Manufacturing method of fibers for industrial materials

A core-sheath structured fiber using polyethylene terephthalate and oxyalkylene group-containing polyvinyl alcohol is spun at controlled temperatures to address durability and thermal decomposition issues, ensuring seaweed adhesion and water absorbency in aquaculture materials.

JP7584121B2Active Publication Date: 2024-11-15NB SEIREN CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2020160578
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-25
Publication Date
2024-11-15
Estimated Expiration
2040-09-25

Smart Images

  • Figure 0007584121000001
    Figure 0007584121000001
Patent Text Reader

Abstract

To obtain a fiber for industrial materials composed of a polyester-based fiber comprising oxyalkylene group-containing polyvinyl alcohol while reducing the thermal decomposition of oxyalkylene group-containing polyvinyl alcohol upon melt spinning as much as possible.SOLUTION: A fiber for industrial materials has a sheath-core structure, in which a core component is composed of a first polyester resin having a melting point of 220 to 260°C and a melt viscosity of 200 Pa s [shear velocity 1,000 s-1] or less at 280°C, and a sheath component is composed of a second polyester resin comprising oxyalkylene group-containing polyvinyl alcohol and having a melting point lower than the core component.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This invention relates to fibers for industrial materials. of It relates to a manufacturing method. [Background technology]

[0002] Vinylon fiber is used as a material for cultivating marine products because it has good adhesion and survival properties for seaweed. Vinylon fiber also has excellent water retention properties, so it can retain water even in areas with large tidal ranges and long low tides. However, vinylon fiber has the problem of being poor in durability.

[0003] On the other hand, Patent Document 1 describes a fiber for aquaculture materials, which has good adhesion and rooting properties for seaweed, is excellent in durability, and is suitable for obtaining aquaculture materials that can be used in places with severe wave conditions, and a seaweed culture net using the fiber. The fiber described in Patent Document 1 is formed of a polyamide containing a modified polyvinyl alcohol resin. As the modified polyvinyl alcohol resin, an oxyalkylene group-containing polyvinyl alcohol is preferably used. As the polyamide, polycapramide (nylon 6) is preferably used.

[0004] This fiber is made of polyamide containing modified polyvinyl alcohol resin, and therefore has excellent durability and excellent adhesion and adhesion of seaweed, and even when used in places with severe wave conditions such as outside a bay, seaweed adhesion is good and seaweed can be maintained until harvest time, achieving a high yield. Therefore, it is suitable as a seaweed cultivation net, and is also suitable as a cultivation material such as ropes and twisted yarns. Seaweed cultivation nets using this cultivation material fiber have excellent characteristics as described above, and are therefore particularly suitable as a cultivation net for seaweed.

[0005] Oxyalkylene group-containing polyvinyl alcohol has a melting point of 200°C and a thermal decomposition temperature of 230°C to 240°C. In producing fibers, it is desirable to spin the material between the melting point and the thermal decomposition temperature. However, nylon 6 containing the material has a melting point of 225°C. Therefore, in order to obtain a good spinning condition, the spinning temperature must be increased to 250°C or higher.

[0006] That is, in general, when melt spinning a resin, raw material resin such as pellets is melt-kneaded by a melt extruder, extruded out of the machine and fed to a spinning nozzle, the resin is spun from the spinning nozzle, and then cooled and solidified. For this reason, the oxyalkylene group-containing polyvinyl alcohol contained in the nylon 6 resin is heated to the above-mentioned 250°C or higher inside the melt extruder in order to melt the nylon 6 resin well inside the melt spinning machine, and is sent to the spinning nozzle while maintaining the elevated temperature and subjected to spinning. Then, the oxyalkylene group-containing polyvinyl alcohol is exposed to a temperature above the decomposition temperature for a considerable time from melt mixing to spinning. As a result, there is a problem that acetic acid is generated by decomposition, resulting in a foul odor.

