indicates that by suppressing the amount of impurities injected into the channel layer 3, crystal defects in this region can be suppressed, and as a result, the leakage current that increases over time through the crystal defects in the channel layer 3 is suppressed, improving the reliability characteristics of the nitride semiconductor device. Note that the reliability life here refers to the life in an accelerated test in an off state (a state in which there are no carriers in a portion directly below the gate layer), during high temperature operation (e.g., 150° C. or higher) and high voltage operation (e.g., drain voltage 600 V or higher).

[0044] This semiconductor laminated structure can provide the same effects as those of the embodiment, the first modification, and the second modification. -3 or less, crystal defects in the channel layer can be suppressed, and as a result, the leakage current that increases over time through crystal defects in the channel layer 3 can be effectively suppressed, and the reliability characteristics of the nitride semiconductor device can be further improved compared to the embodiment, the first modified example, and the second modified example.

[0045] Next, a nitride semiconductor device according to a fourth modification of the embodiment will be described. In the present semiconductor stacked structure, in the embodiment shown in FIGS. 1 to 4, the impurity concentration at the depth of the interface between the barrier layer 4 and the channel layer 3 in the element isolation region 10 is 3E+19 cm -3 The present invention is characterized by the following. In addition, although the present modification is described using a group III nitride semiconductor, the present invention is not limited thereto. In addition, the present semiconductor laminated structure shows a minimum configuration, and is not limited thereto.

[0046] 8 is a diagram showing characteristics of a nitride semiconductor device according to a fourth modification of the embodiment. More specifically, FIG. 8 shows a correlation between the impurity concentration at the depth of the interface between the barrier layer 4 and the channel layer 3 in the element isolation region 10 and the reliability life. As shown in FIG. 8, the lower the impurity concentration at the interface between the barrier layer 4 and the channel layer 3, the longer the reliability life. -3It can be seen that the reliability is significantly improved below. This shows that by suppressing the amount of impurities injected into the channel layer 3, particularly into the region of the channel layer 3 close to the barrier layer 4, i.e., the region of the two-dimensional electron gas layer 5 where electrons easily flow, and into the interface between the barrier layer 4 and the channel layer 3, crystal defects in this region can be suppressed, and as a result, the leakage current that increases over time through the crystal defects in the channel layer 3 is suppressed, and the reliability characteristics of the nitride semiconductor device are improved. Note that the reliability life referred to here is the life in an accelerated test in an off state (a state in which there are no carriers in a part directly below the gate layer), during high temperature operation (for example, 150° C. or higher) and high voltage operation (for example, drain voltage 600 V or higher).

[0047] This semiconductor laminated structure can provide the same effects as those of the embodiment, the first modification, and the second modification. In addition, the impurity concentration at the depth of the interface between the barrier layer 4 and the channel layer 3 is 3E+19 cm -3 Since this is equal to or less than this, crystal defects in the two-dimensional electron gas layer 5 region in the channel layer can be suppressed, and as a result, the leakage current that increases over time through crystal defects in the channel layer 3 can be effectively suppressed, and the reliability characteristics of the nitride semiconductor device can be further improved compared to the embodiment, the first variant, and the second variant.

[0048] Next, a nitride semiconductor device according to a fifth modification of the embodiment will be described. In this semiconductor stacked structure, in the modification of the embodiment shown in FIGS. 3 and 4, the impurity concentration at the depth of the interface 14 between the high C layer 11 and the channel layer 3 is 5E+17 cm -3 The above is a characteristic of the present invention. In addition, although the present modified example is described using a group III nitride semiconductor, the present invention is not limited thereto. In addition, the present semiconductor laminated structure shows a minimum configuration, and is not limited thereto.

[0049] Fig. 9 is a diagram showing characteristics of a nitride semiconductor device according to a fifth modified example of the embodiment. More specifically, Fig. 9 shows the correlation between the impurity concentration at the depth of interface 14 between high C layer 11 and channel layer 3 in element isolation region 10 and the source leakage current under high temperature and high voltage. Note that the high temperature and high voltage referred to here are, for example, an off state, 150°C or higher, and a drain voltage of 600V or higher. Fig. 9 shows that the smaller the impurity concentration at the depth of interface 14 between high C layer 11 and channel layer 3, the higher the source leakage current, and that when the impurity concentration is 5E+17cm -3 It can be seen that the impurity concentration at the depth of the interface 14 between the high C layer 11 and the channel layer 3 in the element isolation region 10 is significantly increased below 5E+17 cm. This is because the amount and depth of the impurity implanted near the interface 14 between the high C layer 11 and the channel layer 3 in the element isolation region 10 is insufficient, so that the lower region of the channel layer 3 in the element isolation region 10 is not sufficiently inactivated and made highly resistant, and a source leakage current occurs via the lower region of the channel layer 3 in the element isolation region 10 under high temperature and high voltage conditions. Therefore, the impurity concentration at the depth of the interface 14 between the high C layer 11 and the channel layer 3 is 5E+17 cm. -3 More than this is desirable.

