Epoxy resin composition and optical semiconductor device

The epoxy resin composition with crystalline silica and titanium oxide fillers addresses low transmittance and expansion issues, enhancing the performance of side-type photocouplers by maintaining high light transmission and reducing peeling and oxidation.

JP7584079B2Active Publication Date: 2024-11-15PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020109987
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-06-25
Publication Date
2024-11-15
Estimated Expiration
2040-06-25

AI Technical Summary

Technical Problem

Conventional sealing materials for side-type photocouplers result in low light transmittance and increased linear expansion coefficient differences, leading to peeling and oxidation issues, which affect the optical semiconductor device's performance.

Method used

An epoxy resin composition containing crystalline silica and titanium oxide as fillers, along with a curing agent, to maintain a low linear expansion coefficient while enhancing transmittance.

Benefits of technology

The composition achieves high transmittance and low linear expansion, reducing peeling and oxidation, thereby improving the optical semiconductor device's performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007584079000002
    Figure 0007584079000002
  • Figure 0007584079000001
    Figure 0007584079000001
Patent Text Reader

Abstract

To provide an epoxy resin composition that retains a low linear expansion coefficient and yet gives a cured product having a high transmittance.SOLUTION: An epoxy resin composition contains an epoxy resin (A), a curing agent (B) and a filler (C). The filler (C) contains crystalline silica (c1) and titanium oxide (c2).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an epoxy resin composition and an optical semiconductor device, and more particularly to an epoxy resin composition containing an epoxy resin, a curing agent and a filler, and an optical semiconductor device including an encapsulant made from the epoxy resin composition. [Background technology]

[0002] A photocoupler is an optical semiconductor device that transmits an optical signal from a light-emitting element, which is an optical semiconductor element, to a light-receiving element, thereby enabling transmission of an electrical signal while achieving electrical insulation. Conventional photocouplers are of the opposed type in which the light-emitting element and the light-receiving element face each other, and the material used to seal the light-emitting element and the light-receiving element is generally a composition containing an epoxy resin and fused silica as a filler (see Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2009-29926 A Summary of the Invention [Problem to be solved by the invention]

[0004] Since such a facing type photocoupler has a complex structure and is costly to manufacture, recently, a side-type photocoupler in which a light-emitting element and a light-receiving element are arranged in parallel has been considered. However, when the conventional sealing material is used, the transmittance level of the light transmitted from the light-emitting element to the light-receiving element is low, and therefore, there is a problem that the characteristics of the optical semiconductor device cannot be fully satisfied.

[0005] Although the transmittance can be improved by reducing the amount of filler in the encapsulating material, the difference in linear expansion coefficient between the encapsulating material and the package member of the optical semiconductor device becomes large, which may cause peeling inside the package after molding, and the peeled area is prone to oxidation, resulting in discoloration and a decrease in transmittance. Therefore, it is necessary to improve the transmittance of the encapsulating material while maintaining a low linear expansion coefficient in accordance with the package member.

[0006] An object of the present disclosure is to provide an epoxy resin composition that maintains a low linear expansion coefficient and has high transmittance when cured, and an optical semiconductor device including an encapsulant made from this epoxy resin composition. [Means for solving the problem]

[0007] An epoxy resin composition according to one embodiment of the present disclosure is an epoxy resin composition containing an epoxy resin (A), a curing agent (B) and a filler (C). The filler (C) contains crystalline silica (c1) and titanium oxide (c2).

[0008] An optical semiconductor device according to one aspect of the present disclosure includes an optical semiconductor element and an encapsulant that encapsulates the optical semiconductor element. The encapsulant includes a cured product of the resin composition. Effect of the Invention

[0009] According to the present disclosure, it is possible to provide an epoxy resin composition that maintains a low linear expansion coefficient and has high transmittance when cured, and an optical semiconductor device including an encapsulant made from this epoxy resin composition. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a schematic cross-sectional view of an optical semiconductor device according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] 1. Overview The epoxy resin composition according to this embodiment (hereinafter also referred to as composition (X)) contains an epoxy resin (A), a curing agent (B) and a filler (C). The filler (C) contains crystalline silica (c1) and titanium oxide (c2).

