Resin composition
A resin composition with surface-treated silica particles of varying sizes addresses high viscosity and permeability issues, enhancing fluidity and gap penetration in semiconductor encapsulation.
Patent Information
- Application Number
- JP2020176729
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-21
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2040-10-21
AI Technical Summary
Existing resin compositions used in semiconductor encapsulation face issues with high viscosity due to small silica particle sizes, leading to poor permeability and fluidity, especially in narrow gaps, despite improvements in dispersibility.
A resin composition is developed using two types of spherical silica particles, one with a D50 of 0.3 μm to 1.0 μm and the other with a D50 of 0.1 μm to 0.2 μm, both surface-treated with a phenyl coupling agent, blended in specific proportions with an epoxy resin, to enhance fluidity and permeability.
The composition achieves improved viscosity characteristics and excellent permeability into narrow gaps, addressing the limitations of previous technologies.
Smart Images

Figure 0007584272000001 
Figure 0007584272000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition, and more particularly to a resin composition suitable for use as a semiconductor encapsulant. [Background technology]
[0002] In recent years, as electronic devices become more compact and lightweight while still offering higher performance, the semiconductor packages they are fitted with are becoming more highly integrated, denser and thinner. To commercialize such semiconductor packages, it is essential to not only design integrated circuits but also develop encapsulants suited to those designs.
[0003] For example, flip-chip mounting is a technology for mounting a semiconductor chip (semiconductor element) to a wiring board. Flip-chip mounting is a mounting method in which protruding electrodes (bumps) are formed on the surface of a semiconductor chip, and this surface is directly connected to the wiring board. To protect the connected semiconductor chip, wiring board, and bumps, a sealing resin called an underfill is filled between the semiconductor chip and wiring board.
[0004] Epoxy resin is mainly used for underfill agents. Epoxy resin, semiconductor chip, and wiring board each have a different linear expansion coefficient. Therefore, if the connection cannot absorb the stress, cracks may occur at the connection. To prevent the occurrence of such cracks, fillers with a relatively small linear expansion coefficient, such as silica, are dispersed in the underfill agent. In this case, in order to suppress the linear expansion coefficient of the sealing material, it is required to increase the filling amount of the low expansion coefficient filler.
[0005] On the other hand, with the progress of miniaturization of semiconductor elements, the gaps through which the encapsulant must flow are narrowing, making it necessary to reduce the filler size diameter, and amorphous silica powder with a particle diameter of about 0.1 μm or more and 1.0 μm or less has been used. However, since a filler with a small particle size has a large specific surface area, it generally has strong cohesion and poor dispersibility, and it has been found that when it is made into a resin composition, the viscosity of the resin composition increases, causing insufficient penetration into the gap.
[0006] In order to solve the problem of poor penetration into gaps, a resin composition has been proposed that uses a hydrophilic dry silica powder that has a particle size in the range of 0.1 μm or more and 1.0 μm or less, yet has extremely low coagulation properties, excellent dispersibility, a small dispersed particle size, and a narrow particle size distribution when dispersed (Patent Document 1).
[0007] On the other hand, it has been proposed that the dispersibility of highly cohesive silica powder in resins can be improved by surface-treating the powder (Patent Document 2). [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2014-152048 A [Patent Document 2] JP 2014-201461 A Summary of the Invention [Problem to be solved by the invention]
[0009] However, in the resin composition using the silica powder described in Patent Document 1, although the permeability into gaps is improved, the dispersed particle size of the silica powder is small, which induces a thickening effect on the resin composition, resulting in an increase in viscosity, which remains an issue.
[0010] On the other hand, in Patent Document 2, although the dispersibility in resin can be improved by surface treating silica, the viscosity characteristics of the resin composition are still insufficient, and further improvement in the viscosity characteristics is required.
[0011] Therefore, an object of the present invention is to provide a resin composition having excellent flowability by incorporating a silica filler having a small particle size in a high proportion. [Means for solving the problem]
[0012] The present inventors conducted extensive research to solve the above problems and discovered that by using silica particles that have been surface-treated with a phenyl-based coupling agent and each having a different particle size, a resin composition with excellent viscosity characteristics can be obtained, thereby completing the present invention.
