Etching solution and method for manufacturing semiconductor device

A tailored etching solution with controlled hydrofluoric acid, nitric acid, and water concentrations addresses the etching stop issue in SiGe compounds, ensuring stable etching and improved production efficiency in semiconductor manufacturing.

JP7584275B2Active Publication Date: 2024-11-15TOKYO OHKA KOGYO CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020180113
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-25
Filing Date
2020-10-28
Publication Date
2024-11-15
Estimated Expiration
2040-10-28

AI Technical Summary

Technical Problem

Existing etching solutions for SiGe compounds in semiconductor manufacturing cause etching stop, leading to unstable transistor characteristics and reduced yield due to unintentional etching of Si layers, and increase production complexity and cost.

Method used

An etching solution with specific concentrations of hydrofluoric acid (0.002% to 1.0% by mass), nitric acid (10% to 55% by mass), and water (5% to 40% by mass) is used to selectively etch SiGe compounds, suppressing etching stop and improving etching rates.

Benefits of technology

The solution enables stable etching of SiGe compounds without affecting Si, Ge, or their oxides, reducing etching stop occurrences and enhancing production efficiency by allowing longer etching times, thus improving yield and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007584275000001
    Figure 0007584275000001
  • Figure 0007584275000002
    Figure 0007584275000002
  • Figure 0007584275000003
    Figure 0007584275000003
Patent Text Reader

Abstract

To provide an etching solution which is able to selectively perform an etching process on a compound represented by a General Formula Si1-xGex with respect to Si, Ge, and oxides thereof, and with which etching stops do not easily occur, and a method for manufacturing a semiconductor using the etching solution.SOLUTION: An etching solution for selectively performing an etching process on a compound represented by a General Formula Si1-xGex (where x is more than 0 and less than 1) with respect to Si, Ge, and oxides thereof includes hydrofluoric acid, nitric acid, and water. A content ratio of the hydrofluoric acid in the entire etching solution, is 0.002% by mass or more and 1.0% by mass or less, a content ratio of the nitric acid in the entire etching solution is 10% by mass or more, and a content ratio of the water in the entire etching solution is 40% by mass or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an etching solution and a method for manufacturing a semiconductor device. [Background technology]

[0002] Traditionally, the scaling of features within integrated circuits has allowed for an increased density of functional units on a semiconductor chip: for example, the reduction in transistor size has allowed more memory elements to be fitted onto a chip, leading to the production of products with increased capacity.

[0003] Ge is used as a semiconducting crystalline material other than silicon in the fabrication of field effect transistors (FETs) for integrated circuit devices. Ge has several advantageous characteristics compared to silicon in some cases, including high charge carrier (hole) mobility, band gap offset, different lattice constant, and ability to alloy with silicon to form the semiconducting binary alloy SiGe.

[0004] Ge materials (especially those with the general formula Si 1-x Ge x A compound represented by the formula: where x is greater than 0 and less than 1. Hereinafter, this may simply be referred to as a "SiGe compound." Various etching solutions with high selectivity for SiGe have been proposed. For example, an etching solution containing hydrofluoric acid (DHF) and nitric acid is known to have a high etching ratio of a SiGe compound relative to Si, SiO2, and the like (see, for example, Patent Document 1).

[0005] On the other hand, when etching with an etching solution containing hydrofluoric acid (DHF) and nitric acid is continued for a long time, for example when selectively etching only SiGe in a stacked structure consisting of Si / SiGe / Si, the etching of the SiGe layer stops halfway (so-called etching stop occurs). As a result, when removing SiGe, the etching of the Si layer proceeds unintentionally, making it impossible to obtain a stable shape, causing variations in transistor characteristics and further reducing yields.