[0050] This semiconductor laminated structure can provide the same effects as those of the first, second, third and fourth modifications. In addition, the impurity concentration at the depth of the interface 14 between the high C layer 11 and the channel layer 3 is 5E+17 cm -3 For the above reasons, the occurrence of source leakage current that flows via the lower region of channel layer 3 under high temperature and high voltage conditions can be suppressed, and the reliability characteristics of the nitride semiconductor device can be further improved.

[0051] Next, cross-sectional views showing a method for manufacturing the nitride semiconductor device shown in Figs. 1 to 4 are shown in Fig. 10. Note that this manufacturing method describes a minimum configuration, and is not limited to this. Also, the order of this manufacturing method is not limited to this. Note that the manufacturing method of the nitride semiconductor device shown in Figs. 1 and 2 corresponds to the manufacturing method shown in Fig. 10 in which the high C layer 11 is not epitaxially grown between the buffer layer 2 and the channel layer 3 (not shown).

[0052] First, a suitable (111) Si substrate 1 (or other substrates such as sapphire, SiC, GaN, AlN, etc.) is prepared. On the substrate 1, a suitable buffer layer 2 (for example, a single layer or multiple layers of a group III nitride semiconductor such as GaN, AlGaN, AlN, InGaN, InN, AlInGaN, etc.) is formed using a known epitaxial growth technique such as MOCVD, and a high C layer 11 (for example, a single layer or multiple layers of a high C group III nitride semiconductor such as GaN, AlGaN, AlN, InGaN, InN, AlInGaN, etc.) is formed thereon. On the channel layer 3 made of GaN (for example, a single layer or multiple layers of a group III nitride semiconductor such as InGaN, InN, AlGaN, AlInGaN, etc.) is formed thereon. On the channel layer 3 made of GaN (for example, a single layer or multiple layers of a group III nitride semiconductor such as InGaN, InN, AlGaN, AlInGaN, etc.) is formed. On the channel layer 4 made of AlGaN (for example, a group III nitride semiconductor such as GaN, InGaN, AlGaN, AlN, AlInGaN, etc.) is formed. A cap layer 15 made of p-GaN (other group III nitride semiconductors such as p-InGaN, p-InN, p-AlGaN, and p-AlInGaN) is formed thereon (FIG. 10(a)).

[0053] The cap layer 15 may be p-GaN containing Mg, i-GaN (insulated-GaN, other group III nitride semiconductors such as i-InGaN, i-InN, i-AlGaN, i-AlInGaN, etc.) containing C or the like, or n-GaN (other group III nitride semiconductors such as n-InGaN, n-InN, n-AlGaN, n-AlInGaN, etc.) containing n-type impurities such as Si. Since the channel layer 3 needs to efficiently pass electrons, it is preferable that there are fewer unnecessary levels and that the C concentration is low. Specifically, the C concentration in the channel layer 3 is 1E+18 cm -3 Less than 5E+17cm if possible -3 On the other hand, in order to increase the resistance of the high C layer 11 and reduce the drain-substrate leakage current, the C concentration is preferably 1E+18 cm -3 Above, 1E+19cm if possible -3It is preferable that the thickness of the barrier layer 4 is 10 nm or more, and preferably about 20 nm. The C concentration in the III-nitride semiconductor layer is adjusted by changing the growth temperature, growth rate, growth pressure, gas flow rate, and the like. When the cap layer 15 is a p-type III-nitride semiconductor, a pn junction is formed directly below the cap layer 15, and the two-dimensional electron gas layer 5 is depleted and becomes normally-off when no gate voltage is applied to the gate electrode 9. The barrier layer 4 at this time varies depending on the threshold voltage (Vth) to be set. When the barrier layer 4 is AlGaN, the thickness of the AlGaN must be within the range of 10 nm to 25 nm, and preferably about 20 nm, in a part directly below the gate layer 8, when the Al composition of the AlGaN of the barrier layer 4 is 20%. When the cap layer 15 is p-GaN, the thickness may be within the range of 50 nm to 500 nm, and preferably about 100 nm. When the p-type impurity is Mg, the doping concentration is 1E+19 cm -3 More than 10E+19cm -3 Within the following range, preferably 5E+19cm -3 It is fine if Mg is 5E+19cm -3 The carrier concentration of p-GaN doped to a certain extent is essentially 1E+17 cm because the activation rate of Mg is very low, at less than a few percent. -3 Above 5E+17cm -3 It is about the following.