[0013] That is, the present invention provides a composition comprising first spherical silica particles (A) surface-treated with a silane coupling agent having a phenyl group, second spherical silica particles (B) surface-treated with a silane coupling agent having a phenyl group, and a resin (C), The first spherical silica particles (A) have a volume-based cumulative 50% diameter (D50) of 0.3 μm to 1.0 μm as measured by a laser diffraction scattering method; The second spherical silica particles (B) have a volume-based cumulative 50% diameter (D50) of 0.1 μm to 0.2 μm as measured by a laser diffraction scattering method; the total amount of the spherical silica particles (A) and (B) is 50 to 900 parts by mass per 100 parts by mass of the resin (C); And when the total of (A) and (B) is 100% by mass, the proportion of (B) is 5 to 30% by mass. the law of nature, The silane coupling agent is phenyltrimethoxysilane or phenyltriethoxysilane. This is a liquid resin composition for use as an underfill agent. Effect of the Invention
[0014] According to the present invention, it is possible to provide a resin composition having excellent viscosity characteristics. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, an embodiment of the present invention will be described in detail. However, the present invention is not limited to the following embodiment.
[0016] The resin composition of the present invention contains two types of spherical silica and a resin as essential components. Each component constituting the resin composition will be described below.
[0017] <First spherical silica particles> The first component used in the resin composition of the present invention is spherical silica particles surface-treated with a silane coupling agent having a phenyl group, and the spherical silica particles have a cumulative 50% diameter (hereinafter referred to as "D50") on a volume basis measured by a laser diffraction scattering method in the range of 0.3 μm to 1.0 μm. In the present invention, such spherical silica particles are referred to as first spherical silica particles.
[0018] The first spherical silica particles must be surface-treated with a silane coupling agent having a phenyl group. That is, a phenyl group must be present on the surface of the silica particles. This phenyl group (sometimes abbreviated as Ph) may be directly bonded to a silicon atom, such as Ph-Si-, or may have a spacer-like organic group between the silicon atom and the phenyl group. In addition, one or more hydrogen atoms of the phenyl group may be substituted with other groups.
[0019] The carbon content in the first spherical silica particles is preferably 0.01% by mass to 2% by mass, more preferably 0.03% by mass to 1% by mass. The carbon content is a representative evaluation index showing the degree of surface treatment. The carbon content may be measured using a trace carbon analyzer using a combustion oxidation method. Specifically, a spherical silica particle sample is heated to 1350°C in an oxygen atmosphere, and the obtained carbon content is calculated by converting it to a value per unit mass. The silica particles to be measured are heated at 80°C as a pretreatment, and the system is reduced in pressure to remove moisture adsorbed in the air, and then the carbon content is measured. In general, a surface treatment agent modifies only the surface of silica, and does not modify (or cannot come into contact with) the inside without communicating holes, so the increase in the carbon content may be regarded as the surface carbon content.
[0020] In the present invention, if the D50 of the first spherical silica particles is smaller than 0.3 μm, the viscosity of the resin composition increases and the flowability deteriorates. Also, if the silica particles have a D50 of more than 1.0 μm, the permeability into narrow gaps deteriorates. It is preferably 0.5 μm or less. In order to further improve the permeability into narrow gaps, it is particularly preferable that the silica particles do not substantially contain silica particles of 1.0 μm or more. In this case, the D50 is 0.7 μm or less.
[0021] The first spherical silica particles in the present invention are spherical in shape. Here, being spherical means that the average circularity of the silica particles is 0.8 or more. The average circularity is preferably 0.85 or more. The average circularity is obtained by obtaining an SEM image observed with a scanning electron microscope (SEM), determining a value C (circularity) defined by the following formula (1) for each particle by image analysis, and calculating the circularity C as an arithmetic mean value for 2000 or more particles.
[0022] C=4πS / L2 (1) [In formula (1), S represents the area (projected area) that the silica particle occupies in the image. L represents the length (perimeter) of the outer periphery of the particle in the image.] The closer the average circularity is to 1, the closer the particle shape is to a perfect sphere.
[0023] The first spherical silica particles having the above physical properties are not limited in the manufacturing method as long as they satisfy the above characteristics, but can be preferably manufactured by the following method. That is, the spherical silica manufactured by the "dry method (also called the combustion method)" of burning a silicon compound as described in WO / 2020 / 175160 is surface-treated with a silane coupling agent having a phenyl group by a known method.
[0024] In addition, since there is essentially no change in D50 before and after surface treatment with a silane coupling agent, it is sufficient to adjust the conditions for producing spherical silica by a dry method so that D50 is 0.3 to 1.0 μm before surface treatment.