[0007] Therefore, the applicant of the present application developed a fiber for aquaculture materials with a cross section of a core-sheath structure, in which the core component is made of a first polyamide resin and the sheath component is made of a second polyamide resin containing oxyalkylene group-containing polyvinyl alcohol and having a lower melting point than the core component (Patent Document 2). In the fiber for aquaculture materials in Patent Document 2, the melting point of the second polyamide resin of the sheath component is set to 130°C to 160°C, thereby suppressing thermal decomposition of the oxyalkylene group-containing polyvinyl alcohol and achieving good operability. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2005-117972 A [Patent Document 2] JP 2018-150632 A Summary of the Invention [Problem to be solved by the invention]

[0009] Since aquaculture materials and fishing materials require water absorption, polyvinyl alcohol fibers and polyamide fibers are generally used. In response to this, the inventors of the present invention have investigated the application of fibers other than the commonly used polyvinyl alcohol fibers and polyamide fibers to aquaculture materials.

[0010] In this regard, polyester fibers used for land nets and the like have not been applied to aquaculture materials because they do not have water absorbency. Moreover, in order to provide polyester fibers that can be applied to such aquaculture materials, the following technical problems must be overcome:

[0011] That is, polyethylene terephthalate, which is commonly used as a polyester, has a melting point of 256°C, which is 30°C higher than the melting point of 225°C of the above-mentioned nylon 6. Therefore, when spinning polyethylene terephthalate, the spinning temperature must be at least 270°C to 280°C. This spinning temperature is also higher than the spinning temperature of nylon 6, which is 250°C. In other words, the temperature difference between the spinning temperature of 270°C to 280°C and the thermal decomposition temperature of oxyalkylene group-containing polyvinyl alcohol, which is 230°C to 240°C, is also significantly larger than that of nylon 6.

[0012] Therefore, when using polyester fibers, such as polyethylene terephthalate fibers, and incorporating an oxyalkylene group-containing polyvinyl alcohol as a modified polyvinyl alcohol resin into the polyester used to construct the fibers, and obtaining fibers for aquaculture materials by melt spinning, the problem of thermal decomposition of the modified polyvinyl alcohol resin becomes more pronounced than when polyamide fibers are used.

[0013] Therefore, an object of the present invention is to solve such problems and to obtain a fiber for industrial materials composed of a polyester fiber containing an oxyalkylene group-containing polyvinyl alcohol while minimizing the thermal decomposition of the oxyalkylene group-containing polyvinyl alcohol during melt spinning. [Means for solving the problem]

[0014] In order to achieve this object, the present invention provides a fiber for industrial materials. The manufacturing method is to manufacture a polymer with a melt viscosity of 200 Pa·s at 280°C [shear rate of 1000 s -1 or less is used as a first polyester resin for the core component, and a polyester resin containing an oxyalkylene group-containing polyvinyl alcohol and having a melting point of 130°C to 170°C is used as a second polyester resin for the sheath component, and a fiber having a core-sheath structure is produced by melt spinning, and at that time, the set temperature of the melt extruder for the sheath component is set to 180°C to 190°C. It is characterized by:

[0015] Fiber for industrial materials according to the present invention Manufacturing method According to The spinning temperature of the first polyester resin of the core component, polyethylene terephthalate, is set to 270°C to 280°C. is preferred. Effect of the Invention

[0017] Fiber for industrial materials according to the present invention According to the manufacturing method of The melt viscosity at 280°C is 200 Pa·s [shear rate 1000 s -1 ] or less Polyethylene terephthalate First polyester resin The core component is melt-spun as Therefore, even if the spinning temperature is set to 270°C to 280°C, which is lower than that of typical polyester resins, good fluidity can be exhibited and the core component can be melt-spun without any problems. To Contains oxyalkylene group-containing polyvinyl alcohol The melting point is 130℃ to 170℃. A second polyester resin with a lower melting point than the core component. Using Therefore, it is not necessary to melt-knead the second polyester resin at a high temperature suitable for the melting point of the first polyester resin, and the second polyester resin is melt-kneaded at a lower temperature suitable for the melting point of the second polyester resin. 180℃~190℃It is sufficient to perform melt kneading at a temperature of 100° C. Therefore, the sheath component can be melt kneaded at a temperature equal to or lower than the thermal decomposition temperature of the oxyalkylene group-containing polyvinyl alcohol, and only during spinning after melt kneading, a high temperature state based on the melting point of the first polyester resin needs to be maintained for a short period of time. Therefore, it is possible to obtain polyester resin-based industrial fiber containing the oxyalkylene group-containing polyvinyl alcohol while minimizing thermal decomposition of the oxyalkylene group-containing polyvinyl alcohol, which exhibits hydrophilicity and is particularly excellent in adhesiveness and adhesion to seaweed.