[0054] Next, a resist pattern 16 is formed using a known photolithography technique, and a known ion implantation technique is used to implant impurities 17 into a portion of the upper surface side of the cap layer 15 to cause crystal defects, inactivate the cap layer, and form an isolation region 10 with high resistance (FIG. 10(b)). The impurities 17 implanted into the isolation region 10 are elements that increase the resistance of the III nitride semiconductor layer. Specifically, it is preferable that the impurities 17 are one or more of H, He, B, C, N, O, F, Mg, Cl, Ar, Ca, Ti, Cr, Fe, Cu, Zn, As, and Ru. It is preferable that the ion implantation is performed with a tilt of slightly less than 10° from the c-axis direction of the III nitride semiconductor crystal so that the implanted impurities 17 hit the crystal lattice or crystal atoms and are retained in the crystal. The implantation depth is adjusted so that the implantation energy and the implantation dose reach the high C layer 11 from the upper surface side of the cap layer 15 (so that the buffer layer 2 is reached (not shown) in the manufacturing method of the structure shown in FIGS. 1-2). The depth of the element isolation region 10 is defined as "the impurity concentration is 1E+17 cm -3 When the depth is set to "a depth of at least 500 nm", in order to form the element isolation region 10 so as to reach the high C layer 11 from the upper surface of the cap layer 15, the element isolation region 10 needs to be at least 500 nm deep, preferably 800 nm deep. For this purpose, it is necessary to inject the impurities at a fairly high energy, and an injection energy of 100 keV or more, preferably 180 keV or more is required. When the impurities 17 are injected once into the III-nitride semiconductor layer by ion implantation, the distribution in the depth direction is not uniform, and the impurity concentration has a peak in the depth direction, and the distribution in the depth direction is approximately normal distribution centered on the peak. Therefore, in order to inactivate the impurities by uniformly increasing the resistance from the upper surface side of the cap layer 15 etc. to the deep region of the high C layer 11 etc., it is desirable to have two or more impurity concentration peaks in the depth direction. Since each peak is formed by one ion implantation, the same resist pattern 16 is used to perform ion implantation multiple times with different injection energies and doses. For example, 1E+14 cm at 50 keV is used. -3 , 3E+14cm at 100keV -3 , 5E+14cm at 200keV -3 Inject three times in this manner.

[0055] Subsequently, the resist pattern 16 is removed using a known oxygen ashing technique or an organic resist removal technique (not shown). Next, a resist pattern 18 is formed using a known photolithography technique, and the cap layer 15 is selectively removed using a known dry etching technique to form a gate layer 8 (otherwise, for example, a group III nitride semiconductor such as p-InGaN, p-AlGaN, p-AlInGaN, i-GaN, i-InGaN, i-InGaN, i-AlGaN, i-AlInGaN, n-GaN, n-InGaN, n-AlGaN, n-AlInGaN, etc.) (FIG. 10(c)).

[0056] Subsequently, the resist pattern 18 is removed using a known oxygen ashing technique or an organic resist removal technique (not shown).

[0057] Next, when the gate layer 8 contains Mg as a p-type impurity, activation annealing is performed for about 30 minutes in nitrogen gas at a temperature of 800°C to activate the Mg (not shown). This activation annealing breaks the hydrogen bonds that inactivate the p-type element Mg, improving the activation rate of Mg, and the gate layer 8 containing the p-type impurity forms a depletion layer due to the pn junction, depleting the two-dimensional electron gas layer 5 directly below. As a result, the threshold voltage of the gate layer 8 acting as the gate of the transistor becomes positive, resulting in a normally-off operation.

[0058] Next, the source electrode 6 and the drain electrode 7 are formed at a distance from the gate layer 8 by using a known photolithography technique, deposition technique, lift-off technique, sputtering technique, dry etching technique, or the like (FIG. 10(d)). The source electrode 6 and the drain electrode 7 are made of an electrode made of one or a combination of two or more metals such as Ti, Al, Mo, and Hf that are in ohmic contact with either the two-dimensional electron gas layer 5, the barrier layer 4, or the channel layer 3, and may be electrically connected to the two-dimensional electron gas layer 5. The source electrode 6 and the drain electrode 7 may be formed, for example, on the upper surface of the barrier layer 4, and may be in contact with a part of the two-dimensional electron gas layer 5, the barrier layer 4, or the channel layer 3 by using a known ohmic recess technique (not shown). The source electrode 6 and the drain electrode 7 may be annealed to reduce contact resistance.