[0025] The method of surface treatment with a silane coupling agent having a phenyl group is not particularly limited, and any known method may be appropriately selected and adopted, and may be either a so-called dry type or a wet type, or may be either a batch type or a continuous type. The reaction apparatus may be a fluidized bed type, a fixed pressure type, a stirrer, a mixer, or a stationary type. Among them, in consideration of the uniformity and promotion of the reaction, it is more preferable to fluidize the silica particles and react them in a fluidized bed type, a stirrer, a mixer, or the like.
[0026] The amount of the silane coupling agent having a phenyl group used when producing the first silica particles is not particularly limited, but if it is too small, the surface treatment is insufficient, and if it is too large, the amount present on the silica powder surface becomes too excessive, and the tendency of forming agglomerates is strong.Therefore, the amount of the silane coupling agent used is preferably 0.05-80 parts by mass, more preferably 0.1-40 parts by mass, and most preferably 0.5-5 parts by mass, relative to 100 parts by mass of silica particles.
[0027] The silane coupling agent having a phenyl group used for producing the first spherical silica particle is not particularly limited as long as it can introduce a phenyl group to the surface of the silica particle, and examples thereof include phenyltrimethoxysilane, phenyltriethoxysilane, p-styryltrimethoxysilane, and N-phenyl-3-aminopropyltrimethoxysilane. Note that the silane coupling agent in the present invention is not limited to those having an alkoxy group as a hydrolyzable group as listed here, and also includes compounds in which the hydrolyzable group is another group. Examples of such compounds include phenyltrichlorosilane, etc.
[0028] Considering the storage stability of the resin composition, the cost, the ease of production, and the ease of purification (prevention of impurities from being mixed into silica), among these silane coupling agents, phenyltrimethoxysilane and phenyltriethoxysilane are particularly preferred.
[0029] <Second spherical silica particles> The second component used in the present invention is spherical silica surface-treated with a silane coupling agent having a phenyl group, and the spherical silica particles have a D50 in the range of 0.1 μm to 0.2 μm. In the present invention, such spherical silica particles are referred to as second spherical silica particles.
[0030] The second spherical silica particles also need to be surface-treated with a silane coupling agent having a phenyl group. That is, a phenyl group needs to be present on the surface of the silica particles. This phenyl group (sometimes abbreviated as Ph) may be directly bonded to a silicon atom, such as Ph-Si-, or may have a spacer-like organic group between the silicon atom and the phenyl group. In addition, one or more hydrogen atoms of the phenyl group may be substituted with other groups.
[0031] The carbon content in the second spherical silica particles is preferably 0.01% by mass to 3% by mass, and more preferably 0.05% by mass to 2% by mass.
[0032] From the viewpoint of improving the packing property, the size of the second silica particles is preferably 0.2 μm or less. On the other hand, spherical silica having a D50 of less than 0.1 μm is often difficult to obtain, and therefore, from the economic viewpoint, it is preferable that the size is 0.1 μm or more.
[0033] The second spherical silica particles in the present invention are also spherical in shape, like the first spherical silica particles.
[0034] The second method for producing spherical silica particles is not particularly different from the first method for producing spherical silica particles, except that spherical silica particles with a D50 of 0.1 to 0.2 μm are used as the spherical silica particles to be treated with a silane coupling agent. Spherical silica with a D50 of 0.1 to 0.2 μm can be produced by the dry method disclosed in JP-A-2008-019157. In this case too, the D50 should be adjusted to 0.1 to 0.2 μm before the surface treatment.
[0035] The second spherical silica particles preferably have a coefficient of variation (CV value) in the volume-based particle size distribution measured using a laser diffraction scattering method of 35% to 50%, from the viewpoints of improving dispersibility in the resin and improving the viscosity characteristics of the resin composition.
[0036] In addition, in the measurement of the first spherical silica particles and the second spherical silica particles in the present invention by the laser diffraction scattering method, 0.1 g of spherical silica particles are weighed on an electronic balance, about 40 mL of ethanol is added, and the dispersion obtained by dispersing using an ultrasonic homogenizer at an output of 40 W for a processing time of 2 minutes is used as the measurement sample.
[0037] <Resin> The third component in the resin composition of the present invention is a resin (C). Examples of the resin (C) include epoxy resins, silicon resins, phenolic resins, melamine resins, urea resins, unsaturated polyester resins, acrylic resins (methacrylic resins), silicone resins, and fluororesins. When the resin composition of the present invention is used as a semiconductor encapsulant, epoxy resins are preferred.