[0006] In order to solve the above problems, Patent Document 1 proposes the following method. (Method 1) While rotating the substrate with the SiGe layer, the fluoronitric acid solution is sprayed on it for a short period of time (several tens of seconds) to etch the SiGe layer. Then, while rotating the substrate, spraying of the fluoronitric acid solution is stopped. After that, new fluoronitric acid solution is sprayed on the substrate again while rotating the substrate. (Method 2) The substrate with the SiGe layer is immersed in the fluoronitric acid solution stored in the etching tank, and the SiGe layer is wet-etched for a short time of about 1 minute. The substrate is then removed from the etching tank and immersed in a water washing tank for a water washing process. The substrate is then immersed again in the fluoronitric acid solution stored in the etching tank, and wet-etched for a short time of about 1 minute. In this manner, the etching process and water washing process are repeated multiple times. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2008-160073 A Summary of the Invention [Problem to be solved by the invention]

[0008] However, the method described in Patent Document 1 has the problem that the number of steps in the manufacturing process is increased, making it impractical in terms of production efficiency and manufacturing costs. The present invention has been made in view of the above circumstances, and relates to a compound represented by the general formula Si 1-x Ge x The present invention aims to provide an etching solution capable of selectively etching a compound represented by the following formula (I) and which is less likely to cause an etch stop, and a method for manufacturing a semiconductor using the etching solution. [Means for solving the problem]

[0009] In order to solve the above problems, the present invention employs the following configuration.

[0010] The first aspect of the present invention is to provide a compound represented by the general formula Si 1-x Ge x (wherein x is greater than 0 and less than 1), the etching solution contains hydrofluoric acid, nitric acid, and water, the content of the hydrofluoric acid in the entire etching solution is 0.002% by mass or more and 1.0% by mass or less, the content of the nitric acid in the entire etching solution is 10% by mass or more, and the content of the water in the entire etching solution is 40% by mass or less.

[0011] The second aspect of the present invention is to use the etching solution to form a compound having the general formula Si 1-x Ge x The present invention relates to a method for manufacturing a semiconductor device, the method including the step of etching an object to be treated, the object including a compound represented by the formula: Effect of the Invention

[0012] According to the etching solution of the present invention, the general formula Si 1-x Ge x The compound represented by the formula (I) can be selectively etched while suppressing etch stop. In addition, according to the semiconductor manufacturing method of the present invention, the general formula Si 1-x Ge x It is possible to manufacture a semiconductor in which the compound represented by the formula (I) is selectively etched. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] (etchant) The etching solution according to the first aspect of the present invention contains hydrofluoric acid, nitric acid, and water. The etching solution according to this aspect has a general formula Si 1-x Ge x The compound represented by the formula (where x is greater than 0 and less than 1) (hereinafter, sometimes simply referred to as a "SiGe compound") is used for selective etching treatment.

[0014] <Hydrogen fluoride> The etching solution according to this embodiment contains hydrofluoric acid (DHF). The content of hydrofluoric acid in the entire etching solution is 0.002 mass% or more and 1.0 mass% or less, preferably 0.005 mass% or more and 0.9 mass% or less, more preferably 0.001 mass% or more and 0.8 mass% or less, even more preferably 0.01 mass% or more and 0.7 mass% or less, and still more preferably 0.02 mass% or more and 0.6 mass% or less. When the content of hydrofluoric acid is within the above range, the etching rate for the SiGe compound is improved.

[0015] <Nitric acid> The etching solution in this embodiment contains nitric acid (HNO3). The content of nitric acid in the entire etching solution is 10% by mass or more, preferably 10% by mass or more and 55% by mass or less, more preferably 11% by mass or more and 55% by mass or less, even more preferably 12% by mass or more and 54% by mass or less, and even more preferably 15% by mass or more and 54% by mass or less. When the content of nitric acid is within the above range, the SiGe compound is easily oxidized, and the etching rate for the SiGe compound is improved.

[0016] <Water> The etching solution of the present embodiment contains water. The water may contain trace components that are inevitably mixed in. The water used in the etching solution of the present embodiment is preferably water that has been subjected to a purification treatment, such as distilled water, ion-exchanged water, or ultrapure water, and more preferably ultrapure water that is generally used in semiconductor manufacturing. The water content in the entire etching solution is 40 mass% or less, preferably 5 mass% or more and 40 mass% or less, more preferably 6 mass% or more and 38 mass% or less, even more preferably 7 mass% or more and 36 mass% or less, and still more preferably 8 mass% or more and 35 mass% or less. When the water content is within the above range, the etching rate of SiGe can be controlled.

[0017] <Other ingredients> The etching solution of the present embodiment may contain other components in addition to the above components, as long as the effects of the present invention are not impaired. Examples of other components include a solvent, phosphoric acid and / or its derivatives, a pH adjuster, a passivation agent, and a surfactant.