[0012] According to this embodiment, the composition (X) can reduce the linear expansion coefficient, and the difference in the linear expansion coefficient between the optical semiconductor device and the package member can be reduced. Therefore, peeling is unlikely to occur inside the package during molding of the optical semiconductor device, and the decrease in transmittance caused by peeling can be suppressed. In addition, the composition (X) can increase the transmittance of the cured product. Therefore, the composition (X) can be used as an encapsulating material in, for example, a side-type photocoupler, and the characteristics of the optical semiconductor device can be made sufficiently satisfactory.

[0013] According to this embodiment, by using crystalline silica (c1) and titanium oxide (c2) as the filler (C), the linear expansion coefficient of the composition (X) can be reduced while the transmittance of the cured product can be increased. The reason is presumed to be as follows. When the filler (C) is added to the epoxy resin composition in order to reduce the linear expansion coefficient, the transmittance generally decreases. However, the present inventors have found that, when crystalline silica (c1) is used as the filler (C), the decrease in the linear expansion coefficient is reduced, but the decrease in the transmittance can be suppressed to a small extent. Furthermore, they have found that the transmittance can be increased by adding titanium oxide (c2) in addition to crystalline silica (c1). As a result, it is considered that the composition (X) can maintain a low linear expansion coefficient while increasing the transmittance of the cured product by containing crystalline silica (c1) and titanium oxide (c2) as the filler (C).

[0014] 2. Details <Epoxy resin composition> The composition (X) according to the present embodiment contains an epoxy resin (A), a curing agent (B), and a filler (C). The composition (X) may further contain additives other than the above components.

[0015] [Epoxy resin (A)] The epoxy resin (A) is not particularly limited as long as it is a compound having two or more epoxy groups in one molecule.

[0016] Examples of the epoxy resin (A) include bisphenol type epoxy resins, hydrogenated bisphenol type epoxy resins, biphenyl type epoxy resins, naphthalene ring-containing epoxy resins, alicyclic epoxy resins, dicyclopentadiene type epoxy resins, phenol novolac type epoxy resins, cresol novolac type epoxy resins, triphenylmethane type epoxy resins, aliphatic epoxy resins, triglycidyl isocyanurate, glycidyl group-containing silicone resins, and glycidylamine type epoxy resins.

[0017] The ratio of the epoxy resin (A) to the entire composition (X) is preferably 10% by mass or more and 50% by mass or less. In this case, the flowability of the composition (X) during molding and the physical properties of the produced encapsulant can be improved. This ratio is more preferably 20% by mass or more and 45% by mass or less.

[0018] [Hardening agent (B)] The curing agent (B) is not particularly limited as long as it is a compound capable of undergoing a curing reaction with the epoxy resin (A).

[0019] Examples of the curing agent (B) include phenol-based curing agents, acid anhydrides, amines, imidazoles, hydrazides, polymercaptans, Lewis acid-amine complexes, etc. The curing agent (B) preferably contains a phenol-based curing agent. The phenol-based curing agent has better curing properties than other curing agents, and this can increase the strength of the produced sealing material.

[0020] Examples of the phenol-based curing agent include novolac type resins such as phenol novolac resin, cresol novolac resin, and naphthol novolac resin; aralkyl type resins such as phenol aralkyl resins having a phenylene skeleton or a biphenylene skeleton, and naphthol aralkyl resins having a phenylene skeleton or a biphenylene skeleton; polyfunctional phenol resins such as triphenolmethane type resins; dicyclopentadiene type phenol resins such as dicyclopentadiene type phenol novolac resin and dicyclopentadiene type naphthol novolac resin; terpene-modified phenol resins; bisphenol type resins such as bisphenol A and bisphenol F; and triazine-modified novolac resins.

[0021] The proportion of the curing agent (B) in the entire composition (X) is preferably from 5% by mass to 30% by mass, and more preferably from 10% by mass to 25% by mass.