[0038] As the epoxy resin, an oligomer or polymer having two or more epoxy groups in one molecule is suitable. For example, biphenyl type epoxy resin, stilbene type epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, triphenol methane type epoxy resin, alkyl modified triphenol methane type epoxy resin, dicyclopentadiene modified phenol type epoxy resin, naphthol type epoxy resin, triazine nucleus-containing epoxy resin, etc. can be mentioned. One of these can be used alone or a mixture of two or more can be used.
[0039] <Other> The resin composition of the present invention essentially contains the above three components. In addition to these, the resin composition may contain various components known for the purpose or use of the resin composition, depending on the purpose or use of the resin composition.
[0040] <Resin composition> The resin composition of the present invention contains the above-mentioned three components, namely, the first spherical silica particles (A), the second spherical silica particles (B), and the resin (C), and the total amount of the first spherical silica particles (A) and the second spherical silica particles (B) is in the range of 50 to 900 parts by mass relative to 100 parts by mass of the resin (C). Preferably, it is in the range of 80 to 800 parts by mass. Furthermore, when the total of the first spherical silica (A) and the second spherical silica (B) is taken as 100% by mass, the proportion of (B) in the entire spherical silica particles is 5 to 30% by mass. By setting the blending ratio of the spherical silica particles (A) and (B) to the resin composition and the proportion of the spherical silica particles (B) in the entire spherical silica particles in the above ranges, a resin composition having a low linear expansion coefficient and excellent viscosity characteristics and penetration into narrow gaps can be obtained.
[0041] The resin composition of the present invention, which is composed of the above-mentioned blending components, has excellent viscosity characteristics. The reason is not clear, but is presumed to be as follows. Both the spherical silica particles having a D50 of 0.3 μm to 1.0 μm and the spherical silica particles having a D50 of 0.1 μm to 0.2 μm are surface-treated with a silane coupling agent having a phenyl group, thereby improving the wettability between the silica particles and the resin. In addition, by using the spherical silica particles having a D50 of 0.3 μm to 1.0 μm in combination with the spherical silica particles having a D50 of 0.1 μm to 0.2 μm in a predetermined ratio, the flowability of the silica particles as a whole is improved. For these reasons, the flowability of the resin composition is improved, and as a result, the viscosity characteristics of the resin composition are improved.
[0042] <Method of producing resin composition> The method for producing the resin composition of the present invention is not particularly limited, but for example, the resin composition can be obtained by stirring, mixing, dispersing, etc., the first spherical silica particles (A), the second spherical silica particles (B), and the resin (C) as well as other components used as needed, all at once or separately. The device for mixing, stirring, dispersing, etc., of these components is not particularly limited, and examples thereof include a Raikai machine equipped with a stirring device, a heating device, etc., a three-roll mill, a ball mill, a planetary mixer, a bead mill, etc. The resin composition can be obtained by mixing and kneading the above components using these devices and degassing them as needed. EXAMPLES
[0043] The present embodiment will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0044] <Production of first spherical silica particles> Spherical silica particles having a D50 of 0.36 μm produced by the dry method described in WO2020 / 175160 were prepared. A rocking mixer (RM-30 manufactured by Aichi Electric) was used as a surface treatment mixer, and the spherical silica particles (2.97 kg) and phenyltrimethoxysilane (KBM-103 manufactured by Shin-Etsu Silicone, 14.70 g, 25 μmol / g) as a surface treatment agent were supplied at 2 mL / min using a verist pump (SJ-1211 II-H manufactured by ATTA) and mixed. The temperature was raised from room temperature to 40 ° C. in 20 minutes, and then maintained at 40 ° C. for 60 minutes. After that, the temperature was raised to 150 ° C. in 60 minutes, and then maintained at 150 ° C. for 180 minutes. Heating and mixing were stopped and cooled to obtain the first spherical silica particles (A).
[0045] <Production of second spherical silica particles> Spherical silica particles having a D50 of 0.12 μm and a D50 of 0.11 μm were prepared by the dry method described in JP 2008-019157 A. Using these spherical silica particles, the same manufacturing method as for the first spherical silica particles was carried out, except that the amount of the surface treatment agent was changed as shown in Table 1, to obtain second spherical silica particles (B-1) and (B-2).
[0046] The physical properties of the produced spherical silica particles were evaluated as follows.
[0047] (1) BET specific surface area The BET specific surface area S (m 2 / g) was measured.