[0018] ·solvent The etching solution of the present embodiment can be prepared by mixing hydrofluoric acid, nitric acid, water, and other optional components in a solvent. The solvent is not particularly limited, and examples thereof include polar organic solvents.

[0019] Polar organic solvents The etching solution of the present embodiment may contain a polar organic solvent within a range that does not impair the effects of the present invention. Examples of the polar organic solvent include organic carboxylic acid solvents (e.g., acetic acid, formic acid, etc.), alcohol solvents (e.g., methanol, ethanol, ethylene glycol, propylene glycol, glycerin, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, diethylene glycol, dipropylene glycol, furfuryl alcohol, and 2-methyl-2,4-pentanediol, etc.), dimethyl sulfoxide, and ether solvents (e.g., ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, and propylene glycol dimethyl ether). Among these, the polar organic solvent is preferably an organic carboxylic acid solvent, and more preferably acetic acid.

[0020] In the etching solution of the present embodiment, the polar organic solvent may be used alone or in combination of two or more kinds. When the etching solution of the present embodiment contains a polar organic solvent, the content of the polar organic solvent is, for example, 10 to 90 mass % relative to the total mass of the etching solution, preferably 11 to 85 mass %, and more preferably 12 to 80 mass %.

[0021] Phosphoric acid and / or its derivatives The etching solution of the present embodiment may contain phosphoric acid and / or a derivative thereof as a solvent within a range that does not impair the effects of the present invention. Examples of phosphoric acid and / or a derivative thereof include compounds represented by the following general formula (1).

[0022] [ka] [In the formula, each R is independently a hydrogen atom or an alkyl group having 1 to 20 carbon atoms.]

[0023] In the formula (1), examples of the alkyl group having 1 to 20 carbon atoms for R include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, an undecyl group, a dodecyl group, a tridecyl group, an isotridecyl group, a tetradecyl group, a pentadecyl group, a hexadecyl group, an isohexadecyl group, a heptadecyl group, an octadecyl group, a nonadecyl group, an icosyl group, and each isomer of the above alkyl groups. Of these, R is preferably a hydrogen atom or an alkyl group having 1 to 10 carbon atoms, and more preferably a hydrogen atom.

[0024] In the etching solution of the present embodiment, the phosphoric acid and / or its derivatives may be used alone or in combination of two or more kinds. When the etching solution of the present embodiment contains phosphoric acid and / or a derivative thereof, the content of the phosphoric acid and / or a derivative thereof is, for example, 1 to 40 mass% relative to the total mass of the etching solution, preferably 2 to 38 mass%, more preferably 3 to 37 mass%, and further preferably 5 to 35 mass%.

[0025] pH adjuster The etching solution of the present embodiment may contain a pH adjuster in order to further improve the etching rate for the SiGe compound. The pH adjuster is preferably at least one selected from the group consisting of acids and their salts. Specifically, methanesulfonic acid, trifluoromethanesulfonic acid, oxalic acid dihydrate, citric acid, tartaric acid, picolinic acid, succinic acid, acetic acid, lactic acid, sulfosuccinic acid, benzoic acid, propionic acid, formic acid, pyruvic acid, maleic acid, malonic acid, fumaric acid, malic acid, ascorbic acid, mandelic acid, heptanoic acid, butyric acid, valeric acid, glutaric acid, phthalic acid, hypophosphorous acid, salicylic acid, 5-sulfosalicylic acid, hydrochloric acid, ethanesulfonic acid, butanesulfonic acid, p-toluenesulfonic acid, dichloroacetic acid, difluoroacetic acid, monochloroacetic acid, monofluoroacetic acid, trichloroacetic acid, trifluoroacetic acid, hydrobromic acid (62% by weight), sulfuric acid, ammonium acetate, sodium acetate, potassium acetate, tetramethylammonium acetate, and other tetraacetates. alkylammonium, phosphonium acetate, ammonium butyrate, ammonium trifluoroacetate, ammonium carbonate, ammonium chloride, ammonium sulfate, phosphoric acid, diammonium hydrogen phosphate, ammonium dihydrogen phosphate, bis(tetramethylammonium) hydrogen phosphate, disodium hydrogen phosphate, sodium dihydrogen phosphate, dipotassium hydrogen phosphate, potassium dihydrogen phosphate, ditetraalkylammonium hydrogen phosphate, ditetraalkylammonium dihydrogen phosphate, diphosphonium hydrogen phosphate, phosphonium dihydrogen phosphate, ammonium phosphonate, tetraalkylammonium phosphonate, sodium phosphonate, potassium phosphonate, phosphonium phosphonate, etidronic acid, and salts thereof. Of these, ammonium acetate or ammonium sulfate is preferred.