[0018] Fiber for industrial materials according to the present invention According to the manufacturing method By setting the melting point of the second polyester resin of the sheath component to 130°C to 170°C, the melt-kneading temperature of the sheath component can be reliably lowered below the thermal decomposition temperature of oxyalkylene group-containing polyvinyl alcohol, which is 230°C to 240°C.

[0019] According to the method for producing fibers for industrial materials of the present invention, when producing the fibers for industrial materials, the melt extruder for the sheath component is set to 180°C to 190°C, whereby thermal decomposition of the oxyalkylene group-containing polyvinyl alcohol during melt kneading can be reliably prevented. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The present invention Obtained by the manufacturing method The fiber for industrial materials has a core-sheath structure, with the core component being composed of a first polyester resin and the sheath component being composed of a second polyester resin that contains an oxyalkylene group-containing polyvinyl alcohol and has a lower melting point than the core component.

[0021] The first polyester resin constituting the core component teeth , polyethylene terephthalate is .

[0022] The first polyester resin constituting the core component has a melt viscosity of 200 Pa·s at 280°C [shear rate of 1000 s -1If the melt viscosity is higher than 200 Pa s, the viscosity is high, and therefore a higher temperature must be set for good melt spinning.

[0023] The first polyester resin may contain various inorganic particles such as titanium oxide, silicon oxide, calcium carbonate, silicon nitride, clay, talc, crosslinked polymer particles, various metal particles, etc., within the range not impairing the effects of the present invention. In addition, conventionally known additives such as antiaging agents, antioxidants, coloring inhibitors, light fasteners, inclusion compounds, antistatic agents, various colorants, various surfactants, and various reinforcing fibers may also be added within the range not impairing the effects of the present invention.

[0024] Specifically, the oxyalkylene group-containing polyvinyl alcohol contained in the sheath component is obtained by copolymerizing vinyl acetate with a polyoxyalkylene (meth)allyl ether such as polyoxyethylene (meth)allyl ether or polyoxypropylene (meth)allyl ether, followed by saponification. In this case, the copolymerization ratio (content) of the polyoxyalkylene (meth)allyl ether is preferably 0.1 mol% to 20 mol%, and more preferably 0.1 mol% to 5 mol%. The condensation degree of the polyoxyalkylene in the polyoxyalkylene (meth)allyl ether is preferably 1 to 300, and more preferably 3 to 50. The ratio of the oxyalkylene unit in the entire oxyalkylene group-containing polyvinyl alcohol is preferably 3 mass% to 40 mass%. This indicates that there is an optimal range for the degree of localization-delocalization of the oxyalkylene unit in the copolymer and the length of the oxyalkylene unit.

[0025] The degree of saponification of the vinyl acetate unit in the oxyalkylene group-containing polyvinyl alcohol is preferably 50 mol% to 100 mol%, more preferably 70 mol% to 99 mol%. The average degree of polymerization of the polyvinyl alcohol is preferably 150 to 1500, more preferably 200 to 1000. Note that, as the copolymerization component, components other than the polyoxyalkylene (meth)allyl ether, such as ethylene, propylene, α-olefins such as long-chain α-olefins, ethylenically unsaturated carboxylic acid monomers, acrylates, methacrylates, acrylonitrile, methacrylonitrile, vinyl chloride, vinyl ether, etc., may be contained in an amount of about 30 mol% or less.

[0026] The oxyalkylene group-containing polyvinyl alcohol preferably contains 0.01% to 5% by mass, and particularly preferably 0.1% to 0.5% by mass, of at least one of a phenolic compound, a thioether compound, and a phosphite compound, each having a melting point of 50°C to 250°C. This can improve the thermal stability of the fiber. If the amount of these compounds added is less than 0.01% by mass, no improvement in thermal stability can be expected, and if it exceeds 5% by mass, it will result in a decrease in the adhesion of seaweed.