[0048] (2) Volumetric particle size distribution by laser diffraction scattering method Approximately 0.1 g of spherical silica particles were weighed out using an electronic balance into a 50 mL glass bottle, and approximately 40 mL of ethanol was added. The particles were dispersed using an ultrasonic homogenizer (BRANSON, Sonifier 250) at 40 W for 10 minutes. The volume-based 50% diameter (D50) (μm) and coefficient of variation (CV) of the spherical silica particles were then measured using a laser diffraction / scattering particle size distribution analyzer (Beckman Coulter, LS 13 320).
[0049] (3) Surface carbon measurement The carbon content (mass%) of the spherical silica particles was measured by a combustion oxidation method (Horiba, Ltd., EMIA-511). Specifically, the spherical silica particle sample was heated to 1350°C in an oxygen atmosphere, and the carbon content was calculated by converting it to a unit mass. The spherical silica particles to be measured were heated at 80°C as a pretreatment, and the moisture adsorbed in the air was removed by reducing the pressure in the system, and then the carbon content was measured.
[0050] Table 1 shows the physical properties of each of the spherical silica particles obtained by the coupling agent treatment according to the above method.
[0051] [Table 1] Examples 1 to 4, Comparative Example 1 Resin compositions were prepared using these silicas, and their viscosity characteristics were evaluated. The resin composition preparation method and viscosity characteristic measurement method are as follows.
[0052] (4) Resin composition preparation method 18 g of spherical silica particles (A) and (B) in the ratios shown in Table 2 were added to 12 g of bisphenol A+F type epoxy resin (ZX-1059, manufactured by Nippon Steel Chemical & Material Co., Ltd.) and hand-kneaded. The hand-kneaded resin composition was pre-kneaded with a planetary centrifugal mixer (THINKY, Awatori Rentaro AR-500) (kneading: 1000 rpm, 8 minutes, degassing: 2000 rpm, 2 minutes). The pre-kneaded resin composition was stored in a thermostatic water bath at 25°C, and then kneaded with a three-roll machine (BR-150HCV, manufactured by Imex Co., Ltd., roll diameter φ63.5). The kneading conditions were a kneading temperature of 25°C, a roll distance of 20 μm, and a kneading count of 8 times. The obtained resin composition was degassed for 30 minutes under reduced pressure using a vacuum pump (TSW-150, manufactured by Sato Vacuum Co., Ltd.).
[0053] (5) Viscosity measurement The viscosity of the kneaded resin composition was measured using a rheometer (HAAKE MARS40, manufactured by Thermo Fisher Scientific Co.) The measurement temperature was 25° C., and the sensor used was C35 / 1 (cone-plate type, diameter 35 mm, angle 1°, material titanium).
[0054] In addition, the shear rate measured at 25°C using a rheometer is 1 s -1 The viscosity value at a shear rate of 10 s -1 The value obtained by dividing the viscosity by the viscosity at 100° C. was taken as the TI (thixotropic index) value of the resin composition.
[0055] The results for each Example and Comparative Example are shown in Table 2. The viscosity was measured at a temperature of 25° C. and a shear rate of 1 s -1 The value at .
[0056] [Table 2] In Examples 1 to 4, both the viscosity and the TI value were better than those of Comparative Example 1 which did not contain the second spherical silica particles.
Claims
1. The composition comprises first spherical silica particles (A) which have been surface-treated with a silane coupling agent having a phenyl group, second spherical silica particles (B) which have been surface-treated with a silane coupling agent having a phenyl group, and a resin (C), the first spherical silica particles (A) have a volume-based cumulative 50% diameter (D50) measured by a laser diffraction scattering method of 0.3 μm to 1.0 μm; the second spherical silica particles (B) have a cumulative 50% diameter (D50) on a volume basis measured by a laser diffraction scattering method of 0.1 μm to 0.2 μm; the total amount of the spherical silica particles (A) and (B) is 50 parts by mass to 900 parts by mass per 100 parts by mass of the resin (C); and when the total of (A) and (B) is 100% by mass, the proportion of (B) is 5 to 30% by mass; The liquid resin composition for underfill material, wherein the silane coupling agent is phenyltrimethoxysilane or phenyltriethoxysilane.
2. The liquid resin composition according to claim 1 , wherein the resin (C) is an epoxy resin.
3. A semiconductor sealing material comprising the liquid resin composition according to claim 1 or 2.
Citation Information
Patent Citations
Surface-modified spherical silica, method of manufacturing the same and resin composition for sealing
JP2005022915A
Epoxy resin material and multilayer board
JP2013040298A
Resin composition
JP2014012763A
Dry-process silica fine particle
JP2014152048A
Hydrophobized dry silica microparticle
JP2014201461A