[0026] The etching solution of the present embodiment may contain a basic compound as a pH adjuster. As such a basic compound, an organic alkaline compound or an inorganic alkaline compound can be used, and suitable examples of the organic alkaline compound include quaternary ammonium salts such as organic quaternary ammonium hydroxides, and salts of alkylamines and their derivatives such as trimethylamine and triethylamine. Examples of inorganic alkaline compounds include inorganic compounds containing alkali metals or alkaline earth metals and their salts, such as lithium hydroxide, sodium hydroxide, potassium hydroxide, rubidium hydroxide, and cesium hydroxide.

[0027] In the etching solution of the present embodiment, the pH adjuster may be used alone or in combination of two or more kinds. When the etching solution of the present embodiment contains a pH adjuster, the content of the pH adjuster is, for example, 0.01 to 10 mass % relative to the total mass of the etching solution, preferably 0.02 to 4.5 mass %, more preferably 0.03 to 4 mass %, and even more preferably 0.05 to 3 mass %. When the content of the pH adjuster is within the above range, the etching rate for the SiGe compound is more likely to be improved.

[0028] Passivation agent The etching solution of this embodiment may contain a passivation agent for germanium. Passivation agents include ascorbic acid, L(+)-ascorbic acid, isoascorbic acid, ascorbic acid derivatives, boric acid, ammonium diborate, borate salts (e.g., ammonium pentaborate, sodium tetraborate, and ammonium diborate), alanine, arginine, asparagine, aspartic acid, cysteine, glutamic acid, glutamine, histidine, isoleucine, leucine, lysine, methionine, phenylalanine, proline, serine, threonine, tryptophan, tyrosine, valine, sodium bromide, potassium bromide, rubidium bromide, magnesium bromide, calcium bromide, and amines of the formula NR 1 R 2 R 3 R 4 Br (wherein, R 1 , R 2 , R 3 and R 4can be the same or different from each other and are selected from the group consisting of hydrogen and branched or straight chain C1-C6 alkyl (e.g., methyl, ethyl, propyl, butyl, pentyl, hexyl).

[0029] In the etching solution of the present embodiment, the passivation agent may be used alone or in combination of two or more kinds. When the etching solution of the present embodiment contains a passivation agent, the content of the passivation agent is preferably 0.01 to 5 mass %, and more preferably 0.1 to 1 mass %, relative to the total mass of the etching solution.

[0030] Surfactants The etching solution of the present embodiment may contain a surfactant for the purpose of adjusting the wettability of the etching solution to the object to be treated, etc. As the surfactant, a nonionic surfactant, an anionic surfactant, a cationic surfactant, or an amphoteric surfactant may be used, and these may be used in combination.

[0031] Examples of nonionic surfactants include polyalkylene oxide alkyl phenyl ether surfactants, polyalkylene oxide alkyl ether surfactants, block polymer surfactants consisting of polyethylene oxide and polypropylene oxide, polyoxyalkylene distyrene-type phenyl ether surfactants, polyalkylene tribenzyl phenyl ether surfactants, and acetylene polyalkylene oxide surfactants.

[0032] Examples of anionic surfactants include alkylsulfonic acids, alkylbenzenesulfonic acids, alkylnaphthalenesulfonic acids, alkyldiphenylethersulfonic acids, fatty acid amidesulfonic acids, polyoxyethylene alkylether carboxylic acids, polyoxyethylene alkylether acetic acids, polyoxyethylene alkylether propionic acids, alkylphosphonic acids, and salts of fatty acids. Examples of "salts" include ammonium salts, sodium salts, potassium salts, and tetramethylammonium salts.

[0033] Examples of cationic surfactants include quaternary ammonium salt surfactants and alkylpyridinium surfactants.