[0027] As described above, the oxyalkylene group-containing polyvinyl alcohol has a melting point of 200°C and a thermal decomposition temperature of 230°C to 240°C.

[0028] Fibers for industrial materials When the raw materials are melt-kneaded to obtain the sheath component, the melt-kneading temperature, i.e., the set temperature of the melt extruder, must be 180°C to 190°C in order to avoid thermal decomposition of the above-mentioned oxyalkylene group-containing polyvinyl alcohol. Therefore, the second polyester resin constituting the sheath component must be capable of being melt-extruded at this temperature of 180°C to 190°C. For this purpose, the second polyester resin must have a lower melting point than the first polyester resin, specifically, a melting point of 130°C to 170°C. It is necessary , 150~165℃ desirableIf the melting point is 170°C or less, it can be melt-extruded well at the above-mentioned temperature of 180°C to 190°C. On the other hand, if the melting point is 130°C or more, it maintains heat resistance during practical use, and can be stretched well without fusing the fibers together during hot stretching in the fiber manufacturing process. As such a polyester-based resin, a copolymer polyester resin can be used. Specifically, a copolymer polyester obtained by copolymerizing a copolymerization component in which ethylene terephthalate is used as the main repeating unit, and dicarboxylic acids such as isophthalic acid, naphthalenedicarboxylic acid, 5-sodium sulfoisophthalic acid, phthalic anhydride, sebacic acid, adipic acid, succinic acid, ε-caprolactone, etc. are used, and diol components such as ethanediol, propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, cyclohexanedimethanol, etc. are used is an example.

[0029] The ratio of the second polyester resin to the oxyalkylene group-containing polyvinyl alcohol in the sheath component is preferably 10% by mass to 40% by mass, more preferably 15% by mass to 35% by mass. If the content of the oxyalkylene group-containing polyvinyl alcohol is less than 10% by mass, sufficient adhesion of seaweeds cannot be obtained. If the content of the oxyalkylene group-containing polyvinyl alcohol exceeds 40% by mass, the oxyalkylene group-containing polyvinyl alcohol peels off or dissolves from the sheath component, which tends to reduce the adhesion of seaweeds and to reduce spinnability and operability during fiber production.

[0030] Fibers for industrial materials As described above, the fiber has a core-sheath structure, and the core of the fiber has the above-mentioned Polyethylene terephthalate The first polyester resin is disposed in the fiber, which allows the fiber to have the required strength when used to make fibers for aquaculture materials and fibers for industrial materials such as seaweed farming nets.

[0031] On the other hand, Fibers for industrial materialsIn order to develop hydrophilicity in the fiber, it is sufficient that the oxyalkylene group-containing polyvinyl alcohol is contained on the surface of the fiber, not in the entire fiber. Therefore, it is sufficient that the oxyalkylene group-containing polyvinyl alcohol is contained only in the sheath of the core-sheath structure as described above. In the sheath, the oxyalkylene group-containing polyvinyl alcohol is mixed with the second polyester resin. This can prevent the oxyalkylene group-containing polyvinyl alcohol from peeling off or eluting from the fiber, and can thereby maintain the hydrophilic effect.

[0032] From the above viewpoints, the core-sheath composite ratio of the core component and the sheath component is preferably (core component) / (sheath component)=60 / 40 to 80 / 20 in mass ratio.

[0033] Fibers for industrial materials When the fiber is a multifilament, the single filament fineness is preferably 3.3 dtex to 22 dtex, and the total fineness is preferably 55 dtex to 2200 dtex. On the other hand, when the fiber for industrial materials is a monofilament, the fineness is preferably 55 dtex to 1100 dtex, and more preferably 220 dtex to 670 dtex. Fibers for industrial materials When the fiber is used for aquaculture materials and a seaweed farming net using the fiber, it is preferable that the fiber is a multifilament in order to increase the contact area with water. Furthermore, from the viewpoint of increasing the contact area with water, the multifilament may be subjected to Taslan processing.