[0059] Finally, the gate electrode 9 is formed by using known photolithography, deposition, lift-off, sputtering, dry etching, etc. (FIG. 10(e)). The gate electrode 9 may be an electrode made of one or a combination of two or more metals such as Ti, Ni, Pd, Pt, Au, W, WSi, Ta, TiN, Al, Mo, Hf, Zr, etc. However, when the gate layer 8 is p-type, the gate electrode 9 may be in ohmic contact or Schottky contact with the gate layer 8. However, since the gate electrode has higher reliability when the gate layer 8 is in ohmic contact, it is preferable to use an electrode made of one or a combination of two or more metals having low contact resistance such as Ni, Pt, Pd, Au, Ti, Cr, In, Sn, Al, etc.

[0060] Next, Fig. 11 shows a plan view illustrating the planar structure of the nitride semiconductor device shown in Figs. 1 to 4. Fig. 11 is a plan view of Figs. 1 to 4 seen from above, and is a plan view seen from above at the point of time of Fig. 10(d) where the source electrode 6 and the drain electrode 7 have been formed. The gate layer 8 used in this description uses p-GaN, and has a FET structure that operates normally off. This nitride semiconductor device shows a minimum configuration, and is not limited to this.

[0061] The gate layer 8 is formed so as to surround the source electrode 6. This forms a normally-off pn junction between the source and drain directly below the gate layer 8, thereby blocking the leak path between the source and drain when the device is off, thereby reducing the source-drain leak current. The gate layer 8 is also aggregated at the gate aggregated portion 19 (aggregated on the left side in the figure). The gate aggregated portion 19 is connected to the gate pad of the element isolation region 10 (not shown). The element isolation region 10 is located outside the source electrode 6, the drain electrode 7, and the gate layer 8, but a part of the end of the aggregated gate layer 8 (left side in the figure) and the gate aggregated portion 19 form the element isolation region 10. The source electrode 6 and the drain electrode 7 are repeatedly formed in a plurality of sets as shown in FIG. 11, but it is preferable in terms of reliability to use the source electrode 6 as the outermost electrode (upper and lower sides in FIG. 11) because this can ease the electric field distribution with the outside of the element isolation region 10.

[0062] Although the nitride semiconductor device and the manufacturing method thereof according to the present invention have been described above based on the embodiment and modifications 1 to 5, the present invention is not limited to these embodiment and modifications 1 to 5. As long as they do not deviate from the gist of the present invention, various modifications conceived by a person skilled in the art to the embodiment and modifications 1 to 5, and other forms constructed by combining some of the components in the embodiment and modifications 1 to 5 are also included within the scope of the present invention. [Industrial Applicability]

[0063] The present invention can be used as a nitride semiconductor device, in particular as a nitride semiconductor device that reduces drain leakage current and source leakage current under high temperature and high voltage conditions, improves reliability, and thereby improves the performance of a power device. [Explanation of symbols]

[0064] 1 Board 2. Buffer layer 3. Channel Layer 4. Barrier Layer 5 Two-dimensional electron gas layer 6 Source Electrode 7 Drain electrode 8 Gate Layer 9 Gate electrode 10. Element isolation region 11 High C layer 12 Impurity concentration peak in the depth direction 13. Interface between barrier layer and channel layer 14 Interface between channel layer and high C layer 15 Cap Layer 16, 18 Resist pattern 17 Impurities 19 Gate consolidation section

Claims

1. A substrate; a high carbon (C) concentration nitride semiconductor layer formed on the substrate, the carbon (C) concentration being 1E+18 cm −3 or more; a channel layer formed on the high C concentration nitride semiconductor layer and having a lower C concentration than the high C concentration nitride semiconductor layer; a barrier layer formed on and in direct contact with the channel layer, the barrier layer having a larger band gap than the channel layer and made of a nitride semiconductor layer; An element isolation region into which an impurity is implanted is formed in the semiconductor laminate structure, the element isolation region extends from an upper surface side of the semiconductor stack to the high C concentration nitride semiconductor layer, The maximum concentration of the impurity at a depth of the channel layer is 70 times or less than the concentration of the impurity at a depth of the interface between the high C concentration nitride semiconductor layer and the channel layer. Nitride semiconductor devices.