[0034] Examples of amphoteric surfactants include betaine type surfactants, amino acid type surfactants, imidazoline type surfactants, and amine oxide type surfactants.

[0035] These surfactants are generally commercially available. The surfactants may be used alone or in combination of two or more.

[0036] <Object to be treated> The etching solution of the present embodiment is used for etching a SiGe compound, and an object to be treated containing a SiGe compound is the subject of etching treatment. The object to be treated is not particularly limited as long as it contains a SiGe compound, and examples thereof include a substrate having a SiGe compound-containing layer (SiGe compound-containing film). The substrate is not particularly limited, and examples thereof include various substrates such as a semiconductor wafer, a glass substrate for a photomask, a glass substrate for a liquid crystal display, a glass substrate for a plasma display, a substrate for an FED (Field Emission Display), a substrate for an optical disk, a substrate for a magnetic disk, and a substrate for a magneto-optical disk. The substrate is preferably a substrate used for manufacturing a semiconductor device. In addition to the SiGe compound-containing layer and the substrate base material, the substrate may have various layers and structures, such as metal wiring, a gate structure, a source structure, a drain structure, an insulating layer, a ferromagnetic layer, and a nonmagnetic layer, as appropriate. In addition, the top layer of the device surface of the substrate does not need to be a SiGe compound-containing layer, and for example, an intermediate layer of a multilayer structure may be a SiGe compound-containing layer. The size, thickness, shape, layer structure, etc. of the substrate are not particularly limited and can be appropriately selected depending on the purpose.

[0037] The SiGe compound-containing layer is preferably a layer containing a SiGe compound, more preferably a SiGe compound film. The thickness of the SiGe compound-containing layer on the substrate is not particularly limited and can be appropriately selected according to the purpose. The thickness of the SiGe compound-containing layer can be, for example, in the range of 1 to 200 nm or 1 to 20 nm.

[0038] The workpiece may contain at least one selected from the group consisting of Si, Ge, and oxides thereof, in addition to the SiGe compound, and preferably contains SiO2.

[0039] The etching solution of the present embodiment may be used for microfabrication of a SiGe compound-containing layer in a substrate, may be used for removing a SiGe compound-containing deposit attached to a substrate, or may be used for removing impurities such as particles from a processing object having a SiGe compound-containing layer on the surface thereof.

[0040] The etching solution of the present embodiment described above contains specific amounts of hydrofluoric acid, nitric acid, and water, and therefore can react with Si, Ge, and their oxides with the general formula Si 1-x Ge x It is possible to selectively etch a compound represented by the formula (SiGe compound) and suppress the etching stop of the SiGe compound. The reason for this is unclear, but is presumed to be as follows. When the etching solution of this embodiment is brought into contact with a workpiece containing a SiGe compound, the SiGe compound is oxidized by nitric acid. The oxide of the SiGe compound is oxidized by fluoride ions (F - Specifically, SiGe is removed by the electrochemical reaction of the following formula (1): Si(Ge)+HNO3+6HF→H2Si(Ge)F6+HNO2+H2O+H2…(1) As shown in the above formula (1), if a SiGe compound is etched for a long period of time using an etching solution containing hydrofluoric acid and nitric acid, the oxidation rate of Ge by nitric acid or nitrous acid is faster than that of Si, so that the Ge concentration at the top surface during etching decreases, and etching of the SiGe layer may stop midway, which is known as etching stop. However, since the etching solution of the present embodiment has the hydrofluoric acid, nitric acid, and water contents within specific ranges, it is presumed that the oxidation rates of Si and Ge become equal, and the SiGe compound can be selectively etched while suppressing the etching stop of the SiGe compound.

[0041] (Method of manufacturing semiconductor device) A method for manufacturing a semiconductor device according to a second aspect of the present invention is characterized by including a step of etching an object to be processed containing a SiGe compound with the etching solution according to the first aspect.

[0042] Examples of the object to be processed containing a SiGe compound include the same as those described in "<Object to be processed>" in "(Etching solution)" above, and a preferred example is a substrate having a SiGe compound-containing layer. The method for forming the SiGe compound-containing layer on the substrate is not particularly limited, and a known method can be used. Examples of such methods include sputtering, chemical vapor deposition (CVD), epitaxial growth, and atomic layer deposition (ALD). The raw material of the SiGe compound-containing layer used when forming the SiGe compound-containing layer on the substrate is also not particularly limited, and can be appropriately selected depending on the film formation method. The workpiece may contain at least one selected from the group consisting of Si, Ge, and oxides thereof, in addition to the SiGe compound, and preferably contains SiO2.