[0034] Fibers for industrial materials When producing the fiber, the raw resins such as pellets constituting the core and sheath components are melt-kneaded separately in a melt extruder, and then extruded out of the machine and fed to a spinning nozzle. In the spinning nozzle, the resin is dissolved in a state in which the core component is disposed in the core portion and the sheath component is disposed in the sheath portion. The dissolved resin is then cooled and solidified to obtain a fiber.

[0035] At this time, the core component has a melt viscosity of 200 Pa·s [at 280°C and a shear rate of 1000 s-1 Since the polyethylene terephthalate is polyethylene terephthalate having a melting point of 180°C or less, the spinning temperature in the spinning nozzle is set to about 270°C to 280°C. In contrast, for the sheath component, the temperature of the melt extruder is set to 180°C to 200°C from the viewpoint of preventing thermal decomposition of the oxyalkylene group-containing polyvinyl alcohol and from the viewpoint of the melting point of the second polyester resin. However, the temperature of the sheath component in the spinning nozzle must be raised to 270°C to 280°C in accordance with the core component. Therefore, the sheath component is heated to 270°C to 280°C only when it is sent to the spinning nozzle and spun into a sheath-core fiber.

[0036] In this way, the sheath component is heated in the spinning nozzle to a temperature exceeding the thermal decomposition temperature of the oxyalkylene group-containing polyvinyl alcohol, but the time is short, so that the occurrence of thermal decomposition can be prevented as much as possible. In the melt extruder, the set temperature is 180 to 200°C as described above, so that the thermal decomposition of the oxyalkylene group-containing polyvinyl alcohol does not proceed.

[0037] Therefore, according to the present invention, when a polyester resin having a high melting point is used to obtain fibers for industrial materials that exhibit hydrophilicity and have excellent adhesiveness and adhesion properties, particularly for seaweed, the thermal decomposition of the oxyalkylene group-containing polyvinyl alcohol can be reduced as much as possible. EXAMPLES

[0038] Example 1 The core component has a melting point of 254°C and a melt viscosity at 280°C (ηmelt) of 186 Pa·s (shear rate 1000 s -1The sheath component was a mixture of a copolymerized polyester and an oxyalkylene group-containing polyvinyl alcohol in a mass ratio of (copolymerized polyester) / (oxyalkylene group-containing polyvinyl alcohol)=85 / 15. The copolymerized polyester used was the following: an oligomer obtained by esterification reaction of a terephthalic acid component with ethylene glycol, the molar ratio of the terephthalic acid component to the ethylene glycol component being 1:1.13, was copolymerized with ε-caprolactone in a ratio of 15 mol % relative to the acid component and 50 mol % relative to the 1,4-butanediol component, to obtain a copolymer having a melting point of 160°C, a melt viscosity [ηmelt] of 105 Pa s [shear rate 1000 s -1 A copolymer polyester was used.

[0039] First, melt kneading was performed using a general composite melt spinning device. The conditions were as follows: for the core component, the set temperatures of each part of the melt extruder were 300°C in the supply section, 270°C in the compression section, and 270°C in the metering section. For the sheath component, the set temperatures were 180°C in the supply section, 190°C in the compression section, and 200°C in the metering section.

[0040] Next, spinning was performed. A core-sheath type composite spinneret with a hole diameter of 0.5 mm and 192 holes was used. The spinneret temperature was set to 275°C, and the core-sheath mass ratio was set to (core) / (sheath) = 70 / 30. The spun yarn was passed through a heating cylinder with a set temperature of 250°C and a length of 200 mm, which was installed directly below the spinneret.