[0022] The equivalent of the curing agent (B) relative to 1 equivalent of the epoxy resin (A) is, for example, 0.6 or more and 1.4 or less.

[0023] [Filler (C)] The filler (C) contains crystalline silica (c1) and titanium oxide (c2). The filler (C) preferably further contains amorphous silica (c3). By including amorphous silica (c3) in the filler (C), the linear expansion coefficient of the composition (X) can be further reduced.

[0024] The average particle size of the filler (C) is the median size determined from the particle size distribution obtained from the measurement results by a laser diffraction / scattering method. The filler (C) may contain two or more components with different average particle sizes in order to adjust the physical properties of the composition (X).

[0025] The average value of the ratio of the major axis to the minor axis of the filler (C) (hereinafter also referred to as the major axis / minor axis ratio) can be obtained, for example, by observing the shapes of 50 random particles using a scanning electron microscope (SEM) and averaging the major axis / minor axis ratios of these particles. The filler (C) may contain two or more components with different major axis / minor axis ratios in order to adjust the physical properties of the composition (X).

[0026] (Crystalline Silica (c1)) The crystalline silica (c1) means crystalline SiO2, which has a maximum peak intensity at 2θ=30 to 32° in the XRD pattern, and commercially available crystalline silica can be used. The crystalline silica (c1) is usually particulate.

[0027] The average particle size of the crystalline silica (c1) is preferably from 5 μm to 40 μm, and more preferably from 15 μm to 20 μm.

[0028] The long axis / short axis ratio of the crystalline silica (c1) is preferably 1.6 or less, more preferably 1.5, and even more preferably 1.4 or less. The long axis / short axis ratio may be, for example, 1.0 or more, 1.1 or more, 1.2 or more, or 1.3 or more. It is considered that the long axis / short axis ratio of the crystalline silica (c1) in the above range can be more highly packed in the composition (X). This can further increase the transmittance of the cured product of the composition (X).

[0029] The proportion of crystalline silica (c1) in the entire composition (X) is preferably 5% by mass or more and 40% by mass or less. In this case, the transmittance of the cured product of the composition (X) can be further increased. The proportion of crystalline silica (c1) is more preferably 6% by mass or more and 30% by mass or less, even more preferably 7% by mass or more and 26% by mass or less, and particularly preferably 8% by mass or more and 24% by mass or less.

[0030] (Titanium dioxide (c2)) Titanium oxide (c2) refers to an oxide of titanium and is represented by the general formula TiOx (x=1.0 to 2.0). Titanium oxide (c2) is usually in the form of particles.

[0031] The average particle size of titanium oxide (c2) is preferably 2 μm or less, more preferably 1 μm or less, even more preferably 0.7 μm or less, and particularly preferably 0.4 μm or less. When the average particle size of titanium oxide (c2) is 1 μm or less, the transmittance of the cured product of composition (X) can be particularly increased. The lower limit of the average particle size of titanium oxide (c2) is not particularly limited, but is, for example, 0.1 μm.

[0032] The ratio of titanium oxide (c2) to the entire composition (X) is preferably 1% by mass or less, more preferably 0.2% by mass or less, even more preferably 0.1% by mass or less, and particularly preferably 0.01% by mass or less. When the ratio of titanium oxide (c2) is 0.1% by mass or less, the transmittance of the cured product of the composition (X) can be particularly increased. The ratio of titanium oxide (c2) is preferably 0.001% by mass or more, more preferably 0.005% by mass or more.

[0033] (Amorphous Silica (C3)) Amorphous silica (c3) is composed of a network structure of Si-O and does not have a fixed crystal structure, and commercially available amorphous silica can be used. Amorphous silica (c3) is usually particulate. Examples of amorphous silica (c3) include fused silica, spherical silica, and spherical fused silica. It is preferable that amorphous silica (c3) contains fused silica.

[0034] The average particle size of the amorphous silica (c3) is preferably 0.1 μm or more and 30 μm or less, and more preferably 20 μm or more and 30 μm or less.