[0043] <Step of Etching Object> This step is a step of etching a workpiece containing a SiGe compound using the etching solution according to the first embodiment, and includes an operation of contacting the workpiece with the etching solution. The etching method is not particularly limited, and a known etching method can be used. Examples of such methods include, but are not limited to, a spray method, a dipping method, a liquid puddle method, and the like. In the spray method, for example, the object to be treated is conveyed or rotated in a predetermined direction, and the etching solution according to the first aspect is sprayed into the space formed by the conveyed object to contact the etching solution with the object to be treated. If necessary, the etching solution may be sprayed while rotating the substrate using a spin coater. In the immersion method, the object to be treated is immersed in the etching solution according to the first aspect to bring the etching solution into contact with the object to be treated. In the puddle method, the etching liquid according to the first aspect is puddled on the object to be treated, and the object to be treated is brought into contact with the etching liquid. These etching methods can be appropriately selected depending on the structure, material, etc. of the object to be treated. In the case of the spray method or the puddle method, the amount of the etching liquid supplied to the object to be treated may be an amount that allows the surface of the object to be treated to be sufficiently wetted with the etching liquid.

[0044] The purpose of the etching process is not particularly limited, and may be fine processing of a surface of a workpiece containing a SiGe compound (e.g., a SiGe compound-containing layer on a substrate), removal of a SiGe compound-containing deposit adhering to a workpiece (e.g., a substrate having a SiGe compound-containing layer), or cleaning of a surface of a workpiece containing a SiGe compound (e.g., a SiGe compound-containing layer on a substrate).

[0045] The temperature at which the etching process is carried out is not particularly limited, and may be any temperature at which the SiGe compound dissolves in the etching solution. The etching temperature may be, for example, 15 to 60°C. In any of the spray method, the immersion method, and the puddle method, the etching rate increases by increasing the temperature of the etching solution, but the processing temperature can be appropriately selected while keeping the composition change of the etching solution small, and taking into consideration workability, safety, cost, etc.

[0046] The time for performing the etching process may be appropriately selected depending on the purpose of the etching process, the amount of the SiGe compound to be removed by etching (e.g., the thickness of the SiGe compound-containing layer, the amount of SiGe compound deposits, etc.), and the etching process conditions.

[0047] <Other processes> The method for manufacturing a semiconductor device according to the present embodiment may include other steps in addition to the etching process. The other steps are not particularly limited, and include known steps carried out when manufacturing a semiconductor device. Examples of such steps include, but are not limited to, channel formation, High-K / metal gate formation, metal wiring, gate structure, source structure, drain structure, insulating layer, ferromagnetic layer, and nonmagnetic layer structure formation steps (layer formation, etching other than the above etching process, chemical mechanical polishing, transformation, etc.), resist film formation step, exposure step, development step, heat treatment step, cleaning step, inspection step, etc. These other steps may be carried out as necessary before or after the above etching process step.

[0048] According to the method for manufacturing a semiconductor device of the present embodiment described above, an etching process for an object to be treated is performed using the etching solution according to the first aspect, which contains specific amounts of hydrofluoric acid, nitric acid, and water. The etching solution has a general formula Si 1-x Ge xIt is possible to selectively etch a compound represented by the formula (SiGe compound) and suppress the etching stop of the SiGe compound. Therefore, according to the manufacturing method of the semiconductor element of this embodiment, a semiconductor element in which the SiGe compound is selectively etched can be obtained without substantially affecting Si, Ge, and their oxides. Furthermore, according to the manufacturing method of the semiconductor element of this embodiment, since the etching stop of the SiGe compound is suppressed, the SiGe compound can be selectively etched for a longer period of time (for example, 3 minutes or more) than in the past. Therefore, the manufacturing method of the semiconductor element of this embodiment does not require a complicated etching process, and not only improves the etching uniformity in the surface, but also shortens the processing time, resulting in low costs and high practicality. EXAMPLES

[0049] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0050] <Preparation of etching solution (1)> (Examples 1 to 6, Comparative Examples 1 to 6) The components shown in Table 1 were mixed to prepare the etching solutions of the respective examples.