2. A substrate; a high carbon (C) concentration nitride semiconductor layer formed on the substrate, the carbon (C) concentration being 1E+18 cm −3 or more; a channel layer formed on the high C concentration nitride semiconductor layer and having a lower C concentration than the high C concentration nitride semiconductor layer; a barrier layer formed on and in direct contact with the channel layer, the barrier layer having a larger band gap than the channel layer and made of a nitride semiconductor layer; An element isolation region into which an impurity is implanted is formed in the semiconductor laminated structure, the element isolation region extends from an upper surface side of the semiconductor stack to the high C concentration nitride semiconductor layer, The concentration of the impurity at a depth of the interface between the barrier layer and the channel layer is 40 times or less than the concentration of the impurity at a depth of the interface between the high C concentration nitride semiconductor layer and the channel layer. Nitride semiconductor devices.

3. The maximum concentration of the impurity in the channel layer is 6E+19 cm -3 Is less than or equal to The nitride semiconductor device according to claim 1 .

4. The concentration of the impurity at a depth of the interface between the barrier layer and the channel layer is 3E+19 cm -3 Is less than or equal to The nitride semiconductor device according to claim 1 .

5. The semiconductor stack further includes a gate layer formed on a portion of the barrier layer and made of a p-type nitride semiconductor, The impurities are also present in the gate layer. The nitride semiconductor device according to any one of claims 1 to 4.

6. The depth of the impurity directly below the gate layer is the same as the depth of the impurity in a region where the gate layer is not present. The nitride semiconductor device according to claim 5 .

7. The concentration of the impurity at a depth of the interface between the high C concentration nitride semiconductor layer and the channel layer is 5E+17 cm -3 That's all. The nitride semiconductor device according to any one of claims 1 to 6.

8. The C concentration of the high C concentration nitride semiconductor layer is 1E+18 cm -3 That's all. The C concentration of the channel layer is 1E+18 cm -3 is less than The nitride semiconductor device according to any one of claims 1 to 7.

9. The impurities are one or more of the following elements: H, He, B, C, O, F, Mg, Cl, Ar, Ca, Ti, Cr, Fe, Cu, Zn, As, and Ru. The nitride semiconductor device according to any one of claims 1 to 8.

10. a step of forming a semiconductor laminated structure by preparing a substrate, forming a high carbon (C) concentration nitride semiconductor layer having a C (carbon) concentration of 1E+18 cm −3 or more on the substrate, forming a channel layer made of a nitride semiconductor layer on the high carbon concentration nitride semiconductor layer, and forming a barrier layer made of a nitride semiconductor layer having a larger band gap than the channel layer on the channel layer; and forming an element isolation region by injecting impurities from above the semiconductor laminated structure, In the step of forming the element isolation region, The impurity is injected so that the element isolation region reaches the high C concentration nitride semiconductor layer from the upper surface side of the semiconductor stacked structure; The impurity is implanted so that the maximum concentration of the impurity in the channel layer becomes 70 times or less than the concentration of the impurity at a depth of the interface between the high C concentration nitride semiconductor layer and the channel layer. A method for manufacturing a nitride semiconductor device.

11. a step of forming a semiconductor laminated structure by preparing a substrate, forming a high carbon (C) concentration nitride semiconductor layer having a C (carbon) concentration of 1E+18 cm −3 or more on the substrate, forming a channel layer made of a nitride semiconductor layer on the high carbon concentration nitride semiconductor layer, and forming a barrier layer made of a nitride semiconductor layer having a larger band gap than the channel layer on the channel layer; and forming an element isolation region by injecting impurities from above the semiconductor laminated structure, In the step of forming the element isolation region, The impurity is injected so that the element isolation region reaches the high C concentration nitride semiconductor layer from the upper surface side of the semiconductor stacked structure; The impurity is implanted so that the concentration of the impurity at a depth of the interface between the barrier layer and the channel layer is 40 times or less than the concentration of the impurity at a depth of the interface between the high C concentration nitride semiconductor layer and the channel layer. A method for manufacturing a nitride semiconductor device.

Citation Information

Patent Citations

  • Semiconductor device and its manufacturing method

    JP2004095640A

  • Semiconductor device and method of manufacturing the same

    JP2013235873A

  • Heterojunction field effect transistor and manufacturing thereof

    JP2014099523A

  • Nitride semiconductor device and method for manufacturing same

    WO2018180021A1