[0035] The long axis / short axis ratio of the amorphous silica (c3) is preferably 1.6 or less, more preferably 1.5 or less, and even more preferably 1.4 or less. The long axis / short axis ratio may be, for example, 1.0 or more, 1.1 or more, 1.2 or more, or 1.3 or more. By setting the long axis / short axis ratio of the amorphous silica (c3) within the above range, the transmittance of the cured product of the composition (X) can be further increased.

[0036] The difference in the long axis / short axis ratio between the crystalline silica (c1) and the amorphous silica (c3) is preferably 0.4 or less, more preferably 0.2 or less, even more preferably 0.1 or less, and particularly preferably 0. In this case, the transmittance of the cured product of the composition (X) can be further increased.

[0037] The proportion of amorphous silica (c3) in the entire composition (X) is preferably 10% by mass or more and 60% by mass or less. In this case, the linear expansion coefficient of the composition (X) can be further reduced. The proportion of amorphous silica (c3) is more preferably 15% by mass or more and 50% by mass or less, even more preferably 28% by mass or more and 48% by mass or less, and particularly preferably 35% by mass or more and 45% by mass or less.

[0038] The ratio of crystalline silica (c1) to the total of crystalline silica (c1) and amorphous silica (c3) is preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, and particularly preferably 35% by mass or more. This ratio is preferably 70% by mass or less, more preferably 60% by mass or less, even more preferably 50% by mass or less, and particularly preferably 45% by mass or less. By setting the ratio of crystalline silica (c1) within the above range, the transmittance of the cured product of the composition (X) can be further increased.

[0039] The total ratio of crystalline silica (c1) and amorphous silica (c3) to the entire composition (X) is preferably 30% by mass or more and 80% by mass or less. In this case, the permeability of the cured product of the composition (X) can be further increased. This ratio is more preferably 35% by mass or more and 70% by mass or less, even more preferably 35% by mass or more and 60% by mass or less, and particularly preferably 35% by mass or more and 45% by mass or less.

[0040] The filler (C) may contain components other than those described above. Examples of the filler (C) other than those described above include crushed silica, spherical alumina, magnesium oxide, boron nitride, aluminum nitride, silicon nitride, talc, barium sulfate, calcium carbonate, mica powder, etc. The ratio of the filler (C) other than those described above to the entire composition (X) is, for example, 0.01% by mass or more and 10% by mass or less.

[0041] The ratio of the filler (C) to the entire composition (X) is preferably 30% by mass or more and 85% by mass or less. In this case, the transmittance of the cured product of the composition (X) can be further increased. The ratio of the filler (C) is more preferably 35% by mass or more and 70% by mass or less.

[0042] [Additives] The composition (X) may contain additives other than the above components within the range that does not impair the effect of this embodiment. Examples of the additives include a curing accelerator, a coupling agent, a mold release agent, a flame retardant, a flame retardant assistant, an ion trapping agent, a pigment such as carbon black, a colorant, a stress reducing agent, a tackifier, and a silicone flexibilizer.

[0043] Examples of the curing accelerator include imidazoles such as 2-methylimidazole, 2-ethylimidazole, 2-phenylimidazole, and 2-ethyl-4-methylimidazole; cycloamidines such as 1,8-diazabicyclo[5.4.0]undecene-7, 1,5-diazabicyclo[4.3.0]nonene-5, and 5,6-dibutylamino-1,8-diazabicyclo[5.4.0]undecene-7; tertiary amines such as 2-(dimethylaminomethyl)phenol, triethylenediamine, benzyldimethylamine, triethanolamine, dimethylaminoethanol, and tris(dimethylaminomethyl)phenol; tributylphosphine, methyldiphenylphosphine, and the like. Organic phosphines such as phenylphosphine, triphenylphosphine, tris(4-methylphenyl)phosphine, diphenylphosphine, an addition reaction product of triphenylphosphine and parabenzoquinone, and phenylphosphine; tetra-substituted phosphonium and tetra-substituted borates such as tetraphenylphosphonium tetraphenylborate, tetraphenylphosphonium ethyltriphenylborate, and tetrabutylphosphonium tetrabutylborate; quaternary phosphonium salts having a counter anion other than borate; and tetraphenylboron salts such as 2-ethyl-4-methylimidazole tetraphenylborate and N-methylmorpholine tetraphenylborate. The ratio of the curing accelerator to the entire composition (X) is, for example, 0.1% by mass or more and 2% by mass or less.