[0051] [Table 1]

[0052] In Table 1, the abbreviations have the following meanings: DHF: Hydrofluoric acid HNO3: Nitric acid AcOH: acetic acid DIW: Water

[0053] <Etching of object to be treated (1)> A SiGe film was epitaxially grown on a silicon substrate to obtain a processed object (1) on which a SiGe film was formed. A test piece was cut from the obtained processed object (1) and the thickness of the SiGe film was measured by fluorescent X-ray analysis, and the thickness was found to be 50 nm. The etching solution of each example was placed in a beaker, and the test piece was immersed in the etching solution of each example for 5 minutes at room temperature (23°C) to perform an etching process. After the etching process, the test piece was dried by nitrogen blowing, and the thickness of the SiGe film was measured by fluorescent X-ray analysis. The etching rate (nm / min) for SiGe was calculated from the thickness of the SiGe film before and after the etching process. The results are shown in Table 2.

[0054] <Etching of object to be treated (2)> A silicon oxide film was formed on a silicon substrate by thermal oxidation to obtain a processed object (2). A test piece was cut from the obtained processed object (2) and the thickness of the silicon oxide film was measured by spectroscopic ellipsometry, and the thickness was 100 nm. The etching solution of each example was placed in a beaker, and the test piece was immersed in the etching solution of each example for 5 minutes at room temperature (23°C) to carry out an etching treatment. After the etching treatment, the test piece was dried by nitrogen blowing, and the thickness of the silicon oxide film was measured by spectroscopic ellipsometry. From the thickness of the silicon oxide film before and after the etching treatment, Not. The etching rate (nm / min) for 2 was calculated. The results are shown in Table 2.

[0055] <Etching of object to be treated (3)> A test piece was cut from the SOI (100) substrate to obtain the treated object (3). The thickness of the Si film of the treated object (3) was measured by spectroscopic ellipsometry, and the thickness was 100 nm. The etching solution of each example was placed in a beaker, and the test piece was immersed in the etching solution of each example for 5 minutes at room temperature (23°C) to perform an etching treatment. After the etching treatment, the test piece was dried by nitrogen blowing, and the thickness of the Si film was measured by spectroscopic ellipsometry. The etching rate (nm / min) for Si was calculated from the thickness of the Si film before and after the etching treatment. The results are shown in Table 2.

[0056] <Evaluation of Etching Selectivity (1)> Based on the etching rate results obtained in the above "etching process (1) of processed object", "etching process (2) of processed object" and "etching process (3) of processed object", the etching selectivity ratio of processed object (1) / processed object (2) and the etching selectivity ratio of processed object (1) / processed object (3) were calculated. The results are shown in Table 2.

[0057] <Evaluation of Etching Stop (1)> In the above "etching treatment of treated object (1)", the etching rate (nm / min) for SiGe was calculated when the etching treatment time was changed as follows according to the obtained SiGe etching rate (nm / min), and evaluated according to the following criteria. When the SiGe etching rate is 10nm / min or less Etching times of 1 minute, 3 minutes, and 5 minutes were compared and evaluated according to the following evaluation criteria. ◎: The etching rate (nm / min) for SiGe after 1 minute of etching treatment varies by 20% or less from the etching rate for SiGe after 5 minutes of etching treatment. △: The etching rate (nm / min) for SiGe after 1 minute of etching process varies by more than 20% from the etching rate for SiGe after 5 minutes of etching process. ×: Etching rate for SiGe after 5 minutes of etching is 0.6 nm / min or less ·SiGe etching rate is over 10nm / min and 20nm / min or less The etching times were compared at 30 seconds, 90 seconds, and 150 seconds, and the results were evaluated according to the following criteria. ◎: The etching rate (nm / min) for SiGe after 30 seconds of etching treatment varies by 20% or less from the etching rate for SiGe after 150 seconds of etching treatment. △: The etching rate (nm / min) for SiGe after 30 seconds of etching process varies by more than 20% from the etching rate for SiGe after 150 seconds of etching process. ×: Etching rate for SiGe after 5 minutes of etching is 0.6 nm / min or less ·SiGe etching rate is over 20nm / min and 50nm / min or less The etching times were compared at 20 seconds, 40 seconds, and 60 seconds, and the results were evaluated according to the following criteria. ◎: The etching rate (nm / min) for SiGe after 20 seconds of etching treatment varies by 20% or less from the etching rate for SiGe after 60 seconds of etching treatment. △: The etching rate (nm / min) for SiGe after 20 seconds of etching process varies by more than 20% from the etching rate for SiGe after 60 seconds of etching process. ×: Etching rate for SiGe after 5 minutes of etching is 0.6 nm / min or less