[0041] Next, the spun yarn was applied with an oil and taken up by a non-heated first roller, and then it was paralleled at 1.01 times by a second roller set at a temperature of 100 ° C., and passed through a steam treatment machine in which two orifices with a diameter of 2.2 mm were arranged symmetrically in the yarn path and steam at a temperature of 500 ° C. and a pressure of 0.3 MPa was blown out at an angle of 45 degrees toward the direction of fiber travel from each of them, and further it was stretched 5.5 times by a third roller at a temperature of 130 ° C., and a 3.8% relaxation treatment was performed by a fourth roller at a temperature of 130 ° C. After that, it was relaxed by 0.2% and wound on a winder at a speed of 2500 m / min, thereby obtaining a multifilament yarn of 1100 dtex / 96 filaments consisting of thermal adhesive long fibers of a core-sheath type composite form with a circular cross section in which the core and sheath are arranged approximately concentrically. The breaking strength of this multifilament yarn was 4.1 cN / dtex. Three of the multifilaments obtained were bundled together and first twisted at S-100T / m, and then three of these first twists were bundled together to obtain a rope made of Z-60T / m ply yarn.

[0042] Comparative Example 1 The core component used was the same polyethylene terephthalate as used in Example 1. The sheath component used was a mixture of the same polyethylene terephthalate as the core component in Example 1 and oxyalkylene group-containing polyvinyl alcohol in a mass ratio of (polyethylene terephthalate) / (oxyalkylene group-containing polyvinyl alcohol)=85 / 15.

[0043] Then, melt kneading was performed using a general composite melt spinning apparatus similar to that in Example 1. As for the conditions, the set temperatures of each part of the melt extruder for the core component were the same as those in Example 1, i.e., 300°C in the supply section, 270°C in the compression section, and 270°C in the metering section. As for the sheath component, the set temperatures of each part of the melt extruder were also the same as those in Example 1, i.e., 300°C in the supply section, 270°C in the compression section, and 270°C in the metering section.

[0044] Next, spinning was carried out under the same conditions as in Example 1.

[0045] However, an unpleasant odor was generated during melt spinning, and the yarn was unstable, resulting in frequent breakage of the yarn.

[0046] Comparative Example 2 Twelve vinylon monofilaments of 300 dtex were bundled together and first twisted at S-100 T / m. Three of these first twists were then bundled together to obtain a rope made of Z-60 T / m ply yarn.

[0047] The seaweed attachment ability was evaluated using the ropes of Example 1 and Comparative Example 2. The evaluation method was as follows.

[0048] That is, the seaweed seedlings were evaluated. In detail, a 0.5m x 1m square frame was prepared using a PVC pipe with an outer diameter of 26mm and an elbow and a tee that matched it. Then, the ropes of Example 1 and Comparative Example 2 were each wrapped around the frame 5 times. Furthermore, zoospores released from the wakame sporangium were attached to the fiber surface of the rope. After that, it was immersed in a tank containing seawater, and the attachment state of the zoospores was confirmed under a microscope. The number of attachments was counted at 100x magnification, and the average of 15 fields of view was calculated. The measurements were also taken on the day, 1 day later, and 6 days later.

[0049] The results obtained in Example 1 and Comparative Example 2 are shown in Table 1.

[0050] [Table 1]

[0051] As shown in Table 1, in Example 1, not only was there a large number of zoospores on the day, but many zoospores were still attached 1 and 6 days later. On the other hand, in Comparative Example 2, compared to Example 1, there were fewer attached zoospores and more shed zoospores, with the number decreasing by about 40% after 6 days.

Claims

1. A method for producing fibers for industrial materials, comprising the steps of: using polyethylene terephthalate having a melt viscosity at 280°C of 200 Pa·s [shear rate of 1000 s -1 ] or less as a first polyester-based resin for a core component; using a polyester-based resin containing an oxyalkylene group-containing polyvinyl alcohol and having a melting point of 130°C to 170°C as a second polyester-based resin for a sheath component; producing fibers having a core-sheath structure by melt spinning; and setting the melt extruder for the sheath component at a temperature of 180°C to 190°C.

2. A method for producing fibers for industrial materials as described in claim 1, characterized in that the spinning temperature of the first polyester resin of the core component, polyethylene terephthalate, is 270°C to 280°C.

Citation Information

Patent Citations

  • Production of fine polyester fiber

    JP1999350250A

  • Fiber for culture material and seaweed culture net using the same

    JP2005117972A

  • Hydrophilic fiber

    JP2005120529A

  • Polyester-based composite short fiber

    JP2014189913A

  • Pile knitted fabric and manufacturing method of the same and washing tool or cleaning tool using the same