[0044] The coupling agent can improve the affinity of the filler (C) with the epoxy resin (A) and the curing agent (B). Examples of the coupling agent include silane coupling agents, titanate coupling agents, aluminum coupling agents, and aluminum / zirconium coupling agents. Examples of the silane coupling agent include glycidoxysilanes such as γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; aminosilanes such as N-β(aminoethyl)-γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, and N-phenyl-γ-aminopropyltrimethoxysilane; alkylsilanes; ureidosilanes; and vinylsilanes. The ratio of the coupling agent to the total amount of the filler (C) and the coupling agent is, for example, 0.01% by mass or more and 1% by mass or less.

[0045] Examples of the release agent include carnauba wax, stearic acid, montanic acid, carboxyl group-containing polyolefin, ester wax, polyethylene oxide, metal soap, etc. The ratio of the release agent to the entire composition (X) is, for example, 0.01 mass % or more and 1 mass % or less.

[0046] Examples of the flame retardant include magnesium hydroxide, aluminum hydroxide, and red phosphorus.

[0047] Examples of colorants include carbon black, red iron oxide, titanium oxide, phthalocyanine, and perylene black.

[0048] Examples of the stress reducing agent include silicone elastomers, silicone resins, silicone oils, butadiene-based rubbers, etc. Examples of the butadiene-based rubbers include methyl acrylate-butadiene-styrene copolymers, methyl methacrylate-butadiene-styrene copolymers, etc.

[0049] Composition (X) can be suitably used for encapsulating semiconductor devices, and is particularly suitable for encapsulating optical semiconductor elements in optical semiconductor devices.

[0050] <Method of producing the composition> The composition (X) can be prepared, for example, by mixing the components of the composition (X). More specifically, raw materials including, for example, the epoxy resin (A), the curing agent (B) and the filler (C) are mixed in a mixer, blender or the like until sufficiently uniform, and then melt-mixed in a heated state using a kneading machine such as a heat roll or a kneader, and then cooled to room temperature. The mixture thus obtained is pulverized by a known means to produce the powdered composition (X). The composition (X) does not have to be in a powder form, and may be, for example, in a tablet form. When the composition (X) is in a tablet form, it is preferable that the size and mass of the composition (X) are suitable for the molding conditions.

[0051] <Characteristics> The composition (X) is preferably a solid at 25° C. In this case, the composition (X) can be molded by a pressure molding method such as injection molding, transfer molding, or compression molding to produce an encapsulant. The composition (X) is more preferably a solid at any temperature in the range of 15° C. to 25° C., and even more preferably a solid at any temperature in the range of 5° C. to 35° C.

[0052] The transmittance of light having a wavelength of 800 nm or more and 980 nm or less in the cured product of the composition (X) is preferably 20% or more. In this case, even if the cured product of the composition (X) is used as an encapsulant for a side-type photocoupler or the like, the characteristics of the optical semiconductor device can be sufficiently satisfactory. The transmittance is more preferably 30% or more, even more preferably 35% or more, particularly preferably 40% or more, and most preferably 45% or more. The upper limit of the transmittance is not particularly limited, but is, for example, 60%. The transmittance of the composition (X) is a value when the thickness of the cured product obtained by curing is 1 mm.

[0053] The linear expansion coefficient of the cured product of the composition (X) is preferably 40 ppm / °C or less. In this case, the difference in linear expansion coefficient between the lead frame member of the optical semiconductor device, which usually has a linear expansion coefficient of 15 to 20 ppm / °C, and the cured product can be made smaller. Therefore, during molding of the optical semiconductor device, peeling inside the package can be suppressed, and discoloration due to oxidation caused by peeling can be suppressed, so that the transmittance can be increased. The linear expansion coefficient is more preferably 30 ppm / °C or less, and even more preferably 25 ppm / °C or less. In addition, the linear expansion coefficient is preferably 15 ppm / °C or more.