[0058] [Table 2]

[0059] From the results shown in Table 2, it was confirmed that the etching solutions of Examples 1 to 6 had higher SiGe etching selectivity and suppressed the etching stop of SiGe, as compared with the etching solutions of Comparative Examples 1 to 6.

[0060] (Examples 7 to 10, Comparative Example 7) The components shown in Table 3 were mixed to prepare the etching solutions of the respective examples.

[0061] [Table 3]

[0062] In Table 3, the abbreviations have the following meanings: DHF: Hydrofluoric acid HNO3: Nitric acid AcOH: acetic acid H3PO4: Phosphoric acid DIW: Water

[0063] <Etching of object to be treated (4)> The etching rate (nm / min) for SiGe was calculated in the same manner as in "<Etching treatment of treated object (1)>" above, except that the etching solutions of Comparative Example 7 and Examples 7 to 10 were used. The results are shown in Table 4.

[0064] <Etching of object to be treated (5)> The etching rate (nm / min) for Si was calculated in the same manner as in "<Etching treatment of treated object (2)>" above, except that the etching solutions of Comparative Example 7 and Examples 7 to 10 were used. The results are shown in Table 4.

[0065] <Etching of object to be treated (6)> The etching rate (nm / min) for Si was calculated in the same manner as in "<Etching treatment of treated object (3)>" above, except that the etching solutions of Comparative Example 7 and Examples 7 to 10 were used. The results are shown in Table 4. <Evaluation of Etching Selectivity (2)> Based on the etching rate results obtained in the above "etching process (4) of processed object," "etching process (5) of processed object," and "etching process (6) of processed object," the etching selectivity ratio of processed object (4) / processed object (5) and the etching selectivity ratio of processed object (4) / processed object (6) were calculated. The results are shown in Table 4.

[0066] <Evaluation of Etching Stop (2)> In the above "etching of the processed object (4)", the etching rate (nm / min) for SiGe was calculated when the etching time was changed in the same manner as in the above "Evaluation of etching stop (1)" according to the obtained SiGe etching rate (nm / min), and evaluated according to the same criteria as in the above "Evaluation of etching stop (1)". The results are shown in Table 4.

[0067] [Table 4]

[0068] From the results shown in Table 4, it was confirmed that the etching solutions of Examples 7 to 10 had higher SiGe etching selectivity than the etching solution of Comparative Example 7, and also suppressed the etching stop of SiGe.

Claims

1. General formula Si 1-x Ge x An etching solution for etching a compound represented by the formula: (wherein x is greater than 0 and less than 1), Contains hydrofluoric acid, nitric acid, and water, The content of the hydrofluoric acid in the entire etching solution is 0.02 mass% or more and 0.1 mass% or less, The content of the nitric acid in the entire etching solution is 10% by mass or more and 40% by mass or less, The content ratio of the water in the entire etching solution is 9.9 mass% or more and 40 mass% or less, Further, the etching solution contains acetic acid as a polar solvent.

2. The etching solution according to claim 1 , further comprising phosphoric acid and / or a derivative thereof.

3. The etching solution according to claim 1 or 2 is used to form a compound having the general formula Si 1-x Ge x A method for manufacturing a semiconductor device, comprising the step of etching a processing object containing a compound represented by the formula:

Citation Information

Patent Citations

  • Etching agent

    JP2003183652A

  • PAA system etching liquid, etching method utilizing it, and structure of resultant material

    JP2005303305A

  • Method of manufacturing semiconductor device

    JP2007227602A

  • Method of manufacturing semiconductor device

    JP2008160073A

  • Etching compositions for silicon germanium and etching methods using the same

    US20040242015A1