[0054] The spiral flow length of the composition (X) is preferably 90 cm or more. In this case, the composition (X) tends to have particularly good moldability. The spiral flow length is more preferably 100 cm or more, and even more preferably 120 cm or more. The upper limit of the spiral flow length is not particularly limited, but is, for example, 200 cm.

[0055] The gel time of the composition (X) is preferably 40 seconds or less. In this case, the molding cycle when preparing the encapsulant can be shortened, and the productivity of the optical semiconductor device can be increased. The lower limit of the gel time is not particularly limited, but is, for example, 20 seconds.

[0056] The details of the methods for measuring the transmittance, the linear expansion coefficient, the spiral flow length and the gel time will be described in the Examples section below.

[0057] <Optical semiconductor device> The optical semiconductor device according to this embodiment includes an optical semiconductor element and an encapsulant that encapsulates the optical semiconductor element. The encapsulant contains a cured product of a composition (X).

[0058] 1 shows a cross-sectional view of an example of a side-type photocoupler that is an optical semiconductor device 1. This optical semiconductor device 1 includes a light-emitting element 4 and a light-receiving element 5 as optical semiconductor elements 3, 3, an encapsulant 2 that encapsulates the optical semiconductor elements 3, 3, two lead frames 6, 6 that are conductors connected to the optical semiconductor elements 3, 3, and a highly reflective resin layer 7 that covers the encapsulant 2.

[0059] The encapsulant 2 includes a cured product of the composition (X). The light-emitting element 4 may be, for example, a light-emitting diode. The light-receiving element 5 may be, for example, a photodiode. The highly reflective resin layer 7 is formed of a resin having a reflectance of, for example, 70% or more. The optical semiconductor elements 3, 3 in the optical semiconductor device 1 may be encapsulated, for example, by injecting the composition (X) into a predetermined mold and curing it by heating under predetermined conditions. This provides an optical semiconductor device 1 in which the optical semiconductor elements 3, 3 are encapsulated by the cured product of the composition (X).

[0060] 1, the optical semiconductor device 1 may include an optical semiconductor element 3 and an encapsulant 2 that encapsulates the optical semiconductor element 3. The optical semiconductor device 1 may not include, for example, the highly reflective resin layer 7. Furthermore, the light emitting element 4 and the light receiving element 5 do not need to be arranged in parallel, and may have, for example, a face-to-face structure. EXAMPLES

[0061] The present disclosure will be described in more detail below with reference to examples, but the present disclosure is not limited to these examples in any way.

[0062] 1. Preparation of the Composition The raw materials shown in Table 1 were mixed and dispersed uniformly in a mixer, and then heated and kneaded at a material temperature of 120°C using a twin-screw kneader to obtain a mixture. The mixture was then cooled and pulverized. The obtained powder was then compressed into tablets to obtain a tablet-shaped composition. The details of the raw materials are as follows. -Epoxy resin: Cresol novolac type epoxy resin. Epoxy equivalent: 195g / eq -Hardening agent: Phenol-based hardener. Phenol novolac resin. OH equivalent: 105g / eq. -Filling material: ·Crystalline silica 1 (major axis / minor axis ratio = 1.3): Average particle size 18 μm. ·Crystalline silica 2 (major axis / minor axis ratio = 1.5): Average particle size 15μm. ·Amorphous silica 1 (major axis / minor axis ratio = 1.1): Average particle size 20 μm. ·Amorphous silica 2 (major axis / minor axis ratio = 1.3): Average particle size 20 μm. ·Amorphous silica 3 (major axis / minor axis ratio = 1.5): Average particle size 30μm. Titanium dioxide: average particle size 0.3μm. -Cure accelerator: triphenylphosphine. -Release agent: natural carnauba. -Coupling agent: Silane coupling agent. 3-glycidoxypropylmethyldiethoxysilane.

[0063] 2. Evaluation (1) Transmittance The composition was molded by transfer molding using a transfer molding machine (Shinto Metal Industries Co., Ltd.) under conditions of a mold temperature of 175°C, injection pressure of 6.9 MPa, and curing time of 180 seconds, and then post-cured by heating at 175°C for 6 hours to produce a disk-shaped cured product with a diameter of 50 mm and a thickness of 1 mm. The light transmittance of this cured product at a wavelength of 940 nm was measured using a spectrophotometer (Shimadzu Corporation MPC-3100).

[0064] (2) Linear expansion coefficient Using a transfer molding machine (manufactured by Shinto Metal Industries Co., Ltd.), the composition was molded by transfer molding under conditions of a mold temperature of 175°C, injection pressure of 6.9MPa, and curing time of 180 seconds, and then post-cured by heating at 175°C for 6 hours to prepare a test piece with dimensions of 5mmΦ×30mm. Using a horizontal thermal dilatometer (DLY-9000 manufactured by Advance Riko Co., Ltd.), the test piece was heated from 20°C to 280°C at a rate of 5°C per minute, and the average linear expansion coefficient of this test piece in the length direction from 80°C to 100°C was measured.

[0065] (3) Spiral flow length Using a transfer molding machine (manufactured by Shinto Metal Industry Co., Ltd.), the composition was injected into a dedicated spiral flow mold made based on ASRM D 3123 under conditions of a mold temperature of 175°C, an injection pressure of 6.9 MPa, and a curing time of 180 seconds, and the length that the composition flowed was measured.

[0066] (4) Gel Time The torque value was measured using a curastometer (JSR Corporation, Curastometer III PS type) while heating the composition at 175°C. The time until the torque value reached 4.9 N / m (0.5 kgf cm) was defined as the gel time.

[0067] The results of the above evaluation are shown in Table 1.

[0068] [Table 1]

Claims

1. An epoxy resin composition comprising an epoxy resin (A), a curing agent (B) and a filler (C), The filler (C) contains crystalline silica (c1) and titanium oxide (c2), The average particle size of the titanium oxide (c2) is 1 μm or less, The ratio of the titanium oxide (c2) is 0.1 mass% or less, The average ratio of the major axis to the minor axis of the crystalline silica (c1) is 1.2 or more and 1.6 or less; The epoxy resin composition, wherein the proportion of the filler (C) is 35% by mass or more and 70% by mass or less.

2. The epoxy resin composition according to claim 1, wherein the filler (C) further comprises amorphous silica (c3).

3. 3. The epoxy resin composition according to claim 2, wherein the average ratio of the major axis to the minor axis of the amorphous silica (c3) is 1.0 or more and 1.5 or less.

4. 4. The epoxy resin composition according to claim 2, wherein the proportion of the crystalline silica (c1) is 10 mass% or more and 70 mass% or less with respect to the total of the crystalline silica (c1) and the amorphous silica (c3).

5. 5. The epoxy resin composition according to claim 2, wherein a total proportion of the crystalline silica (c1) and the amorphous silica (c3) is 30% by mass or more and 60% by mass or less.

6. 6. The epoxy resin composition according to claim 1, wherein the epoxy resin composition has a transmittance of 30% or more for light having a wavelength of 800 nm or more and 980 nm or less when the cured product obtained by curing has a thickness of 1 mm.

7. An optical semiconductor element; an encapsulant for encapsulating the optical semiconductor element; Equipped with An optical semiconductor device, wherein the encapsulant comprises a cured product of the epoxy resin composition according to claim 1 .

Citation Information

Patent Citations

  • Photo coupling semiconductor device

    JP1979080691A

  • Epoxy resin composition for sealing optical semiconductor

    JP1995025987A

  • Epoxy resin composition and sealed device of electronic part

    JP1996245755A

  • Sealing resin composition and semiconductor device using the same

    JP2005089645A

  • Resin composition for sealing photo-semiconductor, and photo-semiconductor device

    JP2009029926A